Structure and manufacturing method of high electron mobility transistor

By forming a passivation layer in the same growth chamber without interrupting the growth process, the method enhances the quality and stability of high electron mobility transistors, addressing defects and improving performance metrics such as sheet resistance and breakdown voltage.

JP7594613B2Active Publication Date: 2024-12-04GLOBALWAFERS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023007573
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-05-12
Filing Date
2023-01-20
Publication Date
2024-12-04
Estimated Expiration
2043-01-20

AI Technical Summary

Technical Problem

The ease with which gallium bonds with oxygen in passivation layers of high electron mobility transistors (HEMTs) leads to increased surface defects and instability, resulting in leakage current issues.

Method used

A method for manufacturing high electron mobility transistors involves forming a passivation layer in the same growth chamber without interruption, controlling the growth temperature to maintain continuity with the barrier layer, and ensuring minimal changes in temperature, pressure, and atmosphere, thereby enhancing the quality of the passivation layer and its boundary with the barrier layer.

Benefits of technology

This approach reduces defects and improves the stability and performance of high electron mobility transistors by maintaining a minimal change in sheet resistance value of 1% or less over three months, achieving high breakdown voltage and low surface roughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594613000003
    Figure 0007594613000003
  • Figure 0007594613000004
    Figure 0007594613000004
  • Figure 0007594613000005
    Figure 0007594613000005
Patent Text Reader

Abstract

To provide a high electron mobility transistor structure and a manufacturing method, thereby providing a passivation layer with good quality and improving performance of a high electron mobility transistor.SOLUTION: A method of manufacturing a high electron mobility transistor structure comprises controlling a passivation layer and a barrier layer to uninterruptedly grow in a same growth chamber.EFFECT: The present invention can avoid defects of the passivation layer generated in a growth process by a drastic change in a temperature, a pressure or atmosphere, and deterioration in quality of an interface between the passivation layer and the barrier layer, thereby providing the passivation layer with good quality and an interface between the passivation layer and the barrier layer with good quality, so that an objective of improving performance of the high electron mobility transistor structure can be achieved.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to semiconductor technology, and in particular to high electron mobility transistors. [Background technology]

[0002] A known high electron mobility transistor (HEMT) is a transistor with a two dimensional electron gas (2-DEG) adjacent to a heterogeneous junction between two materials with different energy bands. The high electron mobility transistor does not use a doped region as a transistor carrier channel, but uses a two dimensional electron gas with high electron mobility as a transistor carrier channel. Therefore, the high electron mobility transistor has characteristics such as high breakdown voltage, high electron mobility, low on-resistance and low input capacitance, and is widely applied in high power semiconductor devices.

[0003] In order to improve the performance, it is common to grow a passivation layer, such as gallium nitride, on the barrier layer in a high electron mobility transistor. However, gallium is easily bonded to oxygen, which increases defects on the surface, and the device becomes less stable and has problems such as increased leakage current. Therefore, how to provide a passivation layer to improve the performance of high electron mobility transistors is an issue that needs to be solved as soon as possible. Summary of the Invention [Problem to be solved by the invention]

[0004] SUMMARY OF THE PRESENT EMBODIMENTS In view of the above, an object of the present invention is to provide a high electron mobility transistor structure and manufacturing method, thereby providing a high quality passivation layer and improving the performance of the high electron mobility transistor. [Means for solving the problem]

[0005] In order to achieve the above object, the present invention provides a method for fabricating a high electron mobility transistor, comprising the steps of: Step A of providing a substrate; Step B of forming a nucleation layer above the substrate; Step C of forming a buffer layer above the nucleation layer; Step D of forming a channel layer above the buffer layer; a step E of depositing a barrier layer over the channel layer, the growth temperature of the barrier layer being a first growth temperature, and a two-dimensional electron gas region being formed in the channel layer along an interface between the channel layer and the barrier layer, the step E being performed in a growth chamber; and after step E, step F of depositing a passivation layer over the barrier layer in the growth chamber without interruption and controlling the growth temperature of the passivation layer to increase from the first growth temperature through a heating zone to a second growth temperature.

