Colored jade-effect ceramic rock slab and its manufacturing method

By using colored glass cullet with chromium(III) oxide for ceramic tiles, the issues of high costs and surface defects in existing ceramic tiles are addressed, resulting in a stable, cost-effective, and aesthetically superior product.

JP7594684B2Active Publication Date: 2024-12-04MONALISA GRP CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2023552200
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-31
Filing Date
2021-12-03
Publication Date
2024-12-04
Estimated Expiration
2041-12-03

AI Technical Summary

Technical Problem

Existing ceramic tiles with imitation stone effect face issues such as high costs due to expensive frits and pigments, dispersion of pigments at high temperatures leading to blurred patterns, and surface defects like bubbles and dents, affecting the aesthetic appearance and flatness.

Method used

Use colored glass cullet instead of frits and pigments, utilizing chromium(III) oxide for color, which remains stable at high temperatures, ensuring even surface and reduced costs through controlled application and firing processes.

Benefits of technology

Achieves a flat, strong three-dimensional effect with reduced costs, avoiding pigment dispersion and surface defects, while maintaining production stability and energy efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594684000001
    Figure 0007594684000001
  • Figure 0007594684000002
    Figure 0007594684000002
Patent Text Reader

Abstract

This invention relates to a ceramic rock slab with a colored jade effect and a method for manufacturing the same. The manufacturing method includes the steps of pressing a raw material containing a ceramic substrate and colored glass cullet to obtain a ceramic body, and then drying and firing the ceramic body to form a ceramic rock slab with colored jade effect particles dispersed on the surface of the body, where the ratio of colored glass cullet to the ceramic substrate is 3-5 wt%. By using colored glass cullet instead of frit and pigment to manufacture the colored jade effect ceramic rock slab, there is no pigment dispersion after high-temperature firing, and the rock slab surface after firing has no micro-protrusions. After polishing, the surface is smoother and less dented, resulting in a better surface effect. This significantly reduces costs, turning waste into treasure, and allows for the production of better-effect ceramic products instead of expensive frit.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a colored jade effect ceramic rock slab and its manufacturing method, which belongs to the technical field of architectural ceramics manufacturing. [Background technology]

[0002] In recent years, with the rapid development of China's industry, its economic strength has improved rapidly, and people's pursuit of quality of life has improved, especially the requirements for living environment have become more stringent. Architectural ceramic tiles, which are widely used in the home decoration industry as decorative materials to beautify living space, have also undergone major changes. Existing architectural ceramic tiles have evolved from polished tiles to glazed tiles, and then to the current soluble salt tiles, ceramic slabs, rock slabs, etc. Soluble salt tiles have the advantages of both polished tiles and glazed tiles, and are deeply loved by consumers, while ceramic slabs and rock slabs are becoming increasingly popular in the field of home decoration.

[0003] At present, most of the imitation stone effect large-grain ceramic soluble salt tiles on the market are generally realized by adding frits to the ceramic base, and these frits are many in variety and expensive. If you want to achieve color effects, you need to add corresponding pigments, and these pigments are easy to disperse at high temperatures, which may cause the pattern to become blurred after firing. In addition, these frits are mostly medium-low temperature frits, so potassium and sodium ions melt rapidly at high temperatures to produce a glass phase, and as the temperature increases, the base continues to be exhausted until sintering, and because the initial melting point is low, the area where the frit is applied will react locally with the base, and air bubbles will continue to be exhausted, causing the base to shrink, and the tile surface may sink locally after high-temperature firing. This not only increases the cost, but also worsens the tile surface effect and polishing effect, affecting the flatness and aesthetics of the tile surface. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] China Patent Application Publication No. 109455934 [Patent Document 2] China Patent Application Publication No. 102515876 Summary of the Invention [Problem to be solved by the invention]

[0005] In response to the problems presented in the background art, the present invention uses colored glass cullet instead of expensive frit and pigment to produce ceramic rock slab with colored jade effect, so that after high-temperature firing, there is no pigment dispersion phenomenon, and the surface of the rock slab after firing has micro-protrusions, and after polishing, the surface is more flat and has no dents, the surface effect is better, the cost is greatly reduced, waste is turned into treasure, and ceramic products with better effects can be produced. [Means for solving the problem]

[0006] Meanwhile, the present invention provides a method for manufacturing a ceramic rock slab with colored jade effect, which includes the steps of pressing a raw material containing a ceramic base material and colored glass cullet to obtain a ceramic body, and drying and firing the ceramic body to form a ceramic rock slab with colored jade effect particles dispersed on the surface of the body.

