Polishing body and wafer polishing method

The polishing body with symmetrically inclined voids addresses the inefficiencies and damage issues in wafer polishing, achieving high efficiency and quality standards while reducing environmental impact.

JP7595498B2Active Publication Date: 2024-12-06NORITAKE MACHINE TECHNO CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021051298
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-25
Publication Date
2024-12-06
Estimated Expiration
2041-03-25

AI Technical Summary

Technical Problem

Existing wafer polishing methods, particularly in the CMP process, fail to meet high quality requirements for scratch-free and distortion-free surfaces, with uneven damage and local distortion occurring when using abrasive particles, and inefficiencies in polishing efficiency and surface roughness.

Method used

A polishing body made of resin with a base material containing pores and abrasive particles, featuring voids that are symmetrically inclined around a central axis, ensuring equal distances and angles of intersection with the axis, promoting uniform polishing across all directions.

Benefits of technology

The polishing body achieves high polishing efficiency and excellent surface roughness, meeting stringent quality requirements while reducing scratches and directional abrasion, and allows reuse of polishing liquid, thereby lowering manufacturing costs and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595498000002
    Figure 0007595498000002
  • Figure 0007595498000003
    Figure 0007595498000003
  • Figure 0007595498000004
    Figure 0007595498000004
Patent Text Reader

Abstract

To provide a polishing body that provides a processed wafer capable of meeting high quality requirements.SOLUTION: A polishing body 41 of the present invention is used in a wafer polishing device including a machine platen 7 and a carrier 5. The machine platen 7 has a first fixation surface 7b extending in a direction orthogonal to a first shaft center O1 and rotates around the first shaft center O1. The carrier 5 has a second fixation surface 5a extending in a direction orthogonal to a second shaft center O2 parallel with the first shaft center O1 and facing the first fixation surface 7b, and rotates around the second shaft center O2. A tabular wafer 1 is fixed to the second fixation surface 5a. The polishing body 41 has a front surface 41a, a rear surface 41a, and numerous voids 37 that are recesses in the front surface 41a and the rear surface 41b. Each of the voids 37 is near the first shaft center O1 in the surface and away from the first shaft center O1 in the rear surface 41b, around the first shaft center O1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing body and ,cormorant The present invention relates to a wafer polishing method. [Background technology]

[0002] A wafer polishing apparatus including a base plate and a carrier is known. The base plate has a first fixed surface extending in a direction perpendicular to a first axis, and is rotated about the first axis. The carrier has a second fixed surface extending in a direction perpendicular to a second axis parallel to the first axis, facing the first fixed surface, and is rotated about the second axis. The polishing body has a first surface fixed to the first fixed surface, and a second surface facing in the opposite direction to the first surface and spaced apart from the first surface in the thickness direction.

[0003] When using this wafer polishing apparatus to polish flat wafers such as SiC and GaN, a first surface of the polishing body is fixed to a first fixing surface of the surface plate, and the flat wafer is fixed to a second fixing surface of the carrier. Then, the surface plate and the carrier are rotated while the polishing body and the wafer are brought into contact with each other under a predetermined surface pressure in the presence of a polishing liquid.

[0004] When the polishing body is made of a general nonwoven fabric or hard urethane, the polishing liquid contains abrasive particles. Also, as disclosed in Patent Documents 1 to 3, when the polishing body is made of resin and has a base material with a plurality of pores formed therein and abrasive particles held in the base material or the pores, a polishing liquid that does not contain abrasive particles can be used. In this way, the wafer is polished. When the polishing liquid contains a chemical such as an alkali, the wafer is polished in a CMP (Chemical Mechanical Polishing) process. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 4266579 [Patent Document 2] Patent No. 5511266 [Patent Document 3] Patent No. 6636634 Summary of the Invention [Problem to be solved by the invention]

[0006] However, as the performance of devices using semiconductors has improved in recent years, the quality requirements for processed wafers have become stricter.

[0007] In particular, in the CMP process, which is the finishing process for wafer processing, there is a need to eliminate internal distortion in addition to being scratch-free. It has also been found that when wafers are polished using a free abrasive method in which the polishing liquid contains abrasive particles, the damage to the wafer surface is uneven, and distortion remains locally. In addition to preventing wafer damage, high polishing efficiency and excellent surface roughness are also required.

