Antibacterial fabric

Combining POM fibers with biodegradable polyester resin and natural fibers through melt-spinning creates fabrics with enhanced antibacterial properties, addressing durability and dyeability issues, while maintaining natural fiber qualities.

JP7595935B2Active Publication Date: 2024-12-09PLAISIR CO LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2021085897
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-21
Publication Date
2024-12-09
Estimated Expiration
2041-05-21

AI Technical Summary

Technical Problem

Existing fibers, both natural and synthetic, lack inherent antibacterial properties, and methods to impart antibacterial properties often result in durability issues and discoloration, while POM fibers are difficult to use due to high crystallinity and poor dyeability.

Method used

Development of monolayer or multilayer fibers using an alloy of 50 to 100 wt% POM and 0 to 50 wt% biodegradable polyester resin, combined with natural fibers like silk, cotton, or wool, to create fabrics with excellent antibacterial properties and texture, utilizing a melt-spinning process to achieve fine fibers.

Benefits of technology

The resulting fabrics exhibit superior antibacterial performance, maintain the luxury feel and moisture retention of natural fibers, and are durable against bacterial growth, with improved dyeability and resistance to moth damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595935000001
    Figure 0007595935000001
  • Figure 0007595935000002
    Figure 0007595935000002
  • Figure 0007595935000003
    Figure 0007595935000003
Patent Text Reader

Abstract

To solve the problem of natural fibers that, though various antibacterial agents have been proposed because the natural fibers such as silk, cotton, wool and hemp which are materials for a woven fabric which have been commonly used for a long period of time basically have no antibacterial property and tend to cause deterioration such as yellowing, odor and corrosion, these antibacterial agents fall off by abrasion or washing to lose effect in an early stage.SOLUTION: There is provided a hybrid fabric or a nonwoven fabric in which a single layer or a multilayer synthetic fiber having a fiber diameter of 0.5 to 100 μm obtained from an alloy of 50 to 100 wt.% of a polyacetal resin (POM) and 0 to 50 wt.% of a biodegradable polyester resin (including POM alone) accounts for 30 to 80 wt.% of the whole fabric, and natural fibers such as silk, cotton, wool and hemp account for 20 to 70 wt.% of the whole fabric. The hybrid fabric or the nonwoven fabric has a high antimicrobial property, and does not lose its effect for a long period of time. The hybrid fabric or a nonwoven fabric can be formed into a product which has a good antibacterial property while maintaining touch feeling, high-class feeling, dyeability, reliability and the like of the natural fibers, and is economically acceptable.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an antibacterial textile in which single-layer or multi-layer synthetic fibers, consisting of 50-100 wt% POM and 0-50 wt% biodegradable polyester resin, account for 30 wt% to 70 wt% of the entire textile, and natural fibers such as silk, cotton, wool, and hemp account for 30 to 70 wt%. [Background technology]

[0002] Natural fibers or synthetic resin fibers are used as important products in various fields, not only in clothing, and are indispensable in our lives. Many of these products require antibacterial properties. However, natural fibers such as silk, wool, hemp, and cotton, which have been widely used as conventional fibers, and synthetic fibers such as polyester fibers, polyamide fibers, polyolefin fibers, acrylic fibers, and polyurethane fibers do not have antibacterial properties, and therefore various techniques for imparting antibacterial properties have been proposed. Patent Documents 1 and 2 disclose a technique for attaching an antibacterial agent to a fiber via a binder resin. Another method, such as a method of kneading an antibacterial agent into a resin, is disclosed in Patent Documents 3 and 4. Many antibacterial agents use silver ions, and those supported by inorganic compounds such as apatite, glass, zeolite, and clay compounds have been proposed. Although these methods are effective at first, the inorganic compounds supporting the antibacterial agent fall off due to wear and washing, and the effect of the antibacterial agent is lost early. In addition, they also have disadvantages such as discoloration due to processing steps after spinning and changes over time.

[0003] Many fibers themselves do not have antibacterial properties, and in order to make them antibacterial, the above-mentioned methods must be adopted, but POM is the only fiber whose resin itself has antibacterial properties, and it is usefully used in applications around water as injection molded or extrusion molded products. However, POM has excellent crystallinity, a fast crystallization rate, and a high degree of crystallization, so it has been considered difficult to use as a fiber. In recent years, there has been active research into using POM as a fiber. POM fiberization technology is disclosed in Patent Document 5, Patent Document 6, Patent Document 7, etc.

[0004] Patent Document 8 also discloses that POM is made into fibers in order to take advantage of its germ-repellent and antibacterial properties. However, as mentioned above, POM has a drawback in that it is difficult to stretch due to its fast crystallization rate and high crystallinity, making it difficult to make thin fibers. Another characteristic of POM is that it is difficult to dye. In order to use POM fibers for clothing applications, it is preferable that they can be easily dyed using conventional methods. Natural fibers such as silk, cotton, wool, and hemp have unique textures, touch, luster, and moisture retention, and are reliable because they have been used by humans for a long time. However, natural fibers have problems such as poor antibacterial, antifungal, and insect-repellent properties, and are sometimes very expensive. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 11-279952 [Patent Document 2] Japanese Patent Application Publication No. 10-325075 [Patent Document 3] Japanese Patent Application Publication No. 7-238421 [Patent Document 4] Japanese Patent Application Publication No. 7-3527 [Patent Document 5] Japanese Patent Application Publication No. 1-272821 [Patent Document 6] Japanese Patent Application Publication No. 8-144128 [Patent Document 7] Japanese Patent Application Publication No. 11-293523 [Patent Document 8] WO2016 / 147998A1 Summary of the Invention [Problem to be solved by the invention]

