Polishing Pad
The polyurethane resin foam polishing pad with controlled viscoelastic properties and bubble diameters addresses the need for enhanced polishing speed and surface flatness, achieving high efficiency and reduced surface defects.
Patent Information
- Application Number
- JP2020212406
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-22
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-12-22
AI Technical Summary
Existing polishing pads fail to adequately increase polishing speed and improve the flatness of polished surfaces, particularly for materials like silicon wafers and glass plates.
A polishing pad composed of polyurethane resin foam with specific viscoelastic properties, characterized by a tan δ value of 0.1 to 0.4 within 25°C to 75°C and bubble diameters ranging from 100 μm to 200 μm, ensuring balanced viscosity and elasticity, which enhances polishing efficiency and surface flatness.
The polishing pad significantly increases polishing rate and maintains excellent surface flatness by controlling viscoelastic properties and suppressing bubble collapse, reducing scratches and improving surface roughness.
Smart Images

Figure 0007594431000003 
Figure 0007594431000004 
Figure 0007594431000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing pad. [Background technology]
[0002] 2. Description of the Related Art As a polishing pad for polishing a workpiece such as a silicon wafer or a glass plate, a polishing pad having a polishing surface formed of a polyurethane resin foam is known (for example, Patent Document 1, etc.).
[0003] As a method for polishing an object to be polished using the polishing pad, for example, the following method is available. First, a disk-shaped object to be polished is attached to the lower surface of an upper platen of a polishing machine, and a disk-shaped polishing pad is attached to the upper surface of the lower platen of the polishing machine. The lower surface (surface to be polished) of the object to be polished is then pressed against the upper surface (polishing surface) of the polishing pad by the upper and lower surface plates. Next, with the object to be polished pressed against the polishing pad, a polishing slurry is supplied onto the polishing pad while the upper platen and the lower platen are rotated, thereby polishing the object to be polished. As the polishing slurry, a polishing slurry containing water and abrasive grains is used. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2010-274361 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, there has been an increasing demand to sufficiently increase the polishing rate of an object to be polished while improving the flatness of the polished surface after polishing, but it cannot be said that sufficient research has been carried out on this issue.
[0006] In view of the above-mentioned demand, an object of the present invention is to provide a polishing pad that can sufficiently increase the polishing rate of an object to be polished while improving the flatness of the polished surface after polishing. [Means for solving the problem]
[0007] The polishing pad according to the present invention comprises: A polishing pad comprising a polyurethane resin foam, having a polished surface, the polishing surface is formed by the surface of the polyurethane resin foam, The polyurethane resin foam has a tan δ value of 0.1 or more and less than 0.4 within a temperature range of 25° C. or more and 75° C. or less, a volumetric cell diameter distribution curve of the polyurethane resin foam has a first peak when plotted with the cell diameter on the horizontal axis and the cell volume on the vertical axis; The bubble diameter at the peak top of the first peak is within the range of 100 μm or more and 200 μm or less. Effect of the Invention
[0008] According to the present invention, it is possible to provide a polishing pad capable of sufficiently increasing the polishing rate of an object to be polished while improving the flatness of the polished surface after polishing. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic diagram showing a state in which a polishing pad is used. [Diagram 2] 4 is a graph showing the results of measuring tan δ (loss tangent) for the polishing pads of each example. [Diagram 3] 6 is a graph showing the results of determining the volumetric bubble diameter distribution curve for the polishing pads according to the respective examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, one embodiment of the present invention (hereinafter also referred to as the present embodiment) will be described.
[0011] The polishing pad according to this embodiment includes a polyurethane resin foam containing a polyurethane resin. The polishing pad according to this embodiment has a polishing surface, which is constituted by the surface of the polyurethane resin foam.
[0012] As shown in FIG. 1, the polishing pad 1 according to this embodiment is used for polishing the surface of an object 2 to be polished in a polishing apparatus 100.
[0013] The polishing pad 1 according to this embodiment has a polishing surface 1a for polishing an object 2 to be polished, and the polishing surface 1a is composed of the surface of the polyurethane resin foam. The polishing pad 1 of this embodiment polishes the surface 2a to be polished by placing a polishing slurry containing abrasive grains between the polishing surface 1a and the surface 2a to be polished, thereby bringing the polishing surface 1a and the surface 2a to be polished into sliding contact with each other.
[0014] In the polishing pad 1 according to this embodiment, the polyurethane resin foam has a tan δ (loss tangent; loss modulus E″ / storage modulus E′) value of 0.1 or more and less than 0.4 within a temperature range of 25° C. or more and 75° C. or less. In the temperature range of 25° C. or more and 75° C. or less, the value of tan δ is preferably 0.15 or more and 0.3 or less. In the polishing pad 1 according to this embodiment, tan δ, which is the minimum value of tan δ within the temperature range of 25° C. or more and 75° C. or less, MIN The maximum value of tanδ in the range of 25°C to 75°C for MAX Ratio of (tan δ MAX / tanδ MIN ) may be 2.0 or less. In addition, in the polishing pad 1 according to this embodiment, tan δ MAX / tanδ MIN may be 0.8 or more and less than 1.5.
