Separators for electrochemical devices
The separator for electrochemical devices, comprising a polyvinylidene fluoride resin and inorganic particles supported on a fiber aggregate, addresses the issues of high internal resistance and poor ion conduction in existing separators, achieving improved output characteristics and heat resistance.
Patent Information
- Application Number
- JP2020066080
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-01
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-04-01
AI Technical Summary
Existing separators for electrochemical devices, such as those described in Patent Document 1, suffer from poor ion conduction characteristics and high internal resistance, which hinder the development of power sources with improved output characteristics and heat resistance.
A separator for electrochemical devices comprising a polyvinylidene fluoride resin, inorganic particles, and a fiber aggregate, where the inorganic particles are supported on the fiber aggregate by the polyvinylidene fluoride resin, with a Gurley value optimized between 8 and 44 seconds/100cc, utilizing a fiber aggregate with specific properties to enhance ion conduction and reduce internal resistance.
The proposed separator design improves ion conduction properties and reduces internal resistance, enabling power sources with lower resistance and enhanced output characteristics, while maintaining heat resistance and preventing internal short circuits.
Smart Images

Figure 0007595425000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a separator for an electrochemical element. [Background technology]
[0002] In recent years, there has been a demand for improved output characteristics of power sources, for example, to extend the driving distance of electric vehicles, hybrid cars, drones, etc., and to meet the demand for smaller and lighter electrical equipment. To realize such power sources, separators for electrochemical elements, such as secondary batteries and capacitors, which are components of the power sources, are required to reduce the internal resistance of the power source and improve the output characteristics of the power source.
[0003] Furthermore, separators for electrochemical elements are required to have improved heat resistance so that internal short circuits in power sources can be prevented even when exposed to high temperature conditions or when heat is generated. Thus, separators for electrochemical elements having excellent heat resistance, in which inorganic particles are supported on a porous substrate by a binder resin, are being considered.
[0004] As such a separator for an electrochemical element, International Publication WO2014 / 147888 (Patent Document 1) discloses a separator for an electrochemical element in which inorganic particles are supported on a porous substrate by a polyvinylidene fluoride resin. Patent Document 1 discloses that, from the viewpoint of ion permeability of a separator for an electrochemical element, the Gurley value measured in accordance with JIS P8117 is preferably 400 sec / 100 cc or less, and discloses in the examples that a separator for an electrochemical element having a Gurley value of 130 to 257 sec / 100 cc was produced. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] WO2014 / 147888 (claims, 0068, 0103, examples, etc.) Summary of the Invention [Problem to be solved by the invention]
[0006] However, as a result of the applicant's continued research, it was found that separators for electrochemical elements according to the conventional technology such as that disclosed in Patent Document 1 still have inferior ion passing characteristics and high internal resistance, and therefore cannot provide a power source with excellent output characteristics. Therefore, there was a demand for a separator for electrochemical elements that can realize a power source with lower internal resistance and improved output characteristics. [Means for solving the problem]
[0007] The present invention relates to "A separator for electrochemical elements comprising a polyvinylidene fluoride resin, inorganic particles, and a fiber aggregate, The fibers constituting the fiber assembly are only fibers composed of organic polymers, the inorganic particles are supported on the fiber assembly by the polyvinylidene fluoride resin; A separator for electrochemical elements having a Gurley value of 8 seconds / 100cc or more and 35 seconds / 100cc or less (however, The fiber aggregate does not include conductive fibers, and the inorganic particles do not include conductive particles. )」 It is. Effect of the Invention
[0008] As a result of studies by the applicant of the present application, it has been found that in a separator for electrochemical elements having a configuration in which "the separator for electrochemical elements comprises a polyvinylidene fluoride resin, inorganic particles, and a fiber aggregate, the inorganic particles being supported on the fiber aggregate by the polyvinylidene fluoride resin," by optimizing the Gurley value of the separator for electrochemical elements, it is possible to provide a separator for electrochemical elements having superior ion-permeability characteristics and lower internal resistance than conventional techniques.
[0009] In general, the smaller the Gurley value of a separator for electrochemical elements, the more excellent the air permeability is, and the easier it is for fluid to pass between the two main surfaces of the separator for electrochemical elements. Specifically, the applicant of the present application has found, through the preparation of examples and comparative examples described below, that a separator for electrochemical elements having a lower internal resistance can be provided when the Gurley value is less than 44 seconds / 100 cc. It has been believed that in electrochemical element separators with a small Gurley value, the internal resistance is reduced because ions can easily pass between the two main surfaces. In other words, based on this knowledge, it has been believed that the closer the Gurley value is to 0 sec / 100 cc, the better the ion permeability of the electrochemical element separator will be.
[0010] However, contrary to this idea, the applicant of the present application has discovered a phenomenon in which when the separator for an electrochemical element includes a fiber assembly with an excessively small Gurley value, the internal resistance of the separator for an electrochemical element increases. The reason why this phenomenon occurs has not been fully elucidated, but the applicant of the present application believes that when a separator for electrochemical elements having the configuration according to the present invention includes a fiber assembly with an excessively small Gurley value of 6 seconds / 100 cc or less, the presence of few fibers constituting the separator for electrochemical elements causes the electrolyte to be unable to be sufficiently retained in the separator for electrochemical elements (between the constituent fibers), resulting in reduced electrolyte retention and an increase in the internal resistance of the separator for electrochemical elements.
[0011] In summary, in the separator for electrochemical elements having the configuration according to the present invention, the smaller the Gurley value, the easier it is for a fluid to pass between the two main surfaces, and therefore the ion permeability is improved. However, when the Gurley value is 6 sec / 100 cc or less, the liquid retention is reduced, and therefore it is considered that the internal resistance of the separator for electrochemical elements increases. The inventors have found that, as a result of these two effects being exerted, in a separator for electrochemical elements having the configuration according to the present invention, the overall ion permeability is improved when the Gurley value is greater than 6 sec / 100 cc and less than 44 sec / 100 cc.