[0006] The object of the present invention is to create a never-before-seen textile by utilizing the antibacterial properties of POM fibers while taking advantage of the luxury, dyeability, moisture retention, and reliability of natural fibers. Fibers using antibacterial agents have problems with long-term antibacterial durability and discoloration. On the other hand, synthetic fibers made of POM or alloys of POM and specific biodegradable polyester resins have excellent antibacterial performance without the use of antibacterial agents. In particular, alloys of POM and PBS or PLA are easy to draw during spinning, and it is easy to produce fine fibers (fiber diameter 20 μm or less). Since fine fiberization is advantageous for exerting antibacterial properties, the above-mentioned fine fiberization properties of the alloy are desirable. [Means for solving the problem]

[0007] The present inventors have found that a hybrid fabric made of a single-layer or multi-layer fiber consisting of an alloy (including POM alone) of 50-100 wt% POM and 0-50 wt% specific biodegradable polyester resin, and a synthetic fiber with a fiber diameter of 0.5-100 μm combined with natural fibers such as silk, cotton, wool, hemp, and kenaf, has extremely excellent antibacterial properties and provides a new fabric having the texture, feel, luster, and moisture retention of natural fibers. As the biodegradable polyester resin to be used in combination with POM, PBS or a resin with a similar structure to PBS or PLA with a melt flow rate (MFR) of 4-30 g / 10 min is preferable. As the form of the fabric, it can be used in the form of knitted fabric, woven fabric, nonwoven fabric, web, etc., and can be easily used for clothing, bedding, interior decoration, etc.

[0008] The synthetic fibers made of POM or POM and a specific biodegradable polyester resin used by the present inventors can be produced by a normal melt spinning method. Single-layer or multi-layer synthetic fibers having a fiber diameter of 0.5 to 100 μm can be produced by melt spinning fibers having a fiber diameter of 20 to 500 μm and drawing them in one or multiple stages to have a fiber diameter of 0.5 to 100 μm. Polyacetal alloy resin fibers having high extensibility can be produced into ultrafine fibers with extremely high production efficiency using a normal melt spinning device.

[0009] That is, the present invention is as follows. 1) Antibacterial hybrid fabrics in which single-layer or multi-layer synthetic fibers with a fiber diameter of 0.5 to 100 μm obtained from an alloy of 50 to 100 wt% POM and 0 to 50 wt% biodegradable polyester resin (including POM alone) account for 30 wt% to 70 wt% of the entire fabric, and natural fibers account for 30 wt% to 70 wt% of the entire fabric.

[0010] 2) The antibacterial hybrid fabric according to claim 1, wherein the synthetic fibers account for 50 to 70% of the entire fabric, and the natural fibers account for 30 to 50% of the entire fabric.

[0011] 3) The hybrid fabric according to any one of claims 1 to 3, wherein the biodegradable polyester resin is one or more resins selected from the group consisting of PLA, PBS, polybutylene succinate adipate (PBSA), polyhydroxybutyrate (PHB), polyhydroxybutyrate-co-hydroxyvalerate (PHBV), polybutylene adipate-terephthalate (PBAT), and polyhydroxybutyrate-hydroxyhexanoate (PHBH).

[0012] 4) A hybrid fabric in which the synthetic fiber has a core-sheath structure, the core is any of polyolefin resin, polyester resin, polyamide resin, acrylic resin, polyurethane resin, or POM, and the sheath is 50-100wt% POM and 0-50wt% PBS with an MFR of 4-30g / 10min or a resin with a similar structure to PBS or PLA.

[0013] 5) The antibacterial hybrid woven or nonwoven fabric according to claim 1, which is composed of 50-90 wt% POM and 10-45 wt% PBS or a resin with a similar structure to PBS, or PLA, having a melt flow rate (MFR) of 4-30 g / 10 min. Effect of the Invention

[0014] The fibers of the present invention, which are mainly composed of polyacetal (POM) resin, have excellent antibacterial properties by themselves. Hybrid woven or nonwoven fabrics that combine 30wt%-70% POM fiber and natural fibers have the texture, feel, luster, and moisture retention of natural fibers. This makes it possible to provide excellent woven or nonwoven fabrics that combine the reliability that has long been used by humans with the antibacterial properties that are characteristic of POM fibers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] <Manufacturing methods for synthetic fibers> The method for producing the fibers made of POM or POM and a biodegradable polyester resin, for example, PBS or a resin with a similar structure to PBS, or an alloy of PLA, used in the antibacterial woven or nonwoven fabric of the present invention, can be produced by a known melt spinning method. That is, POM or POM and PBS or a resin with a similar structure, or POM and PLA, are melt-kneaded in advance in a predetermined ratio using a single-screw or twin-screw extruder to produce pellets. At this time, it is preferable to add 0.1 to 5 wt% of a carbodiimide compound to 100 wt% of PBS or a resin with a similar structure to PBS or an alloy of PLA. The synthetic fibers can have a single-layer or multi-layer structure. When a multi-layer structure is used, the outermost layer can be made of POM or a resin made of POM and a biodegradable polyester resin, for example, PBS or a resin with a similar structure to PBS, or an alloy of PLA, and the inner layer can be made of a polyolefin resin, a polyester resin, a polyamide resin, an acrylic resin, a polyurethane resin, or POM. Next, the obtained POM composition is melted in a spinning machine, extruded through a fiber die, and taken up by a winder to produce spun fibers.

[0016] Further, the spun fiber is stretched to adjust it to a desired fineness. The stretching can be performed by a known stretching method. Examples of the stretching method include wet stretching in a warm water bath, dry stretching in dry air or using a heated metal roll, and steam stretching in a superheated steam atmosphere heated to a temperature of 100°C or higher. Among these, when producing the polyacetal resin (POM) composition fiber of the present invention, it is preferable to perform wet stretching in a warm water bath at 40 to 100°C, preferably a warm water bath at 50 to 90°C. Alternatively, the extruded fiber can be brought into contact with a hot plate at 80 to 120°C to perform dry stretching.

