Etching solution
The etching solution enhances molybdenum etching by incorporating hydrogen peroxide, acidic substances, amine compounds, and molybdenum erosion promoting ions, addressing residue issues and achieving efficient copper/molybdenum film processing.
Patent Information
- Application Number
- JP2020159428
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-09-24
AI Technical Summary
Existing etching solutions for copper/molybdenum multilayer films fail to effectively adjust the etching rate of molybdenum, leading to residue formation during the etching process.
An etching solution containing hydrogen peroxide, an acidic substance, an amine compound, a hydrogen peroxide decomposition inhibitor, and molybdenum erosion promoting ions, specifically iron or silver ions, is used to enhance the etching rate of molybdenum, preventing residue formation.
The solution effectively increases the etching rate of molybdenum, ensuring complete removal without residue, thereby facilitating efficient processing of copper/molybdenum two-layer films.
Smart Images

Figure 0007595273000004 
Figure 0007595273000001 
Figure 0007595273000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an etching solution for etching a multilayer film of molybdenum and copper, and provides an etching solution that is particularly suitable for eliminating molybdenum residues. [Background technology]
[0002] In LCD devices, pixels are turned on and off using TFTs (thin film transistors). In other words, TFTs are arranged across the entire screen. Power is supplied to these from the edges of the screen. Therefore, as the screen gets larger, the length of the wiring to the pixels in the center of the screen becomes longer. This makes it impossible to ignore the wiring resistance, and it has become necessary to use low-resistance materials for the wiring.
[0003] Traditionally, aluminum and other materials have been used for wiring in display devices, but in recent years, copper, which has a lower resistivity, has been used. In addition, a metal such as molybdenum is laid as an undercoat to ensure adhesion to the substrate, and a double-structure wiring is used.
[0004] Wet etching is essential to form a large number of pixels on a large screen at once, and many etching solutions have been proposed for etching copper / molybdenum two-layer wiring.
[0005] Patent Document 1 aims to provide an etching solution for a copper / molybdenum-based multilayer thin film that reduces damage to an oxide semiconductor layer such as IGZO, and a method for selectively etching a copper / molybdenum-based multilayer thin film relative to an oxide semiconductor layer using the same, and discloses an etching solution that contains (A) hydrogen peroxide, (B) an inorganic acid that does not contain fluorine atoms, (C) an organic acid, (D) an amine compound having 2 to 10 carbon atoms and having an amino group and at least one group selected from an amino group and a hydroxyl group, (E) an azole, and (F) a hydrogen peroxide stabilizer, and that has a pH of 2.5 to 5. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2013 / 015322 Summary of the Invention [Problem to be solved by the invention]
[0007] When etching a copper / molybdenum bilayer, there was an issue that molybdenum residue was left behind. Molybdenum is about 5-8% of the thickness of copper, but has a smaller etching rate than copper. Also, while several methods have been found to adjust the etching rate of copper, no method has been found to selectively adjust the etching rate of molybdenum. [Means for solving the problem]
[0008] The present invention has been made in view of the above problems, and provides an etching solution that uses metal ions having strong oxidizing power (the ability to steal electrons from a molybdenum film) as molybdenum erosion-promoting ions, thereby increasing the etching rate of molybdenum and preventing the generation of molybdenum residues.
[0009] More specifically, the etching solution according to the present invention is An etching solution for etching a copper and molybdenum bilayer film, Hydrogen peroxide, acidic substance Quality and , An amine compound, A hydrogen peroxide decomposition inhibitor; Iron ions or silver ions are used as ions accelerating molybdenum erosion. N Has When the iron ion is used, 100ppm to 9000ppm (1.79 x 10 per 100 g of etching solution -4 mol or more 1.61×10 -2 mol or less), In addition, when the silver ions are used, 80ppm to 5000ppm (7.41 x 10 per 100 g of etching solution -5 mol or more 4.63×10 -3 mol or less), Phosphoric acid compounds, hydrofluoric acid compounds, hydrochloric acid and It is characterized by not containing azoles. Effect of the Invention
[0010] The etching solution according to the present invention can increase the etching rate of molybdenum by containing specific metal ions, i.e., molybdenum erosion promoting ions, and therefore can etch a copper / molybdenum bilayer film without leaving any molybdenum residue. [Brief description of the drawings]
[0011] [Figure 1] The images were taken of the Si substrate of the bilayer film sample after processing, (a) for the sample basic composition solution 2, and (b) for the comparative sample solution. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The etching solution according to the present invention will be described below with reference to examples. Note that the following description is merely an example of one embodiment of the present invention and an example, and the present invention is not limited to the following description. The following description can be modified without departing from the spirit of the present invention. Note that in the following description, the atomic weight of silver is 108, and the atomic weight of iron is 56.
