CURABLE RESIN COMPOSITION, DRY FILM, CURED PRODUCT, AND PRINTED WIRING BOARD
A curable resin composition with surface-treated barium and silica, combined with rubber particles, addresses the challenge of achieving high resolution and crack resistance in solder resist layers by minimizing thermal stress and enhancing the composition's stability under severe conditions.
Patent Information
- Application Number
- JP2023173218
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-10-04
- Filing Date
- 2023-10-04
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-10-04
AI Technical Summary
Conventional curable resin compositions used in solder resist layers of printed wiring boards face challenges in achieving both high resolution and crack resistance, particularly under severe thermal stress conditions, due to the addition of inorganic fillers like silica which inhibit light transmission and cause undercutting during development.
A curable resin composition is formulated with surface-treated barium compounds and silica, along with rubber particles, maintaining a specific mass ratio of 1:1 to 1:4, to enhance both resolution and crack resistance, utilizing the low coefficient of thermal expansion and stress-alleviating properties of these components.
The composition achieves improved resolution and crack resistance under harsher thermal conditions, such as those encountered in thermal shock tests, by minimizing dimensional changes and stress through the balanced use of surface-treated barium and silica, along with rubber particles.
Smart Images

Figure 0007595725000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable resin composition, particularly to a curable resin composition suitable for forming a solder resist layer. The present invention further relates to a dry film having a resin layer made of the curable resin composition, a cured product of the curable resin composition or the resin layer of the dry film, and a printed wiring board having the cured product. [Background technology]
[0002] In recent years, with the miniaturization and high performance of electronic devices, there is an increasing need for finer patterns on printed wiring boards, smaller mounting areas, and higher density component mounting. Therefore, a curable resin composition for forming a solder resist on a printed wiring board is required to have high resolution. On the other hand, since high heat is applied at various stages in the manufacture and use of a printed wiring board, the solder resist on the printed wiring board is also required to have resistance to thermal stress.
[0003] Conventionally, in order to improve resistance to such thermal stress, attempts have been made to control the coefficient of linear thermal expansion (CTE) of a curable resin composition by adding a highly heat-resistant resin or inorganic material to the curable resin composition. In particular, silica is generally added to a curable resin composition not only to lower the CTE of the curable resin composition, but also from the viewpoint of physical properties such as crack resistance, cost, and ease of handling.
[0004] However, when an inorganic filler with low light transmittance such as silica, particularly spherical silica, is added to a curable resin composition, the silica inhibits light transmission and reduces the curability of the curable resin composition deep in the coating film when the coating film of the curable resin composition is cured by light irradiation to form an opening pattern. As a result, a phenomenon occurs in which the bottom of the opening pattern of the solder resist is excessively dissolved during development (so-called undercut), which causes a problem of reduced resolution such as poor formation of a fine line pattern.
[0005] In order to improve the resolution when silica is added to a curable resin composition, a method of adding barium sulfate in addition to silica is known. For example, Patent Document 1 discloses that a solder resist formed from a curable resin composition containing spherical silica and barium sulfate in a volume ratio of 1:(0.5-5) exhibits excellent resistance to a temperature cycling test (TCT).
[0006] Incidentally, in recent years, FC-BGA (Flip Chip-Ball Grid Array) substrates are increasingly used in semiconductor packages from the viewpoint of high speed and multi-function. Furthermore, in semiconductor packages, finer patterns and larger chips are required from the viewpoint of high speed and multi-function. On the other hand, as the chip area increases, the amount of heat generated during operation increases, so that semiconductor packages are required to be more reliable against severe temperature changes than ever before. Therefore, higher reliability is also required for solder resists used in manufacturing FC-BGA substrates. Conventionally, TCT has been used to evaluate the reliability of solder resists, but in recent years, solder resists have become highly reliable, and it is difficult to determine the difference using TCT, making it difficult to evaluate the reliability of solder resists. Therefore, in order to evaluate the reliability of solder resists for FC-BGA substrates, thermal shock tests (TST), which have more severe conditions, are generally performed instead of the conventional TCT. TCT is a thermal cycle test performed in an air bath, whereas TST is a thermal cycle test performed in a liquid bath. Because liquid has a higher thermal conductivity than gas, the board is exposed to more rapid temperature changes in TST than in TCT, and as a result, cracks are more likely to occur in the solder resist formed on the board in TST than in TCT. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2019-178305 A Summary of the Invention [Problem to be solved by the invention]
[0008] Under these circumstances, a technical problem exists to provide a curable resin composition capable of forming a cured product having both good resolution and good crack resistance under conditions more severe than those of conventional TCT.
[0009] Therefore, an object of the present invention is to provide a curable resin composition capable of forming a cured product having both good resolution and good crack resistance under conditions more severe than those of conventional TCTs, a dry film having a resin layer made of the curable resin composition, a cured product of the curable resin composition or the resin layer of the dry film, and a printed wiring board including the cured product. [Means for solving the problem]
[0010] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by further blending (D) rubber particles in a curable resin composition containing (A) a curable resin, (B) a surface-treated barium compound, and (C) a surface-treated silica, adjusting the total content of (B) the surface-treated barium compound and (C) the surface-treated silica to 20-80 mass% based on the solid content relative to the total mass of the solid content of the curable resin composition, and adjusting the mass ratio of (B) the surface-treated barium compound and (C) the surface-treated silica to 1:1-1:4 based on the solid content. The present invention is based on such findings. That is, the gist of the present invention is as follows.
