Fabrication of ohmic contacts and electronic devices having ohmic contacts
The method of wet chemical etching and radical rinsing in ultra-high vacuum addresses the challenges of high resistance and low-temperature operation in compound semiconductors, achieving low contact resistances and linear current-voltage characteristics.
Patent Information
- Application Number
- JP2021561594
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-15
- Filing Date
- 2020-04-02
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-04-02
AI Technical Summary
Existing methods for manufacturing ohmic contacts in compound semiconductors, particularly II-VI and III-V semiconductors, face challenges such as high temperature damage and oxidation, leading to high electrical resistance and unsuitable operation at low temperatures.
A method involving wet chemical etching followed by rinsing with radicals, preferably hydrogen radicals, in ultra-high vacuum, to create semiconductor connections with minimal damage, using etching media like K2Cr2O7+HBr+H2O or N.H.3+H2O2+H2O, and filling holes with doped semiconductors via molecular beam epitaxy to achieve low electrical resistance.
Enables near-perfect linear current-voltage characteristics and extremely low contact resistances at room and low temperatures, improving the manufacturing process for compound semiconductors like ZnSe.
Smart Images

Figure 0007594545000001 
Figure 0007594545000002 
Figure 0007594545000003
Abstract
Description
[Technical field]
[0001] METHOD FOR MANUFACTURING OHMIC CONTACTS TO ELECTRONIC DEVICES The present invention relates to electronic devices with ohmic contacts for buried semiconductors. [Background technology]
[0002] An ohmic contact is a junction between a metal and a semiconductor that has a low electrical resistance.
[0003] A buried semiconductor is a semiconductor that is inside an electronic device. A buried semiconductor is usually a layer of semiconductor sandwiched between two other layers.
[0004] A local ohmic contact for a buried semiconductor is a conductor or semiconductor made of the metal of the ohmic contact that penetrates a hole in an electronic device and contacts the buried semiconductor.
[0005] To produce an electronic device, one or more layers can be applied (deposited) to the substrate. One or more layers can consist of a semiconductor. One or more of these applied semiconductor layers can consist of a doped semiconductor, in particular an n-doped semiconductor. The semiconductor can be doped, for example, with chlorine or iodine. Doping with fluorine is also possible, but in principle less suitable than chlorine and iodine. p-doping is also possible, but in many cases less suitable. An electrically insulating top layer can be applied to the one or more semiconductor layers applied to the substrate. The one or more semiconductor layers are then buried semiconductor layers in the sense of the present invention. To produce an ohmic contact for the buried semiconductor layer, a hole can be made that penetrates through the top layer to the buried semiconductor layer. This hole can be made by etching. After making the hole, the hole can be filled with a metal to produce a local ohmic contact that can be electrically contacted above the top layer. In this way, for example, the electronic device can be later equipped with an additional gate electrode that is required for a unipolar device, such as a field effect transistor or an electron spin qubit.
[0006] In electronic devices containing GaAs and AlGaAs or Si and SiGe substrates and / or layers, metals can be thermally alloyed at high temperatures into holes created in the top layer to contact the buried semiconductor and create local ohmic contacts. Additional dopants can be locally introduced prior to the alloying of the metals by ion implantation to create suitably good ohmic contacts.
[0007] Known methods for producing local ohmic contacts are not suitable for all compound semiconductors. For example, the II-VI compound semiconductor ZnSe cannot withstand the high temperatures required for efficient alloying of metals. Ion implantation can seriously damage the crystal structure of such compound semiconductors, significantly reducing their conductivity. The production of junctions with low electrical resistance between metal and semiconductor is then not possible with this method. This problem occurs mainly with II-VI compound semiconductors. However, III-V compound semiconductors can also be affected by this problem.
