Positive electrode active material for non-aqueous electrolyte secondary batteries

A composite oxide with a specific crystal structure and composition enhances discharge voltage and capacity in non-aqueous electrolyte secondary batteries, addressing the limitations of existing materials.

JP7946276B2Active Publication Date: 2026-11-09PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024511215
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2022-12-12
Publication Date
2026-11-09
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

Existing positive electrode active materials for non-aqueous electrolyte secondary batteries do not achieve high discharge voltages effectively.

Method used

A composite oxide with a crystal structure belonging to the space group Fm-3m, represented by the general formula Li x TM tm M y O 2-f F f, where x+tm+y satisfies 1.75≦x+tm+y≦2 and 0

Benefits of technology

The composite oxide material achieves higher discharge voltages and discharge capacities compared to conventional materials, improving the performance of non-aqueous electrolyte secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007946276000002
    Figure 0007946276000002
  • Figure 0007946276000003
    Figure 0007946276000003
  • Figure 0007946276000004
    Figure 0007946276000004
Patent Text Reader

Abstract

A positive electrode active material for nonaqueous electrolyte secondary batteries according to the present invention is characterized by being a composite oxide which is represented by general formula LixTMtmMyO2-fFf and has a crystal structure that belongs to the space group Fm-3m. In the general formula, TM represents a transition metal; M represents a non-transition metal; x, tm, y and f satisfy 1.75 ≤ x + tm + y ≤ 2 and 0 < f ≤ 0.7; and if Q = 2 × tm × (1 - (1 - f / 2)5), 0.8 ≤ Q ≤ 1.5 is satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technology of positive electrode active materials for non-aqueous electrolyte secondary batteries.

Background Art

[0002] As high-output, high-energy-density secondary batteries, for example, non-aqueous electrolyte secondary batteries that include a positive electrode, a negative electrode, and a non-aqueous electrolyte, and perform charge and discharge by moving lithium ions and the like between the positive electrode and the negative electrode are widely used.

[0003] For example, Patent Document 1 discloses a composite oxide that has a crystal structure belonging to the space group Fm-3m, contains lithium and molybdenum, and is substantially free of chromium, as a positive electrode active material used in non-aqueous electrolyte secondary batteries.

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Summary of the Invention

[0005] An object of the present disclosure is to provide a positive electrode active material for non-aqueous electrolyte secondary batteries with a high discharge voltage.

[0006] The positive electrode active material for non-aqueous electrolyte secondary batteries, which is one aspect of the present disclosure, has a crystal structure belonging to the space group Fm-3m and is a composite oxide represented by the general formula: Li x TM tm M y O 2-f F f In the above general formula, TM is a transition metal, M is a non-transition metal, x, tm, y, and f satisfy 1.75≦x+tm+y≦2 and 0<f≦0.7, and when Q=2×tm×{1-(1-f / 2) 5}, it is characterized by satisfying 0.8≦Q≦1.5.

[0007] According to one aspect of this disclosure, a positive electrode active material for a non-aqueous electrolyte secondary battery with a high discharge voltage can be provided. [Brief explanation of the drawing]

[0008] [Figure 1] This is a cross-sectional view of a non-aqueous electrolyte secondary battery, which is an example of an embodiment. [Figure 2] This figure shows the X-ray diffraction results for Example 1. [Figure 3] This figure shows the X-ray diffraction results for Example 11. [Figure 4] This figure shows the X-ray diffraction results for Comparative Example 1. [Figure 5] This figure shows the charge and discharge curves for Example 1. [Figure 6] This figure shows the charge and discharge curves for Example 11. [Figure 7] This figure shows the charge and discharge curve for Comparative Example 1. [Modes for carrying out the invention]

[0009] The following describes an example of a non-aqueous electrolyte secondary battery using the positive electrode active material for non-aqueous electrolyte secondary batteries described herein.

