Photosensitive transfer material, resin pattern manufacturing method, circuit wiring manufacturing method, and touch panel manufacturing method
The photosensitive transfer material stabilizes resin pattern line widths by controlling double bond reaction region ratios, addressing the issue of line width changes over time in existing resin compositions, ensuring consistent pattern formation in touch panel manufacturing.
Patent Information
- Application Number
- JP2022550420
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-17
- Filing Date
- 2021-08-19
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2041-08-19
AI Technical Summary
The existing photosensitive resin compositions used in forming patterns for conductive layers in touch panels experience significant changes in line width over time due to prolonged exposure times, especially in roll-to-roll processes, leading to inconsistent pattern formation.
A photosensitive transfer material with a photosensitive resin layer containing an alkali-soluble resin, ethylenically unsaturated compound, and photopolymerization initiator, where the ratio of double bond reaction region widths before and after exposure is controlled to minimize line width changes, using specific exposure amounts and photopolymerization components to stabilize the pattern.
The solution ensures minimal changes in resin pattern line width over time, enabling consistent and reliable pattern formation even with extended exposure times, suitable for roll-to-roll processes.
Smart Images

Figure 0007596393000029 
Figure 0007596393000030 
Figure 0007596393000031
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a photosensitive transfer material, a method for manufacturing a resin pattern, a method for manufacturing circuit wiring, and a method for manufacturing a touch panel. [Background technology]
[0002] In display devices (such as organic electroluminescence (EL) display devices and liquid crystal display devices) equipped with a touch panel such as a capacitance-type input device, conductive layer patterns such as an electrode pattern corresponding to the sensor of the visible area, and wiring of the peripheral wiring portion and the extraction wiring portion are provided inside the touch panel. Generally, in forming a patterned layer, the number of steps required to obtain a desired pattern shape is small, and therefore a method is widely used in which a layer of a photosensitive resin composition provided on a substrate using a photosensitive transfer material is exposed through a mask having a desired pattern and then developed.
[0003] Furthermore, as a conventional photosensitive resin composition, the one described in Patent Document 1 is known. Patent Document 1 describes a photosensitive resin composition in which, when an exposure curing reaction is carried out so that the reaction rate of an ethylenically unsaturated compound contained as a photosensitive component on the exposed surface is 70%, and then the plate is stored in a dark place, the reaction rate of the unsaturated compound on the entire plate does not substantially change, and the difference in local reaction rate between the exposed surface and the non-exposed surface remains 20% or more even after 24 hours.
[0004] Patent Document 1: Japanese Patent Application Laid-Open No. 2001-356493 Summary of the Invention [Problem to be solved by the invention]
[0005] In the wiring formation process using a photosensitive transfer material, when a photosensitive resin layer attached to a substrate having a conductive layer is exposed to light, the time elapsed from the completion of exposure to development varies for each photosensitive resin layer, and in some cases this can be as long as several hours. In addition, the exposed photosensitive resin layer may not be developed immediately but may be left for a certain period of time, in which case the time elapsed from the completion of exposure is further extended. The above-mentioned post-exposure leave-and-leave time tends to be long, especially when a roll-to-roll process is performed, because it takes time to transport the roll from the unwinding section to the core section.
[0006] An object of one embodiment of the present invention is to provide a photosensitive transfer material that exhibits little change in line width of a resin pattern over time after exposure. Another problem to be solved by another embodiment of the present invention is to provide a method for producing a resin pattern using the above-mentioned photosensitive transfer material, a method for producing circuit wiring, and a method for producing a touch panel. [Means for solving the problem]
[0007] Means for solving the above problems include the following aspects. <1> The present invention has a temporary support and a photosensitive resin layer containing an alkali-soluble resin, an ethylenically unsaturated compound, and a photopolymerization initiator, and the photosensitive resin layer is heated to a temperature of 1000° C. for 24 hours at 100° C. for 24 hours. 2 After exposing a 10 μm / 10 μm line and space pattern with an exposure dose Ep in units of 10 μm, the double bond reaction region width W3 after 3 hours and the double bond reaction region width W after 24 hours were measured. 24 But, W 24 A photosensitive transfer material that satisfies / W3≦1.05. W3 and W 24 is the double bond reaction region width obtained by secondary ion mass spectrometry after dyeing the exposed photosensitive transfer material with bromine, The above Ep satisfies Ep = 2 × Eb, The above Eb is measured after the photosensitive resin layer is attached to the substrate and then projected through a 15-step step wedge at an illuminance of 20 mW / cm 2Exposure dose of 180 mJ / cm 2 The exposure amount is the amount of exposure that indicates the number of steps that gives a remaining layer thickness that is within ±1% of the layer thickness of the photosensitive resin layer after exposure and development. <2> The photosensitive resin layer was exposed to a 10 μm / 10 μm line and space pattern at the exposure dose Ep, and the double bond reaction region width W3 after 3 hours and the double bond reaction region width W after 72 hours were measured. 72 But, W 72 / W3≦1.10 <1> 2. The photosensitive transfer material according to claim 1 . W 72 is the double bond reaction region width obtained by secondary ion mass spectrometry after bromine dyeing of the exposed photosensitive transfer material. <3> The ethylenically unsaturated compound includes an ethylenically unsaturated compound having a bisphenol structure. <1> or <2> 2. The photosensitive transfer material according to claim 1 . <4> The photopolymerization initiator contains a biimidazole compound and a benzophenone compound. <1> ~ <3> 10. The photosensitive transfer material according to claim 9, <5> The photosensitive resin layer further contains a polymerization inhibitor. <1> ~ <4> 10. The photosensitive transfer material according to claim 9, <6> The polymerization inhibitor contains at least one compound selected from the group consisting of phenothiazine, phenoxazine, and compounds having a hindered phenol structure. <5> 2. The photosensitive transfer material according to claim 1 . <7> When the content of the photopolymerization initiator in the photosensitive resin layer is Rc and the content of the polymerization inhibitor is Rd, the mass ratio Rd / Rc is 0.02 or more and 0.1 or less. <5> or <6> 2. The photosensitive transfer material according to claim 1 . <8> The mass ratio Rd / Rc is 0.03 or more and 0.05 or less. <7> 2. The photosensitive transfer material according to claim 1 . <9> <1> ~ <8> a step of contacting and laminating the outermost layer of the photosensitive transfer material described in any one of the above items 1 to 5 with a substrate, a step of exposing the photosensitive resin layer to a pattern, and a step of developing the exposed photosensitive resin layer to form a resin pattern, in that order. <10> At least a part of the resin pattern includes a line and space pattern, and the width of at least one pair of a line and a space in the line and space pattern is 20 μm or less in total. <9> 2. A method for producing a resin pattern according to claim 1 . <11> <1> ~ <8> a step of contacting and laminating the outermost layer of the photosensitive transfer material described in any one of the above items 1 to 5, the photosensitive resin layer being on the side of the temporary support that has the photosensitive resin layer, with a substrate having a conductive layer; a step of exposing the photosensitive resin layer to a pattern; a step of developing the exposed photosensitive resin layer to form a resin pattern; and a step of etching the substrate in an area where the resin pattern is not arranged. <12> <1> ~ <8> A method for manufacturing a touch panel, comprising the steps of: contacting and laminating the outermost layer of the photosensitive transfer material described in any one of claims 1 to 5, the side having a photosensitive resin layer relative to the temporary support, with a substrate having a conductive layer; exposing the photosensitive resin layer to a pattern; developing the exposed photosensitive resin layer to form a resin pattern; and etching the substrate in an area where the resin pattern is not arranged. Effect of the Invention
[0008] According to one embodiment of the present invention, it is possible to provide a photosensitive transfer material in which the change in line width of the resin pattern is small with the passage of time after exposure to light. According to other embodiments of the present invention, it is possible to provide a method for producing a resin pattern using the above-mentioned photosensitive transfer material, a method for producing circuit wiring, and a method for producing a touch panel. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic diagram showing an example of the configuration of the photosensitive transfer material of the first embodiment. [Diagram 2] FIG. 11 is a schematic diagram showing an example of the configuration of a photosensitive transfer material according to a second embodiment. [Diagram 3] FIG. 2 is a schematic plan view showing pattern A. [Figure 4] FIG. 13 is a schematic plan view showing pattern B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present disclosure will be described below with reference to the accompanying drawings, in which reference numerals may be omitted. In addition, in this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower limit and upper limit. In addition, in this specification, "(meth)acrylic" refers to both or either of acrylic and methacrylic, "(meth)acrylate" refers to both or either of acrylate and methacrylate, and "(meth)acryloyl" refers to both or either of acryloyl and methacryloyl. Furthermore, in this specification, when a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the corresponding substances present in the composition, unless otherwise specified. In this specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved. In the description of groups (atomic groups) in this specification, when there is no indication of substituted or unsubstituted, the term encompasses both unsubstituted and substituted groups. For example, the term "alkyl group" encompasses not only alkyl groups without a substituent (unsubstituted alkyl groups) but also alkyl groups with a substituent (substituted alkyl groups). In this specification, unless otherwise specified, "exposure" includes not only exposure using light, but also drawing using particle beams such as electron beams and ion beams. In addition, examples of light used for exposure generally include the bright line spectrum of a mercury lamp, far ultraviolet light represented by an excimer laser, extreme ultraviolet light (EUV light), X-rays, electron beams, and other actinic rays (active energy rays). In addition, chemical structural formulas in this specification may be described as simplified structural formulas in which hydrogen atoms are omitted. In the present disclosure, "mass %" and "weight %" are synonymous, and "parts by mass" and "parts by weight" are synonymous. Also, in the present disclosure, combinations of two or more preferred aspects are more preferred aspects. In addition, unless otherwise specified, the weight average molecular weight (Mw) and number average molecular weight (Mn) in the present disclosure are molecular weights detected by a gel permeation chromatography (GPC) analyzer using columns of TSKgel GMHxL, TSKgel G4000HxL, or TSKgel G2000HxL (all product names manufactured by Tosoh Corporation) in a solvent of THF (tetrahydrofuran) and a differential refractometer, and converted using polystyrene as a standard substance. In this specification, the term "total solid content" refers to the total mass of the components excluding the solvent from the entire composition of the composition. As described above, the term "solid content" refers to the components excluding the solvent, and may be, for example, solid or liquid at 25°C.
[0011] (Photosensitive transfer material) The photosensitive transfer material according to the present disclosure has a temporary support and a photosensitive resin layer containing an alkali-soluble resin, an ethylenically unsaturated compound, and a photopolymerization initiator, and the photosensitive resin layer is heated to a temperature of 1000° C. for 1 hour at 40° C. for 1 hour at 40° C. 2 After exposing a 10 μm / 10 μm line and space pattern with an exposure dose Ep in units of 10 μm, the double bond reaction region width W3 after 3 hours and the double bond reaction region width W after 24 hours were measured. 24 But, W 24 / W3≦1.05 is satisfied. W3 and W 24 is the double bond reaction region width obtained by secondary ion mass spectrometry after dyeing the exposed photosensitive transfer material with bromine, The above Ep satisfies Ep = 2 × Eb, The above Eb is measured after the photosensitive resin layer is attached to the substrate and then projected through a 15-step step wedge at an illuminance of 20 mW / cm 2 Exposure dose of 180 mJ / cm 2 The exposure amount is the amount of exposure that indicates the number of steps that gives a remaining layer thickness that is within ±1% of the layer thickness of the photosensitive resin layer after exposure and development.
[0012] As a result of detailed investigations, the inventors have found that a conventional photosensitive transfer material having a negative-type photosensitive resin layer formed from the photosensitive resin composition described in Patent Document 1 has a problem in that the line width of the resin pattern changes significantly with the passage of time after exposure to light. In the photosensitive transfer material according to the present disclosure, the photosensitive resin layer is 2 After exposing a 10 μm / 10 μm line and space pattern with an exposure dose Ep in units of 10 μm, the double bond reaction region width W3 after 3 hours and the double bond reaction region width W after 24 hours were measured. 24 But, W 24 By satisfying / W3≦1.05, the photosensitive resin layer in which the above-mentioned change in double bond reaction region width over time is small has the reaction sufficiently suppressed in the half-exposed portion at the end of the exposed region, and the difference in the polymerization reaction degree between the exposed region and the unexposed region is large. Therefore, even if there is some variation in the development conditions such as the delay time after exposure, dissolution during development in the region where the polymerization reaction has progressed sufficiently is suppressed, and the line width change of the resin pattern with the passage of the delay time after exposure (also called "line width change with delay time") is estimated to be small.
[0013] The photosensitive transfer material according to the present disclosure is a photosensitive resin layer having a photoirradiation efficiency of 1000 nm or less, mJ / cm 2 After exposing a 10 μm / 10 μm line and space pattern with an exposure dose Ep in units of 10 μm, the double bond reaction region width W3 after 3 hours and the double bond reaction region width W after 24 hours were measured. 24 But, W 24 / W3≦1.05 is satisfied. W3 and W 24 is the double bond reaction region width obtained by secondary ion mass spectrometry after dyeing the exposed photosensitive transfer material with bromine, The above Ep satisfies Ep = 2 × Eb, The above Eb is measured after the photosensitive resin layer is attached to the substrate and then projected through a 15-step step wedge at an illuminance of 20 mW / cm 2 Exposure dose of 180 mJ / cm 2The exposure amount is the amount of exposure that indicates the number of steps that gives a remaining layer thickness that is within ±1% of the layer thickness of the photosensitive resin layer after exposure and development.
[0014] The photosensitive transfer material according to the present disclosure has a line width change with time, a line width change of the resin pattern with a change in development temperature (also called "development temperature line width change"), and sensitivity. 24 It is preferable that W3≦1.04 is satisfied, and W 24 It is more preferable that W3≦1.03 be satisfied, and 1.00≦W 24 It is particularly preferable that / W3≦1.03 be satisfied.
[0015] In addition, in terms of line width change with time to exposure and line width change with development temperature, the photosensitive transfer material according to the present disclosure is exposed to a 10 μm / 10 μm line and space pattern at the exposure dose Ep, and then the double bond reaction region width W3 after 3 hours has elapsed and the double bond reaction region width W after 72 hours have elapsed. 72 But, W 72 It is preferable that W3≦1.15 is satisfied, and W 72 It is more preferable that / W3≦1.10 is satisfied, and 1.00≦W 72 It is particularly preferable that / W3≦1.10 be satisfied. In addition, W 72 is the double bond reaction region width obtained by secondary ion mass spectrometry after bromine dyeing of the exposed photosensitive transfer material.
[0016] The method for measuring Eb and the method for calculating Ep in this disclosure are shown below. The photosensitive transfer material is laminated onto a substrate (a 200 nm thick copper layer formed by sputtering on a 100 μm polyethylene terephthalate (PET) film) using a sheet laminator. The lamination conditions are a roll temperature of 100°C, a lamination speed of 2 m / min, and a lamination pressure of 0.5 MPa. A 15-step step wedge (manufactured by Fujifilm Corporation) was placed on the temporary support of the laminated photosensitive transfer material, and 20 mW / cm 2 180mJ / cm 2After the exposure, the support is peeled off, and the layer is developed for 30 seconds in a 0.9% by mass aqueous solution of sodium carbonate at 25° C., and Eb (Eb is calculated from the remaining film thickness at each step after the photosensitive resin layer is attached to the substrate and then exposed to light at an illumination intensity of 20 mW / cm through a 15-step wedge) is calculated. 2 Exposure dose of 180 mJ / cm 2 The exposure amount (indicating the number of steps that gives a remaining layer thickness that is within ±1% of the layer thickness of the photosensitive resin layer after exposure and development) is determined. In addition, the calculated Eb (mJ / cm 2 ) and calculate Ep (mJ / cm 2 ) is calculated. Ep = 2 × Eb
[0017] The exposed photosensitive transfer material in this disclosure is dyed with bromine, and the double bond reaction region width W3, W4 obtained by secondary ion mass spectrometry 24 and W 72 The measurement method is shown below. The photosensitive transfer material is laminated onto the substrate (a 100 μm PET film with a 200 nm thick copper layer formed by sputtering) using a sheet laminator. The lamination conditions are: roll temperature 100° C., lamination speed 2 m / min, and lamination pressure 0.5 MPa. The photosensitive transfer material laminated on the substrate was brought into contact with a photomask having a line and space of 10 μm / 10 μm on the temporary support, and Ep=2×Eb (mJ / cm 2 ) for 3, 24 or 72 hours after exposure, the temporary support, thermoplastic resin layer and intermediate layer are peeled off with tape, 5 mL of bromine water (0.2%) is dispensed into a 50 mL container, the sample is fixed in the container so as not to come into contact with the dispensed solution and left to stand for 5 minutes at room temperature (25°C). The sample is then stored under high vacuum for half a day to degas the residual bromine. This produces a sample with bromine-modified carbon-carbon double bonds. The sample was analyzed by secondary ion mass spectrometry (ION-TOF SIMS 5, primary ion source: Bi 3+(30kV, measurement range: 50mm, surface resolution: 512×512pixel, integration: 32 times, measurement mode: high spatial resolution mode (Fast Imaging), charging correction: using electron gun) - Evaluate the area of the area. C2HBr - The width of the area with low strength is measured at three points, and the average of the three measurements is taken to determine the width of the area where polymerization has progressed, W3, W 24 Or W 72 Let us assume that.
[0018] The above-mentioned Eb value in the photosensitive transfer material according to the present disclosure is set to 20 mJ / cm from the viewpoints of delay time line width change, development temperature line width change, and sensitivity. 2 ~200mJ / cm 2 and preferably 30 mJ / cm 2 ~150mJ / cm 2 More preferably, 35 mJ / cm 2 ~100mJ / cm 2 and preferably 35 mJ / cm 2 ~70mJ / cm 2 It is particularly preferred that:
[0019] Furthermore, the value of W3 in the photosensitive transfer material according to the present disclosure is preferably 9.0 μm to 10.5 μm, more preferably 9.2 μm to 10.3 μm, and particularly preferably 9.5 μm to 10.2 μm, from the viewpoints of the delay time line width change, the development temperature line width change, and the sensitivity. W in the photosensitive transfer material according to the present disclosure 24 From the viewpoints of the delay time line width change, the development temperature line width change, and the sensitivity, the value of is preferably from 9.0 μm to 11.0 μm, more preferably from 9.3 μm to 10.7 μm, and particularly preferably from 9.5 μm to 10.5 μm. W in the photosensitive transfer material according to the present disclosure 72 From the viewpoints of the delay time line width change, the development temperature line width change, and the sensitivity, the value of is preferably from 9.0 μm to 12.0 μm, more preferably from 9.5 μm to 11.5 μm, and particularly preferably from 9.7 μm to 11.0 μm.
[0020] The photosensitive transfer material according to the present disclosure has a temporary support and a photosensitive resin layer containing an alkali-soluble resin, an ethylenically unsaturated compound, and a photopolymerization initiator. In the photosensitive transfer material, the temporary support and the photosensitive resin layer may be laminated directly without any other layer therebetween, or may be laminated via another layer. Also, another layer may be laminated on the surface of the photosensitive resin layer opposite to the surface facing the temporary support. Examples of layers other than the temporary support and the photosensitive resin layer include a thermoplastic resin layer, an intermediate layer, and a protective film.
[0021] An example of the embodiment of the photosensitive transfer material according to the present disclosure is shown below, but is not limited thereto. (1) "Temporary support / photosensitive resin layer / refractive index adjusting layer / protective film" (2) "Temporary support / photosensitive resin layer / protective film" (3) "Temporary support / intermediate layer / photosensitive resin layer / protective film" (4) "Temporary support / thermoplastic resin layer / intermediate layer / photosensitive resin layer / protective film" In each of the above configurations, the photosensitive resin layer is preferably a negative photosensitive resin layer. It is also preferable that the photosensitive resin layer is a colored resin layer. The photosensitive transfer material according to the present disclosure may be used as a photosensitive transfer material for a wiring protection film, or as a photosensitive transfer material for an etching resist, as described below. When the photosensitive transfer material is used as a wiring protective film, the photosensitive transfer material preferably has the structure of, for example, the above-mentioned structure (1) or (2). When the photosensitive transfer material is used as an etching resist, the photosensitive transfer material preferably has the configurations (2) to (4) described above.
[0022] In the photosensitive transfer material, when the photosensitive resin layer further has other layers on the side opposite the temporary support side, the total thickness of the other layers arranged on the side opposite the temporary support side of the photosensitive resin layer is preferably 0.1% to 30%, and more preferably 0.1% to 20%, of the thickness of the photosensitive resin layer.
[0023] The photosensitive transfer material according to the present disclosure will be described below by taking an example of a specific embodiment. The photosensitive transfer material of the first embodiment below is suitable for use as a photosensitive transfer material for etching resist, and the photosensitive transfer material of the second embodiment below is suitable for use as a photosensitive transfer material for wiring protection film.
[0024] Photosensitive transfer material of the first embodiment An example of the photosensitive transfer material of the first embodiment will be described below. The photosensitive transfer material 20 shown in FIG. 1 has a temporary support 11, a transfer layer 12 including a thermoplastic resin layer 13, an intermediate layer 15 and a photosensitive resin layer 17, and a protective film 19, in this order. Although the photosensitive transfer material 320 shown in FIG. 1 has a protective film 19 disposed thereon, the protective film 19 does not necessarily have to be disposed. Further, the photosensitive transfer material 20 shown in FIG. 1 has a form in which the thermoplastic resin layer 13 and the intermediate layer 15 are arranged, but the thermoplastic resin layer 13 and the intermediate layer 15 do not necessarily have to be arranged. Each element constituting the photosensitive transfer material of the first embodiment will be described below.
[0025] [Temporary Support] The photosensitive transfer material used in the present disclosure has a temporary support. The temporary support is a peelable support that supports the photosensitive resin layer or the laminate including the photosensitive resin layer.
[0026] The temporary support preferably has light transmittance from the viewpoint of enabling exposure of the photosensitive resin layer through the temporary support when the photosensitive resin layer is subjected to patternwise exposure. In this specification, "having light transmittance" means that the transmittance of light of the wavelength used for patternwise exposure is 50% or more. From the viewpoint of improving the exposure sensitivity of the photosensitive resin layer, the temporary support preferably has a transmittance of 60% or more, more preferably 70% or more, for light having a wavelength used for pattern exposure (more preferably a wavelength of 365 nm). The transmittance of a layer of a photosensitive transfer material is the ratio of the intensity of emitted light that has passed through the layer to the intensity of incident light when light is incident in a direction perpendicular to the main surface of the layer (thickness direction), and is measured using an MCPD Series manufactured by Otsuka Electronics Co., Ltd.
[0027] Examples of materials constituting the temporary support include a glass substrate, a resin film, and paper. From the viewpoints of strength, flexibility, and light transmittance, a resin film is preferred. Examples of the resin film include a polyethylene terephthalate (PET) film, a cellulose triacetate film, a polystyrene film, and a polycarbonate film. Among these, a PET film is preferable, and a biaxially stretched PET film is more preferable.
[0028] The thickness (layer thickness) of the temporary support is not particularly limited, and may be selected according to the material from the standpoints of strength as a support, flexibility required for bonding to a substrate for forming circuit wiring, and light transmittance required in the initial exposure step. The thickness of the temporary support is preferably in the range of 5 μm to 100 μm, and from the viewpoints of ease of handling and versatility, more preferably in the range of 10 μm to 50 μm, further preferably in the range of 10 μm to 20 μm, particularly preferably in the range of 10 μm to 16 μm. The thickness of the temporary support is preferably 50 μm or less, and more preferably 25 μm or less, from the viewpoints of resolution and linearity when exposure is performed through the temporary support.
[0029] Furthermore, the film used as the temporary support is preferably free from deformations such as wrinkles, scratches, defects, and the like. From the viewpoint of pattern formability during pattern exposure through the temporary support and the transparency of the temporary support, it is preferable that the number of fine particles, foreign matter, defects, precipitates, etc. contained in the temporary support is small. The number of fine particles, foreign matter, and defects with a diameter of 1 μm or more is 50 / 10 mm. 2 It is preferable that the number of pieces is less than 10 pieces / 10 mm. 2 More preferably, 3 pieces / 10 mm or less. 2 More preferably, 0 pieces / 10 mm or less. 2 It is particularly preferred that:
[0030] Preferred embodiments of the temporary support are described, for example, in paragraphs 0017 to 0018 of JP 2014-85643 A, paragraphs 0019 to 0026 of JP 2016-27363 A, paragraphs 0041 to 0057 of WO 2012 / 081680 A, paragraphs 0029 to 0040 of WO 2018 / 179370 A, and paragraphs 0012 to 0032 of JP 2019-101405 A, the contents of which are incorporated herein by reference.
[0031] [Photosensitive resin layer] The photosensitive transfer material according to the present disclosure has a photosensitive resin layer. The photosensitive resin layer is preferably a negative photosensitive resin layer in which the solubility of the exposed portion in a developer is reduced by exposure, and the non-exposed portion is removed by development.
[0032] The photosensitive resin layer contains an alkali-soluble resin, an ethylenically unsaturated compound, and a photopolymerization initiator, and from the viewpoints of the laying time line width change, the development temperature line width change, and the sensitivity, it preferably contains an alkali-soluble resin, an ethylenically unsaturated compound, a biimidazole compound, and a benzophenone compound, and more preferably contains an alkali-soluble resin, an ethylenically unsaturated compound, a hexaarylbiimidazole compound, and a benzophenone compound. In addition, from the viewpoints of the delay time line width change, the development temperature line width change, and the sensitivity, it is preferable that the photosensitive resin layer further contains a polymerization inhibitor. The photosensitive resin layer preferably contains, relative to the total mass of the photosensitive resin layer, 10% by mass to 90% by mass of an alkali-soluble resin, 5% by mass to 70% by mass of an ethylenically unsaturated compound, and 0.01% by mass to 20% by mass of a photopolymerization initiator. Each component will be described in turn below.
[0033] <Alkali-soluble resin> The photosensitive resin layer contains an alkali-soluble resin. In this specification, the term "alkali-soluble" means that the solubility in 100 g of a 1% by mass aqueous solution of sodium carbonate at 22°C is 0.1 g or more. The alkali-soluble resin is not particularly limited, and suitable examples thereof include known alkali-soluble resins used in etching resists. The alkali-soluble resin is preferably a binder polymer. The alkali-soluble resin is preferably an alkali-soluble resin having an acid group. Among these, the alkali-soluble resin is preferably polymer A described below.
[0034] -Polymer A- The alkali-soluble resin preferably contains polymer A. The acid value of polymer A is preferably 220 mgKOH / g or less, more preferably less than 200 mgKOH / g, and even more preferably less than 190 mgKOH / g, from the viewpoint of suppressing swelling of the photosensitive resin layer by the developer and thereby achieving superior resolution. The lower limit of the acid value of polymer A is not particularly limited, but from the viewpoint of better developability, it is preferably 60 mgKOH / g or more, more preferably 120 mgKOH / g or more, even more preferably 150 mgKOH / g or more, and particularly preferably 170 mgKOH / g or more.
[0035] The acid value is the mass [mg] of potassium hydroxide required to neutralize 1 g of sample. In this specification, the unit is expressed as mgKOH / g. The acid value can be calculated, for example, from the average content of acid groups in the compound. The acid value of the polymer A may be adjusted by changing the type of structural unit constituting the polymer A and the content of the structural unit containing an acid group.
[0036] The weight average molecular weight of the polymer A is preferably 5,000 to 500,000. The weight average molecular weight of 500,000 or less is preferable from the viewpoint of improving resolution and developability. The weight average molecular weight is more preferably 100,000 or less, even more preferably 60,000 or less, and particularly preferably 50,000 or less. On the other hand, the weight average molecular weight of 5,000 or more is preferable from the viewpoint of controlling the properties of the development aggregate and the properties of the unexposed film such as edge fuse property and cut chip property when the film is made into a photosensitive resin laminate. The weight average molecular weight is more preferably 10,000 or more, even more preferably 20,000 or more, and particularly preferably 30,000 or more. The edge fuse property refers to the degree of the tendency of the photosensitive resin layer to protrude from the end face of the roll when the photosensitive transfer material is wound into a roll. The cut chip property refers to the degree of the tendency of the chip to fly when the unexposed film is cut with a cutter. If these chips adhere to the upper surface of the photosensitive resin laminate, they will be transferred to a mask in a subsequent exposure step, causing defective products. The polydispersity of polymer A is preferably 1.0 to 6.0, more preferably 1.0 to 5.0, even more preferably 1.0 to 4.0, and particularly preferably 1.0 to 3.0. In the present disclosure, the molecular weight is a value measured using gel permeation chromatography. The polydispersity is the ratio of the weight average molecular weight to the number average molecular weight (weight average molecular weight / number average molecular weight).
[0037] From the viewpoint of suppressing line width thickening and deterioration of resolution when the focal position is shifted during exposure, the photosensitive resin layer preferably contains a monomer component having an aromatic hydrocarbon group as the polymer A. Examples of such aromatic hydrocarbon groups include substituted or unsubstituted phenyl groups and substituted or unsubstituted aralkyl groups. The content of the monomer component having an aromatic hydrocarbon group in the polymer A is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, particularly preferably 45% by mass or more, and most preferably 50% by mass or more, based on the total mass of all monomer components. The upper limit is not particularly limited, but is preferably 95% by mass or less, more preferably 85% by mass or less. In the case where multiple types of polymer A are contained, the content of the monomer component having an aromatic hydrocarbon group was calculated as a weight average value.
[0038] Examples of the monomer having an aromatic hydrocarbon group include a monomer having an aralkyl group, styrene, and a polymerizable styrene derivative (e.g., methylstyrene, vinyltoluene, tert-butoxystyrene, acetoxystyrene, 4-vinylbenzoic acid, styrene dimer, styrene trimer, etc.). Among them, a monomer having an aralkyl group or styrene is preferred. In one embodiment, when the monomer component having an aromatic hydrocarbon group in the polymer A is styrene, the content of the styrene monomer component is preferably 20% by mass to 50% by mass, more preferably 25% by mass to 45% by mass, further preferably 30% by mass to 40% by mass, and particularly preferably 30% by mass to 35% by mass, based on the total mass of all the monomer components.
[0039] Examples of the aralkyl group include a substituted or unsubstituted phenylalkyl group (excluding a benzyl group) and a substituted or unsubstituted benzyl group, with a substituted or unsubstituted benzyl group being preferred.
[0040] An example of the monomer having a phenylalkyl group is phenylethyl (meth)acrylate.
