All solid state battery

The all-solid-state battery with dual negative electrode active materials provides clear discharge curve flat portions for easy end point detection, addressing the challenge of steep voltage drops in existing batteries and ensuring stable charging.

JP7594866B2Active Publication Date: 2024-12-05TAIYO YUDEN KK
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020111789
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-29
Publication Date
2024-12-05
Estimated Expiration
2040-06-29

AI Technical Summary

Technical Problem

Existing batteries face challenges in accurately detecting the end point of discharge due to a steep voltage drop at the end of the discharge curve, making it difficult to charge before the cell voltage drops significantly below the end point voltage.

Method used

The all-solid-state battery incorporates an oxide-based solid electrolyte layer with a positive electrode layer and a negative electrode layer containing two different negative electrode active materials with distinct average operating potentials, ensuring a clear two-step potential flat portion in the discharge curve for easy end point detection.

Benefits of technology

This design allows for easy detection of the end point, preventing significant voltage drops and ensuring the cell voltage remains above the necessary level for charging, thereby maintaining operational effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594866000002
    Figure 0007594866000002
  • Figure 0007594866000003
    Figure 0007594866000003
  • Figure 0007594866000004
    Figure 0007594866000004
Patent Text Reader

Abstract

To provide an all-solid-state battery with easy endpoint detection.SOLUTION: An all-solid-state battery includes an oxide solid electrolyte layer, a positive electrode layer provided on the first main surface of the oxide solid electrolyte layer and containing a positive electrode active material, and a negative electrode layer, provided on a second main surface of the oxide solid electrolyte layer, containing a first negative electrode active material and a second negative electrode active material whose average operating potentials (vs Li / Li+) are different from each other.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an all-solid-state battery. [Background technology]

[0002] In recent years, secondary batteries have been used in various fields. Secondary batteries using electrolytes have problems such as electrolyte leakage. Therefore, all-solid-state batteries that have a solid electrolyte and other components made of solids are being developed.

[0003] A solid electrolyte has a wider potential window (wide range of voltage stability) than an electrolytic solution. In particular, an oxide-based solid electrolyte that exhibits high ionic conductivity by sintering has the advantage of having a wider potential window and being relatively stable in air compared to electrolytic solution systems and other solid electrolyte systems. For example, an all-solid-state battery obtained by co-firing an oxide-based solid electrolyte with a negative electrode active material has been disclosed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2014 / 038311 Summary of the Invention [Problem to be solved by the invention]

[0005] To operate devices such as ICs (Integrated Circuits), it is necessary to control the voltage so that it does not drop below 1.8V. For this reason, many batteries are designed to have an end-point voltage (lower limit voltage) and to begin charging when the monitored cell voltage drops to the end-point voltage. The discharge curve of a typical battery changes to a steeper slope compared to the slope of the voltage drop in the potential plateau at the end of discharge when the battery level is low. The voltage drop in a short period of time is what makes it difficult to detect the end point.

[0006] The present invention has been made in consideration of the above problems, and has an object to provide an all-solid-state battery in which the end point can be easily detected. [Means for solving the problem]

[0007] The all-solid-state battery according to the present invention includes an oxide-based solid electrolyte layer, a positive electrode layer provided on a first main surface of the oxide-based solid electrolyte layer and containing a positive electrode active material, and a positive electrode layer provided on a second main surface of the oxide-based solid electrolyte layer and containing an average operating potential (vs Li / Li + and a negative electrode layer including a first negative electrode active material and a second negative electrode active material having mutually different properties.

[0008] In the above all-solid-state battery, the average operating potential (vs Li / Li + ) is 2.0 V or less, and the average operating potential (vs Li / Li + ) may be 2.4V or more.

[0009] In the above all-solid-state battery, the first negative electrode active material is TiO2, Li 1-2x M x TiOPO4 (M is a divalent metal element, 0≦x≦0.5), Li 3x La 2 / 3-x Any of TiO3, Nb2O5, and Nb-Ti-O based compounds may be used.

[0010] In the above all-solid-state battery, the second negative electrode active material may be a Ti-containing phosphate having a NASICON-type crystal structure or TiP2O7.

[0011] In the above all-solid-state battery, the Ti-containing phosphate is Li 1+y A y Ti 2-y It may be (PO4)3, where A is a trivalent metallic element and 0≦y≦0·7.