[0010] Figure 1 is a cross-sectional view of a non-aqueous electrolyte secondary battery, which is an example of an embodiment. The non-aqueous electrolyte secondary battery 10 shown in Figure 1 comprises a wound electrode body 14 in which a positive electrode 11 and a negative electrode 12 are wound around a separator 13, a non-aqueous electrolyte, insulating plates 18 and 19 arranged above and below the electrode body 14, respectively, and a battery case 15 that houses the above components. The battery case 15 is composed of a case body 16 and a sealing body 17 that closes the opening of the case body 16. In addition, other forms of electrode bodies may be used instead of the wound electrode body 14, such as a laminated electrode body in which the positive electrode and negative electrode are alternately stacked with a separator. Examples of battery cases 15 include metal cases such as cylindrical, rectangular, coin-shaped, and button-shaped cases, and resin cases (laminated batteries) formed by laminating resin sheets.

[0011] Non-aqueous electrolytes include, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of non-aqueous solvents include esters, ethers, nitriles, amides, and mixtures of two or more of these. The non-aqueous solvent may also contain halogen-substituted solvents in which at least some of the hydrogen atoms in the solvent are replaced with halogen atoms such as fluorine. Examples of lithium salts such as LiPF6 are used as electrolyte salts. Note that non-aqueous electrolytes are not limited to liquid electrolytes and may also be solid electrolytes using gel-like polymers.

[0012] The case body 16 is, for example, a metal container in the shape of a bottomed cylinder. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has, for example, a protruding portion 22 that supports the sealing body 17, which is a part of the side surface that protrudes inward. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the case body 16, and its upper surface supports the sealing body 17.

[0013] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked in order from the electrode body 14 side. Each component constituting the sealing body 17 has, for example, a disc shape or a ring shape, and each component except the insulating member 25 is electrically connected to one another. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, with the insulating member 25 interposed between their respective peripheral edges. When the internal pressure of the non-aqueous electrolyte secondary battery 10 rises due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 24 deforms and ruptures, pushing the upper valve body 26 towards the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. If the internal pressure rises further, the upper valve body 26 ruptures, and gas is discharged from the opening of the cap 27.

[0014] In the non-aqueous electrolyte secondary battery 10 shown in Figure 1, the positive electrode lead 20 attached to the positive electrode 11 extends through a through-hole in the insulating plate 18 towards the sealing body 17, and the negative electrode lead 21 attached to the negative electrode 12 extends outside the insulating plate 19 towards the bottom of the case body 16. The positive electrode lead 20 is connected by welding or the like to the lower surface of the filter 23, which is the bottom plate of the sealing body 17, and the cap 27, which is the top plate of the sealing body 17 and is electrically connected to the filter 23, becomes the positive electrode terminal. The negative electrode lead 21 is connected by welding or the like to the inner surface of the bottom of the case body 16, and the case body 16 becomes the negative electrode terminal.

[0015] The positive electrode 11, negative electrode 12, and separator 13 are described in detail below.

[0016] <Positive electrode> The positive electrode 11 comprises a positive electrode current collector and a positive electrode composite layer disposed on the positive electrode current collector. The positive electrode current collector can be made of a metal foil that is stable in the positive electrode potential range, such as aluminum, or a film with the metal disposed on its surface. The thickness of the positive electrode current collector is preferably in the range of 1 μm to 20 μm.

[0017] The positive electrode composite layer preferably contains a positive electrode active material and further contains a binder, conductive material, etc. The thickness of the positive electrode composite layer is preferably in the range of 10 μm to 300 μm.

[0018] The positive electrode 11 is obtained, for example, by applying and drying a positive electrode composite slurry containing a positive electrode active material, a binder, a conductive material, etc., onto a positive electrode current collector to form a positive electrode composite layer on the positive electrode current collector, and then rolling the positive electrode composite layer.

[0019] The positive electrode active material contains a composite oxide having a crystalline structure belonging to the space group Fm-3m.