[0012] As described above, the present invention can provide a separator for an electrochemical element that can realize a power source with low internal resistance and improved output characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] In the present invention, various configurations can be appropriately selected, for example, the following configurations. In addition, the various measurements described in the present invention were performed under normal pressure and at a temperature of 25°C unless otherwise specified. In addition, the various measurement results described in the present invention were measured to a value one order of magnitude smaller than the desired value, and the desired value was calculated by rounding the value up or down unless otherwise specified. As a specific example, when the desired value is to the first decimal place, the value was measured to the second decimal place, and the obtained value was rounded up or down to the first decimal place to calculate the value up to the first decimal place, and this value was used as the desired value. Moreover, the upper limit values and lower limit values exemplified in the present invention can be combined in any desired manner.
[0014] The fiber assembly constituting the separator for an electrochemical element of the present invention mainly plays a role of forming the skeleton of the separator for an electrochemical element.
[0015] The type of fiber assembly can be appropriately selected, and may be, for example, a fabric such as a nonwoven fabric, a fiber web, a woven fabric, or a knitted fabric, and these materials alone, multiple layers of a single type of material, or multiple layers of multiple types of materials can be used. In particular, since the random presence of fibers makes it easy to provide a separator for an electrochemical element that can realize a power source with low internal resistance and improved output characteristics, it is preferable that the fiber assembly includes a fiber web or a nonwoven fabric, and it is more preferable that the fiber assembly is composed of only a fiber web or a nonwoven fabric.
[0016] In particular, a two-layer fiber assembly in which short fibers and / or pulp-like fibers having fibrils have penetrated the voids in a nonwoven fabric or fiber web is preferable because the pore size of the fiber assembly is uniform and the structure is dense, which makes it easier to provide a separator for electrochemical elements that is excellent in preventing short circuits caused by dendrites and can realize a power source with low internal resistance and improved output characteristics.
[0017] The fibers constituting the fiber assembly are, for example, polyolefin resins (e.g., polyethylene, polypropylene, polymethylpentene, polyolefin resins having a structure in which a portion of a hydrocarbon is substituted with a cyano group or a halogen such as fluorine or chlorine, etc.), styrene resins, polyvinyl alcohol resins, polyether resins (e.g., polyether ether ketone, polyacetal, modified polyphenylene ether, aromatic polyether ketone, etc.), polyester resins (e.g., polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polycarbonate, polyarylate, wholly aromatic polyester resins, etc.), polyimide resins, It can be constructed using known organic polymers such as polyamideimide resin, polyamide-based resin (e.g., aromatic polyamide resin, aromatic polyetheramide resin, nylon resin, etc.), resin having a nitrile group (e.g., polyacrylonitrile, etc.), urethane-based resin, epoxy-based resin, polysulfone-based resin (e.g., polysulfone, polyethersulfone, etc.), fluorine-based resin (e.g., polytetrafluoroethylene, polyvinylidene fluoride, etc.), cellulose fiber, polybenzimidazole resin, acrylic resin (e.g., polyacrylonitrile-based resin copolymerized with acrylic acid ester or methacrylic acid ester, modacrylic resin copolymerized with acrylonitrile and vinyl chloride or vinylidene chloride, etc.).
[0018] These organic polymers may be either linear or branched polymers, may be block or random copolymers, may have any three-dimensional structure, may have any crystallinity, or may be a mixture of multiple organic polymers.
[0019] In particular, since it is easy to provide a separator for electrochemical elements having excellent heat resistance, it is preferable that the fiber assembly has heat-resistant fibers (e.g., aramid fibers, polyethylene terephthalate fibers, etc.) as its constituent fibers, and it is more preferable that the constituent fibers of the fiber assembly are only such fibers.
[0020] The constituent fibers of the fiber aggregate can be obtained by known methods such as a dry spinning method, a wet spinning method, a direct spinning method (e.g., a meltblowing method, a spunbonding method, an electrostatic spinning method, a method of discharging a spinning solution and a gas flow in parallel to spin the fibers (e.g., the method disclosed in JP 2009-287138 A)), a method of extracting fibers having a small fiber diameter by removing one or more types of resin components from composite fibers, and a method of beating fibers to obtain divided fibers.
[0021] The fiber aggregate may contain fibers having irregular cross sections other than those having a substantially circular or elliptical cross section as constituent fibers. Examples of irregular cross section fibers include fibers having a cross section having a polygonal shape such as a triangular shape, an alphabetic shape such as a Y shape, an irregular shape, a multi-lobed shape, a symbolic shape such as an asterisk shape, or a shape in which multiple of these shapes are combined.
[0022] The fibers constituting the fiber assembly may be composed of one type of organic polymer or multiple types of organic polymers. Fibers composed of multiple types of organic polymers may be in the form of what is generally called composite fibers, such as core-sheath type, sea-island type, side-by-side type, orange type, bimetal type, etc.
[0023] The fiber assembly may contain adhesive fibers as constituent fibers. By containing adhesive fibers, the strength of the fiber assembly can be improved, which is preferable. The type of adhesive fiber is appropriately selected, but for example, a core-sheath type adhesive fiber, a side-by-side type adhesive fiber, or a full melt type adhesive fiber can be used.
[0024] When the fiber aggregate is a nonwoven fabric, examples of the nonwoven fabric include dry nonwoven fabrics in which fibers are entangled by feeding the fibers to a carding device or an air-laying device to form a nonwoven fabric, wet nonwoven fabrics in which a dispersion of fibers dispersed in a liquid is woven into a sheet form to form a nonwoven fabric or a fiber web, and nonwoven fabrics obtained by spinning fibers using a direct spinning method (e.g., melt-blowing method, spunbonding method, electrostatic spinning method, a method of discharging a spinning solution and a gas flow in parallel to spin the fibers (e.g., the method disclosed in JP-A-2009-287138) and collecting the fibers). A two-layer nonwoven fabric may also be prepared by woven into a sheet form a dispersion of fibers on the main surface of the nonwoven fabric.
[0025] The method of entangling and / or integrating the constituent fibers of the fiber assembly can be appropriately selected, and examples of the method include a method of entangling the fibers with needles or water flow, a method of integrating the fibers with a binder, or, in the case of including fibers containing a thermoplastic resin, a method of melting or softening the thermoplastic resin by heat treatment to integrate the fibers. As the heat treatment method, for example, a method of heating and pressurizing with a calendar roll, a method of heating with a hot air dryer, a method of melting the thermoplastic resin fibers by irradiating infrared rays under no pressure, etc. can be used. Alternatively, the fiber assembly may be prepared by collecting fibers spun using a direct spinning method.