[0015] Tan δ can be calculated by measuring the loss modulus E″ and the storage modulus E′. The loss modulus E'' and the storage modulus E' can be measured under the following conditions in accordance with JIS K7244-4:1999 "Plastics - Test methods for dynamic mechanical properties - Part 4: Tensile vibration - Non-resonant method". (Measurement conditions for loss modulus E'' and storage modulus E') Measurement temperature range: 10℃~100℃ Heating rate: 5℃ / min Frequency: 1Hz Distortion: 0.5%
[0016] In the polishing pad 1 of this embodiment, the distribution curve of the volumetric bubble diameter of the polyurethane resin foam has a first peak when plotted with the horizontal axis representing the bubble diameter and the vertical axis representing the bubble volume, and the bubble diameter at the peak top of the first peak is in the range of 100 μm or more and 200 μm or less. More specifically, in the polishing pad 1 of this embodiment, the distribution curve of the volumetric bubble diameter of the polyurethane resin foam, when plotted with the horizontal axis representing the bubble diameter and the vertical axis representing the bubble volume, has one or more peaks, and the bubble diameter at the peak top of one of the one or more peaks is in the range of 100 μm or more and 200 μm or less. That is, when the volumetric cell diameter distribution curve of the polyurethane resin foam has one peak, this peak is the first peak, and the cell diameter at the peak top of the first peak is in the range of 100 μm or more and 200 μm or less, and when the volumetric cell diameter distribution curve of the polyurethane resin foam has two or more peaks, the cell diameter at the peak top of the first peak, which is one of the two or more peaks, is in the range of 100 μm or more and 200 μm or less.
[0017] The bubble diameter at the peak top of the first peak is preferably in the range of 100 μm or more and 180 μm or less, and more preferably in the range of 100 μm or more and 160 μm or less.
[0018] Here, because polyurethane resin foam is a viscoelastic material, in a polishing pad whose polishing surface is formed by polyurethane resin foam, unless the viscoelastic properties are properly controlled, when polishing an object to be polished such as a silicon wafer or a glass plate, micro-vibrations may occur between the polishing surface of the polishing pad and the polished surface of the object to be polished, making it impossible to ensure a sufficient flatness of the polished surface after polishing (as the pad becomes less likely to behave as a viscous material, it becomes impossible to ensure a sufficient flatness of the polished surface after polishing). Furthermore, if polishing progresses before the compressed polishing pad has fully recovered, it may become impossible to ensure a sufficient flatness of the polished surface after polishing (as the pad becomes less likely to behave as an elastic material, it becomes impossible to ensure a sufficient flatness of the polished surface after polishing). Furthermore, when a polishing pad having a polishing surface formed from polyurethane resin foam is used to polish a workpiece such as a silicon wafer or a glass plate, the polishing begins at a temperature of about 25°C, but the temperature of the polishing surface of the polishing pad may rise to about 75°C during polishing due to frictional heat generated by polishing the workpiece with the polishing pad. Therefore, it is preferable that a polishing pad having a polishing surface formed of a polyurethane resin foam exhibits suitable viscoelastic properties within a temperature range of 25°C or higher and 75°C or lower.
[0019] As described above, in the polishing pad 1 according to this embodiment, the value of tan δ is 0.1 or more and less than 0.4 within the temperature range of 25° C. or more and 75° C. or less. That is, in the polishing pad 1 according to this embodiment, the value of the loss modulus E″ as a viscous term and the value of the storage modulus E′ as an elastic term are appropriately controlled and suitably balanced (viscosity and elasticity are suitably balanced). This makes it possible to ensure sufficient flatness of the polished surface after polishing.
[0020] Furthermore, in the polishing pad 1 according to this embodiment, as described above, when the distribution curve of the volumetric bubble diameter of the polyurethane resin foam is plotted with the horizontal axis representing the bubble diameter and the vertical axis representing the bubble volume, it has a first peak, and the bubble diameter at the peak top of the first peak is in the range of 100 μm or more and 200 μm or less. In other words, since the bubble diameter at the peak top of the first peak is relatively large, the polyurethane resin foam is stretched during polishing, which prevents the bubbles from collapsing. Furthermore, when the polishing surface of the polishing pad is dressed, the polyurethane resin foam is stretched, which prevents the air cells from collapsing. Therefore, the polishing pad 1 of this embodiment can adequately retain the polishing slurry, thereby ensuring a sufficient polishing rate, and also ensuring sufficient flatness of the polished surface after polishing.
[0021] From a microscopic point of view, within the area where the workpiece is in contact during polishing, the temperature of the polishing surface may locally exceed the above range (25° C. or higher and 75° C. or lower). In such a case, in order to allow the relevant portion to exhibit excellent flexibility, the polyurethane resin foam may contain a component that exhibits a glass transition temperature (Tg) or melting temperature (Tm) higher than the above range. That is, the polyurethane resin foam may have a peak value in the range of more than 75° C. and not more than 100° C. in a graph showing the change in tan δ with temperature (FIG. 2 described in the Examples section). The peak value is preferably within the range of tan δ from 25° C. to 75° C.