[0020] The crystal structure belonging to space group Fm-3m means that the diffraction pattern obtained by X-ray diffraction (XRD) measurement has peaks that can be assigned to space group Fm-3m. Note that "-3" in the space group "Fm-3m" represents the symmetry element of a 3-fold rotoinversion axis, and should originally be expressed with a bar "-" placed above "3". The X-ray diffraction pattern of the composite oxide can be obtained by powder X-ray diffraction measurement using an X-ray diffractometer ("MiniFlexII" manufactured by Rigaku Corporation), with a radiation source of CuKα rays, a tube voltage of 40 kV, and a tube current of 15 mA. At this time, diffracted X-rays pass through a 30 μm thick Kβ filter and are detected by a high-speed one-dimensional detector (D / teX Ultra 2). In addition, the sampling width is 0.02°, the scan speed is 10° / min, the divergence slit width is 0.625°, the light-receiving slit width is 13 mm (OPEN), and the scattering slit width is 8 mm. Then, the crystal structure of the composite oxide can be identified by Rietveld analysis using the "RIETAN-FP" program (F. Izumi and K. Momma, Solid State Phenom., 130, 15-20 (2007)) based on the obtained X-ray diffraction pattern. Note that the X-ray diffractometer is not limited to the above apparatus, and the X-ray source is not limited either. The X-ray diffraction measurement conditions are not limited to the above conditions. Furthermore, the analysis method for the obtained X-ray diffraction pattern is not limited to the above method.

[0021] The composite oxide having a crystal structure belonging to space group Fm-3m is represented by the general formula: Li x TM tm M y O 2-f F f wherein in the general formula, TM is a transition metal, M is a non-transition metal, x, tm, y, and f satisfy 1.75≦x+tm+y≦2 and 0<f≦0.7, and Q=2×tm×{1-(1-f / 2) 5}, 0.8≦Q≦1.5 is satisfied. Here, Q represents the number of oxygen atoms bonded to the transition metal that bonds with fluorine. By using such a composite oxide, the discharge voltage of the positive electrode active material can be increased. Note that the above crystal structure may have vacancies where Li atoms, TM atoms, and M atoms are not arranged. Here, "having vacancies" means that vacancies not filled with Li atoms, TM atoms, and M atoms exist in the composite oxide in the positive electrode active material taken out by disassembling the secondary battery immediately after production or in a discharged state. The molar ratio of vacancies is preferably 0.05 or more and 0.25 or less.

[0022] In the general formula, x, tm, y, and f preferably satisfy 1.0<x≦1.4, 0.4≦tm<1.0, 0≦y≦0.2, and 0.2≦f≦0.6, for example, from the viewpoint that a higher discharge voltage can be obtained.

[0023] The composite oxide preferably contains Mn as the transition metal (TM), for example, from the viewpoint that a higher discharge voltage can be obtained or the discharge capacity can be improved, and in the general formula, the molar ratio tm_Mn of Mn in tm is preferably 0.6<tm_Mn<0.8.

[0024] The composite oxide preferably contains Mn and a transition metal other than Mn, for example, from the viewpoint of obtaining a higher discharge voltage or improving the discharge capacity. Examples of transition metals other than Mn include Ni, Co, Fe, Ti, Y, Zr, Nb, Mo, Sc, W, V, Gd, Ce, and Ta, with Ce, Gd, and Nb being more preferred.

[0025] Examples of the non-transition metal (M) contained in the composite oxide include Al, Mg, Sb, Bi, Ca, Sr, Mg, K, Ga, Sn, and Zn, with Ga and Mg being more preferred.

[0026] The composite oxide preferably contains Mn, for example, in terms of obtaining a higher discharge voltage or improving discharge capacity, and further preferably contains at least one of the five elements: the transition metals (TM) Gd, Ce, Nb, and the non-transition metals (M) Mg, Ga, and more preferably contains at least three of the above five elements. Furthermore, the molar ratios of Mg, Gd, Ce, Nb, and Ga in the composite oxide are preferably greater than 0 and 0.025 or less, respectively.

[0027] The composition of the composite oxide can be confirmed by inductively coupled plasma emission spectroscopy, X-ray photoelectron spectroscopy, and Rietveld analysis of parameters obtained from powder X-ray diffraction.