[0013] <Target for etching> The etching solution according to the present invention is used for a two-layer film of molybdenum and copper, and is particularly suitable for use with a molybdenum film having a thickness of 10 nm to 50 nm and a copper film having a thickness of 450 nm to 900 nm.
[0014] <Composition of Etching Solution> The etching solution according to the present invention is characterized by containing hydrogen peroxide, an acidic substance, amines, a hydrogen peroxide decomposition inhibitor, molybdenum erosion promoting ions, and water. Other minute additives may also be contained. The molybdenum erosion promoting ions are specific metal ions derived from a molybdenum erosion promoting agent having a specific metal ion.
[0015] <Hydrogen peroxide> In the etching of copper, copper is oxidized to become copper oxide (CuO), which is dissolved by acid (organic acid). In the etching of molybdenum, molybdenum is oxidized to become molybdenum oxide (MoO3), which is dissolved. Hydrogen peroxide is used as an oxidizing agent to oxidize copper and molybdenum. Note that hydrogen peroxide and hydrogen peroxide are synonymous. The amount of hydrogen peroxide is preferably 3.0% by mass to 8.0% by mass, more preferably 3.5% by mass to 6.0% by mass, based on the total amount of the etching solution.
[0016] <Acidic substances> Acidic substances include organic acids and inorganic acids. Organic acids are used to control the cross-sectional shape of etched interconnects.
[0017] Inorganic acids are used to adjust the pH of the etching solution together with amine compounds described later, and mainly contribute to dissolving oxidized copper and molybdenum. They also serve to maintain metal ions in an ionic state. When inorganic acids are used, it is preferable not to use phosphoric acid compounds, hydrofluoric acid compounds, or hydrochloric acid in order to reduce the environmental load when disposing of the etching solution. Nitric acid and sulfuric acid can be suitably used. Inorganic acids are contained in an amount of 0.01% by mass or more and 2.00% by mass or less, preferably 0.02% by mass or more and 1.50% by mass or less, of the total amount of the etching solution.
[0018] Preferred examples of the organic acid include aliphatic carboxylic acids having 1 to 18 carbon atoms, aromatic carboxylic acids having 6 to 10 carbon atoms, and amino acids having 1 to 10 carbon atoms.
[0019] Preferred examples of the aliphatic carboxylic acid having 1 to 18 carbon atoms include formic acid, acetic acid, propionic acid, lactic acid, glycolic acid, diglycolic acid, pyruvic acid, malonic acid, butyric acid, hydroxybutyric acid, tartaric acid, succinic acid, malic acid, maleic acid, fumaric acid, valeric acid, glutaric acid, itaconic acid, adipic acid, caproic acid, adipic acid, citric acid, propanetricarboxylic acid, trans-aconitic acid, enanthic acid, caprylic acid, lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, and linolenic acid.
[0020] Preferred examples of the aromatic carboxylic acid having 6 to 10 carbon atoms include benzoic acid, salicylic acid, mandelic acid, phthalic acid, isophthalic acid, and terephthalic acid.
[0021] Preferred examples of the amino acid having 1 to 10 carbon atoms include carbamic acid, alanine, glycine, asparagine, aspartic acid, sarcosine, serine, glutamine, glutamic acid, 4-aminobutyric acid, iminodibutyric acid, arginine, leucine, isoleucine, and nitrilotriacetic acid.
[0022] The organic acids may be used in combination. The acidic organic acid is preferably contained in an amount of 1% by mass to 10% by mass based on the total amount of the etching solution.