[0011] [1] (A) a curable resin; (B) a surface-treated barium compound; (C) surface-treated silica; (D) Rubber particles and A curable resin composition comprising: the total content of the (B) surface-treated barium compound and the (C) surface-treated silica is 20 to 80 mass% on a solid content basis with respect to the total mass of the solid content of the curable resin composition; A curable resin composition, characterized in that a mass ratio of the (B) surface-treated barium compound to the (C) surface-treated silica is 1:1 to 1:4 based on solid contents. [2] The curable resin composition according to [1], wherein the (A) curable resin comprises (A-1) a photocurable resin. [3] The curable resin composition according to [1] or [2], wherein the (A) curable resin contains (A-2) a thermosetting resin. [4] The curable resin composition according to any one of [1] to [3], wherein the (D) rubber particles include core-shell rubber particles. [5] The curable resin composition according to any one of [1] to [4], further comprising (E) a photopolymerization initiator. [6] A dry film comprising a first film and a resin layer formed on at least one surface of the first film, the resin layer being made of the curable resin composition according to any one of [1] to [5]. [7] A cured product obtained by curing the curable resin composition according to any one of [1] to [5] or the resin layer of the dry film according to [6]. [8] A printed wiring board comprising the cured product according to [7]. Effect of the Invention
[0012] According to the present invention, there are provided a curable resin composition capable of forming a cured product having both good resolution and good crack resistance under conditions harsher than conventional TCT, a dry film having a resin layer made of the curable resin composition, a cured product of the curable resin composition or the resin layer of the dry film, and a printed wiring board having the cured product. In particular, according to the present invention, in the cured product of the curable resin composition, it is possible to achieve both good resolution and good crack resistance under TST, which is harsher than TCT. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Sclerotic resin composition] The curable resin composition of the present invention comprises, as essential components, (A) a curable resin, (B) a surface-treated barium compound, (C) surface-treated silica, and (D) rubber particles, and is characterized in that the total content of the (B) surface-treated barium compound and the (C) surface-treated silica is adjusted to 20 to 80 mass% on a solid content basis relative to the total mass of the solid contents of the curable resin composition, and the mass ratio of the (B) surface-treated barium compound to the (C) surface-treated silica on a solid content basis (mass of the surface-treated barium compound:mass of the surface-treated silica) is adjusted to 1:1 to 1:4. The curable resin composition of the present invention can form a cured product that has both good resolution and good crack resistance in TST, which is harsher than TCT, by particularly containing (D) rubber particles, adjusting the total content of (B) surface-treated barium compound and (C) surface-treated silica to 20-80 mass% based on solid content based on the total mass of the solid content of the curable resin composition, and adjusting the mass ratio of (B) surface-treated barium compound and (C) surface-treated silica based on solid content to 1:1-1:4. In this way, when rubber particles are blended in the curable resin composition, the total content of the surface-treated barium compound and surface-treated silica is adjusted to 20-80 mass% based on solid content based on the total mass of the solid content of the curable resin composition, and the mass ratio of the surface-treated barium compound and surface-treated silica based on solid content is adjusted to 1:1-1:4, the reason why good resolution and good crack resistance under conditions harsher than conventional TCT can be achieved at the same time is not clear, but it is inferred as follows. Fillers such as silica and barium have a low coefficient of linear thermal expansion (CTE), and therefore, by incorporating surface-treated silica or barium into a curable resin composition, the dimensional change of the curable resin composition during thermal cycles is reduced, suppressing the generation of stress, and as a result, it is believed that the crack resistance of the curable resin composition can be improved.In particular, silica has a low CTE, so it is effective in improving crack resistance by blending it into a curable resin composition. On the other hand, the crack resistance of the curable resin composition can be improved by increasing the blending amount of surface-treated silica, but if the blending amount is too large, the resolution may decrease. On the other hand, if a part of the surface-treated silica is blended in place of a surface-treated barium compound, the resolution in forming a small diameter pattern can be improved. This is because the difference in refractive index between barium sulfate and the resin component is small, so that light tends to go straight through the curable resin composition in the exposure process, and as a result, it is thought that the resolution can be improved. However, since silica has a lower CTE than barium sulfate, it is thought that it is preferable to blend a large amount of silica in order to improve crack resistance. On the other hand, if rubber particles are blended into the curable resin composition, the stress generated in the thermal cycle is alleviated, and the blending amount of surface-treated silica can be reduced while maintaining good crack resistance, and high resolution can be obtained. That is, by blending rubber particles to relieve the stress generated in the thermal cycle, the blending amount of surface-treated silica required for improving crack resistance can be reduced, and further, by making the total content of the surface-treated barium compound and the surface-treated silica, and the mass ratio based on the solid content thereof, within the above-mentioned specific range, it is considered that the effect of improving crack resistance by the surface-treated silica and the effect of improving resolution by the surface-treated barium can be obtained at the same time. Hereinafter, each component of the curable resin composition of the present invention will be described in detail. Note that each component may be a commercially available product or may be appropriately synthesized.
[0014] (curable resin) The curable resin composition of the present invention contains (A) a curable resin. The curable resin can be used without any particular limitation as long as it is a resin that is cured by the action of heat, light, or the like. Specifically, the curable resin can be a photocurable resin, a thermosetting resin, or the like. The curable resin may be used alone or in combination of two or more kinds. For example, a thermosetting resin or a photocurable resin may be used alone or in combination. The curable resin composition preferably contains a photocurable resin and a thermosetting resin.
[0015] The curable resin composition may contain a photocurable resin (A-1) as a curable resin. As the photocurable resin, a known and commonly used photocurable resin may be used. Among them, from the viewpoint of photocurability and development resistance, a photocurable resin that can be cured by a radical addition polymerization reaction with active energy rays is preferably used, and a photocurable resin having an ethylenically unsaturated group in the molecule is more preferably used. The ethylenically unsaturated group is preferably derived from acrylic acid or methacrylic acid or a derivative thereof. The photocurable resin may be used alone or in combination of two or more kinds. As the photocurable resin, a carboxyl group-containing photosensitive resin described later is preferably used.
[0016] As the photocurable resin having an ethylenically unsaturated group in the molecule, a known and commonly used photopolymerizable oligomer and a photopolymerizable monomer are used. Among them, the photopolymerizable oligomer includes an unsaturated polyester oligomer and a (meth)acrylate oligomer. As the (meth)acrylate oligomer, an epoxy (meth)acrylate such as phenol novolac epoxy (meth)acrylate, cresol novolac epoxy (meth)acrylate, and bisphenol type epoxy (meth)acrylate, an urethane (meth)acrylate, an epoxy urethane (meth)acrylate, a polyester (meth)acrylate, a polyether (meth)acrylate, and a polybutadiene-modified (meth)acrylate are listed.
[0017] On the other hand, as the photopolymerizable monomer, a monomer having an ethylenically unsaturated group is preferably used. Examples of such photopolymerizable monomers include commonly known polyester (meth)acrylates, polyether (meth)acrylates, urethane (meth)acrylates, carbonate (meth)acrylates, and epoxy (meth)acrylates. Specifically, alkyl acrylates such as 2-ethylhexyl acrylate and cyclohexyl acrylate; hydroxyalkyl acrylates such as 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; mono- or diacrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; acrylamides such as N,N-dimethylacrylamide, N-methylolacrylamide, and N,N-dimethylaminopropylacrylamide; aminoalkyl acrylates such as N,N-dimethylaminoethyl acrylate and N,N-dimethylaminopropyl acrylate; hexanediol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, dipentaerythritol, and trishydroxyethyl isocyanurate. Polyhydric acrylates such as polyhydric alcohols or their alkylene oxide adducts or ε-caprolactone adducts; phenols such as phenoxy acrylate and bisphenol A diacrylate or their alkylene oxide adducts; glycidyl ether acrylates such as glycerin diglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; and acrylates obtained by directly acrylate polyols such as polyether polyols, polycarbonate diols, hydroxyl group-terminated polybutadienes, and polyester polyols or by urethane acrylate via diisocyanates, melamine acrylates, and at least one of the methacrylates corresponding to the acrylates can be appropriately selected and used. The photopolymerizable monomer may be used alone or in combination of two or more. The photopolymerizable monomer can also be used as a reactive diluent.The term "photopolymerizable monomer" refers to a compound that is a monomer, particularly among photocurable resins. As the photopolymerizable monomer, a bifunctional to hexafunctional photopolymerizable monomer is preferably used. Examples of the bifunctional to hexafunctional photopolymerizable monomer include dipentaerythritol hexaacrylate (DPHA), pentaerythritol pentaacrylate, tricyclodecane dimethanol diacrylate, tricyclodecane dimethanol dimethacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, and trimethylol tripropane triacrylate.
[0018] The content of the photocurable resin in the curable resin composition is not particularly limited as long as the effects of the present invention are achieved, and can be, for example, 10 to 50 mass% on a solid content basis with respect to the total mass of the solid contents of the curable resin composition.
[0019] The curable resin may preferably contain a carboxyl group-containing resin in order to impart alkaline developability to the curable resin composition. As the carboxyl group-containing resin, various conventionally known resins having a carboxyl group in the molecule may be used. Specific examples of the carboxyl group-containing resin include the following compounds (which may be either oligomers or polymers):
[0020] (1) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, isobutylene, etc.
