Method for manufacturing a semiconductor device
A peeling method using hydrogen-containing layers and laser separation addresses the challenges of manufacturing flexible and reliable semiconductor and display devices at low cost and high yield, suitable for large substrates and low temperatures.
Patent Information
- Application Number
- JP2023103991
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-11-30
- Filing Date
- 2023-06-26
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2037-08-28
AI Technical Summary
Existing methods for manufacturing semiconductor and display devices face challenges in achieving low-cost, high-yield, and high-productivity processes, particularly for large-sized substrates, while also requiring low temperatures and ensuring flexibility, thinness, and resistance to damage.
A peeling method involving the formation of a first material layer containing hydrogen, oxygen, and water, and a second resin layer, followed by separation using light irradiation, specifically laser light, to break hydrogen bonds and separate the layers at the interface, with controlled conditions for wavelength, energy density, and absorption rates.
The method enables low-cost, high-yield manufacturing of semiconductor and display devices on large-sized substrates at low temperatures, with reduced power consumption, enhanced reliability, flexibility, and resistance to damage, while maintaining display quality.
Smart Images

Figure 0007596453000006 
Figure 0007596453000007 
Figure 0007596453000008
Abstract
Description
[Technical field]
[0001] One embodiment of the present invention relates to a peeling method, a manufacturing method of a semiconductor device, and a manufacturing method of a display device. .
[0002] Note that one embodiment of the present invention is not limited to the above technical field. Examples of the semiconductor device include a semiconductor device, a display device, a light-emitting device, a power storage device, a memory device, an electronic device, a lighting device, Input devices (e.g., touch sensors, etc.), input / output devices (e.g., touch panels, etc.), These driving methods and manufacturing methods can be cited as examples.
[0003] In this specification and the like, a semiconductor device is a device that can function by utilizing semiconductor characteristics. Transistors, semiconductor circuits, display devices, light-emitting devices, input devices, input / output devices The semiconductor device may be an imaging device, an electro-optical device, or the like. Power generation devices (including thin-film solar cells, organic thin-film solar cells, etc.) and electronic devices have semiconductor devices. This may be the case. [Background technology]
[0004] Organic EL (Electro Luminescence) elements and liquid crystal elements are used. In addition, light emitting diodes (LEDs) are also known. A light-emitting device that uses a light-emitting element such as a light-emitting diode, and displays images using an electrophoretic method, etc. Electronic paper and the like are also examples of display devices.
[0005] The basic structure of an organic EL element is a layer containing a light-emitting organic compound sandwiched between a pair of electrodes. By applying a voltage to this element, light is emitted from the light-emitting organic compound. A display device using such an organic EL element is thin, lightweight, and has high controllability. It is possible to realize a display device that is both durable and consumes low power.
[0006] In addition, semiconductor elements such as transistors and organic electroluminescence (EL) elements are mounted on a flexible substrate (film). By forming display elements such as L elements, a flexible display device can be realized.
[0007] In Patent Document 1, a support substrate (glass) on which a heat-resistant resin layer and an electronic element are provided via a sacrificial layer is The heat-resistant resin layer is peeled off from the glass substrate by irradiating the glass substrate with laser light. A method for making a flexible display is disclosed. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2015-223823 A Summary of the Invention [Problem to be solved by the invention]
[0009] One embodiment of the present invention is a novel peeling method, a method for manufacturing a semiconductor device, or a method for manufacturing a display device. One aspect of the present invention is to provide a peeling method that is low cost and has high mass productivity. It is an object of the present invention to provide a method for manufacturing a semiconductor device, or a method for manufacturing a display device. An object of one embodiment of the present invention is to provide a peeling method with high yield. One object of one embodiment of the present invention is to manufacture a semiconductor device or a display device using a large-sized substrate. An object of one embodiment of the present invention is to manufacture a semiconductor device or a display device at low temperature. It shall be one.
[0010] An object of one embodiment of the present invention is to provide a display device with low power consumption. An object of one embodiment of the present invention is to provide a highly reliable display device. One object of the present invention is to reduce the thickness or weight of a display device. It is an object of the present invention to provide a display device having a curved surface. An object of the present invention is to provide a display device that is not easily damaged. It is an object of the present invention to provide a display device, an input / output device, an electronic device, or the like.
[0011] Note that the description of these problems does not preclude the existence of other problems. However, it is not necessary to solve all of these problems. It is possible to extract other issues from the description in the section. [Means for solving the problem]
[0012] One aspect of the present invention includes forming a first material layer on a substrate, depositing a second material layer on the first material layer, and forming a layer and separating the first and second material layers. A method for fabricating a biocompatible device. A first layer of material is formed by mixing one or more of hydrogen, oxygen, and water. The second material layer includes a resin. The first material layer and the second material layer are bonded to each other by hydrogen bonds. The hydrogen bonds are broken by irradiation with light. In addition, the hydrogen bonds between the first material layer and the second material layer are broken, and the first material layer is Preferably, the separation occurs at or near the interface between the layer of material and the layer of the second material.
[0013] Alternatively, one aspect of the present invention includes a method for forming a first material layer on a substrate, forming a second material layer on the first material layer, and forming a second material layer and separating the first material layer and the second material layer using light. The first material layer is a layer containing hydrogen, oxygen, and water. The first material layer and the second material layer include one or more of the following: The layers are separated by breaking the hydrogen bonds. Laser light is used as the light. In this case, the cutting is performed by irradiating the laser beam to the interface between the first material layer and the second material layer or in the vicinity thereof. This is done by
[0014] Alternatively, one aspect of the present invention includes a method for forming a first material layer on a substrate, forming a second material layer on the first material layer, and forming a second material layer; heating the first material layer and the second material layer in a laminated state; and separating the first material layer from the second material layer. The first material layer includes one or more of hydrogen, oxygen, and water. The second material layer includes a resin. In the heating process, the interface between the first material layer and the second material layer is heated. In the separation step, water is precipitated at the interface or in the vicinity of the interface. When the water is irradiated with light, the first material layer and the second material layer are separated.
[0015] The second material layer has an average transmittance of 70 for light having a wavelength in the range of 450 nm to 700 nm. The second material layer is preferably formed so that the wavelength is 400 nm or more and 7 It is preferable that the average transmittance of light in the range of 00 nm or less is 70% or more. It is preferable that the second material layer is formed so that the thickness is 80% or more. Preferably, the second material layer comprises acrylic. Alternatively, the second material layer may comprise polyimide. is preferred.
[0016] The light irradiated in the separation process has a wavelength range of 180 nm to 450 nm. It is preferable that the light has a wavelength range of 308 nm or thereabouts. It is preferable that the substrate, the first material layer, and the second material layer are laminated in such a manner that the first material layer is irradiated with the first light. The absorption rate of the light irradiated during the separation process (e.g., light with a wavelength of 308 nm) is 80% or more. It is preferably 0% or less, and more preferably 85% or more and 100% or less.
[0017] The light is preferably irradiated using a laser device. The light is preferably irradiated using a linear laser device. It is preferable that the target object is shot.
[0018] The light is 300mJ / cm 2 More than 360mJ / cm 2 The following energy density is applied: is preferred.
[0019] The first material layer is preferably formed so as to have a lower adhesion to the second material layer than to the substrate. It is.
[0020] The first material layer may be titanium, molybdenum, aluminum, tungsten, silicon, indium, etc. The semiconductor device is formed having one or more of the following: aluminum, zinc, gallium, tantalum, and tin. It is preferable that the first material layer contains one or both of titanium and titanium oxide. The first material layer is preferably formed so as to have a laminated structure of titanium and titanium oxide. It is preferable that the insulating layer is formed so as to have the following structure:
[0021] The second material layer is formed to have a region having a thickness of 0.1 μm or more and 5 μm or less. is preferred.
[0022] The second layer of material is formed having a residue of a compound represented by formula (100). is preferred.
[0023] [ka]
[0024] In the step of forming the first material layer, a metal layer is formed on a substrate, and a surface of the metal layer is subjected to plasma treatment. In the plasma treatment, oxygen or water vapor is used to form a metal oxide layer. It is preferable to expose the surface of the metal layer to an atmosphere containing one or both of (H2O).
[0025] The step of separating the first material layer and the second material layer is carried out while supplying a liquid to the separation interface. Preferably, the liquid comprises water.
[0026] In one embodiment of the present invention, a metal oxide layer is formed on a substrate, and a 0.1 μm thick film is formed on the metal oxide layer. A resin layer is formed on the resin layer so as to have an area of 5 μm or more and 5 μm or less. A transistor having a metal oxide is formed on the resin by irradiating the metal oxide layer with light. The method for manufacturing a semiconductor device further comprises the steps of:
[0027] A metal layer is formed on a substrate, and a plasma treatment is performed on the surface of the metal layer to form a metal oxide layer. In the plasma treatment, oxygen or water vapor (H2O) is used. It is preferable to expose the surface of the metal layer to an atmosphere containing either or both of them.
[0028] The resin layer has an average light transmittance of 70% or more for wavelengths between 450 nm and 700 nm. It is preferred that the ion exchange resin is formed so that
[0029] Using a linear laser, light is applied from the substrate side to the interface between the metal oxide layer and the resin layer or to the vicinity thereof. Irradiation is preferred. Effect of the Invention
[0030] According to one embodiment of the present invention, a novel peeling method, a method for manufacturing a semiconductor device, or a method for manufacturing a display device According to one aspect of the present invention, a peeling method that is low-cost and highly productive can be provided. In addition, a method for manufacturing a semiconductor device or a method for manufacturing a display device can be provided. According to one aspect of the present invention, a peeling method with high yield can be provided. In this case, a semiconductor device or a display device can be manufactured using a large-sized substrate. As a result, a semiconductor device or a display device can be manufactured at a low temperature.
[0031] According to one embodiment of the present invention, a display device with low power consumption can be provided. In this manner, a highly reliable display device can be provided. According to one aspect of the present invention, the device can be made thin and lightweight. According to one aspect of the present invention, a display device having a curved surface can be provided. According to one embodiment of the present invention, a novel display device and an input / output device can be provided. , or electronic devices, etc. can be provided.
[0032] The description of these effects does not preclude the existence of other effects. However, it is not necessary to have all of these effects. However, it is possible to extract effects other than these. [Brief description of the drawings]
[0033] [Figure 1] FIG. [Diagram 2] FIG. [Diagram 3] FIG. [Figure 4] FIG. 2 is a schematic diagram showing an example of an interface between a metal oxide layer and a resin layer. [Diagram 5] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 6] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 7] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 8] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 9] 1A and 1B are a cross-sectional view and a top view illustrating an example of a manufacturing method of a display device. [Figure 10] 1A and 1B are a cross-sectional view and a top view illustrating an example of a manufacturing method of a display device. [Figure 11] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 12] 1A and 1B are a top view and a cross-sectional view illustrating an example of a display device. [Figure 13] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 14] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 15] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 16] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 17] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 18] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 19] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 20] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 21] 1A and 1B are a top view and a cross-sectional view illustrating an example of a display device. [Figure 22] FIG. 2 is a diagram showing an example of an apparatus for producing a laminate. [Figure 23] FIG. 2 is a diagram showing an example of a laser irradiation unit. [Figure 24] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Diagram 25] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 26] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 27] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 28] 1A and 1B are a top view and a cross-sectional view illustrating an example of a display device. [Figure 29] FIG. 1 is a perspective view showing an example of a display device. [Diagram 30] FIG. 1 is a cross-sectional view showing an example of a display device. [Diagram 31] FIG. 1 is a flow diagram showing an example of a method for manufacturing a display device. [Diagram 32] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Diagram 33] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Diagram 34] FIG. 1 is a cross-sectional view showing an example of an input / output device. [Diagram 35] FIG. 1 is a flow diagram showing an example of a method for manufacturing a display device. [Diagram 36] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 37] 1A to 1C are cross-sectional views illustrating an example of a method for manufacturing a display device. [Figure 38] FIG. 1 is a cross-sectional view showing an example of an input / output device. [Figure 39] FIG. 2 is a diagram showing an example of a display module. [Diagram 40] 1A and 1B are diagrams illustrating examples of electronic devices. [Diagram 41] 1A and 1B are diagrams illustrating examples of electronic devices. [Diagram 42] FIG. 1 shows the peeling results of Example 1. [Diagram 43] 1 is a cross-sectional STEM photograph of a sample of Example 1. [Diagram 44] FIG. 4 is a diagram showing an example of laser processing conditions. [Diagram 45] FIG. 13 shows the peeling results of Example 2. [Diagram 46] 5A to 5C are diagrams showing a method for preparing and peeling off a sample in Example 2. [Figure 47] 4 is a microscopic photograph showing the shape of the light-shielding layer formed in Example 2. [Figure 48] 13 is a microscope photograph of the peeled surface on the glass substrate side in Example 2. [Figure 49] 13 is a microscope photograph of the peeled surface on the glass substrate side in Example 2. [Figure 50] 1 is a microscope photograph of the peeled surface on the film substrate side in Example 2. [Figure 51] FIG. 13 shows the peeling results of Example 2. [Figure 52] FIG. 13 is a graph showing the light transmittance in Example 4. [Diagram 53] Photographs showing the peeling results of Example 4. [Figure 54] Photograph of a cross section of the sample of Example 4 after peeling. [Figure 55] FIG. 13 is a graph showing the Id-Vg characteristics of a transistor according to Example 5. [Figure 56] 11 is a display photograph of the flexible OLED display of Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] The embodiment will be described in detail with reference to the drawings. However, the present invention is not limited to the following description. The present invention is not limited to the above embodiment, and various changes and modifications may be made in the form and details without departing from the spirit and scope of the present invention. It will be easily understood by those skilled in the art that the above-mentioned invention can be obtained by the following embodiments. It should not be construed as being limited to the contents described.
[0035] In the configuration of the invention described below, the same parts or parts having similar functions are referred to as the same parts. The same reference numerals are used in common among different drawings, and the repeated explanations are omitted. When referring to a function, the same hatch pattern may be used and no particular reference number may be given.
[0036] In addition, the position, size, range, etc. of each component shown in the drawings are not necessarily the same as in the actual embodiment, in order to facilitate understanding. Therefore, the disclosed invention may not necessarily represent the position, size, range, etc. Furthermore, the present invention is not limited to the position, size, range, etc. disclosed in the drawings.
[0037] The words "film" and "layer" may be interchangeable depending on the circumstances. For example, the term "conductive layer" can be replaced with "conductive film" Alternatively, for example, the term "insulating film" can be changed to " The term "insulating layer" may be changed to "insulating layer."
[0038] In this specification, the term "metal oxide" refers to a metal oxide in a broad sense. Metal oxides are oxide insulators and oxide conductors (including transparent oxide conductors). , oxide semiconductor (also called OS) For example, when a metal oxide is used for the semiconductor layer of a transistor, the metal An oxide may be called an oxide semiconductor. In other words, the transistor can be a transistor including a metal oxide or an oxide semiconductor.
[0039] In the present specification and the like, metal oxides having nitrogen are also referred to as metal oxides. Nitrogen-containing metal oxides are also called metal oxynitrides (met de). It may also be called tetrahydrofuran (tetrahydrofuran) oxynitride.
[0040] (Embodiment 1) In this embodiment, a peeling method and a manufacturing method of a display device according to one embodiment of the present invention will be described with reference to FIGS. This will be explained using 23.
[0041] In this embodiment, a display device having a transistor and an organic EL element (active matrix The display device has a substrate that is made of a flexible substrate. By using a flexible material, a flexible device can be obtained. One aspect of the invention is a light-emitting device, a display device, and an input / output device (touch panel) using an organic EL element. The present invention is not limited to semiconductor devices, light-emitting devices, display devices, and input / output devices using other functional elements. The present invention can be applied to various devices such as an output device.
[0042] In this embodiment, first, a first material layer, here a metal oxide layer, is formed on a substrate. Then, a second material layer, a resin layer in this example, is formed on the metal oxide layer. This separates the metal oxide layer from the resin layer.
[0043] In this embodiment mode, a base layer (also called a base layer) is formed between the substrate and the resin layer. The undercoat layer is a layer that has lower adhesion (bonding) to the resin layer than the substrate. The following description will be given taking as an example a case where a metal oxide layer is used as the underlayer, but the present invention is not limited thereto. .
[0044] It is preferable to use light when separating the metal oxide layer from the resin layer. It is preferable that the light is irradiated to the interface with the resin layer or in the vicinity thereof (also referred to as the interface or the vicinity of the interface). The light may be irradiated into the metal oxide layer. The light may be irradiated into the resin layer. In this specification, etc., "the interface between A and B or its vicinity" and "the interface between A and B" may be used. "at or near the interface between A and B" includes at least the interface between A and B, and , which includes a range within 20% of the thickness of either A or B.
[0045] By irradiating light, the interface between the metal oxide layer and the resin layer (and also the metal oxide layer and the resin By heating the metal oxide layer (in the resin layer), the adhesion (bonding) between the metal oxide layer and the resin layer can be reduced. Furthermore, the metal oxide layer and the resin layer can be separated.
[0046] An example of the principle of separating a metal oxide layer from a resin layer will be described with reference to FIGS.
[0047] First, referring to FIG. 1 and FIG. 2, H2O inhibits adhesion between the metal oxide layer 20 and the resin layer 23. The inhibitory effect will be explained below.
[0048] In FIG. 1, a metal oxide layer 20 is provided on a fabrication substrate 14, and a resin is formed on the metal oxide layer 20. A fat layer 23 is provided.
[0049] The interface between the metal oxide layer 20 and the resin layer 23, and one or both of the metal oxide layers 20 The elements are H2O, hydrogen (H), oxygen (O), hydroxyl (OH), and hydrogen radicals (H * ),acid Elementary radical (O * ), hydroxyl radical (OH * ) may be present. These include a process for forming the metal oxide layer 20, a doping process after forming the metal oxide layer 20, and In step (i) of FIG. 1, a metal oxide layer 20 and a resin layer 21 are formed. The interface with the oil layer 23 and the metal oxide layer 20 contain HO, H, O, etc. Here is an example.
[0050] The interface between the metal oxide layer 20 and the resin layer 23 and the H, O The H2O and the like solidify (harden) the resin layer 23 (e.g., polyimide, acrylic, etc.). In the process of annealing (for example, heating at 350°C), H2O may precipitate at the interface. In this case, H2O precipitated at the interface between the metal oxide layer 20 and the resin layer 23 is There is a possibility that the adhesion between the metal oxide layer 20 and the resin layer 23 is impaired. The H2O precipitated at the interface between the resin layer 23 and the metal layer 24 has an inhibitory effect on adhesion. In step (ii) of FIG. 1, H2O in the metal oxide layer 20 is mixed with the metal oxide layer 20 and the resin. In step (ii) of FIG. 1, the metal oxide layer 23 is deposited at the interface with the metal oxide layer 23. Hydrogen and hydroxyl groups (OH) in the metal oxide layer 20 are converted into H2O at the interface between the metal oxide layer 20 and the resin layer 23. Here is an example of precipitation.
[0051] Next, the laminate having the prepared substrate 14, the metal oxide layer 20, and the resin layer 23 is irradiated with light. In step (iii) of FIG. 2, the laminate is placed with the preparation substrate 14 facing upward. In step (iii) of FIG. 2, a conveying mechanism (not shown) is used to convey the By moving the laminate in the direction of the arrow, light is emitted from the right side to the left side of the figure. The interface between the metal oxide layer 20 and the resin layer 23 or its vicinity is irradiated through the substrate 14. Here, an example using a linear laser beam is shown. In iv), a linear beam 26 is irradiated onto a processing region 27 through a substrate 14. By the light irradiation, the interface between the metal oxide layer 20 and the resin layer 23 (and further the metal oxide layer 2 The metal oxide layer 20 and the resin layer 23 are heated. The H2O present at the interface with the 23 is instantly vaporized (evaporated) by high energy and abraded. To explode (also called to explode).
[0052] Step (v) in FIG. 2 shows an example of inverting the stack. Step (vi) in FIG. In the example shown in FIG. 1, the metal oxide layer 20 and the resin layer 23 are separated. O turns into water vapor and expands in volume. This causes the metal oxide layer 20 and the resin layer 23 to adhere to each other. The adhesion is weakened, and the metal oxide layer 20 and the resin layer 23 can be separated.
[0053] Next, the bond between the metal oxide layer 20 and the resin layer 23 will be described with reference to FIG.
[0054] In FIG. 3, a metal oxide layer 20 and a resin layer 23 are laminated.
[0055] It is believed that bonding occurs between the metal oxide layer 20 and the resin layer 23. Specifically, Chemical bonds such as covalent bonds, ionic bonds, and hydrogen bonds are formed between the metal oxide layer 20 and the resin layer 23. This is occurring.
[0056] In step (i) of FIG. 3, the metal M contained in the metal oxide layer 20 and the carbon contained in the resin layer 23 are Here is an example where element C is bonded by oxygen O.
[0057] The laminated structure of the metal oxide layer 20 and the resin layer 23 is irradiated with light (see laser light 55 in FIG. 3). Here, an example using a linear laser beam is shown. By moving the substrate and the light source relatively, The laser light 55 is scanned and irradiated over the area to be separated.
[0058] By the light irradiation, the interface between the metal oxide layer 20 and the resin layer 23 (and further, the metal oxide layer 20 and The resin layer 23 is heated, and the reaction of formula (1) (see below and FIG. 3) occurs. By doing so, H2O (water vapor) breaks the metal M-oxygen O-carbon C bond. And, The bond between the metal oxide layer 20 and the resin layer 23 is a hydrogen bond.
[0059] MO-C+H2O→M-OH+C-OH (1)
[0060] In step (ii) of FIG. 3, the metal M and oxygen O contained in the metal oxide layer 20 are bonded to form a resin. This shows an example in which the carbon C in the layer 23 is bonded to another oxygen O. The two oxygens are respectively: It forms a covalent bond with another hydrogen. Also, the two oxygens are bonded to each other. It forms hydrogen bonds with the hydrogen at the
[0061] Hydrogen bonds are much weaker than covalent bonds and can be broken easily. In addition, the energy of light irradiation causes water to evaporate and become water vapor. The force of expansion at this time is Therefore, the hydrogen bonds between the metal oxide layer 20 and the resin layer 23 may be broken. Therefore, the metal oxide layer 20 and the resin layer 23 can be easily separated.
[0062] In step (iii) of Figure 3, the oxygen and hydrogen bonded together are separated, forming a metal oxide. In this example, the metal oxide layer 20 and the resin layer 23 are separated. An oxygen atom O is bonded to the carbon atom C of the resin layer 23, and another oxygen atom O is bonded to the carbon atom C of the resin layer 23. The two oxygen atoms are , each of which forms a covalent bond with another hydrogen.
[0063] As described above, by irradiating the laminated structure of the metal oxide layer 20 and the resin layer 23 with light, H However, the strong bond between the metal oxide layer 20 and the resin layer 23 is changed to a weak hydrogen bond. This reduces the force required to separate the metal oxide layer 20 and the resin layer 23. In addition, the energy of the light irradiation causes the H2O to expand, and the metal oxide layer 2 0 and the resin layer 23 can be separated.
[0064] Next, the above-mentioned inhibitory action and H2O involved in the reaction shown in the above formula (1) will be described.
[0065] H2O is contained in the metal oxide layer 20, the resin layer 23, and between the metal oxide layer 20 and the resin layer 23. It may be present at the interface.
[0066] In addition, in the metal oxide layer 20, in the resin layer 23, and at the interface between the metal oxide layer 20 and the resin layer 23 Hydrogen (H), oxygen (O), hydroxyl group (OH), hydrogen radical (H * ), Oxygen radical (O * ), hydroxyl radical (OH * ) etc., when heated, become H2O. There is a match.
[0067] The inside of the metal oxide layer 20, the surface of the metal oxide layer 20 (the surface in contact with the resin layer 23), or the At the interface between the metal oxide layer 20 and the resin layer 23, H2O, hydrogen (H), oxygen (O), and hydroxyl groups (OH ), hydrogen radical (H * ), oxygen radical (O * ), hydroxyl radical (OH * )brain It is preferable to add one or more of these.
[0068] In the peeling method of the present embodiment, the above-mentioned inhibiting action and the reaction of formula (1) shown above are In this case, the adhesion between the metal oxide layer 20 and the resin layer 23 may be further improved. In other words, the peelability between the metal oxide layer 20 and the resin layer 23 can be further increased. It is estimated that this is possible.
[0069] In the metal oxide layer 20, in the resin layer 23, and at the interface between the metal oxide layer 20 and the resin layer 23, etc. , HO, hydrogen (H), oxygen (O), hydroxyl group (OH), hydrogen radical (H * ), oxygen radio Cal (O * ), hydroxyl radical (OH * It is preferable that the aryl group has a large amount of aryl groups such as aryl, ... By adding more H2O, the reaction can be promoted and the force required for separation can be reduced. can.
[0070] For example, when forming the metal oxide layer 20, 0On the surface, H2O, hydrogen, oxygen, hydroxyl groups, hydrogen radicals (H * ), oxygen radical (O * ) , hydroxyl radical (OH * It is preferable to include a large amount of
[0071] Specifically, a metal layer is formed, and the surface of the metal layer is subjected to radical treatment to form a metal oxide layer 2. In the radical treatment, oxygen radicals and hydroxyl radicals are preferably formed. It is preferable to expose the surface of the metal layer to an atmosphere containing at least one of the following: Plasma processing is performed in an atmosphere containing either hydrogen or water vapor (H2O) or both. is preferred.
[0072] Alternatively, a metal oxide layer 20 is formed, and the surface of the metal oxide layer 20 is subjected to radical treatment. In the radical treatment, oxygen radicals, hydrogen radicals, and hydroxyl radicals are preferably used. It is preferable to expose the surface of the metal oxide layer 20 to an atmosphere containing at least one of the above. For example, the plasma is heated in an atmosphere containing one or more of oxygen, hydrogen, or water vapor (H2O). It is preferable to carry out Zuma processing.
[0073] The radical treatment can be carried out using a plasma generator or an ozone generator.
[0074] For example, oxygen plasma treatment, hydrogen plasma treatment, water plasma treatment, ozone treatment, etc. The oxygen plasma treatment can be carried out by generating plasma in an atmosphere containing oxygen. The hydrogen plasma treatment can be performed by generating plasma in an atmosphere containing hydrogen. Water plasma treatment is performed by generating plasma in an atmosphere containing water vapor (H2O). In particular, by performing the water plasma treatment, moisture can be removed from the surface or inside of the metal oxide layer 20. It is preferable that a large amount of
[0075] Contains two or more of oxygen, hydrogen, water (water vapor), and inert gas (typically argon). The plasma treatment may be performed in an atmosphere containing oxygen. and hydrogen, and plasma treatment in an atmosphere containing oxygen and water. , plasma treatment in an atmosphere containing water and argon, and plasma treatment in an atmosphere containing oxygen and argon or plasma treatment in an atmosphere containing oxygen, water, and argon. By using argon gas as one of the gases for plasma processing, it is possible to form a metal layer or This is preferable because it is possible to perform plasma treatment while damaging the metal oxide layer 20. It is appropriate.
[0076] Two or more plasma treatments may be performed in succession without exposure to the atmosphere. After the nitrogen plasma treatment, a water plasma treatment may be performed.
[0077] As a result, hydrogen, oxygen, water, etc. are released onto the surface or inside of the metal oxide layer 20 as shown in FIG. Elementary radical (H * ), oxygen radical (O * ), hydroxyl radical (OH * ) etc. In addition, in FIG. 4, the resin layer 23 has hydrogen H bonded to carbon C and hydroxyl groups OH These can be heated by heat treatment or exposure to light to become H2O. It is possible.
[0078] The light can be emitted using a lamp, a laser device, or the like.
[0079] It is preferable to irradiate the laser beam using a linear laser device. S (Low Temperature Poly-Silicon) etc. Since laser devices can be used, these devices can be effectively utilized. For example, The linear laser device used in the LTPS crystallization process turns the substrate upside down and The laser beam is irradiated from directly above onto the surface 14, It can be used for the light irradiation process. In addition, the existing LTPS production line can be used for oxide semiconductor ( Applied to the manufacturing line of top-gate self-aligned transistors using OS In this way, the existing LTPS manufacturing equipment can be used for the separation process according to one embodiment of the present invention and the OS It can be easily switched to a manufacturing facility having a transistor manufacturing process.
[0080] The linear laser is focused into a long rectangular shape (formed into a linear laser beam) and the metal oxide layer and the resin are The interface with the layer is irradiated with light.
[0081] The light is preferably irradiated so as to have a wavelength range of 180 nm to 450 nm. More preferably, the light is irradiated to have a wavelength range of 308 nm or thereabouts. It is.
[0082] In one embodiment of the present invention, a laminate structure of a fabricated substrate 14, a metal oxide layer 20, and a resin layer 23 It is preferable that the laser light absorption rate of the laminated structure is high. The absorptance of 8 nm light is preferably 80% or more and 100% or less, and more preferably 85% or more and 10 It is preferable that the laser beam is absorbed by the laminated structure. This can increase the yield of separation. In addition, the irradiation of the laser light to the functional element is suppressed. This makes it possible to suppress the deterioration of the reliability of the functional element.
[0083] The light energy density is 250 mJ / cm 2 More than 400mJ / cm 2 The following is preferred: 2 50mJ / cm 2 More than 360mJ / cm 2 The following is more preferred:
[0084] When irradiating light using a laser device, the number of shots of laser light irradiated to the same location is: It can be 1 shot or more and 50 shots or less, and 1 shot or more and 10 shots or less. Lower is preferable, and more than 1 shot and up to 5 shots is more preferable.
