Method for manufacturing solid-state battery and solid-state battery
By incorporating buried layers with controlled conductivity at the ends of electrodes, the manufacturing process for solid-state batteries is enhanced to prevent short circuits, ensuring high performance and quality.
Patent Information
- Application Number
- JP2020030269
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-26
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2040-02-26
AI Technical Summary
In the manufacturing of solid-state batteries, misalignment and deformation during thermocompression bonding can lead to short circuits between the electrodes, reducing the performance and quality of the battery.
The electrodes are designed with buried layers of lower electronic conductivity at their ends, ensuring a specific ratio of the buried layer area to the main electrode surface, which supports the ends of the electrodes and prevents direct contact during lamination and thermocompression, thereby suppressing short circuits.
This design effectively reduces the occurrence of short circuits and maintains consistent performance by stabilizing the electrode structure during manufacturing, resulting in high-quality solid-state batteries.
Smart Images

Figure 0007596071000007 
Figure 0007596071000008 
Figure 0007596071000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a solid-state battery and a solid-state battery. [Background technology]
[0002] 2. Description of the Related Art Solid-state batteries having a structure in which an electrolyte layer is provided between a pair of electrodes, a positive electrode and a negative electrode, are known. Regarding such solid-state batteries, for example, Patent Document 1 describes a technique in which one or both ends of an electrode and an electrolyte layer are covered with an insulating material and then pressurized to prevent deformation or falling off of the ends, contact or short circuit at the ends of the electrodes sandwiching the electrolyte layer. Patent Document 2 describes a technique in which the thickness of the electrodes is continuously increased from the ends toward the center to prevent breakage and film tearing of laminate cells by hydrostatic pressing. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-38425 A [Patent Document 2] JP 2014-116136 A Summary of the Invention [Problem to be solved by the invention]
[0004] In a solid-state battery including a laminate of an electrolyte layer and an electrode pair sandwiching the electrolyte layer, during the manufacturing process, the electrodes may come into contact with each other and cause a short circuit due to misalignment of the electrode pair sandwiching the electrolyte layer, deformation or poor compression bonding during thermocompression bonding, deformation during firing, and the like.
[0005] In one aspect, the present invention aims to realize a solid-state battery in which the occurrence of short circuits is suppressed. [Means for solving the problem]
[0006] In one embodiment, the method includes forming a first electrode including a first electrode layer and a second electrode layer facing the first electrode layer, the first electrode being provided with a first buried layer having a lower electronic conductivity than the first electrode layer and the second electrode layer, between the first electrode layer and the second electrode layer and around a first portion where the first electrode layer and the second electrode layer are in contact with each other. and the ratio of the area of the first buried layer to the area of the main surface of the first electrode is 4.9% or more and 7.8% or less. A method for manufacturing a solid-state battery is provided.
[0007] In one embodiment, the semiconductor device includes a first electrode having a first region and a second region surrounding the first region, and a first buried layer provided in the second region excluding a part of a side end surface of the first electrode and having a lower electronic conductivity than the first electrode. and the ratio of the area of the first buried layer to the area of the main surface of the first electrode is 4.9% or more and 7.8% or less. A solid-state battery is provided. Effect of the Invention
[0008] In one aspect, it will be possible to realize a solid-state battery in which the occurrence of short circuits is suppressed. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a diagram illustrating one step of a method for manufacturing a solid-state battery. [Diagram 2] FIG. 2 is a diagram illustrating an example of an electrode of a solid-state battery. [Diagram 3] 10A to 10C are diagrams illustrating another example of electrodes of a solid-state battery. [Figure 4] 11A to 11C are diagrams illustrating an example of a method for forming a positive electrode part. [Diagram 5] 11A to 11C are diagrams illustrating an example of a method for forming a negative electrode part. [Figure 6] FIG. 1 is a diagram (part 1) for explaining one configuration example of a solid-state battery. [Figure 7] FIG. 2 is a diagram (part 2) for explaining a configuration example of a solid-state battery. [Figure 8] 11A to 11C are diagrams showing an example of a process for forming a positive electrode part in a cross section perpendicular to the terminal surface. [Figure 9] 11A to 11C are diagrams showing an example of a process for forming a negative electrode part in a cross section perpendicular to the terminal surface. [Figure 10] 1A to 1C are diagrams showing an example of a process for forming a green laminate in a cross section perpendicular to the terminal surface. [Figure 11] 1A to 1C are diagrams illustrating an example of a cutting step and a heat treatment step in a cross section perpendicular to a terminal surface. [Figure 12] 11A to 11C are diagrams showing an example of a process for forming a positive electrode part in a cross section parallel to the terminal surface. [Figure 13] 11A to 11C are diagrams showing an example of a process for forming a negative electrode part in a cross section parallel to the terminal surface. [Figure 14] 1A to 1C are diagrams showing an example of a process for forming a green laminate in a cross section parallel to the terminal surfaces. [Figure 15] 11A to 11C are diagrams illustrating an example of a cutting step and a heat treatment step in a cross section parallel to the terminal surface. [Figure 16] FIG. 2 is a diagram illustrating an electrode configuration of a solid-state battery. [Figure 17] FIG. 1 is a diagram showing an example of a cross-sectional observation result of a solid-state battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In recent years, with the rapid development of information-related devices such as personal computers, mobile phones, and electric vehicles, as well as communication devices and transportation-related devices, the development of batteries as their power sources has become important. Among various types of batteries, secondary batteries such as lithium-ion batteries and solid-state batteries have attracted attention due to their safety, high energy density, and the ability to be charged and discharged.
[0011] A lithium-ion battery generally has a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, and an electrolyte layer provided between them. Lithium-ion batteries that use a flammable organic electrolyte as the electrolyte layer provided between the positive electrode and the negative electrode require safety measures to prevent leakage, short circuit, overcharging, etc. High-capacity, high-energy density lithium-ion batteries require further improvement in safety. Therefore, research and development of solid-state batteries using oxide-based solid electrolytes or sulfide-based solid electrolytes as electrolytes is being conducted.
[0012] One process in the manufacturing method of a solid-state battery is a doctor blade method or a screen printing method. In the doctor blade method, ceramic powder such as inorganic oxide before firing is mixed with binders such as polyvinyl alcohol (PVA), polyvinyl butyral (PVB), polyvinylylene fluoride (PVDF), acrylic resin, or ethyl methyl cellulose, and solvents to form a slurry, which is then coated or printed to produce a thin green sheet. Positive electrode sheets, negative electrode sheets, and solid electrolyte sheets are produced in this way, and then stacked and sintered.
[0013] In screen printing, a paste is prepared by mixing ceramic powder such as inorganic oxide before firing with a binder such as PVA, PVB, PVDF, acrylic resin or ethyl methyl cellulose, and a solvent. A screen mask is placed on the object to be printed, and the paste is placed on top of it. When the paste is stretched from the edge of the screen mask with a squeegee and pressed against the object, the paste fills the holes not covered by the screen mask and is transferred onto the object.
