METAL-CONTAINING FILMS AND METHOD FOR MANUFACTURING METAL-CONTAINING FILMS
A laminate structure metal-containing film with controlled thickness and supercooling elements addresses grain boundary issues, improving semiconductor device performance and manufacturing efficiency by maintaining low resistance and mechanical strength.
Patent Information
- Application Number
- JP2021101521
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-18
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-06-18
AI Technical Summary
Existing metal-containing films used in semiconductor manufacturing often suffer from issues such as high resistance, mechanical weakness, and atomic diffusion due to grain boundaries, which affect the performance and manufacturing process of semiconductor devices.
A metal-containing film with a laminate structure is developed, where each layer has a thickness below the critical diameter for crystal nucleation, and an element that increases the degree of supercooling is added to stabilize the amorphous state, preventing grain boundaries and facilitating the formation of a film without crystal grain boundaries.
The laminate structure metal-containing film maintains low resistance and mechanical strength, reducing issues like grain boundary scattering, stress concentration, and diffusion, thereby enhancing the performance and manufacturing efficiency of semiconductor devices.
Smart Images

Figure 0007595527000002 
Figure 0007595527000003 
Figure 0007595527000004
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE The present disclosure relates to metal-containing films and methods for making metal-containing films. [Background technology]
[0002] When manufacturing a semiconductor device, metal-containing films are often used as wiring, electrodes, barrier films, metal hard masks, etc. Such metal-containing films are required to have properties such as low resistance, high mechanical strength, and small atomic diffusion depending on the respective applications, and various techniques have been proposed for this purpose. For example, Patent Document 1 describes that by using CoW as a seed layer for a metal wiring layer mainly composed of tungsten (W), the crystals of the metal wiring layer can be made fine, and the deposition resistance value of the metal wiring layer can be suppressed to be small. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-73949 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present disclosure provides metal-containing films and methods for producing metal-containing films having good properties depending on the application. [Means for solving the problem]
[0005] A metal-containing film according to one embodiment of the present disclosure has a laminate structure that does not include grain boundaries, and is formed by alternately laminating a first metal-containing unit film having a thickness less than the critical diameter for crystal nucleation and a second metal-containing unit film having a thickness less than the critical diameter for crystal nucleation and different from the first metal-containing unit film. At least one of the first metal-containing unit film and the second metal-containing unit film is doped with an element that increases the degree of supercooling. . Effect of the Invention
[0006] The present disclosure provides a metal-containing film having good properties suited to various applications and a method for producing the metal-containing film. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a cross-sectional view illustrating a metal-containing film according to an embodiment. [Diagram 2] FIG. 1 shows calculated values of the crystal nucleation critical diameter D* of major metals. [Diagram 3] This is an SEM photograph of sample A, in which a metal-containing film with an Al-Ti laminate structure was produced by sputtering, in which the thickness of the Al film was made less than 1.7 nm. [Figure 4] This is an SEM image of sample B, in which a metal-containing film with an Al-Ti laminate structure was produced by sputtering, in which the thickness of the Al film was set to 1.7 nm or more. [Diagram 5] This is an SEM photograph of sample C, which was manufactured under the same conditions as sample A, except that the total film thickness was set to 1000 nm. [Figure 6] 1 is an enlarged SEM photograph showing a cross section of sample C. [Figure 7] FIG. 2 is a diagram showing the transition of free energy during phase transition from a metastable amorphous state to a stable crystalline state. [Figure 8] FIG. 1 is a diagram showing the relationship (calculated values) between the degree of supercooling and the critical nucleus radius r* of various metals. [Figure 9] FIG. 2 is a diagram showing the relationship between the degree of supercooling and the cooling rate in an Al-Si alloy. [Figure 10] 1 is a SEM photograph showing a state in which a metal-containing film having an Al-Ti laminate structure and a metal-containing film having an (AlSi)-Ti laminate structure are formed by sputtering to a film thickness of 500 nm and 1000 nm. [Figure 11] FIG. 2 is a diagram showing the relationship between the degree of supercooling and the cooling rate in an Al-Mg alloy. [Figure 12] 1 shows SEM images of a metal-containing film with an (AlSi)-Ti laminate structure and a metal-containing film with an (AlMg)-Ti laminate structure. [Figure 13] FIG. 1 is an Al-Si phase diagram. [Figure 14] FIG. 1 is an Al-Mg phase diagram. [Figure 15] 1 is a cross-sectional view showing an example of a fine wiring structure in which a metal-containing film according to an embodiment is applied to fine wiring. [Figure 16] 1 is a cross-sectional view showing an example of a fine wiring structure in which a metal film according to an embodiment is used as a barrier film. [Figure 17] 1 is a cross-sectional view showing an example of a capacitor in which a metal-containing film according to an embodiment is applied to an electrode having a pillar structure. [Figure 18] 1 is a cross-sectional view showing an example of a capacitor in which a metal-containing film according to an embodiment is applied to an electrode having a cylindrical structure. [Figure 19] FIG. 1 is a cross-sectional view showing an example of a structure in which a metal-containing film according to an embodiment is used as a hard mask. [Figure 20] FIG. 1 is a cross-sectional view showing an example of a plasma sputtering apparatus for forming a film by PVD. [Figure 21] FIG. 1 is a cross-sectional view showing an example of a film formation apparatus for forming a film by ALD or CVD. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment will be described with reference to the accompanying drawings.
[0009] <Metal-containing film> 1 is a cross-sectional view showing a metal-containing film according to an embodiment. The metal-containing film 1 has a laminate structure in which a first metal-containing unit film 2 and a second metal-containing unit film 3 different from the first metal-containing unit film are alternately stacked, and is formed on a substrate W. The first metal-containing unit film 2 and the second metal-containing unit film 3 each have a thickness less than the critical diameter for crystal nucleation, and the metal-containing film 1 does not include a crystal grain boundary. Examples of the substrate W include a semiconductor substrate and an FPD substrate.
[0010] The radius of the nucleus is the critical nuclear radius r *If the energy due to the volume increase cannot exceed the surface energy, nucleation is not promoted and no crystal nuclei are formed. However, if the radius of the nucleus is less than the critical nucleus radius r * Above this threshold, nucleation is promoted and crystal nuclei are formed. In other words, the critical nucleus radius r * is the critical crystal nucleus size above which a crystal nucleus is formed, and can be rephrased as the critical radius for crystal nucleation. The diameter of the nucleus at this point is the critical diameter for crystal nucleation D * Therefore, the thickness of the first metal-containing unit film 2 and the second metal-containing unit film 3 is set to the crystal nucleation critical diameter D * By keeping the diameter of the nuclei below the critical diameter D * This makes it possible, in theory, to suppress crystallization of the first metal-containing unit film 2 and the second metal-containing unit film 3. As a result, the metal-containing film 1 can be a film that does not include crystal grain boundaries.