[0026] When the fiber assembly is a woven or knitted fabric, it can be prepared by weaving or knitting the fibers prepared as described above.
[0027] The smaller the average fiber diameter of the fibers constituting the fiber assembly, the easier it is to provide a separator for an electrochemical element capable of realizing a power source with low internal resistance and improved output characteristics, and the strength of the fiber assembly can be improved to prevent breakage of the separator for an electrochemical element, and the size of the voids can be made uniform and small to prevent the occurrence of internal short circuits. Therefore, the average fiber diameter of the fibers constituting the fabric is, for example, preferably 20 μm or less, more preferably 10 μm or less, and most preferably 5 μm or less. Although there is no particular lower limit to the average fiber diameter of the fibers, it is practical for the average fiber diameter of single fibers that are not pulp-like fibers having fibrils to be 0.1 μm or more. In the present invention, the "average fiber diameter" refers to the arithmetic mean value of fiber diameters of 100 fibers selected from fibers seen in electron microscope photographs of the main surface or cross section of a fiber assembly or a separator for electrochemical devices, and the fiber diameter refers to the diameter of a circle having the same area as the cross-sectional area of the fiber.
[0028] The fiber length of the fibers constituting the fiber assembly is also appropriately selected, and the fiber length of the fibers constituting the nonwoven fabric substrate is preferably 0.1 to 20 mm, more preferably 0.5 to 15 mm, and even more preferably 1 to 10 mm so that the fibers are uniformly dispersed and the electrolyte is easily held uniformly. The "fiber length" means the length in the direction of fiber extension when observing an electron microscope photograph of the main surface of the nonwoven fabric substrate or separator. Since the fiber assembly is uniformly dispersed, it is easy to provide a separator for electrochemical elements that can hold the electrolyte uniformly and realize a power source with low internal resistance and improved output characteristics, so the fiber length is preferably 0.1 to 20 mm, more preferably 0.5 to 15 mm, and even more preferably 1 to 10 mm. Alternatively, the fiber may be continuous depending on the manufacturing method of the fiber. The "fiber length" refers to the length in the direction in which the fibers extend when observing an electron microscope photograph of the main surface of a fiber assembly or a separator for an electrochemical device.
[0029] The fiber assembly may also contain two or more types of fibers that differ in average fiber diameter and / or fiber length.
[0030] The constituent fibers of the fiber aggregate may be pulp-like fibers having fibrils, or may be fibers that do not have pulp-like fibers having fibrils. However, if the constituent fibers contain pulp-like fibers having fibrils, the pore size of the fiber aggregate will be uniform and the structure will be dense, and it will be easier to provide a separator for electrochemical elements that is excellent in preventing short circuits due to dendrites and has low internal resistance and improved output characteristics.
[0031] The fiber assembly may be subjected to a hydrophilization treatment. The method for hydrophilizing the fiber assembly may be appropriately selected, and examples of the method include subjecting the fiber assembly to a plasma treatment, a sulfonation treatment, a fluorine treatment, or a corona charging treatment.
[0032] The various configurations of the fiber assembly, such as the thickness and basis weight, are appropriately adjusted so as to obtain a separator for an electrochemical element capable of realizing a power source with low internal resistance and improved output characteristics. Weight is 3~40g / m 2 and 5 to 25 g / m 2 In the present invention, the "weight" is the weight per square meter of the main surface. 2 In the present invention, the term "principal surface" refers to the surface having the largest area. The thickness may be 5 to 60 μm, or 8 to 40 μm. The "thickness" in the present invention refers to the average value of 10 randomly selected points measured using an outside micrometer (0 to 25 mm) specified in JIS B7502, according to the measurement method of JIS C2111 5.1(1).
[0033] In the separator for electrochemical elements of the present invention, the inorganic particles mainly impart heat resistance and also serve to reduce the size of voids in the fiber assembly, thereby preventing the occurrence of internal short circuits.
[0034] The type of inorganic particles is appropriately selected. For example, SiO2 (Silica), Al 2 O 3 (alumina), alumina-silica composite oxide, TiO 2 , BaTiO 2 oxides such as aluminum nitride and silicon nitride; poorly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium sulfate; covalent crystals such as silicon and diamond; clays such as talc and montmorillonite; and substances derived from mineral resources or man-made products such as boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica.
[0035] The shape of the inorganic particles used can be appropriately selected from, for example, spherical (approximately spherical or true spherical), fibrous, needle-like, tabular, polygonal cubic, feathery, etc. It is preferable to employ spherical (approximately spherical or true spherical) inorganic particles, since the inorganic particles are uniformly present on the surface and in the voids of the fiber assembly, thereby making it possible to reduce the size of the voids in the fiber assembly and prevent the occurrence of internal short circuits, and to provide a separator for electrochemical elements having excellent heat resistance.
[0036] The average particle size of the inorganic particles that can be used in the present invention is adjusted as appropriate, but the uniform presence of the inorganic particles on the surface and in the voids of the fiber aggregate can reduce the size of the voids in the fiber aggregate to prevent the occurrence of internal short circuits, and the average particle size of the inorganic particles can be, for example, 2 μm or less, and can be 1 μm or less, so as to provide a separator for electrochemical elements that has excellent heat resistance.
[0037] The lower limit of the average particle size of the inorganic particles is adjusted as appropriate, but if the average particle size of the inorganic particles is too small, the voids in the fiber assembly are likely to be blocked by the inorganic particles, resulting in a separator for electrochemical devices with poor ion passing properties and high internal resistance. Therefore, the average particle size of the inorganic particles is preferably 0.05 μm or more, more preferably 0.1 μm or more, and most preferably 0.2 μm or more.
[0038] The average particle size of inorganic particles can be determined from particle size measurement data obtained from scattering intensity by subjecting inorganic particles to a dynamic light scattering method (measurement range: 3 nm to 5000 nm) manufactured by Otsuka Electronics Co., Ltd., and performing continuous measurement for 3 minutes. That is, particle size measurements are performed five times, and the particle size measurement data obtained by the measurements are arranged in order of narrowest particle size distribution width, and the particle size D at the 50% cumulative value point of the inorganic particles in the data showing the third narrowest particle size distribution width is determined. 50 (Hereafter, D 50 The average particle size of the inorganic particles is determined as the average particle size of the inorganic particles. The temperature of the dispersion liquid used in the measurement is adjusted to 25°C, and water at 25°C is used as a blank for the scattering intensity.
