Oxide Complex
By supporting inorganic oxide particles around silver particles with controlled properties, the composite stabilizes silver nanoparticles, enhancing resistance to elution, maintaining antibacterial and antiviral efficacy, and ensuring transparency and adhesion.
Patent Information
- Application Number
- JP2024053056
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2044-03-28
AI Technical Summary
Existing technologies face challenges in maintaining the stability of silver nanoparticles in liquids, preventing their elution into water, while ensuring antibacterial and antiviral properties, adhesion to substrates, and maintaining transparency.
A structure is developed where inorganic oxide fine particles, such as titania, are supported around silver particles, with controlled primary and secondary particle sizes, surface coverage, and random distribution, enhancing dispersion stability and adhesion.
The oxide composite achieves improved resistance to silver elution, maintains antibacterial and antiviral properties, and ensures high transparency and adhesion to substrates.
Smart Images

Figure 0007596581000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an oxide composite. [Background technology]
[0002] Patent Document 1 discloses metal nanoparticle-supported titania nanoparticles in which metal nanoparticles are supported on the surface of titania nanoparticles, the titania nanoparticles having acyloxy groups bonded to at least some of the titanium atoms present on the surface, and when the titania nanoparticles are heated to 600°C using a simultaneous differential thermal and thermogravimetric analyzer, a mass loss at 200°C or higher is 5% by mass or more, and the metal nanoparticles are supported on the surface in an amount of 90% by mass or less relative to the titanium oxide in the titania nanoparticles, and a photocatalyst containing the metal nanoparticle-supported titania nanoparticles. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2021-154233 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide an oxide composite having improved resistance to silver elution in water, improved adhesion to a substrate, and improved transparency. [Means for solving the problem]
[0005] The present invention encompasses the following oxide complexes:
[0006] Section 1. An oxide composite, (A) A part of the surface of the silver fine particles is covered with (B) inorganic oxide fine particles, The (A) silver fine particles have an average primary particle diameter of 1 nm to 1,000 nm, The (B) inorganic oxide fine particles have an average primary particle diameter of 1 nm to 100 nm. Oxide complex.
[0007] Section 2. 2. The oxide composite according to item 1, wherein the (A) silver fine particles have an average primary particle size of 1 nm to 200 nm.
[0008] Section 3. 2. The oxide composite according to item 1, wherein the (A) silver fine particles have a surface coverage of 1 surface % or more.
[0009] Section 4. 2. The oxide composite according to item 1, wherein the (A) silver fine particles have a surface coverage of 5 surface % to 95 surface %.
[0010] Section 5. The ratio of the average primary particle size of the (A) silver fine particles to the average primary particle size of the (B) inorganic oxide fine particles ((A) average primary particle size of silver fine particles / (B) average primary particle size of inorganic oxide fine particles) is 2. The oxide composite according to item 1, wherein the ratio is 0.5 or more.
[0011] Section 6. The ratio of the average primary particle size of the (A) silver fine particles to the average primary particle size of the (B) inorganic oxide fine particles ((A) average primary particle size of silver particles / (B) average primary particle size of inorganic oxide) is 2. The oxide composite according to item 1, wherein the molecular weight is 1 or more and 200 or less.
[0012] Section 7. 2. The oxide composite according to item 1, wherein the (B) inorganic oxide fine particles covering the (A) silver fine particles have a random ratio of 50% or more.
[0013] Section 8. A mass ratio of the silver mass (Ag mass) in the silver fine particles (A) to the titanium oxide mass (TiO2 mass) in the inorganic oxide fine particles (B) ((A) Ag mass in silver particles / (B) TiO2 mass in inorganic oxide particles) is 2. The oxide complex according to item 1, wherein the Mn content is ≦10 (10 or less).
[0014] Section 9. In the oxide composite, 2. The oxide composite according to item 1, wherein the sum of the solid contents of the (A) silver fine particles and the (B) inorganic oxide fine particles is 50 mass % or less.
[0015] Section 10. 2. The oxide composite according to item 1, wherein the (B) inorganic oxide fine particles are (B1) titania fine particles.
[0016] Section 11. The (B1) titania fine particles are The surface is protected with organic acid. The mass of the organic acid is 1% by mass or more relative to the weight of the titanium oxide. Item 11. The oxide composite according to item 10.
[0017] Section 12. The organic acid is At least one organic acid selected from the group consisting of monocarboxylic acids having 1 to 4 carbon atoms and hydroxycarboxylic acids having 2 to 3 carbon atoms, or An acyloxy group derived from at least one organic acid selected from the group consisting of monocarboxylic acids having 1 to 4 carbon atoms and hydroxycarboxylic acids having 2 to 3 carbon atoms. Item 12. The oxide complex according to item 11,
[0018] Section 13. Item 12. The oxide complex according to item 11, wherein the organic acid is at least one organic acid selected from the group consisting of acetic acid and lactic acid.
[0019] Section 14. 11. The oxide composite according to item 10, wherein the (B1) titania fine particles are positively charged.
[0020] Section 15. The oxide composite according to any one of items 1 to 14, and water, A dispersion containing 0.5% by mass or more of water.
[0021] Section 16. Item 16. The dispersion according to item 15, wherein the pH of the dispersion is 1 to 8.
[0022] Section 17. The oxide composite according to any one of items 1 to 14, or The dispersion according to any one of items 15 to 16. Paint containing.
[0023] Section 18. Item 18. A coating film formed by the coating material according to item 17.
[0024] The present invention relates to an oxide composite in which the surface of fine silver particles is partially coated with fine inorganic oxide particles (fine titanium oxide particles, etc.). The oxide composite of the present invention has improved resistance to dissolution of the silver compound in water and improved adhesion to a substrate. Effect of the Invention
[0025] The present invention makes it possible to provide an oxide composite having improved resistance to dissolution of a silver compound in water, improved adhesion to a substrate, and the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The present invention will be described in detail below.
[0027] The embodiments of the present invention are intended to provide a better understanding of the gist of the invention, and unless otherwise specified, do not limit the content of the invention.
[0028] In this specification, the terms "comprise" and "containing" are concepts which encompass all of "comprise," "consist essentially of," and "consist only of."
[0029] In this specification, when a numerical range is indicated as "A to B," it means "A or more and B or less."
[0030] In this specification, the designations parts, % etc. are generally used.
[0031] In this specification, unless otherwise specified, all parts by mass or % by mass (wt%) are used.
[0032] [1] Oxide complex In the conventional technology (Patent Document 1), a uniform dispersion of titania nanoparticles carrying metal nanoparticles is prepared by ultrasonic waves, etc. In the conventional technology, silver is supported on titanium oxide (support), and the secondary particle size of the silver nanoparticle-supported titania nanoparticles is relatively large, so further study is required on the dispersion stability in the liquid and the elution of silver nanoparticles into water.
[0033] The conventional technology has a structure in which silver is supported around titanium oxide, that is, the titanium oxide is covered with silver. In general, silver is easily ionized and dissolved in water, so the durability of antibacterial and antiviral properties is low. Methods for imparting resistance to silver dissolution in water include supporting silver on a carrier in the form of silver nanoparticles, or immobilizing silver by embedding it in a binder or the like. However, further study is required to achieve the simultaneous antibacterial and antiviral properties, transparency, and resistance of silver to dissolution in water in the conventional technology.
[0034] The present invention relates to a structure in which inorganic oxide fine particles (titania, etc.) are supported around silver fine particles (support). The present invention relates to a structure in which inorganic oxide fine particles (titania, etc.) cover the periphery of silver fine particles (support). The oxide composite of the present invention is produced by carrying out a high-pressure dispersion treatment and controlling the secondary particle diameter of the inorganic oxide fine particles (silver fine particles supported on titania nanoparticles), thereby coating the periphery of silver with titanium oxide, thereby making it possible to produce a dispersion liquid in which silver is uniformly and stably dispersed in liquid.
[0035] The oxide composite of the present invention improves the resistance of silver to elution into water by coating silver nanoparticles with a sol of inorganic oxide fine particles (titanium oxide, etc.), thereby making it possible to maintain the antibacterial and antiviral properties of the silver contained in the oxide composite, as well as the adhesion of the oxide composite to a substrate and the transparency of the oxide composite, etc.