[0011] critical nuclear radius r * can be calculated for each metal using the maximum degree of undercooling ΔTmax and the melting point Tm, using a relational equation proportional to Tm / TΔmax. * is the critical nuclear radius r calculated in this way. * The critical diameter for crystal nucleation of major metals, D * The calculated values of are shown in Figure 2. As shown in Figure 2, most metals have a critical diameter D * is 1.4 to 2.6 nm, and by setting the film thicknesses of the first metal-containing unit film 2 and the second metal-containing unit film 3 to less than this value, crystallization can be suppressed.
[0012] As a method for forming the first metal-containing unit film 2 and the second metal-containing unit film 3 having such a film thickness, general thin film formation techniques such as PVD represented by sputtering, ALD, which is a chemical film formation method using gas, and CVD can be used.
[0013] It is preferable to select a combination that is as small as possible in reactivity or a combination that has a two-phase coexistence relationship between the first metal-containing unit film 2 and the second metal-containing unit film 3. If an interface reaction occurs between these layers and a chemical potential difference occurs, diffusion (atomic movement) occurs, which makes it easier for a phase transition from a metastable state to a stable state, and makes it easier for crystallization to occur.
[0014] The first metal-containing unit film 2 and the second metal-containing unit film 3 may be metal nitride films or metal films. Examples of combinations of the first metal-containing unit film 2 and the second metal-containing unit film 3 include a combination in which one of them is a metal nitride film and the other is a metal film, a combination in which both are metal nitride films, and a combination in which both are metal films.
[0015] The metal nitride film constituting the first metal-containing unit film 2 or the second metal-containing unit film 3 may be any of TiN, NbN, VN, WN, TaN, MoN, and W2N3, and the metal film may be any of Ru, Co, Ni, Mo, W, Al, Ti, V, Mn, Si, and Mg.
[0016] Preferable combinations of the first metal-containing unit film 2 and the second metal-containing unit film 3 include the following. Combination of metal nitride films TiN-TaN, TiN-NbN, TiN-MoN, TiN-W2N3, TaN-NbN, TaN-W2N3 Combination of metal nitride film and metal film TiN-W, TiN-Mo, TiN-Ru, TaN-W, TaN-Mo, TaN-Ru Combination of metal films Si-Al, W-Al, Mg-Al, W-Ti, V-Ti, Mg-Ti
[0017] The above-mentioned preferable combinations are combinations with as little reactivity as possible or combinations with a two-phase coexistence relationship, and diffusion (atomic movement) due to an interface reaction is unlikely to occur, and crystallization is unlikely to occur.
[0018] However, even if the combination of the first metal-containing unit film 2 and the second metal-containing unit film 3 is reactive, it is possible to form a metal-containing film that does not include grain boundaries. For example, the combination of Al-Ti is a combination in which Al and Ti are reactive. In addition, since Al-Ti is a pure metal system, the bond is a metallic bond and is weak. Therefore, the combination of Al-Ti is a combination in which it is difficult to maintain an amorphous state, which is a metastable state. Even with such a combination, a metal-containing film that does not actually include grain boundaries was obtained as a result of forming a metal-containing film with a laminate structure under the following conditions. Al film thickness: 1.6 nm (D * (less than 1.7 nm, the calculated value of Ti film thickness: 0.8 nm (D * (less than 2.7 nm, the calculated value of Film deposition method: Sputtering Al and Ti film thickness ratio (Al:Ti): 77:23, 66:34, 55:45 Total film thickness (target value): 35 nm
[0019] In addition, when manufacturing a metal-containing film with an Al-Ti laminate structure by sputtering, sample A, in which the thickness of the Al film was set to 1.6 nm (less than 1.7 nm), was compared with sample B, in which the thickness was set to 1.8 nm (1.7 nm or more). In forming the film, the thickness ratio of Al to Ti was set to 2:1, and the total thickness was set to 100 nm.
[0020] As a result, the thickness of the Al film was D * In sample A, the thickness of the Al film was less than 1.7 nm, which is the calculated value of 1.0 nm, and the film was amorphous without grain boundaries, as shown in the SEM photograph in Figure 3. * In sample B, where the calculated value was 1.7 nm or more, crystallization was observed as shown in the SEM photograph in Figure 4.
[0021] Next, sample C was manufactured under the same conditions as sample A, except that the total film thickness was set to 1000 nm. As a result, crystallization occurred, as shown in the SEM photograph in Figure 5. Figure 6 is an SEM photograph showing an enlarged cross section of sample C, in which the crystal grain size on the substrate side is small, while the crystal grain size on the surface side is large. From this, it is believed that crystallization occurred because heat was input from the surface side during sputtering film formation, and the film thickness became thicker, which increased the influence of the heat input. In addition, the difference in crystal grain size between the substrate side and the surface side is believed to be due to the substrate side being the cooling side and the surface side being the heat input side, which means that the degree of supercooling is different.
[0022] In this manner, the first metal-containing unit film 2 and the second metal-containing unit film 3 have a thickness equal to or larger than the critical diameter D * Even if the temperature is less than 100° C., crystallization may occur due to heat input. FIG. 7 is a diagram showing the transition of free energy when a phase transition occurs from a metastable amorphous state to a stable crystalline state. As shown in this figure, activation energy ΔEa is required for a phase transition from a metastable amorphous state to a stable crystalline state. However, when heat input is present, the activation barrier (ΔEa) is overcome by heat input to reach a crystalline state. Therefore, in order to maintain the amorphous state without crystallization even when heat input is present, it is necessary to either reduce the free energy Gα of the amorphous state to make the amorphous state more stable, or to increase the activation energy ΔEa to raise the barrier of phase transition, or both.
[0023] Since amorphous materials are formed when supercooled liquid is solidified, it is believed that the greater the maximum degree of supercooling, the easier it is to maintain a metastable amorphous state. In other words, it is believed that the greater the maximum degree of supercooling, the smaller Gα becomes, and the more stable the amorphous state becomes. Therefore, in order to stabilize the amorphous state, it is effective to add elements that increase the degree of supercooling.
[0024] Figure 8 shows the relationship between the degree of supercooling and the critical nucleus radius r of various metals. *The right end of the supercooling curve for each metal is the maximum degree of supercooling. From this figure, it can be seen that both Al and Ti have small maximum degrees of supercooling and are materials that have difficulty maintaining an amorphous state.
[0025] Therefore, when manufacturing a metal-containing film with an Al-Ti laminate structure, we tried to stabilize the amorphous state by adding an element that increases the degree of supercooling to the Al film. Figure 9 shows the relationship between the degree of supercooling and the cooling rate in an Al-Si alloy (source: Ichikawa et al., Castings vol. 46 (1973), 1, 25, fig. 8). From this figure, we can see that Si increases the degree of supercooling of pure Al.