[0039] In addition, the particle size distribution of the inorganic particles is appropriately adjusted. However, when a large number of inorganic particles with a large particle size are present, the inorganic particles may fall off and pinholes may be easily formed, whereas when a large number of inorganic particles with a small particle size are present, the voids in the fiber aggregate may be easily blocked. Therefore, the particle size distribution of inorganic particles is (D 50 / 2) or more (D 50 ×2) The particle size distribution of the inorganic particles is determined from particle size measurement data obtained from scattering intensity obtained by the dynamic light scattering method described above.
[0040] In electrochemical element separators in which the percentage of the mass of inorganic particles in the mass of the electrochemical element separator is high, the inorganic particles tend to easily fall off during handling during transportation or manufacturing of the electrochemical element, and / or during use of the electrochemical element. Since an electrochemical element comprising a separator for electrochemical element from which inorganic particles have fallen off may unintentionally decrease in its charge / discharge performance and safety, the percentage of the mass of inorganic particles in the mass of the separator for electrochemical element is preferably less than 40 mass%, and preferably 36.7 mass% or less.
[0041] In the separator for electrochemical elements of the present invention, the polyvinylidene fluoride resin mainly plays a role of supporting inorganic particles on the fiber assembly. The polyvinylidene fluoride resin in the present invention is a resin having a molecular structure containing (-CH 2 -CF 2 -), an organic resin having the chemical structure. Examples of polyvinylidene fluoride resins include polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, and polyvinylidene fluoride-acrylic copolymer. In particular, polyvinylidene fluoride-acrylic copolymers have an excellent ability to support inorganic particles on a fiber assembly (for example, superior to polyvinylidene fluoride-hexafluoropropylene copolymers), and also have excellent performance in that they can maintain the ability to support inorganic particles on a fiber assembly even under high temperature conditions. Therefore, it is more preferable to adopt polyvinylidene fluoride-acrylic copolymers as polyvinylidene fluoride resins so that the separator for electrochemical elements can realize a power source with low internal resistance and improved output characteristics even under high temperature conditions.
[0042] In addition, polyvinylidene fluoride resins can function as a barrier layer that prevents the diffusion of metal ions by interacting with metal ions. As a result, it is possible to provide a separator for electrochemical elements that can be charged and discharged again even after overdischarge, maintains good cycle characteristics, and is excellent in preventing short circuits caused by dendrites. Furthermore, polyvinylidene fluoride resins have excellent heat resistance. As a result, polyvinylidene fluoride resins are unlikely to melt during the heating and drying process in the manufacturing process or during use, and it is possible to provide a separator for electrochemical elements that has excellent heat resistance.
[0043] Although polyethylene oxide is also a resin that can function as a barrier layer that prevents the diffusion of metal ions by interacting with metal ions, the melting point of polyethylene oxide is about 66°C, and is inferior in heat resistance to polyvinylidene fluoride resins that have a high melting point exceeding 100°C. Therefore, in electrochemical element separators that employ polyethylene oxide as a binder resin (particularly, electrochemical element separators that employ only polyethylene oxide as a binder resin), the polyethylene oxide melts during the heating and drying process in the manufacturing process or during use, and the structure of the electrochemical element separator is easily changed. As a result, it becomes impossible to provide a power supply with low internal resistance and improved output characteristics, and / or this causes an internal short circuit in the power supply.
[0044] Furthermore, if a solvent or dispersion medium such as water remains in the produced separator for electrochemical elements, the performance of the power source may be reduced. In order to prevent such problems from occurring, it is preferable to dry the fiber assembly or the separator for electrochemical elements at a temperature of 80° C. or higher, 90° C. or higher, and preferably 100° C. or higher, in the manufacturing process of the separator for electrochemical elements. It is preferable to use a polyvinylidene fluoride resin so that the structure of the separator for electrochemical elements is not easily changed even when the separator is subjected to such a drying process.
[0045] Furthermore, by using a polyvinylidene fluoride resin, it is possible to provide a separator for an electrochemical element having excellent high-rate characteristics. In order to more efficiently exert the above-mentioned effects, it is preferable that the inorganic particles are supported on the fiber assembly only by the polyvinylidene fluoride resin.
[0046] The method for supporting inorganic particles on a fiber assembly using a polyvinylidene fluoride resin is appropriately selected. For example, 1. A coating liquid (hereinafter sometimes referred to as coating liquid) is prepared by mixing a polyvinylidene fluoride resin and inorganic particles in a solvent or dispersion medium, and a fiber assembly is immersed in the coating liquid. 2. Spray the coating liquid onto the fiber assembly. 3. A coating liquid is applied to one or both main surfaces of the fiber assembly using a coating method such as a kiss coater method using a gravure roll. After carrying out the above steps, the fiber assembly containing the coating liquid can be dried to remove the solvent and dispersion medium in the coating liquid and to cause the inorganic particles to be supported on the constituent fibers of the fiber assembly by the polyvinylidene fluoride resin.
[0047] The method for drying the fiber assembly containing the coating liquid is appropriately selected, and examples of methods that can be used include a method of removing the solvent or dispersion medium by subjecting the fiber assembly containing the coating liquid to a heating means such as a near-infrared heater, a far-infrared heater, a halogen heater, etc., or a method of removing the solvent or dispersion medium by hot air or air blowing, etc. Also, known methods can be used, such as a method of leaving the fiber assembly containing the coating liquid at room temperature (25° C.), a method of exposing it to reduced pressure conditions, a method of exposing it to an atmosphere at a temperature at or above the temperature at which the solvent or dispersion medium can volatilize, a contact type Yankee dryer, a can dryer, etc.
[0048] In addition, when the polyvinylidene fluoride resin is present in the coating liquid in the form of a solid such as particles, the inorganic particles can be supported on the fiber assembly by the polyvinylidene fluoride resin by evaporating the water, which is the dispersion solvent, during the drying process described above. By employing a coating liquid in which a particulate polyvinylidene fluoride resin is dispersed, it is possible to prevent the voids in the fiber assembly from being blocked by the polyvinylidene fluoride resin, and it is preferable to provide a separator for electrochemical elements having better ion-permeability. In this case, the shape of the polyvinylidene fluoride resin particles dispersed and present in the coating liquid is appropriately selected, and can be appropriately selected from, for example, spherical (approximately spherical or true spherical), fibrous, needle-like, flat, polygonal cubic, and the like.
