Adhesive Sheet
The adhesive sheet with an epoxy resin and film-forming aid, combined with a curing agent or accelerator in the coating layer, addresses the issue of room temperature storage and handling issues, enabling cost-effective and efficient use by suppressing curing reactions until heated for application.
Patent Information
- Application Number
- JP2024526976
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-12-06
- Filing Date
- 2023-12-05
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2043-12-05
AI Technical Summary
Existing adhesive sheets containing thermosetting resins cannot be stored at room temperature due to the presence of curing agents and accelerators, leading to undesired sticking and blocking during handling, and require refrigerated storage to prevent curing reactions.
An adhesive sheet with an adhesive layer containing an epoxy resin and a film-forming aid, and a coating layer with an epoxy resin curing agent or accelerator, which suppresses curing at room temperature and allows for storage and immediate use without refrigeration.
The adhesive sheet can be stored at room temperature, reducing storage and transportation costs, and ensures easy handling and immediate use with excellent workability by preventing tackiness and allowing for curing when heated.
Smart Images

Figure 0007596603000001 
Figure 0007596603000002 
Figure 0007596603000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive sheet, and more specifically to an adhesive sheet which is easy to work with and can be stored at room temperature for long periods of time. [Background technology]
[0002] Adhesive sheets are used in various fields, such as reinforcing rivet joints in building construction materials, bonding decorative panels for furniture and building materials, automotive interior materials, interlayer adhesion and structural adhesion of carbon fiber reinforced plastics (CFRP), and bonding coverlay films for flexible electronic circuit boards. The applicant of the present application has proposed an adhesive sheet having an adhesive layer made of a composition for the adhesive layer containing a thermosetting resin, and a coating layer formed on the adhesive layer and containing a resin, the coating layer exhibiting no tack at room temperature, and at least a part of the coating layer disappearing in the range from the interface between the adhesive layer and the coating layer to the surface of the coating layer by heating the adhesive sheet to a temperature equal to or higher than the curing start temperature of the adhesive layer (see Patent Document 1). The adhesive sheet of Patent Document 1 can prevent undesired sticking and blocking during the work before the adhesive layer is heat-cured, and can achieve excellent workability. However, the adhesive sheet of Patent Document 1 cannot be stored at room temperature because the adhesive layer contains a base agent, a curing agent, and a curing accelerator, and therefore there is room for improvement in terms of storage stability. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-163694 A Summary of the Invention [Problem to be solved by the invention]
[0004] Therefore, an object of the present invention is to provide an adhesive sheet that can be stored at room temperature and has excellent workability. [Means for solving the problem]
[0005] In view of the above problems, the present inventors have conducted extensive research and found that, in an adhesive sheet having an adhesive layer made of a composition for an adhesive layer containing an epoxy resin and a film-forming aid, and a coating layer formed on the adhesive layer and containing a thermoplastic resin, at least one of an epoxy resin curing agent and an epoxy resin curing accelerator is added to the coating layer to suppress the curing reaction in the adhesive layer, thereby obtaining an adhesive sheet that can be stored at room temperature and has excellent workability, and have come up with the present invention. That is, the adhesive sheet of the present invention has an adhesive layer made of a composition for an adhesive layer containing an epoxy resin and a film-forming aid, and a coating layer formed on the adhesive layer and containing a thermoplastic resin, the coating layer contains at least one of an epoxy resin curing agent and an epoxy resin curing accelerator, does not show tack at room temperature, the heat generation ratio of the adhesive sheet after being left at 40°C for 14 days is 80% or more, and at least a part of the coating layer disappears in the range from the interface between the adhesive layer and the coating layer to the surface of the coating layer by heating the adhesive sheet to a temperature equal to or higher than the curing start temperature of the adhesive layer.
[0006] The film-forming auxiliary and the thermoplastic resin are each preferably at least one selected from the group consisting of a phenoxy resin, a polyvinyl acetal resin, a polyester resin, and an acrylic resin. The epoxy resin curing agent contained in the coating layer may be at least one selected from the group consisting of dicyandiamide, imidazole compounds, and tertiary amines. The epoxy resin curing accelerator contained in the coating layer may be at least one selected from the group consisting of imidazole compounds, tertiary amines, and phosphorus-based compounds. The coating layer may contain at least one of the epoxy resin curing agents and at least one of the epoxy resin curing accelerators (excluding those of the same type as the epoxy resin curing agent). In addition, the adhesive sheet of the present invention may be configured such that the adhesive layer contains an epoxy resin curing agent, and the epoxy resin curing agent is at least one selected from dicyandiamide, an imidazole compound, a tertiary amine, and an acid anhydride, and the coating layer contains an epoxy resin curing accelerator, and the epoxy resin curing accelerator is at least one selected from imidazole compounds, tertiary amines, and phosphorus-based compounds (excluding those of the same type as the curing agent). Effect of the Invention
[0007] The adhesive sheet of the present invention is characterized in that the curing reaction of the epoxy resin is suppressed during storage, and when the adhesive sheet is used, the components of the adhesive layer and the components of the coating layer formed on the upper part are mixed, the reaction is promoted, and the curing proceeds. Therefore, the adhesive sheet of the present invention can be stored at room temperature, and it is easy to secure a storage space, and refrigerated transportation is not required, so that the cost of transportation and storage can be reduced. In addition, in the conventional adhesive sheet that required refrigerated storage to suppress the progress of the curing reaction at room temperature, when using it, in order to avoid the adverse effect on the adhesive sheet due to condensation, it was opened after acclimatizing to room temperature. However, since the adhesive sheet of the present invention can be stored at room temperature, it can be used immediately after taking it out, and it is expected to speed up the work. The heating conditions when using the adhesive sheet of the present invention are not particularly limited, and by adjusting the material composition of the adhesive layer and the coating layer, a cured epoxy resin can be obtained under heating conditions equivalent to those of existing adhesive sheets. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The following describes in detail the embodiments of the present invention, but the present invention should not be construed as being limited thereto. Various changes, modifications, and improvements can be made based on the knowledge of those skilled in the art without departing from the scope of the present invention. In this specification, the term "to" indicating a range of values indicates a range including the values given as the upper and lower limits. When a unit is given only for the upper limit of a range of values, it means that the lower limit is expressed in the same unit as the upper limit. In the present specification, in which numerical ranges are described in stages, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in this specification, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples. In this specification, the content or amount of each component in a composition means, when multiple substances corresponding to each component are present in the composition, the total content or amount of those multiple substances present in the composition, unless otherwise specified.
[0009] The adhesive sheet of this embodiment has an adhesive layer made of a composition for the adhesive layer containing an epoxy resin and a film-forming aid, and a coating layer formed on the adhesive layer and containing a thermoplastic resin, the coating layer containing at least one of an epoxy resin curing agent and an epoxy resin curing accelerator, exhibiting no tack at room temperature, the heat generation ratio of the adhesive sheet after being left at 40°C for 14 days being 80% or more, and being characterized in that at least a portion of the coating layer disappears in the range from the interface between the adhesive layer and the coating layer to the surface of the coating layer when the adhesive sheet is heated to a temperature equal to or higher than the curing initiation temperature of the adhesive layer.