[0026] In fact, metal-containing films of Al-Ti laminate structure and (AlSi)-Ti laminate structure were formed by sputtering with film thicknesses of 500 nm and 1000 nm. The amount of Si added to the AlSi film was 6 at%, and the film thicknesses of the Al film and AlSi film were 1.6 nm. Figure 10 shows SEM images of these films. As is clear from the SEM images, the Al-Ti laminate structure did not crystallize at a film thickness of 500 nm, but did crystallize at a film thickness of 1000 nm. In contrast, the (AlSi)-Ti laminate structure did not crystallize even at a film thickness of 1000 nm. From this, it is considered that by adding Si to Al to increase the degree of supercooling of pure Al, Gα became smaller and the amorphous state, which is a metastable state, could be maintained. In addition, the addition of elements itself leads to an increase in entropy, which is advantageous for decreasing Gα.
[0027] Besides Si, Mg is also known as an element that increases the degree of supercooling in Al films. Figure 11 shows the relationship between the degree of supercooling and the cooling rate in Al-Mg alloys (Source: Ichikawa et al., Castings vol. 46 (1973), 1, 25, Figure 4). From this figure, we can see that Mg can be an additive element that increases the degree of supercooling in pure Al.
[0028] In addition, a metal-containing film with an (AlMg)-Ti laminate structure was actually formed by sputtering to a thickness of 1000 nm. The amount of Mg added to the AlMg film was 6 at%, and the film thickness was 1000 nm. Figure 12 shows SEM images of the above-mentioned metal-containing film with an (AlSi)-Ti laminate structure and this metal-containing film with an (AlMg)-Ti laminate structure. As is clear from the SEM images, the (AlSi)-Ti laminate structure did not crystallize at a thickness of 1000 nm, whereas the (AlMg)-Ti laminate structure crystallized at a thickness of 1000 nm.
[0029] Thus, although both Si and Mg are additive elements that increase the degree of supercooling of Al, Mg did not show any effect of stabilizing the amorphous state. This difference was examined based on phase diagrams. Figure 13 is an Al-Si phase diagram, and Figure 14 is an Al-Mg phase diagram. As is clear from these figures, Al-Si is a phase separation system (eutectic system), whereas Al-Mg is an intermetallic compound forming system. In other words, Si and Mg have very different interactions with Al; Al-Si repels each other and separates into a phase mainly composed of Al and a phase mainly composed of Si, whereas Al-Mg attracts each other and is easily arranged (ordered) as Al-Mg-Al.
[0030] Such interactions can be understood by the interaction parameter of the mixing enthalpy of a binary system (Nishizawa, Sudo et al., Metallography, Maruzen (published August 31, 1972)). The mixing enthalpy of a binary system of pure substances A and B at 0 K is 0 H mix can be expressed by the following formula (1). In formula (1), 0 H A , 0 H B is the enthalpy of pure substances A and B at 0 K, and X B is the atomic fraction of pure substance B, 0 Ω AB is the interaction parameter. 0 Ω AB is expressed by the following formula (2). In formula (2), N is the total number of atoms A and B, z is the coordination number, e AB , eAA , e BB are the bond energies of AB, AA, and BB, respectively.
number
[0031] Interaction parameters 0 Ω AB The physical meaning of the value is as follows: (1) 0 Ω AB >0: In this case, e AB >(e AA +e BB ) / 2, which means that the energy of the AB pair is higher than the average energy of the AA and BB pairs and is unstable, meaning that A and B are repulsive and tend to separate into a phase mainly composed of A and a phase mainly composed of B. This makes it a combination that is likely to form an amorphous material. The Al-Si system mentioned above is an example of this. (2) 0 Ω AB <0: In this case, e AB <(e AA +e BB ) / 2, and since the energy of the AB pair is lower and more stable than the average energy of the AA and BB pairs, A and B tend to attract each other, meaning that ordering along the ABAB order is likely to occur. This makes it difficult to become amorphous. The Al-Mg system mentioned above is an example of this. (2) 0 Ω AB =0: In this case, e AB =(e AA +e BB ) / 2, and since the energy of the AB pair is equal to the average energy of the AA pair and the BB pair, there is no interaction between A and B, and the arrangement of A and B is disordered. This type of solid solution is called an ideal solution, and is a combination that is likely to form an amorphous material.
[0032] Enthalpy of mixing for such a binary system 0 H mix is related to the activation energy ΔEa when the phase transition occurs from the amorphous state to the crystalline state, 0 Ω AB It is thought that ΔEa changes depending on the value (positive or negative) of . The difference in behavior when Si and Mg are added to Al as described above is due to the following. 0 Ω AB This can be explained by the difference in ΔEa due to the positive and negative values of 0 Ω AB > 0, the added Si repels the Al matrix, increasing ΔEa. On the other hand, in the Al-Mg system, 0 Ω AB <0, the added Mg bonds with the Al matrix and orders the Al, thereby decreasing ΔEa.
[0033] As described above, by adding an element that increases the degree of supercooling to either or both of the first metal-containing unit film 2 and the second metal-containing unit film 3, it is possible to lower Gα and stabilize the amorphous state, thereby suppressing crystallization due to heat input. In addition, as an element that increases the degree of supercooling, the interaction parameter 0 Ω AB but, 0 Ω AB It is preferable to select one that is ≧0.
[0034] Such an additive element for increasing the degree of supercooling is effective when the first metal-containing unit film 2 and the second metal-containing unit film 3 are metal films, and can be appropriately selected according to the material. For example, as described above, when the material is Al, Si is suitable as the additive element, and when the material is Ru, Ir, Pd, Ni, Co, and Mn are suitable as the additive element, and when the material is Co, Ni, Cu, Pd, and Ru are suitable. When the material is W, Mo, Ta, Nb, Ti, and Mn are suitable as the additive element, when the material is Mo, W, Ta, Nb, Ti, and Mn are suitable, when the material is Ti, Zr, Hf, V, W, Mo, Nb, and Ta are suitable, and when the material is Mn, Ru, Fe, Mo, and W are suitable.
[0035] <How we arrived at the laminated metal-containing film> Next, the process by which the metal-containing film having a laminate structure in this embodiment was achieved will be described. In semiconductor devices, metal-containing films such as W, Cu, TiN, and TaN are used for various applications, such as wiring metals for fine wiring, electrodes with pillar or cylinder structures used in capacitors, barrier films, metal hard masks, etc. Such metal-containing films generally have a crystalline structure, and crystal grain boundaries can cause problems in the semiconductor device itself and in the manufacturing process of the semiconductor device.
[0036] For example, in fine wiring, the wiring resistance increases due to grain boundary scattering and interface scattering due to unevenness based on the grain boundary. In addition, in metal hard masks used in fine processing, if there are crystal grain boundaries, the shape of the grain boundary part may be transferred directly to the workpiece, and deformation (wiggling) may occur due to film stress caused by grain boundary sliding. Furthermore, in fine wiring, twisting may occur due to stress concentration caused by grain boundary sliding, which may increase interface resistance and induce misalignment due to interference between adjacent wirings. In electrodes with pillar structure or cylinder structure, the mechanical strength decreases due to grain boundary sliding, and plastic deformation such as leaning (collapse) occurs during the manufacturing process due to shear stress applied to the grain boundaries. Furthermore, barrier films are used as diffusion barriers for halogen-based impurities, etc., but if there are crystal grain boundaries, the barrier properties are significantly reduced due to bypass diffusion through the grain boundaries.
