Method for manufacturing an electrode assembly for an electrochemical device, an electrode assembly obtained by the method, and a method for manufacturing an electrochemical device
By pressurizing a porous polymer film member with a porosity of 40-70 vol% and forming a separation membrane base material with a thickness reduction to 90% or less, the method addresses deformation and maintains dielectric breakdown voltage, enhancing electrode assembly performance and efficiency.
Patent Information
- Application Number
- JP2023531685
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-02
- Filing Date
- 2022-09-01
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2042-09-01
AI Technical Summary
The challenge in manufacturing electrode assemblies for electrochemical devices is the deformation and thickness reduction of porous polymer film substrates under high-pressure lamination, leading to reduced performance and dielectric breakdown voltage.
A method involving the preparation of a porous polymer film member with a porosity of 40-70 vol% and pressurization to form a separation membrane base material with a thickness reduction to 90% or less, optionally with an organic/inorganic composite coating layer, using a pressure range of 3.0-8.0 MPa, to enhance durability and insulation properties.
The method reduces thickness deformation and maintains dielectric breakdown voltage, improving process efficiency and insulation properties while minimizing damage during lamination, ensuring stable electrode assembly performance.
Smart Images

Figure 0007596536000001 
Figure 0007596536000002
Abstract
Description
[Technical field]
[0001] The present invention claims the benefit of the filing date of Korean Patent Application No. 10-2021-0117235, filed in the Korean Intellectual Property Office on September 2, 2021, the entire contents of which are incorporated herein by reference. The present invention relates to a method for manufacturing an electrode assembly for an electrochemical device, and an electrode assembly manufactured by the method. The present invention also relates to an electrochemical device including the electrode assembly and a method for manufacturing the same. [Background technology]
[0002] Porous polymer film substrates are used as separators for electrochemical devices such as secondary batteries. Typically, electrode assemblies are manufactured through a lamination process in which a separator and an electrode are bonded by heat and pressure, and the higher the heat and pressure applied in this process, the stronger the adhesion between the electrode and the separator. In recent years, as the process speed has increased to improve productivity, the time during which heat is applied to the separator has become shorter, and the adhesive strength is secured by increasing the pressure, but there is a concern that deformation due to high pressure may occur. In addition, during the lamination process, the thickness of the polymer film substrate is significantly reduced and the pores are significantly damaged, which reduces not only the performance of the battery but also the dielectric breakdown voltage of the separator, resulting in problems such as high-pot (high voltage) failure and low-voltage failure. Therefore, there is a need to develop a porous polymer film substrate for separators that is less deformed even under high-pressure lamination conditions. Summary of the Invention [Problem to be solved by the invention]
[0003] An object of the present invention is to provide a separator substrate having a low rate of change in thickness or deformation during a lamination process for manufacturing an electrode assembly and a high breakdown voltage, and an electrode assembly including the separator substrate. Another object of the present invention is to provide a method for manufacturing an electrode assembly having improved performance as described above. Another object of the present invention is to provide an electrochemical device including the electrode assembly and a method for manufacturing the same. It will be readily understood that the objects and advantages of the present invention can be achieved by the means or methods recited in the claims and combinations thereof. [Means for solving the problem]
[0004] A first aspect of the present invention relates to a method for manufacturing an electrode assembly for an electrochemical device, the method comprising: (S100) preparing a porous polymer film member; (S200) compressing the polymer film member to form a porous separator substrate to manufacture a separator for an electrochemical device; and (S300) manufacturing an electrode assembly including the separator, a positive electrode, and a negative electrode; The polymer film member in the step (S100) has a porosity of 40 vol% to 70 vol%, The thickness of the separation membrane substrate after the step (S200) is 90% or less of the thickness of the polymer film member before the pressure application.
[0005] A second aspect of the present invention relates to the first aspect, further comprising a step of forming an organic / inorganic composite coating layer including inorganic particles and a binder resin on one or both sides of the polymer film member obtained in the step (S200).
