Fuel cell separator member and method for manufacturing fuel cell separator member
The fuel cell separator member with a prepreg and resin layer structure, featuring flaky graphite and voids, addresses high resistivity issues, enhancing conductivity and reducing gas leakage.
Patent Information
- Application Number
- JP2021022717
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-16
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2041-02-16
AI Technical Summary
Existing fuel cell separators have high penetration resistivity and volume resistivity, which hinder their conductivity and overall efficiency.
A fuel cell separator member composed of a prepreg layer impregnated with a thermosetting resin containing carbon-based powder and resin layers made of thermosetting resin with graphite, where the resin layer has lower volume resistivity than the prepreg layer, and the graphite is flaky-shaped with voids to enhance conductivity.
The configuration results in a fuel cell separator with significantly reduced penetration and volume resistivity, improving conductivity and maintaining structural integrity while ensuring low gas leakage.
Smart Images

Figure 0007594932000002 
Figure 0007594932000003 
Figure 0007594932000004
Abstract
Description
[Technical Field]
[0001] The present invention relates to a fuel cell separator member, a method for manufacturing a fuel cell separator member, and a fuel cell separator. [Background technology]
[0002] One method for increasing the power generation efficiency of a fuel cell is to improve the conductivity of the fuel cell separator. For example, Patent Document 1 discloses a fuel cell separator using a thermoplastic resin sheet containing conductive powder particles. Patent Document 2 discloses a fuel cell separator using an organic sheet coated with a mixture of carbonaceous powder and resin.
[0003] The conductivity of the fuel cell separator is evaluated using the through resistivity (resistivity in the thickness direction) and the volume resistivity (resistivity per unit volume). The lower the through resistivity and volume resistivity, the better. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Laid-Open No. 2006-332035 [Patent Document 2] Japanese Patent Application Laid-Open No. 2006-172776 Summary of the Invention [Problem to be solved by the invention]
[0005] However, although these fuel cell separators are electrically conductive, they still have the problem of high through-hole resistivity (resistivity in the thickness direction) and volume resistivity (resistivity per unit volume).
[0006] The present invention has been made in consideration of the above circumstances, and aims to provide a fuel cell separator having low through-hole resistivity and volume resistivity, a fuel cell separator member constituting the fuel cell separator, and a method for manufacturing a fuel cell separator member. [Means for solving the problem]
[0007] In order to achieve the above object, [1] the fuel cell separator member according to the present invention comprises a prepreg layer in which a substrate is impregnated with a thermosetting resin composition containing carbon-based powder, and resin layers made of a thermosetting resin composition containing graphite laminated on both sides of the prepreg layer, wherein the volume resistivity of the resin layer is lower than that of the prepreg layer.
[0008] [2] The substrate may also be made of a woven fabric.
[0009] [3] The graphite may have a flaky shape.
[0010] [4] The resin layer may also contain voids.
[0011] [5] The thermosetting resin composition constituting the prepreg layer may contain an epoxy resin and 1 to 100 parts by mass of the carbon-based powder per 100 parts by mass (solid content equivalent) of the epoxy resin.
[0012] [6] The thermosetting resin composition constituting the resin layer may contain an epoxy resin and 100 to 2000 parts by mass of the graphite per 100 parts by mass (solid content equivalent) of the epoxy resin.
[0013] In order to achieve the above object, [7] the method for manufacturing a fuel cell separator member according to the present invention comprises the steps of: impregnating a substrate with a thermosetting resin composition containing carbon-based powder to form a prepreg layer; forming the thermosetting resin composition containing flake-like graphite into a sheet to form a resin layer; and laminating the resin layers on both sides of the prepreg layer and integrating the prepreg layer and the resin layer by applying pressure.
[0014] In order to achieve the above object, [8] the fuel cell separator of the present invention comprises a substrate and a matrix layer containing flake graphite and a resin, the substrate is embedded in the matrix layer, the main surface of the graphite is parallel to or inclined with respect to the main surface of the matrix layer in the surface region of the matrix layer, and the inclination of the main surface of the graphite with respect to the main surface of the matrix layer in the region near the substrate is greater than the inclination of the main surface of the graphite present in the surface region of the matrix layer.
[0015] [9] The density of the graphite in the surface region of the matrix layer is higher than the density of the graphite in the region adjacent to the substrate.
[0016]
[10] Preferably, the resin is made of a thermosetting resin composition.
[0017]
[11] The substrate may also be made of a woven fabric. [Effects of the Invention]
[0018] According to the present invention, it is possible to provide a fuel cell separator having low through-hole resistivity and volume resistivity, a fuel cell separator member constituting the fuel cell separator, and a method for manufacturing a fuel cell separator member. [Brief explanation of the drawings]
[0019] [Figure 1] 1 is a schematic cross-sectional view showing the structure of a fuel cell separator member according to an embodiment. [Figure 2]1 is an overall configuration diagram showing a process for manufacturing a prepreg layer of a fuel cell separator member according to an embodiment. FIG. [Figure 3] 1 is an overall configuration diagram showing a process for manufacturing a resin layer of a fuel cell separator member according to an embodiment. [Figure 4] 1A to 1C are schematic cross-sectional views illustrating a method for producing a fuel cell separator member according to an embodiment. [Figure 5] 1 is a schematic plan view showing the configuration of a fuel cell separator according to an embodiment. [Figure 6] FIG. 6 is a schematic cross-sectional view taken along line VV in FIG. 5. [Figure 7] 1 is a schematic cross-sectional view showing a method for integrating fuel cell separators according to an embodiment. DETAILED DESCRIPTION OF THE INVENTION
[0020] A fuel cell separator member, a method for manufacturing a fuel cell separator member, and a fuel cell separator according to a mode for carrying out the present invention (hereinafter simply referred to as "embodiment") will be described in detail below. The embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.
[0021] In the following description, identical or similar components are denoted by the same reference numerals, and redundant description will be omitted. Furthermore, as terms used in the present invention, "B stage" refers to a state in which the curing reaction of the resin composition has not yet progressed completely, and "C stage" refers to a state in which the curing reaction of the resin composition has progressed almost completely.
[0022] The fuel cell separator member, the manufacturing method of the fuel cell separator member, the fuel cell separator, and the manufacturing method of the fuel cell separator will be described in this order.
