Hard magnetic powder

A hard magnetic powder with a rare earth metal-transition metal-B alloy and a maximum aspect ratio of 5.0 or more addresses the limitation of existing magnetic sheets by enhancing coercive force, enabling effective absorption of high-frequency electromagnetic waves.

JP7596154B2Active Publication Date: 2024-12-09SANYO SPECIAL STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021000530
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-05
Publication Date
2024-12-09
Estimated Expiration
2041-01-05

AI Technical Summary

Technical Problem

Existing magnetic sheets with Fe-Ni-Al-Co alloy powder are not suitable for absorbing electromagnetic waves with extremely high frequencies due to a coercive force of 31 kA/m or less, which limits their effectiveness in high-frequency applications.

Method used

A hard magnetic powder composed of flat particles made from a rare earth metal-transition metal-B alloy, with a maximum aspect ratio of 5.0 or more, is used, featuring a coercive force of 90 kA/m or more, which enhances absorption of high-frequency electromagnetic waves.

Benefits of technology

The magnetic powder effectively absorbs extremely high frequencies by suppressing eddy current loss and increasing coercive force, making it suitable for high-frequency electromagnetic wave absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596154000002
    Figure 0007596154000002
  • Figure 0007596154000003
    Figure 0007596154000003
  • Figure 0007596154000004
    Figure 0007596154000004
Patent Text Reader

Abstract

To provide a powder for a magnetic member capable of absorbing high electromagnetic waves having extremely high frequencies.SOLUTION: A hard magnetic powder is made of many flat particles 6. The material of the particles 6 is a rare earth metal-transition metal- B system alloy. The maximum aspect ratio of this powder is 5.0 or more. The preferable rare earth metal is Nd, and the preferable transition element is Fe. According to a preferable embodiment, the alloy comprises 10.8 atom% or more and 16.0 atom% or less of Nd, 5.4 atom% or more and 9.0 atom% or less of B, 0.3 atom% or more and 1.0% atom% of C, 15 atom% or less of O, and the balance Fe with inevitable impurities.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a powder whose particles are flat and have hard magnetic properties. [Background technology]

[0002] Electronic devices such as personal computers and mobile phones have circuits. Radio noise emitted from electronic components mounted on these circuits causes radio interference between the electronic components and other electronic components, and between electronic circuits and other electronic circuits. Radio interference can cause the electronic devices to malfunction. To prevent malfunction, electromagnetic wave absorbing sheets are inserted into the electronic devices.

[0003] In recent years, efforts are being made to increase the communication speed in information communication. High-frequency radio waves are used in this high-speed communication. Therefore, there is a demand for electromagnetic wave absorbing sheets that are suitable for use in the high-frequency range.

[0004] JP 2020-152979 A describes a magnetic sheet suitable for use in the high frequency range. The magnetic sheet contains powder. The powder is made of a large number of particles having a flat shape. The material of the powder is an Fe-Ni-Al-Co alloy. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication 2020-152979 Summary of the Invention [Problem to be solved by the invention]

[0006] The magnetic sheet absorbs electromagnetic waves through the natural resonance phenomenon. Natural resonance depends on the precession of the magnetic moment. Natural resonance at high frequencies can contribute to the absorption of high-frequency electromagnetic waves. The natural resonance frequency correlates with the coercive force iHc. The coercive force of the powder described in JP 2020-152979 A is 31 kA / m or less. This powder is not suitable for absorbing extremely high-frequency electromagnetic waves.

[0007] An object of the present invention is to provide a powder for a magnetic member capable of absorbing electromagnetic waves having extremely high frequencies. [Means for solving the problem]

[0008] The hard magnetic powder according to the present invention is composed of a large number of flat particles. The material of these particles is a rare earth metal-transition metal-B alloy. The maximum aspect ratio of this powder is 5.0 or more.

[0009] Preferably, the alloy contains Nd as the rare earth metal and Fe as the transition element.