[0008] The present invention has been made in consideration of the above-mentioned conventional circumstances, and has as its object to provide a polishing body that can provide a polishing wafer that meets high quality requirements such as scratch-free after processing. , Books The problem to be solved by the invention is to provide such a wafer polishing method. [Means for solving the problem]

[0009] The polishing body of the present invention is a polishing body used in a wafer polishing apparatus, comprising: a base having a first fixing surface extending in a direction perpendicular to a first axis and rotated about the first axis; and a carrier having a second fixing surface extending in a direction perpendicular to a second axis parallel to the first axis and facing the first fixing surface, the carrier being rotated about the second axis, the carrier having a second fixing surface extending in a direction perpendicular to a second axis parallel to the first axis and facing the first fixing surface, the carrier comprising: The polishing body includes a base material made of resin and having a plurality of pores formed therein, and abrasive particles held in the base material or the pores, a first surface fixed to the first fixing surface, a second surface facing away from the first surface and spaced apart from the first surface in a thickness direction; , which communicates the first surface and the second surface With countless voids, If the distances of the voids to the first axis are equal, the angles of the voids intersecting the first axis are equal, Each of the voids is disposed around the first axis such that one of the first surface and the second surface is closer to the first axis and the other of the first surface and the second surface is farther from the first axis. And, The angle between the void that exists at a position that is closer to the center line that coincides with the first axis and the center line is larger than the angle between the void that exists at a position that is farther from the center line and the center line. It is characterized by:

[0010] The inventors have confirmed that if the polishing body of the present invention is used to polish a wafer by the above-mentioned wafer polishing apparatus, scratches are unlikely to occur, and the wafer can be polished with high polishing efficiency and excellent surface roughness.

[0011] In other words, according to the inventor's tests, in a wafer polishing apparatus in which the platen rotates about a first axis and the carrier rotates about a second axis, if a polishing body such as a typical nonwoven fabric or hard urethane is used, the polishing body cannot polish the wafer efficiently, and scratches are likely to occur on the polished wafer.

[0012] On the other hand, when a polishing body having numerous voids is used, the voids can polish the wafer with a certain degree of efficiency. However, in conventional polishing bodies, the voids are inclined in one direction, so that the wafer is easily worn in a specific direction around the second axis and is not easily worn in another specific direction. For this reason, the surface roughness is poor and the polishing efficiency is still insufficient.

[0013] In contrast, when the polishing body of the present invention is used, each void exists around the first axis, and each void is closer to the first axis on one of the first surface and the second surface, and is farther away from the first axis on the other of the first surface and the second surface. Therefore, the wafer is easily worn in all directions around the second axis. Therefore, in this case, the wafer can be polished with high polishing efficiency and excellent surface roughness.

[0014] Therefore, if the polishing body of the present invention is used in the above-mentioned wafer polishing apparatus, the processed wafers can meet the high quality requirements.

[0015] If the distances of the voids from the first axis are equal, it is preferable that the angles at which the voids intersect with the first axis are equal. In this case, the reproducibility of the polishing efficiency and the like depending on the polishing conditions is excellent. It is considered that the wafer is polished with the same polishing force by the voids at the same distances from the first axis contacting the wafer at the same angle.

[0016] The polishing body is preferably made of resin and has a base material with a plurality of pores formed therein and abrasive particles held in the base material or the pores. The inventor has confirmed the effects of the present invention with this polishing body. In this case, since a polishing liquid that does not have abrasive particles can be used, the polishing liquid can be easily reused, and the manufacturing cost of semiconductor devices can be reduced, while the environmental load can be reduced.

[0017] The method for producing an abrasive body of the present invention includes a first step of preparing a paste containing a base resin, abrasive particles, and a solvent; A second step of forming the paste into a sheet-like molded body; and a third step of immersing the molded body in a replacement liquid to replace the solvent in the molded body with the replacement liquid to form numerous voids. The third step is characterized in that the molded body is immersed horizontally in the replacement liquid.

[0018] The inventors discovered that when the molded body is immersed horizontally in the replacement liquid as in the third step, the voids are inclined symmetrically around the first axis.

[0019] Therefore, by the manufacturing method of the present invention, it is possible to produce an abrasive body of the present invention which has a base material made of resin and having a plurality of pores formed therein, abrasive particles held in the base material or the pores, and a plurality of voids inclined symmetrically about the first axis.