[0006] The present invention further provides a high electron mobility transistor structure comprising, in order, a substrate, a nucleation layer, a buffer layer, a channel layer, a barrier layer, and a passivation layer, wherein a two-dimensional electron gas region is formed in the channel layer along a boundary between the channel layer and the barrier layer, and the two-dimensional electron gas region in the channel layer exhibits a sheet resistance change of 1% or less over a time period, the time period being greater than or equal to three months. Effect of the Invention

[0007] The advantages of the present invention are as follows: Since the passivation layer and the barrier layer are controlled to grow in the same growth chamber without interruption, it is possible to avoid defects during the growth of the passivation layer and deterioration of the quality at the boundary between the passivation layer and the barrier layer caused by drastic changes in temperature, pressure, and atmosphere, and thus to provide a high-quality passivation layer and boundary between the passivation layer and the barrier layer, thereby achieving the purpose of improving the performance of high electron mobility transistors. The present invention also provides a high electron mobility transistor configuration, in which the passivation layer is formed so that the two-dimensional electron gas region in the channel layer has a sheet resistance value that changes by 1% or less over a period of time, the period of time being three months or more, thereby achieving the objective of improving the stability of the high electron mobility transistor. [Brief description of the drawings]

[0008] [Figure 1] 2 is a flow chart of a method for manufacturing a high electron mobility transistor structure in accordance with a preferred embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram of a high electron mobility transistor configuration according to a preferred embodiment of the present invention. [Diagram 3] FIG. 2 is a time-temperature plot of a grown passivation layer according to a preferred embodiment of the present invention. [Figure 4] FIG. 2 is a time-temperature plot of a grown passivation layer according to a preferred embodiment of the present invention. [Diagram 5] FIG. 2 is a time-temperature plot of a grown passivation layer according to a preferred embodiment of the present invention. [Figure 6] FIG. 13 is a time-temperature relationship diagram for a grown passivation layer according to a comparative example. [Figure 7] FIG. 2 is a time-temperature plot of a grown passivation layer according to a preferred embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In order to more clearly explain the present invention, a preferred embodiment will be described below with reference to the drawings. As shown in Figure 1, a method for fabricating a high electron mobility transistor structure according to a preferred embodiment of the present invention includes the following steps:

[0010] Step S02 provides a substrate 10. The substrate 10 may be, for example, a silicon (Si), gallium arsenide (GaAs), gallium nitride (GaN), silicon carbide (SiC), or aluminum oxide (Al2O3) substrate.

[0011] Step S04 forms a nucleation layer 20 above the substrate 10. The nucleation layer 20 may be, for example, an aluminum nitride (AlN) or aluminum gallium nitride (AlGaN) nitride nucleation layer. The nucleation layer 20 may be, for example, formed by metalorganic chemical vapor deposition (MOCVD).

[0012] Step S06 forms a buffer layer 30 above the nucleation layer 20. The buffer layer 30 may be, for example, a gallium nitride (GaN) buffer layer. The buffer layer 30 may be, for example, formed by metalorganic chemical vapor deposition (MOCVD).

[0013] Step S08 forms a channel layer 40 above the buffer layer 30. The channel layer 40 may be, for example, a gallium nitride (GaN) channel layer. The channel layer 40 may be formed by metal-organic chemical vapor deposition (MOCVD).

[0014] Step S10 deposits a barrier layer 50 above the channel layer 40. The growth temperature of the barrier layer 50 is a first growth temperature T1, which is preferably 700 to 1000°C. A two-dimensional electron gas region is formed in the channel layer 40 along the boundary between the channel layer 40 and the barrier layer 50. Step S10 is performed in a growth chamber. The barrier layer 50 may be a nitride barrier layer, for example, aluminum gallium nitride (AlGaN), aluminum nitride (AlN), aluminum indium nitride (AlInN), or aluminum indium gallium nitride (AlInGaN). The barrier layer 50 may be formed by metalorganic chemical vapor deposition (MOCVD) or molecular beam epitaxy (MBE).