[0041] Examples of the monomer having a benzyl group include (meth)acrylates having a benzyl group, such as benzyl (meth)acrylate and chlorobenzyl (meth)acrylate; and vinyl monomers having a benzyl group, such as vinylbenzyl chloride and vinylbenzyl alcohol. Among these, benzyl (meth)acrylate is preferred. In one embodiment, when the monomer component having an aromatic hydrocarbon group in the polymer A is benzyl (meth)acrylate, the content of the benzyl (meth)acrylate monomer component is preferably 50% by mass to 95% by mass, more preferably 60% by mass to 90% by mass, further preferably 70% by mass to 90% by mass, and particularly preferably 75% by mass to 90% by mass, based on the total mass of all monomer components.
[0042] The polymer A containing a monomer component having an aromatic hydrocarbon group is preferably obtained by polymerizing a monomer having an aromatic hydrocarbon group with at least one type of a first monomer described below and / or at least one type of a second monomer described below.
[0043] The polymer A not containing a monomer component having an aromatic hydrocarbon group is preferably obtained by polymerizing at least one type of first monomer described later, and more preferably obtained by copolymerizing at least one type of first monomer with at least one type of second monomer described later.
[0044] The first monomer is a monomer having a carboxy group in the molecule. Examples of the first monomer include (meth)acrylic acid, fumaric acid, cinnamic acid, crotonic acid, itaconic acid, 4-vinylbenzoic acid, maleic anhydride, and maleic acid half ester. Among these, (meth)acrylic acid is preferred. The content of the first monomer in polymer A is preferably 5% by mass to 50% by mass, more preferably 10% by mass to 40% by mass, and even more preferably 15% by mass to 30% by mass, based on the total mass of all monomer components.
[0045] The copolymerization ratio of the first monomer is preferably 10% by mass to 50% by mass based on the total mass of all monomer components. The copolymerization ratio of 10% by mass or more is preferable from the viewpoint of achieving good developability and controlling edge fusing properties, and is more preferably 15% by mass or more, and even more preferably 20% by mass or more. The copolymerization ratio of 50% by mass or less is preferable from the viewpoint of high resolution and foot shape of the resist pattern, and furthermore from the viewpoint of chemical resistance of the resist pattern, and from these viewpoints, it is more preferably 35% by mass or less, even more preferably 30% by mass or less, and particularly preferably 27% by mass or less.
[0046] The second monomer is a monomer that is non-acidic and has at least one polymerizable unsaturated group in the molecule. Examples of the second monomer include (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, cyclohexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; esters of vinyl alcohol such as vinyl acetate; and (meth)acrylonitrile. Among them, methyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-butyl (meth)acrylate are preferred, and methyl (meth)acrylate is particularly preferred. The content of the second monomer in polymer A is preferably 5% by mass to 60% by mass, more preferably 15% by mass to 50% by mass, and even more preferably 20% by mass to 45% by mass, based on the total mass of all monomer components.
[0047] It is preferable to contain a monomer having an aralkyl group and / or styrene as a monomer from the viewpoint of suppressing line width thickening and deterioration of resolution when the focal position is shifted during exposure. For example, a copolymer containing methacrylic acid, benzyl methacrylate, and styrene, or a copolymer containing methacrylic acid, methyl methacrylate, benzyl methacrylate, and styrene is preferable. In one embodiment, the polymer A is preferably a polymer containing 25% to 40% by mass of a monomer component having an aromatic hydrocarbon group, 20% to 35% by mass of a first monomer component, and 30% to 45% by mass of a second monomer component. In another embodiment, the polymer A is preferably a polymer containing 70% to 90% by mass of a monomer component having an aromatic hydrocarbon group, and 10% to 25% by mass of the first monomer component.
[0048] The polymer A may be used alone or in combination of two or more. When using in combination of two or more, it is preferable to use two types of polymer A containing a monomer component having an aromatic hydrocarbon group as a mixture, or to use a polymer A containing a monomer component having an aromatic hydrocarbon group and a polymer A not containing a monomer component having an aromatic hydrocarbon group as a mixture. In the latter case, the proportion of the polymer A containing a monomer component having an aromatic hydrocarbon group is preferably 50% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, and more preferably 90% by mass or more, based on the total amount of the polymer A.
[0049] The polymer A may have a branched structure or an alicyclic structure in the side chain. The polymer A may also have a linear structure in the side chain. For example, a branched structure or an alicyclic structure can be introduced into the side chain of the polymer (A) by using a monomer containing a group having a branched structure in the side chain or a monomer containing a group having an alicyclic structure in the side chain. The group having an alicyclic structure may be monocyclic or polycyclic.
[0050] Examples of monomers containing a group having a branched structure in the side chain include isopropyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isoamyl (meth)acrylate, tert-amyl (meth)acrylate, sec-amyl (meth)acrylate, 2-octyl (meth)acrylate, 3-octyl (meth)acrylate, and tert-octyl (meth)acrylate. Among the above, isopropyl (meth)acrylate, isobutyl (meth)acrylate, and tert-butyl methacrylate are preferred, and isopropyl methacrylate or tert-butyl methacrylate are more preferred.
[0051] Specific examples of the monomer containing a group having an alicyclic structure in the side chain include a monomer having a monocyclic aliphatic hydrocarbon group, a monomer having a polycyclic aliphatic hydrocarbon group, and a (meth)acrylate having an alicyclic hydrocarbon group having 5 to 20 carbon atoms. Examples of monomers containing a group having an alicyclic structure in the side chain include (bicyclo[2.2.1]heptyl-2)(meth)acrylate, 1-adamantyl (meth)acrylate, 2-adamantyl (meth)acrylate, 3-methyl-1-adamantyl (meth)acrylate, 3,5-dimethyl-1-adamantyl (meth)acrylate, 3-ethyladamantyl (meth)acrylate, 3-methyl-5-ethyl-1-adamantyl (meth)acrylate, 3,5,8-triethyl-1-adamantyl (meth)acrylate, 3,5-dimethyl-8-ethyl-1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, 2-ethyl-2-adamantyl (meth)acrylate, Examples of the acrylates include 3-hydroxy-1-adamantyl (meth)acrylate, octahydro-4,7-menthanoinden-5-yl (meth)acrylate, octahydro-4,7-menthanoinden-1-ylmethyl (meth)acrylate, 1-menthyl (meth)acrylate, tricyclodecane (meth)acrylate, 3-hydroxy-2,6,6-trimethyl-bicyclo[3.1.1]heptyl (meth)acrylate, 3,7,7-trimethyl-4-hydroxy-bicyclo[4.1.0]heptyl (meth)acrylate, (nor)bornyl (meth)acrylate, isobornyl (meth)acrylate, fenchyl (meth)acrylate, 2,2,5-trimethylcyclohexyl (meth)acrylate, and cyclohexyl (meth)acrylate.Among the above, cyclohexyl (meth)acrylate, (nor)bornyl (meth)acrylate, isobornyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-adamantyl (meth)acrylate, fenchyl (meth)acrylate, 1-menthyl (meth)acrylate and tricyclodecane (meth)acrylate are preferred, and cyclohexyl (meth)acrylate, (nor)bornyl (meth)acrylate, isobornyl (meth)acrylate, 2-adamantyl (meth)acrylate and tricyclodecane (meth)acrylate are more preferred.
[0052] The synthesis of polymer A is preferably carried out by adding an appropriate amount of a radical polymerization initiator such as benzoyl peroxide or azoisobutyronitrile to a solution obtained by diluting one or more of the monomers described above with a solvent such as acetone, methyl ethyl ketone, or isopropanol, and heating and stirring the solution. In some cases, the synthesis is carried out while dropping a part of the mixture into the reaction solution. After the reaction is completed, further solvent may be added to adjust the concentration to the desired level. As a synthesis method, bulk polymerization, suspension polymerization, or emulsion polymerization may be used in addition to solution polymerization.
[0053] The glass transition temperature Tg of the polymer A is preferably 30° C. or more and 135° C. or less. By using the polymer A having a Tg of 135° C. or less in the photosensitive resin layer, it is possible to suppress line width thickening and deterioration of resolution when the focal position is shifted during exposure. From this viewpoint, the Tg of the polymer A is more preferably 130° C. or less, further preferably 120° C. or less, and particularly preferably 110° C. or less. In addition, it is preferable to use the polymer A having a Tg of 30° C. or more from the viewpoint of improving edge fuse resistance. From this viewpoint, the Tg of the polymer A is more preferably 40° C. or more, further preferably 50° C. or more, particularly preferably 60° C. or more, and most preferably 70° C. or more.
[0054] The photosensitive resin layer may contain a resin other than the alkali-soluble resin. Examples of resins other than alkali-soluble resins include acrylic resins, styrene-acrylic copolymers (with the styrene content being 40 mass% or less), polyurethane resins, polyvinyl alcohol, polyvinyl formal, polyamide resins, polyester resins, polyamide resins, epoxy resins, polyacetal resins, polyhydroxystyrene resins, polyimide resins, polybenzoxazole resins, polysiloxane resins, polyethyleneimines, polyallylamine, and polyalkylene glycols.
[0055] The alkali-soluble resins may be used alone or in combination of two or more. The proportion of the alkali-soluble resin to the total mass of the photosensitive resin layer is preferably in the range of 10% by mass to 90% by mass, more preferably 30% by mass to 70% by mass, and even more preferably 40% by mass to 60% by mass. It is preferable to set the proportion of the alkali-soluble resin to the photosensitive resin layer to 90% by mass or less from the viewpoint of controlling the development time. On the other hand, it is preferable to set the proportion of the alkali-soluble resin to the photosensitive resin layer to 10% by mass or more from the viewpoint of improving edge fuse resistance.
[0056] (Ethylenically unsaturated compounds) The photosensitive resin layer contains an ethylenically unsaturated compound. In this specification, the term "ethylenically unsaturated compound" refers to a compound which is polymerized by the action of a photopolymerization initiator described below, and which is different from the above-mentioned alkali-soluble resin.
[0057] The ethylenically unsaturated compound is preferably an ethylenically unsaturated compound. The ethylenically unsaturated compound is a component that contributes to the photosensitivity (that is, photocurability) of the negative photosensitive resin layer and the strength of the cured film. Also, an ethylenically unsaturated compound is a compound having one or more ethylenically unsaturated groups. The photosensitive resin layer preferably contains, as the ethylenically unsaturated compound, a di- or higher functional ethylenically unsaturated compound. Here, the di- or higher functional ethylenically unsaturated compound means a compound having two or more ethylenically unsaturated groups in one molecule. The ethylenically unsaturated group is more preferably a (meth)acryloyl group. As the ethylenically unsaturated compound, a (meth)acrylate compound is preferred. In addition, from the viewpoints of delay time line width change, development temperature line width change, and sensitivity, it is preferable that the ethylenically unsaturated compound contains an ethylenically unsaturated compound having a bisphenol structure. A preferred example of the ethylenically unsaturated compound having a bisphenol structure is the ethylenically unsaturated compound B1 having a bisphenol structure described below.
[0058] The photosensitive resin layer preferably contains an ethylenically unsaturated compound having a polymerizable group. The polymerizable group of the ethylenically unsaturated compound is not particularly limited as long as it is a group that participates in a polymerization reaction, and examples thereof include groups having an ethylenically unsaturated group such as a vinyl group, an acryloyl group, a methacryloyl group, a styryl group, or a maleimide group; and groups having a cationic polymerizable group such as an epoxy group or an oxetane group. The polymerizable group is preferably a group having an ethylenically unsaturated group, and more preferably an acryloyl group or a methacryloyl group.
[0059] The ethylenically unsaturated compound preferably contains a compound having two or more ethylenically unsaturated groups in one molecule (a polyfunctional ethylenically unsaturated compound) in that the photosensitive resin layer has better photosensitivity. From the viewpoint of obtaining superior resolution and peelability, the number of ethylenically unsaturated groups that the ethylenically unsaturated compound has in one molecule is preferably 6 or less, more preferably 3 or less, and even more preferably 2 or less.
[0060] The photosensitive resin layer preferably contains a bifunctional or trifunctional ethylenically unsaturated compound having two or three ethylenically unsaturated groups in one molecule, and more preferably contains a bifunctional ethylenically unsaturated compound having two ethylenically unsaturated groups in one molecule, in that the photosensitive resin layer has a better balance between photosensitivity, resolution, and peelability. The content of the bifunctional ethylenically unsaturated compound in the photosensitive resin layer relative to the content of the ethylenically unsaturated compound is preferably 60% by mass or more, more preferably more than 70% by mass, and even more preferably 90% by mass or more, from the viewpoint of excellent peelability. The upper limit is not particularly limited, and may be 100% by mass. That is, all of the ethylenically unsaturated compounds contained in the photosensitive resin layer may be bifunctional ethylenically unsaturated compounds. Moreover, the ethylenically unsaturated compound is preferably a (meth)acrylate compound having a (meth)acryloyl group as a polymerizable group.
[0061] -Ethylenically unsaturated compounds B1- The photosensitive resin layer preferably contains an ethylenically unsaturated compound B1 having an aromatic ring and two ethylenically unsaturated groups. The ethylenically unsaturated compound B1 is a bifunctional ethylenically unsaturated compound having one or more aromatic rings in one molecule among the above-mentioned ethylenically unsaturated compounds.
[0062] In the photosensitive resin layer, the mass ratio of the content of the ethylenically unsaturated compound B1 to the content of the ethylenically unsaturated compound is preferably 40% by mass or more, more preferably 50% by mass or more, even more preferably 55% by mass or more, and particularly preferably 60% by mass or more, from the viewpoint of better resolution. The upper limit is not particularly limited, but from the viewpoint of peelability, it is preferably 99% by mass or less, more preferably 95% by mass or less, even more preferably 90% by mass or less, and particularly preferably 85% by mass or less.
[0063] The aromatic ring of the ethylenically unsaturated compound B1 can be exemplified by aromatic hydrocarbon rings such as benzene ring, naphthalene ring and anthracene ring, aromatic heterocycles such as thiophene ring, furan ring, pyrrole ring, imidazole ring, triazole ring and pyridine ring, and condensed rings thereof, preferably aromatic hydrocarbon ring, more preferably benzene ring.The aromatic ring may have a substituent. The ethylenically unsaturated compound B1 may have only one aromatic ring or may have two or more aromatic rings.
[0064] The ethylenically unsaturated compound B1 preferably has a bisphenol structure, since this suppresses swelling of the photosensitive resin layer due to a developer, thereby improving the resolution. Examples of the bisphenol structure include a bisphenol A structure derived from bisphenol A (2,2-bis(4-hydroxyphenyl)propane), a bisphenol F structure derived from bisphenol F (2,2-bis(4-hydroxyphenyl)methane), and a bisphenol B structure derived from bisphenol B (2,2-bis(4-hydroxyphenyl)butane), with the bisphenol A structure being preferred.
[0065] The ethylenically unsaturated compound B1 having a bisphenol structure includes, for example, a compound having a bisphenol structure and two polymerizable groups (preferably (meth)acryloyl groups) bonded to both ends of the bisphenol structure. Both ends of the bisphenol structure may be directly bonded to the two polymerizable groups, or may be bonded via one or more alkyleneoxy groups. The alkyleneoxy groups added to both ends of the bisphenol structure are preferably ethyleneoxy or propyleneoxy, more preferably ethyleneoxy. The number of alkyleneoxy groups added to the bisphenol structure is not particularly limited, but is preferably 4 to 16, more preferably 6 to 14 per molecule. The ethylenically unsaturated compound B1 having a bisphenol structure is described in paragraphs 0072 to 0080 of JP2016-224162A, the contents of which are incorporated herein by reference.
[0066] As the ethylenically unsaturated compound B1, a difunctional ethylenically unsaturated compound having a bisphenol A structure is preferable, and 2,2-bis(4-((meth)acryloxypolyalkoxy)phenyl)propane is more preferable. Examples of 2,2-bis(4-((meth)acryloxypolyalkoxy)phenyl)propane include 2,2-bis(4-(methacryloxydiethoxy)phenyl)propane (FA-324M, Hitachi Chemical Co., Ltd.), 2,2-bis(4-(methacryloxyethoxypropoxy)phenyl)propane, 2,2-bis(4-(methacryloxypentaethoxy)phenyl)propane (BPE-500, Shin-Nakamura Chemical Co., Ltd.), and 2,2-bis(4-(methacryloxydodecaethoxy)phenyl)propane. Examples of the ethoxylated bisphenol A diacrylate include 2,2-bis(4-(tetrapropoxy)phenyl)propane (FA-3200MY, manufactured by Hitachi Chemical Co., Ltd.), 2,2-bis(4-(methacryloxypentadecaethoxy)phenyl)propane (BPE-1300, manufactured by Shin-Nakamura Chemical Co., Ltd.), 2,2-bis(4-(methacryloxydiethoxy)phenyl)propane (BPE-200, manufactured by Shin-Nakamura Chemical Co., Ltd.), and ethoxylated (10) bisphenol A diacrylate (NK Ester A-BPE-10, manufactured by Shin-Nakamura Chemical Co., Ltd.).
[0067] As the ethylenically unsaturated compound B1, from the viewpoints of the delay time line width change, the development temperature line width change, and the sensitivity, it is preferable to include a compound represented by the following formula (Bis).
[0068] [ka]
[0069] In formula (Bis), R1 and R2 each independently represent a hydrogen atom or a methyl group, A is C2H4, B is C3H6, n1 and n3 each independently represent an integer of 1 to 39, and n1+n3 is an integer of 2 to 40, n2 and n4 each independently represent an integer of 0 to 29, and n2+n4 is an integer of 0 to 30, and the arrangement of the repeating units -(AO)- and -(BO)- may be random or block. In the case of block, either -(AO)- or -(BO)- may be on the bisphenol structure side. In one embodiment, n1+n2+n3+n4 is preferably an integer of 2 to 20, more preferably an integer of 2 to 16, and even more preferably an integer of 4 to 12. Furthermore, n2+n4 is preferably an integer of 0 to 10, more preferably an integer of 0 to 4, and even more preferably an integer of 0 to 2, and particularly preferably 0.
[0070] The ethylenically unsaturated compound B1 may be used alone or in combination of two or more kinds. The content of the ethylenically unsaturated compound B1 in the photosensitive resin layer is preferably 10% by mass or more, more preferably 20% by mass or more, based on the total mass of the photosensitive resin layer, from the viewpoint of better resolution. The upper limit is not particularly limited, but is preferably 70% by mass or less, more preferably 60% by mass or less, from the viewpoint of transferability and edge fusion (phenomenon in which components in the photosensitive resin layer bleed out from the edge of the photosensitive transfer material).
[0071] The photosensitive resin layer may contain an ethylenically unsaturated compound other than the above-mentioned ethylenically unsaturated compound B1. The ethylenically unsaturated compound other than the ethylenically unsaturated compound B1 is not particularly limited and can be appropriately selected from known compounds. For example, it can be a compound having one ethylenically unsaturated group in one molecule (monofunctional ethylenically unsaturated compound), a bifunctional ethylenically unsaturated compound without an aromatic ring, and a trifunctional or higher ethylenically unsaturated compound.
[0072] Examples of monofunctional ethylenically unsaturated compounds include ethyl (meth)acrylate, ethylhexyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and phenoxyethyl (meth)acrylate.
[0073] Examples of difunctional ethylenically unsaturated compounds having no aromatic ring include alkylene glycol di(meth)acrylate, polyalkylene glycol di(meth)acrylate, urethane di(meth)acrylate, and trimethylolpropane diacrylate. Examples of alkylene glycol di(meth)acrylates include tricyclodecane dimethanol diacrylate (A-DCP, manufactured by Shin-Nakamura Chemical Co., Ltd.), tricyclodecane dimethanol dimethacrylate (DCP, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,9-nonanediol diacrylate (A-NOD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,6-hexanediol diacrylate (A-HD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), ethylene glycol dimethacrylate, 1,10-decanediol diacrylate, and neopentyl glycol di(meth)acrylate. Examples of polyalkylene glycol di(meth)acrylates include polyethylene glycol di(meth)acrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, and polypropylene glycol di(meth)acrylate. Examples of urethane di(meth)acrylate include propylene oxide modified urethane di(meth)acrylate, and ethylene oxide and propylene oxide modified urethane di(meth)acrylate. Commercially available products include 8UX-015A (manufactured by Taisei Fine Chemical Co., Ltd.), UA-32P (manufactured by Shin-Nakamura Chemical Co., Ltd.), and UA-1100H (manufactured by Shin-Nakamura Chemical Co., Ltd.).
[0074] Examples of tri- or higher functional ethylenically unsaturated compounds include dipentaerythritol (tri / tetra / penta / hexa)(meth)acrylate, pentaerythritol (tri / tetra)(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, trimethylolethane tri(meth)acrylate, isocyanuric acid tri(meth)acrylate, glycerin tri(meth)acrylate, and alkylene oxide modified versions of these. Here, "(tri / tetra / penta / hexa)(meth)acrylate" is a concept that includes tri(meth)acrylate, tetra(meth)acrylate, penta(meth)acrylate, and hexa(meth)acrylate, and "(tri / tetra)(meth)acrylate" is a concept that includes tri(meth)acrylate and tetra(meth)acrylate. In one embodiment, the photosensitive resin layer preferably contains the above-mentioned ethylenically unsaturated compound B1 and a trifunctional or higher ethylenically unsaturated compound, and more preferably contains the above-mentioned ethylenically unsaturated compound B1 and two or more trifunctional or higher ethylenically unsaturated compounds. In this case, the mass ratio of the ethylenically unsaturated compound B1 to the trifunctional or higher ethylenically unsaturated compound is preferably (total mass of the ethylenically unsaturated compound B1):(total mass of the trifunctional or higher ethylenically unsaturated compounds)=1:1 to 5:1, more preferably 1.2:1 to 4:1, and even more preferably 1.5:1 to 3:1. In one embodiment, the photosensitive resin layer preferably contains the above-mentioned ethylenically unsaturated compound B1 and two or more kinds of trifunctional ethylenically unsaturated compounds.
[0075] Examples of alkylene oxide modified trifunctional or higher ethylenically unsaturated compounds include caprolactone modified (meth)acrylate compounds (KAYARAD (registered trademark) DPCA-20 manufactured by Nippon Kayaku Co., Ltd., A-9300-1CL manufactured by Shin-Nakamura Chemical Co., Ltd., etc.), alkylene oxide modified (meth)acrylate compounds (KAYARAD RP-1040 manufactured by Nippon Kayaku Co., Ltd., ATM-35E and A-9300 manufactured by Shin-Nakamura Chemical Co., Ltd., EBECRYL (registered trademark) manufactured by Daicel-Allnex Corporation), etc. No. 135, etc.), ethoxylated glycerin triacrylate (A-GLY-9E, etc., manufactured by Shin-Nakamura Chemical Co., Ltd.), Aronix (registered trademark) TO-2349 (manufactured by Toagosei Co., Ltd.), Aronix M-520 (manufactured by Toagosei Co., Ltd.), and Aronix M-510 (manufactured by Toagosei Co., Ltd.).
[0076] As the ethylenically unsaturated compound other than the ethylenically unsaturated compound B1, the ethylenically unsaturated compounds having an acid group described in paragraphs 0025 to 0030 of JP-A No. 2004-239942 may be used.
[0077] From the viewpoints of resolution and linearity, the ratio Mm / Mb of the content Mm of the ethylenically unsaturated compound in the photosensitive resin layer to the content Mb of the alkali-soluble resin is preferably 1.0 or less, more preferably 0.9 or less, and particularly preferably 0.5 or more and 0.9 or less. Moreover, from the viewpoints of curability and resolution, the ethylenically unsaturated compound in the photosensitive resin layer preferably contains a (meth)acrylic compound. Furthermore, from the viewpoints of curability, resolution and linearity, it is more preferable that the ethylenically unsaturated compound in the photosensitive resin layer contains a (meth)acrylic compound, and that the content of the acrylic compound relative to the total mass of the (meth)acrylic compounds contained in the photosensitive resin layer is 60 mass% or less.
[0078] The molecular weight (weight average molecular weight (Mw) when the molecular weight has a distribution) of the ethylenically unsaturated compound including the ethylenically unsaturated compound B1 is preferably from 200 to 3,000, more preferably from 280 to 2,200, and even more preferably from 300 to 2,200.
[0079] The ethylenically unsaturated compounds may be used alone or in combination of two or more. The content of the ethylenically unsaturated compound in the photosensitive resin layer is preferably 10% by mass to 70% by mass, more preferably 20% by mass to 60% by mass, and further preferably 20% by mass to 50% by mass, based on the total mass of the photosensitive resin layer.
[0080] <Photopolymerization initiator> The photosensitive resin layer contains a photopolymerization initiator. The photopolymerization initiator is a compound that initiates polymerization of an ethylenically unsaturated compound when exposed to active light such as ultraviolet light, visible light, and X-rays. The photopolymerization initiator is not particularly limited, and any known photopolymerization initiator can be used. The photopolymerization initiator in the present disclosure also includes a sensitizer. Examples of the photopolymerization initiator include a photoradical polymerization initiator and a photocationic polymerization initiator, and a photoradical polymerization initiator is preferred.
[0081] Examples of the photoradical polymerization initiator include a photopolymerization initiator having an oxime ester structure, a photopolymerization initiator having an α-aminoalkylphenone structure, a photopolymerization initiator having an α-hydroxyalkylphenone structure, a photopolymerization initiator having an acylphosphine oxide structure, a photopolymerization initiator having an N-phenylglycine structure, and a biimidazole compound.
[0082] Among these, from the viewpoints of the laying time line width change, the development temperature line width change, and the sensitivity, the photopolymerization initiator preferably contains a biimidazole compound, and more preferably contains a biimidazole compound and a benzophenone compound. As the biimidazole compound, a hexaarylbiimidazole compound is preferably used. Examples of the biimidazole compound include 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, and 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer.
[0083] The photosensitive resin layer may contain, as a photopolymerization initiator, one type of biimidazole compound alone or two or more types of biimidazole compounds. From the viewpoints of line width change with exposure time, line width change with development temperature, and sensitivity, the content of the biimidazole compound is preferably 1 mass % or more, more preferably 2 mass % or more, even more preferably 3 mass % to 10 mass %, and particularly preferably 5 mass % to 10 mass %, relative to the total mass of the photosensitive resin layer.
[0084] From the viewpoints of the delay time line width change, the development temperature line width change, and the sensitivity, the photopolymerization initiator preferably contains a benzophenone compound, and more preferably contains a dialkylaminobenzophenone compound. Examples of the benzophenone compound include benzophenone, 2-methylbenzophenone, 3-methylbenzophenone, 4-methylbenzophenone, 4-methoxybenzophenone, 2-chlorobenzophenone, 4-chlorobenzophenone, 4-bromobenzophenone, 2-carboxybenzophenone, 2-ethoxycarbonylbenzophenone, benzophenonetetracarboxylic acid or its tetramethyl ester, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(dicyclohexylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(dihydroxyethylamino)benzophenone, 4-methoxy-4'-dimethylaminobenzophenone, 4,4'-dimethoxybenzophenone, 4-dimethylaminobenzophenone, 4-phenylbenzophenone, isophthalophenone, and 4-benzoyl-4'-methylphenyl sulfide.
[0085] The photosensitive resin layer may contain, as a photopolymerization initiator, one type of benzophenone compound alone or two or more types of benzophenone compounds. From the viewpoints of line width change with delay time, line width change at development temperature, and sensitivity, the content of the benzophenone compound is preferably 0.05% by mass to 5% by mass, more preferably 0.1% by mass to 2% by mass, even more preferably 0.2% by mass to 1.5% by mass, and particularly preferably 0.4% by mass to 0.8% by mass, relative to the total mass of the photosensitive resin layer. In addition, when a biimidazole compound and a benzophenone compound are contained as a photopolymerization initiator, the content of the benzophenone compound is preferably less than the content of the biimidazole compound from the viewpoints of the delay time line width change, the development temperature line width change, and the sensitivity.
[0086] As the photoradical polymerization initiator, for example, the polymerization initiators described in paragraphs 0031 to 0042 of JP-A No. 2011-95716 and paragraphs 0064 to 0081 of JP-A No. 2015-14783 may be used.
[0087] Examples of the photoradical polymerization initiator include ethyl dimethylaminobenzoate (DBE, CAS No. 10287-53-3), benzoin methyl ether, anisyl (p,p'-dimethoxybenzyl), TAZ-110 (trade name: manufactured by Midori Chemical Co., Ltd.), benzophenone, TAZ-111 (trade name: manufactured by Midori Chemical Co., Ltd.), Irgacure OXE01, OXE02, OXE03, OXE04 (manufactured by BASF), Omnirad 651 and 369 (trade names: manufactured by IGM Resins BV), and 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0088] Commercially available photoradical polymerization initiators include, for example, 1-[4-(phenylthio)phenyl]-1,2-octanedione-2-(O-benzoyloxime) (trade name: IRGACURE (registered trademark) OXE-01, manufactured by BASF), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(O-acetyloxime) (trade name: IRGACURE OXE-02, manufactured by BASF), IRGACURE OXE-03 (manufactured by BASF), 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone (trade name: Omnirad 379EG, manufactured by IGM Resins BV), 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one (trade name: Omnirad 907, manufactured by IGM Resins BV), 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one (trade name: Omnirad 127, manufactured by IGM Resins BV), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1 (trade name: Omnirad 369, manufactured by IGM Resins BV), 2-hydroxy-2-methyl-1-phenylpropan-1-one (trade name: Omnirad 1173, manufactured by IGM Resins BV), 1-hydroxycyclohexyl phenyl ketone (trade name: Omnirad 184, manufactured by IGM Resins BV), 2,2-dimethoxy-1,2-diphenylethan-1-one (trade name: Omnirad 651, manufactured by IGM Resins BV), BV), 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (trade name: Omnirad TPO H, IGM Resins BV), bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (trade name: Omnirad 819, IGM Resins BVExamples of photopolymerization initiators include oxime ester-based photopolymerization initiators (trade name: Lunar 6, manufactured by DKSH Japan Co., Ltd.), 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbisimidazole (2-(2-chlorophenyl)-4,5-diphenylimidazole dimer) (trade name: B-CIM, manufactured by Hampford Chemical Industry Co., Ltd.), and 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer (trade name: BCTB, manufactured by Tokyo Chemical Industry Co., Ltd.).
[0089] A photocationic polymerization initiator (photoacid generator) is a compound that generates an acid when exposed to actinic rays. As the photocationic polymerization initiator, a compound that responds to actinic rays having a wavelength of 300 nm or more, preferably 300 to 450 nm, and generates an acid is preferred, but the chemical structure is not limited. In addition, even if a photocationic polymerization initiator is not directly sensitive to actinic rays having a wavelength of 300 nm or more, it can be preferably used in combination with a sensitizer as long as it responds to actinic rays having a wavelength of 300 nm or more and generates an acid when used in combination with a sensitizer. As the photocationic polymerization initiator, a photocationic polymerization initiator that generates an acid having a pKa of 4 or less is preferable, a photocationic polymerization initiator that generates an acid having a pKa of 3 or less is more preferable, and a photocationic polymerization initiator that generates an acid having a pKa of 2 or less is particularly preferable. The lower limit of the pKa is not particularly set, but is preferably, for example, -10.0 or more.