[0049] In order to prevent particles from falling off, heat above the melting point of the polyvinylidene fluoride resin may be applied, but it is preferable to adjust the heating temperature and heating time so as to prevent the voids in the fiber assembly from being blocked by the molten polyvinylidene fluoride resin.
[0050] The average particle size of the polyvinylidene fluoride resin particles present in the coating liquid is appropriately adjusted, but in order to allow the inorganic particles to be uniformly supported on the fiber assembly, the average particle size of the polyvinylidene fluoride resin particles is, for example, preferably 0.1 to 10 μm, more preferably 0.2 to 2 μm, and most preferably 0.3 to 1 μm. The average particle size of the polyvinylidene fluoride resin particles can be measured by the same method as the average particle size of the inorganic particles.
[0051] The type of the solvent or dispersion medium is appropriately selected. For example, water, alcohols, ethers, etc. can be used alone or in combination.
[0052] In order to prevent aggregation of the polyvinylidene fluoride resin and inorganic particles and improve dispersibility, for example, a surfactant (e.g., a cationic surfactant, an anionic surfactant, a nonionic surfactant, etc.) may be added to the coating liquid, and the amount added is adjusted appropriately. Furthermore, the coating liquid may contain an organic polymer other than the polyvinylidene fluoride resin as an organic polymer capable of supporting the inorganic particles on the fiber aggregate, but it is preferable that the coating liquid contains only the polyvinylidene fluoride resin as an organic polymer supporting the inorganic particles on the fiber aggregate so that the effect of preventing the inorganic particles from falling off the electrochemical element separator is efficiently exhibited.
[0053] The mass of the inorganic particles contained in the separator for electrochemical elements is adjusted as appropriate, but the greater the mass of the inorganic particles contained in the separator for electrochemical elements, the more likely it is that a separator for electrochemical elements can be provided that can realize a power source with low internal resistance and improved output characteristics even under high temperature conditions.
[0054] On the other hand, if the mass of the inorganic particles in the separator for electrochemical elements is too large, the voids in the fiber aggregate may be blocked by the inorganic particles, resulting in an unintentional increase in the Gurley value, and it may not be possible to provide a separator for electrochemical elements that can realize a power source with low internal resistance and improved output characteristics.
[0055] Therefore, the mass of inorganic particles contained in the separator for electrochemical elements is 0.5 to 40 g / m 2 and preferably 1 to 30 g / m 2 It is preferable that the thickness is 2 to 20 g / m 2 It is preferable that:
[0056] In addition, the mass of the polyvinylidene fluoride resin contained in the separator for electrochemical elements is adjusted as appropriate, but if the mass of the polyvinylidene fluoride resin in the separator for electrochemical elements is too great, the voids in the fiber assembly may be blocked by the polyvinylidene fluoride resin, unintentionally increasing the Gurley value, and it may not be possible to provide a separator for electrochemical elements that can realize a power source with low internal resistance and improved output characteristics.
[0057] On the other hand, if the mass of the polyvinylidene fluoride resin contained in the separator for electrochemical elements is too small, there is a risk that inorganic particles will fall off from the separator for electrochemical elements, and the areas where the inorganic particles have fallen off may become pinholes, which may cause an internal short circuit in the electrochemical element. Therefore, the mass of the polyvinylidene fluoride resin contained in the separator for electrochemical elements is 0.01 to 3 g / m 2 It is preferable that the thickness is 0.05 to 2.5 g / m 2 It is preferable that the thickness is 0.1 to 2 g / m 2 It is preferable that:
[0058] The various configurations of the separator for electrochemical elements, such as the thickness and basis weight, are appropriately adjusted so as to realize a power source with low internal resistance and improved output characteristics. However, if the basis weight is too low, the strength tends to be low. Therefore, the basis weight is set to 5 to 50 g / m. 2 and can be 8 to 45 g / m 2 and 10 to 40 g / m 2 The thickness is preferably from 8 to 100 μm, more preferably from 9 to 60 μm, and most preferably from 10 to 30 μm.
[0059] In order to reduce the internal resistance of the separator in the electrochemical element, it is preferable that the separator for electrochemical elements has a high liquid retention rate. The liquid retention rate of the separator for electrochemical elements is preferably 10% or more, more preferably 15% or more, even more preferably 20% or more, and even more preferably 25% or more. The liquid retention rate can be determined by the following measurement.
[0060] (Method of measuring liquid retention rate) (1) Take a circular test piece (diameter 25 mm) from the object to be measured and measure its mass (A). (2) The test piece is immersed in propylene carbonate and the voids in the test piece are filled with propylene carbonate. (3) Three sheets of filter paper (model number: ADVANTEC-TYPE2) are placed on each of the two main surfaces of the test specimen, and the test specimen is compressed at a pressure of 2.1 MPa while still sandwiched between the filter papers, and the propylene carbonate contained in the test specimen is absorbed by the filter papers. (4) Measure the mass (B) of the test piece after the propylene carbonate has been absorbed, and calculate the liquid retention rate (R, unit: %) using the following formula. R = 100 × (BA) / A It should be noted that a higher value (unit: %) means that the separator for electrochemical elements has better liquid retention properties.
[0061] The porosity of the separator for electrochemical elements is appropriately selected, but in order to realize a power source with low internal resistance and improved output characteristics, the porosity is preferably 20% or more, more preferably 30% or more, and even more preferably 40% or more. On the other hand, if the porosity is too high, the strength decreases and the separator for electrochemical elements becomes more susceptible to cracking, so a porosity of 80% or less is practical. In the present invention, the "void ratio" refers to a value obtained by the following formula. Porosity={1-W / (T×d)}×100 Here, W is the basis weight of the object to be measured (g / m 2 ), T is the thickness of the object to be measured (μm), and d is the mass average density (g / cm 3For example, if there is a part by mass of resin A with density d1 and b parts by mass of inorganic component B with density d2, the mass average density (d) can be calculated by the following formula: Mass average density (d)=1 / {(a / 100 / d1)+(b / 100 / d2)}
[0062] The maximum pore size and average pore size of the separator for electrochemical elements are appropriately selected, but in order to realize a power source with low internal resistance and improved output characteristics, the maximum pore size is preferably 0.5 to 50 μm, more preferably 0.8 to 20 μm, and more preferably 1 to 10 μm, and the average pore size is preferably 0.1 to 5 μm, and more preferably 0.2 to 3 μm. In the present invention, the average pore size refers to the average flow pore size measured by the bubble point method, and the maximum pore size refers to the maximum flow pore size measured by the same method as described above. The average flow pore size and the maximum flow pore size can be measured using a porometer (manufactured by Coulter).