[0015] In step S12, after step S10, a passivation layer 60 is deposited uninterruptedly above the barrier layer 50 in the growth chamber, and the growth temperature of the passivation layer 60 is controlled to increase from the first growth temperature T1 to a second growth temperature T2 through a temperature rise region RT. The second growth temperature T2 is 1000° C. or higher. The passivation layer 60 is silicon nitride. The passivation layer 60 may be formed by metal organic chemical vapor deposition (MOCVD) or molecular beam epitaxy (MBE). The total thickness of the passivation layer 60 is 100 nm or less. The total thickness means the distance from the boundary between the passivation layer 60 and the barrier layer 50 to the upper surface of the passivation layer 60.

[0016] In other words, after the barrier layer 50 is formed in the growth chamber of the metalorganic chemical vapor deposition (MOCVD) or molecular beam epitaxy (MBE) working equipment, the workpiece after step S10 is not moved from the growth chamber, that is, the barrier layer 50 is not exposed to air or the environment outside the growth chamber, and step S12 is performed in the growth chamber to form the passivation layer 60. In other words, the barrier layer 50 and the passivation layer 60 are formed under the same growth conditions of space, pressure, and atmosphere, and the initial growth temperature of the passivation layer 60 is the same as that of the barrier layer 50. The above-mentioned same atmosphere means that the same carrier gas, for example hydrogen or nitrogen, is used.

[0017] Furthermore, since the passivation layer 60 and the barrier layer 50 are controlled to grow uninterrupted in the same growth chamber, it is possible to avoid defects occurring during the growth of the passivation layer 60 and deterioration of quality at the boundary between the passivation layer 60 and the barrier layer 50 due to drastic changes in temperature, pressure, and atmosphere, thereby providing a high-quality passivation layer 60 and a high-quality boundary between the passivation layer 60 and the barrier layer 50, thereby achieving the objective of improving the performance of high electron mobility transistors.

[0018] Wherein, step S12 includes controlling the high temperature maintaining region HT to maintain the second growth temperature T2. In other words, as shown in Fig. 3, the first growth temperature T1 is maintained for a predetermined time t1 to grow the barrier layer 50, and then the passivation layer 60 is grown. The passivation layer 60 has the same initial growth temperature as the barrier layer 50, and is heated to the second growth temperature T2 through the temperature increasing region RT, and then the second growth temperature T2 is maintained for another predetermined time t2 to grow the passivation layer 60 to a required thickness. Wherein, the growth thickness of the passivation layer 60 in the high temperature maintaining region HT accounts for more than 50% of the total thickness of the passivation layer.

[0019] In another embodiment, as shown in FIG. 4, step S12 includes controlling the growth temperature of the passivation layer 60 to first maintain the first growth temperature T1 in the low temperature maintaining region LT, then raise the temperature through the temperature increasing region RT, and then maintain the second growth temperature T2 in the high temperature maintaining region HT. The total thickness of the passivation layer 60 is the total thickness of the passivation layer 60 grown in the low temperature maintaining region LT, the temperature increasing region RT, and the high temperature maintaining region HT. In addition, the proportion of the growth thickness of the passivation layer 60 in the low temperature maintaining region LT to the total thickness of the passivation layer 60 is 0 to 25%. The proportion of the growth thickness of the passivation layer 60 in the temperature increasing region RT to the total thickness of the passivation layer 60 is 0 to 25%.

[0020] In another embodiment, the growth thickness in the low temperature maintained region LT accounts for 0% of the total thickness of the passivation layer 60, the growth thickness in the temperature increased region RT accounts for 5-25% of the total thickness of the passivation layer 60, and the growth thickness in the high temperature maintained region HT accounts for 75-95% of the total thickness of the passivation layer 60. In other words, in step S12, the growth temperature of the passivation layer 60 is first raised from the first growth temperature T1 to the second growth temperature T2 in the temperature increased region RT as shown in Fig. 3, and then the second growth temperature is maintained for a predetermined time t2 to grow the passivation layer 60 to a required thickness.

[0021] In another embodiment, the growth thickness of the passivation layer 60 in the low temperature maintained region LT accounts for 0 to 25% of the total thickness of the passivation layer 60, the growth thickness of the passivation layer 60 in the temperature increased region RT accounts for 5 to 25% of the total thickness of the passivation layer 60, and the growth thickness of the high temperature maintained region HT accounts for 50 to 95% of the total thickness of the passivation layer 60.

