Lanthanum-based perovskite-type catalyst compositions stable against degradation in three-way catalytic cracking

The combination of perovskite-type compounds with non-redox active components in the catalyst composition addresses the deactivation issue of traditional TWCs, ensuring high temperature stability and maintaining catalytic efficiency for NO, CO, and HC conversion.

JP7595016B2Active Publication Date: 2024-12-05JOHNSON MATTHEY PLC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021550072
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-06
Filing Date
2020-03-27
Publication Date
2024-12-05
Estimated Expiration
2040-03-27

AI Technical Summary

Technical Problem

Existing three-way catalysts (TWCs) for internal combustion engines, typically composed of platinum group metals (PGMs) on alumina and ceria-zirconia supports, face deactivation under severe degrading conditions, necessitating the development of alternative catalyst compositions that are stable at high temperatures.

Method used

A novel catalyst composition comprising a perovskite-type compound, such as La z B 1-q B' q O 3±δ, combined with non-redox active components like alumina or ZrO 2, prepared via methods like flame spray pyrolysis, which maintains catalytic activity even after exposure to high temperatures and degrading conditions.

Benefits of technology

The perovskite-based catalysts exhibit high NO, CO, and HC conversion rates that are retained after aging, with minimal degradation, achieving NO conversion rates above 500-600°C and CO/HC conversion rates above 500°C with less than 20% reduction post-aging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595016000004
    Figure 0007595016000004
  • Figure 0007595016000005
    Figure 0007595016000005
  • Figure 0007595016000001
    Figure 0007595016000001
Patent Text Reader

Abstract

Formula (I): La z B 1-q B' q O 3±δ or formula (II): [BO x ] y :[La z BO 3±δ ] 1-y and a non-redox active component, wherein B or B' is Fe, Mn, Co, Ni, Cu, Ti, or Zr; q is in the range of about 0 to about 0.5; x is in the range of about 1 to about 2.5; y is in the range of about 1 to about 30 wt %; z is in the range of about 0.6 to about 1.1; and δ is in the range of about 0 to about 0.6.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The compositions and methods of the present invention relate to novel catalyst compositions comprising a perovskite-type compound and a non-redox active component, their use as three-way catalysts (TWCs) in the exhaust systems of internal combustion engines, and methods for treating exhaust gases from internal combustion engines. [Background technology]

[0002] In internal combustion engines, hydrocarbons (HC), carbon monoxide (CO), and nitrogen oxides (NO x In gasoline engines, exhaust gases are produced that contain a variety of pollutants, including carbon monoxide (CO), sulphur dioxide (SO2), and toluene (NO3). Emissions control systems, including exhaust gas catalysts, are widely used to reduce the amount of these pollutants emitted into the atmosphere. The catalyst typically used in gasoline engine applications is the TWC. The TWC performs three main functions: (1) the oxidation of carbon monoxide (CO), (2) the oxidation of unburned hydrocarbons, and (3) the oxidation of NO x is reduced to N2. Summary of the Invention [Problem to be solved by the invention]

[0003] TWCs, typically consisting of platinum group metals (PGMs) dispersed on high surface area alumina and ceria-zirconia supports, were first introduced for gasoline engine aftertreatment in the early 1980s. With the need to meet increasingly stringent emission limits, the discovery of alternative catalyst compositions utilizing fewer or no PGMs remains an active research topic. Perovskite-type oxides (ABO3) have long been proposed as TWCs. Although there have been ongoing efforts to understand and improve the catalytic properties of perovskites for automotive applications, such catalysts often exhibit deactivation when exposed to severe aging conditions. Thus, there remains a need to improve new TWC compounds that are stable to high temperature aging.

[0004] According to an embodiment of the present invention, the three-way catalyst composition comprises a catalyst having the formula (I): La zB 1-q B' q O 3±δ Or formula (II): [BO x ] y :[La z BO 3±δ ] 1-y and a non-redox active component, where B and B' are Fe, Mn, Co, Ni, Cu, Ti, or Zr, z is in the range of about 0.6 to about 1.1, q is in the range of about 0 to about 0.5, δ is in the range of about 0 to about 0.6, x is in the range of about 1 to about 2.5, and y is in the range of about 1 to about 30 wt %. In some embodiments, the non-redox active component includes, for example, an oxide, alumina, ZrO2, or a combination thereof. In some embodiments, the ZrO2 is doped.

[0005] In some embodiments, the catalyst may be completely free of platinum group metals or substantially free of platinum group metals.

[0006] In some embodiments, the perovskite compound is present in an amount of about 5 wt% to about 75 wt% of the catalyst composition. In some embodiments, the non-redox active component is present in an amount of about 25 wt% to about 95 wt% of the catalyst composition. In some embodiments, the perovskite compound and the non-redox active component are present in a weight ratio of about 0.5:1 to about 3:1.

[0007] In some embodiments, the perovskite compounds are prepared by flame spray pyrolysis. The perovskite compounds have a high surface area.

[0008] According to some aspects of the present invention, a catalytic article for treating exhaust gases includes a substrate and a three-way catalyst composition described herein.