[0023] (Fuel cell separator member 10) A fuel cell separator member 10 according to an embodiment will now be described. As shown in FIG. 1, the fuel cell separator member 10 has a configuration in which a resin layer 11 is laminated on each side of a prepreg layer 13. The fuel cell separator member 10 is obtained by laminating the resin layer 11 on the prepreg layer 13, and then heating the prepreg layer 13 and the resin layer 11 at a temperature at which the prepreg layer 13 and the resin layer 11 adhere to each other. The cured state of the fuel cell separator member 10 is in the B stage. The fuel cell separator member 10 having such a configuration can be used as a component of a fuel cell separator 60 that constitutes a fuel cell (a component before being processed into a fuel cell separator).
[0024] The prepreg layer 13 and the resin layer 11 will be described.
[0025] (Prepreg layer 13) The prepreg layer 13 is formed by impregnating a base material with a thermosetting resin composition containing carbon-based powder. The cured state of the prepreg layer 13 is in the B stage.
[0026] The thickness of the prepreg layer 13 depends on the thickness of the fuel cell separator itself, but is preferably 40 to 200 μm, and from the viewpoint of electrical conductivity, more preferably 50 to 150 μm.
[0027] From the viewpoint of ensuring the conductivity of the fuel cell separator, the volume resistivity of the prepreg layer 13 is preferably 500 mΩ·cm or less, and more preferably 400 mΩ·cm or less. Here, the cured state of the prepreg layer 13 used in measuring the volume resistivity is C-stage.
[0028] The substrate preferably has openings from the viewpoint of heating the fuel cell separator member 10 composed of the resin layer 11 and the prepreg layer 13 and flowing the resin components of the molten resin layer 11 and the prepreg layer 13. An example of a substrate having openings is a woven fabric.
[0029] The woven fabric is a fabric made by weaving warp threads and weft threads. The weave is not particularly limited, but examples thereof include plain weave, twill weave, and satin weave.
[0030] The woven fabric has gaps between the warp and weft yarns, i.e., openings, which are formed when the weft yarns are woven into the warp yarns. The size of the openings is preferably 0.01 to 0.20 mm, from the viewpoint of reducing the penetration resistance of the fuel cell separator 60 after molding the fuel cell separator member 10. 2 Furthermore, the presence of these openings improves the fluidity of the resin when the resin component of the fuel cell separator member 10 is melted during the process of producing the fuel cell separator 60 (particularly the process of heating and pressurizing), which will be described later.
[0031] The intersections of the warp and weft threads (intersections of the warp and weft threads) are preferably fused, welded, or glued together to facilitate the formation of conductive paths due to the carbon powder. An example of a woven fabric in which the intersections of the warp and weft threads are fused together is polyester mesh.
[0032] The material of the substrate is not particularly limited, but examples thereof include resin-based materials, glass-based materials, and carbon-based materials.
[0033] Examples of resin-based materials include thermosetting resins such as polyimide, and thermoplastic resins such as polyamide, polyamideimide, polyphenylene sulfide, polyethersulfone, polyethylene, polypropylene, polyethylene terephthalate, and polyethylene naphthalate.
[0034] Examples of glass-based materials include T-glass, E-glass, C-glass, S-glass, and D-glass. From the viewpoint of availability, E-glass is preferred.
[0035] Examples of carbon-based materials include PAN (polyacrylonitrile)-based carbon and pitch-based carbon.
[0036] The thickness of the substrate is preferably 40 to 200 μm from the viewpoint of obtaining a prepreg layer 13 that is thin and lightweight and has high strength.
[0037] From the viewpoint of improving the adhesion between the substrate and the thermosetting resin composition, the surface of the substrate is preferably subjected to a silane coupling treatment, a plasma treatment, or a surface roughening treatment.
[0038] The thermosetting resin composition constituting the prepreg layer 13 is not particularly limited, but is preferably an epoxy-based resin composition containing an epoxy resin as a main component.
[0039] The epoxy resin is not particularly limited, but at least one selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, novolac epoxy resin, amine epoxy resin, biphenyl epoxy resin, and alicyclic epoxy resin can be used. From the viewpoints of processability and heat resistance, novolac epoxy resin is preferred.
[0040] The material constituting the carbon-based powder is not particularly limited, but examples thereof include carbon black, graphite, carbon chop, etc. From the viewpoints of conductivity and processability, carbon black is preferred. Two or more types of carbon-based powders can be used in combination.
[0041] The carbon black is not particularly limited, but examples thereof include furnace black, channel black, thermal black, and acetylene black. Two or more types of carbon black may be mixed. From the viewpoint of improving conductivity, acetylene black is preferred.
[0042] The amount of the carbon-based powder is 1 to 100 parts by mass relative to 100 parts by mass of the epoxy resin (solid content equivalent), and from the viewpoint of processability, it is more preferably 5 to 50 parts by mass.
[0043] (Resin layer 11) The resin layer 11 is made of a thermosetting resin composition containing graphite, and is in a B-stage cured state.
[0044] The thickness of the resin layer 11 depends on the thickness of the fuel cell separator itself, but is preferably 50 to 400 μm, and from the viewpoint of maintaining lightness and strength, is 100 to 300 μm.
[0045] From the viewpoint of ensuring the conductivity of the fuel cell separator, the volume resistivity of the resin layer 11 is preferably 20 mΩ·cm or less, and more preferably 15 mΩ·cm or less. Here, the cured state of the resin layer 11 used in measuring the volume resistivity is C-stage.
[0046] The thermosetting resin composition constituting the resin layer 11 is not particularly limited, and examples thereof include an epoxy resin composition mainly composed of an epoxy resin, a phenolic resin composition mainly composed of a phenolic resin, a polyimide resin composition mainly composed of a thermosetting polyimide resin, a melamine resin composition mainly composed of a melamine resin, a urethane resin composition mainly composed of a urethane resin, a diallyl phthalate resin composition mainly composed of a diallyl phthalate resin, an unsaturated polyester resin composition mainly composed of an unsaturated polyester resin, and a cyanate ester resin composition mainly composed of a cyanate ester resin. From the viewpoints of heat resistance, durability, and processability, an epoxy resin composition is preferred.