[0021] (2) Carboxylic acid-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0022] (3) Carboxylic acid-containing photosensitive urethane resins obtained by polyaddition reaction of diisocyanates with partially acid anhydride-modified products of reaction products of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins and biphenol type epoxy resins with monocarboxylic acid compounds having ethylenically unsaturated groups such as (meth)acrylic acid, carboxyl group-containing dialcohol compounds and diol compounds.
[0023] (4) A photosensitive urethane resin containing a carboxyl group, which is terminated with (meth)acrylation by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (3).
[0024] (5) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acryloyl group obtained by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (3) described above.
[0025] (6) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride to the hydroxyl groups present in the side chains.
[0026] (7) A carboxyl group-containing photosensitive resin obtained by reacting a multifunctional epoxy resin with the hydroxyl groups of a bifunctional (solid) epoxy resin further epoxidized with epichlorohydrin, with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.
[0027] (8) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.
[0028] (9) A carboxyl group-containing photosensitive resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl group of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, or the like.
[0029] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0030] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0031] (12) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to any one of the resins (1) to (11). In this specification, (meth)acrylate is a term that collectively refers to acrylate, methacrylate, and mixtures thereof, and the same applies to other similar expressions.
[0032] The acid value of the carboxyl group-containing resin is preferably in the range of 30 to 150 mgKOH / g, more preferably 50 to 120 mgKOH / g. If the acid value of the carboxyl group-containing resin is 30 mgKOH / g or more, alkaline development can be performed appropriately, while if it is 150 mgKOH / g or less, dissolution of the exposed area by the developer does not proceed, so that the exposed area and the unexposed area can be dissolved and peeled off in a distinguishing manner by the developer, which is preferable since it is easy to draw a normal resist pattern.
[0033] The weight-average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, but is generally in the range of 2,000 to 150,000, and more preferably 5,000 to 100,000. If the weight-average molecular weight is 2,000 or more, the moisture resistance of the coating film after exposure is good, there is no film loss during development, and excellent resolution is easily obtained. On the other hand, if the weight-average molecular weight is 150,000 or less, good developability and good storage stability are easily obtained. The weight-average molecular weight can be measured by gel permeation chromatography (GPC).
[0034] The carboxyl group-containing resins are not limited to those listed above, and may be used alone or in combination of two or more. Among them, carboxyl group-containing resins synthesized using a compound having a phenolic hydroxyl group as a starting material, such as the above-mentioned carboxyl group-containing resins (10) and (11), are preferably used because of their excellent HAST resistance and PCT resistance.
[0035] The curable resin composition may contain a thermosetting resin (A-2) as a curable resin. By adding a thermosetting resin to the curable resin composition, it is expected that the heat resistance, chemical resistance, and adhesion of the curable resin composition are improved. The thermosetting resin may be used alone or in combination of two or more. Any known thermosetting resin may be used as the thermosetting resin. For example, known thermosetting resins such as amino resins such as melamine resins, benzoguanamine resins, melamine derivatives, and benzoguanamine derivatives, isocyanate compounds, blocked isocyanate compounds, cyclocarbonate compounds, epoxy compounds, oxetane compounds, oxazoline compounds, episulfide resins, bismaleimides, and carbodiimide resins may be used. Each of these thermosetting resins may be monofunctional or polyfunctional.
[0036] Epoxy compounds include epoxidized vegetable oils, bisphenol A type epoxy resins, hydroquinone type epoxy resins, bisphenol type epoxy resins, thioether type epoxy resins, brominated epoxy resins, novolac type epoxy resins, phenol novolac type epoxy resins, biphenol novolac type epoxy resins, bisphenol F type epoxy resins, hydrogenated bisphenol A type epoxy resins, glycidylamine type epoxy resins, hydantoin type epoxy resins, alicyclic epoxy resins, trihydroxyphenylmethane type epoxy resins, bixylenol type or biphenol type epoxy resins, or or mixtures thereof; bisphenol S type epoxy resin; bisphenol A novolac type epoxy resin; tetraphenylolethane type epoxy resin; heterocyclic epoxy resin; diglycidyl phthalate resin; tetraglycidyl xylenoylethane resin; naphthalene group-containing epoxy resin; epoxy resin having a dicyclopentadiene skeleton; glycidyl methacrylate copolymer epoxy resin; cyclohexylmaleimide and glycidyl methacrylate copolymer epoxy resin; epoxy-modified polybutadiene rubber derivative; CTBN-modified epoxy resin, etc., but are not limited thereto. These epoxy resins may be used alone or in combination of two or more.
[0037] As the oxetane compound, a polyfunctional oxetane compound having two or more oxetanyl groups in one molecule is preferably used. Examples of the polyfunctional oxetane compound include bis[(3-methyl-3-oxetanyl methoxy) methyl] ether, bis[(3-ethyl-3-oxetanyl methoxy) methyl] ether, 1,4-bis[(3-methyl-3-oxetanyl methoxy) methyl] benzene, 1,4-bis[(3-ethyl-3-oxetanyl methoxy) methyl] benzene, (3-methyl-3-oxetanyl) methyl acrylate, (3-ethyl-3-oxetanyl) methyl acrylate, and the like. Examples of the oxetanes include polyfunctional oxetanes such as acrylate, (3-methyl-3-oxetanyl)methyl methacrylate, (3-ethyl-3-oxetanyl)methyl methacrylate, and their oligomers or copolymers, as well as ethers of oxetane alcohols and novolac resins, poly(p-hydroxystyrene), cardo-type bisphenols, calixarenes, calixresorcinarenes, or resins having hydroxyl groups such as silsesquioxane. Other examples include copolymers of unsaturated monomers having an oxetane ring and alkyl (meth)acrylates.
[0038] Examples of oxazoline compounds include possible compounds having two or more oxazoline groups in one molecule. Examples of such oxazoline compounds include oxazoline group-containing polymers such as polymers of oxazoline group-containing monomers and copolymers of oxazoline group-containing monomers and other monomers. Examples of oxazoline group-containing monomers include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, 2-isopropenyl-5-ethyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4,4-dimethyl-2-oxazoline, etc.
[0039] The episulfide resin may be, for example, a compound in which the oxygen atom constituting the epoxy group in any epoxy compound is replaced with a sulfur atom. The epoxy compound may be the same as those mentioned above. In addition, the method of replacing the oxygen atom constituting the epoxy group in the epoxy compound with a sulfur atom may be a conventionally known method.
[0040] Examples of amino resins such as melamine derivatives and benzoguanamine derivatives include methylolmelamine compounds, methylolbenzoguanamine compounds, methylolglycoluril compounds, and methylolurea compounds.
[0041] The isocyanate compound may be a polyisocyanate compound. Examples of the polyisocyanate compound include aromatic polyisocyanates such as 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, naphthalene-1,5-diisocyanate, o-xylylene diisocyanate, m-xylylene diisocyanate and 2,4-tolylene dimer; aliphatic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, 4,4-methylenebis(cyclohexyl isocyanate) and isophorone diisocyanate; alicyclic polyisocyanates such as bicycloheptane triisocyanate; and adducts, biuret and isocyanurates of the above-mentioned isocyanate compounds.