[0007] The color of colored glass cullet is due to the fact that its composition contains chromium (III) oxide, which is the main color-producing substance. Chromium (III) oxide is very stable, with a melting point of about 2266±25°C and a boiling point of about 4000°C, and is generally produced from chromium oxide at 1100°C or higher. Since the temperature in the ceramic firing process does not exceed 1200°C, and the melting temperature of glass is far above 1200°C, colored glass cullet that has been melted at high temperatures will not change due to the influence of the atmosphere and temperature of the kiln, and the structure of colored glass cullet will not be damaged during the high-temperature sintering process of ceramics. According to the manufacturing method of the present invention, by utilizing the characteristics of colored glass cullet being stable at high temperatures and not dispersing pigments, the obtained rock plate has a flat surface and a strong three-dimensional effect after firing. In addition, the use of glass cullet greatly reduces manufacturing costs, facilitates industrial production, and is energy-saving and environmentally friendly.

[0008] By controlling the mass percentage of colored glass cullet to the ceramic substrate at 3-5wt%, the required color jade effect can be achieved while ensuring the stability of production and not affecting the original production process. If the mass percentage of colored glass cullet to the ceramic substrate exceeds 5wt%, it will affect the production process, for example, the volume density distribution of the green body in the pressing step will be uneven, which will reduce the strength of the green body and affect the subsequent steps of transportation, drying, etc. The reason for the above effect is mainly because the pressing of the green body has certain requirements for powder materials, such as particle grading, moisture, unit volume mass, etc. The physical and chemical properties of colored glass cullet and the ceramic substrate are very different, so under the premise of meeting the normal process of the green body, the dosage of colored glass cullet should not be too large.

[0009] Preferably, the chemical composition of the ceramic substrate is, in mass percentage, SiO 2 : 65-69%, Al 2 O 3 : 18~22%, alkali metal oxide: 4~9%. If the alkali metal content is too high, it lowers the firing temperature of the base material, affecting the water absorption rate, strength and tile shape of the base material.

[0010] The selection principle for the colored glass cullet of the present invention is that the material does not react with the ceramic substrate or produce chemicals that are unfavorable to the formation of ceramics, and the colored glass cullet can be stable and colored at high temperatures. Preferably, the chemical composition of the colored glass cullet is, in mass percentage, SiO 2 : 65-70%, Al 2 O 3 : 2-4%, alkaline earth metal oxides: 9-13%, alkali metal oxides: 10-16%.

[0011] Preferably, the ceramic body has a maximum firing temperature of 1200° C. or less and a firing cycle of 63 to 105 minutes.

[0012] Preferably, the colored glass cullet has a particle size of 6-8 mesh.

[0013] Preferably, the colored glass cullet has a linear expansion coefficient of 6.8×10 -6 ~7.2×10 -6 / K (0 to 400°C), and the linear expansion coefficient of the ceramic substrate is 7.0 × 10 -6 ~7.8×10 -6 / K (0 to 400°C). The coefficient of expansion of glass cullet is close to that of ceramic substrates, with a difference of generally 0.2 to 0.6 × 10 -6 / K (0~400℃). This prevents cracks from occurring after high-temperature sintering due to the mismatch in expansion coefficient between the glass particles and the base material, which can affect the decorative effect.

[0014] Preferably, the ceramic substrate is applied first before pressing, and then the colored glass cullet is applied to the top layer of the ceramic substrate. Preferably, the colored glass cullet is applied to the top layer of the ceramic substrate.

[0015] Meanwhile, the present invention provides a ceramic rock slab with colored jade effect obtained by any one of the manufacturing methods described above. In some embodiments, the surface of the ceramic rock slab has micro-protrusions with a height of 0.2 mm or less. Preferably, the height of the micro-protrusions is 0.1-0.2 mm.