[0006] A third aspect of the present invention is the first or second aspect, wherein the porosity of the porous separator substrate after performing the step (S200) is 30 vol % to 60 vol %.
[0007] A fourth aspect of the present invention is directed to any one of the first to third aspects, wherein (S200) is performed using a pressure roller or a pressure jig.
[0008] A fifth aspect of the present invention is any one of the first to fourth aspects, wherein (S200) is carried out by a hot pressing method.
[0009] A sixth aspect of the present invention is any one of the first to fifth aspects, wherein the pressurization is carried out at a pressure in the range of 3.0 MPa to 8.0 MPa.
[0010] A seventh aspect of the present invention is any one of the first to sixth aspects, wherein the polymeric film member contains a polyolefin resin.
[0011] An eighth aspect of the present invention is any one of the first to seventh aspects, wherein the polymer film member is manufactured by a wet manufacturing method in which pores are formed by extracting a pore-forming agent.
[0012] A ninth aspect of the present invention is any one of the first to eighth aspects, wherein the polymer film member is manufactured by a dry manufacturing method in which a polymer resin is melted / extruded and then stretched to form pores.
[0013] A tenth aspect of the present invention relates to an electrode assembly for an electrochemical element, the electrode assembly being obtained by a method according to any one of the first to ninth aspects, and including a separator, a positive electrode, and a negative electrode, and the separator includes a porous separator substrate.
[0014] An eleventh aspect of the present invention relates to an electrode assembly for an electrochemical element, the electrode assembly being obtained by a method according to any one of the second to ninth aspects, and the separator comprising the porous separator substrate and an organic / inorganic composite coating layer on one or both sides of the porous separator substrate, the organic / inorganic composite coating layer comprising inorganic particles and a binder resin.
[0015] A twelfth aspect of the present invention relates to a method for manufacturing an electrochemical device, the method including an electrode assembly obtained by a method according to any one of the first to ninth aspects, the electrode assembly including a separator, a positive electrode, and a negative electrode, and the separator includes a porous separator substrate.
[0016] In a thirteenth aspect of the present invention, in the twelfth aspect, the electrode assembly is manufactured by disposing a separator between a positive electrode and a negative electrode and laminating them.
[0017] A fourteenth aspect of the present invention relates to a method for manufacturing an electrochemical device, the electrode assembly comprising: an electrode assembly obtained by the method according to the second aspect, the electrode assembly comprising a separator, a positive electrode, and a negative electrode; the separator comprises a porous separator substrate and an organic / inorganic composite coating layer on one or both sides of the porous separator substrate; and the organic / inorganic composite coating layer comprises inorganic particles and a binder resin. Effect of the Invention
[0018] The method for manufacturing an electrode assembly according to the present invention uses a pre-compressed separator substrate, so that the separator thickness is reduced due to the pressure applied during the lamination process for manufacturing the electrode assembly. Therefore, the separator of the electrode assembly according to the manufacturing method has excellent insulation characteristics without a decrease in dielectric breakdown voltage. Furthermore, even if a high voltage is applied during the lamination process, the separator is less damaged, and the process speed can be increased, improving processability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will be described in detail below. Prior to that, the terms or words used in the present specification and claims should not be interpreted limited to their ordinary or dictionary meanings, but should be interpreted with a meaning and concept that matches the technical idea of the present invention, in accordance with the principle that the inventor can appropriately define the concept of the term to best describe his / her invention. Therefore, it should be understood that the embodiments described in this specification and the configurations shown in the drawings are merely the most preferred embodiments of the present invention, and do not fully represent the technical idea of the present invention, and therefore there may be various equivalents and modifications that can replace them at the time of this application.
[0020] Throughout the specification of this application, when a part is said to "comprise" certain elements, this means that it can further include other elements, rather than excluding other elements, unless specifically stated to the contrary.
[0021] In addition, the terms "about," "substantially," and the like used throughout the specification of this application are used to mean a numerical value or a approximation thereof when the manufacturing and material tolerances inherent in the stated meaning are given, and are used to prevent unscrupulous infringers from unfairly exploiting the disclosure in which precise or absolute numerical values are stated to aid in the understanding of this application.