[0022] To explain again, the temperature rise rate in the temperature rise region RT is preferably 10 to 30°C / min, the temperature rise region RT includes a plurality of temperature rise stages as shown in FIG. 5, among which the number of temperature rise stages is preferably 1 to 15 stages, and the temperature is raised by 30 to 60°C for each stage. Moreover, by controlling the temperature rise rate to be 60°C / min or less, good quality of the passivation layer 60 can be obtained.

[0023] The high electron mobility transistor structure 1 produced by the manufacturing method of the high electron mobility transistor structure has a thin film with good density, good surface roughness, and high voltage resistance. The refractive index of the passivation layer 60 is 2.05 to 2.28, the surface roughness RMS of the passivation layer 60 is 0.5 nm or less, and the breakdown voltage value per unit thickness of the passivation layer 60 is 1 to 1.15 V / nm. The refractive index is measured by an ellipsometer.

[0024] To be more specific, the method for manufacturing the high electron mobility transistor structure includes measuring the sheet resistance of the two-dimensional electron gas region in the channel layer 40 as a first sheet resistance, and measuring the sheet resistance of the two-dimensional electron gas region in the channel layer 40 as a second sheet resistance after a period of time has passed. The period of time is three months or more. The proportion of change in the sheet resistance is defined as (the second sheet resistance - the first sheet resistance) / the first sheet resistance * 100%. The high electron mobility transistor structure 1 manufactured by the method for manufacturing the high electron mobility transistor structure has an absolute value of the proportion of change in the sheet resistance of 0.1% or less. In other words, the high electron mobility transistor structure 1 manufactured by the method for manufacturing the high electron mobility transistor structure has a good stability of the sheet resistance.

[0025] Below, some comparative examples and some examples will be described with reference to Table 1. In the above description, the second sheet resistance value was measured again four months after the first sheet resistance value was measured, and the proportion of the change in the sheet resistance value is defined as above, so the description will not be repeated. [Comparative example AB]

[0026] In Comparative Example AB, no passivation layer was deposited above the barrier layer. The difference between Comparative Example A and Comparative Example B is that the structure according to Comparative Example A was subjected to the RCA cleaning process after measuring the first sheet resistance value, while the structure according to Comparative Example B was not subjected to the RCA cleaning process after measuring the first sheet resistance value. As shown in Table 1, the sheet resistance value of the structure according to Comparative Example A significantly improved from 372.7 ohm / sq to 687 ohm / sq before and after the RCA cleaning process, while the structure according to Comparative Example B did not undergo the RCA cleaning process, but the change in sheet resistance was as high as 3.57%. [Comparative example CE]

[0027] In Comparative Example CE, a passivation layer is intermittently deposited on the barrier layer. Intermittently means that after the barrier layer is deposited, the passivation layer is not continuously grown at the same temperature, pressure, or atmosphere in the deposition chamber for depositing the deposited barrier layer. The difference between Comparative Example C and Comparative Example E is that the configurations of Comparative Examples C and D were subjected to the RCA cleaning process after measuring the first sheet resistance, while the configuration of Comparative Example E was not subjected to the RCA cleaning process after measuring the first sheet resistance.

[0028] As shown in Table 1, the structures of Comparative Examples C and D did not show any clear difference in the sheet resistance measured before and after the RCA cleaning process, and the sheet resistance was improved by 1.8 times compared to the sheet resistance before and after the cleaning process in Comparative Example A, which can be said to be a significant improvement. In other words, by depositing a passivation layer above the barrier layer, the stability of the sheet resistance can be slightly improved. Although the structure of Comparative Example E did not undergo the RCA cleaning process, the change in the sheet resistance was still high at -0.87%. [Examples AB]

[0029] In Example AB, a passivation layer is deposited without interruption above the barrier layer by the manufacturing method of the high electron mobility transistor structure. The difference between Example A and Example B is that the structure according to Example A is subjected to the RCA cleaning process after measuring the first sheet resistance value, while the structure according to Example B is not subjected to the RCA cleaning process after measuring the first sheet resistance value. As shown in Table 1, the structure according to Example A shows no clear difference in the sheet resistance values ​​measured before and after the RCA cleaning process, and the sheet resistance change ratios of the structures according to Examples A and B are both -0.05%. In other words, the high electron mobility transistor structure produced by the manufacturing method of the high electron mobility transistor structure has good stability in sheet resistance value, and the absolute value of the sheet resistance change ratio can be suppressed to 0.1% or less.