[0012] In the all-solid-state battery, the second negative electrode active material may have an average crystal grain size of 0.5 μm or more and 50 μm or less. Effect of the Invention

[0013] According to the present invention, it is possible to provide an all-solid-state battery in which the end point can be easily detected. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a basic structure of an all-solid-state battery. [Diagram 2] FIG. 2 is a diagram illustrating a discharge curve when the negative electrode contains one type of negative electrode active material. [Diagram 3] FIG. 4 is a schematic cross-sectional view of a second internal electrode. [Figure 4] 10 is a diagram illustrating a discharge curve in a second internal electrode when the second internal electrode contains a first negative electrode active material and a second negative electrode active material. FIG. [Diagram 5] FIG. 1 is a schematic cross-sectional view of an all-solid-state battery according to an embodiment. [Figure 6] FIG. 1 is a schematic cross-sectional view of another all-solid-state battery. [Figure 7] FIG. 1 is a diagram illustrating a flow of a method for producing an all-solid-state battery. [Figure 8] 1(a) and (b) are diagrams illustrating the lamination process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment will be described with reference to the drawings.

[0016] (Embodiment) Fig. 1 is a schematic cross-sectional view showing the basic structure of an all-solid-state battery 100. As illustrated in Fig. 1, the all-solid-state battery 100 has a structure in which a solid electrolyte layer 30 is sandwiched between a first internal electrode 10 and a second internal electrode 20. The first internal electrode 10 is formed on a first main surface of the solid electrolyte layer 30. The second internal electrode 20 is formed on a second main surface of the solid electrolyte layer 30.

[0017] When the all-solid-state battery 100 is used as a secondary battery, one of the first internal electrode 10 and the second internal electrode 20 is used as a positive electrode, and the other is used as a negative electrode. In the present embodiment, as an example, the first internal electrode 10 is used as a positive electrode, and the second internal electrode 20 is used as a negative electrode.

[0018] The solid electrolyte layer 30 is mainly composed of a solid electrolyte having ion conductivity. The solid electrolyte of the solid electrolyte layer 30 is, for example, an oxide-based solid electrolyte having lithium ion conductivity. The solid electrolyte is, for example, a phosphate-based solid electrolyte having a NASICON structure. The phosphate-based solid electrolyte having a NASICON structure has a high electrical conductivity and is stable in the air. The phosphate-based solid electrolyte is, for example, a phosphate containing lithium. The phosphate is not particularly limited, but examples thereof include a composite lithium phosphate salt with Ti (for example, LiTi2(PO4)3). Alternatively, Ti can be partially or completely replaced with a tetravalent transition metal such as Ge, Sn, Hf, or Zr. In order to increase the Li content, it may be partially replaced with a trivalent transition metal such as Al, Ga, In, Y, or La. More specifically, for example, Li 1+x Al x Ge 2-x (PO4)3 and Li 1+x Al x Zr 2-x (PO4)3, Li 1+x Al x Ti 2-x(PO4)3. For example, Li-Al-Ge-PO4-based material to which the same transition metal as that contained in the phosphate having an olivine crystal structure contained in the first internal electrode 10 and the second internal electrode 20 is added in advance is preferable. For example, when the first internal electrode 10 and the second internal electrode 20 contain a phosphate containing Co and Li, it is preferable that the solid electrolyte layer 30 contains a Li-Al-Ge-PO4-based material to which Co is added in advance. In this case, the effect of suppressing the elution of the transition metal contained in the electrode active material into the electrolyte is obtained. When the first internal electrode 10 and the second internal electrode 20 contain a phosphate containing a transition element other than Co and Li, it is preferable that the solid electrolyte layer 30 contains a Li-Al-Ge-PO4-based material to which the transition metal is added in advance.

[0019] The first internal electrode 10 used as a positive electrode contains a substance having an olivine type crystal structure as an electrode active material. It is preferable that the second internal electrode 20 also contains the electrode active material. An example of such an electrode active material is a phosphate containing a transition metal and lithium. The olivine type crystal structure is a crystal that natural olivine has, and can be identified by X-ray diffraction.

[0020] A typical example of an electrode active material having an olivine crystal structure is LiCoPO4 containing Co. Phosphates in which the transition metal Co is substituted in this chemical formula can also be used. Here, the ratio of Li and PO4 can vary depending on the valence. Note that it is preferable to use Co, Mn, Fe, Ni, etc. as the transition metal.

