Flexible boot for constant velocity universal joint and constant velocity universal joint

The flexible boot for constant velocity universal joints, made with a specific blend of HNBR and EPDM, addresses the challenge of balancing heat and cold resistance, oil resistance, and ozone resistance, ensuring durability and performance across diverse environmental conditions.

JP7595517B2Active Publication Date: 2024-12-06NTN CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021080172
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-11
Publication Date
2024-12-06
Estimated Expiration
2041-05-11

AI Technical Summary

Technical Problem

Constant velocity universal joints in automobiles face challenges with flexible boots that require both high heat and cold resistance, as well as oil and ozone resistance, due to the inverse proportional relationship between cold and oil resistance, and the materials' performance under harsh environmental conditions.

Method used

A flexible boot for constant velocity universal joints composed of 50 to 80 parts by weight of HNBR with 15 to 21% acrylonitrile content and 20 to 50 parts by weight of EPDM, with an elastic recovery rate of 18% or more at -40°C, combined with appropriate additives, to achieve balanced cold and oil resistance and improved ozone resistance.

Benefits of technology

The solution provides flexible boots with enhanced heat, cold, oil, and ozone resistance, ensuring durability and performance under varying temperature and operational conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595517000003
    Figure 0007595517000003
  • Figure 0007595517000004
    Figure 0007595517000004
  • Figure 0007595517000005
    Figure 0007595517000005
Patent Text Reader

Abstract

To provide a flexible boot for a constant-velocity universal joint that has required heat resistance and also has sufficient levels of cold resistance, oil resistance and ozone resistance, and the constant-velocity universal joint having the boot attached thereto.SOLUTION: A flexible boot for a constant-velocity universal joint comprises attachment parts to partner members at both ends thereof, and comprises a bending part that absorbs deformation associated with operation of the constant-velocity universal joint, the bending part provided between both attachment parts. The flexible boot is composed of a rubber material comprising 50-80 pts.wt. of HNBR with an acrylonitrile quantity of 15-21 wt.% and 20-50 pts.wt. of EPDM, and includes a rubber material having an elastic recovery of 18% or greater at -40°C in a TR test.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a constant velocity universal joint and a flexible boot for a constant velocity universal joint which are incorporated in the power transmission mechanisms of automobiles and various industrial machines. [Background technology]

[0002] Boots attached to constant velocity joints on automobile drive shafts or axles and to propeller shafts that constantly rotate at high speeds require grease resistance (oil resistance), so CR (chloroprene rubber) is generally used. However, chloroprene rubber does not have sufficient dynamic ozone resistance or air heat aging resistance, so there is a problem that the boots crack over time and the grease dissipates. In particular, the tendency for temperatures to rise in the engine compartment of an automobile makes this problem even more serious. For example, constant velocity joints (also abbreviated as CVJ) installed in automobiles can be exposed to ambient temperatures of 130°C or more due to the location of use, the increase in engine power, and the compactness of the engine compartment.

[0003] Therefore, in order to meet the demand for higher heat resistance, flexible boots using HNBR (hydrogenated nitrile rubber) material are also used (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-159989 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in recent years, constant velocity universal joints mounted on automobiles are often used in harsh environments, and it is expected that flexible boots for constant velocity universal joints will be used not only at high temperatures but also at low temperatures, such as -40°C. At low temperatures, the elastic modulus of rubber decreases, which may cause problems such as adhesion to the shaft and abnormal deformation at start-up, and flexible boots for constant velocity universal joints that are excellent in not only heat resistance but also cold resistance are required. However, cold resistance and oil resistance are generally inversely proportional to each other, and there is a risk that improving cold resistance will deteriorate oil resistance.

[0006] In addition to temperature conditions and oil resistance, flexible boots for constant velocity joints are used in harsh environments where they are exposed to centrifugal forces associated with high speed rotation, large deformation due to high operating angles, flying stones, and other elements, so ozone resistance is also required to maintain excellent compliance and durability in order to withstand these conditions.

[0007] The object of the present invention is to provide a flexible boot for a constant velocity universal joint which has the heat resistance required for a constant velocity universal joint, and which also has fully satisfactory cold resistance, oil resistance and ozone resistance, and a constant velocity universal joint equipped with such a boot. [Means for solving the problem]

[0008] In order to achieve this object, the invention described in claim 1 has mounting parts for mounting to mating members at both ends, and a bent part is provided between the mounting parts to absorb deformation caused by the operation of the constant velocity universal joint. Used in automobile drive shafts and propeller shafts This flexible boot for constant velocity universal joints is made by blending 50 to 80 parts by weight of HNBR containing 15 to 21% by weight of acrylonitrile and 20 to 50 parts by weight of EPDM, and uses a rubber material with an elastic recovery rate of 18% or more at -40°C in a TR test.