[0008] It may be of interest to be able to operate electronic devices at low temperatures, which may be required, for example, for electron spin qubits in quantum computers. Summary of the Invention [Problem to be solved by the invention]
[0009] The object of the present invention is to be able to produce ohmic contacts to electronic components, in particular local ohmic contacts for embedded III-V or II-VI compound semiconductors in electronic components. Preferably, this should also be possible for II-VI compound semiconductors, which may be doped with chlorine. The ohmic contacts should also preferably allow for low temperature operation of the associated electronic components. [Means for solving the problem]
[0010] The problem according to the invention is solved by a method having the features of claim 1 and by an electronic device having the features of the additional claims. Advantageous embodiments are according to the dependent claims.
[0011] To solve this problem, a method for producing an ohmic contact for an electronic component is provided. To produce the electronic component, a layer made of a semiconductor, i.e. a semiconductor layer, is applied to a substrate, either indirectly or directly. When the semiconductor layer is applied directly onto the substrate, there are no other layers between the semiconductor layer and the substrate. When the semiconductor layer is applied indirectly onto the substrate, there are one or more layers between the substrate and the semiconductor layer.
[0012] The contacted surface of the semiconductor is wet-chemically etched; the wet-chemically etched surface is rinsed with radicals; a conductor or semiconductor is applied to the surface rinsed with radicals. In this way, it is possible to produce connections to semiconductors that can be easily damaged by normal manufacturing processes such that it is not possible to produce a joint with a low electrical resistance. Surprisingly, it has been found that such a problem can be solved by chemical etching and subsequent rinsing with radicals, even if the surface has previously been subjected to a damaging treatment such as ion etching.
[0013] A radical is an atom or molecule that has at least one unpaired valence electron. Rinsing with hydrogen radicals has been found to be effective. Hydrogen radicals have been found to be suitably reactive.
[0014] Wet chemical etching followed by a radical rinse has been found to be a crucial step for contacting sensitive II-VI and III-V compound semiconductors such that extremely low contact resistance as well as nearly perfect linear current-voltage characteristics can be achieved at room and very low temperatures.
[0015] Preferably, the rinsing is carried out in the absence of oxygen. Preferably, the rinsing is carried out in ultra-high vacuum and therefore also in the absence of oxygen to obtain further improved results. This embodiment is particularly advantageous for compound semiconductors that can oxidize quickly in air. ZnSe is an example of a compound semiconductor that can oxidize quickly in air. Oxidation can lead to the formation of a non-conductive surface oxide layer that constitutes a barrier to current transport. This can prevent a joint with a low electrical resistance.
[0016] Results can be further improved by rinsing at elevated temperatures, for example 100°C to 200°C.
[0017] Rinsing is preferably carried out for several minutes, for example, from 2 to 10 minutes, to achieve the desired results.
[0018] In wet chemical etching, the chemical bonds of the material being treated are broken by the etching medium and converted into soluble components. Commonly used etching media are K2Cr2O7+HBr+H2O or NH3+H2O2+H2O or K2Cr2O7+H2SO4+H2O.
[0019] Preferably, the wet chemical etch is carried out for a few seconds, such as 2 to 10 seconds, to ensure proper contact of the compound semiconductor.
[0020] The semiconductors prepared for the production of ohmic contacts by wet chemical etching and subsequent radical rinsing can be II-VI or III-V compound semiconductors. II-VI compound semiconductors, which may be doped with chlorine, benefit most from the advantages of this method. Examples of such II-VI compound semiconductors are (Zn,Mg)Se, (Zn,Cd)Se, (Zn,Mg)SSe, (ZnCd)SSe, ZnSe, CdSe, or ZnSSe.
[0021] The metal of the compound semiconductor is preferably selected from zinc (Zn), cadmium (Cd), magnesium (Mg) and / or beryllium (Be). The non-metal of the compound semiconductor is preferably selected from selenium (Se) and / or sulfur (S).