[0036] The oxide composite of the present invention is (A) A part of the surface of the silver fine particles is covered with (B) inorganic oxide fine particles, The (A) silver fine particles have an average primary particle diameter of 1 nm to 1,000 nm, The (B) inorganic oxide fine particles have an average primary particle size of 1 nm to 100 nm.
[0037] (1-1)(A) Silver nanoparticles The oxide composite of the present invention has a structure in which inorganic oxide particles (titania, etc.) are supported around silver particles (support), or a structure in which inorganic oxide particles (titania, etc.) cover the periphery of silver particles (support). In the oxide composite, a part of the surface of the silver particles (A) is covered with inorganic oxide particles (B), and the silver particles (A) have an average primary particle diameter of 1 nm to 1,000 nm.
[0038] The average primary particle diameter of the (A) silver fine particles is 1 nm to 1,000 nm, preferably 1 nm to 500 nm, more preferably 1 nm to 200 nm, and even more preferably 1 nm to 100 nm. The average primary particle diameter of the silver nanostructure is measured by a transmission electron microscope (TEM).
[0039] The sample is prepared by adjusting the concentration of the compound with the larger solid content, either silver or inorganic oxide, that constitutes the inorganic oxide composite to 0.2% by mass (wt%), dropping it onto a TEM grid, and drying it at a temperature below room temperature. At this time, if the compound concentration is less than 0.2% by mass, the concentration is not adjusted, but the sample is dropped onto a TEM grid and dried at a temperature below room temperature.
[0040] By adjusting the average particle size of the supported silver nanostructures within this range, a dispersion with high dispersion stability can be obtained, and a film with improved visible light catalytic activity and transparency can be formed.
[0041] The form of the silver nanostructure is not particularly limited, and from the viewpoints of silver stability, antibacterial activity in light and dark places (particularly in dark places), antiviral activity, and the like, it is preferable to use silver nanoparticles, silver nanorods, silver nanowires, etc.
[0042] (A) Surface coverage of silver particles The (A) fine silver particles preferably have a surface coverage of 1 surface % or more, and more preferably a surface coverage of 5 surface % to 95 surface %.
[0043] Definition of coverage An oxide composite having a structure in which inorganic oxide particles (titania (Ti) etc.) are supported around silver (Ag) particles (support) is imaged using an electron microscope (scanning electron microscope (SEM) or transmission electron microscope (TEM)), and the locations of the A particles and Ti particles are clarified by elemental analysis (energy dispersive X-ray analysis (EDS), electron probe microanalyzer (EPMA), electron energy loss spectroscopy (EELS), etc.).
[0044] Then, 10 random Ag particles are selected and arranged in order of particle size. Then, the fifth and sixth smallest Ag nanoparticles are selected and binarized using image processing software such as the image analysis software WinROOF (Mitani Shoji Co., Ltd.).
[0045] (A) Particle size ratio α(Ag) / β(Ti) The particle diameter of silver (Ag) particles is α (nm), and the particle diameter of titania (Ti) particles is β (nm). Based on this, α / β is calculated. α / β is preferably 1 / 2 or more.
[0046] By adjusting α(Ag particle) / β(Ti particle) to 1 / 2 or more (silver nanoparticles being relatively large), the particle size of the titanium oxide particles can be satisfactorily maintained relative to the silver nanoparticles (the particle size of the titanium oxide particles is not too large relative to the particle size of the silver nanoparticles), and the transparency of the dispersion containing the oxide complex can be satisfactorily maintained. α(Ag) / β(Ti) is more preferably adjusted to 1 to 1,000, and even more preferably adjusted to 1 to 100.
[0047] (B) Coverage of Ag particles As a result of this binarization process, the area of the Ag particles is A, and the area of the inorganic oxide particles that overlap with the Ag nanoparticles is B. Based on this result, the coverage rate is defined as B (inorganic oxide particles) / A (Ag particles) x 100 (%).
[0048] When the Ag particles are completely covered with the inorganic oxide particles, the coverage rate is 100%.
[0049] When the Ag particle exists alone, the coverage rate is 0%, and the Ag particle is not covered with the inorganic oxide particle.
[0050] The oxide complex has a coverage value of 1 surface% to 99 surface%, preferably 5 surface% to 95 surface%, more preferably 10 surface% to 80 surface%, and even more preferably 15 surface% to 65 surface%. By adjusting the coverage value of the titania within the above range, the oxide complex exhibits good antibacterial and antiviral activity, a dispersion containing the oxide complex has good dispersion stability, and a coating film containing the oxide complex has improved resistance to silver elution into water and adhesion to a substrate.
[0051] When the coverage of the oxide complex exceeds 99%, the exposure rate of the Ag particles decreases, and the antiviral performance may decrease. When the coverage of the oxide complex is less than 1%, the stability of the Ag particles in the oxide complex or in the dispersion may decrease. By adjusting the coverage (B (inorganic oxide particles) / A (Ag particles)×100(%)) to 1 surface% to 99 surface%, the oxide complex of the present invention can partially cover the surface of the Ag particles, improving the antiviral performance, providing good stability for a dispersion containing the oxide complex, and improving the resistance of silver to elution in water and adhesion to a substrate.
[0052] (C) Random ratio of inorganic oxide particle (Ti, etc.) islands The random ratio of Ag particles is defined as follows:
[0053] As a result of binarization processing using image processing software (WinROOF), the coordinate positions of Ag particles are defined as follows: AgXmax (maximum value of X coordinate of Ag particle) AgXmin (minimum value of the X coordinate of an Ag particle) AgYmax (maximum Y coordinate of Ag particles) AgYmin (minimum value of Y coordinate of Ag particle)
[0054] Next, N inorganic oxide particles are extracted from the inorganic oxide particles by measuring the shape characteristics of the inorganic oxide particles using WinROOF. The n-th inorganic oxide particle is defined as On when the inorganic oxide particles are arbitrarily assigned numbers 1, 2, 3, and so on.
[0055] For On, the coordinate position is defined as follows: Onx (X coordinate of the center of gravity of the nth inorganic oxide particle) Ony (Y coordinate of the center of gravity of the nth inorganic oxide particle)
[0056] Next, the region of the Ag particle is divided as follows: AgX1=AgXmin (first X coordinate) AgXm+1=AgXm+(AgXmax-AgXmin) / N (m+1th X coordinate) AgY1=AgYmin (first Y coordinate) AgYm+1=AgYm+(AgYmax-AgYmin) / N (m+1th Y coordinate)
[0057] The number of inorganic oxide particles in each of the divided regions and the maximum value thereof are defined as follows. The number of Onx contained within the coordinates of AgXm and AgXm+1 is defined as NOmx. Furthermore, the maximum value of NOmx is defined as NOxmax. The number of Ony contained within the coordinates of AgYm and AgYm+1 is defined as NOmy. Furthermore, the maximum value of NOmx is defined as NOymax.
[0058] The random rate in the X-axis direction (Ranx) and the random rate in the Y-axis direction (Rany) are as follows: Ranx = (1-NOxmax / N) x 100 Rany = (1-NOymax / N) x 100
[0059] This allows the measurement of the random ratios (Ranx, Rany). Each of the random ratios Ranx, Rany is preferably 50% or more, more preferably 70% or more, and even more preferably 90% or more. In the oxide composite of the present invention, a high random ratio means that the number of Ti particles coated on the Ag particles is large and that they are well-dispersed.
[0060] By adjusting the random ratios Ranx and Rany, the oxide composite of the present invention can efficiently expose Ag particles while increasing the dispersibility of the Ag particles, thereby improving the dispersion stability and antiviral activity of the Ag particles and preventing the elution of Ag from the inorganic oxide composite.
[0061] (1-2)(B) Inorganic oxide fine particles The oxide composite of the present invention has a structure in which inorganic oxide particles (titania, etc.) are supported around silver particles (support), or a structure in which inorganic oxide particles (titania, etc.) cover the periphery of silver particles (support). In the oxide composite of the present invention, a part of the surface of the silver particles (A) is covered with inorganic oxide particles (B), and the inorganic oxide particles (B) have an average primary particle diameter of 1 nm to 100 nm.
[0062] The (B) inorganic oxide fine particles are silica, alumina, ceria, calcium oxide, titanium oxide, tungsten oxide, and zinc oxide, and preferably (B1) titania fine particles.