[0010] As described above, the adhesive sheet according to the present embodiment is characterized in that it can suppress the progress of the curing reaction of the epoxy resin in the adhesive layer at room temperature. For this purpose, any one of the following configurations is adopted: (i) an epoxy resin curing agent and an epoxy resin curing accelerator are added to the coating layer, and neither an epoxy resin curing agent nor an epoxy resin curing accelerator is added to the adhesive layer; (ii) an epoxy resin curing agent is added to the coating layer, and an epoxy resin curing accelerator is added to the adhesive layer; (iii) an epoxy resin curing accelerator is added to the coating layer, and an epoxy resin curing agent is added to the adhesive layer; and (iv) an epoxy resin curing agent is added to the coating layer, and neither an epoxy resin curing agent nor an epoxy resin curing accelerator is added to the adhesive layer. Details of each configuration will be described later.
[0011] In the adhesive sheet according to the present embodiment, the coating layer does not exhibit tack (stickiness) at room temperature, and therefore it is possible to prevent a decrease in workability caused by tack, etc. The presence or absence of tack in the coating layer can be evaluated by the following method. The sheet in which the coating layer was laminated on the release film was cut into a size of 5 cm x 5 cm, and the sheets were sandwiched between 1 mm thick glass plates, with the coating layers facing each other and with the release film facing the coating layer. A load of 100 g was placed on the sheets, and the sheets were left in a room temperature (25°C) environment for 24 hours, after which the load was removed and the glass plate was spread up and down to check the peeling state, thereby evaluating the tackiness of the coating layer. Specific evaluation criteria will be described later.
[0012] The adhesive sheet according to this embodiment is characterized in that the heat generation ratio after being left standing at 40° C. for 14 days, as measured by the method described below, is 80% or more. The adhesive sheet according to this embodiment, in which the heat generation ratio after being left at 40°C for 14 days is 80% or more, can suppress the progress of curing of the epoxy resin even when stored at room temperature. Therefore, the adhesive sheet according to this embodiment can be stored at room temperature, making it easy to secure a storage space, and does not require refrigerated transportation, thereby reducing the costs of transportation and storage. In addition, since the adhesive sheet according to this embodiment can be stored at room temperature, it can be used immediately after being taken out, and this is expected to speed up the work. The heat generation ratio after being left at 40° C. for 14 days is preferably 85% or more, and more preferably 90% or more.
[0013] In the adhesive sheet according to this embodiment, by heating the adhesive layer to a temperature equal to or higher than the curing start temperature, at least a part of the coating layer disappears in the range from the interface between the adhesive layer and the coating layer to the surface of the coating layer. The term "the coating layer disappears" refers to the fact that the coating layer is softened by applying heat exceeding the glass transition temperature of the resin forming the coating layer to the adhesive sheet according to this embodiment, and the resin of the coating layer is mixed with the epoxy resin (before curing) forming the adhesive layer and integrated with the adhesive layer, so that the coating layer that was present on the adhesive layer apparently disappears. The presence or absence of loss of the coating layer can be judged from the ratio (Pm / Pc) of the measured tensile shear bond strength (Pc) of the coating layer alone between steel sheets A and B to the measured tensile shear bond strength (Pm) of the laminate after heating between steel sheets A and B. The specific method will be described later. The specific configuration of the adhesive sheet according to this embodiment will be described below.
[0014] (1) Adhesive layer The adhesive layer of the adhesive sheet according to this embodiment (hereinafter also simply referred to as "adhesive layer") is made of a composition for adhesive layers that contains an epoxy resin and a film-forming auxiliary. 1) Epoxy resin The epoxy resin used in the adhesive layer is not particularly limited. Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, hydantoin type epoxy resins, biphenyl type epoxy resins, alicyclic epoxy resins, triphenylmethane type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, naphthol novolac type epoxy resins, dicyclopentadiene / phenol epoxy resins, alicyclic amine epoxy resins, aliphatic amine epoxy resins, and epoxy resins modified by various methods such as CTBN modification and halogenation. Among these, bisphenol A type epoxy resins and novolac type epoxy resins are preferred from the viewpoint of heat resistance and availability. In addition, these epoxy resins can be used alone or in combination. The epoxy resin used in the adhesive layer is preferably a mixture of a liquid epoxy resin and a solid epoxy resin at room temperature (25°C) in order to improve the stickiness of the adhesive layer when processed into an adhesive sheet and ensure flexibility when the adhesive sheet is processed into a roll.
[0015] The epoxy equivalent (WPE) of the epoxy resin used in the adhesive layer is preferably 150 or more, more preferably 180 or more, and preferably 1000 or less, more preferably 700 or less. If the WPE is lower than 150, a cured product with high heat resistance due to many crosslinking points is obtained, but the toughness is low and it may become brittle. If the WPE is higher than 1000, the heat resistance may decrease due to the small number of crosslinking points. The "epoxy equivalent" is defined as the molecular weight of the epoxy resin per epoxy group. Here, the "epoxy group" includes oxacyclopropane (oxirane ring), which is a three-membered ring ether, and includes glycidyl groups (including glycidyl ether groups and glycidyl ester groups) in addition to epoxy groups in the narrow sense. The WPE is determined by the method (perchloric acid-tetraethylammonium bromide method) described in JIS K7236, Determination of epoxy equivalent of epoxy resin (2001), etc. In this specification, when a plurality of epoxy resins are used, the above epoxy equivalent means the epoxy equivalent of the epoxy resins after mixing.
[0016] 2) Film-forming assistant In this embodiment, the adhesive layer contains a film-forming auxiliary. By adding the film-forming auxiliary to the adhesive layer, the adhesive layer surface on which the adhesive layer composition is applied and dried does not suffer from repellency or uneven application, and thus the application properties can be improved. Examples of film-forming aids that can be used in the adhesive layer include thermoplastic resins such as phenoxy resin, polyester resin, polyurethane resin, polyacetal resin, polyamide resin, polypropylene, polyvinyl butyral resin, polyvinyl acetal resin, polyvinyl acetate, nylon, and acrylic resin; and rubber materials such as polybutadiene, styrene-butadiene rubber, styrene-butadiene-styrene copolymer, styrene-ethylene-butylene-styrene copolymer, butyl rubber, chloroprene rubber, acrylonitrile-butadiene copolymer, acrylonitrile-butadiene-acrylic acid copolymer, acrylonitrile-butadiene-styrene copolymer, natural rubber, isoprene rubber, chloroprene rubber, nitrile rubber, fluororubber, and acrylic rubber. Among these, from the viewpoint of affinity with epoxy resin, it is preferable to use at least one selected from phenoxy resin, polyvinyl acetal resin, polyester resin and acrylic resin.Furthermore, phenoxy resin, polyvinyl acetal resin and polyester resin having a hydroxyl group are more preferable.These film forming assistants can be used alone or in combination.
[0017] The phenoxy resin refers to a high molecular weight thermoplastic polyether resin based on a diphenol such as bisphenol A or bisphenol F and an epihalohydrin such as epichlorohydrin. The weight average molecular weight of the phenoxy resin is preferably 20,000 to 100,000. When the weight average molecular weight is 20,000 or more, film-forming properties can be imparted. On the other hand, when the weight average molecular weight is 100,000 or less, the viscosity during coating film formation does not become too high, and a smooth and uniform coating film can be obtained. The phenoxy resin is not particularly limited, and examples thereof include those having one or more skeletons selected from a bisphenol A skeleton, a bisphenol F skeleton, a bisphenol S skeleton, a bisphenolacetophenone skeleton, a novolac skeleton, a biphenyl skeleton, a fluorene skeleton, a dicyclopentadiene skeleton, a norbornene skeleton, a naphthalene skeleton, anthracene skeleton, an adamantane skeleton, a terpene skeleton, and a trimethylcyclohexane skeleton.