[0021] The electrode active material having an olivine crystal structure acts as a positive electrode active material in the first internal electrode 10 acting as a positive electrode. For example, when only the first internal electrode 10 contains an electrode active material having an olivine crystal structure, the electrode active material acts as a positive electrode active material. When the second internal electrode 20 also contains an electrode active material having an olivine crystal structure, the second internal electrode 20 acting as a negative electrode exhibits the effects of increasing the discharge capacity and increasing the operating potential with discharge, which are presumed to be based on the formation of a partial solid solution state with the negative electrode active material, although the mechanism of action is not completely clear.

[0022] When both the first internal electrode 10 and the second internal electrode 20 contain an electrode active material having an olivine crystal structure, each electrode active material preferably contains a transition metal that may be the same or different from each other. "May be the same or different from each other" means that the electrode active materials contained in the first internal electrode 10 and the second internal electrode 20 may contain the same type of transition metal, or may contain different types of transition metals. The first internal electrode 10 and the second internal electrode 20 may contain only one type of transition metal, or may contain two or more types of transition metals. Preferably, the first internal electrode 10 and the second internal electrode 20 contain the same type of transition metal. More preferably, the electrode active materials contained in both electrodes have the same chemical composition. If the first internal electrode 10 and the second internal electrode 20 contain the same type of transition metal or contain an electrode active material of the same composition, the similarity of the compositions of the two internal electrode layers is increased, so that even if the terminals of the all-solid-state battery 100 are attached in the opposite direction, there is an effect that the battery can withstand practical use without malfunction depending on the application.

[0023] The second internal electrode 20 contains a negative electrode active material. By containing the negative electrode active material in only one electrode, it becomes clear that the one electrode acts as a negative electrode and the other electrode acts as a positive electrode. It is also possible to contain a material that is known as a negative electrode active material in both electrodes. For the negative electrode active material of the electrode, reference can be made to conventional techniques in secondary batteries as appropriate, and examples thereof include compounds such as titanium oxide, lithium titanium composite oxide, lithium titanium composite phosphate, carbon, and lithium vanadium phosphate.

[0024] In the preparation of the first internal electrode 10 and the second internal electrode 20, in addition to these electrode active materials, a solid electrolyte having ion conductivity, a conductive material (conductive assistant), etc. are added. For these members, a paste for the internal electrodes can be obtained by uniformly dispersing a binder and a plasticizer in water or an organic solvent. The conductive assistant may contain a carbon material, etc. The conductive assistant may contain a metal. Examples of the metal of the conductive assistant include Pd, Ni, Cu, Fe, and alloys containing these. The solid electrolyte contained in the first internal electrode 10 and the second internal electrode 20 may be the same as the main solid electrolyte of the solid electrolyte layer 30, for example.

[0025] Here, a case where the second internal electrode 20 contains one type of negative electrode active material will be considered. FIG. 2 is a diagram illustrating an example of a discharge curve of the second internal electrode 20 in this case. In FIG. 2, the horizontal axis indicates the discharge amount (capacity / μAh), and the vertical axis indicates the cell voltage. As illustrated in FIG. 2, even if the discharge progresses, the cell voltage remains approximately constant, and the slope of the cell voltage with respect to the discharge amount becomes small. However, at the end of the discharge when the remaining battery power becomes low, the slope of the cell voltage with respect to the discharge amount becomes suddenly large, and the cell voltage drops suddenly. In this case, even if charging is started after detecting the end point voltage, there is a risk that the cell voltage will drop significantly below the end point voltage. Therefore, it is difficult to detect the end point.

[0026] Therefore, in this embodiment, the second internal electrode 20 has an average operating potential (vs Li / Li +) are different from each other. For example, these two types of negative electrode active materials are different in at least one of the contained components and the composition ratio. Of the two types of negative electrode active materials, the negative electrode active material with the lower average operating potential is called the first negative electrode active material, and the negative electrode active material with the higher average operating potential is called the second negative electrode active material. The average operating potential is defined as the average cell voltage from 10% to 90% discharge, assuming that the current capacity when a half cell (metallic lithium arranged at the counter electrode) using the active material and the electrolyte is discharged from full charge to 3V at 0.05C (Li desorption) is 100%.

[0027] Fig. 3 is a schematic cross-sectional view of the second internal electrode 20. As illustrated in Fig. 3, in the second internal electrode 20, crystal grains of the first negative electrode active material 25 and crystal grains of the second negative electrode active material 26 are mixed. Note that, in reality, the second internal electrode 20 contains a solid electrolyte, a conductive assistant, and the like, but these are omitted in Fig. 3.