[0037] In contrast, in this embodiment, a metal-containing film 1 that does not include crystal grain boundaries is obtained by laminating a first metal-containing unit film 2 and a second metal-containing unit film 3. Therefore, there is no increase in resistance due to grain boundary scattering or interface scattering due to unevenness based on grain boundaries, and there are advantages in that the shape is easily traced during processing and a flat cross section is easily obtained. Furthermore, there is no stress concentration or strength reduction due to grain boundary sliding, and bypass diffusion via grain boundaries does not occur. Therefore, it is suitable for applications such as wiring metal for fine wiring, electrodes with pillar structure or cylinder structure, barrier film, and metal hard mask.
[0038] As a metal-containing film without grain boundaries, amorphous structures and single crystals called amorphous metals and glass metals have been known. However, many of the conventional metal-containing films with amorphous structures are alloys made by combining multiple metals, and the degree of freedom in the combination of metal elements is small, which greatly restricts the performance of semiconductor devices and the manufacturing process of semiconductor devices. In addition, a high-temperature process is required to obtain a single crystal, and the process is limited and complicated, which makes manufacturing difficult. Also, the materials that can be grown are limited.
[0039] In contrast, in this embodiment, since it is only necessary to form a laminate structure of the first metal-containing unit film 2 and the second metal-containing unit film 3, it can be manufactured by combining existing film formation processes and does not involve difficulties in manufacturing. In addition, there is a high degree of freedom in the selection of materials, and the combination of materials for the first metal-containing unit film 2 and the second metal-containing unit film 3 can be selected according to the required performance of the device and the requirements and constraints of the process. Furthermore, it is also possible that new functional materials can be obtained by simply combining existing processes.
[0040] <Uses of metal-containing films> Next, applications of the metal-containing film according to this embodiment will be described in more detail. Applications of the metal-containing film of this embodiment include wiring metal for fine wiring, barrier films, electrodes with pillar or cylinder structures, metal hard masks, and the like.
[0041] The wiring metal using the metal-containing film according to this embodiment can be used as a substitute for, for example, W films, Cu films, and TiN films used in existing fine wiring.
[0042] Fig. 15 is a cross-sectional view showing an example of a micro-wiring in which the metal-containing film of one embodiment is applied to the wiring metal. In the micro-wiring 110 of Fig. 15, an insulating film 102 having a recess such as a trench or a hole provided on a substrate 101 having a substructure (not shown) is formed, and a metal-containing film 105 of this embodiment, which becomes a wiring metal, is embedded in the recess via a barrier film 104. When the metal-containing film constituting the wiring metal has grain boundaries, as described above, grain boundary scattering and interface scattering due to unevenness based on the grain boundaries cause an increase in wiring resistance and twisting due to grain boundary sliding. However, since the metal-containing film 105 of this embodiment does not include grain boundaries, such inconveniences do not occur.
[0043] The first metal-containing unit film and the second metal-containing unit film constituting the metal-containing film 105 that becomes the wiring metal can be appropriately selected in combination according to the required characteristics such as resistance value. For example, as described above, a combination of one metal nitride film and the other metal film, a combination of both metal nitride films, or a combination of both metal films can be used. A representative example of the combination can be a combination of a TiN film (thickness 1 to 2 nm) and a WN film (thickness 1 to 2 nm). In addition, a combination of a TiN film (thickness 1 to 2 nm) and a Ru film (thickness 1.3 nm or less), a TiN film (thickness 1 to 2 nm) and a Mn film (thickness 2.2 nm or less), a TiN film (thickness 1 to 2 nm) and an Al film (thickness 1.6 nm or less), and a TiN film (thickness 1 to 2 nm) and a Ti film (thickness 2.6 nm or less) can be mentioned.
[0044] A barrier film using a metal-containing film according to an embodiment can be used as a replacement for, for example, a TaN film or a TiN film that is used in existing barrier films.
[0045] Fig. 16 is a cross-sectional view showing an example of a fine wiring structure in which the metal film of one embodiment is applied to a barrier film. In the fine wiring structure 111 of Fig. 16, a structure in which an insulating film 102 having a recess such as a trench or a hole is formed on a substrate 101 having a substructure not shown similar to that of Fig. 15 is formed, a metal-containing film 114 of this embodiment is formed as a barrier film in the recess, and a fine wiring 115 is embedded in the recess. When the metal-containing film constituting the barrier film has grain boundaries, as described above, the barrier properties are significantly reduced due to bypass diffusion through the grain boundaries if the grain boundaries are present, but the metal-containing film 114 of this embodiment does not have grain boundaries and does not have such a disadvantage.
[0046] The first metal-containing unit film and the second metal-containing unit film constituting the metal-containing film 114 serving as the barrier film can be selected in an appropriate combination according to the required barrier properties. For example, as described above, a combination of one being a metal nitride film and the other being a metal film, a combination of both being metal nitride films, or a combination of both being metal films can be used. A representative example of the combination is a combination of a TiN film (thickness 1 nm) and a WN film, a VN film, or a NbN film (all 1 nm thick).
[0047] An electrode having a pillar structure or a cylinder structure using a metal-containing film according to an embodiment can be used, for example, as a replacement for a TiN film or the like used in existing electrodes.
[0048] FIG. 17 is a cross-sectional view showing an example of a capacitor in which the metal-containing film of one embodiment is applied to an electrode having a pillar structure. In this example, the lower electrode of a capacitor 120 has a pillar structure, and the metal-containing film 122 of this embodiment, which becomes the lower electrode having a pillar structure, is formed on a contact 121a formed on a substrate 121. For example, a first TiO2 film 123, a ZrO2 film 124, and a second TiO2 film 125 are formed on the metal-containing film 122 as a dielectric film, and an upper electrode 126 is formed on the second TiO2 film 125. However, the material and number of layers of the dielectric film are not limited to this example. In the manufacturing process of the capacitor in FIG. 17, the insulating film supporting the lower electrode of the pillar structure is removed, the lower electrode is made to stand on its own, and then a dielectric film and the like are formed. At this time, if a crystal grain boundary exists in the lower electrode, the mechanical strength is reduced due to grain boundary sliding, and plastic deformation such as leaning (falling, collapsing) may occur due to the shear stress applied to the grain boundary. In contrast, in this example, the metal-containing film 122 of the present embodiment, which does not include grain boundaries, is used as the lower electrode of the pillar structure. Therefore, a decrease in mechanical strength due to grain boundary sliding does not occur, and plastic deformation such as leaning due to a decrease in strength is unlikely to occur.