[0022] Throughout the specification of this application, the phrase "A and / or B" means "A or B, or both."
[0023] In the present specification, porous properties mean that the object contains a plurality of pores with an interconnected structure between the pores that allows the passage of gas and / or liquid fluids from one side of the object to the other side.
[0024] The present invention relates to a separator substrate applicable to a separator of an electrode assembly for an electrochemical device, and an electrode assembly including the separator substrate. The present invention also relates to an electrochemical device including the electrode assembly. Finally, the present invention also relates to a method for manufacturing the electrode assembly and the electrochemical device. In the present invention, the electrochemical device is a device that converts chemical energy into electrical energy by an electrochemical reaction, and is a concept that encompasses primary batteries and secondary batteries. In this specification, the secondary battery is capable of being charged and discharged, and refers to a lithium ion secondary battery, a nickel-cadmium battery, a nickel-hydrogen battery, etc.
[0025] In the present specification, the separator has a porous property including a plurality of pores and serves as a porous ion-conducting barrier that allows ions to pass while blocking electrical contact between the negative electrode and the positive electrode in the electrochemical device.
[0026] In the present invention, the separator of the electrode assembly includes a porous separator substrate. As described below, the separator substrate is prepared by pressing a porous polymer film member. In addition, the separator may have another layer additionally disposed on at least one surface of the separator substrate depending on the material or function. In one embodiment of the present invention, the separator may have an organic / inorganic composite coating layer including inorganic particles and / or a binder resin formed on at least one or both surfaces of the porous substrate.
[0027] Next, a manufacturing method of an electrode assembly according to the present invention and the electrode assembly according to the manufacturing method will be described in more detail.
[0028] The method for manufacturing an electrode assembly according to the present invention includes the steps of: (S100) preparing a polymer film member; (S200) compressing the polymer film member to form a porous separator substrate to manufacture a separator for an electrochemical device; and (S300) manufacturing an electrode assembly including the separator, a positive electrode, and a negative electrode;
[0029] The polymer film member in the (S100) step has a porosity of 40 vol% to 70 vol%, and the thickness of the separation membrane substrate obtained after performing the (S200) step is smaller than the thickness of the polymer film member before the pressurization.
[0030] The polymer film member is a porous membrane containing a polymer material, and from the standpoint of battery output and cycle characteristics, may have a porosity of 40 vol % to 70 vol %.
[0031] In the present invention, the term "porosity" means the ratio of the volume occupied by pores to the total volume, and is expressed in units of vol%. It can be used in the same sense as terms such as porosity and porosity. In the present invention, the measurement of the porosity is not particularly limited, and can be measured, for example, by a BET (Brunauer-Emmett-Teller) measurement method using nitrogen gas or a mercury penetration method (Hg porosimeter) according to one embodiment of the present invention. Alternatively, in one embodiment of the present invention, the true density of the electrode active material layer is calculated from the density (apparent density) of the obtained electrode (electrode active material layer), the composition ratio of the materials contained in the electrode (electrode active material layer), and the density of each component, and the porosity of the electrode active material layer can be calculated from the difference between the apparent density and the true density (net density).
[0032] In one embodiment of the present invention, the polymer film member may have a pore diameter of 10 nm to 100 nm. The pore size may be calculated from a pore size distribution measured using a capillary flow porometer. For example, a separation membrane substrate to be measured is first wetted with a wetting agent such as Galwick solution, and then the air pressure on one side of the substrate is gradually increased. At this time, when the applied air pressure becomes greater than the capillary attraction of the wetting agent present in the pores, the wetting agent blocking the pores is expelled, and the pore size and distribution can be measured based on the pressure and flow rate at the moment of expulsion. In one embodiment, the air pressure may be controlled to a range of 30 to 450 psi.