[0016] The specifications of the above mentioned ceramic rock slabs are width (600-1600) mm x length (600-3600) mm x thickness (9.5-15) mm. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a diagram showing the effect of the tile surface of the first embodiment. [Diagram 2] FIG. 13 is a diagram showing the effect of the tile surface of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention will be further described below in conjunction with the following embodiments. The following embodiments are for the purpose of illustrating the present invention, but are not intended to limit the present invention. Each "%" content means "mass%" content unless otherwise specified. "Color glass cullet" is also referred to as "glass cullet" or "glass particles" unless otherwise specified.

[0019] The manufacturing method of the ceramic rock slab with colored jade effect of the present invention will be illustrated as follows.

[0020] A ceramic substrate is manufactured. The chemical composition of the ceramic substrate can be in accordance with the production process of ceramic rock slabs. In some embodiments, the chemical composition of the ceramic substrate is, in mass percentage, SiO 2 : 65-69%, Al 2 O 3 : 18 to 22%, alkali metal oxide: 4 to 9%. For example, the chemical composition of the ceramic substrate is, in mass percentage, SiO 2 : 65-69%, Al 2 O 3 : 18-22%, Fe 2 O 3: 0.2-0.4%, TiO 2 :0.01~0.2%, CaO:0.3~0.5%, MgO:0.5~0.9%, K 2 O: 2-4%, Na 2 O: 2-5%, ZrO 2 : 0.2~0.5%, P 2 O 5 : 0.1-0.2%, SO 3 It may contain 0.1 to 0.2%, and loss on ignition: 3 to 5%.

[0021] The raw material blend of the ceramic substrate can be adjusted according to its chemical composition, for example, potassium feldspar, nepheline, spherical clay, bentonite, black talc, and iron aluminium are selected and blended. The ceramic substrate can be manufactured by the following steps. 100% raw material, 40-50% water, and 0.1-0.5% sodium tripolyphosphate are mixed and ground in a ball mill, and sieved to form a slurry. The grinding time in the ball mill may be 5-10 minutes. The sieve residue of the slurry on a 325 mesh is ≦1wt%. The slurry is dried and ground to form a ceramic substrate with a moisture content of ≦9wt%. If the moisture content of the ceramic substrate is within the above range, it is advantageous for molding.

[0022] The colored glass cullet is applied to the surface of the ceramic substrate. Preferably, a positioning application method is adopted, that is, the colored glass cullet is applied to the appropriate position according to the requirements of the tile surface effect. For example, according to the tile effect, the adhesive is sprayed on the corresponding position of the ceramic substrate surface, and then the colored glass cullet is applied, and the excess colored glass cullet is removed by an electric fan. The color of the colored glass cullet can be green, red, etc.

[0023] The chemical composition of the colored glass cullet is, in mass percentage, SiO 2 : 65-70%, Al 2 O 3 : 2 to 4%, alkaline earth metal oxide: 9 to 13%, and alkali metal oxide: 10 to 16%. As an example, the chemical composition of the colored glass cullet may include, in mass percentage, SiO 2 : 65-70%, Al 2 O3 : 2-4%, Fe 2 O 3 :0.2~0.4%, CaO:8~10%, MgO:1~2%, K 2 O: 0.5-1%, Na 2 O: 10-15%, P 2 O 5 0.2~0.4%, Ba0:0.1~0.3%, Cr 2 O 3 : 0.1-0.2%, SO 3 : Contains 0.1 to 0.2% of the above colored glass cullet. 2 O 3 Very low TiO content 2 This prevents black or yellow spots from appearing and ensures the decorative effect of the substrate.

