Method for producing lithium silicate and silicon

By prioritizing carbon dioxide production over silicon carbide formation through controlled heating and layering of powders, the method enhances the yield and purity of lithium silicate and silicon, addressing the challenges of SiC formation and impurity separation in the synthesis process.

JP7596101B2Active Publication Date: 2024-12-09OSAKA TITANIUM TECHNOLOGIES
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020155262
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-16
Publication Date
2024-12-09
Estimated Expiration
2040-09-16

AI Technical Summary

Technical Problem

The production of silicon carbide (SiC) during the synthesis of lithium silicate and silicon from silicon powder, lithium carbonate powder, and silicon dioxide powder reduces the yield and increases the bulk density of the product, making it difficult to handle and separate carbon impurities, especially when heated above the melting point of lithium carbonate.

Method used

A method that prioritizes the production of carbon dioxide (CO2) over silicon carbide (SiC) by controlling the reaction conditions, including heating the mixed powders under reduced pressure and specific temperature ranges, and layering the powders to prevent direct contact, thereby reducing SiC formation and enhancing the production of lithium silicate and silicon.

Benefits of technology

This method effectively reduces the production of silicon carbide, improving the yield and handling of lithium silicate and silicon, while minimizing the presence of carbon impurities, thus facilitating the production of high-purity lithium-containing silicon oxide powder suitable for use as an active material in lithium ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596101000001
    Figure 0007596101000001
Patent Text Reader

Abstract

To provide a method capable of reducing the formation of silicon carbide in the formation of lithium silicate and silicon from silicon powder, lithium carbonate powder, and silicon dioxide powder.SOLUTION: In the method, lithium silicate (SiLixOy) and silicon (Si) are generated from lithium carbonate (Li2CO3) powder, silicon dioxide (SiO2) powder, and silicon (Si) powder in the same system so that discharges of carbon dioxide (CO2) take priority over generations of silicon carbide (SiC).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing lithium silicate and silicon from lithium carbonate powder, silicon dioxide powder and silicon powder in the same system. [Background technology]

[0002] In the past, it has been proposed that "a mixture of silicon powder, lithium carbonate powder, and, if necessary, silicon dioxide powder is used as the primary raw material, and the mixed powder is placed in a reaction vessel and heated and sintered to produce the secondary raw materials of lithium silicate and silicon" and that "the secondary raw material is heated to simultaneously generate SiO gas and Li gas from the raw material" (for example, see WO 2018 / 074175). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2018 / 074175 Summary of the Invention [Problem to be solved by the invention]

[0004] However, as described above, when silicon powder, lithium carbonate powder, and silicon dioxide powder are mixed and the mixed powder is heated at a temperature above the melting point of lithium carbonate (723°C), lithium carbonate reacts with silicon to produce silicon carbide (SiC) as a by-product. When silicon carbide is produced in this way, not only does the yield of the desired lithium silicate and silicon decrease, but the handling of the product (i.e., lithium silicate, silicon, and silicon carbide) becomes difficult as the bulk density increases. In addition, Patent Document 1 describes that impurity elements are more easily separated by performing the superheating and sintering of the primary raw material under reduced pressure, but as for carbon impurities, although impurities in the form of carbonate groups can be separated, once the impurities become in the form of silicon carbide (SiC), it becomes difficult to separate the carbon impurities even under reduced pressure.

[0005] The object of the present invention is to provide a method capable of reducing the production of silicon carbide when producing lithium silicate and silicon from silicon powder, lithium carbonate powder and silicon dioxide powder. [Means for solving the problem]

[0006] In the method according to the first aspect of the present invention, lithium silicate and silicon are produced from lithium carbonate (Li2CO3) powder, silicon dioxide (SiO2) powder, and silicon (Si) powder in the same system so that the emission of carbon dioxide (CO2) takes precedence over the production of silicon carbide (SiC). Here, the lithium silicate and silicon may each be single-phase (a compound (i.e., powder, etc.) consisting of a single phase) or may be a compound represented by the general formula SiLi x O y The compound represented by the formula: xThe reaction may be a multi-phase substance (a compound consisting of multiple phases) consisting of a lithium silicate phase (Li2Si2O5 phase, Li2SiO3 phase, etc.). Here, "lithium silicate and silicon are produced" may also include the case where silicon remains as it is before any reaction. Here, the system is preferably in a vacuum (reduced pressure). Here, examples of the method for prioritizing the emission of carbon dioxide over the production of silicon carbide include (i) a method of prioritizing the progress of the reaction Li2CO3→Li2O+CO2↑ over the progress of the reaction Li2CO3+Si→Li2SiO3+SiC, (ii) a method of prioritizing the progress of the reaction Li2CO3+SiO2→SiLi↑ over the progress of the reaction Li2CO3+Si→Li2SiO3+SiC, and (iii) a method of prioritizing the progress of the reaction Li2CO3+SiO2→SiLi↑ over the progress of the reaction Li2CO3+Si→Li2SiO3+SiC. x O y A method of giving priority to the progress of the reaction represented by +CO2↑ is mentioned. x O y The composition represented by is a multi-phase material (a composition consisting of multiple phases) consisting of a silicon phase, a silicon oxide phase (SiOx phase), a lithium silicate phase (Li2Si2O5 phase, Li2SiO3 phase, etc.), a lithium oxide phase (Li2O) phase, etc.

[0007] In this method, the emission of carbon dioxide takes precedence over the production of silicon carbide, and therefore, in this method, the production of silicon carbide can be reduced.

[0008] A method according to a second aspect of the present invention is the method according to the first aspect, in which a mixed powder of lithium carbonate powder, silicon dioxide powder, and silicon powder is heated in a reduced pressure atmosphere at a temperature within a range of 400° C. or higher and lower than the melting point of lithium carbonate.

