Method for manufacturing positive electrode active material for lithium secondary battery and positive electrode active material manufactured by the same

By forming a stable NiO phase on the surface of high-nickel lithium transition metal oxide particles through hot water washing, the method addresses structural instability and reactivity issues, enhancing the performance of lithium secondary batteries.

JP7595793B2Active Publication Date: 2024-12-06LG ENERGY SOLUTION LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023574680
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-11-24
Filing Date
2022-11-02
Publication Date
2024-12-06
Estimated Expiration
2042-11-02

AI Technical Summary

Technical Problem

Existing high-nickel cathode active materials for lithium secondary batteries suffer from structural instability, gas generation, and increased leakage current due to high reactivity with the electrolyte, limiting their capacity and performance.

Method used

A method involving the production of a lithium transition metal oxide with a nickel content of 70 mol% or more, followed by washing with hot water above 90°C to form a stable NiO phase on the particle surface, reducing surface reactivity and enhancing structural stability.

Benefits of technology

The method reduces gas generation and leakage current under high voltage or temperature conditions, improving the battery's capacity and stability by stabilizing the electrode surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595793000002
    Figure 0007595793000002
  • Figure 0007595793000003
    Figure 0007595793000003
  • Figure 0007595793000001
    Figure 0007595793000001
Patent Text Reader

Abstract

The present invention relates to a method for producing a positive electrode active material for a lithium secondary battery and a positive electrode active material produced thereby, the method comprising: a first step of mixing a transition metal precursor containing 70 mol % or more of nickel based on the total moles of transition metals and a lithium raw material, followed by calcining the mixture to produce a lithium transition metal oxide; and a second step of washing the lithium transition metal oxide with hot water at a temperature of over 90°C, wherein after the second step, an EELS analysis result for the particle surfaces of the lithium transition metal oxide satisfies Equation 1.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0163458 filed on November 24, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a method for producing a positive electrode active material for a lithium secondary battery, a positive electrode active material produced thereby, and a lithium secondary battery including the positive electrode active material. [Background technology]

[0003] Recently, with the rapid spread of electronic devices using batteries, such as mobile phones, notebook computers, and electric vehicles, the demand for secondary batteries that are small, lightweight, and have a relatively high capacity is rapidly increasing. In particular, lithium secondary batteries, which are lightweight and have high energy density, are attracting attention as a driving power source for portable devices. Therefore, active research and development efforts are being made to improve the performance of lithium secondary batteries.

[0004] Lithium secondary batteries generate electrical energy through oxidation and reduction reactions that occur when lithium ions are inserted and extracted at the positive and negative electrodes, with an organic or polymer electrolyte filled between the positive and negative electrodes, which are made of active materials that allow for the intercalation and deintercalation of lithium ions.

[0005] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMn2O4, etc.), lithium iron phosphate compound (LiFePO4), etc. have been used as positive electrode active materials for lithium secondary batteries. In addition, as a method for maintaining the excellent reversible capacity of LiNiO2 and improving its low thermal stability, lithium composite metal oxides in which part of nickel (Ni) is replaced with cobalt (Co) and manganese (Mn) (hereinafter simply referred to as "NCM-based lithium composite transition metal oxides") have been developed. However, the capacity characteristics of the previously developed NCM-based lithium composite transition metal oxides were insufficient, and their application was limited.

[0006] To address these issues, recent research has been conducted to increase the Ni content in NCM-based lithium transition metal composite oxides. However, in the case of high-nickel (High-Ni) positive electrode active materials with a high nickel content, there are problems in that the high reactivity of nickel generates a large amount of gas during charging and discharging, and the instability of the lattice structure increases due to cation mixing and oxygen desorption, which can cause the structure to collapse.