[0047] The epoxy resin used as the main component in the epoxy resin composition is not particularly limited, but at least one selected from the group consisting of bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, novolac epoxy resins, amine epoxy resins, biphenyl epoxy resins, and alicyclic epoxy resins can be used. From the viewpoints of processability and heat resistance, novolac epoxy resins are preferred.
[0048] Examples of graphite include artificial graphite and natural graphite. From the viewpoint of cost, natural graphite is preferred. Among natural graphite, from the viewpoint of conductivity, expanded graphite, flake graphite, or exfoliated graphite is preferred. Two or more types can be used in combination.
[0049] The graphite preferably has a flaky shape having a main surface, from the viewpoint of improving the electrical conductivity of the fuel cell separator, i.e., from the viewpoint of reducing the through-hole resistivity and volume resistivity. Examples of the flaky shape having a main surface include a leaf shape and a scale shape.
[0050] The size of the graphite is 1 to 100 μm from the viewpoint of exhibiting the electrical conductivity of the resin layer 11 and maintaining the shape and strength of the resin layer 11 when processed into a sheet. The size of the graphite refers to the longest distance between two ends on the main surface of the graphite.
[0051] The amount of graphite is 100 to 2000 parts by mass per 100 parts by mass of epoxy resin (solid content equivalent) from the viewpoints of electrical conductivity and processability, and more preferably 150 to 400 parts by mass from the viewpoints of gas leakage prevention and electrical conductivity of the fuel cell separator.
[0052] The resin layer 11 contains voids. The voids exist between the graphite particles contained in the thermosetting resin composition that constitutes the resin layer 11. The presence of these voids promotes the flow of the resin. That is, when the resin layer 11 is heated, the resin of the thermosetting resin composition that constitutes the resin layer 11 melts, and the molten resin enters the voids, promoting the flow of the resin. As a result, the graphite is also arranged in a manner that reduces the through resistance and volume resistivity of the fuel cell separator.
[0053] The volume resistivity of the resin layer 11 is lower than the volume resistivity of the prepreg layer 13. As a result, when the fuel cell separator member 10 is processed into a fuel cell separator 60, the through-hole resistivity and volume resistivity of the fuel cell separator 60 are reduced. The cured state of the resin layer 11 and the prepreg layer 13 used in measuring the volume resistivity is C-stage.
[0054] Another layer may be laminated between the resin layer 11 and the prepreg layer 13, and may be a single layer or multiple layers. For example, when the other layer is a single layer, the other layer is composed of, for example, a thermoplastic resin composition or the above-mentioned thermosetting resin composition. The presence of the other layer improves the gas barrier properties of the fuel cell separator.
[0055] When the other layer is composed of a thermoplastic resin composition, examples of the thermoplastic resin composition include an acrylic resin composition mainly composed of an acrylic resin, a polyimide resin composition mainly composed of a thermoplastic polyimide resin, a polyamide resin composition mainly composed of a polyamide resin, a polyethersulfone resin composition mainly composed of a polyethersulfone resin, a phenoxy resin composition mainly composed of a phenoxy resin, a polypropylene resin composition mainly composed of a polypropylene resin, a polycarbonate resin composition mainly composed of a polycarbonate resin, a polyethylene resin composition mainly composed of a polyethylene resin, a polyester resin composition mainly composed of a polyester resin, an acrylonitrile butadiene styrene resin composition mainly composed of an acrylonitrile butadiene styrene (ABS) resin, a polystyrene resin composition mainly composed of a polystyrene (PS) resin, a polyphenylene sulfide resin composition mainly composed of a polyphenylene sulfide (PPS) resin composition, and a polyamideimide resin composition mainly composed of a polyamideimide (PAI) resin.
[0056] From the viewpoints of heat resistance, durability, adhesion, and processability, polyethersulfone-based resin compositions and polypropylene-based resin compositions are preferred, and from the viewpoint of gas barrier properties, polyethersulfone-based resin compositions are preferred. Two or more types of resin compositions may be mixed and used.
[0057] Next, a method for manufacturing the fuel cell separator member 10 according to the embodiment will be described.
[0058] (Method for manufacturing fuel cell separator member 10) The manufacturing method of the fuel cell separator member 10 of the embodiment includes the steps of: impregnating a substrate with a thermosetting resin composition containing carbon-based powder to form a prepreg layer 13; forming the thermosetting resin composition containing flake-like graphite into a sheet to form a resin layer 11; and laminating resin layers 11 on both sides of the prepreg layer 13 and integrating the prepreg layer 13 and the resin layer 11 by applying pressure.
[0059] First, a method for producing the prepreg layer 13 by impregnating a substrate with a thermosetting resin composition containing carbon-based powder will be described.
[0060] (Method of manufacturing prepreg layer 13) 2 shows an apparatus for producing the prepreg layer 13. In FIG. 2, upstream and downstream refer to the upstream and downstream in the conveying direction, and top and bottom refer to the top and bottom directions in the production line 20 for the prepreg layer 13.
[0061] The substrate 90 before processing is wound around the outer periphery of the delivery roll 110. The delivery roll 110 supplies the substrate 90 downstream. The substrate 90 is transported via guide rolls 101 and 102 to a resin impregnation section 120 filled with resin 121 made of a thermosetting resin composition containing carbon-based powder. The substrate 90 is impregnated with the resin 121 in the resin impregnation section 120, and then transported via guide roll 103 to a resin drying section 130 where the resin 121 is dried.
[0062] After passing through the resin drying section 130, the upper and lower surfaces of the substrate 90 are covered with the separation films 160 and 150 supplied from the separation film supply section 106 and the separation film supply section 107. The substrate 90 is pressed by the laminating rolls 104 and 105 with the upper and lower surfaces covered with the separation films 160 and 150.
[0063] The pressed substrate 90 is taken up by a take-up roll 140. The taken-up substrate 90 is a prepreg layer 13 in which the substrate 90 is impregnated with a thermosetting resin composition containing carbon-based powder.
[0064] The substrate 90 after passing through the resin drying section 130 corresponds to the prepreg layer 13 in FIG.