[0022] To fabricate an ohmic contact for a buried semiconductor, the fabrication method includes the following steps: applying one or more semiconductor layers to a substrate; applying a non-conductive top layer, which may consist of a non-conductive dielectric material, to the applied one or more semiconductor layers; making holes through the top layer down to the semiconductor layer; wet-chemical etching as described above of said surface of the semiconductor layer accessible through the holes; - rinsing the wet-chemically etched surface with radicals as described above; applying a doped semiconductor to the radical-rinsed surface; applying a metal, for example aluminum, to the applied doped semiconductor; may include.
[0023] The electronic components produced in this way can subsequently be provided with, for example, gate electrodes.
[0024] The holes made in the top layer that penetrate the top layer may be partially or completely filled with a doped semiconductor. The holes made in the top layer may penetrate one or more additional layers below the top layer to reach the desired semiconductor layer. One or more of the additional layers may be semiconducting layers, i.e. may consist of a semiconductor.
[0025] To fabricate multiple local ohmic contacts, multiple holes can be made in the top layer.
[0026] The filling of the holes with the doped semiconductor is preferably carried out by molecular beam epitaxy. This allows selective growth. Thus, the growth can be limited to the area of the holes. Such application by molecular beam epitaxy is known under the name of regrowth process. Such a process simplifies the manufacturing. An additional step is omitted, namely the etching away of the doped semiconductor between the holes. However, this does not exclude, in one embodiment of the invention, the etching away of a metal layer subsequently applied between the holes or between the fabricated ohmic contacts. Advantageously, the metal layer subsequently applied between the holes or between the fabricated ohmic contacts is then also etched away in this step so that one or more additional gate electrodes are then produced independently of the ohmic contacts.
[0027] To produce an electronic component, which may be a finished unipolar component (element), which may also be used at low temperatures, one or more semiconductor layers can be applied to a substrate in ultra-high vacuum. A top layer can subsequently be applied to the one or more semiconductor layers deposited in ultra-high vacuum. During the application process, in this configuration, the surface of the layer is not exposed to the atmosphere, and therefore the surface to which the top layer is applied is also not exposed to the atmosphere.
[0028] Adjacent semiconductor layers are made of different semiconductor materials and / or are at least differently doped.
[0029] Thus, for example, a first semiconductor layer may be applied to a substrate. Subsequently, a second semiconductor layer may be applied to the first semiconductor layer. Subsequently, a third semiconductor layer may be applied to the second semiconductor layer. Subsequently, a top layer may be applied to the third semiconductor layer. However, more than three semiconductor layers may be applied before applying the top layer.
[0030] The applied first and / or third semiconductor layer may consist of (Zn,Mg)Se, (Zn,Cd)Se, Zn(S,Se) or (Zn,Mg)(S,Se). The second layer may consist of ZnSe or CdSe. These materials are particularly suitable for the manufacture of unipolar components that can also be used at low temperatures to function as qubits in quantum computers. The second layer may be manufactured as a doped layer. However, this is not necessary.
[0031] The top layer may consist of an oxide ceramic. For example, the top layer may consist of aluminum oxide, silicon oxide or hafnium oxide. However, the top layer may also consist of another material, such as silicon nitride. These materials may serve as optimal gate dielectrics for the manufacture of unipolar elements, such as 2D or 3D field effect transistors or electrostatically defined electron-spin qubits. The invention therefore also relates to this type of unipolar element.
[0032] Generally, non-conductive dielectric materials are suitable as the top layer material for fabricating unipolar elements.
[0033] The substrate may be made of a semiconductor. The substrate may be made of a III-V semiconductor or a II-VI compound semiconductor, so that a II-VI semiconductor layer can be suitably manufactured on the substrate. Thus, the substrate may be made of GaAs, ZnSe, (In,Ga)As, InAs, (In,Ga)P, (In,Ga,Al)P, InAs, or InP.
[0034] The holes through the top layer can be made by wet chemical etching, in particular with HF, or alternatively, the holes can be made by reactive ion etching, in particular with CHF3+O2.