[0030] Table 1 TIFF0007594613000001.tif161159

[0031] The following will be described based on a comparative example and several examples. First, in comparative example 1 and examples 1-4, after depositing a barrier layer, the passivation layer is continuously and uninterruptedly grown in the growth chamber for depositing the barrier layer at the same temperature, pressure or atmosphere. The first growth temperature T1 is 900°C, the second growth temperature T2 is 1000°C, and the total thickness of the passivation layer 60 is the sum of the thicknesses of the passivation layer 60 grown in the low temperature maintaining region LT, the temperature rising region RT and the high temperature maintaining region HT, as described above, and the total thickness of the passivation layer according to comparative example 1 and examples 1-4 is the same. Furthermore, the thickness proportion of the passivation layer 60 in the high temperature maintenance region HT is the proportion of the growth thickness of the passivation layer 60 in the high temperature maintenance region HT to the entire thickness of the passivation layer 60, the thickness proportion of the passivation layer 60 in the temperature rising region RT is the proportion of the growth thickness of the passivation layer 60 in the temperature rising region RT to the entire thickness of the passivation layer 60, and the thickness proportion of the passivation layer 60 in the low temperature maintenance region LT is the proportion of the growth thickness of the passivation layer 60 in the low temperature maintenance region LT to the entire thickness of the passivation layer 60. Comparative Example 1

[0032] In Comparative Example 1, as shown in Fig. 6, the growth temperature of the passivation layer is controlled to be the same as the first growth temperature T1. That is, the growth temperature of the passivation layer is controlled to be the first growth temperature T1 in the low temperature maintained region LT for a predetermined time t3, and the barrier layer is grown to a predetermined thickness at the same growth temperature as the passivation layer. As shown in Table 2, the passivation layer according to Comparative Example 1 has a thickness proportion of 100% in the low temperature maintained region LT, a thickness proportion of 0% in the temperature rise region RT, and a thickness proportion of 0% in the high temperature maintained region HT. Example 1

[0033] In Example 1, as shown in FIG. 7, the growth temperature when growing the passivation layer is the second growth temperature T2. That is, the growth temperature of the controlled passivation layer is rapidly increased from the first growth temperature T1 to the second growth temperature T2, and the second growth temperature is maintained in the high temperature maintaining region HT for a predetermined time t4, so that the passivation layer is grown to a predetermined thickness. As shown in Table 2, the passivation layer according to Example 1 has a thickness proportion of 0% in the low temperature maintaining region LT, a thickness proportion of 0% in the temperature increasing region RT, and a thickness proportion of 100% in the high temperature maintaining region HT. It will be explained again that the time for the growth temperature of the passivation layer to increase from the first growth temperature T1 to the second growth temperature T2 is extremely short, so that the growth thickness of the passivation layer in the temperature increasing region RT is close to zero. Example 2-3

[0034] In Examples 2 and 3, as shown in Fig. 3, when the growth temperature of the passivation layer rises from the first growth temperature T1 to the second growth temperature T2 through the temperature rising region RT, the second growth temperature T2 is controlled to be maintained for a predetermined time t2 in the high temperature maintaining region HT. As shown in Table 2, the passivation layer according to Example 2 has a thickness proportion of 0% in the low temperature maintaining region LT, a thickness proportion of 25% in the temperature rising region RT, and a thickness proportion of 75% in the high temperature maintaining region HT. The passivation layer according to Example 3 has a thickness proportion of 0% in the low temperature maintaining region LT, a thickness proportion of 5% in the temperature rising region RT, and a thickness proportion of 95% in the high temperature maintaining region HT. Example 4

[0035] In Example 4, as shown in Fig. 4, the growth temperature of the passivation layer is controlled so that the first growth temperature T1 is first maintained for a predetermined time ta in the low temperature maintaining region LT, the first growth temperature is raised to the second growth temperature T2 for a predetermined time tb through the temperature increasing region RT, and then the second growth temperature T2 is maintained for a predetermined time tc in the high temperature maintaining region HT. As shown in Table 2, the passivation layer according to Example 4 has a thickness proportion of 25% in the low temperature maintaining region LT, a thickness proportion of 25% in the temperature increasing region RT, and a thickness proportion of 50% in the high temperature maintaining region HT.