[0007] For this reason, active technological development has been conducted to improve the structural stability of NCM-based lithium transition metal composite oxides by applying coating or doping. However, since coating or doping alone does not provide a uniform effect of improving structural stability throughout the oxide surface and lattice, a technology to solve this problem is needed. Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made to solve the above problems, and aims to provide a positive electrode active material that has a high nickel content and can exhibit high capacity, and has high structural stability and can help reduce the amount of leakage current and gas generation in a lithium secondary battery. [Means for solving the problem]

[0009] The present invention relates to A first step of producing a lithium transition metal oxide by mixing and calcining a transition metal precursor containing 70 mol % or more of nickel based on the total moles of the transition metal and a lithium source material; and a second step of washing the lithium transition metal oxide with hot water at above 90°C; The method for producing a positive electrode active material for a lithium secondary battery is provided, in which after the second step, an EELS analysis result for the surface of the lithium transition metal oxide particles satisfies the following formula 1: [Formula 1] I(853eV) / I(855.5eV)≧1 In the above formula 1, I(853 eV) is the peak intensity shown near 853 eV, I(855.5 eV) is the peak intensity observed near 855.5 eV.

[0010] The present invention also provides a lithium transition metal oxide containing 70 mol % or more of nickel based on the total number of moles of transition metals,

[0011] The positive electrode active material for a lithium secondary battery is provided, in which the EELS analysis result for the surface of the lithium transition metal oxide particles satisfies the formula 1.

[0012] The present invention also provides a positive electrode comprising a positive electrode active material layer including the positive electrode active material for a lithium secondary battery according to the present invention.

[0013] The present invention also provides a lithium secondary battery comprising the positive electrode according to the present invention. Effect of the Invention

[0014] The method for manufacturing a positive electrode active material according to the present invention provides a method for adjusting the surface reactivity by adjusting the water washing conditions during synthesis of a high-nickel (High-Ni) positive electrode active material, and when the positive electrode active material manufactured thereby is applied to a lithium secondary battery, it is possible to reduce leakage current and gas generation that occur under high voltage or high temperature conditions. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a diagram showing EELS spectra for the surfaces of the positive electrode active materials produced in Examples 1 and 2 of the present invention and Comparative Examples 1 and 2. [Diagram 2] FIG. 2 is a diagram showing EELS spectra relating to the surfaces of the positive electrode active materials produced in Examples 1 and 2 of the present invention and Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] In the following, the present invention will be described in more detail in order to facilitate understanding of the present invention.

[0017] In the present invention, the term "primary particle" refers to a particle unit that does not appear to have grain boundaries when observed at a magnification of 5,000 to 20,000 times using a scanning electron microscope, and the term "secondary particle" refers to a particle formed by aggregation of multiple primary particles.

[0018] In the present invention, the term "EELS analysis result" refers to an EELS spectrum obtained by electron energy-loss spectroscopy (EELS). The EELS spectrum can be obtained using an HR-TEM device, with the horizontal axis indicating the loss energy region and the vertical axis indicating the peak intensity.

[0019] In formula 1 of the present invention, "around 853 eV" means a region of 853±0.5 eV, and "around 855.5 eV" means a region of 855.5±0.5 eV.

[0020] In the present invention, the "particle surface" refers to a region located within a distance of 100 nm from the surface of the particle toward the center.

[0021] Method for producing positive electrode active material First, a method for producing a positive electrode active material according to the present invention will be described.

[0022] A method for producing a positive electrode active material for a lithium secondary battery according to one embodiment of the present invention includes a first step of mixing a transition metal precursor containing 70 mol % or more of nickel based on the total moles of the transition metals and a lithium raw material, and calcining the mixture to produce a lithium transition metal oxide; and a second step of washing the lithium transition metal oxide with hot water at above 90°C; After the second step, the EELS analysis result for the surface of the lithium transition metal oxide particles satisfies the following formula 1.

[0023] [Formula 1] I(853eV) / I(855.5eV)≧1

[0024] In the above formula 1, I(853 eV) is the peak intensity shown near 853 eV, I(855.5 eV) is the peak intensity observed near 855.5 eV.

[0025] High Ni positive active materials, which contain 70 mol% or more of Ni among transition metals, have the advantage of being able to achieve high capacity, but not only does it increase the amount of gas generated due to side reactions with the electrolyte during charging and discharging, it also experiences frequent changes in lattice constant, i.e., changes in the volume within the unit lattice. In particular, when the Ni content exceeds 80 mol%, a phase transition occurs around 4.2V, causing the lattice to suddenly shrink. Such volume changes cause cracks to occur within the active material, and these cracks can cause voids to occur within the active material, leading to a decrease in battery performance.