[0085] At both ends of the beam in the short axis direction, there are areas of low light intensity. Set an overlap between one shot and the next shot that is greater than or equal to the width of the lower part. Therefore, the number of shots of the laser light is preferably 1.1 or more. It is preferable that the number of shots is 1.25 or more, and more preferable that the number of shots is 1.25 or more.
[0086] In this specification, the number of shots of laser light refers to the number of shots of laser light irradiated on a certain point (area). This refers to the number of shots, and is determined by the beam width, scan speed, frequency, or overlap rate. In addition, between pulses that move the linear beam in a certain scanning direction, That is, there is an overlap between one shot and the next, and the overlap The ratio is the overlap rate. Note that the closer the overlap rate is to 100%, the The number of shots is high, the further away the fewer the number of shots, and the faster the scan speed. The faster you are, the fewer shots you will need.
[0087] The number of laser shots mentioned above is 1.1, which means that there is no beam between two consecutive shots. This indicates that the overlap is about one-tenth the width of the original. Similarly, 1.25 shots means that there is a quarter of a beam between two successive shots. This indicates that there is an overlap of about 1%, which means that the overlap rate is 25%.
[0088] Here, the energy density of the light irradiated in the LTPS laser crystallization process is high, for example 3 50mJ / cm 2 More than 400mJ / cm 2 The following are included. Also, the number of laser shots For example, 10 to 100 shots are required.
[0089] On the other hand, in the present embodiment, the photochemical treatment for separating the metal oxide layer 20 from the resin layer 23 is performed. The irradiation has a lower energy density or less scattering than the conditions used in the laser crystallization process. This allows the number of substrates that can be processed by a laser device to be increased. In addition, the frequency of laser device maintenance can be reduced, and the running time of the laser device can be improved. Therefore, it is possible to reduce the manufacturing cost of a display device, etc. can.
[0090] In addition, the light irradiation is performed at an energy density lower than that used in the laser crystallization process, or Since the number of shots is small, damage to the substrate caused by laser light irradiation is reduced. Therefore, even if the board is used once, its strength is not easily reduced and it can be reused. Therefore, it is possible to reduce costs.
[0091] In this embodiment, the metal oxide layer 20 is disposed between the fabrication substrate 14 and the resin layer 23. By using the metal oxide layer 20, the light is more diffusive than when the metal oxide layer 20 is not used. Irradiation may be possible at a lower energy density or with a reduced number of shots.
[0092] When irradiating light through the production substrate, foreign matter such as dust is attached to the light irradiation surface of the production substrate. When the resin layer is peeled off, the light irradiation becomes uneven, forming a portion with low peelability, and the metal oxide layer and the resin layer are separated. Therefore, before or after the light irradiation, During this time, it is preferable to clean the light irradiated surface. For example, an organic solvent such as acetone, The light irradiation surface of the substrate can be cleaned with water or the like. This can reduce unevenness in the light irradiation and improve the separation process. The retention can be improved.
[0093] Alternatively, in this embodiment, a metal oxide layer is first formed on a substrate. A resin layer is then formed on the substrate. An insulating layer is then formed on the substrate and the resin layer to cover the end of the resin layer. Next, a transistor having a metal oxide in a channel forming region is formed on the resin layer via an insulating layer. Next, light is irradiated onto the interface between the metal oxide layer and the resin layer or the vicinity thereof. Next, at least a part of the resin layer is separated from the metal oxide layer to determine the starting point of separation. Then, the metal oxide layer and the resin layer are separated.
[0094] The substrate is provided with a portion that is in contact with the resin layer and a portion that is in contact with the insulating layer. The insulating layer is provided to cover the end portion of the resin layer. The insulating layer has a higher density with respect to the metal oxide layer than the resin layer. By covering the end of the resin layer with an insulating layer, For example, the resin layer can be prevented from peeling off from the substrate unintentionally after the laser irradiation. This prevents the resin layer from peeling off when the substrate is transported to a new location. By forming the dots, the metal oxide layer and the resin layer can be separated at the desired timing. That is, in this embodiment, the timing of separation of the metal oxide layer and the resin layer can be controlled. In addition, the force required for separation is small. This makes it possible to easily separate the metal oxide layer and the resin layer. The yield in the manufacturing process of the display device can be increased.
[0095] The display device of this embodiment mode has a metal oxide in a channel formation region of a transistor. The metal oxide can function as an oxide semiconductor.
[0096] The transistor channel formation region is made of low temperature polysilicon (LTPS). When using a layered polysilicon, the temperature is about 500 to 550°C. Since heat is required, the resin layer must be heat resistant. In order to mitigate damage caused by the above, it may be necessary to make the resin layer thicker.
[0097] On the other hand, transistors that use metal oxide in the channel formation region can be heated to temperatures below 350°C and even It can be formed at temperatures below 300° C. Therefore, the resin layer does not require high heat resistance. Therefore, the heat resistance temperature of the resin layer can be lowered, and the range of materials to be selected is expanded.
[0098] In addition, a transistor using a metal oxide for a channel formation region does not require a laser crystallization process. In this embodiment, the conditions are lower than those used in the laser crystallization process. It is possible to irradiate light with a low energy density or a small number of shots. In the process, the laser light is irradiated onto the resin layer without passing through the substrate. The resin layer is irradiated through the substrate and the metal oxide layer. Since the thickness of the resin layer can be thin, the resin layer does not require high heat resistance. By making the LTP thin, it is expected that the cost of device fabrication will be significantly reduced. This is preferable compared to the case where S is used, since the process can be simplified.
[0099] However, in the display device of one embodiment of the present invention, a metal oxide For example, the display device of this embodiment is not limited to a structure having a transistor channel. Silicon can be used for the panel formation region. Crystalline silicon can be microcrystalline silicon or crystalline silicon. Examples of the silicon include silicon, polycrystalline silicon, and single crystal silicon.
[0100] It is preferable to use LTPS for the channel formation region. The GaN can be formed at a lower temperature than single crystal silicon and has a higher thermal conductivity than amorphous silicon. It has field effect mobility and high reliability.
[0101] The thickness of the resin layer 23 may be 0.1 μm or more and 5 μm or less. This allows the display device to be manufactured at low cost. In addition, the display device can be made lighter and thinner. In addition, the flexibility of the display device can be improved.
[0102] The resin layer 23 is not particularly limited in terms of the transmittance of visible light. For example, it may be a colored layer. Here, when the resin layer 23 is located on the display surface side of the display device, the resin If the layer 23 is colored, the light extraction efficiency decreases. This may result in problems such as changes in color and reduced display quality.
[0103] The resin layer 23 is formed by using a wet etching device, a dry etching device, an ashing device, or the like. In particular, the resin layer 23 can be removed by ashing using oxygen plasma. It is preferable to remove
[0104] In this embodiment, the metal oxide layer 20 is provided between the fabrication substrate 14 and the resin layer 23. Since the oxide layer 20 has a function of absorbing light, even if the light absorption rate of the resin layer 23 is low, the light Therefore, the resin layer 23 having a high transmittance of visible light is used. Therefore, even if the resin layer 23 is located on the display surface side of the display device, high display quality can be achieved. In order to improve the display quality, the colored resin layer 23 is removed. In addition, the range of materials that can be selected for the resin layer 23 is expanded.
[0105] The average transmittance of the resin layer 23 for light in the wavelength range of 450 nm to 700 nm is 70%. More preferably, 80% to 100% is more preferable, and more preferably, 90% to 100% is more preferable. The following is more preferred:
[0106] In this embodiment, a transistor or the like is formed at a temperature equal to or lower than the heat resistance temperature of the resin layer. The heat resistance of the material can be evaluated, for example, by the weight loss rate due to heating, specifically, the 5% weight loss temperature. In the peeling method and the manufacturing method of the display device of this embodiment mode, the maximum temperature in the process is lowered. For example, in this embodiment, the 5% weight loss temperature of the resin layer is set to 200° C. or higher. 650℃ or less, 200℃ to 500℃, 200℃ to 400℃, or 200℃ The temperature can be set to 350°C or higher. This allows for a wider range of materials to be selected. The 5% weight loss temperature of the layer may be greater than 650°C.
[0107] It is preferable to supply a liquid containing water to the separation interface before or during the separation. The presence of water reduces the adhesion or bonding strength between the resin layer 23 and the metal oxide layer 20. This reduces the force required for separation. By supplying the resin layer 23 with the metal oxide layer 20, the bond between the resin layer 23 and the metal oxide layer 20 can be weakened or broken. By utilizing the chemical bond with the liquid, the resin layer 23 and the metal oxide layer 20 can be effectively bonded to each other. For example, the resin layer 23 and the metal oxide layer 24 can be separated by cutting the bond between them. When hydrogen bonds are formed between the water and the tree, the supply of water-containing liquid causes the water and tree to form hydrogen bonds. Hydrogen bonds are formed between the resin layer 23 and the metal oxide layer 20, It is believed that hydrogen bonds between the layer 20 are broken.
[0108] The metal oxide layer 20 preferably has a small surface tension and is highly wettable by liquids including water. This allows the water-containing liquid to spread over the entire surface of the metal oxide layer 20, The water spreads over the entire metal oxide layer 20, so that the liquid containing water can be easily supplied to the metal oxide layer 20. Can be peeled off.
[0109] The contact angle of the metal oxide layer 20 with a liquid including water is preferably greater than 0° and equal to or less than 60°. More preferably, the angle is greater than 0° and less than or equal to 50°. When the contact angle is high (e.g., when the contact angle is less than about 20°), it is difficult to obtain an accurate value of the contact angle. The metal oxide layer 20 is preferably more wettable with respect to liquids including water. Therefore, even if the wettability with liquids including water is high, it is difficult to obtain an accurate value of the contact angle. good.
[0110] The presence of a liquid containing water at the separation interface dissipates the static electricity generated during separation into the layer to be peeled off. This prevents the negative effects on the functional elements (such as the destruction of semiconductor elements by static electricity) In addition, the surface of the layer to be peeled off that is exposed by the separation can be neutralized using an ionizer or the like. good.
[0111] When a liquid is supplied to the separation interface, the surface of the layer to be peeled that is exposed by the separation may be dried. .
[0112] A manufacturing method of the display device of this embodiment mode will be specifically described below.
[0113] The thin films (insulating films, semiconductor films, conductive films, etc.) constituting the display device are formed by sputtering, Chemical Vapor Deposition (CVD) method, Air evaporation method, Pulsed Laser Deposition (PLD) n) method, Atomic Layer Deposition (ALD) method, etc. The CVD method can be plasma enhanced chemical vapor deposition (PECVD). :Plasma Enhanced Chemical Vapor Depositi The thermal CVD method may be a metal-organic chemical vapor deposition (MOCVD) method. CVD (Metal Organic CVD) method may also be used.
[0114] Thin films (insulating films, semiconductor films, conductive films, etc.) that make up the display device are formed by spin coating, dipping, Spray application, inkjet, dispensing, screen printing, offset printing, document printing For methods such as tar knife, slit coat, roll coat, curtain coat, knife coat, etc. It can be formed more.
[0115] When processing the thin films that make up the display device, lithography methods can be used. Alternatively, island-shaped thin films may be formed by a film-forming method using a shadow mask. Alternatively, the thin film is processed by nanoimprinting, sandblasting, lift-off, etc. In the photolithography method, a resist mask is formed on the thin film to be processed. The thin film is then processed by etching or the like, and the resist mask is then removed. After forming a thin film having the above-mentioned properties, the thin film is exposed to light and developed to be processed into a desired shape. And there is.
[0116] When light is used in the lithography method, the light used for exposure is, for example, i-line (wavelength 365 nm). m), g-ray (wavelength 436 nm), h-ray (wavelength 405 nm), or a mixture of these In addition, ultraviolet light, KrF laser light, ArF laser light, etc. can be used. Also, exposure may be performed by immersion lithography. Examples of light that can be used include extreme ultraviolet (EUV) and X-rays. Alternatively, an electron beam may be used in place of the light used for exposure. Extremely fine processing is possible using ultraviolet light, X-rays, or electron beams, and is therefore preferred. When exposure is performed by scanning a beam such as an electron beam, a photomath No sc is required.
[0117] For etching thin films, there are dry etching, wet etching, and sandblasting methods. etc. can be used.
[0118] [Removal method] First, a metal oxide layer 20 is formed on a substrate 14 (FIG. 5(A1)). A metal layer 19 and a metal oxide layer 20 are laminated on the substrate 14 (FIG. 5(A2)).
[0119] The substrate 14 to be manufactured has a rigidity sufficient for easy transportation and is resistant to the temperatures involved in the manufacturing process. The substrate 14 can be made of, for example, glass, Examples include quartz, ceramic, sapphire, resin, semiconductor, metal, and alloy. Examples of the glass include non-alkali glass, barium borosilicate glass, and aluminoborosilicate glass. Examples include acid glass.
[0120] As described above, in this embodiment, a base layer is formed between the fabrication substrate 14 and the resin layer 23. The base layer is a layer that has lower adhesion (bonding) to the resin layer 23 than the preparation substrate 14. In the embodiment, the case where the metal oxide layer 20 is used will be described as an example, but the present invention is not limited to this. .
[0121] Specifically, the underlayer may include titanium, molybdenum, aluminum, tungsten, silicon, etc. , indium, zinc, gallium, tantalum, tin, hafnium, yttrium, zirconium One or more of the following: aluminum, magnesium, lanthanum, cerium, neodymium, bismuth, and niobium The underlayer may be a layer having one or more of a metal, an alloy, or a compound thereof. The underlayer may contain titanium, molybdenum, aluminum, etc. One of the following: aluminum, tungsten, silicon, indium, zinc, gallium, tantalum, and tin It is preferred to have one or more.
[0122] The material of the underlayer is not limited to inorganic materials, but may be organic materials. For example, organic E Various organic materials that can be used for the EL layer of an LED device may be used as the base layer. Therefore, a vapor deposition film of an organic material can be used, which allows the formation of a film with low adhesion.
[0123] The metal layer 19 can be made of various metals, alloys, and the like.
[0124] The metal oxide layer 20 can be made of oxides of various metals. For example, titanium dioxide (TiO x ), molybdenum oxide, aluminum oxide, tungsten oxide Indium Tin Oxide with Silicon (ITSO), Indium Zinc Oxide, In-G Examples include a-Zn oxide.
[0125] Other metal oxides include indium oxide, indium oxide containing titanium, titanium Indium oxide with tin oxide (ITO), ITO with titanium , Indium zinc oxide containing tungsten, zinc oxide (ZnO), Zn containing gallium O, hafnium oxide, yttrium oxide, zirconium oxide, gallium oxide, tantalum oxide , magnesium oxide, lanthanum oxide, cerium oxide, neodymium oxide, tin oxide, bismuth oxide Examples of the salt include smuth, titanates, tantalates, and niobates.
[0126] There is no particular limitation on the method for forming the metal oxide layer 20. For example, sputtering, plasma C It can be formed by using the VD method, the vapor deposition method, the sol-gel method, the electrophoresis method, the spray method, etc. .
[0127] After the metal layer is formed, oxygen is introduced into the metal layer to form a metal oxide layer 20. In this case, only the surface of the metal layer or the entire metal layer is oxidized. In this case, by introducing oxygen into the metal layer, a laminated structure of a metal layer 19 and a metal oxide layer 20 is formed. (Figure 5(A2)).
[0128] For example, the metal layer can be oxidized by heating the metal layer in an atmosphere containing oxygen. It is preferable to heat the metal layer while flowing a gas containing oxygen. The temperature is preferably 100° C. or higher and 500° C. or lower, and more preferably 100° C. or higher and 450° C. or lower. The temperature is preferably 100° C. or higher and 400° C. or lower, and more preferably 100° C. or higher and 350° C. or lower. stomach.
[0129] The metal layer is preferably heated to a temperature below the maximum temperature in the fabrication of the transistor. This makes it possible to prevent the maximum temperature in the manufacture of the display device from becoming too high. By keeping the temperature below the maximum temperature in the manufacture of transistors, This allows existing equipment to be reused, reducing the need for additional capital investment. Therefore, the production cost of the display device can be reduced. When the manufacturing temperature of the capacitor is up to 350° C., the heat treatment temperature is preferably 350° C. or less. I wish.
[0130] Alternatively, the metal layer can be oxidized by performing a radical treatment on the surface of the metal layer. In the radical treatment, the reaction is carried out in an atmosphere containing at least one of oxygen radicals and hydroxyl radicals. It is preferable to expose the surface of the metal layer to oxygen or water vapor (H2O). It is preferable to carry out the plasma treatment in an atmosphere containing one or both of them.
[0131] As described above, hydrogen, oxygen, hydrogen radicals (H * ) , oxygen radical (O * ), hydroxyl radical (OH * ) and other metal oxides. This also reduces the force required to separate the metal oxide layer 20 from the resin layer 23. It is preferable to perform radical treatment or plasma treatment in forming 20 .
[0132] When the metal layer is oxidized by performing radical treatment or plasma treatment on the surface of the metal layer This eliminates the need for a process of heating the metal layer at a high temperature. This can prevent the temperature from increasing.
[0133] Alternatively, the metal oxide layer 20 can be formed under an oxygen atmosphere. A metal oxide film is formed by sputtering while a gas containing metal oxide is flowing. In this case, too, the surface of the metal oxide layer 20 is subjected to radical treatment. In the radical treatment, oxygen radicals, hydrogen radicals, and hydroxyl radicals are preferably used. It is preferable to expose the surface of the metal oxide layer 20 to an atmosphere containing at least one of the following: For example, the plasma is processed in an atmosphere containing one or more of oxygen, hydrogen, or water vapor (H2O). It is preferable to carry out plasma treatment.
[0134] For details of the radical treatment, please refer to the above-mentioned contents.
[0135] Other methods for introducing oxygen, hydrogen, water, etc. include ion implantation, ion doping, A plasma immersion ion implantation method or the like can be used.
[0136] The thickness of the metal layer 19 is preferably 1 nm or more and 100 nm or less, and more preferably 1 nm or more and 50 nm or less. It is more preferable that the thickness is 1 nm or more and 20 nm or less.
[0137] The thickness of the metal oxide layer 20 is preferably, for example, 1 nm or more and 200 nm or less, and more preferably 5 nm or more. The thickness is preferably 100 nm or less, and more preferably 5 nm to 50 nm. When the metal oxide layer 20 is formed using can be greater than the thickness of the deposited metal layer.
[0138] Before or during the separation, a liquid containing water is supplied to the interface between the metal oxide layer 20 and the resin layer 23. By so doing, it is possible to reduce the force required for separation. The smaller the contact angle, the greater the effect of liquid supply. The contact angle of the solid layer 20 with a liquid including water is preferably greater than 0° and less than 60°. A maximum of 50° or less is more preferable.
[0139] For the metal oxide layer 20, titanium oxide, tungsten oxide, etc. are suitable. In this case, the cost can be reduced compared to tungsten oxide, which is preferable.
[0140] The metal oxide layer 20 may have a photocatalytic function. By irradiating the metal oxide layer with light, a photocatalytic reaction can be induced. The adhesive strength with the fat layer may be weakened, and the metal oxide layer 20 may be easily separated. For example, the metal oxide layer 20 can be irradiated with light having a wavelength that activates the metal oxide layer 20. For example, after the metal oxide layer 20 is formed, the metal oxide layer 20 is irradiated with ultraviolet light without passing through any other layer. The metal oxide layer 20 may be directly irradiated with ultraviolet light. Examples of ultraviolet lamps include mercury lamps, mercury xenon lamps, Metal halide lamps, etc. Alternatively, a laser irradiation step performed before separation can be used to The metal oxide layer 20 may be activated.
[0141] Titanium oxide doped with metal or nitrogen may also be used. When metal oxide layer 20 is formed using tungsten, it can be activated by visible light, but not by ultraviolet light. It is possible.
[0142] Next, a first layer 24 is formed on the metal oxide layer 20 (FIG. 5(B)).
[0143] FIG. 5B shows an example in which the first layer 24 is formed on the entire surface of the metal oxide layer 20 by using a coating method. The first layer 24 may be formed by a method other than the above, such as a printing method. On the layer 20, an island-shaped first layer 24, a first layer 24 having an opening or a concave-convex shape, etc. are formed. This is also fine.
[0144] The first layer 24 can be formed using various resin materials (including resin precursors).
[0145] The first layer 24 is preferably formed using a material having thermosetting properties.
[0146] The first layer 24 may be formed using a material having photosensitivity, or a material having no photosensitivity ( The insulating layer 11 may be formed using a non-photosensitive material.
[0147] When a photosensitive material is used, a part of the first layer 24 can be removed by a lithography method using light. Then, the resin layer 23 can be formed in a desired shape.
[0148] The first layer 24 is made of a material containing a polyimide resin, a polyimide resin precursor, or an acrylic resin. The first layer 24 is preferably formed using a material such as a polyimide resin and a solvent. Materials containing polyamic acid and a solvent, materials containing acrylic resin and a solvent, etc. The first layer 24 can be formed using a polyimide resin or The use of a material containing a precursor is preferable because it can relatively increase heat resistance. When a material containing an acrylic resin is used for the layer 24, the translucency in visible light can be improved. Polyimide resin and acrylic resin are suitable for use as planarizing films for display devices. Since the material is suitable for use in the above-mentioned applications, it is possible to share the same deposition equipment and materials. Therefore, no new device or material is required to realize the configuration of one embodiment of the present invention. The first layer 24 does not need to be made of a special material and can be made of a resin material used in display devices. This allows for cost reduction.
[0149] Specifically, the resin layer 23 is made of a compound (oxydiphthalic acid) represented by the structural formula (100). It is preferred that the aryl group has a residue.
[0150] [ka]
[0151] The resin layer 23 contains an acid component containing oxydiphthalic acid or an oxydiphthalic acid derivative, and an aromatic and an amine component containing an aromatic amine or an aromatic amine derivative, The oxydiphthalic acid derivative is, for example, oxydiphthalic anhydride. The resin layer 23 may include fluorine. When the fluorine is contained, hydrogen bonds are formed between the metal oxide layer 20 and the resin layer 23 using the fluorine. This can sometimes happen.
[0152] Also, polyimide resin or polyimide resin that can be suitably used for the first layer 24 The physical properties of the materials including the precursor are shown in Table 1.
[0153] [Table 1]
[0154] The resin layer 23 can be formed using materials A to E shown in Table 1. In order to improve the reliability, the glass transition temperature (Tg) and 5% weight loss temperature of the material are , it is preferable that each is higher.
[0155] Other examples of resin materials that can be used to form the first layer 24 include epoxy. Silicone resin, polyamide resin, polyimide amide resin, siloxane resin, benzocyclobutene resins, phenolic resins, and precursors of these resins.
[0156] The first layer 24 is preferably formed by using a spin coater. This makes it possible to form a uniform thin film on a large substrate.
[0157] The first layer 24 has a viscosity of 5 cP or more and less than 500 cP, preferably 5 cP or more and less than 100 cP. It is preferable to form the film using a solution having a viscosity of less than 10 cP and more preferably 50 cP or more. The lower the viscosity of the solution, the easier it is to apply. Also, the lower the viscosity of the solution, the less air bubbles will be trapped. This can suppress the formation of a high-quality film.
[0158] Other methods for forming the first layer 24 include dipping, spray coating, and inkjet. , Dispense, Screen printing, Offset printing, Doctor knife, Slit coat, Examples include roll coating, curtain coating, and knife coating.
[0159] Next, the first layer 24 is subjected to a heat treatment to form a resin layer 23 (FIG. 5(C) ).
[0160] The heat treatment may be carried out, for example, by filling the chamber of a heating device with oxygen, nitrogen, and a rare gas (such as argon). The process can be carried out while flowing a gas containing one or more of the following: The treatment can be carried out in an air atmosphere using a heating chamber, hot plate, etc. Cut.
[0161] When the heating is performed in an air atmosphere or while a gas containing oxygen is flowing, the resin layer 23 becomes discolored due to oxidation. However, the transmittance of visible light may decrease.
[0162] Therefore, it is preferable to perform heating while flowing nitrogen gas. The amount of oxygen contained therein can be reduced compared to the air atmosphere, and oxidation of the resin layer 23 can be suppressed. This can increase the transparency of the resin layer 23 to visible light.
[0163] The heat treatment can reduce degassed components (e.g., hydrogen, water, etc.) in the resin layer 23. In particular, it is preferable to heat the resin layer 23 at a temperature equal to or higher than the manufacturing temperature of each layer to be formed on the resin layer 23. This significantly suppresses degassing from the resin layer 23 during the transistor manufacturing process. It can be controlled.
[0164] For example, when the manufacturing temperature of the transistor is up to 350° C., the film to be the resin layer 23 is Heating is preferably performed at 0°C or higher and 450°C or lower, more preferably 400°C or lower, and more preferably 375°C or lower. This makes it possible to prevent the resin layer 23 from being damaged during the transistor manufacturing process. This can significantly suppress outgassing from the gas.
[0165] The temperature of the heat treatment is preferably equal to or lower than the maximum temperature in the manufacture of a transistor. By keeping the temperature below the maximum temperature in the transistor manufacturing process, This allows the reuse of existing manufacturing equipment, reducing additional capital investment. Therefore, the production cost of the display device can be reduced. If the transistor manufacturing temperature is up to 350° C., the heat treatment temperature is 350° C. or less. It is preferable to do so.
[0166] If the maximum temperature in the transistor manufacturing process is set to the same as the temperature of the heat treatment, By doing so, the maximum temperature in the manufacture of the display device can be prevented from becoming too high, and the resin layer 23 This is preferable since it is possible to reduce degassed components.
[0167] By increasing the treatment time, the heating temperature can be increased even if the heating temperature is relatively low. Therefore, it is possible to achieve peelability equivalent to that achieved under the above conditions by changing the configuration of the heating device. If the heat temperature cannot be increased, it is preferable to extend the treatment time.
[0168] The heat treatment time is, for example, preferably from 5 minutes to 24 hours, and more preferably from 30 minutes to 12 hours. More preferably, the heat treatment time is from 1 hour to 6 hours, and even more preferably from 1 hour to 6 hours. For example, the heat treatment may be performed by RTA (Rapid Thermal Anneal). In some cases, such as when using the annealing method, the time may be less than 5 minutes.
[0169] Heating devices include electric furnaces and resistance heating elements that use heat conduction or heat radiation. Various equipment can be used, such as equipment that heats the workpiece with a gas. For example, as Rapid Thermal Anneal) equipment, LRTA (Lamp Rap) An RTA device such as a LR id Thermal Anneal device can be used. TA equipment includes halogen lamps, metal halide lamps, xenon arc lamps, carbon Light emitted from lamps such as arc lamps, high-pressure sodium lamps, and high-pressure mercury lamps (electromagnetic The GRTA device uses high-temperature gas to heat the material being treated. By using an RTA device, the processing time can be shortened. This is preferable for mass production. In addition, the heat treatment is performed using an in-line heating device. It is acceptable to do so.
[0170] The thickness of the resin layer 23 may be changed from the thickness of the first layer 24 by the heat treatment. For example, the solvent contained in the first layer 24 is removed, and the hardening progresses, causing the density to decrease. As a result, the volume of the resin layer 23 may decrease, and the resin layer 23 may become thinner than the first layer 24. do.
[0171] Before the heat treatment, a heat treatment (pre-bake) is performed to remove the solvent contained in the first layer 24. The temperature of the pre-baking process is appropriately determined depending on the material used. For example, the temperature range can be 50°C or higher and 180°C or lower, 80°C or higher and 150°C or lower, or 9 The heating process can be performed at 0°C to 120°C. Alternatively, the heating process can be performed as a pre-bake process. Alternatively, the solvent contained in the first layer 24 may be removed by a heat treatment.
[0172] The resin layer 23 has flexibility. The preparation substrate 14 has lower flexibility than the resin layer 23.
[0173] The thickness of the resin layer 23 is preferably 0.01 μm or more and less than 10 μm. More preferably, the thickness is from 0.5 μm to 3 μm. By forming a thin resin layer, the display device can be manufactured at low cost. This allows the display device to be made lighter and thinner. In addition, the flexibility of the display device can be improved. By using a low viscosity solution, it becomes easy to form a thin resin layer 23. However, The thickness of the resin layer 23 is not limited to this, and may be 10 μm or more. The thickness of the resin layer 3 may be set to 10 μm or more and 200 μm or less. This is preferable because it is possible to increase the rigidity of the display device.
[0174] The thermal expansion coefficient of the resin layer 23 is preferably 0.1 ppm / ° C. or more and 50 ppm / ° C. or less. It is preferable that the temperature is 0.1 ppm / ℃ or more and 20 ppm / ℃ or less. It is more preferable that the thermal expansion coefficient of the resin layer 23 is 10 ppm / °C or more and 20 ppm / °C or less. The lower the temperature, the more likely it is that cracks will occur in the layers that make up the transistors, etc., due to heating, and This can prevent damage to resistors, etc.
[0175] Next, a peeled layer 25 is formed on the resin layer 23 (FIG. 5(D)).
[0176] As the peeled layer 25, for example, an insulating layer or a functional element (transistor, display element, etc.) is provided. It is possible.
[0177] The layer to be peeled 25 preferably has an insulating layer. The insulating layer is formed in a subsequent heating step. The metal oxide layer 20 and the resin layer 23 are used to block hydrogen, oxygen, and water released from the metal oxide layer 20 and the resin layer 23. It is preferable that the ion exchange resin has a function of
[0178] The layer to be peeled off is, for example, a silicon nitride film, a silicon oxynitride film, or a silicon nitride oxide film. For example, a silicon nitride film is preferably formed by evaporating a mixture of silane gas, hydrogen gas, and ammonium nitrate. The insulating layer is formed by the plasma CVD method using a deposition gas containing NH3 gas. The thickness of the film is not particularly limited. For example, the thickness is 50 nm or more and 600 nm or less, and preferably 100 nm or less. The thickness of the insulating layer can be from 100 nm to 300 nm.