[0033] In the present invention, the polymer film substrate may have a thickness of 5 μm to 30 μm. If the thickness of the porous substrate is less than this range, it is difficult to ensure a suitable thickness for the separation membrane substrate after pressure application, while if the thickness is too much greater than this range (i.e., too thick), the resistance of the separation membrane may increase excessively.
[0034] Meanwhile, in one embodiment of the present invention, the polymer material may contain a thermoplastic resin from the viewpoint of imparting a shutdown function, which refers to a function in which, when the battery temperature becomes high, the polymer resin melts and blocks the pores of the porous substrate, thereby blocking the movement of ions between the positive electrode and the negative electrode, thereby preventing thermal runaway of the battery.
[0035] As such a thermoplastic resin, a thermoplastic resin having a melting point of less than 200°C can be used, and in particular, a polyolefin-based polymer resin can be included. Examples of the polyolefin-based polymer resin include polyethylene, polypropylene, polypentene, etc. In one embodiment of the present invention, the thermoplastic resin can include two or more selected from polyethylene, polypropylene, and polypentene.
[0036] Meanwhile, in a specific embodiment of the present invention, the polymer film member may further include at least one polymer resin, such as polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyether sulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalene, as necessary.
[0037] In one embodiment of the present invention, the polymer film member may be manufactured by a method (dry method) in which a polymer material is melt-extruded to form a sheet, and then stretched to induce microcracks between lamellae, which are crystalline parts of the polymer, to form micropores, or by a method (wet method) in which a polymer material is kneaded with a plasticizer at high temperature to form a single phase, and the polymer material and the plasticizer are phase-separated during cooling, and the plasticizer is extracted to form pores.
[0038] After the polymer film member is prepared as described above, it is then compressed to prepare a porous separator substrate (S200).
[0039] In one embodiment of the present invention, the pressing is preferably performed by a surface pressure method rather than a line pressure, in order to apply a constant and uniform pressure over the entire surface of the polymer film member. Specifically, the pressing can be performed using a flat jig. The pressing can also be performed by a hot pressing method. For example, the pressing can be performed by a hot press method. In one embodiment of the present invention, in the pressing step, the temperature can be adjusted within a range of about 50°C to 80°C, the pressure can be adjusted within a range of 3.0MPa to 8.0MPa, and the time can be adjusted within a range of 1 second to 20 seconds. The temperature, pressure, and time conditions are independently controlled. However, the pressing step conditions of the present invention are not limited to the above ranges, and can be appropriately adjusted within a range in which a porous separator substrate having an appropriate thickness and porosity can be obtained by pressing the polymer film member.
[0040] In the present invention, the thickness of the separation membrane substrate obtained after performing the step (S200) is smaller than that of the polymer film member before the pressure application. In a specific embodiment of the present invention, the thickness of the separation membrane substrate may be 99% to 70% of the thickness of the polymer film member before the pressure application.
[0041] Meanwhile, in the present invention, the porosity of the porous separator substrate after the step (S200) may be 50 vol% to 80 vol% of the porosity of the polymer film member, and the porosity of the porous separator substrate after the step (S200) may be 30 vol% to 60 vol%.
[0042] Meanwhile, in one embodiment of the present invention, the separator may further include an organic / inorganic composite coating layer formed on at least one surface of the separator substrate.
[0043] The organic / inorganic composite coating layer includes a binder resin and inorganic particles, and has a porous characteristic. In one embodiment of the present invention, the organic / inorganic composite coating layer may include the binder resin and the inorganic particles in a weight ratio of 1:99 to 30:70. The ratio may be appropriately adjusted within the above range, and for example, the total of the binder resin and the inorganic particles is 100 wt%, the binder resin may be 1 wt% or more, 5 wt% or more, or 10 wt% or more, and the inorganic particles may be 80 wt% or more, 85 wt% or more, 90 wt% or more, or 95 wt% or more.
[0044] The organic / inorganic composite coating layer may be formed by binding inorganic particles with a binder resin and accumulating on the sides, and the pores in the organic / inorganic composite coating layer may be due to interstitial volumes, which are void spaces between the inorganic particles.