[0009] According to some embodiments of the present invention, a method for treating exhaust gas from an internal combustion engine includes contacting the exhaust gas with a catalyst article comprising a substrate and a three-way catalyst composition as described herein. In some embodiments, the three-way catalyst composition of the present invention provides (1) a NO conversion at 500-600°C when fresh, and (2) a NO conversion at 500-600°C after aging the catalyst in the presence of water vapor at a temperature of at least 700°C for 20 hours, with a difference (delta) between the fresh NO conversion and the aging NO conversion being less than a 20% decrease. In some embodiments, the difference between the fresh NO conversion and the aging NO conversion being less than a 15% decrease. In some embodiments, the three-way catalyst composition of the present invention provides (1) a HC or CO conversion at 500°C when fresh, and (2) a HC or CO conversion at 500°C after aging the catalyst in the presence of water vapor at a temperature of at least 700°C for 20 hours, with a difference between the fresh HC or CO conversion and the aging HC or CO conversion being less than a 50% decrease. In some embodiments, the difference between the fresh and aged HC or CO conversion is less than a 40% decrease. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 shows TEM images of fresh and aged Comparative Catalyst 4 (1a and 1b) and Catalyst 5A (1c and 1d), respectively. [Diagram 2] Figure 2 shows particle size analysis of the TEM images in Figure 1, where (2a) is MnOx:La0.9MnO3 after aging (Comparative Catalyst 4), (2b) is MnOx:La0.9MnO3 with doped ZrO2 when fresh (Catalyst 5A), and (2c) is MnOx:La0.9MnO3 with doped ZrO2 after aging (Catalyst 5A), where x-axis: particle size, y-axis: particle number. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The compositions and methods of the present invention relate to novel catalyst compositions comprising perovskite-type compounds and non-redox active components. Such compositions can be used as three-way catalysts (TWCs) in exhaust systems for internal combustion engines and as part of a method for treating exhaust gases from internal combustion engines. It has been found that the catalysts of the present invention can provide advantages related to high temperature stability.

[0012] Perovskite Compounds Formula (I): La z B 1-q B' q O 3±δ The catalyst composition of the present invention contains a perovskite-type compound. In some embodiments, the perovskite-type compound has the formula (I): La z B 1-q B' q O 3±δ has. wherein B or B' is Fe, Mn, Co, Ni, Cu, Ti, or Zr, and preferably B or B' is Fe or Mn. In some embodiments, B or B' is Fe. In other embodiments, B or B' is Mn. The character q is in the range of 0 to 0.5, preferably 0 to 0.2, and more preferably 0. z is in the range of about 0.6 to about 1.1, preferably about 0.7 to about 1.0, and more preferably about 0.7 to about 0.9. δ is in the range of about 0 to about 0.6, preferably about 0 to about 0.5, and more preferably about 0.15 to about 0.3.

[0013] Compounds of formula (I) can be prepared by co-precipitation, flame spray pyrolysis (FSP), ball milling, and the like.

[0014] FSP is a combustion method to directly obtain nanocrystalline particles by combusting precursors soluble in organic solvents in a CH4 / O2 flame.

[0015] Co-precipitation is not necessarily a one-step process: unlike other methods, here the precursors in solution are mixed together and slowly precipitated together under controlled pH to form a well-mixed amorphous precipitate, which can then be calcined to obtain crystalline particles of the perovskite phase.

[0016] The perovskite compounds of formula (I) can be prepared by flame spray pyrolysis (FSP). For example, FSP can be a combustion method in which a precursor soluble in an organic solvent is burned in a CH4 / O2 flame to directly obtain nanocrystalline particles. The perovskite compounds of formula (I) can have an average primary crystal size of less than 60 nm. In some embodiments, the compounds of formula (I) have an average primary crystal size of less than 30, 25, 20, 15, 10, or 5 nm. In some embodiments, the compounds of formula (I) have an average primary crystal size of 5 nm to 60 nm, 5 nm to 50 nm, 5 nm to 40 nm, 5 nm to 30 nm, or 5 nm to 20 nm. The phase purity of the perovskite compounds of formula (I) can be at least 90%. In some embodiments, the phase purity of the perovskite compounds is at least 95%, 96%, 97%, 98%, or 99%. The perovskite compounds of formula (I) may have the morphology of spherical primary particles. The compounds of formula (I) may have an irregular surface as evidenced by TEM.

[0017] As used herein, the term "percent" in relation to perovskite materials means: %purity=I ペロブスカイト相 / (I ペロブスカイト相 +I 混入物相 ), where I=the intensity of the crystalline phase identified by XRD.

[0018] Alternatively, the compounds of formula (I) may have a hexagonal, cubic, rod-like, flower-like or faceted primary particle morphology.

[0019] Perovskite compounds prepared by FSP have primary particle morphology with average primary particle size in the range of 5-20 nm and spherical shape, as highlighted in the TEM image of LaFeO3-based perovskite. The crystallite size calculated from XRD also matches with the primary particle size observed in TEM. Nanocrystalline materials have somewhat disordered / amorphous-like surface as evident from TEM, which can create more oxygen vacancies at the surface and / or can have higher concentration of active B-site cations at the surface, thus improving the activity of TWC. Primary nanoparticles aggregate to form larger particles, which can be micron-sized in powder form, but have high surface area (e.g., >40 m). 2 g -1 ) The high surface area results in a higher concentration of active B cations at the surface as evidenced by XPS, a higher concentration of surface oxygen vacancies as evidenced by O2-TPD, and improved reducibility of B cations at temperatures below 500°C as evidenced by H2-TPR.

[0020] The phase purity of the compound of formula (I) is also important for optimal activity, the presence of other crystalline phases such as La(OH)3, La2O3, Fe2O3 etc. reduces activity. Perovskites prepared by FSP have the morphology of spherical primary particles with sizes ranging from 5 to 60 nm, preferably 5 to 30 nm, which may agglomerate but not exceed 40 nm. 2 g -1 The nanoparticles have a high surface area exceeding 100 nm and have a disordered surface.

[0021] Alternatively, the perovskite compound of formula (I) has a specific surface area of ​​at least 6 m 2 / g, 8m 2 / g, 20m 2 / g, 30m 2 / g, or 40m 2 / g.

[0022] In some embodiments, the compound of formula (I) may further comprise a promoter. The promoter metal is any metal recognized to have catalytic activity used in the catalytic industry, particularly metals known to have catalytic activity for treating exhaust gases derived from combustion processes. The promoter metal should be broadly construed and specifically includes copper, nickel, zinc, iron, tungsten, molybdenum, cobalt, titanium, zirconium, manganese, chromium, vanadium, niobium, as well as tin, bismuth, and antimony. Preferred transition metals are base metals, and preferred base metals include those selected from the group consisting of chromium, manganese, iron, cobalt, nickel, and copper, and mixtures thereof. In some embodiments, suitable base metals include those selected from the group consisting of iron, cobalt, nickel, manganese, and copper, and mixtures thereof. In some embodiments, the promoter metal is copper, manganese, iron, or a combination thereof. In some embodiments, the promoter metal is manganese, iron, or a combination thereof. In some embodiments, the promoter metal is copper. In some embodiments, the promoter metal is iron. In some embodiments, the promoter metal is manganese.