[0023] <Amine compounds> The amine compound is responsible for adjusting the pH of the etching solution. The etching solution according to the present invention improves the etching rate of molybdenum not only by oxidizing the copper film or molybdenum film with hydrogen peroxide, but also by strong oxidation with metal ions (taking away electrons from molybdenum). Therefore, the metal ions must exist in an ionic state. Therefore, the pH of the etching solution must be controlled to 1 to 5. The amine compound adjusts the pH for this purpose.
[0024] Examples of the amine compound include the following substances. As the amine compound, those having 2 to 10 carbon atoms can be suitably used. More specifically, ethylenediamine, trimethylenediamine, tetramethylenediamine, N,N,N,N-tetramethylethylenediamine, 1,2-propanediamine, 1,3-propanediamine, N,N,N,N-tetramethyl-1,3-propanediamine, N,N-dimethyl-1,3-propanediamine, N,N-diethyl-1,3-propanediamine, 1,3-diaminobutane, 2,3-diaminobutane, pentamethylenediamine, 2,4-diaminopentane, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, polyamines such as diamine, nonamethylenediamine, N-methylethylenediamine, N,N-dimethylethylenediamine, trimethylethylenediamine, N-ethylethylenediamine, N,N-diethylethylenediamine, triethylethylenediamine, 1,2,3-triaminopropane, hydrazine, tris(2-aminoethyl)amine, tetra(aminomethyl)methane, diethylenetriamine, triethylenetetramine, tetraethylpentamine, heptaethyleneoctamine, nonaethylenedecamine, and diazabicycloundecene;Ethanolamine, N-Methylethanolamine, N-Methyldiethanolamine, N-Ethylethanolamine, N-Aminoethylethanolamine, N-Propylethanolamine, N-Butylethanolamine, Diethanolamine, Triethanolamine, 1-Amino-2-propanol, N-Methylisopropanolamine, N-Ethylisopropanolamine, N-Propylisopropanolamine, 2-Aminopropan-1-ol, N-Methyl-2-amino-propane -1-ol, N-ethyl-2-amino-propan-1-ol, 1-aminopropan-3-ol, N-methyl-1-aminopropan-3-ol, N-ethyl-1-aminopropan-3-ol, 1-aminobutan-2-ol, N-methyl-1-aminobutan-2-ol, N-ethyl-1-aminobutan-2-ol, 2-aminobutan-1-ol, N-methyl-2-aminobutan-1-ol, N-ethyl-2-aminobutan-1-ol, 3-aminobutan-1-ol, N-Methyl-3-aminobutan-1-ol, N-Ethyl-3-aminobutan-1-ol, 1-Aminobutan-4-ol, N-Methyl-1-aminobutan-4-ol, N-Ethyl-1-aminobutan-4-ol, 1-Amino-2-methylpropan-2-ol, 2-Amino-2-methylpropan-1-ol, 1-Aminopentan-4-ol, 2-Amino-4-methylpentan-1-ol, 2-Aminohexan-1-ol, 3-Aminoheptan-4-ol, 1-Amino Preferred examples of the alkanolamines include octan-2-ol, 5-aminooctan-4-ol, 1-aminopropane-2,3-diol, 2-aminopropane-1,3-diol, tris(oxymethyl)aminomethane, 1,2-diaminopropan-3-ol, 1,3-diaminopropan-2-ol, 2-(2-aminoethoxy)ethanol, 2-(2-aminoethylamino)ethanol, and diglycolamine, and these can be used alone or in combination.
[0025] The amine compound is preferably contained in an amount of 0.5% by mass to 4.5% by mass, and more preferably 1.5% by mass to 3.5% by mass, based on the total amount of the etching solution.
[0026] <Hydrogen peroxide decomposition inhibitor> In the multilayer film etching solution according to the present invention, hydrogen peroxide is used as an oxidizing agent. Since hydrogen peroxide decomposes by itself, a decomposition inhibitor is added to suppress the decomposition. The hydrogen peroxide decomposition inhibitor is also called a hydrogen peroxide stabilizer (or a "hydrogen peroxide stabilizer").