[0009] In this method, the mixed powder is first heated in a reduced pressure atmosphere at a temperature in the range of 400°C or higher and lower than the melting point of lithium carbonate, and the decarbonation reaction of lithium carbonate (Li2CO3→Li2O+CO2↑ reaction) is promoted while suppressing the progress of the silicon carbide production reaction (Li2CO3+Si→Li2SiO3+SiC). Then, when it is heated at a temperature in the range of 1150°C or higher and 1400°C or lower, SiLi x Oy The reaction of +(y-1)Si→xLi↑+ySiO↑, in which Li and SiO are generated simultaneously, proceeds. Therefore, this method can reduce the generation of silicon carbide when producing lithium silicate and silicon from silicon powder, lithium carbonate powder, and silicon dioxide powder.

[0010] A method according to a third aspect of the present invention is the method according to the first aspect, in which lithium carbonate powder, silicon dioxide powder, and silicon powder are laid out in layers so that a layer of silicon dioxide powder is located between a layer of lithium carbonate powder and a layer of silicon powder, and heated at a temperature equal to or higher than the melting point of lithium carbonate. The upper limit of the heating temperature is 1400°C.

[0011] In this method, as described above, a layer of silicon dioxide powder is positioned between a layer of lithium carbonate powder and a layer of silicon powder. That is, in this method, the lithium carbonate powder and the silicon powder do not come into contact with each other, but the lithium carbonate powder and the silicon dioxide powder come into contact with each other. Therefore, in this method, when these powders are heated at a temperature equal to or higher than the melting point of lithium carbonate, the reaction of producing silicon carbide (Li2CO3+Si→Li2SiO3+SiC) proceeds more rapidly than the reaction of producing silicon carbide (Li2CO3+SiO2→SiLiC). x O y The reaction shown by +CO2↑ takes precedence. If it is then heated to a temperature in the range of 1150°C to 1400°C, SiLi x O y The reaction +(y-1)Si→xLi↑+ySiO↑ can proceed. Therefore, this method can reduce the production of silicon carbide when producing lithium silicate and silicon from silicon powder, lithium carbonate powder, and silicon dioxide powder.

[0012] A method according to a fourth aspect of the present invention is the method according to the first aspect, in which the mixed powder and silicon powder are laid out in layers so that a layer of the mixed powder of lithium carbonate powder and silicon dioxide powder is adjacent to a layer of silicon powder, and the mixed powder and silicon powder are heated at a temperature equal to or higher than the melting point of lithium carbonate. The upper limit of the heating temperature is 1400°C.

[0013] In this method, as described above, lithium carbonate powder and silicon dioxide powder are mixed together and layered, and the layer is adjacent to a layer of silicon powder. Therefore, in this method, when these powders are heated at a temperature equal to or higher than the melting point of lithium carbonate, the reaction of producing silicon carbide (Li2CO3+Si→Li2SiO3+SiC) proceeds more rapidly than the reaction of producing Li2CO3+SiO2→SiLi. x O y The reaction +CO2↑ takes precedence, and when it is heated to a temperature in the range of 1150°C to 1400°C, SiLi x O y The reaction +(y-1)Si→xLi↑+ySiO↑ can proceed. Therefore, this method can reduce the production of silicon carbide when producing lithium silicate and silicon from silicon powder, lithium carbonate powder, and silicon dioxide powder.

[0014] A method according to a fifth aspect of the present invention is the method according to the third or fourth aspect, in which the layer of silicon powder is the bottom layer.

[0015] The melting point of silicon is 1414°C, and the melting point of lithium silicate is lower than that of silicon (for example, the melting point of Li2SiO3 is 1201°C). Therefore, in this method, SiLi x O y In the reaction stage of +(y-1)Si→xLi↑+ySiO↑, the molten lithium silicate naturally penetrates into the gaps between the silicon powder, which increases the contact area between the lithium silicate and the silicon, thus accelerating the progress of the reaction.

[0016] A method according to a sixth aspect of the present invention is the method according to the first aspect, in which silicon powder is added into the system while the mixed powder of lithium carbonate powder and silicon dioxide powder is being heated.

[0017] Therefore, in this method, Li2CO3+SiO2→SiLi x O y If silicon powder is added at the point where the reaction indicated by +CO2↑ is assumed to be complete, SiLi x O y The reaction +(y-1)Si→xLi↑+ySiO↑ can proceed. Therefore, in this method, when lithium silicate and silicon are produced from silicon powder, lithium carbonate powder, and silicon dioxide powder, the production of silicon carbide can be suppressed. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a schematic diagram of a manufacturing apparatus for lithium-containing silicon oxide powder according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The method for producing lithium-containing silicon oxide powder according to the embodiment of the present invention is a method for producing lithium silicate and silicon from silicon powder, lithium carbonate powder and silicon dioxide powder, and then producing lithium-containing silicon oxide powder from lithium silicate and silicon, and reduces the production of silicon carbide during the process.The lithium-containing silicon oxide powder obtained by this method for producing lithium-containing silicon oxide powder is used, for example, as the active material of the negative electrode of a lithium ion secondary battery.

[0020] Incidentally, the method for producing lithium-containing silicon oxide powder according to the embodiment of the present invention can be carried out, for example, by forming a thin film of lithium-containing silicon oxide powder on a substrate and then scraping the thin film off the substrate, but from the viewpoint of reducing production costs, it is preferable to carry out the method using a vapor deposition apparatus 100 as shown in Fig. 1. Therefore, first, the vapor deposition apparatus 100 will be described, and then the method for producing lithium-containing silicon oxide powder using the vapor deposition apparatus 100 will be described. Here, four examples of the production method will be shown.

[0021] <Deposition equipment explanation> As shown in FIG. 1, the deposition apparatus 100 is mainly composed of a crucible 110, a heater 120, a deposition drum 130, a scraper 141, a granular guide 143, a chamber 150, a raw material supply hopper 160, a raw material introduction pipe 170, a recovery container 180, a first valve VL1, and a second valve VL2.

[0022] The crucible 110 is a heat-resistant container with an opening at the center of the top wall as shown in FIG. 1, and is installed in the chamber 150. A through hole (not shown) is formed at one location on the periphery of the top wall of the crucible 110, and a raw material introduction pipe 170 is inserted into the through hole. That is, the raw material in the raw material supply hopper 160 is supplied to the crucible 110 through the raw material introduction pipe 170. A gas guide Gg is disposed on the upper side of the top wall of the crucible 110. The gas guide Gg is a member that guides the raw material gas generated in the crucible 110 to the deposition drum 130, and is installed on the upper surface of the top wall so as to surround the central portion of the top wall as shown in FIG. 1.