[0018] Commercially available phenoxy resins include, for example, trade names PKHB, PKHC, PKHH, and PKHJ (all manufactured by HUNTSMAN), jER (registered trademark) 1256, 4250, and 4275 (all manufactured by Mitsubishi Chemical Corporation), YP-50, YP-50S, YP-70, ZX-1356-2, and FX-316 (all manufactured by Nippon Steel Chemical & Material Co., Ltd.). Phenoxy resins dissolved in a solvent are also commercially available, and these can be used in the same manner. For example, jER 1256B40, 1255HX30, YX6954BH30, YX6954B35, YX8100BH30, YL7174BH40 (all manufactured by Mitsubishi Chemical Corporation), YP-40ASM40, YP-50EK35, YPB-40PXM40, ERF-001M30, YPS-007A30, FX-293AT40 (all manufactured by Nippon Steel Chemical & Material Co., Ltd.), etc. can be mentioned. These phenoxy resins can be used alone or in combination.
[0019] Examples of polyvinyl acetal resins include those sold under the trade name S-LEC (registered trademark) KS-23Z, KS-1, KS-5, BX-1, and BM-S (all manufactured by Sekisui Chemical Co., Ltd.). Examples of polyester resins include Vylon (registered trademark) series (manufactured by Toyobo MC Co., Ltd.), Nichigo Polyester TP series (manufactured by Mitsubishi Chemical Corporation), and Elitel (registered trademark) UE series (manufactured by Unitika Ltd.).
[0020] The mass ratio of the epoxy resin to the film-forming aid in the adhesive layer (epoxy resin: film-forming aid) is preferably in the range of 3:1 to 20:1, more preferably in the range of 3:1 to 15:1, and particularly preferably in the range of 4:1 to 12:1. By adjusting the mass ratio of the epoxy resin to the film-forming aid in the adhesive layer within the above range, repellency and uneven coating during coating of the adhesive layer composition are improved, and the coatability is further improved, and the surface stickiness and peelability from the release film can be improved, resulting in an adhesive layer with excellent heat resistance.
[0021] 3) Epoxy resin hardener The adhesive sheet according to this embodiment is characterized in that it is possible to inhibit the progress of the curing reaction of the adhesive sheet at room temperature. To achieve this, as described above, it is necessary to adopt any one of the following configurations: (i) a configuration in which an epoxy resin curing agent and an epoxy resin curing accelerator are added to the coating layer, and neither an epoxy resin curing agent nor an epoxy resin curing accelerator is added to the adhesive layer; (ii) a configuration in which an epoxy resin curing agent is added to the coating layer, and an epoxy resin curing accelerator is added to the adhesive layer; (iii) a configuration in which an epoxy resin curing accelerator is added to the coating layer, and an epoxy resin curing agent is added to the adhesive layer; and (iv) a configuration in which an epoxy resin curing agent is added to the coating layer, and neither an epoxy resin curing agent nor an epoxy resin curing accelerator is added to the adhesive layer. In the configurations (i), (ii), and (iv), the adhesive layer does not contain an epoxy resin curing agent, so the following describes the epoxy resin curing agent in the configuration (iii).
[0022] In the configuration of (iii), the epoxy resin curing agent contained in the adhesive layer is at least one selected from dicyandiamide (DICY), an imidazole compound, a tertiary amine, and an acid anhydride, and the coating layer contains at least one epoxy resin curing accelerator selected from an imidazole compound, a tertiary amine, and a phosphorus-based compound. However, the epoxy resin curing accelerator contained in the coating layer and the epoxy resin curing agent contained in the adhesive layer must be different types of compounds. For example, when dicyandiamide is added to the adhesive layer as an epoxy resin curing agent, at least one of imidazole compounds, tertiary amines, and phosphorus compounds can be added to the coating layer as an epoxy resin curing accelerator. In an adhesive sheet composed of such an adhesive layer and coating layer, the progress of the curing reaction of the epoxy resin can be suppressed during storage at room temperature, and by heating the adhesive sheet during use, the epoxy resin and epoxy resin curing agent in the adhesive layer and the epoxy resin curing accelerator in the coating layer are mixed together, and the curing reaction of the epoxy resin progresses.
[0023] Examples of the imidazole compound include 2-methylimidazole, 2-phenyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,4-diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine, 2-ethyl-4-methylimidazole, and 2-phenyl-4,5-dihydroxymethylimidazole.
[0024] Examples of the tertiary amines include 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo[5.4.0]-7-undecene, triethylenediamine, N,N-dimethylbenzylamine, 4-dimethylaminopyridine, 2-dimethylaminomethylphenol, and 1,5-diazabicyclo[4.3.0]-5-nonene.
[0025] Examples of the acid anhydride include phthalic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, methylbicyclo[2.2.1]heptane-2,3-dicarboxylic anhydride, bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride, 4-methylcyclohexane-1,2-dicarboxylic anhydride, bicyclo[2.2.1]heptane-2,3-dicarboxylic anhydride, 1,2,4,5-cyclohexane Tetracarboxylic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, 1,2,3,4-cyclopentane tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 2,2',3,3'-diphenyl tetracarboxylic dianhydride, 2,3,3',4-biphenyl tetracarboxylic dianhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, ethylene glycol bistrimellitic anhydride, 4,4'-[propane-2,2-diylbis(1,4-phenyleneoxy)]diphthalic dianhydride, and the like.
[0026] In the configuration (iii), a commercially available product of dicyandiamide to be added to the adhesive layer includes the product name DICY7 (manufactured by Mitsubishi Chemical Corporation). In addition, a commercially available product of an imidazole compound includes the product names Curesol (registered trademark) 2MZA-PW, 2P4MHZ-PW, 2E4MZ, and 2PHZ (all manufactured by Shikoku Chemical Industry Co., Ltd.). Commercially available products of tertiary amines include the product names Ancamine (registered trademark) series (manufactured by Evonik Corporation), DBU (registered trademark), and U-CAT (registered trademark) series (all manufactured by San-Apro Co., Ltd.).
[0027] The amount of epoxy resin curing agent is calculated from the equivalent ratio with the epoxy resin used, and the suitable range of the equivalent ratio is 0.2 to 2.0. For example, when the epoxy resin curing agent is dicyandiamide, the amount is preferably in the range of 2 to 20 parts by mass, more preferably in the range of 5 to 15 parts by mass, per 100 parts by mass of the epoxy resin. If the amount of the epoxy resin curing agent is less than 2 parts by mass, it is difficult to cure sufficiently, and there is a possibility that the characteristics of the epoxy resin, such as heat resistance and chemical resistance, cannot be fully exhibited. On the other hand, if the amount is more than 20 parts by mass, an excessive exothermic reaction occurs during curing, and unreacted epoxy resin curing agent remains in the cured product, which may affect the resin properties.
[0028] 4) Epoxy resin curing accelerator In the case of the constitution (iii), when dicyandiamide is added as an epoxy resin curing agent to the adhesive layer, the imidazole compound and tertiary amines added as an epoxy resin curing accelerator to the coating layer can be the above-mentioned ones. Examples of phosphorus-based compounds include organic phosphines such as tributylphosphine, triphenylphosphine, and tri-p-tolylphosphine, and phosphonium salts such as triphenylborane-triphenylphosphine complex and tetrakis(4-methylphenyl)borane-tetraphenylphosphine complex. These epoxy resin curing accelerators can be used alone or in combination as long as they are not the same type as the epoxy resin curing agent contained in the adhesive layer.