[0063] The (B1) titania fine particles preferably have a surface protected with an organic acid, and the mass of the organic acid is 1 mass % or more relative to the weight of titanium oxide. The organic acid is preferably
[0064] At least one organic acid selected from the group consisting of monocarboxylic acids having 1 to 4 carbon atoms and hydroxycarboxylic acids having 2 to 3 carbon atoms, or
[0065] The acyloxy group is derived from at least one organic acid selected from the group consisting of monocarboxylic acids having 1 to 4 carbon atoms and hydroxycarboxylic acids having 2 to 3 carbon atoms.
[0066] The organic acid is preferably at least one organic acid selected from the group consisting of acetic acid and lactic acid.
[0067] The (B1) titania fine particles are preferably positively charged.
[0068] Water, inorganic acids, free organic acids, etc. generally evaporate almost completely at temperatures below 200°C.
[0069] (B1) When titania microparticles are heated using a thermogravimetric and differential thermal analyzer (TG-DTA), the mass loss at temperatures above 200°C indicates the weight of organic acids or acetoxy groups present on the surface of the titania microparticles.
[0070] When the (B1) titania fine particles are heated to 600°C by a thermogravimetry-differential thermal analyzer (TG-DTA), the mass loss at 200°C or higher is 5% by mass or more, preferably 7% by mass to 20% by mass. By adjusting the mass loss amount within this range, the aggregation of titania nanoparticles during drying or firing can be suppressed, so cracks, peeling, etc. are unlikely to occur, and the coating property and transparency are particularly excellent. (B) inorganic oxide fine particles (preferably (B1) titania fine particles) can suppress cracks, peeling, etc., and are easy to firmly support metals, so that they also have excellent visible light catalytic activity. The detailed conditions of the thermogravimetry-differential thermal analyzer (TG-DTA) are atmosphere: air, heating rate: 3°C / min.
[0071] The organic acid protecting the titania fine particles (B1) is preferably at least one organic acid selected from the group consisting of monocarboxylic acids having 1 to 4 carbon atoms and hydroxycarboxylic acids having 2 to 3 carbon atoms, or an acyloxy group (-OCOR) derived from at least one organic acid selected from the group consisting of monocarboxylic acids having 1 to 4 carbon atoms and hydroxycarboxylic acids having 2 to 3 carbon atoms.
[0072] In -OCOR, the alkyl group of R is preferably a methyl group, an ethyl group, an n-propyl group, etc. In -OCOR, the monocarboxylic acid is preferably formic acid, acetic acid, propionic acid, butyric acid, etc.
[0073] In -OCOR, the hydroxyalkyl group of R is preferably a hydroxymethyl group, a 1-hydroxyethyl group, a 2-hydroxyethyl group, etc. In -OCOR, the hydroxycarboxylic acid is preferably glycolic acid, lactic acid, etc.
[0074] In -OCOR, from the viewpoints of volatility, toxicity, and decomposability, R is preferably a hydrogen atom, or a methyl group, a hydroxymethyl group, a 1-hydroxyethyl group, a 2-hydroxyethyl group, or the like.
[0075] In -OCOR, from the viewpoints of water solubility and odor, R is preferably a methyl group, a 1-hydroxyethyl group, a 2-hydroxyethyl group, or the like.
[0076] From the viewpoints of volatility, toxicity and decomposability, -OCOR is preferably a monocarboxylic acid such as formic acid or acetic acid.
[0077] From the viewpoints of volatility, toxicity and decomposability, -OCOR is preferably a hydroxycarboxylic acid such as glycolic acid or lactic acid.
[0078] From the viewpoints of water solubility and odor, particularly preferred -OCORs are acetic acid, glycolic acid, lactic acid, and the like.
[0079] The organic acid may be at least one compound selected from the group consisting of the above organic acids. These organic acids may be used alone or in combination (blend) of two or more depending on the purpose.
[0080] The average primary particle diameter of the (B) inorganic oxide fine particles is preferably 1 nm to 100 nm, more preferably 1 nm to 50 nm, even more preferably 1 nm to 10 nm, and particularly preferably 2 nm to 6 nm. The average primary particle diameter of the (B) inorganic oxide fine particles (supported side) is preferably smaller than the average primary particle diameter of the (A) silver fine particles (support, supporting side). By adjusting the average particle diameter of the (B) inorganic oxide fine particles to the above range, the (B) inorganic oxide fine particles can be supported appropriately and more firmly around the (A) silver fine particles (support), and the (B) inorganic oxide fine particles can form a film with higher visible light catalytic activity and higher transparency.
[0081] The average secondary particle diameter of the (B) inorganic oxide fine particles is 1,000 nm or less, more preferably 5 nm to 500 nm, and even more preferably 5 nm to 100 nm.
[0082] The average secondary particle diameter of the oxide composite is measured by observation with a particle size distribution meter.
[0083] (B) The average particle size of inorganic oxide microparticles is measured by observation with a transmission electron microscope (TEM). The sample is adjusted by adjusting the compound concentration of silver or inorganic oxide, whichever has the greater solid content, to 0.2%, dropping it onto a TEM grid, and drying it at 25°C or less. At this time, for samples with a compound concentration of less than 0.2 mass% (wt%), the concentration is not adjusted and the sample is dropped onto a TEM grid and dried at 25°C or less.
[0084] (B) The specific surface area of the inorganic oxide fine particles is preferably 150 m 2 / g~500m 2 / g, more preferably 200m 2 / g~400m 2 / g, and more preferably 210 to 300 m 2 By adjusting the specific surface area of the (B) inorganic oxide fine particles within the above range, the (B) inorganic oxide fine particles can be supported appropriately and more firmly around the (A) silver fine particles (carrier), and the (B) inorganic oxide fine particles can form a film that has higher visible light catalytic activity and higher transparency.
[0085] (B) The specific surface area of the inorganic oxide fine particles is measured by the BET method.
[0086] The titania nanoparticles can have the concentrations of N, Cl, and S elements each preferably in the range of 0 to 5,000 ppm, more preferably 0 to 1,000 ppm. By adjusting the concentrations of N, Cl, and S elements in the titania nanoparticles to within this range, corrosion of the substrate can be suppressed. The concentrations of N, Cl, and S elements in the titania nanoparticles mean that there is no impurity derived from the acidic titania precursor such as TiCl4 or TiOSO4, or there are only a very small amount of such impurities.
[0087] The concentrations of N, Cl, and S elements in (B) inorganic oxide fine particles (preferably (B1) titania fine particles) are measured by WDX (fluorescent X-ray).
[0088] The crystal form of the (B1) titania fine particles is preferably anatase type, and the (B1) titania fine particles are preferably 100% anatase type, not including any crystal form other than anatase type. By adopting the (B1) titania fine particles of anatase type, the visible light catalytic activity is improved.
[0089] (1-3) Oxide complex In the oxide composite, the ratio of the average primary particle size of the (A) silver microparticles to the average primary particle size of the (B) inorganic oxide microparticles (average primary particle size of the (A) silver microparticles / average primary particle size of the (B) inorganic oxide microparticles) is preferably 0.5 or more.
[0090] In the oxide composite, the ratio of the average primary particle size of the (A) silver microparticles to the average primary particle size of the (B) inorganic oxide microparticles (average primary particle size of the (A) silver microparticles / average primary particle size of the (B) inorganic oxide) is preferably 1 or more and 200 or less.
[0091] In the oxide composite, the random ratios (Ranx, Rany) of the inorganic oxide microparticles (B) covering the silver microparticles (A) are preferably 50% or more, more preferably 70% or more, and even more preferably 90% or more.
[0092] In the oxide complex, the mass ratio of the silver mass (Ag mass) in the (A) silver fine particles to the titanium oxide mass (TiO2 mass) in the (B) inorganic oxide fine particles (preferably, (B1) titania fine particles) (Ag mass in the (A) silver fine particles / TiO2 mass in the (B) inorganic oxide fine particles) is preferably ≦10 (10 or less), more preferably 0.0001 to 5, and even more preferably 0.001 to 1. By adjusting the Ag mass in the (A) silver fine particles / TiO2 mass in the (B) inorganic oxide fine particles to ≦10 (10 or less), the antimicrobial activity (antibacterial activity and antiviral activity) and the stability of the oxide complex can be well maintained, and the strength and transparency of the coating film can be maintained.
[0093] In the oxide composite, the total solid content of the (A) silver fine particles and the (B) inorganic oxide fine particles is preferably 50 mass % or less.
[0094] (1-4) Dispersions, paints, and coatings The present invention encompasses a dispersion containing the oxide complex of the present invention and water, the dispersion containing 0.5 mass % or more of water.