[0028] FIG. 4 is a diagram illustrating a discharge curve in the second internal electrode 20 when the second internal electrode 20 contains the first negative electrode active material 25 and the second negative electrode active material 26. As illustrated in FIG. 4, after the start of discharge, a first potential plateau appears where the degree of decrease (slope) of the cell voltage relative to the discharge amount becomes smaller than a threshold value. The first potential plateau is caused by the first negative electrode active material. As the discharge proceeds, the degree of decrease (slope) of the cell voltage relative to the discharge amount becomes larger, and then a second potential plateau appears where the degree of decrease (slope) of the cell voltage relative to the discharge amount becomes smaller than a threshold value. The second potential plateau is caused by the second negative electrode active material. Thereafter, as the discharge proceeds, the degree of decrease of the cell voltage increases rapidly. The potential plateau is defined as a range where the absolute value of the slope of the discharge curve is 2 mV / cap.% or less when the total current capacity during discharge is 100 cap.%.

[0029] If this second potential plateau is detected as the end point, it becomes easy to detect the end point, and charging can be started before the cell voltage drops significantly below the end point voltage, thereby ensuring the required cell voltage.

[0030] For example, if the difference between the average operating potential (first average operating potential) of the first negative electrode active material 25 and the average operating potential (second average operating potential) of the second negative electrode active material 26 is small, it may be difficult to detect the second average operating potential. Therefore, it is preferable to set an upper limit on the average operating potential of the first negative electrode active material 25 and a lower limit on the average operating potential of the second negative electrode active material 26. For example, the first average operating potential is preferably 1.9V or less, more preferably 1.8V or less, and even more preferably 1.7V or less. The average operating potential of the second negative electrode active material is preferably 2.2V or more, more preferably 2.3V or more, and even more preferably 2.4V or more. The difference between the average operating potential of the first negative electrode active material 25 and the average operating potential of the second negative electrode active material 26 is difficult to detect if they are too close, so it is preferably 0.3V or more, more preferably 0.5V or more, and even more preferably 0.7V or more.

[0031] For example, the first negative electrode active material 25 may be TiO2, Li 1-2x M x TiOPO4 (M is a divalent metal element, 0≦x≦0.5), Li 3x La 2 / 3-x It can be any of TiO3, Nb2O5, and Nb-Ti-O based compounds.

[0032] For example, the second negative electrode active material 26 may be a Ti-containing phosphate having a NASICON-type crystal structure or TiP2O7. 1+y A y Ti 2-y It can be expressed as (PO4)3, where A is a trivalent metallic element and 0≦y≦0·7.

[0033] If the average crystal grain size of the second negative electrode active material 26 is too small, there is a risk of mutual diffusion reactions occurring between the components during firing, and if it is too large, there is a risk of the operating rate of the active material decreasing, the rate characteristics deteriorating, etc. Therefore, it is preferable to set a lower limit and an upper limit to the average crystal grain size of the second negative electrode active material 26. For example, the average crystal grain size of the second negative electrode active material 26 is preferably 0.5 μm or more and 50 μm or less, more preferably 1.0 μm or more and 30 μm or less, and even more preferably 1.5 μm or more and 20 μm or less.

[0034] If the average crystal grain size of the first negative electrode active material 25 is too small, there is a risk of mutual diffusion reaction occurring between the members during firing, and if it is too large, there is a risk of the operating rate of the active material decreasing, the rate characteristics deteriorating, etc. Therefore, it is preferable to set a lower limit and an upper limit to the average crystal grain size of the first negative electrode active material 25. For example, the average crystal grain size of the first negative electrode active material 25 is preferably 0.5 μm or more and 50 μm or less, more preferably 1.0 μm or more and 30 μm or less, and even more preferably 1.5 μm or more and 20 μm or less.

[0035] If the amount of the first negative electrode active material 25 is too large, it may be difficult to detect the end point. Therefore, it is preferable to set an upper limit on the amount of the first negative electrode active material 25. On the other hand, if the amount of the second negative electrode active material 26 is too large, the energy density may decrease. Therefore, it is preferable to set a lower limit on the amount of the second negative electrode active material 26. For example, in the cross section of the second internal electrode 20, the ratio of the area of ​​the first negative electrode active material 25 to the total area of ​​the first negative electrode active material 25 and the second negative electrode active material 26 is 85% or more, 90% or more, or 95% or more. Also, in the cross section of the second internal electrode 20, the ratio of the area of ​​the second negative electrode active material 26 to the total area of ​​the first negative electrode active material 25 and the second negative electrode active material 26 is 5% or more, 10% or more, or 15% or more.