[0090] The photocationic polymerization initiator includes an ionic photocationic polymerization initiator and a nonionic photocationic polymerization initiator. Examples of the ionic photocationic polymerization initiator include onium salt compounds such as diaryliodonium salts and triarylsulfonium salts, and quaternary ammonium salts. As the ionic photocationic polymerization initiator, the ionic photocationic polymerization initiators described in paragraphs 0114 to 0133 of JP-A-2014-85643 may be used.
[0091] Examples of nonionic photocationic polymerization initiators include trichloromethyl-s-triazines, diazomethane compounds, imide sulfonate compounds, and oxime sulfonate compounds. As trichloromethyl-s-triazines, diazomethane compounds, and imide sulfonate compounds, compounds described in paragraphs 0083 to 0088 of JP 2011-221494 A may be used. As oxime sulfonate compounds, compounds described in paragraphs 0084 to 0088 of WO 2018 / 179640 may be used.
[0092] The sensitizer is not particularly limited, and known sensitizers, dyes and pigments can be used. Examples of sensitizers include dialkylaminobenzophenone compounds, pyrazoline compounds, anthracene compounds, coumarin compounds, xanthone compounds, thioxanthone compounds, acridone compounds, oxazole compounds, benzoxazole compounds, thiazole compounds, benzothiazole compounds, triazole compounds (e.g., 1,2,4-triazole), stilbene compounds, triazine compounds, thiophene compounds, naphthalimide compounds, triarylamine compounds, and aminoacridine compounds.
[0093] The photosensitive resin layer may contain one type of photopolymerization initiator alone, or may contain two or more types of photopolymerization initiators. The content of the photopolymerization initiator in the photosensitive resin layer is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1.0% by mass or more, based on the total mass of the photosensitive resin layer. The upper limit is not particularly limited, but is preferably 10% by mass or less, and more preferably 5% by mass or less, based on the total mass of the photosensitive resin layer.
[0094] <Dye> From the viewpoints of visibility of exposed and unexposed parts, pattern visibility after development, and resolution, the photosensitive resin layer preferably contains a dye, and more preferably contains a dye (also simply referred to as "dye N") whose maximum absorption wavelength in the wavelength range of 400 nm to 780 nm during color development is 450 nm or more and whose maximum absorption wavelength changes with an acid, a base, or a radical. When dye N is contained, the adhesion with adjacent layers (for example, a temporary support and an intermediate layer) is improved, and the resolution is more excellent, although the detailed mechanism is unknown.
[0095] In this specification, the dye "whose maximum absorption wavelength changes due to an acid, a base, or a radical" may mean any of an embodiment in which a dye in a colored state is decolorized by an acid, a base, or a radical, a dye in a decolorized state is colored by an acid, a base, or a radical, and a dye in a colored state is changed to a colored state of another hue. Specifically, the dye N may be a compound that changes from a decolorized state to a colored state by exposure to light, or may be a compound that changes from a colored state to a decolored state by exposure to light. In this case, the dye may be a dye whose colored or decolored state changes when an acid, base, or radical is generated and acts in the photosensitive resin layer by exposure to light, or a dye whose colored or decolored state changes when the state (e.g., pH) in the photosensitive resin layer changes due to an acid, base, or radical. Alternatively, the dye may be a dye whose colored or decolored state changes when it is directly stimulated by an acid, base, or radical without exposure to light.
[0096] Among these, from the viewpoints of visibility and resolution of exposed and unexposed areas, dye N is preferably a dye whose maximum absorption wavelength changes in response to an acid or a radical, and more preferably a dye whose maximum absorption wavelength changes in response to a radical. From the viewpoints of visibility of exposed and unexposed areas and resolution, the photosensitive resin layer preferably contains both a dye N whose maximum absorption wavelength changes due to radicals, and a photoradical polymerization initiator. From the viewpoint of visibility of exposed and unexposed areas, dye N is preferably a dye that develops color in response to an acid, a base, or a radical.
[0097] An example of the color-developing mechanism of dye N in the present disclosure is an embodiment in which a photoradical polymerization initiator, a cationic photopolymerization initiator (photoacid generator), or a photobase generator is added to a photosensitive resin layer, and after exposure, a radical-reactive dye, an acid-reactive dye, or a base-reactive dye (e.g., a leuco dye) develops color due to a radical, acid, or base generated from the photoradical polymerization initiator, the photocationic photopolymerization initiator, or the photobase generator.
[0098] From the viewpoint of visibility of exposed and unexposed areas, dye N preferably has a maximum absorption wavelength of 550 nm or more in the wavelength range of 400 nm to 780 nm upon color development, more preferably 550 nm to 700 nm, and even more preferably 550 nm to 650 nm. Furthermore, dye N may have only one maximum absorption wavelength in the wavelength range of 400 nm to 780 nm when it develops color, or may have two or more maximum absorption wavelengths. When dye N has two or more maximum absorption wavelengths in the wavelength range of 400 nm to 780 nm when it develops color, the maximum absorption wavelength having the highest absorbance among the two or more maximum absorption wavelengths may be 450 nm or more.
[0099] The maximum absorption wavelength of dye N is obtained by measuring the transmission spectrum of a solution containing dye N (liquid temperature 25°C) in the range of 400 nm to 780 nm using a spectrophotometer UV3100 (manufactured by Shimadzu Corporation) in an atmospheric environment and detecting the wavelength at which the light intensity is minimum (maximum absorption wavelength).
[0100] Examples of the dye that develops or loses color upon exposure to light include leuco compounds. Examples of dyes that are decolorized by exposure to light include leuco compounds, diarylmethane dyes, oxazine dyes, xanthene dyes, iminonaphthoquinone dyes, azomethine dyes, and anthraquinone dyes. As the dye N, a leuco compound is preferable from the viewpoint of visibility of exposed and non-exposed areas.
[0101] Examples of the leuco compound include leuco compounds having a triarylmethane skeleton (triarylmethane-based dyes), leuco compounds having a spiropyran skeleton (spiropyran-based dyes), leuco compounds having a fluoran skeleton (fluoran-based dyes), leuco compounds having a diarylmethane skeleton (diarylmethane-based dyes), leuco compounds having a rhodamine lactam skeleton (rhodamine lactam-based dyes), leuco compounds having an indolylphthalide skeleton (indolylphthalide-based dyes), and leuco compounds having a leucoauramine skeleton (leucoauramine-based dyes). Among these, triarylmethane dyes or fluoran dyes are preferred, and leuco compounds having a triphenylmethane skeleton (triphenylmethane dyes) or fluoran dyes are more preferred.
[0102] From the viewpoint of visibility of the exposed and non-exposed parts, the leuco compound preferably has a lactone ring, a sultine ring, or a sultone ring. This allows the lactone ring, the sultine ring, or the sultone ring of the leuco compound to react with a radical generated from a photoradical polymerization initiator or an acid generated from a photocationic polymerization initiator, thereby changing the leuco compound to a ring-closed state to cause discoloration, or changing the leuco compound to a ring-open state to cause color development. The leuco compound is preferably a compound having a lactone ring, a sultine ring, or a sultone ring, which is opened by a radical or an acid to develop color, and more preferably a compound having a lactone ring, which is opened by a radical or an acid to develop color.
[0103] Examples of the dye N include the following dyes and leuco compounds. Specific examples of dyes among the dyes N include brilliant green, ethyl violet, methyl green, crystal violet, basic fuchsin, methyl violet 2B, quinaldine red, rose bengal, metanil yellow, thymolsulfophthalein, xylenol blue, methyl orange, paramethyl red, Congo red, benzopurpurin 4B, α-naphthyl red, Nile blue 2B, Nile blue A, methyl violet, malachite green, parafuchsin, Victoria Pure Blue-naphthalenesulfonate, Victoria Pure Blue BOH (manufactured by Hodogaya Chemical Industry Co., Ltd.), Oil Blue #603 (manufactured by Orient Chemical Industry Co., Ltd.), Oil Pink #312 (manufactured by Orient Chemical Industry Co., Ltd.), Oil Red 5B (manufactured by Orient Chemical Industry Co., Ltd.), Oil Scarlet #308 (manufactured by Orient Chemical Industry Co., Ltd.), Examples of the oil-soluble pigments that can be used include Orient Chemical Industry Co., Ltd.), Oil Red OG (Orient Chemical Industry Co., Ltd.), Oil Red RR (Orient Chemical Industry Co., Ltd.), Oil Green #502 (Orient Chemical Industry Co., Ltd.), Spiron Red BEH Special (Hodogaya Chemical Industry Co., Ltd.), m-Cresol Purple, Cresol Red, Rhodamine B, Rhodamine 6G, Sulforhodamine B, Auramine, 4-p-diethylaminophenyliminonaphthoquinone, 2-carboxyanilino-4-p-diethylaminophenyliminonaphthoquinone, 2-carboxystearylamino-4-pN,N-bis(hydroxyethyl)amino-phenyliminonaphthoquinone, 1-phenyl-3-methyl-4-p-diethylaminophenylimino-5-pyrazolone, and 1-β-naphthyl-4-p-diethylaminophenylimino-5-pyrazolone.
[0104] Specific examples of the leuco compound among the dyes N include p,p',p"-hexamethyltriaminotriphenylmethane (leuco crystal violet), Pergascript Blue SRB (manufactured by Ciba-Geigy), crystal violet lactone, malachite green lactone, benzoyl leucomethylene blue, 2-(N-phenyl-N-methylamino)-6-(Np-tolyl-N-ethyl)aminofluoran, 2-anilino-3-methyl-6-(N-ethyl-p-toluidino)fluoran, 3,6-dimethoxyfluoran, 3-(N,N-diethylamino)-5-methyl-7-(N,N-dibenzylamino)fluoran, 3-(N-cyclohexyl-N-methylamino)-6-(N-cyclohexyl-N-methylamino)fluoran, and the like. -methyl-7-anilinofluoran, 3-(N,N-diethylamino)-6-methyl-7-anilinofluoran, 3-(N,N-diethylamino)-6-methyl-7-xylidinofluoran, 3-(N,N-diethylamino)-6-methyl-7-chlorofluoran, 3-(N,N-diethylamino)-6-methoxy-7-aminofluoran, 3-(N,N-diethylamino)-7-(4-chloroanilino)fluoran, 3-(N,N-diethylamino)-7-chlorofluoran, 3-(N,N-diethylamino)- 3-(N,N-diethylamino)-7-benzylaminofluoran, 3-(N,N-diethylamino)-7,8-benzofluoran, 3-(N,N-dibutylamino)-6-methyl-7-anilinofluoran, 3-(N,N-dibutylamino)-6-methyl-7-xylidinofluoran, 3-piperidino-6-methyl-7-anilinofluoran, 3-pyrrolidino-6-methyl-7-anilinofluoran, 3,3-bis(1-ethyl-2-methylindol-3-yl)phthalide, 3,3-bis(1-n-butyl-2-methylindol-3-yl)phthalide 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-ethyl-2-methylindol-3-yl)phthalide, 3,3-bis(p-dimethylaminophenyl)-6-dimethylaminophthalide, 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-ethyl-2-methylindol-3-yl)phthalide, 3-(4-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)phthalide, and 3',6'-bis(diphenylamino)spiroisobenzofuran-1(3H),9'-[9H]xanthen-3-one.
[0105] From the viewpoints of visibility of exposed and unexposed areas, pattern visibility after development, and resolution, dye N is preferably a dye whose maximum absorption wavelength changes in response to radicals, and more preferably a dye that develops color in response to radicals. As dye N, leuco crystal violet, crystal violet lactone, brilliant green, or Victoria Pure Blue-naphthalenesulfonate is preferred.
[0106] The dyes may be used alone or in combination of two or more. From the viewpoints of visibility of exposed and unexposed areas, pattern visibility after development, and resolution, the content of the dye is preferably 0.1 mass % or more, more preferably 0.1 mass % to 10 mass %, even more preferably 0.1 mass % to 5 mass %, and particularly preferably 0.1 mass % to 1 mass %, relative to the total mass of the photosensitive resin layer. In addition, from the viewpoints of visibility of exposed and unexposed areas, pattern visibility after development, and resolution, the content of dye N is preferably 0.1 mass % or more, more preferably 0.1 mass % to 10 mass %, even more preferably 0.1 mass % to 5 mass %, and particularly preferably 0.1 mass % to 1 mass %, relative to the total mass of the photosensitive resin layer.
[0107] The content of dye N means the content of dye when all of dye N contained in the photosensitive resin layer is in a color-developing state. A method for quantifying the content of dye N will be described below using a dye that develops color by radicals as an example. Two types of solutions are prepared by dissolving 0.001 g or 0.01 g of dye in 100 mL of methyl ethyl ketone. A photoradical polymerization initiator Irgacure OXE01 (product name, BASF Japan Co., Ltd.) is added to each of the obtained solutions, and radicals are generated by irradiating with 365 nm light, causing all of the dyes to develop color. Then, in an air atmosphere, the absorbance of each solution at a liquid temperature of 25°C is measured using a spectrophotometer (UV3100, manufactured by Shimadzu Corporation) to create a calibration curve. Next, the absorbance of the solution in which all the dyes have been colored is measured in the same manner as above, except that the photosensitive resin layer 3g is dissolved in methyl ethyl ketone instead of the dye. The content of the dye contained in the photosensitive resin layer is calculated based on the calibration curve from the absorbance of the solution containing the photosensitive resin layer obtained.
[0108] <Polymerization inhibitor> From the viewpoints of storage stability, delay time line width change, and development temperature line width change, it is preferable that the photosensitive resin layer further contains a polymerization inhibitor. The polymerization inhibitor preferably contains a radical polymerization inhibitor. The polymerization inhibitor is not particularly limited, and any known polymerization inhibitor can be used. Examples of the polymerization inhibitor include phenothiazine, phenoxazine, hydroquinone, chloranil, phenol indophenol sodium, m-aminophenol, p-methoxyphenol, di-t-butyl-p-cresol, pyrogallol, t-butylcatechol, benzoquinone, 4,4'-thiobis(3-methyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), N-nitrosophenylhydroxyamine salt (ammonium salt, cerous salt, etc.), 2,2,6,6-tetramethylpiperidine-1-oxyl, etc. The polymerization inhibitor may also function as an antioxidant.
[0109] Furthermore, examples of the polymerization inhibitor include the thermal polymerization inhibitors described in paragraph 0018 of Japanese Patent No. 4,502,784. Other polymerization inhibitors include naphthylamine, cuprous chloride, nitrosophenylhydroxyamine aluminum salt, diphenylnitrosamine, etc. In order not to impair the sensitivity of the photosensitive resin layer, it is preferable to use nitrosophenylhydroxyamine aluminum salt as the radical polymerization inhibitor.
[0110] Among these, from the viewpoints of storage stability, delay time line width change, development temperature line width change, and sensitivity, the polymerization inhibitor preferably contains at least one compound selected from the group consisting of phenothiazine, phenoxazine, and compounds having a hindered phenol structure, more preferably contains at least one compound selected from the group consisting of phenothiazine and phenoxazine, and particularly preferably contains phenothiazine.
[0111] The polymerization inhibitor may be used alone or in combination of two or more kinds. From the viewpoints of storage stability, delay time line width change, development temperature line width change, and sensitivity, the content of the polymerization inhibitor is preferably 0.005 mass % to 2 mass %, more preferably 0.01 mass % to 1 mass %, even more preferably 0.05 mass % to 0.5 mass %, and particularly preferably 0.2 mass % to 0.4 mass %, relative to the total mass of the photosensitive resin layer.
[0112] Furthermore, when the content of the photopolymerization initiator in the photosensitive resin layer is Rc and the content of the polymerization inhibitor is Rd, the value of the mass ratio Rd / Rc is preferably 0.01 or more and 0.2 or less, more preferably 0.02 or more and 0.1 or less, and particularly preferably 0.03 or more and 0.05 or less, from the viewpoints of the delay time line width change, the development temperature line width change, and the sensitivity.
[0113] <Thermal crosslinkable compound> The photosensitive resin layer preferably contains a thermally crosslinkable compound from the viewpoints of the strength of the obtained cured film and the adhesion of the obtained uncured film. In this specification, the thermally crosslinkable compound having an ethylenically unsaturated group described later is not treated as an ethylenically unsaturated compound but as a thermally crosslinkable compound. Examples of the thermally crosslinkable compound include methylol compounds and blocked isocyanate compounds. Among these, blocked isocyanate compounds are preferred from the viewpoints of the strength of the resulting cured film and the adhesion of the resulting uncured film. Since the blocked isocyanate compound reacts with a hydroxy group and a carboxy group, for example, when an alkali-soluble resin and / or an ethylenically unsaturated compound has at least one of a hydroxy group and a carboxy group, the hydrophilicity of the formed film tends to decrease, and the functionality tends to be enhanced when the film obtained by curing the photosensitive resin layer is used as a protective film. The blocked isocyanate compound refers to a compound having a structure in which the isocyanate group of an isocyanate is protected (so-called masked) with a blocking agent.
[0114] The dissociation temperature of the blocked isocyanate compound is not particularly limited, but is preferably from 100°C to 160°C, and more preferably from 130°C to 150°C. The dissociation temperature of a blocked isocyanate means "the temperature of an endothermic peak accompanying the deprotection reaction of a blocked isocyanate when measured by DSC (Differential Scanning Calorimetry) analysis using a differential scanning calorimeter." As the differential scanning calorimeter, for example, a differential scanning calorimeter (model: DSC6200) manufactured by Seiko Instruments Inc. can be suitably used. However, the differential scanning calorimeter is not limited to this.
[0115] Examples of blocking agents having a dissociation temperature of 100°C to 160°C include active methylene compounds [malonic acid diesters (dimethyl malonate, diethyl malonate, di-n-butyl malonate, di-2-ethylhexyl malonate, etc.)] and oxime compounds (compounds having a structure represented by -C(=N-OH)- in the molecule, such as formaldoxime, acetaldoxime, acetoxime, methylethylketoxime, and cyclohexanoneoxime). Among these, the blocking agent having a dissociation temperature of 100° C. to 160° C. preferably contains an oxime compound, for example, from the viewpoint of storage stability.
[0116] The blocked isocyanate compound preferably has an isocyanurate structure from the viewpoints of, for example, improving the brittleness of the film and improving the adhesive strength to the transfer target. A blocked isocyanate compound having an isocyanurate structure can be obtained, for example, by protecting hexamethylene diisocyanate by converting it into an isocyanurate. Among blocked isocyanate compounds having an isocyanurate structure, a compound having an oxime structure in which an oxime compound is used as a blocking agent is preferred from the viewpoints that it is easier to set the dissociation temperature in a preferred range and to reduce development residues than a compound not having an oxime structure.
[0117] The blocked isocyanate compound may have a polymerizable group. The polymerizable group is not particularly limited, and any known polymerizable group can be used, with a radically polymerizable group being preferred. Examples of the polymerizable group include ethylenically unsaturated groups such as a (meth)acryloxy group, a (meth)acrylamide group, and a styryl group, as well as groups having an epoxy group such as a glycidyl group. Among these, as the polymerizable group, an ethylenically unsaturated group is preferable, a (meth)acryloxy group is more preferable, and an acryloxy group is even more preferable.
[0118] As the blocked isocyanate compound, commercially available products can be used. Examples of commercially available blocked isocyanate compounds include Karenz (registered trademark) AOI-BM, Karenz (registered trademark) MOI-BM, Karenz (registered trademark) MOI-BP, and the like (all manufactured by Showa Denko K.K.), and the blocked Duranate series (e.g., Duranate (registered trademark) TPA-B80E, Duranate (registered trademark) WT32-B75P, and the like, manufactured by Asahi Kasei Chemicals Corporation). In addition, as the blocked isocyanate compound, a compound having the following structure can also be used.
[0119] [ka]
[0120] The thermally crosslinkable compounds may be used alone or in combination of two or more. When the photosensitive resin layer contains a thermally crosslinkable compound, the content of the thermally crosslinkable compound is preferably 1 mass % to 50 mass %, and more preferably 5 mass % to 30 mass %, based on the total mass of the photosensitive resin layer.
[0121] <Other ingredients> The photosensitive resin layer may contain components other than the above-mentioned alkali-soluble resin, ethylenically unsaturated compound, photopolymerization initiator, dye, polymerization inhibitor, and thermally crosslinkable compound.
[0122] -Surfactants- From the viewpoint of thickness uniformity, the photosensitive resin layer preferably contains a surfactant. Examples of the surfactant include anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants, with nonionic surfactants being preferred. Examples of the surfactant include those described in paragraph 0017 of Japanese Patent No. 4502784 and paragraphs 0060 to 0071 of JP-A-2009-237362.
[0123] The surfactant is preferably a fluorine-based surfactant or a silicone-based surfactant. Commercially available fluorine-based surfactants include, for example, Megafac (product name) F-171, F-172, F-173, F-176, F-177, F-141, F-142, F-143, F-144, F-437, F-444, F-475, F-477, F-479, F-482, F-551-A, F-552, F-554, F-555-A, F-556, F-557, F-558, F-5 59, F-560, F-561, F-565, F-563, F-568, F-575, F-780, EXP, MFS-330, EXP.MFS-578, EXP.MFS-578-2, EXP .MFS-579, EXP.MFS-586, EXP.MFS-587, EXP.MFS-628, EXP.MFS-631, EXP.MFS-603, R-41, R-41-LM, R-01, R-40, R-40-LM, RS-43, TF-1956, RS-90, R-94, RS-72-K, DS-21 (all manufactured by DIC Corporation), Fluorard (product name) FC430, FC431, FC171 (all manufactured by Sumitomo 3M Limited), Surflon (product name) S-382, SC-101, SC-103, SC-104, SC-105, SC-1068, SC-381, SC-383 , S-393, KH-40 (all manufactured by AGC Corporation), PolyFox (trade name) PF636, PF656, PF6320, PF6520, PF7002 (all manufactured by OMNOVA), Futergent (trade name) 710FM, 610FM, 601AD, 601ADH2, 602A, 215M, 245F (all manufactured by NEOS Corporation), and U-120E (manufactured by Unichem Co., Ltd.). In addition, the fluorosurfactant may be an acrylic compound that has a molecular structure with a functional group containing a fluorine atom, and when heat is applied, the functional group containing the fluorine atom is broken and the fluorine atom is volatilized. Examples of such fluorosurfactants include the Megafac (product name) DS series manufactured by DIC Corporation (The Chemical Daily (February 22, 2016), Nikkei Business Daily (February 23, 2016)), for example, Megafac (product name) DS-21.
[0124] As the fluorine-based surfactant, it is also preferable to use a polymer of a fluorine atom-containing vinyl ether compound having a fluorinated alkyl group or a fluorinated alkylene ether group and a hydrophilic vinyl ether compound. The fluorine-based surfactant may be a block polymer. The fluorine-based surfactant may be a fluorine-containing polymer compound that includes a structural unit derived from a (meth)acrylate compound having a fluorine atom and a structural unit derived from a (meth)acrylate compound having two or more (preferably five or more) alkyleneoxy groups (preferably ethyleneoxy groups, propyleneoxy groups). The fluorine-based surfactant may be a fluorine-containing polymer having an ethylenically unsaturated group in the side chain, such as Megafac (trade name) RS-101, RS-102, RS-718K, and RS-72-K (all manufactured by DIC Corporation).
[0125] Examples of nonionic surfactants include glycerol, trimethylolpropane, trimethylolethane, and their ethoxylates and propoxylates (e.g., glycerol propoxylate, glycerol ethoxylate, etc.), polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyethylene glycol dilaurate, polyethylene glycol distearate, sorbitan fatty acid esters, Pluronic (trade names) L10, L31, L61, L62, 10R5, 17R2, 25R2 (all manufactured by BASF), Tetronic (trade names) 304, 701, 704, 901, 904, 150R1, and HYDROPALAT WE. 3323 (all manufactured by BASF), Solsperse (trade name) 20000 (all manufactured by Lubrizol Nippon Co., Ltd.), NCW-101, NCW-1001, NCW-1002 (all manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.), Paionin (trade name) D-1105, D-6112, D-6112-W, D-6315 (all manufactured by Takemoto Oil Co., Ltd.), Olfine E1010, Surfynol 104, 400, 440 (all manufactured by Nissin Chemical Industry Co., Ltd.). From the viewpoint of improving environmental compatibility, it is preferable that the fluorosurfactant be a surfactant derived from an alternative material to compounds having a linear perfluoroalkyl group having 7 or more carbon atoms, such as perfluorooctanoic acid (PFOA) and perfluorooctanesulfonic acid (PFOS).
[0126] Examples of silicone surfactants include linear polymers formed from siloxane bonds, and modified siloxane polymers in which organic groups have been introduced into the side chains or ends. Specific examples of silicone surfactants include EXP.S-309-2, EXP.S-315, EXP.S-503-2, and EXP.S-505-2 (all manufactured by DIC Corporation). , DOWSIL (trade name) 8032 ADDITIVE, Toray Silicone DC3PA, Toray Silicone SH7PA, Toray Silicone DC11PA, Toray Silicone SH21PA, Toray Silicone SH28PA, Toray Silicone SH29PA, Toray Silicone SH30PA, Toray Silicone SH8400 (all manufactured by Toray Dow Corning Co., Ltd.), as well as X-22-4952, X-22-4272, X-22-626 6, KF-351A, K354L, KF-355A, KF-945, KF-640, KF-642, KF-643, X-22-6191, X-22-4515, KF-6004, KP-341, K F-6001, KF-6002, KP-101KP-103, KP-104, KP-105, KP-106, KP-109, KP-109, KP-112, KP-120, KP-121, KP-12 4. KP-125, KP-301, KP-306, KP-310, KP-322, KP-323, KP-327, KP-341, KP-368, KP-369, KP-611, KP-620, KP-621, KP-626, KP-652 (all manufactured by Shin-Etsu Chemical Co., Ltd.), F-4440, TSF-4300, TSF-4445, TSF-4460, TSF-4452 (all manufactured by Momentive Puff Examples of such compounds include BYK300, BYK306, BYK307, BYK310, BYK320, BYK323, BYK325, BYK330, BYK313, BYK315N, BYK331, BYK333, BYK345, BYK347, BYK348, BYK349, BYK370, BYK377, BYK378, and BYK323 (all manufactured by BYK-Chemie). Moreover, in recent years, because there have been concerns about the environmental compatibility of compounds having a linear perfluoroalkyl group having seven or more carbon atoms, it is preferable to use surfactants that use alternative materials to perfluorooctanoic acid (PFOA) and perfluorooctanesulfonic acid (PFOS).
[0127] The photosensitive resin layer may contain one type of surfactant alone, or may contain two or more types of surfactants. The content of the surfactant is preferably from 0.001% by mass to 10% by mass, and more preferably from 0.01% by mass to 3% by mass, based on the total mass of the photosensitive resin layer.
[0128] -Additives- The photosensitive resin layer may contain known additives, if necessary, in addition to the above components. Examples of additives include plasticizers, heterocyclic compounds, benzotriazoles, carboxybenzotriazoles, pyridines (isonicotinamide, etc.), purine bases (adenine, etc.), and solvents. The photosensitive resin layer may contain one type of each additive alone or two or more types.
[0129] Examples of benzotriazoles include 1,2,3-benzotriazole, 1-chloro-1,2,3-benzotriazole, bis(N-2-ethylhexyl)aminomethylene-1,2,3-benzotriazole, bis(N-2-ethylhexyl)aminomethylene-1,2,3-tolyltriazole, and bis(N-2-hydroxyethyl)aminomethylene-1,2,3-benzotriazole.
[0130] Examples of carboxybenzotriazoles include 4-carboxy-1,2,3-benzotriazole, 5-carboxy-1,2,3-benzotriazole, N-(N,N-di-2-ethylhexyl)aminomethylenecarboxybenzotriazole, N-(N,N-di-2-hydroxyethyl)aminomethylenecarboxybenzotriazole, N-(N,N-di-2-ethylhexyl)aminoethylenecarboxybenzotriazole, etc. Examples of carboxybenzotriazoles that can be used include commercially available products such as CBT-1 (Johoku Chemical Industry Co., Ltd., trade name).
[0131] The total content of benzotriazoles and carboxybenzotriazoles is preferably 0.01% by mass to 3% by mass, and more preferably 0.05% by mass to 1% by mass, based on the total mass of the photosensitive resin layer. A content of 0.01% by mass or more is preferable from the viewpoint of imparting storage stability to the photosensitive resin layer. On the other hand, a content of 3% by mass or less is preferable from the viewpoint of maintaining sensitivity and suppressing discoloration of the dye.
[0132] The photosensitive resin layer may contain at least one selected from the group consisting of plasticizers and heterocyclic compounds. Examples of the plasticizer and heterocyclic compound include the compounds described in paragraphs 0097-0103 and 0111-0118 of WO 2018 / 179640.
[0133] The photosensitive resin layer may contain a solvent. When the photosensitive resin layer is formed from a photosensitive resin composition containing a solvent, the solvent may remain in the photosensitive resin layer.
[0134] The photosensitive resin layer may further contain known additives such as metal oxide particles, antioxidants, dispersants, acid multipliers, development accelerators, conductive fibers, thermal radical polymerization initiators, thermal acid generators, ultraviolet absorbers, thickeners, crosslinking agents, and organic or inorganic suspending agents. Additives contained in the photosensitive resin layer are described in paragraphs
[0165] to
[0184] of JP2014-85643A, the contents of which are incorporated herein by reference.
[0135] <Impurities, etc.> The photosensitive resin layer may contain a predetermined amount of impurities. Specific examples of impurities include sodium, potassium, magnesium, calcium, iron, manganese, copper, aluminum, titanium, chromium, cobalt, nickel, zinc, tin, halogens, and ions thereof. Among them, halide ions, sodium ions, and potassium ions are easily mixed in as impurities, so the following contents are preferable.
[0136] The content of impurities in the photosensitive resin layer is preferably 80 ppm or less, more preferably 10 ppm or less, and even more preferably 2 ppm or less, by mass. The content of impurities can be 1 ppb or more, and may be 0.1 ppm or more, by mass.
[0137] Methods for keeping the amount of impurities within the above range include selecting raw materials for the composition that contain a small amount of impurities, preventing impurities from being mixed in during the preparation of the photosensitive resin layer, and removing the impurities by washing. By such methods, the amount of impurities can be kept within the above range.
[0138] Impurities can be quantified by known methods such as ICP (Inductively Coupled Plasma) emission spectrometry, atomic absorption spectrometry, and ion chromatography.