[0179] In this specification, the term "silicon oxynitride" refers to a material having a higher content of oxygen than nitrogen. In this specification, the term "silicon oxynitride" refers to a material having a high content of The composition of the material contains more nitrogen than oxygen.
[0180] Then, a protective layer is formed on the peeled layer 25. The protective layer is a layer located on the outermost surface of the display device. The protective layer preferably has high transparency to visible light. By having such a structure, it is possible to suppress scratches and cracks on the surface of the display device. This is preferable.
[0181] FIG. 5D shows an example in which a substrate 75a is bonded onto the peeled layer 25 using an adhesive layer 75b. show.
[0182] The adhesive layer 75b may be a light-curing adhesive such as an ultraviolet-curing adhesive, a reaction-curing adhesive, or a heat-curing adhesive. Various curing adhesives such as anaerobic adhesives and adhesive sheets can be used. It's fine.
[0183] The substrate 75a is made of, for example, polyethylene terephthalate (PET), polyethylene naphtha Polyester resins such as polyacrylonitrile resins, acrylic resins, Polyimide resin, polymethyl methacrylate resin, polycarbonate (PC) resin, polyethylene Polyethersulfone (PES) resin, polyamide resin (nylon, aramid, etc.), polysiloxane San resin, cycloolefin resin, polystyrene resin, polyamide-imide resin, polyurethane Tan resin, polyvinyl chloride resin, polyvinylidene chloride resin, polypropylene resin, polytetrafluoroethylene Polytetrafluoroethylene (PTFE) resin, ABS resin, cellulose nanofiber, etc. The substrate 75a may be made of glass, quartz, resin, or the like having a thickness sufficient to provide flexibility. Various materials such as metals, alloys, and semiconductors may be used.
[0184] Next, the laser beam 55 is irradiated (FIG. 6(A)). The laser beam 55 is, for example, In this case, the linear laser beam is scanned from left to right, and its long axis is aligned along the scanning direction and In the laser device, the substrate 14 is on the upper side. The laminate is placed so that the laser beam is irradiated from above the laminate (the substrate 14). 55 is irradiated.
[0185] The laser light 55 is incident on the interface between the metal oxide layer 20 and the resin layer 23 or on the interface between the metal oxide layer 20 and the resin layer 23 via the production substrate 14. It is preferable that the laser be irradiated in the vicinity of the processing area 640 in FIG. 6(A). The light 55 may be irradiated into the metal oxide layer 20 or into the resin layer 23 .
[0186] The metal oxide layer 20 absorbs the laser light 55. The resin layer 23 absorbs the laser light 55. Good too.
[0187] The absorptance of the laser light 55 in the laminated structure of the fabricated substrate 14 and the metal oxide layer 20 is 50% or more. Preferably, the ratio is 75% or more and 100% or less, more preferably 75% or more and 100% or less, and more preferably 80% or more and 100% or less. % or less. The laminated structure absorbs most of the laser light 55, It is possible to reliably separate the oxide layer from the resin layer 23 at the interface between the oxide layer and the resin layer 23. Reduces damage caused by light.
[0188] The adhesion or bonding between the metal oxide layer 20 and the resin layer 23 is reduced by the irradiation of the laser light 55. Irradiation with the laser light 55 may weaken the resin layer 23.
[0189] At least a part of the laser light 55 is transmitted through the substrate 14 and is incident on the metal oxide layer 14. The laser light 55 is selected from the wavelengths absorbed by the laser 20. For example, light having a wavelength of 180 nm or more and 450 nm or less is preferable. Preferably, the wavelength is 200 nm or more and 400 nm or less, and more preferably, the wavelength is 250 nm or more and 35 Light below 0 nm can be used.
[0190] The laser light 55 has an energy higher than the energy gap of the metal oxide layer 20. For example, the energy gap of titanium oxide is about 3.2 eV. Therefore, when titanium oxide is used for the metal oxide layer 20, the light has an energy higher than 3.2 eV. It is preferable that the fluorine-containing compound has an energy content of 1000 to 2000.
[0191] In particular, it is preferable to use an excimer laser with a wavelength of 308 nm, since this has excellent productivity. The Shima laser is also used for laser crystallization in LTPS, so it is compatible with existing LTPS manufacturing lines. This is preferable because the existing equipment can be reused and no new capital investment is required. The energy of light at 8 nm is about 4.0 eV. When using a laser, an excimer laser with a wavelength of 308 nm is suitable. Solid-state UV lasers (semiconductor UV lasers) such as a 355 nm UV laser, which is the third harmonic of the A solid-state laser does not use gas, so it is not an excimer laser. In comparison, the running costs can be reduced, which is preferable. may also be used.
[0192] When a linear laser beam is used as the laser beam 55, the substrate 14 and the light source are relatively The laser beam 55 is scanned by moving the laser beam 55 to the area to be separated. do.
[0193] Here, if foreign matter 18 such as dust adheres to the light irradiation surface of the production substrate 14, the light irradiation becomes uneven. In FIG. 7A, a resin layer 23 is formed on and in contact with a production substrate 14. In FIG. 7A, the interface between the substrate 14 and the resin layer 23 or its vicinity is In this example, the light-irradiated area 16 is interrupted directly below the foreign object 18. The portion has a lower peelability than the other portions, and therefore, in the process of separating the production substrate 14 and the resin layer 23, There is a concern that yields will decrease.
[0194] On the other hand, in this embodiment, a base layer is formed between the fabrication substrate 14 and the resin layer 23. As the layer, a metal layer 19, a metal oxide layer 20, or, as shown in FIG. 7B, a metal layer 1 The underlayer may be a laminate of a metal oxide layer 20 and a base layer 9. For example, when the thermal conductivity of the metal layer 19 shown in FIG. Even if a foreign object 18 is attached to the irradiated surface, the metal layer 19 around the foreign object 18 is heated, Heat is conducted uniformly to the entire metal layer 19. Heat is also conducted to the part of the metal layer 19 that is in the shadow of the foreign object 18. As shown in Figure 7(B), the generation of areas with low peelability can be suppressed. At or near the interface between the metal layer 19 and the metal oxide layer 20, including directly below the foreign matter 18 A heated area 17 is formed over the entire surface.
[0195] At the interface between the metal oxide layer 20 and the resin layer 23 or in the vicinity thereof, the area not exposed to light is The area of the region not exposed to light is not particularly limited. For example, 1 μm 2 More than 1cm 2 In some cases, the light may The area of the non-contact region is 1 μm 2 Less than or equal to 1cm 2 It may be more than that.
[0196] Next, the fabricated substrate 14 is separated from the resin layer 23. Adhesion between the metal oxide layer 20 and the resin layer 23 Since the adhesion or the like is low, separation occurs at the interface between the metal oxide layer 20 and the resin layer 23 ( 6(B1)). Also, separation may occur in the weakened resin layer 23.
[0197] For example, a pulling force is applied to the resin layer 23 in a vertical direction, so that the substrate 14 and the resin layer Specifically, a part of the upper surface of the substrate 75a is attracted and then pulled upward. By pulling, the resin layer 23 can be peeled off from the preparation substrate 14 .
[0198] Here, during separation, a liquid containing water, such as water or an aqueous solution, is added to the separation interface, and the liquid is By performing separation so that the particles penetrate the surface, separation can be easily performed. The static electricity that is generated can adversely affect functional elements such as transistors (semiconductor elements are In FIG. 6B2, the liquid supply mechanism 21 is used to 2 shows an example of supplying liquid to the separation interface.
[0199] The liquid to be supplied may be water (preferably pure water), neutral, alkaline, or acidic aqueous solution. Examples of solvents include aqueous solutions containing dissolved salts, ethanol, acetone, etc. Additionally, various organic solvents may be used.
[0200] Before the separation, a part of the resin layer 23 is separated from the production substrate 14 to form a starting point for separation. For example, a sharp tool such as a blade may be inserted between the fabrication substrate 14 and the resin layer 23. Alternatively, a sharp tool may be inserted from the substrate 75a side to form a separation starting point. Alternatively, the resin layer 23 may be cut by laser ablation to form a starting point for separation. The starting point of separation may be formed by a method using a laser such as a laser beam splitting method.
[0201] In this embodiment, the metal oxide layer 20 and the resin layer 23 are laminated and then irradiated with light. This can reduce the adhesion or bonding strength between the metal oxide layer 20 and the resin layer 23. Therefore, the preparation substrate 14 and the resin layer 23 can be easily separated.
[0202] By using the peeling method of the present embodiment, a peeling method with low cost and high mass productivity, or a semiconductor For example, in the peeling method of the present embodiment, A substrate 14 (e.g., a glass substrate) or a laminate of a prepared substrate 14 and a metal oxide layer 20 Since the material can be reused multiple times, production costs can be reduced.
[0203] [Production method example 1] Next, an example of a method for manufacturing the display device of this embodiment will be described. Descriptions of similar parts may be omitted.
[0204] First, a metal oxide layer 20 is formed on a substrate 14 (FIG. 8(A)). For details about No. 0, please refer to the description of the peeling method above.
[0205] Next, a first layer 24 is formed on the metal oxide layer 20 (FIG. 8(B)). For details, please refer to the description of the peeling method.
[0206] In this embodiment, the first layer 24 is formed using a material having photosensitivity and thermosetting properties. The first layer 24 may be formed using a non-photosensitive material.
[0207] After the first layer 24 is formed, a heat treatment (pre-baking treatment) is performed to remove the solvent. After that, a photomask is used to expose the film. Then, development is performed to remove the unnecessary parts. Next, the first layer 24 processed into a desired shape is subjected to a heat treatment. In FIG. 8(C), the island-shaped resin layer 23 is An example of how to form the
[0208] The shape of the resin layer 23 is not limited to one island shape, but may be, for example, a shape of multiple islands or a shape having an opening. Also, exposure techniques using half-tone masks or gray-tone masks are possible. Alternatively, a concave-convex shape may be formed on the surface of the resin layer 23 by using a technique such as a multi-exposure technique or a multi-layer exposure technique.
[0209] A mask such as a resist mask or a hard mask is formed on the first layer 24 or the resin layer 23. By etching, it is possible to form the resin layer 23 in a desired shape. This is particularly suitable when a non-photosensitive material is used.
[0210] For example, an inorganic film is formed on the resin layer 23, and a resist mask is formed on the inorganic film. After etching the inorganic film using a hard mask, the inorganic film is used as a hard mask to form a resin layer. 23 can be etched.
[0211] Inorganic films that can be used as hard masks include various inorganic insulating films and conductive layers. Examples of the film include a metal film and an alloy film that can be used.
[0212] The mask can be formed to an extremely thin thickness and can be removed at the same time as etching. This is preferable because it can eliminate the step of removing the mask.
[0213] For details of the heat treatment, the description of the heat treatment in the above peeling method can be referred to.
[0214] Next, the insulating layer 31 is formed on the resin layer 23 (FIG. 8(D)). The resin layer 23 is not provided on the metal oxide layer 20. Therefore, the insulating layer 31 can be formed on and in contact with the metal oxide layer 20. Cut.
[0215] The insulating layer 31 is formed at a temperature equal to or lower than the heat-resistant temperature of the resin layer 23. It is preferable to form the film at a high speed.
[0216] The insulating layer 31 prevents impurities contained in the resin layer 23 from being transferred to transistors and display elements to be formed later. For example, the insulating layer 31 can be a resin layer. When the resin layer 23 is heated, moisture contained in the resin layer 23 diffuses into the transistors and display elements. It is preferable to prevent this from happening, and therefore it is preferable that the insulating layer 31 has high barrier properties.
[0217] The insulating layer 31 may be, for example, a silicon nitride film, a silicon oxynitride film, a silicon oxide film, Using inorganic insulating films such as silicon oxynitride film, aluminum oxide film, and aluminum nitride film In addition, a hafnium oxide film, a yttrium oxide film, a zirconium oxide film, Gallium oxide film, tantalum oxide film, magnesium oxide film, lanthanum oxide film, cerium oxide film A film, a neodymium oxide film, etc. may be used. In addition, two or more of the above-mentioned insulating films may be stacked. In particular, a silicon nitride film is formed on the resin layer 23, and a silicon oxide film is formed on the silicon nitride film. It is preferable to form a silicon film.
[0218] The higher the deposition temperature, the denser and more effective the inorganic insulating film becomes, so it is formed at a high temperature. It is preferable.
[0219] The substrate temperature during the deposition of the insulating layer 31 is preferably from room temperature (25° C.) to 350° C. C. or higher and 300.degree. C. or lower is more preferable.
[0220] Next, a transistor 40 is formed on the insulating layer 31 (FIG. 8(E)).
[0221] The structure of the transistor in the display device is not particularly limited. For example, The transistor may be a staggered type transistor, or an inverse staggered type transistor. In addition, the transistor may be of either a top gate structure or a bottom gate structure. Alternatively, gate electrodes may be provided above and below the channel.
[0222] Here, the transistor 40 is a bottom-gate transistor having a metal oxide layer 44. The metal oxide layer 44 serves as a semiconductor layer of the transistor 40. The metal oxide can function as an oxide semiconductor.
[0223] In this embodiment, an oxide semiconductor is used as the semiconductor of the transistor. If a semiconductor material with a wider band gap and lower carrier density is used, This is preferable because it can reduce the current when the transistor is in the off state.
[0224] The transistor 40 is formed at a temperature equal to or lower than the heat-resistant temperature of the resin layer 23. It is preferable to form the insulating film at a temperature lower than the temperature of the heat treatment.
[0225] Specifically, first, the conductive layer 41 is formed on the insulating layer 31. The conductive layer 41 is formed by depositing a conductive film. Then, a resist mask is formed, the conductive film is etched, and the resist mask is removed. It can be formed by removing
[0226] The substrate temperature during the deposition of the conductive film is preferably from room temperature to 350° C., and more preferably from room temperature to 300° C. is more preferred.
[0227] The conductive layer of the display device is made of aluminum, titanium, chromium, nickel, or copper. , yttrium, zirconium, molybdenum, silver, tantalum, or tungsten, etc. Metals or alloys mainly made of metals can be used as single-layer or multi-layer structures. Alternatively, indium oxide, indium tin oxide (ITO), or indium containing tungsten Indium Zinc Oxide, Indium Zinc Oxide with Tungsten, Indium Oxide with Titanium materials, titanium-containing ITO, indium zinc oxide, zinc oxide (ZnO), gallium-containing A conductive material having light-transmitting properties, such as ZnO or ITO containing silicon, may also be used. In addition, polycrystalline silicon or oxide semiconductors that have been made low-resistance by including impurity elements, etc. Alternatively, a semiconductor such as silicon or a silicide such as nickel silicide may be used. A film containing graphene can also be used. The film containing graphene can be, for example, a film containing graphene oxide. In addition, a film containing an oxide semiconductor or the like containing an impurity element can be formed. A semiconductor may be used, or a conductive paste such as silver, carbon, or copper, or The conductive paste may be formed using a conductive polymer such as polythiophene. Conductive polymers are preferred because they are easy to apply.
[0228] Next, the insulating layer 32 is formed. The insulating layer 32 is made of an inorganic insulating material that can be used for the insulating layer 31. The velum can be used.
[0229] Next, the metal oxide layer 44 is formed. The metal oxide layer 44 is formed after the metal oxide film is formed. A resist mask is formed, the metal oxide film is etched, and then the resist mask is removed. It can be formed by removing
[0230] The substrate temperature during the deposition of the metal oxide film is preferably 350°C or less, and more preferably from room temperature to 200°C or less. The temperature is more preferably from room temperature to 130° C., and even more preferably from room temperature to 130° C.
[0231] The metal oxide film is formed using either or both of an inert gas and oxygen gas. In addition, there is no particular limitation on the flow rate ratio of oxygen (oxygen partial pressure) during the formation of the metal oxide film. However, in order to obtain a transistor with high field effect mobility, metal oxide The flow rate ratio of oxygen (oxygen partial pressure) during the deposition of the film is preferably 0% or more and 30% or less. % or more and 30% or less is more preferable, and 7% or more and 15% or less is even more preferable.
[0232] The metal oxide film preferably contains at least indium or zinc. It is preferred that the metal comprises zinc and zinc.
[0233] The metal oxide preferably has an energy gap of 2 eV or more, and more preferably 2.5 eV or more. More preferably, the energy is 3 eV or more, and even more preferably, the energy is 3 eV or more. By using metal oxides with a wide energy gap, the off-state current of transistors can be reduced. This can be done.
[0234] The metal oxide film can be formed by a sputtering method. A PECVD method, a thermal CVD method, an ALD method, a vacuum deposition method, or the like may also be used.
[0235] Next, the conductive layer 43a and the conductive layer 43b are formed. The conductive layer 43a and the conductive layer 43b are After forming a conductive film, a resist mask is formed, the conductive film is etched, and then a resist is formed. The conductive layer 43a and the conductive layer 43b can be formed by removing the mask. , and is connected to the metal oxide layer 44 .
[0236] When the conductive layers 43a and 43b are processed, the metal that is not covered with the resist mask is A portion of the metal oxide layer 44 may be thinned by etching.
[0237] The substrate temperature during the deposition of the conductive film is preferably from room temperature to 350° C., and more preferably from room temperature to 300° C. is more preferred.
[0238] In this manner, the transistor 40 can be manufactured (FIG. 8(E)). In this case, a part of the conductive layer 41 functions as a gate, and a part of the insulating layer 32 functions as a gate insulating layer. The conductive layer 43a and the conductive layer 43b function as either a source or a drain. It functions as one side.
[0239] Next, an insulating layer 33 is formed to cover the transistor 40 (FIG. 9(A)). It can be formed in a similar manner to the edge layer 31.
[0240] The insulating layer 33 may be a silicon oxide film or a silicon oxynitride film formed in an atmosphere containing oxygen. It is preferable to use an oxide insulating film such as a silicon oxide film. This involves laminating an insulating film, such as a silicon nitride film, on a silicon oxide film, which is difficult for oxygen to diffuse or penetrate. It is preferable that the oxide insulating film formed in an atmosphere containing oxygen releases a large amount of oxygen when heated. Such an oxide insulating film that releases oxygen and an insulating film that releases oxygen can be used. By laminating an insulating film that is difficult for metal oxide to diffuse or penetrate, heat treatment is performed. As a result, oxygen vacancies in the metal oxide layer 44 and Defects at the interface between the metal oxide layer 44 and the insulating layer 33 can be repaired and the defect level can be reduced. This makes it possible to realize a display device with extremely high reliability.
[0241] Through the above steps, the insulating layer 31, the transistor 40, and the insulating layer 33 are formed on the resin layer 23. This can be achieved (Figure 9(A)).
[0242] At this stage, the transistor 40 is separated from the fabrication substrate 14 using a method to be described later. By this, a device without a display element can be fabricated. For example, Transistor 4 0 and the transistor 40, a capacitor, a resistor, a wiring, and the like are formed. A semiconductor device can be manufactured.
[0243] Next, an insulating layer 34 is formed on the insulating layer 33 (FIG. 9(A)). Since the layer has a surface on which a display element is to be formed, it preferably functions as a planarizing layer. The insulating layer 34 can be made of an organic insulating film or an inorganic insulating film that can be used for the insulating layer 31. do.
[0244] The insulating layer 34 is formed at a temperature equal to or lower than the heat resistance temperature of the resin layer 23. It is preferable to form the film at a temperature lower than the temperature.
[0245] When an organic insulating film is used for the insulating layer 34, the temperature applied to the resin layer 23 during the formation of the insulating layer 34 is The temperature is preferably from room temperature to 350°C, and more preferably from room temperature to 300°C.
[0246] When an inorganic insulating film is used for the insulating layer 34, the substrate temperature during film formation is preferably from room temperature to 350° C. The heating temperature is preferably from 100°C to 300°C, and more preferably from 100°C to 300°C.
[0247] Next, an opening is formed in the insulating layer 34 and the insulating layer 33 down to the conductive layer 43b.
[0248] Then, the conductive layer 61 is formed. A part of the conductive layer 61 serves as a pixel electrode of the light emitting element 60. The conductive layer 61 is formed by forming a conductive film, forming a resist mask, and then masking the conductive film. The resist mask can be removed after etching.
[0249] The conductive layer 61 is formed at a temperature equal to or lower than the heat resistant temperature of the resin layer 23. It is preferable to form the film at a temperature lower than the temperature.
[0250] The substrate temperature during the deposition of the conductive film is preferably from room temperature to 350° C., and more preferably from room temperature to 300° C. is more preferred.
[0251] Next, the insulating layer 35 is formed to cover the end of the conductive layer 61. An organic insulating film or an inorganic insulating film that can be used can be used.
[0252] The insulating layer 35 is formed at a temperature equal to or lower than the heat resistance temperature of the resin layer 23. It is preferable to form the film at a temperature lower than the temperature.
[0253] When an organic insulating film is used for the insulating layer 35, the temperature applied to the resin layer 23 during the formation of the insulating layer 35 is The temperature is preferably from room temperature to 350°C, and more preferably from room temperature to 300°C.
[0254] When an inorganic insulating film is used for the insulating layer 35, the substrate temperature during film formation is preferably from room temperature to 350° C. The heating temperature is preferably from 100°C to 300°C, and more preferably from 100°C to 300°C.
[0255] Next, the EL layer 62 and the conductive layer 63 are formed. It functions as a common electrode.
[0256] The EL layer 62 can be formed by a method such as a vapor deposition method, a coating method, a printing method, or a discharging method. When the L layer 62 is made for each pixel, a deposition method using a shadow mask such as a metal mask is used. The EL layer 62 can be formed for each pixel by a method such as a laser beam splitter or an ink jet method. If this is not possible, a deposition method that does not use a metal mask can be used.
[0257] The EL layer 62 may be made of either a low molecular weight compound or a high molecular weight compound. The compound may be included.
[0258] The conductive layer 63 can be formed by vapor deposition, sputtering, or the like.
[0259] The conductive layer 63 is formed at a temperature equal to or lower than the heat resistance temperature of the resin layer 23 and equal to or lower than the heat resistance temperature of the EL layer 62. In addition, it is preferable to form the insulating film at a temperature lower than the temperature of the heat treatment.
[0260] In this manner, the light emitting element 60 can be formed (FIG. 9(A)). The conductive layer 61, a part of which functions as a pixel electrode, the EL layer 62, and a part of which functions as a common electrode are provided. It has a structure in which functional conductive layers 63 are laminated.
[0261] Here, an example of fabricating a top-emission type light-emitting element as the light-emitting element 60 is shown. However, one embodiment of the present invention is not limited thereto.
[0262] The light-emitting elements are top emission type, bottom emission type, and dual emission type. For the electrode from which light is extracted, a conductive film that transmits visible light is used. In addition, it is preferable to use a conductive film that reflects visible light for the electrode on the side from which light is not extracted. .
[0263] Next, an insulating layer 74 is formed to cover the conductive layer 63 (FIG. 9(A)). The light emitting element 60 functions as a protective layer that prevents impurities such as water from diffusing into the light emitting element 60. The conductive layer 63 is sealed by the insulating layer 74. After the conductive layer 63 is formed, the insulating layer 74 is sealed by the insulating layer 74 without exposing it to the air. It is preferred to form a border layer 74 .
[0264] The insulating layer 74 is formed at a temperature equal to or lower than the heat resistance temperature of the resin layer 23 and the heat resistance temperature of the light emitting element 60. The insulating layer 74 is preferably formed at a temperature lower than the temperature of the heat treatment.
[0265] The insulating layer 74 is, for example, an inorganic insulating material having a high barrier property that can be used for the insulating layer 31 described above. It is preferable that the insulating film is formed by laminating an inorganic insulating film and an organic insulating film. It's fine.
[0266] The insulating layer 74 can be formed by using an ALD method, a sputtering method, or the like. The ALD method is preferable because it allows low-temperature film formation. 74 has good coverage, which is preferable.
[0267] Next, a protective layer 75 is formed on the insulating layer 74 (FIG. 9(A)). As shown in (D), an adhesive layer 75b and a substrate 75a may be used.
[0268] Next, the laser light 55 is irradiated (FIG. 9(B1)). The laser light 55 is, for example, ) is a linear laser beam that scans from left to right, and its long axis is along the scanning direction. In the laser device, the substrate 14 is The laminate is placed so that the laminate is on the side of the substrate 14. The light 55 is irradiated.
[0269] For the laser light irradiation step, the description of the peeling method can be referred to.
[0270] In addition, when forming multiple display devices from one production substrate (multiple panels), one resin layer A plurality of display devices can be formed by using the resin layer 23. Alternatively, a plurality of display devices can be formed by using the resin layer 23. In this case, the resin layer 23 may be formed for each display device. This is an example having a resin layer 23. Figures 9(B3) and (B4) show a case where four resin layers 23 are formed on a fabrication substrate. This is an example that has
[0271] Laser equipment can be difficult or expensive to process large substrates. Therefore, depending on the size of the substrate, the substrate may be divided as shown in FIG. 9(B4). After that, each of the cut fabrication substrates may be irradiated with laser light.
[0272] Next, starting points for separation are formed in the resin layer 23 (FIGS. 10(A) to (C)).
[0273] For example, a sharp tool such as a blade may be inserted from the protective layer 75 side to the inside of the end of the resin layer 23. Insert 65 and make cuts 64 in a frame shape.
[0274] Alternatively, the resin layer 23 may be irradiated with laser light in a frame shape.
[0275] As described above, multiple display devices can be formed using one resin layer 23 by multiple panel cutting. For example, multiple display devices can be arranged inside the gap 64 in FIG. This makes it possible to separate a plurality of display devices from the formation substrate at once.
[0276] Alternatively, a plurality of resin layers 23 may be used, with each resin layer 23 being created for each display device. FIG. 10(C) shows an example in which four resin layers 23 are formed on a fabricated substrate. 3 By making frame-shaped cuts 64 in each, each display device is produced at a different time. It can be separated from the substrate.
[0277] In the manufacturing method example 1, the resin layer 23 is formed on the metal oxide layer 20 at a portion where the resin layer 23 is in contact with the insulating layer 31. The adhesion (bonding) between the metal oxide layer 20 and the insulating layer 31 is determined by the metal oxide. The adhesiveness (bonding) between the metal oxide layer 20 and the resin layer 23 is higher than that between the metal oxide layer 20 and the resin layer 23. This can prevent the oxide layer 20 from peeling off unintentionally. In this way, the metal oxide layer 20 and the resin layer 23 can be separated at a desired timing. Therefore, the timing of separation can be controlled and the force required for separation is small. The yield of the separation process and the manufacturing process of the display device can be increased.
[0278] Next, the metal oxide layer 20 and the resin layer 23 are separated (FIG. 11(A)).
[0279] Then, a substrate 29 is attached to the exposed resin layer 23 using an adhesive layer 28 (FIG. 11 (B)).
[0280] The substrate 29 can function as a support substrate for the display device. It is preferable to use a resin film, and it is particularly preferable to use a resin film. In addition, display devices using film substrates can be made lighter and thinner than glass or metal. In addition, the display device can be made more flexible. do.
[0281] By using the peeling method of the present embodiment, the transistor 40 and The light emitting element 60 and the like can be peeled off from the fabrication substrate 14 and transferred to the substrate 29 .
[0282] The adhesive layer 28 may be made of any of the materials that can be used for the adhesive layer 75b. The material 29 can be any material that can be used for the substrate 75a.
[0283] In the example of the manufacturing method 1, the metal oxide layer 20 and the resin layer 23 are laminated and irradiated with light. This can reduce the adhesion or bonding strength between the metal oxide layer 20 and the resin layer 23. Therefore, the preparation substrate 14 and the resin layer 23 can be easily separated.
[0284] [Display device configuration example 1] FIG. 12(A) is a top view of the display device 10A. 1 is a cross-sectional view of a display unit 381 of the display device 10A and an example of a cross-sectional view of a connection portion with an FPC 372. do.
[0285] The display device 10A can be manufactured using the above-mentioned manufacturing method example 1. It is possible to hold the bent state and to be repeatedly bent.
[0286] The display device 10A has a protective layer 75 and a substrate 29. The protective layer 75 side is the display surface of the display device. The display device 10A includes a display unit 381 and a drive circuit unit 382. FPC372 is attached to 0A.
[0287] The conductive layer 43c and the FPC 372 are electrically connected via the connector 76 (FIG. 12). (B, (C)). The conductive layer 43c is made of the same material as the source and drain of the transistor. The insulating layer 14 and the insulating layer 15 can be formed in the same process.
[0288] The connector 76 may be made of various anisotropic conductive films (ACFs). Conductive Film) and Anisotropic Conductive Paste (ACP) Conductive Paste) can be used.
[0289] The display device shown in FIG. 12C does not include the transistor 40 but includes a transistor 49. 12(B) in that a colored layer 97 is provided on the insulating layer 33. When a bottom emission type light emitting element 60 is used, the light emitting element 60 is attached closer to the substrate 29 than the light emitting element 60. In the above-mentioned manufacturing method example 1, the resin layer 23 has a visible light transmittance of Therefore, the light from the light emitting element 60 can be taken through the resin layer 23. This makes it possible to achieve high display quality even on display devices that emit large amounts of light.
[0290] The transistor 49 shown in FIG. 12C has the same structure as the transistor 40 shown in FIG. In addition, it has a conductive layer 45 which functions as a gate.
[0291] The transistor 49 has a structure in which a semiconductor layer in which a channel is formed is sandwiched between two gates. By adopting such a configuration, the threshold voltage of the transistor can be controlled. By connecting the two gates together and applying the same signal to them, Such transistors have field effect transistors compared to other transistors. This allows for increased mobility and increased on-current. Furthermore, the area occupied by the circuit portion can be reduced. By using transistors with a large on-state current, it is possible to enlarge the display device, Even if the number of wirings increases when the resolution is increased, the signal delay in each wiring can be reduced. This makes it possible to suppress display unevenness.