[0020] The wafer polishing method of the present invention is a method of polishing a wafer by contacting a flat wafer and a flat polishing body under a predetermined surface pressure in the presence of a polishing liquid, the method comprising the steps of: 2The wafer is rotated around an axis, and the polishing body extends in a thickness direction. 2 Parallel to the axis 1 A wafer polishing method for polishing a wafer by rotating the polishing body around an axis, comprising: The polishing body includes a base material made of resin and having a plurality of pores formed therein, and abrasive particles held in the base material or the pores, The polishing body has a first surface and an opposite surface to the first surface. and spaced apart from the first surface in a thickness direction. a second surface; and a recessed portion formed from the first surface and the second surface. , which communicates the first surface and the second surface With countless voids, If the distances of the voids to the first axis are equal, the angles of the voids intersecting the first axis are equal, Each of the voids is closer to the first axis on one of the first surface and the second surface and is farther from the first axis on the other of the first surface and the second surface, around the first axis; The angle formed between the void located at a short distance from the center line coinciding with the first axis and the center line is larger than the angle formed between the void located at a long distance from the center line and the center line.

[0021] Since the wafer polishing method of the present invention uses the polishing body of the present invention, the processed wafers can meet high quality requirements. Effect of the Invention

[0022] By using the polishing body of the present invention, the processed wafer can meet the high quality requirements. Books The wafer polishing method of the invention ensures that the processed wafers meet high quality requirements. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 is a schematic enlarged cross-sectional view of the polishing pad obtained by the manufacturing method of Examples 1 and 2. [Diagram 2] FIG. 2 is a schematic enlarged cross-sectional view of the polishing pad obtained by the manufacturing method of Comparative Example 1. [Diagram 3]FIG. 3 is a graph showing the relationship between the distance from the center line and the angle each void makes with the center line in the polishing pads obtained by the manufacturing methods of Examples 1 and 2. [Figure 4] FIG. 4 is a schematic cross-sectional view of a wafer polishing apparatus used in the wafer polishing method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The base resin used to manufacture the polishing body may be polyethersulfone (PES), polyvinylidene fluoride (PVDF), polyvinyl fluoride, vinyl fluoride-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, polyethylene, polymethyl methacrylate, etc. These may be used alone or in a mixture of two or more.

[0025] As a solvent used for manufacturing the polishing body, dimethylformamide, dimethylsulfoxide, acetone, ethyl acetate, methyl ethyl ketone, etc. can be used. These may be used alone or in combination of two or more. The solvent is selected according to the binder resin.

[0026] As abrasive particles that can be used to manufacture the polishing body or that can be contained in the polishing liquid, silica, ceria, alumina, zirconia, titania, diamond, manganese oxide, barium carbonate, chromium oxide, iron oxide, etc. These may be used alone or in a mixture of two or more kinds.

[0027] The paste used to manufacture the polishing body may contain alkaline fine particles such as sodium carbonate, piperazine, potassium hydroxide, sodium hydroxide, calcium oxide, potassium carbonate, and magnesium oxide, in addition to the base resin, the polishing particles, and the solvent. The paste may also contain a water repellent such as a fluorine-based water repellent, a silicon-based water repellent, a hydrocarbon-based water repellent, and a metal compound-based water repellent. Furthermore, the paste may contain a pigment such as an inorganic pigment such as titanium dioxide, calcium carbonate, or carbon black, or an organic pigment such as an azo pigment or a polycyclic pigment. These may be used alone or in a mixture of two or more types.

[0028] In the method for manufacturing an abrasive body, when an oil-based solvent is used, a water-based liquid such as tap water can be used as the replacement liquid to replace the solvent.

[0029] When a polishing liquid is used, the polishing liquid may be pure water, may be oil-based, or may contain an acidic or alkaline chemical.

[0030] (Examples and Comparative Examples) Examples 1 and 2 embodying the present invention and Comparative Example 1 will be described below.

[0031] First, in the first step, the following base resin, abrasive particles, and solvent were prepared. (Base resin) PES (Polyethersulfone) (abrasive particles) Silica (SiO2) (average particle size: 0.3 μm) (solvent) NMP (N-methyl-2-pyrrolidone)

[0032] These were mixed at 20% by volume of base resin, 25% by volume of abrasive particles, and 55% by volume of solvent to obtain pastes of Examples 1 and 2 and Comparative Example 1.