[0026] Specifically, Ni was deposited on the surface of the transition metal oxide particles. 2+Less stable than Ni 3+ When there are a lot of ions, they may react with the electrolyte and accelerate the decomposition of the electrolyte, shortening the battery life and also causing oxygen release from the crystal structure. The released oxygen oxidizes the electrolyte and increases the amount of gas generated, which reduces the stability of the battery, and the problem becomes more serious especially under high temperature and high voltage conditions.

[0027] Therefore, the present inventors have attempted to suppress the surface reactivity of the positive electrode active material to the maximum extent possible. In the case where the temperature of the washing solution is increased in the water washing step performed after calcining the precursor during synthesis of the positive electrode active material, lithium impurities present on the surfaces of not only the secondary particles but also the primary particles are washed away, so that Ni is not present on the surfaces of both the secondary particles and the primary particles. 2+ We focused on the fact that Ni is easily exposed. 2+ It was confirmed that, although NiO forms a highly stable NiO phase by bonding with O on the surface, in the case of the present invention, NiO phase is formed even on the surface of the primary particles, so that the surface reactivity can be effectively reduced. In other words, it was discovered that, since the surfaces of not only the secondary particles but also the primary particles exist in a reduced state, it is possible to prevent the phenomenon of oxygen being released by the reduction of nickel ions, and to reduce the phenomenon in which the released oxygen reacts with the electrolyte to change the surface properties of the electrode or generate gas. It was also confirmed that the effect of reducing the leakage current value during continuous charging and discharging is achieved by surface stabilization.

[0028] 1) First step First, a transition metal precursor and a lithium source material are mixed and calcined to produce a lithium transition metal oxide.

[0029] Here, the transition metal precursor may be a commercially available precursor such as nickel-cobalt-manganese hydroxide, or may be prepared by a method known in the art.

[0030] Specifically, the transition metal precursor used in the present invention is a transition metal hydroxide containing nickel, cobalt, and manganese, and containing 70 mol% or more of nickel based on the total number of moles of the entire transition metal, and preferably can be a nickel cobalt manganese hydroxide containing 80 mol% or more of nickel. When the nickel content in the transition metal precursor satisfies the above range, high capacity characteristics can be realized.

[0031] Specifically, the transition metal precursor can be represented by the following Chemical Formula 2.

[0032] [Chemical Formula 2] Ni b1 Co c1 Mn d1 Q e1 (OH)2

[0033] In Chemical Formula 2, b1, c1, d1, and e1 are respectively 0.7 ≦ b1 < 1.0, 0 < c1 ≦ 0.25, 0 < d1 ≦ 0.25, 0 ≦ e1 ≦ 0.1, and b1 + c1 + d1 + e1 = 1.0. Q is any one or more selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo.

[0034] Preferably, Q may be any one or more selected from the group consisting of Al, Mg, V, Ti, and Zr.

[0035] In one embodiment of the present invention, b1, c1, d1, and e1 in Chemical Formula 2 can be respectively 0.8 ≦ b1 < 1.0, 0 < c1 ≦ 0.15, 0 < d1 ≦ 0.15, and 0 ≦ e1 ≦ 0.05, and more preferably can be 0.85 ≦ b1 < 1.0, 0 < c1 ≦ 0.10, 0 < d1 ≦ 0.10, and 0 ≦ e1 ≦ 0.03.

[0036] The transition metal precursor may be prepared, for example, by introducing an aqueous transition metal solution, an ammonium cation complexing agent, and a basic compound into a reactor and carrying out a coprecipitation reaction while stirring.

[0037] The transition metal aqueous solution can be prepared by dissolving a transition metal-containing raw material in a solvent such as water, for example, by dissolving a nickel-containing raw material, a cobalt-containing raw material, and a manganese-containing raw material in water. If necessary, the transition metal aqueous solution can further contain the Q metal-containing raw material.

[0038] Meanwhile, the transition metal-containing raw material may be an acetate, carbonate, nitrate, sulfate, halide, sulfide, or oxide of a transition metal.