[0292] Alternatively, a potential for controlling the threshold voltage is applied to one of the two gates, and a drive potential is applied to the other. By applying a potential for the gate, the threshold voltage of the transistor can be controlled.
[0293] [Production method example 2] First, in the same manner as in the above-mentioned peeling method, the metal oxide layer 20 to the insulating layer 31 are removed from the substrate 14. (FIG. 13(A)).
[0294] Next, a transistor 80 is formed on the insulating layer 31 (FIG. 13(B)).
[0295] Here, transistor 80 is a transistor having a metal oxide layer 83 and two gates. This shows the case where a printer is made.
[0296] The transistor 80 is formed at a temperature equal to or lower than the heat-resistant temperature of the resin layer 23. Formation at low temperatures is preferred.
[0297] Specifically, first, the conductive layer 81 is formed on the insulating layer 31. The conductive layer 81 is formed by depositing a conductive film. Then, a resist mask is formed, the conductive film is etched, and the resist mask is removed. It can be formed by removing
[0298] Next, the insulating layer 82 is formed. The insulating layer 82 is made of an inorganic insulating material that can be used for the insulating layer 31. The velum can be used.
[0299] Next, a metal oxide layer 83 is formed. The metal oxide layer 83 is formed after forming the metal oxide film. A resist mask is formed, the metal oxide film is etched, and then the resist mask is removed. The metal oxide layer 83 can be formed by removing the metal oxide that can be used for the metal oxide layer 44. Materials can be used.
[0300] Next, the insulating layer 84 and the conductive layer 85 are formed. The insulating layer 84 is used for the insulating layer 31. The insulating layer 84 and the conductive layer 85 are made of an insulating material that is capable of forming the insulating layer 84. After forming a film and a conductive film that will become the conductive layer 85, a resist mask is formed, and the insulating film and The conductive film is then etched, and the resist mask is then removed.
[0301] Next, the insulating layer 33 is formed to cover the metal oxide layer 83, the insulating layer 84, and the conductive layer 85. The edge layer 33 can be formed in a similar manner to the insulating layer 31 .
[0302] The insulating layer 33 preferably contains hydrogen. The hydrogen contained in the insulating layer 33 The metal oxide diffuses into the adjacent metal oxide layer 83, causing a part of the metal oxide layer 83 to have a low resistance. Since a portion of layer 83 functions as a low resistance region, the on-current of transistor 80 is increased and The field effect mobility can be improved.
[0303] Next, an opening is formed in the insulating layer 33 down to the metal oxide layer 83 .
[0304] Subsequently, the conductive layer 86a and the conductive layer 86b are formed. After forming a conductive film, a resist mask is formed, the conductive film is etched, and then a resist is formed. The conductive layer 86a and the conductive layer 86b can be formed by removing the mask. , and is electrically connected to the metal oxide layer 83 through the opening in the insulating layer 33 .
[0305] In the above manner, the transistor 80 can be manufactured (FIG. 13B). In this case, a part of the conductive layer 81 functions as a gate, and a part of the insulating layer 84 functions as a gate insulating layer. A portion of the insulating layer 82 serves as a gate insulating layer, and a portion of the conductive layer 85 serves as a gate The metal oxide layer 83 has a channel region and a low resistance region. The low resistance region overlaps with the conductive layer 85 via the insulating layer 84. The low resistance region is connected to the conductive layer 86a. and a portion connected to conductive layer 86b.
[0306] Next, the insulating layer 34 to the light emitting element 60 are formed on the insulating layer 33 (FIG. 13(C)). For these steps, see Preparation Method 1.
[0307] In addition, steps in Fig. 14(A) to (C) are carried out independently of steps in Fig. 13(A) to (C). First, in the same manner as in the process of forming the metal oxide layer 20 on the preparation substrate 14, A metal oxide layer 92 is then formed on the metal oxide layer 20 (FIG. 14(A)). Similar to the process of forming 23, a first layer is formed on the metal oxide layer 92 and then heat-treated. In this way, a resin layer 93 is formed (FIG. 14(B)). Then, an insulating layer 31 is formed on the resin layer 23. In the same manner as in the forming process, an insulating layer 95 is formed on the resin layer 93 so as to cover the end portion of the resin layer 93. (Figure 14(B)).
[0308] Next, a colored layer 97 and a light-shielding layer 98 are formed on the insulating layer 95 (FIG. 14(C)).
[0309] A color filter or the like can be used as the colored layer 97. The colored layer 97 is Place it so that it overlaps with the display area of the
[0310] A black matrix or the like can be used as the light-shielding layer 98. The light-shielding layer 98 is an insulating layer. Place it so that it overlaps with 35.
[0311] Next, the surface of the fabrication substrate 14 on which the transistors 80 and the like are formed and the resin layer of the fabrication substrate 91 are The surface on which 93 and the like are formed is attached using an adhesive layer 99 (FIG. 14(D)).
[0312] Next, the laser beam 55 is irradiated (FIG. 15). For example, in FIG. , a linear laser beam scanned from left to right, the long axis of which is the scanning direction and the input The laser device is set so that the substrate 14 is on the upper side. The laminate is placed on the substrate 14. The laminate is irradiated with laser light 55 from above the laminate (the substrate 14). Be shot.
[0313] Either the fabrication substrate 14 or the fabrication substrate 91 may be separated first. An example in which the preparation substrate 14 is separated beforehand will be described.
[0314] The laser light 55 is incident on the interface between the metal oxide layer 20 and the resin layer 23 or on the interface between the metal oxide layer 20 and the resin layer 23 via the production substrate 14. It is preferable that the laser beam 55 is irradiated to the vicinity of the metal oxide layer 20. Alternatively, irradiation may be performed into the resin layer 23 .
[0315] The metal oxide layer 20 absorbs the laser light 55. The resin layer 23 absorbs the laser light 55. Good too.
[0316] The adhesion or bonding between the metal oxide layer 20 and the resin layer 23 is reduced by the irradiation of the laser light 55. Irradiation with the laser light 55 may weaken the resin layer 23.
[0317] Most of the laser light 55 is incident on the fabrication substrate, the metal oxide layer, and the The laser beam 55 is absorbed by the three resin layers. Only one of the adhesion between the layer 20 and the resin layer 23 or the adhesion between the metal oxide layer 92 and the resin layer 93 is required. The timing of separation can be changed between the production substrate 14 and the production substrate 91. Therefore, the preparation substrate 14 and the preparation substrate 91 can be separated in separate steps. This makes it possible to increase the yield in the separation process and the manufacturing process of the display device.
[0318] For the laser light irradiation step, the description of the peeling method can be referred to.
[0319] Next, it is preferable to form a separation starting point in the resin layer 23. For example, A sharp blade or the like is inserted between the substrates 91 to bond the substrate 14 and the substrate 91 to the adhesive layer 99. Therefore, it is preferable to separate the bonded parts.
[0320] In the second example of the manufacturing method, the metal oxide layer 20 is provided with a portion where the resin layer 23 is in contact and a portion where the insulating layer 31 is in contact. The adhesion (bonding) between the metal oxide layer 20 and the insulating layer 31 is determined by the metal oxide. The adhesiveness (bonding) between the metal oxide layer 20 and the resin layer 23 is higher than that between the metal oxide layer 20 and the resin layer 23. It is possible to suppress unintentional peeling off from the oxide layer 20. Similarly, on the metal oxide layer 92, The metal oxide layer 92 has a portion that is in contact with the resin layer 93 and a portion that is in contact with the insulating layer 95. The adhesiveness (bonding) between the metal oxide layer 92 and the insulating layer 95 is determined by the adhesiveness (bonding) between the metal oxide layer 92 and the resin layer 93. Therefore, the resin layer 93 is prevented from being unintentionally peeled off from the metal oxide layer 92. It can be suppressed.
[0321] Next, the manufacturing substrate 14 and the transistor 80 are separated (FIG. 16(A)). In the adhesive layer 99, separation occurs in the portion outside the end of the resin layer 23 (adhesive layer 99) is a non-limiting example of the adhesive layer 99 and the insulating layer 9 5 or the insulating layer 33 (also called interfacial failure or adhesive failure). ) in some cases.
[0322] In the example of the manufacturing method 2, the metal oxide layer 20 and the resin layer 23 are laminated and irradiated with light. This can reduce the adhesion or bonding strength between the metal oxide layer 20 and the resin layer 23. Therefore, the preparation substrate 14 and the resin layer 23 can be easily separated.
[0323] Next, the resin layer 23 exposed by being separated from the fabricated substrate 14 and the substrate 29 are bonded to the adhesive layer 2 8 is used to attach the display device (FIG. 16(B)). The substrate 29 functions as a support substrate for the display device. It is possible.
[0324] Next, the laser beam 55 is irradiated (FIG. 17). For example, in FIG. , a linear laser beam scanned from left to right, the long axis of which is the scanning direction and the input The laser device is set so that the substrate 91 is on the upper side. The laminate is placed on the substrate 91. The laminate is irradiated with laser light 55 from above the laminate (substrate 91). Be shot.
[0325] The laser light 55 is incident on the interface between the metal oxide layer 92 and the resin layer 93 or on the interface between the metal oxide layer 92 and the resin layer 93 via the fabrication substrate 91. It is preferable that the laser beam 55 is irradiated to the vicinity of the metal oxide layer 92. Alternatively, irradiation may be performed into the resin layer 93 .
[0326] The metal oxide layer 92 absorbs the laser light 55. The resin layer 93 absorbs the laser light 55. Good too.
[0327] The adhesion or bonding between the metal oxide layer 92 and the resin layer 93 is reduced by the irradiation of the laser light 55. Irradiation with the laser light 55 may weaken the resin layer 93.
[0328] For the laser light irradiation step, the description of the peeling method can be referred to.
[0329] Next, starting points for separation are formed in the resin layer 93 (FIG. 18(A)).
[0330] In FIG. 18A, a sharp object such as a blade is inserted from the substrate 29 side to the inside of the end of the resin layer 93. The tool 65 is inserted into the substrate 29 to make a frame-shaped cut. be.
[0331] Alternatively, in the same manner as when the starting point of separation is formed in the resin layer 23, the resin layer 9 3 may be irradiated with laser light in a frame shape.
[0332] By forming the starting point of separation, the fabricated substrate 91 and the resin layer 93 can be separated at a desired timing. Therefore, the timing of separation can be controlled and the force required for separation can be controlled. This makes it possible to increase the yield of the separation process and the manufacturing process of the display device. do.
[0333] Next, the manufacturing substrate 91 and the transistor 80 are separated (FIG. 18(B)). 9 shows an example in which an inner portion of the substrate 91 is separated from the cut portion.
[0334] In the example of the manufacturing method 2, a metal oxide layer 92 and a resin layer 93 are laminated and irradiated with light. This can reduce the adhesion or bonding strength between the metal oxide layer 92 and the resin layer 93. Therefore, the preparation substrate 91 and the resin layer 93 can be easily separated.
[0335] Next, the resin layer 93 exposed by being separated from the fabricated substrate 91 and the substrate 22 are bonded to the adhesive layer 1. 3 is used to attach the display device (FIG. 19(A)). The substrate 22 functions as a support substrate for the display device. It is possible.
[0336] In FIG. 19A, the light emitted from the light emitting element 60 is transmitted through the colored layer 97, the insulating layer 95, and the resin layer 9 The visible light is then taken out of the display device through the resin layer 93. In one embodiment of the present invention, the thickness of the resin layer 93 can be made thin. Therefore, the visible light transmittance of the resin layer 93 is increased, and the decrease in the light extraction efficiency of the light emitting element 60 is prevented. It can be suppressed.
[0337] In one embodiment of the present invention, a light emitting layer is formed on or near the interface between the metal oxide layer 92 and the resin layer 93. The metal oxide layer 92 absorbs a part of the light. Therefore, the light absorptance of the resin layer 93 is Even if the temperature is low, the metal oxide layer 92 and the resin layer 93 can be easily separated. The resin layer 93 can be made of a material having a high transmittance for visible light. The decrease in the light extraction efficiency of 0 can be suppressed.
[0338] The resin layer 93 may be removed. This further increases the light extraction efficiency of the light emitting element 60. In FIG. 19(B), the resin layer 93 is removed, and the insulating layer 9 is bonded to the insulating layer 9 by using the adhesive layer 13. 5 shows an example in which a substrate 22 is bonded to the substrate 22.
[0339] For the adhesive layer 13, the materials that can be used for the adhesive layer 75b can be used.
[0340] The substrate 22 may be made of any of the materials that can be used for the substrate 75a.
[0341] In the manufacturing method example 2, a display device is manufactured by performing the peeling method of one embodiment of the present invention twice. In one embodiment of the present invention, all of the functional elements constituting the display device are formed on a substrate. Even in the case of manufacturing a high-definition display device, a flexible substrate is required to have a high position. No high alignment accuracy is required. Therefore, flexible substrates can be easily attached. do.
[0342] [Variations] In the second example of the manufacturing method (FIG. 14D), the adhesive layer 99 is formed between the metal oxide layer 20 and the insulating layer 31. and the area where the metal oxide layer 92 and the insulating layer 95 are in contact with each other. The cases where it can be provided are shown below.
[0343] The adhesion (bonding) between the metal oxide layer 20 and the insulating layer 31, and the adhesion between the metal oxide layer 92 and the insulating layer 95 The adhesion (adhesion) of the metal oxide layer 20 and the resin layer 23 is, respectively, the adhesion (adhesion) of the metal oxide layer 20 and the resin layer 23. The adhesion (bonding) between the metal oxide layer 92 and the resin layer 93 is also higher.
[0344] Peeling occurs at the interface between the metal oxide layer 20 and the insulating layer 31 or at the interface between the metal oxide layer 92 and the insulating layer 95 If this is done, peeling yield may decrease, such as peeling failure. After forming a frame-shaped separation starting point in the fat layer, only the part overlapping with the resin layer is separated from the fabricated substrate. The procedure is preferable.
[0345] On the other hand, as shown in FIGS. 20(A) and 20(B), the adhesive layer 99 is formed between the metal oxide layer 20 and the insulating layer 3 The contact area between the metal oxide layer 92 and the insulating layer 95 is not overlapped with the contact area between the metal oxide layer 92 and the insulating layer 95. This can reduce the occurrence of peeling defects.
[0346] For example, if an adhesive with low fluidity or an adhesive sheet is used for the adhesive layer 99, the adhesive layer 9 It is easy to form the insulating layer 9 in an island shape (FIG. 20(A)).
[0347] Alternatively, a frame-shaped partition 96 is formed, and an adhesive layer 99 is filled and hardened inside the partition 96. (FIG. 20(B)).
[0348] When the partition 96 is used as a component of a display device, the partition 96 is made of a hardened resin. In this case, it is preferable that the partition wall 96 is also in contact with the metal oxide layer 20 and the insulating layer 31. It is preferable that the insulating layer 95 and the metal oxide layer 92 are not overlapped with each other. stomach.
[0349] When the partition 96 is not used as a component of a display device, the partition 96 may be provided with an uncured or semi-cured In this case, the partition wall 96 is preferably made of the metal oxide layer 20 and the insulating layer 31. and one of the portions where the metal oxide layer 92 and the insulating layer 95 are in contact with each other, or You can also stack both.
[0350] In this embodiment, the partition wall 96 is made of an uncured resin, and the partition wall 96 is insulated from the metal oxide layer 20. The portion where the metal oxide layer 92 and the insulating layer 95 are in contact with each other. Here is an example of no overlap.
[0351] [Display device configuration example 2] FIG. 21(A) is a top view of the display device 10B. FIG. 21(B) is a front view of the display device 10B. 3 is a cross-sectional view of a display portion 381 and a cross-sectional view of a connection portion with an FPC 372.
[0352] The display device 10B can be manufactured using the above-mentioned manufacturing method example 2. It is possible to hold the bent state and to be repeatedly bent.
[0353] The display device 10B has a substrate 22 and a substrate 29. The substrate 22 side is the display side of the display device 10B. The display device 10B includes a display unit 381 and a drive circuit unit 382. FPC372 is attached to 10B.
[0354] It is preferable to use a film for the substrate 22 and the substrate 29, and in particular, a resin film is used. This allows the display device to be made lighter and thinner. Display devices using plates are less susceptible to breakage than those using glass or metal. The flexibility of the display device can be increased.
[0355] The conductive layer 86c and the FPC 372 are electrically connected via the connector 76 (FIG. 21 (B) The conductive layer 86c is made of the same material and has the same structure as the source and drain of the transistor. It can be formed in a process.
[0356] [Example of laminate manufacturing equipment] Next, an example of a laminate manufacturing apparatus will be described with reference to Fig. 22. Manufacturing of the laminate shown in Fig. 22 The device peels off a layer to be peeled off from a preparation substrate by using the peeling method of this embodiment mode, and separates the layer to be peeled off. The stack manufacturing apparatus shown in FIG. A laminate for a display device or the like can be produced.
[0357] The laminate manufacturing apparatus shown in FIG. 22 includes a laser irradiation unit 610, a substrate reversing unit 630, and a , a plurality of conveying rollers (conveying rollers 643, 644, 645, 646, etc.), a tape reel 6 02, a take-up reel 683, a direction changing roller 604, and a pressure roller 606.
[0358] The laminate 56 that can be processed by the laminate manufacturing apparatus shown in FIG. The laminate 56 has a structure in which the object 56a and the support 56b are laminated. The peeled object 56a has, for example, a resin layer, and the support 56b has, for example, a fabrication substrate. It has a plate.
[0359] The laminate manufacturing apparatus shown in FIG. 22 is a device for manufacturing a laminate 56 by attaching a support 601 to the laminate 56. The object to be peeled 56a is peeled off from the laminate 56 by pulling the support 601. The layer 56 can be automatically separated, shortening the work time and improving the production yield. It can be done.
[0360] The peeled body 56a separated from the support 56b is attached to the support 671 using an adhesive. As a result, the support 601, the object to be peeled 56a, and the support 671 are laminated in this order. Thus, a laminate 59 can be produced.
[0361] The plurality of conveying rollers can convey the laminate 56. The mechanism is not limited to conveying rollers, but a belt conveyor, a conveying robot, or the like may also be used. Furthermore, the laminate 56 may be placed on a stage on a transport mechanism.
[0362] The conveying rollers 643, 644, 645, and 646 are each This is one of the conveying rollers arranged at a predetermined interval and conveys the laminate 56 and the peeled object 56 a, or in the sending direction of the support 56b (the clockwise direction indicated by the solid arrow). The multiple conveying rollers arranged are each rotated by a drive unit (motor, etc.) not shown. Be moved.
[0363] The laser irradiation unit 610 is a unit that irradiates the laminate 56 with a laser. For example, an excimer laser that outputs ultraviolet light with a wavelength of 308 nm can be used. Alternatively, a high-pressure mercury lamp or a UV-LED may be used.
[0364] As shown in FIG. 22, the laminate 56 is irradiated with laser in a state where the support 56b is located on the upper side. Transported to unit 610.
[0365] Excimer lasers are high-power pulsed lasers, and the beam is shaped into a linear form by an optical system. By moving the substrate at the irradiation position of the linear laser beam, the entire substrate can be The linear beam can be irradiated to a portion of the substrate to be used. If the length is equal to or greater than the side, the entire substrate can be irradiated with laser light by simply moving the substrate in one direction. The oscillation frequency of the pulse laser is preferably 1 Hz or more and 300 Hz or less. , and around 60 Hz is more preferable.
[0366] Excimer laser devices include devices equipped with one laser oscillator as well as devices equipped with two or more laser oscillators. In the case of an apparatus equipped with a plurality of laser oscillators, The laser beams output from each laser oscillator are synchronized and combined by an optical system. By combining the two, it is possible to obtain a laser beam with a high energy density. In applications with this shape, 3.5th generation (600mm x 720mm) and above, 6th generation (1 500mm x 1850mm) or more, 7th generation (1870mm x 2200mm) or more, Processing of glass substrates of 8th generation (2160mm x 2460mm) or larger is required. In addition, in a device equipped with multiple laser oscillators, each laser oscillator can emit a The output laser beams complement each other to eliminate output variations, so the intensity variation for each pulse is The number of oscillators is reduced, and high yield processing can be achieved. Alternatively, an excimer laser device such as the above may be used.
[0367] FIG. 23(A) shows an example of a laser irradiation unit 610 using an excimer laser. Laser light 610a, 61b is output from an excimer laser device 660 having a laser oscillator. 0b are synthesized by the optical system 635. The laser light expanded horizontally by the optical system 635 is The light 610c enters the lens 680 via the mirror 650. The laser beam 610d is reduced in size compared to the laser beam 610c. The processed region 640 of the laminate 56 is irradiated through the support 56b (for example, a glass substrate). In the following, the portion of the laser beam 610d that is irradiated onto the processing region 640 will be described. The portion is referred to as a linear beam 610e.
[0368] Although an example having two laser oscillators is shown here, a laser having one laser oscillator may also be used. This can simplify the device. This can increase the intensity of the linear beam 610e.
[0369] Then, the laminate 56 is moved in the direction of the arrow in the figure by the conveying rollers 644, so that the processing Area 640 can be irradiated with linear beam 610e.
[0370] As shown in FIG. 23(A), the laminate 56 is conveyed at a constant speed by conveying rollers 644. By irradiating the linear beam 610e, the process time can be shortened. The laminate 56 is placed on a stage that is movable in at least one direction, and the stage is moved. However, the linear beam 610e may be irradiated while the stage is being used. A stage that can move in the lateral and height directions relative to the row direction is used to generate a linear beam 610e It is preferable to have a configuration in which the position and depth of the focus can be adjusted. Although the configuration in which the linear beam 610e is irradiated by moving the laminate 56 has been illustrated, For example, the laminate 56 is fixed, and the excimer laser device 660 or the like is moved. The linear beam 610e may be irradiated onto the laminate 56 by moving the optical axis.
[0371] In FIG. 23A, the processing area 640 irradiated with the linear beam 610e is located at the edge of the laminate 56. In this example, the area outside the processing area 640 is densely packed. Since the adhesiveness is maintained at a high level, peeling during transportation can be suppressed. The width of the linear beam 610e is equal to or greater than the width of the laminate 56. In this case, the entire stack 56 can be irradiated with the linear beam 610e.
[0372] FIG. 23B shows how the linear beam 610e is irradiated onto the processing region 640 of the laminate 56. The laminate 56 includes a fabrication substrate 58, a first layer 57a, and a second layer 57b. Here, the portion including the preparation substrate 58 and the second layer 57b corresponds to the support 56b, and the portion including the first layer 5 The portion including 7a corresponds to the object to be peeled 56a.
[0373] For example, the first layer 57a corresponds to the resin layer 23, and the second layer 57b corresponds to the metal oxide layer 23. Equivalent to 20.
[0374] The laser light 610d passes through the substrate 58, and the linear beam 610e penetrates the first layer 57a and It is preferable that the linear beam is irradiated to the interface of the second layer 57b or its vicinity. 610e is a focal point located at or near the interface between the first layer 57a and the second layer 57b. It is preferable.
[0375] In addition, the focal point of the linear beam 610e is located at the interface between the first layer 57a and the second layer 57b. As a result, water that may be present at the interface between the first layer 57a and the second layer 57b is evaporated, and the volume of the water is reduced. In this case, the first layer 57a and the second layer 57b may expand suddenly as the volume of the water expands. It is presumed that the peeling occurs at or near the interface with layer 57b.
[0376] In addition, the amorphous silicon film is crystallized by irradiating the amorphous silicon film with laser light. In this technology, a laser beam is focused inside the amorphous silicon film. However, in one embodiment of the present invention, as shown in FIG. The focal point of the light (here, the linear beam 610e) is the first layer 57a, the second layer 57b, and the In this way, one aspect of the present invention is that the focal position of the laser beam is This is different from the technique for crystallizing a rufous silicon film.
[0377] In addition, when the focal depth of the linear beam 610e is sufficiently large (deep), the first layer 57a and the second layer 57b are The first layer 57a and the second layer 57b are not only at or near the interface of the first layer 57a and the second layer 57b, but also in the entire thickness direction of the first layer 57a and the second layer 57b. Through the entire thickness of layer 57b, or through the entire thickness of both first layer 57a and second layer 57b The focus of the linear beam 610e may be located anywhere along the line.
[0378] The excimer laser used has a wavelength of 308 nm or longer. If the wavelength is 308 nm or more, when a glass substrate is used for the support 56b, Even in this case, the laser light necessary for processing can be sufficiently transmitted.
[0379] The substrate reversing unit 630 shown in FIG. 22 is a unit that reverses the top and bottom of the laminate 56. For example, the conveying rollers are provided to sandwich the laminate 56 from above and below, and the conveying rollers are provided with a mechanism for rotating the conveying rollers. The configuration of the substrate reversing unit 630 is not limited to this. The conveying rollers for sandwiching the laminate 56 from above and below may be arranged in a spiral shape, or may be inverted. A configuration having a transfer arm capable of transferring the data may also be used.
[0380] The laminate 56 that has passed through the substrate inversion unit 630 is divided into the peeled objects 56a as shown in FIG. is positioned on the upper side.
[0381] The tape reel 602 can unwind the support 601 in the form of a roll sheet. The speed at which 601 is unwound is preferably variable. For example, the speed can be set relatively slow. This can suppress poor peeling of the laminate or the occurrence of cracks in the peeled members.
[0382] The take-up reel 683 can take up the laminate 59 .
[0383] Tape reel 602 and take-up reel 683 are used to apply tension to support 601. This can be done.
[0384] The support 601 is fed continuously or intermittently. This is preferable because peeling can be performed at a uniform speed and with a uniform force. It is preferable that the peeling proceeds continuously without stopping midway, and the peeling proceeds at a constant speed. It is more preferable to stop the peeling process midway and then start peeling again from that region. Unlike the case where the peeling continues, the area is subject to strain. Changes in the microstructure or characteristics of electronic devices in the area may occur, e.g., display In devices, the effects of this can appear on the display.
[0385] The support 601 is a roll sheet made of organic resin, metal, alloy, glass, or the like. A film may be used.
[0386] In FIG. 22, a support 601 is provided with a device to be manufactured, such as a flexible substrate. The support 601 is a carrier tape. The component may be a member that is not a component of the device to be manufactured, such as a mold.
[0387] The direction of the support 601 can be changed by the direction-changing roller 604. In the example, the direction-changing roller 604 is located between the tape reel 602 and the pressure roller 606. Here is an example.
[0388] The support 601 is pressed against the laminate 56 (to be peeled) by the pressure roller 606 and the conveying roller 645. The adhesive layer 56 is attached to the body 56a.
[0389] In the configuration of FIG. 22, the support 601 comes into contact with the laminate 56 just before it reaches the pressure roller 606. Therefore, it is possible to prevent air bubbles from being mixed between the support 601 and the laminate 56. can be suppressed.
[0390] The pressure roller 606 is rotated by a drive unit (motor or the like) not shown. By rotating 606, a force is applied to the laminate 56 to peel off the object 56a to be peeled off. At this time, it is preferable that a peeling starting point is formed in the laminate 56. The object to be peeled 56a starts to peel from the peeling starting point. 56a and the support 56b.
[0391] The mechanism for peeling the object 56a from the laminate 56 is not limited to the pressing roller 606. (It can also be said that the surface is convex.) For example, a structure having a circle Use cylindrical (including cylindrical, right circular, elliptical, parabolic, etc.) and spherical structures For example, a roller such as a drum roller can be used. An example of a shape is a cylinder with a curved bottom (a cylinder with a perfect circle bottom, or an elliptical bottom). A cylinder with a straight or curved base (such as an elliptical cylinder with a semicircular or semielliptical base) When the shape of the structure is one of these cylinders, the convex surface is This corresponds to the curved surface of the cylinder.
[0392] The material of the structure may be metal, alloy, organic resin, rubber, etc. The structure has a cavity inside. The rubber may have a gap or a cavity. Examples of materials that can be used include neoprene rubber. When rubber is used, static electricity is generated due to friction or peeling. It is preferable to use materials that are not easily damaged or to take measures to prevent static electricity. The pressure roller 606 shown in FIG. 22 is a hollow cylinder 606a made of rubber or organic resin and a circular and a cylinder 606b made of a metal or alloy, located inside the cylinder 606a.
[0393] It is preferable that the rotation speed of the pressure roller 606 is variable. By controlling the above, the yield of peeling can be further increased.
[0394] The pressure roller 606 and the multiple transport rollers are movable in at least one direction (for example, up and down, left and right, or The convex surface of the pressure roller 606 and the support surface of the conveying roller may be movable forward and backward. It is preferable that the distance between the electrodes is variable, since this allows peeling of laminates of various thicknesses.
[0395] There is no particular limitation on the angle at which the pressure roller 606 folds the support 601. 6 shows an example in which the angle at which the roller 606 folds the support 601 is an obtuse angle.
[0396] The laminate manufacturing apparatus shown in FIG. 22 further includes a roller 617. The roller 617 has a convex The support 601 can be fed from the pressure roller 606 to the take-up reel 683 along the surface. Cut.
[0397] Rollers 617 are movable in one or more directions.
[0398] As the axis of the roller 617 moves, the roller 617 applies tension to the support 601. In other words, the roller 617 can be called a tension roller. The support 601 can be pulled in the changed feed direction by the pressure roller 606. do.
[0399] By moving the shaft of the roller 617, the roller 617 moves so that the pressure roller 606 is in contact with the support 601. The folding angle can be controlled.