[0045] In one embodiment of the present invention, the porosity of the organic / inorganic composite coating layer may be 30vol% to 70vol%. If the porosity is 70vol% or less, it is possible to ensure mechanical properties that can withstand the pressing process for bonding with the electrode, and since the surface opening ratio is not too high, it is suitable for ensuring adhesive strength. On the other hand, if the porosity is 30vol% or more, it is advantageous in terms of ion permeability.
[0046] The organic / inorganic composite coating layer may have a thickness of 1 μm to 20 μm on either side of the separator substrate, but is not limited thereto. The thickness can be adjusted to an appropriate range by those skilled in the art in terms of heat resistance and electrical resistance.
[0047] In the present invention, non-limiting examples of binder resins that can be used in the organic / inorganic composite coating layer include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene-vinyl acetate copolymer, polyethylene oxide, and the like. Examples of the polymer resin include any one selected from the group consisting of polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, and carboxyl methyl cellulose, or a mixture of two or more of these polymer resins, but are not limited thereto.
[0048] In a specific embodiment of the present invention, the inorganic particles usable in the organic / inorganic composite coating layer are not particularly limited as long as they are electrochemically stable. That is, the inorganic particles usable in the present invention are within the range of the operating voltage of the applied electrochemical device (for example, Li / Li + There are no particular limitations as long as the oxidation and / or reduction reaction does not occur at a potential of 0 to 5 V relative to the reference potential.
[0049] Non-limiting examples of the inorganic particles include BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT, 0 <x<1、0<y<1)、Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, SiC, Al(OH)3, TiO2, aluminum peroxide, zinc tin hydroxide (ZnSn(OH)6), tin-zinc oxide (Zn2SnO4, ZnSnO3), antimony trioxide (Sb2O3), antimony tetroxide (Sb2O4), antimony pentoxide (Sb2O5), etc., and one or more of these may be included.
[0050] In addition, the average diameter of inorganic particles (D 50 ) is not particularly limited, but is preferably in the range of 0.3 μm to 1 μm in order to form a coating layer of uniform thickness and to have a suitable porosity. If it is less than 0.3 μm, the dispersibility of inorganic particles in the slurry prepared for producing an organic / inorganic composite coating layer may decrease, and if it exceeds 1 μm, the thickness of the coating layer formed may increase.
[0051] In one embodiment of the present invention, the organic / inorganic composite coating layer may be formed, for example, as follows. First, a binder resin is dissolved in a suitable organic solvent to prepare a polymer solution. The solvent preferably has a solubility index similar to that of the binder polymer to be used and a low boiling point. This is to facilitate uniform mixing and subsequent solvent removal. Non-limiting examples of usable solvents include acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or a mixture thereof.
[0052] Next, inorganic particles are added and dispersed in the prepared polymer solution. In the present invention, the content ratio of the inorganic particles to the binder is as described above, and is appropriately adjusted in consideration of the thickness, pore size, and porosity of the organic / inorganic composite coating layer of the present invention to be finally prepared.
[0053] Next, the inorganic particle slurry prepared as above is applied to at least one side of the prepared separation membrane substrate and dried. The method of applying the slurry to the surface of the separation membrane substrate is not limited to any particular method, and any common method known in the art can be used. For example, various methods such as dip coating, die coating, roll coating, comma coating, or a combination thereof can be used.
[0054] The drying process is performed by appropriately setting temperature and time conditions to minimize the occurrence of surface defects in the organic / inorganic composite coating layer, and drying auxiliary devices such as a drying oven or hot air may be used within an appropriate range.
[0055] After preparing the separator as described above, an electrode assembly including the separator, a positive electrode, and a negative electrode is manufactured (S300).