[0035] If the hole is to continue to the layer below, this can be done by reactive ion etching, typically with Cl2+Ar, Cl2+BCl3, or CH4+H2+Ar in the case of compound semiconductors consisting of (Zn,Mg)Se, Zn(S,Se), CdSe, or ZnSe, for example.
[0036] Dry etching processes can seriously damage the crystalline structure of compound semiconductors near the surface. However, the problems that arise can be eliminated by subsequent wet chemical etching and rinsing with radicals, so that it is still possible to produce joints with low electrical resistance. In particular, rinsing is carried out in the absence of oxygen, in cases where the corresponding semiconductors can be easily oxidized.
[0037] An etching mask may be applied to the top layer in order to create holes through the top layer by etching. The top layer may consist of a photoresist with holes. The resist with holes may be produced by photolithography.
[0038] After creating holes through the top layer by etching to the desired depth, the contacted surface of the applied semiconductor may be wet chemically etched as previously described.
[0039] After this final etching, the etching mask is removed. For technical reasons, it is recommended here to clean with a solvent, for example isopropanol. In particular, the contacted surfaces of the applied semiconductor, i.e. the semiconductor layer provided for the ohmic contact, should then be cleaned.
[0040] In order to further improve the desired technical result, it is advantageous to heat treat the element after etching and preferably also after cleaning. The heat treatment can be carried out at a temperature that can be between 100°C and 200°C. The heat treatment can last for several minutes, for example at least 15 minutes. The heat treatment can be completed after 60 minutes at the latest, since after that time no further beneficial effects are usually obtained. Thus, for example, a treatment time of about 30 minutes is sufficient.
[0041] In order to obtain further improved technical results, the heat treatment is preferably carried out in an ultra-high vacuum, in this way adverse environmental influences can be appropriately avoided.
[0042] The heat treatment can be followed by a rinse with radicals, in particular hydrogen radicals, preferably for several minutes, preferably in an ultra-high vacuum, particularly preferably in an ultra-high vacuum prepared for the heat treatment, in particular in this way avoiding the parts to be produced coming into contact with the atmosphere after the heat treatment and before the rinse with radicals.
[0043] Advantageously, after rinsing with radicals, the contacted surface of the semiconductor layer is treated with metal vapor. The metal vapor contains metals that are also present in the semiconductor. Thus, if the semiconductor consists, for example, of ZnSe, the metal vapor contains zinc as the metal. The metal vapor is thus generated by a zinc source in the case of ZnSe. The metal is thermally evaporated by such a metal source. In this way, any metal defects that may be present can be filled, which may lead to a further improved desired technical result. The treatment with metal vapor is preferably carried out in an ultra-high vacuum, preferably in an ultra-high vacuum that has already been prepared in a previous step. As mentioned above, contact with the atmosphere is prevented in the process.
[0044] Finally, the holes can be filled completely or partially with a semiconductor, which in principle corresponds to the semiconductor to be contacted. For example, if a layer made of ZnSe is to be contacted, the holes are preferably filled completely or partially with ZnSe. However, the two semiconductors can differ in terms of their doping. Thus, to contact a layer made of undoped ZnSe, the holes can be filled completely or partially with n-doped ZnSe.
[0045] The holes are preferably filled with the semiconductor at a temperature particularly suitable for growth, for example 200° C. to 400° C. For example, a temperature of 300° C. is suitable for ZnSe. The filling of the holes is carried out in an ultra-high vacuum, preferably also already prepared in a previous step, in order to further prevent contact with the atmosphere.
[0046] Once the holes are completely or partially filled with the semiconductor, a metal is finally applied to the semiconductor. This is done, for example, by a deposition system for metals. Preferably, this is again done consistently in the above-mentioned ultra-high vacuum, so that contact with the atmosphere is consistently prevented. Thus, for example, the semiconductor produced by regrowth cannot oxidize before the metal is deposited.
[0047] Aluminum is particularly suitable as the metal, titanium or magnesium being equally suitable.