[0023] The heater 120 is for heating the crucible 110 to a high temperature, and is disposed so as to surround the outer periphery of the crucible 110 .

[0024] The deposition drum 130 is, for example, a cylindrical horizontal drum, and is disposed above an opening OP in the top wall of the crucible 110 as shown in FIG. 1, and its lower portion is surrounded by a gas guide Gg. The deposition drum 130 is rotated in one direction by a driving mechanism (not shown). The deposition drum 130 is provided with a temperature regulator (not shown) for keeping the outer peripheral surface at a constant temperature. The temperature regulator cools the outer peripheral surface temperature of the deposition drum 130 to a temperature suitable for deposition of the deposition source gas by a cooling medium supplied from the outside. The outer peripheral surface temperature of the deposition drum 130 may affect the crystallinity of the precipitate deposited on the precipitate remaining on the deposition drum. If the temperature is too low, the texture of the precipitate may become too sparse, and conversely, if the temperature is too high, crystal growth due to disproportionation reaction may proceed. This temperature is preferably 900°C or lower, more preferably within the range of 150°C or higher and 800°C or lower, and particularly preferably within the range of 150°C or higher and 700°C or lower.

[0025] The scraper 141 is a member that serves to scrape off the thin film formed on the deposition drum from the deposition drum 130, and is disposed in the vicinity of the deposition drum 130 as shown in FIG. 1. The flakes (active material particles) scraped off by the scraper 141 fall into a granule guide 143. The material of the scraper 141 affects impurity contamination of the active material particles. From the viewpoint of suppressing the influence, the material of the scraper 141 is preferably stainless steel or ceramics, and particularly preferably ceramics. The scraper 141 is preferably not brought into contact with the outer circumferential surface of the deposition drum 130. This is because it is possible to prevent impurity contamination that may occur due to direct contact between the deposition drum 130 and the scraper 141 from being mixed into the recovered active material particles.

[0026] The granular guide 143 is, for example, a vibrating conveying member, and as shown in FIG. 1, is arranged so as to incline downward as it moves from the vicinity of the deposition drum toward the collection section 152 of the chamber 150. The granular guide 143 receives thin film fragments scraped off by the scraper 141 arranged above it and sends them to the collection section 152 of the chamber 150.

[0027] As shown in FIG. 1, the chamber 150 is mainly formed of a chamber main body 151, a recovery section 152, and an exhaust pipe 153. As shown in FIG. 1, the chamber main body 151 is a box-shaped section having a deposition chamber RM therein, and accommodates the crucible 110, the heater 120, the deposition drum 130, the scraper 141, and the particle guide 143. As shown in FIG. 1, the recovery section 152 is a section that protrudes outward from the side wall of the chamber main body 151, and has a space that communicates with the deposition chamber RM of the chamber main body 151. As described above, the tip section of the particle guide 143 is located in the recovery section 152.

[0028] 1, the raw material supply hopper 160 is a raw material supply source, and an outlet thereof is connected to a raw material introduction pipe 170. That is, the raw material fed into the raw material supply hopper 160 is supplied to the crucible 110 via the raw material introduction pipe 170 at an appropriate timing. The raw material supplied to the crucible 110 becomes molten Sr, and then vaporizes to become raw material gas.

[0029] The raw material introduction pipe 170 is a round-hole nozzle for supplying the solid raw material charged in the raw material supply hopper 160 to the crucible 110, and is arranged in the central part of the top plate of the crucible 110 with its mouth facing upward.

[0030] The collection container 180 is a container for collecting the thin film pieces that have passed through the first valve VL1 and the second valve VL2.

[0031] The first valve VL1 and the second valve VL2 are used to adjust the amount of thin film pieces collected in the collection container 180 by opening and closing, and are provided on a collection pipe 190 that connects the collection part 152 of the chamber 150 and the collection container 180.

[0032] <Description of an Example of a Method for Producing Lithium-Containing Silicon Oxide Powder According to the Present Embodiment> (1) First Example In this example, a mixed powder of lithium carbonate powder, silicon dioxide powder, and silicon powder is charged into the crucible 110 as a raw material. The mass ratio of the lithium carbonate powder, silicon dioxide powder, and silicon powder in this mixed powder is preferably 1:0.81-7.73:0.76-3.99 (this mass ratio is determined assuming that the molar ratio (Li / O) of lithium element (Li) to oxygen element (O) is in the range of 0.10 to 0.66). The raw materials may be charged from the raw material supply hopper 160 via the raw material introduction pipe 170, or directly into the crucible 110.

[0033] After the raw materials are put into the crucible 110, the heater 120 heats the crucible 110 to a temperature within a range of 400°C or higher and lower than the melting point of lithium carbonate while reducing the pressure inside the precipitation chamber RM. If the pressure inside the precipitation chamber RM is too high, carbon dioxide and other gases are not easily desorbed from the raw materials, and the reaction that generates SiO gas is not easily generated. For this reason, the pressure inside the precipitation chamber RM is reduced to 8000 Pa or lower. The pressure inside the precipitation chamber RM at this time is preferably 5000 Pa or lower, more preferably 2000 Pa or lower, and particularly preferably 1000 Pa or lower. The temperature inside the crucible 110 affects the progress rate of the decarbonation reaction (the reaction of Li2CO3 → Li2O + CO2↑) and the reaction of generating silicon carbide (Li2CO3 + Si → Li2SiO3 + SiC). If the temperature is too low, the decarbonation reaction rate slows down, and if the temperature is higher than the melting point of lithium carbonate, the reaction of generating silicon carbide progresses. From this viewpoint, the temperature in the crucible 110 is preferably in the range of 425°C to 720°C, more preferably in the range of 450°C to 715°C, even more preferably in the range of 475°C to 710°C, even more preferably in the range of 500°C to 705°C, and particularly preferably in the range of 525°C to 700°C. The pressure reduction and temperature increase can be performed in any order. The raw material powder in this example maintains its powder shape as it is. Note that lithium oxide (Li2O) after the decarbonation reaction may absorb CO2 and return to Li2CO3. For this reason, when it is necessary to take out lithium oxide (Li2O) into the atmosphere, it is desirable to heat it at a temperature in the range of 800°C to 1400°C after making the inside of the deposition chamber RM into an inert gas atmosphere in advance. By treating in this way, lithium oxide (Li2O) is taken into silicon dioxide to become lithium silicate, which is less likely to absorb CO2.