[0022] In the polishing pad 1 of this embodiment, the distribution curve of the volumetric bubble diameter of the polyurethane resin foam, when plotted with the horizontal axis representing the bubble diameter and the vertical axis representing the bubble volume, further has a second peak, and it is preferable that the bubble diameter at the peak top of the second peak is less than 100 μm. More specifically, in the polishing pad 1 of this embodiment, the distribution curve of the volumetric bubble diameter of the polyurethane resin foam has two or more peaks when plotted with the bubble diameter on the horizontal axis and the bubble volume on the vertical axis, and it is preferable that the bubble diameter at the peak top of the second peak, which is one of the two or more peaks, is less than 100 μm. As described above, the bubble diameter at the peak top of the first peak, which is one of the two or more peaks, is in the range of 100 μm or more and 200 μm or less.
[0023] As described above, by making the bubble diameter at the peak top of the second peak less than 100 μm, the flatness of the polished surface after polishing can be more sufficiently improved. The present inventors consider the reason why the flatness of the polished surface after polishing can be more sufficiently improved by having the bubble diameter at the peak top of the second peak within the above numerical range as follows.
[0024] In a polishing pad containing a polyurethane resin foam, the air bubbles contained in the polyurethane resin foam form convex portions on the polishing surface of the polishing pad, and these convex portions serve as contact points (hereinafter also referred to as contact points) with the workpiece (e.g., a silicon wafer, etc.). Furthermore, when the polyurethane resin foam contains small-diameter bubbles having a bubble diameter of less than 100 μm, the convex portions formed on the polishing surface of the polishing pad become smaller, and the contact points between the convex portions and the workpiece become smaller. At such small contact points, the contact area between the polishing pad and the workpiece is relatively small, and the contact resistance between the polishing pad and the workpiece is small, which is thought to enable the polishing of the workpiece by the polishing pad to be carried out smoothly. That is, when the polyurethane resin foam contains small-diameter bubbles having a bubble diameter of less than 100 μm, the polishing of the workpiece with a polishing pad containing the polyurethane resin foam proceeds relatively smoothly, and the planarization characteristics (surface roughness (arithmetic mean surface roughness Ra) and ΔGBIR described below) of the polished surface of the workpiece are considered to be good. In particular, when there are relatively many small protrusions on the polishing surface of the polishing pad, the planarization characteristics of the polished surface of the workpiece are considered to be even better. Furthermore, if the contact point is small, the contact pressure generated at the contact point during polishing of the workpiece by the polishing pad can be made relatively small, thereby preventing excessive contact pressure from being applied to the polished surface of the workpiece. This is believed to be able to suppress the occurrence of scratches (e.g., microscratches) on the polished surface of the workpiece. In particular, when the polishing surface of the polishing pad has a relatively large number of small protrusions, it is believed that the occurrence of scratches on the polished surface of the workpiece can be further suppressed.
[0025] It is more preferable that the bubble diameter at the peak top of the second peak is within a range of 80 μm or less. The bubble diameter at the peak top of the second peak is preferably in the range of 20 μm or more.
[0026] The polyurethane resin foam preferably has an average cell diameter of 30 μm or more and 70 μm or less, and more preferably 40 μm or more and 70 μm or less. When the average bubble diameter is within the above range, the polishing rate of the object to be polished can be more sufficiently increased while the flatness of the surface of the object to be polished can be more sufficiently increased.
[0027] The volumetric bubble diameter distribution curve can be obtained as follows using an X-ray CT scanner (for example, TDM1000H-I manufactured by Yamato Scientific Co., Ltd.). That is, the volume of each bubble contained in the measurement range of the polyurethane resin foam (e.g., planar dimensions: 1.6 mm × 1.6 mm, thickness 0.7 mm) is measured, and the diameter of each bubble is determined as the diameter of a true sphere with the same volume. Here, the above "average bubble size" refers to the arithmetic average bubble size calculated from the volume of each bubble [= total value of "each bubble size" / (number of bubbles)]. The volumetric bubble diameter distribution curve can be obtained based on the data of the number-based bubble diameter distribution curve. That is, the number of bubbles is calculated at regular intervals starting from a bubble diameter of 0 μm, and the "number of bubbles at each interval" is set as the "number of bubbles at the upper limit bubble diameter at each interval" to calculate a number-based bubble diameter distribution curve. Based on the data of this number-based bubble diameter distribution curve, the sum of the bubble volumes is calculated at regular intervals starting from a bubble diameter of 0 μm, and the "sum of bubble volumes" is set as the "volume at the upper limit bubble diameter at each interval" to calculate a volume-based bubble diameter distribution curve. From the viewpoint of determining the peak position with greater accuracy, the above-mentioned constant interval is preferably set to 20 μm or less.
[0028] The cell diameter at the peak top of the first peak is the cell diameter at the point where the differential value obtained by differentiating the cell count in the volumetric cell diameter distribution curve with respect to the cell diameter three times becomes 0. The cell diameter at the peak top of the second peak is also the cell diameter at the point where the differential value obtained by differentiating the cell count in the volumetric cell diameter distribution curve with respect to the cell diameter three times becomes 0.
[0029] Furthermore, the polyurethane resin foam preferably has a difference between the bubble diameter at a cumulative volume frequency of 80% and the bubble diameter at a cumulative volume frequency of 10%, calculated from a volumetric bubble diameter distribution curve (bubble diameter at a cumulative volume frequency of 80% - bubble diameter at a cumulative volume frequency of 10%) of 60 μm or more, and more preferably 70 μm or more. By setting the difference between the bubble diameter at a cumulative volume frequency of 80% and the bubble diameter at a cumulative volume frequency of 10% within the above range, the bubble diameters can be distributed over a relatively wide range. This makes it possible to prevent the bubbles from collapsing during polishing. In addition, it is possible to prevent the bubbles from collapsing when the polishing surface of the polishing pad is dressed.