[0017] Synthetic fibers obtained from POM fibers or alloys of POM and biodegradable polyester resin are produced as monofilament or multifilament fibers, but a method for producing ultrafine fibers is preferably a method for producing multifilament. In the production of multifilament, molten resin is extruded from multiple die holes and cooled, the obtained fiber is taken up by a take-up roll, and then the fiber is drawn by a drawing roll. Alternatively, melt-spun fibers with a fiber diameter of 20 to 100 μm can be taken up once and drawn to a fiber diameter of 0.5 to 20 μm by a separate drawing machine.

[0018] <Manufacturing method for hybrid fabrics made from synthetic and natural fibers> The POM fiber thus produced or the synthetic fiber obtained from an alloy of POM and biodegradable polyester resin is wound onto a bobbin, and natural fibers are used for the warp threads of the loom and POM fibers for the weft, or vice versa, to create a hybrid fabric in which POM and natural fibers are woven vertically and horizontally. The finished woven fabric will be more beautiful if the thickness (decitex) of the fibers used vertically and horizontally is roughly the same. The ratio of POM fibers to natural fibers can be adjusted by the number of bobbins used vertically and horizontally.

[0019] It is also possible to produce a single fiber by twisting together the desired number of synthetic fibers, obtained from POM fibers or an alloy of POM resin and biodegradable polyester resin, and natural fibers. By adjusting the number of POM fibers and natural fibers when feeding the fibers from each bobbin to a twisting machine, a yarn with the desired POM fiber ratio can be easily obtained. By weaving this yarn into cloth on a knitting machine, a fabric made of a blend of POM fibers and natural fibers can be produced.

[0020] <Manufacturing method for hybrid nonwoven fabrics of synthetic and natural fibers (1)> A hybrid nonwoven fabric of synthetic and natural fibers obtained from POM fiber or an alloy of POM resin and biodegradable polyester resin is first produced by melt spinning a resin composition containing 50-100wt% POM resin and 0-50wt% PBS or a resin with a similar structure to PBS or PLA with a melt flow rate (MFR) of 4-30g / 10min. The fiber is stretched to a size of 0.5-20μm and wound on a bobbin. A bobbin wound with natural fiber of the desired fineness is prepared separately, and the raw cotton is produced by introducing the raw cotton into a crimping machine in the desired ratio with POM fiber or POM alloy fiber. Next, the raw cotton is carded to align the fiber orientation direction, and then the fibers are entangled with each other using a needle punch device, thereby producing a nonwoven fabric of a mixture of synthetic and natural fibers.

[0021] <Melt-blown synthetic and natural fiber nonwoven fabric manufacturing method (2)> Alternatively, a resin composition consisting of 50-100wt% POM and 0-50wt% PBS or a resin with a similar structure to PBS or PLA resin with a melt flow rate (MFR) of 4-30g / 10min is heated and melted in an extruder, and as it is extruded from a nozzle it is blown away forcefully with compressed air and collected in a wire mesh collector. The POM or POM alloy fiber cotton thus obtained and separately prepared natural fiber cotton are introduced into a carding device in the desired ratio, the fibers are entangled to align the fiber orientation, and then the fibers are entangled with each other in a needle punch device to produce a nonwoven fabric.

[0022] When manufacturing a nonwoven fabric, the entire fabric is heated and compressed with a hot plate press after needle punching, and the synthetic fibers are thermally fused together to increase the tensile strength of the nonwoven fabric. In this case, the synthetic fibers are made into a core-shell type double-structure fiber, and the shell is made of POM resin and PBS resin or a resin with a similar structure to PBS or an alloy resin with 0-50 wt% PLA resin. The shells, which have a melting point 10 to 50°C lower than that of the POM resin, are thermally fused together, and a strong nonwoven fabric can be manufactured without melting the POM resin in the core. In particular, when PBS or a resin with a similar structure to PBS and an alloy of POM are used for the shell, the melting point difference with the POM core is 10°C to 50°C, so the tensile strength of the nonwoven fabric after heat fusion is large, and a strong nonwoven fabric can be manufactured.

[0023] <Manufacturing method of polyacetal resin> As the POM in the present invention, a POM homopolymer or copolymer can be used. The POM copolymer can be used alone or in the form of a mixture of POM copolymers having different types and amounts of comonomers. The POM copolymer has an oxyalkylene unit represented by the following formula (1) in addition to the oxymethylene unit in the molecule. Note that polyacetal resin and polyoxymethylene resin are synonymous.

[0024] [ka] (In the formula, R0 and R0' may be the same or different and each represents a hydrogen atom, an alkyl group, a phenyl group, or an alkyl group interrupted by one or more ether bonds, and m is an integer of 2 to 6.)

[0025] The alkyl group is an unsubstituted or substituted linear or branched alkyl group having 1 to 20 carbon atoms, preferably a linear or branched alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group include methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, t-butyl, pentyl, hexyl, decyl, dodecyl, and octadecyl. Examples of the substituent include a hydroxy group, an amino group, an alkoxy group, an alkenyloxymethyl group, and a halogen. Examples of the alkoxy group include methoxy, ethoxy, and propoxy. Examples of the alkenyloxymethyl group include allyloxymethyl.

[0026] The phenyl group is unsubstituted, or substituted with an unsubstituted or substituted alkyl group, an unsubstituted or substituted aryl group, or a halogen-substituted phenyl group, where aryl groups include phenyl, naphthyl, anthracyl, and the like.

[0027] The alkyl group interrupted by one or more ether bonds includes a group represented by the following formula (2). -CH2-O-(R3-O)P-R4 (2) (In the formula, R3 is an alkylene group, P represents an integer of 0 to 20, and R4 is a hydrogen atom, an alkyl group, a phenyl group, or a glycidyl group, and each (R3-O) unit may be the same or different.)

[0028] The alkylene group is a linear or branched, unsubstituted or substituted alkylene group having 2 to 20 carbon atoms, and examples thereof include ethylene, propylene, butylene, 2-ethylhexylene, etc. The alkylene represented by R1 is preferably ethylene or propylene.