[0039] Specifically, the nickel-containing source material can be, for example, NiO, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, nickel halides, or combinations thereof.

[0040] The cobalt-containing source material can be, for example, CoSO4, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, CoSO4·7H2O, or combinations thereof.

[0041] The manganese-containing source material can be, for example, Mn2O3, MnO2, Mn3O4, MnCO3, Mn(NO3)2, MnSO4·H2O, manganese acetate, manganese halides, or combinations thereof.

[0042] The Q metal-containing raw material may be an aluminum-containing raw material, such as Al2O3, Al(OH)3, Al(NO3)3, Al2(SO4)3, (HO)2AlCH3CO2, HOAl(CH3CO2)2, Al(CH3CO2)3, aluminum halide, or a combination thereof. However, in the case of Al, it may not be added to the transition metal aqueous solution, but may be added together with the lithium raw material in the calcination step described below. In addition, it may be acetate, carbonate, nitrate, sulfate, halide, sulfide, or oxide of the Q metal.

[0043] The input amount of each of the transition metal-containing raw materials may be determined in consideration of the molar ratio of the transition metal in the final cathode active material to be produced.

[0044] Meanwhile, the ammonium cation complexing agent may include at least one compound selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and NH4(CO3)2, and may be added to the reactor in the form of a solution in which the compound is dissolved in a solvent. Here, the solvent may be water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water.

[0045] The basic compound may be at least one compound selected from the group consisting of NaOH, KOH, and Ca(OH)2, and may be added to the reactor in the form of a solution in which the compound is dissolved in a solvent, where the solvent may be water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water.

[0046] As described above, when the aqueous transition metal solution, the ammonium cation complexing agent, and the basic compound are charged into a reactor and stirred, the transition metal in the aqueous transition metal solution is coprecipitated to produce precursor particles in the form of transition metal hydroxide.

[0047] Here, the aqueous transition metal solution, the ammonium cation complex forming agent and the basic compound are added in amounts such that the pH of the reaction solution falls within a desired range.

[0048] When the precursor particles are formed by the above-mentioned method, the particles are separated from the reaction solution to obtain the transition metal precursor. For example, the reaction solution is filtered to separate the transition metal precursor from the reaction solution, and the separated transition metal precursor is washed with water and dried to obtain the transition metal precursor. Here, if necessary, a process such as pulverization and / or classification may be performed.

[0049] Next, the transition metal precursor and a lithium source material are mixed and calcined to produce a lithium transition metal oxide, where a Q metal-containing source material can be mixed and calcined as necessary.

[0050] The lithium source material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, for example, Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or a mixture thereof.

[0051] Meanwhile, the lithium source material and the positive electrode active material precursor may be mixed so that the molar ratio of Li:total metals in the precursor is 1:1 to 1.2:1, preferably 1.02:1 to 1.05:1. When the mixing ratio of the lithium source material and the metals in the positive electrode active material precursor satisfies the above range, the layered crystal structure of the positive electrode active material is well developed, and a positive electrode active material having excellent capacity characteristics and structural stability can be produced.

[0052] In one embodiment of the present invention, the first step of calcination can be carried out in an oxygen atmosphere at 750° C. to 830° C., preferably 750° C. to 780° C., for 10 hours to 17 hours. The calcination temperature and time within the above ranges are preferred in terms of ensuring structural stability through sufficient reaction and optimal electrochemical properties.

[0053] Second step In the present invention, the lithium transition metal oxide produced in the first step is washed with hot water of over 90°C, preferably hot water of 95°C to 150°C, more preferably hot water of 95°C to 130°C, to remove Ni from not only the secondary particles but also the surfaces of the primary particles. 2+ The ions are exposed to the surface, so that the NiO phase can be formed on the surface of both the secondary particles and the primary particles. A hot water temperature of more than 90°C is favorable for the formation of the NiO phase on the surface, but an excessively high temperature can cause damage to the surface of the active material and reduce its structural stability, so it is preferable to set the temperature at 150°C or less.

[0054] Specifically, the washing can be performed by stirring the lithium transition metal oxide together with warm water in a stirrer using a magnet bar at 800 rpm.