[0042] The blocked isocyanate compound may be an addition reaction product of an isocyanate compound and an isocyanate blocking agent. Examples of isocyanate compounds that can react with an isocyanate blocking agent include the polyisocyanate compounds described above. Examples of isocyanate blocking agents include phenol-based blocking agents, lactam-based blocking agents, active methylene-based blocking agents, alcohol-based blocking agents, oxime-based blocking agents, mercaptan-based blocking agents, acid amide-based blocking agents, imide-based blocking agents, amine-based blocking agents, imidazole-based blocking agents, and imine-based blocking agents.
[0043] The content of the thermosetting resin in the curable resin composition is not particularly limited as long as the effects of the present invention are achieved, and can be, for example, 3 to 50 mass% on a solid content basis with respect to the total mass of the solid contents of the curable resin composition.
[0044] (Filler) The curable resin composition of the present invention contains (B) a surface-treated barium compound and (C) a surface-treated silica as a filler. The total content of the surface-treated barium compound and the surface-treated silica in the curable resin composition is 20 to 80 mass% based on the solid content, preferably 20 to 50 mass%, more preferably 30 to 40 mass%, based on the total mass of the solid content of the curable resin composition. In addition, the mass ratio of the surface-treated barium compound and the surface-treated silica based on the solid content in the curable resin composition is 1:1 to 1:4, preferably 1:1 to 1:3, more preferably 1:1.5 to 1:2. By setting the total content of the surface-treated barium compound and the surface-treated silica and the mass ratio based on the solid content in such a range, it is possible to achieve both good resolution and crack resistance.
[0045] Regarding the surface-treated barium compound, the barium compound is a concept that includes barium alone and various compounds containing barium. That is, the surface-treated barium compound includes a compound that is surface-treated with barium alone and a compound that is surface-treated with a compound containing barium. The surface-treated barium compound may be used alone or in combination of two or more.
[0046] The barium-containing compound is not particularly limited as long as it is a compound that can be used as a filler, and examples thereof include barium sulfate, barium titanate, barium oxide, barium hydroxide, etc. As the barium-containing compound, barium sulfate is preferably used. As commercially available barium sulfate products, for example, B-30, B-33, etc. manufactured by Sakai Chemical Industry Co., Ltd. can be mentioned.
[0047] The surface treatment of the barium compound is not particularly limited as long as it is a treatment that imparts a reactive functional group to the surface of the barium compound, and a conventionally known surface treatment of fillers can be performed. Examples of the reactive functional group imparted to the surface of the barium compound include a methacryl group, a carboxyl group, a hydroxyl group, a sulfonic acid group, an amino group, an epoxy group, a vinyl group, a mercapto group, and an acid anhydride. The surface-treated barium compound may have one type of reactive functional group, or may have two or more types of reactive functional groups. In addition, when two or more types of surface-treated barium compounds are used, they may have the same reactive functional group or different reactive functional groups. As the surface-treated barium compound, a barium compound having a methacryl group on its surface is preferably used.
[0048] A method for obtaining a surface-treated barium compound, that is, a method for providing a reactive functional group to the surface of a barium compound, can be a conventional method. For example, a method of bonding various coupling agents having a reactive functional group (for example, a silane compound (a so-called silane-based coupling agent)) with a barium compound (bonding a barium compound with a reactive functional group via a coupling agent) can be mentioned. In this specification, the "bond" between a coupling agent and a barium compound includes not only a bond that involves a chemical reaction between the coupling agent and the barium compound (chemical adsorption), but also a bond that does not involve such a chemical reaction (physical adsorption).
[0049] Examples of the coupling agent include silane-based, aluminate-based, titanate-based, and zircoaluminate-based agents. Of these, silane-based coupling agents are preferably used. Examples of the silane-based coupling agent include vinyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminomethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-anilinopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane. The coupling agent may be used alone or in combination of two or more.
[0050] When the surface-treated barium compound is obtained by a method of bonding a coupling agent having a reactive functional group with a barium compound, a conventionally known method can be used as the method. Specifically, a method of dispersing a powdered barium compound in a solution in which a coupling agent having a reactive functional group is dissolved in a solvent (removing the solvent as necessary) and contacting the two, a method of directly adding a powdered barium compound to a coupling agent having a reactive functional group, mixing, and contacting the two, etc. may be mentioned. In addition, if necessary, a step of heating after contacting the coupling agent having a reactive functional group with the powdered barium compound may be included. The amount of the coupling agent having a reactive functional group to be contacted with the powdered barium compound (treatment amount of the coupling agent) can be appropriately set depending on the method of bonding the coupling agent having a reactive functional group with the barium compound, the type of reactive functional group, the type of coupling agent, etc.
[0051] The particle size of the surface-treated barium compound is not particularly limited and can be set appropriately, but the average particle size is preferably 0.1 to 1 μm, more preferably 0.1 to 0.5 μm. By setting the average particle size of the surface-treated barium compound in such a range, good resolution can be obtained. In this specification, the average particle size of the filler is the average particle size before being mixed into the curable resin composition, and is the value of D50 measured by a laser diffraction method. As a measuring device for the average particle size (D50) by the laser diffraction method, Microtrac MT3300EXII manufactured by Microtrac Bell Co., Ltd. is used.
[0052] The content of the surface-treated barium compound in the curable resin composition is not particularly limited as long as it satisfies the total content of the above-mentioned surface-treated barium compound and surface-treated silica based on solid content and the range of the mass ratio based on solid content thereof, for example, it is 7 to 28 mass% based on solid content based on the total mass of the solid content of the curable resin composition.Note that, when two or more surface-treated barium compounds are used in combination, the content of the above-mentioned surface-treated barium compound refers to the total content of all surface-treated barium compounds.
[0053] As the silica constituting the surface-treated silica, any of silicas such as amorphous silica, non-crystalline silica, crystalline silica, fused silica, and spherical silica can be used. Silica may be used alone or in combination of two or more. As the silica, spherical silica is preferably used. Examples of commercially available spherical silica include SO-C2 and SO-E2 manufactured by Admatechs Co., Ltd., and SFP-20M manufactured by Denka Co., Ltd.
[0054] The type and method of the surface treatment of the silica are not particularly limited, and may be the same as the surface treatment of the barium compound described above, for example.
[0055] The particle size of the surface-treated silica is not particularly limited and can be appropriately set, but can be, for example, an average particle size of 0.01 to 1 μm, etc. By setting the average particle size of the surface-treated silica in this range, good resolution can be obtained.
[0056] The content of surface-treated silica in the curable resin composition is not particularly limited as long as it satisfies the above-mentioned total content of surface-treated barium compound and surface-treated silica based on solid content and the range of mass ratio based on solid content thereof, for example, it is 13-52 mass% based on solid content based on the total mass of the solid content of the curable resin composition.Note that, when two or more kinds of surface-treated silica are used in combination, the content of the above-mentioned surface-treated silica refers to the total content of all surface-treated silica.
[0057] The curable resin composition may further contain other fillers in addition to the above-mentioned surface-treated barium compound and surface-treated silica.The other fillers can be known inorganic or organic fillers, such as hydrotalcite, talc, and metal oxides such as titanium oxide for obtaining white appearance and flame retardancy, and metal hydroxides such as aluminum hydroxide.