[0139] The content of compounds such as benzene, formaldehyde, trichloroethylene, 1,3-butadiene, carbon tetrachloride, chloroform, N,N-dimethylformamide, N,N-dimethylacetamide, and hexane in the photosensitive resin layer is preferably small. The content of these compounds relative to the total mass of the photosensitive resin layer is preferably 100 ppm or less, more preferably 20 ppm or less, and even more preferably 4 ppm or less, by mass. The lower limit, based on mass, can be 10 ppb or more, and can be 100 ppb or more, based on the total mass of the photosensitive resin layer. The content of these compounds can be suppressed in the same manner as the above-mentioned metal impurities. Also, they can be quantified by known measurement methods.
[0140] The water content in the photosensitive resin layer is preferably from 0.01% by mass to 1.0% by mass, and more preferably from 0.05% by mass to 0.5% by mass, from the viewpoint of improving reliability and lamination properties.
[0141] <Residual monomer> The photosensitive resin layer may contain residual monomers corresponding to the respective structural units of the alkali-soluble resin described above. From the viewpoints of patterning property and reliability, the content of the residual monomer is preferably 5,000 ppm by mass or less, more preferably 2,000 ppm by mass or less, and even more preferably 500 ppm by mass or less, based on the total mass of the alkali-soluble resin. Although there is no particular lower limit, it is preferably 1 ppm by mass or more, and more preferably 10 ppm by mass or more. From the viewpoints of patterning property and reliability, the residual monomer of each structural unit of the alkali-soluble resin is preferably 3,000 mass ppm or less, more preferably 600 mass ppm or less, and even more preferably 100 mass ppm or less, based on the total mass of the photosensitive resin layer. Although there is no particular lower limit, it is preferably 0.1 mass ppm or more, and more preferably 1 mass ppm or more.
[0142] The amount of residual monomers in the synthesis of an alkali-soluble resin by a polymer reaction is also preferably within the above range. For example, when the alkali-soluble resin is synthesized by reacting glycidyl acrylate with a carboxylic acid side chain, the content of glycidyl acrylate is preferably within the above range. The amount of the residual monomer can be measured by a known method such as liquid chromatography or gas chromatography.
[0143] <Physical properties etc.> From the viewpoints of developability and resolution, the thickness of the photosensitive resin layer is preferably 20 μm or less, more preferably 10 μm or less, further preferably 8 μm or less, and particularly preferably 1 μm to 5 μm. The thickness of each layer in the photosensitive transfer material is measured by observing a cross section perpendicular to the main surface of the photosensitive transfer material using a scanning electron microscope (SEM), measuring the thickness of each layer at 10 or more points based on the obtained observation image, and calculating the average value.
[0144] From the viewpoint of superior adhesion, the transmittance of the photosensitive resin layer at a wavelength of 365 nm is preferably 10% or more, more preferably 30% or more, and even more preferably 50% or more. There is no particular upper limit, but it is preferably 99.9% or less.
[0145] <Formation method> The method for forming the photosensitive resin layer is not particularly limited as long as it is a method capable of forming a layer containing the above components. Examples of methods for forming a photosensitive resin layer include a method in which a photosensitive resin composition containing an alkali-soluble resin, an ethylenically unsaturated compound, a photopolymerization initiator, a solvent, etc. is prepared, the photosensitive resin composition is applied to a surface of a temporary support or the like, and the coating film of the photosensitive resin composition is dried to form the photosensitive resin layer.
[0146] Examples of the photosensitive resin composition used to form the photosensitive resin layer include compositions containing an alkali-soluble resin, an ethylenically unsaturated compound, a photopolymerization initiator, the above-mentioned optional components, and a solvent. The photosensitive resin composition preferably contains a solvent in order to adjust the viscosity of the photosensitive resin composition and facilitate the formation of the photosensitive resin layer.
[0147] -solvent- The solvent contained in the photosensitive resin composition is not particularly limited as long as it can dissolve or disperse the alkali-soluble resin, the ethylenically unsaturated compound, the photopolymerization initiator, and the above-mentioned optional components, and any known solvent can be used. Examples of the solvent include alkylene glycol ether solvents, alkylene glycol ether acetate solvents, alcohol solvents (methanol, ethanol, etc.), ketone solvents (acetone, methyl ethyl ketone, etc.), aromatic hydrocarbon solvents (toluene, etc.), aprotic polar solvents (N,N-dimethylformamide, etc.), cyclic ether solvents (tetrahydrofuran, etc.), ester solvents, amide solvents, lactone solvents, and mixed solvents containing two or more of these. When preparing a photosensitive transfer material having a temporary support, a thermoplastic resin layer, an intermediate layer, and a photosensitive resin layer, the photosensitive resin composition preferably contains at least one selected from the group consisting of an alkylene glycol ether solvent and an alkylene glycol ether acetate solvent. Among them, a mixed solvent containing at least one selected from the group consisting of an alkylene glycol ether solvent and an alkylene glycol ether acetate solvent, and at least one selected from the group consisting of a ketone solvent and a cyclic ether solvent is more preferable, and a mixed solvent containing at least three of at least one selected from the group consisting of an alkylene glycol ether solvent and an alkylene glycol ether acetate solvent, a ketone solvent, and a cyclic ether solvent is even more preferable.
[0148] Examples of alkylene glycol ether solvents include ethylene glycol monoalkyl ethers, ethylene glycol dialkyl ethers, propylene glycol monoalkyl ethers, propylene glycol dialkyl ethers, diethylene glycol dialkyl ethers, dipropylene glycol monoalkyl ethers, and dipropylene glycol dialkyl ethers. Examples of alkylene glycol ether acetate solvents include ethylene glycol monoalkyl ether acetate, propylene glycol monoalkyl ether acetate, diethylene glycol monoalkyl ether acetate, and dipropylene glycol monoalkyl ether acetate. As the solvent, the solvents described in paragraphs 0092 to 0094 of International Publication No. 2018 / 179640 and the solvents described in paragraph 0014 of JP-A-2018-177889 may be used, the contents of which are incorporated herein by reference.
[0149] The photosensitive resin composition may contain one type of solvent alone or two or more types of solvents. The content of the solvent when applying the photosensitive resin composition is preferably 50 to 1,900 parts by mass, and more preferably 100 to 900 parts by mass, per 100 parts by mass of the total solid content in the photosensitive resin composition.
[0150] The method for preparing the photosensitive resin composition is not particularly limited, and examples thereof include a method in which each component is dissolved in the above-mentioned solvent to prepare a solution in advance, and the obtained solutions are mixed in a predetermined ratio to prepare the photosensitive resin composition. The photosensitive resin composition is preferably filtered using a filter having a pore size of 0.2 μm to 30 μm before forming a photosensitive resin layer.
[0151] The method for applying the photosensitive resin composition is not particularly limited, and may be a known method, such as printing, spraying, roll coating, bar coating, curtain coating, spin coating, and die coating (i.e., slit coating). The photosensitive resin layer may be formed by applying a photosensitive resin composition onto a protective film described below and drying it.
[0152] As a method for drying the coating film of the photosensitive resin composition, heat drying and reduced pressure drying are preferred. The drying temperature is preferably 80° C. or higher, and more preferably 90° C. or higher. The upper limit is preferably 130° C. or lower, and more preferably 120° C. or lower. Drying can also be performed by continuously changing the temperature. The drying time is preferably 20 seconds or more, more preferably 40 seconds or more, and even more preferably 60 seconds or more. Although there is no particular upper limit, the drying time is preferably 600 seconds or less, and more preferably 300 seconds or less.
[0153] [Thermoplastic resin layer] The photosensitive transfer material may include a thermoplastic resin layer. The photosensitive transfer material preferably has a thermoplastic resin layer between the temporary support and the photosensitive resin layer. By providing the thermoplastic resin layer between the temporary support and the photosensitive resin layer, the photosensitive transfer material has improved conformability to the substrate in the bonding step, and the inclusion of air bubbles between the substrate and the photosensitive transfer material is suppressed, improving the adhesion to an adjacent layer (e.g., temporary support).
[0154] <Alkali-soluble resin> The thermoplastic resin layer preferably contains an alkali-soluble resin as the thermoplastic resin. Examples of the alkali-soluble resin include acrylic resin, polystyrene resin, styrene-acrylic copolymer, polyurethane resin, polyvinyl alcohol, polyvinyl formal, polyamide resin, polyester resin, polyamide resin, epoxy resin, polyacetal resin, polyhydroxystyrene resin, polyimide resin, polybenzoxazole resin, polysiloxane resin, polyethyleneimine, polyallylamine, and polyalkylene glycol.
[0155] As the alkali-soluble resin, from the viewpoints of developability and adhesion to adjacent layers, an acrylic resin is preferred. Here, the acrylic resin refers to a resin having at least one type of structural unit selected from the group consisting of structural units derived from (meth)acrylic acid, structural units derived from (meth)acrylic acid esters, and structural units derived from (meth)acrylic acid amides. The acrylic resin preferably contains a total content of constituent units derived from (meth)acrylic acid, constituent units derived from (meth)acrylic acid ester, and constituent units derived from (meth)acrylic acid amide of 50 mass% or more relative to the total mass of the acrylic resin. In particular, the total content of the structural units derived from (meth)acrylic acid and the structural units derived from (meth)acrylic acid esters is preferably 30% by mass to 100% by mass, and more preferably 50% by mass to 100% by mass, relative to the total mass of the acrylic resin.
[0156] The alkali-soluble resin is preferably a polymer having an acid group. Examples of the acid group include a carboxy group, a sulfo group, a phosphoric acid group, and a phosphonic acid group, with the carboxy group being preferred. From the viewpoint of developability, the alkali-soluble resin is preferably an alkali-soluble resin having an acid value of 60 mgKOH / g or more, and more preferably a carboxy group-containing acrylic resin having an acid value of 60 mgKOH / g or more. The upper limit of the acid value of the alkali-soluble resin is not particularly limited, but is preferably 200 mgKOH / g or less, and more preferably 150 mgKOH / g or less.
[0157] The carboxyl group-containing acrylic resin having an acid value of 60 mgKOH / g or more is not particularly limited, and can be appropriately selected from known resins. Examples of the alkali-soluble resin include a carboxy group-containing acrylic resin having an acid value of 60 mgKOH / g or more among the polymers described in paragraph 0025 of JP-A 2011-95716, a carboxy group-containing acrylic resin having an acid value of 60 mgKOH / g or more among the polymers described in paragraphs 0033 to 0052 of JP-A 2010-237589, and a carboxy group-containing acrylic resin having an acid value of 60 mgKOH / g or more among the alkali-soluble resins described in paragraphs 0053 to 0068 of JP-A 2016-224162. The copolymerization ratio of the structural unit having a carboxy group in the carboxy group-containing acrylic resin is preferably 5% by mass to 50% by mass, more preferably 10% by mass to 40% by mass, and even more preferably 12% by mass to 30% by mass, based on the total mass of the acrylic resin. As the alkali-soluble resin, from the viewpoints of developability and adhesion to adjacent layers, an acrylic resin having a structural unit derived from (meth)acrylic acid is particularly preferred.
[0158] The alkali-soluble resin may have a reactive group. The reactive group may be any group capable of addition polymerization, and examples of the reactive group include ethylenically unsaturated groups, polycondensable groups such as hydroxyl groups and carboxyl groups, and polyaddition reactive groups such as epoxy groups and (blocked) isocyanate groups.
[0159] The weight average molecular weight (Mw) of the alkali-soluble resin is preferably 1,000 or more, more preferably from 10,000 to 100,000, and even more preferably from 20,000 to 50,000.
[0160] The thermoplastic resin layer may contain one type of alkali-soluble resin alone or two or more types of alkali-soluble resins. From the viewpoints of developability and adhesion to adjacent layers, the content of the alkali-soluble resin is preferably 10% by mass to 99% by mass, more preferably 20% by mass to 90% by mass, even more preferably 40% by mass to 80% by mass, and particularly preferably 50% by mass to 70% by mass, relative to the total mass of the thermoplastic resin layer.
[0161] <Dye> The thermoplastic resin layer preferably contains a dye (also simply referred to as "dye B") that has a maximum absorption wavelength of 450 nm or more in the wavelength range of 400 nm to 780 nm when colored and whose maximum absorption wavelength changes depending on an acid, a base, or a radical. The preferred embodiments of dye B are the same as the preferred embodiments of dye N, except for the points described below.
[0162] From the viewpoints of visibility of exposed and unexposed areas and resolution, dye B is preferably a dye whose maximum absorption wavelength changes in response to an acid or a radical, and more preferably a dye whose maximum absorption wavelength changes in response to an acid. From the viewpoints of visibility and resolution of exposed and unexposed areas, it is preferable that the thermoplastic resin layer contains both a dye B whose maximum absorption wavelength changes in response to acid, and a compound that generates an acid when exposed to light, as described below.
[0163] The dye B may be used alone or in combination of two or more kinds. From the viewpoint of visibility of exposed and non-exposed areas, the content of dye B is preferably 0.2 mass% or more, more preferably 0.2 mass% to 6 mass%, even more preferably 0.2 mass% to 5 mass%, and particularly preferably 0.25 mass% to 3.0 mass%, relative to the total mass of the thermoplastic resin layer.
[0164] Here, the content of dye B means the content of dye when all of dye B contained in the thermoplastic resin layer is in a colored state. A method for quantifying the content of dye B will be described below using a dye that develops color by radicals as an example. Prepare solutions by dissolving 0.001 g and 0.01 g of dye in 100 mL of methyl ethyl ketone. Add a photoradical polymerization initiator Irgacure OXE01 (product name, BASF Japan Co., Ltd.) to each of the obtained solutions, and irradiate with 365 nm light to generate radicals and make all the dyes colored. Then, measure the absorbance of each solution at a liquid temperature of 25°C using a spectrophotometer (UV3100, manufactured by Shimadzu Corporation) in an air atmosphere, and create a calibration curve. Next, the absorbance of the solution in which all the dye has been colored is measured in the same manner as above, except that 0.1 g of the thermoplastic resin layer is dissolved in methyl ethyl ketone instead of the dye. The amount of the dye contained in the thermoplastic resin layer is calculated based on the calibration curve from the absorbance of the solution containing the thermoplastic resin layer obtained.
[0165] <Compounds that generate acids, bases, or radicals when exposed to light> The thermoplastic resin layer may contain a compound that generates an acid, a base or a radical when exposed to light (also simply referred to as "compound C"). Compound C is preferably a compound that generates an acid, a base, or a radical upon exposure to actinic rays such as ultraviolet light and visible light. Known photoacid generators, photobase generators, and photoradical polymerization initiators (photoradical generators) can be used as the compound C. Among them, photoacid generators are preferred.
[0166] -Photoacid generator- From the viewpoint of resolution, the thermoplastic resin layer preferably contains a photoacid generator. Examples of the photoacid generator include the above-mentioned cationic photopolymerization initiators which may be contained in the photosensitive resin layer, and preferred aspects are also the same except for the points described below.
[0167] From the viewpoints of sensitivity and resolution, the photoacid generator preferably contains at least one compound selected from the group consisting of an onium salt compound and an oxime sulfonate compound, and from the viewpoints of sensitivity, resolution and adhesion, it is more preferable that the photoacid generator contains an oxime sulfonate compound. As the photoacid generator, a photoacid generator having the following structure is also preferred.
[0168] [ka]
[0169] -Photoradical polymerization initiator- The thermoplastic resin layer may contain a photoradical polymerization initiator (photoradical polymerization initiator). As the photoradical polymerization initiator, the above-mentioned photoradical polymerization initiators which may be contained in the photosensitive resin layer can be mentioned, and the preferred embodiments are also the same.
[0170] -Photobase generator- The thermoplastic resin layer may contain a photobase generator. The photobase generator is not particularly limited as long as it is a known photobase generator, and examples thereof include 2-nitrobenzylcyclohexylcarbamate, triphenylmethanol, O-carbamoylhydroxylamide, O-carbamoyloxime, {[(2,6-dinitrobenzyl)oxy]carbonyl}cyclohexylamine, bis{[(2-nitrobenzyl)oxy]carbonyl}hexane-1,6-diamine, 4-(methylthiobenzoyl)-1-methyl-1-morpholinoethane, (4-morpholinobenzoyl) -1-benzyl-1-dimethylaminopropane, N-(2-nitrobenzyloxycarbonyl)pyrrolidine, hexaamminecobalt(III) tris(triphenylmethylborate), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2,6-dimethyl-3,5-diacetyl-4-(2-nitrophenyl)-1,4-dihydropyridine, and 2,6-dimethyl-3,5-diacetyl-4-(2,4-dinitrophenyl)-1,4-dihydropyridine.
[0171] The thermoplastic resin layer may contain one type of compound C alone, or may contain two or more types. The content of compound C is preferably 0.1 to 10% by mass, and more preferably 0.5 to 5% by mass, based on the total mass of the thermoplastic resin layer, from the viewpoints of visibility and resolution of exposed and non-exposed areas.
[0172] <Plasticizer> The thermoplastic resin layer preferably contains a plasticizer from the viewpoints of resolution, adhesion to adjacent layers, and developability. The plasticizer preferably has a smaller molecular weight (weight average molecular weight (Mw) in the case of an oligomer or polymer) than the alkali-soluble resin. The molecular weight (weight average molecular weight (Mw)) of the plasticizer is preferably 200 to 2,000. The plasticizer is not particularly limited as long as it is a compound that is compatible with the alkali-soluble resin and exhibits plasticity, but from the viewpoint of imparting plasticity, the plasticizer preferably has an alkyleneoxy group in the molecule, more preferably a polyalkylene glycol compound. The alkyleneoxy group contained in the plasticizer more preferably has a polyethyleneoxy structure or a polypropyleneoxy structure.
[0173] From the viewpoints of resolution and storage stability, the plasticizer preferably contains a (meth)acrylate compound. From the viewpoints of compatibility, resolution, and adhesion to adjacent layers, it is more preferable that the alkali-soluble resin is an acrylic resin and the plasticizer contains a (meth)acrylate compound. Examples of the (meth)acrylate compound used as the plasticizer include the (meth)acrylate compounds described above as the ethylenically unsaturated compound contained in the photosensitive resin layer. In the photosensitive transfer material, when the thermoplastic resin layer and the photosensitive resin layer are laminated in direct contact with each other, it is preferable that both the thermoplastic resin layer and the photosensitive resin layer contain the same (meth)acrylate compound, because the thermoplastic resin layer and the photosensitive resin layer each contain the same (meth)acrylate compound, which suppresses component diffusion between the layers and improves storage stability.
[0174] When the thermoplastic resin layer contains a (meth)acrylate compound as a plasticizer, it is preferable that the (meth)acrylate compound does not polymerize even in the exposed area after exposure, from the viewpoint of adhesion to adjacent layers. In addition, the (meth)acrylate compound used as a plasticizer is preferably a polyfunctional (meth)acrylate compound having two or more (meth)acryloyl groups in one molecule, from the viewpoints of resolution, adhesion to adjacent layers, and developability. Furthermore, as the (meth)acrylate compound used as the plasticizer, a (meth)acrylate compound having an acid group or a urethane (meth)acrylate compound is also preferred.
[0175] The thermoplastic resin layer may contain one type of plasticizer alone, or may contain two or more types of plasticizers. From the viewpoints of resolution, adhesion to adjacent layers, and developability, the content of the plasticizer is preferably 1% by mass to 70% by mass, more preferably 10% by mass to 60% by mass, and particularly preferably 20% by mass to 50% by mass, relative to the total mass of the thermoplastic resin layer.
[0176] <Surfactant> From the viewpoint of thickness uniformity, the thermoplastic resin layer preferably contains a surfactant. As the surfactant, the surfactant which may be contained in the photosensitive resin layer described above can be mentioned, and the preferred embodiments are also the same.
[0177] The thermoplastic resin layer may contain one type of surfactant alone, or may contain two or more types of surfactants. The content of the surfactant is preferably from 0.001% by mass to 10% by mass, and more preferably from 0.01% by mass to 3% by mass, based on the total mass of the thermoplastic resin layer.
[0178] <Sensitizer> The thermoplastic resin layer may contain a sensitizer. The sensitizer is not particularly limited, and examples thereof include the sensitizers that may be contained in the photosensitive resin layer described above.
[0179] The thermoplastic resin layer may contain one type of sensitizer alone or two or more types of sensitizers. The content of the sensitizer can be appropriately selected depending on the purpose, but from the viewpoints of improving sensitivity to the light source and visibility of exposed and non-exposed areas, it is preferably in the range of 0.01 mass % to 5 mass %, and more preferably in the range of 0.05 mass % to 1 mass %, relative to the total mass of the thermoplastic resin layer.
[0180] <Additives, etc.> The thermoplastic resin layer may contain known additives, if necessary, in addition to the above components. In addition, the thermoplastic resin layer is described in paragraphs
[0189] to
[0193] of JP2014-85643A, the contents of which are incorporated herein by reference.
[0181] <Physical properties etc.> The thickness of the thermoplastic resin layer is not particularly limited, but is preferably 1 μm or more, more preferably 2 μm or more, from the viewpoint of adhesion with adjacent layers. The upper limit is not particularly limited, but is preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less, from the viewpoint of developability and resolution.
[0182] <Formation method> The method for forming the thermoplastic resin layer is not particularly limited as long as it is a method capable of forming a layer containing the above-mentioned components. Examples of methods for forming the thermoplastic resin layer include a method in which a thermoplastic resin composition containing the above-mentioned components and a solvent is prepared, the thermoplastic resin composition is applied to a surface of a temporary support or the like, and the coating of the thermoplastic resin composition is dried to form a layer. The thermoplastic resin composition preferably contains a solvent in order to adjust the viscosity of the thermoplastic resin composition and facilitate the formation of the thermoplastic resin layer.
[0183] -solvent- The solvent contained in the thermoplastic resin composition is not particularly limited as long as it can dissolve or disperse the above-mentioned components contained in the thermoplastic resin layer. As the solvent contained in the thermoplastic resin composition, the solvent which may be contained in the photosensitive resin composition described above can be mentioned, and the preferred embodiments are also the same.
[0184] The solvent contained in the thermoplastic resin composition may be one type alone or two or more types. The content of the solvent when applying the thermoplastic resin composition is preferably 50 to 1,900 parts by mass, and more preferably 100 to 900 parts by mass, per 100 parts by mass of the total solid content in the thermoplastic resin composition.
[0185] The preparation of the thermoplastic resin composition and the formation of the thermoplastic resin layer may be carried out in accordance with the above-mentioned method for preparing the photosensitive resin composition and the method for forming the photosensitive resin layer. For example, a solution is prepared in advance by dissolving each component contained in the thermoplastic resin layer in the above-mentioned solvent, and the obtained solutions are mixed in a predetermined ratio to prepare a thermoplastic resin composition, and then, The obtained thermoplastic resin composition is applied to the surface of a temporary support, and the coating of the thermoplastic resin composition is dried to form a thermoplastic resin layer. In addition, after forming a photosensitive resin layer and an intermediate layer on a protective film described below, a thermoplastic resin layer may be formed on the surface of the intermediate layer.
[0186] [Middle class] The photosensitive transfer material preferably has an intermediate layer between the thermoplastic resin layer and the photosensitive resin layer, which can prevent the components from mixing when applying multiple layers and during storage after application. The intermediate layer is preferably a water-soluble layer from the viewpoints of developability and suppressing mixing of components when applying a plurality of layers and during storage after application. In this specification, the term "water-soluble" means that the solubility in 100 g of water having a liquid temperature of 22°C and a pH of 7.0 is 0.1 g or more.
[0187] The intermediate layer may be an oxygen-blocking layer having an oxygen-blocking function, which is described as a "separation layer" in JP-A-5-72724. When the intermediate layer is an oxygen-blocking layer, the sensitivity during exposure is improved, the time load of the exposure machine is reduced, and productivity is improved, which is preferable. The oxygen barrier layer used as the intermediate layer may be appropriately selected from known layers described in the above publications, etc. Among them, an oxygen barrier layer that exhibits low oxygen permeability and disperses or dissolves in water or an alkaline aqueous solution (a 1% by mass aqueous solution of sodium carbonate at 22° C.) is preferred.
[0188] The intermediate layer preferably contains a resin. Examples of resins contained in the intermediate layer include polyvinyl alcohol-based resins, polyvinylpyrrolidone-based resins, cellulose-based resins, acrylamide-based resins, polyethylene oxide-based resins, gelatin, vinyl ether-based resins, polyamide resins, and copolymers thereof. The resin contained in the intermediate layer is preferably a water-soluble resin. In addition, from the viewpoint of suppressing mixing of components between multiple layers, it is preferable that the resin contained in the intermediate layer is a resin different from both the polymer A contained in the photosensitive resin layer and the thermoplastic resin (e.g., an alkali-soluble resin) contained in the thermoplastic resin layer.
[0189] From the viewpoints of oxygen barrier properties and suppressing mixing of components when multiple layers are applied and during storage after application, the intermediate layer preferably contains polyvinyl alcohol, and more preferably contains both polyvinyl alcohol and polyvinylpyrrolidone.
[0190] The intermediate layer may contain one type of the above resin alone, or may contain two or more types. The resin content in the intermediate layer is not particularly limited, but from the viewpoints of oxygen barrier properties and suppressing mixing of components when multiple layers are applied and during storage after application, the resin content is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, even more preferably 80% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass, relative to the total mass of the intermediate layer. Furthermore, the intermediate layer may contain additives such as a surfactant, if necessary.
[0191] The thickness of the intermediate layer is not particularly limited, but is preferably 0.1 μm to 5 μm, and more preferably 0.5 μm to 3 μm. When the thickness of the intermediate layer is within the above range, the oxygen barrier properties are not reduced, mixing of components can be suppressed when multiple layers are applied and during storage after application, and an increase in the time required to remove the intermediate layer during development can be suppressed.
[0192] The method for forming the intermediate layer is not particularly limited, and examples thereof include a method in which an intermediate layer composition containing the above-mentioned resin and any additives is prepared, applied to the surface of a thermoplastic resin layer or a photosensitive resin layer, and the coating of the intermediate layer composition is dried to form an intermediate layer. The intermediate layer composition preferably contains a solvent in order to adjust the viscosity of the intermediate layer composition and to facilitate the formation of the intermediate layer.
[0193] The solvent contained in the intermediate layer composition is not particularly limited as long as it is capable of dissolving or dispersing the above-mentioned resin, and is preferably at least one selected from the group consisting of water and water-miscible organic solvents, and more preferably water or a mixed solvent of water and a water-miscible organic solvent. Examples of the water-miscible organic solvent include alcohols having 1 to 3 carbon atoms, acetone, ethylene glycol, and glycerin, with alcohols having 1 to 3 carbon atoms being preferred, and methanol or ethanol being more preferred.
[0194] [Protective film] The photosensitive transfer material preferably has a protective film in contact with the surface of the photosensitive resin layer that does not face the temporary support.
[0195] Materials constituting the protective film include resin films and paper, with resin films being preferred from the standpoints of strength and flexibility. Examples of the resin film include a polyethylene film, a polypropylene film, a polyethylene terephthalate film, a cellulose triacetate film, a polystyrene film, and a polycarbonate film. Among these, a polyethylene film, a polypropylene film, or a polyethylene terephthalate film is preferable.
[0196] The thickness (layer thickness) of the protective film is not particularly limited, but is preferably from 5 μm to 100 μm, and more preferably from 10 to 50 μm. The arithmetic mean roughness Ra value of the surface of the protective film in contact with the photosensitive resin layer (hereinafter also simply referred to as the "surface of the protective film") is preferably 0.3 μm or less, more preferably 0.1 μm or less, and even more preferably 0.05 μm or less, from the viewpoint of superior resolution. It is believed that the uniformity of the layer thickness of the photosensitive resin layer and the formed resin pattern is improved when the Ra value of the surface of the protective film is within the above range. There is no particular lower limit for the Ra value of the surface of the protective film, but it is preferably 0.001 μm or more.
[0197] The Ra value of the surface of the protective film is measured by the following method. Using a three-dimensional optical profiler (New View7300, manufactured by Zygo), the surface of the protective film is measured under the following conditions to obtain a surface profile of the optical film. The measurement and analysis software used is the Microscope Application of MetroPro ver8.3.2. Next, the Surface Map screen is displayed in the analysis software, and histogram data is obtained in the Surface Map screen. From the obtained histogram data, the arithmetic mean roughness is calculated, and the Ra value of the protective film surface is obtained. When a protective film is attached to the photosensitive transfer material, the protective film may be peeled off from the photosensitive transfer material, and the Ra value of the surface on the peeled side may be measured.
[0198] The method for bonding the protective film to the photosensitive resin layer or the like is not particularly limited, and may be any known method. Examples of a device for laminating a protective film to a photosensitive resin layer or the like include known laminators such as a vacuum laminator and an autocut laminator. The laminator is preferably equipped with any heatable roller, such as a rubber roller, and is capable of applying pressure and heat.
[0199] The photosensitive transfer material may include layers other than the above-mentioned layers (hereinafter, also referred to as "other layers"). Examples of the other layers include a contrast enhancement layer. The contrast enhancement layer is described in paragraph 0134 of WO 2018 / 179640. The other layers are described in paragraphs 0194 to 0196 of JP 2014-85643 A. The contents of these publications are incorporated herein by reference.
[0200] In order to better exert the effects of the present disclosure, the total thickness of each layer in the photosensitive transfer material, excluding the temporary support and the protective film, is preferably 20 μm or less, more preferably 10 μm or less, even more preferably 8 μm or less, and particularly preferably 2 μm or more and 8 μm or less. In addition, from the viewpoint of better exerting the effects of the present disclosure, the total thickness of the photosensitive resin layer, intermediate layer and thermoplastic resin layer in the photosensitive transfer material is preferably 20 μm or less, more preferably 10 μm or less, even more preferably 8 μm or less, and particularly preferably 2 μm or more and 8 μm or less.
[0201] The photosensitive transfer material according to the present disclosure can be suitably used in various applications requiring precise microfabrication by photolithography. After patterning the photosensitive resin layer, etching may be performed using the photosensitive resin layer as a coating, or electroforming mainly using electroplating may be performed. The cured film obtained by patterning may be used as a permanent film, for example, an interlayer insulating film, a wiring protective film, or a wiring protective film having an index matching layer. The photosensitive transfer material according to the present disclosure can be suitably used in applications such as various wiring formation applications for semiconductor packages, printed circuit boards, and sensor boards, touch panels, electromagnetic wave shielding materials, conductive films such as film heaters, liquid crystal sealants, and the formation of structures in the fields of micromachines and microelectronics.