[0030] The polyurethane resin foam preferably has a JIS-A hardness of 65 or more and 80 or less. By having the JIS-A hardness within the above range, it is possible to more sufficiently increase the polishing rate of the object to be polished while more sufficiently increasing the flatness of the surface of the object to be polished.
[0031] The JIS-A hardness of the polyurethane resin foam can be measured as follows. (JIS-A hardness measurement method) JIS-A hardness is measured using a method (Type A) that complies with JIS K6253-3:2012. In this measurement, if the thickness of the polyurethane resin foam is less than 12 mm, a plurality of polyurethane resin foams are laminated to make the thickness of the laminate 12 mm or more, and the hardness of the laminate is measured. The JIS-A hardness is the hardness (instantaneous value) measured by pressing a needle into the polished surface.
[0032] The polyurethane resin foam contains a plurality of cells and has an apparent density of 0.3 g / cm 3 More than 0.6g / cm 3 It is preferable that: The apparent density of the polyurethane resin foam is 0.4 g / cm 3 More than 0.6g / cm 3 More preferably, it is 0.4 g / cm or less. 3 More than 0.5g / cm 3 It is even more preferable that: The apparent density can be measured based on JIS K 7222:2005.
[0033] The polyurethane resin foam preferably has a compressibility of 3% or more and 10% or less, and more preferably 4% or more and 9% or less. When the compression ratio is within the above range, the polishing speed of the object to be polished can be more sufficiently increased, while the flatness of the surface of the object to be polished can be more sufficiently increased. The compression ratio can be calculated according to the following procedure. (1) A compression elasticity tester according to JIS L1096:2010 (indenter area: 50 mm 2 ) with a pressure of 641gf / cm 2 While applying a pressure of this magnitude, the polyurethane resin foam is pressed in the thickness direction and maintained for 60 seconds, and then the thickness T1 of the polyurethane resin foam is measured. (2) 5161 gf / cm with pressure probe 2 While applying a pressure of this magnitude, the polyurethane resin foam is pressed in the thickness direction and maintained for 60 seconds, and then the thickness T2 of the polyurethane resin foam is measured. (3) Calculate the compression ratio using the following formula: Compression ratio = (T1-T2)×100 / T1
[0034] The polyurethane resin foam according to this embodiment preferably has a porosity of 50% or more. The porosity of the polyurethane resin foam is more preferably 60% or more, and further preferably 65% or more. The porosity is preferably 80% or less, and more preferably 78% or less.
[0035] The porosity can be determined as follows using an X-ray CT scanner (for example, TDM1000H-I manufactured by Yamato Scientific Co., Ltd.). That is, the volume of each bubble contained in the measurement range of the polyurethane resin foam (e.g., two portions of 0.7 mm x 1.6 mm x 1.6 mm) can be measured, and the ratio of the total volume of the bubbles to the volume of the measurement range of the polyurethane resin foam can be calculated.
[0036] The polyurethane resin contained in the polyurethane resin foam may be the same as that used in general polishing pads. The polyurethane resin contains a polyisocyanate compound (for example, a prepolymer having isocyanate groups at both ends of the molecular chain) and a curing agent. That is, the polyurethane resin foam according to the present embodiment is prepared by preparing a liquid mixture containing the polyisocyanate compound and the curing agent, incorporating air bubbles into the mixture, and curing the mixture.
[0037] The polyurethane resin foam preferably contains a polyurethane resin containing a curing agent in a ratio of 10 parts by mass or more and 30 parts by mass or less per 100 parts by mass of a polyisocyanate compound. The ratio of the curing agent to the polyisocyanate compound is more preferably 10 parts by mass or more and 20 parts by mass or less.
[0038] The polyurethane resin is preferably prepared so that the R value (active hydrogen / NCO), which is the equivalent ratio of the active hydrogen group of the curing agent to the isocyanate group present at the end of the polyisocyanate compound, is 0.6 or more and 0.9 or less. The R value is more preferably 0.75 or more and 0.85 or less.
[0039] The polyisocyanate compound of the present embodiment may be, for example, a urethane prepolymer that contains, as constituent units, one or more types of polyols and one or more types of polyisocyanates and has an isocyanate group at its terminal. The polyisocyanate compound of the present embodiment may be a mixture of a plurality of urethane prepolymers, or may be one or more of the polyisocyanates described later. The polyisocyanate compound of the present embodiment may be a mixture of one or more types of urethane prepolymers and one or more types of polyisocyanates.
[0040] Examples of the polyol include aromatic polyols such as 1,4-benzenedimethanol and 1,4-bis(2-hydroxyethoxy)benzene; aliphatic polyols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, and 2-methyl-1,8-octanediol; alicyclic polyols such as 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, and water-added bisphenol A; and polyfunctional polyols such as glycerin, trimethylolpropane, tributyrolpropane, pentaerythritol, and sorbitol.