[0058] (rubber particles) The curable resin composition of the present invention contains (D) rubber particles. The material constituting the rubber particles is not particularly limited as long as it is a material having excellent flexibility, and examples thereof include various elastomers such as butadiene-based elastomers, silicone-based elastomers, styrene-based elastomers, acrylic-based elastomers, polyolefin-based elastomers, and silicone / acrylic composite elastomers. As the material constituting the rubber particles, butadiene-based elastomers are preferably used. The rubber particles may be used alone or in combination of two or more kinds.
[0059] The rubber particles preferably have a core-shell structure, more preferably a core-shell structure having a core layer made of a material with excellent flexibility and a shell layer made of a material with excellent affinity for other components (core-shell rubber particles). When the rubber particles have a core-shell structure, the core layer contributes to impact resistance, and the shell layer contributes to dispersibility in the curable resin composition, and as a result, a high stress relaxation effect of the curable resin composition can be obtained.
[0060] The material constituting the core layer is not particularly limited as long as it has excellent flexibility, and examples thereof include the various elastomers mentioned above.
[0061] The material constituting the shell layer is a material having excellent affinity for other components, and can be appropriately set in relation to the components other than the rubber particles blended in the curable resin composition. For example, when the curable resin composition contains an epoxy resin, the shell layer is composed of a material having excellent affinity for the epoxy resin, such as an acrylic resin or an epoxy resin.
[0062] The rubber particles may have a curable reactive group on the surface thereof that undergoes a curing reaction with the curable resin. The curable reactive group may be a photocurable reactive group or a thermosetting reactive group. The rubber particles may have one type of curable reactive group alone, or may have two or more types of curable reactive groups in combination.
[0063] Examples of the photocurable reactive group include a vinyl group, a styryl group, a methacryl group, and an acrylic group.
[0064] Examples of the thermosetting reactive group include a hydroxyl group, a carboxyl group, an isocyanate group, an imino group, an epoxy group, an oxetanyl group, a mercapto group, a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an ethoxyethyl group, and an oxazoline group.
[0065] The method for introducing a curable reactive group to the surface of the rubber particle is not particularly limited, and a known and commonly used method can be used. For example, when forming a shell layer around a core layer, a material having a curable reactive group different from the functional group for polymerization reaction with the core layer can be introduced into the core layer by polymerization as a material for constituting the shell layer.
[0066] The particle size of the rubber particles is not particularly limited and can be appropriately set, and can be, for example, 0.001 to 0.5 μm as the average particle size. By setting the average particle size of the rubber particles in this range, good resolution can be obtained. In this specification, the average particle size of the rubber particles is the average particle size before being mixed into the curable resin composition, and is the value of D50 measured by a laser diffraction method. As a measuring device for the average particle size (D50) by the laser diffraction method, a laser diffraction / scattering type particle size distribution measuring device Microtrack MT3300 manufactured by Microtrack Bell Co., Ltd. is used.
[0067] The content of the rubber particles in the curable resin composition is not particularly limited and can be appropriately set, for example, 0.3 to 5 mass% based on the solid content with respect to the total mass of the solid content of the curable resin composition. By setting the content of the rubber particles in this range, good crack resistance can be obtained.
[0068] (Photopolymerization initiator) When the curable resin composition of the present invention contains a photocurable resin, the curable resin composition preferably further contains (E) a photopolymerization initiator. Any known photopolymerization initiator can be used. The photopolymerization initiator may be used alone or in combination of two or more.
[0069] Specific examples of the photopolymerization initiator include bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, and bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentane. Bisacylphosphine oxides such as 2,6-dimethoxybenzoyldiphenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, and bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphinic acid methyl ester, 2-methylbenzoyldiphenylphosphine oxide, pivaloyl monoacylphosphine oxides such as phenylphosphinic acid isopropyl ester and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; ethyl phenyl(2,4,6-trimethylbenzoyl)phosphinate, 1-hydroxy-cyclohexyl phenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, benzoin n-butyl ether, and other benzoins; benzoin alkyl ethers; benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bisdiethylaminobenzophenone, and other benzophenones;Acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl)-1-[4-(4-morpholinyl)phenyl] -1-butanone, N,N-dimethylaminoacetophenone and other acetophenones; thioxanthones such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone; anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-a Anthraquinones such as mil anthraquinone and 2-amino anthraquinone; ketals such as acetophenone dimethyl ketal and benzil dimethyl ketal; benzoic acid esters such as ethyl 4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and p-dimethylbenzoic acid ethyl ester; 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3 -yl]-, 1-(O-acetyloxime) and other oxime esters; bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium and other titanocenes; 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholinophenyl)-butan-1-one and other alkylphenones;Examples of the disulfide include phenyl disulfide 2-nitrofluorene, butyroin, anisoin ethyl ether, azobisisobutyronitrile, and tetramethylthiuram disulfide. Examples of commercially available photopolymerization initiators include Omnirad TPO H (2,4,6-trimethylbenzoyldiphenylphosphine oxide), IRGACURE OXE02 (ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyloxime)), Omnirad 369E (2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone), Omnirad 907 (2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one), and Omnirad 819 (bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide), all manufactured by IGM Resins BV;
[0070] A photoinitiator assistant or a sensitizer may be used in combination with the above-mentioned photopolymerization initiator. Examples of the photoinitiator assistant or the sensitizer include benzoin compounds, anthraquinone compounds, thioxanthone compounds, ketal compounds, benzophenone compounds, tertiary amine compounds, and xanthone compounds. In particular, it is preferable to use thioxanthone compounds such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2-isopropylthioxanthone, and 4-isopropylthioxanthone. By including a thioxanthone compound, it is possible to improve the deep curing property. Although these compounds may be used as photopolymerization initiators, it is preferable to use them in combination with a photopolymerization initiator. In addition, the photoinitiator assistant or the sensitizer may be used alone or in combination of two or more.
[0071] In addition, since these photopolymerization initiators, photoinitiator assistants, and sensitizers absorb specific wavelengths, in some cases the sensitivity is reduced and they may function as ultraviolet absorbers. However, they are not used only for the purpose of improving the sensitivity of the curable resin composition. If necessary, they can absorb light of a specific wavelength to increase the photoreactivity of the surface, change the line shape and opening of the resist to a vertical, tapered, or reverse tapered shape, and improve the accuracy of the line width and opening diameter.
[0072] (Thermosetting catalyst) When the curable resin composition of the present invention contains a thermosetting resin, the curable resin composition preferably further contains a thermosetting catalyst. Examples of the thermosetting catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole, and 2-phenyl-4,5-dihydroxymethylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. In addition, examples of commercially available products include 2MZ-A, 2MZ-OK, 2PHZ, 2PHZ-PW, 2P4BHZ, and 2P4MHZ (all trade names of imidazole-based compounds) manufactured by Shikoku Chemical Industry Co., Ltd., and U-CAT 3513N (a trade name of a dimethylamine-based compound), DBU, DBN, and U-CAT SA 102 (all bicyclic amidine compounds and their salts) manufactured by San-Apro Co., Ltd. In particular, the present invention is not limited to these, and any material that promotes the reaction of at least one of an epoxy resin or oxetane compound with a carboxyl group and at least one of an epoxy group and an oxetanyl group with a carboxyl group may be used alone or in combination of two or more types. Also usable are S-triazine derivatives such as guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine·isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-S-triazine·isocyanuric acid adduct, and it is preferable to use these compounds that also function as adhesion-imparting agents in combination with a heat curing catalyst. The heat curing catalyst may be used alone or in combination of two or more.As the thermosetting catalyst, preferably melamine or dicyandiamide (DICY) is used, and more preferably, melamine and dicyandiamide are used in combination.