[0009] Here, it is preferable that the rubber material shows 100% or less swelling in an immersion test with IRM903 oil.

[0010] Furthermore, the rubber material preferably has an elastic recovery rate of 21% or more at −40° C. in a TR test.

[0011] The present invention is also characterized by a constant velocity universal joint equipped with a flexible boot for a constant velocity universal joint according to any one of claims 1 to 3. Effect of the Invention

[0012] The flexible boot for constant velocity universal joints of the present invention is molded from a rubber material that is a blend of HNBR and EPDM containing 15 to 21% by weight of acrylonitrile, and has an elastic recovery rate of 18% or more at -40°C in the TR test, so that it maintains heat resistance while also achieving satisfactory cold resistance, oil resistance, and ozone resistance. [Brief description of the drawings]

[0013] [Figure 1] 1 is a central vertical cross-sectional view showing one embodiment of a cross groove type constant velocity universal joint and a flexible boot for the same joint to which the present invention is applied. [Diagram 2] 1 is a central vertical cross-sectional view showing an embodiment of a tripod-type constant velocity universal joint and a flexible boot for the joint to which the present invention is applied. [Diagram 3] 1 is a central vertical cross-sectional view showing an embodiment of a double offset type constant velocity universal joint and a flexible boot for the joint to which the present invention is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A flexible boot for a constant velocity universal joint and a constant velocity universal joint according to the present invention will be described in detail with reference to the following embodiments.

[0015] The flexible boot for constant velocity universal joint of the present invention is characterized in that it is molded from a rubber material having an elastic recovery rate of 18% or more at -40°C in a cold resistance test (TR test), with a base rubber material being a blend of 50 to 80 parts by weight of HNBR (hydrogenated nitrile rubber) with an acrylonitrile content of 15 to 21% by weight and 20 to 50 parts by weight of EPDM (ethylene propylene diene rubber).

[0016] HNBR is known to have excellent heat resistance (for example, Patent Document 1). It is also known that, as the amount of acrylonitrile added to HNBR increases, the oil resistance improves, but the cold resistance decreases, which is a contradictory relationship. According to the experiments of the present inventors, when the acrylonitrile content is 23 to 26% by weight, the elastic recovery rate in the TR test is 10% or less, and the cold resistance is poor and cannot be used as a boot material. On the other hand, when the acrylonitrile content is low, there is a problem that the oil resistance is reduced, and therefore, it is important for the HNBR used as a boot material to have a good balance between cold resistance and oil resistance.

[0017] For this reason, the amount of acrylonitrile in the HNBR used in the present invention is preferably in the range of 15 to 21% by weight, which provides an excellent balance between cold resistance and oil resistance.

[0018] The addition of EPDM also makes it possible to achieve both cold resistance and ozone resistance. In CVJ boot ozone durability tests, damage was confirmed in boots that did not contain EPDM, but it was found that this improved as the amount of EPDM added increased. By increasing the amount of EPDM added, ozone resistance improved, and no damage to boots was confirmed when 10 parts by weight or more of EPDM was added. Furthermore, when 20 parts by weight or more of EPDM was added, no cracks were confirmed in the boots, and ozone resistance was further improved. On the other hand, a decrease in oil resistance was observed as the amount of EPDM added increased. In other words, excessive addition of EPDM reduces oil resistance.

[0019] In addition, oil resistance can be improved by reducing the amount of EPDM blended. As a result of an immersion test in IRM903 oil, it was found that a rubber material with 50 parts by weight of EPDM blended would swell by 100% or more, while a rubber material with 40 parts by weight or less would swell by 100% or less. It has been empirically found that if the swelling in IRM903 oil is within 100%, the swelling in the grease actually sealed and used in the flexible boot for constant velocity universal joints will be within 30%, and it has been confirmed that there are no practical problems with durability, sealing properties, etc. For this reason, it is preferable for a rubber material to swell by 100% or less in an immersion test in IRM903 oil.

[0020] In other words, it was found that the ozone resistance can be improved if the amount of EPDM is 10 parts by weight or more and 50 parts by weight or less, and more preferably, the ozone resistance can be improved if the amount of EPDM is 20 parts by weight or more and 50 parts by weight or less. In particular, when the amount of EPDM is 30 to 40 parts by weight, the swelling of the rubber material is 100% or less, and it is more preferable because it can be applied under severe conditions such as high speed, high operating angle, and high temperature. In addition, the rubber material containing 50 parts by weight of EPDM did not satisfy the requirement of 100% or less swelling as a result of the experiment, but it passed the CVJ boot high temperature rotation test and the CVJ boot low temperature rotation test, and it was found that it can be used as an actual boot depending on the usage conditions of the constant velocity universal joint.