[0048] In order to be able to carry out the latter step in situ in ultra-high vacuum, the equipment required for this is connected to one another by ultra-high vacuum. Thus, there exists a chamber capable of generating ultra-high vacuum. This chamber is equipped with a molecular beam epitaxy system for compound semiconductors, an evaporation system for metals, e.g. aluminum, an atomic layer deposition system and a radical source, e.g. for hydrogen radicals.
[0049] Comparative tests have shown that in the case of sensitive compound semiconductors, ohmic contacts can be provided in this way with significantly better properties compared to the known prior art.
[0050] The invention also relates to an electronic device that can be produced according to the above method, comprising a plurality of semiconductor layers on a substrate, with a top layer on one or more of the semiconductor layers applied to the substrate, the top layer being made of a non-conductive dielectric. Adjacent semiconductor layers are made of different II-VI semiconductors, so that a heterojunction is present. Due to the holes created, there is a passageway through the top layer to the semiconductor layer. The passageway is at least partially filled with II-VI semiconductor. A metal contact is applied to the II-VI semiconductor. The II-VI semiconductor at least completely fills the passageway, so that the metal contact extends at least to the outside of the top layer. Usually the metal contact protrudes outwards with respect to the top layer. The metal contact is in particular made of aluminium.
[0051] The applied first and / or third semiconductor layer preferably consists of (Zn,Mg)Se, Zn(S,Se), (Zn,Cd)Se or (Zn,Mg)(S,Se). In particular, the second semiconductor layer consists of ZnSe or CdSe. The top layer preferably consists of aluminum oxide, silicon oxide, hafnium oxide or silicon nitride. The substrate may consist of GaAs, ZnSe, AlAs, InAs, GaP, AlP or InP or mixed forms such as (In,Ga)As or (In,Al)GaP.
[0052] The invention further relates to a unipolar element that can be constructed as described above. The unipolar element can be a field effect transistor or a high mobility transistor. The unipolar element can be an electron-spin qubit element.
[0053] The invention will now be explained in more detail by way of examples. [Brief description of the drawings]
[0054] [Figure 1] FIG. 2 shows a layer structure with a ZnSe layer. [Diagram 2] FIG. 2 shows a layer structure having a hole. [Diagram 3] FIG. 2 shows a layer structure having holes partially filled with a semiconductor. [Figure 4] FIG. 2 shows a layer structure with applied aluminum. [Diagram 5] FIG. 1 shows a layer structure with completed local ohmic contacts. [Figure 6] FIG. 1 shows measured current-voltage characteristics. [Figure 7] 1A-1C show further structures for electronic devices having buried semiconductor layers and local ohmic contacts. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0055] FIG. 1 shows a substrate 1 of gallium arsenide on which a first buried semiconductor layer 2 of (Zn,Mg)Se is deposited in ultra-high vacuum. On the first semiconductor layer 2, a second buried semiconductor layer 3 of ZnSe is deposited in situ in ultra-high vacuum. On the second semiconductor layer 3, a third buried semiconductor layer 4 of (Zn,Mg)Se is deposited in situ in ultra-high vacuum. On the third semiconductor layer 4, a top layer 5 of Al2O3 is deposited in situ in ultra-high vacuum. The deposition is carried out, for example, by atomic layer deposition. These layers can be several tens of nanometers thick, for example 20 nm thick.
[0056] By "in situ" it is meant that the structure fabricated in FIG. 1 was not removed from ultra-high vacuum during its fabrication and therefore no deleterious oxidation processes could occur.
[0057] After deposition of the Al2O3 layer, the structure is removed from the ultra-high vacuum. By conventional optical lithography, a mesh mask with holes is defined in the previously applied photoresist, in which ohmic contacts will later be made by regrowth. At the locations of the holes, the Al2O3 layer 5 is first opened, either wet-chemically with HF or by reactive ion etching with CHF3+O2. The underlying (Zn,Mg)Se layer 4 and the ZnSe layer 3 are then opened by reactive ion etching with Cl2+Ar. Thus, an etch down is performed to make holes 6, as shown in FIG. 2. The semiconductor layer 3 can be contacted through these holes 6.