[0033] In the second step, the paste obtained in the first step is molded into a sheet-like molded body using a molding device such as a T-die. The molding method is not limited to this as long as it can achieve a certain degree of uniformity in thickness.

[0034] In the third step, in Examples 1 and 2, the molded body was immersed horizontally in the replacement liquid, whereas in Comparative Example 1, the molded body was immersed in the replacement liquid at an angle, and after a predetermined time had elapsed, each was removed from the replacement liquid and dried.

[0035] During this time, according to the inventor's observation, the solvent in each molded body was replaced with the replacement liquid, generating voids. In the parts other than the voids, fine pores were generated. At this time, the molded body gradually shrinks due to the replacement of the solvent with the replacement liquid. For this reason, in the manufacturing methods of Examples 1 and 2, as shown in FIG. 1, each void was inclined around the central axis O so that it approached the center line O on the replacement liquid side and moved away from the center line O on the opposite side. On the other hand, in the manufacturing method of Comparative Example 1, as shown in FIG. 2, each void was inclined in one direction regardless of its orientation around the central axis O.

[0036] After a predetermined time, the molded body was pulled out from the replacement liquid. The entire solvent in the molded body was replaced by the replacement liquid and solidified, forming a solidified body. The solidified body was dried and ground to a predetermined thickness to obtain a polishing pad 41 as a polishing body having a diameter of 30 cm.

[0037] Each polishing pad 41 obtained by the manufacturing method of Examples 1 and 2 has a base material made of resin with a plurality of pores formed therein, abrasive particles held in the base material or the pores, and a plurality of voids 37 inclined symmetrically about the central axis O. Each polishing pad 41 also has a front surface 41a and a back surface 41b. One of the front surface 41a and the back surface 41b corresponds to the first surface, and the other of the front surface 41a and the back surface 41b corresponds to the second surface.

[0038] The polishing pad 41 obtained by the manufacturing method of Comparative Example 1 is similar to the polishing pad 41 obtained by the manufacturing method of Examples 1 and 2 in that it has a base material and abrasive particles, and has countless voids 37 connecting the front surface 41a and the back surface 41b.

[0039] For each polishing pad 41 obtained by the manufacturing method of Examples 1 and 2, the relationship between the distance from the center line O and the angle θ that the void 37 makes with the center line O was obtained. The results are shown in FIG. 3. As shown in FIG. 1 and FIG. 3, it can be seen that each void 37 obtained by the manufacturing method of Examples 1 and 2 is close to the center line O on the front surface 41a and far from the center line O on the back surface 21b. In addition, the angle θ1 between the void 37 present at a position with a short distance from the center line O and the center line O is larger than the angle θ2 between the void 37 present at a position with a long distance from the center line O and the center line O. Furthermore, as shown in FIG. 4, if the distance from the center line O to each void 37 is equal, the angle θ at which each void 37 intersects with the center line O is equal.

[0040] On the other hand, in each polishing pad 41 obtained by the manufacturing method of Comparative Example 1, as shown in FIG. 2, regardless of the center line O, each void 37 was inclined in one direction.

[0041] Example 1 was a case where the front surface 41a of the polishing pad 41 obtained by the manufacturing method of Examples 1 and 2 was used as the polishing surface, and Example 2 was a case where the back surface 41b of the polishing pad 41 obtained by the manufacturing method of the Example was used as the polishing surface. The polishing pad of Comparative Example 1 was obtained by the manufacturing method of Comparative Example 1. The polishing pad of Comparative Example 2 was a known one made of hard urethane (urethane pad IC1000 (manufactured by Nitta Haas)). A wafer polishing device (Engis EJW-380) was prepared, and wafer 1 was polished using the polishing pads of Examples 1 and 2 and Comparative Examples 1 and 2.