[0095] The pH of the dispersion is preferably pH = 1 to 8, and more preferably pH = 2 to 5. By setting the pH of the dispersion in this range, the stability and transparency of the dispersion become good, and it is possible to prevent cracks in the coating film when the dispersion is applied to a substrate and dried.
[0096] The present invention includes a coating material containing the oxide complex or dispersion of the present invention, and a coating film formed by the coating material of the present invention.
[0097] [2] Manufacturing method for oxide composite The oxide composite of the present invention has a structure in which inorganic oxide particles (such as titania) are supported around silver particles (support), or a structure in which inorganic oxide particles (such as titania) cover the periphery of silver particles (support).
[0098] In the present invention, the method for supporting (B) inorganic oxide fine particles (preferably, (B1) titania fine particles or titania sol) around (A) silver fine particles (carrier) is preferably a method in which (A) silver compound and (B) inorganic oxide fine particles are mixed, and then silver nanoparticles are formed by irradiating with light, while the surfaces of the silver nanoparticles are coated with the inorganic oxide fine particles (preferably, (B1) titania fine particles or titania sol).
[0099] A preferred method for supporting inorganic oxide fine particles (B) around silver fine particles (support) is to mix the silver compound (A) with the inorganic oxide fine particles (B), and then coat the surfaces of the silver nanoparticles with inorganic oxide fine particles (preferably (B1) titania fine particles or titania sol) while forming silver nanoparticles with a reducing agent. A preferred method for supporting inorganic oxide fine particles (B) around silver fine particles (support) is to contact the silver fine particles (A) with the inorganic oxide fine particles (B), mix them, or allow them to stand, and support them.
[0100] The method for producing inorganic oxide fine particles is preferably (Step A) Step (B) includes a step of heating a dispersion liquid obtained by mixing a substance containing inorganic oxide fine particles, an organic acid, and water at a temperature higher than 90° C. for 1 hour or more.
[0101] (Step B) In the method for producing an oxide composite, preferably, after step (A), the dispersion containing inorganic oxide fine particles (B) obtained in step (A) is subjected to a pressure treatment of 30 MPa or more (high pressure dispersion method).
[0102] The method for producing an oxide composite preferably includes step (C) (step (C1), (C2), (C3) or (C4)) after step (B).
[0103] (Step C1) is a step of performing a chemical reduction treatment on the dispersion obtained by mixing the dispersion obtained in step (B) with a precursor of silver fine particles. In step (C1), the loading efficiency can be improved by applying energy from the outside.
[0104] Step C2 is a step of irradiating the dispersion obtained by mixing the dispersion obtained in step (B) with the silver fine particles (A) with ultraviolet light. Step (C2) can improve the loading efficiency by applying energy from the outside.
[0105] Step C3 is a step of mixing the dispersion obtained in step B with (A) fine silver particles. Step C3 can prevent the dispersion of (B) fine inorganic oxide particles from becoming too viscous, and can obtain uniform particles.
[0106] (Step C4) This is a step of adding (A) fine silver particles to the dispersion liquid obtained in step (B) and allowing it to stand.
[0107] By carrying out steps (C1), (C2), (C3), and (C4) at 25° C. or lower, it is possible to further improve the particle size controllability of the (A) silver particles.
[0108] [2-1] Process (A) In step (A), a dispersion is obtained by mixing a substance containing inorganic oxide fine particles (B), an organic acid, and water. The inorganic oxide fine particles (B) are preferably titania fine particles (B1).
[0109] (B1) Preparation of titania particles The titanium-containing substance used is preferably a substance that becomes titanium oxide when heated. The titanium-containing substance is preferably titanium oxide and / or a titanium oxide precursor, and more preferably titanium oxide; titanium hydroxide; titanium alkoxide; titanium halide such as titanium trichloride or titanium tetrachloride (particularly, one neutralized with a base); metallic titanium, etc.
[0110] From the viewpoints of dispersibility, coatability, and visible light catalysis of the resulting titania, the titanium-containing substance is preferably titanium alkoxide, titanium hydroxide, or titanium halide (particularly, one neutralized with a base). From the viewpoints of purity, dispersibility, coatability, transparency, and visible light catalysis, the titanium-containing substance is more preferably titanium alkoxide.
[0111] The titanium alkoxide is preferably titanium tetraisopropoxide, titanium tetra n-butoxide, titanium tetra n-propoxide, titanium tetraethoxide, etc. From the viewpoints of cost, water solubility of by-products, coatability, and visible light catalytic property, the titanium alkoxide is more preferably titanium tetraisopropoxide.
[0112] The titanium-containing substance may be at least one compound selected from the group consisting of the titanium-containing substances described above. These titanium-containing substances may be used alone or in combination (blend) of two or more types depending on the purpose.
[0113] Depending on the combination of titanium alkoxide and organic acid, the titania obtained may be used as a catalyst to liberate ester compounds that are difficult to dissolve in water. There is no problem with titania itself. For example, in the combination of titanium tetra n-butoxide and acetic acid, butyl acetate is generated and liberated at the stage of mixing and heating, but from the viewpoint of obtaining a uniform dispersion, it is preferable to adopt a combination of organic acid and titanium alkoxide that can obtain an organic acid alkoxide with excellent water solubility.
[0114] Titanium halides (titanium tetrachloride, titanium trichloride, etc.) are preferably neutralized with a base and the precipitate is washed from the viewpoints of impurities (halogens), corrosion of the reactor during mass production, crystallinity control, coating properties, transparency, and visible light catalysis. Titanium halides are preferably used without drying from the viewpoint of dispersibility of the obtained titania.
[0115] When a solid such as titanium oxide or metallic titanium is used as the titanium-containing substance, the average primary particle size is preferably 100 nm or less, more preferably 50 nm or less. There is no particular lower limit for the average particle size of the titanium-containing substance, and it is preferably about 1 nm.
[0116] When the particle size is large, it is preferable to use a planetary ball mill, a paint shaker or the like for dry or wet pulverization.
[0117] The average particle size of solids such as titanium oxide and titanium metal is measured by observation using a transmission electron microscope (TEM).
[0118] The concentration of the titanium-containing substance in the dispersion produced in step (A) is preferably 0.01 mol / L to 5 mol / L, and more preferably 0.05 mol / L to 3 mol / L, from the viewpoints of productivity, viscosity of the reaction liquid, coatability, transparency, and visible light catalytic properties.
[0119] The acid used in the reaction is an organic acid, and since it is preferable that it is a volatile acid, it is preferably an acid represented by the chemical formula C n H 2n+1 Monocarboxylic acids represented by COOH (n=0 to 3) (monocarboxylic acids having 1 to 4 carbon atoms), hydroxycarboxylic acids having 2 to 3 carbon atoms, etc. are used.
[0120] The monocarboxylic acid is preferably formic acid (n=0) or acetic acid (n=1) from the viewpoints of volatility, toxicity and decomposability.
[0121] The hydroxycarboxylic acid is preferably glycolic acid, lactic acid, etc., and from the viewpoints of water solubility and odor, more preferably acetic acid, glycolic acid, lactic acid, etc.
[0122] The organic acid may be at least one compound selected from the group consisting of the above organic acids. These organic acids may be used alone or in combination (blend) of two or more depending on the purpose.
[0123] The amount of organic acid used is adjusted so that the number of moles of organic acid is preferably 0.5 moles or more, particularly preferably 1 mole or more, per mole of titanium in the titanium-containing substance, from the viewpoints of dispersibility, coatability, transparency, and cost. The more organic acid is used, the more the stability over time, coatability, transparency, etc. can be improved. The upper limit of the amount of organic acid used is not particularly limited, and is preferably adjusted so that the number of moles of acyloxy groups is 10 moles or less per mole of titanium in the titanium-containing substance.
[0124] The concentration of the organic acid in the dispersion obtained in step (A) is preferably 0.02 mol / L to 10 mol / L, and more preferably 0.1 mol / L to 7 mol / L, from the viewpoints of dispersibility, coatability, transparency, visible light catalytic properties, and cost.
[0125] The reaction solvent is preferably an aqueous solvent such as water, the main component being preferably 50% by mass or more. The reaction solvent may contain an alcohol or an ester during the reaction.
