Flexographic printing original plate, flexographic printing plate, and method for manufacturing flexographic printing plate
The flexographic printing plate with a structured ink receiving layer addresses ink accumulation and uneven tones by ensuring proper ink entanglement and dot thickness, improving the quality and durability of printed materials.
Patent Information
- Application Number
- JP2022580683
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-10
- Filing Date
- 2022-02-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-02-10
AI Technical Summary
Flexographic printing plates using CTP technology face issues with ink accumulation in relief recesses leading to plate smearing, uneven tones due to thickened halftone dots, and poor ink entanglement, which affects the quality of printed materials.
A flexographic printing original plate with a specific structure comprising a support, photosensitive resin composition layer, and an ink receiving layer with a thickness of 5 μm to 50 μm, containing polymer particles with carboxyl groups and hydroxyl groups, and a binder resin, which enhances ink entanglement and prevents dot thickening.
The solution results in a flexographic printing plate with improved ink entanglement, preventing dot thickening and maintaining even tones, thus enhancing the quality and durability of printed materials.
Smart Images

Figure 0007595685000005 
Figure 0007595685000006 
Figure 0007595685000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a flexographic printing original plate, a flexographic printing plate, and a method for producing a flexographic printing plate. [Background technology]
[0002] Flexographic printing is a type of letterpress printing, and has the advantage that it can be applied to a variety of substrates because soft materials such as rubber and synthetic resin are used for the flexographic printing plates. Conventional methods for manufacturing flexographic printing plates used in flexographic printing include a method using negative film to make plates, and a method using computer-generated platemaking technology (hereinafter referred to as CTP technology), in which information processed on a computer is directly drawn on the printing plate to create a relief. In the method using CTP technology, the manufacturing process of negative film is unnecessary, and it is possible to reduce costs and the time required for manufacturing negative film, so in recent years, the method using CTP technology is becoming mainstream.
[0003] When using CTP technology, the original plate for a flexographic printing plate (hereinafter also referred to as a "flexographic printing original plate") is generally made by laminating a photosensitive resin composition layer, a protective layer (barrier layer), and an infrared ablation layer in this order on a substrate such as a PET resin.
[0004] The preparation of a flexographic printing plate using the CTP technique is carried out, for example, as follows. First, a uniform cured layer is provided by performing back exposure in which ultraviolet light is irradiated to the entire surface of the photosensitive resin composition layer through a substrate made of a film such as PET resin. Next, a laser is irradiated to the infrared ablation layer on the photosensitive resin composition layer to draw, thereby removing a part of the infrared ablation layer to prepare an image mask. Furthermore, relief exposure is performed in which ultraviolet light is irradiated to the photosensitive resin composition layer through the image mask, thereby photocuring the part where the infrared ablation layer has been removed. Thereafter, the unexposed part of the photosensitive resin composition layer (i.e., the part not photocured) is removed to form a relief image, which is a desired image, to obtain a flexographic printing plate.
[0005] When a flexographic printing original plate is irradiated with ultraviolet light to perform relief exposure, if oxygen is present, oxygen radicals generated from the oxygen inhibit the photocuring reaction of the photosensitive resin composition, resulting in insufficient photocuring of the photosensitive resin composition layer.
[0006] In view of this, conventionally, a technique has been disclosed for adjusting the shape of the printed dots, or for forming a printed dot structure having a flat top and a steep shoulder by laminating a laser-ablationable mask layer on the photosensitive resin composition layer and providing a barrier layer for blocking oxygen on the mask layer (see, for example, Patent Document 1). The barrier layer is removed after the photosensitive resin composition layer is irradiated with light.
[0007] Furthermore, a technique has been disclosed in which a water-soluble barrier layer is provided on a flexographic printing original plate for the purpose of blocking oxygen in the atmosphere and protecting the surface of the photosensitive resin composition layer (see, for example, Patent Document 2). The barrier layer is removed together with the uncured portion of the photosensitive resin composition layer during development, and the barrier layer that was on the photocured portion of the photosensitive resin composition layer is also removed.
[0008] In either case, the barrier layer is intended to protect the photosensitive resin composition, and is removed before use as a printing plate.
[0009] In addition, flexographic printing plates have a problem in that ink accumulates in the recesses of the relief, soiling the printed matter. In particular, when printing is continued for a long time, ink often seeps into the recesses of the printing plate (hereinafter also referred to as "plate surface soiling"), and parts that are not the original image are printed. In such cases, it is necessary to stop printing and wipe the surface of the printing plate with a cloth or the like using a cleaning solution such as alcohol, which is economically disadvantageous.
[0010] To improve this, it has been proposed to incorporate an organosilicon compound into the photosensitive resin composition of the flexographic printing plate (see, for example, Patent Document 3). However, simply adding an organosilicon compound to the photosensitive resin composition causes problems such as a decrease in the transparency of the photosensitive resin composition and a decrease in the ability to maintain the shape of the composition even when heat or load is applied to the composition during storage or transportation (cold flow resistance), so it is important to design an appropriate organosilicon compound.
[0011] However, if a photosensitive resin composition is designed so that ink does not easily accumulate in the relief recesses, the relief surface formed from the same resin composition will naturally be less likely to accept ink. To solve this problem, a flexographic printing plate has been proposed that has a two-layer structure consisting of a cap layer that accepts ink and a composition layer that repels ink, with the difference in surface tension between the two layers being 5 dynes / cm or more (see, for example, Patent Document 4). [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Special Publication No. 2014-507677 [Patent Document 2] Patent No. 5573675 [Patent Document 3] WO2007-116941 [Patent Document 4] Special Publication No. 2015-513700 Summary of the Invention [Problem to be solved by the invention]
[0013] However, the flexographic printing plate described in Patent Document 4 has a large surface tension difference, and the surface tension of the photosensitive resin composition layer is too low, so that the ink repelled from the recesses wraps around the ink-receiving areas, and more ink than necessary is supplied. As a result, there was a problem that the halftone dots in the highlight areas of the print are unintentionally thicker than the desired size, the continuous change in tone (gradation) from dark to light colors disappears, and steps occur in the tone, making it impossible to properly express gradation, a phenomenon known as "tone jump."
[0014] In view of the problems with the conventional technology, the present invention aims to provide a flexographic printing original plate capable of producing a flexographic printing plate having excellent printing characteristics, including good ink adhesion and no thickening of dots in highlighted areas, as well as a flexographic printing plate and a method for producing the same. [Means for solving the problem]
[0015] As a result of intensive research into solving the above problems, the inventors discovered that the above problems could be solved by forming an ink-receiving layer of a prescribed thickness, and thus completed the present invention.
[0016] That is, the present invention is as follows. [1] A flexographic printing original plate comprising at least a support, a photosensitive resin composition layer, an ink-receiving layer, and an infrared ablation layer laminated in this order, The thickness of the ink receiving layer is 5 μm or more and 50 μm or less, the ink receiving layer contains polymer particles having a butadiene skeleton and having a carboxyl group and / or a hydroxyl group, and / or polymer particles in which a monobasic or polybasic acid monomer is polymerized; The content of the polymer particles is 20% by mass or more and 95% by mass or less with respect to 100% by mass of the ink receiving layer. Flexographic printing plate. [2] The ink receiving layer further contains a binder resin having a basic group. The flexographic printing plate precursor according to [1]. [3] The binder resin having a basic group includes a polyamide resin and / or a polyurethane resin. The flexographic printing plate precursor according to [2]. [4] The ink receiving layer further contains a polyvinyl alcohol resin. The flexographic printing plate precursor according to any one of [1] to [3]. [5] The ink receiving layer further comprises swellable mica. The flexographic printing plate precursor according to any one of [1] to [4]. [6] The ink receiving layer further contains a water-soluble photopolymerization initiator and a water-soluble polymerizable compound. The flexographic printing plate precursor according to any one of [1] to [5]. [7] The water-soluble polymerizable compound has an amide skeleton and / or a urethane skeleton. The flexographic printing plate precursor according to [6]. [8] the ink receiving layer further contains a water-soluble resin having an alkylene oxide chain; The flexographic printing plate precursor according to any one of [1] to [7]. [9] A flexographic printing plate comprising at least a support, a photocured photosensitive resin composition layer, and an ink-receiving layer laminated in this order, The thickness of the ink receiving layer is 5 μm or more and 50 μm or less, the ink receiving layer contains polymer particles having a butadiene skeleton and having a carboxyl group and / or a hydroxyl group, and / or polymer particles in which a monobasic or polybasic acid monomer is polymerized; Flexographic printing plate.
[10] The difference (Ei-Ep) between the surface free energy Ei of the ink receiving layer and the surface free energy Ep of the photocured photosensitive resin composition layer is 0 mJ / m 2 Greater than 5mJ / m 2 Below is the The flexographic printing plate according to [9].
[11] The difference (Ei-Ep) between the surface free energy Ei of the ink receiving layer and the surface free energy Ep of the photocured photosensitive resin composition layer is 0 mJ / m 2 Greater than 4mJ / m 2 Below is the The flexographic printing plate according to
[10] .
[12] The difference (Ei-Ep) between the surface free energy Ei of the ink receiving layer and the surface free energy Ep of the photocured photosensitive resin composition layer is 0.5 mJ / m 2 Greater than 3.5mJ / m 2 Below is the The flexographic printing plate according to
[10] .
[13] The ink receiving layer further comprises a water-soluble polymer having an alkylene oxide chain. The flexographic printing plate according to any one of items [9] to
[12] .
[14] The content of the polymer particles is 20% by mass or more and 95% by mass or less with respect to 100% by mass of the ink receiving layer. The flexographic printing plate according to any one of items [9] to
[13] .
[15] The film zeta potential of the ink receiving layer is positive. The flexographic printing plate according to any one of [9] to
[14] .
[16] The ink receiving layer further contains a binder resin having a basic group. The flexographic printing plate according to any one of [9] to
[15] .
[17] The binder resin having a basic group includes a polyamide resin and / or a polyurethane resin. The flexographic printing plate according to
[16] .
[18] The ink receiving layer further contains a polyvinyl alcohol resin. The flexographic printing plate according to any one of [9] to
[17] .
[19] The ink receiving layer further contains swellable mica. The flexographic printing plate according to any one of [9] to
[18] .
[20] The ink receiving layer further contains a water-soluble photopolymerization initiator and a water-soluble polymerizable compound. The flexographic printing plate according to any one of [9] to
[19] . 〔twenty one〕 The water-soluble polymerizable compound has an amide skeleton and / or a urethane skeleton. The flexographic printing plate according to
[20] . 〔twenty two〕 1. A method for producing a flexographic printing plate, comprising the steps of: A step of laser ablating the infrared ablation layer of the flexographic printing plate precursor according to any one of [1] to [8] to produce a negative pattern; an exposure step of exposing the photosensitive resin composition layer through the ink receiving layer; removing unexposed portions of the photosensitive resin composition layer and the ink-receiving layer; A method for producing a flexographic printing plate comprising the steps of: Effect of the Invention
[0017] According to the present invention, it is possible to provide a flexographic printing original plate capable of producing a flexographic printing plate having excellent printing characteristics, including good ink adhesion and no thickening of dots in highlighted areas, as well as a flexographic printing plate and a method for producing the same. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a schematic cross-sectional view of a flexographic printing original plate according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing one embodiment of a method for producing a flexographic printing plate using the flexographic printing base plate of the present embodiment. [Diagram 3] FIG. 2 is a schematic diagram showing another embodiment of a method for producing a flexographic printing plate using the flexographic printing plate precursor of the present embodiment. [Figure 4]FIG. 2 is a schematic diagram for explaining ink adhesion. [Diagram 5] FIG. 1 is a schematic cross-sectional view of a flexographic printing plate obtained using the flexographic printing original plate of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Below, we will explain in detail the form for implementing the present invention (hereinafter referred to as the "present embodiment"). However, the present invention is not limited to this, and various modifications are possible without departing from the gist of the present invention.
[0020] 1. Flexographic printing plate The flexographic printing plate precursor of this embodiment has at least a support, a photosensitive resin composition layer, an ink-receiving layer, and an infrared ablation layer laminated in that order, the ink-receiving layer having a thickness of 5 μm or more and 50 μm or less, the ink-receiving layer containing, as polymer particles (a-2), polymer particles (a-2-1) having a butadiene skeleton and having a carboxyl group and / or a hydroxyl group, and / or polymer particles (a-2-2) formed by polymerization of a monobasic or polybasic acid monomer, and the content of the polymer particles (a-2) is 20% by mass or more and 95% by mass or less relative to 100% by mass of the ink-receiving layer.
[0021] 1 shows a schematic cross-sectional view of the flexographic printing plate blank of this embodiment. The flexographic printing plate blank 10 of this embodiment is formed by sequentially laminating a support 11, a photosensitive resin composition layer 12 on which the concave-convex pattern of the flexographic printing plate is formed, an ink receiving layer 13 disposed on the top of the concave-convex pattern of the flexographic printing plate, and an infrared ablation layer 14 that functions as a mask when the concave-convex pattern of the flexographic printing plate is formed. If necessary, a functional layer such as an adhesive layer may be provided between these layers. The configuration of the flexographic printing plate blank of this embodiment will be described in detail below.
[0022] 1.1.Support The support used in the flexographic printing original plate of the present embodiment is not particularly limited, and examples thereof include polypropylene film, polyethylene film, polyester films such as polyethylene terephthalate and polyethylene naphthalate, polyamide film, etc. Among these, polyester film is preferable as the support.
[0023] The thickness of the support is preferably 75 μm to 300 μm.
[0024] Furthermore, for the purpose of increasing the adhesive strength between the support and the photosensitive resin composition layer, an adhesive layer may be provided between the support and the photosensitive resin composition layer.
[0025] The material for the adhesive layer is not particularly limited, but examples thereof include compositions having a binder polymer such as polyurethane, polyamide, or thermoplastic elastomer, and an active adhesive component such as an isocyanate compound or an ethylenically unsaturated compound.
[0026] Furthermore, various auxiliary additives such as plasticizers, thermal polymerization inhibitors, ultraviolet absorbers, antihalation agents, light stabilizers, photopolymerization initiators, photopolymerizable monomers, dyes, etc. may be added to the adhesive layer.
[0027] In order to further increase the adhesive strength between the adhesive layer and the support, at least one undercoat layer may be provided between the adhesive layer and the support.
[0028] 1.2. Photosensitive resin composition layer The flexographic printing plate precursor of this embodiment has a photosensitive resin composition layer on a support. As a material for the photosensitive resin composition layer, for example, a photosensitive resin composition containing a thermoplastic elastomer (a-1), polymer particles (a-2), a photopolymerizable monomer (a-3), and a photopolymerization initiator (a-4) can be preferably mentioned. In addition to the upper components, the photosensitive resin composition layer may contain a liquid diene silicone compound (a-6) (f) or the like as necessary. These components (a) to (f) will be described in detail below, but as these components, for example, those described in "JP Patent Publication No. 2018-120131" may be used.
[0029] 1.2.1. Thermoplastic elastomer (a-1) The thermoplastic elastomer (a-1) is not particularly limited, but may be, for example, a thermoplastic elastomer having a structural unit derived from a conjugated diene and / or a vinyl aromatic hydrocarbon. The thermoplastic elastomer may be a homopolymer or a copolymer. In the case of a copolymer, the thermoplastic elastomer may be a random polymer or a block polymer.
[0030] Among these, thermoplastic elastomers containing at least one polymer block mainly composed of a conjugated diene and at least one polymer block mainly composed of a vinyl aromatic hydrocarbon are preferred.
[0031] The term "mainly composed of" as used throughout this specification means that 60% by weight or more of a polymer block is composed of a given monomer.
[0032] In the polymer block mainly composed of a conjugated diene, the content of the conjugated diene unit in the polymer block is preferably 80% by mass or more, and more preferably 90% by mass or more.
[0033] The conjugated diene is not particularly limited, but examples thereof include monomers such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, and chloroprene. Among these, 1,3-butadiene is particularly preferred from the viewpoint of wear resistance. These monomers may be used alone or in combination of two or more.
[0034] In the polymer block mainly composed of a conjugated diene, the vinyl content is preferably 5 to 50 mol%, more preferably 8 to 50 mol%, and even more preferably 10 to 40 mol%, based on the total amount of conjugated diene units from the viewpoint of printing plate formability. Here, the "vinyl content" refers to, for example, the content of 1,2-butadiene or 3,4-isoprene.
[0035] The number average molecular weight of the polymer block mainly composed of a conjugated diene is preferably from 20,000 to 250,000, more preferably from 30,000 to 200,000, and even more preferably from 40,000 to 150,000, from the viewpoint of printing durability.
[0036] The polymer block mainly made of conjugated diene may contain an alkylene unit. The method of introducing the alkylene unit is not particularly limited, but examples thereof include a method of polymerizing a monoolefin such as ethylene or butylene as a raw material monomer of the polymer block mainly made of conjugated diene, and a method of hydrogenating the conjugated diene polymer block. In particular, from the viewpoint of availability, the method of hydrogenating the polymer block mainly made of conjugated diene is preferred.
[0037] In the polymer block mainly composed of a conjugated diene, the content of the alkylene unit is preferably 5 to 50 mol%, more preferably 10 to 35 mol%, and even more preferably 10 to 25 mol%, based on the total amount of the monomer units constituting the polymer block. When the content of the alkylene unit is 5 mol% or more, the solvent resistance tends to be further improved. Also, when the content of the alkylene unit is 50 mol% or less, the transparency of the photosensitive resin composition layer tends to be further improved.