[0010] Preferably, the alloy comprises: Nd: 10.8 atomic% or more and 16.0 atomic% or less B: 5.4 atomic% or more and 9.0 atomic% or less C: 0.3 atomic% or more and 1.0 atomic% or less and O: 15 atomic% or less The balance is Fe and unavoidable impurities.

[0011] Preferably, the powder has a coercive force iHc of 90 kA / m or more. Preferably, the powder has a median diameter D50 of 5 μm or more and 60 μm or less. Preferably, the powder has a tap density TD of 0.50 g / cm. 3 More than 3.50g / cm 3 The following is the result.

[0012] According to another aspect, the magnetic member of the present invention comprises a matrix based on a polymer and a hard magnetic powder dispersed in the matrix. The hard magnetic powder is composed of a large number of flat particles. The material of the particles is a rare earth metal-transition metal-B alloy. The maximum aspect ratio of the hard magnetic powder is 5.0 or more. Effect of the Invention

[0013] In a magnetic member in which the hard magnetic powder according to the present invention is used, extremely high frequencies can be absorbed. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a part of a magnetic member according to one embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged view showing flat particles contained in the magnetic member of FIG. [Diagram 3] FIG. 3 is a backscattered electron image showing a cross section of a particle of the powder according to Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, the present invention will be described in detail based on preferred embodiments with reference to the drawings as appropriate.

[0016] [Magnetic sheet] FIG. 1 shows a magnetic sheet 2 (magnetic member). This magnetic sheet 2 is made of a polymer composition. This magnetic sheet 2 has a base polymer matrix 4 and powder dispersed in this matrix 4. The base polymer is rubber or resin. The powder is a collection of many particles 6.

[0017] [Particle shape] Fig. 2 shows a cross section of one particle 6. In Fig. 1, the reference symbol L1 indicates the length of the major axis of the particle 6, and the reference symbol T1 indicates the thickness of the particle 6. The length L1 is greater than the thickness T1. In other words, the particle 6 is flat.

[0018] The flat particles 6 have shape anisotropy. This anisotropy increases the real permeability μ' of the magnetic member. Furthermore, in a magnetic sheet 2 containing flat particles 6 with a small thickness T1, eddy current loss is suppressed, so relaxation of the real permeability μ' is unlikely to occur. The magnetic sheet 2 containing these flat particles 6 can absorb high-frequency electromagnetic waves.

[0019] Maximum aspect ratio The maximum aspect ratio of this powder is 5.0 or more. In a powder with a maximum aspect ratio of 5.0 or more, the particles are significantly distorted during flattening. Therefore, the coercive force of this powder is large. In a powder with a maximum aspect ratio of 5.0 or more, the shape anisotropy of the particles 6 is large. Furthermore, in a magnetic sheet 2 containing a powder with a maximum aspect ratio of 5.0 or more and a small particle thickness, eddy current loss is suppressed. Therefore, a magnetic sheet 2 containing a powder with a maximum aspect ratio of 5.0 or more can absorb high-frequency electromagnetic waves.

[0020] From the viewpoint of electromagnetic wave absorption in the high frequency range, the maximum aspect ratio is more preferably 8.0 or more, and particularly preferably 10.0 or more. The maximum aspect ratio is preferably 100 or less. In a magnetic member using a powder with a maximum aspect ratio of 100 or less, the particles 6 are prevented from coming into contact with other particles 6, and loss due to eddy currents is prevented. From this viewpoint, the maximum aspect ratio is more preferably 50 or less, and particularly preferably 30 or less.

[0021] To measure the aspect ratio, a resin-embedded sample is used that allows observation of the thickness direction of flat particles 6. This sample is polished, and the polished surface is observed with a scanning electron microscope (SEM). The magnification of the image during observation is 1000 times. The obtained backscattered electron image data is subjected to image analysis. This image data is binarized using image analysis software. When the binarized image of particle 6 is approximated to an ellipse, the ratio of the length of the major axis to the length of the minor axis of this ellipse is the aspect ratio of this particle 6. The largest aspect ratio (maximum aspect ratio) is selected from the aspect ratios of the many binarized particles obtained in the four fields of view.