[0126] When titanium tetraisopropoxide is used as a raw material, the reaction solvent reacts with an organic acid to produce isopropyl alcohol. Heating may produce an isopropyl ester of the organic acid. The alcohol or ester may be added to the dispersion obtained by step (A), or may be generated in the system. The alcohol or ester may be removed by heating in an open system at 100°C or less, or may be removed by reducing pressure, or may remain in the reaction liquid.
[0127] When alcohol is contained in the dispersion, the average particle size of the obtained titania nanoparticles and metal-supported titania nanoparticles tends to become small, and therefore alcohol may be intentionally added in order to control the average particle size.
[0128] In general, inorganic acids (especially strong inorganic acids) such as nitric acid, hydrochloric acid, and sulfuric acid are often used in the hydrothermal synthesis reaction of titania nanoparticles. Not only do the crystal forms of the resulting titania nanoparticles contain a mixture of anatase and brookite types, but it is preferable not to use them in principle from the viewpoints of the storage stability of the resulting dispersion, corrosion of the equipment, impurities, wastewater, etc.
[0129] Inorganic acids can be used supplementarily in the range of, for example, 0.01 mol / L or less, to enhance the dispersibility, transparency, uniformity, etc. of the raw material and to facilitate handling, without impairing the effect. The concentrations of N, Cl, and S elements in the dispersion obtained in step (A) are all 0.01 mol / L or less.
[0130] The pH of the dispersion obtained in step (A) is preferably 2 or more and less than 6, and more preferably 2.1 to 5, from the viewpoints of equipment corrosion, handling safety, dispersibility, and the like.
[0131] In step (A), the method of preparing the dispersion is not particularly limited, and the titanium-containing substance, the organic acid, and water (solvent) may be mixed simultaneously or sequentially. On a mass production scale, from the viewpoint of preventing aggregation and forming large lumps and facilitating continued stirring, it is preferable to mix the organic acid and water (solvent) and then add the titanium-containing substance while stirring. On a laboratory scale, it is preferable to mix the titanium-containing substance and the organic acid and then add water while stirring.
[0132] The obtained dispersion is heated at a temperature higher than 90°C for 1 hour or more. The heating is preferably performed under normal pressure, or under pressure in a closed container. From the viewpoint of reducing the average particle size of the titania nanoparticles and the titania nanoparticles carrying metal nanoparticles, the heating is preferably performed under normal pressure. The heating is preferably performed under conditions of 0.09 MPa to 0.11 MPa. When the heating is performed under pressure, from the viewpoint of easily forming a film having high visible light catalytic activity and high transparency, the reaction is preferably performed at 0.2 MPa or less (0.11 MPa to 0.2 MPa) for a short time (about 5 minutes to 30 minutes).
[0133] During heating, stirring is preferably performed from the viewpoint of sufficiently reacting the titanium-containing substance, the organic acid, and the water. The stirring method is not particularly limited and follows a conventional method. The stirring time is preferably 1 hour or more, more preferably 1.5 hours or more, from the viewpoint of sufficiently reacting the titanium-containing substance, the organic acid, and the water. The upper limit of the stirring time is not particularly limited and is preferably 240 hours.
[0134] The heating temperature is preferably higher than 90° C., and more preferably 92° C. or higher. If the heating temperature is lower than 90° C., the crystal growth of the titanium oxide fine particles cannot be controlled, and the dispersion stability tends to decrease over time after heating is completed, and precipitation tends to occur when the silver fine particles are combined. The upper limit of the heating temperature is not particularly limited, and is preferably 120° C. when the reaction is carried out at normal pressure.
[0135] The pH of the dispersion obtained in step (A) is preferably 2 or more and less than 6, and more preferably 2.1 to 5, from the viewpoints of equipment corrosion, handling safety, dispersibility, and the like.
[0136] [2-2] Process (B) <High pressure dispersion method (pressure treatment)> In the step (B), the dispersion liquid containing the inorganic oxide fine particles (B) obtained in the step (A) is subjected to a pressure treatment of 30 MPa or more (high pressure dispersion method). The inorganic oxide fine particles (B) are preferably titania fine particles (B1).
[0137] When the high-pressure dispersion method is employed, the dispersion liquid containing the inorganic oxide fine particles (B) is preferably subjected to a pressurization treatment at 30 MPa or more.
[0138] By applying the pressure treatment, the primary particles and / or secondary particles of the (B) inorganic oxide microparticles are atomized, improving the dispersion stability and transparency of the (B) inorganic oxide microparticles, thereby improving the reactivity and uniformity in step (C), and making it possible for the (B) inorganic oxide microparticles to better cover the surfaces of the (A) silver microparticles when combined with the (A) silver microparticles.
[0139] The pressure level when carrying out the pressure treatment is not particularly limited as long as it can sufficiently atomize the inorganic oxide fine particles (B). The pressure level is preferably adjusted to 30 MPa or more, more preferably adjusted to 50 MPa to 400 MPa, and further preferably adjusted to 100 MPa to 300 MPa. The pressure treatment is preferably carried out using a high-pressure dispersion device, a supercritical water preparation device, or the like. The high-pressure dispersion device can disperse the inorganic oxide fine particles (B) by applying mechanical pressure. The supercritical water preparation device can increase the pressure of the system by heating water.
[0140] Depending on the pressure, for example, (i) causing two or more dispersions of (B) inorganic oxide fine particles to collide with each other; (ii) (B) Collision of a material dispersion of inorganic oxide fine particles with a metal or ceramic material (a material having high hardness such as silicon carbide or alumina); (iii) (B) A dispersion of inorganic oxide particles is placed on a substrate having a cross-sectional area of 1 cm 2 Passing through the following spaces The following processing is performed:
[0141] By applying pressure, it is possible to make the pressure conditions stronger, (B) the inorganic oxide fine particles can be atomized more efficiently, and the treatment time can be further reduced.
[0142] The pressurization operation is preferably carried out two or more times, and more preferably three or more times.
[0143] The temperature during pressurization is not particularly limited. The temperature during pressurization is adjusted so that the inorganic oxide fine particles can be sufficiently dispersed and the solvent does not boil. Therefore, the temperature during pressurization is preferably 0°C to 99°C, and more preferably 10°C to 90°C. Since the temperature rises during pressurization due to pressurization and collision, it is preferable to cool the mixture using a heat exchanger or the like. By setting the temperature within this range, it is possible to prevent re-aggregation of the (B) inorganic oxide fine particles.
[0144] When the pressurized treatment is carried out, it is preferable to use a preliminary treatment (pretreatment) in combination with a dispersion treatment using other dispersion devices such as ordinary mechanical stirring, a dispersion treatment using an emulsifying device, or a dispersion treatment using a bead mill, etc. This can have the effect of preventing clogging in a high-pressure dispersion device, etc.
[0145] The more powerful the dispersion treatment in this pretreatment, the more preferable. For example, in the case of dispersion treatment using an emulsifier, the rotation speed is preferably 5,000 to 100,000 rpm, and more preferably 10,000 to 50,000 rpm.
[0146] [2-3] Process (C1) In the step (C1), a dispersion liquid obtained by mixing the dispersion liquid containing the inorganic oxide fine particles (B) obtained in the step (B) with a silver salt (A) is subjected to a chemical reduction treatment.
[0147] Silver salt The silver salt used as the precursor of the silver fine particles is preferably used to prevent the dispersion (sol) containing inorganic oxide fine particles (titania nanoparticles) (B) obtained in steps (A) and (B) from becoming alkaline after step (C1). The silver salt is preferably a silver salt whose aqueous solution is acidic or neutral. The silver salt is preferably silver chloride (I), silver nitrate (I), organic acid silver (silver lactate (I), silver acetate (I), silver citrate (I), silver myristate (I), etc.), silver sulfide (I), silver oxide (I), silver phosphate (I), silver carbonate (I), silver bromide (I), silver iodide (I), etc.
[0148] The precursor of the silver particles may be at least one compound selected from the group consisting of the silver salts described above. These silver salts may be used alone or in combination (blend) of two or more types depending on the purpose.
[0149] In step (C1), the amount of silver fine particles used is, from the viewpoints of dispersibility, transparency, antimicrobial activity (antibacterial activity and antiviral activity), stability of the inorganic oxide fine particles (titania nanoparticles, etc.), etc., such that the mass ratio of the silver mass (Ag mass) in the silver fine particles (A) to the titanium oxide mass (TiO2 mass) in the inorganic oxide fine particles (B) (Ag mass in silver fine particles (A) / titanium oxide mass (TiO2 mass) in inorganic oxide fine particles (B)) is preferably ≦10 (10 or less), more preferably 0.0001 to 5, and even more preferably 0.001 to 1.