[0029] Commercially available phosphorus compounds include Hokuko TPP (registered trademark), TPTP, TPP-S, TPP-K, and TPP-MK (all manufactured by Hokuko Chemical Industry Co., Ltd.).
[0030] In this embodiment, the epoxy resin curing accelerator is contained in a layer different from the epoxy resin and the epoxy resin curing agent, so that the epoxy resin curing accelerator can be blended without significantly affecting the storage stability of the adhesive sheet. When an epoxy resin curing accelerator that is solid at room temperature is used, the blending amount of the epoxy resin curing accelerator is preferably 20 parts by mass or less per 100 parts by mass of the thermoplastic resin. By setting the blending amount of the epoxy resin curing accelerator within the above range, the dispersion stability and viscosity of the coating layer forming coating liquid become good, and it becomes possible to prepare a coating layer with good smoothness. In addition, it is also possible to suppress the remaining of unreacted matter during thermal curing, so that it becomes possible to prepare an adhesive sheet with excellent heat resistance.
[0031] Next, the epoxy resin curing accelerator added to the adhesive layer in the configuration (ii) will be described. A phosphorus-based compound can be added as the epoxy resin curing accelerator. Imidazole compounds and tertiary amines function as epoxy resin curing agents by themselves, so they cannot be added as epoxy resin curing accelerators in the configuration of (ii). In such an adhesive sheet composed of an adhesive layer and a coating layer, the progress of the curing reaction of the epoxy resin can be suppressed during storage at room temperature, and by heating the adhesive sheet during use, the epoxy resin and the epoxy resin curing accelerator in the adhesive layer and the epoxy resin curing agent in the coating layer are mixed together, and the curing reaction of the epoxy resin progresses.
[0032] In the configuration (ii), the amount of the epoxy resin curing accelerator added to the adhesive layer is preferably, for example, 5 parts by mass or less per 100 parts by mass of the epoxy resin. However, in this embodiment, since the epoxy resin curing accelerator is contained in a layer different from the epoxy resin curing agent, even if the amount of the epoxy resin curing accelerator exceeds 5 parts by mass, the storage stability of the adhesive sheet is not significantly affected.
[0033] 5) Other additives The adhesive layer composition forming the adhesive layer may contain other additives that can be added as optional components, such as thickeners (amorphous silica, calcium carbonate, talc, etc.), thermal foaming agents, foaming assistants, various fillers, foam stabilizers, antioxidants, ultraviolet absorbers, flame retardants, colorants, etc.
[0034] (2) Coating layer The coating layer of the adhesive sheet according to this embodiment (hereinafter, simply referred to as the "coating layer") is formed on the adhesive layer and is made of a composition containing a thermoplastic resin. The coating layer contains at least one of an epoxy resin curing agent and an epoxy resin curing accelerator, and does not exhibit tack at room temperature. Furthermore, when the adhesive sheet is used, by heating the adhesive layer to a temperature equal to or higher than the curing initiation temperature, at least a portion of the coating layer disappears from the interface between the adhesive layer and the coating layer to the surface of the coating layer, and at least a portion of the adhesive layer after heat curing is exposed at the portion of the adhesive sheet that contacts the adherend, thereby functioning as an adhesive sheet. The components constituting the coating layer will be described below.
[0035] 1)Thermoplastic resin The thermoplastic resin used in the coating layer can be one described as a thermoplastic resin in the film-forming assistant used in the adhesive layer. From the viewpoint of affinity with epoxy resin, it is preferable to use at least one thermoplastic resin selected from phenoxy resin, polyvinyl acetal resin, polyester resin, and acrylic resin. Among these, phenoxy resin, polyvinyl acetal resin, and polyester resin having a hydroxyl group are more preferable. The thermoplastic resin can be used alone or in combination. Specifically, better affinity is achieved in a configuration in which the film-forming aid used in the adhesive layer is a phenoxy resin and the thermoplastic resin used in the coating layer is a phenoxy resin and / or a polyvinyl acetal resin and / or a polyester resin having a hydroxyl group, and in a configuration in which the film-forming aid used in the adhesive layer is a polyvinyl acetal resin and the thermoplastic resin used in the coating layer is a phenoxy resin and / or a polyvinyl acetal resin and / or a polyester resin having a hydroxyl group.
[0036] 2) Epoxy resin hardener and / or epoxy resin hardening accelerator As described above, the adhesive sheet according to the present embodiment is characterized in that the progress of the curing reaction of the epoxy resin in the adhesive layer at room temperature is suppressed. For this purpose, it is necessary to adopt any one of the following configurations: (i) a configuration in which an epoxy resin curing agent and an epoxy resin curing accelerator are added to the coating layer, and neither an epoxy resin curing agent nor an epoxy resin curing accelerator is added to the adhesive layer; (ii) a configuration in which an epoxy resin curing agent is added to the coating layer, and an epoxy resin curing accelerator is added to the adhesive layer; (iii) a configuration in which an epoxy resin curing accelerator is added to the coating layer, and an epoxy resin curing agent is added to the adhesive layer; and (iv) a configuration in which an epoxy resin curing agent is added to the coating layer, and neither an epoxy resin curing agent nor an epoxy resin curing accelerator is added to the adhesive layer. The configuration of (iii) is as described above, so the configurations of (i), (ii), and (iv) will be described below.
[0037] (i) A structure in which an epoxy resin curing agent and an epoxy resin curing accelerator are added to the coating layer, and neither an epoxy resin curing agent nor an epoxy resin curing accelerator is added to the adhesive layer. In this configuration, the epoxy resin curing agent added to the coating layer is preferably at least one selected from dicyandiamide, an imidazole compound, and a tertiary amine, and the epoxy resin curing accelerator is preferably at least one selected from an imidazole compound, a tertiary amine, and a phosphorus-based compound, except for those of the same type as the epoxy resin curing agent. Details of each component are as described above. Among the above, a configuration using dicyandiamide as an epoxy resin curing agent and an imidazole compound as an epoxy resin curing accelerator is preferred, since it suppresses the progress of the curing reaction of the epoxy resin even when stored at room temperature for a long period of time, and also completely removes the coating layer when heated during use, thereby realizing better adhesion.
[0038] (ii) A structure in which an epoxy resin curing agent is added to the coating layer and an epoxy resin curing accelerator is added to the adhesive layer. In this configuration, when an epoxy resin curing agent is added to the coating layer, the epoxy resin curing agent is preferably at least one selected from dicyandiamide, an imidazole compound, and a tertiary amine. The details of each component are as described above. The epoxy resin curing accelerator is also as described above.
[0039] (iv) A structure in which an epoxy resin curing agent is added to the coating layer, and neither an epoxy resin curing agent nor an epoxy resin curing accelerator is added to the adhesive layer. In this configuration, when an epoxy resin curing agent is added to the coating layer, the epoxy resin curing agent is preferably at least one selected from an imidazole compound and a tertiary amine. Details of each component are as described above. Among the above, a configuration using an imidazole compound as an epoxy resin curing agent is preferable because it suppresses the progress of the curing reaction of the epoxy resin even when stored at room temperature for a long period of time, and the coating layer disappears when heated during use, thereby achieving excellent adhesion.