[0056] As described above, the method for manufacturing an electrode assembly according to the present invention pressurizes a polymer film member and uses the resultant product as a separator substrate. The separator substrate is prepared by being pressurized before being used in the manufacture of an electrode assembly, so that thickness deformation of the separator can be reduced during a lamination process for manufacturing an electrode assembly. In addition, when the separator includes an organic / inorganic composite porous layer, damage caused by pressure of inorganic particles on a surface of the separator substrate facing the organic / inorganic composite porous layer during a lamination process can be reduced.
[0057] The electrode assembly can be manufactured by a lamination process in which the separator obtained by the above-mentioned method is interposed between the negative electrode and the positive electrode, and the layers are bonded by applying heat and / or pressure. In one embodiment of the present invention, the lamination process can be performed by a roll press device including a pair of pressure rollers. That is, the negative electrode, the separator, and the positive electrode can be sequentially laminated and then inserted between the pressure rollers to achieve interlayer bonding. At this time, the lamination process can be performed by a hot pressing method. As described above, since the separator substrate is pressurized and prepared before the lamination process for manufacturing the electrode assembly, thickness deformation of the separator due to pressure applied in the lamination process can be reduced, and damage to the surface of the porous substrate due to the pressure of inorganic particles contained in the organic / inorganic composite porous layer can be reduced.
[0058] Meanwhile, the present invention provides a secondary battery including the electrode assembly, the battery including an electrode assembly including an anode, a cathode, and a separator interposed between the anode and the cathode, the separator including a separator substrate obtained by pressing a polymer film member as described above.
[0059] In the present invention, the positive electrode comprises a positive electrode current collector and a positive electrode active material layer on at least one surface of the current collector, the positive electrode active material layer including a positive electrode active material, a conductive material, and a binder resin. The positive electrode active material may be a layered compound such as lithium manganese composite oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; 1+x Mn 2-x Lithium manganese oxides such as LiMnO4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, and Cu2V2O7; and the chemical formula LiNi 1-x M x Lithium nickel oxide with Ni site represented by the chemical formula LiMnO2 (where M=Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x=0.01 to 0.3); 1-x M x The compounds may include one or a mixture of two or more of the following: lithium manganese composite oxides represented by Li2Mn3MO8 (where M is Co, Ni, Fe, Cr, Zn, or Ta, and x is 0.01 to 0.1) or Li2Mn3MO8 (where M is Fe, Co, Ni, Cu, or Zn); LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion; disulfide compounds; and Fe2(MoO4)3.
[0060] In the present invention, the negative electrode comprises a negative electrode current collector and a negative electrode active material layer on at least one surface of the current collector, the negative electrode active material layer including a negative electrode active material, a conductive material, and a binder resin. The negative electrode comprises a lithium metal oxide, carbon such as non-graphitizable carbon and graphite-based carbon; LixFe2O3 (0≦x≦1), LixWO2 (0≦x≦1), Sn x Me 1-x Me' y O zMetal composite oxides such as (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Group 1, Group 2, Group 3 elements of the periodic table, halogen; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8), etc.; lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, and Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials; one or more mixtures selected from titanium oxides can be included.
[0061] In a specific embodiment of the present invention, the conductive material can be, for example, any one selected from the group consisting of graphite, carbon black, carbon fiber or metal fiber, metal powder, conductive whisker, conductive metal oxide, activated carbon, and polyphenylene derivative, or a mixture of two or more of these conductive materials. More specifically, it can be one or a mixture of two or more conductive materials selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide.
[0062] The current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery. For example, stainless steel, copper, aluminum, nickel, titanium, fired carbon, or those surface-treated with carbon, nickel, titanium, silver, etc. on the surface of aluminum or stainless steel can be used.
[0063] The binder resin may be a polymer commonly used in electrodes in the art. Non-limiting examples of such binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene-vinyl acetate copolymer, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. Examples of suitable cellulose acetate copolymers include, but are not limited to, cyanoethyl acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, and carboxyl methyl cellulose.
[0064] The electrode assembly prepared as above can be placed in a suitable case and an electrolyte can be injected to manufacture a battery.