[0073] (Organic solvent) An organic solvent may be blended into the curable resin composition of the present invention for the purpose of adjusting the viscosity during preparation thereof or when applying it to a substrate or film. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha. Conventionally known organic solvents can be used. The organic solvent may be used alone or in combination of two or more kinds.
[0074] The amount of the organic solvent in the curable resin composition is not particularly limited, and can be appropriately changed depending on the components constituting the curable resin composition and their amounts.
[0075] In the present invention, the organic solvent can be evaporated and dried using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, or the like (a method in which hot air in a dryer equipped with a heat source of an air heating type using steam is brought into countercurrent contact with the substrate, or a method in which hot air is blown onto the substrate from a nozzle).
[0076] (Other added ingredients) The curable resin composition of the present invention may further contain, as necessary, colorants, photoinitiator assistants, cyanate compounds, elastomers, mercapto compounds, urethane catalysts, thixotropic agents, adhesion promoters, block copolymers, chain transfer agents, polymerization inhibitors, copper inhibitors, antioxidants, rust inhibitors, thickeners such as organic bentonite and montmorillonite, at least one of silicone-based, fluorine-based, and polymer-based defoamers and leveling agents, silane coupling agents such as imidazole-based, thiazole-based, and triazole-based, and flame retardants such as phosphorus compounds such as phosphinates, phosphate ester derivatives, and phosphazene compounds. These may be known in the field of electronic materials.
[0077] The curable resin composition of the present invention may be used in a liquid form or in the form of a dry film as described below. When used in a liquid form, the composition may be one-component or two or more-component.
[0078] [Dry film] The curable resin composition of the present invention can also be in the form of a dry film having a first film and a resin layer made of the curable resin composition formed on the first film. The first film in the present invention refers to a film that is at least adhered to the resin layer when a base material such as a substrate and a layer (resin layer) made of the curable resin composition formed on the dry film are laminated by heating or the like so that they are in contact with each other to form an integral mold. The first film may be peeled off from the resin layer in a process after lamination. In particular, in the present invention, it is preferable to peel off from the resin layer in a process after exposure. When forming a dry film, the curable resin composition of the present invention is diluted with the above organic solvent to adjust the viscosity to an appropriate level, and applied to a uniform thickness on the first film using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, or the like, and usually dried at a temperature of 50 to 130 ° C. for 1 to 30 minutes to obtain a film. There is no particular restriction on the coating thickness, but it is generally appropriately selected within the range of 1 to 150 μm, preferably 5 to 60 μm, in terms of the thickness after drying.
[0079] As the first film, any known film can be used without any particular limitation, and for example, a film made of a thermoplastic resin such as a polyester film such as polyethylene terephthalate or polyethylene naphthalate, a polyimide film, a polyamideimide film, a polypropylene film, or a polystyrene film can be suitably used. Among these, a polyester film is preferred from the viewpoints of heat resistance, mechanical strength, handling, etc. A laminate of these films can also be used as the first film.
[0080] From the viewpoint of improving mechanical strength, the above-mentioned thermoplastic resin film is preferably a film stretched in a uniaxial or biaxial direction.
[0081] The thickness of the first film is not particularly limited, but can be, for example, 5 μm to 150 μm.
[0082] After forming a resin layer of the curable resin composition of the present invention on the first film, it is preferable to further laminate a peelable second film on the surface of the resin layer for the purpose of preventing dust from adhering to the surface of the resin layer. The second film refers to a film that is peeled off from the resin layer before lamination when a base material such as a substrate and a layer (resin layer) of the curable resin composition formed on a dry film are laminated by heating or the like so as to be in contact with each other to be integrally molded. As the peelable second film, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, a surface-treated paper, etc. can be used. The second film may be any film that has a smaller adhesive strength between the resin layer and the second film than the adhesive strength between the resin layer and the first film when the second film is peeled off.
[0083] The thickness of the second film is not particularly limited, but can be, for example, 5 μm to 150 μm.
[0084] The dry film may be prepared by forming a resin layer by applying the curable resin composition of the present invention onto the second film and drying the same, and then laminating the first film on the surface of the resin layer. That is, in the present invention, either the first film or the second film may be used as the film to which the curable resin composition of the present invention is applied when producing the dry film.
[0085] (cured product) The cured product of the present invention is obtained by curing the above-mentioned curable resin composition or the resin layer of the dry film of the present invention, and has high dielectric properties and good resolution, which are particularly required for a solder resist layer.
[0086] (Printed Wiring Board) The printed wiring board of the present invention has a cured product obtained from the resin layer of the curable resin composition or dry film of the present invention. As a method for producing the printed wiring board of the present invention, for example, the curable resin composition of the present invention is adjusted to a viscosity suitable for the coating method using the organic solvent described above, and applied to a substrate by a method such as dip coating, flow coating, roll coating, bar coating, screen printing, or curtain coating, and then the organic solvent contained in the composition is evaporated and dried (temporarily dried) at a temperature of 60 to 100 ° C. to form a tack-free resin layer. In addition, in the case of a dry film, the resin layer is attached to the substrate by a laminator or the like so that the resin layer contacts the substrate, and then the first film is peeled off to form a resin layer on the substrate.
[0087] Substrates for printed wiring boards include printed wiring boards and flexible printed wiring boards with circuits already formed using copper etc., as well as materials such as paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, copper-clad laminates for high-frequency circuits made from fluororesin, polyethylene, polyphenylene ether, polyphenylene oxide, cyanate etc., including copper-clad laminates of all grades (FR-4 etc.), as well as metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer plates etc.
[0088] The dry film is preferably laminated onto the substrate under pressure and heat using a vacuum laminator or the like. By using such a vacuum laminator, when a substrate on which a circuit is formed is used, even if the substrate has unevenness on its surface, the dry film adheres closely to the substrate, so that no air bubbles are mixed in, and the filling of recesses on the substrate surface is improved. The pressure condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 120°C.
[0089] The volatilization drying carried out after application of the curable resin composition of the present invention can be carried out using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, or the like (a method in which hot air in a dryer equipped with a heat source of an air heating method using steam is brought into countercurrent contact with the substrate, or a method in which hot air is blown onto the substrate from a nozzle).
[0090] After forming a resin layer on a substrate, the resin layer is selectively exposed to active energy rays through a photomask having a predetermined pattern, and the unexposed portion is developed with a dilute alkaline aqueous solution (e.g., 0.3 to 3 mass% aqueous sodium carbonate solution) to form a pattern of the cured product. In the case of a dry film, after exposure, the first film is peeled off from the dry film and development is performed to form a patterned cured product on the substrate. Note that, as long as the characteristics are not impaired, the first film may be peeled off from the dry film before exposure, and the exposed resin layer may be exposed and developed. Furthermore, the cured product is irradiated with active energy rays and then heat-cured (e.g., 100 to 220°C), or irradiated with active energy rays after heat-curing, or heat-cured only to perform final finish curing (main curing), thereby forming a cured film having excellent properties such as adhesion and hardness. In one embodiment, the above-mentioned exposure and development form an exposed portion (circular opening) of the conductor on the substrate. The diameter of the opening is not particularly limited, but can be, for example, 30 to 120 μm.