[0040] (3) Method for preparing adhesive sheet The composition for the adhesive layer can be obtained by mixing the above-mentioned epoxy resin and film-forming aid with an epoxy resin curing agent or an epoxy resin curing accelerator, various additives, etc., in any order, as necessary. The above raw materials can be mixed using a mixer or kneader such as a mixing roll, a planetary mixer, a butterfly mixer, a kneader, or a single-screw or twin-screw extruder. The mixing temperature varies depending on the composition, but it is preferable to perform the mixing at a temperature lower than the curing initiation temperature. The components of the adhesive layer composition are desirably adjusted so that the adhesive sheet formed from the adhesive layer composition in a sheet form has a curing initiation temperature of 60°C or higher and 200°C or lower.
[0041] The adhesive layer is obtained by dissolving or dispersing the above-mentioned adhesive layer composition in a solvent, applying it to one or both sides of a substrate described later, and drying it as necessary. The adhesive layer can also be obtained by applying the above-mentioned adhesive layer composition to a coating layer described later formed on a separately prepared release film, and drying it as necessary. The adhesive layer can also be obtained by applying the above-mentioned adhesive layer composition to one side of a substrate that has been subjected to a release treatment, and drying it as necessary.
[0042] The method for applying the adhesive layer-forming coating liquid is not particularly limited, and may be a conventionally known application method using a wire bar, applicator, brush, spray, roller, gravure coater, die coater, lip coater, comma coater, knife coater, reverse coater, spin coater, etc. The surface of the release film or substrate to which the adhesive layer-forming coating liquid is applied may be previously subjected to a surface treatment as necessary.
[0043] There is no particular limitation on the method for drying the adhesive layer-forming coating liquid, and any conventionally known drying method such as hot air drying, reduced pressure drying, etc. The drying conditions may be appropriately set depending on the type of adhesive layer composition, the type of solvent used in the adhesive layer-forming coating liquid, the thickness of the adhesive layer, etc., but drying is generally performed at a temperature of about 60 to 200°C.
[0044] The thickness (t1) of the adhesive layer may be appropriately selected depending on the application of the adhesive sheet, but is preferably in the range of 10 μm to 1000 μm, more preferably in the range of 30 μm to 400 μm, and particularly preferably in the range of 30 μm to 200 μm. By making the thickness of the adhesive layer 10 μm or more, for example, it is possible to conform to an adherend having unevenness, and therefore stable adhesive performance can be maintained. By making the thickness (t1) of the adhesive layer 1000 μm or less, it can be suitably used in applications requiring thin films.
[0045] Examples of the solvent include aromatic solvents such as toluene and xylene; ester solvents such as ethyl acetate, butyl acetate, methoxybutyl acetate, and methoxypropyl acetate; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; and ether solvents such as diethyl ether, dibutyl ether, tetrahydrofuran, 1,3-dioxolane, 1,4-dioxane, propylene glycol monomethyl ether acetate, diethylene glycol dimethyl ether, and diethylene glycol ethyl methyl ether, which may be used alone or in combination of two or more.
[0046] The substrate is not particularly limited and may be appropriately selected, and examples thereof include films, nonwoven fabrics, and papers made of synthetic resins such as polyethylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, polycarbonate, triacetyl cellulose, aramid, polyimide, polyamide, polyphenylene sulfide, polyetherimide, polyethersulfone, aromatic polyamide, and polysulfone. The substrate is selected depending on the application of the adhesive sheet. In particular, in applications requiring insulation and heat resistance, it is preferable to use polyimide films and aramid nonwoven fabric sheets.
[0047] The thickness of the substrate can be appropriately selected depending on the application. For example, when the application is for bonding various parts of electronic devices that require insulation as described below, the thickness of the substrate is preferably 25 to 250 μm.
[0048] The composition for the coating layer can be obtained by mixing the above-mentioned thermoplastic resin with an epoxy resin curing agent or an epoxy resin curing accelerator, various additives, etc., in any order, as necessary. The above-mentioned raw materials can be mixed using a mixer or kneader such as a mixing roll, a planetary mixer, a butterfly mixer, a kneader, or a single-screw or twin-screw extruder. The mixing temperature varies depending on the composition, but it is preferable to perform the mixing at a temperature lower than the curing initiation temperature.
[0049] The coating layer is obtained by dissolving or dispersing the above-mentioned composition for the coating layer in a solvent, applying it to one or both sides of the above-mentioned substrate, and drying it as necessary. There is no particular restriction on the method of applying and drying the coating liquid for forming the coating layer, and the same method as the method of applying and drying the coating liquid for forming the adhesive layer described above can be used.
[0050] The thickness (t2) of the coating layer is preferably 100% or less of the thickness (t1) of the adhesive layer before heating, more preferably 50% or less, and particularly preferably 30% or less. By making t2 100% or less of t1, the coating layer is softened by heat and can be easily removed. The mechanism by which the coating layer disappears is as follows: The coating layer softens when heat exceeding the glass transition temperature of the resin that forms the coating layer is applied. This causes the resin (thermoplastic resin) of the coating layer to mix with the epoxy resin (before hardening) that forms the adhesive layer, and become integrated with the adhesive layer (incorporated into the adhesive layer). As a result, the coating layer that was present on the adhesive layer appears to no longer exist.
[0051] If t2 exceeds 100% of t1, the coating layer may not be sufficiently incorporated into the adhesive layer, and as a result, the coating layer may not be removed satisfactorily. In this embodiment, t2 is, for example, preferably 0.5 μm or more and 600 μm or less, more preferably 1 μm or more and 200 μm or less, and particularly preferably 3 μm or more and 100 μm or less.
[0052] It is desirable to determine the resin forming the coating layer so that the glass transition temperature of the coating layer is preferably 60° C. or higher and lower than the curing temperature. If the glass transition temperature of the coating layer is lower than 60° C., the surface of the coating layer becomes sticky (tacky), and it may be difficult to obtain the effects of the present invention. On the other hand, if the temperature exceeds the curing temperature, the coating layer does not soften sufficiently in the heat curing temperature range of the adhesive layer, so that the adhesive strength of the adhesive layer may not be fully exerted.
[0053] The adhesive sheet of this embodiment can be produced by either a wet method or a dry method. The wet method is a method in which a coating layer forming coating liquid in which the components of the coating layer are dissolved or dispersed in a solvent is applied to a substrate, and then, if necessary, dried to obtain a coating layer, and an adhesive layer forming coating liquid in which the components of the adhesive layer are dissolved or dispersed in a solvent is prepared, applied, and dried on the resulting coating layer. On the other hand, the dry method is a method of producing a film by, for example, bonding (laminating) a coating layer formed on a release film and an adhesive layer formed on a release film different from the release film used to form the coating layer.
[0054] <Application> The adhesive sheet according to the present embodiment as described above can be suitably used for, for example, reinforcing rivet joints in building construction materials, laminating decorative panels for furniture and building materials, automotive interior materials, interlayer adhesion and structural adhesion applications for carbon fiber reinforced plastics (CFRP), adhesion of coverlay films for flexible electronic circuit boards, etc. In addition, by using an insulating substrate in the adhesive layer, it can be used for adhesion of various parts of electronic devices that require insulation, such as interlayer insulating films for electronic circuit boards. Furthermore, by introducing a thermally conductive filler into the adhesive layer, it can be used to bond an electronic device to a heat sink. By introducing a thermally foamable filler into the adhesive layer, the gap-filling properties due to thermal foaming can be utilized, and the material can be widely used in the electrical and electronics industries, such as for use as an image display member fixed to an image display device (liquid crystal display, electroluminescence display, plasma display, etc.), or as a gap filler between an optical member (camera, lens, etc.) fixed to a portable electronic device (mobile phone, personal digital assistant, etc.) and a housing (window portion), as well as for use as an interposition material in the gap between adjacent coils of different phases at the coil end portion of a stator used in a motor or generator, or in the gap within the slot groove of a stator core. EXAMPLES
[0055] The following examples are provided to further illustrate the present invention, but are not intended to limit the scope of the invention. In the examples, "%" and "parts" refer to mass % and mass parts, unless otherwise specified.