[0014] A solid-state battery can be manufactured, for example, by laminating a positive electrode, a negative electrode, and an electrolyte layer using a solid electrolyte, or further a current collector layer, thermocompressing them, and co-firing them. In the case of a solid-state battery that utilizes lithium ion conduction, lithium ions are conducted from the positive electrode to the negative electrode through the electrolyte layer during charging and are taken in, and lithium ions are conducted from the negative electrode to the positive electrode through the electrolyte layer during discharging. In a solid-state battery, charging and discharging operations are realized by such lithium ion conduction. The parameters of the positive electrode and the negative electrode that contribute to the performance of the manufactured solid-state battery include lithium ion conductivity and electronic conductivity, and the parameter of the electrolyte layer includes lithium ion conductivity.
[0015] In a solid-state battery including a laminate of an electrolyte layer and a positive electrode and a negative electrode sandwiching the electrolyte layer, during manufacturing, there may occur a misalignment between layers of the laminate or between internal components of each layer, deformation or poor compression during thermocompression, deformation during firing, etc. If such a phenomenon occurs, there is a risk that the positive electrode and the negative electrode will come into contact with each other, causing a short circuit inside the solid-state battery. Such a short circuit will lead to a deterioration in the performance and quality of the solid-state battery.
[0016] Therefore, the following method is used to suppress the occurrence of short circuits inside the solid-state battery, thereby realizing a high-performance, high-quality solid-state battery. [Manufacturing solid-state batteries] Fig. 1 is a diagram for explaining one step of a method for producing a solid-state battery, in which Fig. 1(A) to Fig. 1(D) each show a schematic cross-sectional view of a main part of each step of electrode formation in the production of a solid-state battery.
[0017] 1(A), a first electrode layer 10 is formed. The first electrode layer 10 is formed, for example, in a shape in which the thickness of an inner portion 10b is greater than the thickness of an end portion 10a in a cross-sectional view.
[0018] The first electrode layer 10 is formed, for example, by printing a paste prepared for the electrode layer 10 on a predetermined printing target (not shown) such as an electrolyte layer by screen printing, and drying the paste. The paste for the first electrode layer 10 contains, for example, an active material, a solid electrolyte, a conductive assistant, a binder, a solvent, and the like.
[0019] 1(B), a first buried layer 11 is formed in an end portion 10a of the first electrode layer 10. The first buried layer 11 is formed so as to bury the end portion 10a, which is thinner than an inner portion 10b of the first electrode layer 10, in a cross-sectional view, for example.
[0020] The first buried layer 11 is made of a material having a lower electronic conductivity than the active material contained in the first electrode layer 10 (and the second electrode layer 20 described later), such as an insulating material or a solid electrolyte. -2 S / cm~1×10 -5 The first buried layer 11 is made of a material with an electronic conductivity of 1×10 -9 S / cm~1×10 -10 S / cm material is used.
[0021] The first buried layer 11 is formed, for example, by printing a paste prepared for the buried layer 11 on the region of the first electrode layer 10 excluding the inner portion 10b (on the end portion 10a or on the end portion 10a and its outer region) using a screen printing method, and then drying. The paste for the first buried layer 11 contains, for example, a solid electrolyte, a binder, a plasticizer, a dispersant, a diluent, and the like.
[0022] After the first buried layer 11 is formed, the second electrode layer 20 is formed as shown in Fig. 1(C) . The second electrode layer 20 is formed, for example, in a shape in which the thickness of the inner portion 20b is thicker than the thickness of the end portion 20a in a cross-sectional view.
[0023] The second electrode layer 20 is formed, for example, by printing a paste prepared for the electrode layer 20 on the inner portion 10b of the first electrode layer 10 and on the first embedded layer 11 formed on its end portion 10a using a screen printing method, and then drying the paste. The paste for the second electrode layer 20 contains, for example, an active material, a solid electrolyte, a conductive assistant, a binder, a solvent, and the like.
[0024] Here, the first electrode layer 10 and the second electrode layer 20 are either electrode layers that will become a part of the positive electrode of a solid-state battery, or both electrode layers that will become a part of the negative electrode of a solid-state battery. That is, the first electrode layer 10 and the second electrode layer 20 both contain a positive electrode active material, or both contain a negative electrode active material. The first electrode layer 10 and the second electrode layer 20 are provided so that their inner portions 10b and 20b are in contact with each other. The first embedded layer 11 is provided around the portion 3 where the first electrode layer 10 and the second electrode layer 20 are in contact with each other.
[0025] 1(D), after the second electrode layer 20 is formed, a second buried layer 21 is formed in an end portion 20a of the second electrode layer 20. The second buried layer 21 is formed so as to bury the end portion 20a, which is thinner than an inner portion 20b of the second electrode layer 20, in a cross-sectional view, for example.
[0026] The second buried layer 21 is made of a material having a lower electronic conductivity than the active material contained in the second electrode layer 20 (and the third electrode layer described below), such as an insulating material or a solid electrolyte. -2 S / cm~1×10 -5 The second buried layer 21 is made of a material with an electronic conductivity of 1×10 -9 S / cm~1×10 -10 S / cm material is used.
[0027] The second buried layer 21 is formed, for example, by printing a paste prepared for the buried layer 21 on a region of the second electrode layer 20 excluding the inner portion 20b (on the end portion 20a or on the end portion 20a and its outer region) using a screen printing method, and drying the paste. The paste for the second buried layer 21 contains, for example, a solid electrolyte, a binder, a plasticizer, a dispersant, a diluent, and the like.
[0028] The above-mentioned steps are repeated for the number of layers required as the positive electrode or negative electrode (hereinafter, either or both are simply referred to as "electrodes") of the solid-state battery, for example, for the number of layers that will provide the amount of active material and film thickness required for the electrodes of the solid-state battery to be manufactured. For example, when a third electrode layer (not shown) is formed on the second electrode layer 20 so as to contact the inner portion 20b thereof, a second embedded layer 21 is provided around the portion where they contact.
[0029] An electrode 1 (two electrode layers 10, 20 are shown as an example in FIG. 1(D)) of a solid-state battery is formed by the steps shown in FIG. 1(A) to FIG. 1(D). In manufacturing a solid-state battery, the positive and negative electrodes formed by the above-mentioned steps are stacked with an electrolyte layer (for example, the base of the first electrode layer 10) interposed therebetween, and then thermocompression bonded.
[0030] In the above process, the first buried layer 11 is provided at the end 10a of the first electrode layer 10, and the second electrode layer 20 is provided thereon. As a result, the gap between the end 10a of the first electrode layer 10 and the end 20a of the second electrode layer 20 is filled with the first buried layer 11, and the end 20a of the second electrode layer 20 is supported by the first buried layer 11. When the third electrode layer is formed, the gap between the end 20a of the second electrode layer 20 and the end of the third electrode layer is filled with the second buried layer 21 provided at the end 20a of the second electrode layer 20, and the end of the third electrode layer is supported by the second buried layer 21.
[0031] In this way, in the laminate of electrode layers included in each of the positive and negative electrodes, the end of the upper electrode layer is supported by the embedded layer embedded in the end of the lower electrode layer, thereby suppressing deformation of the electrode layer group in each electrode during lamination and thermocompression bonding after electrode formation. By suppressing deformation of each electrode and its electrode layer group during thermocompression bonding, contact between the electrode pairs stacked with the electrolyte layer sandwiched between them, i.e., the positive electrode and the negative electrode, is suppressed. This effectively suppresses the occurrence of short circuits inside the solid-state battery.