[0058] After reactive ion etching, the generated radiation damage is removed by wet chemical re-etching in a solution of K2Cr2O7+HBr+H2O for about 5 seconds. The photoresist is then removed and the etched ZnSe semiconductor layer 3 is washed with isopropanol and reintroduced into ultra-high vacuum for the regrowth process. The structure is then heated in ultra-high vacuum to 150 °C for 30 minutes, followed by rinsing with hydrogen radicals for 5 minutes. In this way, chemical residues from the etching and cleaning processes are removed, as well as possible oxide residues on the surface. The etched layer is then slowly heated under zinc flux to a suitable growth temperature for the regrowth process of 300 °C. This helps to fill any zinc defects that may remain near the etched surface. This is followed by the growth of a chlorine-doped ZnSe layer 7 by molecular beam epitaxy (MBE) under standard growth parameters. This is shown in Figure 3. The layer 7 should be at least thick enough to fill the holes up to the Al2O3 layer 5. Otherwise, metal 8 on layer 7 would laterally contact layer 4 and thus the semiconductor (Zn,Mg)Se, which can be disadvantageous and should be avoided.
[0059] The newly grown doped ZnSe layer 7 is subsequently coated in situ with aluminum 8 as an ohmic contact material, as shown in Figure 4. The in situ deposited aluminum layer 8 prevents oxide formation between the chlorine doped ZnSe layer 7 and the aluminum layer 8, so that unhindered current transport can occur through the aluminum-ZnSe interface.
[0060] In a final step, photolithography followed by wet chemical etching is used to remove the excess aluminum and ZnSe between the actual local contacts until the structure shown in FIG. 5 is obtained.
[0061] The layer thicknesses in Fig. 5 are only approximate. The two semiconductor layers 2 and 4 may be thicker than the semiconductor layer 3. The top layer 5 may be thinner than the semiconductor layer 3. Advantageously, the semiconductor layer 7 is at least thick enough to reach down to the dielectric layer 5.
[0062] In this way, excellent local ohmic contacts with minimal contact resistance and linear current-voltage characteristics at room and low temperatures can be achieved. Figure 6 shows a diagram of the corresponding linear current-voltage characteristics measured at room temperature RT (solid line) and 4K (dashed line) for the structure shown in Figure 7. The distance between the two ohmic contacts of the component used for the measurements was 30 μm. The measured current in milliamps is plotted against the applied voltage in volts. In addition to the excellent linearity of the current-voltage characteristics, the contact resistance and sheet resistance of the element shown in Figure 7 can be determined from the measurements. At room temperature the contact resistance is ρ K ≦3×10 -5 Ωcm 2 and the sheet resistance is ρ S ≦6×10 -2 Ωcm, and at low temperatures the contact resistance is ρ K ≦8×10 -3 Ωcm 2 and the sheet resistance is ρ S ≦4×10 -2 It is Ωcm.
[0063] The device shown in Fig. 7 comprises a substrate 1 of gallium arsenide. On the substrate there is an undoped ZnSe semiconductor layer 2, approximately 20 nm thick. On the ZnSe semiconductor layer 2 there is a chlorine-doped ZnSe semiconductor layer 3, approximately 800 nm thick. On the semiconductor layer 3 there is a dielectric layer 5 of Al2O3, approximately 20 nm thick. The passages made by holes down to the semiconductor layer 2 are completely filled with chlorine-doped ZnSe, i.e. ZnSe:Cl. On this ZnSe:Cl filling 7 aluminium 8 having a thickness of approximately 120 nm is applied.