[0056] [Examples 1 to 24, Comparative Examples 1 to 5] 1. Preparation of adhesive layer and coating layer forming coating liquid The components shown in Tables 1 to 4 were mixed in the solid content ratio (mass conversion), stirred and mixed with separately prepared methyl ethyl ketone, and degassed under reduced pressure to prepare an adhesive layer forming coating liquid and a coat layer forming coating liquid. The total solid content in each coating liquid was 30% by mass to 50% by mass. The raw materials used are as follows: (A) Epoxy resin (a1) Bisphenol A type liquid resin (epoxy equivalent: 184-194g / eq, liquid at room temperature) (a2) Bisphenol A type solid resin (epoxy equivalent: 600-700g / eq, softening temperature 78℃) (a3) Bisphenol A type solid resin (epoxy equivalent: 1,700-2,200g / eq, softening temperature: 128℃) (B) Film-forming assistant (b1) Phenoxy resin (product name: PHENOXY PKHB (containing bisphenol A skeleton), glass transition temperature: 84°C, weight average molecular weight: 32,000, manufactured by HUNTSMAN) (b2) Polyvinyl acetal resin (product name: S-LEC KS-23Z, glass transition temperature 110°C, manufactured by Sekisui Chemical Co., Ltd.) (b3) Polyester resin (polyester resin having a hydroxyl group, product name: Nichigo Polyester TP-235, glass transition temperature: 65°C, manufactured by Mitsubishi Chemical Corporation) (C) Epoxy resin curing agent and / or epoxy resin curing accelerator (c1) Dicyandiamide (50% particle size: 3 μm) (c2) Imidazole compounds (c2-1) 2-phenyl-4-methyl-5-hydroxymethylimidazole (c2-2) 2,4-diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine (c2-3) 2-phenyl-4,5-dihydroxymethylimidazole (c3) Acid anhydride (c3-1) 3,3',4,4'-biphenyltetracarboxylic dianhydride (c4) Phosphorus compounds (C4-1) Triphenylphosphine (c4-2) Tri-p-tolylphosphine (c5) tertiary amine (C5-1) 2,4,6-Tris(dimethylaminomethyl)phenol
[0057] 2. Preparation of Coating Layer Using a coating solution for forming a coating layer having the composition shown in Tables 1 to 4, a given coating solution for forming a coating layer was applied onto the release layer of release film 1 (thickness 38 μm, PET film with a non-silicone release layer) using a Baker-type applicator so that the coating layer thickness after drying would be the thickness shown in Tables 1 to 4. Thereafter, it was dried at 90° C. for 3 minutes to obtain laminate 1 (laminate of release film 1 and coating layer).
[0058] 3. Preparation of Adhesive Sheet Using the adhesive layer-forming coating liquid shown in Tables 1 to 4, a given adhesive layer-forming coating liquid was applied onto the release layer of release film 2 (38 μm thick, PET film with non-silicone release layer) with a Baker-type applicator so that the adhesive layer thickness after drying would be the thickness shown in Tables 1 to 4. Then, it was dried at 90° C. for 3 minutes to obtain laminate 2 (a laminate of release film 2 and adhesive layer). The adhesive layer surface and the coating layer of laminate 1 were laminated while applying heat of 80° C., and then release film 1 and release film 2 were peeled off to obtain adhesive sheets of the examples and comparative examples.
[0059] 4. Evaluation The adhesive sheets obtained in each of the Examples and Comparative Examples were measured or evaluated for the following items by the following methods. The results are shown in Tables 1 to 4.
[0060] [Coat layer thickness (t2)] For the adhesive sheets obtained in each of the Examples and Comparative Examples, the total thickness of the laminate 1 was measured using a micrometer, and the thickness of the release film 1 was subtracted from the measured value to calculate the thickness.
[0061] [Adhesive layer thickness (t1)] For the adhesive sheets obtained in each of the Examples and Comparative Examples, the total thickness of the laminate 2 was measured using a micrometer, and the thickness was calculated by subtracting the thickness of the release film 2 from the measured value.
[0062] [Coat layer tack] Of the adhesive sheets of each Example and Comparative Example, Laminate 1 (a laminate of release film 1 and coating layer) was cut to a size of 5 cm x 5 cm, and stacked with the coating layers facing each other and with the release film and coating layer facing each other, and sandwiched between glass plates with a thickness of 1 mm. A load of 100 g was placed on top of them, and each was left in a room temperature environment for 24 hours, after which the load was released and the peeling state when the glass plate was spread up and down was confirmed to evaluate the tack of the coating layer. Here, the state of the glass plate when it was spread out vertically was visually observed and evaluated according to the following criteria. ○: No peeling due to contact between the coating layers or between the release film and the coating layer △: Peeling occurs under either condition ×: Peeling occurs under all conditions
[0063] [Applicability] In the process of producing the laminate 2, the state of the adhesive layer was visually observed and evaluated according to the following criteria. 〇: Can be applied evenly without repelling △: Some repelling occurs ×: Repelling occurs on the entire surface
[0064] [Handling] In the process of laminating the coating layer of Laminate 1 onto the adhesive layer surface of Laminate 2, the condition of the adhesive layer surface was evaluated according to the following criteria. 〇: No stickiness △: Stickiness that does not interfere with handling ×: Sticky and difficult to handle
[0065] [Peelability] The releasability of Release Film 1 and Release Film 2 was evaluated according to the following criteria. ○: Each release film can be easily peeled off △: Only one side of the release film can be peeled off ×: The adhesive sheet undergoes cohesive failure when attempting to peel off the release film.
[0066] [Lasting shear adhesive strength and disappearance of coating layer] The adhesive sheet of each Example and Comparative Example was cut to 25 mm x 12.5 mm, placed on a 1.6 mm thick SPCC steel plate (steel plate A) so that the adhesive layer was in contact with it, and laminated using a hand roller (made of rubber) while applying heat of 60 ° C., and a 1.6 mm thick SPCC steel plate (steel plate B) was further placed on the coating layer and fixed with a pinch cock. This laminate was left in an oven heated to the temperature (curing temperature) shown in Tables 1 to 4 for 30 minutes, then removed, cooled at room temperature, and the pinch cock was removed to prepare a test piece. Using an Instron universal testing machine #5982, the steel plates A and B of the laminate after heating were pulled at room temperature parallel to the adhesive surface and in opposite directions (shear direction) at a speed of 5 mm / min. to measure the shear adhesive strength (Pm) (unit: MPa). Note that this evaluation was only performed on those that were evaluated as "good" for all of the above-mentioned coating properties, handling properties, and peelability.