[0021] By blending EPDM, which has excellent cold resistance, with HNBR containing 15 to 21% by weight of acrylonitrile, and further blending the appropriate type and amount of additives, it is possible to satisfy the cold resistance required for a flexible boot for a constant velocity universal joint. In a flexible boot for a constant velocity universal joint using a rubber material with an elastic recovery rate of less than 18% at -40°C in the TR test (low temperature elastic recovery test), the boot mounting part slips at low temperatures, and the boot mounting part and the shaft do not come into good contact with each other, which may cause abnormal deformation or problems with sealing when the boot is started, and it is not suitable for use as a boot. On the other hand, in a flexible boot for a constant velocity universal joint using a rubber material containing 20 parts by weight or more of EPDM, which has an elastic recovery rate of 18% or more at -40°C in the TR test (low temperature elastic recovery test), slipping does not occur at the boot mounting part at low temperatures, and it has been found that it has sufficient cold resistance as a flexible boot for a constant velocity universal joint.

[0022] Here, we will explain about plasticizers and crosslinking agents. Plasticizers are generally used as rubber plasticizers or softeners, and include ester-based plasticizers such as phthalates, polyesters, phosphates, adipates, sebacates, citrates, benzoates, ethers and esters, azelates, and polyethers and thioethers, vegetable oil-based plasticizers such as rapeseed oil, castor oil, and linseed oil, epoxy-based plasticizers, petroleum-based aromatic process oils, naphthenic rubber oils, and paraffinic rubber oils.

[0023] Examples of crosslinking agents include sulfur-based crosslinking agents, thermosetting resin crosslinking agents, peroxide-based crosslinking agents, etc., which are generally used for rubber. In this test, a peroxide-based crosslinking agent was used.

[0024] Examples of peroxide-based crosslinking agents that can be used include dicumyl peroxide, di-t-butyl peroxide, t-butylcumyl peroxide, benzoyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3,2,5-dimethyl-2,5-di(benzoylperoxy)hexyne, and α,α'-bis(t-butylperoxy-m-isopropyl)benzene.

[0025] From the results of the tests conducted by the present inventors, it has been found that by using a rubber material having an elastic recovery rate of 18% or more at -40°C in a TR test, which is made of 50-80 parts by weight of HNBR having an acrylonitrile content of 15-21% by weight and 20-50 parts by weight of EPDM as a base rubber material, the flexible boot for a constant velocity universal joint can be molded with the rubber material having an elastic recovery rate of 18% or more at -40°C in a TR test, and the flexible boot for a constant velocity universal joint can have the heat resistance required for the flexible boot for a constant velocity universal joint, and can also have satisfactory cold resistance, oil resistance, and ozone resistance. In particular, when using a rubber material having an elastic recovery rate of 21% or more at -40°C in a TR test, which is made of 60-70 parts by weight of HNBR having an acrylonitrile content of 15-21% by weight and 30-40 parts by weight of EPDM, it is possible to obtain even higher oil resistance, cold resistance, and ozone resistance.

[0026] The features of the flexible boot for a constant velocity universal joint of the present invention will be described below.

[0027] [Heat resistance] Flexible boots for constant velocity universal joints are made using a rubber material that is a mixture of heat-resistant HNBR (hydrogenated nitrile rubber) with 15 to 21% by weight of acrylonitrile and EPDM (ethylene propylene diene rubber), and further contains appropriate amounts of additives. No damage was observed in high-temperature CVJ boot rotation tests, and the flexible boots for constant velocity universal joints have sufficient heat resistance.

[0028] [About cold resistance] If a rubber material made by blending HNBR with 15-21% by weight of acrylonitrile with EPDM and appropriate additives has an elastic recovery rate of 18% or more at -40°C in a TR test, then there will be no problems in the CVJ boot low-temperature rotation test of a flexible boot for a constant velocity universal joint using this rubber material, and it will have sufficient cold resistance. On the other hand, in the CVJ boot low-temperature rotation test of a flexible boot for a constant velocity universal joint using a rubber material with an elastic recovery rate of less than 18%, slippage will occur at the boot mounting part, and the boot mounting part and the shaft will not come into good contact at low temperatures, which may cause abnormal deformation or problems with sealing when the boot starts, making it unsuitable for use as a boot.

[0029] [Oil resistance] Rubber materials made by blending HNBR with 15-21% by weight of acrylonitrile, 0-40% by weight of EPDM, and appropriate additives in appropriate amounts swell less than 100% in an immersion test with IRM903 oil, and have high oil resistance. Flexible boots for constant velocity universal joints made of rubber materials with swelling less than 100% have little swelling or loss in hardness due to grease, and have little abnormal wear due to deformation or contact when the joint has a high working angle or at high speed rotation, and have sufficient durability. On the other hand, those made with 50 parts by weight of EPDM swell more than 100%, and flexible boots for constant velocity universal joints made of such rubber materials have the risk of abnormal wear due to contact with other parts of the boot when the joint has a high working angle, or abnormal deformation and breakage at high speed rotation. However, they can be used for constant velocity universal joints that do not have a high working angle or are used for low speed rotation.