[0400] The roller 617 can turn the support 601 back and change the feed direction of the support 601. For example, the feed direction of the support 601 may be changed to the horizontal direction. After the support 601 is folded back and the feed direction of the support 601 is changed, the support 601 is wound around the roller 617. The direction-changing rollers 607 located between the take-up reels 683 further change the direction of the support 601. The feed direction may be changed so that the feed direction of the support 601 is horizontal.
[0401] The laminate manufacturing apparatus shown in FIG. 22 further includes guide rollers (guide rollers 631 and 632). , 633, etc.), a take-up reel 613, a liquid supply mechanism 659, a drying mechanism 614, and The device has an ionizer (ionizers 639 and 620).
[0402] The laminate manufacturing device includes a guide roller that guides the support 601 to the take-up reel 683. The guide roller may be a single roller or a plurality of rollers. Like 32, the guide rollers may be capable of applying tension to the support 601.
[0403] A tape 600 (also called a separate film) is attached to at least one surface of a support 601. In this case, the laminate manufacturing device is attached to one surface of the support 601. It is preferable to have a reel onto which the laminated tape 600 can be wound. In FIG. 22, the take-up reel 613 is positioned between the tape reel 602 and the pressure roller 606. Further, the laminate manufacturing device may have a guide roller 634. The guide roller 634 can guide the tape 600 to the take-up reel 613. do.
[0404] The laminate preparation device may have a drying mechanism 614. Since active elements (e.g., transistors and thin film integrated circuits) are sensitive to static electricity, they should be covered with a protective covering before peeling. A liquid is supplied to the interface between the peeling body 56a and the support 56b, or while supplying a liquid to the interface, It is preferable to perform peeling. In addition, the force required for peeling is increased by the presence of liquid in the peeling progress area. The liquid supply mechanism 659 is used to supply liquid to the interface. If the liquid evaporates while still attached to the object to be peeled 56a, water It is preferable to remove the liquid immediately after peeling, as marks may form. Then, the object to be peeled 56a including the functional element is blown, and the remaining part on the object to be peeled 56a is It is preferable to remove the droplets, as this will reduce the occurrence of watermarks. In addition, a carrier plate 609 is provided to prevent the support 601 from bending. Good too.
[0405] While conveying the support 601 in a diagonal direction relative to the horizontal plane, the support 601 is moved downward along the inclination of the support 601. It is preferable to blow air in the direction so that the droplets fall downward.
[0406] The conveying direction of the support 601 may be perpendicular to the horizontal plane. The oblique direction makes the support 601 more stable during transportation, and vibration can be suppressed.
[0407] During the process, at locations where static electricity may be generated, a static eliminator is installed in the laminate manufacturing device. The static electricity remover is not particularly limited, but for example, a corona discharge Ionizers that use an electric current, soft X-rays, ultraviolet rays, or the like can be used.
[0408] For example, an ionizer is provided in the laminate manufacturing device, and air or nitrogen gas is blown from the ionizer. The static electricity is removed by spraying the static electricity onto the object 56a to be peeled off, thereby reducing the effect of static electricity on the functional elements. In particular, the step of bonding two members and the step of separating one member are preferably performed in a single process. In each case, it is preferable to use an ionizer.
[0409] For example, an ionizer 639 is used to generate ions near the interface between the object 56a and the support 56b. The laminate 56 is separated into a peeled body 56a and a support body 56b while removing static electricity. It is preferable to do so.
[0410] The laminate manufacturing apparatus has a substrate loading cassette 641 and a substrate unloading cassette 642. For example, the laminate 56 may be fed to a substrate load cassette 641. The substrate load cassette 641 can supply the laminate 56 to a transport mechanism or the like. In addition, the supports 56 b can be supplied to a substrate unload cassette 642 .
[0411] The tape reel 672 can unwind the support 671 in the form of a roll sheet. The material 671 can be the same as that of the support 601 .
[0412] A tape reel 672 and a take-up reel 683 are used to apply tension to the support 671. This can be done.
[0413] The laminate manufacturing device includes a guide roller 671 that guides the support 671 to a take-up reel 683. 77, 678, 679.
[0414] The direction of feed of the support 671 can be changed by the direction-changing rollers 676 .
[0415] The pressure roller 675 presses the peeled object 56a against the support 671 that is unwound by the tape reel 672. This allows the support 671 and the peeled body 56a to be bonded together while applying pressure. This can prevent air bubbles from getting mixed in between the layers.
[0416] A separation tape 670 may be attached to at least one surface of the support 671. The guide roller 673 can take up the separation tape 670. The tape 670 can be guided to a reel 673 .
[0417] The produced laminate 59 may be wound up or cut into pieces. The take-up reel 683 winds up the laminate 59. In addition, a guide roller for guiding the laminate 59 to the take-up reel 683 may be provided.
[0418] In the laminate manufacturing apparatus shown in FIG. 22, a pressing roller 606 is used to press the laminate 56 against the target material. The body 56a is peeled off, and the peeled body 56a is transferred to the support 671 using a pressure roller 675. It is possible.
[0419] As described above, in the peeling method of the present embodiment, a metal oxide layer and a resin layer are formed on a fabricated substrate. By laminating the resin layer and irradiating the resin layer with light, the peelability of the resin layer with respect to the metal oxide layer can be controlled. In addition, by providing a portion on the metal oxide layer where the resin layer contacts and a portion on the metal oxide layer where the insulating layer contacts, The resin layer can be peeled off from the substrate at a desired timing. By using this type of peeling method, display devices and the like can be manufactured with high yield.
[0420] This embodiment mode can be appropriately combined with other embodiment modes. In the case where a plurality of configuration examples are shown in one embodiment, the configuration examples may be appropriately combined. It is possible to do this.
[0421] (Embodiment 2) In this embodiment, a manufacturing method of a display device according to one embodiment of the present invention will be described with reference to FIGS. He explains.
[0422] In this embodiment, a low-temperature polysilicon (LTPS) is used for the channel formation region of the transistor. The case where the above formula is used will be described.
[0423] When LTPS is used, the resin layer is preferably formed using a material having high heat resistance. Furthermore, it is preferable that the resin layer is formed as a thick film. This allows high-temperature processing. Moreover, damage during the laser crystallization process can be reduced.
[0424] First, a metal oxide layer 20 is formed on a substrate 14 (FIG. 24(A)). The material and forming method of 20 can be referred to in embodiment 1.
[0425] Next, a first layer 24 is formed on the metal oxide layer 20 (FIG. 24(B)).
[0426] The material and the method of forming the first layer 24 can be referred to in the first embodiment. It is preferable that the material of the first layer 24 used in this embodiment has sufficiently high heat resistance.
[0427] Next, the first layer 24 having a desired shape is subjected to a heat treatment to form the resin layer 23. (FIG. 24(C)). Here, island-shaped resin layers 23 are formed.
[0428] The conditions of the heat treatment can be referred to in Embodiment Mode 1.
[0429] In this embodiment, a highly heat-resistant material is used for the material of the first layer 24. A resin layer 23 can be formed.
[0430] In this embodiment, a material with high heat resistance is used for the material of the first layer 24. Heat treatment can be performed at a temperature higher than the heating temperature shown in . For example, The temperature is preferably 400° C. or higher and 600° C. or lower, and more preferably 450° C. or higher and 550° C. or lower. stomach.
[0431] The thickness of the resin layer 23 is preferably 10 μm or more and 200 μm or less. It is more preferable that the thickness is 100 μm or less, and further preferably that the thickness is 10 μm or more and 50 μm or less. It is preferable that the resin layer 23 is sufficiently thick to reduce damage during the laser crystallization process. In addition, the rigidity of the display device can be increased.
[0432] The 5% weight loss temperature of the resin layer 23 is preferably 400° C. or higher and 600° C. or lower, and more preferably 450° C. or higher. The temperature is more preferably 600°C or lower, and even more preferably 500°C or higher and 600°C or lower.
[0433] Next, an insulating layer 31 is formed on the fabrication substrate 14 and the resin layer 23 (FIG. 24(D)).
[0434] The insulating layer 31 is formed at a temperature equal to or lower than the heat-resistant temperature of the resin layer 23. It is preferable to form the film at a temperature lower than the temperature.
[0435] The insulating layer 31 prevents impurities contained in the resin layer 23 from being transferred to transistors and display elements to be formed later. For example, the insulating layer 31 can be a resin layer. When the resin layer 23 is heated, moisture contained in the resin layer 23 diffuses into the transistors and display elements. It is preferable to prevent this from happening, and therefore it is preferable that the insulating layer 31 has high barrier properties.
[0436] For the insulating layer 31, the materials exemplified in the first embodiment can be used.
[0437] Next, a transistor 140 is formed on the insulating layer 31 (FIG. 24(E), FIG. 25(A) to FIG. 25(B)). Figure 25(E)).
[0438] Here, the transistor 140 is a top gate transistor having an LTPS channel formation region. This shows the case of fabricating a transistor having a gate structure.
[0439] First, a semiconductor film is formed on the insulating layer 31 by using a sputtering method, a CVD method, or the like. In this embodiment, a plasma CVD apparatus is used to form an amorphous silicon film having a thickness of 50 nm. A silicon film 161 is formed.
[0440] Next, it is preferable to perform a heat treatment on the amorphous silicon film 161. Hydrogen can be desorbed from the amorphous silicon film 161. It is preferable to heat the amorphous silicon film 161 at a temperature of 550° C. or less. By keeping the amount of hydrogen below 5 atom%, it is possible to increase the production yield in the crystallization process. In addition, when the amount of hydrogen contained in the amorphous silicon film 161 is low, the heat treatment can be omitted. good.
[0441] In this embodiment, since the resin layer 23 has high heat resistance, the amorphous silicon film 161 is heated at a high temperature. This allows the hydrogen in the amorphous silicon film 161 to be sufficiently desorbed and the amorphous silicon film 161 to be bonded. The production yield in the crystallization process can be increased.
[0442] Next, the semiconductor film is crystallized to form a semiconductor film 162 having a crystalline structure (see FIG. 25(A)).
[0443] The semiconductor film can be crystallized by irradiating it with laser light from above. The laser light may be, for example, 193 nm, 248 nm, 308 nm, or 351 nm wavelength. Alternatively, a metal catalyst element may be used to crystallize the semiconductor film. good.
[0444] In this embodiment, the resin layer 23 has high heat resistance and is formed as a thick film. Damage caused during crystallization can be mitigated.
[0445] Next, channel doping may be performed on the semiconductor film 162 having a crystalline structure.
[0446] Next, the semiconductor film 162 having a crystalline structure is processed to form an island-shaped semiconductor film.
[0447] The semiconductor film is processed by either wet etching or dry etching. Either or both can be used.
[0448] Next, an insulating layer 163 and a conductive layer 164 are formed over the insulating layer 31 and the semiconductor film. The insulating layer 163 and the conductive layer 164 may be made of an inorganic insulating material that can be used for the insulating layer 31. The conductive layer 164 is formed by depositing an insulating film that will become the insulating layer 163 and a conductive film that will become the conductive layer 164. A mask is formed, and the insulating film and the conductive film are etched, and then the mask is removed. It can be formed by:
[0449] By adding an impurity element to a part of the semiconductor film, the channel region 162a and the low resistance region 1 62b (which can also be called a source region and a drain region) is formed. Impurity elements are added multiple times. By performing light doping and heavy doping, a channel region 162a and a low resistance region A LDD (Lightly Doped Drain) region may be formed between 162b. The insulating layer 163 and the conductive layer 164, as well as the masks used to form them, are It can function as a mask when doping an impurity element.
[0450] When manufacturing an n-channel transistor, the impurity element is an n-type conductive layer in the semiconductor film. Impurities that give electrical conductivity are used. For example, elements such as P, As, Sb, S, Te, and Se are used. There can be.
[0451] When manufacturing a p-channel transistor, the impurity element is a p-type conductive layer in the semiconductor film. Impurities that impart electrical conductivity are used. For example, elements such as B, Al, and Ga can be used. .
[0452] Next, an insulating layer 165 is formed to cover the semiconductor layer, the insulating layer 163, and the conductive layer 164 (FIG. 2). 5(C)). The insulating layer 165 can be formed in the same manner as the insulating layer 31.
[0453] Next, a heat treatment is performed to activate the impurities added to the semiconductor film. The heat treatment is preferably performed after the insulating layer 165 is formed in order to prevent oxidation of the conductive layer 164. It is.
[0454] In this embodiment, since the resin layer 23 has high heat resistance, the heat treatment for activating the impurities is not required. This can be done at high temperatures, which can improve the transistor characteristics.
[0455] Next, an insulating layer 166 is formed on the insulating layer 165 (FIG. 25(D)). It can be formed in the same manner as the edge layer 31, and in particular, an insulating film containing hydrogen is formed.
[0456] Next, a heat treatment is performed. As a result, hydrogen is removed from the insulating layer 166 into the semiconductor film (especially the carbon nanotube). Hydrogen can be supplied to the semiconductor film (in the panel region 162a) to terminate defects in the semiconductor film with hydrogen. The heat treatment is preferably performed after the insulating layer 166 containing hydrogen is formed. The heat treatment is performed on the amorphous silicon film 161 in order to remove hydrogen. It is also carried out at a low temperature.
[0457] In this embodiment, since the resin layer 23 has high heat resistance, the heat treatment for hydrogenation is performed at a high temperature. This makes it possible to improve the characteristics of the transistor.
[0458] Next, an opening is formed in the insulating layer 165 and the insulating layer 166, reaching the low resistance region 162b of the semiconductor layer. Form.
[0459] Next, the conductive layer 167a and the conductive layer 167b are formed. 7b is a process for forming a conductive film, forming a resist mask, and etching the conductive film. The conductive layer 167a and the conductive layer 167b can be formed by removing the resist mask. are electrically connected to the low resistance region 162b through the openings in the insulating layer 165 and the insulating layer 166, respectively. are connected to the network.
[0460] In the above manner, the transistor 140 can be manufactured (FIG. 25E). In 40, a portion of the conductive layer 164 functions as a gate, and a portion of the insulating layer 163 functions as a gate. The semiconductor layer functions as an insulating layer. The semiconductor layer has a channel region 162a and a low resistance region 162b. The channel region 162a overlaps with the conductive layer 164 via the insulating layer 163. 62b has a portion connected to the conductive layer 167a and a portion connected to the conductive layer 167b. do.
[0461] Next, the insulating layer 34 to the protective layer 75 are formed on the insulating layer 166 (FIG. 26(A)). For these steps, refer to the first embodiment.
[0462] Next, the laser beam 55 is irradiated (FIG. 26(B)). The method of irradiating the laser beam 55 is See form 1.
[0463] Next, starting points for separation are formed in the resin layer 23 (FIG. 26(C)). The method for forming starting points for separation is as follows: Please refer to embodiment 1.
[0464] In this embodiment, the metal oxide layer 20 is provided with a portion where the resin layer 23 is in contact and a portion where the insulating layer 31 is in contact. The adhesion (bonding) between the metal oxide layer 20 and the insulating layer 31 is determined by the metal oxide. The adhesiveness (bonding) between the metal oxide layer 20 and the resin layer 23 is higher than that between the metal oxide layer 20 and the resin layer 23. This can prevent the oxide layer 20 from peeling off unintentionally. In this way, the metal oxide layer 20 and the resin layer 23 can be separated at a desired timing. Therefore, the timing of separation can be controlled and the force required for separation is small. The yield of the separation process and the manufacturing process of the display device can be increased.
[0465] Next, the metal oxide layer 20 and the resin layer 23 are separated (FIG. 27(A)).
[0466] Then, a substrate 29 is attached to the exposed resin layer 23 using an adhesive layer 28 (FIG. 27 (B)).
[0467] The substrate 29 can function as a support substrate for the display device. It is preferable to use a resin film, and it is particularly preferable to use a resin film. In addition, display devices using film substrates can be made lighter and thinner than glass or metal. In addition, the display device can be made more flexible. do.
[0468] As described above, by using a material with high heat resistance and forming a thick resin layer, A display device to which LTPS is applied can be manufactured.
[0469] [Display device configuration example 3] FIG. 28(A) is a top view of the display device 10C. 13 is a cross-sectional view of a display unit 381 of the display device 10C and an example of a cross-sectional view of a connection portion with an FPC 372. do.
[0470] The display device 10C can be held in a bent state and can be repeatedly bent. do.
[0471] The display device 10C has a protective layer 75 and a substrate 29. The protective layer 75 side is the display surface of the display device. The display device 10C includes a display unit 381 and a drive circuit unit 382. FPC372 is attached to 0C.
[0472] The conductive layer 43c and the FPC 372 are electrically connected via the connector 76 (FIG. 28). (B, (C)). The conductive layer 43c is made of the same material as the source and drain of the transistor. The insulating layer 14 and the insulating layer 15 can be formed in the same process.
[0473] The display device shown in FIG. 28(C) does not have the resin layer 23 and the insulating layer 31, but has a resin layer 23a and an insulating layer 31. The laminated structure includes an edge layer 31a, a resin layer 23b, and an insulating layer 31b. By having this, the reliability of the display device can be improved.
[0474] This embodiment mode can be combined with other embodiment modes as appropriate.
[0475] (Embodiment 3) In this embodiment, a display device and an input / output device which can be manufactured by applying one embodiment of the present invention will be described. The device will be described with reference to FIGS.
[0476] The display device of this embodiment has a first display element that reflects visible light and a second display element that emits visible light. and a display element.
[0477] The display device of the present embodiment has a structure in which light reflected by a first display element and light emitted by a second display element are mixed. Either one or both of these functions are capable of displaying images.
[0478] The first display element can be an element that displays by reflecting external light. Since the device does not have a light source (does not use artificial light sources), the power consumption during display is extremely low. It becomes possible to do so.
[0479] The first display element can typically be a reflective liquid crystal element. As a display element, a shutter-type MEMS (Micro Electro Mechanical Systems) anical System) elements, optical interference type MEMS elements, microcapsules method, electrophoresis method, electrowetting method, electronic liquid powder method, etc. Applied elements and the like can be used.
[0480] It is preferable to use a light-emitting element as the second display element. Light has high color reproducibility (wide color gamut) because its brightness and chromaticity are not affected by external light. ), providing high contrast and vivid display.
[0481] The second display element may be, for example, an OLED (Organic Light Emitting Diode), LED(Light Emitting Diode), QLED(Q Self-luminous such as uantum-dot Light Emitting Diode A light emitting element can be used.
[0482] The display device of the present embodiment has a first mode in which an image is displayed using only the first display element, A second mode in which an image is displayed using only the second display element, and a second mode in which an image is displayed using only the first display element and A third mode for displaying an image using a second display element, and these modes are automatically or can be manually switched on and used.
[0483] In the first mode, an image is displayed using the first display element and external light. This is an extremely low power consumption mode because no external light is required. When light is incident (such as in a bright environment), the first display element uses the reflected light to display an image. For example, if the external light is sufficiently strong and is white light or light close to white light, The first mode is suitable for displaying characters. The first mode uses reflected light from outside, providing a display that is gentle on the eyes. This has the effect of reducing eye fatigue.
[0484] In the second mode, an image is displayed using light emitted by the second display element. Extremely vivid (high contrast and high color reproducibility) regardless of brightness or chromaticity of external light. For example, this is useful when the illuminance is extremely low, such as at night or in a dark room. Also, if the surroundings are dark, a bright display may be too bright for the user. To prevent this, it is preferable to display the image with reduced brightness in the second mode. This not only reduces glare, but also reduces power consumption. is a mode suitable for displaying vivid images (still images and moving images).
[0485] In the third mode, both the reflected light from the first display element and the emitted light from the second display element are used. The display is more vivid than the first mode, but less obscuring than the second mode. For example, under indoor lighting or in the morning or evening, when the illuminance is low, This is effective when the chromaticity is relatively low and the chromaticity of the external light is not white.
[0486] By adopting such a configuration, a highly visible and convenient display device can be obtained regardless of the surrounding brightness. Specifically, it is possible to realize a display device that is highly visible and convenient both in outdoor lighting and indoors. This makes it possible to realize this position.
[0487] The third mode can be said to be a mode that uses a hybrid display method.
[0488] The display device and the input / output device of this embodiment are also called a hybrid display. This can be done.
[0489] Hybrid display is a method of displaying images with a single panel that uses both reflected light and self-luminous light to achieve a wide range of colors and tones. is a method of displaying characters and / or images by complementing each other in light intensity. A hybrid display is a display in which multiple display elements are used in the same pixel or subpixel. A method of displaying characters and / or images using light. However, hybrid display is also available. When we look at the hybrid display we are currently working on, we can see that one of the multiple display elements is A pixel or subpixel displayed using a plurality of display elements, and a pixel displayed using two or more of the plurality of display elements Or, the pixel may have a sub-pixel.
[0490] In this specification, the term "a product" refers to a product that satisfies one or more of the above-mentioned expressions. This is called a hybrid display.
[0491] A hybrid display has multiple display elements in the same pixel or subpixel. The display elements may be, for example, reflective elements that reflect light and transparent elements that emit light. The reflective element and the self-luminous element are controlled independently. The hybrid display can utilize both reflected light and self-luminous light in the display area. It has the ability to display characters and / or images using either or both of the above.
[0492] The display device of this embodiment mode includes a first pixel having a first display element and a second pixel having a second display element. The first pixels and the second pixels each have a matrix. It is preferable that the electrodes are arranged in a box shape.
[0493] Each of the first pixel and the second pixel may include one or more sub-pixels. For example, a pixel can have one subpixel (e.g., white (W)), three subpixels (e.g., white (W)), or The configuration (three colors of red (R), green (G), and blue (B), or yellow (Y), shear (C), magenta (M), or a four-subpixel configuration (red ( Four colors: red (R), green (G), blue (B), and white (W), or red (R), green (G), For example, four colors (e.g., blue (B), yellow (Y) and red (C)) can be applied.
[0494] The display device of the present embodiment performs full color display using either the first pixel or the second pixel. Alternatively, the display device of this embodiment mode may have a black and white display in the first pixel. The first pixel displays a first color or a grayscale image, and the second pixel displays a full color image. The black and white or grayscale display using the first pixel can be used to It is suitable for displaying information that does not require color display, such as
[0495] 29 is a schematic perspective view of a display device 300A. The display device 300A includes a substrate 351 and a In FIG. 29, the substrate 361 is shown by a dashed line. do.
[0496] The display device 300A includes a display unit 362, a circuit 364, wiring 365, and the like. 3 shows an example in which an IC (integrated circuit) 373 and an FPC 372 are mounted on a display device 300A. Therefore, the configuration shown in FIG. 29 is a display device having a display device 300A, an IC, and an FPC. It can also be called a display module.
[0497] The circuit 364 can be, for example, a scanning line driver circuit.
[0498] The wiring 365 has a function of supplying signals and power to the display portion 362 and the circuit 364. The signals and power are supplied from the outside via the FPC 372 or from the IC 373 to the wiring 365. is entered.
[0499] In Figure 29, COG (Chip On Glass) or COF (Chip on The following shows an example in which an IC 373 is provided on a substrate 351 by a method such as a film method. 73 can be, for example, an IC having a scanning line driver circuit or a signal line driver circuit. The display device 300A and the display module may be configured without an IC. The IC may be mounted on the FPC using the COF method or the like.
[0500] FIG. 29 shows an enlarged view of a part of the display unit 362. The display unit 362 has a plurality of displays. The electrodes 311b of the element are arranged in a matrix. It has a reflective function and functions as a reflective electrode for the liquid crystal element 180 .
[0501] 29, the electrode 311b has an opening 451. The light emitting element 170 is disposed closer to the substrate 351 than the electrode 311b. The light is emitted to the substrate 361 side through the opening 451 of the electrode 311b. The area of the light emitting region and the area of the opening 451 may be equal. If one of the product and the area of the opening 451 is larger than the other, the margin for misalignment is large. In particular, the area of the opening 451 is preferably larger than the area of the light emitting region of the light emitting element 170. If the opening 451 is small, some of the light from the light emitting element 170 may be reflected by the opening 451. The electrode 311b may block the light and prevent it from reaching the outside. By reducing the light emission, it is possible to prevent the light emitted by the light emitting element 170 from being wasted.
[0502] FIG. 30 shows a part of the area including the FPC 372 and the circuit 3 of the display device 300A shown in FIG. 64 and a part of the area including the display unit 362 are cut away. An example of a surface is shown below.
[0503] The display device 300A shown in FIG. 30 includes a transistor 201 between a substrate 351 and a substrate 361. , transistor 203, transistor 205, transistor 206, liquid crystal element 180, The optical element 170, the insulating layer 220, the colored layer 131, the colored layer 134, etc. are included. The edge layer 220 is bonded via an adhesive layer 141. The substrate 351 and the insulating layer 220 are bonded via an adhesive layer 141. It is attached via 142.
[0504] The substrate 361 is provided with a colored layer 131, a light-shielding layer 132, an insulating layer 121, and a liquid crystal element 180. An electrode 113 that functions as a current-carrying electrode, an alignment film 133b, an insulating layer 117, and the like are provided. The substrate 361 has a polarizing plate 135 on its outer surface. The insulating layer 121 acts as a planarizing layer. The insulating layer 121 can make the surface of the electrode 113 approximately flat. Therefore, the alignment state of the liquid crystal layer 112 can be made uniform. It functions as a spacer to hold the cap. When the insulating layer 117 transmits visible light, Alternatively, the insulating layer 117 may be disposed so as to overlap the display area of the liquid crystal element 180 .
[0505] The liquid crystal element 180 is a reflective liquid crystal element. The liquid crystal element 180 functions as a pixel electrode. The electrode 311a, the liquid crystal layer 112, and the electrode 113 are laminated to form a laminate structure. An electrode 311b that reflects visible light is provided in contact with the substrate 351 side of the electrode 311. b has an opening 451. The electrode 311a and the electrode 113 transmit visible light. An alignment film 133a is provided between the liquid crystal layer 112 and the electrode 311a. An alignment film 133b is provided between them.
[0506] In the liquid crystal element 180, the electrode 311b has a function of reflecting visible light, and the electrode 113 has a function of reflecting visible light. The light incident from the substrate 361 side is polarized by the polarizing plate 135. The light is then transmitted through the electrode 113 and the liquid crystal layer 112, and is reflected by the electrode 311b. 2 and the electrode 113 again and reaches the polarizing plate 135. The orientation of the liquid crystal can be controlled by applying a voltage between the electrodes 113, and the optical modulation of light can be controlled. That is, the intensity of the light emitted through the polarizing plate 135 can be controlled. In addition, the colored layer 131 absorbs light outside a specific wavelength range, so that the light can be extracted. The emitted light is, for example, red light.
[0507] As shown in FIG. 30, the opening 451 is provided with an electrode 311a that transmits visible light. This is preferable. In the region overlapping with the opening 451, the same effect as the other region can be obtained. Since the liquid crystal layer 112 is oriented, alignment defects of the liquid crystal occur at the boundary between these regions, resulting in unintended This can prevent the leakage of bright light.
[0508] In the connection portion 207, the electrode 311b is connected to the transistor 206 via the conductive layer 221b. The transistor 206 is electrically connected to the conductive layer 222a of the liquid crystal element 1. It has the function of controlling the drive of 80.
[0509] A connection portion 252 is provided in a portion of the area where the adhesive layer 141 is provided. 2, a conductive layer obtained by processing the same conductive film as the electrode 311a and one of the electrodes 113 are The portions are electrically connected by the connectors 243. A signal or a voltage is input to the electrode 113 from the FPC 372 connected to the substrate 351 side. The voltage can be provided via connection 252.
[0510] The connector 243 may be, for example, a conductive particle. The surface of organic resin or silica particles coated with a metal material can be used. It is preferable to use nickel or gold as the metal material, since this can reduce the contact resistance. The particles are coated with layers of two or more metal materials, such as nickel coated with gold. It is preferable that the connector 243 is made of a material that is elastically deformable or plastically deformable. In this case, it is preferable that the connectors 243, which are conductive particles, are arranged as shown in FIG. In this way, the connector 243 and the electrical This increases the contact area with the conductive layer that is directly connected to the substrate, reducing contact resistance and preventing connection failures. The occurrence of defects can be suppressed.
[0511] The connector 243 is preferably disposed so as to be covered with the adhesive layer 141. For example, The connectors 243 may be dispersed in the adhesive layer 141.
[0512] The light emitting element 170 is a bottom emission type light emitting element. From the 220 side, an electrode 191 functioning as a pixel electrode, an EL layer 192, and a layer functioning as a common electrode are provided. The electrode 191 is provided on an insulating layer 214. The conductive layer 222a of the transistor 205 is connected through the opening. The transistor 205 has a function of controlling the driving of the light-emitting element 170. The electrode 193 covers the end of the electrode 191. The electrode 193 includes a material that reflects visible light. The electrode 193 includes a material that transmits visible light. An insulating layer 194 is provided to cover the electrode 193. The light emitted by the optical element 170 passes through the colored layer 134, the insulating layer 220, the opening 451, the electrode 311a, etc. The light is then emitted to the substrate 361 side via the
[0513] The liquid crystal element 180 and the light emitting element 170 can display various colors by changing the color of the colored layer depending on the pixel. The display device 300A uses the liquid crystal element 180 to display colors. The display device 300A can perform color display using the light emitting element 170. This can be done.
[0514] Transistor 201, transistor 203, transistor 205, and transistor 20 6 are formed on the surface of the insulating layer 220 on the substrate 351 side. The star can be fabricated using the same process.
[0515] The circuit electrically connected to the liquid crystal element 180 is a circuit electrically connected to the light emitting element 170. It is preferable that the two circuits are formed on the same plane. This eliminates the need to form the two circuits on different planes. The thickness of the display device can be made thinner than when two transistors are used. Because they can be fabricated using the same process, compared to forming two transistors on separate surfaces, Therefore, the manufacturing process can be simplified.