[0034] By heating the raw material as described in the above paragraph, the progress of the reaction for producing silicon carbide (Li2CO3+Si→Li2SiO3+SiC) is suppressed while the decarbonation reaction of lithium carbonate (Li2CO3→Li2O+CO2↑) proceeds. At this time, the progress of the decarbonation reaction of lithium carbonate can be confirmed by monitoring the weight of the raw material, detecting carbon dioxide, or detecting a decrease in the rate of decrease in pressure. In addition, when the method according to this example is repeated after the above confirmation, the progress of the decarbonation reaction of lithium carbonate can also be controlled by time management. In addition, it is also possible to omit the management of the progress of the decarbonation reaction in this example by feeding the powder, which has been decarbonated by heating the raw material as described in the above paragraph using an external device, from the raw material supply hopper 160 through the raw material introduction pipe 170 into the crucible 110.

[0035] The progress of the decarbonation reaction of lithium carbonate is controlled as described above, and from the point when the decarbonation reaction of lithium carbonate is considered to be completed, the pressure (reduced pressure state) of the deposition chamber RM is maintained or further reduced. If the pressure in the deposition chamber RM is too high, the reaction of generating SiO gas from the raw material is difficult to occur. For this reason, the pressure in the deposition chamber RM is preferably 1000 Pa or less, more preferably 750 Pa or less, and particularly preferably 20 Pa or less. After the deposition chamber RM is depressurized, the crucible 110 is heated to a temperature of more than 1050°C by the heater 120. The heating temperature is preferably more than 1100°C, more preferably more than 1150°C, even more preferably more than 1200°C, even more preferably more than 1250°C, and particularly preferably more than 1300°C. The upper limit of the heating temperature is 1400°C. At this time, the raw material may be stirred by a stirrer or the like after a certain time has passed. At this time, the deposition chamber RM is maintained in a reduced pressure state.

[0036] By heating the raw material under reduced pressure as described above, lithium oxide (Li2O) is incorporated into silicon dioxide to form lithium silicate, and SiLi x O yThe reaction represented by +(y-1)Si→xLi↑+ySiO↑ proceeds. When the heating temperature is in the range of 1050°C or more and less than 1150°C, the former reaction proceeds faster than the latter reaction, and when the heating temperature is in the range of 1150°C or more and 1400°C or less, the former reaction and the latter reaction proceed almost simultaneously. Silicon monoxide gas and lithium gas generated from the crucible 110 are supplied to the deposition drum 130 through the gas guide Gg. At this time, the deposition drum 130 is rotated by the drive source. The temperature of the outer peripheral surface of the deposition drum 130 is set lower than the temperature in the deposition chamber RM. More specifically, the temperature is set lower than the condensation temperature of silicon monoxide gas and lithium gas. With this setting, silicon monoxide gas and lithium gas generated from the crucible 110 are deposited and deposited on the outer peripheral surface of the rotating deposition drum 130, and the deposit is scraped off from the deposition drum 130 by the scraper 141. The scraped off pieces of the deposit fall along the outer circumferential surface of the deposition drum 130 into a particle guide 143 .

[0037] (2) Second Example In this example, when the lithium carbonate powder, silicon dioxide powder, and silicon powder are charged into the crucible 110 as raw materials, the lithium carbonate powder, silicon dioxide powder, and silicon powder are stacked in layers so that the layer of silicon dioxide powder is located between the layer of lithium carbonate powder and the layer of silicon powder. That is, in this example, the lithium carbonate powder and the silicon powder do not come into contact with each other, but the lithium carbonate powder and the silicon dioxide powder come into contact with each other. Such raw material charging is performed directly into the crucible 110. In addition, it is preferable that the layer of silicon powder is the bottom layer. In addition, in this case, the layer of lithium carbonate powder and the layer of silicon dioxide powder may be stacked one by one, or the layer of lithium carbonate powder and the layer of silicon dioxide powder may be stacked alternately in multiple layers. Here, the thickness of the lithium carbonate powder layer is preferably in the range of 100 μm to 50 mm, more preferably in the range of 200 μm to 45 mm, even more preferably in the range of 500 μm to 40 mm, and particularly preferably in the range of 1 mm to 35 mm. The thickness of the silicon dioxide powder layer is preferably in the range of 85 μm to 400 mm, more preferably in the range of 170 μm to 360 mm, even more preferably in the range of 430 μm to 320 mm, and particularly preferably in the range of 850 μm to 280 mm. The thickness of the silicon powder layer is preferably in the range of 84 μm to 220 mm, more preferably in the range of 168 μm to 198 mm, even more preferably in the range of 420 μm to 176 mm, and particularly preferably in the range of 840 μm to 154 mm. In addition, the ratio of the thickness of the silicon dioxide powder layer to the thickness of the lithium carbonate powder layer is preferably within a range of 0.25 to 15.0, more preferably within a range of 0.5 to 10.0, even more preferably within a range of 0.75 to 7.5, and particularly preferably within a range of 1.0 to 5.0.In addition, the ratio of the thickness of the silicon powder layer to the thickness of the lithium carbonate powder layer is preferably within a range of 0.25 to 10.0, more preferably within a range of 0.5 to 7.5, even more preferably within a range of 0.75 to 5.0, and particularly preferably within a range of 1.0 to 2.5.