[0036] FIG. 5 is a schematic cross-sectional view of a stacked type all-solid-state battery 100a in which a plurality of battery units are stacked. The all-solid-state battery 100a includes a stacked chip 60 having a substantially rectangular parallelepiped shape. In the stacked chip 60, a first external electrode 40a and a second external electrode 40b are provided so as to contact two side surfaces, which are two of the four surfaces other than the upper and lower surfaces at the ends in the stacking direction. The two side surfaces may be two adjacent side surfaces, or may be two side surfaces facing each other. In this embodiment, the first external electrode 40a and the second external electrode 40b are provided so as to contact two side surfaces facing each other (hereinafter referred to as two end surfaces).

[0037] In the following description, components having the same composition range, thickness range, and particle size distribution range as those of the all-solid-state battery 100 are denoted by the same reference numerals and detailed description thereof will be omitted.

[0038] In the all-solid-state battery 100a, a plurality of first internal electrodes 10 and a plurality of second internal electrodes 20 are alternately stacked with a solid electrolyte layer 30 interposed therebetween. The edges of the plurality of first internal electrodes 10 are exposed to the first end face of the stacked chip 60, but are not exposed to the second end face. The edges of the plurality of second internal electrodes 20 are exposed to the second end face of the stacked chip 60, but are not exposed to the first end face. As a result, the first internal electrodes 10 and the second internal electrodes 20 are alternately conductive to the first external electrode 40a and the second external electrode 40b. The solid electrolyte layer 30 extends from the first external electrode 40a to the second external electrode 40b. In this way, the all-solid-state battery 100a has a structure in which a plurality of battery units are stacked.

[0039] A cover layer 50 is laminated on the upper surface of the laminated structure of the first internal electrode 10, the solid electrolyte layer 30, and the second internal electrode 20 (in the example of FIG. 5, on the upper surface of the first internal electrode 10 of the uppermost layer). In addition, a cover layer 50 is laminated on the lower surface of the laminated structure (in the example of FIG. 5, on the lower surface of the first internal electrode 10 of the lowermost layer). The cover layer 50 is mainly composed of an inorganic material (e.g., Al2O3, ZrO2, TiO2, etc.) containing, for example, Al, Zr, Ti, etc. The cover layer 50 may contain the main component of the solid electrolyte layer 30 as a main component.

[0040] The first internal electrode 10 and the second internal electrode 20 may include a current collector layer. For example, as illustrated in FIG. 6, a first current collector layer 11 may be provided in the first internal electrode 10. Also, a second current collector layer 21 may be provided in the second internal electrode 20. The first current collector layer 11 and the second current collector layer 21 are mainly composed of a conductive material. For example, metal, carbon, etc. can be used as the conductive material of the first current collector layer 11 and the second current collector layer 21. The current collection efficiency is improved by connecting the first current collector layer 11 to the first external electrode 40a and connecting the second current collector layer 21 to the second external electrode 40b.

[0041] Next, a description will be given of a method for manufacturing the all-solid-state battery 100a illustrated in Fig. 5. Fig. 7 is a diagram illustrating a flow of the method for manufacturing the all-solid-state battery 100a.

[0042] (Process for producing raw powder for solid electrolyte layer) First, a raw material powder for the solid electrolyte layer constituting the above-mentioned solid electrolyte layer 30 is prepared. For example, the raw material powder for the solid electrolyte layer can be prepared by mixing raw materials, additives, etc., and using a solid-phase synthesis method, etc. The obtained raw material powder can be adjusted to a desired average particle size by dry pulverizing. For example, the desired average particle size is adjusted using a planetary ball mill using 5 mmφ ZrO2 balls.

[0043] (Cover layer raw powder preparation process) First, the raw material powder of the ceramics constituting the above-mentioned cover layer 50 is prepared. For example, the raw material powder for the cover layer can be prepared by mixing the raw materials, additives, etc., and using a solid-phase synthesis method, etc. The obtained raw material powder can be adjusted to a desired average particle size by dry pulverizing. For example, the desired average particle size is adjusted using a planetary ball mill using 5 mmφ ZrO2 balls.