[0028] The method for producing the composite oxide is not particularly limited and may be any known method in the synthesis of positive electrode active materials, but for example, it can be obtained by treating a lithium source, an additive element source, a fluorine source, etc., by a mechanochemical method. A mechanochemical method (also called a mechanochemical treatment) refers to a synthesis method that utilizes a mechanochemical reaction. A mechanochemical reaction refers to a chemical reaction such as crystallization reaction, solid solution reaction, or phase transition reaction that utilizes high energy locally generated by mechanical energy such as friction and compression during the crushing process of a solid material. Examples of equipment for performing the mechanochemical method include crushing and dispersing machines such as ball mills, bead mills, vibratory mills, turbo mills, mechanofusion machines, and disc mills. Among these, ball mills are preferred. The mechanochemical treatment may be carried out in an inert gas atmosphere such as argon gas, or in an oxygen-containing atmosphere, etc.

[0029] Lithium sources include lithium carbonate and lithium hydroxide. Additive element sources are transition metal-containing compounds and non-transition metal-containing compounds, such as transition metal-containing oxides or hydroxides, non-transition metal-containing oxides or hydroxides, and transition metal and non-transition metal-containing composite oxides or hydroxides. Fluorine sources include fluorides such as lithium fluoride, molybdenum fluoride, and magnesium fluoride. Note that lithium fluoride may be used as a lithium source, transition metal fluorides such as molybdenum fluoride may be used as transition metal-containing compounds that are additive element sources, and non-transition metal fluorides such as magnesium fluoride may be used as non-transition metal-containing compounds that are additive element sources.

[0030] The composite oxide obtained by mechanochemical treatment may be heat-treated. The heating temperature is not particularly limited, but is, for example, in the range of 500°C to 1000°C. The heating time is also not particularly limited, but is, for example, 1 hour to 20 hours. Heating may be carried out in an inert gas atmosphere such as argon gas, or in an oxygen-containing atmosphere.

[0031] The positive electrode active material may consist solely of the above-mentioned composite oxide, but may also contain other active materials besides the above-mentioned composite oxide. Other active materials include, for example, Li x MO y (M represents at least one transition metal) A composite oxide (Li having a layered α-NaFeO2 type crystal structure) represented by this composite oxide (Li having a layered α-NaFeO2 type crystal structure) x CoO2, Li x KiO2, Li x MnO2, Li x Ni α Co (1-α) O2, Li x Ni α Mn β Co (1-α-β) Li such as O2, which has a spinel-type crystal structure x Mn2O4, Li x Ni α Mn (2-α) O4, etc., Li w M' x (XO y ) z(M' represents at least one transition metal, and X represents, for example, P, Si, B, V, etc.), and examples of the polyanion compound represented thereby include LiFePO₄, LiMnPO₄, LiNiPO₄, LiCoPO₄, Li₃V₂(PO₄)₃, Li₂MnSiO₄, Li₂CoPO₄F, and the like.

[0032] has a crystal structure belonging to space group Fm-3m, and is represented by the general formula: Li x TM tm M y O 2-f F f wherein in the general formula, TM is a transition metal, M is a non-transition metal, x, tm, y, and f satisfy 1.75≦x+tm+y≦2 and 0<f≦0.7, and when Q=2×tm×{1-(1-f / 2) 5}, the content of the composite oxide satisfying 0.8≦Q≦1.5 is preferably 50 mass% or more, more preferably 70 mass% or more, and even more preferably 90 mass% or more, relative to the total mass of the positive electrode active material.

[0033] Examples of the conductive material contained in the positive electrode mixture layer include carbon powders such as carbon black, acetylene black, Ketjen black, and graphite. These may be used alone or in combination of two or more thereof.

[0034] As the binder contained in the positive electrode mixture layer, for example, fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), PAN, polyimide-based resins, acrylic resins, polyolefin-based resins, styrene-butadiene rubber (SBR), CMC or salts thereof, polyacrylic acid (PAA) or salts thereof (PAA-Na, PAA-K, etc.), polyvinyl alcohol (PVA), and the like can be used. These may be used alone or in combination of two or more thereof.