[0032] In addition, an electrode including the above-mentioned stack of electrode layers has a recess (a portion corresponding to the above-mentioned gap) between the end of the lower electrode layer and the end of the upper electrode layer, and a buried layer having a lower electronic conductivity than the lower and upper electrode layers is provided in the recess. In a solid-state battery including an electrode having such a structure as a positive electrode or a negative electrode, current is less likely to flow to the side end of the electrode (the end of each electrode layer of the stack), where electrical conductivity is likely to vary. This reduces performance variation among the solid-state batteries produced.
[0033] According to the above process, it is possible to realize a high-performance, high-quality solid-state battery in which the occurrence of short circuits is suppressed. A further description is given of solid state battery electrodes formed using the above process.
[0034] Fig. 2 is a diagram for explaining an example of an electrode of a solid-state battery, in which (A) and (B) are schematic cross-sectional views of a main part of an example of an electrode of a solid-state battery. Electrodes 1 (positive and negative electrodes) of a solid-state battery formed using the steps shown in Fig. 1(A) to Fig. 1(D) include a first layer LY1 and a second layer LY2, as shown in Fig. 2(A), for example. The first layer LY1 includes a first electrode layer 10 and a first embedded layer 11 provided at an end 10a of the electrode layer. The second layer LY2 includes a second electrode layer 20 and a second embedded layer 21 provided at an end 20a of the electrode layer 20.
[0035] Moreover, the electrode 1 (each of the positive electrode and the negative electrode) of the solid-state battery formed using the process shown in the above-mentioned FIG. 1(A) to FIG. 1(D) includes, for example, a first region AR1 and a second region AR2 as shown in FIG. 2(B). The first region AR1 includes an inner portion 10b of the first electrode layer 10 and an inner portion 20b of the second electrode layer 20. A portion 3 where the first electrode layer 10 and the second electrode layer 20 contact each other exists in the first region AR1. The second region AR2 is a region surrounding the first region AR1. The second region AR2 includes an end portion 10a of the first electrode layer 10 and a first embedded layer 11 provided therein, and an end portion 20a of the second electrode layer 20 and a second embedded layer 21 provided therein.
[0036] In the battery 1, a recess 4 recessed toward the first region AR1 is formed between the end 10a of the first electrode layer 10 and the end 20a of the second electrode layer 20 in the second region AR2, and the first buried layer 11 is formed in the recess 4. Similarly, for the second and subsequent layers, a recess 4 is formed between the end 20a of the second electrode layer 20 and the end of the third electrode layer, and the second buried layer 21 is formed in the recess 4.
[0037] In such electrode 1 for a solid-state battery, deformation of electrode layer 10 and electrode layer 20 during lamination and thermocompression bonding is suppressed in second region AR2 including embedded layer 11 and embedded layer 21, and occurrence of a short circuit in the solid-state battery due to deformation is suppressed. Also, in electrode 1, current is less likely to flow through second region AR2, which is more likely to have variation in electrical conductivity than first region AR1, and performance variation among solid-state batteries including electrode 1 is suppressed.
[0038] 2(A) and 2(B) illustrate the boundary between the inner portion 10b of the first electrode layer 10 and the inner portion 20b of the second electrode layer 20. However, firing may be performed in the manufacture of a solid-state battery. The inner portion 10b of the first electrode layer 10 and the inner portion 20b of the second electrode layer 20 may be sintered by such firing at the contact portion 3 therebetween to be integrated.
[0039] 1(A) to 1(D), the electrode 1 is formed in the order of the first electrode layer 10, the first buried layer 11, the second electrode layer 20, and the second buried layer 21, but the order of formation is not limited to the above example. This point will be described with reference to the next FIG. 3.
[0040] 3A and 3B are diagrams for explaining another example of an electrode of a solid-state battery, each of which shows a schematic cross-sectional view of a main part of an example of an electrode. For example, in forming the electrode 1a as shown in Fig. 3(A), first, the first buried layer 11 is formed, for example, by screen printing, and then the first electrode layer 10 is formed, for example, by screen printing, to form the first layer LY1. Thereafter, the second buried layer 21 is formed, for example, by screen printing, and then the second electrode layer 20 is formed, for example, by screen printing, to form the second layer LY2. By forming each layer in this order, the electrode 1a as shown in Fig. 3(A) can also be obtained.
[0041] In forming the electrode 1b as shown in FIG. 3(B), first, the first electrode layer 10 is formed, then the first buried layer 11 is formed, and the first layer LY1 is formed. Thereafter, the second buried layer 21 is formed, then the second electrode layer 20 is formed, and the second layer LY2 is formed. Furthermore, the buried layer 31 is formed on the outside of the first layer LY1 and the second layer LY2. For example, a screen printing method is used to form each layer. By forming each layer in this order, the electrode 1b as shown in FIG. 3(B) can also be obtained.
[0042] [Example] Examples of solid-state batteries and methods for manufacturing the same are described in detail below. First, an example of the formation of the electrolyte sheet, the positive electrode layer paste, the negative electrode layer paste, and the embedding layer paste will be described.
[0043] (Formation of electrolyte sheet) The electrolyte sheet is formed using a paste containing a solid electrolyte, a binder, a plasticizer, a dispersant and a diluent.
[0044] Here, the solid electrolyte of the paste for the electrolyte sheet is, for example, Li, which is a type of NASICON type oxide-based solid electrolyte. 1.5 Al 0.5 Ge 1.5 (PO4)3 (hereinafter referred to as "LAGP") is used. LAGP is also called aluminum-substituted lithium germanium phosphate, etc.
[0045] As an example, the electrolyte sheet paste contains 29.0 wt% (weight%) of amorphous LAGP (hereinafter referred to as "LAGPg") and 3.2 wt% of crystalline LAGP (hereinafter referred to as "LAGPc") as a solid electrolyte, 6.5 wt% of PVB as a binder, 2.2 wt% of plasticizer, 0.3 wt% of a first dispersant, 16.1 wt% of a second dispersant, and 43.4 wt% of ethanol as a diluent. Note that the electrolyte sheet paste may contain one type of material or two or more types of materials for each of the binder, plasticizer, dispersant, and diluent.
[0046] The above-mentioned component materials of the electrolyte sheet paste are mixed and dispersed, for example, by a ball mill for 48 hours, to form the electrolyte sheet paste. The formed electrolyte sheet paste is then coated and dried, for example, by using a sheet forming machine such as a doctor blade, and dried at a temperature of 100° C. for 10 minutes to form the electrolyte sheet.
[0047] (Formation of paste for positive electrode layer) The paste for the positive electrode layer contains a positive electrode active material, a solid electrolyte, a conductive assistant, a binder, a plasticizer, a dispersant, and a diluent.
[0048] Here, for example, lithium cobalt pyrophosphate (Li2CoP2O7, hereinafter referred to as "LCPO") is used as the positive electrode active material of the paste for the positive electrode layer. For example, lithium cobalt phosphate (LiCoPO4), lithium vanadium phosphate (Li3V2(PO4)3) (hereinafter referred to as "LVP"), etc. may be used as the positive electrode active material. One type of material may be used as the positive electrode active material, or two or more types of materials may be used. For example, LAGP is used as the solid electrolyte of the paste for the positive electrode layer. For example, carbon materials such as carbon nanofibers, carbon black, graphite, graphene, and carbon nanotubes are used as the conductive assistant of the paste for the positive electrode layer.