[0055] On the other hand, the weight of the hot water used in the second step can be 1 to 3 times the weight of the lithium transition metal oxide, which is preferable in that the Li by-products and Li ions on the surface of the oxide are thoroughly washed away.

[0056] The second step can be carried out for 10 to 30 minutes. If the surface Li is washed away excessively, problems such as capacity deterioration can occur, so washing for 30 minutes or less is preferable.

[0057] After the second step, a drying step may be performed at a temperature of 130° C. to 150° C. for 12 hours to 24 hours, but is not limited thereto.

[0058] In the present invention, after the second step, the EELS analysis result for the particle surface of the lithium transition metal oxide satisfies the formula 1. 2+ In the case of Ni, near 853 eV 3+ In the case of Ni, it is shown at around 855.5 eV, so by comparing the intensity of each peak, 2+ and Ni 3+ The contents of can be compared.

[0059] Preferably, the I(853 eV) / I(855.5 eV) value may be 1 or more and 3 or less.

[0060] In one embodiment of the present invention, after the second step, Ni is added to the surface of the lithium transition metal oxide particles. 2+ Ni 3+ It may be contained in a larger amount than that.

[0061] positive electrode active material Next, the positive electrode active material according to the present invention will be described.

[0062] The positive electrode active material according to the present invention includes a lithium transition metal oxide containing 70 mol % or more of nickel based on the total moles of transition metals, and the EELS analysis result of the surface of the lithium transition metal oxide particles satisfies the formula 1. The positive electrode active material according to the present invention can be manufactured by the above-mentioned manufacturing method of the present invention, and the description of each component can be cited from the contents of the manufacturing method.

[0063] In one embodiment of the present invention, the lithium transition metal oxide may be a lithium transition metal oxide containing nickel, cobalt and manganese, and containing 70 mol% or more of nickel based on the total moles of all transition metals, and preferably a lithium nickel cobalt manganese oxide containing 80 mol% or more of nickel. When the nickel content satisfies the above range, high capacity characteristics can be achieved.

[0064] Specifically, the lithium transition metal oxide may be represented by the following Formula 1.

[0065] [Chemical formula 1] Li a [Ni b Co c Mn d Q e ]O 2+f

[0066] In the above Chemical Formula 1, a, b, c, d, e, and f are 0.8≦a≦1.5, 0.7≦b<1.0, 0 <c≦0.25、0<d≦0.25、0≦e≦0.1、b+c+d+e=1.0、-0.1≦f≦1.0であり、 Q is one or more selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo.

[0067] In one embodiment of the present invention, Q is one or more selected from the group consisting of Al, Mg, V, Ti and Zr.

[0068] In one embodiment of the present invention, a in Chemical Formula 1 may be 1.0≦a≦1.5, or 1.0≦a≦1.2.

[0069] In one embodiment of the present invention, b, c, d and e in the above Chemical Formula 1 are each independently 0.8≦b<1.0, 0 <c≦0.15、0<d≦0.15および0≦e≦0.05であることができる。

[0070] In addition, the surface of the lithium transition metal oxide particles is provided with Ni 2+ Ni 3+ It may be contained in a larger amount than that.

[0071] positive electrode Next, the positive electrode according to the present invention will be described.

[0072] The positive electrode according to the present invention includes a positive electrode active material layer including the positive electrode active material according to the present invention. Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and including the positive electrode active material.

[0073] In the positive electrode, the positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can usually have a thickness of 3 to 500 μm, and fine irregularities can be formed on the surface of the positive electrode current collector to increase the adhesive force of the positive electrode active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0074] The positive electrode active material layer may contain a conductive material and a binder in addition to the positive electrode active material.

[0075] The conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery to be constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; carbon-based materials such as carbon fibers and carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and one or more of these can be used alone or in combination. The conductive material can usually be contained in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, based on the total weight of the positive electrode active material layer.

[0076] The binder serves to improve the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, more preferably 1 to 10% by weight, based on the total weight of the positive electrode active material layer.

[0077] The positive electrode may be manufactured by a conventional method for manufacturing a positive electrode. For example, the positive electrode may be manufactured by mixing a positive electrode active material, a binder, and / or a conductive material in a solvent to prepare a positive electrode slurry, applying the positive electrode slurry onto a positive electrode current collector, and then drying and rolling the positive electrode slurry. Here, the types and contents of the positive electrode active material, binder, and conductive material are as described above.