[0035] <Negative Electrode> The negative electrode 12 comprises a negative electrode current collector, such as a metal foil, and a negative electrode composite layer formed on the negative electrode current collector. The negative electrode current collector can be a metal foil that is stable in the negative electrode potential range, such as copper, or a film with the metal arranged on its surface. The negative electrode composite layer includes, for example, a negative electrode active material and a binder.

[0036] The negative electrode active material contained in the negative electrode composite layer is not particularly limited as long as it is a material capable of intercalating and releasing lithium ions. Examples include carbon materials, elements capable of forming alloys with lithium, or compounds containing such elements. Examples of carbon materials include graphites such as natural graphite, non-graphitizable carbon, and artificial graphite, as well as coke. Examples of elements capable of forming alloys with lithium or compounds containing such elements include silicon and tin, and silicon oxide and tin oxide, which are formed by the bonding of these elements with oxygen. In addition to the above, materials such as lithium titanate, which have a higher charge-discharge potential for metallic lithium than carbon materials, can also be used. The binder contained in the negative electrode composite layer is the same as that used for the positive electrode.

[0037] <Separator> The separator 13 may be, for example, a porous sheet having ion permeability and insulating properties. Specific examples of porous sheets include microporous thin films, woven fabrics, and nonwoven fabrics. Suitable materials for the separator 13 include polyethylene, olefin resins such as polypropylene, and cellulose. The separator 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin, or a separator 13 with an aramid resin or the like coated on its surface may be used. [Examples]

[0038] The present disclosure will be further illustrated by the following examples, but the present disclosure is not limited to these examples.

[0039] <Example 1> [Fabrication of positive electrode active material] Lithium fluoride (LiF), lithium manganese oxide (LiMnO2), manganese(III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), gadolinium oxide (Gd2O3), and cerium oxide (CeO2) were used as starting materials for the composite oxide. These materials were weighed and mixed so that the molar ratio of Li:Mn:Mg:Gd:Ce:F was 1.225:0.705:0.005:0.01:0.005:0.6. The mixed powder was placed in a planetary ball mill (Fritsch Premium-Line P7, rotation speed: 600 rpm, container: zirconia 4.5 mL pot, balls: zirconia φ 3 mm balls) and processed in an Ar atmosphere at room temperature for 35 hours (35 cycles of 1 hour operation followed by a 10 minute rest). In this way, Li 1.225 Mn 0.705 Mg 0.005 Gd 0.01 Ce 0.005 O 1.4 F 0.6 A composite oxide represented by was obtained.

[0040] Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the results are shown in Figure 2. Analysis of the crystal structure confirmed that the composite oxide belongs to the space group Fm-3m. The conditions for the powder X-ray diffraction measurements were as described above (the same conditions were used for other examples and comparative examples).

[0041] [Fabrication of the positive electrode] A slurry for the positive electrode composite layer was prepared by mixing 70 parts by mass of the above composite oxide, 20 parts by mass of acetylene black, and 10 parts by mass of polyvinylidene fluoride, and using N-methyl-2-pyrrolidone (NMP) as a dispersion medium. Next, the slurry for the positive electrode composite layer was applied to a 15 μm thick aluminum foil and dried, and the resulting coating was rolled to produce a positive electrode in which positive electrode composite layers were formed on both sides of the aluminum foil.

[0042] [Preparation of non-aqueous electrolytes] A non-aqueous electrolyte was prepared by dissolving lithium hexafluoride phosphate (LiPF6) at a concentration of 1 mole / liter in a mixed solvent of fluoroethylene carbonate (FEC) and methyl propionate (FMP) in a volume ratio of 1:3.

[0043] [Preparation of test cells] Electrode leads were attached to the metallic lithium used as the positive and negative electrodes. An electrode body was then fabricated with a separator interposed between the positive and negative electrodes. This electrode body was placed in an aluminum laminate film, the non-aqueous electrolyte was injected, and the film was sealed. This was designated as the test cell (non-aqueous electrolyte secondary battery) of Example 1.