[0065] The delivery roll 110 is disposed at the most upstream side of the transport path. The delivery roll 110 is rotatably supported. This allows the delivery roll 110 to deliver the substrate 90. The delivery roll 110 can be rotated by a drive mechanism such as a motor. The delivery roll 110 may be configured as a mechanism that can follow the rotation of the take-up roll 140.
[0066] The resin impregnation section 120 is disposed downstream of the delivery roll 110. A container of the resin impregnation section 120 is filled with resin 121 made of a thermosetting resin composition containing carbon-based powder, the viscosity of which is adjusted to a level suitable for application.
[0067] An impregnation roll 122 is installed in the resin impregnation section 120. The impregnation roll 122 is installed so that at least a portion of the impregnation roll 122 is immersed in the resin 121. The substrate 90 transported by the guide roll 102 passes through the resin 121 along the outer periphery of the impregnation roll 122.
[0068] At this time, the base material 90 is impregnated with the resin 121. The amount of the resin 121 to be impregnated is adjusted by the viscosity of the resin 121 and the speed at which the base material 90 is conveyed. This makes it possible to adjust the thickness of the prepreg layer 13, i.e., the amount of the resin 121 to be impregnated into the base material 90.
[0069] The resin drying section 130 is disposed downstream of the resin impregnation section 120. The resin drying section 130 dries the resin 121 impregnated into the substrate 90 by blowing air. Drying may be performed by blowing air while heating. Drying conditions are adjusted appropriately depending on the amount of resin 121 impregnated into the substrate 90, the cured state of the resin 121 after passing through the resin drying section 130, the length of the resin drying section 130, and the conveying speed.
[0070] After passing through the resin drying section 130, the cured state of the resin 121 impregnated into the substrate 90 is in the B stage.
[0071] The separation film supply unit 106 , the separation film supply unit 107 , the laminating roll 104 , and the laminating roll 105 are disposed between the resin drying unit 130 and the winding roll 140 .
[0072] The separation film supply unit 106 supplies the separation film 160 to the upper surface of the base material 90. The separation film supply unit 107 supplies the separation film 150 to the lower surface of the base material 90.
[0073] The laminating rolls 104 and 105 bond the separate films 150 and 160 supplied to the upper and lower surfaces of the substrate 90 while applying pressure.
[0074] A heating device may be attached to the laminating rolls 104 and 105, and the separating film 150 and the separating film 160 may be bonded to the laminating rolls 104 and 105 in a heated state.
[0075] It is preferable that at least the surfaces of the separate films 150 and 160 that come into contact with the substrate 90 are subjected to a release treatment.
[0076] The separate film 150 and the separate film 160 may be subjected to different release treatments to have different peel strengths. By utilizing this difference in peel strength, the separate film attached to the base material 90 can be easily peeled off. Also, the separate film can be peeled off only from one side of the base material 90.
[0077] Although it depends on the surface condition of the resin 121 after drying, if the surface of the substrate 90 that has passed through the resin drying section 130 is not sticky (tacky), it is not necessary to use a separate film. This allows the production line 20 to be simplified.
[0078] The take-up roll 140 is installed at the most downstream side of the transport path. The take-up roll 140 is supported in a rotatable state. The take-up roll 140 takes up the laminate 170, which is made up of the separation film 160, the base material 90 (prepreg layer 13), and the separation film 150 laminated in this order from the top.
[0079] Next, a method for producing the resin layer 11 by forming a thermosetting resin composition containing flaky graphite into a sheet will be described.
[0080] (Method of manufacturing resin layer 11) 3 shows an apparatus for producing the resin layer 11. In FIG. 3, upstream and downstream refer to the upstream and downstream in the conveying direction, and top and bottom refer to the top and bottom directions in the production line 30 for the resin layer 11.
[0081] The delivery roll 111 has a separation film 151 wound around its outer periphery. The delivery roll 111 supplies the separation film 151. The separation film 151 passes under a resin coating unit 210 that coats a resin 220 for a resin layer, which is made of a thermosetting resin composition containing graphite. In the resin coating unit 210, the resin 220 for a resin layer is coated on the upper surface of the separation film 151, and the separation film 151 is transported to a resin drying unit 131 that dries the resin 220 for a resin layer.
[0082] The separation film 151 that has passed through the resin drying section 131 is taken up by the take-up roll 141. The taken-up separation film 151 has a sheet-shaped resin 220 for a resin layer formed on the upper surface of the separation film 151.
[0083] The delivery roll 111 is disposed at the most upstream side of the transport path. The delivery roll 111 is rotatably supported. This allows the delivery roll 111 to deliver the separation film 151. The delivery roll 111 can be rotated by a drive mechanism such as a motor. It may also be configured as a mechanism that can follow the rotation of the take-up roll 141. The surface (upper surface) of the separation film 151 delivered from the delivery roll 111, on which the resin 220 for the resin layer is applied, is subjected to a release treatment.
[0084] The resin coating unit 210 is disposed downstream of the delivery roll 111. The resin coating unit 210 coats the upper surface of the release-treated separation film 151 with a resin 220 for the resin layer. The resin coating unit 210 is not particularly limited, but examples thereof include known coaters. Examples include a die coater, a comma coater, and a gravure coater. The amount of the resin 220 for the resin layer supplied from the resin coating unit 210 is adjusted according to the viscosity, conveyance speed, etc. of the resin 220 for the resin layer so that the thickness of the resin layer 11 after drying is 100 to 300 μm.
[0085] The resin drying unit 131 is disposed downstream of the resin application unit 210. The resin drying unit 131 dries the resin 220 for the resin layer applied to the separation film 151 by blowing air. Drying may be performed by blowing air while heating. Drying conditions are adjusted appropriately depending on the amount of the applied resin 220 for the resin layer, the cured state of the resin 220 for the resin layer after passing through the resin drying unit 131, the length of the resin drying unit 131, and the conveying speed.
[0086] The cured state of the resin 220 for the resin layer that has passed through the resin drying section 131 is in the B stage. After passing through the resin drying section 131, the resin 220 for the resin layer (not shown) that has been formed into a sheet corresponds to the resin layer 11 in FIG.
[0087] The winding roll 141 is installed at the most downstream side of the transport path. The winding roll 141 winds up a laminate (not shown) in which the resin for the resin layer 220 (resin layer 11) formed in a sheet shape and the separation film 151 are laminated in this order from the top.