[0030] [Ozone resistance] In an ozone durability test using a flexible boot for constant velocity joints, damage to the boot was confirmed when HNBR was used alone. By increasing the amount of EPDM blended, ozone resistance was improved, and no damage to the boot was confirmed when 10 parts by weight or more of EPDM was blended. When 20 parts by weight or more of EPDM was blended, no cracks were confirmed in the boot, and ozone resistance was further improved.

[0031] The rubber material according to the above-described embodiment satisfies the requirements for heat resistance, cold resistance, oil resistance and ozone resistance, and is therefore suitable for flexible boots for constant velocity universal joints.

[0032] Here, the constant velocity universal joint is not limited to a specific joint structure and can take any form. For example, it is not limited to a sliding type constant velocity universal joint having a mechanism for sliding in the axial direction of the outer joint member, such as the cross groove type illustrated in Fig. 1, the tripod type illustrated in Fig. 2, and the double offset type illustrated in Fig. 3, but can also be used as a fixed type constant velocity universal joint using balls, such as the Rzeppa type and the Barfield type. The tripod type constant velocity universal joint may be either a double roller type or a single roller type.

[0033] Furthermore, the shape of the flexible boot for a constant velocity universal joint to be attached to a constant velocity universal joint is not limited to a specific shape, as long as it has mounting portions for mounting to mating members at both ends and a bent portion between the two mounting portions to absorb deformation associated with the operation of the constant velocity universal joint.For example, it may be a boot having a U-shaped curved bent portion, a boot having a bellows-shaped bent portion with multiple peaks and valleys, or a boot having a bent portion with one peak and valley.

[0034] Specifically, as shown in Fig. 1, a cross groove type constant velocity universal joint 1 includes an inner joint member 3 having a plurality of track grooves 7 formed on its outer circumferential surface, and an outer joint member 2 located on the outer periphery of the inner joint member 3 and having track grooves 6 formed on its inner circumferential surface in the same number as the track grooves 7 of the inner joint member 3. The track grooves 7 of the inner joint member 3 and the track grooves 6 of the outer joint member 2 are inclined in opposite directions with respect to the axis, and balls 4 are incorporated at the intersections of pairs of track grooves 7 and track grooves 6. A cage 5 is disposed between the inner joint member 3 and the outer joint member 2, and the balls 4 are held in pockets of the cage 5.

[0035] Here, the boot 9 is attached between the outer joint member 2 and the shaft 8 connected to the inner joint member 3 via the annular member 10 attached to the outer joint member 2, and covers the constant velocity universal joint so as to seal it. A lubricant such as grease (not shown) is filled in this sealed space. The boot 9 includes an outer cylinder end (large diameter mounting portion) 9a fixed to the end of the annular member 10 attached to the outer joint member 2, an inner cylinder end (small diameter mounting portion) 9b fixed to the shaft 8 connected to the inner joint member 3, and a bellows portion provided therebetween and having a U-shaped bent portion 9c. The provision of the U-shaped bent portion 9c suppresses the whirling of the boot bent portion when the cross groove type constant velocity universal joint 1 rotates at high speed, and improves the durability of the boot.

[0036] The outer cylinder end 9a of the boot 9 is sealed by being fixed to the annular member 10. As a fixing method, as shown in FIG. 1, a recess 10a is provided in the annular member 10, and the tip of the outer cylinder end 9a of the boot 9 is fitted into the recess 10a to tighten the recess 10a of the annular member 10. The fixing method of the outer cylinder end 9a and the annular member 10 is one example and is not limited thereto. For example, the outer cylinder end 9a may be fixed to the annular member 10 by a fastening band 11 or the like, or the annular member 10 may be integrally molded with the boot 9 and attached to the outer joint member 2. Reference numeral 12 in the figure denotes an air vent groove that prevents the grease filled inside the boot from leaking out. Although an iron metal ring is generally used as the annular member 10, it may be made of other metals such as aluminum or resin.

[0037] Furthermore, the inner cylinder end 9b of the boot 9 is sealed by being fixed to the shaft 8. A boot groove 8a is formed on the outer circumferential surface of the portion of the shaft 8 where the inner cylinder end 9b is fixed, and the inner cylinder end 9b fits into this boot groove 8a and is fixed with a fastening band or the like. Furthermore, by providing annular protrusions 8b on both sides of the boot groove 8a, the fixation of the inner cylinder end 9b inserted in the boot groove 8a to the shaft 8 can be further strengthened.