[0029] It is preferable that R0 and R0' are the same and are a hydrogen atom. The oxyalkylene unit represented by formula (1) includes an oxyethylene unit, an oxypropylene unit, an oxybutylene unit, an oxypentylene unit, and an oxyhexylene unit, preferably an oxyethylene unit, an oxypropylene unit, and an oxybutylene unit, and more preferably an oxydimethylene unit, an oxytrimethylene unit, and an oxytetramethylene unit.

[0030] The polyoxymethylene (POM) copolymer may further include a unit represented by the following formula (3): -CH(CH3)-CHR5- (3) (wherein R5 is a group represented by the following formula (4)) -O-(R3-O)P-R6 (4) (In the formula, R6 is a hydrogen atom, an alkyl group, an alkenyl group, a phenyl group, or a phenylalkyl group, and R3 and P are as defined in formula (2).

[0031] The alkenyl group is a straight-chain or branched, unsubstituted or substituted alkenyl group having 2 to 20 carbon atoms, and examples thereof include vinyl, allyl, and 3-butenyl. The alkyl moiety and phenyl moiety in the phenylalkyl group are exemplified by the alkyl group and phenyl group described above. Examples of the phenylalkyl group include benzyl, phenylethyl, phenylbutyl, 2-methoxybenzyl, 4-methoxybenzyl, and 4-(allyloxymethyl)benzyl. In the present invention, when present, the alkenyl group and glycidyl group in the group represented by formula (2) or the alkenyl group in the group represented by formula (4) can be a crosslinking point in a further polymerization reaction, thereby forming a crosslinked structure.

[0032] The method for producing polyoxymethylene (POM) copolymer is not particularly limited, but may be, for example, a method of bulk polymerizing trioxane, which is a trimer of formaldehyde, and a comonomer, using a cationic polymerization catalyst such as boron trifluoride as necessary. Examples of the comonomer include cyclic ethers having 2 to 8 carbon atoms, such as ethylene oxide, 1,3-dioxolane, 1,3,5-trioxepane, and 1,3,6-trixocane; and cyclic formals having 2 to 8 carbon atoms, such as cyclic formals of glycol and cyclic formals of diglycol. These comonomers form an oxyalkylene unit represented by formula (1), in which R0 and R0' are the same and are hydrogen atoms.

[0033] In the present invention, the polyoxymethylene (POM) copolymer includes a binary copolymer and a multi-component copolymer. Therefore, as the POM copolymer of the present invention, a POM copolymer having an oxymethylene unit and an oxyalkylene unit represented by the above formula (1), a POM copolymer containing an oxymethylene unit, an oxyalkylene unit represented by the above formula (1) and a unit represented by the formula (3), and the above copolymer further having a crosslinked structure can be widely used. In the present invention, the unit represented by the formula (1) in which R0 and R0' are not simultaneously hydrogen atoms can be formed, for example, by copolymerizing a glycidyl ether compound or an epoxy compound, and the unit represented by the formula (3) can be formed, for example, by copolymerizing an allyl ether compound.

[0034] Examples of the glycidyl ether and the epoxy compound include, but are not limited to, epichlorohydrin; alkyl glycidyl formals such as methyl glycidyl formal, ethyl glycidyl formal, propyl glycidyl formal, and butyl glycidyl formal; diglycidyl ethers such as ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, hexamethylene glycol diglycidyl ether, raisoncinol diglycidyl ether, bisphenol A diglycidyl ether, hydroquinone diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and polybutylene glycol diglycidyl ether; triglycidyl ethers such as glycerin triglycidyl ether and trimethylolpropane triglycidyl ether; and tetraglycidyl ethers such as pentaerythritol tetraglycidyl ether.

[0035] Examples of allyl ether compounds include polyethylene glycol allyl ether, methoxypolyethylene glycol allyl ether, polyethylene glycol-polypropylene glycol allyl ether, polypropylene glycol allyl ether, butoxypolyethylene glycol-polypropylene glycol allyl ether, polypropylene glycol diallyl ether, phenylethyl allyl ether, phenylbutyl allyl ether, 4-methoxybenzyl allyl ether, 2-methoxybenzyl allyl ether, and 1,4-diallyloxymethylbenzene.

[0036] Among them, from the viewpoint of mass productivity and thermal stability, a polyoxymethylene (POM) copolymer obtained by adding 0.5 to 30 parts by weight, preferably 1 to 15 parts by weight, of a comonomer consisting of one or more cyclic ethers and / or cyclic formals other than trioxane to 100 parts by weight of trioxane is preferred. If the comonomer is 0.5 parts by weight or more, the heat resistance required for melt spinning is sufficient, and the POM copolymer is less likely to decompose or foam in the stagnant part inside the extruder or the spinning nozzle, and the processability is excellent. If the comonomer is 30 parts by weight or less, the yield when producing the POM copolymer is improved. In addition, the amounts of the glycidyl ether compound, the epoxy compound, and the allyl ether compound are not particularly limited, but preferably 0.05 to 20 parts by weight of the glycidyl ether compound, the epoxy compound, and the allyl ether compound can be added to 100 parts by weight of trioxane.

[0037] The polyacetal resin (POM) used in the present invention preferably has an MFR of 50 g / 10 min or less according to ISO 1133. The higher the MFR, the more suitable it is for obtaining thin threads by melt spinning, but if the MFR is 50 g / 10 min or less, there is an advantage that the mechanical properties (especially toughness) are excellent. The MFR can be adjusted by appropriately adjusting the amount of chain transfer agent in the polymerization reaction of POM.

[0038] <Manufacturing method of polybutylene succinate resin (PBS)> PBS can be produced by a known method using succinic acid and butanediol as raw materials. For example, it can be produced by a general melt polymerization method in which succinic acid and butanediol are subjected to an esterification reaction and / or transesterification reaction, followed by a polycondensation reaction under reduced pressure, or a known solution heating dehydration condensation method using an organic solvent. From the viewpoint of economy and simplicity of the production process, a method of producing PBS by melt polymerization in the absence of a solvent is preferred.