[0088] If the surface of the resin 220 for the resin layer is sticky (tacky) after drying, the lower surface of the separate film 151 may also be subjected to a release treatment. That is, both surfaces of the separate film 151 may be subjected to a release treatment. This makes it possible to prevent adhesion between the lower surface of the separate film 151 and the resin 220 for the resin layer (resin layer 11) even when the take-up roll 141 is wound up with a laminate in which the resin 220 for the resin layer (resin layer 11) and the separate film 151 are laminated in this order.
[0089] As another method, the separation film supply unit and laminating roll may be installed between the resin drying unit 131 and the winding roll 141. This allows the exposed surface of the resin 220 for the resin layer to be covered with the separation film, so that even when the resin 220 for the resin layer is wound up by the winding roll 141, the resin 220 for the resin layer will not stick to the underside of the separation film 151.
[0090] Next, a method of laminating resin layers 11 on both sides of prepreg layer 13 and then applying pressure to integrate prepreg layer 13 and resin layer 11 will be described.
[0091] (Integration of prepreg layer 13 and resin layer 11) FIG. 4 shows an apparatus for laminating resin layers 11 on both sides of prepreg layer 13 and integrating them.
[0092] First, the prepreg layer 13 (laminate 170) is cut to a predetermined size. The separate film 150 and the separate film 160 are peeled off from the laminate 170 to obtain the prepreg layer 13.
[0093] Next, the sheet-like resin 220 for the resin layer formed on the upper surface of the separate film 151, i.e., the resin layer 11 formed on the upper surface of the separate film 151, is cut to the same size as the prepreg layer 13. After cutting, the separate film 151 is peeled off to obtain the resin layer 11.
[0094] Next, the obtained prepreg layer 13 and resin layer 11 are integrated. Resin layers 11 are laminated on both sides of the prepreg layer 13. After lamination, pressure is applied in the direction of the arrow using a press 300, and heating is performed to integrate the prepreg layer 13 and the resin layer 11 so that they adhere to each other. The integrated laminate is the fuel cell separator member 10. The cured state of the fuel cell separator member 10 is in the B stage.
[0095] At the time of integration, the separate film 151 may be integrated without being peeled off from the resin layer 11 (sheet-shaped resin 220 for resin layer).
[0096] The conditions for heating and pressing can be appropriately selected depending on the thickness of the fuel cell separator member 10, but are typically 20 to 350°C, 0.1 to 50 MPa, and 5 to 300 seconds. The prepreg layer 13 and resin layer 11 of this laminate (fuel cell separator member 10) are in a B-stage cured state.
[0097] In the above-described method for producing the prepreg layer 13 and the resin layer 11, an organic solvent can be added to the resin composition that constitutes the prepreg layer 13 and the resin layer 11. This makes it possible to adjust the viscosity of the resin composition, and to produce the prepreg layer 13 and the resin layer 11.
[0098] Examples of organic solvents that can be used include alcohols such as methanol and ethanol; glycols such as ethylene glycol and propylene glycol; glycol monoalkyl ethers such as ethylene glycol monomethyl ether and ethylene glycol monoethyl ether; glycol dialkyl ethers such as ethylene glycol dimethyl ether and ethylene glycol diethyl ether; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene; aliphatic hydrocarbons such as hexane, cyclohexane, and octane; amides such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; cyclic ethers such as tetrahydrofuran and dioxane, methyl acetate, ethyl acetate, and propyl acetate.
[0099] (Another method for manufacturing the fuel cell separator member 10) The fuel cell separator member 10 can also be produced by other methods.
[0100] First, prepare a resin layer 11 and a resin sheet made of a thermosetting resin composition containing carbon-based powder. The resin sheet made of a thermosetting resin composition containing carbon-based powder is produced in the same manner as the resin layer 11 is produced by forming a thermosetting resin composition containing flaky graphite into a sheet.
[0101] These are laminated on both sides of the substrate 90 in the order closest to the substrate 90, with the substrate 90 before being impregnated with resin at the center, the resin sheet, and the resin layer 11. After lamination, these are heated and pressurized to be integrated, thereby obtaining the fuel cell separator member 10.
[0102] The fuel cell separator member 10 can also be produced by other methods.
[0103] First, prepare a resin layer 11 and a resin sheet made of a thermosetting resin composition containing carbon-based powder. The resin sheet made of a thermosetting resin composition containing carbon-based powder is produced in the same manner as the resin layer 11 is produced by forming a thermosetting resin composition containing flaky graphite into a sheet.
[0104] These are laminated on both sides of the base material 90, with the base material 90 before being impregnated with resin at the center. After lamination, these are heated and pressed to obtain the prepreg layer 13.
[0105] Next, the resin layer 11 and the prepreg layer 13 are laminated in the order of resin layer 11, prepreg layer 13, and resin layer 11. After lamination, the laminate is heated and pressurized. This causes the resin layer 11 and the prepreg layer 13 to adhere to each other, thereby obtaining the fuel cell separator member 10.
[0106] The fuel cell separator member 10 can also be produced by other methods.
[0107] First, prepare a resin layer 11 and a resin sheet made of a thermosetting resin composition containing carbon-based powder. The resin sheet made of a thermosetting resin composition containing carbon-based powder is produced in the same manner as the resin layer 11 is produced by forming a thermosetting resin composition containing flaky graphite into a sheet.
[0108] These are laminated in the following procedure.
[0109] First, a resin sheet is laminated on one side of the base material 90 before it is impregnated with resin. After lamination, the prepreg layer 13 is obtained by heating and pressing.
[0110] Next, resin layers 11 are laminated on both sides of the prepreg layer 13. After lamination, these are heated and pressurized. This causes the resin layer 11 and the prepreg layer 13 to adhere to each other, and a fuel cell separator member 10 is obtained.
[0111] At this time, the thickness of the resin sheet is preferably at least twice the thickness of the base material 90 in order to allow the base material 90 to be uniformly impregnated with the resin.
[0112] Next, a fuel cell separator 60 according to an embodiment will be described. Note that descriptions that overlap with the description of the fuel cell separator member 10 will be omitted.