[0036] Referring to Table 2, as shown in Example 1-4, when the passivation layer satisfies that the growth thickness in the low temperature maintenance region LT is 0 to 25% of the total thickness of the passivation, and the growth thickness in the temperature rising region RT is 0 to 25% of the total thickness of the passivation, the refractive index of the thin film in Example 1-4 is 2.074 to 2.11, which is better than the refractive index of the thin film in Comparative Example 1, which is 2.014.

[0037] As shown in Example 2-3, when the passivation layer satisfies that the growth thickness in the low temperature maintaining region LT is 0% of the total thickness of the passivation, the growth thickness in the temperature rising region RT is 5-25% of the total thickness of the passivation, and the growth thickness in the high temperature maintaining region HT is 75-95% of the total thickness of the passivation, the breakdown voltages of Example 2-3 are 1.05 and 1.1 V / nm, respectively, and the RMS roughnesses are smaller than 0.5 nm, while the breakdown voltage of Comparative Example 1 is 0.96 V / nm, and the RMS roughness is larger than 0.5 nm. In other words, the structure of Example 2-3 has a better breakdown voltage level and a better RMS roughness than Comparative Example 1.

[0038] As shown in Example 2-4, when the passivation layer satisfies that the growth thickness in the temperature rising region RT is 5-25% of the total thickness of the passivation and the growth thickness in the high temperature maintaining region HT is 50-95% of the total thickness of the passivation, the sheet resistance change amount in Example 2-4 is 0.1% or less, while the sheet resistance change amount in Comparative Example 1 is larger than 0.5%. That is, the configuration in Example 2-4 has a better stability of sheet resistance than Comparative Example 1. Also, as can be seen directly from the results in Example 2-4, when the passivation layer is growing, if the first growth temperature T1 is controlled to rise to the second growth temperature in a time period through the temperature rising region RT (Example 2-4), a configuration having a better stability of sheet resistance can be obtained, compared to completing the growth of the passivation layer entirely in the low temperature maintaining region (Comparative Example 1) or the high temperature maintaining region (Example 1).

[0039] Table 2 TIFF0007594613000002.tif66136

[0040] The present invention further provides another high electron mobility transistor structure 1. As shown in FIG. 2, the high electron mobility transistor structure 1 includes a substrate 10, a nucleation layer 20, a buffer layer 30, a channel layer 40, a barrier layer 50, and a passivation layer 60 in order. Among them, a two-dimensional electron gas region is formed in the channel layer 40 along the boundary between the channel layer and the barrier layer 50. The channel layer 40 has a sheet resistance value change of 1% or less in the two-dimensional electron gas region during a time period, and the time period is three months or more. By forming the passivation layer 60, the two-dimensional electron gas region in the channel layer 40 has a sheet resistance value change of 1% or less during the time period. The time period is three months or more. And the purpose of improving the stability of the high electron mobility transistor can be achieved. In this embodiment, the high electron mobility transistor structure 1 is produced by the manufacturing method of the high electron mobility transistor structure.

[0041] Wherein, the passivation layer 60 is made of silicon nitride, the total thickness of the passivation layer 60 is 100 nm or less, the refractive index of the passivation layer 60 is 2.05 to 2.28, the surface roughness RMS of the passivation layer 60 is 0.5 nm or less, and the breakdown voltage value per unit thickness of the passivation layer 60 is 1 to 1.15 V / nm. That is, the high electron mobility transistor configuration 1 provided by the present invention is a thin film with good density, has good surface roughness, and has high stability of withstand voltage level and sheet resistance value. Thus, the objective of improving the stability of the high electron mobility transistor can be achieved.