[0039] Examples of products (commercially available products) that can be used as PBS-based resins include Mitsubishi Chemical's "BioPBS" (registered trademark), Showa Denko's "Bionolle" (registered trademark), PBS resin manufactured by Shandong Fuwin New Material Co., Ltd., and BASF's polybutylene adipate terephthalate-based resin "Ecoflex" (registered trademark).

[0040] There are resins (resins with similar structures) that have a similar structure to the PBS-based resins. These resins with similar structures include polybutylene succinate adipate (PBSA), polyhydroxybutyrate (PHB), polyhydroxybutyrate-co-hydroxyvalerate (PHBV), polybutylene adipate-terephthalate (PBAT), and polyhydroxybutyrate-hydroxyhexanoate (PHBH). In the resin composition of the present invention, these resins can be treated as equivalent to polybutylene succinate resin (PBS).

[0041] The optimal MFR for PBS or similar structures is 4 to 30 g / 10 min. If the MFR is a high molecular weight of 4 g / 10 min or less, or if the MFR is a low molecular weight of 30 g / 10 min or more, the compatibility of the resin with POM is poor, and the fibers cannot be stretched to a high degree.

[0042] <Manufacturing method of polylactic acid resin (PLA)> PLA can be poly-L-lactic acid obtained by polymerizing only the L-form of lactic acid, poly-D-lactic acid obtained by polymerizing only the D-form, or poly-DL-lactic acid obtained by randomly polymerizing or block polymerizing the D-form and L-form. PLA can be produced by known methods. For example, in the lactide method generally used in industrial processes, lactic acid is heated and polymerized to obtain an oligomer, which is further decomposed by heating under reduced pressure to obtain lactide, which is a dimer of lactic acid, and this is polymerized in the presence of a metal salt catalyst to obtain PLA. Alternatively, in the direct polymerization method, PLA can be produced by heating lactic acid in a solvent such as diphenyl ether under reduced pressure and polymerizing it while removing water.

[0043] PLA is manufactured as a polymer by the American company Cargill Dow and supplied under the product name Nature Works. It is imported into Japan and processed by Kanebo Gohsen Co., Ltd., Kuraray Co., Ltd., Unitika Co., Ltd., and Mitsui Chemicals Co., Ltd., who sell it in a wide range of applications including packaging containers, agricultural and civil engineering products, compost-related products, sportswear, and bedding products. Unitika Co., Ltd. sells PLA under the registered trademark "Terramac."

[0044] In the present invention, 0.1 to 5 wt% of a carbodiimide compound can be added to 100 wt% of PBS, a resin with a similar structure to PBS, or a polylactic acid resin. The carbodiimide compound may be any compound having one or more carbodiimide groups in the molecule. For example, dicyclohexylcarbodiimide, dimethyl Carbodiimide, diisobutylcarbodiimide, dioctylcarbodiimide, t-butylisopropylcarbodiimide, diphenylcarbodiimide, di-t -butylcarbodiimide and the like.

[0045] In addition, additives that are commonly added to POM, PBS, or PLA, such as oxidation stabilizers, internal lubricants, nucleating agents, UV absorbers, colorants, etc., can be used as long as they do not impair the performance of the fiber.

[0046] An alloy of POM and PBS having an MFR of 4 to 30 g / 10 min or a resin with a similar structure, or an alloy of POM and PLA can be obtained by kneading using a single-screw or twin-screw extruder according to a known method.

[0047] The ratio of PBS or a resin with a similar structure, or the ratio of PLA is preferably 0 to 50 wt%. In particular, by making the fiber diameter 20 μm or less, preferably 10 μm or less, higher antibacterial properties can be obtained, but to make the fiber diameter thinner, an alloy with PBS or a resin with a similar structure, or an alloy with PLA, at 10 to 40 wt% of POM, can be used to obtain a fiber with excellent stretchability.

[0048] By adding 0.1 to 5 wt% of a carbodiimide compound to 100 wt% of PBS or a resin with a similar structure to PBS or PLA, the thermal stability of the polyacetal resin composition is improved, enabling stable thinning (drawing) of the fibers during the spinning process. This is particularly effective when the spinning temperature is high. If the amount is more than 5 wt%, no further effect can be expected and it becomes uneconomical.

[0049] In the multilayer fiber of the present invention, the resin used for the inner layer excluding the outermost layer, for example, the core layer of the fiber having a core-sheath structure, is polyolefin resin, polyester resin, etc. The resins are either polyolefin, polyamide, acrylic, polyurethane, or POM. Polyolefin resins include polypropylene and polyethylene. It is preferable that the polyester resin or polyamide resin is a copolymer having a melting point of 240° C. or less.

[0050] In the present invention, the natural fibers used together with the single-layer or multi-layer antibacterial fiber with a fiber diameter of 0.5 to 20 μm, which is made of a resin composition containing 50 to 100 wt% POM and PBS or a resin with a similar structure to PBS, or 0 to 50 wt% PLA, are representative plant fibers such as cotton and hemp, but also fruit fibers such as coconut, kenaf, rush, and wheat straw. Cellulosic regenerated fibers or semi-synthetic fibers such as rayon, cupra, polynosic, acetate, triacetate, and promix are also used. Representative animal fibers are silk and wool, but also feather fibers such as down and feathers can be used.

[0051] The antibacterial hybrid fabric of the present invention is less susceptible to insect damage and odor generation during storage. In addition, compared to 100% natural fiber fabrics, it is easier to handle, such as being easier to dry after washing. Generally, silk and wool fabrics are expensive and are often stored for long periods of time, and require careful attention to insect control, but the hybrid fabric of the present invention is easy to maintain. In addition, natural fibers such as cotton and linen are the most comfortable materials to wear in the summer because they absorb sweat easily and have excellent ventilation, but there is a problem that Moraxella bacteria, which cause odor, are easily propagated. The hybrid fabric of the present invention can prevent the generation of this odor-causing bacteria.