[0049] FIG. 18 is a cross-sectional view showing an example of a capacitor in which the metal-containing film of one embodiment is applied to an electrode having a cylindrical structure. In this example, the lower electrode of a capacitor 130 has a cylindrical structure, and the metal-containing film 132 of this embodiment, which becomes the lower electrode having a cylindrical structure, is formed on a contact 131a formed on a substrate 131. For example, a first TiO2 film 133, a ZrO2 film 134, and a second TiO2 film 135 are formed as dielectric films on the metal-containing film 132, and an upper electrode 136 is formed on the second TiO2 film 135. However, the material and the number of layers of the dielectric film are not limited to this example. In the manufacturing process of the capacitor of FIG. 18, the insulating film supporting the lower electrode of the cylindrical structure is removed, the lower electrode is made to stand on its own, and then a dielectric film and the like are formed. Even in the case of a cylinder structure, the presence of grain boundaries may cause plastic deformation such as leaning (collapse). However, since metal-containing film 132 that does not contain grain boundaries is used as the lower electrode, there is no decrease in mechanical strength due to grain boundary sliding, and plastic deformation such as leaning due to the decrease in strength is unlikely to occur.
[0050] The first metal-containing unit film and the second metal-containing unit film constituting the metal-containing films 122, 132 that become the electrodes of the pillar structure or cylinder structure can be selected in an appropriate combination according to the required characteristics such as resistance value. For example, as described above, a combination of one being a metal nitride film and the other being a metal film, a combination of both being metal nitride films, or a combination of both being metal films can be used. A representative example of the combination is a combination of a TiN film (thickness 1 to 2 nm) and a WN film, a VN film, or a NbN film (all of which are 1 to 2 nm thick).
[0051] A metal hard mask using a metal-containing film according to an embodiment can be used as a replacement for, for example, a TiN film used in existing metal hard masks.
[0052] FIG. 19 is a cross-sectional view showing an example of a structure in which the metal-containing film of one embodiment is applied to a hard mask. The structure 140 of this example is configured by forming an etching target film 142 on a substrate 141, and forming a metal-containing film 143 of this embodiment as a metal hard mask thereon. The etching target film 142 is not particularly limited, but examples thereof include a tungsten film, a GST (GeSbTe) film, a Poly-Si film, a carbon film, a SiO2 film, and a SiON film. The etching target film 142 may also be a laminated film in which a plurality of films are laminated. When the metal-containing film constituting the metal hard mask has grain boundaries, as described above, the shape of the grain boundary portion is directly transferred to the etching target film 142, which is the workpiece, and deformation (wiggling) occurs due to film stress caused by grain boundary sliding. In contrast, the metal-containing film 143 of this example does not include grain boundaries, so such inconvenience does not occur.
[0053] The first and second metal-containing unit films constituting the metal-containing film 143 serving as the hard mask may be any of the above-mentioned combinations, in which one is a metal nitride film and the other is a metal film, both are metal nitride films, or both are metal films. An appropriate combination may be selected from these depending on the material of the film 142 to be etched.
[0054] <Metal-containing film manufacturing method> Next, a method for producing a metal-containing film according to an embodiment will be described. The film formation method of this embodiment alternately performs a step of forming a first metal-containing unit film 2 with a thickness less than the critical diameter for crystal nucleation and a step of forming a second metal-containing unit film 3 different from the first metal-containing unit film 2 with a thickness less than the critical diameter for crystal nucleation, thereby producing a metal-containing film 1 with a laminate structure that does not include grain boundaries.
[0055] The first metal-containing unit film 2 and the second metal-containing unit film 3 can be formed by a general thin film formation technique such as PVD, typically sputtering, or ALD and CVD, which are chemical film formation techniques using gas. These techniques may also be used in combination. For example, the first metal-containing unit film 2 and the second metal-containing unit film 3 may be formed by a combination of PVD and ALD, a combination of PVD and CVD, or a combination of ALD and CVD. These techniques will be described below.
[0056] [Film formation by PVD] FIG. 20 is a cross-sectional view showing an example of a plasma sputtering apparatus for forming a film by PVD. The apparatus in FIG. 20 shows an ICP type plasma sputtering apparatus, which is a type of ionized PVD apparatus.
[0057] 20, this plasma sputtering apparatus 200 has a grounded processing vessel 201 made of metal, and a bottom 202 of the processing vessel 201 is provided with an exhaust port 203 and a gas inlet 207. An exhaust pipe 204 is connected to the exhaust port 203, and a throttle valve 205 for adjusting pressure and a vacuum pump 206 are connected to the exhaust pipe 204. A gas supply pipe 208 is connected to the gas inlet 207, and a gas supply source 209 is connected to the gas supply pipe 208 for supplying a plasma excitation gas such as Ar gas and other necessary gases, such as N2 gas. A gas control unit 210 including a gas flow rate controller, a valve, and the like is provided in the gas supply pipe 208.
[0058] A mounting mechanism 212 for mounting a substrate W thereon is provided in the processing vessel 201. The mounting mechanism 212 has a disk-shaped mounting table 213 and a hollow cylindrical support 214 supporting the mounting table 213. The mounting table 213 is made of a conductive material and is grounded via the support 214. A cooling jacket 215 is provided in the mounting table 213, and a coolant is supplied therein to cool the mounting table. A resistance heater 237 covered with an insulating material is embedded on the cooling jacket 215 in the mounting table 213. The supply of the coolant to the cooling jacket 215 and the power supply to the resistance heater 237 are controlled to control the substrate temperature to a predetermined temperature.
[0059] An electrostatic chuck 216, which is configured by embedding an electrode 216b in a dielectric member 216a, is provided on the upper surface side of the mounting table 213 for electrostatically attracting the substrate W. The lower part of the support pillar 214 extends downward through an insertion hole 217 formed in the center of the bottom 202 of the processing vessel 201. The support pillar 214 can be raised and lowered by a lifting mechanism (not shown), whereby the entire mounting mechanism 212 is raised and lowered.
[0060] An expandable metal bellows 218 is provided to surround the support 214. An upper end of the metal bellows 218 is joined to the lower surface of the mounting table 213, and a lower end of the metal bellows 218 is joined to the upper surface of the bottom 202 of the processing vessel 201, so that the mounting mechanism 212 can be moved up and down while maintaining the airtightness inside the processing vessel 201.
[0061] On the bottom 202, for example, three support pins 219 (only two are shown) are vertically provided facing upward. On the mounting table 213, pin insertion holes 220 corresponding to the support pins 219 are formed, and when the mounting table 213 is lowered, the upper ends of the support pins 219 passing through the pin insertion holes 220 receive the substrate W, and the substrate W can be transferred between the substrate W and a transfer arm (not shown) entering from the outside. On the lower side wall of the processing vessel 201, a transfer port 221 is provided to allow the transfer arm to enter, and the transfer port 221 is provided with a gate valve 238 that can be opened and closed.
[0062] A chuck power supply 223 is connected to the electrode 216b of the electrostatic chuck 216 via a power supply line 222, and a DC voltage is applied from the chuck power supply 223 to the electrode 216b, thereby attracting and holding the substrate W by electrostatic force. A bias high-frequency power supply 224 is also connected to the power supply line 222, and a bias high-frequency power is supplied to the electrode 216b of the electrostatic chuck 216 via the power supply line 222, so that the bias power is applied to the substrate W. The frequency of this high-frequency power is preferably 400 kHz to 60 MHz, and for example, 13.56 MHz is adopted.