[0516] The pixel electrode of the liquid crystal element 180 is connected to the light emitting element 1 via a gate insulating layer of the transistor. It is located opposite to the pixel electrode 70 .
[0517] Here, a transistor 20 having a metal oxide in a channel formation region and an extremely low off-state current 6 or a memory element electrically connected to the transistor 206 is used. In the above, when a still image is displayed using the liquid crystal element 180, the writing operation to the pixel is stopped. In other words, it is possible to maintain the gradation even if the frame rate is extremely low. In one embodiment of the present invention, the frame rate can be made extremely small. Therefore, driving with low power consumption can be performed.
[0518] The transistor 203 is a transistor (switching The transistor 205 is a light emitting transistor. This is a transistor that controls the current flowing through the element 170 (also called a drive transistor).
[0519] On the substrate 351 side of the insulating layer 220, the insulating layer 211, the insulating layer 212, the insulating layer 213, and the insulating layer The insulating layer 211 is provided with insulating layers such as 214. A part of the insulating layer 211 is a gate of each transistor. The insulating layer 212 functions as a first insulating layer. The insulating layer 212 is provided to cover the transistor 206 and the like. The insulating layer 213 is provided to cover the transistor 205 and the like. The number of insulating layers covering the transistor is not limited, and a single insulating layer may be used. There may be one or more layers.
[0520] At least one of the insulating layers that covers each transistor is designed to prevent impurities such as water and hydrogen from diffusing. It is preferable to use a material that can make the insulating layer function as a barrier film. With this structure, impurities are prevented from diffusing into the transistor from the outside. It is therefore possible to effectively suppress the above-mentioned problems, thereby achieving a highly reliable display device.
[0521] Transistor 201, transistor 203, transistor 205, and transistor 20 6 is a conductive layer 221a functioning as a gate, an insulating layer 211 functioning as a gate insulating layer , the conductive layer 222a and the conductive layer 222b functioning as a source and a drain, and Here, the same hack is applied to multiple layers obtained by processing the same conductive film. It has a matching pattern.
[0522] The transistors 201 and 205 are transistors 203 and 2 In addition to the structure of 06, a conductive layer 223 that functions as a gate is provided.
[0523] The transistor 201 and the transistor 205 each have two semiconductor layers in which a channel is formed. In this case, the gate of the transistor is sandwiched between the gates of the transistors. The threshold voltage of the transistor can be controlled by connecting the two gates together and applying the same signal to them. Such a transistor may be driven by a It is possible to increase the field effect mobility compared to conventional MOSFETs, and to increase the on-current. As a result, a circuit capable of high speed operation can be fabricated. It is possible to reduce the area occupied by the device by using a transistor with a large on-state current. Even if the number of wirings increases when the display device is made larger or has higher resolution, It is possible to reduce the signal delay in the display, and to suppress display unevenness.
[0524] Alternatively, a potential for controlling the threshold voltage is applied to one of the two gates, and a drive potential is applied to the other. By applying a potential for the gate, the threshold voltage of the transistor can be controlled.
[0525] There is no limitation on the structure of the transistors included in the display device. The transistors included in the display portion 362 may have the same structure or different structures. The multiple transistors in the circuit 364 may all have the same structure, or may be two types of transistors. The above-mentioned structures may be used in combination. The transistors may all have the same structure, or two or more types of structures may be combined. It may be possible to do so.
[0526] It is preferable to use a conductive material containing an oxide for the conductive layer 223. When the conductive film is formed, the film is formed in an oxygen-containing atmosphere, so that oxygen is added to the insulating layer 212. The ratio of oxygen gas in the deposition gas is set to 90% or more and 100% or less. The oxygen supplied to the insulating layer 212 is preferably converted into the semiconductor layer 23 by a subsequent heat treatment. 1, oxygen vacancies in the semiconductor layer 231 can be reduced.
[0527] In particular, it is preferable to use a metal oxide with low resistance for the conductive layer 223. It is preferable to use an insulating film that releases hydrogen, such as a silicon nitride film, for the insulating layer 213. Hydrogen is supplied to the conductive layer 223 during the formation of the insulating layer 213 or by a heat treatment thereafter. As a result, the electrical resistance of the conductive layer 223 can be effectively reduced.
[0528] The colored layer 134 is provided in contact with the insulating layer 213. It's covered.
[0529] A connection portion 204 is provided in the area where the substrate 351 and the substrate 361 do not overlap. In the portion 204, the wiring 365 is electrically connected to the FPC 372 via the connection layer 242. The connection part 204 has a similar structure to the connection part 207. The conductive layer obtained by processing the same conductive film as the electrode 311a is exposed. The portion 204 and the FPC 372 can be electrically connected via a connection layer 242 .
[0530] The polarizing plate 135 disposed on the outer surface of the substrate 361 may be a linear polarizing plate, but a circular polarizing plate may also be used. A circular polarizer can also be used. For example, a linear polarizer and a quarter-wave retardation plate can be used as a circular polarizer. This can suppress the reflection of external light. In addition, depending on the type of polarizing plate, the cell gap, orientation, A desired contrast is achieved by adjusting the driving voltage and the like.
[0531] Various optical members can be disposed on the outside of the substrate 361. Examples of the optical members include: Polarizing plates, retardation plates, light diffusion layers (diffusion films, etc.), anti-reflection layers, and light-collecting films, etc. In addition, the outside of the substrate 361 is provided with an antistatic film to prevent dust from adhering, It is equipped with a water-repellent film that makes it difficult for the product to get dirty, and a hard coat film that prevents scratches from occurring during use. Good too.
[0532] The substrate 351 and the substrate 361 are made of glass, quartz, ceramic, sapphire, or tantalum. The substrate 351 and the substrate 361 may be made of a flexible material. This can increase the flexibility of the display device.
[0533] The liquid crystal element 180 may be, for example, a vertical alignment (VA) liquid crystal element. A liquid crystal element in which the MV t) mode is applied can be used. A (Multi-Domain Vertical Alignment) mode, PV A(Patterned Vertical Alignment) mode, ASV(A Advanced Super View (AVC) mode can be used.
[0534] The liquid crystal element 180 can be a liquid crystal element to which various modes are applied. For example, In addition to the VA mode, TN (Twisted Nematic) mode and IPS (In- Plane-Switching mode, FFS (Fringe Field Switching) mode tching) mode, ASM(Axially Symmetric aligned) Micro-cell mode, OCB (Optically Compensated) d Birefringence mode, FLC (Ferroelectric Li quid Crystal) mode, AFLC (AntiFerroelectric) mode Liquid Crystal) mode, STN (Super Twisted Nem atic mode, TBA (Transverse Bend Alignment) mode Electrically Controlled Birefring (ECB) A liquid crystal element to which a guest-host mode or a guest-sensing mode is applied can be used.
[0535] A liquid crystal element is an element that controls the transmission or non-transmission of light by the optical modulation action of liquid crystals. The optical modulation of liquid crystals is caused by the electric field applied to the liquid crystal (horizontal electric field, vertical electric field or oblique electric field). The liquid crystal used in the liquid crystal element is thermotropic. Low molecular weight liquid crystal, polymer liquid crystal, polymer dispersed liquid crystal (PDLC) ispersed Liquid Crystal, Polymer Network Liquid Crystal (PN LC: Polymer Network Liquid Crystal), ferroelectric liquid These liquid crystal materials can be used as colloidal liquid crystals, antiferroelectric liquid crystals, etc. It shows telic phase, smectic phase, cubic phase, chiral nematic phase, isotropic phase, etc. .
[0536] The liquid crystal material may be either a positive type liquid crystal or a negative type liquid crystal. The optimum liquid crystal material can be used depending on the mode and design.
[0537] An alignment film can be provided to control the alignment of the liquid crystal. In this case, a liquid crystal that exhibits a blue phase without using an alignment film may be used. The blue phase is one of the liquid crystal phases. When the temperature of cholesteric liquid crystal is increased, the phase immediately transitions from the cholesteric phase to the isotropic phase. The blue phase appears only in a narrow temperature range, so it is necessary to improve the temperature range. In order to achieve this, a liquid crystal composition containing a chiral agent of several percent by weight or more is used. A liquid crystal composition containing a liquid crystal exhibiting the above formula and a chiral agent has a short response time and is optically isotropic. In addition, a liquid crystal composition containing a liquid crystal exhibiting a blue phase and a chiral agent does not require an alignment treatment, The viewing angle dependency is small. In addition, since there is no need to provide an alignment film, rubbing treatment is also unnecessary. Therefore, electrostatic damage caused by the rubbing process can be prevented, and This makes it possible to reduce defects and damage to the liquid crystal display device.
[0538] When a reflective liquid crystal element is used, a polarizing plate 135 is provided on the display surface side. In addition, it is preferable to dispose a light diffusion plate on the display surface side, since this improves visibility.
[0539] A front light may be provided outside the polarizing plate 135. The front light may be: It is preferable to use an edge-lit front light. It is preferable to use a MOSFET since it is possible to reduce power consumption.
[0540] Materials that can be used for light-emitting elements, transistors, insulating layers, conductive layers, adhesive layers, connection layers, etc. For each of the above, please refer to the description in the first embodiment.
[0541] <Application Examples> In one embodiment of the present invention, a display device equipped with a touch sensor (hereinafter referred to as an input / output device or a touch panel) It is possible to create a thin film (also called a "nel").
[0542] There is no limitation on a detection element (also referred to as a sensor element) included in the input / output device of one embodiment of the present invention. Or various sensors that can detect the proximity or contact of a detection object such as a stylus. , can be applied as a sensing element.
[0543] For example, the sensor types include capacitance type, resistive film type, surface acoustic wave type, and infrared type. Various methods such as optical methods and pressure-sensitive methods can be used.
[0544] In this embodiment, an input / output device having a capacitance type sensing element will be described as an example.
[0545] The capacitive touch sensor includes a surface capacitive touch sensor and a projected capacitive touch sensor. The electrostatic capacitance type includes the self-capacitance type and the mutual capacitance type. This is preferable because it enables simultaneous multi-point detection.
[0546] In the input / output device of one embodiment of the present invention, a display device and a detector element that are separately manufactured are attached to each other. The display panel has a pair of substrates, and electrodes constituting a sensing element are provided on one or both of the substrates. Various configurations can be applied, such as a configuration in which
[0547] In the following, we will discuss an input / output device that is configured by bonding a display device and a detector element that are separately manufactured. 31 and 35 are flow diagrams of a manufacturing method of a display device of one embodiment of the present invention. FIG. 32 and FIG. 33(A) and (B) show cross-sectional views of a display device being manufactured. 31. Similarly, FIG. 33(A) corresponds to step S7, FIG. B) corresponds to step S8. Also, FIG. 36 and FIG. 37 are cross-sectional views of a display device being manufactured. FIG. 36 corresponds to step S26 shown in FIG. 35. Similarly, FIG. 37 corresponds to step Compatible with S27.
[0548] As shown in FIG. 31, first, a metal layer 19 is formed on a preparation substrate 14 (step S1). Then, the metal layer 19 is oxidized to form a metal oxide layer 20 (step S2). In the present embodiment, the metal layer 19 is oxidized by performing H2O plasma treatment to form a metal oxide layer 20. For the method of forming the metal oxide layer 20, reference can be made to the first embodiment.
[0549] Next, a first layer 24 is formed on the metal oxide layer 20 (step S3). The layer 24 is cured to form the resin layer 23 (step S4). The resin layer 23 is formed by applying and baking the resin layer 23. , please refer to embodiment 1.
[0550] Next, transistors and the like are formed on the resin layer 23 (step S5). A light emitting element electrically connected to the stator is formed and sealed (step S6). The components formed in the above will be described with reference to FIG. Please refer to the above description.
[0551] As shown in FIG. 32, a metal oxide layer 20 is formed on a preparation substrate 14. A resin layer 23 is formed on the insulating layer 115. The insulating layer 115 preferably has high barrier properties. On the insulating layer 115, an electrode 311a, an electrode 311b, and an electrode 311c are provided. The electrodes 311a and 311c are laminated in this order. The electrodes 311a and 311c are located outside the ends and are in contact with each other. A conductive film that transmits light is used. A conductive film that reflects visible light is used for the electrode 311b. The electrode 311b is provided with an opening 451. The opening 451 is a light-emitting region of the light-emitting element 170. An insulating layer 220a is provided on the electrode 311c. A conductive layer 224 is provided on the insulating layer 220b. The conductive layer 224 functions as one electrode of the capacitor. A transistor 203, a transistor 205, and a transistor 206 are provided. The source or drain of the transistor 206 is connected to the electrode 311c at the connection portion 207. The transistor 205 has two gates. The two gates are The source or drain of the transistor 205 is electrically connected to the conductive layer 22. 8 and is electrically connected to the electrode 191 of the light emitting element 170. Covered with edge layer 212, insulating layer 213, insulating layer 214, insulating layer 225, and insulating layer 215. It is preferable that one or more of these insulating layers have high barrier properties. 2 shows an example in which a material with high barrier properties is used for the insulating layer 213 and the insulating layer 225. The insulating layer 3 is provided to cover the ends of the insulating layer 220a, the insulating layer 220b, the insulating layer 212, etc. The edge layer 225 is provided over the edge of the insulating layer 214. The coating 226 reflects visible light. The coating film 226 reflects a part of the light emitted from the light emitting element 170 and transmits it to the opening 451 side. The lens 227 has a function of transmitting the light emitted from the light emitting element 170. The lens 227 overlaps the light emitting area of the light emitting element 170. The light emitting element 170 is The EL layer 192 is painted for each sub-pixel. The end of the electrode 191 is covered with an insulating layer 216. The insulating layer 217 is a spacer. The adhesive layer 142 bonds the light emitting element 170 to the substrate 351. They are combined.
[0552] The material of one or both of the insulating layers 214 and 215 has a refractive index of 1.55 or less. is a material with a refractive index of 1.66 or close to that, acrylic resin, polyimide Resins and the like can be used.
[0553] The material of the coating film 226 may be a metal. Specifically, a material containing silver, The coating film 226 can be formed using a material containing silver and palladium, a material containing silver and copper, or the like. do.
[0554] The refractive index of the lens 227 is preferably 1.3 or more and 2.5 or less. The insulating film can be formed using either or both of inorganic and organic materials.
[0555] The material of the lens 227 may be, for example, a material containing an oxide or a sulfide, or a material containing a resin. Examples of materials that include oxides or sulfides include cerium oxide. , hafnium oxide, lanthanum oxide, magnesium oxide, niobium oxide, tantalum oxide, oxide Titanium oxide, yttrium oxide, zinc oxide, oxides containing indium and tin, indium and gallium Examples of materials that contain resin include oxides containing lithium and zinc, zinc sulfide, etc. Resins containing chlorine, bromine or iodine, heavy metal atoms, and aromatic rings Resins with sulfur introduced, resins with sulfur introduced, etc. A material containing nanoparticles of a material with a high refractive index can be used for the lens 227. For the nanoparticles, for example, tungsten or zirconium oxide can be used.
[0556] Next, the transistors and the like are peeled off from the fabrication substrate 14 and transferred to the substrate 351 side (step S 7) In this example, the interface between the metal oxide layer 20 and the resin layer 23 or the interface between the metal oxide layer 20 and the resin layer 23 via the substrate 14 is Laser light is irradiated to the vicinity of the metal oxide layer 20. Separation occurs at the interface between the metal oxide layer 20 and the resin layer 23. As a result, the resin layer 23 is exposed (FIG. 33(A)).
[0557] Next, the resin layer 23 is removed to expose the insulating layer 115 (step S8). A part or the whole of the insulating layer 115 may be removed to expose the electrode 311a. By leaving the high insulating layer 115, moisture may penetrate into the transistor and the light emitting element 170. This can suppress the above-mentioned problem, thereby improving the reliability of the display device. The resin layer 23 is removed (FIG. 33(B)).
[0558] Then, the liquid crystal element 180 is formed (step S9). An alignment film 133a is formed on one surface of the substrate 361. The insulating layer 121, the insulating layer 232, the electrode 113, the insulating layer 117, and the alignment film 133b are formed in this order. FIG. 34 shows an example in which the colored layer 131 does not overlap the light-emitting region of the light-emitting element 170. However, the colored layer 131 may be provided so as to overlap the light-emitting region of the light-emitting element 170. The insulating layer 232 functions as an overcoat. The electrode 113 functions as a common electrode for the liquid crystal element 180. The insulating layer 117 The insulating layer 117 functions as a spacer to maintain the cell gap of the semiconductor device 180. Transmits visible light.
[0559] The substrate 351 and the alignment film 133b are arranged so that the liquid crystal layer 112 is sandwiched between the alignment film 133a and the alignment film 133b. The liquid crystal element 180 is formed by bonding the substrate 361 to the liquid crystal element 180. It has an electrode 311 a , an electrode 311 b , an electrode 311 c , a liquid crystal layer 112 , and an electrode 113 .
[0560] Furthermore, a diffusion film 233 and a polarizing plate 135 are attached to the other surface of the substrate 361. Then, a substrate 235 having a touch sensor on one surface is attached to the polarizing plate 135. In addition, in FIG. 34, the adhesive layer is omitted in some places. It is preferable that the surface of the display be treated with an anti-reflective coating. For example, the surface of the display may be treated with an anti-glare coating. It is preferable that the uneven surface diffuses reflected light and reduces glare. An insulating layer 234c is provided between the conductive layer 234a and the conductive layer 234b of the touch sensor. The conductive layer 234b is covered with an insulating layer 234d.
[0561] In this manner, the input / output device 310A shown in FIG. 34 is formed. Then, ICs and the like are mounted (step S10), and the display can be checked (step S11). ).
[0562] The flow shown in FIG. 31 includes a step of removing the resin layer 23 peeled off from the fabrication substrate 14. On the other hand, FIG. 35 shows a flow in which this step is not included.
[0563] As shown in FIG. 35, first, a metal layer 19 is formed on a production substrate 14 (step S21). Then, the metal layer 19 is oxidized to form the metal oxide layer 20 (step S22). Here, the metal layer 19 is oxidized by performing H2O plasma treatment to form a metal oxide layer 20. For the method of forming the metal oxide layer 20, reference can be made to the first embodiment.
[0564] Next, a first layer 24 is formed on the metal oxide layer 20 (step S23). The layer 24 is cured to form the resin layer 23 (step S24). The resin layer 23 is formed by applying the resin 24 and baking it. For details, refer to the first embodiment. In this embodiment, the resin layer 23 having the opening is formed. For example, by opening the resin layer 23 at the portion where the conductive layer is to be exposed, after peeling, The conductive layer can be exposed without removing the resin layer 23. If the transmittance of visible light is low, the resin layer 23 should be opened at the portion from which the light is to be extracted. Therefore, after peeling, the resin layer 23 does not need to be removed, and a decrease in the light extraction efficiency can be suppressed.
[0565] Next, a transistor or the like is formed on the metal oxide layer 20 and the resin layer 23 (step S 25). Then, a light-emitting element electrically connected to the transistor is formed and sealed (sten Each component will be explained with reference to FIG. 36. For details, please refer to the above description.
[0566] As shown in FIG. 36, a metal oxide layer 20 is formed on a preparation substrate 14. A resin layer 23 is formed on the insulating film 20. The resin layer 23 has an opening. The area where the metal oxide layer 20 and the electrode 311a are in contact with each other, and There is a region where the metal oxide layer 20 and the insulating layer 213 are in contact with each other. On the lipid layer 23, an electrode 311a, an electrode 311b, and an electrode 311c are laminated in this order. The ends of the electrodes 311a and 311c are positioned outside the ends of the electrodes 311b. The electrodes 311a and 311c are disposed in contact with each other. A conductive film that reflects visible light is used for the electrode 311b. The light emitting region of the light emitting element 170 is provided in the portion where the insulating layer 311c is not formed. 220a is provided, and a conductive layer 224 is provided on the insulating layer 220a. An insulating layer 220b is provided on the conductive layer 224. The conductive layer 224 is a The insulating layer 220b functions as an electrode. , and a transistor 206. The source or drain of the transistor 206 The transistor 2 is electrically connected to the electrode 311c at the connection portion 207. 05 has two gates. The two gates are electrically connected. The source or drain of the capacitor 205 is connected to the electrode 19 of the light emitting element 170 via a conductive layer 228. Each transistor is electrically connected to an insulating layer 212, an insulating layer 213, and an insulating layer 211. 4, insulating layer 225, and insulating layer 215. In FIG. 36, the insulating layer 213 and the insulating layer 225 have a high barrier property. The insulating layer 213 is made of an insulating layer 220a and an insulating layer 220b. The insulating layer 225 is provided to cover the end of the insulating layer 214. The coating film 226 is a film that reflects visible light. The lens 227 has a function of reflecting a part of the light emitted from the element 170 and supplying it to the lower side of the drawing. The lens 227 has a function of transmitting the light emitted from the light emitting element 170. The light-emitting element 170 includes an electrode 191, an EL layer 192, and an electrode 193. The EL layer 192 is applied to each sub-pixel. The insulating layer 217 functions as a spacer. Thus, the light emitting element 170 and the substrate 351 are bonded together.
[0567] Next, the transistors and the like are peeled off from the fabrication substrate 14 and transferred to the substrate 351 side (step S 27) In this case, the interface between the metal oxide layer 20 and the resin layer 23 through the substrate 14 or Laser light is irradiated to the vicinity of the metal oxide layer 20. Separation occurs at the interface between the metal oxide layer 20 and the resin layer 23. As a result, the resin layer 23 is exposed (FIG. 37). In the first embodiment, separation occurs at the interface between the metal oxide layer 20 and the electrode 311a, exposing the electrode 311a. The electrode 311a is made of a material that has low adhesion to the metal oxide layer 20. In addition, the smaller the contact area between the electrode 311a and the metal oxide layer 20, the This is preferable because separation at the interface becomes easier.
[0568] Then, the liquid crystal element 180 is formed (step S28). An alignment film 133a is formed on one surface of the substrate 361. 121, an insulating layer 232, an electrode 113, an insulating layer 117, and an alignment film 133b are formed in this order. These configurations are the same as those in FIG. 34, so the explanation will be omitted.
[0569] The substrate 351 and the alignment film 133b are arranged so that the liquid crystal layer 112 is sandwiched between the alignment film 133a and the alignment film 133b. The liquid crystal element 180 is formed by bonding the substrate 361 to the liquid crystal element 180. It has an electrode 311 a , an electrode 311 b , an electrode 311 c , a liquid crystal layer 112 , and an electrode 113 .
[0570] Furthermore, a diffusion film 233 and a polarizing plate 135 are attached to the other surface of the substrate 361. Then, a substrate 235 having a touch sensor on one surface is attached to the polarizing plate 135. These configurations are the same as those in FIG. 34, so the description will be omitted.
[0571] In this manner, the input / output device 310B shown in FIG. 38 is formed. Then, ICs and the like are mounted (step S29), and the display can be checked (step S30). ).
[0572] As described above, the display device of the present embodiment has two types of display elements and can display a plurality of display modes. Since it can be used by switching between the two, it is highly visible and convenient regardless of the surrounding brightness. expensive.
[0573] This embodiment mode can be combined with other embodiment modes as appropriate.
[0574] (Embodiment 4) In this embodiment, a metal that can be used for a transistor disclosed in one embodiment of the present invention will be described. In the following, we will explain about oxides. In particular, we will discuss metal oxides and CAC (Cloud-Aligned This article explains the details of the 3D Composite OS.
[0575] CAC-OS or CAC-metal oxide is a material that has the function of electrical conductivity. A part of the material has an insulating function, and the material as a whole has a semiconductor function. Note that CAC-OS or CAC-metal oxide is used as the channel of a transistor. When used in a forming region, the conductive function is to allow the flow of electrons (or holes) that serve as carriers. The insulating function is to prevent the flow of electrons, which act as carriers. The function of switching (O Add the function to turn the power on / off to CAC-OS or CAC-metal oxide. In the case of CAC-OS or CAC-metal oxide, By separating these functions, the functionality of both can be maximized.
[0576] In addition, CAC-OS or CAC-metal oxide has a conductive region and an insulating region. The conductive region has the above-mentioned conductive function, and the insulating region has the above-mentioned insulating function. In addition, the conductive and insulating regions in the material are formed at the nanoparticle level. In addition, the conductive and insulating regions may be separated by a metal. In addition, the conductive area may be observed as a cloud-like connected area with a blurred periphery. There may be cases where this occurs.
[0577] In addition, in the CAC-OS or CAC-metal oxide, the conductive region and the insulating region are The peripheral region is 0.5 nm to 10 nm, preferably 0.5 nm to 3 nm. The following sizes may be present in the material:
[0578] In addition, CAC-OS or CAC-metal oxide has different band gaps. For example, CAC-OS or CAC-metal oxi de is a component with a wide gap due to the insulating region and a component with a narrow gap due to the conductive region. In the case of this configuration, when a carrier flows, In the narrow gap component, carriers mainly flow. The component having a narrow gap acts complementary to the component having a wide gap. Carriers also flow to the wide gap component in conjunction with the component with a large gap. AC-OS or CAC-metal oxide is placed in the channel formation region of the transistor. When used, the transistor has a high current driving force in the on-state, i.e., a large on-current. And high field effect mobility can be obtained.
[0579] That is, CAC-OS or CAC-metal oxide is a matrix composite material. (matrix composite), or metal matrix composite It can also be called a composite matrix.
[0580] For example, the elements constituting the metal oxide in the CAC-OS are 0.5 nm or more and 10 nm or less. Preferably, the material is unevenly distributed in a size range of 1 nm to 2 nm or less, or in the vicinity thereof. In the following, we will consider metal oxides in which one or more metal elements are unevenly distributed. The region having the metal element has a size of 0.5 nm to 10 nm, preferably 1 nm to 2 A state in which particles are mixed in sizes of less than or close to that size is called a mosaic or patch-like state. cormorant.
[0581] The metal oxide preferably contains at least indium. It is preferable that the metal contains zinc. In addition to the above, aluminum, gallium, yttrium, Aluminum, copper, vanadium, beryllium, boron, silicon, titanium, iron, nickel, germanium nium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum One or more of the following elements are included: tungsten, tungsten, magnesium, etc. It may be possible.
[0582] For example, CAC-OS made of In-Ga-Zn oxide (In-Ga-Zn oxide is one of the CAC-OS) a-Zn oxide may be specifically referred to as CAC-IGZO. (Hereinafter, InO X1 (X1 is a real number greater than 0.) or indium zinc oxide In X2 Zinc Y2 O Z2 (X2, Y2, and Z2 are real numbers greater than 0) ) and gallium oxide (GaO X3 (X3 is a real number greater than 0). ), or gallium zinc oxide (Ga X4 Zinc Y4 O Z4 (X4, Y4, and Z4 (is a real number greater than 0).) The material is separated into a mosaic shape, Mosaic InO X1 , or In X2 Zinc Y2 O Z2 is uniformly distributed in the film (Hereinafter, this will also be referred to as cloud-like.)
[0583] In other words, CAC-OS is X3 The region where In is the main component and X2 Zinc Y2 O Z2 , or InO X1 A composite metal oxide having a structure in which a region in which In this specification, for example, the atomic ratio of In to the element M in the first region is The first region has an atomic ratio of In to the element M in the second region that is greater than the atomic ratio of In in the second region. The concentration of In is higher than in the region
[0584] Note that IGZO is a common name and refers to a compound made of In, Ga, Zn, and O. A typical example is InGaO3(ZnO). m1 (m1 is a natural number), or In(1 +x0) Ga (1-x0) O3(ZnO) m0 (-1≦x0≦1, m0 is an arbitrary number) Examples of such crystalline compounds include those that are
[0585] The crystalline compounds may have a single crystal structure, a polycrystalline structure, or a c-axis aligned crystal structure (CAAC). The CAAC structure is a structure in which multiple IGZO The nanocrystals have a c-axis orientation and are connected in ab-plane without being oriented. do.
[0586] On the other hand, CAC-OS is a material structure of metal oxide. CAC-OS is a material structure of In, Ga In the material composition containing Zn, and O, nanoparticles mainly composed of Ga were observed in some parts. The regions where the In is mainly contained are observed as nanoparticles, and the regions where the In is mainly contained as nanoparticles are observed. Therefore, in the CAC-OS, the crystal structure is a secondary element.
[0587] It should be noted that the CAC-OS does not include a laminated structure of two or more films having different compositions. For example, a structure consisting of two layers, a film mainly made of In and a film mainly made of Ga, is not included. do not have.
[0588] In addition, GaO X3 The region where In is the main component and X2 Zinc Y2 O Z2 , or InO X1 but In some cases, a clear boundary between the region of the main component and the region of the main component may not be observed.
[0589] Instead of gallium, aluminum, yttrium, copper, vanadium, and beryllium can be used. , boron, silicon, titanium, iron, nickel, germanium, zirconium, molybdenum , lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, or magnesium If one or more selected types of sodium, etc. are included, CAC-OS will The region observed is a nanoparticle of the metal element as the main component, and the region observed is a nanoparticle of In as the main component. The nanoparticle-like regions are randomly distributed in a mosaic pattern. say.
[0590] CAC-OS is formed by sputtering without intentionally heating the substrate. In addition, when the CAC-OS is formed by a sputtering method, the deposition gas and The gas to be used should be selected from an inert gas (typically argon), oxygen gas, and nitrogen gas. In addition, the ratio of oxygen gas to the total flow rate of the deposition gas during deposition may be For example, the flow rate ratio of oxygen gas is preferably 0% or more and less than 30%. It is preferable that the content be 0% or more and 10% or less.
[0591] CAC-OS is a type of X-ray diffraction (XRD) measurement method. When measured using the θ / 2θ scan by the out-of-plane method, In other words, no clear peaks are observed in the measurement region from the X-ray diffraction. It can be seen that no orientation in the ab plane direction or the c-axis direction is observed.