[0038] The polymer block mainly composed of conjugated diene preferably contains an alkylene unit, more preferably contains all of a 1,4-butadiene unit, a 1,2-butadiene (vinyl) unit and a butylene (alkylene) unit. In this case, the polymer block mainly composed of conjugated diene more preferably contains 25 to 70 mol% of a 1,4-butadiene unit, 0 to 50 mol% of a 1,2-butadiene (vinyl) unit and 10 to 50 mol% of a butylene unit. Such a polymer block can be obtained by hydrogenating a polymer block mainly composed of butadiene.
[0039] The conjugated diene, the vinyl content of the conjugated diene, and the content and ratio of vinyl aromatic hydrocarbons were measured using a nuclear magnetic resonance spectrometer ( 1 H-NMR can be used to measure the
[0040] The vinyl aromatic hydrocarbon is not particularly limited, but examples thereof include monomers such as styrene, t-butylstyrene, divinylbenzene, 1,1-diphenylstyrene, N,N-dimethyl-p-aminoethylstyrene, N,N-diethyl-p-aminoethylstyrene, vinylpyridine, p-methylstyrene, tertiary butylstyrene, α-methylstyrene, and 1,1-diphenylethylene. Styrene is particularly preferred because it allows the flexographic printing plate precursor to be smoothly molded at a relatively low temperature (hereinafter, also referred to as "high moldability"). These monomers may be used alone or in combination of two or more.
[0041] The number average molecular weight of the polymer block mainly composed of vinyl aromatic hydrocarbon is preferably 100,000 or less from the viewpoint of preventing orientation from appearing on the printing plate, and is preferably 3,000 or more from the viewpoint of chipping resistance during plate making and printing. The number average molecular weight of the polymer block mainly composed of vinyl aromatic hydrocarbon is more preferably 5,000 to 80,000, and further preferably 5,000 to 60,000.
[0042] The content of vinyl aromatic hydrocarbon in the block copolymer is preferably 13 to 25 mass%, more preferably 15 to 24 mass%, and even more preferably 16 to 23 mass%, based on the total amount of the block copolymer. By making the content of vinyl aromatic hydrocarbon 25 mass% or less, the photosensitive resin composition tends to have high moldability, the convex portion of the printing plate tends to have high chipping resistance, and the printing plate hardness tends to be high when ink components are attached. On the other hand, by making the content of vinyl aromatic hydrocarbon 13 mass% or more, the cold flow resistance of the flexographic printing plate precursor tends to be further improved.
[0043] From the viewpoint of printing durability during printing, the content of the thermoplastic elastomer (a-1) in the photosensitive resin composition layer is preferably 15 to 90 mass%, more preferably 15 to 80 mass%, and even more preferably 20 to 75 mass%, when the total amount of the photosensitive resin composition is 100 mass%.
[0044] 1.2.2. Polymer particles (a-2) Polymer particles (a-2) are polymer particles in which monomer is internally crosslinked. Such polymer particles are not particularly limited, but can be, for example, prepared by dispersing polymer particles as dispersoid in water by emulsion polymerization to prepare water-dispersed latex, and then removing water from the water-dispersed latex obtained.
[0045] The monomer constituting the polymer particle (a-2) is not particularly limited as long as it has a polymerizable double bond, and examples thereof include monobasic acid monomers, polybasic acid monomers, conjugated dienes, aromatic vinyl compounds, (meth)acrylic acid esters, monomers having a hydroxyl group, unsaturated dibasic acid alkyl esters, maleic anhydride, vinyl cyanide compounds, (meth)acrylamide and its derivatives, vinyl esters, vinyl ethers, vinyl halides, basic monomers having an amino group, vinylpyridine, olefins, silicon-containing α,β-ethylenically unsaturated monomers, allyl compounds, etc. In addition, the monomer constituting the polymer particle (a-2) may contain a reactive emulsifier used in emulsion polymerization described later.
[0046] The monobasic acid monomer is not particularly limited, but examples thereof include monomers having a carboxyl group, such as acrylic acid, methacrylic acid, crotonic acid, vinylbenzoic acid, and cinnamic acid; and monomers having a sulfonic acid group, such as styrenesulfonic acid.
[0047] The content of the monobasic acid monomer is preferably 1 to 30 mass %, more preferably 2 to 20 mass %, even more preferably 3 to 15 mass %, and still more preferably 5 to 10 mass %, based on the total amount of the polymer particles (a-2).
[0048] The polybasic acid monomer is not particularly limited, but examples thereof include monomers having two or more carboxyl groups, such as itaconic acid, fumaric acid, maleic acid, citraconic acid, and muconic acid; monomers having an acid anhydride group; and monomers having a polybasic acid group such as a phosphate group.
[0049] The conjugated diene is not particularly limited, but examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 2-methyl-1,3-butadiene, 1,3-pentadiene, chloroprene, 2-chloro-1,3-butadiene, and cyclopentadiene.
[0050] The content of the conjugated diene is preferably from 45 to 75% by mass, more preferably from 50 to 70% by mass, and further preferably from 55 to 65% by mass, based on the total amount of the polymer particles (a-2).
[0051] The aromatic vinyl compound is not particularly limited, but examples thereof include styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, ethylstyrene, vinyltoluene, vinylxylene, bromostyrene, vinylbenzyl chloride, pt-butylstyrene, chlorostyrene, alkylstyrene, divinylbenzene, and trivinylbenzene.
[0052] The content of the aromatic vinyl compound is preferably from 3 to 25% by mass, more preferably from 5 to 20% by mass, and further preferably from 7.5 to 15% by mass, based on the total amount of the polymer particles (a-2).
[0053] The (meth)acrylic acid ester is not particularly limited, and examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-amyl (meth)acrylate, isoamylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, cyclohexyl (meth)acrylate, and the like. ) acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, 2-ethyl-hexyl (meth)acrylate, glycidyl (meth)acrylate, ethylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,5-pentanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexane Diol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, allyl (meth)acrylate, bis(4-acryloxypolyethoxyphenyl)propane , methoxypolyethylenglycol (meth)acrylate, β-(meth)acryloyloxyethyl hydrogen phthalate, β-(meth)acryloyloxyethyl hydrogen succinate, 3-chloro-2-hydroxypropyl (meth)acrylate, stearyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, 2-hydroxy-1,3-di(meth)acryloxypropane, 2,2-bis[4-((meth)acryloxyethoxy)phenyl]propane, 2,Examples of the acrylate copolymer include 2-bis[4-((meth)acryloxy-diethoxy)phenyl]propane, 2,2-bis[4-((meth)acryloxy-polyethoxy)phenyl]propane, and isobornyl(meth)acrylate.
[0054] The content of the (meth)acrylic acid ester is preferably from 10 to 35% by mass, more preferably from 15 to 30% by mass, and further preferably from 20 to 25% by mass, based on the total amount of the polymer particles (a-2).
[0055] The monomer having a hydroxyl group is not particularly limited, and examples thereof include ethylenic monocarboxylic acid alkyl ester monomers such as 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 1-hydroxypropyl acrylate, 1-hydroxypropyl methacrylate, and hydroxycyclohexyl (meth)acrylate.
[0056] The unsaturated dibasic acid alkyl ester is not particularly limited, but examples thereof include crotonic acid alkyl ester, itaconic acid alkyl ester, fumaric acid alkyl ester, and maleic acid alkyl ester.
[0057] The vinyl cyanide compound is not particularly limited, but examples thereof include acrylonitrile and methacrylonitrile.
[0058] The (meth)acrylamide and its derivatives are not particularly limited, but examples thereof include (meth)acrylamide, N-methylol(meth)acrylamide, and N-alkoxy(meth)acrylamide.
[0059] The vinyl esters are not particularly limited, but examples thereof include vinyl acetate, vinyl butyrate, vinyl stearate, vinyl laurate, vinyl myristate, vinyl propionate, vinyl versatate, and the like.
[0060] The vinyl ethers are not particularly limited, but examples thereof include methyl vinyl ether, ethyl vinyl ether, propyl vinyl ether, butyl vinyl ether, amyl vinyl ether, and hexyl vinyl ether.
[0061] The vinyl halides are not particularly limited, but examples thereof include vinyl chloride, vinyl bromide, vinyl fluoride, vinylidene chloride, and vinylidene fluoride.
[0062] The basic monomer having an amino group is not particularly limited, but examples thereof include aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and diethylaminoethyl (meth)acrylate.
[0063] The olefin is not particularly limited, but examples thereof include ethylene.
[0064] The silicon-containing α,β-ethylenically unsaturated monomer is not particularly limited, but examples thereof include vinyltrichlorosilane, vinyltriethoxysilane, and the like.
[0065] The allyl compound is not particularly limited, but examples thereof include allyl esters and diallyl phthalates.
[0066] In addition, a monomer having three or more double bonds, such as triallyl isocyanurate, can also be used.
[0067] These monomers may be used alone or in combination of two or more. Among them, it is preferable to use a monomer having an acidic group such as a monobasic acid monomer or a polybasic acid monomer (hereinafter simply referred to as an "acidic monomer") and a monomer having a hydrophobic group such as a conjugated diene, an aromatic vinyl compound, or a (meth)acrylic acid ester (hereinafter simply referred to as a "hydrophobic monomer"). The conjugated diene, aromatic vinyl compound, and (meth)acrylic acid ester corresponding to the above hydrophobic monomers have a hydrocarbon group, and those having a hydrophilic group such as a hydroxyl group are excluded from the hydrophobic monomer even if they are (meth)acrylic acid esters or the like.
[0068] The content of the acidic monomer is preferably 1 to 30% by mass, more preferably 2 to 20% by mass, even more preferably 3 to 15% by mass, and even more preferably 5 to 10% by mass, based on the total amount of the polymer particles (a-2). By making the content of the acidic monomer 1% by mass or more, the aqueous development performance tends to be further improved. In addition, by making the content 30% by mass or less, an increase in the moisture absorption amount of the photosensitive resin composition and an increase in the swelling amount of the ink can be prevented, and deterioration of the processability during mixing of the photosensitive resin composition can be prevented.
[0069] The content of the monomer having a hydrophobic group is preferably 70 to 99 mass%, more preferably 80 to 98 mass%, further preferably 85 to 97 mass%, and further preferably 90 to 95 mass%. When the polymer particles (a-2) have such a composition, the rubber elasticity of the photosensitive resin composition tends to be further improved.
[0070] The polymer constituting the polymer particles (a-2) is not particularly limited, and examples thereof include polymers having a butadiene skeleton, such as polybutadiene, acrylonitrile-butadiene copolymer, styrene-butadiene copolymer, and (meth)acrylate-butadiene copolymer; polymers having an isoprene skeleton, such as polyisoprene and polychloroprene; polymers obtained by further polymerizing a monomer having a carboxyl group and / or a hydroxyl group on the polymer having the butadiene skeleton or isoprene skeleton; polymers obtained by further polymerizing a (meth)acrylic acid ester on the polymer having the butadiene skeleton or isoprene skeleton; polymers obtained by further polymerizing a (meth)acrylic acid ester and a monomer having a carboxyl group and / or a hydroxyl group on the polymer having the butadiene skeleton or isoprene skeleton; polyurethane, vinylpyridine polymer, butyl polymer, thiokol polymer, acrylate polymer, and natural rubber.
[0071] The monomer having a carboxyl group herein means the above-mentioned monobasic acid monomer and / or polybasic acid monomer.
[0072] Among these, preferred are polymers having a butadiene skeleton, polymers having an isoprene skeleton, and polymers obtained by further polymerizing the above-mentioned polymers having a butadiene skeleton or an isoprene skeleton with a (meth)acrylic acid ester and / or a monomer having a carboxyl group and / or a hydroxyl group, and more preferred are polymers obtained by further polymerizing the above-mentioned polymers having a butadiene skeleton with a (meth)acrylic acid ester and / or a monomer having a carboxyl group and / or a hydroxyl group. The polymer particles (a-2) may be used alone or in combination of two or more kinds.
[0073] Among the above, polymer particles (a-2-1) containing a butadiene skeleton and having a carboxyl group and / or a hydroxyl group, and polymer particles (a-2-2) polymerized with a monobasic or polybasic acid monomer are more preferred. By using such polymer particles (a-2), the adhesion between the ink receiving layer and the photosensitive resin composition layer tends to be further improved during the development process.
[0074] The average particle size of the polymer particles (a-2) is preferably 500 nm or less, more preferably 100 nm or less. When the average particle size is 500 nm or less, the aqueous developability of the flexographic printing plate precursor tends to be further improved.
[0075] The toluene gel fraction of the polymer particles (a-2) is preferably 60% to 99%. If the toluene gel fraction is 60% or more, the resulting printing plate tends to have sufficient strength for practical use. If the toluene gel fraction is 99% or less, the mixability of the polymer particles (a-2) and the thermoplastic elastomer (a-1) tends to be good.
[0076] Here, the toluene gel fraction refers to a mass fraction (%) obtained by dropping an appropriate amount of a dispersion of about 30% by mass of polymer particles (a-2) onto a Teflon (registered trademark) sheet and drying at 130°C for 30 minutes to obtain 0.5 g of polymer particles (a-2), immersing this in 30 mL of toluene at 25°C, shaking for 3 hours using a shaker, filtering through a 320 SUS mesh, and drying the non-passing portion at 130°C for 1 hour, and dividing the mass by 0.5 (g).
[0077] From the viewpoint of developability during production of a printing plate, the content of the polymer particles (a-2) is preferably 10 to 70 mass%, more preferably 15 to 60 mass%, and even more preferably 20 to 50 mass%, when the total amount of the photosensitive resin composition is taken as 100 mass%.
[0078] (Production method of polymer particles (a-2)) The synthesis method of polymer particles (a-2) is not particularly limited, but for example, it is preferable that the polymer is synthesized by emulsion polymerization.As the emulsion polymerization method of polymer particles (a-2), a method can be mentioned in which a predetermined amount of water, emulsifier, and other additives are charged in advance into a reaction system adjusted to a polymerization temperature, and a polymerization initiator, a monomer, an emulsifier, a regulator, etc. are added to this system by batch operation or continuous operation into the reaction system.In addition, a predetermined amount of seed latex, polymerization initiator, monomer, and other regulators may be charged in advance into the reaction system of emulsion polymerization.
[0079] In addition, by devising a method for adding a monomer, an emulsifier, other additives, and a regulator to the reaction system, it is possible to change the layer structure of the synthesized polymer particles stepwise. In this case, representative physical properties of the structure of each layer include hydrophilicity, glass transition point, molecular weight, crosslink density, etc. In addition, the number of steps of this layer structure is not particularly limited.
[0080] Hereinafter, each component other than the monomers already mentioned will be described.
[0081] The emulsifier (surfactant) used during emulsion polymerization is not particularly limited, and examples thereof include reactive emulsifiers and / or non-reactive emulsifiers. Among these, it is preferable to use a reactive emulsifier.
[0082] The reactive emulsifier is preferably a reactive emulsifier that contains a radically polymerizable double bond, a hydrophilic functional group, and a hydrophobic group in its molecular structure and has emulsifying, dispersing, and wetting functions similar to those of general emulsifiers. Among these, an emulsifier (surfactant) that gives an average particle size of 5 to 500 nm of the resulting polymer particles when 0.1 parts by mass or more of the reactive emulsifier is used per 100 parts by mass of all monomers other than the reactive emulsifier is preferred.
[0083] The hydrophilic functional group possessed by the reactive emulsifier is not particularly limited, and examples thereof include anionic groups such as sulfate group, nitrate group, phosphate group, borate group, and carboxyl group, cationic groups such as amino group, polyoxyalkylene chain structures such as polyoxyethylene, polyoxymethylene, and polyoxypropylene, and hydroxyl group, etc. Depending on the type of the hydrophilic functional group, the reactive emulsifier can be classified into anionic emulsifiers, nonionic emulsifiers, cationic emulsifiers, amphoteric emulsifiers, etc.
[0084] The hydrophobic group of the reactive emulsifier is not particularly limited, and examples thereof include an alkyl group, a phenyl group, etc. The radically polymerizable double bond of the reactive emulsifier is not particularly limited, and examples thereof include a vinyl group, an acryloyl group, a methacryloyl group, etc. The molecular structure may contain multiple types of radically polymerizable double bonds, hydrophilic functional groups, and hydrophobic groups.
[0085] The reactive emulsifier can be a commercially available surfactant, and examples of commercially available anionic surfactants include, but are not limited to, Adeka Reasoap SE (manufactured by Asahi Denka Kogyo Co., Ltd.), Aqualon HS, BC, and KH (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Latemul S (manufactured by Kao Corporation), Antox MS (manufactured by Nippon Nyukazai Co., Ltd.), Adeka Reasoap SDX and PP (manufactured by Asahi Denka Kogyo Co., Ltd.), Hitenol A (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Eleminol RS (manufactured by Sanyo Chemical Industries Co., Ltd.), and Spinomer (manufactured by Toyo Soda Kogyo Co., Ltd.). Also, examples of commercially available nonionic surfactants include, but are not limited to, Aqualon RN and Noigen N (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Adeka Reasoap NE (manufactured by Asahi Denka Kogyo Co., Ltd.), and the like. These may be used alone or in combination of two or more types.
[0086] The amount of reactive emulsifier used is preferably 1 to 20 parts by mass per 100 parts by mass of polymer particles (a-2) calculated from the amount of raw materials charged. When the amount of reactive emulsifier used is 1 part by mass or more, the image reproducibility of the obtained printing plate tends to improve. Also, when the amount of reactive emulsifier used is 20 parts by mass or less, the printing resistance of the obtained printing plate tends to improve.