[0024] The temperature during glass melting (including the glass refining stage and the glass homogenization stage) is usually higher than 1200°C, and can reach 1200-1300°C, even 1200-1600°C. The firing temperature of the ceramic substrate (i.e., the firing temperature during the manufacture of ceramic rock slabs) is lower than the melting temperature of the glass particles. In the high-temperature firing process of the ceramic substrate, the glass particles will not form a large number of bubbles in the glass particles due to over-firing at this temperature, so there are fewer pores in the polishing process, the anti-fouling effect is not affected, and the decorative effect of the tile surface is better. In addition, under the firing temperature of the ceramic substrate, the glass cullet in the ceramic base will not appear in a "boiling" state due to the low temperature. When the "boiling" state appears, the softened granules will diffuse to positions other than the original position of the granules, and the content of the particles in the original position will decrease, so that a certain depression will be formed in the original position when cooled. Since the glass particles have a low temperature, the "boiling" state will not appear, and accordingly, no depression will occur. In addition, the firing of glass particles is a secondary firing, and the ignition loss and the volume change before and after firing are small. The sintering of the ceramic base material is a sintering of raw materials, and the ignition loss after high-temperature firing is larger than that of the glass particles. In this way, the overall volume of the base material is small and the volume change of the glass particles is small, so no dents are generated after high-temperature firing.

[0025] The fineness of the colored glass cullet may be sufficient as long as it satisfies the performance of the production process, for example, molding. The particle size of the colored glass cullet may be appropriately adjusted according to the size and thickness specifications of the base material. For example, for a base material with a large standard thickness, the glass cullet particles may be appropriately increased. The particle size of the colored glass cullet is preferably 6 to 8 mesh. If the particle size of the colored glass cullet is small, the colored glass cullet may react with the ceramic substrate under high temperature, which may affect the color effect. If the particle size of the colored glass cullet is large, the uneven distribution of the particles and the ceramic substrate during molding of the base material may cause the distribution of the density of the base material to be uneven, which may cause defects such as broken or cracked tiles in the finished product.

[0026] In some embodiments, the dosage of colored glass cullet to the ceramic substrate is controlled to be 3 wt% to 5 wt%.

[0027] After applying the raw materials, the ceramic body is obtained by pressing. The ceramic body is then dried. The drying time may be 1.5 to 2 hours. The moisture content of the dried ceramic body is controlled to 0.3 to 0.5 wt%.

[0028] The ceramic base is dried and fired to obtain a ceramic rock slab with a color jade effect. The drying time may be 10 minutes. The maximum firing temperature of the ceramic rock slab is 1200°C or less. For example, the maximum firing temperature may be 1183-1190°C, and the firing cycle may be 63-105 minutes.

[0029] In some embodiments, a pattern is inkjet printed onto the surface of the ceramic body prior to firing, and the ink penetrates the dried ceramic body to form a pattern on the surface of the body, thus enhancing the decorative effect of the ceramic rock slab.

[0030] The fired ceramic rock slabs are taken out of the kiln and polished, edge-polished and graded according to demand, then packaged and stored. For example, they are polished with elastic modules. The polishing modules can be arranged in combinations of 240 mesh x 4, 300 mesh x 8, 400 mesh x 8, 600 mesh x 4, 800 mesh x 4, 1000 mesh x 4, 1500 mesh x 4, 2000 mesh x 4, and 3000 mesh x 8.

[0031] Since the color glass cullet does not change color after firing, the color jade effect particles can be seen distributed on the surface of the ceramic body after polishing treatment. The size of the color jade effect particles can reach 2~4mm (corresponding to 6 mesh~8 mesh).

[0032] The purpose of the present invention is to protect the use of colored glass cullet in colored jade effect ceramic rock slab, and the method of applying raw materials is not limited to the present invention. Other methods can be used to form the ceramic body. For example, the colored glass cullet is added to the ceramic substrate and mixed uniformly, then the raw materials are applied and pressed to form the ceramic body. Also, the colored glass cullet can be dried and then added to the ceramic substrate, mixed uniformly, then the raw materials are applied, preferably positioned, and pressed to form the ceramic body.

[0033] The present invention will be described in more detail with reference to the following examples. The following examples are merely for further explanation of the present invention and do not limit the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention are also within the scope of protection of the present invention. Specific process variables in the following examples are merely examples within the applicable range, that is, those skilled in the art can select within an appropriate range based on the description of the present invention, and are not limited to the specific numerical values ​​in the following examples.