[0202] [Method of producing photosensitive transfer material] The method for producing the photosensitive transfer material used in the present disclosure is not particularly limited, and any known production method, for example, any known method for forming each layer, can be used. Hereinafter, a method for producing a photosensitive transfer material according to the present disclosure will be described with reference to Fig. 1. However, the photosensitive transfer material according to the present disclosure is not limited to the configuration shown in Fig. 1. Fig. 1 is a schematic cross-sectional view showing an example of a layer structure in one embodiment of the photosensitive transfer material according to the present disclosure. The photosensitive transfer material 20 shown in Fig. 1 has a structure in which a temporary support 11, a thermoplastic resin layer 13, a water-soluble resin layer 15, a photosensitive resin layer 17, and a protective film 19 are laminated in this order.
[0203] Examples of a method for producing the above-mentioned photosensitive transfer material 20 include a method including the steps of applying a thermoplastic resin composition to the surface of the temporary support 11 and then drying the coating of the thermoplastic resin composition to form a thermoplastic resin layer 13, applying a water-soluble resin layer composition to the surface of the thermoplastic resin layer 13 and then drying the coating of the water-soluble resin layer composition to form a water-soluble resin layer 15, and applying a photosensitive resin composition containing an alkali-soluble resin and an ethylenically unsaturated compound to the surface of the water-soluble resin layer 15 and then drying the coating of the photosensitive resin composition to form a photosensitive resin layer 17. In the above manufacturing method, it is preferable to use a thermoplastic resin composition containing at least one selected from the group consisting of alkylene glycol ether solvents and alkylene glycol ether acetate solvents, a water-soluble resin layer composition containing at least one selected from the group consisting of water and water-miscible organic solvents, and a photosensitive resin composition containing at least one selected from the group consisting of an alkali-soluble resin, an ethylenically unsaturated compound, and an alkylene glycol ether solvent and an alkylene glycol ether acetate solvent. This can suppress the mixing of the components contained in the thermoplastic resin layer 13 and the components contained in the water-soluble resin layer 15 during the application of the water-soluble resin layer composition to the surface of the thermoplastic resin layer 13 and / or the storage period of a laminate having a coating film of the water-soluble resin layer composition, and can also suppress the mixing of the components contained in the water-soluble resin layer 15 and the components contained in the photosensitive resin layer 17 during the application of the photosensitive resin composition to the surface of the water-soluble resin layer 15 and / or the storage period of a laminate having a coating film of the photosensitive resin composition.
[0204] A protective film 19 is pressure-bonded to the photosensitive resin layer 17 of the laminate produced by the above-mentioned production method, thereby producing a photosensitive transfer material 20. A manufacturing method for the photosensitive transfer material used in the present disclosure preferably includes a step of providing a protective film 19 in contact with the second surface of the photosensitive resin layer 17, thereby manufacturing a photosensitive transfer material 20 having a temporary support 11, a thermoplastic resin layer 13, a water-soluble resin layer 15, a photosensitive resin layer 17 and a protective film 19. After the photosensitive transfer material 20 is produced by the above-mentioned production method, a photosensitive transfer material in a roll form may be produced and stored by winding up the photosensitive transfer material 20. The photosensitive transfer material in a roll form can be provided in that form as it is to the step of laminating the material to a substrate in a roll-to-roll system described later.
[0205] The photosensitive transfer material according to the present disclosure can be suitably used in various applications requiring precise microfabrication by photolithography. After patterning the photosensitive resin layer, etching may be performed using the photosensitive resin layer as a coating, or electroforming mainly using electroplating may be performed. The cured film obtained by patterning may be used as a permanent film, for example, an interlayer insulating film, a wiring protective film, or a wiring protective film having an index matching layer. The photosensitive transfer material according to the present disclosure may be suitably used in applications such as various wiring formation applications for semiconductor packages, printed circuit boards, and sensor boards, touch panels, electromagnetic wave shielding materials, conductive films such as film heaters, liquid crystal sealants, and the formation of structures in the field of micromachines or microelectronics.
[0206] In addition, the photosensitive transfer material of the first embodiment also preferably has an embodiment in which the photosensitive resin layer is a colored resin layer containing a pigment. In addition to the above, the colored resin layer is preferably used for forming colored pixels or black matrices of color filters used in liquid crystal displays (LCDs) and solid-state imaging devices (e.g., CCDs (charge-coupled devices) and CMOSs (complementary metal oxide semiconductors)). The configuration of the colored resin layer other than the pigment is the same as that described above.
[0207] <Pigments> The photosensitive resin layer may be a colored resin layer containing a pigment. In some cases, in order to protect the liquid crystal display window of recent electronic devices, a cover glass having a black frame-shaped light-shielding layer formed on the periphery of the back surface of a transparent glass substrate, etc. is attached to the liquid crystal display window. A colored resin layer can be used to form such a light-shielding layer. The pigment may be appropriately selected according to the desired hue, and may be selected from black pigments, white pigments, and pigments of chromatic colors other than black and white. Among them, when a black pattern is to be formed, a black pigment is preferably selected as the pigment.
[0208] As the black pigment, known black pigments (organic pigments, inorganic pigments, etc.) can be appropriately selected as long as the effects of the present disclosure are not impaired. Among them, from the viewpoint of optical density, suitable black pigments include, for example, carbon black, titanium oxide, titanium carbide, iron oxide, titanium oxide, and graphite, and carbon black is particularly preferred. As the carbon black, from the viewpoint of surface resistance, carbon black at least a part of the surface of which is coated with a resin is preferred.
[0209] From the viewpoint of dispersion stability, the particle size of the black pigment is preferably from 0.001 μm to 0.1 μm, more preferably from 0.01 μm to 0.08 μm, in terms of number average particle size. Here, the particle size refers to the diameter of a circle whose area is equal to the area of a pigment particle, calculated from a photograph of the pigment particle taken with an electron microscope, and the number average particle size is the average value obtained by calculating the above particle size for any 100 particles and averaging the particle sizes of the 100 particles thus calculated.
[0210] As a pigment other than the black pigment, the white pigment described in paragraphs 0015 and 0114 of JP-A-2005-007765 can be used. Specifically, among the white pigments, the inorganic pigment is preferably titanium oxide, zinc oxide, lithopone, precipitated calcium carbonate, white carbon, aluminum oxide, aluminum hydroxide, or barium sulfate, more preferably titanium oxide or zinc oxide, and even more preferably titanium oxide. As the inorganic pigment, rutile or anatase titanium oxide is more preferable, and rutile titanium oxide is particularly preferable. The surface of titanium oxide may be subjected to a silica treatment, an alumina treatment, a titania treatment, a zirconia treatment, or an organic treatment, or may be subjected to two or more of these treatments, which suppresses the catalytic activity of titanium oxide and improves heat resistance, fading resistance, etc. From the viewpoint of reducing the thickness of the photosensitive resin layer after heating, the surface treatment of the titanium oxide is preferably at least one of alumina treatment and zirconia treatment, and particularly preferably both alumina treatment and zirconia treatment.
[0211] In addition, when the photosensitive resin layer is a colored resin layer, it is also preferable that the photosensitive resin layer further contains a chromatic pigment other than the black pigment and the white pigment from the viewpoint of transferability. When the chromatic pigment is contained, the particle size of the chromatic pigment is preferably 0.1 μm or less, and more preferably 0.08 μm or less, in terms of excellent dispersibility. Examples of chromatic pigments include Victoria Pure Blue BO (Color Index (CI) 42595), Auramine (CI 41000), Fat Black HB (CI 26150), Monolight Yellow GT (CI Pigment Yellow 12), Permanent Yellow GR (CI Pigment Yellow 17), Permanent Yellow HR (CI Pigment Yellow 83), Permanent Carmine FBB (CI Pigment Red 146), Hoster Balm Red ESB (CI Pigment Violet 19), Permanent Ruby FBH (CI Pigment Red 11), Fastel Pink B Supra (CI Pigment Red 81), Monastral Fast Blue (CI Pigment Red 146 ... Permanent Yellow GR (CI Pigment Yellow 17), Permanent Yellow HR (CI Pigment Yellow 83), Permanent Carmine FBB (CI Pigment Red 146), Permanent Yellow GR (CI Pigment Yellow 17), Permanent Yellow HR (CI Pigment Yellow 83), Permanent Carmine FBB (CI Pigment Red 146), Permanent Yellow GR (CI Pigment Yellow 17), Permanent Yellow HR (CI Pigment Yellow 83), Permanent Carmine FBB (CI Pigment Red 146), Permanent Yellow Examples of pigments that can be used include CI Pigment Blue 15), Monolight Fast Black B (CI Pigment Black 1) and Carbon, CI Pigment Red 97, CI Pigment Red 122, CI Pigment Red 149, CI Pigment Red 168, CI Pigment Red 177, CI Pigment Red 180, CI Pigment Red 192, CI Pigment Red 215, CI Pigment Green 7, CI Pigment Blue 15:1, CI Pigment Blue 15:4, CI Pigment Blue 22, CI Pigment Blue 60, CI Pigment Blue 64, and CI Pigment Violet 23. Of these, CI Pigment Red 177 is preferred.
[0212] When the photosensitive resin layer contains a pigment, the content of the pigment is preferably more than 3 mass% and not more than 40 mass%, more preferably more than 3 mass% and not more than 35 mass%, even more preferably more than 5 mass% and not more than 35 mass%, and particularly preferably 10 mass% or more and not more than 35 mass%, relative to the total mass of the photosensitive resin layer.
[0213] When the photosensitive resin layer contains pigments other than the black pigment (white pigments and chromatic pigments), the content of the pigments other than the black pigment is preferably 30% by mass or less, more preferably 1% by mass to 20% by mass, and even more preferably 3% by mass to 15% by mass, relative to the black pigment.
[0214] In addition, when the photosensitive resin layer contains a black pigment and is formed from a photosensitive resin composition, the black pigment (preferably carbon black) is preferably introduced into the photosensitive resin composition in the form of a pigment dispersion. The dispersion may be prepared by adding a mixture of a black pigment and a pigment dispersant to an organic solvent (or vehicle) and dispersing the mixture with a dispersing machine. The pigment dispersant may be selected according to the pigment and the solvent, and for example, a commercially available dispersant may be used. The vehicle refers to the medium portion in which the pigment is dispersed when the pigment dispersion is prepared, and is liquid, and includes a binder component that holds the black pigment in a dispersed state and a solvent component (organic solvent) that dissolves and dilutes the binder component.
[0215] The dispersing machine is not particularly limited, and examples thereof include known dispersing machines such as kneaders, roll mills, attritors, super mills, dissolvers, homomixers, and sand mills. Furthermore, fine pulverization may be performed by utilizing frictional force through mechanical grinding. For details of dispersing machines and fine pulverization, see the description in "Encyclopedia of Pigments" (written by Kunizo Asakura, 1st Edition, Asakura Shoten, 2000, pp. 438 and 310).
[0216] [Photosensitive transfer material of second embodiment] An example of the photosensitive transfer material of the second embodiment will be described below. The photosensitive transfer material 10 shown in FIG. 2 includes a temporary support 1, a transfer layer 2 including a photosensitive resin layer 3 and a refractive index adjusting layer 5, and a protective film 7, in this order. Furthermore, the photosensitive transfer material 10 shown in FIG. 2 has a refractive index adjusting layer 5 disposed therein, but the refractive index adjusting layer 5 does not necessarily have to be disposed. Each element constituting the photosensitive transfer material of the second embodiment will be described below. The temporary support and protective film used in the photosensitive transfer material of the second embodiment are similar to the temporary support and protective film in the photosensitive transfer material of the first embodiment, and preferred aspects are also similar.
[0217] [Photosensitive resin layer] The photosensitive transfer material has a photosensitive resin layer. After the photosensitive resin layer is transferred onto a transfer-receiving body, exposure and development are carried out, whereby a pattern can be formed on the transfer-receiving body. Components that may be contained in the photosensitive resin layer will be described in detail below.
[0218] <Alkali-soluble resin> The photosensitive resin layer contains an alkali-soluble resin. Examples of the alkali-soluble resin include (meth)acrylic resin, styrene resin, epoxy resin, amide resin, amide epoxy resin, alkyd resin, phenol resin, ester resin, urethane resin, epoxy acrylate resin obtained by reacting an epoxy resin with (meth)acrylic acid, and acid-modified epoxy acrylate resin obtained by reacting an epoxy acrylate resin with an acid anhydride.
[0219] One preferred embodiment of the alkali-soluble resin is a (meth)acrylic resin, which has excellent alkali developability and film formability. In this specification, the (meth)acrylic resin means a resin having a structural unit derived from a (meth)acrylic compound. The content of the structural unit derived from a (meth)acrylic compound is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, based on the total structural units of the (meth)acrylic resin. The (meth)acrylic resin may be composed only of structural units derived from (meth)acrylic compounds, or may contain structural units derived from polymerizable monomers other than (meth)acrylic compounds. That is, the upper limit of the content of structural units derived from (meth)acrylic compounds is 100% by mass or less based on the total structural units of the (meth)acrylic resin.
[0220] Examples of the (meth)acrylic compound include (meth)acrylic acid, (meth)acrylic acid esters, (meth)acrylamide, and (meth)acrylonitrile. Examples of the (meth)acrylic acid ester include (meth)acrylic acid alkyl ester, (meth)acrylic acid tetrahydrofurfuryl ester, (meth)acrylic acid dimethylaminoethyl ester, (meth)acrylic acid diethylaminoethyl ester, (meth)acrylic acid glycidyl ester, (meth)acrylic acid benzyl ester, 2,2,2-trifluoroethyl (meth)acrylate, and 2,2,3,3-tetrafluoropropyl (meth)acrylate, and (meth)acrylic acid alkyl ester is preferred. Examples of (meth)acrylamides include acrylamides such as diacetone acrylamide.
[0221] Examples of the (meth)acrylic acid alkyl ester include (meth)acrylic acid alkyl esters having an alkyl group having 1 to 12 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, and dodecyl (meth)acrylate. As the (meth)acrylic acid ester, a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 4 carbon atoms is preferred, and methyl (meth)acrylate or ethyl (meth)acrylate is more preferred.
[0222] The (meth)acrylic resin may have a structural unit other than the structural unit derived from the (meth)acrylic compound. The polymerizable monomer that forms the above-mentioned structural unit is not particularly limited as long as it is a compound other than a (meth)acrylic compound that is copolymerizable with a (meth)acrylic compound, and examples thereof include styrene compounds that may have a substituent at the α-position or aromatic ring, such as styrene, vinyl toluene, and α-methylstyrene, vinyl alcohol esters such as acrylonitrile and vinyl-n-butyl ether, maleic acid monoesters such as maleic acid, maleic anhydride, monomethyl maleate, monoethyl maleate, and monoisopropyl maleate, fumaric acid, cinnamic acid, α-cyanocinnamic acid, itaconic acid, and crotonic acid. These polymerizable monomers may be used alone or in combination of two or more.
[0223] In order to improve the alkali developability, the (meth)acrylic resin preferably has a structural unit having an acid group. Examples of the acid group include a carboxy group, a sulfo group, a phosphoric acid group, and a phosphonic acid group. Among these, the (meth)acrylic resin more preferably has a structural unit having a carboxy group, and even more preferably has a structural unit derived from the above-mentioned (meth)acrylic acid.
[0224] The content of the structural unit having an acid group in the (meth)acrylic resin (preferably a structural unit derived from (meth)acrylic acid) is preferably 10% by mass or more based on the total mass of the (meth)acrylic resin in terms of excellent developability. The upper limit is not particularly limited, but is preferably 50% by mass or less, more preferably 40% by mass or less, in terms of excellent alkali resistance.
[0225] Moreover, the (meth)acrylic resin more preferably has a structural unit derived from the above-mentioned (meth)acrylic acid alkyl ester. The content of structural units derived from an alkyl (meth)acrylate in the (meth)acrylic resin is preferably 50% by mass to 90% by mass, more preferably 60% by mass to 90% by mass, and even more preferably 65% by mass to 90% by mass, based on all structural units of the (meth)acrylic resin.
[0226] As the (meth)acrylic resin, a resin having both a structural unit derived from (meth)acrylic acid and a structural unit derived from a (meth)acrylic acid alkyl ester is preferred, and a resin composed only of a structural unit derived from (meth)acrylic acid and a structural unit derived from a (meth)acrylic acid alkyl ester is more preferred. Furthermore, as the (meth)acrylic resin, an acrylic resin having a structural unit derived from methacrylic acid, a structural unit derived from methyl methacrylate, and a structural unit derived from ethyl acrylate is also preferred.
[0227] In addition, in terms of achieving better effects in the present disclosure, the (meth)acrylic resin preferably has at least one selected from the group consisting of structural units derived from methacrylic acid and structural units derived from an alkyl methacrylate ester, and preferably has both structural units derived from methacrylic acid and structural units derived from an alkyl methacrylate ester. The total content of the structural units derived from methacrylic acid and the structural units derived from methacrylic acid alkyl ester in the (meth)acrylic resin is preferably 40% by mass or more, more preferably 60% by mass or more, based on the total structural units of the (meth)acrylic resin, from the viewpoint of obtaining superior effects in the present disclosure. The upper limit is not particularly limited, and may be 100% by mass or less, and is preferably 80% by mass or less.
[0228] In addition, in terms of achieving better effects in the present disclosure, it is also preferable that the (meth)acrylic resin has at least one selected from the group consisting of structural units derived from methacrylic acid and structural units derived from an alkyl methacrylate ester, and at least one selected from the group consisting of structural units derived from acrylic acid and structural units derived from an alkyl acrylate ester. In order to obtain better effects in the present disclosure, the total content of the structural units derived from methacrylic acid and the structural units derived from an alkyl methacrylate ester is preferably 60 / 40 to 80 / 20 in mass ratio relative to the total content of the structural units derived from acrylic acid and the structural units derived from an alkyl acrylate ester.
[0229] The (meth)acrylic resin preferably has an ester group at the end, in view of excellent developability of the photosensitive resin layer after transfer. The terminal portion of the (meth)acrylic resin is composed of a portion derived from the polymerization initiator used in the synthesis. The (meth)acrylic resin having an ester group at the terminal can be synthesized by using a polymerization initiator that generates a radical having an ester group.
[0230] Moreover, the alkali-soluble resin is preferably an alkali-soluble resin having an acid value of 60 mgKOH / g or more, for example, from the viewpoint of developability. Moreover, the alkali-soluble resin is more preferably a resin having a carboxy group with an acid value of 60 mgKOH / g or more (so-called carboxy group-containing resin), and even more preferably a (meth)acrylic resin having a carboxy group with an acid value of 60 mgKOH / g or more (so-called carboxy group-containing (meth)acrylic resin), from the viewpoint of, for example, being thermally crosslinked with the crosslinking component by heating and easily forming a strong film. When the alkali-soluble resin has a carboxy group, the three-dimensional crosslinking density can be increased by, for example, adding a thermally crosslinkable compound such as a blocked isocyanate compound to thermally crosslink the resin. In addition, when the carboxy group of the resin having a carboxy group is dehydrated and hydrophobized, the humidity and heat resistance can be improved.
[0231] The carboxyl group-containing (meth)acrylic resin having an acid value of 60 mgKOH / g or more is not particularly limited as long as it satisfies the above-mentioned acid value condition, and can be appropriately selected from known (meth)acrylic resins. For example, among the polymers described in paragraph 0025 of JP-A-2011-095716, carboxyl group-containing acrylic resins having an acid value of 60 mgKOH / g or more, and among the polymers described in paragraphs 0033 to 0052 of JP-A-2010-237589, carboxyl group-containing acrylic resins having an acid value of 60 mgKOH / g or more can be preferably used.
[0232] Another preferred embodiment of the alkali-soluble resin is a styrene-acrylic copolymer. In this specification, the styrene-acrylic copolymer refers to a resin having a structural unit derived from a styrene compound and a structural unit derived from a (meth)acrylic compound, and the total content of the structural unit derived from the styrene compound and the structural unit derived from the (meth)acrylic compound is preferably 30% by mass or more, more preferably 50% by mass or more, based on the total structural units of the copolymer. The content of the structural units derived from a styrene compound is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 5 to 80% by mass, based on all the structural units of the copolymer. The content of the structural units derived from the (meth)acrylic compound is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass to 95% by mass, based on all structural units of the copolymer.
[0233] The alkali-soluble resin preferably has an aromatic ring structure, and more preferably has a constituent unit having an aromatic ring structure, in terms of achieving better effects in the present disclosure. Examples of monomers that form structural units having an aromatic ring structure include styrene compounds such as styrene, tert-butoxystyrene, methylstyrene, and α-methylstyrene, as well as benzyl (meth)acrylate. Of these, styrene compounds are preferred, and styrene is more preferred. In addition, the alkali-soluble resin more preferably has a constitutional unit represented by the following formula (S) (a constitutional unit derived from styrene), in terms of achieving better effects in the present disclosure.
[0234] [ka]
[0235] When the alkali-soluble resin has a structural unit having an aromatic ring structure, the content of the structural unit having an aromatic ring structure is preferably 5% by mass to 90% by mass, more preferably 10% by mass to 70% by mass, and further preferably 20% by mass to 60% by mass, based on the total structural units of the alkali-soluble resin, in terms of better effects in the present disclosure. Furthermore, the content of the structural units having an aromatic ring structure in the alkali-soluble resin is preferably 5 mol% to 70 mol%, more preferably 10 mol% to 60 mol%, and even more preferably 20 mol% to 60 mol%, based on the total structural units of the alkali-soluble resin, in terms of better effects in the present disclosure. Furthermore, the content of the structural unit represented by the above formula (S) in the alkali-soluble resin is preferably 5 mol% to 70 mol%, more preferably 10 mol% to 60 mol%, even more preferably 20 mol% to 60 mol%, and particularly preferably 20 mol% to 50 mol%, based on all structural units of the alkali-soluble resin, in terms of better effects in the present disclosure. In this specification, when the content of the "structural unit" is specified by a molar ratio, the "structural unit" is synonymous with the "monomer unit". In addition, in this specification, the "monomer unit" may be modified after polymerization by a polymer reaction or the like. The same applies hereinafter.
[0236] The alkali-soluble resin preferably has an aliphatic hydrocarbon ring structure in terms of better effects in the present disclosure. That is, the alkali-soluble resin preferably has a structural unit having an aliphatic hydrocarbon ring structure. In particular, the alkali-soluble resin more preferably has a ring structure in which two or more aliphatic hydrocarbon rings are condensed.
[0237] Examples of the ring that constitutes the aliphatic hydrocarbon ring structure in the structural unit having an aliphatic hydrocarbon ring structure include a tricyclodecane ring, a cyclohexane ring, a cyclopentane ring, a norbornane ring, and an isoborone ring. Among these, from the viewpoint of more excellent effects in the present disclosure, a ring in which two or more aliphatic hydrocarbon rings are condensed is preferred, and a tetrahydrodicyclopentadiene ring (tricyclo[5.2.1.0 2,6 ]decane ring) is more preferred. Examples of monomers that form a structural unit having an aliphatic hydrocarbon ring structure include dicyclopentanyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate. In addition, in terms of better effects in the present disclosure, the alkali-soluble resin more preferably has a constitutional unit represented by the following formula (Cy), and more preferably has a constitutional unit represented by the above formula (S) and a constitutional unit represented by the following formula (Cy).
[0238] [ka]
[0239] In the formula (Cy), R M represents a hydrogen atom or a methyl group, R Cy represents a monovalent group having an aliphatic hydrocarbon ring structure.
[0240] R in formula (Cy) M is preferably a methyl group. R in formula (Cy) Cy is preferably a monovalent group having an aliphatic hydrocarbon ring structure having 5 to 20 carbon atoms, more preferably a monovalent group having an aliphatic hydrocarbon ring structure having 6 to 16 carbon atoms, and even more preferably a monovalent group having an aliphatic hydrocarbon ring structure having 8 to 14 carbon atoms, in terms of achieving better effects in the present disclosure. R in formula (Cy) Cy The aliphatic hydrocarbon ring structure in may be a monocyclic structure or a polycyclic structure. In addition, R in formula (Cy)Cy In terms of achieving better effects in the present disclosure, the aliphatic hydrocarbon ring structure in is preferably a cyclopentane ring structure, a cyclohexane ring structure, a tetrahydrodicyclopentadiene ring structure, a norbornane ring structure, or an isoborone ring structure, more preferably a cyclohexane ring structure or a tetrahydrodicyclopentadiene ring structure, and even more preferably a tetrahydrodicyclopentadiene ring structure. Furthermore, R in formula (Cy) Cy In terms of achieving better effects in the present disclosure, the aliphatic hydrocarbon ring structure in is preferably a ring structure in which two or more aliphatic hydrocarbon rings are condensed, and more preferably a ring in which two to four aliphatic hydrocarbon rings are condensed. Furthermore, R in formula (Cy) Cy is preferably a group in which the oxygen atom of -C(=O)O- in formula (Cy) is directly bonded to an aliphatic hydrocarbon ring structure, i.e., an aliphatic hydrocarbon ring group, more preferably a cyclohexyl group or a dicyclopentanyl group, and even more preferably a dicyclopentanyl group, in terms of achieving better effects in the present disclosure.
[0241] The alkali-soluble resin may have one type of structural unit having an aliphatic hydrocarbon ring structure, or may have two or more types of structural units having an aliphatic hydrocarbon ring structure. When the alkali-soluble resin has a structural unit having an aliphatic hydrocarbon ring structure, the content of the structural unit having an aliphatic hydrocarbon ring structure is preferably 5% by mass to 90% by mass, more preferably 10% by mass to 80% by mass, and even more preferably 20% by mass to 70% by mass, based on the total structural units of the alkali-soluble resin, in terms of better effects in the present disclosure. Furthermore, the content of the structural units having an aliphatic hydrocarbon ring structure in the alkali-soluble resin is preferably 5 mol % to 70 mol %, more preferably 10 mol % to 60 mol %, and even more preferably 20 mol % to 50 mol %, based on the total structural units of the alkali-soluble resin, in terms of better effects in the present disclosure. Furthermore, the content of the structural unit represented by the above formula (Cy) in the alkali-soluble resin is preferably 5 mol % to 70 mol %, more preferably 10 mol % to 60 mol %, and even more preferably 20 mol % to 50 mol %, based on the total structural units of the alkali-soluble resin, in terms of better effects in the present disclosure.
[0242] When the alkali-soluble resin has a structural unit having an aromatic ring structure and a structural unit having an aliphatic hydrocarbon ring structure, the total content of the structural units having an aromatic ring structure and the structural units having an aliphatic hydrocarbon ring structure is preferably 10% by mass to 90% by mass, more preferably 20% by mass to 80% by mass, and even more preferably 40% by mass to 75% by mass, relative to all structural units of the alkali-soluble resin, in terms of better effects in the present disclosure. Furthermore, in terms of obtaining superior effects in the present disclosure, the total content of the structural units having an aromatic ring structure and the structural units having an aliphatic hydrocarbon ring structure in the alkali-soluble resin is preferably 10 mol% to 80 mol%, more preferably 20 mol% to 70 mol%, and even more preferably 40 mol% to 60 mol%, relative to all the structural units in the alkali-soluble resin. Furthermore, in terms of obtaining superior effects in the present disclosure, the total content of the structural units represented by the formula (S) and the structural units represented by the formula (Cy) in the alkali-soluble resin is preferably 10 mol% to 80 mol%, more preferably 20 mol% to 70 mol%, and even more preferably 40 mol% to 60 mol%, relative to all structural units of the alkali-soluble resin. In addition, in the alkali-soluble resin, the molar amount nS of the constitutional unit represented by the above formula (S) and the molar amount nCy of the constitutional unit represented by the above formula (Cy) are, from the viewpoint of obtaining superior effects in the present disclosure, It is preferable that the relationship shown in the following formula (SCy) is satisfied, it is more preferable that the relationship shown in the following formula (SCy-1) is satisfied, and it is even more preferable that the relationship shown in the following formula (SCy-2) is satisfied. 0.2≦nS / (nS+nCy)≦0.8 Formula (SCy) 0.30≦nS / (nS+nCy)≦0.75 Formula (SCy-1) 0.40≦nS / (nS+nCy)≦0.70 Formula (SCy-2)
[0243] The alkali-soluble resin preferably has a structural unit having an acid group, since the effects of the present disclosure are more excellent. Examples of the acid group include a carboxy group, a sulfo group, a phosphonic acid group, and a phosphoric acid group, with the carboxy group being preferred. As the structural unit having an acid group, a structural unit derived from (meth)acrylic acid shown below is preferred, and a structural unit derived from methacrylic acid is more preferred.
[0244] [ka]
[0245] The alkali-soluble resin may have one type of structural unit having an acid group alone, or may have two or more types of structural units having an acid group. When the alkali-soluble resin has a structural unit having an acid group, the content of the structural unit having an acid group is preferably 5% by mass to 50% by mass, more preferably 5% by mass to 40% by mass, and even more preferably 10% by mass to 30% by mass, based on the total structural units of the alkali-soluble resin, in terms of better effects in the present disclosure. Furthermore, the content of the structural units having an acid group in the alkali-soluble resin is preferably 5 mol% to 70 mol%, more preferably 10 mol% to 50 mol%, and even more preferably 20 mol% to 40 mol%, based on the total structural units of the alkali-soluble resin, in terms of better effects in the present disclosure. Furthermore, the content of the (meth)acrylic acid-derived structural units in the alkali-soluble resin is preferably 5 mol% to 70 mol%, more preferably 10 mol% to 50 mol%, and even more preferably 20 mol% to 40 mol%, based on the total structural units of the alkali-soluble resin, in terms of better effects in the present disclosure.
[0246] The alkali-soluble resin preferably has a reactive group, and more preferably has a structural unit having a reactive group, in terms of achieving better effects in the present disclosure. The reactive group is preferably a radical polymerizable group, more preferably an ethylenically unsaturated group. In addition, when the alkali-soluble resin has an ethylenically unsaturated group, the alkali-soluble resin preferably has a structural unit having an ethylenically unsaturated group in a side chain. In this specification, the term "main chain" refers to the relatively longest bond chain in the molecule of the polymer compound that constitutes the resin, and the term "side chain" refers to an atomic group branching off from the main chain. The ethylenically unsaturated group is more preferably an allyl group or a (meth)acryloxy group. Examples of structural units having a reactive group include, but are not limited to, those shown below.
[0247] [ka]
[0248] The alkali-soluble resin may have one type of structural unit having a reactive group, or may have two or more types of structural units having a reactive group. When the alkali-soluble resin has a structural unit having a reactive group, the content of the structural unit having a reactive group is preferably 5% by mass to 70% by mass, more preferably 10% by mass to 50% by mass, and even more preferably 20% by mass to 40% by mass, based on the total structural units of the alkali-soluble resin, in terms of better effects in the present disclosure. In addition, the content of the structural unit having a reactive group in the alkali-soluble resin is preferably 5 mol % to 70 mol %, more preferably 10 mol % to 60 mol %, and even more preferably 20 mol % to 50 mol %, based on the total structural units of the alkali-soluble resin, in terms of better effects of the present invention.