[0041] The polyol may be, for example, a polyol polymer such as a polyester polyol, a polyester polycarbonate polyol, a polyether polyol, or a polycarbonate polyol. The polyol polymer may be a polyfunctional polyol polymer having three or more hydroxy groups in the molecule.
[0042] Examples of the polyester polyol include polyethylene adipate glycol, polybutylene adipate glycol, polycaprolactone polyol, and polyhexamethylene adipate glycol.
[0043] Examples of the polyester polycarbonate polyol include a reaction product of a polyester glycol such as polycaprolactone polyol with an alkylene carbonate, and a reaction product obtained by reacting ethylene carbonate with a polyhydric alcohol, which is then reacted with an organic dicarboxylic acid.
[0044] Examples of the polyether polyol include polytetramethylene ether glycol (PTMG), polypropylene glycol (PPG), polyethylene glycol (PEG), and ethylene oxide-added polypropylene polyol.
[0045] Examples of the polycarbonate polyol include reaction products of diols such as 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, polyethylene glycol, polypropylene glycol, or polytetramethylene ether glycol with phosgene, diallyl carbonate (e.g., diphenyl carbonate), or cyclic carbonate (e.g., propylene carbonate).
[0046] Examples of the polyisocyanate include aromatic isocyanates, aliphatic isocyanates, and alicyclic isocyanates.
[0047] Examples of the aromatic isocyanate include tolylene diisocyanate (TDI), 1,5-naphthalene diisocyanate, xylylene diisocyanate, 1,3-phenylene diisocyanate, and 1,4-phenylene diisocyanate. Examples of the aromatic isocyanate include diphenylmethane diisocyanate (MDI) and modified products of diphenylmethane diisocyanate (MDI).
[0048] Examples of modified diphenylmethane diisocyanate (MDI) include carbodiimide modified, urethane modified, allophanate modified, urea modified, biuret modified, isocyanurate modified, oxazolidone modified, etc. Specific examples of such modified products include carbodiimide-modified diphenylmethane diisocyanate (carbodiimide-modified MDI).
[0049] Examples of the aliphatic diisocyanate include ethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate (HDI).
[0050] Examples of the alicyclic diisocyanate include 1,4-cyclohexane diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, isophorone diisocyanate, norbornane diisocyanate, and methylenebis(4,1-cyclohexylene) diisocyanate.
[0051] The curing agent in this embodiment may be, for example, a polyamine.
[0052] Examples of the polyamine include 4,4'-methylenebis(2-chloroaniline) (MOCA), 4,4'-methylenedianiline, trimethylenebis(4-aminobenzoate), 2-methyl-4,6-bis(methylthio)benzene-1,3-diamine, 2-methyl-4,6-bis(methylthio)-1,5-benzenediamine, 2,6-dichloro-p-phenylenediamine, 4,4'-methylenebis(2,3-dichloroaniline), Examples of the toluene diamine include 3,5-bis(methylthio)-2,4-toluenediamine, 3,5-bis(methylthio)-2,6-toluenediamine, 3,5-diethyltoluene-2,4-diamine, 3,5-diethyltoluene-2,6-diamine, trimethylene glycol-di-p-aminobenzoate, 1,2-bis(2-aminophenylthio)ethane, and 4,4'-diamino-3,3'-diethyl-5,5'-dimethyldiphenylmethane.
[0053] The curing agent may be the polyol. The curing agent may be a mixture of the polyol and the polyamine.
[0054] Water may be used as a foaming agent for foaming the polyurethane resin. The apparent density of the polyurethane resin foam can be adjusted by the amount of water added, the R value, and the like. When water is used as a blowing agent, the amount of water added is preferably 0.2 parts by mass or more and 1 part by mass or less per 100 parts by mass of the polyisocyanate compound, so that the polyurethane resin foam can be easily prepared to have the above-mentioned apparent density. The amount of water added per 100 parts by mass of the polyisocyanate compound is more preferably 0.3 parts by mass or more and 1 part by mass or less.
[0055] The polyurethane resin foam may contain a catalyst for promoting the reaction between the polyisocyanate compound and the curing agent, and a foam stabilizer for controlling the formation of bubbles.
[0056] When the polyurethane resin foam contains the catalyst, examples of the catalyst include amine-based catalysts such as N,N-dimethylaminoethyl ether, triethylenediamine, dimethylethanolamine, triethanolamine, N,N,N',N'-tetramethylhexamethylenediamine, and N-methylimidazole, and organometallic catalysts such as dioctyltin dilaurate. The catalysts may be used alone or in combination of two or more.
[0057] When the polyurethane resin foam contains the catalyst, the content of the catalyst in the polyurethane resin foam is preferably 0.03 parts by mass or more and 0.1 parts by mass or less per 100 parts by mass of the polyisocyanate compound, since this makes it easy to adjust the size and number of air bubbles to the desired state. The content of the catalyst is more preferably 0.05 parts by mass or more and 0.1 parts by mass or less.
[0058] The foam stabilizer used in this embodiment includes, for example, a silicone surfactant.
[0059] The content of the foam stabilizer in the polyurethane resin foam is preferably 1 part by mass or more and 10 parts by mass or less based on 100 parts by mass of the polyisocyanate compound in order to ensure the effect of the foam stabilizer.