[0027] Suitable examples of hydrogen peroxide decomposition inhibitors that can be used include 2-butoxyethanol (ethylene glycol monobutyl ether), phenylurea, allylurea, 1,3-dimethylurea, thiourea, phenylacetic acid amide, phenylethylene glycol, 1-propanol, and 2-propanol.
[0028] In particular, ethylene glycol monobutyl ether (CAS number 111-76-2: hereinafter also referred to as "BG"), phenylurea (CAS number 64-10-8), and 1-propanol (CAS number: 71-23-8) are preferably used because they have a strong tendency to maintain the etching rate even when the Cu concentration in the etching solution increases.
[0029] The amount of the hydrogen peroxide decomposition inhibitor is preferably 0.1% by mass or more and 2.0% by mass or less, and more preferably 0.5% by mass or more and 1.2% by mass or less, based on the total amount of the etching solution.
[0030] <Molybdenum corrosion promoting ions> In the etching solution according to the present invention, iron ions or silver ions are used as molybdenum erosion promoting ions that remove electrons from molybdenum, oxidize it, and promote etching. A compound that supplies the molybdenum erosion promoting ions is called a molybdenum erosion promoting agent.
[0031] As the molybdenum erosion accelerator having iron ions, iron chloride, iron nitrate, iron sulfate, etc. can be suitably used. As the molybdenum erosion accelerator having silver ions, silver chloride, silver nitrate, silver sulfate, etc. can be suitably used. In particular, from the viewpoint of waste disposal of the etching solution, iron nitrate and silver nitrate can be suitably used.
[0032] The content of the molybdenum erosion promoting ions is preferably 0.08 mass% (80 ppm) or more and less than 1.0 mass% (10,000 ppm) relative to the total amount of the etching solution, and more preferably 0.1 mass% (100 ppm) or more and 0.5 mass% (5,000 ppm) or less. The molybdenum erosion promoting agent that supplies the molybdenum erosion promoting ions is supplied in the form of a salt, and the ratio of the molybdenum erosion promoting agent to the total amount of the etching solution varies depending on the anion ions in the salt. This adjustment may be made by adjusting the composition ratio of water.
[0033] For example, if the molybdenum erosion promoting ion is silver ion, 0.08 g of silver ion (7.41 × 10 -4 When supplying 1000 mol of molybdenum using silver nitrate, 0.126 g of silver nitrate must be supplied, but when supplying silver sulfate, 0.116 g must be supplied. The number and weight of silver ions are the same in both cases, but the weight of the salt (molybdenum erosion accelerator) is different. This difference can be adjusted by the amount of water, since the amount of molybdenum erosion accelerator ions is very small.
[0034] <Other> In addition to these components, the etching solution according to the present invention may contain water as a solvent and various additives that are commonly used within a range that does not impair the etching performance. Also, azoles may be included as an etching regulator for the Cu film. Since the water is intended for precision processing, it is preferable that it is free of foreign matter. Pure water or ultrapure water is preferable. It goes without saying that the range of the content ratio of each component described above is appropriately adjusted so that the total amount of the etching solution is 100 mass%.
[0035] In addition, since the etching solution according to the present invention contains metal ions, it is desirable to adjust the pH of the etching solution to within the range of 1-5. EXAMPLES
[0036] <Changes in molybdenum etching rate due to metal ions> The etching target was a silicon substrate with a molybdenum (300 nm) film formed on it. This is called the "molybdenum film sample."
[0037] The composition of the etching solution varies depending on the purpose, but the following composition was used as the basic composition for a copper / molybdenum two-layer film (hereinafter referred to as "sample basic composition solution 1").
[0038] (Sample basic composition solution 1) Hydrogen peroxide 5.8% by mass, As inorganic acidic substances, 1.3% by mass of nitric acid, As an organic acidic substance, 1.7% by mass of malonic acid, As the amine compound, 2.5% by mass of NNDPA (N,N-diethyl-1,3-propanediamine), As a water stabilizer, BG 0.7% by mass, The remainder was water and molybdenum erosion promoting ions. The molybdenum erosion promoting ions were 80 ppm or more and did not exceed 1.0 mass% relative to the total amount of sample basic composition solution 1. If there were too many molybdenum erosion promoting ions, the decomposition of hydrogen peroxide would proceed too quickly even if a hydrogen peroxide stabilizer was added.