[0049] As an example, the paste for the positive electrode layer contains 11.8 wt% LCPO as the positive electrode active material, 17.7 wt% LAGPg as the solid electrolyte, 2.7 wt% carbon nanofiber as the conductive assistant, 7.9 wt% PVB as the binder, 0.3 wt% plasticizer, 0.6 wt% first dispersant, and 59.1 wt% terpineol as the diluent. Note that the binder, plasticizer, dispersant, and diluent of the paste for the positive electrode layer may each be one type of material, or two or more types of materials may be used.
[0050] The component materials of the positive electrode layer paste as described above are mixed and dispersed, for example, in a ball mill for 72 hours and then in a triple roll mill, and mixed and dispersed using a particle gauge until the agglomerates are 1 μm or less, thereby forming a positive electrode layer paste.
[0051] (Formation of negative electrode layer paste) The negative electrode layer paste contains a negative electrode active material, a solid electrolyte, a conductive assistant, a binder, a plasticizer, a dispersant, and a diluent.
[0052] Here, the negative electrode active material of the paste for the negative electrode layer is, for example, anatase-type titanium oxide (TiO2). The negative electrode active material is Li, which is a type of NASICON-type oxide-based solid electrolyte. 1.3 Al 0.3 Ti 1.7(PO4)3 (hereinafter referred to as "LATP"), LVP, etc. may be used. As the negative electrode active material, one type of material may be used, or two or more types of materials may be used. As the solid electrolyte of the negative electrode layer paste, for example, LAGP is used. As the conductive assistant of the negative electrode layer paste, for example, carbon materials such as carbon nanofiber, carbon black, graphite, graphene, and carbon nanotubes are used.
[0053] As an example, the negative electrode layer paste contains 11.8 wt% TiO2 as the negative electrode active material, 17.7 wt% LAGPg as the solid electrolyte, 2.7 wt% carbon nanofiber as the conductive assistant, 7.9 wt% PVB as the binder, 0.3 wt% plasticizer, 0.6 wt% first dispersant, and 59.1 wt% terpineol as the diluent. Note that the binder, plasticizer, dispersant, and diluent of the negative electrode layer paste may each be one type of material, or two or more types of materials may be used.
[0054] The component materials of the negative electrode layer paste as described above are mixed and dispersed, for example, in a ball mill for 72 hours and then in a triple roll mill, and mixed and dispersed using a particle gauge until the agglomerates are 1 μm or less, thereby forming the negative electrode layer paste.
[0055] (Formation of embedding layer paste) As the embedding layer paste, a paste containing a solid electrolyte, a binder, a plasticizer, a dispersant and a diluent is used.
[0056] Here, for example, LAGP is used as the solid electrolyte of the embedding layer paste. As an example, the embedding layer paste contains 25.4 wt% LAGPg and 2.8 wt% LAGPc as the solid electrolyte, 8.5 wt% PVB as the binder, 0.2 wt% plasticizer, 1.9 wt% first dispersant, and 61.2 wt% terpineol as the diluent. Note that the binder, plasticizer, dispersant, and diluent of the embedding layer paste may each be one type of material, or two or more types of materials.
[0057] The component materials of the embedding layer paste as described above are mixed and dispersed, for example, in a ball mill for 72 hours and then in a three-roll mill, and mixed and dispersed using a particle gauge until the agglomerates are 1 μm or less, thereby forming the embedding layer paste.
[0058] Next, an example of manufacturing a solid-state battery using the electrolyte sheet, the positive electrode layer paste, the negative electrode layer paste, and the embedding layer paste prepared as described above will be described with reference to FIGS.
[0059] (Manufacturing solid-state batteries) Fig. 4 is a diagram for explaining an example of a method for forming a positive electrode part. Fig. 4(A) shows a schematic plan view of a main part of an example of a positive electrode layer forming step. Fig. 4(B) shows a schematic plan view of a main part of an example of a buried layer forming step.
[0060] As shown in Fig. 4(A), a positive electrode layer paste is applied onto an electrolyte sheet 101, and the applied positive electrode layer paste is dried to form a first positive electrode layer 110. The positive electrode layer paste is applied by using, for example, a screen printing method. The applied positive electrode layer paste is dried, for example, at a temperature of 90°C for 5 minutes.
[0061] The positive electrode layer 110 (positive electrode layer paste) is provided in a region for forming a plurality of solid-state batteries on one electrolyte sheet 101. As an example, Fig. 4(A) illustrates positive electrode layers 110 of two different sizes, large and small, in which the small-sized positive electrode layer 110 is used as the positive electrode layer for one solid-state battery, and the large-sized positive electrode layer 110 is used as the positive electrode layer for two solid-state batteries. In Fig. 4(A), each location (three locations for convenience) used as the positive electrode layer for one solid-state battery is illustrated by a dotted frame.
[0062] After the first positive electrode layer 110 is formed, as shown in FIG. 4(B), a paste for embedding layer is applied around the positive electrode layer 110 on the electrolyte sheet 101, and the applied paste for embedding layer is dried to form a first embedded layer 111 of the positive electrode part. The embedded layer 111 (paste for embedding layer) is formed so as to cover (cover) the end of the positive electrode layer 110. The embedding layer paste is applied by using, for example, a screen printing method. The applied embedding layer paste is dried, for example, at a temperature of 90° C. for 5 minutes.
[0063] The steps as shown in FIG. 4(A) and FIG. 4(B) are repeated for a predetermined number of layers, for example, the number of layers that will have the amount of active material and film thickness required to function as a positive electrode of a solid-state battery, to form a positive electrode part.
[0064] Fig. 5 is a diagram for explaining an example of a method for forming a negative electrode part. Fig. 5(A) shows a schematic plan view of a main part of an example of a negative electrode layer forming step. Fig. 5(B) shows a schematic plan view of a main part of an example of a buried layer forming step.
[0065] 5(A), a paste for a negative electrode layer is applied onto an electrolyte sheet 101, and the applied paste for a negative electrode layer is dried to form a first negative electrode layer 120. The application of the paste for a negative electrode layer is performed, for example, by using a screen printing method. The applied paste for a negative electrode layer is dried, for example, at a temperature of 90° C. for 5 minutes.
[0066] The negative electrode layer 120 (negative electrode layer paste) is provided in a region for forming a plurality of solid-state batteries on one electrolyte sheet 101. Fig. 5(A) illustrates, as an example, a single size of negative electrode layer 120, which is used as the negative electrode layer for two solid-state batteries. Fig. 5(A) illustrates, with dotted lines, the locations (three locations for convenience) of the negative electrode layer 120 that are used as the negative electrode layer for one solid-state battery.
[0067] After the first negative electrode layer 120 is formed, as shown in FIG. 5(B), a paste for embedding layer is applied around the negative electrode layer 120 on the electrolyte sheet 101, and the applied paste for embedding layer is dried to form the first embedded layer 121 of the negative electrode part. The embedded layer 121 (paste for embedding layer) is formed so as to cover (cover) the end of the negative electrode layer 120. The embedding layer paste is applied by using, for example, a screen printing method. The applied embedding layer paste is dried, for example, at a temperature of 90° C. for 5 minutes.