[0063] The separator for an electrochemical element of the present invention is characterized in that the Gurley value is higher than 6 sec / 100 cc and lower than 44 sec / 100 cc. The applicant of the present application has discovered that in a separator for electrochemical elements comprising "a polyvinylidene fluoride resin, inorganic particles, and a fiber assembly, in which the inorganic particles are supported on the fiber assembly by the polyvinylidene fluoride resin," when the Gurley value of the separator for electrochemical elements is within the above-mentioned range, the ion passing characteristics are improved overall.
[0064] The Gurley value range of the separator for electrochemical elements according to the present invention can be appropriately adjusted within the above-mentioned range depending on the properties required for the electrochemical element, but can be 7 to 40 seconds / 100 cc, or 8 to 35 seconds / 100 cc. In the present invention, the Gurley value is a value calculated by taking a test piece from a separator for electrochemical elements and subjecting it to the method specified in "JIS P8117:2009 (Paper and paperboard-Determination method for air permeability and air resistance (intermediate range)-Gurley method) 5 Gurley tester method."
[0065] The above-mentioned separator for electrochemical elements can be used alone, but if necessary, a sheet-like substrate such as a film or fabric may be laminated on the separator for electrochemical elements. The method for laminating the separator for electrochemical elements and the substrate can be appropriately selected, but a method of simply stacking them, a method of partially melt-bonding the components of the separator for electrochemical elements and / or the substrate, or a method of laminating and integrating them with a binder can be adopted.
[0066] The separator for electrochemical elements or the laminate of separators for electrochemical elements produced as described above may be subjected to a pressure treatment such as a reliant press treatment to adjust the thickness, a hydrophilization treatment such as a sulfonation treatment, a plasma treatment, or a fluorine gas treatment, or may be subjected to various secondary processes such as punching out a shape or molding, depending on the application or mode of use.
[0067] The separator for electrochemical elements of the present invention can be used as a separator for electrochemical elements, for example, primary batteries (e.g., lithium batteries, manganese batteries, magnesium batteries, etc.), secondary batteries (e.g., lithium ion batteries, nickel hydrogen batteries, nickel cadmium batteries, zinc batteries, air batteries, all-solid-state batteries, redox flow batteries, etc.), capacitors, etc., regardless of whether they are aqueous or non-aqueous. The shape of the separator for electrochemical elements can be appropriately adjusted, for example, to a flat plate shape or a wound shape, depending on the application.
[0068] When the separator for electrochemical elements of the present invention is used as a separator for a lithium ion secondary battery, for example, a positive electrode can be used in which a current collector is supported with a slurry of a lithium or sodium-containing transition metal compound or a sulfur-based compound, and a negative electrode can be used in which a current collector is supported with a material that can be alloyed with lithium metal or lithium (for example, a tin-based alloy, a silicon-based alloy, or the like), a polyacene capable of absorbing and releasing lithium, a carbon material (for example, carbon, natural graphite, artificial graphite, or the like), a vanadium-based compound, or a lithium titanate-based compound, and a non-aqueous electrolyte (for example, a mixed solvent of ethylene carbonate and diethyl carbonate containing LiPF 6 The cell structure that can be prepared is also appropriately selected, and may be, for example, a cylindrical type, a square type, a coin type, or the like. EXAMPLES
[0069] The present invention will be specifically described below with reference to examples, but the scope of the present invention is not limited thereto.
[0070] (Preparation of nonwoven fabric A) The following fibers were dispersed in water to prepare a fiber dispersion. Pulp-like fully aromatic polyamide fiber with fibrils (freeness: 80mlCSF, decomposition temperature: approx. 500℃) Polyethylene terephthalate unstretched short fiber (fiber diameter: 4 μm, melting point: 260°C, cross-sectional shape: circular) Polyethylene terephthalate short fiber (fiber diameter 2μm, melting point: 260℃, cross-sectional shape: circular) After the fiber dispersion was drawn up, the water, which was the dispersion medium, was removed by suction to form a fiber web. The fiber web was then passed between heat rolls to be heated and pressurized, and the fibers were bonded by polyethylene terephthalate unstretched short fibers to form a single-layered nonwoven fabric A (basis weight: 10.8 g / m 2 ) was prepared.
[0071] (Preparation of nonwoven fabric A1) A single-layered nonwoven fabric A1 (basis weight: 6.0 g / m) was prepared in the same manner as described above in (Preparation of nonwoven fabric A), except that the amount of fiber dispersion to be woven was changed. 2 ) was prepared.
[0072] (Preparation of Nonwoven Fabric B) The following fibers were dispersed in water to prepare a fiber dispersion. Pulp-like fully aromatic polyamide fiber with fibrils (freeness: 80mlCSF, decomposition temperature: approx. 500℃) Polyethylene terephthalate unstretched short fiber (fiber diameter: 4 μm, melting point: 260°C, cross-sectional shape: circular) A single-layered nonwoven fabric B (basis weight: 12.0 g / m) was prepared in the same manner as described above in (Preparation of nonwoven fabric A), except that the fiber dispersion thus prepared was used. 2 ) was prepared. (Preparation of Nonwoven Fabric C) The following fibers were dispersed in water in a blending ratio different from that used in the preparation of nonwoven fabric B to prepare a fiber dispersion. Pulp-like fully aromatic polyamide fiber with fibrils (freeness: 80mlCSF, decomposition temperature: approx. 500℃) Polyethylene terephthalate unstretched short fiber (fiber diameter: 4 μm, melting point: 260°C, cross-sectional shape: circular) After the fiber dispersion was spread onto one main surface of the nonwoven fabric A1, the water, which was the dispersion medium, was removed by suction to form a laminate having a fiber web on one main surface of the nonwoven fabric A1, and the laminate was then dried. After that, the fabric is heated and pressurized through heat rolls, and the fibers are bonded with unstretched polyethylene terephthalate short fibers to form a two-layered nonwoven fabric C (basis weight: 10.8 g / m 2 ) was prepared. The two-layer nonwoven fabric C prepared in this manner had a structure in which short fibers and / or pulp-like fibers having fibrils that had been woven onto one main surface of nonwoven fabric A1 had penetrated into the voids in the fiber layer derived from nonwoven fabric A1.