[0039] Example 1 In the sample basic composition solution 1, nitrates of silver, iron, zinc, copper, manganese, nickel, and aluminum were used as metal ion sources, and the amount of each metal ion was adjusted to 1000 ppm (0.1 mass%). The sample etching solutions were silver solution (meaning a solution prepared using silver nitrate as a metal ion source so that the amount of silver ions was 1000 ppm; the same applies below), iron solution, zinc solution, copper solution, manganese solution, nickel solution, and aluminum solution. The solution without the metal ion source was used as the reference solution.
[0040] A molybdenum film (300 nm) sample was immersed in each sample etching solution while maintaining the temperature at 30° C., and observed until the molybdenum film was completely dissolved, and the etching rate of molybdenum was calculated. The results are shown in Table 1.
[0041] [Table 1]
[0042] Silver ions, iron ions, and copper ions were effective in improving the etching rate of molybdenum, while zinc ions, manganese ions, nickel ions, and aluminum ions had etching rates almost the same as that of the reference solution. It was found that silver ions and iron ions were particularly effective in increasing the etching rate of molybdenum.
[0043] From the above experiments, silver ions and copper ions were determined as molybdenum erosion promoting ions, and a metal ion supply source capable of supplying molybdenum erosion promoting ions was determined as a molybdenum erosion promoting agent. For reference, 1000 ppm (0.1 mass%) of silver ions and iron ions are 0.018 mol % and 0.035 mol %, respectively, in sample basic composition solution 1, and the weight percentages listed below can be converted to mol % in the same manner.
[0044] Example 2 Next, the concentration of silver ions and iron ions was changed to confirm how the etching rate of molybdenum was changed. The same molybdenum film sample as in Example 1 was used for etching.
[0045] The results for silver ions are shown in Table 2, and those for iron ions are shown in Table 3. In addition, "copper film samples" were prepared by depositing 600 nm of Cu on a Si substrate, and the etching rates of Cu were also measured by immersing them in sample solutions containing 1000 ppm of silver ions in Table 2 and 1000 ppm of iron ions in Table 3. The temperature of each sample solution was maintained at 30°C.
[0046] [Table 2]
[0047] [Table 3]
[0048] With reference to Table 2, at 10 ppm of silver ions, the etching rate of molybdenum was 71 [nm / min], which was higher than the 14 [nm / min] of the reference liquid (see Example 1). Also, the higher the silver ion concentration, the higher the etching rate of molybdenum. However, at 8000 ppm (0.8 mass%), silver precipitated. Therefore, the silver ions must be at least 10 ppm or more and less than 8000 ppm (9.26 x 10 per 100 g of etching liquid). -6 mol or more 7.41×10 -3 mol), more preferably 80 ppm or more and 5000 ppm or less (7.41 × 10 per 100 g of etching solution). -5 mol or more 4.63×10 -3 mol or less). 80 ppm is the value at which the etching rate of molybdenum becomes 90 nm / min or more, and is a value required for practical use. In other words, experimental results showed that if the etching rate of molybdenum is 90 nm / min or more, no Mo residue was observed.
[0049] On the other hand, referring to Table 3, iron ions showed an etching rate of 90 [nm / min] at 100 ppm, and the higher the iron ion concentration, the higher the etching rate of molybdenum. However, at 10,000 ppm (1.0 mass%), abnormal decomposition of hydrogen peroxide occurred, and the etching solution could no longer be maintained. Therefore, the iron ion concentration should be between 100 ppm and 10,000 ppm (1.79 x 10 per 100 g of etching solution). -4 mol or more 1.79×10 -2 mol), and more preferably 100 ppm or more and 9000 ppm or less (1.79 × 10 per 100 g of etching solution). -4 mol or more 1.61×10 -2It has been confirmed that abnormal decomposition of hydrogen peroxide does not occur at 9000 ppm.
[0050] In addition, the etching rate of copper was 637 nm / min in an etching solution containing 1000 ppm of silver ions and 542 nm / min in the absence of silver ions, and the etching rate of copper was 610 nm / min in an etching solution containing 1000 ppm of iron ions and 563 nm / min in the absence of iron ions.