[0052] A new effect of the present invention is the change in the texture of the woven fabric. This texture is what is called the touch or feel, and is difficult to evaluate objectively because it is extremely sensory. However, universal values ​​can be obtained by measuring the bending, tensile, shear strength, compressive strength, and surface roughness of the woven fabric. In particular, the measurement method for the drape coefficient is specified in JIS L1096, and the stiffness and softness of the fabric can be expressed by the drape coefficient. For example, the drape coefficient of silk is 0.2 to 0.4, but a woven fabric in which it is blended with about 50% POM fiber has a drape coefficient of 0.7 to 0.9, and the fabric has a slightly crisp feel and is suitable for casual wear. The same tendency occurs when the natural fiber is wool. The drape coefficient of cotton and linen does not change much when blended with POM, but it becomes smooth to the touch. Such a change in feel is considered to be useful for developing uses for fibers that are different from conventional uses. When combining silk and POM fibers to achieve both antibacterial properties and a casual feel, it is desirable for the synthetic fibers to make up 40-60% of the total fabric, and the natural fibers to make up 40-60% of the total fabric. A similar ratio is also recommended for wool, an animal fiber. This blend ratio gives the fabric an easy-to-handle, casual feel while retaining the luxury of natural fibers. The combination of POM fiber and vegetable fibers such as cotton or hemp does not have a large effect on the drape coefficient, but the difference in texture is apparent when viewed visually or by touch. On the other hand, the antibacterial properties drop sharply when the POM fiber content is 30% or less, so the preferable range for antibacterial properties and texture is 50% to 70% POM fiber and 30% to 50% vegetable natural fibers. The drapeability of nonwoven fabrics is more influenced by the thickness of the fibers, the entanglement of the fibers, or the thermal fusion of the fibers than by the combination of fiber materials, and therefore the drapeability of nonwoven fabrics was not measured in the present invention. EXAMPLES

[0053] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to the examples shown below as long as the gist of the present invention is not exceeded. <Examples and Comparative Examples>

[0054] <Raw materials> Polyacetal resin (POM) is POM-1: Iupital F20-02 (manufactured by Mitsubishi Engineering Plastics) POM-2: Iupital F30-03 (manufactured by Mitsubishi Engineering Plastics Corporation) was used. POM-3: Iupital F40-03 (manufactured by Mitsubishi Engineering Plastics Corporation) was used. Polybutylene succinate (PBS) resin is PBS-1: Bio BPS FZ71 (manufactured by Mitsubishi Chemical) with MFR of 22 PBS-2: Bio BPS FZ91 (manufactured by Mitsubishi Chemical) with MFR of 5 PBS-3: Bionolle #1001 (Showa Denko) with MFR of 1.5 PBS-4: Bio BPS FZ71 with 3% by weight calcium stearate The mixture was melt extruded at a resin temperature of 200°C and the MFR was adjusted to 35. AONILEX (manufactured by Kaneka) was used as the PHBH resin. The polylactic acid resin (PLA) used was Terramac TP-4000 (manufactured by Unitika). The polypropylene (PP) resin is Prime Polypro F-730NV (manufactured by Prime Polymer), and the polyester (PET) resin is MA-1. The polyamide (PA) resin used was 5034 (manufactured by Ube Industries), a 6 / 66 copolymer. The carbodiimide compound used was Carbodilite LA-1 (manufactured by Nisshinbo Chemical).

[0055] <Preparation of resin composition for evaluation> The synthetic resin samples for evaluation were commercially available POM, which was dried with hot air at 120°C for 4 hours, then placed in the spinning machine hopper and melt-spun. For resins with similar structure or alloys of PLA, the components shown in Tables 1 and 2 are weighed, then dry blended, and placed in the hopper of a twin-screw kneader. The mixture was melt-kneaded at 205°C to produce pellets of the desired composition. The pellets were dried and then used in a spinning experiment. Carbodiimide was used as a stabilizer. LA-1 was added at 1.0 wt% to PBS resin, resin with a similar structure to PBS, or polylactic acid resin.

[0056] <Melt spinning> For melt spinning, a spinning machine consisting of two vertical single-screw extruders (A and B) was used. When producing a single-layer fiber, the same material was fed into each of A and B and extruded. When producing a double-layer fiber, different materials were fed into extruders A and B, allowing the production of fibers with different properties in the core-shell structure. Extruders A and B have a screw with an axis diameter of 25 mm and a heating cylinder around it, and the molten resin is guided to the die through a flow path connected to the die. The die hole has 24 holes arranged in a circle, and each die hole has a double structure. The molten resin is guided from extruder A to the inner die hole and from extruder B to the outer die hole, and the core-shell molten resin is discharged in the form of a thread. The outer diameter of the die hole is 300 μm, and the inner diameter of the core part is 200 μm. The extruder screw, cylinder, inner surface of the flow path through which the molten resin flows, and inner surface of the die are chrome plated.

[0057] The temperature of the extruder and the die can be controlled to 160 to 250°C depending on the melting temperature of the resin used. The molten resin discharged from the nozzle is taken up by five rollers, and usually, the rotation speed of each roller can be increased in sequence to be stretched. In this case, it is effective to control the surface temperature of the rollers to 80 to 120°C. In this way, core-shell fibers with a fiber diameter of 20 to 100 μm were produced. In the case of single-layer fibers, the same material was fed into extruders A and B and spun. In the case of multi-layer fibers, different materials were fed into extruders A and B. Multi-layer fibers with a fiber diameter of 20 to 100 μm and a core-sheath structure in which the resin fed into A is the core and the resin fed into B is the sheath were produced.