[0078] The solvent may be a solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to have a viscosity that can dissolve or disperse the positive electrode active material, conductive material, and binder and provide excellent thickness uniformity during subsequent coating for the production of a positive electrode, taking into consideration the coating thickness of the slurry and the manufacturing yield.

[0079] Alternatively, the positive electrode can be produced by casting the positive electrode slurry on a separate support, peeling the resulting film from the support, and laminating the film on a positive electrode current collector.

[0080] Lithium secondary battery Next, the lithium secondary battery according to the present invention will be described.

[0081] The lithium secondary battery of the present invention includes the positive electrode according to the present invention. Specifically, the lithium secondary battery includes a positive electrode, a negative electrode facing the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, the positive electrode being as described above. The lithium secondary battery may also optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0082] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0083] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of usually 3 to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0084] The negative electrode active material layer includes a negative electrode active material, and optionally a binder and a conductive material.

[0085] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β (0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the above-mentioned metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used.

[0086] Also, a metallic lithium thin film may be used as the negative electrode active material. Also, the carbonaceous material may be either low crystalline carbon or high crystalline carbon. Typical low crystalline carbons are soft carbon and hard carbon, and typical high crystalline carbons are amorphous, plate-like, flaky, spherical or fibrous natural graphite or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, mesocarbon microbeads, mesophase pitches, and high temperature fired carbons such as petroleum or coal tar pitch derived cokes.

[0087] The conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery to be constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; carbon-based materials such as carbon fibers and carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and one or more of these can be used alone or in combination. The conductive material can usually be contained in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, based on the total weight of the negative electrode active material layer.

[0088] The binder serves to improve the adhesion between the negative electrode active material particles and the adhesive strength between the negative electrode active material and the negative electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, more preferably 1 to 10% by weight, based on the total weight of the negative electrode active material layer.

[0089] For example, the negative electrode active material layer may be manufactured by applying a negative electrode slurry containing a negative electrode active material, and optionally a binder and a conductive material, onto a negative electrode current collector and drying the applied negative electrode slurry, or by casting the negative electrode slurry onto a separate support, peeling the negative electrode slurry from the support, and laminating the resulting film onto the negative electrode current collector.

[0090] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent humidification ability of the electrolyte solution is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, etc., can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used as a single layer or a multilayer structure.

[0091] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.

[0092] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0093] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethyl alcohol and isopropyl alcohol, nitriles such as R-CN (R is a C2-C20 straight-chain, branched or cyclic hydrocarbon group that can contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of a battery and a low-viscosity straight-chain carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferred.

[0094] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used as the lithium salt. The concentration of the lithium salt is preferably within a range of 0.1 to 5.0M, preferably 0.1 to 3.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0095] In addition to the electrolyte components, the electrolyte may further contain additives for the purpose of improving the life characteristics of the battery, suppressing the decrease in the battery capacity, and improving the discharge capacity of the battery. For example, the additives may be haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethyl alcohol amine, cyclic ethers, ethylene diamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethyl alcohol, or aluminum trichloride, which may be used alone or in combination, but are not limited thereto. The additives may be contained in an amount of 0.1 to 10% by weight, preferably 0.1 to 5% by weight, based on the total weight of the electrolyte.

[0096] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention rate, and is therefore useful in portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0097] According to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.

[0098] The battery module or the battery pack may be used as a power source for one or more medium- to large-sized devices including a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0099] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the embodiments of the present invention will be described in detail so that those skilled in the art can easily carry out the present invention.