[0038] 2 shows one embodiment of a tripod type constant velocity universal joint. In this tripod type constant velocity universal joint 13, three linear track grooves 15 are formed in the axial direction on the inner surface of the outer joint member 14. A tripod member (inner joint member) 16 assembled inside the outer joint member 14 is provided with three trunnions 17. A spherical roller 18 is inserted on the outer side of each trunnion 17, and a needle 19 is assembled between the spherical roller 18 and the trunnion 17 to support the spherical roller 18 rotatably and axially slidably, and the spherical roller 18 is inserted in the track groove 15 so as to be freely rollable. A boot 21, which is a molded body of the rubber composition, is attached from the outer joint member 14 to a shaft 20 connected to the tripod member 16.

[0039] Here, the boot 21 includes an outer cylinder end (large diameter mounting portion) 21a that is fitted and fixed to the outer joint member 14, an inner cylinder end (small diameter mounting portion) 21b that is fitted and fixed to the shaft 20 connected to the inner joint member 16, and a bellows-shaped bent portion (hereinafter also referred to as a "bellows portion") 21c having multiple peaks and valleys that connects between the outer cylinder end 21a and the inner cylinder end 21b, and covers the constant velocity universal joint so as to seal it. A lubricant such as grease (not shown) is sealed in this sealed space. The boot 21 fits the outer cylinder end 21a to the outer joint member 14 and fixes it with a fastening band 22a or the like, while the inner cylinder end 21b is fixed to the shaft 20 with a fastening band 22b or the like. A boot groove 20a is formed on the outer circumferential surface of the portion of the shaft 20 where the inner cylinder end 21b is fixed, and the inner cylinder end 21b is fitted into the boot groove 20a. Furthermore, by providing annular projections 20b on both sides of the boot groove 20a, the inner cylinder end 21b inserted in the boot groove 20a can be fixed to the shaft 20 more firmly.

[0040] Further, FIG. 3 shows an embodiment of a double offset type constant velocity universal joint. In this double offset type constant velocity universal joint 23, a plurality of linear track grooves 26, 27 are formed in the axial direction on the inner surface of the outer joint member 24 and the outer surface of the inner ring (inner joint member) 25. The balls 28 assembled between the track grooves 26, 27 are supported by a cage 29, the outer periphery of which is a spherical surface 29a, and the inner periphery of which is a spherical surface 29b that fits the outer periphery of the inner ring 25. The centers (a) and (b) of the spherical surfaces 29a, 29b are shifted in the axial direction on the axis of the outer joint member 24. A boot 31, which is a molded body of the above rubber composition, is attached from the outer joint member 24 to the shaft 30 connected to the inner ring 25. The structure and mounting structure of the boot 31 are the same as those of the boot 21 in FIG. 2. A lubricant such as grease (not shown) is filled in the space sealed by the boot 31.

[0041] 2 and 3, the bellows shape of each boot 21, 31 has a smaller curvature of the outer circumferential surface of the valleys of the bellows portion than the curvature of the outer circumferential surface of the peaks. In other words, by making the radius of curvature of the bellows valleys larger than the radius of curvature of the peaks, deformation of the compression side phase of the boot valleys when an operating angle is taken is suppressed, improving the durability of the valleys. If the curvature of the outer circumferential surface of the valleys is equal to or greater than the curvature of the outer circumferential surface of the peaks, the valleys will be significantly crushed, making them more likely to become the starting point of cracks.

[0042] Also, a structure can be adopted in which a connection part is provided at the end of the bellows portion on the small diameter mounting portion side, which is smoothly continuous with the small diameter mounting portion and has an outer surface formed in an arc shape having a center of curvature outside the boot, the radius of curvature of the outer surface of this connection part is set to be larger than the radius of curvature of the outer surface of the peak part of the bellows portion, and the thickness of the connection part at any point is made greater than the thickness of the connection part at the end of the large diameter mounting portion side.

[0043] In addition, a structure can be adopted in which the small diameter mounting portion has a shaft mounting portion having an engaging groove formed on its outer diameter surface for mounting a boot band, and a thin-walled portion that is connected from the shaft mounting portion to the bellows portion via a thick-walled portion to allow buckling-like displacement relative to the shaft mounting portion and the bellows portion.

[0044] Furthermore, a structure can be adopted in which the boot band is a circular ring-shaped body without a folded-back portion, and the axial outer peripheral edge of the boot band is folded or curved toward the outer diameter side, so that when the boot band is in a contracted state, a gap is formed between the axial outer peripheral edge and the corresponding bottom end of the fitting groove of the boot, thereby avoiding interference.

[0045] A constant velocity universal joint used in an automobile drive shaft (propeller shaft) which is a molded article of the above-mentioned specified rubber composition and is fitted with a boot of the above structure has excellent heat resistance, cold resistance, oil resistance and ozone resistance.