[0058] The fiber was then heated again and stretched to produce a fiber with a diameter of 0.5 to 20 μm. The fiber wound on the bobbin was introduced into a stretching device, where the stretch ratio was adjusted by the difference between the speed of the rotating roll before the stretching heating device and the rotation speed and diameter of the take-up roll after the heating device. The heating device was a method in which the fiber was passed through an air heater at 100 to 140°C. Other methods such as passing the fiber through a hot water bath or oil bath are also effective. The heating device may be a single stage, or multiple stages may be used to increase the stretching degree to the desired level.

[0059] <Preparation of hybrid fabric> Natural fibers such as silk, cotton, wool, and hemp that are used in combination with single-layer or multi-layer fibers produced by spinning POM or POM alloy resin can be commercially available. The fineness of the fibers is preferably approximately the same as that of the synthetic resin, as this will result in a smooth woven fabric. Hybrid fabrics of POM or POM alloy resin and natural fibers can be manufactured by using each fiber for the warp or weft, or by twisting POM resin or POM alloy resin and natural fibers into a single thread and weaving it. The ratio of each fiber is adjusted so that synthetic fibers account for 30wt% to 70wt% of the entire fabric, and natural fibers such as silk, cotton, wool, and hemp account for 30wt% to 70wt% of the entire fabric.

[0060] <Preparation of hybrid nonwoven fabric> There are two methods for manufacturing nonwoven fabrics: melt spinning and melt blowing. The melt spinning method is suitable for precisely controlling the fiber diameter, whereas the melt blowing method allows nonwoven fabrics to be manufactured relatively inexpensively. However, the resin used in the melt blowing method must have high fluidity. In the melt spinning method, a core-shell double-structure fiber is melt spun using a resin composition with POM as the core, 50-100wt% POM as the shell, and PBS or a resin with a similar structure to PBS or 0-50wt% PLA with a melt flow rate (MFR) of 4-30g / 10min. The fiber is stretched to a size of 0.5-20μm and wound on a bobbin. A bobbin wound with natural fiber of the desired fineness is prepared separately, and the POM core-shell fiber and natural fiber are introduced into a crimper in the desired ratio to produce raw cotton. Next, the raw cotton is carded to align the fiber orientation, then the fibers are entangled with each other using a needle punch device, and finally, the fabric is heated and compressed at 100 to 150°C to produce a nonwoven fabric. In the melt-blowing method, a resin composition consisting of POM resin as the core, 50-100wt% POM as the shell, and PBS or a resin with a similar structure to PBS or 0-50wt% PLA with a melt flow rate (MFR) of 4-30g / 10min is used, which is heated and melted in an extruder, blown out vigorously with compressed air as it is extruded from a nozzle, and collected with a collector made of wire mesh. The resulting core-shell type POM fiber cotton and a separately prepared natural fiber cotton are introduced into a carding device in the desired ratio, the fibers are entangled to align the fiber orientation direction, and then the fibers are entangled with each other in a needle punch device to produce a nonwoven fabric. The resulting cotton is then heat-compressed at 100℃ to 150℃ for 1 minute to produce a nonwoven fabric.

[0061] <Measuring method for texture> The hand feel was measured using the JIS L1096 bending resistance measurement method (drape coefficient method). First, five circular test pieces with a diameter of 254 mm were cut out from the hybrid woven fabric or nonwoven fabric, and a hole with a diameter of 10 mm was drilled in the center of each test piece. Next, the test pieces were placed with the measurement side facing up on the sample stage (diameter 127 mm) of the drape tester, fixed with the sample presser, and the sample stage was vibrated up and down three times, then left for one minute, and the drape shape area at that time was measured for both the front and back of the sample piece. The drape coefficient was calculated using the following formula, and the average value for the front and back was calculated and rounded to three decimal places. Df=Ad-S1 / S2-S1 Df: Drape coefficient Ad: Vertical projection area of ​​the sample stage (drape shape area) (mm 2 ) S1: Area of ​​the sample stage (mm 2 ) S2: Area of ​​sample (mm 2 ) Natural silk has a drape coefficient of 0.2 to 0.4, which is soft and smooth to the touch. On the other hand, hybrid fabrics made with silk and POM fibers in a 50:50 ratio for the warp and weft have a drape coefficient of 0.7 to 0.9, which is firm and crisp to the touch. The drape coefficient is multiplied by 100 and expressed as a percentage.

[0062] <Evaluation of antibacterial properties of textiles> The bacterial liquid absorption method is specified in JIS L1902. This method is a test that simulates the wearing of clothing, and evaluates the antibacterial effect by comparing the growth of bacteria on a standard cloth and a test cloth. The test bacteria used were (1) Staphylococcus aureus NBRC12732 for Staphylococcus aureus and (2) Escherichia coli NBRC3301 for Escherichia coli, and samples were sterilized in an autoclave before testing. The inoculum concentration (CFU / ml) was 1.5*10 5 The antibacterial properties of the fibers are expressed as the antibacterial activity value [A]. This antibacterial activity value is calculated by the following formula (1). A=(LogCb-LogCa)-(LogC2-LogC1) (1 set) Ca: Viable bacteria count on standard cloth Cb: Viable bacteria count on standard cloth after 18 hours of incubation C1: Number of viable bacteria in the evaluation sample C2: Number of viable bacteria in the evaluation sample after 18 hours of incubation

[0063] <Result> Samples 1-a to 1-i in Table 1-1 used in the examples show hybrid woven fabrics of POM fiber with silk, cotton, wool, and linen, and Table 1-2 shows the results of antibacterial tests on these. The POM fiber used was either POM alone or POM alloy resin fiber. All of them have a high antibacterial activity value [A] of 5 or more. According to the JIS standard, an [A] of 2 or more is considered an antibacterial product, and according to the SEK standard, an [A] of 2.2 or more is considered an antibacterial product, and these products show antibacterial properties far superior to those values.