[0068] The steps as shown in FIG. 5(A) and FIG. 5(B) are repeated for a predetermined number of layers, for example, the number of layers that will have the amount of active material and film thickness required to function as the negative electrode of a solid-state battery, to form a negative electrode part.
[0069] The positive electrode part formed by repeating the steps shown in FIG. 4(A) and FIG. 4(B) for a predetermined number of layers and the negative electrode part formed by repeating the steps shown in FIG. 5(A) and FIG. 5(B) for a predetermined number of layers are alternately stacked and thermocompressed by a uniaxial press. Thermocompression is performed, for example, under conditions of a pressure of 20 MPa and a temperature of 45°C. By such thermocompression, a laminate (laminate green) having a structure in which the positive electrode part and the negative electrode part are alternately stacked is formed. The formed laminate green is cut at a predetermined position using a cutting machine, and then degreased by heat treatment under conditions of holding at a temperature of 500°C for 10 hours in an oxygen-containing atmosphere, and further sintered by heat treatment under conditions of holding at 600°C for 2 hours in a nitrogen-containing atmosphere. In this way, a solid-state battery is obtained.
[0070] 6 and 7 are diagrams for explaining an example of a configuration of a solid-state battery. Fig. 6(A) shows a schematic perspective view of the exterior of a solid-state battery, Fig. 6(B) shows a schematic example of a cut surface along the plane P1 as shown in Fig. 6(A), and Fig. 6(C) shows a schematic perspective view of the exterior of a solid-state battery provided with external terminals. Fig. 7(A) shows a schematic perspective view of the exterior of a solid-state battery, and Fig. 7(B) shows a schematic example of a cut surface along the plane P2 as shown in Fig. 7(A).
[0071] The solid-state battery 100 shown in FIG. 6(A) and FIG. 7(A) is manufactured by cutting the above-mentioned green laminate using a cutting machine and performing a heat treatment. Here, the laminate green has a structure in which positive electrode parts 115 and negative electrode parts 125 are alternately laminated and thermocompression bonded, as shown in Fig. 6(B) and Fig. 7(B). The positive electrode part 115 includes an electrolyte sheet 101 (electrolyte layer 105) and a plurality of layers (for example, two layers) of positive electrode layers 110 and embedded layers 111 provided thereon. The negative electrode part 125 includes an electrolyte sheet 101 (electrolyte layer 105) and a plurality of layers (for example, two layers) of negative electrode layers 120 and embedded layers 121 provided thereon.
[0072] Such a laminate green is cut as shown in Figures 6(B) and 7(B), at a position where the positive electrode layer 110 is exposed on one end surface and the negative electrode layer 120 is exposed on the other end surface, as shown in Figure 6(B), and is further heat-treated to obtain a solid-state battery 100.
[0073] The positive electrode layers 110 of the positive electrode parts 115 (for example, two layers) and the negative electrode layers 120 of the negative electrode parts 125 (for example, two layers) are sintered and integrated by, for example, heat treatment performed after cutting. A part of the embedded layer 111 is interposed between the ends 110a of the positive electrode layers 110 of the positive electrode parts 115, and a part of the embedded layer 121 is interposed between the ends 120a of the negative electrode layers 120 of the negative electrode parts 125.
[0074] One end surface where the positive electrode layer 110 is exposed is used as a positive electrode terminal surface 130, and the other end surface where the negative electrode layer 120 is exposed is used as a negative electrode terminal surface 140. On the positive electrode terminal surface 130, a side end surface of the positive electrode layer 110 of the positive electrode part 115, a side end surface of the electrolyte layer 105 obtained by cutting the electrolyte sheet 101, and a side end surface of the embedded layer 121 of the negative electrode part 125 are exposed, and the negative electrode layer 120 is not exposed. On the negative electrode terminal surface 140, a side end surface of the negative electrode layer 120 of the negative electrode part 125, a side end surface of the electrolyte layer 105, and a side end surface of the embedded layer 111 of the positive electrode part 115 are exposed, and the positive electrode layer 110 is not exposed. In the intermediate region between the positive electrode terminal surface 130 and the negative electrode terminal surface 140 as shown in FIG. 7(A), the positive electrode layer 110 of the positive electrode part 115 and the negative electrode layer 120 of the negative electrode part 125 are alternately stacked with the electrolyte layer 105 interposed therebetween, as shown in FIG. 7(B) (and FIG. 6(B)).
[0075] Then, as shown in FIG. 6(C), a positive electrode terminal 131 and a negative electrode terminal 141 are formed as external terminals on the positive electrode terminal surface 130 and the negative electrode terminal surface 140 of the solid-state battery 100 as shown in FIG. 6(A) and FIG. 6(B) (and FIG. 7(A)), respectively. The positive electrode terminal 131 is formed so as to be connected to the side end surface of the positive electrode layer 110 exposed on the positive electrode terminal surface 130, and the negative electrode terminal 141 is formed so as to be connected to the side end surface of the negative electrode layer 120 exposed on the negative electrode terminal surface 140. This realizes a chip-type solid-state battery 100 in which a plurality of battery cells each including a pair of the positive electrode layer 110 and the negative electrode layer 120 and the electrolyte layer 105 therebetween are electrically connected in parallel.
[0076] An example of the formation of the solid-state battery 100 having the above configuration will be described in detail with attention to a cross section taken along the plane P1 in FIG. 6(A), i.e., a cross section perpendicular to the positive terminal surface 130 and the negative terminal surface 140 (hereinafter referred to as the "terminal surface perpendicular direction"), and a cross section taken along the plane P2 in FIG. 7(A), i.e., a direction parallel to the positive terminal surface 130 and the negative terminal surface 140 (hereinafter referred to as the "terminal surface parallel direction").
[0077] Fig. 8 is a diagram showing an example of a process for forming a positive electrode part in a cross section perpendicular to the terminal surface, Fig. 9 is a diagram showing an example of a process for forming a negative electrode part in a cross section perpendicular to the terminal surface, Fig. 10 is a diagram showing an example of a process for forming a green laminate in a cross section perpendicular to the terminal surface, and Fig. 11 is a diagram showing an example of a cutting process and a heat treatment process in a cross section perpendicular to the terminal surface. Figs. 8(A) to 8(E), 9(A) to 9(E), 10(A) to 10(C), and 11(A) and 11(B) each show a schematic cross-sectional view of a main part of each process.
[0078] Fig. 12 is a diagram showing an example of a process for forming a positive electrode part in a cross section parallel to the terminal surface, Fig. 13 is a diagram showing an example of a process for forming a negative electrode part in a cross section parallel to the terminal surface, Fig. 14 is a diagram showing an example of a process for forming a green laminate in a cross section parallel to the terminal surface, and Fig. 15 is a diagram showing an example of a cutting process and a heat treatment process in a cross section parallel to the terminal surface. Figs. 12(A) to 12(E), 13(A) to 13(E), 14(A) to 14(C), 15(A) and 15(B) each show a schematic cross-sectional view of a main part of each process.