[0073] (Preparation of Nonwoven Fabric D) A wet-laid nonwoven fabric (basis weight: 5.5 g / m) consisting of polyethylene terephthalate unstretched short fibers (fiber diameter: 4 μm, melting point: 260°C, cross-sectional shape: circular) and stretched short fibers (fiber diameter: 2 μm, melting point: 260°C, cross-sectional shape: circular) was used. 2 ) was prepared. The following fibers were dispersed in water to prepare a fiber dispersion. Pulp-like fully aromatic polyamide fiber with fibrils (freeness: 80mlCSF, decomposition temperature: approx. 500℃) Polyethylene terephthalate unstretched short fiber (fiber diameter: 4 μm, melting point: 260°C, cross-sectional shape: circular) After the fiber dispersion was spread onto one main surface of a wetlaid nonwoven fabric, the water, which was the dispersion medium, was removed by suction to form a laminate having a fiber web on one main surface of the wetlaid nonwoven fabric, and the laminate was then dried. Then, the fabric is heated and pressurized through heat rolls, and the fibers are bonded with polyethylene terephthalate unstretched short fibers to form a two-layered nonwoven fabric D (basis weight: 10.0 g / m 2 ) was prepared. The two-layer nonwoven fabric D prepared in this manner had a structure in which short fibers and / or pulp-like fibers having fibrils that had been woven onto one main surface of the wetlaid nonwoven fabric had penetrated into the voids in the fiber layer derived from the wetlaid nonwoven fabric.
[0074] (Preparation of Nonwoven Fabric D1, Nonwoven Fabric D2, and Nonwoven Fabric D3) A two-layered nonwoven fabric D1 (basis weight: 9.5 g / m) was prepared in the same manner as described above in (Preparation of nonwoven fabric D), except that the amount of fiber dispersion to be woven was changed. 2 ) and nonwoven fabric D2 (weight: 8.3 g / m 2 ) and nonwoven fabric D3 (weight: 10.5 g / m 2 ) was prepared. Each of the two-layer nonwoven fabrics prepared in this manner had a structure in which short fibers and / or pulp-like fibers having fibrils that had been woven onto one main surface of the wetlaid nonwoven fabric had penetrated into the voids in the fiber layer derived from the wetlaid nonwoven fabric.
[0075] (Preparation of Nonwoven Fabric E) Another wet-laid nonwoven fabric (basis weight: 7.5 g / m) was made of polyethylene terephthalate unstretched staple fibers (fiber diameter: 4 μm, melting point: 260°C, cross-sectional shape: circular) and stretched staple fibers (fiber diameter: 2 μm, melting point: 260°C, cross-sectional shape: circular). 2 ) was prepared, and this was designated as single-layer nonwoven fabric E.
[0076] (Preparation of Dispersion A) A silica particle dispersion (shape: spherical, particle diameter: 450 nm, solvent: water, solid content: 45% by mass) was prepared. Polyvinylidene fluoride-acrylic copolymer particles (particle diameter: 250 nm, melting point: 165° C.) were dispersed in the silica particle dispersion to prepare dispersion A. The solid mass ratio of the silica particles to the polyvinylidene fluoride-acrylic copolymer particles contained in the dispersion A prepared in this manner was 92 parts by mass:8 parts by mass.
[0077] (Preparation of Dispersion B) A silica particle dispersion (particle diameter: 450 nm, solvent: water, solid content: 45% by mass) was prepared. Polyethylene oxide powder (melting point: 66° C.) was dissolved in the silica particle dispersion to prepare dispersion B. The solid mass ratio of the silica particles to the polyethylene oxide particles contained in the dispersion B thus prepared was 97 parts by mass:3 parts by mass.
[0078] (Examples 1 to 5, Comparative Examples 1 to 4) Using a gravure roll coater, dispersion A was applied to one of the principal surfaces of nonwoven fabrics A to E. For two-layered nonwoven fabrics C and D, and nonwoven fabrics D1 and D2, dispersion A was applied to the principal surface on the side where the amount of pulp-like wholly aromatic polyamide fibers was small (the side opposite to the side where the fiber dispersion was papered up). Thereafter, the dispersion medium contained in the dispersion liquid A was removed by subjecting the dispersion liquid A to a dryer with the heating temperature adjusted to 100°C, and silica particles were supported on the surface of each of the constituent fibers of the nonwoven fabrics A to E by a polyvinylidene fluoride-acrylic copolymer, thereby preparing separators for various electrochemical elements.
[0079] Comparative Example 5 Dispersion B was applied to the main surface of the nonwoven fabric D3 on the side where the amount of pulp-like wholly aromatic polyamide fibers was small (the side opposite to the side where the fiber dispersion was papered) using a gravure roll coater. The nonwoven fabric D3 was then subjected to a dryer with a heating temperature adjusted to 100° C. to remove the dispersion medium contained in dispersion B, and the polyethylene oxide particles were used to support silica particles on the surfaces of the fibers that constitute the nonwoven fabric D3, thereby preparing a separator for an electrochemical device.
[0080] The configurations of the separators for electrochemical elements of the Examples and Comparative Examples produced as described above, as well as the various physical properties evaluated by the measurements described below, are summarized in Table 1.