[0087] The non-reactive emulsifier is not particularly limited, but examples thereof include anionic surfactants such as fatty acid soap, rosin acid soap, sulfonate, sulfate, phosphate ester, polyphosphate ester, and salicosinic acid acyl; cationic surfactants such as nitrile oil derivatives, oil derivatives, fatty acid derivatives, and α-olefin derivatives; and nonionic surfactants such as alcohol ethoxylates, alkylphenol ethoxylates, propoxylates, aliphatic alkanolamides, alkyl polyglycosides, polyoxyethylene sorbitan fatty acid esters, and oxyethylene oxypropylene block copolymers. These may be used alone or in combination of two or more.
[0088] The sulfonate is not particularly limited, but may be, for example, alkyl sulfonate, alkyl sulfate, alkyl sulfosuccinate, polyoxyethylene alkyl sulfate, sulfonated fats and oils, alkyl diphenyl ether disulfonate, α-olefin sulfonate, alkyl glyceryl ether sulfonate, N-acyl methyl taurate, etc. Examples of non-reactive emulsifiers other than those described above are not particularly limited, but may be, for example, those described in "Surfactant Handbook (Takahashi, Namba, Koike, Kobayashi: Kogyo Tosho, 1972)".
[0089] The amount of the non-reactive emulsifier used is preferably less than 1 part by mass per 100 parts by mass of the polymer particles (a-2) calculated from the amount of the raw materials charged. By using an amount of the non-reactive emulsifier of less than 1 part by mass, the resulting printing plate has an appropriate water swelling ratio, and it is possible to prevent a decrease in abrasion resistance when ink is attached and a decrease in image reproducibility after moisture absorption.
[0090] The polymerization initiator is not particularly limited, but may be, for example, a radical polymerization initiator. The radical polymerization initiator is not particularly limited, but may be, for example, a radical decomposition initiator in the presence of heat or a reducing substance to initiate addition polymerization of a monomer, and may be either an inorganic initiator or an organic initiator.
[0091] The radical polymerization initiator is not particularly limited, and examples thereof include water-soluble or oil-soluble peroxodisulfates, peroxides, azobis compounds, etc., and specifically include potassium peroxodisulfate, sodium peroxodisulfate, ammonium peroxodisulfate, hydrogen peroxide, t-butyl hydroperoxide, benzoyl peroxide, 2,2-azobisbutyronitrile, cumene hydroperoxide, etc. In addition, as the radical polymerization initiator, compounds described in POLYMER HANDBOOK (3rd edition), written by J. Brandrup and EH Immergut, published by John Willy & Sons (1989) can also be used. In addition, a so-called redox polymerization method can be adopted in which a reducing agent such as acidic sodium sulfite, ascorbic acid or its salt, erythorbic acid or its salt, or Rongalit is used in combination with the polymerization initiator. Among these, peroxodisulfates are suitable as the polymerization initiator.
[0092] The amount of the polymerization initiator used is usually 0.1 to 5.0% by mass, preferably 0.2 to 3.0% by mass, based on the total amount of monomers used in the polymerization of the polymer particles (a-2). When the amount of the polymerization initiator used is 0.1% by mass or more, high stability is obtained during the synthesis of the polymer particles (a-2). In addition, when the amount of the polymerization initiator used is 5.0% by mass or less, the moisture absorption amount of the photosensitive resin composition can be suppressed to a practically good range.
[0093] In the polymerization process of the polymer particles (a-2), a known chain transfer agent can be used. As the chain transfer agent, a chain transfer agent containing a sulfur element can be suitably used. As the chain transfer agent containing a sulfur element, there is no particular limitation, but for example, alkanethiols such as t-dodecyl mercaptan and n-dodecyl mercaptan; thioalkyl alcohols such as mercaptoethanol and mercaptopropanol; thioalkyl carboxylic acids such as thioglycolic acid and thiopropionic acid; thiocarboxylate alkyl esters such as thioglycolic acid octyl ester and thiopropionic acid octyl ester; and sulfides such as dimethyl sulfide and diethyl sulfide.
[0094] Other chain transfer agents are not particularly limited, but may include, for example, halogenated hydrocarbons such as terpinolene, dipentene, t-terpinene, and carbon tetrachloride. Among these chain transfer agents, alkanethiol is preferred because it has a high chain transfer rate and the physical properties of the resulting polymer are well balanced. These chain transfer agents may be used alone or in combination of two or more.
[0095] These chain transfer agents are mixed with the monomers and fed to the reaction system, or added alone at a predetermined time in a predetermined amount. The amount of these chain transfer agents used is preferably 0.1 to 10 mass% based on the total amount of monomers used in the polymerization of the polymer particles (a-2). By making the amount 0.1 mass% or more, the processability during mixing of the photosensitive resin composition is good, and by making the amount 10 mass% or less, the molecular weight of the polymer particles (a-2) can be made practically sufficient.
[0096] A polymerization inhibitor can be used for the polymerization of the polymer particles (a-2) as necessary. The polymerization inhibitor is a compound that reduces the radical polymerization rate by adding it to an emulsion polymerization system. More specifically, the polymerization inhibitor is a polymerization rate retarder, a polymerization inhibitor, a chain transfer agent with low radical reinitiation reactivity, and a monomer with low radical reinitiation reactivity. The polymerization inhibitor is generally used to adjust the polymerization rate and the physical properties of the latex. These polymerization inhibitors are added to the reaction system in a batch operation or a continuous operation. When the polymerization inhibitor is used, the strength of the latex coating is improved and the printing durability is improved. Although the details of the reaction mechanism are unknown, the polymerization inhibitor is considered to be closely related to the three-dimensional structure of the polymer, and it is presumed that this is effective in adjusting the physical properties of the latex coating.
[0097] The polymerization reaction inhibitor is not particularly limited, but examples thereof include quinones such as o-, m-, or p-benzoquinone; nitro compounds such as nitrobenzene, o-, m-, or p-dinitrobenzene; amines such as diphenylamine; catechol derivatives such as tertiary butylcatechol; 1,1-disubstituted vinyl compounds such as 1,1-diphenylethylene, α-methylstyrene, and 2,4-diphenyl-4-methyl-1-pentene; 1,2-disubstituted vinyl compounds such as 2,4-diphenyl-4-methyl-2-pentene and cyclohexene; etc. In addition, compounds described as polymerization inhibitors or polymerization inhibitors in "POLYMER HANDBOOK 3rd Ed. (J. Brandup, EH Immergut: John Wiley & Sons, 1989)" and "Revised Chemistry of Polymer Synthesis (Otsu: Kagaku Dojin, 1979.)" are also included.
[0098] Among these, 2,4-diphenyl-4-methyl-1-pentene (α-methylstyrene dimer) is particularly preferred from the viewpoint of reactivity. These polymerization reaction inhibitors may be used alone or in combination of two or more.
[0099] The amount of the polymerization reaction inhibitor used is preferably 10% by mass or less based on the total amount of monomers used in the polymerization of the polymer particles (a-2). By making the amount 10% by mass or less, a polymerization rate sufficient for practical use tends to be obtained.
[0100] During the synthesis of the polymer particles (a-2), various polymerization regulators such as a pH regulator and a chelating agent may be added, if necessary.
[0101] The pH adjuster is not particularly limited, but examples thereof include sodium hydroxide, potassium hydroxide, ammonium hydroxide, sodium hydrogen carbonate, sodium carbonate, and disodium hydrogen phosphate.
[0102] The chelating agent is not particularly limited, but examples thereof include sodium ethylenediaminetetraacetate.
[0103] Furthermore, other additives that may be added include various additives such as alkali-sensitive latex, viscosity reducers such as hexametaphosphoric acid, water-soluble polymers such as polyvinyl alcohol and carboxymethyl cellulose, thickeners, various anti-aging agents, ultraviolet absorbers, preservatives, bactericides, defoamers, dispersants such as sodium polyacrylate, water-resistant agents, metal oxides such as zinc oxide, crosslinking agents such as isocyanate compounds and epoxy compounds, lubricants, and water retention agents.
[0104] The method of adding these additives is not particularly limited, and they can be added either during or after the synthesis of the polymer particles (a-2).
[0105] The polymerization temperature in emulsion polymerization of the polymer particles (a-2) is usually 60 to 120° C. Polymerization may be performed at a lower temperature by the redox polymerization method, etc. Furthermore, a metal catalyst, such as a divalent iron ion, a trivalent iron ion, or a copper ion, may be used as an oxidation-reduction catalyst.
[0106] 1.2.3. Photopolymerizable monomer (a-3) The photopolymerizable monomer (a-3) is not particularly limited, but examples thereof include esters of acids such as acrylic acid, methacrylic acid, fumaric acid, and maleic acid; acrylamide and methacrylamide derivatives; allyl esters, styrene and its derivatives; and N-substituted maleimide compounds.
[0107] The photopolymerizable monomer (a-3) is not particularly limited, and examples thereof include diacrylates and dimethacrylates of alkanediols such as 1,6-hexanediol and 1,9-nonanediol; diacrylates and dimethacrylates of ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, polyethylene glycol, butylene glycol, and dicyclopentadienyl; trimethylolpropane tri(meth)acrylate, dimethyloltricyclodecane di(meth)acrylate, isobornyl(meth)acrylate, phenoxypolyethylene glycol(meth)acrylate, pentaerythritol tetraacetate, and the like. Examples of the acrylate include methacrylate, N,N'-hexamethylenebisacrylamide and methacrylamide, styrene, vinyltoluene, divinylbenzene, diacrylphthalate, triallyl cyanurate, diethyl fumarate, dibutyl fumarate, dioctyl fumarate, distearyl fumarate, butyloctyl fumarate, diphenyl fumarate, dibenzyl fumarate, dibutyl maleate, dioctyl maleate, bis(3-phenylpropyl) fumarate, dilauryl fumarate, dibehenyl fumarate, and N-laurylmaleimide. These may be used alone or in combination of two or more.
[0108] From the viewpoint of even higher chipping resistance of the raised portions of the printing plate, the photopolymerizable monomer (a-3) is preferably a di(meth)acrylate monomer having two (meth)acrylate groups in one molecule. The content of such a di(meth)acrylate monomer is preferably 2.0 mass% or more, more preferably 2.0 to 20 mass%, and even more preferably 5.0 to 16 mass%, based on the total amount of the photosensitive resin composition.
[0109] From the viewpoint of obtaining bright prints, the content of the photopolymerizable monomer (a-3) is preferably 1 to 25 mass%, more preferably 5 to 20 mass%, and even more preferably 8 to 15 mass%, when the total amount of the photosensitive resin composition is taken as 100 mass%.
[0110] 1.2.4. Photopolymerization initiator (a-4) The photopolymerization initiator (a-4) is a compound that absorbs light energy and generates radicals. Various known photopolymerization initiators can be used, and various organic carbonyl compounds, and particularly aromatic carbonyl compounds, are preferred.
[0111] The photopolymerization initiator (a-4) is not particularly limited, and examples thereof include thioxanthones such as benzophenone, 4,4-bis(diethylamino)benzophenone, t-butylanthraquinone, 2-ethylanthraquinone, 2,4-diethylthioxanthone, isopropylthioxanthone, and 2,4-dichlorothioxanthone; diethoxyacetophenone, 2,2-dimethoxyphenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 1-hydroxycyclohexyl-phenyl ketone, 2-methyl-2-morpholino(4-thiomethylphenyl)propan-1-one, and 2-benzyl-2-dimethylamino-1- Examples of the compounds include acetophenones such as (4-morpholinophenyl)-butanone, benzoin ethers such as benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether, acylphosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, methylbenzoyl formate, 1,7-bisacridinylheptane, 9-phenylacridine, and 2,6-di-t-butyl-p-cresol. These compounds may be used alone or in combination of two or more.
[0112] From the viewpoints of improving plate formability during plate making and obtaining bright prints, the content of the photopolymerization initiator (a-4) is preferably 0.1 to 10.0 mass%, more preferably 1.0 to 8.0 mass%, and even more preferably 1.5 to 5.0 mass%, when the total amount of the photosensitive resin composition is taken as 100 mass%.
[0113] As the photopolymerization initiator (a-4), a decomposition type photopolymerization initiator and a hydrogen abstraction type photopolymerization initiator may be used in combination. In order to improve the image reproducibility and abrasion resistance of the printing plate, the amount of the hydrogen abstraction type photopolymerization initiator in the photosensitive resin composition is preferably 1.0% by mass or less, and more preferably 0.5% by mass or less.
[0114] 1.2.5. Liquid diene (a-5) The photosensitive resin composition layer may contain a liquid diene (a-5). A liquid diene is a compound having a liquid carbon-carbon double bond. In this specification, the term "liquid" in "liquid diene" means a property of being easily fluid and deformed and being able to be solidified in the deformed shape by cooling, and is a term corresponding to an elastomer having a property of being instantly deformed in response to an external force when the external force is applied and recovering the original shape in a short time when the external force is removed.
[0115] The liquid diene (a-5) is not particularly limited, but examples thereof include liquid polybutadiene, liquid polyisoprene, modified liquid polybutadiene, modified liquid polyisoprene, liquid acrylonitrile-butadiene copolymer, and liquid styrene-butadiene copolymer. The liquid diene is a copolymer containing 50% by mass or more of a diene component.
[0116] Among these, from the viewpoint of the mechanical properties of the flexographic printing plate precursor of this embodiment and the flexographic printing plate precursor using the same, liquid polybutadiene is preferred as the liquid diene (a-5).
[0117] The number average molecular weight of the liquid diene (a-5) is not particularly limited as long as it is liquid at 20°C. From the viewpoint of printing durability and handling of a flexographic printing plate obtained using the flexographic printing base plate of this embodiment, the number average molecular weight is preferably 500 or more and 60,000 or less, more preferably 500 or more and 50,000 or less, and even more preferably 800 or more and 50,000 or less.
[0118] From the viewpoint of the printing durability of the flexographic printing plate precursor of this embodiment and the flexographic printing plate using the same, the content of the liquid diene (a-5) in the photosensitive resin composition layer is preferably 10 to 40 mass%, more preferably 15 to 40 mass%, and even more preferably 20 to 40 mass%, when the total amount of the photosensitive resin composition layer (b) is taken as 100 mass%.
[0119] 1.2.6. Silicone compounds (a-6) Examples of the silicone compound (a-6) include silicone oil, a silane coupling agent, a silane compound, silicone rubber, silicone resin, etc. Among them, silicone oil is preferred because the components are easily transferred to the surface and it is highly effective in lowering the surface energy.
[0120] The silicone compound (a-6) is not particularly limited, and may be, for example, a compound having a polyalkylsiloxane such as polydimethylsiloxane or polydiethylsiloxane in the main chain. The silicone compound (a-6) may also be a compound having a polysiloxane structure in a part of the molecule. Furthermore, the silicone compound (a-6) may be a compound having a specific organic group introduced into the polysiloxane structure. Specifically, a compound having an organic group introduced into the side chain of the polysiloxane, a compound having an organic group introduced into both ends of the polysiloxane, a compound having an organic group introduced into one end of the polysiloxane, a compound having an organic group introduced into both the side chain and the end of the polysiloxane, etc. may be used.
[0121] The organic group to be introduced into the polysiloxane structure is not particularly limited, but examples thereof include an amino group, a carboxyl group, a carbinol group, an aryl group, an alkyl group, an alkoxycarbonyl group, an alkoxy group, a linear or branched alkyl group substituted with at least one aryl group, and a polyoxyalkylene group (hereinafter also referred to as a polyether group).
[0122] Among these, silicone compound (a-6) is more preferably a silicone oil having polysiloxane as a main skeleton and having at least one group selected from the group consisting of amino group, polyether group, and carbinol group at at least one end.By using such silicone compound (a-6), the transparency of the photosensitive resin composition layer tends to be improved.In addition, the commercially available product of such silicone compound is not particularly limited, but for example, KF-6000 manufactured by Shin-Etsu Chemical Co., Ltd. can be mentioned.
[0123] The content of the silicone compound (a-6) is preferably 0.1 to 5.0 mass %, more preferably 0.5 to 3.0 mass %, and further preferably 0.5 to 2.0 mass %, based on the total amount of the photosensitive resin composition layer.
[0124] 1.3.Ink Receptive Layer The flexographic printing plate precursor of this embodiment has an ink-receiving layer between the photosensitive resin composition layer and an infrared ablation layer described later. The ink-receiving layer must adhere to the photosensitive resin composition layer and remain on the obtained flexographic printing plate even when exposed to a developer such as water or a solvent during the development process, or when rubbed with a development brush or nonwoven fabric. Therefore, the ink-receiving layer in the flexographic printing plate precursor is preferably thick. In addition, as described later, in terms of forming microcells, it is preferable that the ink-receiving layer in the flexographic printing plate precursor is thick, because this makes it easier to process the convex parts of the dots (see FIG. 5).
[0125] On the other hand, the depth of the recesses between the dots on the relief is approximately 100 μm. Therefore, the thicker the ink-receiving layer, the more the dots themselves are formed from the components of the ink-receiving layer. This makes it easier for ink to accumulate between the dots (recesses).
[0126] Considering the balance between these factors, the thickness of the ink receiving layer is from 5 μm to 50 μm, preferably from 10 μm to 45 μm, and more preferably from 10 μm to 40 μm.