[0023] The promoter metal-containing perovskite compound composition can be obtained by any known method, such as an impregnation method.

[0024] The promoter metals may be present in the composition in a concentration of up to 20 weight percent (wt%), e.g., 0.1 wt% to 20 wt%, 0.5 wt% to 10 wt%, 0.5 to 1 wt%, 1 to 5 wt%, or 2 to 4 wt%, based on the total weight of the composition. In embodiments using copper, iron, manganese, or combinations thereof, the concentration of these promoter metals in the composition may be 1 to 15 wt%, 1 to 10 wt%, 1 to 5 wt%, or 1 to 3 wt%.

[0025] Formula (II): [BO x ] y :[La z BO3±δ ] 1-y In some embodiments, the perovskite compound has the formula (II): [BO x ] y :[La z BO 3±δ ] 1-y is a compound of wherein B is Fe, Mn, Co, or Ni, preferably B is Fe or Mn. In some embodiments, B is Fe. In other embodiments, B is Mn. x is from about 1 to about 2.5. y is about 1 to about 30 wt %. z is about 0.7 to about 1.1. δ is in the range of about 0 to about 0.6, preferably about 0 to about 0.5, and more preferably about 0.1 to about 0.3.

[0026] Formula (IIa): [MnO x ] y :[La z MnO 3±δ ] 1-y In some embodiments, B is Mn. In further embodiments, La z MnO 3±δ is a crystalline perovskite phase. Also, in separate alternative or additional embodiments, the recited compositions (in embodiments where B is Mn) or MnO x Or La z MnO 3±δ As such, if necessary, (a) x may be a value in the range of about 1 to about 1.1, about 1.1 to about 1.2, about 1.2 to about 1.3, about 1.3 to about 1.4, about 1.4 to about 1.5, about 1.5 to about 1.6, about 1.6 to about 1.7, about 1.7 to about 1.8, about 1.8 to about 1.9, about 1.9 to about 2.0, about 2.0 to about 2.1, about 2.1 to about 2.2, about 2.2 to about 2.3, about 2.3 to about 2.4, about 2.4 to about 2.5, or a value defined by a range including two or more of these ranges, for example, about 1.6 to about 2.5. xThe notation "MnO" refers to any binary oxide of manganese with an atomic ratio of O:Mn of x. For example, the notation includes Mn3O4 (x=1.33), Mn5O8 (x=1.6), etc. Thus, the value x defines the composition of any of the individual formulae of oxides of manganese or mixtures thereof, as described elsewhere herein. In certain independent embodiments, MnO x is primarily Mn3O4 (x=1.33), Mn5O8 (x=1.6), or a combination thereof; (b) y may be greater or less than the ranges in the preceding paragraphs. In certain embodiments, y is a value in the range of about 0 to about 1 wt % (i.e., La z MnO3 itself), 1 to about 2 wt%, about 2 to about 3 wt%, about 3 to about 4 wt%, about 4 to about 5 wt%, about 5 to about 6 wt%, about 6 to about 7 wt%, about 7 to about 8 wt%, about 8 to about 9 wt%, about 9 to about 10 wt%, about 10 to about 11 wt%, about 11 to about 12 wt%, about 12 to about 13 wt%, about 13 to about 14 wt%, about 14 to about 15 wt%, about 15 to about 16 wt%, about 16 to about 17 wt%, about 17 to about 18 wt%, about y may be a value in the range of 18 to about 19 wt%, about 19 to about 20 wt%, about 20 to about 21 wt%, about 21 to about 22 wt%, about 22 to about 23 wt%, about 23 to about 24 wt%, about 24 to about 25 wt%, about 25 to about 26 wt%, about 26 to about 27 wt%, about 27 to about 28 wt%, about 28 to about 29 wt%, or about 29 to about 30 wt%, or y may be defined as any two or more of these ranges, for example, about 2 to about 5 wt%, (c) z can be a value in the range of about 0.7 to about 0.75, about 0.75 to about 0.8, about 0.8 to about 0.85, about 0.85 to about 0.9, about 0.9 to about 0.95, about 0.95 to about 0.98, about 0.98 to about 0.99, about 0.99 to about 1, about 1 to about 1.05, or about 1.05 to about 1.1, or z can be defined as any two or more of these ranges, for example, about 0.75 to about 1.1, or about 0.8 to about 1, or about 0.8 to about 0.99, or about 0.8 to about 0.95.

[0027] In an independent alternative or additional embodiment, the MnO xMnO may be amorphous, nanocrystalline, or crystalline, or may be a mixture of amorphous, nanocrystalline, and crystalline materials. x If the composition is characterized as amorphous, or any other component, the composition will not exhibit any discernible PXRD peaks attributable to oxides of manganese (although their presence can be determined, for example, by TEM measurements). x When MnO is characterized as nanocrystalline, the composition exhibits only broad and poorly shaped PXRD peaks that are attributable to oxides of manganese. x When characterized as crystalline, the composition exhibits sharp, well-defined PXRD peaks attributable to oxides of manganese.