[0038] After the raw materials are put into the crucible 110, the crucible 110 is heated by the heater 120 to a temperature equal to or higher than the melting point of lithium carbonate. The temperature inside the crucible 110 affects the desorption rate of carbon dioxide. If the temperature is too low, the desorption rate slows down, and if the temperature is too high, lithium carbonate and silicon melt together, causing the layers to collapse and the lithium carbonate and silicon to come into contact with each other, resulting in the production of silicon carbide. From this viewpoint, the temperature inside the crucible 110 is preferably within a range of 800°C to 1400°C, more preferably within a range of 900°C to 1300°C, and even more preferably within a range of 1000°C to 1200°C. The upper limit of this temperature is 1400°C. At this stage, in order to prioritize the desorption of carbon dioxide over the generation of SiO gas, the pressure inside the deposition chamber RM is set to 1000 Pa to atmospheric pressure + 1000 Pa. At this time, an inert gas such as argon (Ar) gas is supplied to the deposition chamber RM.

[0039] By heating the raw material as described in the above paragraph, the reaction of producing silicon carbide (Li2CO3+Si→Li2SiO3+SiC) is suppressed while the decarbonation reaction of lithium carbonate (Li2CO3→Li2O+CO2↑) proceeds. The progress of the decarbonation reaction of lithium carbonate can be realized by time management. In addition, by feeding the powder that has been decarbonated by heating the raw material as described in the above paragraph using an external device from the raw material supply hopper 160 through the raw material introduction pipe 170 into the crucible 110, it is possible to omit the management of the progress of the decarbonation reaction in this example.

[0040] The progress of the decarbonation reaction of lithium carbonate is controlled as described above, and the pressure in the deposition chamber RM is reduced from the point when the decarbonation reaction of lithium carbonate is considered to be completed. If the pressure in the deposition chamber RM is too high, the reaction of generating SiO gas from the raw material becomes difficult. For this reason, the pressure in the deposition chamber RM is preferably 1000 Pa or less, more preferably 750 Pa or less, and particularly preferably 20 Pa or less. After the pressure reduction is completed, the crucible 110 is heated by the heater 120. The heating temperature is preferably over 1050°C, more preferably over 1100°C, even more preferably over 1150°C, even more preferably over 1200°C, even more preferably over 1250°C, and particularly preferably over 1300°C. The upper limit of this temperature is 1400°C. At this time, the raw material may be stirred by a stirrer or the like after a certain time has passed.

[0041] By heating the raw materials under reduced pressure as described in the above paragraph, the reaction of silicon carbide formation (Li2CO3+Si→Li2SiO3+SiC) proceeds more rapidly than the reaction of Li2CO3+SiO2→SiLi x O y The reaction shown by +CO2↑ takes precedence. Then, SiLi x O y The reaction +(y-1)Si→xLi↑+ySiO↑ proceeds. Silicon monoxide gas and lithium gas generated from the crucible 110 are supplied to the deposition drum 130 through the gas guide Gg. At this time, the deposition drum 130 is rotated by the drive source. The temperature of the outer peripheral surface of the deposition drum 130 is set lower than the temperature in the deposition chamber RM. More specifically, the temperature is set lower than the condensation temperature of silicon monoxide gas and lithium gas. With this setting, silicon monoxide gas and lithium gas generated from the crucible 110 are deposited (precipitated) and accumulated on the outer peripheral surface of the rotating deposition drum 130, and the deposit is scraped off from the deposition drum 130 by the scraper 141. Pieces of the scraped deposit fall along the outer peripheral surface of the deposition drum 130 into the particle guide 143.

[0042] (3) Third Example In this example, when lithium carbonate powder, silicon dioxide powder, and silicon powder are charged into the crucible 110 as raw materials, the lithium carbonate powder and the silicon dioxide powder are mixed, and the mixed powder and the silicon powder are stacked in layers so that the layer of the mixed powder and the layer of the silicon powder are adjacent to each other. The mass ratio of the lithium carbonate powder and the silicon dioxide powder in this mixed powder is preferably 1:0.3 to 0.6 (this mass ratio is determined assuming that the molar ratio (Li / O) of the lithium element (Li) and the oxygen element (O) is in the range of 0.10 to 0.66). Such raw material charging is performed directly into the crucible 110. In this case, it is preferable that the layer of the silicon powder is disposed below the layer of the mixed powder, and it is preferable that the layer of the silicon powder is the lowest layer. In addition, at this time, the mixed powder layer and the silicon powder layer may be laminated one by one, or the mixed powder layer and the silicon powder layer may be alternately stacked in multiple layers. Here, the thickness of the mixed powder layer is preferably in the range of 185 μm to 450 mm, more preferably in the range of 370 μm to 405 mm, even more preferably in the range of 930 μm to 360 mm, and particularly preferably in the range of 1.85 mm to 315 mm. In addition, the thickness of the silicon powder layer is preferably in the range of 84 μm to 220 mm, more preferably in the range of 168 μm to 198 mm, even more preferably in the range of 420 μm to 176 mm, and particularly preferably in the range of 840 μm to 154 mm. In addition, the ratio of the thickness of the mixed powder layer to the thickness of the silicon powder layer is preferably in the range of 0.3 to 0.7, more preferably in the range of 0.33 to 0.65, even more preferably in the range of 0.37 to 0.6, and particularly preferably in the range of 0.4 to 0.55.

[0043] After the raw materials are put into the crucible 110, the crucible 110 is heated by the heater 120 to a temperature equal to or higher than the melting point of lithium carbonate. The temperature inside the crucible 110 affects the desorption rate of carbon dioxide. If the temperature is too low, the desorption rate slows down, and if the temperature is too high, lithium carbonate and silicon melt together, causing the layers to collapse and the lithium carbonate and silicon to come into contact with each other, resulting in the production of silicon carbide. From this viewpoint, the temperature inside the crucible 110 is preferably within a range of 800°C to 1400°C, more preferably within a range of 900°C to 1300°C, and even more preferably within a range of 1000°C to 1200°C. The upper limit of this temperature is 1400°C. At this stage, in order to prioritize the desorption of carbon dioxide over the generation of SiO gas, the pressure inside the deposition chamber RM is set to 1000 Pa to atmospheric pressure + 1000 Pa. At this time, an inert gas such as argon (Ar) gas is supplied to the deposition chamber RM.