[0065] In the present invention, the electrolyte is A+ B - A salt having the structure: + Li + , Na + , K + or a combination thereof, such as B - PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2)2 - , C(CF2SO2)3 - or a combination thereof, dissolved or dissociated in an organic solvent such as, but not limited to, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma butyrolactone (g-butyrolactone), or a mixture thereof.
[0066] The present invention also provides a battery module including a battery having the electrode assembly as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source. Specific examples of the device include, but are not limited to, a power tool powered by a battery-type motor, electric vehicles including electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), and the like, electric two-wheeled vehicles including electric bicycles (E-bikes) and electric scooters (E-scooters), electric golf carts, and power storage systems.
[0067] The present invention will be described in detail below with reference to examples. However, the examples of the present invention can be modified in various different forms, and the scope of the present invention should not be construed as being limited to the examples detailed below. The examples of the present invention are provided to more completely explain the present invention to those having ordinary skill in the art. EXAMPLES
[0068] 1. Preparation of separation membrane substrate Polymer film members (thickness: about 15 μm) made of polyethylene were prepared as shown in Table 1 below. Each of these was pressurized using a hot press to change the thickness. The thickness reduction rate was calculated using Equation 1 below. The pressurization was performed under conditions of 60° C., 5.2 MPa, and 10 seconds.
[0069] [Number 1] Thickness reduction rate = {(thickness of polymer film member - thickness of porous substrate) / thickness of polymer film member} x 100
[0070] [Table 1]
[0071] 2.Separation membrane production Next, an organic / inorganic composite coating layer was formed on the surface of the separation membrane substrate obtained in each Example and Comparative Example to prepare a separation membrane.
[0072] PVDF-HFP was prepared as a binder resin and added to acetone, a solvent, to prepare a polymer solution with a solid concentration of 18 wt%. Inorganic particles, Al2O3, were added to the polymer solution to prepare a slurry for forming a coating layer. The binder resin and inorganic particles in the slurry were in a ratio of 10:90 based on the weight ratio. The slurry was then applied to both sides of each separation membrane substrate and dried to form an organic / inorganic composite coating layer with a thickness of 8 μm.
[0073] 3. Manufacturing the electrode assembly 1) Manufacturing of positive electrodes Cathode active material (LiNi 0.8 Mn 0.1 Co 0.1 O2), conductive material (carbon black), dispersant, and binder resin (a mixture of PVDF-HFP and PVDF) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for a positive electrode active material layer with a concentration of 50 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of an aluminum thin film (thickness 10 μm) and dried to prepare a positive electrode having a positive electrode active material layer (thickness 120 μm).
[0074] 2) Manufacturing of negative electrodes Graphite (a blend of natural graphite and artificial graphite), conductive material (carbon black), dispersant, and binder resin (a mixture of PVDF-HFP and PVDF) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for the negative electrode active material layer with a concentration of 50 wt% of the remaining components excluding water. The slurry was then applied to the surface of a copper thin film (thickness 10 μm) and dried to prepare a negative electrode having a negative electrode active material layer (thickness 120 μm).
[0075] 3) Lamination process The negative electrode and the positive electrode were laminated with a separator interposed therebetween to obtain an electrode assembly, which was then subjected to a lamination process at 70° C. and 5.2 MPa for 10 seconds using a hot press.
[0076] 4. Physical property evaluation The negative and positive electrodes were peeled off from the obtained electrode assembly, and the separator was taken out. The organic / inorganic composite coating layer of the separator was then removed using acetone to obtain a porous substrate.
[0077] [Table 2]
[0078] In Table 2, the thickness reduction rate after lamination is a comparison between the thickness (A) of the porous substrate before the manufacture of the electrode assembly and the thickness (B) of the porous substrate obtained by separating the porous substrate after the manufacture of the electrode assembly, and is expressed as a percentage by dividing the difference between A and B by A.
[0079] The laminate air permeability was measured by measuring the air permeability of the porous substrate after removing the organic / inorganic composite coating layer, using an EG01-55-1MR device manufactured by Asahi Seiko Co., Ltd.