[0592] In addition, the CAC-OS uses an electron beam with a probe diameter of 1 nm (also called a nano-beam electron beam). In the electron beam diffraction pattern obtained by irradiating the sample with electrons, a ring-shaped region of high brightness and the Therefore, the electron diffraction pattern indicates that the CAC-OS The crystal structure is nc (nano-crystal) which has no orientation in the planar direction and cross-sectional direction. It can be seen that it has a crystalline structure.
[0593] For example, in the case of CAC-OS made of In-Ga-Zn oxide, energy dispersive X-ray Spectroscopy (EDX: Energy Dispersive X-ray spectroscopy) The EDX mapping obtained using a GaO X3 The region where is the main component and , In X2 Zinc Y2 O Z2 , or InO X1 The areas where the main component is It can be confirmed that the compound has the structure shown in FIG.
[0594] CAC-OS has a structure different from that of IGZO compounds in which metal elements are uniformly distributed. It has different properties from ZO compounds. That is, CAC-OS is GaO X3 The main ingredients are In a certain area, X2 Zinc Y2 O Z2 , or InO X1 The region where is the main component and The phase is separated into two layers, and the regions each containing one element as a main component are arranged in a mosaic pattern.
[0595] Here, In X2 Zinc Y2 O Z2 , or InO X1 The area where GaO is the main component X3 This region has a higher electrical conductivity than the region where In is the main component. X2 Zinc Y 2O Z2 , or InO X1The carriers flow through the area where the main component is oxidized. Therefore, the conductivity of In is expressed as a semiconductor. X2 Zinc Y2 O Z2 , or InO X The region where 1 is the main component is distributed in a cloud-like shape in the oxide semiconductor, which results in a high electric field effect. Mobility (μ) can be achieved.
[0596] On the other hand, GaO X3 The region where the main components are In X2 Zinc Y2 O Z2 , or InO X This region has higher insulating properties than the region where GaO X3 etc. The distribution of the main component in the oxide semiconductor suppresses leakage current and provides good switching performance. Switching operation can be achieved.
[0597] Therefore, when CAC-OS is used in a semiconductor device, GaO X3 Insulation caused by In X2 Zinc Y2 O Z2 , or InO X1 The conductivity caused by the This results in a high on-state current (I on ) and high field-effect mobility (μ) can be achieved. Cut.
[0598] In addition, semiconductor devices using CAC-OS have high reliability. It is ideal for a variety of semiconductor devices, including displays.
[0599] This embodiment mode can be combined with other embodiment modes as appropriate.
[0600] (Embodiment 5) In this embodiment, a display module and an electronic device according to one embodiment of the present invention will be described.
[0601] The display module 8000 shown in FIG. 39(A) includes an upper cover 8001 and a lower cover 800 Between the display panel 8006 connected to the FPC 8005, the frame 8009, and the printer The device has a support board 8010 and a battery 8011.
[0602] For example, a display device manufactured according to one embodiment of the present invention can be used for the display panel 8006. This makes it possible to manufacture display modules with a high yield.
[0603] The upper cover 8001 and the lower cover 8002 are adapted to the size of the display panel 8006. The shape and dimensions can be changed as appropriate.
[0604] A touch panel may be provided over the display panel 8006. A resistive or capacitive touch panel is superimposed on the display panel 8006. In addition, a touch panel may not be provided, and the display panel 8006 may be provided with a touch panel function. It is also possible to make it so that the
[0605] The frame 8009 protects the display panel 8006 and also prevents the operation of the printed circuit board 8010. It also functions as an electromagnetic shield to block electromagnetic waves generated by the frame. The plate 8009 may function as a heat sink.
[0606] The printed circuit board 8010 includes a power supply circuit, a signal circuit for outputting a video signal, and a clock signal. The power supply circuit is supplied with power from an external commercial power source. Alternatively, the power source may be a battery 8011 provided separately. This can be omitted if a commercial power source is used.
[0607] In addition, the display module 8000 includes additional components such as a polarizing plate, a retardation plate, and a prism sheet. It may also be provided as such.
[0608] FIG. 39(B) is a schematic cross-sectional view of a display module 8000 equipped with an optical touch sensor. be.
[0609] The display module 8000 includes a light emitting unit 8015 and a light receiving unit 8016 provided on a printed circuit board 8010. The upper cover 8001 and the lower cover 8002 are provided with a portion 8016. The light guiding portion 8017 has a pair of light guiding portions (light guiding portion 8017a and light guiding portion 8017b) in the light guiding portion 8017a.
[0610] The upper cover 8001 and the lower cover 8002 may be made of, for example, plastic. In addition, the upper cover 8001 and the lower cover 8002 can each be made thin. For example, the thickness of each cover can be set to 0.5 mm or more and 5 mm or less. This allows the display module 8000 to be extremely lightweight. Since the lower cover 8002 and the lower cover 8001 can be fabricated, the fabrication cost can be reduced.
[0611] The display panel 8006 is connected to a printed circuit board 8010 and a battery via a frame 8009. The display panel 8006 and the frame 8009 are disposed so as to overlap with the light guide unit 8 017a and fixed to the light guiding portion 8017b.
[0612] Light 8018 emitted from the light emitting portion 8015 is guided to the display panel 800 by the light guiding portion 8017a. 6, and reaches the light receiving section 8016 through the light guiding section 8017b. A touch operation is detected when the light 8018 is blocked by a detection object such as an illustration. It is possible.
[0613] A plurality of light emitting sections 8015 are provided, for example, along two adjacent sides of the display panel 8006 . A plurality of light receiving sections 8016 are provided at positions facing the light emitting sections 8015. It is possible to obtain information on the position where the touch operation was performed.
[0614] The light emitting unit 8015 may be a light source such as an LED element. 015, a light source that emits infrared rays that are invisible to the user and harmless to the user It is preferable to use:
[0615] The light receiving section 8016 is a photoelectric element that receives the light emitted by the light emitting section 8015 and converts it into an electrical signal. Preferably, a photodiode capable of receiving infrared rays can be used. Cut.
[0616] The light guiding portion 8017a and the light guiding portion 8017b are made of a material that transmits at least the light 8018. By using the light guiding portion 8017a and the light guiding portion 8017b, the light emitting portion 8 The light receiving unit 8015 and the light receiving section 8016 can be disposed under the display panel 8006, and external light is received. In particular, it is possible to prevent the light from reaching the light unit 8016 and causing the touch sensor to malfunction. It is preferable to use a resin that absorbs infrared rays and transmits infrared rays. This prevents the touch sensor from malfunctioning. This can suppress the work more effectively.
[0617] According to one embodiment of the present invention, an electronic device having a curved surface and high reliability can be manufactured. According to one embodiment, a flexible and highly reliable electronic device can be manufactured.
[0618] Examples of electronic devices include television sets, desktop or notebook PCs, etc. Computers, monitors for computers, digital cameras, digital video cameras Cameras, digital photo frames, mobile phones, portable game consoles, personal digital assistants, audio playback Examples of such devices include large gaming machines such as pachinko machines.
[0619] In addition, the display device of one embodiment of the present invention can achieve high visibility regardless of the intensity of external light. Therefore, portable electronic devices, wearable electronic devices, and It can be suitably used for child book terminals and the like.
[0620] A mobile information terminal 800 shown in FIGS. 40A and 40B includes a housing 801, a housing 802, a display unit 8 03, and a hinge portion 805.
[0621] The housing 801 and the housing 802 are connected by a hinge portion 805. The mobile information terminal 800 includes: It can be unfolded from the folded state (Figure 40(A)) to the state shown in Figure 40(B). This makes it easy to carry around and convenient to use due to its large display area. , and has excellent visibility.
[0622] The portable information terminal 800 has a housing 801 and a housing 802 connected by a hinge portion 805. A flexible display unit 803 is provided.
[0623] A display device manufactured according to one embodiment of the present invention can be used for the display portion 803. This makes it possible to manufacture portable information terminals with a high yield.
[0624] The display unit 803 is capable of displaying at least one of document information, still images, and moving images. When document information is displayed on the display unit, the mobile information terminal 800 is used as an electronic book terminal. It can be used as such.
[0625] When the mobile information terminal 800 is unfolded, the display unit 803 is held in a largely curved state. For example, the radius of curvature is 1 mm or more and 50 mm or less, preferably 5 mm or more and 30 mm or less. The display unit 803 is supported by the housing 801 and the cover 802. 802, pixels are continuously arranged, enabling a curved display.
[0626] The display unit 803 functions as a touch panel and can be operated by a finger, a stylus, etc. can.
[0627] It is preferable that the display unit 803 is composed of one flexible display. This makes it possible to perform continuous display without interruption between the housing 801 and the housing 802. In addition, a display may be provided on each of the housings 801 and 802. You may do so.
[0628] The hinge portion 805 is a portion that connects the housing 801 and the housing 802 when the mobile information terminal 800 is unfolded. It is preferable to have a locking mechanism to prevent the angle from becoming larger than a predetermined angle. For example, the angle at which the door will lock (will not open any further) must be greater than 90 degrees and less than 180 degrees. Typically, the angle is 90 degrees, 120 degrees, 135 degrees, 150 degrees, or 17 degrees. 5 degrees, etc. This improves the convenience, safety, and Reliability can be improved.
[0629] If the hinge unit 805 has a locking mechanism, the display unit 803 can be opened without applying excessive force. Therefore, it is possible to prevent the display unit 803 from being damaged. It can be achieved.
[0630] The housing 801 and the housing 802 are provided with a power button, an operation button, an external connection port, a speaker, a microphone, and a It may have an inch or the like.
[0631] A wireless communication module is provided in either the housing 801 or the housing 802. Internet, LAN (Local Area Network), Wi-Fi (registered trademark ) and the like.
[0632] A portable information terminal 810 shown in FIG. 40C includes a housing 811, a display unit 812, and an operation button 81. 3, an external connection port 814, a speaker 815, a microphone 816, a camera 817, etc.
[0633] A display device manufactured according to one embodiment of the present invention can be used for the display portion 812. This makes it possible to manufacture portable information terminals with a high yield.
[0634] The mobile information terminal 810 has a touch sensor on the display unit 812. All operations, such as inputting characters, can be performed by touching the display 812 with a finger or a stylus. It can be done.
[0635] In addition, the operation button 813 is operated to turn the power on and off, and to display information on the display unit 812. For example, you can change the type of image displayed on the main screen from the email composition screen. You can switch to the menu screen.
[0636] In addition, a detection device such as a gyro sensor or an acceleration sensor is installed inside the mobile information terminal 810. By providing the above, the orientation of the mobile information terminal 810 (vertical or horizontal) can be determined and the screen of the display unit 812 can be adjusted. The display orientation can be switched automatically. The screen orientation can also be switched by The input is made by touching the display unit 812, by operating the operation button 813, or by inputting voice using the microphone 816. It can also be performed by using force or the like.
[0637] The mobile information terminal 810 is, for example, one or more devices selected from a telephone, a notebook, an information viewing device, etc. Or it has multiple functions. Specifically, it can be used as a smartphone. The information terminal 810 is, for example, a mobile phone, an electronic mail, a text reading and writing, a music playback, a video It can run various applications such as playback, internet communication, and games. do.
[0638] The camera 820 shown in FIG. 40(D) includes a housing 821, a display unit 822, an operation button 823, and a shutter. The camera 820 also has a removable lens 826. It is attached.
[0639] A display device manufactured according to one embodiment of the present invention can be used for the display portion 822. This allows the camera to be manufactured with a high yield.
[0640] Here, the camera 820 and the lens 826 can be removed from the housing 821 and replaced. However, the lens 826 and the housing 821 may be integrated together.
[0641] The camera 820 captures still or moving images by pressing the shutter button 824. In addition, the display unit 822 has a function as a touch panel. It is also possible to take a picture by touching 2.
[0642] The camera 820 can be equipped with a strobe device, viewfinder, etc. Alternatively, these may be incorporated into the housing 821.
[0643] 41A to 41E are diagrams showing electronic devices. , a display unit 9001, a speaker 9003, and operation keys 9005 (power switch or operation switch switch), connection terminal 9006, sensor 9007 (force, displacement, position, speed, acceleration, Angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemicals, sound, time, hardness, electric field, current The ability to measure voltage, power, radiation, flow rate, humidity, gradient, vibration, odor or infrared The device has a microphone 9008 and the like.
[0644] A display device manufactured according to one embodiment of the present invention can be suitably used for the display portion 9001. This allows electronic devices to be manufactured with high yields.
[0645] The electronic devices shown in Figures 41(A) to (E) can have various functions. Functions for displaying various information (still images, videos, text images, etc.) on the display unit, touch panel function Functions such as displaying calendars, dates, or times, and various software (programs) ) to control processing, wireless communication function, and wireless communication function to connect various computers The function to connect to a data network, and the function to transmit or receive various data using wireless communication functions. The function to be performed, read out the program or data recorded on the recording medium and display it on the display unit The electronic device shown in Figs. 41(A) to (E) can have the following functions. The functions are not limited to these, and other functions may be included.
[0646] FIG. 41(A) shows a wristwatch-type portable information terminal 9200, and FIG. 41(B) shows a wristwatch-type portable information 9201. FIG.
[0647] The portable information terminal 9200 shown in FIG. 41A is a terminal for mobile telephone, e-mail, and document viewing and creation. It supports a variety of applications such as music playback, Internet communication, and computer games. In addition, the display surface of the display unit 9001 is curved. The portable information terminal 9200 can display information on a display surface. For example, a wireless headset can be used By communicating with each other, you can talk hands-free. The 9200 has a connection terminal 9006 and can directly exchange data with other information terminals via a connector. Also, charging can be performed via the connection terminal 9006. The charging operation may be performed by wireless power supply without going through the connection terminal 9006.
[0648] The portable information terminal 9201 shown in FIG. 41(B) is different from the portable information terminal shown in FIG. The display surface of the display unit 9001 is not curved. The shape is non-rectangular (circular in FIG. 41(B)).
[0649] 41(C) to (E) are perspective views showing a foldable portable information terminal 9202. FIG. 41C is a perspective view of the portable information terminal 9202 in an unfolded state, and FIG. The mobile information terminal 9202 changes from one of the unfolded state and the folded state to the other. FIG. 41(E) is a perspective view of the portable information terminal 9202 in a folded state. FIG.
[0650] The portable information terminal 9202 is highly portable when folded, and has a seam when unfolded. The display area of the portable information terminal 9202 is large and has excellent visibility. 9001 is supported by three housings 9000 connected by hinges 9055 . The two housings 9000 are bent via the hinge 9055, so that the portable information terminal 9 202 can be reversibly transformed from an unfolded state to a folded state. For example, The portable information terminal 9202 can be bent with a radius of curvature of 1 mm or more and 150 mm or less.
[0651] This embodiment mode can be combined with other embodiment modes as appropriate. EXAMPLES
[0652] In this example, the results of peeling a resin layer from a production substrate will be described.
[0653] A method for fabricating a sample in this embodiment will be described with reference to FIGS.
[0654] First, a metal oxide layer 20 was formed on a preparation substrate 14 (FIG. 5(A1)).
[0655] The substrate 14 used was a glass substrate having a thickness of about 0.7 mm. A titanium oxide film was formed. Specifically, a titanium oxide film was first formed to a thickness of about 5 nm by sputtering. After that, a mixture of nitrogen gas and oxygen gas (580NL / min, By baking for 1 hour at 450℃ while flowing oxygen (20%), a titanium oxide film was formed. was formed.
[0656] Next, a first layer 24 was formed on the metal oxide layer 20 (FIG. 5(B)). The first layer 24 was The material was formed using a material containing a non-photosensitive soluble polyimide resin. The film thickness was approximately 2.0 μm.
[0657] Next, the first layer 24 was subjected to a heat treatment to form a resin layer 23 (FIG. 5(C)). The heat treatment was performed by baking in a N2 atmosphere at 350°C for 1 hour.
[0658] Then, a UV peeling tape was attached to the resin layer 23 (see FIG. 5(D)). (equivalent to 75a).
[0659] The sample of this embodiment was irradiated with laser light from the side of the substrate 14 (FIG. 6(A)). The entire surface of the sample was irradiated with the laser light when viewed from the top. A mask (not shown) was provided.
[0660] A XeCl excimer laser with a wavelength of 308 nm was used as the laser oscillator for the laser light. The focal width on the short axis of the beam is 625 μm, and the energy density is approximately 440 mJ / cm 2 In addition, The material was divided into four areas with different laser light irradiation conditions. The number of shots in each area was The repetition rates were 10, 20, 30, and 40 shots. The number of shots was set to 60Hz. The scanning speed differs depending on the number of shots. The area of 10 shots is 3.75mm / sec, 20 shot area is 1.90mm / sec, 30 shot area is 1. The speed was 25 mm / sec, and the 40 shot area was 0.93 mm / sec.
[0661] The absorptance of light having a wavelength of 308 nm in the laminate structure of the fabricated substrate 14 and the metal oxide layer 20 is The transmittance was about 75%, and the transmittance was about 13%. The interface between the metal oxide layer 20 and the resin layer 23, the metal oxide layer 20, and the resin layer 23 are irradiated with laser light. It is thought that.
[0662] After the laser light irradiation, a cut is made from the substrate 75a side of the sample to the inside from the outer periphery with a cutter. By so doing, the preparation substrate 14 was peeled off from the sample (FIG. 6(B1)).
[0663] As shown in Figure 42, in the range of 10 to 40 shots, Even if the substrate 75a was peeled off from the preparation substrate 14, the substrate 75a could be peeled off.
[0664] Figure 43 shows a cross-sectional STEM (Scanning TEM) image of a sample with 10 shots. Transmission Electron Microscopy (TEM) observations The results are shown.
[0665] Fig. 43(A) shows a cross-sectional STEM image of the sample before peeling. The thickness of the metal oxide layer 20 is The thickness was about 14 nm. Fig. 43(B) shows a cross-sectional STEM image of the peeled substrate 75a side. No metal oxide layer 20 was observed between the resin layer 23 and the coating layer formed for the observation purpose. In addition, energy dispersive X-ray spectroscopy (EDX) In the analysis using 3D-ray spectroscopy, titanium was detected on the resin layer 23 side. FIG. 43(C) shows a cross-sectional STEM image of the peeled-off preparation substrate 14 side. The thickness of the oxide layer 20 was about 11 nm. From the above results, it is clear that the metal oxide layer 20 and the resin It is believed that separation was achieved at the interface with layer 23.
[0666] From the results of this example, it is clear that the metal oxide layer 20 and the resin layer 2 It was confirmed that the preparation substrate 14 could be peeled off from the interface between the preparation substrate 14 and 3.
[0667] In addition, the energy density is approximately 306 mJ / cm 2 Condition: about 324 mJ / cm 2 The conditions, Approximately 342mJ / cm 2 and about 360 mJ / cm 2 Even under these conditions, metal oxide It was confirmed that the fabricated substrate 14 could be peeled off at the interface between the layer 20 and the resin layer 23 (Fig. (The number of shots was 10 for each.) From this, it can be seen that the conditions are higher than those used in the laser crystallization process. It was found that processing can be performed with a lower energy density than that of the conventional laser. This increases the number of substrates that can be processed at once. It also enables the laser device to be used for a long period of time. This reduces the running costs of the laser device.
[0668] The resin layer used in this embodiment has high light transmittance (particularly high visible light transmittance) and light absorptance. However, the color of the resin layer is lower than that of the colored resin layer. A laminated structure of a metal oxide layer (titanium oxide film) and a resin layer (polyimide film) with a wavelength of 308 The absorptance of the light at 1 nm was about 87%. The absorption rate was higher than that of the 308 nm wavelength light (approximately 81%). By providing a metal oxide layer between the resin layer and the .
[0669] FIG. 44 shows an example of laser processing conditions that can be used in the peeling method according to one embodiment of the present invention. Region A is the substrate (glass substrate) and metal oxide layer (titanium oxide film) used in this example. These are conditions that can be applied to a peeling method using a laminated structure of a resin layer (polyimide film). Region B is a resin layer (having a high visible light transmittance) used in this embodiment in contact with the fabrication substrate (glass substrate). This is a condition that can be applied to a peeling method using a structure formed with a thin polyimide film. By providing the layer, the energy density of the laser light and the number of shots can be reduced. Specifically, when a colored resin layer is used, one embodiment of the present invention is applied. In this case, the energy density and number of shots of the laser beam could be equivalent to those of the conventional laser beam.
[0670] As described above, in one embodiment of the present invention, no special laser processing conditions are required, and the manufacturing cost is low. In addition, by using a resin layer with high visible light transmittance, Therefore, even if the resin layer is located on the display surface side of the display device, high display quality can be achieved. In addition, in order to improve the display quality, a process for removing the colored resin layer is also performed. In addition, the range of materials that can be selected for the resin layer is expanded. EXAMPLES
[0671] In this example, the results of peeling a resin layer from a production substrate will be described.
[0672] First, a display device of the comparative example was manufactured and the display state was confirmed. ), a resin layer (polyimide film) is formed on the resin layer, and a peeled layer (transistor and Then, the resin layer was irradiated with laser light through the formation substrate. In this manner, a display device was manufactured through a step of peeling the layer to be peeled off from the formation substrate.
[0673] As a result, if the energy density of the laser light is too high, soot (a type of powder made from carbonized resin) is produced. It was found that the occurrence of
[0674] In addition, if the energy density is low, the generation of soot can be suppressed, but the soot on the substrate (glass substrate) is It was found that the resin layer (polyimide film) remains on the surface, and the peeling yield is easily reduced. I did.
[0675] When irradiating light through the production substrate, foreign matter such as dust was attached to the light irradiation surface of the production substrate. This is believed to have caused uneven light irradiation, which resulted in peeling not occurring at the desired position.
[0676] In this way, when forming a resin layer on a substrate, the range of suitable laser light irradiation conditions is The area is small and can be difficult to control.
[0677] In this example, a stacked structure to which one embodiment of the present invention is applied is manufactured, and three types of evaluations are performed. The first evaluation was conducted on the effect of the laser energy density on the peelability of the sample. In the remaining two evaluations, the dust on the surface of the fabrication substrate that was irradiated with the laser light was investigated. The effect of these foreign objects on the peelability of the samples was investigated.
[0678] <Evaluation 1> A method for producing the sample for evaluation 1 will be described with reference to FIGS.
[0679] First, a metal oxide layer 20 was formed on a preparation substrate 14 (FIG. 5(A1)).
[0680] The substrate 14 used was a glass substrate having a thickness of about 0.7 mm. A titanium oxide film was formed. Specifically, a titanium oxide film was first formed to a thickness of about 10 nm by sputtering. Next, the surface of the titanium film was treated with H2O plasma to remove the gold. A titanium oxide film was formed as the metal oxide layer 20. The bias power for the H2O plasma treatment was 4500W, ICP power 0W, pressure 15Pa, processing time 600sec. The process gas used was water vapor at a flow rate of 250 sccm. The thickness of the titanium oxide film was about 26 nm. It was.
[0681] Next, a first layer 24 was formed on the metal oxide layer 20 (FIG. 5(B)). The first layer 24 was The photosensitive material was formed by using a material containing a polyimide resin precursor. The thickness of the film when spread was about 2.0 μm.
[0682] Next, the first layer 24 was subjected to a heat treatment to form a resin layer 23 (FIG. 5(C)). The heat treatment was performed by baking in a N2 atmosphere at 450°C for 1 hour.
[0683] Then, a substrate 75a was attached to the resin layer 23 using an adhesive layer 75b (FIG. 5(D)).
[0684] The sample of this embodiment was irradiated with laser light from the side of the substrate 14 (FIG. 6(A)). The entire surface of the sample was irradiated with the laser light when viewed from the top. A mask (not shown) was provided.
[0685] A XeCl excimer laser with a wavelength of 308 nm was used as the laser oscillator for the laser light. The focal width on the minor axis of the beam was 625 μm, the number of shots was 10, and the repetition frequency was 60 Hz. The scanning speed was 3.75 mm / sec. The samples were scanned under five different laser irradiation conditions. The energy density of each of the five regions is approximately 263 mJ / cm 2 ,about 306mJ / cm 2 , about 350mJ / cm 2 , about 394mJ / cm 2 , about 438mJ / c m 2 It was decided.
[0686] After the laser light irradiation, a cut is made from the substrate 75a side of the sample to the inside from the outer periphery with a cutter. By so doing, the preparation substrate 14 was peeled off from the sample (FIG. 6(B1)).
[0687] As shown in Figure 45, the energy density is about 263 mJ / cm 2 from about 438 mJ / cm 2 In all of these regions, the substrate 75a could be peeled off from the preparation substrate 14. No soot generation was observed even at high energy densities.
[0688] <Evaluation 2> Next, a laminate structure to which one embodiment of the present invention is applied (sample A) and a comparative laminate structure (comparative sample B ) was prepared, and the resin layer was peeled off from the prepared substrate. The results are described below.
[0689] The preparation method and peeling method of sample A and comparative sample B will be explained with reference to FIG. has a metal oxide layer 20, whereas comparative sample B does not have a metal oxide layer 20.
[0690] First, a metal oxide layer 20 was formed on a substrate 14 for preparing the sample A (FIG. 46(A1)). Preparation of Comparative Sample B No metal oxide layer 20 was formed on the substrate 14 (FIG. 46(A2)). .
[0691] The substrate 14 used was a glass substrate having a thickness of about 0.7 mm. A titanium oxide film was formed. Specifically, a titanium oxide film was first formed to a thickness of about 10 nm by sputtering. Next, the surface of the titanium film was treated with H2O plasma to remove the gold. A titanium oxide film was formed as the metal oxide layer 20. The bias power for the H2O plasma treatment was 4500W, ICP power 0W, pressure 15Pa, processing time 600sec. The process gas used was water vapor at a flow rate of 250 sccm. The thickness of the titanium oxide film was about 26 nm. It was.
[0692] Next, in sample A, a resin layer 23 was formed on the metal oxide layer 20 (FIG. 46(A1)). In the comparative sample B, a resin layer 23 was formed on a fabrication substrate 14 (FIG. 46(A2)). The photosensitive material 23 is formed using a material containing a polyimide resin precursor. The thickness of the coating was approximately 2.0 μm. After coating, the coating was heated in a nitrogen atmosphere. Then, the substrate was baked at 450° C. for 1 hour.
[0693] Then, the substrate 75a was attached to the resin layer 23 using the adhesive layer 75b (FIG. 46(A1), (A2)). The adhesive layer 75b is made of epoxy resin. The substrate 75a is made of PET film. We used the
[0694] Next, a plurality of light-shielding layers 15 were formed on the surface of the fabricated substrate 14 on which the resin layer 23 and the like were not formed. (FIGS. 46(B1) and (B2)). The light-shielding layer 15 is formed by sputtering to a thickness of about 30 mm. The light-shielding layer 15 was formed by depositing a titanium film with a thickness of 0 nm using a metal mask. The size of the light-shielding layer 15 was 220 μm×220 μm, 520 μm×520 μm, and m, 300μm×1100μm, 820μm×1000μm, 1000μm×2000μm m. A plurality of light-shielding layers 15 of each size were formed on the fabrication substrate 14.
[0695] 47(A) to (F) show micrographs of the light-shielding layer 15. The digital microscope used was a VHX-100 manufactured by Epson.
[0696] 47(A) to (C) show the pattern shape of the light-shielding layer 15 formed on the sample A. A) is a 300μm×1100μm pattern, and FIG. 47(B) is a 820μm×1000 47(C) is a 1000 μm × 2000 μm pattern.
[0697] 47(D) to (F) show the pattern shape of the light-shielding layer 15 formed in the comparative sample B. 7(D) is a 300μm×1100μm pattern, and FIG. 47(E) is a 820μm×10 47(F) is a 1000 μm × 2000 μm pattern.
[0698] Next, for sample A and comparative sample B, laser light was applied from the preparation substrate 14 side (light-shielding layer 15 side). The laser beam was irradiated onto the entire surface of the sample when viewed from above (Fig. 46(C1) and (C2)). During irradiation, a light-shielding mask (not shown) was provided around the outer periphery of the sample.
[0699] A XeCl excimer laser with a wavelength of 308 nm was used as the laser oscillator for the laser light. The focal width on the short axis of the beam is 625 μm, and the energy density is approximately 352 mJ / cm 2 , shot count is 1 0 shots, the repetition frequency was 60 Hz, and the scan speed was 3.75 mm / s.
[0700] The absorptance of the laminated structure of the fabricated substrate 14 and the metal oxide layer 20 for light with a wavelength of 308 nm is On the other hand, the absorptance of the prepared substrate 14 alone at a wavelength of 308 nm was about 51%. %.
[0701] After the laser light is irradiated, a cut is made from the substrate 75a side from the outer periphery to the inside with a cutter. In this way, the preparation substrate 14 was peeled off from each sample (FIGS. 46(D1) and (D2)).
[0702] 48(A) to (F) and 49(A) to (D) are microscopic images of the peeled surface on the side of the preparation substrate 14. Figure 48 (A) to (F) show photographs taken with a digital microscope manufactured by Keyence Corporation. The results of observation using the VHX-100 microscope are shown in Figure 49 (A) to (D). The results of observation using a semiconductor / FPD inspection microscope manufactured by Epson are shown below.
[0703] 48(A) to (C) and 49(A) and (B) show the peeled surface of the preparation substrate 14 side of the sample A. FIG. 48(A) shows a light-shielding layer 15 having a pattern of 300 μm×1100 μm. Similarly, FIG. 48(B) corresponds to the portion where the 820 μm×1000 μm Patterns, Fig. 48(C) and Fig. 49(A) are 1000 μm × 2000 μm patterns, FIG. 49(B) corresponds to a pattern of 220 μm×220 μm.