[0127] The difference (Ei-Ep) between the surface free energy Ei of the ink receiving layer and the surface free energy Ep of the photosensitive resin composition layer is 0 mJ / m 2 Greater than 5mJ / m 2 Less than or equal to 0 mJ / m is preferable. 2 Greater than 4mJ / m 2 Less than or equal to 0.5 to 3.5 mJ / m is more preferable. 2 More preferably, 1.0 to 3.5 mJ / m 2 On the other hand, it is more preferable that the difference (Ei-Ep) between the surface free energy of the ink receiving layer and the surface free energy of the photosensitive resin composition layer is 5 mJ / m 2 By setting the above to the range, the ink receptive property of the obtained flexographic printing plate is improved, and the adhesion between the ink-receptive layer and the photosensitive resin composition layer tends to be maintained even after development. It is preferable that the surface free energy Ei of the ink-receptive layer is greater than the surface free energy Ep of the photosensitive resin composition layer. For example, as described in the above-mentioned Patent Document 4, it is preferable that the surface free energy Ei of the ink-receptive layer is 5 mJ / m higher than the surface free energy Ep of the photosensitive resin composition layer. 2 If it exceeds this value, it is not suitable for printing in high definition and highlight areas, and the dots on the printed matter tend to become thicker. This is because the surface free energy Ei of the ink-receiving layer is 5 mJ / m lower than the surface free energy Ep of the photosensitive resin composition layer. 2 It is speculated that when the amount is excessive, the ink is less likely to accumulate in the recesses of the photosensitive resin, but instead, an excess of ink is supplied to the protruding parts.
[0128] Here, the surface free energy was evaluated as a resin characteristic of each of the ink-receptive layer and the photosensitive resin composition. The surface free energy of the ink-receptive layer refers to the outermost surface of the resin plate exposed to development (see Figure 5), and the surface free energy of the photosensitive resin composition was evaluated using the "back surface" part shown in Figure 5.
[0129] From the same viewpoint as above, the surface free energy Ei of the ink receiving layer is preferably 33 to 43 mJ / m 2 and preferably 34 to 42 mJ / m 2and more preferably 35 to 41 mJ / m 2 The surface free energy Ep of the photosensitive resin composition layer is preferably 30 to 40 mJ / m 2 and preferably 31 to 39 mJ / m 2 and more preferably 32 to 38 mJ / m 2 The surface free energy can be determined by the method described in the Examples.
[0130] Zeta potential The zeta potential of the ink receiving layer in this embodiment is preferably a positive value. When the ink receiving layer has a positive zeta potential, the concentration of the transferred aqueous ink tends to be high when a flexographic printing plate obtained from the flexographic printing plate master is used to print and transfer the aqueous ink onto a film.
[0131] The reason why the concentration of the transferred aqueous ink increases when the zeta potential of the ink receiving layer is positive is not clear in detail, but the present inventors speculate as follows. A method of printing with aqueous ink using the flexographic printing plate of this embodiment will be described later, but aqueous inks often use a binder resin having a salt structure in which a carboxyl group and ammonium are used as their counter cation, or a binder resin similar thereto, in order to improve the "redissolubility" problem described above. When using such aqueous ink, if the ink receiving layer of this embodiment is a positively charged film, i.e., has a positive zeta potential, it is likely to interact with the carboxyl group of the binder resin of the aqueous ink, and therefore the amount of aqueous ink held in the ink receiving layer increases, and the ink concentration of the printed matter is improved.
[0132] The zeta potential of the ink-receiving layer can be measured using a membrane zeta potential measuring device (ELSZ, Otsuka Electronics Co., Ltd.). Specifically, after placing a measurement sample in a measurement cell, an electric field is applied parallel to the membrane of the sample using a 10 mM NaCl aqueous solution, and the speed of the induced electroosmotic flow is observed as the motion speed of polystyrene latex (500 nm) that is not charged due to modification with hydroxypropyl cellulose, and the zeta potential can be calculated from the motion speed.
[0133] Furthermore, it is preferable that the ink-receiving layer can be washed with the same washing liquid as the infrared ablation layer and / or the photosensitive resin composition layer in the manufacturing process of the flexographic printing plate described below. Since the ink-receiving layer has such washability, the ink-receiving layer can be washed together with the photosensitive resin composition layer and the like, and therefore there is no need to add a special process for washing the ink-receiving layer, which is preferable from the viewpoint of simplicity of the manufacturing process of the flexographic printing plate.
[0134] In addition, although not particularly limited, in the manufacturing process of a flexographic printing plate, it is preferable to prepare a cover film on which an infrared ablation layer and an ink receptive layer are successively wet-coated, and then to produce the flexographic printing plate precursor of the present invention by adhering / bonding the cover film to a photosensitive resin composition layer. As described below, since the infrared ablation layer mainly contains a hydrophobic compound, it is preferable to use a hydrophilic component for the ink receptive layer to be applied on the infrared ablation layer. This makes it possible to apply the infrared ablation layer and the ink receptive layer without mixing them.
[0135] From the above viewpoint, it is preferable that the ink receiving layer contains a hydrophilic component. The components contained in such an ink receiving layer are not particularly limited, but may include, for example, polymer particles (b-1), thickeners (b-2), silicone compounds (b-3), binder resins (b-4), inorganic layered compounds (b-5), water-soluble photopolymerization initiators (b-6), water-soluble polymerizable compounds (b-7), water-soluble crosslinkers (b-8), and surfactants (b-9). Among these, it is preferable that the ink receiving layer contains polymer particles (b-1), thickeners (b-2), and silicone compounds (b-3). Each component contained in the ink receiving layer will be described in detail below.
[0136] 1.3.2. Polymer particles (b-1) The ink-receiving layer must adhere to the photosensitive resin composition layer and remain on the obtained flexographic printing plate even when exposed to a developer such as water or a solvent during the development process, or when rubbed with a developing brush or nonwoven fabric.
[0137] From this viewpoint, the ink receiving layer contains a predetermined polymer particle (b-1). The polymer particle (b-1) is not particularly limited, but includes, for example, a polymer particle (b-1-1) having a butadiene skeleton and a carboxyl group and / or a hydroxyl group, and / or a polymer particle (b-1-2) in which a monobasic or polybasic acid monomer is polymerized. The polymer particle (b-1-1) and the polymer particle (b-1-2) may be the same as the polymer particle (a-2-1) and the polymer particle (a-2-2) contained in the photosensitive resin composition layer. By using such a polymer particle (b-1), the adhesion between the ink receiving layer and the photosensitive resin composition layer tends to be further improved during the development process.
[0138] In addition, the polymer particles (b-1) are preferably other polymers having a butadiene skeleton, polymers having an isoprene skeleton, and polymers obtained by further polymerizing the above-mentioned polymers having an isoprene skeleton with a (meth)acrylic acid ester and / or a monomer having a carboxyl group and / or a hydroxyl group. By using such polymer particles (b-1), the adhesion between the ink receiving layer and the photosensitive resin composition layer tends to be further improved during the development process.
[0139] In particular, the use of polymer particles containing a butadiene skeleton tends to improve the adhesion between the ink-receiving layer and the photosensitive resin composition layer, and the ink-receiving layer tends to be easily maintained even after development. Furthermore, surprisingly, the use of polymer particles containing a butadiene skeleton tends to enable the ink-receiving layer to exhibit higher lithography performance, and the moldability of microcells tends to be improved.
[0140] The polymer constituting the polymer particles (b-1) having a butadiene skeleton or an isoprene skeleton is not particularly limited, and examples thereof include polymers having a butadiene skeleton, such as polybutadiene, acrylonitrile-butadiene copolymer, styrene-butadiene copolymer, and (meth)acrylate-butadiene copolymer; and polymers having an isoprene skeleton, such as polyisoprene and polychloroprene.
[0141] The polymer constituting the polymer particles (b-1) containing a butadiene skeleton and having a carboxyl group and / or a hydroxyl group is not particularly limited, but may be, for example, a polymer obtained by further polymerizing a monomer having a carboxyl group and / or a hydroxyl group to the polymer constituting the polymer particles containing the butadiene skeleton. Here, the monomer having a carboxyl group means the monobasic acid monomer and / or the polybasic acid monomer. The polymer particles (b-2) may be used alone or in combination of two or more kinds.
[0142] The polymer particles (b-1) may have a polar group such as the above-mentioned carboxyl group and / or hydroxyl group. Such polar groups are not particularly limited, but examples thereof include hydrophilic groups such as carboxyl groups, hydroxyl groups, phosphoric acid groups, sulfonic acid groups, and salts of these groups. By having such a polar group, the hydrophilicity of the ink-receiving layer tends to be improved. As described below, in the manufacturing process of a flexographic printing plate precursor, an infrared ablation layer and an ink-receiving layer are successively wet-coated on a cover film, and then the flexographic printing plate precursor of the present invention is produced by adhering / bonding the layer to a photosensitive resin composition layer. At this time, since the infrared ablation layer is mainly formed using a hydrophobic component, it is preferable that the ink-receiving layer applied thereon uses a hydrophilic component. In this way, by improving the hydrophilicity of the ink-receiving layer, the mixing of the infrared ablation layer and the ink-receiving layer tends to be suppressed in the wet process of the manufacturing process of the flexographic printing plate precursor.
[0143] In addition, the ink receiving layer containing the polymer particles (b-1) as described above will be cured in the manufacturing process of a flexographic printing plate precursor, described below, even if it does not contain the water-soluble photopolymerization initiator (b-6) or the water-soluble polymerizable compound (b-7). The reason for this is not clear in detail, but the present inventors speculate as follows. The mechanism assumed is that, in the manufacturing process of a flexographic printing plate, the heat generated when the infrared ablation layer described below is irradiated with an IR laser to ablate it diffuses to the ink receiving layer below the infrared ablation layer, and the polymer particles (b-1) fuse and heat-cure, and / or, when the photosensitive resin composition layer is irradiated with visible light to perform photoradical polymerization, the generated radicals diffuse to the ink receiving layer, and the butadiene skeleton contained in the polymer particles (b-1) is crosslinked by the radicals.
[0144] Surprisingly, the ink receiving layer containing the polymer particles (b-1) as described above is cured in the manufacturing process of the flexographic printing plate precursor described below even when it does not contain the water-soluble photopolymerization initiator (b-6) or the water-soluble polymerizable compound (b-7), and curing also occurs when the ink receiving layer contains a polymerization inhibitor, which is considered to be as described above. However, the mechanism is not limited to the above.
[0145] The commercially available polymer particles (b-1) are not particularly limited, but examples thereof include SB Latex L7430, A2730, A7141, A6006, and L5390 manufactured by Asahi Kasei Corporation, and Lackstar DN703, 1570B, and 6541G manufactured by DIC Corporation.
[0146] The content of the polymer particles (b-1) in the ink-receiving layer of the flexographic printing plate of this embodiment is preferably 20% by mass or more, more preferably 35% by mass or more, even more preferably 50% by mass or more, even more preferably 65% by mass or more, and even more preferably 80% by mass or more, based on the total amount of the ink-receiving layer, from the viewpoint of ensuring adhesion with the photosensitive resin composition layer. The content of the polymer particles (b-1) is preferably 95% by mass or less, based on the total amount of the ink-receiving layer. When the content of the polymer particles (b-1) in the ink-receiving layer is 20% by mass or more, the adhesion between the ink-receiving layer and the photosensitive resin composition layer in the obtained flexographic printing plate tends to be further improved.
[0147] 1.3.3. Thickener (b-2) In order to adjust the thickness of the ink-receiving layer when it is applied, the ink-receiving layer may contain a thickener (b-2).
[0148] The thickener (b-2) is not particularly limited, but is preferably water-soluble. Examples of water-based thickeners include SEPIGEL 305, NS, EG, FL, SEPIPLUS265, S, 400, SEPINOV EMT10, P88, SEPIMAX ZEN (manufactured by Seiwa Kasei Co., Ltd.), Aron A-10H, A-20P-X, A-20L, A-30, A-7075, A-7100, A-7185, A-7195, A-7255, B-300K, B-500K, JURYMER (registered trademark) AC-10LHPK, AC-10SHP, RHEOGIC 260H, 845H, JUNRON PW-120 (manufactured by Toagosei Co., Ltd.), DISPERBYK 410, 411, 415, 420, 425, 428, 430, 431, 7410ET, 7411ES, 7420ES, OPTIFLO-L1400 (manufactured by BYK-Chemie), COSCUTT GA468 (manufactured by Osaka Organic Chemical Industry Co., Ltd.), cellulose derivative materials (carboxymethylcellulose, methylcellulose, hydroxycellulose, etc.), protein materials (casein, sodium caseinate, ammonium caseinate, etc.), alginic acid materials (sodium alginate, etc.), polyvinyl materials (polyvinyl alcohol, polyvinylpyrrolidone, polyvinyl benzyl ether copolymer, etc.), polyacrylic acid materials Examples of thickeners include polyamide waxes (polysodium acrylate, polyacrylic acid-(meth)acrylic acid copolymers, etc.), polyether-based materials (ethylene oxide-propylene oxide copolymers (Meisei Chemical Industry Co., Ltd., ALKOX EP-10), Pluronic polyethers (Pluronic: registered trademark), polyether dialkyl esters, polyether dialkyl ethers, polyether urethane modified products, polyether epoxy modified products, etc.), and maleic anhydride copolymer-based materials (partial esters of vinyl ether-maleic anhydride copolymers, drying oil fatty acid allyl alcohol ester-maleic anhydride half esters, etc.). Examples of thickeners include polyamide wax salts, acetylene glycol, polysaccharides such as xanthan gum, diutan gum, and zentane gum, and oligomers or polymers having polar groups at the molecular end or side chain. The thickeners may be used alone or in combination of two or more types.
[0149] Among these, the ink receiving layer preferably contains a water-soluble resin having an alkylene oxide chain as a thickener, since the inclusion of such a thickener tends to further improve water developability.
[0150] The content of the thickener (b-2) is preferably from 1 to 10% by mass, more preferably from 1.5 to 8% by mass, and even more preferably from 2 to 5% by mass, when the total amount of the ink receiving layer is taken as 100% by mass.
[0151] 1.3.4. Silicone compounds (b-3) The ink-receiving layer can be formed, for example, by applying a material for forming the ink-receiving layer onto the infrared ablation layer. In order to uniformly apply the ink-receiving layer onto the infrared ablation layer, the ink-receiving layer preferably contains a silicone compound (b-3) and a surfactant (b-9) from the viewpoint of controlling the surface energy.
[0152] The silicone compound (b-3) is not particularly limited, and examples thereof include compounds having polyalkylsiloxanes such as polydimethylsiloxane and polydiethylsiloxane in the main chain. The silicone compound (b-3) may also be a compound having a polysiloxane structure in a part of the molecule. Furthermore, the silicone compound (b-3) may also be a compound having a specific organic group introduced into the polysiloxane structure. Specifically, a compound having an organic group introduced into the side chain of the polysiloxane, a compound having an organic group introduced into both ends of the polysiloxane, a compound having an organic group introduced into one end of the polysiloxane, a compound having an organic group introduced into both the side chain and the end of the polysiloxane, etc. can be used.
[0153] Among these, from the viewpoint of ensuring adhesion between the ink receiving layer and the photosensitive resin composition layer, it is preferable to use a silicone compound having an organic group introduced therein.
[0154] The organic group to be introduced into the polysiloxane structure is not particularly limited, but examples thereof include an amino group, a carboxyl group, a carbinol group, an aryl group, an alkyl group, an alkoxycarbonyl group, an alkoxy group, a linear or branched alkyl group substituted with at least one aryl group, and a polyoxyalkylene group (hereinafter also referred to as a polyether group).
[0155] The silicone compound is not particularly limited, but examples of the silicone compound that can be used include modified silicone oil (KF-351A, Shin-Etsu Chemical Co., Ltd.) manufactured by Shin-Etsu Chemical Co., Ltd., various organic group-substituted silicone oils manufactured by Wacker Asahi Kasei Silicone Co., Ltd., GE Toshiba Silicone Co., Ltd., and Dow Corning Toray Silicone Co., Ltd.
[0156] The content of the silicone compound (b-3) is preferably from 1 to 10% by mass, more preferably from 1.5 to 8% by mass, and even more preferably from 2 to 5% by mass, when the total amount of the ink receiving layer is taken as 100% by mass.
[0157] 1.3.5. Binder resin (b-4) The ink receiving layer may contain a binder resin (b-4). The binder resin (b-4) may be any polymer resin having a water-soluble polar group and dissolving in water, or emulsion particles having the polar group and existing in a dispersed state in water, and may be used without any particular limitation. Specific examples include water-soluble poly(ethylene-vinyl alcohol) copolymers, polyvinyl alcohol, partially saponified polyvinyl acetate, partially saponified poly(ethylene oxide vinyl acetate) graft copolymers, polyvinyl butyral, polyvinyl pyrrolidone, polyurethane, polyester, polyether, cellulose, polyamide, polyurethane, water-soluble phenols, etc. Also, these may be used alone or in combination of two or more.
[0158] Among the water-soluble binder resins (b-4), it is particularly preferable to use water-soluble cationic resins or cationic resin particles. The cationic resin particles can be added as a cationic resin emulsion. The above resin has cationic groups, and can interact with the carboxyl groups of the binder resin contained in the water-based ink described below, and has high affinity with the water-based ink.
[0159] As the cationic resin, a binder resin (b-4) having a basic group, such as a resin having a basic group in a structural unit, a resin having a basic group introduced therein, or a resin having a surface treated to be basic, can be used. For example, as the cationic resin, a resin having one or more cationic sites such as amine, ammonium salt, pyridinium salt, imidazolidinone salt, etc. can be used. By using such a binder resin, the affinity with the water-based ink tends to be further improved.
[0160] Specifically, the cationic resin may be polyvinylamine, polyallylamine, a copolymer of acrylamide, polyamide, or a derivative thereof. In addition, the cationic resin may be a resin having a basic group introduced into the resin skeleton of a urethane resin, an acrylic resin, a vinyl acetate resin, or the like, or a resin having a basic surface treated with such a resin. In addition, the cationic resin may be an acrylic resin having a radical polymerizable monomer such as a primary to tertiary amine or a quaternary ammonium as a constituent monomer, such as dimethylaminoethyl methacrylate. These may be used alone or in combination of two or more.