[0079] (Formation of positive electrode parts) In forming the positive electrode part 115, first, as shown in FIG. 8(A) and FIG. 12(A), an electrolyte sheet 101 is prepared.
[0080] 8(B) and 12(B), a paste for a positive electrode layer is applied to a predetermined region (region for forming a plurality of solid-state batteries) on the electrolyte sheet 101 by using a screen printing method, and then dried to form a first positive electrode layer 110. The first positive electrode layer 110 formed in each region by using the screen printing method is formed on the electrolyte sheet 101 in a shape such that the thickness of an inner portion 110b is greater than the thickness of an end portion 110a around the entire periphery.
[0081] 8(C) and 12(C), a paste for embedding layer is applied around the first positive electrode layer 110 on the electrolyte sheet 101 by screen printing and dried to form the first embedded layer 111. The first embedded layer 111 is formed so as to cover the end portion 110a of the first positive electrode layer 110 and to expose the inner portion 110b thereof.
[0082] Next, as shown in FIG. 8(D) and FIG. 12(D), a paste for a positive electrode layer is applied onto the first positive electrode layer 110 by using a screen printing method, and the paste is dried to form a second positive electrode layer 110 so as to be laminated on the first positive electrode layer 110. As with the first positive electrode layer 110, the second positive electrode layer 110 is also formed in a shape such that the thickness of the inner portion 110b is thicker than the thickness of the end portion 110a of the entire periphery. A part of the first buried layer 111 formed to cover the end portion 110a of the first positive electrode layer 110 is interposed between the end portions 110a of the first and second positive electrode layers 110.
[0083] 8(E) and 12(E), a paste for embedding layer is applied around the second positive electrode layer 110 by screen printing and dried to form the second embedded layer 111. The second embedded layer 111 is formed so as to cover the end portion 110a of the second positive electrode layer 110 and expose the inner portion 110b thereof.
[0084] For example, by steps such as those shown in Figures 8(A) to 8(E) and Figures 12(A) to 12(E), a positive electrode part 115 is formed in which multiple layers (two layers in this example) of positive electrode layers 110 are stacked and their ends 110a are each covered with an embedded layer 111.
[0085] (Formation of negative electrode parts) In forming the negative electrode part 125, first, as shown in FIG. 9(A) and FIG. 13(A), an electrolyte sheet 101 is prepared.
[0086] 9(B) and 13(B), a paste for the negative electrode layer is applied to a predetermined region (region for forming a plurality of solid-state batteries) on the electrolyte sheet 101 by using a screen printing method, and then dried to form the first negative electrode layer 120. The first negative electrode layer 120 formed in each region by using the screen printing method is formed on the electrolyte sheet 101 in a shape such that the thickness of the inner portion 120b is thicker than the thickness of the end portion 120a around the entire periphery.
[0087] 9(C) and 13(C), a paste for embedding layer is applied around the first negative electrode layer 120 on the electrolyte sheet 101 by screen printing and dried to form the first embedded layer 121. The first embedded layer 121 is formed so as to cover the end portion 120a of the first negative electrode layer 120 and expose the inner portion 120b thereof.
[0088] Next, as shown in Fig. 9(D) and Fig. 13(D), a paste for the negative electrode layer is applied onto the first negative electrode layer 120 by using a screen printing method, and the paste is dried to form the second negative electrode layer 120 so as to be laminated on the first negative electrode layer 120. As with the first negative electrode layer 120, the second negative electrode layer 120 is also formed in a shape in which the thickness of the inner portion 120b is greater than the thickness of the end portion 120a of the entire periphery. A part of the first buried layer 121 formed to cover the end portion 120a of the first negative electrode layer 120 is interposed between the end portions 120a of the first and second negative electrode layers 120.
[0089] 9(E) and 13(E), a paste for embedding layer is applied around the second negative electrode layer 120 by screen printing and dried to form the second embedded layer 121. The second embedded layer 121 is formed so as to cover the end portion 120a of the second negative electrode layer 120 and expose the inner portion 120b thereof.
[0090] For example, by steps such as those shown in Figures 9(A) to 9(E) and Figures 13(A) to 13(E), a negative electrode part 125 is formed in which multiple layers (two layers in this example) of negative electrode layers 120 are stacked and their ends 120a are each covered by an embedded layer 121.
[0091] (Formation of laminate green) The positive electrode parts 115 and the negative electrode parts 125 obtained as described above are alternately stacked and thermocompression bonded to form a green laminate. For example, as shown in FIG. 10(A) and FIG. 14(A), the first positive electrode part 115 is stacked on the first negative electrode part 125, and further, as shown in FIG. 10(B) and FIG. 14(B), the second negative electrode part 125 is stacked on the first positive electrode part 115. Similarly, as shown in FIG. 10(C) and FIG. 14(C), the second positive electrode part 115 is stacked on the second negative electrode part 125, and the electrolyte sheet 101 is further stacked on the top layer. These are thermocompression bonded to form the green laminate 150.
[0092] When the laminate green 150 is formed in this manner, the negative electrode part 125 and the positive electrode part 115 are laminated so that the opposing negative electrode layers 120 and the opposing positive electrode layers 110 partially overlap each other in a cross section (cross section along the plane P1 in FIG. 6A) in the direction perpendicular to the terminal surface, as shown in FIG. 10A to FIG. 10C. That is, in a cross section in the direction perpendicular to the terminal surface, the negative electrode part 125 and the positive electrode part 115 are laminated so that the upper layer positive electrode layer 110 is positioned so as to straddle the adjacent negative electrode layers 120 in the lower layer, and the upper layer negative electrode layer 120 is positioned so as to straddle the adjacent positive electrode layers 110 in the lower layer. Alternatively, in the process of forming the negative electrode part 125 and the positive electrode part 115, screen printing is performed so that the negative electrode layer 120 and the positive electrode layer 110 are in such a positional relationship that they partially overlap each other in the cross section in the direction perpendicular to the terminal surface when they are laminated.
[0093] On the other hand, in a cross section in a direction parallel to the terminal surfaces (a cross section along plane P2 in FIG. 7(A)), as shown in FIG. 14(A) to FIG. 14(C), the negative electrode part 125 and the positive electrode part 115 are laminated so that the negative electrode layers 120 and the positive electrode layers 110 entirely overlap each other. Alternatively, in the process of forming the negative electrode part 125 and the positive electrode part 115, screen printing is performed so that when these are laminated, the negative electrode layer 120 and the positive electrode layer 110 are positioned so as to entirely overlap each other in this manner in a cross section in a direction parallel to the terminal surfaces.
[0094] (Cutting and heat treatment) The green laminate 150 obtained as described above is cut at positions DL1 as shown by dashed lines in Figs. 10(C) and 14(C) using a cutting machine. As a result, a plurality of individual pieces 150a of the green laminate 150 are formed as shown in Figs. 11(A) and 15(A). Further, a heat treatment for degreasing and firing is performed to form individual solid-state batteries 100 as shown in Figs. 11(B) and 15(B) (and Figs. 6(B) and 7(B)). Each solid-state battery 100 includes a plurality of battery cells each including the cut electrolyte sheet 101 as an electrolyte layer 105, and a positive electrode layer 110 and a negative electrode layer 120 provided via the electrolyte layer 105. In each solid-state battery 100, during the heat treatment performed when it is formed, the stacked negative electrode layers 120 in each negative electrode part 125 are integrated together by sintering, and the stacked positive electrode layers 110 in each positive electrode part 115 are integrated together by sintering to form a structure.