[0113] (Fuel cell separator 60) The fuel cell separator 60 of the embodiment is obtained by heating and pressurizing a fuel cell separator member 10 (cured in a B-stage) in which resin layers 11 are laminated and bonded to both sides of a prepreg layer 13. This heating and pressurizing melts the resin components constituting the prepreg layer 13 and the resin components constituting the resin layer 11, integrating the prepreg layer 13 and the resin layer 11. The fuel cell separator 60 in which the resin components constituting the prepreg layer 13 and the resin components constituting the resin layer 11 are integrated includes a substrate 90 and a matrix layer 500 containing flake graphite 62 and a resin, and the substrate 90 is embedded in the matrix layer 500. The substrate 90 is the substrate constituting the prepreg layer 13. The matrix layer 500 is a thermosetting resin composition containing carbon-based powder that constitutes the prepreg layer 13, and a thermosetting resin composition containing graphite that constitutes the resin layer 11. In the following description, a woven fabric is used as the substrate 90.
[0114] 5, the substrate 90 indicated by the dashed line is embedded in the matrix layer 500. The surface of the fuel cell separator 60 is formed by the matrix layer 500.
[0115] Fig. 6 is a VV cross-sectional view of the fuel cell separator 60 shown in Fig. 5. As shown in Fig. 6, the fuel cell separator 60 includes a substrate 90 and a matrix layer 500, and the substrate 90 is embedded in the matrix layer 500.
[0116] The fuel cell separator 60 is in a C-stage cured state.
[0117] The fuel cell separator 60 having such a configuration has low through resistance and volume resistivity, and is suitable for use as a fuel cell separator that constitutes a fuel cell.
[0118] The state of the graphite 62 present in the matrix layer 500 will be described.
[0119] As shown enlarged in circle 1 in FIG. 6 , a plurality of flake-shaped graphite particles 62 are present in the vicinity of the substrate 90 embedded in the matrix layer 500. Most of these graphite particles 62 are present with their principal surfaces tilted relative to the principal surface of the matrix layer 500. This tilt is greater than the tilt of the graphite particles 62 present in the surface region of the matrix layer 500. Here, the surface region of the matrix layer 500 refers to a region extending from the principal surface of the matrix layer 500 to a depth approximately equal to 10% of the thickness of the matrix layer 500. The region near the substrate 90 refers to a region extending from the surface of the substrate 90 to a depth approximately equal to 10% of the thickness of the matrix layer 500. The tilt of the graphite particles 62 is the average tilt of the tilts of the plurality of graphite particles 62 observed when a cross section of the matrix layer 500 is observed using a scanning electron microscope.
[0120] The inventors speculate that the reason why the fuel cell separator 60 having such a configuration has a low through-hole resistivity and volume resistivity is as follows.
[0121] As shown enlarged in circle 1 in FIG. 6, the graphite particles 62 with a large inclination are present in large numbers in the region near the substrate 90. Carbon-based powder (not shown) is also present in the matrix layer 500. This carbon-based powder is also present between the multiple graphite particles 62 that are present in large numbers in the region near the substrate 90, making it easier to form conductive circuits. In other words, conductive paths are more easily formed in the thickness direction of the fuel cell separator 60. As a result, the through resistance of the fuel cell separator 60 is lowered.
[0122] As shown enlarged in circle 2 in Figure 6, flake-like graphite 62 is also present in the surface region of the matrix layer 500. The graphite 62 is present in greater amounts in the surface region of the matrix layer 500 than in the region adjacent to the substrate 90, and the density of the graphite 62 is higher. This improves the conductivity of the fuel cell separator 60. Furthermore, in the surface region of the matrix layer 500, the main surfaces of the graphite 62 are present parallel to or inclined relative to the main surfaces of the matrix layer 500. This makes it easier to form conductive paths in the direction of the main surfaces of the matrix layer 500, and reduces the volume resistivity of the fuel cell separator 60.
[0123] Such a structure is formed when the fuel cell separator member 10 is heated and pressurized to melt and flow the resin components constituting the prepreg layer 13 and the resin components constituting the resin layer 11, and the molten resin components move into the voids contained in the resin layer 11 that constitutes the fuel cell separator member 10.
[0124] Furthermore, due to this flow of the resin component, in the surface region of the matrix layer 500, the main surface of the graphite 62 tends to be arranged at an inclination that is parallel or nearly parallel to the main surface of the matrix layer 500. Furthermore, in the region near the substrate 90, particularly near the openings of the substrate 90, the flow of the resin increases, so the main surface of the graphite 62 tends to be arranged at a large inclination to the main surface of the surface of the matrix layer 500. Note that the substrate 90 having openings is embedded in the matrix layer 500, and the matrix layer 500 is also present in the openings. Although the matrix layer 500 is present in the openings, the term "openings" will be used as is for the purpose of explanation.
[0125] The main surface refers to the surface of the fuel cell separator 60 (the surface of the matrix layer 500) that is parallel to the horizontal direction when the fuel cell separator 60 is placed on a horizontal table.
[0126] Next, a method for manufacturing the fuel cell separator 60 will be described.
[0127] (Method for manufacturing fuel cell separator 60) 7, the fuel cell separator 60 is obtained by inserting the fuel cell separator member 10 in a B-stage state between molds 400, and applying pressure in the direction of the arrow using a press 310 and heating it. The hardened state of the fuel cell separator 60 obtained at this time is in a C-stage.
[0128] The surface shape of the fuel cell separator 60 is formed by a mold 400 .
[0129] The heating and pressurizing conditions are appropriately set depending on the thickness of the fuel cell separator member 10. For example, the conditions are 100 to 200°C, 5 to 30 MPa, and 5 to 120 seconds.
[0130] The mold 400 is, for example, a mold having grooves with concave and convex shapes formed therein. These grooves become flow paths for gases and the like in the fuel cell. [Example]
[0131] The present invention will be explained in more detail with reference to the following examples and comparative examples, but the present invention is not limited to these examples.
[0132] In the examples and comparative examples, the following materials were used.