[0060] Examples of objects to be polished with the polishing pad according to this embodiment include optical materials, semiconductor devices, hard disks, glass plates, silicon wafers, and the like. Moreover, the polishing pad according to this embodiment is suitable for use in polishing silicon wafers and glass plates. Furthermore, the polishing pad according to this embodiment is suitable for use in finish polishing, precision polishing, and the like.
[0061] Next, a method for producing the polishing pad according to this embodiment will be described.
[0062] In the method for manufacturing a polishing pad according to this embodiment, a polishing pad having a polyurethane resin foam is manufactured. In addition, in the manufacturing method of the polishing pad according to this embodiment, a urethane prepolymer having an isocyanate group as a terminal group, microcapsules, and a foam stabilizer are mixed to obtain a dispersion liquid in which the microcapsules and air as bubbles are dispersed. The dispersion is mixed with a curing agent having a plurality of active hydrogens in the molecule, followed by polymerization, to obtain a polishing pad having a polyurethane resin foam. In addition, by using a urethane prepolymer having polypropylene glycol (PPG) as a soft segment and a urethane prepolymer having polytetramethylene ether glycol (PTMG) as a soft segment, and using 4,4'-methylenebis(2-chloroaniline) (MOCA) as a curing agent, it becomes easy to adjust the tan δ value of the polyurethane foam to 0.1 or more and less than 0.4 within a temperature range of 25°C or more and 75°C or less, and to adjust the cell diameter at the peak top of the first peak to 100 μm or more and 200 μm or less.
[0063] The microcapsules include thermally expandable microcapsules (thermally expandable hollow fine particles). The thermally expandable microcapsules may be used in an unexpanded state, or in an expanded state obtained by thermal expansion. The microcapsules are also called "microspheres" or "microspheres". The thermally expandable microcapsule comprises a hollow body formed of a thermoplastic resin and a liquid hydrocarbon contained in the hollow portion of the hollow body. The thermally expandable microcapsules are expanded by vaporizing liquid hydrocarbons due to heat.
[0064] Examples of the thermoplastic resin include acrylonitrile resin and polyvinylidene chloride resin. The thermoplastic resin is preferably a thermoplastic resin having a glass transition temperature of 70 to 130° C., from the viewpoint that the heat of polymerization reaction can sufficiently expand the thermally expandable microcapsules. The glass transition temperature can be measured by the method described in JIS K7121:1987 "Method of measuring glass transition temperature of plastics." Specifically, the measurement is carried out as follows. That is, using a differential scanning calorimeter DSC6220 (manufactured by SII NanoTechnology Inc.), 6 mg of a sample was packed tightly at the bottom of an aluminum measurement container, and the sample was heated from 30°C to 300°C at a heating rate of 20°C / min under conditions of a nitrogen gas flow rate of 20 mL / min. From the DSC curve obtained, the midpoint glass transition temperature was calculated using analysis software attached to the device. Alumina is used as the reference material. The midpoint glass transition temperature is determined by the method described in JIS K7121:1987 "Method of measuring transition temperature of plastics", 9.3 "Determination of glass transition temperature".
[0065] Examples of the liquid hydrocarbon include butane (isobutane, normal butane), pentane (isopentane, neopentane, normal pentane), and the like. As the liquid hydrocarbon, butane and pentane are preferable from the viewpoint that the thermally expandable microcapsules can be sufficiently expanded by the polymerization reaction. Moreover, hydrocarbons having a boiling point of -20°C to 30°C are preferred.
[0066] The polishing pad according to the present invention is not limited to the above embodiment. The polishing pad according to the present invention is not limited by the above-mentioned action and effect. Furthermore, the polishing pad according to the present invention can be modified in various ways without departing from the gist of the present invention. EXAMPLES
[0067] The present invention will now be described in more detail with reference to examples and comparative examples. The following examples are provided to further explain the present invention in detail, and are not intended to limit the scope of the present invention.
[0068] Example 1 The prepolymer and the foam stabilizer shown in Table 1 below were mixed at 70° C. in the blending ratio shown in Table 1 below to obtain a dispersion in which air was dispersed as bubbles. Next, the dispersion and a curing agent were mixed in the blending ratio shown in Table 1 below and polymerized to obtain a polishing pad as a polyurethane resin foam.
[0069] The materials in Table 1 below are specifically as follows. Prepolymer 1: Urethane prepolymer obtained by reacting polypropylene glycol (PPG) with tolylene diisocyanate (TDI) (urethane prepolymer having an isocyanate group as a terminal group) (NCO mass%: 5.8) (Takenate L1150, manufactured by Mitsui Chemicals, Inc.) Prepolymer 2: Urethane prepolymer (NCO mass%: 9.2) obtained by reacting polytetramethylene ether glycol (PTMG) with TDI (Hyprene L213, manufactured by Mitsui Chemicals, Inc.) Hardener: MOCA (4,4'-methylenebis(2-chloroaniline)) Foam stabilizer: Silicone surfactant (Decostab B8465, Evonik) The blending ratio of prepolymer 1 and prepolymer 2 was prepolymer 1:prepolymer 2=60:40.