[0044] By heating the raw material as described in the above paragraph, the reaction of producing silicon carbide (Li2CO3+Si→Li2SiO3+SiC) is suppressed while the decarbonation reaction of lithium carbonate (Li2CO3→Li2O+CO2↑) proceeds. The progress of the decarbonation reaction of lithium carbonate can be realized by time management. In addition, by feeding the powder that has been decarbonated by heating the raw material as described in the above paragraph using an external device from the raw material supply hopper 160 through the raw material introduction pipe 170 into the crucible 110, it is possible to omit the management of the progress of the decarbonation reaction in this example.

[0045] The progress of the decarbonation reaction of lithium carbonate is controlled as described above, and the pressure in the deposition chamber RM is reduced from the point when the decarbonation reaction of lithium carbonate is considered to be completed. If the pressure in the deposition chamber RM is too high, the reaction of generating SiO gas from the raw material becomes difficult. For this reason, the pressure in the deposition chamber RM is preferably 1000 Pa or less, more preferably 750 Pa or less, and particularly preferably 20 Pa or less. After the pressure reduction is completed, the crucible 110 is heated by the heater 120. The heating temperature is preferably over 1050°C, more preferably over 1100°C, even more preferably over 1150°C, even more preferably over 1200°C, even more preferably over 1250°C, and particularly preferably over 1300°C. The upper limit of this temperature is 1400°C. At this time, the raw material may be stirred by a stirrer or the like after a certain time has passed.

[0046] By heating the raw materials under reduced pressure as described in the above paragraph, the reaction of silicon carbide formation (Li2CO3+Si→Li2SiO3+SiC) proceeds more rapidly than the reaction of Li2CO3+SiO2→SiLi x O y The reaction shown by +CO2↑ takes precedence. Then, SiLi x O y The reaction +(y-1)Si→xLi↑+ySiO↑ proceeds. Silicon monoxide gas and lithium gas generated from the crucible 110 are supplied to the deposition drum 130 through the gas guide Gg. At this time, the deposition drum 130 is rotated by the drive source. The temperature of the outer peripheral surface of the deposition drum 130 is set lower than the temperature in the deposition chamber RM. More specifically, the temperature is set lower than the condensation temperature of silicon monoxide gas and lithium gas. With this setting, silicon monoxide gas and lithium gas generated from the crucible 110 are deposited (precipitated) and accumulated on the outer peripheral surface of the rotating deposition drum 130, and the deposit is scraped off from the deposition drum 130 by the scraper 141. Pieces of the scraped deposit fall along the outer peripheral surface of the deposition drum 130 into the particle guide 143.

[0047] (4) Fourth Example In this example, first, a mixed powder of lithium carbonate powder and silicon dioxide powder is charged into the crucible 110 as a raw material. Note that the mass ratio of the lithium carbonate powder and the silicon dioxide powder in this mixed powder is preferably 1:0.8 to 7.7 (note that this mass ratio is determined assuming that the molar ratio (Li / O) of lithium element (Li) to oxygen element (O) is in the range of 0.10 to 0.66). The raw material may be charged from the raw material supply hopper 160 via the raw material introduction pipe 170, or directly into the crucible 110.

[0048] After the raw material is charged into the crucible 110, the crucible 110 is heated to a temperature equal to or higher than the melting point of lithium carbonate by the heater 120. In this case, the pressure inside the precipitation chamber RM may be reduced, or an inert gas may be passed through the precipitation chamber RM. Here, the inert gas is, for example, a rare gas (such as argon gas) or nitrogen gas.

[0049] By heating the raw materials as described above, Li2CO3+SiO2→SiLi x O y Only the reaction indicated by +CO2↑ can be carried out with priority. At this time, the progress of the reaction can be confirmed by monitoring the weight of the raw material or detecting carbon dioxide. In addition, when the method according to this example is repeated after the above confirmation, the progress of the reaction can be controlled by time management.

[0050] The progress of the reaction is controlled as described above, and silicon powder is charged into the crucible 110 from the raw material supply hopper 160 through the raw material introduction pipe 170 when the reaction is considered to be completed. If the deposition chamber RM has already been depressurized before the silicon powder is charged, the above-mentioned depressurization degree and temperature may be maintained as they are, or may be appropriately changed. If the deposition chamber RM has not been depressurized before the silicon powder is charged, the deposition chamber RM is depressurized. If the pressure in the deposition chamber RM is too high, the reaction of generating SiO gas from the raw material is difficult to occur. For this reason, the pressure in the deposition chamber RM is preferably 1000 Pa or less, more preferably 750 Pa or less, and particularly preferably 20 Pa or less. The temperature in the deposition chamber RM affects the reaction rate of SiO, and if the temperature is too low, the reaction rate will be slow, and if the temperature is too high, there are concerns about the progression of side reactions due to the melting of the raw material and the decrease in energy efficiency. From this viewpoint, the temperature in the precipitation chamber RM is preferably above 1050° C., more preferably above 1100° C., even more preferably above 1150° C., still more preferably above 1200° C., still more preferably above 1250° C., and particularly preferably above 1300° C. The upper limit of this temperature is 1400° C. At this time, the raw materials may be stirred and mixed by a stirrer or the like.

[0051] And, SiLi x O yThe reaction +(y-1)Si→xLi↑+ySiO↑ proceeds. Silicon monoxide gas and lithium gas generated from the crucible 110 are supplied to the deposition drum 130 through the gas guide Gg. At this time, the deposition drum 130 is rotated by the drive source. The temperature of the outer peripheral surface of the deposition drum 130 is set lower than the temperature in the deposition chamber RM. More specifically, the temperature is set lower than the condensation temperature of silicon monoxide gas and lithium gas. With this setting, silicon monoxide gas and lithium gas generated from the crucible 110 are deposited (precipitated) and accumulated on the outer peripheral surface of the rotating deposition drum 130, and the deposit is scraped off from the deposition drum 130 by the scraper 141. Pieces of the scraped deposit fall along the outer peripheral surface of the deposition drum 130 into the particle guide 143.