[0161] Among these, it is preferable to use a polyamide resin and / or a polyurethane resin as the binder resin (b-4) having a basic group. By using such a binder resin (b-4), it is possible to further improve the affinity between the ink receiving layer and the water-based ink, and the ink concentration of the obtained recorded matter tends to be further improved. A flexographic printing plate having such an ink receiving layer is more suitable for water-based flexographic ink for film applications.
[0162] The cationic resin is not particularly limited, but examples thereof include "HIMAX SC-103, SC-506" manufactured by HYMO Co., Ltd., "PP-17" manufactured by Meisei Chemical Industry Co., Ltd., "SUPERFLEX 620, 650" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "HYDRAN CP7610, CP7050" (polyurethane resin) and "DIC FINE FZ-1000" (styrene-acrylic resin emulsion) manufactured by DIC Corporation, "HARSIZE CP-300, CP800" (styrene-acrylic resin emulsion) manufactured by Harima Chemical Group, Inc., and "POLYSOL AP-1370" manufactured by Showa Denko K.K.
[0163] In addition, the polyamide resin is not particularly limited, but can be, for example, a substance obtained by polymerizing a hydrophilic monomer and caprolactam.Commercially available products of such polyamide resins are not particularly limited, but specifically, can be water-soluble nylon (manufactured by Toray Industries, Inc., product name: AQ nylon A series) which is a polycondensation product of 2-aminoethylpiperazine adipate and ε-caprolactam, water-soluble nylon (manufactured by Toray Industries, Inc., product name: AQ nylon P series) which is a polycondensation product of polyethylene glycol diammonium adipate and ε-caprolactam, water-soluble nylon (manufactured by Toray Industries, Inc., product name: AQ nylon T series) which is a polycondensation product of 2-aminoethylpiperazine adipate, polyethylene glycol diammonium adipate, and ε-caprolactam, and can be preferably used.
[0164] The content of the cationic resin binder resin (b-4) is preferably 10% by mass or more and 50% by mass or less, and more preferably 10% by mass or more and 40% by mass or less, when the total amount of the ink receiving layer is taken as 100% by mass. When the cationic resin is 10% by mass or more, many basic groups are provided on the surface of the ink receiving layer, which facilitates interaction with the water-based ink, and the ink concentration of the obtained recorded matter tends to be improved. Also, when the cationic resin is 10% by mass or less, the ink tends to be less likely to get tangled in the recesses.
[0165] In addition, in order to improve the ink density of the solid portion of the aqueous ink, it is preferable to make the depth of the microcell surface unevenness deeper. In order to provide such fine surface unevenness, it is preferable that the ink receiving layer has oxygen inhibition ability. An example of the binder resin (b-4) having such oxygen inhibition ability is the above-mentioned polyvinyl alcohol (PVA). In addition, it is more preferable to use the inorganic layered compound (b-5) described later in combination. By using polyvinyl alcohol, the ink density of the obtained recorded matter tends to be further improved. A flexographic printing plate having such an ink receiving layer is more suitable for aqueous flexographic ink for film applications.
[0166] Polyvinyl alcohol (PVA) may be partially substituted with esters, ethers, and acetals as long as it contains a substantial amount of unsubstituted vinyl alcohol units having the required water solubility. It may also contain other copolymerization components. Specific examples of polyvinyl alcohol include those that are 71 to 100 mol % hydrolyzed and have a degree of polymerization in the range of 300 to 2400.
[0167] Commercially available polyvinyl alcohol products are not particularly limited, but specific examples include JMR-8M manufactured by Nippon Vinyl Acetate & Poval, and PVA-105, PVA-110, PVA-117, PVA-117H, PVA-12, PVA-124, PVA124H, PVA-CS, PVA-CST, PVA-HC, PVA-203, PVA-204, PVA-205, PVA-210, PVA-217, PVA-220, PVA-224, PVA-217EE, PVA-217E, PVA-220E, PVA-224E, PVA-405, PVA-420, PVA-613, and L-8 manufactured by Kuraray Co., Ltd.
[0168] The content of the binder resin (b-4) which is a PVA resin is preferably 10% by mass or more and 50% by mass or less, and more preferably 10% by mass or more and 40% by mass or less, when the total amount of the ink receiving layer is taken as 100% by mass. When the PVA resin is 10% by mass or more, the surface unevenness of the ink receiving layer surface becomes deeper, and the ink concentration of the water-based ink tends to be improved. Also, when the PVA resin is 50% by mass or less, the ink tends to be less likely to get tangled in the recesses.
[0169] In addition, although the contents of the cationic resin and PVA are shown above, the total content of the binder resin (b-4) is preferably 10% by mass or more and 50% by mass or less, and more preferably 10% by mass or more and 40% by mass or less, when the total amount of the ink receiving layer is taken as 100% by mass. When the binder resin (b-4) is 10% by mass or more, the ink concentration of the obtained recorded matter tends to be improved. Also, when the binder resin (b-4) is 10% by mass or less, the ink tends to be less likely to get tangled in the recesses.
[0170] 1.3.6. Inorganic layered compounds (b-5) In this embodiment, the term "inorganic layered compound" refers to an inorganic compound in which unit crystal layers are overlapped to form one layered particle. As the inorganic layered compound (b-5), a compound that swells and / or cleaves in water is preferable, and for example, a clay compound that swells in water is exemplified. In addition, a compound containing aluminum hydroxide, barium sulfate, or potassium titanate dispersed in water is exemplified. Among these compounds, a clay compound that swells in water and a compound containing aluminum hydroxide dispersed in water are particularly preferable.
[0171] Among these, swellable mica is preferred, since the use of swellable mica effectively exhibits oxygen blocking properties, and the ink concentration of the resulting recorded matter tends to be improved.
[0172] The size of the inorganic layered compound (b-5) is preferably such that the inorganic layered compound (b-5) is uniformly arranged in the ink receiving layer, the labyrinth effect is more effective, and the oxygen barrier property of the ink receiving layer is particularly high. From this viewpoint, the inorganic layered compound (b-5) preferably has an average particle size of 10 μm or less and a thickness of 500 nm or less, more preferably an average particle size of 10 μm or less and a thickness of 100 nm or less.
[0173] When the inorganic layered compound (b-5) has an average particle size of 1 μm or more, the ink receiving layer tends to exhibit sufficient oxygen barrier properties. Also, when the average particle size is 10 μm or less, the occurrence of uneven appearance tends to be prevented. Also, when the inorganic layered compound (b-5) has a thickness of 10 nm or more, the particle shape can be maintained, which is suitable for practical use. When the thickness is 500 nm or less, uniform coating is possible, and sufficient oxygen barrier properties tend to be exhibited.
[0174] Examples of commercially available inorganic layered compounds (b-5) include, but are not limited to, micromica (synthetic mica), Somasif MEB-3 (registered trademark of Katakura Co-op Agri Co., Ltd., swelling mica), Kunipia (registered trademark of Kunimine Kogyo Co., Ltd., montmorillonite), Sumecton (registered trademark of Kunimine Kogyo Co., Ltd.) SA (synthetic saponite) manufactured by Kunimine Kogyo Co., Ltd., Bengel (registered trademark of Hojun Co., Ltd., refined natural bentonite) manufactured by Hojun Co., Ltd., Aluminasol F-1000, F-3000, 5N manufactured by Kawaken Fine Chemical Co., Ltd., plate-shaped alumina powder Seraph 00610, 02025, 02050, 05025, 05070, 07070, 10030 manufactured by Kinsei Matec Co., Ltd., Tismo D, Tismo N manufactured by Otsuka Chemical Co., Ltd., and the like.
[0175] The content of the inorganic layer compound (b-5) is preferably 10% by mass or less, more preferably 1 to 8% by mass, and even more preferably 3 to 7% by mass, when the total amount of the ink receiving layer is taken as 100% by mass. By having the content of the inorganic layer compound (b-5) within the above range, the ink concentration of the obtained recorded matter tends to be further improved.
[0176] 1.3.7. Water-soluble photopolymerization initiator (b-6) The ink receiving layer according to the present embodiment preferably contains a water-soluble photoinitiator (b-6) and a water-soluble polymerizable compound (b-7). By containing these components, the ink receiving layer can be photocured, the printing durability is improved, and the adhesion between the ink receiving layer and the photosensitive resin composition layer tends to be improved.
[0177] The photopolymerization initiator (b-6) contained in the ink receiving layer is preferably water-soluble from the viewpoint of coating the ink receiving layer as an aqueous film in the production method thereof as described above.
[0178] Examples of the photopolymerization initiator (b-6) include 2,2-diethoxyacetophenone, 2,4-diethoxyacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (Omnirad 2959 (IGM Resins acetophenone-based photopolymerization initiators such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzil dimethyl ketal; benzophenone-based photopolymerization initiators such as benzophenone, benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, and 4-benzoyl-4'-methyldiphenyl sulfide; oxime ester-based photopolymerization initiators such as 1,2-octadione, 1-[4-(phenylthio)-2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime), and PBG305 (manufactured by Changzhou Strong Electronic Materials Co., Ltd., product name); and photopolymerization initiator mixtures such as 1-Irgacure754 (manufactured by BASF Ltd., product name). The photopolymerization initiators may be used alone or in combination of two or more.
[0179] Among these, from the viewpoint of adhesion between the photosensitive resin composition layer and the ink receiving layer after pattern formation, the acetophenone-based photopolymerization initiators and oxime ester-based photopolymerization initiators are preferred.
[0180] The content of the water-soluble photopolymerization initiator (b-6) is preferably 1% by mass or more and 10% by mass or less, more preferably 1.5% by mass or more and 8% by mass or less, and even more preferably 2% by mass or more and 6% by mass or less, when the total amount of the ink receiving layer is taken as 100% by mass. By having the content of the water-soluble photopolymerization initiator (b-6) within the above range, printing durability is further improved, and the adhesion between the ink receiving layer and the photosensitive resin composition layer also tends to be further improved.
[0181] 1.3.8.Water-soluble polymerizable compound (b-7) The water-soluble polymerizable compound (b-7) contained in the ink receiving layer according to this embodiment is preferably water-soluble from the viewpoint of coating as an aqueous film in the production method thereof as described above.
[0182] The water-soluble polymerizable compound (b-7) is not particularly limited, and examples thereof include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, glyceryl (meth)acrylate, (meth)acrylic acid, polyethylene glycol mono(meth)acrylate, tris(2-hydroxyethyl)isocyanurate triacrylate (Sartomer SR368, manufactured by Arkema), dipentaerythritol pentaacrylate (SR399, manufactured by Arkema), and the like, which may be used alone or in combination of two or more kinds.
[0183] In addition, the water-soluble polymerizable compound (b-7) is more preferably one having an amide skeleton or a urethane skeleton. By using such a water-soluble polymerizable compound (b-7), the affinity with the binder resin contained in the water-based ink is improved, and the ink concentration of the obtained recorded matter tends to be improved.
[0184] The water-soluble polymerizable compound (b-7) having an amide skeleton is not particularly limited, but examples thereof include N,N-dimethyl(meth)acrylamide, N-vinylacetamide, N-vinylformamide, N-vinyl-2-pyrrolidone, and acrylamide monomers (FOM-03010, 03006, 03007, 03008, 03009 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)).
[0185] The water-soluble polymerizable compound (b-7) having a urethane skeleton is not particularly limited, but commercially available products such as Art Resin TX-1N, Art Resin TX-17N, Art Resin TX-36N (manufactured by Negami Chemical Industries Co., Ltd.), UA-W2A, UA-W2, UA-7000, UA-7100, UA-7200 (manufactured by Shin-Nakamura Chemical Co., Ltd.), and aliphatic urethane (meth)acrylates (Sartomer CN981, CN1963, CN989 (manufactured by Arkema)) can be used.
[0186] The content of the water-soluble polymerizable compound (b-7) is preferably from 5% by mass to 60% by mass, more preferably from 10% by mass to 50% by mass, and even more preferably from 20% by mass to 40% by mass, when the total amount of the ink-receiving layer is taken as 100% by mass.
[0187] 1.3.9. Water-soluble crosslinker (b-8) The ink receiving layer of this embodiment may contain a water-soluble crosslinking agent (b-8). By using the water-soluble crosslinking agent (b-8), compounds having amino groups contained in the ink receiving layer can be crosslinked. This promotes crosslinking of the ink receiving layer, increases physical resistance to brushes during the development process, and makes it easier for a film to remain.
[0188] It is preferable that the water-soluble crosslinking agent (b-8) is one that exists chemically stable without crosslinking in the coating liquid during the process of applying a coating liquid consisting of the ink-receiving layer composition to the infrared ablation layer described below, and that crosslinking is promoted by heat during the coating and drying process.
[0189] From the above viewpoint, the water-soluble crosslinking agent (b-8) is not particularly limited, but it is preferable to use, for example, water-soluble methylolmelamine or a water-dispersible and / or water-soluble blocked isocyanate compound. For example, the water-soluble methylolmelamine may be Nika Resin (manufactured by Nippon Carbide Industries Co., Ltd.), and the water-dispersible and / or water-soluble blocked isocyanate compound may be blocked isocyanate SU-268A, Meikanate CX, DM-6400, or Meikanate TP-10 (manufactured by Meisei Chemical Industry Co., Ltd.).
[0190] In addition, for the purpose of promoting crosslinking between the compound having an amino group and the water-soluble polymerizable compound, a blocked isocyanate monomer can be used, such as Karenz MOI-BM, MOI-BP, and MOI-DEM (manufactured by Showa Denko K.K.).
[0191] The content of the water-soluble crosslinking agent (b-8) is preferably 10% by mass or less, more preferably 1 to 8% by mass, and even more preferably 3 to 7% by mass, based on the total amount of the ink receiving layer. By having the content of the water-soluble crosslinking agent (b-8) within the above range, printing durability tends to be further improved.
[0192] 1.3.10.Surfactants (b-9) Examples of the surfactant include anionic surfactants, ionic surfactants, nonionic surfactants, anionic reactive surfactants, and nonionic reactive surfactants.
[0193] The surfactant is not particularly limited, but examples thereof include sodium polyoxyethylene styrenated phenyl ether sulfate, sodium polyoxyalkylene branched decyl ether sulfate, ammonium polyoxyethylene isodecyl ether sulfate, sodium polyoxyethylene tridecyl ether sulfate, sodium polyoxyethylene alkyl (C8 to C20) ether sulfate, ammonium polyoxyethylene oleyl cetyl ether sulfate, sodium polyoxyethylene oleyl cetyl ether sulfate, polyoxyethylene tridecyl ether phosphate, polyoxyethylene alkyl (C2 to C16) ether phosphate, polyoxyethylene ammonium sulfate ... anionic surfactants such as alkyl (C2-C16) ether phosphate monoethanolamine salt, sodium alkyl (C2-C16) phosphate, alkyl (C2-C16) phosphate monoethanolamine salt, disodium lauryl sulfosuccinate, disodium lauryl polyoxyethylene sulfosuccinate, disodium polyoxyethylene alkyl (C2-C20) sulfosuccinate, sodium linear alkylbenzene sulfonate, linear alkylbenzene sulfonic acid, sodium alpha-olefin sulfonate, phenol sulfonic acid, sodium dioctyl sulfosuccinate, sodium lauryl sulfate, and potassium salts of higher fatty acids;
[0194] Ionic surfactants such as alkyl (C8-C20) trimethyl ammonium chloride, alkyl (C8-C20) dimethyl ethyl ammonium chloride, didecyl dimethyl ammonium chloride, lauryl dimethyl benzyl ammonium chloride, stearyl dimethyl hydroxyethyl ammonium paratoluenesulfonate, stearyl dimethyl aminopropyl amide, tributyl benzyl ammonium chloride, lauryl dimethyl amino acetate betaine, lauric acid amidopropyl betaine, coconut oil fatty acid amidopropyl betaine, octanoic acid amidopropyl betaine, and lauryl dimethyl amine oxide; Polyoxyalkylene tridecyl ether, polyoxyethylene isodecyl ether, polyoxyalkylene lauryl ether, polyoxyalkylene alkyl ether, mixture of polyoxyalkylene ether and polyether polyol, polyether polyol, polyoxyethylene sulfonated phenyl ether, polyoxyethylene naphthyl ether, phenoxyethanol, polyoxyethylene phenyl ether, polyoxyethylene polyoxypropylene glycol, polyoxyethylene lauryl ether, polyoxyethylene oleyl cetyl ether, polyoxyethylene oleic acid ester, polyoxyethylene distearate acid ester, polyoxyethylene glyceryl isostearate, polyoxyethylene hydrogenated castor oil, coconut oil fatty acid diethanolamide, Examples of the surfactant include nonionic surfactants such as polyoxyethylene alkylamine, sorbitan trioleate, sorbitan sesquioleate, sorbitan monooleate, sorbitan monococolate, sorbitan monocaprate, polyoxyethylene sorbitan monococoate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, octyl polyglycoside, butyl polyglycoside, sucrose benzoate, sucrose acetate, and sucrose fatty acid ester; anionic reactive surfactants such as polyoxyethylene-1-(allyloxymethyl) alkyl ether ammonium sulfate and polyoxyethylene nonylpropenyl phenyl ether ammonium sulfate; and nonionic reactive surfactants such as polyoxyethylene nonylpropenyl phenyl ether.
[0195] The surfactants may be used alone or in combination of two or more.
[0196] The surfactant may be added to the ink receiving layer as well as other layers, such as a photosensitive resin composition layer, and when the total amount of the layer to which the surfactant is added is taken as 100 mass %, the surfactant is preferably contained in an amount of 0.1 mass % or more and 5.0 mass % or less, more preferably 0.5 mass % or more and 3.0 mass % or less, and even more preferably 0.5 mass % or more and 2.0 mass % or less.