[0046] The above-described embodiment is one example of a preferred embodiment of the present invention, but the present invention is not limited to this embodiment and various modifications can be made without departing from the gist of the present invention. EXAMPLES

[0047] Various rubber materials (Examples 1-4 and Comparative Examples 1-4) were prepared by varying the compounding ratio of HNBR and EPDM and the type and amount of additives, and a TR test, a CVJ boot low-temperature rotation test, a CVJ boot high-temperature rotation test, a CVJ boot ozone durability test, and an IRM903 oil immersion test were carried out. In these tests, the HNBR used as the base rubber material contained 15-21% by weight of acrylonitrile, which provides both the heat resistance and cold resistance required for a constant velocity universal joint flexible boot.

[0048] Here, in Examples 1 to 4 and Comparative Examples 1 and 2, 50 to 100 parts by weight of HNBR, 0 to 50 parts by weight of EPDM were blended, as well as 30 parts by weight of an ester-based plasticizer, 10 parts by weight of a peroxide-based crosslinking agent, and 70 parts by weight of carbon black.

[0049] Comparative Example 3 contained 70 parts by weight of HNBR, 30 parts by weight of EPDM, 30 parts by weight of an ester plasticizer, 3 parts by weight of a peroxide crosslinking agent, and 70 parts by weight of carbon black.

[0050] Comparative Example 4 contained 70 parts by weight of HNBR, 30 parts by weight of EPDM, 30 parts by weight of vegetable oil-based plasticizer, 10 parts by weight of peroxide-based crosslinking agent, and 70 parts by weight of carbon black.

[0051] The chemicals used in this test are as follows:

[0052] [Table 1] In this test, an ester-based plasticizer was used as the plasticizer A in the examples, and a vegetable oil-based plasticizer was used as the plasticizer B in the comparative example 4. In addition, a peroxide-based crosslinking agent was used as the crosslinking agent.

[0053] [Boot shape] In this test, a flexible boot for a constant velocity universal joint shown in Figure 1 was used.

[0054] The compositions of the examples and comparative examples and the results of various tests are shown in Table 2 below.

[0055] [Table 2]

[0056] [TR Test] A TR test was carried out on rubber materials made by compounding EPDM with HNBR containing 15-21% by weight of acrylonitrile, and a low-temperature rotation test was also carried out on flexible boots for constant velocity universal joints.

[0057] The TR test used data obtained with reference to ISO2921 to confirm the recovery rate at -40℃.

[0058] In Examples 1 to 4 and Comparative Examples 1 and 2, the type and amount of additive was fixed and the compounding ratio of HNBR and EPDM was changed, and the elastic recovery rate was 18% or more in Examples 1 to 4 where the EPDM compounding amount was 20 parts by weight or more. On the other hand, in Comparative Examples 1 and 2 where the EPDM compounding amount was 10 parts by weight or less, it was less than 18%.

[0059] In Comparative Example 3, the compounding ratio of HNBR and EPDM was the same as in Example 3, but the compounding amount of the crosslinking agent was changed, and the elastic recovery rate was less than 18%.

[0060] In Comparative Example 4, the compounding ratio of HNBR and EPDM was the same as in Example 3, but the type of plasticizer was changed, and the elastic recovery rate was less than 18%.

[0061] The test results showed that a sufficient elastic recovery rate was achieved by appropriately mixing the types and amounts of additives and by mixing 20 parts by weight or more of EPDM. Rubber materials containing 30 parts by weight or more of EPDM have an elastic recovery rate of 21% or more, which is even more preferable.

[0062] [CVJ boot low temperature rotation test] The CVJ boot low-temperature rotation test was carried out under conditions of an operating angle of 5 degrees, an ambient temperature of -40°C, a rotation speed of 500 rpm, and a durability cycle of 10 cycles, to check for slippage at the boot mounting part.

[0063] A low-temperature rotation test was conducted on a flexible boot for a constant velocity universal joint made of the rubber material of Example 4 having an elastic recovery rate of 18%, and it was confirmed that although slight slippage occurred in some areas at the boot mounting parts, the boot had sufficient cold resistance.

[0064] When a low-temperature rotation test was conducted on flexible boots for constant velocity universal joints using the rubber materials of Examples 1 to 3 having elastic recovery rates of 21% or more, it was confirmed that no slippage occurred at the boot mounting portion and that the boots had higher cold resistance.

[0065] On the other hand, when a low-temperature rotation test was conducted on flexible boots for constant velocity universal joints using rubber materials with elastic recovery rates of less than 18% in Comparative Examples 1 to 4, slippage occurred at the boot attachment area. Those containing 20 parts by weight or more had an elastic recovery rate of 18% or more, and presented no problems in the low-temperature rotation test (no slippage at the boot attachment area), so it was determined that they had sufficient cold resistance. Those containing 30 parts by weight or more were even more preferable, as they had an elastic recovery rate of 21% or more and no slippage occurred at the boot attachment area.