[0042] As shown in FIG. 8, the wafer polishing apparatus includes a plurality of carriers 5, a surface plate 7, a driving device 9, and a polishing liquid supplying device 11. Although FIG. 8 shows only a single carrier 5, the wafer polishing apparatus has a plurality of carriers 5. Each carrier 5 is in the shape of a horizontal disk. A second fixing surface 5a is recessed in the lower surface of each carrier 5, and a wafer 1 is fixed to the second fixing surface 5a. A carrier rotation shaft 5b protrudes vertically from the upper surface of each carrier 5. Each wafer 1 is a 4H-SiC single crystal having a diameter of 4 inches. The polished surface 1a, which is the Si surface of each wafer 1, faces downward.

[0043] The surface plate 7 is in the shape of a horizontal disk that contains all the carriers 5. A surface plate rotation shaft 7a is vertically protruding from the lower surface of the surface plate 7. The upper surface of the surface plate 7 is a first fixing surface 7b. A disk-shaped polishing pad 41 is fixed to the first fixing surface 7b with an adhesive so as to face each wafer 1. The center line O of the polishing pad 41 coincides with the first axis O1.

[0044] The driving device 9 has a main driving device 9a, a sub-driving device 9b, and a pressure device 9c. The main driving device 9a drives the base plate rotation shaft 7a to rotate around the first axis O1 at a predetermined speed. The sub-driving device 9b drives each carrier rotation shaft 5b to rotate around the second axis O2 at a predetermined speed. The pressure device 9c presses each carrier rotation shaft 5b and the sub-driving device 9b toward the base plate 7 with a predetermined load.

[0045] The polishing liquid supplying device 11 is provided above the platen 7. The polishing liquid supplying device 11 provides a polishing liquid 11a between each wafer 1 and the polishing pad 41. In the polishing methods of Examples 1 and 2 and Comparative Example 1, a polishing liquid 11a consisting of an aqueous potassium permanganate solution and not containing abrasive particles was used. In the polishing method of Comparative Example 2, a commercially available polishing liquid 11a (DSC-201 (manufactured by Fujimi Incorporated)) containing alumina as abrasive particles was used.

[0046] In this wafer polishing apparatus, each wafer 1 was polished under the following conditions. Flow rate of polishing liquid 11a: 10 mL / min Load: 30kPa Rotation speed of surface plate 7: 60 rpm Carrier 5 rotation speed: 60 rpm Processing time: 60 minutes

[0047] The polishing efficiency (μm / h), the surface roughness Sa (nm) of the polished wafer 1, and the presence or absence of scratches were evaluated. The evaluation of the polishing efficiency was ◯ if it was 1.2 μm / h or more, △ if it was 1.0 μm / h or more and less than 1.2 μm / h, and × if it was less than 1.0 μm / h. The evaluation of the surface roughness Sa was ◯ if it was 0.095 nm or less, △ if it was 0.095 nm or more and less than 0.100 nm, and × if it was less than 0.100 nm. The presence or absence of scratches was observed with a differential interference microscope, and was evaluated as ◯ if there were no scratches and × if there were scratches. For each evaluation item, ◯ was given 2 points, △ was given 1 point, and × was given 0 points, and in the overall evaluation, 5 points or more was ◯, 3 to 4 points was △, and 2 points or less was ×. The results are shown in Table 1.

[0048] [Table 1]

[0049] From Table 1, it can be seen that in a wafer polishing apparatus in which the platen 7 rotates around the first axis O1 and the carrier 5 rotates around the second axis O2, when the polishing pad of Comparative Example 2 made of general hard urethane is used, the polishing pad is unable to polish the wafer 1 efficiently and scratches are likely to occur on the wafer 1 after polishing.

[0050] On the other hand, when the polishing pad of Comparative Example 1 is used, the polishing pad has numerous voids 37, so that the wafer 1 can be polished with a certain degree of efficiency. However, in the polishing pad of Comparative Example 1, the voids 37 are inclined in one direction, so that the surface roughness is poor and the polishing efficiency is still insufficient. It is considered that a directionality occurs in which the wafer 1 is easily worn in a specific direction around the second axis O2 and is not easily worn in another specific direction.

[0051] In contrast, when the polishing pad 41 of Examples 1 and 2 is used, the wafer 1 can be polished with high polishing efficiency and excellent surface roughness. This is thought to be because, in the polishing pad 41 of Examples 1 and 2, each void 37 exists around the first axis O1, and each void 37 is close to the first axis O1 on the front surface 41a or the back surface 41b and is far from the first axis O1 on the back surface 41b or the front surface 41a, so that the wafer 1 is easily worn in all directions around the second axis O2.