[0197] By containing 0.1% by mass or more of a surfactant, the washing speed during development after exposure can be improved, while by containing 5.0% by mass or less of a surfactant, swelling of the flexographic printing plate precursor tends to be suppressed.
[0198] 1.4.Infrared ablation layer The flexographic printing original plate of this embodiment has an infrared ablation layer on a photosensitive resin composition layer via an ink-receptive layer. The infrared ablation layer can be patterned by infrared rays and serves as a mask image when the photosensitive resin composition layer is exposed and cured. When the unexposed parts of the photosensitive resin composition layer are washed out after the exposure, the infrared ablation layer is also removed at the same time.
[0199] The infrared ablation layer preferably comprises a binder polymer and an infrared sensitive material.
[0200] Examples of the binder polymer include polyamide, polyester, and copolymers of monovinyl-substituted aromatic hydrocarbons and conjugated dienes. In particular, copolymers of monovinyl-substituted aromatic hydrocarbons such as styrene, α-methylstyrene, and vinyltoluene and conjugated dienes such as 1,3-butadiene and isoprene are preferred. By using such a binder polymer to form the infrared ablation layer, the affinity with the ink receiving layer is high and the adhesion is good.
[0201] Furthermore, when a polyester is used as the binder polymer, the number average molecular weight thereof is preferably from 300 to 10,000. Furthermore, the polyester is not particularly limited, but suitable examples thereof include those synthesized from an alkanediol and adipic acid, those synthesized from an alkanediol and phthalic acid, polycaprolactone, and combinations of two or more of these polyesters.
[0202] The polyester may contain various functional groups such as amino groups, nitro groups, sulfonic acid groups, and halogens, to the extent that compatibility with other binder polymers, infrared-sensitive substances, and non-infrared radiation shielding substances is not impaired.
[0203] The infrared-sensitive substance is not particularly limited, but for example, a simple substance or compound that has strong absorption in the range of 750 to 2000 nm is preferably used.
[0204] Examples of such infrared-sensitive materials include, but are not limited to, inorganic pigments such as carbon black, graphite, copper chromite, and chromium oxide; dyes such as polyphthalocyanine compounds, cyanine dyes, and metal thiolate dyes; and the like.
[0205] The content of these infrared-sensitive substances is within a range that provides sensitivity that allows ablation with the laser beam used. The content of the infrared-sensitive substance is preferably 10 to 80% by mass based on the total amount of the infrared ablation layer.
[0206] In addition, the infrared-sensitive material may be a material that reflects or absorbs radiation such as ultraviolet rays. Radiation absorbers for ultraviolet rays, carbon black, graphite, etc. are good examples, and the amount added is set so that the required optical density can be achieved. In general, it is preferable to add the material so that the optical density is 2 or more, preferably 3 or more.
[0207] 2. How flexographic printing plates are manufactured Examples of methods for producing a flexographic printing plate from a flexographic printing original plate include a back exposure step of irradiating ultraviolet light from the support side, an infrared irradiation step of irradiating an infrared ablation layer with infrared light to draw and process a pattern, a relief exposure step of irradiating a photosensitive resin composition layer with ultraviolet light through an ink receptive layer using the infrared ablation layer on which the pattern has been drawn and processed as a mask, and a development step of removing unexposed areas of the infrared ablation layer, the ink receptive layer, and the photosensitive resin composition layer.
[0208] A schematic diagram showing a method for producing a flexographic printing plate using a flexographic printing plate precursor of this embodiment is shown in Figure 2. Each step will be described in detail below.
[0209] 2.1. Back exposure process First, in the back exposure step S1, the entire surface of the flexographic printing original plate 10 is exposed to ultraviolet light through the support 11 (back exposure), and the photosensitive resin composition layer 12 is cured to form a thin, uniform cured layer (back surface 12a). Note that this back surface 12a is a part included in the photocured photosensitive resin composition layer 12a formed in the relief exposure step S3. The exposure method at this time is not particularly limited, and can be performed using a known irradiation unit.
[0210] The source of ultraviolet light is not particularly limited, but examples thereof include low pressure mercury lamps, high pressure mercury lamps, extra high pressure mercury lamps, metal halide lamps, xenon lamps, zirconium lamps, carbon arc lamps, and ultraviolet fluorescent lamps.
[0211] The back exposure step may be performed before the infrared irradiation step, or may be performed simultaneously with the back exposure step S1 and the relief step S3 as shown in Fig. 3. Fig. 3 is the same as that shown in Fig. 2 except for the order of the steps.
[0212] 2.2. Infrared irradiation process Next, in the infrared irradiation step S2, the infrared ablation layer 14 on the photosensitive resin composition layer 12 is laser-drawn, i.e., laser-ablated, to produce a negative pattern 14a. If the flexographic printing plate 10 has a cover film on the infrared ablation layer 14, the cover film is first peeled off before infrared irradiation. Then, the infrared ablation layer is irradiated with infrared rays in a pattern to decompose the resin in the irradiated areas, and a pattern is drawn and processed. This allows a mask of the infrared ablation layer to be formed on the photosensitive resin composition layer via the ink-receptive layer.
[0213] In addition, the heat generated at this time may cause the polymer particles (b-1) of the ink-receiving layer 13 located below the infrared ablation layer 14 to fuse and heat-cure, or may cause the binder resin (b-4), the polymerizable compound (b-7), and the water-soluble crosslinking agent (b-8) to harden.
[0214] 2.3. Relief exposure process In the relief exposure process S3, the infrared ablation layer 14a on which a negative pattern is formed is used as a mask to perform image exposure (relief exposure) on the photosensitive resin composition layer 12 through the ink-receiving layer 13, thereby forming a photocured photosensitive resin composition layer 12a.
[0215] At this time, the light passing through the mask promotes the curing reaction of the photosensitive resin composition layer, and the pattern formed on the infrared ablation layer is transferred to the photosensitive resin composition layer with the concaves and convexes reversed. Note that the entire surface of the flexographic printing plate may be irradiated with ultraviolet light.
[0216] In addition, the radicals generated at this time may crosslink the unsaturated bonds contained in the polymer particles (b-1) of the ink-receiving layer 13 on the photosensitive resin composition layer 12, or may harden the binder resin (b-4), the polymerizable compound (b-7), or the water-soluble crosslinking agent (b-8).
[0217] 2.4.Developing process Thereafter, in the development step, the unexposed portions of the infrared ablation layer 14a, the ink receiving layer 13, and the photosensitive resin composition layer 12 are removed. The removal method is not particularly limited, but for example, the unexposed portions are washed away with a solvent-based developer or a water-based developer, or the unexposed portions heated to 40° C. to 200° C. are brought into contact with an absorbing layer capable of absorbing the exposed portions, and the absorbing layer is removed to remove the unexposed portions.
[0218] Development can also be carried out by heat. In the case of thermal development, no solvent is used. Instead, the photosensitive resin composition layer and the ink-receptive layer are heated after imagewise exposure in contact with an absorbent material. The absorbent material can be, for example, a porous nonwoven fabric made of nylon, polyester, cellulose, or inorganic materials. The layer is heated to a temperature at which the uncured parts of the layer are liquefied and can be absorbed by the nonwoven fabric. The saturated nonwoven fabric is then removed. Details regarding thermal development are disclosed, for example, by U.S. Pat. No. 3,264,103, U.S. Pat. No. 5,175,072, WO 96 / 14603, or WO 01 / 88615. If necessary, the mask can be removed beforehand by a suitable solvent or similarly by heat.
[0219] Furthermore, if necessary, the plate is then exposed to a post-treatment to obtain a flexographic printing plate. As the post-treatment exposure, the surface is irradiated with light having a wavelength of 300 nm or less. If necessary, light having a wavelength longer than 300 nm may also be used.
[0220] The exposure from the infrared ablation layer side (relief exposure) and the exposure from the support film side (back exposure) may be performed in any order, or both may be performed simultaneously. Examples of the exposure light source include a high-pressure mercury lamp, an ultraviolet fluorescent lamp, a carbon arc lamp, a xenon lamp, etc.
[0221] For laser drawing, an infrared laser can be used, and the infrared laser preferably has a wavelength of 750 to 2000 nm. Infrared lasers with this wavelength are generally semiconductor lasers with a wavelength of 750 to 880 nm and Nd-YAG lasers with a wavelength of 1060 nm.
[0222] When the unexposed portion of the photosensitive resin composition layer is developed with a solvent-based developer, suitable examples of the developer include esters such as heptyl acetate, 3-methoxybutyl acetate, etc.; hydrocarbons such as petroleum fractions, toluene, decalin, etc.; mixtures of chlorine-based organic solvents such as tetrachloroethylene with alcohols such as propanol, butanol, pentanol, etc.; and ethers such as polyoxyalkylene alkyl ether.
[0223] The unexposed areas can be washed out by spraying from a nozzle and / or by brushing with a brush.
[0224] When the unexposed portion of the photosensitive resin composition layer is developed with an aqueous developer, the aqueous developer is a developer containing water as a main component, and may be water itself or, for example, water blended with a nonionic or anionic surfactant, a pH adjuster, a cleaning promoter, and the like.
[0225] The nonionic surfactant is not particularly limited, but examples thereof include polyoxyalkylene alkyl or alkenyl ethers, polyoxyalkylene alkyl or alkenyl phenyl ethers, polyoxyalkylene alkyl or alkenyl amines, polyoxyalkylene alkyl or alkenyl amides, ethylene oxide / propylene oxide block adducts, and the like.
[0226] The anionic surfactant is not particularly limited, but examples thereof include linear alkylbenzene sulfonates having an alkyl group with an average of 8 to 16 carbon atoms, α-olefin sulfonates having an average of 10 to 20 carbon atoms, dialkyl sulfosuccinates having an alkyl or alkenyl group with 4 to 10 carbon atoms, sulfonates of fatty acid lower alkyl esters, alkyl sulfates having an average of 10 to 20 carbon atoms, alkyl ether sulfates having a linear or branched alkyl or alkenyl group with an average of 10 to 20 carbon atoms and to which an average of 0.5 to 8 moles of ethylene oxide have been added, and saturated or unsaturated fatty acid salts having an average of 10 to 22 carbon atoms.
[0227] The pH adjuster is not particularly limited, but examples thereof include sodium borate, sodium carbonate, sodium silicate, sodium metasilicate, sodium succinate, sodium acetate, etc. Among the above, sodium silicate is preferred because it is easily dissolved in water.
[0228] The cleaning promoter is a combination of the above surfactant and a pH adjuster, which enhances the cleaning (developing) ability of the developer.
[0229] The cleaning accelerator is not particularly limited, but examples thereof include amines such as monoethanolamine, diethanolamine, and triethanolamine, ammonium salts such as tetramethylammonium hydroxide, and paraffin-based hydrocarbons.
[0230] One or more selected from the group consisting of nonionic, anionic and other surfactants, pH adjusters, and cleaning promoters can be added and mixed in the developer in an amount of preferably 0.1 to 50% by mass, more preferably 1 to 10% by mass.
[0231] During development, the flexographic printing plate precursor may be subjected to auxiliary vibrations such as ultrasonic waves, or the surface of the printing plate precursor may be rubbed with a mechanical means such as a brush.
[0232] From the viewpoint of obtaining a flexographic printing plate having excellent ink adhesion and ink transferability, it is preferable to blend 0.01% by mass or more to 5% by mass of a silicone compound in the solvent-based and aqueous developers. That is, the flexographic printing plate of the present embodiment is preferably a flexographic printing plate obtained by developing a flexographic printing original plate after pattern formation and exposure in a developer containing 0.01% by mass or more to 5% by mass of a silicone compound.
[0233] The silicone compound is not particularly limited, and examples thereof include silicone oil containing a siloxane unit (hereinafter simply referred to as silicone oil), a silane coupling agent, a silane compound, silicone rubber, a silicone resin, etc. Among the silicone compounds, the silicone compound to be contained in the developer is preferably a silicone oil modified with an amino group, a polyether group, a carbinol group, etc.
[0234] 3. Flexographic printing plates The flexographic printing plate of the present embodiment is a flexographic printing plate comprising at least a support, a photocured photosensitive resin composition layer, and an ink-receiving layer laminated in that order, the ink-receiving layer having a thickness of 5 μm to 50 μm, and the ink-receiving layer contains polymer particles having a butadiene skeleton and having a carboxyl group and / or a hydroxyl group, and / or polymer particles in which a monobasic or polybasic acid monomer is polymerized.
[0235] FIG. 4 shows a schematic diagram for explaining ink adhesion, and FIG. 5 shows a schematic cross-sectional view of the flexographic printing plate of this embodiment.
[0236] First, ink entanglement will be described. As shown in the left diagram of Fig. 4, ideally, ink 301 adheres only to the tops of the relief of the flexographic printing plate 100, and the ink 301 is transferred to the printing substrate 310. However, in the conventional flexographic printing plate 200, there is a problem that ink 302 accumulates in the relief recesses 210, and the ink 302 is also transferred to the printing substrate 310 together with the transfer of the ink 301. In particular, when printing is continued for a long period of time, the ink 302 often enters the relief recesses 210 of the printing plate 200 (ink entanglement), and even parts 303 that are not the original image are printed.
[0237] In contrast, in the present embodiment, by providing an ink-receiving layer 13 on the top of the photocured photosensitive resin composition layer 12a, the recesses of the photocured photosensitive resin composition layer 12a can be made to have properties that make them less susceptible to ink entanglement, while the top (ink-receiving layer 13) can be made to have properties that provide excellent printing characteristics.
[0238] 5, the flexographic printing plate 100 has a support 11, a photocured photosensitive resin composition layer 12a on which an arbitrary concavo-convex pattern has been formed by relief exposure, and an ink-receiving layer 13 disposed on the top of the photocured photosensitive resin composition layer 12a. The ink-receiving layer 13 is formed on the top of the photocured photosensitive resin composition layer 12a, and during printing, ink adheres to the ink-receiving layer 13, and the ink adhered to the ink-receiving layer 13 adheres to the printed material, thereby performing flexographic printing.
[0239] 3.1.Support The support is not particularly limited, but for example, the same supports as those exemplified for the flexographic printing plate precursor can be used.
[0240] 3.2. Photocured photosensitive resin composition layer The photocured photosensitive resin composition layer 12a has a concave-convex pattern formed thereon.
[0241] 3.3.Ink-receiving layer The ink receiving layer 13 is not particularly limited, but for example, the same layer as that exemplified in the flexographic printing plate precursor can be used.
[0242] The ink-receiving layer 13 is formed on top of the photocured photosensitive resin composition layer 12a. In the ink-receiving layer 13, a solid portion without unevenness, microcells, or halftone dots may be formed as shown in FIG. 5, depending on the image to be printed. In order to create a print with high saturation, it is preferable that the ink-receiving layer 13 carries a large amount of ink, and it is particularly preferable that unevenness such as microcells is provided. Here, the microcells refer to portions in which unevenness is created by introducing fine patterns that do not affect the design into the surface, thereby improving the transferability of the ink.
[0243] The deeper the microcell recesses, the more ink they can hold, but if they are too deep, the diameter of the recesses becomes large, limiting the area in which recesses can be formed in the highlights. Taking these factors into consideration, the depth of the recesses caused by the microcells formed on the flexographic printing plate is preferably 1 μm to 12 μm, more preferably 3 μm to 10 μm, and even more preferably 5 μm to 10 μm (see Figure 5).
[0244] Other configurations of the flexographic printing plate 100 can be the same as those already described for the flexographic printing plate blank 10. Other configurations of the flexographic printing plate 100 are exemplified below, but for parts not exemplified, the description of the flexographic printing plate blank 10 can be referred to.
[0245] In forming microcells, a thicker ink-receiving layer in the flexographic printing plate is also preferable because it makes it easier to process the convex portions of the dots (see Figure 5). On the other hand, the depth of the concave portions between the dots on the relief is formed to be around 100 μm. Therefore, the thicker the ink-receiving layer is, the more the dots themselves are formed from the components of the ink-receiving layer. This makes it easier for ink to accumulate between the dots (concave portions). Taking these balances into consideration, the thickness of the ink-receiving layer is 5 μm or more and 50 μm or less, preferably 10 μm or more and 45 μm or less, and more preferably 10 μm or more and 40 μm or less.
[0246] For example, the difference (Ei-Ep) between the surface free energy Ei of the ink receiving layer and the surface free energy Ep of the photosensitive resin composition layer is 0 mJ / m 2 Greater than 5mJ / m 2 Less than or equal to 0 mJ / m is preferable. 2 Greater than 4mJ / m 2 Less than or equal to 0.5 to 3.5 mJ / m is more preferable. 2 More preferably, 1.0 to 3.5 mJ / m 2 On the other hand, it is more preferable that the difference (Ei-Ep) between the surface free energy of the ink receiving layer and the surface free energy of the photosensitive resin composition layer is 5 mJ / m 2By setting the content below, the ink receptivity of the resulting flexographic printing plate is further improved, and the adhesion between the ink-receiving layer and the photosensitive resin composition layer tends to be maintained even after development.
[0247] In addition, it is preferable that the surface free energy Ei of the ink-receiving layer is greater than the surface free energy Ep of the photosensitive resin composition layer, and it is preferable that the film zeta potential of the ink-receiving layer exhibits a positive value. For example, it is preferable that the surface free energy Ei of the ink-receiving layer is 5 mJ / m higher than the surface free energy Ep of the photosensitive resin composition layer. 2 If it exceeds this value, it is not suitable for printing in high definition and highlight areas, and the dots on the printed matter tend to become thicker. This is because the surface free energy Ei of the ink-receiving layer is 5 mJ / m lower than the surface free energy Ep of the photosensitive resin composition layer. 2 It is speculated that when the amount is excessive, the ink is less likely to accumulate in the recesses of the photosensitive resin, but instead, an excess of ink is supplied to the protruding parts.