[0028] In alternative or additional embodiments, the composite has a thickness of about 25 to about 60 mm. 2 / g, preferably about 27 to about 45 m 2 In an independent alternative or additional embodiment, the particles have an average surface area in the range of about 25 to about 27 m. 2 / g, approx. 27~29m 2 / g, approx. 29~31m 2 / g, approx. 31~33m 2 / g, approx. 33~35m 2 / g, approx. 35~37m 2 / g, approx. 37~39m 2 / g, approx. 39~41m 2 / g, approx. 41~43m 2 / g, approx. 43~45m 2 / g, approx. 45~47m 2 / g, approx. 47 to approx. 49m 2 / g, approx. 49~51m 2 / g, approx. 51~53m 2 / g, approx. 53~55m 2 / g, approx. 55~57m 2 / g, approx. 57~60m 2 / g, or the particles may be characterized as having an average surface area spanning two or more of these ranges, e.g., from about 27 to about 45 m 2 / g. These surface areas are most conveniently measured by porosimetry using an inert gas (e.g., nitrogen or argon) and analyzed using the BET equation. Specific values ​​cited herein can be obtained on a 3Flex surface property analyzer (Micrometrics) at 77 K using N2.

[0029] In alternative or additional embodiments, the particles include aggregated and / or fused primary particles, and the primary particles are individually MnO x and La z The composition of MnO3. x and La z The size of the primary particles of MnO3 may be the same or different. In the context of the present disclosure, the term "agglomerated and / or fused" refers to the fact that the primary particles, including individual crystallites, are further bonded together in a bonding mode ("fused") to form larger aggregate particles.

[0030] In some embodiments, these primary particles are present in a size range of about 10 nm to about 60 nm, about 10 nm to about 50 nm, about 12 nm to about 50 nm, about 14 nm to about 50 nm, and / or about 14 nm to about 25 nm. In alternative or additional embodiments, the primary particles are present in a size range of about 10 nm to about 12 nm, about 12 nm to about 14 nm, about 14 nm to about 16 nm, about 16 nm to about 18 nm, about 18 nm to about 20 nm, about 20 nm to about 25 nm, about 25 nm to about 30 nm, about 30 nm to about 35 nm, about 35 nm to about 40 nm, about 40 nm to about 45 nm, about 45 nm to about 50 nm, about 50 nm to about 55 nm, about 55 nm to about 60 nm, or the size of the primary particles can be defined as a range including two or more of these ranges, for example, about 14 nm to about 25 nm. Unless otherwise specified, definitions of primary particle size ranges are determined by TEM measurements, even though it is recognized that using a TEM as the primary measurement approach introduces errors associated with particle counting statistics.

[0031] The size of the particles can also be determined by analyzing the line broadening of the reflections in the XRD pattern (using Rietveld analysis). In this approach, the repeat distance of the unit cell in a particular direction of the reflection lattice plane is measured. In this case, the sizes measured tend to be characterized at the lower end of these ranges and have a narrower distribution, suggesting that even these primary particles exist as one or more crystallites in the described compositions. For example, the range of about 14 to about 25 nm in size of the primary particles is consistent with the size of typical crystallite sizes measured by XRD. In one example, primary particles measured by TEM to have a size in the range of about 10 nm to about 60 nm were found to have a size in the range of about 10 nm to about 60 nm by XRD (i.e., the average calculated based on the line broadening) of La. 0.9 The sizes were determined to be about 12-20 nm for MnO3, about 12-30 nm for Mn3O4, and about 15 nm for La2O2CO3.

[0032] MnO x and La z MnO3, especially La z The size of the primary particles of MnO3 generally forms the basis of an embodiment independent of the composition described above, i.e., an embodiment in which the limit of y is relaxed to 0. That is, in an independent embodiment, the composition is z The primary particles of MnO3 may be described exclusively (i.e., excluding other Mn- or La-containing materials) as having a size ranging from about 10 to about 60 nm, or any permutation or combination of subranges of primary particle size. Consistent with the particle sizes described elsewhere herein, the primary particles may aggregate into larger structures.

[0033] Alternatively, or in addition, crystalline La zMnO3, whether present as a component in the composition or by itself, has a molecular weight of about 0.7 to about 0.72, about 0.72 to about 0.74, about 0.74 to about 0.76, about 0.76 to about 0.78, about 0.78 to about 0.8, about 0.8 to about 0.82, about 0.82 to about 0.84, about 0.84 to about 0.86, about 0.86 to about 0.88, about 0.88 to about 0.90, about 0.90 to about 0.92, about 0.92 to about 0.9 4, about 0.94 to about 0.96, about 0.96 to about 0.98, about 0.98 to about 1.0, about 1.0 to about 1.02, about 1.02 to about 1.04, about 1.04 to about 1.06, about 1.06 to about 1.08, or about 1.08 to about 1.1, or two or more of these ranges can be defined as, for example, about 0.90 to about 1.0, or about 0.92 to about 0.98.

[0034] In further embodiments, the disclosed compositions further comprise an oxide, hydroxide, and / or carbonate of lanthanum, such as LaOOH and / or La2O2CO3. x Similarly, the lanthanum component may be amorphous, nanocrystalline, and / or crystalline.

[0035] Non-redox active ingredients The catalyst composition of the present invention contains a non-redox active component, such as one or more non-redox active oxides. Suitable non-redox active oxides include, for example, alumina, ZrO2, doped ZrO2, such as ZrO2 doped with Nb, Nd, Y, or La, or combinations thereof. Suitable types of alumina include, for example, γ-, δ-, θ-, and α-alumina.

[0036] Three-way catalyst composition Another aspect of the present disclosure relates to a three-way catalyst composition comprising a perovskite compound and a non-redox active component. In some embodiments, the three-way catalyst is completely free of platinum group metals. In some embodiments, the three-way catalyst is substantially free of platinum group metals. In some embodiments, the three-way catalyst is essentially free of platinum group metals.

[0037] In some embodiments, the three-way catalyst composition comprises a weight ratio of the perovskite compound to the non-redox active component of about 0.5:1 to about 3:1, about 0.7:1 to about 2.7:1, about 1:1 to about 2.5:1, about 1.3:1 to about 2.5:1, about 1.5:1 to about 2.5:1, about 1.7:1 to about 2.2:1, or about 2:1.