[0150] Chemical reduction treatment In the step (C1), the chemical reduction treatment is not particularly limited, and preferably, a method using a reducing agent such as sodium borohydride, a polyol reduction method, an ethanol reduction method, etc. When a reducing agent is used, the reduction is preferably carried out at a temperature of 0° C. or higher and lower than 20° C. (room temperature) from the viewpoints of dispersion stability and prevention of discoloration.
[0151] Step (C1) may be carried out under an air atmosphere or an anaerobic atmosphere. The anaerobic atmosphere in step (C1) is preferably an inert gas atmosphere such as a nitrogen atmosphere or an argon atmosphere.
[0152] In the step (C1), the chemical reduction treatment is preferably performed with stirring in order to sufficiently react the dispersion obtained in the step (B) with the fine silver particles. The stirring method is not particularly limited and may be performed according to a conventional method.
[0153] The pH of the resulting dispersion varies depending on the type of metal added and the amount of the metal added, but is preferably 1 to 5, and more preferably 2 to 4, from the viewpoint of coatability.
[0154] Thereafter, the oxide composite having (A) silver particles (carrier) coated with (B) inorganic oxide particles (preferably (B1) titania particles or titania sol) can be recovered by precipitating and centrifuging the oxide composite in a conventional manner.
[0155] [2-4] Process (C2) In the step (C2), the dispersion containing the inorganic oxide fine particles (B) obtained in the step (B) and the silver salt described in the step (C1) are mixed together to obtain a dispersion, which is then irradiated with ultraviolet rays.
[0156] UV exposure In step (C2), from the viewpoints of ease of supporting (B) inorganic oxide fine particles (preferably (B1) titania fine particles, titania sol) around (A) silver fine particles (carrier), reaction rate, reaction controllability and productivity, it is preferable to use an ultraviolet irradiation device including a wavelength of 280 nm to 500 nm. If the wavelength range is shorter than 280 nm, the dispersion stability decreases, and if the wavelength is longer than 500 nm, silver is not reduced and silver nanoparticles are not generated.
[0157] In step (C2), during the ultraviolet light irradiation, the dispersion containing the inorganic oxide fine particles (B) obtained in step (B) is preferably stirred in order to sufficiently react with the silver fine particles (A). The stirring method is not particularly limited and may be performed according to a conventional method.
[0158] Step (C2) may be carried out under an air atmosphere or an anaerobic atmosphere. The anaerobic atmosphere in step (C2) is preferably an inert gas atmosphere such as a nitrogen atmosphere or an argon atmosphere.
[0159] The reaction time in step (C2) is preferably 1.5 hours or more, and more preferably in the range of 1.5 to 36 hours. If the reaction time is shorter than this range, the inorganic oxide fine particles will not surround the silver nanoparticles and gelation will occur, whereas if the reaction time is longer than this range, the particle size of the silver nanoparticles will increase and precipitation will occur.
[0160] The pH of the resulting dispersion varies depending on the type of metal added and the amount of the metal added, but is preferably 1 to 5, and more preferably 2 to 4, from the viewpoint of coatability.
[0161] Thereafter, the oxide composite having (B) inorganic oxide fine particles (preferably (B1) titania fine particles or titania sol) supported around (A) silver fine particles (carrier) can be recovered by precipitating and centrifuging the oxide composite in a conventional manner.
[0162] [2-5] Steps (C3) and (C4) As the step (C3), a step of mixing the dispersion liquid containing the inorganic oxide fine particles (B) obtained in the step (B) with the silver fine particles (A) can be adopted.
[0163] As the step (C4), a step of adding (A) fine silver particles to the dispersion liquid containing the fine inorganic oxide particles (B) obtained in the step (B) and allowing the mixture to stand can be adopted.
[0164] silver fine particles The conditions such as the (A) silver particles and the amount used are the same as those in step (C1). Mix and let stand
[0165] In step (C3), the method of mixing the dispersion liquid obtained in step (B) with the silver fine particles (A) is not particularly limited and follows a conventional method. In step (C3), the silver fine particles (A) are added to the dispersion liquid obtained in step (B) and stirred. The stirring method is not particularly limited and follows a conventional method.
[0166] Steps (C3) and (C4) may be carried out in an air atmosphere or an anaerobic atmosphere. The anaerobic atmosphere in steps (C3) and (C4) is preferably an inert gas atmosphere such as a nitrogen atmosphere or an argon atmosphere.
[0167] The pH of the resulting dispersion varies depending on the type of metal added and the amount of the metal added, but is preferably 1 to 5, and more preferably 2 to 4, from the viewpoint of coatability.
[0168] Thereafter, the oxide composite having (B) inorganic oxide fine particles (preferably (B1) titania fine particles or titania sol) supported around (A) silver fine particles (carrier) can be recovered by precipitating and centrifuging the oxide composite in a conventional manner.
[0169] [3] Dispersions, paints, and coatings containing oxide complexes Dispersion containing oxide complex The dispersion liquid containing the oxide complex of the present invention (photocatalyst dispersion liquid, further, visible light responsive photocatalyst dispersion liquid) uses a reaction liquid that has undergone step (A), step (B), and step (C1), step (C2), step (C3), or step (C4).
[0170] In conventional visible light responsive photocatalyst dispersions, it was impossible to obtain a uniform dispersion unless a dispersing agent was used.
[0171] A dispersant may be added to the dispersion containing the oxide complex of the present invention. Even without adding a dispersant, the dispersion containing the oxide complex of the present invention has much better dispersibility than a typical visible light responsive photocatalyst.
[0172] The dispersion containing the oxide complex of the present invention has good dispersibility, and therefore the coating has excellent crack resistance. The dispersion containing the oxide complex of the present invention does not require the addition of a dispersant, and therefore a dense titania coating is possible, and the dispersion has excellent coatability and transparency, as well as excellent visible light catalytic activity.
[0173] In the dispersion containing the oxide composite, the content of water as the main solvent is preferably 50% by mass or more, and more preferably 60% by mass or more, from the viewpoints of ease of coating, film properties of the coating, etc., with the total amount of the dispersion containing the oxide composite being 100% by mass.
[0174] It is also possible to take out the oxide composite from the reaction solution and change the solvent. Water may be removed from the reaction solution by centrifugation, a filtration membrane, or the like, and replaced with an organic solvent. It is preferable not to dry the oxide composite from the viewpoints of dispersibility, transparency, and the like.
[0175] The organic solvent used in the dispersion liquid is preferably alcohol, etc. The alcohol is preferably an aliphatic alcohol having 1 to 6 carbon atoms, such as methanol, ethanol, propanol, isopropanol, etc., a non-aliphatic alcohol, such as α-terpineol, etc., a glycol-based solvent, such as butyl carbitol (diethylene glycol monobutyl ether), hexylene glycol (2-methyl-2,4-pentanediol), ethylene glycol-2-ethylhexyl ether, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, etc., or a diol, such as 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, etc.
[0176] The organic solvent used in the dispersion liquid is preferably an organic solvent that has affinity with titania and other solvents (water, alcohol, etc.) even if it does not have an OH group. The organic solvent is preferably diethylene glycol butyl methyl ether, tripropylene glycol dimethyl ether, triethylene glycol dimethyl ether, diethylene glycol dibutyl ether, triethylene glycol butyl methyl ether, tetraethylene glycol dimethyl ether, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol diacetate, triethylene glycol diacetate, tetraethylene glycol diacetate, etc. From the viewpoint of boiling point, etc., it is more preferable to use diethylene glycol monobutyl ether acetate, tetraethylene glycol dimethyl ether, etc. as the organic solvent.
[0177] Coatings containing oxide complexes The dispersion containing the oxide complex is preferably adjusted in viscosity according to the application to prepare a paint. When the paint is applied by spin coating, dip coating, spraying, or the like, the viscosity is preferably adjusted to a low level. When the paint is applied by brush coating, squeegee method, or the like, the viscosity is preferably adjusted to a higher level. When the paint is applied by screen printing, the viscosity is preferably adjusted to a higher level to suppress flowability.
[0178] Coating containing oxide complex The resulting coating film containing the oxide complex allows for a dense coating.