[0095] 11(B), the side end face of the positive electrode layer 110 is exposed on one end face in the direction perpendicular to the terminal face of each solid-state battery 100, and the side end face of the negative electrode layer 120 is exposed on the other end face in the direction perpendicular to the terminal face of each solid-state battery 100. That is, in the direction perpendicular to the terminal face, the side where the side end face of the positive electrode layer 110 is exposed becomes the positive electrode terminal face 130, and the side where the side end face of the negative electrode layer 120 is exposed becomes the negative electrode terminal face 140. A positive electrode terminal 131 and a negative electrode terminal 141 as shown in FIG. 6(C) are formed on the positive electrode terminal face 130 and the negative electrode terminal face 140, respectively, to realize a chip-type solid-state battery 100.
[0096] In the solid-state battery 100 obtained by the above-mentioned process, when a plurality of positive electrode layers 110 are laminated to obtain a positive electrode part 115, the positive electrode layers 110 are laminated after covering their end portions 110a, which are thinner than their inner portions 110b, with embedding layers 111. Similarly, when a plurality of negative electrode layers 120 are laminated to obtain a negative electrode part 125, the negative electrode layers 120 are laminated after covering their end portions 120a, which are thinner than their inner portions 120b, with embedding layers 121.
[0097] As a result, when the positive electrode part 115 and the negative electrode part 125 are laminated and thermocompressed to obtain the laminate green 150, the deformation of the positive electrode layer 110 during thermocompression is suppressed compared to when the embedding layer 111 is not provided at the end 110a. Similarly, the deformation of the negative electrode layer 120 during thermocompression is suppressed compared to when the embedding layer 121 is not provided at the end 120a. In addition, the deformation of the positive electrode layer 110 and the negative electrode layer 120 during the subsequent heat treatment is also suppressed, and further, the deformation of the electrolyte layer 105 located between them is also suppressed. By suppressing the deformation of the positive electrode layer 110, the negative electrode layer 120, etc., the occurrence of a short circuit in the solid-state battery 100 due to the deformation is effectively suppressed.
[0098] [Survey on solid-state batteries] The results of investigations into the solid-state battery having the above-mentioned configuration, including the covering distance and covering rate of the embedded layer covering the end of the electrode layer (positive electrode layer or negative electrode layer), the deformation of the end of the electrode layer, the defect rate of the solid-state battery, and the thickness of the end and inner part of the electrode layer, are described below.
[0099] Fig. 16 is a diagram for explaining the electrode configuration of a solid-state battery. Fig. 16(A) shows a schematic cross-sectional view of a main part of a solid-state battery, Fig. 16(B) shows a schematic enlarged partial view of part Q (corresponding to one electrode layer) of Fig. 16(A), and Fig. 16(C) shows a schematic perspective view of part Q of Fig. 16(A).
[0100] For the investigation, a solid-state battery 160 having a structure as shown in FIG. 16(A) is used. The solid-state battery 160 is obtained by stacking ten electrode layers 170 (corresponding to the above-mentioned positive electrode layer 110 or negative electrode layer 120) on an electrolyte layer 105 while covering an end 170a with an embedded layer 180 (corresponding to the above-mentioned embedded layer 111 or embedded layer 121), and performing a heat treatment for degreasing and firing after thermocompression bonding. For convenience, FIG. 16(A) shows only one electrolyte layer 105 and ten electrode layers 170 and embedded layers 180 provided on one surface side thereof. FIG. 16(B) and FIG. 16(C) show an extracted region (Q portion) including one electrode layer 170 in such a solid-state battery 160.
[0101] Here, the distance from the side end of the electrode layer 170 to the embedded layer 180 covering the end 170a of the electrode layer 170 as shown in Fig. 16(B) is defined as "covering distance d". The ratio of the area S1 of the region covered by the embedded layer 180 at the covering distance d to the area S0 of the main surface of the electrode layer 170 (or 10 layers integrated by sintering) as shown in Fig. 16(C) is defined as "covering ratio y" (y = S1 / S0 x 100). Also, the thickness of the inner part 170b of the electrode layer 170 as shown in Fig. 16(B) is defined as "electrode thickness t1", and the thickness of the side end of the electrode layer 170 is defined as "end thickness t2".
[0102] Five types of solid-state batteries 160 having structures A to E with different covering distances d were fabricated and examined. The five types of solid-state batteries 160 have structures A, B, C, D, and E in order of increasing covering distance d.
[0103] (Distance of the buried layer covering the end of the electrode layer and deformation of the end of the electrode layer) For each of the solid-state batteries 160 of structures A to E, the covering distance d [μm] of the embedded layer 180 on the end 170a of the electrode layer 170, the covering ratio y [%], and the presence or absence of deformation (electrode deformation) of the end 170a of the electrode layer 170 were investigated. The results are shown in Tables 1 and 2 and FIG.
[0104] [Table 1]
[0105] [Table 2]
[0106] In structure A, the average covering distance d was 15.6 μm and the average covering rate y was 1.4% (Table 1). In structure B, the average covering distance d was 24.1 μm and the average covering rate y was 2.2% (Table 1). In structure C, the average covering distance d was 34.2 μm and the average covering rate y was 3.2% (Table 1). In structure D, the average covering distance d was 61.9 μm and the average covering rate y was 5.7% (Table 2). In structure E, the average covering distance d was 77.4 μm and the average covering rate y was 7.1% (Table 2).
[0107] Here, an example of the cross-sectional observation result of each solid-state battery 160 of structures A to E is shown in FIG. 17. FIG. 17(A) to FIG. 17(E) are schematic illustrations of cross-sectional photographs obtained for each solid-state battery 160 of structures A to E. As illustrated in FIG. 17(A) to FIG. 17(C), in structures A, B, and C in which the coverage ratio y (average) of the embedding layer 180 covering the end 170a of the electrode layer 170 is relatively small, large electrode deformation was observed in the end 170a of the electrode layer 170. In contrast, as illustrated in FIG. 17(D) and FIG. 17(E), in structures D and E in which the coverage ratio y (average) of the embedding layer 180 covering the end 170a of the electrode layer 170 is relatively large, large electrode deformation was not observed in the end 170a of the electrode layer 170.
[0108] For the sake of convenience, in Tables 1 and 2 (and Tables 3 to 6 below), the solid-state batteries 160 of Structures A, B, and C in which significant electrode deformation was observed are considered to have electrode deformation, and the solid-state batteries 160 of Structures D and E in which no significant electrode deformation was observed are considered to have no electrode deformation.
[0109] The minimum covering ratio y in Structure D and Structure E, in which no significant electrode deformation was observed, was 4.9% (Measurement No. 6 for Structure D), and the maximum covering ratio y was 7.8% (Measurement No. 6 for Structure E). It can be said that it is possible to realize a solid-state battery 160 in which electrode deformation is suppressed by covering the end portion 170a of the electrode layer 170 with the embedding layer 180 so that the covering ratio y is in the range of 4.9%≦y≦7.8%. In addition, when the covering distance d is specified as a manufacturing condition, it can be specified, for example, to a covering distance d such that the covering ratio y is in the range of 4.9%≦y≦6.3%, which is the minimum and maximum range of Structure D.