[0080] The ER after deformation was measured by measuring the resistance of the porous substrate after removing the organic / inorganic composite coating layer. The obtained porous substrate was placed between SUS plates, and an electrolyte was poured into the coin cell to prepare it. The resistance (ER) was measured by EIS. The frequency was in the range of 100,000 to 10,000 Hz.
[0081] When the porosity of the polymer film member is low, the thickness reduction rate is small when the polymer film member is compressed in the thickness direction. However, when the initial porosity is low, the pressure is applied to the polymer film member, and the air permeability and resistance increase, resulting in a decrease in cell performance.
[0082] Meanwhile, in the case of Comparative Example 3, the initial porosity was large and the porosity was still high even after the thickness was reduced by pressing, so the thickness was further reduced significantly during the lamination process in the manufacture of the electrode assembly, which may affect the performance degradation and safety due to continuous deformation even after the manufacture of the battery.
[0083] Meanwhile, when the porosity of the polymer film member is 40vol% to 70vol%, appropriate porosity can be secured even after the separator substrate and electrode assembly are manufactured, and there is little concern about further deformation.In addition, appropriate levels of air permeability and resistance are achieved during battery manufacturing, ensuring physical properties suitable for battery operation.
Claims
1. (S100) preparing a porous polymer film member; (S200) compressing the polymer film member to form a porous separator substrate to manufacture a separator for an electrochemical device; and (S300) manufacturing an electrode assembly including the separator, a positive electrode, and a negative electrode; The polymer film member in the step (S100) has a porosity of 40 vol% to 70 vol%, The thickness of the separation membrane substrate after the step (S200) is 90% or less of the thickness of the polymer film member before the pressure is applied; The pressurization is performed at a pressure in the range of 3.0 MPa to 8.0 MPa and at a temperature in the range of 50° C. to 80° C.
2. 2. The method of claim 1, further comprising the step of forming an organic / inorganic composite coating layer comprising inorganic particles and a binder resin on one or both sides of the polymer film member obtained in the step (S200).
3. 2. The method of claim 1, wherein the porosity of the separator substrate after performing step (S200) is 30 vol % to 60 vol %.
4. 2. The method of claim 1, wherein the step (S200) is performed using a pressure roller or a pressure jig.
5. 2. The method of claim 1, wherein the step (S200) is performed by hot pressing.
6. The polymer film member is manufactured by a wet manufacturing method in which a pore-forming agent is extracted to form pores, 2. The method for manufacturing an electrode assembly for an electrochemical device according to claim 1, wherein the polymer film member comprises a polyolefin resin.
7. 2. The method of claim 1, wherein the polymer film member is manufactured by a dry manufacturing method in which a polymer resin is melted and extruded, and then stretched to form pores.
8. A method for manufacturing an electrochemical device, comprising: an electrode assembly obtained by the method according to any one of claims 1 to 7, the electrode assembly comprising a separator, a positive electrode, and a negative electrode, the separator comprising a porous separator substrate.
9. 9. The method of claim 8, wherein the electrode assembly is manufactured by laminating a separator between a positive electrode and a negative electrode.
10. 3. A method for manufacturing an electrochemical device, comprising: an electrode assembly obtained by the method of claim 2, the electrode assembly comprising a separator, a positive electrode, and a negative electrode; the separator comprising a porous separator substrate and an organic / inorganic composite coating layer on one or both sides of the porous separator substrate; and the organic / inorganic composite coating layer comprising inorganic particles and a binder resin.
Citation Information
Patent Citations
Separator and non-aqueous electrolyte secondary battery using same
JP1997050800A
Porous polymer film and battery separator
JP2010077335A
Nonaqueous electrolyte secondary battery separator
JP2018181546A
Method for manufacturing all-solid-state battery including solid-liquid hybrid electrolyte membrane, and solid-liquid hybrid electrolyte membrane
JP2022542178A
A separator for an electrochemical device and an electrochemical device comprising the same
KR1020200007745A