[0038] In some embodiments, the three-way catalyst composition comprises a perovskite compound in an amount of about 5 wt% to about 75 wt%, about 10 wt% to about 75 wt%, about 15 wt% to about 75 wt%, about 20 wt% to about 70 wt%, about 25 wt% to about 65 wt%, about 30 wt% to about 60 wt%, about 35 wt% to about 55 wt%, about 40 wt% to about 50 wt%, about 15 wt% to about 45 wt%, about 20 wt% to about 40 wt%, about 25 wt% to about 35 wt%, about 45 wt% to about 75 wt%, about 50 wt% to about 70 wt%, or about 55 wt% to about 65 wt% of the catalyst composition.

[0039] In some embodiments, the three-way catalyst composition comprises a non-redox active component in an amount of about 25 wt% to about 95 wt%, about 25 wt% to about 90 wt%, about 25 wt% to about 85 wt%, about 25 wt% to about 80 wt%, about 25 wt% to about 75 wt%, about 30 wt% to about 70 wt%, about 35 wt% to about 65 wt%, about 40 wt% to about 60 wt%, about 45 wt% to about 55 wt%, about 25 wt% to about 50 wt%, about 30 wt% to about 45 wt%, about 35 wt% to about 40 wt%, about 50 wt% to about 75 wt%, about 55 wt% to about 70 wt%, or about 60 wt% to about 65 wt% of the catalyst composition.

[0040] In some embodiments, the three-way catalyst composition comprises a perovskite compound and alumina. In some embodiments, the three-way catalyst composition comprises a perovskite compound and ZrO2. In some embodiments, the three-way catalyst composition comprises a perovskite iron compound and alumina. In some embodiments, the three-way catalyst composition comprises a perovskite manganese compound and alumina. In some embodiments, the three-way catalyst composition comprises a perovskite iron compound and ZrO2. In some embodiments, the three-way catalyst composition comprises a perovskite manganese compound and ZrO2.

[0041] Articles, Systems, and Methods The catalytic article of the present invention may comprise a catalytic composition as described herein and a substrate. In some embodiments, the catalytic article has a surface area of ​​up to about 2 g / in 3 , for example, about 0.5 g / in 3 ~about 2g / in 3 , about 0.5g / in 3 ~ approx. 1.5g / in 3 , or about 1 g / in 3 In some embodiments, the catalyst article comprises a perovskite compound at a loading of up to about 3 g / in 3 , for example, about 0.5 g / in 3 ~About 3g / in 3 , about 1g / in 3 ~About 3g / in 3 , about 1.5g / in 3 ~ approx. 2.5g / in 3 , about 1g / in 3 ~about 2g / in 3 , about 2g / in 3 , or about 1 g / in 3 The non-redox active component is included in the loading amount.

[0042] The catalyst composition may be applied to the substrate by any known means, including the application of a washcoat. Suitable substrates may include flow-through monoliths or wall-flow gasoline particulate filters. Preferably, the substrate is a flow-through monolith.

[0043] The flow-through monolith substrate may have a first surface and a second surface defining a longitudinal direction therebetween. The flow-through monolith substrate has a plurality of channels extending between the first surface and the second surface. The plurality of channels extend longitudinally and provide a plurality of interior surfaces (e.g., surfaces of walls defining each channel). Each of the plurality of channels has an opening at the first surface and an opening at the second surface. For the avoidance of doubt, the flow-through monolith substrate is not a wall-flow filter.

[0044] The first surface is typically at an inlet end of the substrate and the second surface is at an outlet end of the substrate.

[0045] The channels may be of constant width, and each of the plurality of channels may have a uniform channel width.

[0046] Preferably, the monolith substrate has 100 to 900 channels per square inch, preferably 300 to 750 channels per square inch in a plane perpendicular to the longitudinal direction. For example, on the first face, the density of the open first channels and closed second channels is 300 to 750 channels per square inch. The channels may have a cross-section that is rectangular, square, circular, oval, triangular, hexagonal, or other polygonal shape.

[0047] The monolith substrate acts as a support to hold the catalytic material. Suitable materials for forming the monolith substrate include ceramic-like materials such as cordierite, silicon carbide, silicon nitride, zirconia, mullite, spodumene, alumina-silica magnesia or zirconium silicate, or porous refractory metals. Such materials and their use in the manufacture of porous monolith substrates are well known in the art.

[0048] It should be noted that the flow-through monolith substrates described herein are unitary components (i.e., a single brick-like mass). Nevertheless, when forming an exhaust treatment system, the monoliths used may be formed by gluing together multiple channels, or may be formed by gluing together multiple smaller monoliths as described herein. Such techniques, along with suitable casings and configurations of exhaust treatment systems, are known in the art.

[0049] In embodiments in which the catalyst article of the present invention includes a ceramic substrate, the ceramic substrate may be made of any suitable refractory material, such as alumina, silica, titania, ceria, zirconia, magnesia, zeolites, silicon nitride, silicon carbide, zirconium silicate, magnesium silicate, aluminosilicates, and metalloaluminosilicates (such as cordierite and spodumene), or mixtures or mixed oxides of any two or more thereof. Cordierite, magnesium aluminosilicate, and silicon carbide are particularly preferred.

[0050] In embodiments in which the catalytic article of the present invention includes a metal substrate, the metal substrate may be made of any suitable metal, particularly heat-resistant metals and metal alloys such as titanium and stainless steel, and ferritic alloys containing iron, nickel, chromium, and / or aluminum in addition to other trace metals.

[0051] In some embodiments, the catalyst composition is supported / deposited directly on a substrate.

[0052] The present invention also includes an exhaust system for an internal combustion engine comprising the three-way catalyst component of the present invention, wherein the three-way catalyst component may be located in a close-coupled position or an underfloor position.

[0053] The present invention also encompasses the treatment of exhaust gases from internal combustion engines, particularly gasoline engines, which method comprises contacting the exhaust gases with a three-way catalyst component of the present invention.