[0133] (1) Base: cresol novolac epoxy resin, epoxy equivalent 211 g / eq (manufactured by Nippon Kayaku Co., Ltd., EOCN-102S-70), (2) Hardener: Novolac phenolic resin, hydroxyl equivalent 105 g / eq (Aica Kogyo Co., Ltd., BRG-556), (3) Reinforcement agent: phenoxy resin (YP-50, manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.), (4) Curing accelerator: 2-undecylimidazole (manufactured by Shikoku Chemical Industry Co., Ltd., C11Z), (5) Conductive filler A: exfoliated graphite, average particle size 5 μm (manufactured by Denka Co., Ltd., Denka Black 100% pressed), (6) Conductive filler B: exfoliated graphite, average particle size 15 μm (manufactured by Denka Co., Ltd., Denka Black 100% pressed), (7) Conductive filler C: spherical graphite, average particle size 35 μm (manufactured by Denka Co., Ltd., Denka Black 100% pressed), (8) Conductive filler D: Acetylene black (manufactured by Denka Co., Ltd., 100% pressed Denka Black).
[0134] In the examples and comparative examples, the following substrates were used. (1) Polyester mesh (manufactured by Nippon Tokushu Orimono Co., Ltd., TNo. 60SS).
[0135] In the examples and comparative examples, sample preparation, measurement methods, and evaluation methods were as follows.
[0136] The manufacturing, measurement and evaluation methods of the prepreg layer, resin layer and fuel cell separator member will be described using Example 1 as an example.
[0137] (1) (Preparation of prepreg layer) (1-1) (Resin composition for prepreg layer) 100.0 parts by mass of the base resin, 48.8 parts by mass of the curing agent, and 17.5 parts by mass of the reinforcing agent were each dissolved in methyl ethyl ketone, and then added to a container and mixed to prepare a mixed solution. Next, a solution of 3.0 parts by mass of the curing accelerator dissolved in methanol and 43.8 parts by mass of conductive filler D were added to the mixed solution. After addition, the mixture was stirred with a homomixer to obtain a solution of the resin composition for the prepreg layer. The stirring conditions were room temperature, 6000 rpm, and 30 minutes. Methyl ethyl ketone was added to adjust the viscosity of the solution to fall within the range of 100 to 3000 mPa·s, and the resin composition for the prepreg layer was obtained.
[0138] (1-2) Preparation of prepreg layer The resin composition for the prepreg layer was applied to the release surface of a 38 μm-thick release-treated film (PET38X, manufactured by Lintec Corporation) using a bar coater so that the thickness after drying would be 20 μm, and then dried. The drying conditions were 70°C and 4 minutes. After cooling, a resin sheet for the prepreg layer having a thickness of 20 μm was obtained.
[0139] Next, the resin surface of the prepreg layer resin sheet was overlapped with a polyester mesh, and the sheets were bonded together using a laminator (TAISEI LAMINATOR CO., LTD., VA-700) under conditions of 80°C, 0.4 m / min, and 0.6 MPa. After cooling, the release-treated film was peeled off to obtain a prepreg layer.
[0140] (2) (Preparation of resin layer) (2-1) Resin composition for resin layer 100.0 parts by weight of the base resin, 48.4 parts by weight of the curing agent, and 35.0 parts by weight of the reinforcing agent were each dissolved in methyl ethyl ketone, and then mixed in a single container to prepare a mixed solution. Next, a solution of 3.0 parts by weight of the curing accelerator dissolved in methanol and 559.0 parts by weight of conductive filler A were added to the mixed solution and stirred at room temperature to obtain a solution of the resin composition for the resin layer. Furthermore, methyl ethyl ketone was added to adjust the viscosity of the solution to fall within the range of 100 to 3000 mPa·s, and a resin composition for the resin layer was obtained.
[0141] (2-2) Preparation of resin sheet for resin layer The resin composition for the resin layer was applied to the release surface of a 38 μm-thick release-treated film (PET38X, manufactured by Lintec Corporation) using a bar coater so that the thickness after drying would be 250 μm, and then dried. The drying conditions were 70° C. and 7 minutes. After cooling, a resin sheet for the resin layer having a thickness of 250 μm was obtained.
[0142] (3) (Fabrication of fuel cell separator members) The resin sheets for the resin layer were laminated on the front and back surfaces of the prepreg layer so that the resin surfaces of the resin sheets for the resin layer faced each other. The prepreg layers were then bonded together under conditions of 80°C, 0.4 m / min, and 0.6 MPa. After cooling, the release-treated film on the resin layer sheet was peeled off to obtain a fuel cell separator member.
[0143] As samples to be used for various measurements, characteristic evaluation samples were prepared to evaluate the characteristics of a fuel cell separator, a prepreg layer alone, and a resin layer alone. (4) (Preparation of samples for characteristic evaluation) Samples for property evaluation were cut out from each of the fuel cell separator member, the prepreg layer alone, and the resin layer alone, measuring 100 mm x 100 mm square. Next, a 38 μm-thick release-treated film (PET3811 manufactured by Lintec Corporation) was laminated on both sides of each cut-out sample, with the release-treated surface facing the film. Each laminated sample was press-molded at 180°C for 5 minutes at 20 MPa to achieve a C-stage cured state. After cooling, samples for property evaluation of the fuel cell separator, the prepreg layer alone, and the resin layer alone were obtained.
[0144] Here, the fuel cell separator characteristic evaluation sample was designated as characteristic evaluation sample 1, the prepreg layer characteristic evaluation sample was designated as characteristic evaluation sample 2, and the resin layer characteristic evaluation sample was designated as characteristic evaluation sample 3.
[0145] <Volume resistivity measurement> The volume resistivity (mΩ cm) of Characteristic Evaluation Sample 1 was measured using a resistivity meter (Hioki EE, RM3545) by the four-probe method in accordance with JIS K7194. The volume resistivities of Characteristic Evaluation Sample 2 and Characteristic Evaluation Sample 3 were also measured in the same manner.
[0146] <Measurement of penetration resistance> A sample for measuring the penetration resistivity was prepared as follows: First, two sheets of the characteristic evaluation sample 1 prepared in (4) were stacked. After stacking, a gas diffusion layer substrate (GDL MFL manufactured by Mitsubishi Chemical Corporation) was laminated on each of the two outer surfaces to obtain a measurement sample.
[0147] The penetration resistivity was measured by contacting gold-plated electrodes to each of the two outer surfaces of the measurement sample (the two surfaces on which the gas diffusion layer was exposed) and passing a current under a pressure of 1 MPa.