[0249] Examples of a method for introducing a reactive group into an alkali-soluble resin include a method in which a functional group such as a hydroxy group, a carboxy group, a primary amino group, a secondary amino group, an acetoacetyl group, or a sulfo group is reacted with a compound such as an epoxy compound, a blocked isocyanate compound, an isocyanate compound, a vinyl sulfone compound, an aldehyde compound, a methylol compound, or a carboxylic acid anhydride. A preferred example of a method for introducing a reactive group into an alkali-soluble resin is to synthesize a polymer having a carboxy group by polymerization, and then react a part of the carboxy group of the obtained resin with glycidyl (meth)acrylate by a polymer reaction to introduce a (meth)acryloxy group into the polymer. By this method, an alkali-soluble resin having a (meth)acryloxy group in the side chain can be obtained. The polymerization reaction is preferably carried out at a temperature of 70°C to 100°C, and more preferably at a temperature of 80°C to 90°C. The polymerization initiator used in the polymerization reaction is preferably an azo-based initiator, and more preferably, for example, V-601 (trade name) or V-65 (trade name) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. The polymer reaction is preferably carried out at a temperature of 80°C to 110°C. In the polymer reaction, it is preferable to use a catalyst such as an ammonium salt.
[0250] As the alkali-soluble resin, the resins shown below are preferred in terms of achieving better effects in the present disclosure. The content ratios (a to d) of each of the structural units shown below and the weight average molecular weight Mw can be appropriately changed depending on the purpose.
[0251] [ka]
[0252] [ka]
[0253] The alkali-soluble resin may also contain a polymer having a structural unit with a carboxylic acid anhydride structure (hereinafter, also referred to as "polymer X"). The carboxylic acid anhydride structure may be either a chain carboxylic acid anhydride structure or a cyclic carboxylic acid anhydride structure, but is preferably a cyclic carboxylic acid anhydride structure. The ring of the cyclic carboxylic acid anhydride structure is preferably a 5- to 7-membered ring, more preferably a 5- or 6-membered ring, and even more preferably a 5-membered ring.
[0254] The structural unit having a carboxylic acid anhydride structure is preferably a structural unit containing a divalent group obtained by removing two hydrogen atoms from a compound represented by the following formula P-1 in its main chain, or a structural unit in which a monovalent group obtained by removing one hydrogen atom from a compound represented by the following formula P-1 is bonded to the main chain directly or via a divalent linking group.
[0255] [ka]
[0256] In formula P-1, R A1a represents a substituent, n 1a R A1a may be the same or different, Z 1a represents a divalent group forming a ring containing -C(=O)-OC(=O)-, n 1a represents an integer greater than or equal to 0.
[0257] R A1a Examples of the substituent represented by the formula (I) include an alkyl group. Z 1a As the alkylene group, an alkylene group having 2 to 4 carbon atoms is preferable, an alkylene group having 2 or 3 carbon atoms is more preferable, and an alkylene group having 2 carbon atoms is even more preferable. n 1a represents an integer equal to or greater than 0. 1a When represents an alkylene group having 2 to 4 carbon atoms, n 1a is preferably an integer of 0 to 4, more preferably an integer of 0 to 2, and even more preferably 0. n 1a If represents an integer of 2 or more, there are multiple R A1a may be the same or different. In addition, if there are multiple R A1a may be bonded to each other to form a ring, but preferably do not bond to each other to form a ring.
[0258] As a structural unit having a carboxylic acid anhydride structure, a structural unit derived from an unsaturated carboxylic acid anhydride is preferable, a structural unit derived from an unsaturated cyclic carboxylic acid anhydride is more preferable, a structural unit derived from an unsaturated aliphatic cyclic carboxylic acid anhydride is even more preferable, a structural unit derived from maleic anhydride or itaconic anhydride is particularly preferable, and a structural unit derived from maleic anhydride is most preferable.
[0259] Specific examples of structural units having a carboxylic acid anhydride structure are given below, but the structural units having a carboxylic acid anhydride structure are not limited to these specific examples. In the following structural units, Rx represents a hydrogen atom, a methyl group, a CH2OH group, or a CF3 group, and Me represents a methyl group.
[0260] [ka]
[0261] [ka]
[0262] The structural unit having a carboxylic acid anhydride structure in the polymer X may be of one type alone, or of two or more types.
[0263] The total content of the structural units having a carboxylic acid anhydride structure relative to all the structural units of polymer X is preferably from 0 mol % to 60 mol %, more preferably from 5 mol % to 40 mol %, and even more preferably from 10 mol % to 35 mol %.
[0264] The photosensitive resin layer may contain only one type of polymer X, or may contain two or more types. When the photosensitive resin layer contains polymer X, the content of polymer X is preferably 0.1 mass % to 30 mass %, more preferably 0.2 mass % to 20 mass %, even more preferably 0.5 mass % to 20 mass %, and still more preferably 1 mass % to 20 mass %, relative to the total mass of the photosensitive resin layer, in terms of better effects of the present disclosure.
[0265] The weight average molecular weight (Mw) of the alkali-soluble resin is preferably 5,000 or more, more preferably 10,000 or more, further preferably 10,000 to 50,000, and particularly preferably 20,000 to 30,000, in terms of achieving better effects in the present disclosure.
[0266] The acid value of the alkali-soluble resin is preferably from 10 mgKOH / g to 200 mgKOH / g, more preferably from 60 mgKOH / g to 200 mgKOH / g, further preferably from 60 mgKOH / g to 150 mgKOH / g, and particularly preferably from 60 mgKOH / g to 110 mgKOH / g. The acid value of the alkali-soluble resin is a value measured according to the method described in JIS K0070:1992.
[0267] The photosensitive resin layer may contain only one type of alkali-soluble resin, or may contain two or more types of alkali-soluble resin. The content of the alkali-soluble resin is preferably 10% by mass to 90% by mass, more preferably 20% by mass to 80% by mass, and even more preferably 30% by mass to 70% by mass, relative to the total mass of the photosensitive resin layer, in order to obtain better effects in the present disclosure.
[0268] <Ethylenically unsaturated compounds> The photosensitive resin layer contains an ethylenically unsaturated compound. The ethylenically unsaturated group is preferably a (meth)acryloxy group. The ethylenically unsaturated compound in this specification is a compound other than the above-mentioned alkali-soluble resins, and preferably has a molecular weight of less than 5,000. Moreover, preferred embodiments of the ethylenically unsaturated compound used in the second embodiment include the preferred embodiments of the ethylenically unsaturated compound used in the first embodiment described above.
[0269] One preferred embodiment of the ethylenically unsaturated compound is a compound represented by the following formula (M) (also simply referred to as "compound M"). Q 2 -R 1 -Q1 Formula (M) In formula (M), Q 1 and Q 2 each independently represents a (meth)acryloyloxy group; R 1 represents a divalent linking group having a chain structure.
[0270] Q in formula (M) 1 and Q 2 From the viewpoint of ease of synthesis, Q 1 and Q 2 are preferably the same group. In addition, Q in formula (M) 1 and Q 2 is preferably an acryloyloxy group from the viewpoint of reactivity. R in formula (M) 1 As the alkylene group, an alkyleneoxyalkylene group (-L 1 -OL 1 -), or a polyalkyleneoxyalkylene group (-(L 1 -O) p -L 1 -) is preferred, a hydrocarbon group having 2 to 20 carbon atoms or a polyalkyleneoxyalkylene group is more preferred, an alkylene group having 4 to 20 carbon atoms is further preferred, and a linear alkylene group having 6 to 18 carbon atoms is particularly preferred. The hydrocarbon group may have a chain structure at least in a portion thereof, and the portion other than the chain structure is not particularly limited and may be, for example, a branched, cyclic, or linear alkylene group having 1 to 5 carbon atoms, an arylene group, an ether bond, or a combination thereof. An alkylene group or a group combining two or more alkylene groups and one or more arylene groups is preferable, an alkylene group is more preferable, and a linear alkylene group is even more preferable. In addition, the above L 1 each independently represents an alkylene group, preferably an ethylene group, a propylene group, or a butylene group, more preferably an ethylene group or a 1,2-propylene group. p represents an integer of 2 or more, and is preferably an integer of 2 to 10.
[0271] In addition, Q in compound M 1 and Q 2 The number of atoms in the shortest linking chain between and is preferably 3 to 50, more preferably 4 to 40, even more preferably 6 to 20, and particularly preferably 8 to 12, in terms of achieving better effects in the present disclosure. As used herein, "Q 1 and Q 2 The number of atoms in the shortest chain connecting Q 1 R to be connected 1 Q from atoms in 2 R to be connected 1 is the shortest number of atoms that can connect to an atom in
[0272] Specific examples of the compound M include 1,3-butanediol di(meth)acrylate, tetramethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,7-heptanediol di(meth)acrylate, 1,8-octanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 1,4-cyclohexanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, hydrogenated bisphenol A di(meth)acrylate, hydrogenated bisphenol F di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, poly(ethylene glycol / propylene glycol) di(meth)acrylate, and polybutylene glycol di(meth)acrylate. The above ester monomers may also be used as mixtures. Among the above compounds, in terms of better effects in the present disclosure, at least one compound selected from the group consisting of 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, and neopentyl glycol di(meth)acrylate is preferred, at least one compound selected from the group consisting of 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, and 1,10-decanediol di(meth)acrylate is more preferred, and at least one compound selected from the group consisting of 1,9-nonanediol di(meth)acrylate and 1,10-decanediol di(meth)acrylate is even more preferred.
[0273] One of the preferred embodiments of the ethylenically unsaturated compound is a di- or higher functional ethylenically unsaturated compound. In this specification, the term "di- or higher functional ethylenically unsaturated compound" means a compound having two or more ethylenically unsaturated groups in one molecule. As the ethylenically unsaturated group in the ethylenically unsaturated compound, a (meth)acryloyl group is preferred. As the ethylenically unsaturated compound, a (meth)acrylate compound is preferred.
[0274] The difunctional ethylenically unsaturated compound is not particularly limited and can be appropriately selected from known compounds. Examples of the difunctional ethylenically unsaturated compound other than the compound M include tricyclodecane dimethanol di(meth)acrylate and tricyclodecane dimenanol di(meth)acrylate.
[0275] Commercially available bifunctional ethylenically unsaturated compounds include tricyclodecane dimethanol diacrylate (trade name: NK Ester A-DCP, manufactured by Shin-Nakamura Chemical Co., Ltd.), tricyclodecane dimenanol dimethacrylate (trade name: NK Ester DCP, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,9-nonanediol diacrylate (trade name: NK Ester A-NOD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), and 1,6-hexanediol diacrylate (trade name: NK Ester A-HD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.).
[0276] The tri- or higher functional ethylenically unsaturated compound is not particularly limited and can be appropriately selected from known compounds. Examples of the tri- or higher functional ethylenically unsaturated compound include dipentaerythritol (tri / tetra / penta / hexa)(meth)acrylate, pentaerythritol (tri / tetra)(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, isocyanuric acid (meth)acrylate, and (meth)acrylate compounds having a glycerin tri(meth)acrylate skeleton.
[0277] Here, "(tri / tetra / penta / hexa)(meth)acrylate" is a concept that encompasses tri(meth)acrylate, tetra(meth)acrylate, penta(meth)acrylate, and hexa(meth)acrylate, and "(tri / tetra)(meth)acrylate" is a concept that encompasses tri(meth)acrylate and tetra(meth)acrylate.
[0278] Examples of the ethylenically unsaturated compound include caprolactone-modified (meth)acrylate compounds (KAYARAD (registered trademark) DPCA-20 manufactured by Nippon Kayaku Co., Ltd., A-9300-1CL manufactured by Shin-Nakamura Chemical Co., Ltd., etc.), alkylene oxide-modified (meth)acrylate compounds (KAYARAD (registered trademark) RP-1040 manufactured by Nippon Kayaku Co., Ltd., ATM-35E and A-9300 manufactured by Shin-Nakamura Chemical Co., Ltd., EBECRYL (registered trademark) 135 manufactured by Daicel-Allnex Co., Ltd., etc.), and ethoxylated glycerin triacrylate (NK Ester A-GLY-9E manufactured by Shin-Nakamura Chemical Co., Ltd., etc.).
[0279] The ethylenically unsaturated compounds also include urethane (meth)acrylate compounds. Examples of the urethane (meth)acrylate include urethane di(meth)acrylate, such as propylene oxide modified urethane di(meth)acrylate, and ethylene oxide and propylene oxide modified urethane di(meth)acrylate. In addition, the urethane (meth)acrylate may be a trifunctional or higher urethane (meth)acrylate. The lower limit of the number of functional groups is more preferably 6 or more, and even more preferably 8 or more. The upper limit of the number of functional groups is preferably 20 or less. Examples of trifunctional or higher urethane (meth)acrylates include 8UX-015A (manufactured by Taisei Fine Chemical Co., Ltd.), UA-32P (manufactured by Shin-Nakamura Chemical Co., Ltd.), U-15HA (manufactured by Shin-Nakamura Chemical Co., Ltd.), UA-1100H (manufactured by Shin-Nakamura Chemical Co., Ltd.), AH-600 (trade name) manufactured by Kyoeisha Chemical Co., Ltd., and UA-306H, UA-306T, UA-306I, UA-510H, and UX-5000 (all manufactured by Nippon Kayaku Co., Ltd.).
[0280] One of the preferred embodiments of the ethylenically unsaturated compound is an ethylenically unsaturated compound having an acid group. Acid groups include phosphate groups, sulfo groups, and carboxy groups. Among these, the acid group is preferably a carboxy group. Examples of the ethylenically unsaturated compound having an acid group include a trifunctional or tetrafunctional ethylenically unsaturated compound having an acid group [a carboxy group has been introduced into a pentaerythritol tri- or tetraacrylate (PETA) skeleton (acid value: 80 mg KOH / g to 120 mg KOH / g)], a pentafunctional or hexafunctional ethylenically unsaturated compound having an acid group (a carboxy group has been introduced into a dipentaerythritol penta- or hexaacrylate (DPHA) skeleton (acid value: 25 mg KOH / g to 70 mg KOH / g)], and the like. These trifunctional or higher ethylenically unsaturated compounds having an acid group may be used in combination with a difunctional ethylenically unsaturated compound having an acid group, if necessary.
[0281] The ethylenically unsaturated compound having an acid group is preferably at least one selected from the group consisting of di- or higher functional ethylenically unsaturated compounds having a carboxy group and carboxylic acid anhydrides thereof. When the ethylenically unsaturated compound having an acid group is at least one selected from the group consisting of di- or higher functional ethylenically unsaturated compounds having a carboxy group and carboxylic acid anhydrides thereof, the developability and film strength are further improved. The di- or higher functional ethylenically unsaturated compound having a carboxy group is not particularly limited and can be appropriately selected from known compounds. Examples of difunctional or higher ethylenically unsaturated compounds having a carboxy group include ARONIX (registered trademark) TO-2349 (manufactured by Toagosei Co., Ltd.), ARONIX (registered trademark) M-520 (manufactured by Toagosei Co., Ltd.), and ARONIX (registered trademark) M-510 (manufactured by Toagosei Co., Ltd.).
[0282] As the ethylenically unsaturated compound having an acid group, the polymerizable compounds having an acid group described in paragraphs 0025 to 0030 of JP-A No. 2004-239942 are preferred, and the contents of this publication are incorporated herein by reference.
[0283] Examples of the ethylenically unsaturated compound include compounds obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid, compounds obtained by reacting a glycidyl group-containing compound with an α,β-unsaturated carboxylic acid, urethane monomers such as (meth)acrylate compounds having a urethane bond, phthalic acid compounds such as γ-chloro-β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate, β-hydroxyethyl-β'-(meth)acryloyloxyethyl-o-phthalate, and β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate, and (meth)acrylic acid alkyl esters. These may be used alone or in combination of two or more.
[0284] Examples of compounds obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid include bisphenol A-based (meth)acrylate compounds such as 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane, 2,2-bis(4-((meth)acryloxypolypropoxy)phenyl)propane, and 2,2-bis(4-((meth)acryloxypolyethoxypolypropoxy)phenyl)propane; polyethylene glycol di(meth)acrylates having 2 to 14 ethylene oxide groups; polypropylene glycol di(meth)acrylates having 2 to 14 propylene oxide groups; polyethylene polypropylene glycol di(meth)acrylates having 2 to 14 ethylene oxide groups and 2 to 14 propylene oxide groups; trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane ethoxy tri(meth)acrylate, trimethylolpropane diethoxy tri(meth)acrylate, trimethylolpropane triethoxy tri(meth)acrylate, trimethylolpropane tetraethoxy tri(meth)acrylate, trimethylolpropane pentaethoxy tri(meth)acrylate, di(trimethylolpropane) tetraacrylate, tetramethylolmethane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. Among these, ethylenically unsaturated compounds having a tetramethylolmethane structure or a trimethylolpropane structure are preferred, and tetramethylolmethane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, trimethylolpropane tri(meth)acrylate, or di(trimethylolpropane)tetraacrylate are more preferred.
[0285] Examples of the ethylenically unsaturated compound include caprolactone-modified ethylenically unsaturated compounds (e.g., KAYARAD (registered trademark) DPCA-20 manufactured by Nippon Kayaku Co., Ltd., A-9300-1CL manufactured by Shin-Nakamura Chemical Co., Ltd., etc.), alkylene oxide-modified ethylenically unsaturated compounds (e.g., KAYARAD RP-1040 manufactured by Nippon Kayaku Co., Ltd., ATM-35E and A-9300 manufactured by Shin-Nakamura Chemical Co., Ltd., EBECRYL (registered trademark) 135 manufactured by Daicel-Allnex Corporation, etc.), and ethoxylated glycerin triacrylate (A-GLY-9E manufactured by Shin-Nakamura Chemical Co., Ltd., etc.).
[0286] As the ethylenically unsaturated compound, those containing an ester bond are particularly preferred, in that they provide excellent developability of the photosensitive resin layer after transfer. The ethylenically unsaturated compound containing an ester bond is not particularly limited as long as it contains an ester bond in the molecule, but in terms of excellent effects in the present disclosure, an ethylenically unsaturated compound having a tetramethylolmethane structure or a trimethylolpropane structure is preferred, and tetramethylolmethane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, trimethylolpropane tri(meth)acrylate, or di(trimethylolpropane)tetraacrylate is more preferred. From the viewpoint of providing reliability, the ethylenically unsaturated compound preferably contains an ethylenically unsaturated compound having an aliphatic group having 6 to 20 carbon atoms and the above-mentioned ethylenically unsaturated compound having a tetramethylolmethane structure or a trimethylolpropane structure. Examples of ethylenically unsaturated compounds having an aliphatic structure having 6 or more carbon atoms include 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, and tricyclodecane dimethanol di(meth)acrylate.
[0287] One of the preferred embodiments of the ethylenically unsaturated compound is an ethylenically unsaturated compound having an aliphatic hydrocarbon ring structure (preferably a difunctional ethylenically unsaturated compound). The above-mentioned ethylenically unsaturated compound is preferably an ethylenically unsaturated compound having a ring structure in which two or more aliphatic hydrocarbon rings are condensed (preferably a structure selected from the group consisting of a tricyclodecane structure and a tricyclodecene structure), more preferably a bifunctional ethylenically unsaturated compound having a ring structure in which two or more aliphatic hydrocarbon rings are condensed, and even more preferably tricyclodecane dimethanol di(meth)acrylate. As the aliphatic hydrocarbon ring structure, a cyclopentane structure, a cyclohexane structure, a tricyclodecane structure, a tricyclodecene structure, a norbornane structure, or an isoborone structure is preferred in terms of achieving better effects in the present disclosure.
[0288] The molecular weight of the ethylenically unsaturated compound is preferably from 200 to 3,000, more preferably from 250 to 2,600, further preferably from 280 to 2,200, and particularly preferably from 300 to 2,200. Among the ethylenically unsaturated compounds contained in the photosensitive resin layer, the content ratio of ethylenically unsaturated compounds having a molecular weight of 300 or less is preferably 30 mass% or less, more preferably 25 mass% or less, and even more preferably 20 mass% or less, based on the content of all ethylenically unsaturated compounds contained in the photosensitive resin layer.
[0289] As one of the preferred embodiments of the photosensitive resin layer, the photosensitive resin layer preferably contains a difunctional or higher ethylenically unsaturated compound, more preferably contains a trifunctional or higher ethylenically unsaturated compound, and even more preferably contains a trifunctional or tetrafunctional ethylenically unsaturated compound.
[0290] In addition, as one of the preferred embodiments of the photosensitive resin layer, the photosensitive resin layer preferably contains a bifunctional ethylenically unsaturated compound having an aliphatic hydrocarbon ring structure and an alkali-soluble resin having a structural unit having an aliphatic hydrocarbon ring.
[0291] In addition, as one of the preferred embodiments of the photosensitive resin layer, the photosensitive resin layer preferably contains a compound represented by formula (M) and an ethylenically unsaturated compound having an acid group, more preferably contains 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, and a polyfunctional ethylenically unsaturated compound having a carboxylic acid group, and even more preferably contains 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, and a succinic acid modified product of dipentaerythritol pentaacrylate.
[0292] In addition, as one of the preferred embodiments of the photosensitive resin layer, the photosensitive resin layer preferably contains a compound represented by formula (M), an ethylenically unsaturated compound having an acid group, and a thermally crosslinkable compound described later, and more preferably contains a compound represented by formula (M), an ethylenically unsaturated compound having an acid group, and a blocked isocyanate compound described later.
[0293] In addition, as one of the preferred embodiments of the photosensitive resin layer, the photosensitive resin layer preferably contains a difunctional ethylenically unsaturated compound (preferably a difunctional (meth)acrylate compound) and a trifunctional or higher ethylenically unsaturated compound (preferably a trifunctional or higher (meth)acrylate compound).
[0294] In one preferred embodiment of the photosensitive resin layer, the photosensitive resin layer preferably contains a compound M and a bifunctional ethylenically unsaturated compound having an aliphatic hydrocarbon ring structure from the viewpoint of rust prevention. In addition, as one of the preferred embodiments of the photosensitive resin layer, from the viewpoints of substrate adhesion, suppression of development residue, and rust prevention, the photosensitive resin layer preferably contains a compound M and an ethylenically unsaturated compound having an acid group, more preferably contains a compound M, a bifunctional ethylenically unsaturated compound having an aliphatic hydrocarbon ring structure, and an ethylenically unsaturated compound having an acid group, still more preferably contains a compound M, a bifunctional ethylenically unsaturated compound having an aliphatic hydrocarbon ring structure, a tri- or higher functional ethylenically unsaturated compound, and an ethylenically unsaturated compound having an acid group, and particularly preferably contains a compound M, a bifunctional ethylenically unsaturated compound having an aliphatic hydrocarbon ring structure, a tri- or higher functional ethylenically unsaturated compound, an ethylenically unsaturated compound having an acid group, and a urethane (meth)acrylate compound. In addition, as one of the preferred embodiments of the photosensitive resin layer, from the viewpoints of substrate adhesion, development residue suppression, and rust prevention, the photosensitive resin layer preferably contains 1,9-nonanediol diacrylate and a polyfunctional ethylenically unsaturated compound having a carboxylic acid group, preferably contains 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, and a polyfunctional ethylenically unsaturated compound having a carboxylic acid group, more preferably contains 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, dipentaerythritol hexaacrylate, and an ethylenically unsaturated compound having a carboxylic acid group, and particularly preferably contains 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, an ethylenically unsaturated compound having a carboxylic acid group, and a urethane acrylate compound.
[0295] The photosensitive resin layer may contain a monofunctional ethylenically unsaturated compound as the ethylenically unsaturated compound. The content of the di- or higher functional ethylenically unsaturated compound in the above ethylenically unsaturated compound is preferably 60% by mass to 100% by mass, more preferably 80% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass, based on the total content of all ethylenically unsaturated compounds contained in the photosensitive resin layer.
[0296] The ethylenically unsaturated compounds may be used alone or in combination of two or more kinds. The content of the ethylenically unsaturated compound in the photosensitive resin layer is preferably 1% by mass to 70% by mass, more preferably 5% by mass to 70% by mass, even more preferably 5% by mass to 60% by mass, and particularly preferably 5% by mass to 50% by mass, relative to the total mass of the photosensitive resin layer.
[0297] <Photopolymerization initiator> The photosensitive resin layer contains a photopolymerization initiator. Preferred aspects of the photopolymerization initiator used in the second embodiment include the preferred aspects of the photopolymerization initiator used in the first embodiment described above. The photopolymerization initiator may be used alone or in combination of two or more kinds. The content of the photopolymerization initiator is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1.0% by mass or more, based on the total mass of the photosensitive resin layer, and the upper limit is preferably 10% by mass or less, more preferably 5% by mass or less, based on the total mass of the photosensitive resin layer.
[0298] <Heterocyclic compounds> The photosensitive resin layer may contain a heterocyclic compound. The heterocycle contained in the heterocyclic compound may be either a monocyclic or polycyclic heterocycle. Examples of the heteroatom contained in the heterocyclic compound include a nitrogen atom, an oxygen atom, and a sulfur atom. The heterocyclic compound preferably contains at least one atom selected from the group consisting of a nitrogen atom, an oxygen atom, and a sulfur atom, and more preferably contains a nitrogen atom.
[0299] Examples of heterocyclic compounds include triazole compounds, benzotriazole compounds, tetrazole compounds, thiadiazole compounds, triazine compounds, rhodanine compounds, thiazole compounds, benzothiazole compounds, benzimidazole compounds, benzoxazole compounds, and pyrimidine compounds. Among the above, the heterocyclic compound is preferably at least one compound selected from the group consisting of triazole compounds, benzotriazole compounds, tetrazole compounds, thiadiazole compounds, triazine compounds, rhodanine compounds, thiazole compounds, benzimidazole compounds, and benzoxazole compounds, and more preferably at least one compound selected from the group consisting of triazole compounds, benzotriazole compounds, tetrazole compounds, thiadiazole compounds, thiazole compounds, benzothiazole compounds, benzimidazole compounds, and benzoxazole compounds.
[0300] Preferable specific examples of the heterocyclic compound are shown below. As the triazole compound and the benzotriazole compound, the following compounds can be exemplified.
[0301] [ka]
[0302] [ka]
[0303] Examples of the tetrazole compound include the following compounds.
[0304] [ka]
[0305] [ka]
[0306] Examples of the thiadiazole compound include the following compounds.
[0307] [ka]
[0308] Examples of the triazine compound include the following compounds.
[0309] [ka]
[0310] Examples of rhodanine compounds include the following compounds.
[0311] [ka]
[0312] Examples of the thiazole compound include the following compounds.
[0313] [ka]
[0314] Examples of the benzothiazole compound include the following compounds.
[0315] [ka]
[0316] Examples of the benzimidazole compound include the following compounds.
[0317] [ka]
[0318] [ka]
[0319] Examples of the benzoxazole compound include the following compounds.
[0320] [ka]
[0321] The heterocyclic compounds may be used alone or in combination of two or more. When the photosensitive resin layer contains a heterocyclic compound, the content of the heterocyclic compound is preferably 0.01 mass% to 20.0 mass%, more preferably 0.10 mass% to 10.0 mass%, further preferably 0.30 mass% to 8.0 mass%, and particularly preferably 0.50 mass% to 5.0 mass%, relative to the total mass of the photosensitive resin layer.
[0322] <Aliphatic thiol compounds> The photosensitive resin layer may contain an aliphatic thiol compound. When the photosensitive resin layer contains an aliphatic thiol compound, the aliphatic thiol compound undergoes an ene-thiol reaction with the ethylenically unsaturated compound, thereby suppressing the cure shrinkage of the film formed and reducing stress.
[0323] The aliphatic thiol compound is preferably a monofunctional aliphatic thiol compound or a polyfunctional aliphatic thiol compound (that is, a di- or higher functional aliphatic thiol compound). Among the above, as the aliphatic thiol compound, polyfunctional aliphatic thiol compounds are more preferable from the viewpoint of adhesion of the pattern to be formed (particularly adhesion after exposure). In this specification, the term "polyfunctional aliphatic thiol compound" refers to an aliphatic compound having two or more thiol groups (also called "mercapto groups") in the molecule.
[0324] The polyfunctional aliphatic thiol compound is preferably a low molecular weight compound having a molecular weight of at least 100. Specifically, the molecular weight of the polyfunctional aliphatic thiol compound is more preferably 100 to 1,500, and further preferably 150 to 1,000.
[0325] The number of functional groups of the polyfunctional aliphatic thiol compound is preferably 2 to 10, more preferably 2 to 8, and even more preferably 2 to 6, from the viewpoint of adhesion of the formed pattern.
[0326] Examples of polyfunctional aliphatic thiol compounds include trimethylolpropane tris(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane, pentaerythritol tetrakis(3-mercaptobutyrate), 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, trimethylolethane tris(3-mercaptobutyrate), tris[(3-mercaptopropionyloxy)ethyl]isocyanurate, trimethylolpropane tris(3-mercaptopropionyloxy)ethyl]isocyanurate, ester), pentaerythritol tetrakis(3-mercaptopropionate), tetraethylene glycol bis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptopropionate), ethylene glycol bisthiopropionate, 1,4-bis(3-mercaptobutyryloxy)butane, 1,2-ethanedithiol, 1,3-propanedithiol, 1,6-hexamethylenedithiol, 2,2'-(ethylenedithio)diethanethiol, meso-2,3-dimercaptosuccinic acid, and di(mercaptoethyl)ether.
[0327] Among the above, the polyfunctional aliphatic thiol compound is preferably at least one compound selected from the group consisting of trimethylolpropane tris(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane, and 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione.
[0328] Examples of monofunctional aliphatic thiol compounds include 1-octanethiol, 1-dodecanethiol, β-mercaptopropionic acid, methyl-3-mercaptopropionate, 2-ethylhexyl-3-mercaptopropionate, n-octyl-3-mercaptopropionate, methoxybutyl-3-mercaptopropionate, and stearyl-3-mercaptopropionate.
[0329] The photosensitive resin layer may contain one kind of aliphatic thiol compound alone, or may contain two or more kinds of aliphatic thiol compounds. When the photosensitive resin layer contains an aliphatic thiol compound, the content of the aliphatic thiol compound is preferably 5 mass% or more, more preferably 5 mass% to 50 mass%, even more preferably 5 mass% to 30 mass%, and particularly preferably 8 mass% to 20 mass%, relative to the total mass of the photosensitive resin layer.