[0054] effect It has been surprisingly found that combining a perovskite compound with a non-redox active component results in a three-way catalyst composition that is active even after exposure to aging conditions, including high temperature aging conditions. This high temperature stability is beneficial because conventional perovskite three-way catalyst compositions have been found to become deactivated after aging.

[0055] In some embodiments, a three-way catalyst composition of the invention (e.g., including a perovskite compound of Formula (I)) may provide a fresh NO conversion at 500-600° C., and an aged NO conversion at 500-600° C. after aging the catalyst in the presence of water vapor at a temperature of at least 700° C. for 20 hours, where the difference between the fresh and aged conversions is less than a 20%, less than a 15%, less than a 10%, or less than a 5% decrease.

[0056] In other embodiments, a three-way catalyst composition of the invention (e.g., including a perovskite compound of Formula (II)) may provide a CO or HC conversion at 500° C. when fresh, and at 500° C. after aging the catalyst in the presence of water vapor at a temperature of at least 700° C. for 20 hours, where the difference between the fresh and aged CO or HC conversions is less than a 50%, less than a 40%, less than a 30%, or less than a 20% decrease.

[0057] term The term "washcoat" is known in the art and typically refers to an adherent coating that is applied to a substrate during the preparation of a catalyst.

[0058] As used herein, the acronym "PGM" refers to "platinum group metals." The term "platinum group metals" generally refers to metals selected from the group consisting of Ru, Rh, Pd, Os, Ir and Pt, preferably metals selected from the group consisting of Ru, Rh, Pd, Ir and Pt. Generally, the term "PGM" preferably refers to metals selected from the group consisting of Rh, Pt and Pd.

[0059] The term "mixed oxide" as used herein generally refers to a mixture of oxides in a single phase, as conventionally known in the art. The term "complex oxide" as used herein generally refers to a composition of oxides having two or more phases, as conventionally known in the art.

[0060] The term "substantially free" as used herein with respect to a material typically means that the material is present in a small amount, e.g., 5% by weight or less, preferably 2% by weight or less, more preferably 1% by weight or less, in the context of the contents of a region, layer, or zone. The term "substantially free" encompasses the term "free."

[0061] The term "essentially free" as used herein with respect to a material typically means that the material is present in trace amounts, e.g., 1% by weight or less, preferably 0.5% by weight or less, more preferably 0.1% by weight or less, in the context of the contents of a region, layer, or zone. The term "essentially free" encompasses the term "free".

[0062] As used herein, any reference to an amount of dopant expressed as weight percent, particularly a total amount, refers to the weight of the support material or refractory metal oxide thereof.

[0063] As used herein, the term "loading" refers to g / ft2 on a metal weight basis. 3 Refers to the measurement in units of .

[0064] In this disclosure, the singular forms "a," "an," and "the" include plural references unless expressly stated otherwise, and a reference to a particular numerical value includes at least that particular value. Thus, for example, a reference to a "material" is a reference to at least one of such materials and equivalents thereof known to those of ordinary skill in the art, and so forth.

[0065] When values ​​are expressed as approximations by using the descriptor "about", it will be understood that the particular value forms another embodiment. In general, the use of the term "about" indicates an approximation that may vary depending on the desired properties sought to be obtained by the disclosed subject matter and should be interpreted in the particular context in which it is used based on its function. Those skilled in the art will be able to interpret this as a matter of routine. In some cases, the number of significant figures used for a particular value may be one non-limiting way of determining the scope of the word "about". In other cases, the gradations used in a series of values ​​can be used to determine the intended range available to the term "about" for each value. When present, all ranges are inclusive and combinable. That is, reference to values ​​stated in a range includes every value within that range.

[0066] For clarity, it should be understood that certain features of the invention described herein in the context of separate embodiments or aspects may also be provided in combination in a single embodiment or aspect. That is, unless expressly incompatible or specifically excluded, each individual embodiment is considered to be combinable with any other embodiment or aspect, and such combinations are considered to be separate embodiments. Conversely, for brevity, various features of the invention that are described in the context of a single embodiment or aspect may also be provided separately or in any subcombination. Finally, while an embodiment or aspect may be described as part of a series of steps or as part of a more general structure, each step is also considered to be an aspect of an embodiment in its own right and can be combined with other steps.

[0067] The transitional terms "comprising," "consisting essentially of," and "consisting" are intended to encompass their generally accepted meanings in patent terminology, i.e., (i) "comprising" is synonymous with "including," "containing," or "characterized by," and is inclusive or open-ended and does not exclude additional, unrecited elements or method steps; (ii) "consisting of" excludes any element, step, or ingredient not specified in the claim; and (iii) "consisting essentially of" limits the scope of the claim to the specified materials or steps and those that do not "materially affect the basic and novel characteristics" of the claimed invention. An embodiment described with the term "comprising" (or its equivalent) also provides, as an embodiment, an embodiment described independently with the terms "consisting of" and "consisting essentially of." In these embodiments, denoted by the term "consisting essentially of," the basic and novel feature is the ability to reduce NOx by the catalyst composition in a vehicle exhaust system with robustness to air-fuel ratios. x The ability to efficiently treat CO, HC, and CO simultaneously. Materials or processes that do not impair such operability are considered within the scope of such embodiments.

[0068] When a list is presented, unless otherwise stated, it is to be understood that each individual member of that list, and every combination of that list, is a separate embodiment. For example, a list of embodiments or aspects presented as "A, B, or C" should be interpreted as including the embodiments "A," "B," "C," "A or B," "A or C," "B or C," or "A, B, or C."

[0069] Throughout this specification, words should be given their ordinary meaning as understood by those of ordinary skill in the relevant art. However, to avoid any doubt, the meaning of certain terms will be specifically defined or clarified.

[0070] "Optional" or "optionally" means that the subsequently described circumstance may or may not occur. Thus, the description includes instances where the circumstance occurs and instances where it does not occur. Similarly, embodiments that refer to an ingredient or step as "optionally present" include separate and independent embodiments in which the step or ingredient is or is not present. The term "optional" allows for the optional condition to occur, but does not require it.