[0081] (Measuring method for 50% SOC INPUT and 50% SOC OUTPUT) LiNi0.5Co0.2Mn0.3O 2 A flat positive electrode made of natural graphite, a flat negative electrode made of natural graphite, and an electrolyte solution made of LiPF6ED (concentration: 1M) and diethyl carbonate mixed in an equivalent volume ratio were prepared. Then, the measurement object was laminated on one main surface of the flat positive electrode, and the main surface of the flat negative electrode was contacted and laminated on the exposed main surface of the measurement object. In this way, a 45mAh laminate cell type lithium ion secondary battery was produced. (1) Check the battery capacity The lithium-ion secondary battery under test was charged and discharged at a current value of 0.1 CA. The battery capacity of the lithium-ion secondary battery was calculated and confirmed through its behavior in the output voltage range of 2.0 V to 4.2 V during charging and discharging. (2) Check the open circuit voltage at 50% SOC The actual charging time required to charge the lithium-ion secondary battery to 10% of the confirmed battery capacity at a current value of 0.1 CA was confirmed. Based on the charging time calculated from the actual charging time, the battery was charged to 50% and left for 1 hour, after which the battery voltage of the lithium-ion secondary battery was confirmed. The battery voltage measured at this time was defined as the "open circuit voltage at 50% SOC" of the lithium-ion secondary battery. (3) 50% SOC input measurement After checking the "open circuit voltage at 50% SOC," the lithium-ion secondary battery (a lithium-ion secondary battery charged to 50%) was charged and discharged as follows. (i) The lithium ion secondary battery was discharged at a current value of 0.1 CA until the discharge voltage of the battery decreased to 2.0 V. (ii) The battery was charged at a current of 0.1 CA until the battery voltage reached the "open circuit voltage at 50% SOC," and then charged at a current of 0.5 CA for 10 seconds. (iii) The battery was discharged at a current value of 0.1 CA until the battery voltage reached the "open circuit voltage at 50% SOC," and then charged at a current value of 1.0 CA for 10 seconds. (iv) The battery was discharged at a current value of 0.1 CA until the battery voltage reached the "open circuit voltage at 50% SOC," and then charged at a current value of 2.0 CA for 10 seconds. (v) The battery was discharged at a current value of 0.1 CA until the battery voltage reached the "open circuit voltage at 50% SOC," and then charged at a current value of 5.0 CA for 10 seconds. The slope of the straight line formed by plotting each of the charging current values (ii) to (v) above on the X-axis and the voltage value 10 seconds after charging on the Y-axis was taken as "50% SOC INPUT" (unit: Ω). Note that a lower 50% SOC INPUT value (unit: Ω) means that the separator for electrochemical elements has a lower internal resistance. (4) Output measurement at 50% SOC After checking the "open circuit voltage at 50% SOC," the lithium-ion secondary battery (a lithium-ion secondary battery charged to 50%) was charged and discharged as follows. (i) The lithium ion secondary battery was discharged at a current value of 0.1 CA until the discharge voltage of the battery decreased to 2.0 V. (ii) The battery was charged at a current of 0.1 CA until the battery voltage reached the "open circuit voltage at 50% SOC," and then discharged at a current of 0.5 CA for 10 seconds. (iii) The battery was charged at a current of 0.1 CA until the battery voltage reached the "open circuit voltage at 50% SOC," and then discharged at a current of 1.0 CA for 10 seconds. (iv) The battery was charged at a current of 0.1 CA until the battery voltage reached the "open circuit voltage at 50% SOC," and then discharged at a current of 2.0 CA for 10 seconds. (v) The battery was charged at a current of 0.1 CA until the battery voltage reached the "open circuit voltage at 50% SOC," and then discharged at a current of 5.0 CA for 10 seconds. The slope of the straight line formed by plotting the above-mentioned (ii) to (v) discharge current values on the X-axis and the voltage value 10 seconds after discharge on the Y-axis was taken as "50% SOC OUTPUT" (unit: Ω). Note that a lower 50% SOC OUTPUT value (unit: Ω) indicates a separator for electrochemical elements with a lower internal resistance.
[0082] [Table 1]
[0083] Compared with the separators for electrochemical elements of Comparative Example 3 with a Gurley value of 44 sec / 100cc and Comparative Example 4 with a Gurley value of 194 sec / 100cc, the separators for electrochemical elements of the Examples with a Gurley value of less than 44 sec / 100cc both had lower 50% SOC INPUT and 50% SOC OUTPUT values. Therefore, it was found that the separators for electrochemical elements according to the present invention have a Gurley value of less than 44 sec / 100cc, and thus have lower internal resistance.
[0084] On the other hand, compared to the separators for electrochemical elements of Comparative Example 1 with a Gurley value of 1 sec / 100cc and Comparative Example 2 with a Gurley value of 6 sec / 100cc, the separators for electrochemical elements of the Examples satisfying the configuration of the present invention all had low 50% SOC INPUT and 50% SOC OUTPUT values despite their high Gurley values. This was thought to be because the separators for electrochemical elements of the present invention had a higher liquid retention rate than the separators for electrochemical elements of Comparative Examples 1 and 2, and therefore had superior ion permeability. Therefore, it was found that the separators for electrochemical elements according to the present invention had a Gurley value higher than 6 sec / 100cc, and therefore had lower internal resistance.
[0085] From the above, a separator for an electrochemical element that satisfies the configuration of the present invention can realize a power source with low internal resistance and improved output characteristics.
[0086] Furthermore, since the separators for electrochemical elements of the examples had a sufficiently small difference between the measured values at 50% SOC INPUT and 50% SOC OUTPUT, the separators for electrochemical elements satisfying the configuration of the present invention were separators for electrochemical elements that could be charged and discharged again even after overdischarge and could realize a power source with excellent cycle characteristics. Furthermore, in all of the separators for electrochemical elements in the examples, the inorganic particles were unlikely to fall off. Therefore, by using a separator for electrochemical elements satisfying the configuration of the present invention, it is possible to provide an electrochemical element in which the charge / discharge performance and safety are unlikely to be unintentionally deteriorated. [Industrial Applicability]
[0087] The separator for electrochemical devices of the present invention can provide electrochemical devices with high energy density, such as lithium ion secondary batteries and capacitors.
Claims
[Claim 1] A separator for an electrochemical element comprising a polyvinylidene fluoride resin, inorganic particles, and a fiber assembly, The fibers constituting the fiber assembly are only fibers composed of organic polymers, the inorganic particles are supported on the fiber assembly by the polyvinylidene fluoride resin; A separator for an electrochemical element, having a Gurley value of 8 seconds / 100 cc or more and 35 seconds / 100 cc or less (excluding those in which the fiber aggregate contains conductive fibers and those in which the inorganic particles are conductive particles).
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery
JP2016213133A
Separator for nonaqueous secondary batteries, and nonaqueous secondary battery
WO2014147888A1