[0063] Meanwhile, a transmission plate 226 made of a dielectric material is airtightly installed on the ceiling of the processing vessel 201 via a seal member 227. A plasma generation source 228 is installed above the transmission plate 226 to generate plasma in the processing space S inside the processing vessel 201 by converting a plasma excitation gas into plasma.
[0064] The plasma generation source 228 has an induction coil 230 arranged corresponding to the transparent plate 226, and a high-frequency power supply 231 for generating plasma, for example, of 13.56 MHz, is connected to this induction coil 230, so that high-frequency power is introduced into the processing space S via the transparent plate 226 to form an induced electric field.
[0065] A metal baffle plate 232 for diffusing the introduced high frequency power is provided directly below the transmission plate 226. A target 233, for example, with a cross section inclined inward, is provided below the baffle plate 232 so as to surround the upper side of the processing space S. The target 233 is made of the material of the film to be formed. When forming both the first metal-containing unit film 2 and the second metal-containing unit film 3, a plurality of targets 233 may be provided so as to correspond to these materials, respectively. Cosputtering using a plurality of targets may also be performed. A variable voltage DC power supply 234 for the target is connected to the target 233, which applies DC power to attract Ar ions. An AC power supply may be used instead of the DC power supply.
[0066] In addition, a magnet 235 is provided on the outer periphery of the target 233. The target 233 is sputtered by Ar ions in the plasma, and particles are emitted from the target 233, and most of the particles are ionized when passing through the plasma.
[0067] A cylindrical protective cover member 236 is provided below the target 233 so as to surround the processing space S. The protective cover member 236 is grounded. An inner end of the protective cover member 236 is provided so as to surround the outer periphery of the mounting table 213.
[0068] Each component constituting the plasma sputtering apparatus 200 is controlled by a control unit 240. The control unit 240 has a main control unit consisting of a computer (CPU) that controls each component, an input device, an output device, a display device, and a storage device. The storage device stores parameters for various processes executed by the plasma sputtering apparatus 200. The storage device also has a storage medium in which a program for controlling the processes executed by the plasma sputtering apparatus 200, that is, a processing recipe, is stored. The main control unit calls up a predetermined processing recipe stored in the storage medium, and causes the plasma sputtering apparatus 200 to execute a predetermined operation based on the processing recipe.
[0069] In the plasma sputtering apparatus 200 configured as above, the substrate W is carried into the processing vessel 201, placed on the mounting table 213 and attracted by the electrostatic chuck 216, and the following operations are performed under the control of the control unit 240. At this time, the mounting table 213 is temperature-controlled by controlling the supply of coolant to the cooling jacket 215 and the power supply to the resistance heater 237 based on the temperature detected by a thermocouple (not shown).
[0070] First, the vacuum pump 206 is operated to set the processing vessel 201 in a predetermined vacuum state, and the gas control unit 210 is operated to flow Ar gas at a predetermined flow rate while controlling the throttle valve 205 to maintain the processing vessel 201 at a predetermined vacuum level. Thereafter, DC power is applied to the target 233 from the variable voltage DC power supply 234, and further, RF power (plasma power) is supplied from the RF power supply 231 of the plasma generation source 228 to the induction coil 230. Meanwhile, a predetermined RF power for bias is supplied from the bias RF power supply 224 to the electrode 216b of the electrostatic chuck 216.
[0071] As a result, in the processing vessel 201, argon plasma is formed by the high frequency power supplied to the induction coil 230, and argon ions are generated, and these ions are attracted to the DC voltage applied to the target 233 and collide with the target 233, which is sputtered to release particles. At this time, the amount of particles released is optimally controlled by the DC voltage applied to the target 233.
[0072] Furthermore, most of the particles from the sputtered target 233 are ionized as they pass through the plasma and are scattered downward.
[0073] When the ions enter an ion sheath region having a thickness of about several mm that is formed on the surface of the substrate W by the bias high-frequency power applied from the bias high-frequency power supply 224 to the electrode 216b of the electrostatic chuck 216, the ions are attracted to the substrate W side with strong directionality so as to be accelerated, and are deposited on the substrate W. As a result, a desired film is formed on the substrate W.
[0074] When both the first metal-containing unit film 2 and the second metal-containing unit film 3 are formed by sputtering, the metal-containing film 1 can be formed by successively forming these films in the plasma sputtering apparatus 200 simply by switching the targets.
[0075] After the film formation is completed, the processing vessel 201 is purged, the mounting table 213 is lowered, the gate valve 238 is opened, and the substrate W is unloaded.
[0076] [Deposition by ALD or CVD] FIG. 21 is a cross-sectional view showing an example of a film formation apparatus for forming a film by ALD or CVD. As shown in FIG. 21, the film forming apparatus 300 includes a processing vessel 301 , a susceptor 302 , a shower head 303 , an exhaust unit 304 , a gas supply mechanism 305 , and a control unit 307 .
[0077] The processing vessel 301 is made of metal and has a substantially cylindrical shape. A loading / unloading port 311 for loading / unloading the substrate W is formed in a side wall of the processing vessel 301, and the loading / unloading port 311 can be opened and closed by a gate valve 312. An annular exhaust duct 313 having a rectangular cross section is provided on the main body of the processing vessel 301. A slit 313a is formed along the inner peripheral surface of the exhaust duct 313. An exhaust port 313b is formed in the outer wall of the exhaust duct 313. A ceiling wall 314 is provided on the upper surface of the exhaust duct 313 so as to close the upper opening of the processing vessel 301. A seal ring 315 seals the space between the ceiling wall 314 and the exhaust duct 313 airtightly.
[0078] The susceptor 302 is for supporting the substrate W horizontally in the processing vessel 301. The susceptor 302 is in the shape of a disk having a size corresponding to that of the substrate W, and is supported by a support member 323. The susceptor 302 is made of a ceramic material or a metal material, and has a heater 321 for heating the substrate W embedded therein. The heater 321 is powered by a heater power supply (not shown) and generates heat. The output of the heater 321 is controlled by a temperature signal from a thermocouple (not shown) provided near the substrate mounting surface on the upper surface of the susceptor 302, thereby controlling the temperature of the substrate W to a predetermined temperature.
[0079] The susceptor 302 is provided with a cover member 322 made of ceramics such as alumina so as to cover the outer peripheral region of the substrate mounting surface and the side surfaces of the susceptor 302 .
[0080] A support member 323 supporting the susceptor 302 extends from the center of the bottom surface of the susceptor 302 to below the processing vessel 301 through a hole formed in the bottom wall of the processing vessel 301, and its lower end is connected to a lifting mechanism 324. The lifting mechanism 324 enables the susceptor 302 to be raised and lowered via the support member 323 between a processing position shown by a solid line in Fig. 21 and a transfer position shown by a dashed line below the processing position where the substrate W can be transferred. A flange member 325 is attached to the support member 323 below the processing vessel 301, and a bellows 326 is provided between the bottom surface of the processing vessel 301 and the flange member 325 to separate the atmosphere inside the processing vessel 301 from the outside air and to expand and contract as the susceptor 302 is raised and lowered.