[0052] Therefore, it is understood that if the polishing pad 41 of Examples 1 and 2 is used in the above-mentioned wafer polishing apparatus, the processed wafer 1 can meet the high quality requirements.

[0053] In particular, in the polishing pads 41 of Examples 1 and 2, if the distance from the first axis O is equal, the angle at which each void 37 intersects with the first axis O is equal. This provides excellent reproducibility of the polishing efficiency and other characteristics depending on the polishing conditions. It is believed that the voids 37 at the same distance from the first axis O abut against the wafer 1 at the same angle relative to the wafer 1, thereby polishing the wafer 1 with approximately the same polishing force.

[0054] Moreover, the polishing pad 41 of Examples 1 and 2 has a base material made of resin with a plurality of pores formed therein and abrasive particles held in the base material or the pores. Therefore, the polishing liquid 11a without abrasive particles can be used, so that the polishing liquid 11a can be easily reused, and the manufacturing cost of semiconductor devices can be reduced, and the environmental load can be reduced.

[0055] In the above, the present invention has been described based on Examples 1 and 2. However, the present invention is not limited to the above Examples 1 and 2, and it goes without saying that the present invention can be modified as appropriate without departing from the spirit of the present invention. [Industrial Applicability]

[0056] The present invention can be used in semiconductor manufacturing equipment. [Explanation of symbols]

[0057] O1…1st axis center 7b…First fixed surface 7…Fixed plate O2…2nd axis center 5a…Second fixed surface 5…Carrier 1...Wafer 41...Abrasive body (abrasive pad) 41a... Surface (first or second surface) 41b…Back side (2nd or 1st side) 37…Void

Claims

1. A polishing body for use in a wafer polishing apparatus, comprising: a base having a first fixing surface extending in a direction perpendicular to a first axis and rotated about the first axis; and a carrier having a second fixing surface extending in a direction perpendicular to a second axis parallel to the first axis and facing the first fixing surface, the carrier being rotated about the second axis, wherein a flat wafer is fixed to the second fixing surface, The polishing body includes a base material made of resin and having a plurality of pores formed therein, and abrasive particles held in the base material or the pores, a first surface fixed to the first fixing surface, a second surface facing away from the first surface and spaced apart from the first surface in a thickness direction, and a countless number of voids recessed from the first surface and the second surface and communicating between the first surface and the second surface; If the distances of the voids to the first axis are equal, the angles of the voids intersecting the first axis are equal, Each of the voids is closer to the first axis on one of the first surface and the second surface and is farther from the first axis on the other of the first surface and the second surface, around the first axis; A polishing body characterized in that the angle formed between the void located at a short distance from the center line coinciding with the first axis and the center line is larger than the angle formed between the void located at a long distance from the center line and the center line.

2. 1. A wafer polishing method comprising the steps of: bringing a flat wafer into contact with a flat polishing body under a predetermined surface pressure in the presence of a polishing liquid; rotating the wafer around a second axis extending in a thickness direction of the wafer; and rotating the polishing body around a first axis extending in the thickness direction of the polishing body and parallel to the second axis, The polishing body includes a base material made of resin and having a plurality of pores formed therein, and abrasive particles held in the base material or the pores, the polishing body has a first surface, a second surface facing away from the first surface and spaced apart from the first surface in a thickness direction, and a number of voids recessed from the first surface and the second surface and communicating between the first surface and the second surface; If the distances of the voids to the first axis are equal, the angles of the voids intersecting the first axis are equal, Each of the voids is closer to the first axis on one of the first surface and the second surface and is farther from the first axis on the other of the first surface and the second surface, around the first axis; A wafer polishing method, characterized in that the angle formed between the void located at a short distance from the center line coinciding with the first axis and the center line is larger than the angle formed between the void located at a long distance from the center line and the center line.

Citation Information

Patent Citations

  • Production of photo molding material for making stencil

    JP1980011266A

  • Abrasive body and manufacturing method thereof

    JP4266579B2

  • Abrasive body and method of manufacturing the same

    JP6636634B2

  • Polishing pad, and method and apparatus for producing same

    WO2005023487A1

  • Method for polishing GAN single crystal material

    WO2015152021A1