[0034] Example 1 (1) Manufacture a ceramic substrate. The chemical composition of the ceramic substrate is, by mass percentage, SiO 2 : 66.04%, Al 2 O3 : 20.29%, Fe 2 O 3 : 0.38%, TiO 2 :0.16%, CaO:0.39%, MgO:0.62%, K 2 O: 3.15%, Na 2 O: 3.36%, ZrO 2 :0.46%, P 2 O 5 :0.13%, SO 3 : 0.19%, ignition loss: 4.79%. 100% dried ceramic substrate (i.e. all raw materials of ceramic substrate), 50% water, 0.5% sodium tripolyphosphate are mixed in a ball mill and ground for 6 minutes, sieved, 325 mesh sieve residue is ≦ 1wt%, and dried to form ceramic substrate. The moisture content of ceramic substrate is ≦ 9wt%.

[0035] (2) Forming the ceramic body. A method of applying the raw materials twice is used. First, the ceramic base material is applied, and then colored glass cullet is applied to the surface of the ceramic base material at a ratio of 3 to 5 wt% to the ceramic base material, and the ceramic body is formed by pressing. The chemical composition of the colored glass cullet is, by mass percentage, SiO 2 : 68.40%, Al 2 O 3 : 3.43%, Fe 2 O 3 :0.35%, CaO:9.07%, MgO:1.37%, K 2 O: 0.88%, Na 2 O: 14.1%, P 2 O 5 : 0.36%, BaO: 0.23%, Cr 2 O 3 :0.16%, SO 3 : Contains 0.16%. The grain size of colored glass cullet is 6~8 mesh.

[0036] (3) The ceramic body is placed in a kiln and dried. The drying time is 1.5-2.0 hours, and the moisture content of the ceramic body after drying is 0.3-0.5 wt%.

[0037] (4) The design pattern is inkjet printed onto the surface of the ceramic base.

[0038] (5) The ceramic body with the design pattern inkjet printed on it is placed in a kiln to dry, and the drying time is 10 minutes.

[0039] (6) Place in a kiln and fire. The maximum firing temperature is 1190℃, and the firing cycle is 63 minutes.

[0040] (7) Polishing and grading are performed. After removing from the kiln, the material is polished with elastic modules. The polishing module arrangement combinations are 240 mesh x 4 sets, 300 mesh x 8 sets, 400 mesh x 8 sets, 600 mesh x 4 sets, 800 mesh x 4 sets, 1000 mesh x 4 sets, 1500 mesh x 4 sets, 2000 mesh x 4 sets, and 3000 mesh x 8 sets.

[0041] (8) Pack and store.

[0042] As can be seen from Figure 1, after polishing, the jade effect particles are distributed on the surface of the substrate, the particle effect is transparent, and a better texture hierarchy effect is achieved.

[0043] Example 2 It is basically the same as Example 1, except that the chemical composition of the ceramic substrate is, in mass percentage, SiO 2 : 65%, Al 2 O 3 : 18%, Fe 2 O 3 : 0.2%, TiO 2 :0.01%, CaO:0.3%, MgO:0.5%, K 2 O: 2%, Na 2 O: 2%, ZrO 2 :0.2%, P 2 O 5 :0.1%, SO 3 It only contains 0.1% and loss on ignition: 3%.

[0044] Example 3 It is basically the same as Example 1, except that the chemical composition of the ceramic substrate is, in mass percentage, SiO 2: 69%, Al 2 O 3 : 22%, Fe 2 O 3 : 0.4%, TiO 2 :0.2%, CaO:0.5%, MgO:0.9%, K 2 O: 4%, Na 2 O: 5%, ZrO 2 :0.5%, P 2 O 5 :0.2%, SO 3 : 0.2%, Loss on Ignition: 5%.

[0045] Comparative Example 1 This is basically the same as Example 1, with the only difference being that color frit is used instead of glass particles. Color frit is generally composed of transparent frit and pigment. The chemical composition of the color frit is, in mass percentage, SiO 2 : 50.61%, Al 2 O 3 : 2%, Fe 2 O 3 : 0.5%, CaO: 8%, MgO: 8.5%, K 2 O: 5%, Na 2 O:10%, ZnO:5%, BaO:4.23%, CeO 2 :5%, SO 3 0.16%, ignition loss: 1%. The expansion coefficient of the color frit is 5×10 -6 / K~6×10 -6 / K (0~400℃).