[0110] (Defective rate of solid-state batteries) The failure rate [%] due to internal short circuit was investigated for each solid-state battery 160 of structures A to E from the initial battery voltage. In the case of a solid-state battery 160 in which the positive electrode active material is LCPO and the negative electrode active material is TiO2, the initial potential is about minus several mV to minus hundreds of mV, but here, the solid-state battery 160 whose initial potential was measured and whose value was 0V to ±0.1 mV was determined to be defective due to internal short circuit. Thirty solid-state batteries 160 formed in each of structures A to E were randomly selected, and the voltage was measured with a tester, and the proportion of the number of solid-state batteries 160 whose initial potential was 0V to ±0.1 mV was calculated as the failure rate. The results are shown in Tables 3 and 4.
[0111] [Table 3]
[0112] [Table 4]
[0113] In structures A, B, and C in which large electrode deformation was observed, the defect rate for structure A was 93.3%, the defect rate for structure B was 83.3%, and the defect rate for structure C was 70.0% (Table 3). In contrast, in structures D and E in which no large electrode deformation was observed, the defect rate for both was 6.7% (Table 4). It can be said that by adopting the covering distance d and covering rate y as in structures D and E for the solid-state battery 160, it is possible to realize a solid-state battery 160 in which electrode deformation and defect rate are suppressed.
[0114] (Thickness of the electrode layer at the edge and inner part) For each of the solid-state batteries 160 of structures A to E, the electrode thickness t1 [μm] and end thickness t2 [μm] of the electrode layer 170, as well as the thickness difference ratio x [%] between the end thickness t2 and the electrode thickness t1 when the electrode thickness t1 is used as a reference, were investigated. The electrode thickness t1 is the thickness of the inner portion 170b of the electrode layer 170, and the end thickness t2 is the thickness of the side end of the electrode layer 170 (FIG. 16(B)). The thickness difference ratio x was calculated by x=|t2-t1| / t1×100. The results are shown in Tables 5 and 6.
[0115] [Table 5]
[0116] [Table 6]
[0117] In the case of structures A, B, and C in which large electrode deformation was observed, the minimum thickness difference ratio x was 7.5% and the maximum thickness difference ratio x was 79.9% in structure A, the minimum thickness difference ratio x was 1.5% and the maximum thickness difference ratio x was 66.1% in structure B, and the minimum thickness difference ratio x was 1.0% and the maximum thickness difference ratio x was 80.9% in structure C (Table 5). In contrast, in the case of structures D and E in which large electrode deformation was not observed, the minimum thickness difference ratio x was 0.0% and the maximum thickness difference ratio x was 9.4% in structure D, and the minimum thickness difference ratio x was 1.0% and the maximum thickness difference ratio x was 6.2% in structure E (Table 6).
[0118] From the results of structures D and E, it can be said that by adopting an electrode layer 170 in which the thickness difference ratio x between the electrode thickness t1 and the end thickness t2 is in the range of 0%≦x≦9.4% in the solid-state battery 160 and adopting the covering distance d and covering rate y as in structures D and E, it is possible to realize a solid-state battery 160 in which electrode deformation and defect rate are suppressed. [Explanation of symbols]
[0119] 1,1a,1b electrode 3. Contact area 4 Recess 10,20,170 electrode layer 10a, 20a, 110a, 120a, 170a End 10b,20b,110b,120b,170b Inner part 11,21,31,111,121,180 Embedding Layer 100,160 solid state batteries 101 Electrolyte Sheet 105 Electrolyte layer 110 Positive electrode layer 115 Positive electrode parts 120 Negative electrode layer 125 Negative electrode parts 130 Positive terminal surface 131 Positive terminal 140 Negative terminal surface 141 Negative terminal 150 Laminated Green 150a piece AR1 1st area AR2 2nd area LY1 1st layer LY2 2nd layer P1,P2 side DL1 position S0,S1 area t1 Electrode thickness t2 End thickness x Thickness difference ratio d Coverage distance y Coverage rate
Claims
1. forming a first electrode including a first electrode layer and a second electrode layer facing the first electrode layer, the first electrode being provided with a first buried layer having lower electronic conductivity than the first electrode layer and the second electrode layer between the first electrode layer and the second electrode layer and around a first portion where the first electrode layer and the second electrode layer are in contact with each other; A method for manufacturing a solid-state battery, wherein a ratio of an area of the first buried layer to an area of a main surface of the first electrode is 4.9% or more and 7.8% or less.
2. The method for manufacturing a solid-state battery according to claim 1 , wherein each of the first electrode layer and the second electrode layer is thinner in the other portion than in the first portion.
3. The method for manufacturing a solid-state battery according to claim 1 , wherein the first buried layer becomes thicker as it moves away from the first portion toward the outside.
4. 4. The method for manufacturing a solid-state battery according to claim 1, wherein the first electrode layer, the second electrode layer, and the first buried layer are each formed by using a printing method.
5. the first electrode layer includes a first active material; the second electrode layer includes a second active material; 5. The method for manufacturing a solid-state battery according to claim 1, wherein the first buried layer has a lower electronic conductivity than the first active material and the second active material.
6. forming a second electrode including a third electrode layer and a fourth electrode layer facing the third electrode layer, the second electrode being provided with a second buried layer having lower electronic conductivity than the third electrode layer and the fourth electrode layer between the third electrode layer and the fourth electrode layer and around a second portion where the third electrode layer and the fourth electrode layer are in contact with each other; providing an electrolyte layer between the first electrode and the second electrode to form a laminate of the first electrode, the electrolyte layer, and the second electrode; Firing the laminate; The method for producing a solid-state battery according to any one of claims 1 to 5, further comprising:
7. a first electrode having a first region and a second region surrounding the first region; a first buried layer provided in the second region excluding a portion of a side end surface of the first electrode, the first buried layer having lower electronic conductivity than the first electrode; Including, A solid-state battery, wherein a ratio of an area of the first buried layer to an area of a main surface of the first electrode is 4.9% or more and 7.8% or less.
8. the second region has a recess recessed toward the first region, The solid-state battery according to claim 7 , wherein the first buried layer is provided in the recess in the second region.
9. The solid-state battery according to claim 7 or 8, wherein the first buried layer becomes thicker as it moves away from the first region toward the outside.
10. The first electrode contains one or more active materials, 10. The solid-state battery according to claim 7, wherein the first buried layer has a lower electronic conductivity than the active material.
11. a second electrode including a third region and a fourth region surrounding the third region; a second buried layer provided in the fourth region excluding a portion of a side end surface of the second electrode, the second buried layer having lower electronic conductivity than the second electrode; an electrolyte layer provided between the first electrode and the second electrode; The solid-state battery according to any one of claims 7 to 10, comprising:
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery
JP1988013264A
System for opening and closing lid of hermetically closed container, and method of processing substrate using the system
JP2009033016A
Method of manufacturing catalyst layer-electrolyte membrane laminate
JP2012023044A
Method of manufacturing electrode body, and electrode body
JP2012038425A
All-solid secondary battery and method for manufacturing the same
JP2013182842A