[0044] (Internal electrode paste manufacturing process) Next, the internal electrode paste for producing the first internal electrode 10 and the second internal electrode 20 is produced. For example, the internal electrode paste can be obtained by uniformly dispersing a conductive assistant, an electrode active material, a solid electrolyte material, a sintering assistant, a binder, a plasticizer, and the like in water or an organic solvent. The above-mentioned solid electrolyte paste may be used as the solid electrolyte material. A carbon material or the like is used as the conductive assistant. A metal may be used as the conductive assistant. Examples of the metal of the conductive assistant include Pd, Ni, Cu, Fe, and alloys containing these. Pd, Ni, Cu, Fe, alloys containing these, and various carbon materials may also be used. When the first internal electrode 10 and the second internal electrode 20 have different compositions, the respective internal electrode pastes may be produced separately.

[0045] The sintering aid in the internal electrode paste contains one or more glass components such as Li-BO based compounds, Li-Si-O based compounds, Li-CO based compounds, Li-SO based compounds, and Li-PO based compounds.

[0046] (External electrode paste manufacturing process) Next, an external electrode paste for producing the above-mentioned first external electrode 40a and second external electrode 40b is prepared. For example, the external electrode paste can be obtained by uniformly dispersing a conductive material, a glass frit, a binder, a plasticizer, etc. in water or an organic solvent.

[0047] (Solid electrolyte green sheet manufacturing process) The raw material powder for the solid electrolyte layer is uniformly dispersed in an aqueous or organic solvent together with a binder, a dispersant, a plasticizer, etc., and wet-pulverized to obtain a solid electrolyte slurry having a desired average particle size. At this time, a bead mill, a wet jet mill, various kneaders, a high-pressure homogenizer, etc. can be used, and it is preferable to use a bead mill from the viewpoint of simultaneously adjusting the particle size distribution and dispersing. A binder is added to the obtained solid electrolyte slurry to obtain a solid electrolyte paste. The obtained solid electrolyte paste is coated to produce a solid electrolyte green sheet 51. The coating method is not particularly limited, and a slot die method, a reverse coat method, a gravure coat method, a bar coat method, a doctor blade method, etc. can be used. The particle size distribution after wet-pulverization can be measured, for example, using a laser diffraction measurement device using a laser diffraction scattering method.

[0048] (Lamination process) As illustrated in FIG. 8(a), the internal electrode paste 52 is printed on one side of the solid electrolyte green sheet 51. The thickness of the internal electrode paste 52 is equal to or greater than the thickness of the solid electrolyte green sheet 51. In the area on the solid electrolyte green sheet 51 where the internal electrode paste 52 is not printed, a reverse pattern 53 is printed. The reverse pattern 53 may be the same as the solid electrolyte green sheet 51. A plurality of printed solid electrolyte green sheets 51 are stacked with alternating shifts. As illustrated in FIG. 8(b), a laminate is obtained by pressing the cover sheets 54 from above and below in the stacking direction. In this case, a laminate having a substantially rectangular parallelepiped shape is obtained so that the internal electrode paste 52 is exposed alternately on two end faces of the laminate. The cover sheet 54 can be formed by applying a raw material powder for the cover layer in the same manner as in the solid electrolyte green sheet preparation process. The cover sheet 54 is formed to be thicker than the solid electrolyte green sheet 51. The cover sheet 54 may be made thicker during coating, or may be made thicker by stacking a plurality of coated sheets.

[0049] Next, the external electrode paste 55 is applied to each of the two end faces by a dipping method or the like, and then dried. This provides a molded body for forming the all-solid-state battery 100a.

[0050] (Firing process) Next, the obtained laminate is fired. The firing conditions are not particularly limited, and may be in an oxidizing or non-oxidizing atmosphere, and the maximum temperature is preferably 400°C to 1000°C, more preferably 500°C to 900°C, etc. In order to sufficiently remove the binder before the maximum temperature is reached, a step of maintaining the temperature in an oxidizing atmosphere at a temperature lower than the maximum temperature may be provided. In order to reduce process costs, it is desirable to fire at as low a temperature as possible. After firing, a reoxidation treatment may be performed. Through the above steps, an all-solid-state battery 100a is produced.

[0051] In addition, a collector layer can be formed in the first internal electrode 10 and the second internal electrode 20 by sequentially stacking an internal electrode paste, a collector paste containing a conductive material, and an internal electrode paste. EXAMPLES

[0052] An all-solid-state battery was fabricated according to the embodiment below, and its characteristics were examined.