[0330] <Thermal crosslinkable compound> The photosensitive resin layer preferably contains a thermally crosslinkable compound from the viewpoints of the strength of the resulting cured film and the adhesion of the resulting uncured film. As the thermally crosslinkable compound used in the photosensitive resin layer of the second embodiment, the thermally crosslinkable compound described above in the photosensitive resin layer of the first embodiment is suitably used. The thermally crosslinkable compound may be used alone or in combination of two or more kinds. When the photosensitive resin layer contains a thermally crosslinkable compound, the content of the thermally crosslinkable compound is preferably 1 mass % to 50 mass %, and more preferably 5 mass % to 30 mass %, based on the total mass of the photosensitive resin layer.
[0331] <Surfactant> The photosensitive resin layer may contain a surfactant. As the surfactant used in the photosensitive resin layer of the second embodiment, the surfactants described above in the photosensitive resin layer of the first embodiment are suitably used. The surfactants may be used alone or in combination of two or more. When the photosensitive resin layer contains a surfactant, the content of the surfactant is preferably 0.01% by mass to 3.0% by mass, more preferably 0.01% by mass to 1.0% by mass, and further preferably 0.05% by mass to 0.80% by mass, relative to the total mass of the photosensitive resin layer.
[0332] <Polymerization inhibitor> The photosensitive resin layer may contain a polymerization inhibitor. The polymerization inhibitor means a compound having a function of delaying or inhibiting a polymerization reaction. As the polymerization inhibitor, for example, a known compound used as a polymerization inhibitor can be used.
[0333] Examples of the polymerization inhibitor include phenothiazine compounds such as phenothiazine, bis-(1-dimethylbenzyl)phenothiazine, and 3,7-dioctylphenothiazine; bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylenebis(oxyethylene)]2,4-bis[(laurylthio)methyl]-o-cresol, 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl), 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl), 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, and pentaerythritol tetrakis 3-(3,5-di-te nitroso compounds or salts thereof, such as 4-nitrosophenol, N-nitrosodiphenylamine, N-nitrosocyclohexylhydroxylamine, and N-nitrosophenylhydroxylamine; quinone compounds, such as methylhydroquinone, t-butylhydroquinone, 2,5-di-t-butylhydroquinone, and 4-benzoquinone; phenol compounds, such as 4-methoxyphenol, 4-methoxy-1-naphthol, and t-butylcatechol; and metal salt compounds, such as copper dibutyldithiocarbamate, copper diethyldithiocarbamate, manganese diethyldithiocarbamate, and manganese diphenyldithiocarbamate. Among them, in terms of superior effects in the present disclosure, the polymerization inhibitor is preferably at least one selected from the group consisting of a phenothiazine compound, a nitroso compound or a salt thereof, and a hindered phenol compound, and more preferably phenothiazine, bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylene bis(oxyethylene)]2,4-bis[(laurylthio)methyl]-o-cresol, 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl), and N-nitrosophenylhydroxylamine aluminum salt.
[0334] The polymerization inhibitor may be used alone or in combination of two or more kinds. When the photosensitive resin layer contains a polymerization inhibitor, the content of the polymerization inhibitor is preferably 0.01 to 10.0% by mass, more preferably 0.01 to 5.0% by mass, and further preferably 0.04 to 3.0% by mass, based on the total mass of the photosensitive resin layer.
[0335] <Hydrogen donor compound> The photosensitive resin layer may contain a hydrogen donor compound. The hydrogen donor compound has the effect of further improving the sensitivity of the photopolymerization initiator to actinic rays and suppressing the inhibition of polymerization of the ethylenically unsaturated compound by oxygen. Examples of hydrogen donor compounds include amines and amino acid compounds.
[0336] Examples of amines include compounds described in MR Sander et al., Journal of Polymer Society, Vol. 10, p. 3173 (1972), JP-B-020189 / 1969, JP-A-51-082102, JP-A-52-134692, JP-A-59-138205, JP-A-60-084305, JP-A-62-018537, JP-A-64-033104, and Research Disclosure No. 33825. More specifically, 4,4'-bis(diethylamino)benzophenone, tris(4-dimethylaminophenyl)methane (also known as leuco crystal violet), triethanolamine, p-dimethylaminobenzoic acid ethyl ester, p-formyldimethylaniline, and p-methylthiodimethylaniline. Among these, in terms of achieving better effects in the present disclosure, the amine is preferably at least one selected from the group consisting of 4,4'-bis(diethylamino)benzophenone and tris(4-dimethylaminophenyl)methane.
[0337] Examples of the amino acid compound include N-phenylglycine, N-methyl-N-phenylglycine, and N-ethyl-N-phenylglycine. Among these, N-phenylglycine is preferred as the amino acid compound in that it provides superior effects in the present disclosure.
[0338] Further, examples of hydrogen donor compounds include organometallic compounds (such as tributyltin acetate) described in JP-B-48-042965, hydrogen donors described in JP-B-55-034414, and sulfur compounds (such as trithiane) described in JP-A-6-308727.
[0339] The hydrogen donor compounds may be used alone or in combination of two or more kinds. When the photosensitive resin layer contains a hydrogen donor compound, the content of the hydrogen donor compound is preferably 0.01 mass % to 10.0 mass %, more preferably 0.01 mass % to 8.0 mass %, and even more preferably 0.03 mass % to 5.0 mass %, relative to the total mass of the photosensitive resin layer, from the viewpoint of improving the curing rate through a balance between the polymerization growth rate and chain transfer.
[0340] <Impurities, etc.> The photosensitive resin layer may contain a predetermined amount of impurities. The impurities in the photosensitive resin layer of the second embodiment are similar to the preferred aspects of the impurities described above in the photosensitive resin layer of the first embodiment.
[0341] <Residual monomer> The photosensitive resin layer may contain residual monomers corresponding to the respective structural units of the alkali-soluble resin described above. The residual monomers corresponding to each structural unit of the alkali-soluble resin in the photosensitive resin layer of the second embodiment are the same as the preferred aspects of the residual monomers corresponding to each structural unit of the alkali-soluble resin described above in the photosensitive resin layer of the first embodiment.
[0342] <Other ingredients> The photosensitive resin layer may contain components other than those described above (hereinafter, also referred to as "other components"). Examples of the other components include colorants, antioxidants, and particles (e.g., metal oxide particles). Examples of the other components include other additives described in paragraphs 0058 to 0071 of JP-A-2000-310706.
[0343] -particle- The particles are preferably metal oxide particles. The metals in the metal oxide particles include metalloids such as B, Si, Ge, As, Sb, and Te. The average primary particle size of the particles is, for example, preferably from 1 nm to 200 nm, and more preferably from 3 nm to 80 nm, from the viewpoint of the transparency of the cured film. The average primary particle size of particles is calculated by measuring the particle sizes of 200 random particles using an electron microscope and taking the arithmetic mean of the measurement results. If the particle shape is not spherical, the longest side is used as the particle size.
[0344] When the photosensitive resin layer contains particles, it may contain only one type of particles having different metal species, sizes, etc., or may contain two or more types of particles. The photosensitive resin layer does not contain particles, or if the photosensitive resin layer contains particles, the particle content is preferably more than 0 mass% and 35 mass% or less, relative to the total mass of the photosensitive resin layer; more preferably, the photosensitive resin layer does not contain particles, or the particle content is more than 0 mass% and 10 mass% or less, relative to the total mass of the photosensitive resin layer; even more preferably, the photosensitive resin layer does not contain particles, or the particle content is more than 0 mass% and 5 mass% or less, relative to the total mass of the photosensitive resin layer; even more preferably, the photosensitive resin layer does not contain particles, or the particle content is more than 0 mass% and 1 mass% or less, relative to the total mass of the photosensitive resin layer; and it is particularly preferable that the photosensitive resin layer does not contain particles.
[0345] -Coloring agent- The photosensitive resin layer may contain a colorant (pigment, dye, etc.), but preferably does not substantially contain a colorant, for example, from the viewpoint of transparency. When the photosensitive resin layer contains a colorant, the content of the colorant is preferably less than 1% by mass, and more preferably less than 0.1% by mass, based on the total mass of the photosensitive resin layer.
[0346] -Antioxidants- Examples of antioxidants include 3-pyrazolidones such as 1-phenyl-3-pyrazolidone (also known as phenidone), 1-phenyl-4,4-dimethyl-3-pyrazolidone, and 1-phenyl-4-methyl-4-hydroxymethyl-3-pyrazolidone; polyhydroxybenzenes such as hydroquinone, catechol, pyrogallol, methylhydroquinone, and chlorohydroquinone; paramethylaminophenol, paraaminophenol, parahydroxyphenylglycine, and paraphenylenediamine. Among these, 3-pyrazolidones are preferred as the antioxidant, and 1-phenyl-3-pyrazolidone is more preferred, in terms of superior effect in the present disclosure.
[0347] When the photosensitive resin layer contains an antioxidant, the content of the antioxidant is preferably 0.001% by mass or more, more preferably 0.005% by mass or more, and even more preferably 0.01% by mass or more, based on the total mass of the photosensitive resin layer. There is no particular upper limit, but the content is preferably 1% by mass or less.
[0348] <Thickness of photosensitive resin layer> The thickness of the photosensitive resin layer is not particularly limited, but is often 30 μm or less, and is preferably 20 μm or less, more preferably 15 μm or less, even more preferably 10 μm or less, and particularly preferably 5.0 μm or less, in terms of superior effects in the present disclosure. The lower limit is preferably 0.60 μm or more, more preferably 1.5 μm or more, in terms of superior strength of the film obtained by curing the photosensitive resin layer. The thickness of the photosensitive resin layer can be calculated, for example, as the average value of any five points measured by cross-sectional observation using a scanning electron microscope (SEM).
[0349] <Refractive index of photosensitive resin layer> The refractive index of the photosensitive resin layer is preferably from 1.47 to 1.56, and more preferably from 1.49 to 1.54.
[0350] <Color of photosensitive resin layer> The photosensitive resin layer is preferably achromatic. Specifically, the total reflection (incident angle 8°, light source: D-65 (2° field of view)) is CIE1976(L * ,a * ,b * ) color space, L * The value is preferably 10 to 90, * The value is preferably -1.0 to 1.0, and b * The value is preferably between -1.0 and 1.0.
[0351] The pattern obtained by curing the photosensitive resin layer (cured film of the photosensitive resin layer) is preferably achromatic. Specifically, total reflection (incident angle 8°, light source: D-65 (2° field of view)) is * ,a * ,b * ) color space, the L * The value is preferably 10 to 90, and the pattern a * The value is preferably -1.0 to 1.0, and the b * The value is preferably between -1.0 and 1.0.
[0352] [Refractive index adjusting layer] The photosensitive transfer material preferably has a refractive index adjusting layer. The refractive index adjusting layer may be a known refractive index adjusting layer. Examples of materials contained in the refractive index adjusting layer include an alkali-soluble resin, an ethylenically unsaturated compound, a metal salt, and particles. The method for controlling the refractive index of the refractive index adjusting layer is not particularly limited, and examples thereof include a method of using a resin having a predetermined refractive index alone, a method of using a resin and particles, and a method of using a complex of a metal salt and a resin.
[0353] Examples of the alkali-soluble resin and the ethylenically unsaturated compound include the alkali-soluble resin and the ethylenically unsaturated compound described above in the section "Photosensitive resin layer."
[0354] Examples of the particles include metal oxide particles and metal particles. The type of metal oxide particles is not particularly limited, and known metal oxide particles can be used. The metal in the metal oxide particles includes semimetals such as B, Si, Ge, As, Sb, and Te.
[0355] The average primary particle size of the particles is, for example, preferably from 1 nm to 200 nm, and more preferably from 3 nm to 80 nm, from the viewpoint of the transparency of the cured film. The average primary particle size of particles is calculated by measuring the particle sizes of 200 random particles using an electron microscope and taking the arithmetic mean of the measurement results. If the particle shape is not spherical, the longest side is used as the particle size.
[0356] Specifically, the metal oxide particles are preferably at least one selected from the group consisting of zirconium oxide particles (ZrO2 particles), Nb2O5 particles, titanium oxide particles (TiO2 particles), silicon dioxide particles (SiO2 particles), and composite particles thereof. Among these, the metal oxide particles are more preferably at least one type selected from the group consisting of zirconium oxide particles and titanium oxide particles, for example, from the viewpoint of ease of adjusting the refractive index.
[0357] Commercially available metal oxide particles include calcined zirconium oxide particles (manufactured by CIK Nanotech Co., Ltd., product name: ZRPGM15WT%-F04), calcined zirconium oxide particles (manufactured by CIK Nanotech Co., Ltd., product name: ZRPGM15WT%-F74), calcined zirconium oxide particles (manufactured by CIK Nanotech Co., Ltd., product name: ZRPGM15WT%-F75), calcined zirconium oxide particles (manufactured by CIK Nanotech Co., Ltd., product name: ZRPGM15WT%-F76), zirconium oxide particles (Nanouse OZ-S30M, manufactured by Nissan Chemical Industries, Ltd.), and zirconium oxide particles (Nanouse OZ-S30K, manufactured by Nissan Chemical Industries, Ltd.).
[0358] The particles may be used alone or in combination of two or more kinds. The content of the particles in the refractive index adjusting layer is preferably 1% by mass to 95% by mass, more preferably 20% by mass to 90% by mass, and further preferably 40% by mass to 85% by mass, based on the total mass of the refractive index adjusting layer. When titanium oxide is used as the metal oxide particles, the content of the titanium oxide particles is preferably 1 mass % to 95 mass %, more preferably 20 mass % to 90 mass %, and even more preferably 40 mass % to 85 mass %, relative to the total mass of the refractive index adjusting layer.
[0359] The refractive index of the refractive index adjusting layer is preferably higher than the refractive index of the photosensitive resin layer. The refractive index of the refractive index adjusting layer is preferably 1.50 or more, more preferably 1.55 or more, even more preferably 1.60 or more, and particularly preferably 1.65 or more. The upper limit of the refractive index of the refractive index adjusting layer is preferably 2.10 or less, more preferably 1.85 or less, even more preferably 1.78 or less, and particularly preferably 1.74 or less.
[0360] The thickness of the refractive index adjusting layer is preferably from 50 nm to 500 nm, more preferably from 55 nm to 110 nm, and further preferably from 60 nm to 100 nm.
[0361] <Method for producing photosensitive transfer material according to the second embodiment> The method for producing the photosensitive transfer material of the second embodiment is not particularly limited, and any known method can be used. Examples of a method for producing the photosensitive transfer material 10 shown in FIG. 2 include a method including a step of applying a photosensitive resin composition to the surface of the temporary support 1 to form a coating film, and then drying this coating film to form the photosensitive resin layer 3, and a step of applying a composition for forming a refractive index adjustment layer to the surface of the photosensitive resin layer 3 to form a coating film, and then drying this coating film to form the refractive index adjustment layer 5.
[0362] A protective film 7 is pressure-bonded onto the refractive index adjusting layer 5 of the laminate produced by the above-mentioned production method, thereby producing a photosensitive transfer material 10. As a manufacturing method for the photosensitive transfer material of the first embodiment, it is preferable to manufacture a photosensitive transfer material 10 comprising a temporary support 1, a photosensitive resin layer 3, a refractive index adjusting layer 5, and a protective film 7, by including a step of providing a protective film 7 so as to be in contact with the surface of the refractive index adjusting layer 5 opposite the side having the temporary support 1. After the photosensitive transfer material 10 is produced by the above-mentioned production method, a photosensitive transfer material in a roll form may be produced and stored by winding up the photosensitive transfer material 10. The photosensitive transfer material in a roll form can be provided in that form as it is to the lamination step with a substrate in a roll-to-roll system described later.
[0363] The photosensitive transfer material 10 may be produced by forming the refractive index adjusting layer 5 on the protective film 7, and then forming the photosensitive resin layer 3 on the surface of the refractive index adjusting layer 5. In addition, the manufacturing method of the above-mentioned photosensitive transfer material 10 may be a method in which a photosensitive resin layer 3 is formed on a temporary support 1, a refractive index adjustment layer 5 is separately formed on a protective film 7, and the refractive index adjustment layer 5 is bonded to the photosensitive resin layer 3.
[0364] The method for forming the photosensitive resin composition and the photosensitive resin layer in the second embodiment is similar to the method for forming the photosensitive resin composition and the photosensitive resin layer described above in the first embodiment, and the preferred aspects are also similar.
[0365] <Composition for forming refractive index adjusting layer and method for forming refractive index adjusting layer> The composition for forming the refractive index adjusting layer preferably contains various components forming the refractive index adjusting layer described above and a solvent. Note that, in the composition for forming the refractive index adjusting layer, the preferred range of the content of each component relative to the total solid content of the composition is the same as the preferred range of the content of each component relative to the total mass of the refractive index adjusting layer described above. The solvent is not particularly limited as long as it is capable of dissolving or dispersing the components contained in the refractive index adjusting layer, and is preferably at least one selected from the group consisting of water and water-miscible organic solvents, and more preferably water or a mixed solvent of water and a water-miscible organic solvent. Examples of water-miscible organic solvents include alcohols having 1 to 3 carbon atoms, acetone, ethylene glycol, and glycerin, with alcohols having 1 to 3 carbon atoms being preferred, and methanol or ethanol being more preferred. The solvent may be used alone or in combination of two or more. The content of the solvent is preferably 50 parts by mass to 2,500 parts by mass, more preferably 50 parts by mass to 1,900 parts by mass, and even more preferably 100 parts by mass to 900 parts by mass, relative to 100 parts by mass of the total solid content of the composition.
[0366] The method for forming the refractive index adjusting layer is not particularly limited as long as it is a method capable of forming a layer containing the above components, and examples thereof include known coating methods (slit coating, spin coating, curtain coating, inkjet coating, etc.).
[0367] Moreover, by laminating a protective film to the refractive index adjusting layer, the photosensitive transfer material of the second embodiment can be produced. The method for bonding the protective film to the refractive index adjusting layer is not particularly limited, and may be any known method. Examples of a device for bonding the protective film to the refractive index adjusting layer include known laminators such as a vacuum laminator and an autocut laminator. The laminator is preferably equipped with any heatable roller, such as a rubber roller, and is capable of applying pressure and heat.
[0368] (Method for manufacturing resin pattern and method for manufacturing laminate) The method for producing a resin pattern according to the present disclosure is a method for producing a resin pattern by forming a resin pattern on a substrate using a photosensitive transfer material having a temporary support and a photosensitive resin layer. As a method for producing a resin pattern, a method including, in this order, a step of contacting and laminating the outermost layer of the photosensitive transfer material according to the present disclosure, which is on the side having a photosensitive resin layer with respect to the temporary support, with a substrate (hereinafter also referred to as the "lamination step"), a step of exposing the photosensitive resin layer to a pattern (hereinafter also referred to as the "exposure step"), and a step of developing the exposed photosensitive resin layer to form a resin pattern (hereinafter also referred to as the "development step"). Furthermore, in order to better exhibit the effects of the present disclosure, the method for producing a resin pattern according to the present disclosure preferably includes a line and space pattern in at least a portion of the resin pattern, and it is more preferable that at least a portion of the resin pattern includes a line and space pattern, and that the width of at least one pair of line and space in the line and space pattern is 20 μm in total or less.
[0369] The method for producing a laminate according to the present disclosure is a method for producing a laminate having a resin pattern on a substrate using the photosensitive transfer material according to the present disclosure. The method for producing the laminate is preferably a method including, in this order, the protective film peeling step, the laminating step, the exposure step, and the development step.
[0370] <Lamination process> The method for producing a resin pattern or a laminate preferably includes a lamination step. In the lamination step, it is preferable to bring the outermost layer of the photosensitive transfer material on the side having the photosensitive resin layer relative to the temporary support into contact with a substrate (if a conductive layer is provided on the surface of the substrate, the conductive layer) and press the photosensitive transfer material and the substrate together. In the above embodiment, the adhesion between the outermost layer of the photosensitive transfer material on the side having the photosensitive resin layer relative to the temporary support and the substrate is improved, so that the photosensitive transfer material can be suitably used as an etching resist when etching the conductive layer of the patterned photosensitive resin layer after exposure and development.
[0371] When the photosensitive transfer material has a protective film, the protective film may be removed from the surface of the photosensitive resin layer before lamination. Furthermore, in the case where the photosensitive transfer material further comprises a layer other than the protective film (e.g., a high refractive index layer and / or a low refractive index layer) on the surface of the photosensitive resin layer that does not face the temporary support, the lamination process is carried out in such a manner that the surface of the photosensitive resin layer that does not have the temporary support is laminated to the substrate via that layer.
[0372] The method for bonding the substrate and the photosensitive transfer material by pressure is not particularly limited, and known transfer methods and lamination methods can be used. The photosensitive transfer material is preferably laminated to the substrate by overlapping the outermost layer of the photosensitive transfer material on the side having the photosensitive resin layer with the temporary support and the substrate, and applying pressure and heat using a roll or other means. For the lamination, a known laminator such as a laminator, a vacuum laminator, or an autocut laminator that can further increase productivity can be used. The lamination temperature is not particularly limited, but is preferably from 70°C to 130°C, for example.
[0373] The method for producing a resin pattern and the method for producing a circuit wiring, which include the lamination step, are preferably carried out by a roll-to-roll method. The roll-to-roll method will be described below. The roll-to-roll method refers to a method in which a substrate that can be wound up and unwound is used as the substrate, and includes a step of unwinding the substrate or a structure including the substrate (also referred to as an "unwinding step") before any step included in the method for manufacturing a resin pattern or a method for manufacturing a circuit wiring, and a step of winding up the substrate or the structure including the substrate (also referred to as a "winding step") after any step, in which at least any step (preferably all steps, or all steps other than the heating step) is performed while the substrate or the structure including the substrate is being transported. The unwinding method in the unwinding step and the winding method in the winding step are not particularly limited, and any known method may be used in a production method that employs a roll-to-roll system.
[0374] <Substrate> As the substrate used in the method for producing a resin pattern or the method for producing a laminate according to the present disclosure, any known substrate may be used, but a substrate having a conductive layer is preferred, and it is more preferred that the substrate has a conductive layer on its surface. The substrate may have any layer other than the conductive layer, if necessary. Examples of the substrate include a resin substrate, a glass substrate, and a semiconductor substrate. Preferred embodiments of the substrate are described, for example, in paragraph 0140 of International Publication No. 2018 / 155193, the contents of which are incorporated herein by reference.
[0375] Examples of the base material constituting the substrate include glass, silicon, and films. The base material constituting the substrate is preferably transparent. In this specification, the term "transparent" means that the transmittance of light with a wavelength of 400 nm to 700 nm is 80% or more. The refractive index of the substrate constituting the substrate is preferably 1.50 to 1.52.
[0376] The transparent glass substrate may be a tempered glass such as Gorilla Glass manufactured by Corning Inc. In addition, the transparent glass substrate may be made of the materials described in JP-A-2010-86684, JP-A-2010-152809, and JP-A-2010-257492.
[0377] When a film substrate is used as the substrate, it is preferable to use a film substrate having small optical distortion and / or high transparency. Examples of such a film substrate include polyethylene terephthalate (PET), polyethylene naphthalate, polycarbonate, triacetyl cellulose, and cycloolefin polymer.
[0378] When the substrate is produced by a roll-to-roll method, a film substrate is preferable. When a circuit wiring for a touch panel is produced by a roll-to-roll method, the substrate is preferably a sheet-shaped resin composition.
[0379] The conductive layer of the substrate may be a conductive layer used for general circuit wiring or touch panel wiring. From the viewpoints of electrical conductivity and fine line formability, the conductive layer is preferably at least one layer selected from the group consisting of a metal layer, a conductive metal oxide layer, a graphene layer, a carbon nanotube layer, and a conductive polymer layer, more preferably a metal layer, and even more preferably a copper layer or a silver layer. The substrate may have one conductive layer or two or more conductive layers. When the substrate has two or more conductive layers, the conductive layers are preferably made of different materials.
[0380] Materials for the conductive layer include metals and conductive metal oxides. Metals include Al, Zn, Cu, Fe, Ni, Cr, Mo, Ag and Au. Examples of conductive metal oxides include indium tin oxide (ITO), indium zinc oxide (IZO), and SiO2. In this specification, "conductive" means a material having a volume resistivity of 1×10 6 The volume resistivity of conductive metal oxides is less than 1×10 4 Less than Ωcm is preferred.
[0381] When a resin pattern is produced using a substrate having a plurality of conductive layers, at least one of the plurality of conductive layers preferably contains a conductive metal oxide. The conductive layer is preferably an electrode pattern corresponding to a sensor of a visual recognition portion used in a capacitive touch panel or wiring of a peripheral extraction portion. Preferred embodiments of the conductive layer are described, for example, in paragraph 0141 of International Publication No. 2018 / 155193, the contents of which are incorporated herein by reference.
[0382] The substrate having a conductive layer is preferably a substrate having at least one of a transparent electrode and a lead wiring. Such a substrate can be suitably used as a substrate for a touch panel. The transparent electrode can function suitably as an electrode for a touch panel. The transparent electrode is preferably composed of a metal oxide film such as ITO (indium tin oxide) or IZO (indium zinc oxide), a metal mesh, or a metal thin wire such as silver nanowire. Examples of the thin metal wires include thin wires of silver, copper, etc. Among them, conductive silver materials such as silver mesh and silver nanowires are preferred.
[0383] The material of the lead wiring is preferably a metal. Examples of the metal material for the wiring include gold, silver, copper, molybdenum, aluminum, titanium, chromium, zinc, and manganese, and alloys of two or more of these metal elements. The material for the wiring is preferably copper, molybdenum, aluminum, or titanium, and particularly preferably copper.
[0384] The touch panel electrode protective film formed using the photosensitive transfer material according to the present disclosure is preferably provided so as to cover the electrodes, etc. directly or via another layer, for the purpose of protecting the electrodes, etc. (i.e., at least one of the electrodes for the touch panel and the wiring for the touch panel).
[0385] <Exposure process> The method for producing a resin pattern or the method for producing a laminate preferably includes, after the lamination step, a step of pattern-exposing the photosensitive resin layer (exposure step). Here, the term "pattern exposure" refers to a form of exposure in a pattern, that is, exposure in a form in which exposed areas and non-exposed areas exist. The positional relationship between the exposed and unexposed regions in the pattern exposure is not particularly limited and may be appropriately adjusted.
[0386] The detailed arrangement and the specific size of the pattern in the pattern exposure are not particularly limited. For example, in order to improve the display quality of a display device (e.g., a touch panel) equipped with an input device having a circuit wiring manufactured by the manufacturing method for circuit wiring, and to reduce the area occupied by the lead wiring, at least a part of the pattern (preferably the electrode pattern of the touch panel and / or the lead wiring part) preferably includes a thin line having a width of 20 μm or less, more preferably includes a thin line having a width of 10 μm or less.
[0387] The light source used for exposure can be appropriately selected and used as long as it irradiates light with a wavelength (e.g., 365 nm or 405 nm) that can expose the photosensitive resin layer. Specific examples include ultra-high pressure mercury lamps, high pressure mercury lamps, metal halide lamps, and LEDs (Light Emitting Diodes). The exposure dose was 5 mJ / cm 2 ~200mJ / cm 2 is preferred, and 10 mJ / cm 2 ~100mJ / cm 2 is more preferred. Preferred embodiments of the light source, exposure dose, and exposure method used for exposure are described, for example, in paragraphs 0146 to 0147 of WO 2018 / 155193, the contents of which are incorporated herein by reference.
[0388] In the exposure step, the photosensitive resin layer may be exposed to pattern light after the temporary support is peeled off from the photosensitive resin layer, or the temporary support may be exposed to pattern light through the temporary support before peeling off the temporary support. When the temporary support is peeled off before exposure, the mask may be exposed in contact with the photosensitive resin layer, or may be exposed in close proximity without contact. When the temporary support is not peeled off and the mask is exposed, the mask may be exposed in contact with the temporary support, or may be exposed in close proximity without contact. In order to prevent mask contamination due to contact between the photosensitive resin layer and the mask, and to avoid the influence of foreign matter attached to the mask on the exposure, it is preferable to perform pattern exposure without peeling off the temporary support. In the case of contact exposure, the exposure method may be a contact exposure method, and in the case of non-contact exposure, a proximity exposure method, a lens system or mirror system projection exposure method, a direct exposure method using an exposure laser, etc., may be appropriately selected and used. In the case of lens system or mirror system projection exposure, an exposure machine having an appropriate lens numerical aperture (NA) may be used according to the required resolution and focal depth. In the case of the direct exposure method, drawing may be performed directly on the photosensitive resin layer, or reduction projection exposure may be performed on the photosensitive resin layer through a lens. Exposure may be performed not only in the atmosphere but also under reduced pressure or vacuum, and exposure may be performed by interposing a liquid such as water between a light source and the photosensitive resin layer.
[0389] <Peeling process> The method for producing a resin pattern or the method for producing a laminate may include a peeling step of peeling off the temporary support between the laminating step and the exposure step, or between the exposure step and the development step. The method for peeling off the temporary support is not particularly limited, and a mechanism similar to the cover film peeling mechanism described in paragraphs 0161 to 0162 of JP-A No. 2010-072589 can be used.
[0390] <Developing process> The method for producing a resin pattern preferably includes, after the above-mentioned exposure step, a step of developing the exposed photosensitive resin layer to form a resin pattern (development step). When the photosensitive transfer material has a thermoplastic resin and an intermediate layer, the thermoplastic resin layer and the intermediate layer in the non-exposed area are removed together with the photosensitive resin layer in the non-exposed area in the development step. In addition, the thermoplastic resin layer and the intermediate layer in the exposed area may also be removed in a form dissolved or dispersed in the developer in the development step.
[0391] In the development step, the exposed photosensitive resin layer can be developed using a developer. The developer is not particularly limited as long as it can remove the non-image areas (non-exposed areas) of the photosensitive resin layer, and known developers such as the developer described in JP-A-5-72724 can be used. The developer is preferably an aqueous alkaline developer containing a compound having a pKa of 7 to 13 at a concentration of 0.05 mol / L to 5 mol / L (liter). The developer may contain a water-soluble organic solvent and / or a surfactant. Examples of alkaline compounds that can be contained in the alkaline aqueous solution include sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and choline (2-hydroxyethyltrimethylammonium hydroxide). Preferred examples of the developer include the developer described in paragraph 0194 of WO 2015 / 093271. Preferred examples of the development method include the development method described in paragraph 0195 of WO 2015 / 093271.
[0392] The development method is not particularly limited, and may be any of paddle development, shower development, shower and spin development, and dip development. Shower development is a development treatment in which a developer is sprayed by shower onto the photosensitive resin layer after exposure to remove the unexposed area. After the development step, it is preferable to remove development residues by spraying a cleaning agent by showering and scrubbing with a brush. The temperature of the developer is not particularly limited, but is preferably from 20°C to 40°C.