[0704] As shown in FIGS. 48(A) to (C) and 49(A) and (B), in the sample A, the preparation substrate 1 No film residue of the resin layer 23 was observed on the peeled surface on the side 4. During the irradiation, the light-shielding layer 15 was sometimes removed and sometimes remained. In FIG. 49(C) and FIG. 49(B), the light-shielding layer 1 remaining on the surface opposite to the peeled surface on the side of the fabrication substrate 14 is Five patterns were observed.
[0705] 48(D) to (F) and 49(C) and (D) show the peeling of the preparation substrate 14 side of the comparative sample B. FIG. 48(D) shows a light-shielding layer 1 having a pattern of 300 μm×1100 μm. 5. Similarly, FIG. 48(E) corresponds to the portion where 820 μm×1000 μ 48(F) and 49(C) are 1000 μm × 2000 μm patterns. FIG. 49(D) corresponds to a pattern of 220 μm×220 μm.
[0706] As shown in Figures 48(D) to (F) and Figures 49(C) and (D), in the comparative sample B, Residual film of the resin layer 23 was observed on the peeled surface on the plate 14 side. The resin layer 23 was the same as the light-shielding layer 15. They remained in a position that was roughly overlapping.
[0707] 50(A) to (F) show microscopic photographs of the peeled surface on the substrate 75a side. The digital microscope used was a VHX-100 made by ENS.
[0708] 50(A) to (C) are photographs of the peeled surface of the substrate 75a side of the sample A. ) corresponds to the portion where the light-shielding layer 15 having a pattern of 300 μm×1100 μm was provided. Similarly, FIG. 50(B) shows a pattern of 820 μm×1000 μm, and FIG. 50(C) shows Supports patterns of 1000μm x 2000μm.
[0709] As shown in FIGS. 50(A) to (C), in sample A, the resin layer 23 remains over the entire peeled surface. No damage to the resin layer 23 was observed.
[0710] 50(D) to (F) are photographs of the peeled surface of the substrate 75a side of the comparative sample B. (D) shows the portion where the light-shielding layer 15 having a pattern of 300 μm×1100 μm was provided. Similarly, FIG. 50(E) shows a pattern of 820 μm×1000 μm, and FIG. corresponds to a 1000 μm × 2000 μm pattern.
[0711] As shown in FIGS. 50(D) to (F), in the comparative sample B, the portion where the light-shielding layer 15 was provided A defect in the resin layer 23 was observed at a position roughly overlapping with the above.
[0712] The resin layer 23 may remain in the area overlapping the light-shielding layer 15, or the peeled surface on the side of the substrate 14 may be damaged. The test was conducted on 10 pieces of each size of light-shielding layer. The test results are shown below. Shown in 2.
[0713] [Table 2]
[0714] In the comparative sample B, 10 out of 10 pieces of each of the five sizes of light-shielding layers were In the comparative sample B, when light was irradiated through the substrate 14, the film residue of the substrate 14 was observed. Since the light shielding layer 15 was attached to the light irradiated surface of the substrate 14, uneven light irradiation occurred, and peeling occurred. It appears that the project was not carried out in the desired location.
[0715] Similarly, the peeled surface on the side of the production substrate 14 was inspected for the sample A to which one embodiment of the present invention was applied. As a result, for each of the five different sizes of light-shielding layers, one out of ten had a defect in the resin layer 23. In the sample A to which one embodiment of the present invention is applied, the light of the preparation substrate 14 Even if the light-shielding layer 15 was attached to the irradiated surface, the occurrence of a portion with low peelability could be suppressed.
[0716] <Evaluation 3> Next, a laminate structure to which one embodiment of the present invention is applied (sample C) and a comparative laminate structure (comparative sample D) are ) was prepared, and the resin layer was peeled off from the prepared substrate. The results are described below.
[0717] The preparation method and peeling method of sample C and comparative sample D will be described with reference to FIG. has a metal oxide layer 20, whereas comparative sample D does not have a metal oxide layer 20.
[0718] First, a metal oxide layer 20 was formed on the substrate 14 of the sample C (FIG. 46(A1)). Preparation of Comparative Sample D No metal oxide layer 20 was formed on the substrate 14 (FIG. 46(A2)). .
[0719] The substrate 14 used was a glass substrate having a thickness of about 0.7 mm. A titanium oxide film was formed. Specifically, a titanium oxide film with a thickness of about 20 nm was first formed by sputtering. Next, the surface of the titanium film was treated with H2O plasma to remove the gold. A titanium oxide film was formed as the metal oxide layer 20. The bias power for the H2O plasma treatment was 4500W, ICP power 0W, pressure 15Pa, processing time 600sec. The process gas used was water vapor at a flow rate of 250 sccm. The thickness of the titanium oxide film was about 30 nm. It was.
[0720] Next, in sample C, a resin layer 23 was formed on the metal oxide layer 20 (FIG. 46(A1)). In the comparative sample D, a resin layer 23 was formed on the fabrication substrate 14 (FIG. 46(A2)). The photosensitive material 23 is formed using a material containing a polyimide resin precursor. The thickness of the coating was approximately 2.0 μm. After coating, the coating was heated in a nitrogen atmosphere. Then, the substrate was baked at 450° C. for 1 hour.
[0721] Then, the substrate 75a was attached to the resin layer 23 using the adhesive layer 75b (FIG. 46(A1), (A2)).
[0722] In addition, a black oil-based marker pen was used to mark the light-irradiated surface of the fabrication substrate 14 in a size that was visible to the naked eye. Five light-blocking regions (hereinafter, light-blocking regions) with a diameter of about 1 mm were formed on the substrate. The resin layer 23 was irradiated with laser light through the plate 14. After that, the resin layer 23 was removed from the substrate 14. 3 was peeled off, and it was confirmed whether the resin layer 23 remained on the peeled surface of the fabricated substrate 14.
[0723] As shown in FIG. 51(B), in the comparative sample D, the film of the resin layer 23 was formed on the peeled surface of the fabricated substrate 14. There were five remaining areas (areas surrounded by dotted lines). The remaining film overlapped with the light-shielding area. On the other hand, as shown in FIG. 51(A), no film residue of the resin layer 23 was observed in the sample C. In FIG. 51(A), the light-shielding area on the back surface (the surface opposite to the peeled surface) of the preparation substrate 14 is thin. Although it appears small, no resin layer 23 remained on the peeled surface of the fabricated substrate 14.
[0724] From the results of Evaluation 1, it was found that by applying one embodiment of the present invention, the energy density of the laser light was high. It was also found that the generation of soot can be suppressed even if the temperature is low. By applying one embodiment of the present invention, when a foreign object is present on the light irradiation surface, the energy of the laser light is It was found that the resin layer can be prevented from remaining without increasing the density excessively. As described above, the peeling method of one embodiment of the present invention has a wide range of laser irradiation conditions and is easy to control. In addition, by using the peeling method according to one embodiment of the present invention, the peeling yield can be increased. It is possible. EXAMPLES
[0725] The items shown in Table 3 in the peeling method according to one embodiment of the present invention will be described in detail below.
[0726] [Table 3]
[0727] As shown in Example 1 and the like, H2O plasma treatment is suitable for treating the underlayer. The resin layer is preferably made of a material that has photosensitivity and contains a polyimide resin precursor. Alternatively, the material of the resin layer is preferably a material containing a non-photosensitive soluble polyimide resin. be.
[0728] When the resin layer material is applied, uneven application occurs on the outer periphery of the substrate. It is preferable that such unnecessary portions can be easily removed before the resin layer is cured. For example, it can be removed using an organic solvent such as thinner. In some cases, the paint may react with the thinner and become cloudy, gel, or solidify. The material of the resin layer used in Example 1 is soluble in organic solvents such as paint thinner, so the hardness of the resin layer Unnecessary parts can be easily removed before conversion.
[0729] It is preferable to use a photosensitive material because it makes it easier to process the resin layer. The resin layer can be processed by performing the steps of lithography, exposure, and development. Since the above-mentioned manufacturing process is unnecessary, the manufacturing process can be shortened.
[0730] When using a non-photosensitive material, the material is applied and hardened by heating, and then a resist is applied to the resin layer. A resist mask is formed by applying a resist, exposing it to light, and developing it. The resin layer can be processed by performing chipping.
[0731] A process of forming a peelable layer (transistor, display element, etc.) on a resin layer and laminating it to a substrate During the alignment process, it is preferable that the manufacturing device can easily read the alignment marker. Photosensitive materials may be colored compared to non-photosensitive materials. The resin layer has high transparency for all visible light, making it easy to recognize markers and allowing automatic layout control during design. This increases the degree of freedom, which is preferable.
[0732] In the process of irradiating the entire surface of the resin layer with laser light through the substrate, If there is dirt on the surface opposite to the surface on which the oil layer is formed, the light will not be properly irradiated, resulting in poor peeling. In addition, if the laser power is too strong for the resin layer, the resin layer may be altered. For example, soot may be generated. In this case, a base layer is formed between the substrate and the resin layer. Even if the foreign object is not present, the base layer around the foreign object is heated, and heat is evenly conducted to the entire base layer. Therefore, the laser power does not need to be excessively strong, and the laser light penetrates the resin layer. Therefore, in the peeling method according to one embodiment of the present invention, damage to the back surface of the formation substrate can be suppressed. As shown in Table 2, the oxidation The thermal conductivity of titanium is approximately 6.3 W / m K, and that of polyimide is approximately 0.18 It is in W / m K.
[0733] As shown in Example 1, etc., when peeling occurs at the interface between the metal oxide layer and the resin layer, the work after peeling The resin layer does not remain on the substrate. Depending on the thickness of the metal oxide layer, etc., In this way, the resin layer may remain on the substrate after peeling. be.
[0734] When the resin layer is removed after peeling, the through electrodes can be exposed. In order to remove the resin layer, the finished device is preferably removed by rinsing. It is not affected by the color of the
[0735] In the case where the resin layer is not removed after peeling, it is preferable to expose the through electrodes by peeling. When forming the layer, an opening is provided in the resin layer, and a through electrode is formed in the opening. When using the above-mentioned method, an opening can be formed in the resin layer by exposure technology. When a non-photosensitive material is used, a resist mask is used. In this case, the shape of the opening is nearly vertical. The resin layer and the through electrode are exposed by peeling. It is preferable to use a material that has low adhesion to the substrate. The smaller the area, the better. Since the resin layer is not removed, the finished device will have the same color as the resin layer. When using colored resin, it is necessary to reduce the decrease in light extraction efficiency. It is preferable not to provide a resin layer in an unnecessary portion. If used, the light extraction efficiency is unlikely to decrease even if the resin layer remains, which is preferable. EXAMPLES
[0736] In this example, the results of peeling a resin layer from a production substrate will be described.
[0737] A method for fabricating a sample in this embodiment will be described with reference to FIGS.
[0738] First, a metal oxide layer 20 was formed on a preparation substrate 14 (FIG. 5(A1)).
[0739] The substrate 14 used was a glass substrate having a thickness of about 0.7 mm. A titanium oxide film was formed. Specifically, a titanium oxide film with a thickness of about 20 nm was first formed by sputtering. Next, the surface of the titanium film was treated with H2O plasma to remove the gold. A titanium oxide film was formed as the metal oxide layer 20. The bias power for the H2O plasma treatment was 4500W, ICP power 0W, pressure 15Pa, processing time 600sec. The process gas used was water vapor at a flow rate of 250 sccm.
[0740] Next, a first layer 24 was formed on the metal oxide layer 20 (FIG. 5(B)). The first layer 24 was The film was formed using a material containing a photosensitive acrylic resin. The film thickness of the applied material was approximately It was 2 μm.
[0741] Next, the first layer 24 was subjected to a heat treatment to form a resin layer 23 (FIG. 5(C)). The heat treatment was performed by baking in a N2 atmosphere at 300°C for 1 hour.
[0742] Here, the light transmittance of acrylic resin is shown in Figure 52. The sample is a photosensitive resin on a glass substrate. The material containing the acrylic resin was applied to a film thickness of about 2 μm and left in a N2 atmosphere for 1 hour. The baking temperatures were 250℃, 300℃, and 350℃. As shown in FIG. 52, acrylic resin has high transparency to visible light. The acrylic resin used in the above process, formed by baking at 300°C, has high transparency to visible light. It was found that even if the residual film remains after peeling, it is unlikely to adversely affect the transmittance of visible light.
[0743] Then, a substrate 75a (film) was attached to the resin layer 23 using an adhesive layer 75b (FIG. 5 (D)).
[0744] The sample of this embodiment was irradiated with laser light from the side of the substrate 14 (FIG. 6(A)). The entire surface of the sample was irradiated with the laser light when viewed from the top. A mask (not shown) was provided.
[0745] A XeCl excimer laser with a wavelength of 308 nm was used as the laser oscillator for the laser light. The focal width on the minor axis of the beam was 625 μm, the number of shots was 10, and the repetition frequency was 60 Hz. The scanning speed was 3.75 mm / s. The energy density was approximately 352 mJ / cm 2 And, about 396mJ / cm 2 There were two options:
[0746] In the laminated structure of the substrate 14, the metal oxide layer 20, and the resin layer 23 produced in this embodiment, The absorptance of the light having a wavelength of 308 nm was about 92%. The laser beam is incident on the interface between the metal oxide layer 20 and the resin layer 23, in the metal oxide layer 20, and in the resin layer 23. is thought to have been irradiated.
[0747] The absorptance of light with a wavelength of 308 nm in other structures will also be described. The absorptance of light with a wavelength of 308 nm in the glass substrate used in 14 was approximately 51%. In the laminated structure of the fabricated substrate 14 and the metal oxide layer 20 (titanium oxide film), The light absorption rate of the metal oxide layer 20 is about 76% when the thickness of the metal oxide layer 20 is about 10 nm. When the thickness of the metal oxide layer 20 was about 30 nm, the rate was about 85%. It has been confirmed that the peelability is high, which is thought to be due to the high absorption rate of laser light. do.
[0748] After the laser light irradiation, a cut is made from the substrate 75a side of the sample to the inside from the outer periphery with a cutter. By so doing, the preparation substrate 14 was peeled off from the sample (FIG. 6(B1)).
[0749] In this embodiment, the energy density of the laser light is about 352 mJ / cm 2 and about 396 mJ / cm 2 Under all of the above conditions, the substrate 75a could be peeled off from the preparation substrate 14.
[0750] Figure 53 shows that the energy density of the laser beam is about 352 mJ / cm 2 Photographs of samples under the conditions .
[0751] In Figure 54(A) and (B), the energy density of the laser light is about 352 mJ / cm 2 Testing the conditions Cross-section of material STEM (Scanning Transmission Electron The results of microscopy observation are shown below.
[0752] FIG. 54(A) shows a cross-sectional STEM image of the peeled substrate 75a side. No metal oxide layer 20 was observed between the coating layer 30a formed on the surface of the metal oxide layer 20. In (A), the interface between the resin layer 23 and the coating layer 30a and its vicinity are enclosed by a frame. Energy Dispersive X-ray Spectroscopy (EDX) In the analysis using spectroscopy, a noise level peak was observed on the resin layer 23 side. Since only titanium was detected, it is believed that no titanium remains. The cross-sectional STEM photograph of the side of the fabricated substrate 14 separated from the metal oxide layer 20 is shown. No resin layer 23 was observed between the metal oxide layer 20b and the coating layer 30b. It is believed that separation was achieved at the interface between the resin layer 20 and the resin layer 23.
[0753] From the results of this example, it is clear that the metal oxide layer 20 and the resin layer 2 It was confirmed that the preparation substrate 14 could be peeled off from the interface between the preparation substrate 14 and 3.
[0754] In addition, the energy density is approximately 396 mJ / cm 2 Not only the condition of 352 mJ / cm 2 Even under these conditions, the fabricated substrate 14 can be fabricated with the interface between the metal oxide layer 20 and the resin layer 23. It was confirmed that the film could be peeled off (10 shots each). Processing can be performed with energy densities equivalent to or lower than those used in the laser crystallization process. In addition, the conditions were found to be equal to or greater than those used in the laser crystallization process. It was found that processing was possible with a small number of shots (overlap rate).
[0755] The resin layer used in this embodiment has high light transmittance (particularly high visible light transmittance) and light absorptance. However, the color of the resin layer is lower than that of the colored resin layer. A laminated structure of a metal oxide layer (titanium oxide film) and a resin layer (acrylic film), wavelength 308n The light absorption rate of 1000m was about 92%. A higher absorptance was obtained compared to the absorptance of light with a wavelength of 308 nm (approximately 77%). By providing a metal oxide layer between the resin layer and the metal oxide layer, the laser light absorption rate could be increased.
[0756] As described in the first embodiment with reference to FIGS. 7(A) and 7(B), the light irradiation of the production substrate 14 If dust or other foreign matter 18 adheres to the light-emitting surface, uneven light irradiation may occur. In the configuration of this embodiment, foreign matter such as dust present on the surface of the production substrate to be irradiated with the laser light The effect of this on the peelability of the samples was investigated.
[0757] On the light-irradiated surface of the fabricated substrate 14, a black marker pen was used to mark a spot that was visible to the naked eye (approximately 1 mm in diameter). The sample was prepared in the same manner as above. Then, the resin layer 23 is irradiated with laser light through the fabrication substrate 14 and the metal oxide layer 20. The laser light irradiation conditions were the same as above, and the energy density was about 352 mJ / cm. 2 and Thereafter, the resin layer 23 was peeled off from the fabricated substrate 14, and a film was left on the peeled surface of the fabricated substrate 14. As a result, no residual film was found in the sample of this embodiment. .
[0758] From this result, it is possible to prevent the laser from being damaged when a foreign object is present on the light irradiation surface by applying one embodiment of the present invention. The resin layer 23 can be prevented from remaining without excessively increasing the energy density of the laser light. I found out.
[0759] Even if a foreign object is attached to the light irradiated surface of the production substrate 14, the base layer around the foreign object is heated. Therefore, heat may be conducted evenly throughout the entire base layer. It is believed that the heat transfer to the areas where the adhesive is weak can prevent areas from peeling off. Therefore, as a base layer formed between the preparation substrate 14 and the resin layer 23, It is considered preferable to use a layer having a higher thermal conductivity than the above.
[0760] From the results of this example, it is possible to suppress the film residue and to perform peeling by using the peeling method according to one embodiment of the present invention. It was found that this could increase the yield.
[0761] From the above, in one embodiment of the present invention, special laser processing conditions and special resin materials are not required. It was found that this could prevent the increase in production costs from increasing. In addition, the visible light transmittance was high. Therefore, even if the resin layer is located on the display surface side of the display device, It is possible to achieve high display quality. In addition, colored (colored) wood is used to improve the display quality. The process of removing the fat layer can be omitted. In addition, the range of materials that can be selected for the resin layer is expanded. EXAMPLES
[0762] In this embodiment, a transistor and a flexible OLED display are manufactured by applying one embodiment of the present invention. The results of creating each play will now be explained.
[0763] <Transistor fabrication results> A method for fabricating a sample in this embodiment will be described with reference to FIGS.
[0764] First, a metal layer 19 and a metal oxide layer 20 were formed on a substrate 14 (FIG. 5(A2)). .
[0765] The substrate 14 used was a glass substrate having a thickness of about 0.7 mm. A method for forming the layer 20 will be described. First, a thick layer is formed on the substrate 14 by sputtering. A titanium film with a thickness of about 35 nm was formed. Next, the surface of the titanium film was treated with H2O plasma. The titanium film was partially oxidized to form a titanium oxide film. A laminated structure of the titanium film and the titanium oxide film as the metal oxide layer 20 can be formed. The bias power for the H2O plasma treatment was 4500 W, the ICP power was 0 W, and the pressure was 1 The treatment time was 600 seconds, and the process gas was water vapor at a flow rate of 250 sccm. Used.
[0766] Next, a resin layer 23 was formed on the metal oxide layer 20 (FIG. 5(C)). The film was formed using a material that has optical properties and contains a polyimide resin precursor. The material was applied in two layers to a total thickness of about 4.0 μm. Each layer was heated. Each heat treatment consisted of a base treatment at 450°C for 1 hour in a N2 atmosphere. The survey was carried out.
[0767] Then, a transistor having a bottom gate type channel etch structure was formed on the resin layer 23. (This corresponds to the peeled layer 25 in FIG. 5(D)). The semiconductor layer was made of CAC-OS. The length was 4 μm and the channel width was 3 μm.
[0768] Then, a substrate 75a was attached to the peeled layer 25 using an adhesive layer 75b (FIG. 5(D)).
[0769] The sample of this embodiment was irradiated with laser light from the side of the substrate 14 (FIG. 6(A)). The layer 25 to be peeled off was peeled off from the substrate 14. During the peeling, water was supplied to the peeling interface. Provided.
[0770] A XeCl excimer laser with a wavelength of 308 nm was used as the laser oscillator for the laser light. The focal width on the minor axis of the beam was 625 μm, the number of shots was 10, and the repetition frequency was 60 Hz. The scanning speed was 3.75 mm / s, and the energy density was approximately 440 mJ / cm 2 It was decided.
[0771] The Id-Vg characteristics and field-effect mobility (Fi eld effect mobility)μ FE is shown in Figure 55. In Figure 55, Vd = The results for 0.1 V and Vd = 20 V are shown. In FIG. 55, the Id-Vg characteristics before peeling The Id-Vg characteristics after peeling are shown by a thick solid line, the Id-Vg characteristics after peeling are shown by a thin solid line, and the μ FE The thick dotted line indicates peeling. μ after separation FE In FIG. 55, the thick solid line and the thin solid line are , roughly overlap, and the thick dotted line and the thin dotted line are roughly overlapped. As shown in Figure 55 As shown in the figure, there is no significant change in the characteristics before and after peeling. Even with a channel length of 4 μm, It was found that the device exhibited a -off characteristic.
[0772] <Flexible OLED display fabrication results> The flexible OLED display produced in this example has a display area of 8.67 inches diagonally. The effective pixel count is 1080 x 1920, the resolution is 254 ppi, and the aperture ratio is 46.0%. Flexible OLED display is an active matrix type organic EL display. The display has a built-in scan driver, and the source driver is externally connected using the COF. It is attached.
[0773] A channel-etched transistor using CAC-OS was used as the transistor.
[0774] The light-emitting element used was a tandem (stacked) type organic EL element that emits white light. The LED has a top emission structure, and the light from the light-emitting element is projected onto the display through a color filter. It is taken out of Ray.
[0775] In the method for producing a flexible OLED display of this embodiment, transistors and the like are formed. The substrate on which the color filter is formed is bonded to the substrate on which the color filter is formed, and two peeling steps are performed. By carrying out the above steps, transistors, color filters, etc. are transferred onto the film substrate. In the above, one embodiment of the present invention is applied to a peeling step of a formation substrate on which a transistor or the like is formed. Specifically, a transistor, a light-emitting element, etc. are formed on a substrate via a metal oxide layer and a resin layer. The configurations of the metal oxide layer and the resin layer were the same as those in the fabrication of the above transistor. On the other hand, in the peeling process of the substrate on which the color filter etc. is formed, an inorganic peeling layer (titanium oxide) is used. A stainless steel film was used.
[0776] The display result of the flexible OLED display fabricated in this example is shown in Figure 56. As shown in Figure 6, no display defects due to peeling caused by laser irradiation were observed, and the display was emitting light normally. It was confirmed that this was the case. [Explanation of symbols]
[0777] 10A display device 10B Display device 10C display device 13 Adhesive layer 14 Preparation of substrate 15 Light blocking layer 16 areas 17 areas 18 Foreign object 19 Metal layer 20 Metal oxide layer 21 Liquid supply mechanism 22 Substrate 23 Resin layer 23a Resin layer 23b Resin layer 24 First Layer 25 Layer to be peeled 26 Linear Beam 27 Processing area 28 Adhesive layer 29 Substrate 31 Insulating layer 31a Insulating layer 31b Insulating layer 32 Insulating layer 33 Insulating layer 34 Insulating layer 35 Insulating layer 40 Transistor 41 Conductive layer 43a Conductive layer 43b Conductive layer 43c conductive layer 44 Metal Oxide Layer 45 Conductive Layer 49 Transistor 55 Laser light 56 Laminate 56a Object to be peeled 56b Support 57a First Layer 57b Second Layer 58 Preparation Board 59 Laminated body 60 Light emitting element 61 Conductive layer 62 EL layer 63 Conductive Layer 64 Break 65 Equipment 74 Insulating Layer 75 Protective layer 75a Board 75b Adhesive layer 76 Connectors 80 Transistors 81 Conductive Layer 82 Insulating layer 83 Metal Oxide Layer 84 Insulating Layer 85 Conductive Layer 86a Conductive layer 86b Conductive layer 86c Conductive layer 91 Preparation Board 92 Metal oxide layer 93 Resin layer 95 Insulating Layer 96 Bulkhead 97 Colored layer 98 Light blocking layer 99 Adhesive layer 112 Liquid crystal layer 113 Electrode 115 Insulating Layer 117 Insulating Layer 121 Insulating layer 131 Colored layer 132 Light blocking layer 133a Alignment film 133b Alignment film 134 Colored layer 135 Polarizing Plate 140 Transistor 141 Adhesive layer 142 Adhesive layer 162a Channel Region 162b Low resistance region 163 Insulating Layer 164 Conductive Layer 165 Insulating Layer 166 Insulating Layer 167a conductive layer 167b Conductive layer 170 Light emitting element 180 Liquid crystal element 191 Electrode 192 EL layer 193 Electrode 194 Insulating Layer 201 Transistor 203 Transistor 204 Connection 205 Transistor 206 Transistor 207 Connection 211 Insulating layer 212 Insulating layer 213 Insulating Layer 214 Insulating layer 215 Insulating Layer 216 Insulating Layer 217 Insulating Layer 220 Insulating layer 220a Insulating layer 220b Insulating layer 221a Conductive layer 221b Conductive layer 222a conductive layer 222b Conductive layer 223 Conductive Layer 224 Conductive Layer 225 Insulating Layer 226 Coating membrane 227 Lens 228 Conductive Layer 231 Semiconductor Layer 232 Insulating layer 233 Diffusion Film 234a conductive layer 234b Conductive layer 234c Insulating layer 234d Insulating layer 235 Substrate 242 Connection Layer 243 Connectors 252 Connection 300A display device 310A I / O unit 310B I / O device 311a electrode 311b electrode 311c electrode 351 Substrate 361 Substrate 362 Display section 364 circuits 365 Wiring 372 FPC 373 IC 381 Display section 382 Drive circuit section 451 Aperture 600 Tape 601 Support 602 Tape reel 604 Direction changing roller 606 Pressure Roller 606a Cylinder 606b Cylinder 607 Direction changing roller 609 Carrier Plate 610 Laser irradiation unit 610a Laser light 610b Laser light 610c Laser light 610d Laser Light 610e Linear Beam 613 Reel 614 Drying mechanism 617 Lola 620 Ionizer 630 Substrate Reversal Unit 631 Guide roller 632 Guide roller 633 Guide roller 634 Guide roller 635 Optical system 639 Ionizer 640 Processing area 641 PCB Load Cassette 642 PCB Unload Cassette 643 Transport roller 644 Transport roller 645 Transport roller 646 Transport roller 650 Mirror 659 Liquid supply mechanism 660 Excimer Laser Device 665 Guide Roller 666 Guide Roller 670 Separation Tape 671 Support 672 Tape Reel 673 Reel 674 Guide roller 675 Pressure Roller 676 Directional Roller 677 Guide Roller 678 Guide roller 679 Guide Roller 680 Lens 683 Reel 800 Mobile Information Terminals 801 Case 802 Case 803 Display section 805 Hinge part 810 Mobile Information Terminal 811 Case 812 Display section 813 Operation button 814 External connection port 815 Speaker 816 Mike 817 Camera 820 Camera 821 Case 822 Display section 823 Operation button 824 Shutter button 826 Lens 8000 Display Module 8001 Top cover 8002 Lower cover 8005 FPC 8006 Display Panel 8009 Frame 8010 Printed Circuit Board 8011 Battery 8015 Light emitting part 8016 Light receiving section 8017a Light guiding part 8017b Light guiding section 8018 light 9000 Chassis 9001 Display section 9003 Speaker 9005 Operation key 9006 Connection terminal 9007 Sensor 9008 Microphone 9055 Hinge 9200 Mobile Information Terminal 9201 Portable information terminals 9202 Mobile information terminals
Claims
1. forming a first layer of material over a substrate; forming a second layer of material over the first layer of material; a step of heating the first material layer and the second material layer in a stacked state; and separating the first layer of material from the second layer of material; the first material layer comprising one or more of hydrogen, oxygen, and water; the second material layer includes a resin; In the heating step, water is precipitated at or near the interface between the first material layer and the second material layer, In the step of separating, the first material layer and the second material layer are separated by irradiating water present at or near the interface with light; The method for manufacturing a semiconductor device, wherein the light has a wavelength range of 180 nm or more and 450 nm or less.
2. forming a first layer of material over a substrate; forming a second layer of material over the first layer of material; a step of heating the first material layer and the second material layer in a stacked state; and separating the first layer of material from the second layer of material; the first material layer comprising one or more of hydrogen, oxygen, and water; the second material layer includes a resin; In the heating step, water is precipitated at or near the interface between the first material layer and the second material layer, In the step of separating, the first material layer and the second material layer are separated by irradiating water present at or near the interface with light; The method for manufacturing a semiconductor device, wherein the light has a wavelength range of 308 nm or thereabouts.
Citation Information
Patent Citations
Three-time treated water and method for manufacturing the same
JP2003190943A
Water splitting method and water splitting device
JP2014012626A
Peeling method, and semiconductor device
JP2014187356A
Semiconductor device
JP2015144273A
Laminate, method for producing laminate, and method for producing flexible device using the same
JP2015223823A