[0179] The coated product having a coating film is not particularly limited, and examples thereof include building materials, building exteriors, building interiors, window frames, window glass, various lenses, structural members, building facilities such as housing, cooking utensils, textile products, furniture, displays, display protective films, plumbing members, vehicle lighting covers and window glass, mechanical equipment or exteriors of articles, dustproof covers and coatings, display devices, their covers, traffic signs, various display devices, display objects such as billboards, sound insulation walls for roads and railways, exteriors and coatings of bridges and guardrails, interiors and coatings of tunnels, insulators, solar cell covers, solar hot water heater heat collector covers, and other exterior parts of electronic and electrical devices used outside, particularly transparent members, exteriors of vinyl greenhouses, greenhouses, and the like. EXAMPLES
[0180] The present invention will be specifically described below with reference to examples.
[0181] The present invention is not limited to the following specific examples.
[0182] [Example 1] To 142.1 g (0.5 mol) of titanium tetraisopropoxide, 30 g (0.5 mol) of acetic acid was added and stirred for 60 minutes. Next, 538 g of water was added and stirred at normal pressure (0.10 MPa) and 95°C for 3 hours. Then, a high-pressure dispersion treatment (160 MPa) was performed to obtain a dispersion liquid containing titanium oxide microparticles.
[0183] The titanium oxide fine particles contained in this dispersion liquid had primary particles with an average size of 3 nm when observed under a transmission electron microscope, and secondary particles with a particle size distribution analyzer were found to be 30 nm.
[0184] Silver nitrate (I) was added to 15 g of this dispersion (solid content 5.2% by mass) so that silver was 25% by mass based on the metal weight of the titania fine particles (titanium oxide) contained in the dispersion, and the mixture was thoroughly stirred. Then, an ultraviolet lamp was irradiated for 3 hours to obtain a white-ish dispersion. The obtained dispersion did not change in color even after being left for about 3 weeks, and it was confirmed that the silver component was stably present in the solution.
[0185] When this dispersion was evaluated with a transmission electron microscope, the primary particle size of the titanium oxide particles covering the silver particles was 70 nm, the primary particle size of the titanium oxide particles was 4 nm, the coverage rate was 20% of the surface, and the random rate was 98%. This shows that the dispersion contains an oxide complex in which part of the surface of the silver nanoparticles is randomly covered with titanium oxide nanoparticles.
[0186] [ka]
[0187] A 0.7 mm thick, 50 mm square glass sheet with a solid content of 60 mg / m 2 After coating the dispersion liquid, the substrate was dried at 80° C. and measured with a spectrophotometer (Konica Minolta CM-36sG), and the haze change of the coating film was 0.3. It can be seen that the coating film of Example 1 is excellent in transparency.
[0188] Even when the coating surface of the obtained glass substrate was strongly rubbed with a finger, the coating did not slide off, which shows that the coating of Example 1 has a high degree of adhesion between the titania particles and the glass surface.
[0189] The obtained glass substrate was subjected to an antibacterial test according to JIS Z 2801 after being wiped with water under a load of 750 g using a Heidon friction tester, and the antibacterial activity value was 3.0 or more. It was confirmed that the glass substrate having the coating surface of Example 1 maintained its antibacterial properties even after being wiped with water.
[0190] [Example 2] 30g (0.5mol) of acetic acid was added to 142.1g (0.5mol) of titanium tetraisopropoxide and stirred for 60 minutes, then 538g of water was added and stirred at normal pressure (0.10MPa) and 95℃ for 3 hours, and then high pressure dispersion treatment (160Mpa) was performed to obtain a dispersion liquid containing titanium oxide fine particles. The titanium oxide fine particles contained in this dispersion liquid had an average primary particle size of 3nm from observation of a transmission electron microscope image, and secondary particles of 30nm from a particle size distribution analyzer.
[0191] Silver acetate (I) was added to 15 g of this dispersion (solid content 5.2% by mass) so that silver was 5% by mass based on the metal weight of the titania fine particles (titanium oxide) contained in the dispersion, and the mixture was thoroughly stirred. Then, an ultraviolet lamp was irradiated for 3 hours to obtain a white-ish dispersion. The obtained dispersion did not change in color even after being left for about 3 weeks, and it was confirmed that the silver component was stably present in the solution.
[0192] When this dispersion was evaluated using a transmission electron microscope, the titanium oxide particles covering the silver particles had a particle size of 30 nm, a primary particle size of 4 nm, and a surface coverage of 23%. The randomness rate was 99%. This indicates that the dispersion contains an oxide complex in which part of the surface of the silver particles is randomly covered with titanium oxide particles.
[0193] A 0.7 mm thick, 50 mm square glass sheet with a solid content of 60 mg / m 2 After coating the dispersion liquid, the substrate was dried at 80° C. and measured with a spectrophotometer (Konica Minolta CM-36sG), and the haze change of the coating film was 0.2. It can be seen that the coating film of Example 2 is excellent in transparency.
[0194] Even when the coating surface of the obtained glass substrate was strongly rubbed with a finger, the coating did not slide off, which shows that the coating of Example 2 has a high degree of adhesion between the titania particles and the glass surface.
[0195] The obtained glass substrate was subjected to an antibacterial test according to JIS Z 2801 after being wiped with water under a load of 750 g using a Hayden friction tester, and the antibacterial activity value was 3.0 or more. It was confirmed that the glass substrate having the coating surface of Example 2 maintained its antibacterial properties even after being wiped with water.
[0196] [Example 3] A 20% by mass aqueous dispersion of silica fine particles with a primary particle size of 12 nm was diluted 10 times with distilled water and subjected to high pressure dispersion treatment (200 MPa) to obtain 100 g of a 2% by mass aqueous dispersion. The titanium oxide fine particles contained in this dispersion had an average primary particle size of 12 nm from observation of a transmission electron microscope image, and a secondary particle size distribution meter showed that the average particle size was 80 nm.
[0197] Silver microparticles with a particle size of 100 nm were added to this aqueous dispersion so that the weight of silver contained in the silver microparticles was 5 mass% relative to the weight of silica in the silica microparticles, and the mixture was stirred and mixed at room temperature for 24 hours to obtain an aqueous dispersion of silver microparticles coated with silica microparticles.
[0198] When this dispersion was evaluated using a transmission electron microscope, the primary particle size of the silver particles and the silica particles covering the silver particles were 100 nm and 12 nm, respectively, and the coverage rate was 50% of the surface. The random rate was 80%. This indicates that the dispersion contains an oxide complex in which part of the surface of the silver particles is randomly covered with titanium oxide particles.
[0199] A 0.7 mm thick, 50 mm square glass sheet with a solid content of 60 mg / m 2 After coating the dispersion liquid, the substrate was dried at 80° C. and measured with a spectrophotometer (Konica Minolta CM-36sG), and the haze change of the coating film was 0.5. It can be seen that the coating film of Example 3 is excellent in transparency.
[0200] Even when the coating surface of the obtained glass substrate was strongly rubbed with a finger, the coating did not slide off, which shows that the coating of Example 2 has a high degree of adhesion between the titania particles and the glass surface.
[0201] The obtained glass substrate was subjected to an antibacterial test according to JIS Z 2801 after being wiped with water under a load of 750 g using a Hayden friction tester, and the antibacterial activity value was 3.0 or more. It was confirmed that the glass substrate having the coating surface of Example 2 maintained its antibacterial properties even after being wiped with water.
[0202] [Comparative Example 1] (Silver nanoparticles only) A dispersion of commercially available silver nanoparticles (Sigma-Aldrich) with a particle size of 100 nm was applied to a glass substrate.
[0203] When the coating surface of the obtained glass substrate was rubbed with a finger, peeling was confirmed. The coating film of Comparative Example 1 was not able to be used for further evaluation.
[0204] [Comparative Example 2] (silica supported silver) To 100 g of an aqueous dispersion of silica microparticles with a particle size of 150 nm, silver microparticles with a particle size of 15 nm were added so that the amount of silver contained in the silver microparticles was 1 mass% relative to the amount of silica in the silica microparticles. The mixture was stirred and mixed at room temperature for 24 hours to obtain a 25 mass% aqueous dispersion of silver microparticle-supported silica microparticles.
[0205] When the obtained dispersion liquid was left to stand for about one week, the solution became cloudy and a white precipitate was generated.