[0052] EXAMPLES In the following, examples and comparative examples are shown in order to explain the present invention in more detail, but the present invention is not limited to these examples. EXAMPLES

[0053] A mixed powder of lithium carbonate powder, silicon dioxide powder, and silicon powder (lithium carbonate powder:silicon dioxide powder:silicon powder=1:1.63:1.14 (mass ratio)) was charged into the crucible 110 of the deposition apparatus 100 shown in Fig. 1, and the crucible 110 was heated to 410°C by the heater 120 while reducing the pressure inside the deposition chamber RM to 5 Pa. This heating was continued until carbon dioxide was no longer detected in the exhaust gas.

[0054] After it was confirmed that carbon dioxide was no longer detected in the exhaust gas from within the system, the output of the heater 120 was increased to raise the temperature of the crucible 110 to 1100° C., generating silicon monoxide gas and lithium gas. The silicon monoxide gas and lithium gas were then deposited (precipitated) on the outer circumferential surface of the deposition drum 130, and the deposits were scraped off from the deposition drum 130 by the scraper 141.

[0055] At this time, the yield of the lithium-containing silicon oxide powder was 47.1 mass %. A small amount of silicon carbide remained in the crucible 110, and the production rate was 1.4 mass %. EXAMPLES

[0056] A lithium-containing silicon oxide powder was produced in the same manner as in Example 1, except that the initial heating temperature was changed to 700° C., and the heating temperature after confirmation of non-detection of carbon dioxide was changed to 1400° C. The yield of the lithium-containing silicon oxide powder at this time was 96.2% by mass. In addition, almost no silicon carbide remained in the crucible 110, and the production rate was less than 0.1% by mass. EXAMPLES

[0057] A layer of silicon powder was formed in the crucible 110 of the deposition apparatus 100 shown in FIG. 1, a layer of silicon dioxide powder was formed on the silicon powder layer, and a layer of lithium carbonate powder was formed on the silicon dioxide powder layer. In this case, the thickness of the silicon powder layer was set to 16.8 mm, the thickness of the silicon dioxide powder layer was set to 17.0 mm, and the thickness of the lithium carbonate powder layer was set to 20.0 mm. Next, the crucible 110 was heated to 1100° C. by the heater 120 while passing argon (Ar) gas so that the pressure in the deposition chamber RM was atmospheric pressure +100 Pa. After confirming that carbon dioxide was no longer detected in the exhaust from the system, the pressure in the deposition chamber RM was reduced to 5 Pa, and silicon monoxide gas and lithium gas were generated. The silicon monoxide gas and lithium gas were deposited (precipitated) on the outer peripheral surface of the deposition drum 130, and the deposit was scraped off from the deposition drum 130 by the scraper 141.

[0058] At this time, the yield of the lithium-containing silicon oxide powder was 43.7% by mass. Furthermore, almost no silicon carbide remained in the crucible 110, and the production rate was 0.5% by mass. EXAMPLES

[0059] A lithium-containing silicon oxide powder was produced in the same manner as in Example 3, except that the heating temperature was changed to 1400° C. The yield of the lithium-containing silicon oxide powder was 94.1% by mass. In addition, almost no silicon carbide remained in the crucible 110, and the production rate was 0.3% by mass. EXAMPLES

[0060] A layer of silicon powder was formed in the crucible 110 of the deposition apparatus 100 shown in FIG. 1, and a layer of a mixed powder of silicon dioxide powder and lithium carbonate powder (lithium carbonate powder: silicon dioxide powder = 1: 0.42 (mass ratio)) was formed on the silicon powder layer. In this case, the thickness of the silicon powder layer was set to 37.0 mm, and the thickness of the mixed powder layer was set to 16.8 mm. Next, the crucible 110 was heated to 1100°C by the heater 120 while flowing argon (Ar) gas so that the pressure in the deposition chamber RM was atmospheric pressure + 100 Pa. After confirming that carbon dioxide was no longer detected in the exhaust from the system, the pressure in the deposition chamber RM was reduced to 5 Pa, and silicon monoxide gas and lithium gas were generated. The silicon monoxide gas and lithium gas were deposited (precipitated) on the outer peripheral surface of the deposition drum 130, and the deposit was scraped off from the deposition drum 130 by the scraper 141.

[0061] At this time, the yield of the lithium-containing silicon oxide powder was 31.9 mass %. Furthermore, almost no silicon carbide remained in the crucible 110, and the production rate was 0.8 mass %. EXAMPLES

[0062] A lithium-containing silicon oxide powder was produced in the same manner as in Example 5, except that the heating temperature was changed to 1400° C. The yield of the lithium-containing silicon oxide powder was 91.7% by mass. In addition, almost no silicon carbide remained in the crucible 110, and the production rate was 0.5% by mass. EXAMPLES

[0063] A mixed powder of lithium carbonate powder and silicon dioxide powder (lithium carbonate powder:silicon dioxide powder=1:1.63 (mass ratio)) was charged into the crucible 110 of the deposition apparatus 100 shown in Fig. 1, and the crucible 110 was heated to 1400°C by the heater 120 while reducing the pressure inside the deposition chamber RM to 5 Pa. This heating was continued until carbon dioxide was no longer detected in the exhaust gas.

[0064] After it was confirmed that carbon dioxide was no longer detected in the exhaust gas from within the system, silicon powder was introduced from raw material supply hopper 160 through raw material introduction pipe 170 into crucible 110 to generate silicon monoxide gas and lithium gas. The silicon monoxide gas and lithium gas were then deposited (precipitated) on the outer circumferential surface of deposition drum 130, and the deposits were scraped off from deposition drum 130 by scraper 141.

[0065] At this time, the yield of the lithium-containing silicon oxide powder was 75% by mass. Furthermore, almost no silicon carbide remained in the crucible 110, and the production rate was less than 0.1% by mass.