[0064] [Table 1-1]

[0065] [Table 1-2]

[0066] Examples, 2-a to 2-i in Table 2-1 show hybrid nonwoven fabrics of POM fiber and silk, cotton, wool, or hemp, and Table 2-2 shows the antibacterial test results. 2-a to 2-i in Table 2-1 show raw cotton produced by introducing POM or POM alloy fiber of the present invention produced by melt spinning method and natural fiber in a desired ratio into a crimping machine. Next, the raw cotton was aligned in the fiber orientation direction using a carding device, then the fibers were entangled with each other using a needle punch device, and finally, nonwoven fabric was produced by heating and compressing at 100°C to 150°C. The antibacterial test results of the nonwoven fabrics produced by blending these silk, cotton, wool, and hemp yarns are shown in Table 2-2. All of them show high antibacterial activity values ​​[A]. The POM alloy resin used for the shell has a POM resin blend ratio of 50-90wt%, PBS with a melt flow rate (MFR) of 4-30g / 10min or a resin with a similar structure to PBS or PLA at 10-45wt%, and contains a carbodiimide compound in the range of 0-5wt% as a stabilizer. A commercially available POM resin was used for the core.

[0067] [Table 2-1]

[0068] [Table 2-2]

[0069] The sample woven fabrics used in the comparative examples are shown in Table 3-1, and the antibacterial test results are shown in Table 3-2. Comparative examples 2-a to 2-f in Table 3-1 show hybrid fabrics in which POM or POM alloy fibers account for 30% or less of the entire fabric, and the antibacterial test results are shown in Table 3-2. 3-g and 3-h in Table 3-1 use an alloy of POM and PBS resin for the weft, but when PBS with an MFR of 4 or less or 30g / 10min or more was used, the fibers broke. When POM fiber is used at 70% or more of natural fiber, the characteristics such as texture unique to natural fiber are reduced, and the object of the present invention of imparting antibacterial properties of polyacetal fiber while taking advantage of the luxurious feel, dyeability, moisture retention, and reliability of natural fiber, which is the object of the present invention, is not achieved. In order to maintain the luxurious feel and texture of natural fiber, it is desirable to blend at least 30% or more of natural fiber, preferably 40% or more. On the other hand, the antibacterial properties of the woven fabric are expressed when the blending ratio of POM fiber is at least 30% or more, preferably 50% or more. Considering the compatibility of texture and antibacterial properties, the desirable ratio is 50 to 70% synthetic fiber and 30 to 50% natural fiber.

[0070] [Table 3-1]

[0071] [Table 3-2]

[0072] Table 4-1 shows nonwoven fabrics produced by introducing POM resin or POM alloy fiber cotton produced by the melt-blowing method and natural fiber cotton into a carding machine in the desired ratio, entangling the fibers to align the fiber orientation direction, and then entangling the fibers with a needle punching machine. The obtained cotton was heat-compressed at 100°C to 150°C for 1 minute to produce nonwoven fabrics. Table 4-2 shows the results of antibacterial tests, but if the POM or POM alloy fiber content is 30% or less, there is no antibacterial property. The texture of nonwoven fabrics is more difficult to judge than that of woven fabrics, and the difference in drape coefficient is smaller, but if antibacterial properties are also taken into consideration, as with woven fabrics, 50 to 70% synthetic fiber and 30 to 50% natural fiber are preferable.

[0073] [Table 4-1]

[0074] [Table 4-2]

Claims

1. An antimicrobial hybrid fabric comprising synthetic and natural fibers, The synthetic fiber is obtained from an alloy (including POM alone) of 50 to 100 wt % polyacetal resin (hereinafter referred to as POM) and 0 to 50 wt % biodegradable polyester resin, It is a single-layer or multi-layer synthetic fiber with a fiber diameter of 0.5 to 100 μm, the natural fibers are silk, linen, cotton, or wool; The synthetic fibers constitute 50 wt % to 70 wt % of the entire fabric, and The antibacterial hybrid fabric, wherein the natural fibers are 30 wt % to 50 wt % of the entire fabric.

2. The hybrid fabric according to claim 1, wherein the biodegradable polyester resin is one or more resins selected from the group consisting of polylactic acid (hereinafter referred to as PLA), polybutylene succinate (hereinafter referred to as PBS), polybutylene succinate adipate (PBSA), polyhydroxybutyrate (PHB), polyhydroxybutyrate-co-hydroxyvalerate (PHBV), polybutylene adipate-terephthalate (PBAT), and polyhydroxybutyrate-hydroxyhexanoate (PHBH).

3. The synthetic fiber has a core-sheath structure, The core is any one of polyolefin resin, polyester resin, polyamide resin, acrylic resin, polyurethane resin, and POM, 3. The hybrid fabric according to claim 1 or 2, wherein the sheath is obtained from an alloy of 50 to 100 wt % of POM and 0 to 50 wt % of a biodegradable polyester resin (including POM alone).

4. The synthetic fiber, The composite is obtained from an alloy of 50 to 90 wt % of the POM and 10 to 45 wt % of the biodegradable polyester resin, The biodegradable polyester resin is PBS or a resin with a similar structure to PBS, or PLA, The melt flow rate (MFR) of the PBS or a resin having a structure similar to that of the PBS is 4 to 30 g / 10 min; The antibacterial hybrid fabric according to claim 1, wherein the resin having a similar structure to PBS is one or more resins selected from the group consisting of polybutylene succinate adipate (PBSA), polyhydroxybutyrate (PHB), polyhydroxybutyrate-co-hydroxyvalerate (PHBV), polybutylene adipate-terephthalate (PBAT), and polyhydroxybutyrate-hydroxyhexanoic acid (PHBH).

Citation Information

Patent Citations

  • Cotton, viscose and flax airflow fabric

    CN210362749U

  • Extremely drawn linear material of polyoxymethylene having improved flexing resistance

    JP1989272821A

  • Production of modified polyester fiber

    JP1995003527A

  • Method for producing antimicrobial polyester fiber

    JP1995238421A

  • Conjugate fiber and nonwoven fabric and knitted fabric

    JP1996144128A