Claims
1. A method for producing ohmic contacts for electronic components, in which a semiconductor layer (3) is applied indirectly or directly to a substrate (1), comprising the steps of: A top layer (5) made of a non-conductive dielectric is provided on the semiconductor layer (3), creating a hole (6) penetrating the top layer (5) and reaching the semiconductor layer (3); wet-chemically etching the surfaces of the semiconductor layer (3) accessible through the holes (6) and rinsing the wet-chemically etched surfaces with radicals; treating the surface with metal vapor after rinsing with the radicals; The metal vapor contains a metal that is also present in the semiconductor that constitutes the semiconductor layer (3), after treating said surface with metal vapor, at least partially filling said holes (6) with a doped semiconductor (7); A method comprising applying an electrical conductor (8) to said doped semiconductor (7).
2. 2. The method of claim 1, wherein rinsing is performed with hydrogen radicals.
3. 3. The method according to claim 1, wherein the rinsing is carried out in an ultra-high vacuum.
4. Method according to any one of claims 1 to 3, characterized in that the rinsing is carried out at a temperature between 100°C and 200°C.
5. K2Cr 2 O 7 + HBr + H 2 O, or NH 3 +H 2 O 2 +H 2 O or K 2 Cr 2 O7+H 2 SO 4 +H 2 5. The method according to claim 1, characterized in that wet chemical etching is carried out with O.
6. A method according to any one of claims 1 to 5, characterized in that the wet chemical etching is carried out for 1 second to 20 seconds.
7. 7. The method according to claim 1, wherein the semiconductor constituting the semiconductor layer (3) is a II-VI or III-V semiconductor, in particular consisting of (Zn,Mg)Se, Zn(S,Se), ZnSe, CdSe or (Zn,Mg)(S,Se).
8. 8. The method according to claim 1, wherein the semiconducting metal constituting the semiconductor layer (3) is selected from zinc (Zn), cadmium (Cd), magnesium (Mg) and / or beryllium (Be).
9. The method according to any one of the preceding claims, characterized in that the semiconducting nonmetals constituting the semiconducting layer (3) are selected from selenium (Se) and / or sulphur (S).
10. 10. The method according to any one of the preceding claims, characterized in that the semiconductor constituting the semiconductor layer (3) is doped with chlorine (Cl) or can be doped with chlorine (Cl).
11. 1. An electronic device comprising one or more semiconductor layers (2, 3, 4) on a substrate (1) and a top layer (5) on the one or more semiconductor layers (2, 3, 4) applied to the substrate (1), the top layer (5) consisting of a non-conductive dielectric and having holes (6) penetrating through the top layer (5) to a semiconductor layer (3), wherein adjacent semiconductor layers (2, 3, 4) consist of different II-VI semiconductors, the holes (6) being at least partially filled with a doped II-VI semiconductor (7), and metal contacts (8) applied to the doped II-VI semiconductor (7), the metal contacts extending to the outside of the top layer (5) or protruding outward relative to the top layer (5), the electronic device having a contact resistance at room temperature of ρ K ≦3×10 -5 Ωcm 2 and a sheet resistance of ρ S ≦6×10 -2 Ωcm.
12. 12. The electronic device according to claim 11, characterized in that the applied first and / or third semiconductor layer (2, 4) consists of (Zn,Mg)Se, (Zn,Mg)(S,Se), (Zn,Be)Se, Zn(S,Se) and / or the second semiconductor layer (3) consists of ZnSe.
13. 13. Electronic component according to claim 11 or 12, characterized in that the top layer (5) consists of aluminium oxide, silicon oxide, hafnium oxide or silicon nitride.
14. The electronic device according to any one of claims 11 to 13, characterized in that the substrate (1) consists of GaAs, ZnSe, (In,Ga)As, InAs, (In,Ga)P, (In,Ga,Al)P, or InP.
15. The electronic device according to any one of claims 11 to 14, which is a unipolar device.
Citation Information
Patent Citations
Material and formation method of electrode on semiconductor
JP1994252515A
Method and apparatus for manufacturing compound semiconductor device and apparatus
JP2002016051A
Self-aligned trench metal-alloying for iii-v nfets
US20180096885A1