[0044] <Example 2> Li was prepared using lithium fluoride (LiF), lithium manganese oxide (LiMnO2), manganese(III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), gallium oxide (Ga2O3), and niobium oxide (Nb2O5) as starting materials for the composite oxide. The procedure was the same as in Example 1, except that the molar ratio of Li:Mn:Mg:Ga:Nb:F was weighed out to be 1.225:0.7:0.01:0.01:0.005:0.6. 1.225 Mn 0.7 Mg 0.01 Ga 0.01 Nb 0.005 O 1.4 F 0.6 A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.

[0045] And Li 1.225 Mn 0.7 Mg 0.01 Ga 0.01 Nb 0.005 O 1.4 F 0.6 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0046] <Example 3> Li was prepared using lithium fluoride (LiF), lithium manganese oxide (LiMnO2), manganese(III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), niobium oxide (Nb2O5), and cerium oxide (CeO2) as starting materials for the composite oxide. The procedure was the same as in Example 1, except that the molar ratio of Li:Mn:Mg:Nb:Ce:F was weighed out to be 1.143:0.765:0.02:0.01:0.005:0.447. 1.143 Mn 0.765 Mg 0.02 Nb 0.01 Ce 0.005 O 1.553 F 0.447 A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.

[0047] And Li 1.143 Mn 0.765 Mg 0.02 Nb 0.01 Ce 0.005 O 1.553 F 0.447 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0048] <Example 4> Li was prepared using lithium fluoride (LiF), lithium manganese oxide (LiMnO2), manganese(III) oxide (Mn2O3), lithium peroxide (Li2O2), gadolinium oxide (Gd2O3), niobium oxide (Nb2O5), and cerium oxide (CeO2) as the starting materials for the composite oxide, and weighed out so that the molar ratio of Li:Mn:Gd:Nb:Ce:F was 1.168:0.755:0.005:0.01:0.005:0.447, except that the procedure was the same as in Example 1. 1.168 Mn 0.755 Gd 0.005 Nb 0.01 Ce 0.005 O 1.553 F 0.447A composite oxide represented by the formula was obtained. The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.

[0049] Then, using Li 1.168 Mn 0.755 Gd 0.005 Nb 0.01 Ce 0.005 O 1.553 F 0.447 A test cell was fabricated in the same manner as in Example 1 using the composite oxide represented by the formula.

[0050] <Example 5> Using lithium fluoride (LiF), lithium manganate (LiMnO₂), manganese(III) oxide (Mn₂O₃), lithium peroxide (Li₂O₂), gallium oxide (Ga₂O₃), niobium oxide (Nb₂O₅), and cerium oxide (CeO₂) as starting sources for the composite oxide, the same operation as in Example 1 was performed except that the materials were weighed so that the molar ratio of Li:Mn:Ga:Nb:Ce:F was 1.175:0.76:0.005:0.005:0.005:0.45, to obtain Li 1.175 Mn 0.76 Ga 0.005 Nb 0.005 Ce 0.005 O 1.55 F 0.45 A composite oxide represented by the formula was obtained. The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.

[0051] Then, using Li 1.175 Mn 0.76 Ga 0.005 Nb 0.005 Ce 0.005 O 1.55 F 0.45 A test cell was fabricated in the same manner as in Example 1 using the composite oxide represented by the formula.

[0052] <Example 6> LiF was used as the starting material for the composite oxide, and the same procedure as in Example 1 was followed, except that the molar ratio of Li:Mn:Ga:Nb:Ce:F was weighed out to be 1.2:0.685:0.005:0.005:0.005:0.5. 1.2 Mn 0.685 Ga 0.005 Nb 0.005 Ce 0.005 O 1.5 F 0.5 A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.