[0046] As can be seen from FIG. 2, there are dents on the tile surface, and cracks occur at the places where the particles are applied. The frit has a lower temperature than the glass particles, and its components include zinc oxide, which has a higher alkali metal content than the glass particles. In the process of firing the base material at high temperature, the frit undergoes a "boiling" phenomenon, and the liquid phase at high temperature diffuses to the surrounding positions, reducing the content at the original position, and causing the dent phenomenon. From FIG. 2, the transparency of the tile surface is poor and appears hazy. This is related to the frit particles "boiling" at high temperatures. At high temperatures, a large amount of gas is generated in the frit liquid phase, just like water boils, and when the gas is cooled, it is wrapped and remains as bubbles, and when light passes through, the bubbles scatter the light, resulting in poor transparency. In addition, as can be seen from the figure of Comparative Example 1, cracks occur at the places where the frit is applied. This is because the expansion coefficients of the frit and the ceramic substrate are not compatible. The expansion coefficient of the frit is small, so the volume change after high-temperature cooling is small. The base material has a large expansion coefficient and loss on ignition, so it shrinks significantly after cooling from high temperature, and the original volume of the area where the frit is applied is reduced. As such, the volume of the frit particles after firing is larger than the volume of the area of ​​the base material after firing, and there is a certain amount of extrusion, which causes cracks after cooling.

Claims

1. A method for producing a colored jade effect ceramic rock slab, comprising the steps of: The manufacturing method includes: A first step of press-molding a raw material containing a ceramic base material and colored glass cullet to obtain a ceramic body; (wherein the ratio of the colored glass cullet to the ceramic substrate is 3 to 5 wt %, The chemical composition of the ceramic substrate is, in mass percentage, SiO 2 : 65-69%, Al 2 O 3 : 18-22%, alkali metal oxides: 4-9%, The colored glass cullet has a particle size of 6-8 mesh and a chemical composition, in mass percentage, of: SiO 2 : 65-70%, Al 2 O 3 :2~4%, Fe 2 O 3 :0.2-0.4%, CaO: 8-10%, MgO: 1-2%, K 2 O: 0.5-1%, Na 2 O: 10-15%, P 2 O 5 0.2-0.4%, BaO: 0.1-0.3%, Cr 2 O 3 : 0.1-0.2%, SO 3 : 0.1 to 0.2% included, The colored glass cullet has a linear expansion coefficient of 6.8×10 -6 ~7.2×10 -6 / K, and the ceramic substrate has a linear expansion coefficient of 7.0×10 -6 ~7.8×10 -6 / K, and the difference in linear expansion coefficient between the colored glass cullet and the ceramic substrate at 0 to 400°C is 0.2 to 0.6 x 10 -6 / K) a second step of drying and firing the ceramic body; and a third step of polishing the fired ceramic body after it is taken out of the kiln, and after polishing, the color jade effect particles are distributed on the surface of the ceramic body. The ceramic rock slab is characterized in that the pigment is not dispersed and the rock slab surface has minute protrusions with a height of 0.2 mm or less. How to make ceramic rock slabs with colored jade effect.

2. The manufacturing method according to claim 1, characterized in that the ceramic body has a maximum firing temperature of 1200°C or less and a firing cycle of 63 to 105 min.

3. 2. The manufacturing method according to claim 1, characterized in that, before pressing, the ceramic substrate is applied first, and then the colored glass cullet is applied on the upper layer of the ceramic substrate.

4. The method according to claim 3, characterized in that the colored glass cullet is positioned and applied on top of the ceramic substrate.

Citation Information

Patent Citations

  • Production process of novel multiple crystallization combined glass-ceramic clad plate

    CN101177346A

  • Resin acid titanium-iron-bismuth system yellow-series electro-optic water and preparation method thereof

    CN102515876A

  • Flowing color decorative effect ceramic tile and preparation method thereof

    CN109455934A

  • Tairunoseizohoho