[0053] Example 1 The negative electrode active materials were TiO2 and LiTi2(PO4)3, and acetylene black and solid electrolyte LAGP (Li-Al-Ge-PO4 system) were added as conductive additives. They were crushed and mixed in a weight ratio of 50:5:10:35, and kneaded with binder, dispersant, and organic solvent to prepare a negative electrode paste. The negative electrode paste was applied to a sintered pellet of LAGP with a diameter of 15 mm, which was prepared separately, to form a negative electrode layer, and the electrode layer was baked at 600°C in an inert atmosphere. Then, an Au collector was formed on the negative electrode coating surface by sputtering.

[0054] The positive electrode paste was prepared by adding LiCoPO4 as the positive electrode active material, acetylene black as the conductive additive, and the solid electrolyte LAGP in a weight ratio of 55:10:35, respectively, and kneading with a binder, a dispersant, and an organic solvent. The positive electrode paste was applied to a separately prepared Φ15mm LAGP sintered pellet to form a positive electrode layer, and the electrode layer was baked at 600°C in an inert atmosphere. Then, an Au collector was formed on the negative electrode coating surface by sputtering. At this time, the amount of the positive electrode layer applied was adjusted so that the theoretical capacity calculated from the amount of the positive electrode active material was 1.3 times the theoretical capacity calculated from the total amount of the negative electrode active material.

[0055] Then, in an argon atmosphere glove box, the positive and negative electrode layers were placed between a polymer electrolyte film consisting of polyethylene oxide and LiTFSI (lithium bis(trifluoromethane)sulfonimide), and the resulting material was sealed in a 2032-type coin cell to fabricate an all-solid-state battery.

[0056] Example 2 An all-solid-state battery was fabricated in the same manner as in Example 1 using two types of negative electrode active materials, LiTiOPO4 and LiTi2(PO4)3.

[0057] Example 3 The negative electrode active material is TiO2 and Li 1.3 Al 0.3 Ti 1.7 (PO4)3 and an all-solid-state battery was fabricated in the same manner as in Example 1.

[0058] Example 4 The negative electrode active material is LiTiOPO4 and Li 1.3 Al 0.3 Ti 1.7 (PO4)3 and an all-solid-state battery was fabricated in the same manner as in Example 1.

[0059] Example 5 The negative electrode active material is Li 0.33 La 0.55 Two types of materials, TiO3 and LiTi2(PO4)3, were used, and an all-solid-state battery was fabricated in the same manner as in Example 1.

[0060] Example 6 The negative electrode active material is Li 0.33 La 0.55 TiO3 and Li 1.3 Al 0.3 Ti 1.7 (PO4)3 and an all-solid-state battery was fabricated in the same manner as in Example 1.

[0061] Comparative Example 1 An all-solid-state battery was fabricated in the same manner as in Example 1, except that the negative electrode active material was TiO2 alone, and acetylene black and LAGP were further added in a weight ratio of 50:10:35, respectively.

[0062] Comparative Example 2 An all-solid-state battery was produced in the same manner as in Comparative Example 1, except that the negative electrode active material was LiTiOPO4.

[0063] Comparative Example 3 The negative electrode active material is Li 0.33 La 0.55 An all-solid-state battery was fabricated in the same manner as in Comparative Example 1, except that TiO3 was used.

[0064] (analysis) Constant current charge / discharge measurements were carried out on the all-solid-state batteries of Examples 1 to 6 and Comparative Examples 1 to 3 in a thermostatic chamber at 80° C. in the range of 1.0 V to 3.7 V. The results are shown in Table 1. In Example 1, a two-stage potential plateau was observed during both charging and discharging. During discharging, a potential of 2.4 V vs Li / Li was observed at the end of discharging. + A potential plateau was observed near the end of the charge / discharge cycle at about 1 / 10 of the total capacity, and it was determined that this was suitable for end point detection. In Example 2, a two-stage potential plateau was observed in both charge and discharge, similar to Example 1, and a potential plateau of 2.4 V vs Li / Li was observed at the end of discharge. + A potential plateau was observed near the end of the charge / discharge cycle at about 1 / 10 of the total capacity, and it was determined that this was suitable for end point detection. In Example 3, a two-stage potential plateau was observed in both charge and discharge, similar to Example 1, and a potential plateau of 2.4 V vs Li / Li was observed at the end of discharge. +A potential plateau was observed at about 1 / 10 of the total capacity around the 2.4V vs Li / Li charge / discharge end point, which was deemed suitable for end point detection. + A potential plateau was observed near the end of the charge / discharge cycle at about 1 / 10 of the total capacity, and it was determined that this was suitable for end point detection. In Example 5, a two-stage potential plateau was observed in both charge and discharge, similar to Example 1, and a potential plateau of 2.4 V vs Li / Li was observed at the end of discharge. + A potential plateau was observed near the end of the charge / discharge cycle at about 1 / 10 of the total capacity, and it was determined that this was suitable for end point detection. In Example 6, a two-stage potential plateau was observed in both charge and discharge, similar to Example 1, and a potential plateau of 2.4 V vs Li / Li was observed at the end of discharge. + A potential plateau was observed near this point with a capacity of about 1 / 10 of the total capacity, which was deemed suitable for end point detection. These results show that the two-stage potential plateau appears clearly when the negative electrode contains two types of negative electrode active material with different average operating potentials.