[0022] [Material] The material of the flat particles 6 is a rare earth metal-transition metal-B alloy. This alloy contains a rare earth metal M1, a transition metal M2, and boron B. The metal structure of this alloy is an intermetallic compound (M12M2 14 B). This intermetallic compound contributes to the high coercive force of the powder.

[0023] Preferred rare earth metals M1 include Ce, Pr, Nd, Sm, Gd, Tb, Dy, Ho, Er, Ho, Er, Tm, and Y. Two or more rare earth metals M1 may be used in combination. Preferred transition metals M2 include Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zr, Nb, Mo, and W. Two or more transition metals M2 may be used in combination.

[0024] [Preferred alloy] A particularly preferred rare earth metal M1 is Nd. A particularly preferred transition metal M2 is Fe. In other words, a Nd-Fe-B alloy is particularly preferred. The metal structure of this alloy is an intermetallic compound (Nd2Fe 14 B). This intermetallic compound contributes to the high coercive force of the powder.

[0025] The preferred alloy is an Fe-based alloy. The Fe-based alloy has Nd: 10.8 atomic% or more and 16.0 atomic% or less B: 5.4 atomic% or more and 9.0 atomic% or less C: 0.3 atomic% or more and 1.0 atomic% or less and O: 15 atomic% or less Preferably, the balance is Fe and unavoidable impurities.

[0026] [Neodymium (Nd)] This alloy contains a large amount of B, but the main phase that constitutes the metal structure is Nd2Fe 14 B, Nd-rich phase, and a small amount of αFe phase. These phases are crystalline phases, not amorphous phases. Nd is an intermetallic compound (Nd2Fe 14B). Powder containing this intermetallic compound has high saturation magnetization and high coercive force. From this viewpoint, in the present invention, the Nd content is specified to be 10.8 atomic % or more. This content is more preferably 10.9 atomic % or more, and particularly preferably 11.1 atomic % or more. Excess Nd forms excess intermetallic compounds (Nd2Fe 14 B) is precipitated. Excessive precipitation impairs the ductility of the alloy and hinders processing into flat grains with a large aspect ratio. From the viewpoint of ductility, the Nd content is specified to be 16.0 atomic % or less in the present invention. This content is more preferably 15.0 atomic % or less, and particularly preferably 14.0 atomic % or less.

[0027] [Boron (B)] B is an intermetallic compound (Nd2Fe 14 B) is an essential element for the formation of the intermetallic compound. A powder containing this intermetallic compound has high saturation magnetization and high coercive force. From this viewpoint, in the present invention, the B content is specified to be 5.4 atomic % or more. This content is more preferably 5.6 atomic % or more, and particularly preferably 6.3 atomic % or more. The B content is preferably 9.0 atomic % or less, more preferably 8.5 atomic % or less, and particularly preferably 7.9 atomic % or less.

[0028] [Carbon (C)] C is a particularly important element in the present invention. C is mixed into the alloy due to the organic solvent used in the flattening process. C is mainly present in the vicinity of the surface of the flat particle 6. According to the knowledge obtained by the present inventor, the incorporation of C achieves high coercive force of the powder. It is presumed that the reason for this is that the compound obtained by combining C with Nd contributes to the coercive force. From the viewpoint of coercive force, in the present invention, the C content is specified to be 0.3 atomic % or more. This content is particularly preferably 0.4 atomic % or more. The incorporation of C is accompanied by the incorporation of O. As described later, excessive incorporation of O is not preferred. From this viewpoint, in the present invention, the C content is specified to be 1.0 atomic % or less. This content is more preferably 0.9 atomic % or less, and particularly preferably 0.8 atomic % or less.

[0029] Oxygen O inevitably gets mixed into the alloy during atomization and flattening. O reacts with Nd to form oxides, typically Nd2O3. The formation of these oxides is Nd2Fe 14 This leads to a decrease in the amount of B formed, which inhibits the coercivity of the powder. From the viewpoint of coercivity, the O content is specified to be 15 atomic % or less in the present invention. This content is more preferably 13 atomic % or less, and particularly preferably 11 atomic % or less.