[0042] From the above, the effects of the present invention are as follows. Since the passivation layer 60 and the barrier layer 50 are controlled to grow without interruption in the same growth chamber, it is possible to avoid defects during the growth of the passivation layer 60 and deterioration of the quality at the boundary between the passivation layer 60 and the barrier layer 50 due to drastic changes in temperature, pressure, and atmosphere, and thus it is possible to provide a high-quality passivation layer 60 and a high-quality boundary between the passivation layer and the barrier layer, thereby achieving the objective of improving the performance of the high electron mobility transistor. In addition, the high electron mobility transistor configuration 1 further provided by the present invention forms the passivation layer 60, so that the two-dimensional electron gas region in the channel layer 40 has a sheet resistance value change of 1% or less during the time period. The time period is three months or more. And it is possible to achieve the objective of improving the stability of the high electron mobility transistor.

[0043] The above are merely preferred possible embodiments of the present invention, and any equivalent variations made using the specification and claims of the present invention should be included within the patent scope of the present invention. [Explanation of symbols]

[0044] S02, S04, S06, S08, S10, S12 steps 1 High electron mobility transistor configuration 10 Substrate 20 Nucleation layer 30 Buffer Layer 40 Channel Layer 50 Barrier Layer 60 Passivation Layer HT high temperature maintenance area LT Low temperature maintenance area RT Temperature rise region T1 First growth temperature T2 Second growth temperature t1, t2, t3, t4, ta, tb, tc predetermined time

Claims

1. Step A of providing a substrate; Step B of forming a nucleation layer above the substrate; Step C of forming a buffer layer above the nucleation layer; Step D of forming a channel layer above the buffer layer; a step E of depositing a barrier layer over the channel layer, the growth temperature of the barrier layer being a first growth temperature, and a two-dimensional electron gas region being formed in the channel layer along an interface between the channel layer and the barrier layer, the step E being performed in a growth chamber; and after step E, step F of depositing a passivation layer over the barrier layer in the growth chamber without interruption and controlling a growth temperature of the passivation layer to ramp from the first growth temperature through a heating zone to a second growth temperature.

2. 2. The method of claim 1, wherein the barrier layer and the passivation layer are formed under the same growth conditions of pressure and atmosphere.

3. 2. The method of claim 1, wherein step F includes controlling to maintain the second growth temperature in a high temperature sustaining region.

4. 4. The method of claim 3, wherein the thickness of the passivation layer grown in the high temperature maintaining region accounts for 50% or more of the total thickness of the passivation layer.

5. 2. The method of claim 1, wherein the second growth temperature is greater than or equal to 1000[deg.] C.

6. measuring a sheet resistance of the two-dimensional electron gas region in the channel layer as a first sheet resistance; and, after a time period has elapsed, measuring a sheet resistance of the two-dimensional electron gas region in the channel layer as a second sheet resistance; 2. The method of claim 1, wherein the time period is greater than or equal to three months, the absolute value of the proportional change in sheet resistance is less than or equal to 0.1%, and the proportional change in sheet resistance is defined as (the second sheet resistance - the first sheet resistance) / the first sheet resistance * 100%.

7. A substrate; A nucleation layer; A buffer layer; A channel layer; a barrier layer, wherein a two-dimensional electron gas region is formed in the channel layer along a boundary between the channel layer and the barrier layer; a passivation layer; the two-dimensional electron gas region in the channel layer has a sheet resistance value that changes by 1% or less over a period of time, the period of time being three months or more; the passivation layer has an overall thickness of 100 nm or less; The passivation layer has a refractive index of 2.05 to 2.28; The passivation layer has a surface roughness RMS of 0.5 nm or less; The passivation layer has a breakdown voltage per unit thickness of 1 to 1.15 V / nm; 13. A high electron mobility transistor structure, wherein the passivation layer is silicon nitride.

Citation Information

Patent Citations

  • Nitride-based transistors with protective layers and low-damage recesses and methods of making same

    JP2007518265A

  • Field effect transistor

    JP2009224760A

  • Method for fabricating transistor with supported gate electrode and related device

    JP2009524242A

  • CMOS compatible method for manufacturing HEMT device and HEMT device thereof

    JP2013012735A

  • Forming method of silicon nitride passivation film and manufacturing method of semiconductor device