[0091] The exposure machine used for the active energy ray irradiation may be any machine equipped with a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and capable of irradiating ultraviolet rays in the range of 350 to 450 nm. In addition, a direct imaging machine (for example, a laser direct imaging machine that draws an image directly with a laser based on CAD data from a computer) may also be used. The lamp light source or laser light source of the direct imaging machine may have a maximum wavelength in the range of 350 to 450 nm. The exposure dose for forming an image varies depending on the film thickness, etc., but is generally 10 to 1000 mJ / cm. 2 , preferably 20 to 800 mJ / cm 2 The range may be:
[0092] The developing method may be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution may be an alkaline aqueous solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, or the like.
[0093] When curing the curable resin composition of the present invention, if necessary, after the exposure and development by irradiation with active energy rays described above, ultraviolet light may be irradiated to promote further curing (post-UV), or heat may be applied to promote thermal curing (post-cure). By carrying out post-UV and post-cure, the heat resistance, chemical resistance, moisture absorption resistance, adhesion, electrical properties, and other properties of the cured product of the curable resin composition can be further improved. For example, post-UV is carried out by using a UV conveyor or the like to apply 1000 mJ / cm 2 The post-cure can be carried out by irradiating the film with UV light with an integrated exposure amount of 150° C. for 60 minutes using any of the above-mentioned dryers.
[0094] The curable resin composition or dry film of the present invention is preferably used in the manufacture of electronic components such as printed wiring boards. Specifically, it is used to form a cured coating (permanent coating) in electronic components, and is preferably used to form permanent insulating coatings such as solder resists, interlayer insulating layers, and coverlays. More specifically, the curable resin composition or dry film of the present invention is preferably used for printed wiring boards that require high reliability, such as substrates for semiconductor packages, particularly FC-BGA substrates. EXAMPLES
[0095] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" are all based on mass unless otherwise specified.
[0096] [Preparation of Curable Resin Composition] (Example of photocurable resin synthesis) Prior to the preparation of the curable resin composition, a photocurable resin used in this example was prepared according to the procedure described below. First, 456 parts of bisphenol A, 228 parts of water, and 649 parts of 37% formalin were charged into a flask equipped with a cooling tube and a stirrer, and the temperature was kept below 40°C. 228 parts of 25% aqueous sodium hydroxide solution was added, and after the addition was completed, the mixture was reacted at 50°C for 10 hours. After the reaction was completed, the mixture was cooled to 40°C, and while maintaining the temperature below 40°C, a 37.5% aqueous phosphoric acid solution was added to neutralize the mixture to pH 4, and the mixture was allowed to stand to separate the aqueous layer. After the aqueous layer was separated, 300 parts of methyl isobutyl ketone was added and dissolved uniformly, and then the mixture was washed three times with 500 parts of distilled water, and the mixture was reduced in pressure at a temperature below 50°C to remove water, solvent, etc., to obtain a polymethylol compound. The obtained polymethylol compound was dissolved in 550 parts of methanol to obtain 1230 parts of a methanol solution of the polymethylol compound. A part of the obtained methanol solution of the polymethylol compound was dried at room temperature in a vacuum dryer, and the solid content was 55.2%. Next, 500 parts of the resulting methanol solution of the polymethylol compound and 440 parts of 2,6-xylenol were charged and dissolved uniformly at 50°C. After the mixture was dissolved uniformly, methanol was removed under reduced pressure at a temperature of 50°C or less. Then, 8 parts of oxalic acid was added and reacted at 100°C for 10 hours. After the reaction was completed, the distillate was removed under reduced pressure at 180°C and 50 mmHg to obtain 550 parts of novolak resin A.
[0097] Next, 130 parts of the novolak resin A obtained by the above procedure, 2.6 parts of a 50% aqueous sodium hydroxide solution, and 100 parts of toluene / methyl isobutyl ketone (mass ratio = 2 / 1) were charged into an autoclave equipped with a thermometer, a nitrogen introducing device / alkylene oxide introducing device, and a stirrer, and the system was purged with nitrogen while stirring, and then heated to 150 °C and 8 kg / cm 2 45 parts of ethylene oxide was gradually introduced and reacted at a gauge pressure of 0.0 kg / cm 2The reaction was continued for about 4 hours until the reaction solution reached a state where the mixture was cooled to room temperature. 3.3 parts of 36% aqueous hydrochloric acid was added to the reaction solution and mixed to neutralize the sodium hydroxide. The neutralized reaction product was diluted with toluene, washed with water three times, and the solvent was removed using an evaporator to obtain an ethylene oxide adduct of novolac resin A with a hydroxyl value of 175 g / eq. The ethylene oxide adduct of novolac resin A had an average of 1 mole of ethylene oxide added per equivalent of phenolic hydroxyl group.
[0098] Next, 175 parts of the ethylene oxide adduct of the obtained novolak resin A, 50 parts of acrylic acid, 3.0 parts of p-toluenesulfonic acid, 0.1 parts of hydroquinone monomethyl ether, and 130 parts of toluene were charged into a reactor equipped with a stirrer, a thermometer, and an air-inlet tube, and the mixture was stirred while blowing in air, heated to 115°C, and reacted. The reaction was continued for another 4 hours while distilling off the water produced by the reaction as an azeotropic mixture with toluene, and then cooled to room temperature. The resulting reaction solution was washed with a 5% aqueous NaCl solution, and the toluene was removed by distillation under reduced pressure, and diethylene glycol monoethyl ether acetate was added to obtain an acrylate resin solution with a solid content of 68%.
[0099] Next, 312 parts of the obtained acrylate resin solution, 0.1 parts of hydroquinone monomethyl ether, and 0.3 parts of triphenylphosphine were charged into a four-neck flask equipped with a stirrer and a reflux condenser, the mixture was heated to 110°C, 45 parts of tetrahydrophthalic anhydride was added, and the reaction was carried out for 4 hours. After cooling, a solution of a photocurable resin (carboxyl group-containing resin) with a solid content of 70% and an acid value of the solid content of 65 mgKOH / g was obtained.
[0100] (Example of synthesis of surface-treated barium compound) Prior to the preparation of the curable resin composition, the surface-treated barium compound used in this example was prepared according to the procedure described below. First, 700 g of barium sulfate B-30 (average particle size 0.3 μm) manufactured by Sakai Chemical Industry Co., Ltd., 295 g of diethylene glycol monoethyl ether acetate (carbitol acetate) as a solvent, and 5 g of a wetting dispersant were mixed and stirred, and a dispersion treatment was performed using a bead mill until the average particle size became 0.3 μm. After the dispersion treatment, the obtained dispersion was filtered through a 3 μm filter to remove foreign matter and coarse particles, and a barium sulfate slurry with an average particle size of 0.3 μm was obtained. The solid content of the obtained barium sulfate slurry was 70 mass%.
[0101] (Example of synthesis of surface-treated silica) Prior to the preparation of the curable resin composition, the surface-treated silica used in this example was prepared according to the procedure described below. 700g of spherical silica SO-C2 manufactured by Admatechs Co., Ltd. and 300g of propylene glycol monomethyl ether acetate (PMA) as a solvent were mixed and stirred, and a dispersion treatment was performed using a bead mill until the average particle size became 0.7 μm. After the dispersion treatment, the obtained dispersion was filtered through a 3 μm filter to remove foreign matter and coarse particles, and a silica slurry with an average particle size of 0.7 μm was obtained. The solid content of the obtained silica slurry was 70 mass%. Next, a silane coupling agent KBM-503 having a methacryl group manufactured by Shin-Etsu Chemical Co., Ltd. was added to the obtained silica slurry so that the amount was 4 mass%, and the mixture was dispersed in a bead mill for 10 minutes to obtain a spherical silica slurry surface-treated with methacrylsilane. The solid content of the obtained spherical silica slurry was 70 mass%.