[0070] Example 2 As the prepolymers, in addition to prepolymer 1 and prepolymer 2, prepolymer 3 (a urethane prepolymer (NCO mass%: 8.0) (Takenate L1080D, manufactured by Mitsui Chemicals) obtained by reacting PPG with TDI) was used, and microcapsules (unexpanded hollow microparticles, F36D) were used. These were mixed in a mixing tank with a stirring blade to obtain a dispersion. Next, a curing agent (MOCA), a catalyst (Toyocat L33), and water were added to the mixing tank, and then the dispersion, the curing agent, the catalyst, and the water were mixed with a stirring blade to obtain a polishing pad that is a polyurethane resin foam. The mixing ratio of each component is as shown in Table 1 below. The blending ratio of prepolymer 1, prepolymer 2, and prepolymer 3 was prepolymer 1:prepolymer 2:prepolymer 3=70:20:10.
[0071] Example 3 Polishing pads as polyurethane resin foams were obtained in the same manner as in Example 1, except that prepolymers 1 and prepolymer 3 were used as prepolymers, microcapsules were used, and the blending ratios shown in Table 1 below were used. The blending ratio of prepolymer 1 and prepolymer 3 was prepolymer 1:prepolymer 3=30:70.
[0072] Comparative Example 1 A polishing pad as a polyurethane resin foam was obtained in the same manner as in Example 1, except that only Prepolymer 3 was used as the prepolymer in the blending ratio shown in Table 1 below.
[0073] Comparative Example 2 A polishing pad as a polyurethane resin foam was obtained in the same manner as in Example 1, except that only Prepolymer 1 was used as the prepolymer in the blending ratio shown in Table 1 below.
[0074] Comparative Example 3 A polishing pad as a polyurethane resin foam was obtained in the same manner as in Example 1, except that prepolymer 2 and prepolymer 4 (urethane prepolymer (NCO mass%: 7.8) (Takenate L202, manufactured by Mitsui Chemicals) obtained by reacting PTMG with H12MDI) were used as the prepolymers, water was used as the foaming agent, and a catalyst (Toyocat L33) was used.
[0075] Comparative Example 4 A polishing pad as a polyurethane resin foam was obtained in the same manner as in Example 1, except that only prepolymer 1 was used as the prepolymer, water was used as the foaming agent, and a catalyst (Toyocat L33) was used.
[0076] [Apparent density, JIS-A hardness, and compressibility] The apparent density, JIS-A hardness, and compressibility of the polishing pad according to each example were measured by the methods described above. The measurement results are shown in Table 1 below.
[0077] [tan δ] For the polishing pad of each example, tan δ was measured within a temperature range of 25° C. or more and 75° C. or less by the method described above. The results are shown in Figure 2. Table 1 below also shows the value of tan δ at 25°C (tan δ(25°C)), the value of tan δ at 75°C (tan δ(75°C)), and the value of tan δ(75°C) relative to tan δ(25°C) (tan δ(75°C) / tan δ(25°C)). Furthermore, in Table 1 below, the minimum value of tan δ within the temperature range of 25°C to 75°C is MIN, the maximum value of tan δ in the temperature range of 25°C to 75°C MAX , and tan δ MIN tan δ MAX The values shown were:
[0078] [Characteristics of bubbles] A volumetric bubble diameter distribution curve was obtained for each polishing pad according to the present invention, and the results are shown in FIG. The volumetric bubble diameter distribution curve was obtained based on the data of the number-based bubble diameter distribution curve. Then, from the volumetric bubble diameter distribution curve, the bubble characteristics shown in Table 1 below were examined using the method described above. As shown in FIG. 3, the polishing pad of Example 1 only had a peak top of the first peak within the bubble diameter range of 100 μm or more and 200 μm or less, while the polishing pads of Examples 2 and 3 had a peak top of the first peak within the bubble diameter range of 100 μm or more and 200 μm or less, and also had a peak top of the second peak below a bubble diameter of 100 μm. Specifically, the polishing pad of Example 1 had a peak top of the first peak at a bubble diameter of 120 μm, the polishing pad of Example 2 had a peak top of the second peak at a bubble diameter of 60 μm and a peak top of the first peak at a bubble diameter of 140 μm, and the polishing pad of Example 3 had a peak top of the second peak at a bubble diameter of 60 μm and a peak top of the first peak at a bubble diameter of 140 μm.
[0079] [Evaluation test] Using the polishing pad of each example, a workpiece was polished under the conditions below, and the polishing rate, the surface roughness of the workpiece after polishing (arithmetic mean surface roughness Ra), and the ΔGBIR of the workpiece after polishing were determined. · Polishing material: Silicon bare wafer (thickness: approx. 760μm) Polishing machine: Polishing machine PNX332B, manufactured by Okamoto Machine Tools Co., Ltd. Head type: Rubber Polishing slurry flow rate: 600mL / min Number of polishing times: 2 Polishing slurry type: NP7050AH x 10 Polishing time: 2 min Wafer / guide pressure: 11kPa / 16Pa Head speed: 30 rpm Platen speed: 33 rpm
[0080] <Polishing speed> The polishing rate was determined by dividing the thickness reduced by polishing by the polishing time. The thickness was measured using a nanospecAFT5100 manufactured by Nano-metrics. The removal rates are shown in Table 1 below.