[0067] When the coating layer disappears and the adhesive layer adheres to steel plate A and steel plate B, the shear adhesive strength is greater than when only the coating layer adheres to the steel plate. Therefore, the release film of laminate 1 is peeled off, and laminate 1 is placed between steel plate A and steel plate B in the same manner as above, and the shear adhesive strength (Pc) of the coating layer alone is measured. Then, the disappearance of the coating layer was evaluated according to the following criteria using the ratio (Pm / Pc) of the measured shear adhesive strength (Pc) of the coating layer alone to the measured shear adhesive strength (Pm) of the laminate after heating between steel plate A and steel plate B. ◎: (Pm / Pc) value exceeds 110% ○: (Pm / Pc) value was over 100% and 110% or less ×: (Pm / Pc) value was 100% or less
[0068] [Storage stability] The adhesive sheets obtained in each of the Examples and Comparative Examples were cut to a predetermined size to prepare a plurality of samples. The amount of heat generated from the obtained samples was measured by differential scanning calorimetry (DSC) and was defined as the initial amount of heat generated Q0. In addition, release film 1 and release film 2 were laminated on the coating layer surface and adhesive layer surface of another sample, respectively, to obtain laminate 3. Laminate 3 was placed in a thermostatic chamber set at 40°C, left for 14 days, then removed from the thermostatic chamber and allowed to cool, and release film 1 and release film 2 were peeled off, after which the amount of heat generated was measured by DSC and defined as the amount of heat generated after being left at 40°C for 14 days Q1. From the obtained Q0 and Q1, the ratio of the amount of heat generated after being left at 40°C for 14 days was calculated according to the following formula. Heat generation ratio after leaving it at 40℃ for 14 days (%) = (heat generation after leaving it at 40℃ (Q1) / initial heat generation (Q0)) x 100 The conditions for measuring the calorific value by DSC were as follows: Measurement temperature: 30℃~300℃, heating rate: 10℃ / min.
[0069] As shown in Table 1, the adhesive sheet of Comparative Example 1, in which dicyandiamide, an epoxy resin curing agent, and an imidazole compound, an epoxy resin curing accelerator, were added to an adhesive layer containing an epoxy resin and a phenoxy resin, a film-forming aid, was confirmed to have a low heat generation ratio of 60% after being left for 14 days at 40°C. This is believed to be because the curing reaction of the epoxy resin proceeded in an environment of 40°C due to the inclusion of dicyandiamide and the imidazole compound in the adhesive layer. In contrast, in Examples 1 and 2, which have a configuration in which dicyandiamide and an imidazole compound are contained in the coating layer rather than in the adhesive layer, that is, (i) an epoxy resin curing agent and an epoxy resin curing accelerator are added to the coating layer, and neither an epoxy resin curing agent nor an epoxy resin curing accelerator is added to the adhesive layer, the heat generation ratio after being left at 40° C. for 14 days was 100%, confirming that the curing reaction of the epoxy resin was suppressed even in an environment of 40° C. From this, it can be said that the adhesive sheet of the present invention can be adequately stored at room temperature. Furthermore, in Examples 1 and 2 in which dicyandiamide and an imidazole compound were contained in the coating layer, the tensile shear adhesive strength was also increased compared to Comparative Example 1, and it was confirmed that the adhesive performance of the present invention was also improved. Although the amounts of dicyandiamide and an imidazole compound added differ between Examples 1 and 2, it was confirmed that the characteristics were stable over a wide range. Thus, it was confirmed that the present invention can obtain excellent storage stability and adhesive performance by adding an epoxy resin curing agent and / or an epoxy resin curing accelerator to the same extent as in the conventional technology in which an epoxy resin curing agent and / or a curing accelerator is added to the adhesive layer.
[0070] [Table 1]
[0071] Example 3 shows the evaluation results of a configuration in which (ii) an epoxy resin curing agent is added to the coating layer and an epoxy resin curing accelerator is added to the adhesive layer. Here, the epoxy resin curing agent added to the coating layer is (c1) dicyandiamide, and the epoxy resin curing accelerator added to the adhesive layer is (c4) a phosphorus compound (c4-2) tri-p-tolylphosphine, but the other methods were the same as those used in Example 1. As shown in Table 1, it was confirmed that Example 3 had excellent storage stability, high tensile shear adhesive strength, and good coatability, handleability, and peelability. From these results, it was found that the effects of the present invention can be achieved even with the configuration (ii).
[0072] In the adhesive sheet of Comparative Example 2, in which the imidazole compound (c2-1) was added to the adhesive layer and neither the epoxy resin curing agent nor the epoxy resin curing accelerator was added to the coating layer, it was confirmed that the heat generation ratio after 14 days of standing at 40°C was a low value of 64%. From this, it was found that even if the imidazole compound was added alone to the adhesive layer, the curing reaction of the adhesive sheet proceeded. In contrast, in Example 4, in which the same imidazole compound (c2-1) as an epoxy resin curing agent was added to the coating layer, that is, (iv) the epoxy resin curing agent was added to the coating layer and neither the epoxy resin curing agent nor the epoxy resin curing accelerator was added to the adhesive layer, the heat generation ratio after 14 days of standing at 40°C was 100%, even though the amount of (c2-1) was significantly increased, and it was confirmed that the curing reaction of the epoxy resin was suppressed. Furthermore, in Example 4, the tensile shear adhesive strength was improved compared to Comparative Example 2, and the effect of the present invention was confirmed. The adhesive sheets of both Example 4 and Comparative Example 2 were excellent in terms of coatability, handleability and peelability.
[0073] The same tendency was observed in Comparative Example 3 and Example 5 in which the imidazole compound, which is an epoxy resin curing agent, was changed from (c2-1) to (c2-2), confirming the effect of the present invention. In addition, in Comparative Example 4, in which the film-forming aid was removed from the adhesive layer of Example 5, it was found that when the adhesive layer-forming coating liquid was applied to the release sheet, repellency occurred over the entire surface, and a good adhesive layer could not be obtained. In addition, in Example 6 in which (c2-3) 2-phenyl-4,5-dihydroxymethylimidazole was used as the imidazole compound, the heat generation ratio after standing at 40°C for 14 days was 100%, and the coating properties, handling properties and peeling properties were all good, and the effects of the present invention were confirmed.
[0074] In Example 7, like Examples 4 to 6, an epoxy resin curing agent is added to the coating layer (iv), and neither an epoxy resin curing agent nor an epoxy resin curing accelerator is added to the adhesive layer. In Examples 4 to 6, an imidazole compound (c2) was added as an epoxy resin curing agent added to the coating layer, but in Example 7, 2,4,6-tris(dimethylaminomethyl)phenol (c5-1), a tertiary amine (c5), was used, and the curing temperature was changed. As shown in Table 1, it was confirmed that Example 7 had excellent storage stability, high tensile shear adhesive strength, and good coatability, handleability, and peelability. From these results, it was found that the effects of the present invention can be achieved even when a tertiary amine is used as an epoxy resin curing agent in the coating layer in the configuration (iv).
[0075] All of Examples 8 to 12 have a configuration in which (iii) dicyandiamide (c1), which is an epoxy resin curing agent, is added to the adhesive layer, and (c2-2) an imidazole compound, which is an epoxy resin curing accelerator, is added to the coating layer, and were all produced under similar conditions except that the amounts and ratios of (c1) dicyandiamide and (c2-2) the imidazole compound were as shown in Table 2. It was found that all of Examples 8 to 12 had excellent storage stability, high tensile shear adhesive strength, and good coatability, handleability, and peelability.