[0065] In contrast, in Comparative Example 1, a single potential plateau was observed near 3.0 V in both charging and discharging, but the voltage drop at the end of discharging was so steep that it was determined that it would be difficult to detect the end point. In Comparative Example 2, a single potential plateau was observed near 3.3 V in both charging and discharging, but the voltage drop at the end of discharging was so steep that it was determined that it would be difficult to detect the end point. In Comparative Example 3, a single potential plateau was observed near 3.1 V in both charging and discharging, but the voltage drop at the end of discharging was so steep that it was determined that it would be difficult to detect the end point. [Table 1]

[0066] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]

[0067] 10 1st internal electrode 11 First current collector layer 20 Second internal electrode 21 Second collector layer 30 Solid electrolyte layer 40a First external electrode 40b 2nd external electrode 50 Cover Layer 51 Solid electrolyte green sheet 52 Internal electrode paste 53 Reverse pattern 54 Cover Sheet 55 External electrode paste 60 Stacked Chips 100,100a solid state battery

Claims

1. An oxide-based solid electrolyte layer; a positive electrode layer provided on a first main surface of the oxide-based solid electrolyte layer and including a positive electrode active material; A second main surface of the oxide-based solid electrolyte layer is provided with an average operating potential (vs Li / Li + a negative electrode layer including a first negative electrode active material and a second negative electrode active material, the first negative electrode active material and the second negative electrode active material being different from each other; The average operating potential (vs Li / Li) of the first negative electrode active material + ) is 1.9V or less, The average operating potential (vs Li / Li) of the second negative electrode active material + ) is 2.2 V or more.

2. The first negative electrode active material is TiO 2 , Li 1-2x M x TiOPO 4 (M is a divalent metal element, 0≦x≦0.5), Li 3x La 2/3-x TiO 3 , Nb 2 O 5 2. The all-solid-state battery according to claim 1, wherein the compound is any one of a Nb—Ti—O-based compound and a Nb—Ti—O-based compound.

3. The second negative electrode active material is a Ti-containing phosphate having a NASICON crystal structure or TiP 2 O 7 The all-solid-state battery according to claim 1 or 2,

4. The Ti-containing phosphate is Li 1+y A y Ti 2-y (P.O. 4 ) 3 4. The all-solid-state battery according to claim 3, wherein A is a trivalent metal element and 0≦y≦0.

7.

5. The all-solid-state battery according to claim 4 , wherein the average crystal grain size of the second negative electrode active material is 0.5 μm or more and 50 μm or less.

6. An oxide-based solid electrolyte layer; a positive electrode layer provided on a first main surface of the oxide-based solid electrolyte layer and including a positive electrode active material; A second main surface of the oxide-based solid electrolyte layer is provided with an average operating potential (vs Li / Li + a negative electrode layer including a first negative electrode active material and a second negative electrode active material, the first negative electrode active material and the second negative electrode active material being different from each other; the first negative electrode active material is any one of TiO 2 , Li 1-2x M x TiOPO 4 (M is a divalent metal element, 0≦x≦0.5), Li 3x La 2 / 3-x TiO 3 , Nb 2 O 5 , and Nb—Ti—O based compounds; The second negative electrode active material is a Ti-containing phosphate having a NASICON crystal structure or TiP 2 O 7 An all-solid-state battery comprising:

Citation Information

Patent Citations

  • Lithium battery cathode and preparation method thereof as well as lithium battery

    CN103824999A

  • Lithium-ion secondary battery

    JP2008282619A

  • Nonaqueous electrolyte battery and battery pack

    JP2012182077A

  • Composite, method of manufacturing the same, negative electrode active material including the same, negative electrode including the same, and lithium secondary battery employing the same

    JP2013105744A

  • Lithium ion secondary battery, negative electrode and battery system using these

    JP2016081691A