[0071] The following examples are merely illustrative of the present invention, and those of ordinary skill in the art will recognize many variations that are within the spirit and scope of the claims.

[0072] The following examples are merely illustrative of the present invention, and those of ordinary skill in the art will recognize many variations that are within the spirit and scope of the claims. EXAMPLES

[0073] The materials prepared in the examples described below were characterized by one or more of the following analytical methods. Powder X-ray diffraction (PXRD) patterns were collected on a Bruker D8 powder diffractometer using CuKα radiation (40-45 kV, 40 mA) between 5° and 100° (2θ) with a step size of 0.04° and 1 s per step. Transmission electron microscope (TEM) images were obtained on a JEM2800 (scanning) TEM at a voltage of 200 kV. Micropore volume and surface area were measured on a 3Frex surface property analyzer (Micrometrics) at 77 K using N2.

[0074] material All reagent materials are commercially available and were obtained from known sources unless otherwise noted.

[0075] Flame spray pyrolysis (FSP): FSP perovskite materials are typically synthesized by liquid-fed flame pyrolysis. The precursors are dissolved in a suitable solvent at a specific temperature. The solution is then fed into a flame along with a flow of oxygen. The particles are transported through stainless steel ducts to a baghouse equipped with air filter bags, and are collected by reverse pulse washing the filter bags.

[0076] Comparative catalyst 1 (La 0.8 FeO3): Lanthanum(III) 2-ethylhexanoate solution (27.78 g, 0.02 mole) and iron(III) acetylacetonate (8.84 g, 0.025 mole) were dissolved in 150 mL of xylene. The solution (200 mL, 0.33 mol / L) was then fed into a CH4 / O2 (1.5 / 3.2 L / min, mixed) flame at a rate of 10 mL / min, together with an oxygen flow (dispersed, sheath flow rate 20 L / min). The particles were conveyed through a stainless steel duct to a baghouse equipped with an air filter bag (Whatman GF / D filter paper) and were collected by reverse pulse washing the filter bag. The obtained comparative catalyst 1 was phase pure with an average crystallite size of 12 nm as evident from XRD. Comparative catalyst 1 had a spherical particle morphology and was dissolved in water at 80 m. 2 g -1 and a surface composition of La / Fe=1.1 (XPS).

[0077] Catalyst 2 (Comparative catalyst 1 + Al2O3): Catalyst 2 was prepared by physically mixing the powder of Comparative Catalyst 1 with gamma alumina (Al2O3) in a 2:1 weight ratio.

[0078] Catalyst 3 (Comparative Catalyst 1 + ZrO2): Catalyst 3 was prepared by physically mixing the powder of Comparative Catalyst 1 with monoclinic zirconia (ZrO2) in a 2:1 weight ratio.

[0079] Example 1 Comparative Catalyst 1, Catalyst 2, and Catalyst 3 were tested under standard perturbed gasoline conditions at temperatures between 500° C. and 600° C. The catalysts were then aged for 20 hours with temperatures above 700° C. in the presence of water vapor and under rich / lean conditions. The specific conditions are as follows: Test conditions: Perturbed gas mixture (WHSV=750Lg -1 h -1 ), λ±0.05:0.73~2.2%CO+666ppmC3H6+333ppmC3H8+2200ppmNO+0.23~0.69%H2+ * O2 + 14% CO2 + 4% H2O (100% with N2), 3s / perturbation Degradation conditions: Perturbed gas mixture, λ=0.93~1.06: 0.5% CO + 1000ppm C3H8 + 1000ppm NO + 0.27~1.07% O2 + 10% H2O (100% with N2), 5min / perturbation.

[0080] [Table 1]

[0081] [Table 2]

[0082] As shown in Tables 1 and 2 above, Comparative Catalyst 1, when fresh, has a CO / HC / NO conversion rate of over 50% under standard perturbed gasoline conditions at 500-600°C, but when exposed to aging conditions, the catalyst exhibits severe deactivation, resulting in a CO / NO conversion rate of less than 15% at 500-600°C. However, Catalyst 2 (containing alumina) and Catalyst 3 (containing zirconia) were able to retain significantly higher activity after exposure to severe aging conditions. In summary, after aging at high temperatures, Catalyst 1 shows a loss of up to 90% of its CO, HC, and NO conversion capacity, while when the catalyst is mixed with alumina (Catalyst 2) or zirconia (Catalyst 3), the loss of catalytic activity for CO / HC / NO conversion is much smaller, retaining more than 30% activity.

[0083] Comparative catalyst 4 (MnO x :La 0.9 MnO3) KOH (85%, 8.41 g, 0.127 mol) was dissolved in water (200 mL) and the solution was stirred at 400 rpm using a magnetic stir bar and heated to 60 °C. Lanthanum nitrate hexahydrate (7.58 g, 0.0175 mol) and manganese nitrate (50 wt / w% solution, 8.95 g, 0.025 mol) were dissolved in water to bring the total volume of the solution to 100 mL. The salt solution was added to the base at 10 mL / min. After the addition was complete, the precipitate was stirred and aged at 60 °C for 30 min. The material was recovered by filtration, washed to remove adsorbed ions, and dried at 105 °C. The sample was calcined in air at 700 °C for 2 h to form the perovskite phase. The perovskite crystallite size was 12.5 nm and was 90.9% perovskite phase.

[0084] Catalysts 5A-5C (Comparative Catalyst 4 + Doped ZrO2) Mixture (MnO x :La 0.9 MnO3-doped ZrO2) x :La 0.9 MnO3 and doped ZrO2 [dopants: 10.1 wt% Nb2O5 (5A), 13.05% Y2O3 (5B), or 14.7% Nd2O3 (5C)] were separately dispersed in water and subsequently immersed in 6–7 μm d 90 Then, MnO x :La 0.9 The slurry of MnO3 and doped ZrO2 was mixed in a 2:1 ratio for 3-4 hours, dried, ground into powder, and calcined at 700 °C.