[0393] <Protective film peeling process> When the photosensitive transfer material has a protective film, the method for producing a resin pattern or the method for producing a laminate preferably includes a step of peeling the protective film from the photosensitive transfer material. The method for peeling the protective film is not limited, and a known method can be applied.
[0394] <Post-exposure process and post-bake process> The method for producing a resin pattern or a laminate may include a step of exposing the resin pattern obtained by the above-mentioned developing step (a post-exposure step) and / or a step of heating the resin pattern (a post-bake step). When both a post-exposure step and a post-bake step are included, it is preferable to carry out the post-bake step after the post-exposure step.
[0395] <Other processes> The method for producing a resin pattern or a laminate may include any step (other steps) other than the steps described above. For example, the steps described in the method for producing a circuit wiring or the method for producing a touch panel shown below may be included, but are not limited to these steps.
[0396] <Application> The resin pattern produced by the method for producing a resin pattern according to the present disclosure and the laminate produced by the method for producing a laminate according to the present disclosure can be applied to various devices. Examples of devices equipped with the laminate include input devices, etc., and are preferably touch panels, and more preferably capacitive touch panels. The input device can also be applied to displays such as organic electroluminescence displays and liquid crystal displays. When the laminate is applied to a touch panel, the formed resin pattern is preferably used as a protective film for an electrode for a touch panel or a wiring for a touch panel. In other words, the photosensitive transfer material according to the present disclosure is preferably used to form an electrode protective film for a touch panel or a wiring for a touch panel.
[0397] (Circuit Wiring Manufacturing Method) The method for producing the circuit wiring according to the present disclosure is not particularly limited as long as it is a method that uses the photosensitive transfer material according to the present disclosure. The method for manufacturing circuit wiring according to the present disclosure preferably includes, in this order, a step of contacting and laminating the outermost layer of the photosensitive transfer material according to the present disclosure, which is on the side having a photosensitive resin layer relative to the temporary support, with a substrate having a conductive layer, a step of exposing the photosensitive resin layer to a pattern, a step of developing the exposed photosensitive resin layer to form a resin pattern, and a step of etching the substrate in areas where the resin pattern is not arranged (hereinafter also referred to as the "etching step"). Below, each step included in the method for manufacturing circuit wiring will be explained, but unless otherwise specified, the contents explained for each step included in the method for manufacturing resin patterns also apply to each step included in the method for manufacturing circuit wiring.
[0398] <Etching process> The method for producing circuit wiring preferably includes a step of etching the substrate in the region where the resin pattern is not disposed (etching step).
[0399] In the etching process, the conductive layer is etched using the resin pattern formed from the photosensitive resin layer as an etching resist. As the etching method, known methods can be applied, for example, the method described in paragraphs 0209 to 0210 of JP 2017-120435 A, the method described in paragraphs 0048 to 0054 of JP 2010-152155 A, a wet etching method in which the substrate is immersed in an etching solution, and a dry etching method such as plasma etching can be mentioned.
[0400] The etching solution used in the wet etching may be an acidic or alkaline etching solution that is appropriately selected depending on the target to be etched. Examples of the acidic etching solution include an aqueous solution of an acidic component selected from hydrochloric acid, sulfuric acid, nitric acid, acetic acid, hydrofluoric acid, oxalic acid, and phosphoric acid, and an aqueous solution of a mixture of an acidic component and a salt selected from ferric chloride, ammonium fluoride, and potassium permanganate. The acidic component may be a combination of a plurality of acidic components. Examples of the alkaline etching solution include an aqueous solution of an alkaline component selected from sodium hydroxide, potassium hydroxide, ammonia, organic amines, and salts of organic amines (e.g., tetramethylammonium hydroxide), and an aqueous solution of a mixture of an alkaline component and a salt (e.g., potassium permanganate). The alkaline component may be a combination of a plurality of alkaline components.
[0401] <Removal process> In the method for producing circuit wiring, it is preferable to carry out a step of removing the remaining resin pattern (removal step). The removal step is not particularly limited and may be carried out as necessary, but is preferably carried out after the etching step. The method for removing the remaining resin pattern is not particularly limited, but includes a method of removing it by chemical treatment, and a method of removing it by using a removing liquid is preferable. The photosensitive resin layer can be removed by immersing the substrate having the remaining resin pattern in a stirring removal liquid having a liquid temperature of preferably 30°C to 80°C, more preferably 50°C to 80°C, for 1 minute to 30 minutes.
[0402] Examples of the removal liquid include a removal liquid obtained by dissolving an inorganic or organic alkaline component in water, dimethyl sulfoxide, N-methylpyrrolidone, or a mixture thereof. Examples of the inorganic alkaline component include sodium hydroxide and potassium hydroxide. Examples of the organic alkaline component include a primary amine compound, a secondary amine compound, a tertiary amine compound, and a quaternary ammonium salt compound. Alternatively, the removal may be performed by a known method such as a spray method, a shower method, or a paddle method using a removal liquid.
[0403] <Other processes> The method for producing a circuit wiring may include any steps (other steps) other than the steps described above, such as, but not limited to, the following steps. Moreover, examples of the exposure step, development step and other steps that can be applied to the method for producing circuit wiring include the steps described in paragraphs 0035 to 0051 of JP-A No. 2006-23696. Further, other steps include, for example, a step of reducing visible light reflectance described in paragraph 0172 of WO 2019 / 022089, a step of forming a new conductive layer on the insulating film described in paragraph 0172 of WO 2019 / 022089, and the like, but are not limited to these steps.
[0404] -Process to reduce visible light reflectance- The method for manufacturing circuit wiring may include a step of performing a treatment to reduce the visible light reflectance of some or all of the multiple conductive layers of the substrate. Examples of treatments for reducing the visible light reflectance include oxidation treatments. When the substrate has a conductive layer containing copper, the visible light reflectance of the conductive layer can be reduced by oxidizing the copper to copper oxide and blackening the conductive layer. Treatments for reducing visible light reflectance are described in paragraphs 0017 to 0025 of JP 2014-150118 A, and paragraphs 0041, 0042, 0048, and 0058 of JP 2013-206315 A, and the contents of these publications are incorporated herein by reference.
[0405] - A process for forming an insulating film, and a process for forming a new conductive layer on the surface of the insulating film - The method for producing the circuit wiring preferably includes the steps of forming an insulating film on the surface of the circuit wiring, and forming a new conductive layer on the surface of the insulating film. By the above steps, a second electrode pattern insulated from the first electrode pattern can be formed. The step of forming the insulating film is not particularly limited, and may be a known method for forming a permanent film. Alternatively, an insulating film having a desired pattern may be formed by photolithography using a photosensitive material having insulating properties. The step of forming a new conductive layer on the insulating film is not particularly limited, and for example, a new conductive layer having a desired pattern may be formed by photolithography using a photosensitive material having conductivity.
[0406] In the method for producing the circuit wiring, a substrate having a plurality of conductive layers on both surfaces of the substrate is used, and circuits are formed on the conductive layers formed on both surfaces of the substrate, either sequentially or simultaneously. With this configuration, a touch panel circuit wiring can be formed in which a first conductive pattern is formed on one surface of the substrate and a second conductive pattern is formed on the other surface of the substrate. It is also preferable to form the touch panel circuit wiring having such a configuration from both sides of the substrate by roll-to-roll.
[0407] <Circuit wiring applications> The circuit wiring manufactured by the manufacturing method of the circuit wiring can be applied to various devices. An example of a device having the circuit wiring manufactured by the manufacturing method is an input device, preferably a touch panel, more preferably a capacitive touch panel. The input device can also be applied to a display device such as an organic EL display device and a liquid crystal display device.
[0408] (Touch panel manufacturing method) The method for producing a touch panel according to the present disclosure is not particularly limited as long as it is a method using a photosensitive transfer material according to the present disclosure. A method for manufacturing a touch panel according to the present disclosure preferably includes, in this order, a step of contacting and laminating the outermost layer of the photosensitive transfer material according to the present disclosure, which is on the side having a photosensitive resin layer relative to the temporary support, with a substrate having a conductive layer, a step of exposing the photosensitive resin layer to a pattern, a step of developing the exposed photosensitive resin layer to form a resin pattern, and a step of etching the substrate in an area where the resin pattern is not arranged.
[0409] Specific aspects of each step in the method for manufacturing a touch panel, and the order in which each step is performed, are as described above in the sections "Method for manufacturing a resin pattern" and "Method for manufacturing a circuit wiring", and preferred aspects are also the same. The method for manufacturing the touch panel may refer to a known method for manufacturing a touch panel, except that the wiring for the touch panel is formed by the above-mentioned method. Furthermore, the method for manufacturing a touch panel may include any steps (other steps) other than those described above.
[0410] An example of a mask pattern used in manufacturing a touch panel is shown in FIG. 3 and FIG. In the pattern A shown in FIG. 3 and the pattern B shown in FIG. 4, GR is a non-image area (light-shielding area), EX is an image area (exposed area), and DL is an imaginary frame for alignment. In the method for manufacturing a touch panel, for example, by exposing the photosensitive resin layer through a mask having the pattern A shown in FIG. 3, a touch panel having circuit wiring having the pattern A corresponding to EX can be manufactured. Specifically, it can be manufactured by the method shown in FIG. 1 of International Publication No. 2016 / 190405. In one example of the manufactured touch panel, the center part (pattern part where the electrodes are connected) of the exposed part EX is a part where a transparent electrode (electrode for a touch panel) is formed, and the peripheral part (thin line part) of the exposed part EX is a part where wiring of the peripheral extraction part is formed.
[0411] The above-mentioned touch panel manufacturing method produces a touch panel having at least touch panel wiring. The touch panel preferably has a transparent substrate, an electrode, and an insulating layer or a protective layer. Examples of detection methods for touch panels include known methods such as a resistive film method, a capacitance method, an ultrasonic method, an electromagnetic induction method, and an optical method, etc. Among these, the capacitance method is preferable.
[0412] Examples of touch panel types include the so-called in-cell type (e.g., those shown in Figures 5, 6, 7, and 8 of JP-T 2012-517051), the so-called on-cell type (e.g., those shown in Figure 19 of JP-A 2013-168125 and those shown in Figures 1 and 5 of JP-A 2012-89102), the OGS (One Glass Solution) type, the TOL (Touch-on-Lens) type (e.g., those shown in Figure 2 of JP-A 2013-54727), various out-cell types (so-called GG, G1 / G2, GFF, GF2, GF1, G1F, etc.), and other configurations (e.g., those shown in Figure 6 of JP-A 2013-164871). An example of the touch panel is described in paragraph 0229 of JP2017-120435A. EXAMPLES
[0413] The following examples further illustrate the embodiments of the present invention. The materials, amounts, ratios, processing contents, and processing procedures shown in the following examples can be changed as appropriate without departing from the spirit of the embodiments of the present invention. Therefore, the scope of the embodiments of the present invention is not limited to the specific examples shown below. Unless otherwise specified, "parts" and "%" are based on mass.
[0414] Details of the abbreviations of the compounds used in the examples and comparative examples are shown below. <Alkali-soluble resin> A-1: styrene / methacrylic acid / methyl methacrylate=32 / 28 / 40 (mass%), Mw=40,000 A-2: styrene / methacrylic acid / methyl methacrylate=52 / 29 / 19 (mass%), Mw=60,000 A-3: benzyl methacrylate / methacrylic acid=81 / 19 (mass%), Mw=40,000 A-4: Propylene glycol monomethyl ether acetate solution of copolymer of benzyl methacrylate / methacrylic acid / acrylic acid = 75 / 10 / 15 (solid concentration 30.0%, Mw = 30,000, acid value 153 mg KOH / g) A-5: Kuraray Poval PVA-205 (Polyvinyl alcohol, manufactured by Kuraray Co., Ltd.) A-6: Polyvinylpyrrolidone K-30 (manufactured by Nippon Shokubai Co., Ltd.)
[0415] <Ethylenically unsaturated compounds> B-1: NK Ester BPE-500 (2,2-bis(4-(methacryloxypentaethoxy)phenyl)propane, manufactured by Shin-Nakamura Chemical Co., Ltd.) B-2: NK Ester BPE-200 (2,2-bis(4-(methacryloxydiethoxy)phenyl)propane, manufactured by Shin-Nakamura Chemical Co., Ltd.) B-3: Dimethacrylate of polyethylene glycol with an average of 15 moles of ethylene oxide and an average of 2 moles of propylene oxide added to both ends of bisphenol A B-4: Light Acrylate DPE-6A (dipentaerythritol hexaacrylate, manufactured by Kyoeisha Chemical Co., Ltd.) B-5: Aronix M-270 (polypropylene glycol diacrylate, manufactured by Toagosei Co., Ltd.) B-6: NK Ester A-TMPT (trimethylolpropane triacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) B-7: Sartomer SR-454 (ethoxylated (3) trimethylolpropane triacrylate, manufactured by Arkema) B-8: Sartomer SR-502 (ethoxylated (9) trimethylolpropane triacrylate, manufactured by Arkema) B-9: NK Ester A-9300-CL1 (ε-caprolactone modified tris-(2-acryloxyethyl) isocyanurate, manufactured by Shin-Nakamura Chemical Co., Ltd.) B-10: NK Ester A-DCP (tricyclodecane dimethanol diacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.) B-11: 8UX-015A (urethane acrylate, manufactured by Taisei Fine Chemical Co., Ltd.) B-12: Aronix TO-2349 (a polyfunctional ethylenically unsaturated compound having a carboxylic acid group, manufactured by Toagosei Co., Ltd.)
[0416] <Photopolymerization initiator> C-1: B-CIM (2-(2-chlorophenyl)-4,5-diphenylimidazole dimer, manufactured by Kurogane Kasei Co., Ltd.) C-2: SB-PI 701 (4,4'-bis(diethylamino)benzophenone, obtained from Sanyo Trading Co., Ltd.) C-3: Omnirad 907 (2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, manufactured by IGM Resins BV) C-4: Irgacure OXE02 (1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(O-acetyloxime), manufactured by BASF) C-5: 4,4'-bis(diethylamino)benzophenone (Kanto Chemical Co., Ltd.)
[0417] <Polymerization inhibitor> D-1: TDP-G (phenothiazine, manufactured by Kawaguchi Chemical Industry Co., Ltd.) D-2: Phenoxazine (Tokyo Chemical Industry Co., Ltd.) D-3: Irganox 245 (hindered phenol polymerization inhibitor, manufactured by BASF) D-4: N-nitrosophenylhydroxylamine aluminum salt (FUJIFILM Wako Pure Chemical Industries, Ltd.) D-5: MQ (4-methoxyphenol, manufactured by Kawaguchi Chemical Industry Co., Ltd.)
[0418] <Other additives> E-1: Leuco Crystal Violet (color developer, manufactured by Tokyo Chemical Industry Co., Ltd.) E-2: N-phenylcarbamoylmethyl-N-carboxymethylaniline (color developer, Fujifilm Wako Pure Chemical Industries, Ltd.) E-3: Brilliant Green (color developer, manufactured by Tokyo Chemical Industry Co., Ltd.) E-4: CBT-1 (rust inhibitor, carboxybenzotriazole, manufactured by Johoku Chemical Industry Co., Ltd.) E-5: A 1:1 (mass ratio) mixture of 1-(2-di-n-butylaminomethyl)-5-carboxylbenzotriazole and 1-(2-di-n-butylaminomethyl)-6-carboxylbenzotriazole, a rust inhibitor E-6: Phenidone (antioxidant, manufactured by Tokyo Chemical Industry Co., Ltd.) E-7: Megafac F-552 (fluorosurfactant, manufactured by DIC Corporation) E-8: Megafac F-444 (fluorosurfactant, manufactured by DIC Corporation)
[0419] <Solvent> F-1: Methyl ethyl ketone (manufactured by Sankyo Chemical Co., Ltd.) F-2: Propylene glycol monomethyl ether acetate (Showa Denko K.K.) F-3: Ion-exchanged water F-4: Methanol (manufactured by Mitsubishi Gas Chemical Co., Ltd.)
[0420] <Preparation of Thermoplastic Resin Composition> A thermoplastic resin composition was prepared by mixing the following components. ·A-4:42.85 copies ·B-10: 4.63 copies ·B-11: 2.31 parts ·B-12: 0.77 parts ·E-7: 0.03 copies ·F-1:39.50 copies ·F-2: 9.51 copies Compound with the structure shown below (photoacid generator, compound synthesized according to the method described in paragraph 0227 of JP2013-47765A): 0.32 parts
[0421] [ka]
[0422] Compound with the structure shown below (coloring agent that changes color when exposed to acid): 0.08 parts
[0423] [ka]
[0424] <Preparation of Intermediate Layer Composition> An intermediate layer composition was prepared by mixing the following components: ·A-5: 3.22 copies ·A-6: 1.49 copies ·E-8:0.0015 copies ·F-3:38.12 copies ·F-4:57.17 parts
[0425] <Preparation of Photosensitive Resin Composition> Photosensitive resin compositions used in the examples and comparative examples were prepared according to the compositions shown in Table 1 below.
[0426] (Examples 1 to 16 and Comparative Examples 1 to 3) <Preparation of photosensitive transfer material> A polyethylene terephthalate (PET) film having a thickness of 30 μm was prepared as a temporary support. The above-mentioned thermoplastic resin composition was applied to the surface of the temporary support using a slit nozzle so that the coating width was 1.0 m and the layer thickness after drying was 4.0 μm. The formed coating film of the thermoplastic resin composition was dried at 80° C. for 40 seconds to form a thermoplastic resin layer. The intermediate layer composition was applied to the surface of the formed thermoplastic resin layer using a slit nozzle so that the coating width was 1.0 m and the layer thickness after drying was 1.2 μm. The coating of the intermediate layer composition was dried at 80° C. for 40 seconds to form an intermediate layer. A photosensitive resin composition having the composition shown in Table 1 was applied onto the surface of the formed intermediate layer using a slit nozzle so that the coating width was 1.0 m and the layer thickness after drying was the layer thickness shown in Table 1. The coating of the photosensitive resin composition was dried at 80° C. for 40 seconds to form a photosensitive resin layer. A PET film (Lumirror 16QS62, manufactured by Toray Industries, Inc.) was pressure-bonded as a protective film to the surface of the formed photosensitive resin layer, to prepare photosensitive transfer materials of the examples and comparative examples.
[0427] <Evaluation of photosensitive transfer materials> -laminate- The protective film was peeled off from the obtained photosensitive transfer material, and the peeled photosensitive transfer material was laminated on a substrate (a 200 nm thick copper layer was prepared by sputtering on a 100 μm PET film) using a sheet laminator. The lamination conditions were a roll temperature of 100°C, a lamination speed of 2 m / min, and a lamination pressure of 0.5 MPa.
[0428] -Eb measurement and sensitivity evaluation- A 15-step step wedge (manufactured by Fujifilm Corporation) was placed on the temporary support of the laminated photosensitive transfer material, and 20 mW / cm 2 180mJ / cm 2 After the exposure, the support was peeled off and the film was developed for 30 seconds in a 0.9% by mass aqueous solution of sodium carbonate at 25° C., and Eb was calculated from the remaining film thickness at each step. From the viewpoint of suitability for general photolithography processes, there is a preferable range of Eb values. 2 When the intensity is more than 90 mJ / cm, the sensitivity is adequate, the device response is excellent, and Eb is 90 mJ / cm 2 When the exposure time is less than this, the exposure time can be shortened, resulting in excellent productivity. Sensitivity: Eb (mJ / cm 2 ) and evaluated according to the following criteria. As the photosensitive transfer material, A to C are preferable, and A or B is more preferable. A: 35≦Eb(mJ / cm 2 )≦70 B: 25≦Eb(mJ / cm 2 )<35 or 70 <Eb(mJ / cm 2 )≦90 C:90 <Eb(mJ / cm 2 ) D: Eb (mJ / cm 2 )<25
[0429] -Measurement of W3- The photosensitive transfer material laminated on the substrate was brought into contact with a photomask having a line and space of 10 μm / 10 μm on the temporary support, and Ep=2×Eb (mJ / cm 2 ) for 3 hours. After the exposure, the temporary support, thermoplastic resin layer, and intermediate layer were peeled off with tape, and 5 mL of bromine water (0.2%) was dispensed into a 50 mL container. The sample was fixed in the container so as not to come into contact with the dispensed liquid, and allowed to stand at room temperature (25°C) for 5 minutes. The sample was then stored under high vacuum for half a day to degas the residual bromine. This produced a sample with bromine-modified carbon-carbon double bonds. The sample was analyzed by secondary ion mass spectrometry (ION-TOF SIMS 5, primary ion source: Bi 3+ (30kV, measurement range: 50mm, surface resolution: 512×512pixel, integration: 32 times, measurement mode: high spatial resolution mode (Fast Imaging), charging correction: using electron gun) - The area of the area was evaluated. -The area with the smallest strength was determined as the width of the region where polymerization had progressed. The width of the region where polymerization had progressed was measured at three points, and the average value was determined as W3.
[0430] -W 24 Measurement of - The width of the polymerization progressed region W 24 hours after pattern exposure was measured in the same manner as W3, except that the time elapsed after exposure was changed. 24 Also, W 24 The value of / W3 was calculated.
[0431] -W 72 Measurement of - The width of the polymerization progressed region W 72 hours after pattern exposure was measured in the same manner as W3, except that the time elapsed after exposure was changed. 72 Also, W 72 The value of / W3 was calculated.
[0432] <Change in line width when left for 24 hours after exposure> The photosensitive transfer material laminated on the substrate was brought into contact with a photomask having a line and space of 10 μm / 10 μm on the temporary support, and Ep=2×Eb (mJ / cm 2 ) after 3 hours or 24 hours had elapsed since exposure, the temporary support was peeled off, and the unexposed areas were dissolved by showering with a 1% aqueous sodium carbonate solution at 25°C to obtain a resist pattern. The line width of the area where the photosensitive resin layer and the substrate contacted was measured from a scanning electron microscope (SEM) image of the cross section of the obtained resist pattern. The line width developed 3 hours after exposure was designated Wr3, and the line width developed 24 hours after exposure was designated Wr 24 Then, Wr 24 The closer this ratio is to 1, the smaller the line width change when the film is left in the exposure state, and the better the performance. 24 / Wr3 was evaluated according to the following criteria: As the photosensitive transfer material, A or B is preferable. A:Wr 24 / Wr3<1.03 B: 1.03≦Wr 24 / Wr3<1.05 C: 1.05≦Wr 24 / Wr3<1.1 D: 1.1≦Wr 24 / Wr3
[0433] <Changes in line width when development temperature changes> The photosensitive transfer material laminated on the substrate was brought into contact with a photomask having a line and space of 10 μm / 10 μm on the temporary support, and Ep=2×Eb (mJ / cm 2 After 3 hours had passed since the exposure, the temporary support was peeled off and the unexposed area was dissolved by showering with a 1% aqueous sodium carbonate solution at 30°C to obtain a resist pattern. 3b Measure Wr 3b The closer this ratio is to 1, the smaller the line width change when the development temperature fluctuates, and the wider the process robustness, which is preferable. 3b / Wr3 was evaluated according to the following criteria: As the photosensitive transfer material, A or B is preferable. A:Wr 3b / Wr3<1.03 B: 1.03≦Wr 3b / Wr3<1.05 C: 1.05≦Wr 3b / Wr3
[0434] The measurement results and evaluation results are shown in Table 2.
[0435] [Table 1]
[0436] [Table 2]
[0437] As shown in Tables 1 and 2 above, the photosensitive transfer materials of Examples 1 to 16 have smaller changes in line width of the resin pattern with the lapse of time after exposure compared to the photosensitive transfer materials of Comparative Examples 1 to 3. Furthermore, the photosensitive transfer materials of Examples 1 to 16 exhibited little change in line width of the resin pattern due to changes in development temperature, and also had excellent sensitivity.
[0438] (Example 101 (2nd time: PET peeling exposure)) A 150 nm thick ITO film was formed as the second conductive layer on a 100 micron thick PET substrate by sputtering, and a 200 nm thick copper film was formed on top of that as the first conductive layer by vacuum deposition to create a circuit board. The photosensitive transfer material obtained in Example 1 was laminated on the copper layer (laminar roll temperature 120°C, linear pressure 0.8MPa, linear speed 1.0m / min.). The laminated laminate was exposed to contact patterns using a photomask with pattern A shown in FIG. 3, which has a configuration in which conductive layer pads are connected in one direction, without peeling off the temporary support. The temporary support was then peeled off, and development and washing with water were performed to obtain pattern A. Next, the copper layer was etched using a copper etching solution (Cu-02, manufactured by Kanto Chemical Co., Ltd.), and the ITO layer was etched using an ITO etching solution (ITO-02, manufactured by Kanto Chemical Co., Ltd.), thereby obtaining a substrate on which both copper and ITO were drawn with pattern A. The remaining photosensitive resin layer (Pattern A) was peeled off using a stripping solution (KP-301, manufactured by Kanto Chemical Co., Ltd.), and the photosensitive transfer material obtained in Example 1 was laminated again onto the copper layer (laminar roll temperature 120°C, linear pressure 0.8 MPa, linear speed 1.0 m / min.). Next, in the aligned state, the substrate was exposed to a pattern using a photomask of pattern B shown in Fig. 4, developed, and washed with water. Thereafter, the copper layer was etched using Cu-02, and the remaining photosensitive resin layer (pattern B) was peeled off using a stripping solution (KP-301, manufactured by Kanto Chemical Co., Ltd.) to obtain a circuit wiring board. When the obtained circuit wiring board was observed under a microscope, there was no peeling or chipping and the pattern was beautiful. In the pattern A shown in FIG. 3, the gray portion GR is a light-shielding portion, EX is an exposed portion, and the dotted portion DL is a virtual frame for alignment. In addition, in the pattern B shown in FIG. 4, similarly to FIG. 3, the gray portion GR is a light-shielded portion, EX is an exposed portion, and the dotted portion DL is a virtual representation of an alignment frame.
[0439] The disclosure of Japanese Patent Application No. 2020-156353, filed on September 17, 2020, is incorporated herein by reference in its entirety. All publications, patent applications, and technical standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or technical standard was specifically and individually indicated to be incorporated by reference. [Explanation of symbols]
[0440] 1, 11: temporary support, 2, 12: transfer layer, 3, 17: photosensitive resin layer, 5: refractive index adjustment layer, 13: thermoplastic resin layer, 15: intermediate layer, 10, 20: photosensitive transfer material, GR: light-shielding portion (non-image portion), EX: exposed portion (image portion), DL: alignment frame
Claims
1. A temporary support; a photosensitive resin layer including an alkali-soluble resin, an ethylenically unsaturated compound, a polymerization inhibitor, and a photopolymerization initiator; a mass ratio Rd / Rc of 0.02 or more and 0.1 or less, wherein Rc is a content of the photopolymerization initiator in the photosensitive resin layer and Rd is a content of the polymerization inhibitor in the photosensitive resin layer; The photosensitive resin layer is subjected to a dipping process at a temperature of mJ / cm 2 The width W of the double bond reaction region after 3 hours from exposure of a 10 μm / 10 μm line and space pattern with an exposure dose Ep in units of 3 and the width W of the double bond reaction region after 24 hours 24 But, W 24 / W 3 Meets ≦1.05 Photosensitive transfer material. W 3 and W 24 is the double bond reaction region width obtained by secondary ion mass spectrometry after dyeing the exposed photosensitive transfer material with bromine, The Ep satisfies Ep = 2 × Eb, The Eb is measured after the photosensitive resin layer is attached to a substrate, and the illuminance is 20 mW / cm through a 15-step step wedge. 2 The exposure dose was 180 mJ / cm 2 The exposure amount is defined as the number of steps that gives a remaining layer thickness that is within ±1% of the layer thickness of the photosensitive resin layer after exposure and development.
2. The photosensitive resin layer is exposed to a line and space pattern of 10 μm / 10 μm at the exposure dose Ep, and then the double bond reaction region width W after 3 hours has elapsed 3 and the double bond reaction region width W after 72 hours 72 But, W 72 / W 3 The photosensitive transfer material according to claim 1, which satisfies ≦1.
10. W 72 is the double bond reaction region width obtained by secondary ion mass spectrometry after bromine dyeing of the exposed photosensitive transfer material.
3. 3. The photosensitive transfer material according to claim 1, wherein the ethylenically unsaturated compound includes an ethylenically unsaturated compound having a bisphenol structure.
4. 4. The photosensitive transfer material according to claim 1, wherein the photopolymerization initiator comprises a biimidazole compound and a benzophenone compound.
5. 5. The photosensitive transfer material according to claim 1, wherein the polymerization inhibitor comprises at least one compound selected from the group consisting of phenothiazine, phenoxazine, and compounds having a hindered phenol structure.
6. 6. The photosensitive transfer material according to claim 1, wherein the value of the mass ratio Rd / Rc is 0.03 or more and 0.05 or less.
7. a step of contacting an outermost layer of the photosensitive transfer material according to any one of claims 1 to 6, the outermost layer being on a side having a photosensitive resin layer with respect to the temporary support, with a substrate and laminating the same; A step of pattern-exposing the photosensitive resin layer; developing the exposed photosensitive resin layer to form a resin pattern. A method for producing a resin pattern.
8. 8. The method for producing a resin pattern according to claim 7, wherein at least a part of the resin pattern includes a line and space pattern, and the total width of at least one pair of a line and a space in the line and space pattern is 20 [mu]m or less.
9. a step of contacting an outermost layer of the photosensitive transfer material according to any one of claims 1 to 6, the outermost layer being on a side having a photosensitive resin layer with respect to the temporary support, with a substrate having a conductive layer, and laminating the substrate; A step of pattern-exposing the photosensitive resin layer; developing the exposed photosensitive resin layer to form a resin pattern; and etching the substrate in a region where the resin pattern is not disposed. A method for manufacturing circuit wiring.
10. a step of contacting an outermost layer of the photosensitive transfer material according to any one of claims 1 to 6, the outermost layer being on a side having a photosensitive resin layer with respect to the temporary support, with a substrate having a conductive layer, and laminating the substrate; A step of pattern-exposing the photosensitive resin layer; developing the exposed photosensitive resin layer to form a resin pattern; and etching the substrate in a region where the resin pattern is not disposed. A method for manufacturing a touch panel.
Citation Information
Patent Citations
Photosensitive resin composition
JP2001356493A
Photosensitive polyimide composition
JP2018517169A
Photosensitive colored composition for color filter, and color filter
JP2019105713A
Composition for lithography, pattern formation method and compound
WO2019066000A1
Photosensitive transfer material, method for producing resist pattern, method for producing circuit wiring line, touch panel, and touch panel display device
WO2019187364A1