[0030] [Coercivity iHc] Coercive force iHc is the strength of an external magnetic field required to return a magnetized magnetic material to an unmagnetized state. A magnetic sheet 2 containing a powder with a large coercive force iHc can absorb high-frequency electromagnetic waves. From this perspective, the coercive force iHc of the powder is preferably 90 kA / m or more, more preferably 100 kA / m or more, and particularly preferably 150 kA / m or more. This powder is hard magnetic.

[0031] The coercive force is measured by a vibrating sample magnetometer (VSM) under the following measurement conditions: Maximum applied magnetic field: 1204kA / m Powder mass: approx. 70mg The direction of the applied magnetic field is the longitudinal direction of the flat particle 6 .

[0032] [Median diameter D50] From the viewpoint of obtaining a homogeneous magnetic sheet 2 having a smooth surface, the median diameter D50 of the powder is preferably 60 μm or less, more preferably 50 μm or less, and particularly preferably 40 μm or less. From the viewpoint of coercive force, the median diameter D50 is preferably 5 μm or more, more preferably 6.3 μm or more, and particularly preferably 10 μm or more.

[0033] The median diameter D50 is the diameter of the particle 6 at the point where the cumulative curve is 50% when the total volume of the powder is 100%. The median diameter D50 is measured, for example, by a laser diffraction / scattering particle size distribution measuring device "Microtrac MT3000" manufactured by Nikkiso Co., Ltd. The powder is poured into the cell of this device together with pure water, and the median diameter D50 is detected based on the light scattering information of the particle 6.

[0034] [Tap density TD] From the viewpoint of obtaining a magnetic sheet 2 that is homogeneous and has a smooth surface, the tap density TD of the powder is 3.50 g / cm 3 Less than 3.20 g / cm is preferred. 3 Less than 2.91 g / cm is more preferable. 3 The following is particularly preferred: the tap density TD is 0.50 g / cm 3 The above is preferred.

[0035] In the measurement of tap density TD, approximately 20 g of powder is tapped into a volume of 100 cm 3 The measurement conditions are as follows: Drop height: 10mm Number of taps: 200

[0036] [Powder production] The powder according to the present invention is obtained by subjecting a raw material powder to a flattening process. The raw material powder can be obtained by gas atomization, water atomization, disk atomization, pulverization, etc. Gas atomization is preferred. In the gas atomization method, the cooling rate is relatively slow. In the gas atomization method, oxidation is small.

[0037] In the gas atomization method, the raw metal is heated and melted to obtain molten metal. This molten metal flows out of a nozzle. A gas (typically argon gas) is sprayed onto the molten metal. The energy of the gas breaks the molten metal into droplets, which cool as they fall. The droplets solidify to form particles. In the gas atomization method, the molten metal instantly turns into droplets and is cooled at the same time, resulting in a uniform, fine structure. Moreover, because the droplets are formed continuously, the compositional difference between particles is extremely small.

[0038] The raw powder is classified and heat-treated as necessary. The raw powder is then flattened. A typical flattening process is performed using an attritor. A flattening aid such as stearic acid may be used in the flattening process. In the flattening process using a flattening aid, flat powder with a large median diameter D50 can be obtained. The powder after the flattening process is classified as necessary. It is preferable that the powder after the flattening process is not heat-treated. This is because heat treatment reduces the coercive force.

[0039] [Magnetic component molding] To obtain a magnetic member (electromagnetic wave absorber) from this powder, the powder is first kneaded with a base polymer such as resin or rubber to obtain a polymer composition. A known method can be used for kneading. For example, kneading can be performed using an internal kneader, an open roll, or the like.

[0040] Next, a magnetic member is molded from this polymer composition. A known method can be used for molding. Molding can be performed by compression molding, injection molding, extrusion molding, rolling, etc. A typical magnetic member is a magnetic sheet 2 (electromagnetic wave absorbing sheet) shown in Figure 1. Shapes such as a ring, a cube, a rectangular solid, a cylinder, etc. can be used for the magnetic member.