[0085] Example 2 Stabilization effect (after hydrothermal redox degradation) As shown in Figures 1 and 2, after aging, TEM images of Comparative Catalyst 4 show that the size of the primary particles is stabilized in the presence of doped ZrO2 (10.1% Nb2O5; Catalyst 5A). x :La 0.9The size of the MnO3 particles increases from an initial 20-80 nm when fresh to 200-1000 nm after aging. When doped ZrO2 is present (e.g., catalyst 5A), the MnO x :La 0.9 The primary particles of MnO3 remain smaller at 200–500 nm.

[0086] Example 3 Comparative Catalyst 4 and Catalyst 5A were tested under standard perturbed gasoline conditions at 500° C. The catalysts were then aged for 16 hours with temperatures above 950° C. in the presence of water vapor and under rich / lean conditions. The specific conditions are as follows: Test conditions: Perturbed gas mixture (WHSV = 750 Lg -1 h -1 ), λ±0.05:0.73~2.2%CO+666ppmC3H6+333ppmC3H8+2200ppmNO+0.23~0.69%H2+ * O2 + 14% CO2 + 4% H2O (100% with N2), 3s / perturbation Degradation conditions: perturbed gas mixture, λ = 0.93–1.06: 0.5% CO + 1000 ppm C3H8 + 1000 ppm NO + 0.27–1.07% O2 + 10% H2O (100% with addition of N2), 5 min / perturbation.

[0087] [Table 3]

[0088] As shown in Table 3 above, Comparative Catalyst 4 exhibits over 50% CO / HC conversion and over 20% NO conversion under standard perturbed gasoline conditions at 500°C when fresh, but when exposed to aging conditions, the catalyst exhibits severe deactivation, resulting in CO / NO conversion of 30% or less at 500°C. However, Catalyst 5A (containing doped ZrO2) was able to retain higher activity even after exposure to severe aging conditions. In summary, after aging at high temperatures, Comparative Catalyst 4 exhibits a loss of >65-70% of its ability to oxidize CO and HC, but when the catalyst is mixed with doped ZrO2 (e.g., Catalyst 5A), the change in CO and HC conversion at 500°C is only 12-35%.

Claims

1. Formula (I): La z B 1-q B' q O 3±δ In the formula (I), B is Fe; q is 0, δ is in the range of 0 to 0.6; z is 0.6 to 1.1; a perovskite compound and a non-redox active component, the non-redox active component being ZrO 2 doped with Nb; Or the formula (II): [BO x ] y :[La z B.O. 3±δ ] 100-y In the formula (II), B is Mn; δ is in the range of 0 to 0.6; x is 1 to 2.5; y is 1 to 30 wt %, z is 0.6 to 1.1; The perovskite type compound and the non-redox active component are alumina, ZrO 2 , or ZrO doped with Nb, Y or La 2 The three-way catalyst composition, wherein the non-redox active oxide is selected from:

2. 10. The three-way catalyst composition of claim 1, wherein said catalyst composition comprises up to 5 wt.% of a platinum group metal, based on the total weight of the catalyst composition.

3. 3. The three-way catalyst composition of claim 1 or 2, wherein the catalyst composition is free of platinum group metals.

4. A three-way catalyst composition according to any one of claims 1 to 3, wherein the perovskite compound is present in an amount of from 5 wt% to 75 wt% of the catalyst composition.

5. The three-way catalyst composition of any one of claims 1 to 4, wherein the non-redox active component is present in an amount of from 25 wt% to 95 wt% of the catalyst composition.

6. A three-way catalyst composition according to any one of claims 1 to 5, wherein the perovskite compound and the non-redox active component are present in a weight ratio of from 0.5:1 to 3:

1.

7. The perovskite compound has a molecular weight of at least 40 m. 2 The three-way catalyst composition according to any one of claims 1 to 6, having a high surface area of ​​100 / g.

8. 1. A catalytic article for treating exhaust gas, comprising: a. a substrate; b. A catalyst article comprising the three-way catalyst composition according to any one of claims 1 to 7.

9. A method for treating exhaust gas from an internal combustion engine, comprising contacting the exhaust gas with a catalyst article comprising a substrate and a three-way catalyst composition according to any one of claims 1 to 7.

10. The three-way catalyst composition comprises: (1) NO conversion at 500-600°C when fresh, and (2) providing a NO conversion at 500-600° C. after aging the catalyst composition in the presence of water vapor at a temperature of at least 700° C. for 20 hours; 10. The method of claim 9, wherein the difference between the fresh NO conversion rate and the aged NO conversion rate is less than a 20% decrease.

11. 11. The method of claim 10, wherein the difference between the fresh NO conversion rate and the aged NO conversion rate is less than a 15% decrease.

12. The three-way catalyst composition comprises: (1) HC or CO conversion at 500° C. when fresh, and (2) providing a post-aging HC or CO conversion at 500° C. after aging the catalyst composition in the presence of water vapor at a temperature of at least 700° C. for 20 hours; 10. The method of claim 9, wherein the difference between the fresh HC conversion rate and the aged HC conversion rate or the difference between the fresh CO conversion rate and the aged CO conversion rate is less than a 50% decrease.

13. 13. The method of claim 12, wherein the difference between the fresh HC conversion rate and the aged HC conversion rate or the difference between the fresh CO conversion rate and the aged CO conversion rate is reduced by less than 40%.

Citation Information

Patent Citations

  • Catalyst for catalytic reduction of nitrogen oxide

    JP1993076762A

  • Catalyst for purifying exhaust gas

    JP2008012382A

  • Catalyst for exhaust purification, and method for producing the same, and catalyst converter for exhaust purification

    JP2018030100A

  • Non-precious metal three way catalyst

    US5182249A

  • Novel perovskite-type compound for gasoline exhaust gas applications

    WO2018224946A1