[0081] <Surface roughness (arithmetic mean roughness)> The surface roughness (arithmetic mean roughness) was measured under the following conditions. The Ra of the polished object was measured after the second polishing. Equipment: Bruker, Wyko NT9300 Measurement mode: PSI Internal lens: 1 Objective lens: x50 Field of view: 94μm×125μm The results of the arithmetic mean roughness Ra are shown in Table 1 below.
[0082] <ΔGBIR> The GBIR (GBIR1 before polishing, GBIR2 after the second polishing) was measured for the polished object before polishing (before the first polishing, i.e., the initial state) and for the polished object after the second polishing. Then, ΔGBIR was calculated based on the following formula. ΔGBIR = GBIR1-GBIR2 The global backside ideal range (GBIR) was measured using a Nanometro 300TT-A manufactured by Kuroda Precision Industries, Ltd. The results of calculating ΔGBIR are shown in Table 1 below.
[0083] [Table 1]
[0084] It is apparent from Table 1 that in Examples 1 to 3, the polishing rate was high, at least 0.12 μm / min. Furthermore, from Table 1, in Examples 1 to 3, the surface roughness (arithmetic mean surface roughness) was a low value of 0.53 nm or less, and the ΔGBIR value was also a low value of 0.098 or less. In other words, it is understood that Examples 1 to 3 are excellent in flatness. In contrast, in Comparative Example 1, although the polishing rate was as high as 0.12 μm / min, the surface roughness and ΔGBIR values were both high, indicating poor flatness. Moreover, in Comparative Example 2, the polishing rate was as low as 0.08 μm / min, and it is understood that a sufficient polishing rate could not be ensured. Furthermore, in Comparative Example 3, the polishing rate was low at 0.09 μm / min, and the surface roughness (arithmetic mean roughness) was high at 0.78 nm, indicating that both the polishing rate and flatness were not sufficiently ensured. In addition, in Comparative Example 4, the polishing rate was low at 0.09 μm / min, the surface roughness (arithmetic mean roughness) was high at 0.61 nm, and the ΔGBIR value was also high at 0.135, indicating that both the polishing rate and flatness were not sufficiently ensured. From these, it can be seen that the polyurethane resin foam has a tan δ value of 0.1 or more and less than 0.4 within the temperature range of 25°C or more and 75°C or less, and the distribution curve of the volumetric cell diameter of the polyurethane resin foam has a first peak when plotted with the cell diameter on the horizontal axis and the cell volume on the vertical axis, and the cell diameter at the peak top of the first peak is in the range of 100 μm or more and 200 μm or less, thereby enabling the polishing pad to sufficiently increase the polishing speed of the object to be polished while improving the flatness of the polished surface of the object to be polished.
[0085] [Air bubble diameter at 10% cumulative volume frequency and air bubble diameter at 80% cumulative volume frequency] From the volumetric bubble diameter distribution curve shown in Figure 3, the bubble diameter at a cumulative volume frequency of 10% (the bubble diameter when the cumulative volume frequency is 10%, hereinafter also referred to as the cumulative volume 10% diameter) and the bubble diameter at a cumulative volume frequency of 80% (the bubble diameter when the cumulative volume frequency is 80%, hereinafter also referred to as the cumulative volume 80% diameter) were determined for the polishing pads of each example. The difference between the diameter at 80% cumulative volume and the diameter at 10% cumulative volume was also calculated. The results are shown in Table 2 below.
[0086] [Table 2]
[0087] From Table 2, it can be seen that the polishing pads of each embodiment have a high difference between the cumulative volume 80% diameter and the cumulative volume 10% diameter, exceeding 60 μm, i.e., the bubble diameters are distributed over a relatively wide range. [Explanation of symbols]
[0088] 1 polishing pad, 2 object to be polished, 1a Polished surface, 2a Polished surface.
Claims
1. A polishing pad comprising a polyurethane resin foam, having a polished surface, the polishing surface is formed from the surface of the polyurethane resin foam, The polyurethane resin foam has a tan δ value of 0.1 or more and less than 0.4 within a temperature range of 25° C. or more and 75° C. or less, A volumetric cell diameter distribution curve of the polyurethane resin foam has a first peak when plotted with the cell diameter on the horizontal axis and the cell volume on the vertical axis, The bubble diameter at the peak top of the first peak is in the range of 100 μm or more and 200 μm or less. Polishing pad.
2. a distribution curve of the volumetric cell diameter of the polyurethane resin foam, when plotted with the cell diameter on the horizontal axis and the cell volume on the vertical axis, further has a second peak; The bubble diameter at the peak top of the second peak is within a range of less than 100 μm. The polishing pad of claim 1.
3. The polyurethane resin foam has an average cell diameter of 30 μm or more and 70 μm or less.
3. The polishing pad according to claim 1 or 2.
4. The polyurethane resin foam has a JIS-A hardness of 65 or more and 80 or less. The polishing pad according to claim 1 .
5. The polyurethane resin foam has an apparent density of 0.3 g / cm 3 0.6g / cm or more 3 is less than or equal to The polishing pad according to claim 1 .
6. The polyurethane resin foam has a compression ratio of 3% or more and 10% or less. The polishing pad according to claim 1 .
Citation Information
Patent Citations
Polishing pad
JP2010274361A
Polishing pad
JP2018108612A
Polishing pad
JP2019115971A
Polishing pad
JP2020104235A