[0051] That is, the presence of silver ions increases the copper etching rate by about 18%, and the presence of iron ions increases the copper etching rate by about 8%. However, this difference in the copper ion etching rate can be fully adjusted by changing the type and amount of amino compounds and organic acid substances.
[0052] Example 3 Next, the effect of the molybdenum erosion promoting ions was confirmed by etching an actual bilayer film. The etching target was a silicon substrate with a 30 nm thick molybdenum film and a 450 nm thick copper film, which were then partially covered with photoresist to create a step. This was called the "two-layer film sample."
[0053] The etching solution had the following composition, and this etching solution was called "sample basic composition solution 2." (Sample basic composition solution 2) Hydrogen peroxide 5.81% by mass, As inorganic acidic substances, 1.84% by mass of nitric acid; As an organic acidic substance, Malonic acid 3.0% by mass As the amine compound, 3.0% by mass of TMEDA (N,N,N,N-tetramethylethylenediamine), As a water stabilizer, BG 0.88% by mass, 650 ppm of iron ion as an ion that promotes molybdenum erosion, The remainder was water. The iron ions were added as 0.47% by mass of iron nitrate (III) nonahydrate [Fe(NO3)3·9H2O] (a molybdenum erosion promoter). Therefore, the water content was 85.0% by mass.
[0054] Also, an etching solution containing no molybdenum erosion promoting ions was prepared as a "comparative example sample solution."
[0055] (Comparative Example Sample Solution) Hydrogen peroxide 5.81% by mass, As inorganic acidic substances, 1.84% by mass of nitric acid; As an organic acidic substance, Malonic acid 3.0% by mass As the amine compound, 3.0% by mass of TMEDA (N,N,N,N-tetramethylethylenediamine), As a water stabilizer, BG 0.88% by mass, The remainder was water, which accounted for 85.47% by mass.
[0056] The temperature of the sample basic composition solution 2 and the comparative sample solution was maintained at 35°C, and the bilayer film sample was immersed in each for 110 seconds. The just etch was defined as the time when the base (Si) of the part without photoresist was visually confirmed.
[0057] The results are shown in Figure 1. Figure 1 is a photograph of the Si substrate of the bilayer film sample after processing. Referring to Figure 1, Figure (a) is the case of sample basic composition solution 2, and Figure 1 (b) is the case of the comparative sample solution. The scale line is 500 nm. The just etch times were 48 seconds and 53 seconds, respectively.
[0058] In the case of sample basic composition solution 2 in Figure 1(a), it was observed that the molybdenum had been almost completely removed, with only a slight amount of molybdenum residue remaining on the Si substrate. On the other hand, in the case of the comparative sample solution in Figure 1(b), it was observed that densely packed islands of molybdenum of about 50 nm remained on the Si substrate. As described above, the presence of molybdenum erosion promoting ions increased the molybdenum etching rate, solving the problem of molybdenum etching residue remaining on the substrate. [Industrial Applicability]
[0059] The present invention can be suitably used for etching a two-layer film of molybdenum and copper.
Claims
[Claim 1] An etching solution for etching a copper and molybdenum bilayer film, Hydrogen peroxide, An acidic substance; An amine compound, A hydrogen peroxide decomposition inhibitor; Contains iron ions or silver ions as molybdenum erosion promoting ions, When the iron ion is used, 100 ppm or more and 9000 ppm or less (1.79×10 −4 mol or more and 1.61×10 −2 mol or less per 100 g of etching solution), In addition, when the silver ions are used, 80 ppm or more and 5000 ppm or less (7.41×10 −5 mol or more and 4.63×10 −3 mol or less per 100 g of etching solution), An etching solution containing no phosphoric acid compounds, no hydrofluoric acid compounds, no hydrochloric acid, and no azoles.
Citation Information
Patent Citations
Metal etching method
JP1988111186A
A copper alloy containing etching
JP1989503470A
Etching method
JP2004134818A
Tungsten etching solution
JP2011151287A
Etchant composition, and method for etching multi-layered metal film
JP2014027274A