[0081] Three support pins 327 (only two shown) are provided near the bottom surface of the processing vessel 301 so as to protrude upward from a lift plate 327a. The support pins 327 can be raised and lowered via the lift plate 327a by a lift mechanism 328 provided below the processing vessel 301, and can be inserted into through holes 302a provided in the susceptor 302 at the transfer position and can be protruded and retracted relative to the upper surface of the susceptor 302. By raising and lowering the support pins 327 in this manner, the substrate W is transferred between a substrate transfer mechanism (not shown) and the susceptor 302.
[0082] The shower head 303 is a metal member for supplying a processing gas into the processing vessel 301 in a shower-like manner, and is provided to face the susceptor 302 and has approximately the same diameter as the susceptor 302. The shower head 303 has a main body 331 fixed to the top wall 314 of the processing vessel 301 and a shower plate 332 connected below the main body 331. A gas diffusion space 333 is formed between the main body 331 and the shower plate 332, and a gas introduction hole 336 provided to penetrate the center of the main body 331 and the top wall 314 of the processing vessel 301 is connected to the gas diffusion space 333. A circular protrusion 334 protruding downward is formed on the periphery of the shower plate 332, and a gas discharge hole 335 is formed on the inner flat surface of the circular protrusion 334 of the shower plate 332.
[0083] When the susceptor 302 is in the processing position, a processing space 337 is formed between the shower plate 332 and the susceptor 302, and the annular protrusion 334 and the upper surface of the cover member 322 of the susceptor 302 are close to each other to form an annular gap 338.
[0084] The exhaust unit 304 is for exhausting the inside of the processing vessel 301, and includes an exhaust pipe 341 connected to an exhaust port 313b of the exhaust duct 313, and an exhaust mechanism 342 having a vacuum pump, a pressure control valve, etc., connected to the exhaust pipe 341. During processing, gas inside the processing vessel 301 reaches the exhaust duct 313 through the slit 313a, and is exhausted from the exhaust duct 313 through the exhaust pipe 341 by the exhaust mechanism 342 of the exhaust unit 304.
[0085] The gas supply mechanism 305 is for supplying a plurality of process gases for film formation to the shower head 303, and has supply sources and supply pipes for each process gas. The process gases supplied include a film formation source gas, a reaction gas, and an inert gas. The inert gas is used as a purge gas, a carrier gas, and a dilution gas. The supply pipes for each process gas of the gas supply mechanism 305 merge into a pipe 366 and reach the shower head 303.
[0086] As the film-forming raw gas, various gases can be used depending on the metal of the film to be formed. For example, in the case of TiN film and Ti film, TiCl4 gas, TiI4 gas, TiBr4 gas, TiBr3 gas, TiI5 gas, and TiF5 gas can be used. In the case of NbN film, NbCl4 gas, NbF4 gas, NbI4 gas, NbBr5 gas, NbF5 gas, NbOBr3 gas, NbOCl3 gas, NbOBr3 gas, and NbO2F gas can be used. In the case of VN film and V film, VOBr3 gas, VOCl3 gas, VOF3 gas, V(CO)6 gas, VCl4 gas, VF5 gas, VF4 gas, VOBr gas, VOCl gas, VOBr2 gas, VOCl2 gas, and VOF2 gas can be used. In the case of a WN film and a W film, W(CO)6 gas, WBr2 gas, WCl2 gas, WI2 gas, WBr3 gas, WCl3 gas, WBr5 gas, WCl5 gas, WF5 gas, WOBr3 gas, WO2Cl3 gas, WBr6 gas, WCl6 gas, WO2Br2 gas, WO2Cl2 gas, WO2I2 gas, WF6 gas, WOBr4 gas, WOBr4 gas, WOCl4 gas, and WOF4 gas can be used. In the case of a TaN film, TaBr5 gas, TaCl5 gas, TaF5 gas, and TaI5 gas can be used. In the case of a MoN film and a Mo film, Mo(CO)6 gas, MoCl5 gas, MoF5 gas, MoOCl3 gas, MoF5 gas, MoCl3 gas, MoF6 gas, MoOF4 gas, MoOCl4 gas, and MoO2Cl2 gas can be used. In the case of a Ru film, Ru(CO) 12For Co and Ni films, cobalt amidinate and nickel amidinate can be used. For Al films, trimethylaluminum (TMA) gas can be used. For Mn films, MnOF3 gas and MnO3Cl gas can be used.
[0087] Depending on the type of the film-forming source gas and the reactive gas, the gas may be turned into plasma by applying high-frequency power to the shower head 303, for example.
[0088] The control unit 307 has a main control unit consisting of a computer (CPU) that controls each component of the film forming apparatus 300, an input device, an output device, a display device, and a storage device. The storage device stores parameters for various processes executed by the film forming apparatus 300. The storage device also has a storage medium that stores a program for controlling the processes executed by the film forming apparatus 300, that is, a process recipe. The main control unit calls up a predetermined process recipe stored in the storage medium, and causes the film forming apparatus 300 to execute a predetermined operation based on the process recipe.
[0089] In the film forming apparatus 300 configured as above, first, the gate valve 312 is opened, and the substrate W is loaded into the processing vessel 301 via the load / unload port 311 by a transfer device (not shown), and placed on the susceptor 302. Thereafter, the transfer device is retracted, and the susceptor 302 is raised to the processing position. Then, the gate valve 312 is closed, and the inside of the processing vessel 301 is maintained at a predetermined reduced pressure, and the temperature of the susceptor 302 is controlled to a desired temperature by the heater 321.
[0090] In this state, a processing gas is supplied from the gas supply mechanism 305 into the processing vessel 301 to form a desired film on the substrate W by ALD or CVD.
[0091] In film formation by ALD, a source gas and a reactive gas are alternately supplied into the processing vessel 301 with an inert gas purging the processing vessel 301. For example, when forming a TiN film, TiCl4 gas is supplied as a source gas and NH3 gas is supplied as a reactive gas with an inert gas purging. In addition, in film formation by CVD, a source gas and a reactive gas are simultaneously supplied into the processing vessel 301. For example, Ru(CO) 12 In some cases, such as the formation of a Ru film using a gas, film formation may proceed by thermal decomposition of a film-forming source gas without using a reactive gas.
[0092] When both the first metal-containing unit film 2 and the second metal-containing unit film 3 are formed by ALD or CVD, the metal-containing film 1 can be formed by successively forming these films in the film formation apparatus 300 simply by switching the process gas.
[0093] After the film formation is completed, the inside of the processing vessel 301 is purged, the susceptor 302 is lowered, the gate valve 312 is opened, and the substrate W is unloaded.
[0094] <Other applications> Although the embodiments have been described above, the embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims.