[0248] Here, the surface free energy was evaluated as a resin characteristic of each of the ink-receptive layer and the photosensitive resin composition. The surface free energy of the ink-receptive layer refers to the outermost surface of the resin plate exposed to development (see Figure 5), and the surface free energy of the photosensitive resin composition was evaluated using the "back surface" part shown in Figure 5.
[0249] From the same viewpoint as above, the surface free energy Ei of the ink receiving layer is preferably 33 to 43 mJ / m 2 and preferably 34 to 42 mJ / m 2 and more preferably 35 to 41 mJ / m 2 The surface free energy Ep of the photosensitive resin composition layer is preferably 30 to 40 mJ / m 2 and preferably 31 to 39 mJ / m 2 and more preferably 32 to 38 mJ / m 2 The surface free energy can be determined by the method described in the Examples.
[0250] In addition, the components of the ink-receiving layer 13 are not particularly limited, but examples thereof include the same components as those exemplified in the flexographic printing plate precursor, such as the polymer particles (b-1), thickener (b-2), silicone compound (b-3), binder resin (b-4), inorganic layered compound (b-5), water-soluble photopolymerization initiator (b-6), water-soluble polymerizable compound (b-7), water-soluble crosslinking agent (b-8), and surfactant (b-9).
[0251] The ink receiving layer 13 contains polymer particles similar to the polymer particles (b-1). Among these, the polymer particles are preferably polymer particles having a butadiene structure and a carboxylic acid group and / or a hydroxyl group, and polymer particles obtained by polymerizing a monobasic or polybasic acid monomer, and more preferably polymer particles having a butadiene structure and a carboxylic acid group and / or a hydroxyl group. The content of the polymer particles is preferably 20% by mass or more and 95% by mass or less with respect to 100% by mass of the ink receiving layer.
[0252] The ink receiving layer 13 preferably further contains, as the binder resin (b-4), a polyvinyl alcohol resin or a binder resin having a basic group. The binder resin having a basic group more preferably contains a polyamide resin and / or a polyurethane resin.
[0253] It is preferable that the binder resin contains a polyvinyl alcohol resin, a swellable mica, a water-soluble photoinitiator, and a water-soluble polymerizable compound. In addition, the binder resin having a basic group preferably contains a polyamide resin and / or a polyurethane resin. Furthermore, the water-soluble polymerizable compound preferably has an amide skeleton and / or a urethane skeleton.
[0254] 4. Recording method The flexographic printing plate of the present embodiment can be used by being placed on a plate cylinder. The printing method is not particularly limited as long as it is a conventionally known method, but for example, a roller in contact with ink is brought into contact with the flexographic printing plate placed on the plate cylinder, and the ink is held in the ink-receiving layer. Then, the ink held in the ink-receiving layer is transferred to the surface of the printing substrate.
[0255] In response to growing interest in environmental issues, technology related to water-based inks for film printing applications has been disclosed from the perspective of reducing VOC (volatile organic compound) emissions (for example, Patent No. 6380775). Compared to solvent-based inks, water-based inks have issues with adhesion to film, blocking resistance associated with offset of printed images, and "ink resolubility" to reduce tangling stains caused by the ink drying on the plate during long-run printing, and efforts are being made to improve these issues.
[0256] The water-based ink used in flexographic printing refers to water-based ink whose main component is water. The main component of the solvent means that the solvent is 50 wt% or more, preferably 80 wt% or more. The solvent preferably has an alcohol content of 5 wt% or less.
[0257] Flexographic ink is composed of a colorant such as a pigment, a vehicle such as a water-soluble resin or resin, an auxiliary such as a wax or an antifoaming agent, a solvent, and the like, and in this embodiment, a commercially available ink may be used.
[0258] In addition, the flexographic printing plate of this embodiment can also be used with solvent ink. EXAMPLES
[0259] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples in any way.
[0260] [Production Example 1] (Synthesis of hydrophilic copolymer) A pressure-resistant reactor equipped with a stirrer and a jacket for temperature control is initially charged with 125 parts by mass of water and 2 parts by mass of "ADEKA REASOAP" (manufactured by Asahi Denka Kogyo Co., Ltd.), an ammonium salt of (α-sulfo(1-nonylphenoxy)methyl-2-(2-propenyloxy)ethoxy-poly(oxy-1,2-ethanediyl), as a reactive emulsifier. The internal temperature is raised to 80°C, and 10 parts by mass of styrene, 60 parts by mass of butadiene, 23 parts by mass of butyl acrylate, 5 parts by mass of methacrylic acid, and 10 parts by mass of ethyl acetate are added. An oily mixture of a monomer mixture composed of 2 parts by mass of acrylic acid and 2 parts by mass of t-dodecyl mercaptan, and an aqueous solution composed of 28 parts by mass of water, 1.2 parts by mass of sodium peroxodisulfate, 0.2 parts by mass of sodium hydroxide, and 2 parts by mass of the ammonium salt of (α-sulfo(1-nonylphenoxy)methyl-2-(2-propenyloxy)ethoxy-poly(oxy-1,2-ethanediyl) were added at a constant flow rate over 5 hours and 6 hours, respectively.
[0261] The temperature of 80°C was then maintained for 1 hour to complete the polymerization reaction, and the copolymer latex was obtained, which was then cooled. The pH of the copolymer latex thus produced was adjusted to 7 with sodium hydroxide, after which unreacted monomers were removed by steam stripping, and the mixture was filtered through a 200-mesh wire net. Finally, the solid content of the filtrate was adjusted to 40% by mass, to obtain an aqueous dispersion of the hydrophilic copolymer. The aqueous dispersion of the hydrophilic copolymer thus obtained was dried up in a vacuum dryer at 50°C to remove water, and the hydrophilic copolymer was obtained.
[0262] [Production Example 2] (Preparation of a base film (support) having an adhesive layer) To prepare a solution for the adhesive layer to be coated on the base film (support), 55 parts by mass of Tufprene 912 (trade name, manufactured by Asahi Kasei Corporation), a block copolymer of styrene and 1,3-butadiene, 38 parts by mass of paraffin oil (average carbon number 33, average molecular weight 470, density at 15°C 0.868), 2.5 parts by mass of 1,9-nonanediol diacrylate, 1.5 parts by mass of 2,2-dimethoxy-phenylacetophenone, 3 parts by mass of Epoxy Ester 3000M (trade name, manufactured by Kyoeisha Chemical Co., Ltd.), and 1.5 parts by mass of Varifast Yellow 3150 (trade name, manufactured by Orient Chemical Industry Co., Ltd.) were dissolved in toluene to obtain a solution with a solids content of 25%.
[0263] Then, the adhesive was applied to one side of a 100 μm thick polyester film using a knife coater so that the ultraviolet transmittance was 10%, and dried at 80° C. for 1 minute to obtain a base film (support) having an adhesive layer. The UV transmittance of the support was calculated by measuring the transmission intensity with a UV illuminometer MO-2 type (manufactured by Oak Manufacturing, product name, UV-35 filter) using an ultraviolet exposure machine AFP-1500 (manufactured by Asahi Kasei Corporation, product name).
[0264] [Production Example 3] (Preparation of film having infrared ablation layer) 65% by mass of Asaflex 810 (trade name, manufactured by Asahi Kasei Corporation), a block copolymer of styrene and 1,3-butadiene, and 35% by mass of carbon black as an infrared-sensitive material were kneaded in a kneader and cut into pellets. 90 parts by mass of the pellets and 10 parts by mass of 1,6-hexanediol adipate were then dissolved using ultrasound in a mixed solvent prepared with a mass ratio of ethyl acetate / butyl acetate / propylene glycol monomethyl ether acetate = 50 / 30 / 20 to prepare a uniform solution with a solid content of 12% by mass.
[0265] Next, this solution is applied to a polyester film with a thickness of 100 μm to become a cover sheet, so that the coating amount after drying is 4 to 5 g / m 2The coating was performed using a knife coater so that the coating was in the range of 100 to 200 nm, and then dried at 80° C. for 1 minute to obtain a film having an infrared shielding layer (infrared ablation layer) that can be ablated by infrared rays. The optical density of the film having the infrared ablation layer was measured using DM-500 (trade name, manufactured by Dainippon Screen Mfg. Co., Ltd.) and found to be 3 to 4.
[0266] [Production Example 4] (Preparation of cover film (film having ink-receptive layer and infrared ablation layer)) A solution was prepared with an ethanol / distilled water mass ratio of 10 / 90, and 92 mass% of water-dispersible latex (Asahi Kasei Corporation, L7430), 3 mass% of thickener (ethylene oxide / propylene oxide copolymer, Meisei Chemical Industry Co., Ltd., ALKOX EP-10), and 5 mass% of modified silicone oil (Shin-Etsu Chemical Co., Ltd., KF-351A) were added and stirred to prepare the ink-receiving layer coating liquid.
[0267] Next, the ink-receiving layer coating liquid was applied using a bar coater to the infrared ablation layer-forming surface side of the film having the infrared ablation layer produced in Production Example 3, so that the film thickness after drying would be 30 μm. This was then dried at 120° C. for 4 minutes to obtain a cover film having an ink-receiving layer and an infrared ablation layer.
[0268] Example 1 (Preparation of flexographic printing plates) 32 parts by mass of the hydrophilic copolymer obtained in the above Production Example 1 and 28 parts by mass of a styrene-butadiene-styrene copolymer [D-KX405: manufactured by Kraton] were mixed at 140°C using a pressure kneader, and then a liquid mixture of 32 parts by mass of liquid polybutadiene [LBR-352: manufactured by Kuraray], 8 parts by mass of 1,9-nonanediol diacrylate, 5 parts by mass of 1,6-hexanediol dimethacrylate, 2 parts by mass of 2,2-dimethoxyphenylacetophenone, 1 part by mass of 2,6-di-t-butyl-p-cresol, and 1 part by mass of carbinol-modified silicone oil [KF-6000: manufactured by Shin-Etsu Chemical] was gradually added over 15 minutes, and after the addition was completed, the mixture was kneaded for another 20 minutes to obtain a photosensitive resin composition.
[0269] Next, the photosensitive resin composition layer was placed in an extrusion molding machine and extruded from a T-shaped die. The surface of the base film (support) obtained in Production Example 2 above on which the adhesive layer was formed was bonded to one side of the photosensitive resin composition layer. Furthermore, a release film (Diafoil MRV100, manufactured by Mitsubishi Chemical Corporation) was bonded to the side of the photosensitive resin composition layer opposite the support laminate side, thereby obtaining a laminate of the support and the photosensitive resin composition layer.
[0270] Next, the release film was peeled off, and the cover film having the ink-receptive layer and the infrared ablation layer obtained in the above Production Example 4 was laminated so that the ink-receptive layer was in contact with the photosensitive resin composition layer to obtain a flexographic printing original plate. The photosensitive resin composition layer formed as described above is hereinafter referred to as Mode A (water).
[0271] [Examples 2 to 13, 16 to 39, Comparative Examples 1 to 3, 6 to 9] As shown in Tables 1 and 2 below, flexographic printing original plates were obtained in the same manner as in Example 1 above, except that the components used and the thickness of the ink-receiving layer were changed.
[0272] [Examples 14 and 15, Comparative Examples 4 to 5] In producing a photosensitive resin composition, 60 parts by mass of a styrene-butadiene-styrene copolymer [D-KX405: manufactured by Kraton] was mixed at 180°C using a pressure kneader, and then a liquid mixture of 32 parts by mass of liquid polybutadiene [LBR-352: manufactured by Kuraray], 8 parts by mass of 1,9-nonanediol diacrylate, 5 parts by mass of 1,6-hexanediol dimethacrylate, 2 parts by mass of 2,2-dimethoxyphenylacetophenone, 1 part by mass of 2,6-di-t-butyl-p-cresol, and 1 part by mass of amino-modified silicone oil [KF-8000: manufactured by Shin-Etsu Chemical] was gradually added over 15 minutes, and after completion of the addition, the mixture was kneaded for a further 20 minutes to obtain a photosensitive resin composition.
[0273] A flexographic printing original plate was obtained under the same other conditions as in Example 1. The photosensitive resin composition layer formed using the above-mentioned photosensitive resin composition is hereinafter referred to as embodiment B (solvent).
[0274] Comparative Example 10 A photosensitive resin composition was obtained in the same manner as in Example 14, except that 2 parts by mass of a fluoroethylene vinyl ether copolymer (trade name: Lumiflon LF916, manufactured by Asahi Glass Co., Ltd.) was further added.
[0275] The other conditions were the same as those in Example 1 to obtain a flexographic printing original plate. The photosensitive resin composition layer formed using the above-mentioned photosensitive resin composition is hereinafter referred to as embodiment B' (solvent).
[0276] (Flexographic printing plate manufacturing) The flexographic printing plate was exposed from the support side (PET coated with adhesive) using an ultraviolet exposure machine (JE-A2-SS manufactured by Nippon Denshi Seiki Co., Ltd.) so that the pattern height (RD) after curing was about 0.6 mm.
[0277] Next, the cover sheet of the infrared ablation layer was peeled off, and a halftone dot image (AM175 line) was drawn on the infrared ablation layer using an ESKO laser drawing machine (CDI), and then the infrared ablation layer side was exposed to 8000 mJ in the air using the exposure machine. In addition, a portion where a microcell (WSI pattern, ESKO) was provided was provided in the solid image.
[0278] Then, each of the developing methods shown in Tables 2 and 4 was carried out according to the method described below.
[0279] (Water develop) After the relief exposure, an aqueous solution (aqueous developer) of 1% polyoxyalkylene alkyl ether (Newcol 2308: manufactured by Nippon Nyukazai) and 1% potassium carbonate was prepared, and the plate was washed (developed) at 40°C using a cleaning machine (JOW-A3-P) manufactured by Nippon Denshi Seiki Co., Ltd., to remove the unexposed areas. After drying for 10 minutes at 50°C, the plate was exposed to 1500 mJ / cm2 of light over the entire surface of the photopolymer plate after drying using a germicidal lamp (GL-30, manufactured by Toshiba Corporation) with a central wavelength of 254 nm, using an AFP-1216LF (manufactured by Asahi Kasei Corporation, product name) to remove the tackiness of the surface. 2 The post-exposure dose from the germicidal lamp was calculated from the illuminance measured using the UV-25 filter of the "UV-MO2" machine.
[0280] (Solvent development) After the relief exposure, development was performed using 3-methoxybutyl acetate as the developer in an "AFP-1321P" developing machine (manufactured by Asahi Kasei Corporation, product name) at a liquid temperature of 30°C at a speed of 100 mm / min, and then dried at 60°C for 2 hours. Thereafter, as a post-exposure treatment, an AFP-1216LF (manufactured by Asahi Kasei Corporation, product name) was used to apply 2000 mJ / cm2 to the entire surface of the photopolymer plate after drying using a germicidal lamp (manufactured by Toshiba Corporation, GL-30, product name) with a central wavelength of 254 nm. 2 The post-exposure dose from the germicidal lamp was calculated from the illuminance measured using the UV-25 filter of the "UV-MO2" machine.
[0281] (Thermal Development) After the relief exposure, the printing plate was thermally processed in an experimental setup. An exposed piece of the printing plate, measuring 30 cm x 30 cm, was fixed with double-sided adhesive tape to a 35 cm diameter metal roll driven by a motor. A commercially available polyester nonwoven fabric was passed over a 5 cm diameter heatable metal roll. An infrared lamp for relatively fast heating of the printing plate was fixed on the roll holding the printing plate. The infrared lamp was turned on and the heatable metal roll, heated to 170°C, was rotated slowly (approximately 2 rpm) by a motor. Approximately 2.5 x 10 5The plate was conveyed through the nonwoven fabric at a contact pressure of 1 Pa. The roll holding the plate was cycled 14 times to remove the uncured areas.
[0282] [Characteristics evaluation] (Evaluation of flexographic printing plates) <Surface free energy> For the flexographic printing plates obtained in the examples and comparative examples, the surface free energy was calculated from the contact angle measurement. Specifically, the contact angle of the measurement target portion was measured by the droplet method using a solid-liquid interface analyzer DropMaster501 (manufactured by Kyowa Interface Science, product name). After leaving it for one day in a temperature and humidity controlled room at a temperature of 23°C and a relative humidity of 50%, the surface free energy of the plate surface was automatically calculated from the Kitazaki-Hata formula incorporated in the above software using FAMAS analysis software and purified water, ethylene glycol, and diiodomethane (manufactured by Kanto Chemical) as the probe solution. A stainless steel 22G needle (manufactured by Kyowa Interface Science) was used, and the contact angle was automatically measured 15 seconds after each probe solution contacted the plate with the discharge time of 100 ms and the discharge voltage of 4000 mV.
[0283] <Zeta potential> The zeta potential of the surface of the flexographic printing plates obtained in the Examples and Comparative Examples was measured using a membrane zeta potential measuring device (ELSZ, Otsuka Electronics Co., Ltd.). Specifically, after setting the measurement sample in the measurement cell, an electric field was applied parallel to the membrane of the sample using a 10 mM NaCl aqueous solution, and the speed of the induced electroosmotic flow was observed as the motion speed of polystyrene latex (500 nm) that was not charged by modification with hydroxypropyl cellulose, and the zeta potential was calculated from the motion speed.
[0284] <Two-layered evaluation> For the flexographic printing plates obtained in the Examples and Comparative Examples, the morphology of dots formed in the 10% halftone dot area of the AM150 line was observed with a SEM (scanning electron microscope). When the interface between the ink receiving layer and the photosensitive resin composition layer was confirmed, it was determined that the two-layer structure was formed.