[0148] <Bending strength measurement> (1) Preparation of measurement samples The characteristic evaluation sample 1 was cut into a rectangle having a width of 10 mm and a length of 20 mm, which was used as a measurement sample. (2)Measurement method Bending strength was measured using an autograph testing machine (Shimadzu Corporation, AG-10). Measurements were performed using three-point bending (support distance 10 mm, test speed 2 mm / min) to measure the breaking load. Bending strength was calculated from the obtained maximum bending stress (the maximum bending stress that the test piece can withstand) in accordance with JIS K7171.
[0149] <Gas barrier properties> The gas barrier property was evaluated by measuring the water vapor permeability. (1) Preparation of measurement samples The characteristic evaluation sample 1 was cut into a circular shape with a diameter of 76 mm to prepare a measurement sample. (2)Measurement method The water vapor permeability was determined in accordance with JIS Z0208. Specifically, the amount of water vapor that permeates a measurement sample for 24 hours under conditions of 40°C and 90% RH is calculated as 2 Value converted to per unit (g / m 2 24h).
[0150] The evaluation criteria were as follows: Excellent: Water vapor permeability is 13g / m 2 Less than 24 hours. Good: Water vapor permeability is 13g / m 2 ·Over 24 hours, 32g / m 2 Less than 24 hours. Poor: Water vapor permeability is 32g / m 2 - 24 hours or more.
[0151] Examples 2 to 5 were produced in the same manner as in Example 1, except that the types and contents of the components were changed as shown in Table 1. Furthermore, for evaluation, samples for property evaluation were produced in the same manner as in Example 1, and evaluation was carried out.
[0152] The resin layer and fuel cell separator member of Comparative Example 1 will be described.
[0153] (Preparation of Resin Layer and Resin Sheet for Resin Layer) The resin layer was prepared in the same manner as in Example 1.
[0154] (Fabrication of fuel cell separator members) The resin layer resin sheets were laminated on the front and back surfaces of the polyester mesh so that the resin surfaces of the resin layer resin sheets faced each other. Then, they were bonded together under conditions of 80°C, 0.4 m / min, and 0.6 MPa. After cooling, the release-treated film of the resin layer sheet was peeled off to obtain a fuel cell separator member.
[0155] Comparative Examples 2 and 3 were produced in the same manner as Comparative Example 1, except that the types and contents of the components were changed as shown in Table 1.
[0156] (Evaluation of fuel cell separator components and resin layers alone) For the evaluation of Comparative Examples 1 to 3, a sample for evaluating the characteristics of the fuel cell separator (Sample for Evaluation 1) and a sample for evaluating the characteristics of the resin layer alone (Sample for Evaluation 3) were prepared in the same manner as in Example 1 and evaluated.
[0157] [Table 1]
[0158] The results in Table 1 show that the fuel cell separators of Examples 1 to 5 had good through-hole resistivity and volume resistivity. Furthermore, the fuel cell separators of Examples 1 to 5 had good gas barrier properties and bending strength while exhibiting low through-hole resistivity and volume resistivity. Thus, the present invention makes it possible to provide a fuel cell separator that is electrically conductive and has low through-hole resistivity and volume resistivity, a fuel cell separator member that constitutes a fuel cell separator, and a method for manufacturing a fuel cell separator member. [Industrial Applicability]
[0159] The fuel cell separator member, the method for manufacturing a fuel cell separator member, and the fuel cell separator of the present invention have industrial applicability. [Explanation of symbols]
[0160] 10 Fuel cell separator member, 11 resin layer, 13 prepreg layers, 20, 30 production lines, 60 Fuel cell separators, 62 graphite, 90 base material, 101, 102, 103 guide rolls, 104, 105 Laminated roll, 106, 107 Separate film supply unit, 110, 111: Feed rolls; 120 resin impregnated part, 121 resin, 122 impregnation roll, 130, 131 Resin drying section, 140, 141 Winding roll; 150, 151, 160 Separate film, 170 laminates, 210 resin application part, 220 Resin for resin layer, 300, 310 presses, 400 molds, 500 matrix layers.
Claims
1. A prepreg layer in which a substrate having an opening is impregnated with a thermosetting resin composition containing a carbon-based powder; and a resin layer composed of a thermosetting resin composition containing graphite laminated on each of both sides of the prepreg layer, The material of the substrate is polyethylene terephthalate or polyethylene naphthalate, A fuel cell separator member, wherein the resin layer has a volume resistivity lower than a volume resistivity of the prepreg layer.
2. The fuel cell separator member of claim 1 , wherein the substrate is comprised of a woven fabric.
3. 3. The fuel cell separator member according to claim 1, wherein the graphite has a flaky shape.
4. The fuel cell separator member according to claim 1 , wherein the resin layer contains voids.
5. A separator member for a fuel cell described in any one of claims 1 to 4, wherein the carbon-based powder is composed of carbon black.
6. 6. The fuel cell separator member according to claim 1, wherein the thermosetting resin composition constituting the prepreg layer comprises an epoxy resin, and 1 to 100 parts by mass of the carbon-based powder per 100 parts by mass (converted into solid content) of the epoxy resin.
7. 7. The fuel cell separator member according to claim 1, wherein the thermosetting resin composition constituting the resin layer comprises an epoxy resin and 100 to 2000 parts by mass of the graphite per 100 parts by mass of the epoxy resin (converted into solid content).
8. A process for producing a prepreg layer by impregnating a substrate having an opening, the substrate being made of polyethylene terephthalate or polyethylene naphthalate, with a thermosetting resin composition containing carbon-based powder; A step of forming a resin layer by forming a thermosetting resin composition containing flaky graphite into a sheet shape; a step of laminating the resin layers on both sides of the prepreg layer and applying pressure to integrate the prepreg layer and the resin layer; A method for manufacturing a fuel cell separator member comprising the steps of:
Citation Information
Patent Citations
Manufacture of carbon compact for phosphoric acid type fuel battery
JP1993307967A
Separator material for fuel cell, and its manufacturing method
JP2006172776A
Separator for fuel cell, its manufacturing method, and fuel cell using it
JP2006332035A