[0041] Various chemicals may be compounded with the base polymer along with the powder. Examples of chemicals include processing aids such as lubricants and binders. The polymer composition may also contain flame retardants. EXAMPLES

[0042] The effects of the present invention will be clarified by the following examples, but the present invention should not be construed as being limited based on the description of these examples.

[0043] [Example 1] A raw powder was obtained by gas atomization and classification. 500 g of this raw powder was put into an attritor. 1.4 kg of naphthenic solvent was also put into this attritor. SUJ2 of 4.8 mm was used as the powder media. The powder was flattened by this attritor to obtain a powder consisting of flat particles. The composition, median diameter D50, tap density TD, and maximum aspect ratio of this powder are shown in Table 1 below. The contents of Nd, Fe, and B were measured on the powder after atomization but before flattening. For this measurement, an ICP (Inductive Coupled Plasma) emission spectroscopic analyzer was used. The contents of C and O were measured on the powder after flattening. The content of C was measured by a combustion-infrared absorption method. The content of O was measured by an inert gas conveying fusion infrared absorption method. A backscattered electron image of this powder is shown in FIG. 3. FIG. 3 shows a cross section of a particle.

[0044] [Examples 2-6 and Comparative Examples 1-7] Powders of Examples 2-6 and Comparative Examples 1-7 were produced in the same manner as in Example 1, except that the compositions were as shown in Table 1 below. A flattening aid was used for flattening the powders of Example 6 and Comparative Example 3. The powders of Comparative Examples 5-7 were subjected to a heat treatment. In this heat treatment, the powders were held in a high-temperature argon gas atmosphere for 1 hour and then slowly cooled. The atmosphere temperature is shown in Table 1 below. The C and O contents in the powders of Comparative Examples 5-7 were measured after the heat treatment.

[0045] [Measurement of coercive force] The coercive force of the powder was measured by the method described above, and the results are shown in Table 1 below.

[0046] [Table 1]

[0047] As shown in Table 1, the coercive force of the powder of each example is large. From these evaluation results, the superiority of the present invention is clear. [Industrial Applicability]

[0048] The powder according to the present invention is suitable for a variety of magnetic components. [Explanation of symbols]

[0049] 2. Magnetic sheet 4. Matrix 6...Flattened particles

Claims

1. It consists of many flat particles, The material of these particles is Nd: 10.8 at% or more and 16.0 at% or less B: 5.4 at% or more and 9.0 at% or less C: 0.3 at% or more and 1.0 at% or less and O: 15 atomic% or less with the balance being Fe and unavoidable impurities, The maximum aspect ratio is 5.0 or more; A hard magnetic powder having a coercive force iHc of 90 kA / m or more.

2. 2. The hard magnetic powder according to claim 1, wherein the alloy contains Nd as the rare earth metal and Fe as the transition element.

3. 3. The hard magnetic powder according to claim 1, wherein the volume-based median diameter D50 is 5 μm or more and 60 μm or less.

4. Tap density TD is 0.50 g / cm 3 3.50g / cm or more 3 4. The hard magnetic powder according to claim 1, wherein:

5. The magnetic material has a matrix based on a polymer and a hard magnetic powder dispersed in the matrix, The hard magnetic powder is composed of a large number of flat particles, The material of these particles is Nd: 10.8 at% or more and 16.0 at% or less B: 5.4 at% or more and 9.0 at% or less C: 0.3 at% or more and 1.0 at% or less and O: 15 atomic% or less with the balance being Fe and unavoidable impurities, The hard magnetic powder has a maximum aspect ratio of 5.0 or more, A magnetic member, wherein the hard magnetic powder has a coercive force iHc of 90 kA / m or more.

Citation Information

Patent Citations

  • JP152979A

  • Rare-earth bonded magnet and its manufacture

    JP1999224811A

  • Flat leaf-like rare earth-iron-boron magnet alloy particle powder for bonded magnet, manufacture thereof and the bonded magnet

    JP1999288807A

  • Alloy powder for magnetic member

    JP2020152979A