[0100] [Examples and Comparative Examples: Production of Positive Electrode Active Material] Comparative Example 1 After 4 liters of distilled water was added to a coprecipitation reactor (volume 20 L), 100 mL of ammonia solution with a concentration of 28% by weight was added while maintaining the temperature at 50°C, and NiSO4, CoSO4, and MnSO4 were mixed so that the molar ratio of nickel:cobalt:manganese was 0.8:0.1:0.1. A transition metal solution with a concentration of 3.2 mol / L was continuously added to the reactor at 300 mL / hr and ammonia solution with a concentration of 28% by weight was continuously added at 42 mL / hr. The impeller speed was set to 400 rpm for stirring, and a 40% by weight sodium hydroxide solution was added to maintain the pH at 9. The coprecipitation reaction was carried out for 10 hours to form precursor particles. The precursor particles were separated and washed, and then dried in an oven at 130°C to produce a precursor.

[0101] Ni synthesized by coprecipitation reaction 0.8 Co 0.1 Mn 0.1The (OH)2 precursor was mixed with LiOH so that the Li / Me(Ni, Co, Mn) molar ratio was 1.03, and then heat-treated at 770 °C in an oxygen atmosphere for 10 hours to obtain Li[Ni 0.8 Co 0.1 Mn 0.1 ]O2 lithium composite transition metal oxide was prepared.

[0102] Then, 50 g of the prepared lithium transition metal oxide was placed in a beaker, placed on a stirrer, and washed with water at 25° C. for 10 minutes. The amount of water was 50 g. After washing, the mixture was dried in a vacuum at 130° C. for 24 hours to complete the positive electrode active material.

[0103] Comparative Example 2 A positive electrode active material was prepared in the same manner as in Comparative Example 1, except that the washing and drying processes were not performed.

[0104] Comparative Example 3. A positive electrode active material was prepared in the same manner as in Comparative Example 1, except that hot water at 70° C. was used instead of water at 25° C. during the washing.

[0105] Example 1. A positive electrode active material was prepared in the same manner as in Comparative Example 1, except that hot water at 95° C. was used instead of water at 25° C. during the washing.

[0106] Example 2. A positive electrode active material was prepared in the same manner as in Example 1, except that the washing process was carried out for 30 minutes.

[0107] [Experimental example: EELS analysis and performance evaluation] Experimental example 1. EELS analysis The positive electrode active materials prepared in the examples and comparative examples were analyzed in EELS mode from the surface of the particles to 100 nm using a TEM device (FEI Ttitan G2 80-200 ChemiSTEM) to obtain spectra. Figure 1 shows the spectra obtained in Examples 1 and 2 and Comparative Examples 1 and 2, and Figure 2 shows the spectra obtained in Examples 1 and 2 and Comparative Example 3. After confirming the peak intensity at 853 eV and the peak intensity at 855.5 eV in the spectra, the results substituted into the formula 1 are shown in Table 1 below.

[0108] Experimental example 2. Evaluation of continuous charging (1) Manufacture of lithium secondary batteries The positive electrode active materials prepared in the examples and comparative examples, conductive material (carbon black), and binder (PVDF) were mixed in N-methylpyrrolidone in a weight ratio of 96:2:2 to prepare a positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum current collector, dried at 100°C, and then rolled to prepare a positive electrode.

[0109] An electrode assembly was prepared by interposing a porous polyethylene separator between the positive electrode and the lithium metal negative electrode, and the electrode assembly was placed inside a battery case, and an electrolyte was injected into the case to prepare a half-cell lithium secondary battery. The electrolyte was prepared by dissolving LiPF6 at a concentration of 1M in a mixed organic solvent in which ethylene carbonate / dimethyl carbonate / diethyl carbonate were mixed in a volume ratio of 3:4:3.

[0110] (2) Leakage current measurement The lithium secondary batteries thus prepared were each charged at 50° C. and 0.1 C to 4.7 V, and the leakage current value was measured while maintaining the battery in a CV state for 200 hours. The leakage current value generated over 200 hours was integrated and divided by 200 hours to obtain the average leakage current value, as shown in Table 1 below.

[0111] Experimental Example 3: Evaluation of gas generation rate Each of the lithium secondary batteries prepared in Experimental Example 2 was charged to SOC 100%, then disassembled, and the two charged positive electrodes were placed in a pouch together with 200 μl of electrolyte and stored at 70° C. for 14 days. After storage, the amounts of gases such as CO and CO2 generated in the lithium secondary batteries were measured and listed in Table 1 below.