[0206] When this dispersion was evaluated by a transmission electron microscope, the particle size of the silver particles was 15 nm, the particle size of the silica particles was 150 nm, the coverage rate was 100% of the surface, and the random rate was 0%.
[0207] This dispersion was applied to a 50 mm square glass substrate with a thickness of 0.7 mm, and the substrate was dried at 80° C. The haze change of the coating film was measured using a spectrophotometer (Konica Minolta CM-36sG) and found to be 2 or more. It can be seen that the dispersion of Comparative Example 2 is inferior in transparency to those of Examples 1 to 3.
[0208] Even when the coated surface of the obtained glass substrate was strongly rubbed with a finger, the coating did not slide off.
[0209] The obtained glass substrate was subjected to an antibacterial test according to JIS Z 2801 after wiping with water under a load of 750 g using a Heidon friction tester, and the antibacterial activity value was less than 2.0. The glass substrate having the coating surface of Comparative Example 2 was unable to maintain the antibacterial property after wiping with water.
[0210] [Comparative Example 3] (Silver nanoparticles are supported on secondary particles of titanium oxide nanoparticles) To 142.1 g (0.5 mol) of titanium tetraisopropoxide, 30 g (0.5 mol) of acetic acid was added and stirred for 60 minutes. Next, 538 g of water was added and stirred at normal pressure (0.10 MPa) and 85°C for 3 hours. Then, ultrasonic dispersion treatment was performed to obtain a dispersion liquid containing titanium oxide microparticles.
[0211] Observation of a transmission electron microscope image of the titanium oxide fine particles contained in this dispersion revealed that the primary particles had an average size of 5 nm, and a particle size distribution meter revealed that the secondary particles had an average size of 2 μm.
[0212] Silver nitrate (I) was added to 15 g of this dispersion (solid content 5.2% by mass) so that silver was 25% by mass based on the metal weight of the titania fine particles (titanium oxide) contained in the dispersion, and the mixture was thoroughly stirred, and then irradiated with an ultraviolet lamp for 30 minutes to obtain a white-ish dispersion. The obtained dispersion did not maintain dispersion stability after 3 weeks, and precipitation was observed.
[0213] The dispersion immediately after being composited with silver was evaluated with a transmission electron microscope, and it was found that in the titanium oxide nanoparticles covering the silver nanoparticles, the primary particle size of the silver nanoparticles was 40 nm, the primary particle size of the titanium oxide nanoparticles was 4 nm, and the structure was such that the silver nanoparticles were supported on the secondary particles of silver. The coverage rate was 100% of the surface, and the random rate was 0%. This shows that the dispersion has a structure in which the silver nanoparticles are supported on the secondary particles of titanium oxide nanoparticles.
[0214] A 0.7 mm thick, 50 mm square glass sheet with a solid content of 60 mg / m 2After coating the dispersion liquid, the substrate was dried at 80° C. and measured with a spectrophotometer (Konica Minolta CM-36sG), and the haze change of the coating film was 2 or more. It can be seen that the dispersion of Comparative Example 3 is inferior in transparency to Examples 1 to 3.
[0215] Even when the coated surface of the obtained glass substrate was strongly rubbed with a finger, the coating did not slide off.
[0216] The obtained glass substrate was subjected to an antibacterial test according to JIS Z 2801 after wiping with water under a load of 750 g using a Heidon friction tester, and the antibacterial activity value was less than 2.0. The glass substrate having the coating surface of Comparative Example 2 was unable to maintain the antibacterial property after wiping with water.
[0217] [Industrial Applicability] The oxide composite of the present invention has a structure in which inorganic oxide fine particles (titania, etc.) are supported around silver fine particles. The oxide composite of the present invention has a structure in which inorganic oxide fine particles (titania, etc.) cover the periphery of silver fine particles. The oxide composite of the present invention is subjected to high-pressure dispersion treatment to control the secondary particle diameter of the inorganic oxide fine particles (silver fine particles supported with titania nanoparticles), thereby coating the periphery of silver with titanium oxide, and making it possible to prepare a dispersion liquid in which silver is uniformly and stably dispersed in liquid.
[0218] The oxide composite of the present invention improves the resistance of silver to elution into water by coating silver nanoparticles with a sol of inorganic oxide fine particles (titanium oxide, etc.), thereby making it possible to maintain the antibacterial and antiviral properties of the silver contained in the oxide composite, as well as the adhesion of the oxide composite to a substrate and the transparency of the oxide composite, etc.
Claims
1. An oxide composite, (A) A part of the surface of the silver fine particles is covered with (B) inorganic oxide fine particles, the (A) silver fine particles have an average primary particle diameter of 1 nm to 1,000 nm as measured by a transmission electron microscope (TEM); The inorganic oxide fine particles (B) have an average primary particle diameter of 1 nm to 100 nm as measured by observation with a transmission electron microscope (TEM); the ratio of the average primary particle diameter of the (A) silver fine particles to the average primary particle diameter of the (B) inorganic oxide fine particles (average primary particle diameter of the (A) silver fine particles / average primary particle diameter of the (B) inorganic oxide fine particles) is 1 to 1,000; Oxide complex.
2. 2. The oxide composite according to claim 1, wherein the (A) silver fine particles have an average primary particle diameter of 1 nm to 200 nm.
3. 2. The oxide complex according to claim 1, wherein the (A) silver fine particles have a surface coverage of 1 surface % or more.
4. 2. The oxide composite according to claim 1, wherein the (A) silver fine particles have a surface coverage of 5 surface % to 95 surface %.
5. 2. The oxide composite according to claim 1, wherein the ratio of the average primary particle diameter of the (A) silver fine particles to the average primary particle diameter of the (B) inorganic oxide fine particles (average primary particle diameter of the (A) silver fine particles / average primary particle diameter of the (B) inorganic oxide fine particles) is 1 or more and 200 or less.
6. 2. The oxide composite according to claim 1, wherein a ratio of an average primary particle diameter of the (A) silver fine particles to an average primary particle diameter of the (B) inorganic oxide fine particles (average primary particle diameter of the (A) silver fine particles / average primary particle diameter of the (B) inorganic oxide fine particles) is 1 to 100.
7. 2. The oxide composite according to claim 1, wherein the (B) inorganic oxide fine particles covering the (A) silver fine particles have a random ratio of 50% or more.
8. The mass of titanium oxide (TiO 2 (A) the mass ratio of the silver mass (Ag mass) in the silver fine particles to the mass (A) Ag mass in silver particles / (B) TiO in inorganic oxide particles 2 Mass) is ≦10.
9. In the oxide composite, 2. The oxide composite according to claim 1, wherein the sum of the solid contents of the (A) silver fine particles and the (B) inorganic oxide fine particles is 50 mass % or less.
10. 2. The oxide composite according to claim 1, wherein the inorganic oxide fine particles (B) are titania fine particles (B1).
11. The (B1) titania fine particles are The surface is protected with organic acid. The mass of the organic acid is 1% by mass or more relative to the weight of the titanium oxide. The oxide composite according to claim 10.
12. The organic acid is At least one organic acid selected from the group consisting of monocarboxylic acids having 1 to 4 carbon atoms and hydroxycarboxylic acids having 2 to 3 carbon atoms, or An acyloxy group derived from at least one organic acid selected from the group consisting of monocarboxylic acids having 1 to 4 carbon atoms and hydroxycarboxylic acids having 2 to 3 carbon atoms. The oxide complex according to claim 11,
13. 12. The oxide complex according to claim 11, wherein the organic acid is at least one organic acid selected from the group consisting of acetic acid and lactic acid.
14. 11. The oxide composite according to claim 10, wherein the (B1) titania fine particles are positively charged.
15. The oxide composite according to any one of claims 1 to 14, and water, A dispersion containing 0.5% by mass or more of water.
16. 16. The dispersion of claim 15, wherein the pH of the dispersion is pH=1-8.
17. A paint comprising the oxide complex according to any one of claims 1 to 14.
18. A coating film formed by the coating material according to claim 17.
19. A paint comprising the dispersion of claim 15.
20. A coating film formed by the coating material according to claim 19.
Citation Information
Patent Citations
One-step preparation of Ag@TiO2 nanocomposite
CN105834448A
Antibacterial and deodorant material and its production
JP1999349423A
Core-shell type nanoparticles and method for producing the same
JP2009519374A
Metal nanoparticle carrying titania nanoparticle and photocatalyst using the same
JP2021154233A