[0285] Specifically, Au-Pd was coated at a film thickness of 30 nm using a thin-film coating device (vacuum device, MSP-1S), and conductive treatment was performed. After that, a scanning electron microscope (Keyence, VHX-D510) was used to observe secondary electron images at an accelerating voltage of 5 kV. During observation, randomly selected halftone dots were observed at 900x magnification. When importing the observed images into a computer, the contrast was appropriately adjusted using the auto-contrast function before importing. Since there is a contrast between the ink-receptive layer and the photosensitive resin composition layer, the interface between the layers can be seen. When the interface was confirmed, it was determined that the two-layer structure was achieved.
[0286] (Thickness of ink receiving layer) The flexographic printing plate was exposed to ultraviolet light from the support side for 600 seconds using an ultraviolet exposure machine. After the plate was photocured, the sample was processed using a FIB (Focused Ion Beam) device, and the exposed cross section was observed with a SEM (scanning electron microscope) to evaluate the film thickness of the ink-receiving layer.
[0287] <Evaluation of unevenness of ink receiving layer> For the flexographic printing plates obtained in the Examples and Comparative Examples, microcells (Crystal Screen, Koscographic) were introduced to form dots when laser drawing was performed on the infrared ablation layer. The depth of the surface irregularities of the microcells formed on the dot surfaces was measured using a laser microscope (Keyence VK-X100).
[0288] [Printing evaluation] (Evaluation of flexographic printing plates using solvent inks) Using the flexographic printing plates obtained in the Examples and Comparative Examples, actual printing evaluation was carried out. An AI-3 flexographic printing machine (manufactured by Iyo Kikai) was used, and OPP film was used as the substrate. Process X Cyan (product name, manufactured by Toyo Ink Mfg. Co., Ltd.) was used as the solvent ink. The ink was adjusted to a viscosity of 15 seconds using a Zahn Cup #4 manufactured by Rigo Co., Ltd. by adding a solvent. The anilox roll was 800 lpi (cell volume 3.8 cm). 3 / m 2 ), and 3M1020 (product name, manufactured by Sumitomo 3M Limited) was used for the cushion tape. The printing speed was 100 m / min, and 3000 m was printed.
[0289] (Evaluation of flexographic printing plates using water-based inks) Printing was carried out in the same manner as described above (Evaluation of flexographic printing plates) except that a water-based ink prepared according to the following production example was used instead of a solvent-based ink.
[0290] The materials shown below were mixed in a ball mill for 10 minutes to prepare an ink for evaluation. 42 parts by weight of water-based urethane resin synthesized according to the following synthesis example Urethane acrylic composite resin WEM-202U (Taisei Fine Chemical) 3 parts by weight Pigment: CI Pigment Blue 15:3 15 parts by weight Hydrocarbon wax W300 (Mitsui Chemicals) 2 parts by weight Adipic dihydrazide 0.2 parts by mass Ammonia water 0.2 parts by weight Water / isopropyl alcohol (1:1) 37.6 parts by weight
[0291] <Synthesis example: Water-based urethane resin> In a 4-neck 2000 ml flask equipped with a reflux condenser, a dropping funnel, a gas inlet tube, a stirrer, and a thermometer, 57.3 parts of polytetramethylene glycol having a number average molecular weight of 2000, 20 parts of polyethylene glycol having a number average molecular weight of 2000, 13 parts of dimethylolbutanoic acid, 8 parts of bis(2-hydroxypropyl)aniline, and 1.7 parts of 1,4-cyclohexanedimethanol were charged, substituted with dry nitrogen, and heated to 100°C. With stirring, 41.3 parts of isophorone diisocyanate were dropped over 20 minutes, and the temperature was gradually raised to 140°C (NCO / OH=0.98). The reaction was continued for another 30 minutes to obtain a urethane resin. Next, 750 parts of distilled water containing 8.9 parts of 28% aqueous ammonia was added while cooling to obtain an aqueous urethane resin (weight average molecular weight about 40,000).
[0292] <Ink density evaluation> The ink concentration of the print obtained as described above was measured using Spectroeye (product name, manufactured by Sakata Ink Engineering Co., Ltd.). The average value of seven measurements was taken as the ink concentration. The evaluation criteria for the observation results are shown below. In the following evaluation criteria, if the evaluation score is 3 or higher, the print can be used without any problems in practice. (Evaluation Criteria) 5: Ink density of solid areas is 1.9 to 2.0 4: Ink density of solid area is 1.8 or higher but lower than 1.9 3: Ink density of solid area is 1.6 or higher but lower than 1.8 2: Ink density of solid area is 1.4 or higher but lower than 1.6 1: Ink density of solid area is lower than 1.4
[0293] <Tone Jump> The halftone dot images of the printed matter obtained as described above were visually evaluated for the presence or absence of tone jumps. The evaluation criteria for the observation results are as follows: In the following evaluation criteria, if the evaluation score is 3 or higher, the material can be used without any problems in practice. (Evaluation Criteria) 4: The reproducibility of halftone dot images is visually smooth from shadow to highlight areas. 3: The boundary line between the gradation and non-image areas is somewhat thick, and the reproducibility of halftone dot images is somewhat inferior to 4. 2: There is some unevenness in density. 1: Density unevenness is clearly visible.
[0294] <Evaluation of ink adhesion> For the ink entrapment, printing was performed in the same manner as in the printing evaluation described above, except that the anilox pressure was increased by 0.02 mm from the appropriate value in order to supply an excess amount of ink to the photosensitive resin plate in order to accelerate the entrapment evaluation, and the printing pressure was also increased by 0.15 mm from the appropriate value in order to increase the deformation of the relief surface and accelerate the ink entrapment.
[0295] After printing 100m, the anilox was removed from the photopolymer plate. Then, 10m was printed without the photopolymer plate touching the anilox, and excess ink on the surface of the photopolymer plate was removed. After that, the printing machine was stopped, and the ink remaining on the halftone dots of the printing plate was evaluated. The halftone dots to be evaluated were 10 locations in total, with halftone dot areas of 3 and 30% on AM100, 133, 150, 175, and 200 lines arranged in the image. The spaces between the halftone dots (recesses) of the plate after printing were observed with a magnifying glass. The evaluation criteria for the observation results are shown below. If the evaluation criteria below are 3 or higher, it can be used without any problems in practical use. (Evaluation Criteria) 5: There are no tangles at all among the 10 halftone dots. 4: Of the 10 halftone dots, the number of halftone dots with ink entangled over 10% or more of the image area is 1 to 2 3: Of the 10 halftone dots, the number of halftone dots with ink entangled over 30% or more of the image area is 1 to 2 2: Of the 10 halftone dots, the number of halftone dots with ink entangled over 30% or more of the image area is between 3 and 5 1: Of the 10 halftone dots, there are 5 or more halftone dots with ink entangled over 30% or more of the image area.
[0296] The compositions of the ink-receiving layers used in the flexographic printing original plates and flexographic printing plates of Examples 1 to 19 and Comparative Examples 1 to 10, the film thicknesses of the ink-receiving layers, the aspects of the photosensitive resin compositions, and the above-mentioned evaluation results are shown in Tables 1 and 2 below.
[0297] [Table 1]
[0298] [Table 2]
[0299] (component) The components used in the table are as follows: <Polymer particles> SB Latex L7430: SB Latex, manufactured by Asahi Kasei Corporation SB Latex A2730: SB Latex, manufactured by Asahi Kasei Corporation SB Latex A7141: SB Latex, manufactured by Asahi Kasei Corporation SB Latex A6006: SB Latex, manufactured by Asahi Kasei Corporation SB Latex L5930: SB Latex, manufactured by Asahi Kasei Corporation Luckstar DN703: butadiene resin latex, manufactured by DIC Luckstar 1570B: butadiene resin latex, manufactured by DIC Luckstar 6541G: butadiene resin latex, manufactured by DIC ARUFON UC-3080: Acrylic polymer, manufactured by Toagosei Co., Ltd. ARUFON UC-3000: Acrylic polymer, manufactured by Toagosei Co., Ltd. Boncoat EC-905EF: Water-based acrylic resin, manufactured by DIC Tuftec H1051: Hydrogenated styrene-based thermoplastic elastomer, manufactured by Asahi Kasei Corporation Kraton D-KX405: Styrene butadiene block copolymer, manufactured by Kraton <Thickener> Alcox EP-10: Ethylene oxide-propylene oxide copolymer, Meisei Chemical Industry HPC: Hydroxypropyl cellulose (Tokyo Chemical Industry Co., Ltd.) Xanthan Gum (Tokyo Chemical Industry) E-60: Ethylene oxide homopolymer (Meisei Chemical Industry) CP-A2H: Random copolymer of allyl glycidyl ether containing side chain allyl groups, ethylene oxide, and propylene oxide (Meisei Chemical Industry Co., Ltd.) <Silicone compounds> KF-351A: Polyether modified silicone oil, Shin-Etsu Chemical
[0300] [Table 3]
[0301] [Table 4]
[0302] (component) As the components shown in the table, in addition to those shown in Table 1 above, the following were used. <Binder resin> JMR-8M: Polyvinyl alcohol, manufactured by Japan Vinyl Acetate & Poval Co., Ltd. CP-800: Acrylic water-based resin emulsion (styrene-methacrylic copolymer), manufactured by Harima Chemical Group Co., Ltd. Dickfine FZ-1000: Styrene acrylic resin emulsion Hydran CP-7050: Water-based urethane resin, manufactured by DIC AQ nylon T-70: Amine compound, alkylene oxide compound, caprolactam polymer, manufactured by Toray Industries, Inc. AQ Nylon A-90: Amine compound caprolactam polymer, manufactured by Toray Industries, Inc. <Additives> SU-268A: Blocked isocyanate, manufactured by Meisei Chemical Industry Co., Ltd. MEB-3: Swelling mica, Somasif MEB-3, manufactured by Katakura Coop Agri Co., Ltd. F-569: Fluorine-containing additive Megafac, manufactured by DIC Emulgen 350: Polyoxyethylene stearyl ether, manufactured by Kao Corporation <Photopolymerization initiator> Omnirad 2959: 2-Hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, from IGM Resins BV <Polymerizable compound> SR399: Dipentaerythritol pentaacrylate, manufactured by Arkema SR368: Tris(2-hydroxyethyl)isocyanurate triacrylate, manufactured by Arkema FOM-03006: Acrylamide group-containing water-soluble crosslinking agent, manufactured by Fujifilm Corporation CN981: Aliphatic urethane acrylate, manufactured by Arkema CN1963: Aliphatic urethane methacrylate acrylate ester, Arkema CN989: Aliphatic urethane acrylate tripropylene glycol diacrylate, Arkema Karenz MOI-DEM: Blocked isocyanate monomer, manufactured by Showa Denko [Industrial Applicability]
[0303] The present invention has industrial applicability as a flexographic printing plate precursor for obtaining a flexographic printing plate.
Claims
1. A flexographic printing original plate comprising at least a support, a photosensitive resin composition layer, an ink-receiving layer, and an infrared ablation layer laminated in this order, The thickness of the ink receiving layer is 5 μm or more and 50 μm or less, the ink receiving layer contains polymer particles, the polymer particles containing at least one of polybutadiene having a carboxyl group and / or a hydroxyl group, an acrylonitrile-butadiene copolymer having a carboxyl group and / or a hydroxyl group, a styrene-butadiene copolymer having a carboxyl group and / or a hydroxyl group, and a (meth)acrylate-butadiene copolymer having a carboxyl group and / or a hydroxyl group; the content of the polymer particles is 20% by mass or more and 95% by mass or less with respect to 100% by mass of the ink receiving layer, The photosensitive resin composition layer contains a photopolymerization initiator. Flexographic printing plate.
2. The ink receiving layer contains polymer particles having a butadiene skeleton and a carboxyl group and / or a hydroxyl group. The flexographic printing plate precursor according to claim 1.
3. The photosensitive resin composition layer contains a photopolymerizable monomer. The flexographic printing plate precursor according to claim 1.
4. The ink receiving layer further contains a binder resin having a basic group. The flexographic printing plate precursor according to claim 1.
5. The binder resin having a basic group contains a polyamide resin and / or a polyurethane resin. The flexographic printing plate precursor according to claim 4.
6. The ink receiving layer further contains a polyvinyl alcohol resin. The flexographic printing plate precursor according to any one of claims 1 to 5.
7. The ink receiving layer further comprises swellable mica. The flexographic printing plate precursor according to any one of claims 1 to 6.
8. The ink receiving layer further contains a water-soluble photopolymerization initiator and a water-soluble polymerizable compound. The flexographic printing plate precursor according to any one of claims 1 to 7.
9. The water-soluble polymerizable compound has an amide skeleton and / or a urethane skeleton. The flexographic printing plate precursor according to claim 8.
10. the ink receiving layer further contains a water-soluble resin having an alkylene oxide chain; The flexographic printing plate precursor according to any one of claims 1 to 9.
11. A flexographic printing plate comprising at least a support, a photocured photosensitive resin composition layer, and an ink-receiving layer laminated in this order, The thickness of the ink receiving layer is 5 μm or more and 50 μm or less, the ink receiving layer contains polymer particles, the polymer particles containing at least one of polybutadiene having a carboxyl group and / or a hydroxyl group, an acrylonitrile-butadiene copolymer having a carboxyl group and / or a hydroxyl group, a styrene-butadiene copolymer having a carboxyl group and / or a hydroxyl group, and a (meth)acrylate-butadiene copolymer having a carboxyl group and / or a hydroxyl group; At least a portion of the polymer particles are fused together, The photosensitive resin composition layer contains a photopolymerization initiator. Flexographic printing plate.
12. A flexographic printing plate comprising at least a support, a photocured photosensitive resin composition layer, and an ink-receiving layer laminated in that order, The thickness of the ink receiving layer is 5 μm or more and 50 μm or less, the ink receiving layer contains polymer particles, the polymer particles containing at least one of polybutadiene having a carboxyl group and / or a hydroxyl group, an acrylonitrile-butadiene copolymer having a carboxyl group and / or a hydroxyl group, a styrene-butadiene copolymer having a carboxyl group and / or a hydroxyl group, and a (meth)acrylate-butadiene copolymer having a carboxyl group and / or a hydroxyl group; the photosensitive resin composition layer contains a photopolymerization initiator, Manufactured through an infrared irradiation process from a flexographic printing plate having an infrared ablation layer. Flexographic printing plate.
13. The ink receiving layer contains polymer particles having a butadiene skeleton and having a carboxyl group and / or a hydroxyl group.
13. The flexographic printing plate according to claim 11 or 12.
14. The photosensitive resin composition layer contains a photopolymerizable monomer.
13. The flexographic printing plate according to claim 11 or 12.
15. a difference (Ei-Ep) between a surface free energy Ei of the ink receiving layer and a surface free energy Ep of the photocured photosensitive resin composition layer is greater than 0 mJ / m2 and less than or equal to 5 mJ / m2; 13. The flexographic printing plate according to claim 11 or 12.
16. a difference (Ei-Ep) between a surface free energy Ei of the ink receiving layer and a surface free energy Ep of the photocured photosensitive resin composition layer is greater than 0 mJ / m2 and less than or equal to 4 mJ / m2; 16. The flexographic printing plate of claim 15.
17. a difference (Ei-Ep) between a surface free energy Ei of the ink receiving layer and a surface free energy Ep of the photocured photosensitive resin composition layer is greater than 0.5 mJ / m2 and less than or equal to 3.5 mJ / m2; 16. The flexographic printing plate of claim 15.
18. The ink receiving layer further contains a water-soluble polymer having an alkylene oxide chain. The flexographic printing plate according to any one of claims 11 to 17.
19. The content of the polymer particles is 20% by mass or more and 95% by mass or less with respect to 100% by mass of the ink receiving layer. The flexographic printing plate according to any one of claims 11 to 18.
20. The film zeta potential of the ink receiving layer is positive. The flexographic printing plate according to any one of claims 11 to 19.
21. The ink receiving layer further contains a binder resin having a basic group. The flexographic printing plate according to any one of claims 11 to 20.
22. The binder resin having a basic group contains a polyamide resin and / or a polyurethane resin.
22. The flexographic printing plate of claim 21.
23. The ink receiving layer further contains a polyvinyl alcohol resin. The flexographic printing plate according to any one of claims 11 to 22.
24. The ink receiving layer further contains swellable mica. The flexographic printing plate according to any one of claims 11 to 23.
25. The ink receiving layer further contains a water-soluble photopolymerization initiator and a water-soluble polymerizable compound. The flexographic printing plate according to any one of claims 11 to 24.
26. The water-soluble polymerizable compound has an amide skeleton and / or a urethane skeleton.
26. The flexographic printing plate of claim 25.
27. 1. A method for producing a flexographic printing plate, comprising the steps of: A step of laser ablating the infrared ablation layer of the flexographic printing plate precursor according to any one of claims 1 to 10 to produce a negative pattern; an exposure step of exposing the photosensitive resin composition layer through the ink receiving layer; removing unexposed portions of the photosensitive resin composition layer and the ink-receiving layer; The method for producing a flexographic printing plate comprising the steps of:
Citation Information
Patent Citations
Preparation of phthalic anhydride
JP1980073675A
Manufacturing method of original plate for letterpress printing, manufacturing method of letterpress printing plate, and composition for forming ink-receiving layer
JP2008225446A
Method for improving printing performance in flexographic printing plates
JP2014507677A
A clear flexographic printing plate and its manufacturing method.
JP2015513700A
Photosensitive resin composition for flexographic printing
WO2007116941A1