[0102] The components shown in Table 1 below were mixed in the amounts (solid content) shown in the table, premixed with a stirrer, and then kneaded with a three-roll mill to prepare the curable resin compositions of Examples 1 to 7 and Comparative Examples 1 to 5. Details of each component in Table 1 are as follows. (A-1) Photocurable resin: a carboxyl group-containing resin obtained by the synthesis example of the photocurable resin described above (A-2) Thermosetting resin: jER (registered trademark) 834 manufactured by Mitsubishi Chemical Corporation (B) Surface-treated barium compound: Surface-treated barium sulfate slurry obtained by the above-mentioned synthesis example of the surface-treated barium compound (C) Surface-treated silica: Surface-treated spherical silica slurry obtained by the above-mentioned synthesis example of surface-treated silica (D) Rubber particles: butadiene rubber Metablen (registered trademark) C-223A manufactured by Mitsubishi Chemical Corporation (E) Photopolymerization initiator: 2,4,6-trimethylbenzoyldiphenylphosphine oxide Photopolymerizable monomer: acrylate monomer (DPHA: dipentaerythritol hexaacrylate) Heat curing catalyst 1: Melamine Heat curing catalyst 2: Dicyandiamide [Table 1]
[0103] [Preparation of laminated structure] Using each of the curable resin compositions obtained according to the above-mentioned procedure, a laminate structure (dry film) corresponding to each of the curable resin compositions was prepared according to the procedure described below. First, using a bar coater, each curable resin composition was appropriately diluted with methyl ethyl ketone, and then using an applicator, the diluted solution was applied to a PET film FB-50 (thickness 16 μm) manufactured by Toray Industries, Inc., so that the film thickness after drying would be 18 μm. The solution was then dried at 80° C. for 10 minutes to obtain a dry film corresponding to each curable resin composition.
[0104] [Resolution evaluation] Each dry film prepared according to the above-mentioned procedure was chemically polished using MEC Etch Bond CZ-8101 manufactured by MEC Co., Ltd., and a copper circuit was formed on the substrate. The substrate was then heat-laminated at 80°C for 1 minute using a vacuum laminator CVP-300 manufactured by Nikko Materials Co., Ltd. at a temperature of 80°C, a vacuum pressure of 3 hPa, and a pressure of 0.4 MPa, and then pressed with a flat plate at a temperature of 70°C and a pressure of 0.5 MPa to obtain a substrate having a layer (dry film) of each unexposed curable resin composition. Each obtained substrate was exposed to a standard exposure amount using a φ50μm photomask and an exposure device equipped with a high-pressure mercury lamp (short arc lamp), and the PET film was peeled off from the dry film. Then, the substrate was exposed to a standard exposure amount using a φ50μm photomask and a spray pressure of 2kg / cm at 30°C. 2 Under the condition of 1 mass% Na 2 CO 3 The substrate was developed for 60 seconds using an aqueous solution to obtain each sample substrate having a cured product with a micropore pattern formed thereon. Each of the obtained sample substrates was exposed to a cumulative exposure dose of 1000 mJ / cm using a UV conveyor oven. 2 After irradiation with ultraviolet light of 100 ohms, the cured product on each sample substrate was fully cured by heating at 150° C. for 60 minutes.
[0105] After each sample substrate prepared according to the above procedure was subjected to Pt sputtering, the diameter of the bottom of the microhole on each sample substrate was measured using a scanning electron microscope (SEM), and the resolution was evaluated according to the following criteria. The results are shown in Table 1. ◎: The diameter of the bottom is 25 μm or more and less than 50 μm. ◯: The diameter of the bottom is 20 μm or more and less than 25 μm. △: The diameter of the bottom is 15 μm or more and less than 20 μm. ×: The diameter of the bottom is less than 15 μm.
[0106] [Crack resistance evaluation] A substrate having a cured product having a Si chip mounting pattern was obtained in the same procedure as the preparation of the evaluation substrate used in the above-mentioned resolution evaluation, except that the φ50 μm microhole pattern was replaced with a Si chip mounting pattern. Next, Au plating and solder bump formation were performed, and Si chips were mounted to obtain each sample substrate for thermal shock test (TST: Thermal Shock Test). Each obtained sample substrate was placed in a thermal cycler in which temperature cycles of -65°C and 150°C were performed in the liquid layer, and TST was performed. During TST, the surface of the cured product on each sample substrate was observed at 600 cycles, 800 cycles, and 1000 cycles, and the crack resistance was evaluated according to the following evaluation criteria. The results are shown in Table 1. ◎: No abnormalities even after 1000 cycles. ◯: No abnormality at 750 cycles, but cracks observed at 1000 cycles. △: No abnormality at 500 cycles, but cracks are observed at 750 cycles. ×: Cracks were observed after 500 cycles.
[0107] From the evaluation results shown in Table 1, it is understood that the cured products formed from the curable resin compositions of Examples 1 to 7 have both good developability and good crack resistance in TST. On the other hand, it is understood that the cured products formed from the curable resin compositions of Comparative Examples 1 to 5 do not have both good developability and good crack resistance in TST.
Claims
1. (A) a curable resin; (B) a surface-treated barium compound; (C) surface-treated silica; (D) rubber particles; A curable resin composition comprising: The total content of the surface-treated barium compound (B) and the surface-treated silica (C) is 20 to 80 mass% on a solid content basis with respect to the total mass of the solid content of the curable resin composition; The mass ratio of the surface-treated barium compound (B) to the surface-treated silica (C) is 1:1 to 1:4 based on the solid content, The surface-treated barium compound (B) is a barium compound having a reactive functional group chemically or physically adsorbed on the surface thereof, A curable resin composition, wherein the surface-treated silica (C) is silica having a reactive functional group chemically or physically adsorbed on the surface thereof.
2. The curable resin composition according to claim 1, wherein the (A) curable resin comprises (A-1) a photocurable resin.
3. The curable resin composition according to claim 1, wherein the (A) curable resin comprises (A-2) a thermosetting resin.
4. The curable resin composition according to claim 1 , wherein the (D) rubber particles comprise core-shell rubber particles.
5. The curable resin composition according to claim 1 , further comprising (E) a photopolymerization initiator.
6. A dry film comprising a first film and a resin layer formed on at least one surface of the first film, the resin layer being made of the curable resin composition according to claim 1.
7. A cured product obtained by curing the curable resin composition according to claim 1 or the resin layer of the dry film according to claim 6.
8. A printed wiring board comprising the cured product according to claim 7.
Citation Information
Patent Citations
Photosensitive resin composition
JP2016066006A
Curable resin composition, dry film, cured product and printed wiring board
JP2016194669A
Photosensitive resin composition, and dry film, printed wiring board and method for manufacturing printed wiring board using the composition
JP2017116652A
Photosensitive resin composition, photosensitive element, printed wiring board, and method for manufacturing printed wiring board
JP2018169440A
Curable resin composition, dry film composed of the composition, cured product and printed wiring board having the cured product