[0066] [CVJ boot high temperature rotation test] The CVJ boot high temperature rotation test was carried out to confirm the high temperature durability of the boots under the conditions of an operating angle of 5 degrees, an ambient temperature of 130°C, a rotation speed of 2700 rpm, and an operating time of 550 hours. No damage to the boots was observed in Examples 1 to 4 and Comparative Example 1, and it was confirmed that the boots had durability under high temperatures. Note that the tests for Comparative Examples 2 to 4 were omitted.

[0067] [CVJ boots ozone durability test] The CVJ boot ozone durability test was conducted to confirm the ozone durability of the boots under the following conditions: ozone concentration 200 pphm, operating angle 5 degrees, atmospheric temperature 40°C, rotation speed 1200 rpm, and operating time 200 hours.

[0068] In Examples 1 to 4, no cracks were observed after 200 hours of operation, and the ozone durability was good. In Comparative Example 1, the boots were not damaged and the operation was possible, but cracks were observed. In Comparative Example 2, the boots were damaged and operation was impossible. The tests for Comparative Examples 3 and 4 were omitted. This demonstrates that ozone resistance is improved by blending EPDM with HNBR, and that flexible boots for constant velocity universal joints made from rubber material containing 20 parts by weight or more of EPDM showed no visible cracks and had high ozone resistance.

[0069] [IRM903 oil immersion test] [Regarding grease sealed inside constant velocity joints equipped with boots] Grease is sealed inside the constant velocity joint with the boot attached. The grease is composed of a base grease made of a thickener and a base oil. Various additives may also be added to this base grease.

[0070] Examples of grease thickeners include, but are not limited to, soaps such as lithium soap, lithium complex soap, calcium soap, calcium complex soap, aluminum soap, and aluminum complex soap, and urea compounds such as diurea compounds and polyurea compounds.

[0071] Examples of urea-based thickeners include, but are not limited to, diurea compounds and polyurea compounds.

[0072] The diurea compound can be obtained, for example, by the reaction of a diisocyanate with a monoamine. Examples of the diisocyanate include phenylene diisocyanate, diphenyl diisocyanate, phenyl diisocyanate, diphenylmethane diisocyanate, octadecane diisocyanate, decane diisocyanate, and hexane diisocyanate. Examples of the monoamine include octylamine, dodecylamine, hexadecylamine, octadecylamine, oleylamine, aniline, p-toluidine, and cyclohexylamine.

[0073] Polyurea compounds can be obtained, for example, by reacting diisocyanates with monoamines and diamines. The diisocyanates and monoamines include those used to produce diurea compounds, and the diamines include ethylenediamine, propanediamine, butanediamine, hexanediamine, octanediamine, phenylenediamine, tolylenediamine, xylenediamine, etc.

[0074] Examples of base oils for grease include commonly used lubricating oils such as paraffinic or naphthenic mineral oils, ester-based synthetic oils, ether-based synthetic oils, hydrocarbon-based synthetic oils, GTL base oils, fluorine oils, silicone oils, etc., or mixtures thereof, but are not limited to these. In general, mineral oils are often used in consideration of cost, but synthetic oils and their mixtures may also be used in consideration of the temperature range in which they are used.

[0075] The lubricating components may further include various additives such as solid lubricants such as molybdenum disulfide and graphite, friction modifiers such as organic molybdenum, oiliness agents such as amines, fatty acids, and oils, antioxidants such as amines and phenols, rust inhibitors such as petroleum sulfonates, dinonylnaphthalene sulfonate, and sorbitan esters, extreme pressure agents such as sulfur-based and sulfur-phosphorus-based agents, wear inhibitors such as organic zinc and phosphorus-based agents, metal deactivators such as benzotriazole and sodium nitrite, and viscosity index improvers such as polymethacrylate and polystyrene.

[0076] [About the immersion test] Actual constant velocity universal joint boots are used in combination with various greases. Flexible boots for constant velocity universal joints and constant velocity universal joints fitted with these boots are most affected by the base oil of the grease enclosed, so testing with a standard oil whose components are close to those of the base oil of the grease actually used is necessary.

[0077] Therefore, IRM903 oil (body fluid test standard oil used in JIS K6258 ASTM D471 standard inspection of rubber parts), which contains approximately equal amounts of paraffinic and naphthenic mineral oils, was selected as the standard oil for the immersion test, and by checking the oil resistance of IRM903 oil, it was used as an indicator of whether it can be used as a boot material for constant velocity universal joints, which are always in contact with grease.

[0078] The swelling of rubber is greatly affected by the aniline point. The IRM903 oil used in this immersion test has a low aniline point of 70°C, so it is used for testing as a standard grease that has a strong tendency to swell rubber.