[0095] For example, in the above embodiment, the materials of the first metal-containing unit film and the second metal-containing unit film are exemplified, but these are merely examples and other metal-containing films may be used. In addition, the plasma sputtering device 200 is exemplified as a device for forming a film by PVD, and the film forming device 300 is exemplified as a device for forming a film by ALD or CVD, but the present invention is not limited to these, and various devices can be used. Furthermore, in the above embodiment, the film forming method is exemplified as PVD, ALD, and CVD, but the present invention is not limited to these as long as it is a thin film forming technology.
[0096] Furthermore, applications of the metal-containing film have been exemplified by fine wiring, electrodes with pillar or cylinder structures, barrier films, and metal hard masks, but are not limited thereto. [Explanation of symbols]
[0097] 1;Metal-containing film 2: First metal-containing unit membrane 3. Second metal-containing unit membrane 101,121,131,141,W;Substrate 105;Metal-containing film (fine wiring) 110,111;Fine wiring structure 114: Metal-containing films (barrier films) 120,130; Capacitor 122: Metal-containing film (lower electrode of pillar structure) 132: Metal-containing film (bottom electrode of cylindrical structure) 140;Structure 143: Metal-containing film (metal hard mask) 200: Plasma sputtering device 300; Film deposition equipment
Claims
1. a first metal-containing unit film having a thickness less than the critical diameter for crystal nucleation and a second metal-containing unit film having a thickness less than the critical diameter for crystal nucleation and different from the first metal-containing unit film, the first metal-containing unit film being alternately laminated, the second metal-containing unit film having a thickness less than the critical diameter for crystal nucleation and a laminate structure not including a grain boundary; A metal-containing film, wherein an element that increases a degree of supercooling is added to at least one of the first metal-containing unit film and the second metal-containing unit film.
2. The metal-containing film of claim 1 , wherein the element that increases the degree of supercooling has an interaction parameter of 0 or greater with the parent phase material to which it is added.
3. When one of the first metal-containing unit film and the second metal-containing unit film to which the element that increases the degree of supercooling is added is an Al film, the element that increases the degree of supercooling is Si; When one of the first metal-containing unit film and the second metal-containing unit film to which the element for increasing the degree of supercooling is added is a Ru film, the element for increasing the degree of supercooling is selected from Ir, Pd, Ni, Co, and Mn; When the first metal-containing unit film or the second metal-containing unit film to which the element for increasing the degree of supercooling is added is a Co film, the element for increasing the degree of supercooling is selected from Ni, Cu, Pd, and Ru; When one of the first metal-containing unit film and the second metal-containing unit film to which the element for increasing the degree of supercooling is added is a W film, the element for increasing the degree of supercooling is selected from Mo, Ta, Nb, Ti, and Mn; When one of the first metal-containing unit film and the second metal-containing unit film to which the element for increasing the degree of supercooling is added is a Mo film, the element for increasing the degree of supercooling is selected from W, Ta, Nb, Ti, and Mn; When the first metal-containing unit film or the second metal-containing unit film to which the element for increasing the degree of supercooling is added is a Ti film, the element for increasing the degree of supercooling is selected from Zr, Hf, V, W, Mo, Nb, and Ta; 3. The metal-containing film according to claim 2, wherein when one of the first metal-containing unit film and the second metal-containing unit film to which the element that increases the supercooling degree is added is a Mn film, the element that increases the supercooling degree is selected from the group consisting of Ru, Fe, Mo, and W.
4. The metal-containing film according to claim 1 , which is used as an electrode having a metal pillar structure or a cylinder structure.
5. The metal-containing film of claim 1 used as a barrier film.
6. The metal-containing film according to claim 1 , which is used as an interconnect metal.
7. The metal-containing film of claim 1 , which is used as a metal hard mask.
8. A laminate structure having no grain boundaries, comprising a first metal-containing unit film having a thickness less than the critical diameter for crystal nucleation and a second metal-containing unit film having a thickness less than the critical diameter for crystal nucleation and different from the first metal-containing unit film, which are alternately laminated, Metal-containing films used as electrodes in metal pillar or cylinder structures.
9. A laminate structure having no grain boundaries, comprising a first metal-containing unit film having a thickness less than the critical diameter for crystal nucleation and a second metal-containing unit film having a thickness less than the critical diameter for crystal nucleation and different from the first metal-containing unit film, which are alternately laminated, Metal-containing films used as metal hard masks.
10. The metal-containing film according to claim 1 , wherein the first metal-containing unit film and the second metal-containing unit film are metal nitride films or metal films.
11. The metal-containing film of claim 10, wherein the first metal-containing unit film and the second metal-containing unit film are either a combination of one being a metal nitride film and the other being a metal film, a combination of both being metal nitride films, or a combination of both being metal films.
12. The metal nitride film is TiN, NbN, VN, WN, TaN, MoN, W 2 N 3 12. The metal-containing film of claim 11 , wherein the metal film is selected from Ru, Co, Ni, Mo, W, Al, Ti, V, Mn, Si, Mg.
13. The metal-containing film according to claim 11 or 12, wherein the combination of one metal nitride film and the other metal film is selected from TiN-W, TiN-Mo, TiN-Ru, TaN-W, TaN-Mo, and TaN-Ru.
14. The combinations of both metal nitride films are TiN-TaN, TiN-NbN, TiN-MoN, TiN-W 2 N 3 , TaN-NbN, TaN-W 2 N 3 13. The metal-containing film of claim 11 or claim 12, wherein the metal-containing film is selected from:
15. 13. The metal-containing film of claim 11 or claim 12, wherein the both-metal film combination is selected from Si-Al, W-Al, Mg-Al, W-Ti, V-Ti, and Mg-Ti.
16. A method for producing a metal-containing film, comprising alternately performing a step of forming a first metal-containing unit film on a substrate with a thickness less than a critical diameter for crystal nucleation and a step of forming a second metal-containing unit film different from the first metal-containing unit film with a thickness less than the critical diameter for crystal nucleation, and adding an element that increases a degree of supercooling to at least one of the first metal-containing unit film and the second metal-containing unit film, thereby producing a metal-containing film having a laminate structure that does not include grain boundaries.
17. The method for producing a metal-containing film according to claim 16, wherein the first metal-containing unit film and the second metal-containing unit film are formed by any one of PVD, ALD, and CVD.
18. 18. The method for producing a metal-containing film according to claim 16, wherein the first metal-containing unit film and the second metal-containing unit film are metal nitride films or metal films.
19. 20. The method for producing a metal-containing film according to claim 18, wherein the first metal-containing unit film and the second metal-containing unit film are either a combination of one being a metal nitride film and the other being a metal film, a combination of both being metal nitride films, or a combination of both being metal films.
20. 20. The method for producing a metal-containing film according to claim 16, wherein the element that increases the degree of supercooling has an interaction parameter of 0 or more between the element and a parent phase material to which the element is added.
Citation Information
Patent Citations
Semiconductor device
JP1988155743A
Multilayered interconnection
JP1992061125A
Multilayered barrier-metal thin film for copper interconnect by alcvd
JP2002329680A
Semiconductor device and its manufacturing method, and plating solution
JP2003324148A
Laminated circuit material
JP2005294321A