[0076] [Table 2]
[0077] Comparative Example 5 was a configuration in which the film-forming assistant was removed from the adhesive layer of Example 9, and although good coating properties were obtained, problems arose in handleability and peelability. From this, it was confirmed that the configuration of the present invention in which the film-forming assistant is added to the adhesive layer is essential to obtain good handleability and peelability. Moreover, Example 13 was prepared in the same manner as Example 9, except that the thermoplastic resin of the coating layer was changed from (b1) phenoxy resin to (b2) polyvinyl acetal. The tensile shear adhesive strength of Example 13 was equivalent to that of Example 9, and the storage stability was improved compared to Example 7. This shows that polyvinyl acetal can also be suitably used as the thermoplastic resin of the coating layer of the adhesive sheet of the present invention.
[0078] Example 14 was produced in the same manner as Example 9, except that the thermoplastic resin of the coating layer was changed from (b1) phenoxy resin to (b3) polyester resin. The tensile shear adhesive strength and storage stability of Example 14 were improved compared to Example 9. This demonstrated that polyester resins can also be suitably used as the thermoplastic resin of the coating layer of the adhesive sheet of the present invention.
[0079] Table 3 shows the evaluation results of adhesive sheets prepared by adding an epoxy resin curing agent to the adhesive layer (iii) and an epoxy resin curing accelerator to the coating layer. In Examples 15 and 16, an epoxy resin curing agent (c1) dicyandiamide was added to the adhesive layer, and a different type of phosphorus compound (c4) was added to the coating layer as an epoxy resin curing accelerator. As shown in Table 3, it was found that the tensile shear bond strength and storage stability vary depending on the type of phosphorus compound (c4). However, it was confirmed that both Examples 15 and 16 have excellent storage stability, high tensile shear bond strength, and good coating, handling, and peeling properties. In addition, when comparing Examples 15 and 16, it was confirmed that although there was not much difference in storage stability, the tensile shear bond strength of Example 16 was clearly greater. From the above results, it was found that in the configuration (iii), the phosphorus compound (c4) can be used as an epoxy resin curing accelerator added to the coating layer.
[0080] [Table 3]
[0081] Example 17 was produced in the same manner as Example 15, etc., except that (c5-1) 2,4,6-tris(dimethylaminomethyl)phenol, a tertiary amine (c5), was used instead of (c4) phosphorus compound as the epoxy resin curing accelerator added to the coating layer, and the curing temperature was changed from 150° C. to 130° C. As shown in Table 3, it was confirmed that Example 17 also had excellent storage stability, high tensile shear adhesive strength, and good coatability, handleability, and peelability. From the above results, it was found that in the structure of (iii), (c5) tertiary amine can also be used as an epoxy resin curing accelerator added to the coating layer. In addition, the curing temperature of the adhesive sheet of Example 17 is 130°C, which is lower than that of Examples 15 and 16, so it is expected to be applied to fields requiring low-temperature curing properties.
[0082] Examples 18 to 20 in Table 3 show the evaluation results of adhesive sheets prepared by adding an epoxy resin curing agent to the adhesive layer and an epoxy resin curing accelerator to the coating layer in the same manner as Examples 8 to 17. In Examples 18 to 20, (c3) 3,3',4,4'-biphenyltetracarboxylic dianhydride, which is an acid anhydride, was used as the epoxy resin curing agent added to the adhesive layer, and the curing temperature was changed from 150°C to 190°C. In addition, Example 18 used (c2) 2,4-diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine, which is an imidazole compound, as the epoxy resin curing accelerator added to the coating layer, and Examples 19 and 20 used (c5) 2,4,6-tris(dimethylaminomethyl)phenol, which is a tertiary amine, and the amounts added were changed. It was confirmed that all of Examples 18 to 20 had excellent storage stability, high tensile shear adhesive strength, and good coating, handling, and peeling properties. From these results, it is possible to use an acid anhydride as an epoxy resin curing agent in the configuration (iii), and it is expected to be applicable to applications requiring heat resistance in particular.
[0083] Table 4 shows the evaluation results of Examples 21 to 24, in which the thicknesses of the coating layer and the adhesive layer were changed in an adhesive sheet prepared by adding (iii) an epoxy resin curing agent to the adhesive layer and an epoxy resin curing accelerator to the coating layer. Examples 21 to 24 were all produced in the same manner as Example 9, except that the thickness of the adhesive layer or the coating layer was changed. As shown in Table 4, even when the thickness of the adhesive layer or the coating layer was changed, the tensile shear adhesive strength and storage stability of Examples 21 to 24 were equivalent to those of Example 9, and it was confirmed that each thickness can be appropriately selected for use.
[0084] [Table 4]
Claims
1. an adhesive layer made of a composition for an adhesive layer containing an epoxy resin and a film-forming aid and not containing an imidazole compound; an adhesive sheet having a coating layer formed on the adhesive layer and containing a thermoplastic resin, the coating layer contains an epoxy resin curing agent and does not exhibit tack at room temperature, the epoxy resin curing agent being at least one selected from dicyandiamide, an imidazole compound, and a tertiary amine; the heat generation ratio of the adhesive sheet after being left at 40° C. for 14 days is 80% or more; An adhesive sheet in which, by heating the adhesive sheet to a temperature equal to or higher than the curing initiation temperature of the adhesive layer, at least a portion of the coating layer disappears in a range from the interface between the adhesive layer and the coating layer to the surface of the coating layer.
2. 2. The adhesive sheet according to claim 1, wherein the film-forming auxiliary and the thermoplastic resin are each at least one selected from the group consisting of a phenoxy resin, a polyvinyl acetal resin, a polyester resin, and an acrylic resin.
3. 2. The adhesive sheet according to claim 1, wherein the coating layer further comprises an epoxy resin curing accelerator, and the epoxy resin curing accelerator is at least one selected from the group consisting of imidazole compounds, tertiary amines, and phosphorus-based compounds (excluding those of the same type as the epoxy resin curing agent).
4. An adhesive sheet as described in claim 1, wherein the adhesive layer contains an epoxy resin curing accelerator, and the epoxy resin curing accelerator is a phosphorus-based compound.
5. An adhesive layer comprising a composition for an adhesive layer containing an epoxy resin and a film-forming aid and not containing an imidazole compound; an adhesive sheet having a coating layer formed on the adhesive layer and containing a thermoplastic resin, the adhesive layer contains an epoxy resin curing agent, and the epoxy resin curing agent is at least one selected from dicyandiamide, a tertiary amine, and an acid anhydride; the coating layer contains an epoxy resin curing accelerator and does not exhibit tack at room temperature, the epoxy resin curing accelerator being at least one selected from an imidazole compound, a tertiary amine, and a phosphorus-based compound (excluding those of the same type as the epoxy resin curing agent); the heat generation ratio of the adhesive sheet after being left at 40° C. for 14 days is 80% or more; An adhesive sheet in which, by heating the adhesive sheet to a temperature equal to or higher than the curing initiation temperature of the adhesive layer, at least a portion of the coating layer disappears in a range from the interface between the adhesive layer and the coating layer to the surface of the coating layer.
Citation Information
Patent Citations
Tab tape applied with adhesive
JP1996008306A
Manufacture of multilayer printed wiring board
JP1997130053A
Manufacturing multilayered printed wiring board
JP1999186723A
Tape for tab and tab tape formed thereof
JP2000077483A
Adhesive sheet
JP2015163694A