[0079] In the case of flexible boots for constant velocity joints, the expansion of the rubber material does not itself impair the performance of the boot, but the problem is that the expansion in volume causes a decrease in various physical properties. It has been found from experience that if the swelling with IRM903 oil is within 100%, the swelling with the grease actually sealed and used in the flexible boots for constant velocity joints will be within 30%, and it has been confirmed that there are no problems with durability, sealing, etc. in practical use. Therefore, the standard for judgment is whether the swelling is 100% or less.

[0080] Swelling was measured using data obtained with reference to ISO1817, and the rate of change in physical properties of the rubber material after immersion in IRM903 oil at a set temperature of 100°C for 72 hours was confirmed.

[0081] As a result of the test, the swelling of the rubber material of Examples 2 to 4 and Comparative Examples 1 to 2, in which the amount of EPDM compounded is 40 parts by weight or less, was 100% or less. Flexible boots for constant velocity universal joints using this rubber material can suppress contact with the surroundings and abnormal wear. Therefore, it can be applied under severe conditions such as high speed, high operating angle, and high temperature, and can be said to be more preferable as a rubber material for flexible boots for constant velocity universal joints. On the other hand, the swelling of the rubber material of Example 1, in which the amount of EPDM compounded is 50 parts by weight, was 100% or more. From this, it was confirmed that the oil resistance can be improved by suppressing the amount of EPDM compounded. Note that the test was omitted for Comparative Examples 3 and 4.

[0082] Here, the rubber material of Example 1, which contains 50 parts by weight of EPDM, swells by 100% or more, but passes the CVJ boot high temperature rotation test and the CVJ boot low temperature rotation test, and can be used as an actual boot. EPDM was also blended to improve ozone resistance, but blending more than a certain amount of EPDM deteriorated oil resistance (see Example 1). It was confirmed that blending more than a certain amount of EPDM deteriorated oil resistance, and that cold resistance and oil resistance are inversely proportional to each other.

[0083] From the above test results, it has been confirmed that a flexible boot for constant velocity universal joints, which is made using a rubber material that is blended with 30 parts by weight of ester-based plasticizer, 10 parts by weight of peroxide-based crosslinking agent, 70 parts by weight of carbon black, 50 to 80 parts by weight of HNBR with an acrylonitrile content of 15 to 21% by weight, and 20 to 50 parts by weight of EPDM, and has an elastic recovery rate of 18% or more at -40°C in the TR test, and a constant velocity universal joint equipped with such a boot, are heat resistant and also have satisfactory cold resistance and ozone resistance.

[0084] Furthermore, it was confirmed that flexible boots for constant velocity universal joints made of rubber material that swells by 100% or less in an immersion test with IRM903 oil, and constant velocity universal joints equipped with such boots, not only satisfy the above-mentioned functions but also provide high oil resistance.

[0085] Therefore, the flexible boot for constant velocity universal joints using the rubber material of the present invention and the constant velocity universal joints equipped with the boot can be suitably used as constant velocity universal joints for automobile drive shafts and automobile propeller shafts, or universal joints for various machines, and can be suitably used in particular as inboard boots for drive shafts which tend to become hot, and boots for propeller shafts. [Explanation of symbols]

[0086] 1,13,23 Constant velocity universal joint 9,21,31 Flexible boots

Claims

1. A flexible boot for a constant velocity universal joint, which is used for a drive shaft or a propeller shaft of an automobile, has attachment parts for attachment to a mating member at both ends and is provided with a bent part between the attachment parts for absorbing deformation caused by operation of the constant velocity universal joint, The flexible boot contains 50 to 80 parts by weight of HNBR having an acrylonitrile content of 15 to 21% by weight and 20 to 50 parts by weight of EPDM, The rubber material must have an elastic recovery rate of 18% or more at -40°C in the TR test. A flexible boot for a constant velocity universal joint.

2. 2. A flexible boot for a constant velocity universal joint according to claim 1, wherein said rubber material has a swelling of 100% or less in an immersion test with IRM903 oil.

3. 3. A flexible boot for a constant velocity universal joint according to claim 1, wherein said rubber material has an elastic recovery rate of 21% or more at -40° C. in a TR test.

4. A constant velocity universal joint, characterized by being equipped with a flexible boot for a constant velocity universal joint described in any one of claims 1 to 3.

Citation Information

Patent Citations

  • Sealing rubber composition

    JP1990124951A

  • Boots for automobile

    JP1998159989A

  • Rubber composition for high-load transmission belt and high-load transmission belt made of such rubber composition

    JP2003314619A

  • Boot for steering device, constant-velocity universal joint for the steering device, and the steering device

    JP2010078149A

  • Crosslinked rubber composition and sealant including the same

    JP2019206663A