[0066] Comparative Example 1 A mixed powder of lithium carbonate powder, silicon dioxide powder, and silicon powder (lithium carbonate powder:silicon dioxide powder:silicon powder=1:1.63:1.14 (mass ratio)) was charged into crucible 110 of deposition apparatus 100 shown in Fig. 1, and while reducing the pressure inside deposition chamber RM to 5 Pa, crucible 110 was heated to 1400°C by heater 120 to generate silicon monoxide gas and lithium gas. Then, the silicon monoxide gas and lithium gas were deposited by deposition (precipitation) on the outer circumferential surface of deposition drum 130, and the deposit was scraped off from deposition drum 130 by scraper 141.

[0067] At this time, the yield of the lithium-containing silicon oxide powder was 7.3 mass %. Furthermore, silicon carbide remained in the crucible 110, and the production rate thereof was 4.7 mass %.

[0068] Comparative Example 2 A layer of silicon dioxide powder was formed in the crucible 110 of the deposition apparatus 100 shown in FIG. 1, a layer of lithium carbonate powder was formed on the silicon dioxide powder layer, and a layer of silicon was formed on the lithium carbonate powder layer. At this time, the thickness of the silicon dioxide powder layer was set to 17.0 mm, the thickness of the lithium carbonate powder layer was set to 20.0 mm, and the thickness of the silicon powder layer was set to 16.8 mm. Next, while reducing the pressure inside the deposition chamber RM to 5 Pa, the crucible 110 was heated to 1400° C. by the heater 120 to generate silicon monoxide gas and lithium gas. Then, the silicon monoxide gas and lithium gas were deposited by deposition (precipitation) on the outer circumferential surface of the deposition drum 130, and the deposit was scraped off from the deposition drum 130 by the scraper 141.

[0069] At this time, the yield of the lithium-containing silicon oxide powder was 11.7% by mass. Furthermore, silicon carbide remained in the crucible 110, and its production rate was 3.5% by mass.

[0070] Comparative Example 3 A layer of a mixed powder of lithium carbonate powder and silicon powder (lithium carbonate powder:silicon powder=1:1.26 (mass ratio)) was formed in the crucible 110 of the deposition apparatus 100 shown in FIG. 1, and a layer of silicon dioxide powder was formed on the mixed powder layer. In this case, the thickness of the mixed powder layer was set to 36.8 mm, and the thickness of the silicon dioxide powder layer was set to 17.0 mm. Next, while reducing the pressure inside the deposition chamber RM to 5 Pa, the crucible 110 was heated to 1400° C. by the heater 120 to generate silicon monoxide gas and lithium gas. Then, the silicon monoxide gas and lithium gas were deposited by deposition (precipitation) on the outer circumferential surface of the deposition drum 130, and the deposit was scraped off from the deposition drum 130 by the scraper 141.

[0071] At this time, the yield of the lithium-containing silicon oxide powder was 3.9 mass %. Furthermore, silicon carbide remained in the crucible 110, and the production rate thereof was 6.3 mass %.

[0072] Comparative Example 4 A mixed powder of lithium carbonate powder and silicon powder (lithium carbonate powder:silicon powder=1:1.26 (mass ratio)) was placed in the crucible 110 of the deposition apparatus 100 shown in FIG. 1, and the crucible 110 was heated to 1400° C. by the heater 120 while reducing the pressure inside the precipitation chamber RM to 5 Pa.

[0073] After one hour had passed, silicon dioxide powder was introduced from raw material supply hopper 160 through raw material introduction pipe 170 into crucible 110 to generate silicon monoxide gas and lithium gas. The silicon monoxide gas and lithium gas were then deposited (precipitated) on the outer circumferential surface of deposition drum 130, and the deposit was scraped off from deposition drum 130 by scraper 141.

[0074] At this time, the yield of the lithium-containing silicon oxide powder was 2.1 mass %. Furthermore, silicon carbide remained in the crucible 110, and the production rate thereof was 6.5 mass %. [Explanation of symbols]

[0075] 100 Vapor deposition equipment 110 Crucible 120 Heater 130 Evaporation drum 141 Scraper 143 Particle Guide 150 Chamber 151 Chamber body 152 Recovery Department 153 Exhaust pipe 160 Raw material supply hopper 170 Raw material introduction pipe 180 Collection Container 190 Recovery tube Gg Gas Guide OP Opening RM precipitation chamber Sr molten metal VL1 First valve VL2 Second valve

Claims

1. A mixed powder of lithium carbonate powder, silicon dioxide powder, and silicon powder is heated in a reduced pressure atmosphere at a temperature within a range of 400°C or higher and lower than the melting point of the lithium carbonate, and after completion of the decarboxylation reaction of the lithium carbonate, the mixed powder is heated to a temperature exceeding 1050°C. A method for producing lithium silicate (SiLi x O y ) and silicon (Si).

2. The lithium carbonate powder, the silicon dioxide powder and the silicon powder are laid out in layers so that a layer of silicon dioxide powder is positioned between a layer of lithium carbonate powder and a layer of silicon powder, and the layers are heated at a temperature within a range of from the melting point of the lithium carbonate to 1400°C. A method for producing lithium silicate (SiLi x O y ) and silicon (Si).

3. A method of laying out layers of a mixed powder of lithium carbonate powder and silicon dioxide powder and a layer of silicon powder adjacent to each other, and heating the layered mixture at a temperature within a range of from the melting point of the lithium carbonate to 1400°C. A method for producing lithium silicate (SiLi x O y ) and silicon (Si).

4. The silicon powder layer is the bottom layer. The method according to claim 2 or 3.

5. A mixed powder of lithium carbonate powder and silicon dioxide powder is heated, and silicon powder is added to the system after the decarbonation reaction of the lithium carbonate is completed. A method for producing lithium silicate (SiLi x O y ) and silicon (Si).

Citation Information

Patent Citations

  • Method of producing lithium-containing silicon oxide powder, and lithium-containing silicon oxide powder

    JP2014073942A

  • Silicon oxide negative electrode material and production method therefor

    WO2018074175A1

  • Negative electrode material and nonaqueous electrolyte secondary battery

    WO2018101072A1

  • Method for producing silicon oxide powder and negative electrode material

    WO2019189747A1