[0112] [Table 1]

[0113] From the results in Table 1, it can be seen that when a cathode active material satisfying the value of Equation 1 of the present invention is applied to a battery after a step of washing with hot water over 90° C., the average leakage current value and the amount of gas generation can be significantly reduced. Considering that the only difference between the Examples and Comparative Examples is the washing conditions, and in particular, Example 2 in which the hot water washing time was extended to 30 minutes showed the smallest leakage current and gas generation amount, and Comparative Example 3 in which the hot water temperature was 70° C. showed poorer results than the Examples, it can be seen that such effects are due to the Ni oxidation number of the surface of the cathode active material being adjusted to be close to 2+ by adjusting the washing conditions, thereby suppressing the surface reactivity.

Claims

1. A first step of mixing a transition metal precursor containing 70 mol % or more of nickel based on the total moles of the transition metal and a lithium source material, and calcining the mixture to produce lithium transition metal oxide particles; and a second step of washing the lithium transition metal oxide particles with hot water at above 90°C; After the second step, an EELS analysis result on the surface of the lithium transition metal oxide particles satisfies the following formula 1: [Formula 1] I(853eV) / I(855.5eV)≧1 In the above formula 1, I(853 eV) is the peak intensity at 853±0.5 eV; I(855.5 eV) is the peak intensity shown at 855.5±0.5 eV.

2. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1 , wherein the transition metal precursor contains 80 mol % or more of nickel based on the total moles of the transition metals.

3. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the first step of firing is carried out at 750°C to 830°C.

4. After the second step, Ni is added to the surface of the lithium transition metal oxide particles. 2+ Ni 3+ The method for producing a positive electrode active material for a lithium secondary battery according to claim 1 , wherein the amount of the active material is greater than that of the active material.

5. 2. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the weight of the hot water used in the second step is 1 to 3 times the weight of the lithium transition metal oxide.

6. 2. The method for producing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the second step is performed for 10 to 30 minutes.

7. The lithium transition metal oxide particles contain at least 70 mol % of nickel based on the total moles of transition metals, The EELS analysis result of the surface of the lithium transition metal oxide particles satisfies the following formula 1: The lithium transition metal oxide is a positive electrode active material for a lithium secondary battery represented by the following Chemical Formula 1: [Formula 1] I(853eV) / I(855.5eV)≧1 In the above formula 1, I(853 eV) is the peak intensity at 853±0.5 eV; I(855.5 eV) is the peak intensity at 855.5±0.5 eV; [Chemical formula 1] Li a [Ni b Co c Mn d Q e ]O 2+f In the above Chemical Formula 1, a, b, c, d, e and f are 0.8≦a≦1.5, 0.8≦b<1.0, 0<c≦0.15, 0<d≦0.15, 0≦e≦0.05, b+c+d+e=1.0, −0.1≦f≦1.0, Q is one or more selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo.

8. The surface of the lithium transition metal oxide particles is coated with Ni 2+ Ni 3+ The positive electrode active material for a lithium secondary battery according to claim 7, wherein the positive electrode active material is contained in a larger amount than that of the positive electrode active material.

9. The positive electrode active material for a lithium secondary battery according to claim 7 , wherein the lithium transition metal oxide particles are secondary particles formed by agglomeration of a plurality of primary particles.

10. A positive electrode comprising a positive electrode active material layer containing the positive electrode active material for lithium secondary batteries according to claim 7.

11. A lithium secondary battery comprising the positive electrode according to claim 10.

Citation Information

Patent Citations

  • Active material for nonaqueous electrolyte secondary battery, and its manufacturing method

    JP2008258160A

  • Positive electrode active material, positive electrode, nonaqueous electrolyte battery, method of manufacturing positive electrode active material, method of manufacturing positive electrode, and method of manufacturing nonaqueous electrolyte battery

    JP2011119096A

  • Positive electrode material for lithium ion secondary battery, and lithium ion secondary battery

    JP2017216243A

  • Metal coposite oxides, method for preparing the same and lithium rechargeable battery containing the same

    KR1020160139098A

  • High-voltage lithium nickel cobalt manganese oxide precursor, method for preparing the same, and high-voltage lithium nickel cobalt manganese oxide cathode material

    KR1020200041978A