[0053] And Li 1.2 Mn 0.685 Ga 0.005 Nb 0.005 Ce 0.005 O 1.5 F 0.5 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0054] <Example 7> LiF was used as the starting material for the composite oxide, and the same procedure as in Example 1 was followed, except that the molar ratio of Li:Mn:Mg:Ga:Ce:F was weighed out to be 1.175:0.7:0.025:0.025:0.025:0.45. 1.175 Mn 0.7 Mg 0.025 Ga 0.025 Ce 0.025 O 1.55 F 0.45A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.

[0055] And Li 1.175 Mn 0.7 Mg 0.025 Ga 0.025 Ce 0.025 O 1.55 F 0.45 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0056] <Example 8> Li was prepared using lithium fluoride (LiF), lithium manganese oxide (LiMnO2), manganese(III) oxide (Mn2O3), lithium peroxide (Li2O2), gadolinium oxide (Gd2O3), niobium oxide (Nb2O5), and cerium oxide (CeO2) as starting materials for the composite oxide. The procedure was the same as in Example 1, except that the molar ratio of Li:Mn:Gd:Nb:Ce:F was weighed out to be 1.192:0.73:0.005:0.01:0.005:0.298. 1.192 Mn 0.73 Gd 0.005 Nb 0.01 Ce 0.005 O 1.702 F 0.298 A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.

[0057] And Li 1.192 Mn 0.73 Gd 0.005 Nb 0.01 Ce 0.005 O 1.702 F 0.298 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0058] <Example 9> LiF was used as the starting material for the composite oxide, and the same procedure as in Example 1 was followed, except that the molar ratio of Li:Mn:Mg:Ga:Nb:F was weighed out to be 1.2:0.735:0.005:0.005:0.005:0.3. 1.2 Mn 0.735 Mg 0.005 Ga 0.005 Nb 0.005 O 1.7 F 0.3 A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.

[0059] And Li 1.2 Mn 0.735 Mg 0.005 Ga 0.005 Nb 0.005 O 1.7 F 0.3 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0060] <Example 10> LiF was used as the starting material for the composite oxide, and the same procedure as in Example 1 was followed, except that the molar ratio of Li:Mn:Mg:Gd:Nb:F was weighed out to be 1.25:0.73:0.005:0.005:0.01:0.298. 1.25 Mn 0.73 Mg 0.005 Gd 0.005 Nb 0.01 O 1.702 F 0.298A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.

[0061] And Li 1.25 Mn 0.73 Mg 0.005 Gd 0.005 Nb 0.01 O 1.702 F 0.298 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0062] <Example 11> Li was prepared using lithium fluoride (LiF), lithium manganese oxide (LiMnO2), manganese(III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), niobium oxide (Nb2O5), and cerium oxide (CeO2) as the starting materials for the composite oxide. The procedure was the same as in Example 1, except that the molar ratio of Li:Mn:Mg:Nb:Ce:F was weighed out to be 1.15:0.785:0.005:0.005:0.005:0.2. 1.15 Mn 0.785 Mg 0.005 Nb 0.005 Ce 0.005 O 1.8 F 0.2 A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the results are shown in Figure 3. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m. The conditions for the powder X-ray diffraction measurement were as described above.

[0063] And Li 1.15 Mn 0.785 Mg 0.005 Nb 0.005 Ce 0.005 O 1.8 F 0.2 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0064] <Comparative Example 1> Li was prepared using lithium fluoride (LiF), lithium manganese oxide (LiMnO2), manganese(III) oxide (Mn2O3), lithium peroxide (Li2O2), gallium oxide (Ga2O3), niobium oxide (Nb2O5), and cerium oxide (CeO2) as starting materials for the composite oxide. The procedure was the same as in Example 1, except that the molar ratio of Li:Mn:Ga:Nb:Ce:F was weighed out to be 1.25:0.485:0.005:0.005:0.005:0.5. 1.25 Mn 0.485 Ga 0.005 Nb 0.005 Ce 0.005 O 1.5 F 0.5 A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the results are shown in Figure 4. Analysis of the crystal structure confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.

[0065] And Li 1.25 Mn 0.485 Ga 0.005 Nb 0.005 Ce 0.005 O 1.5 F 0.5 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0066] <Comparative Example 2> LiF was used as the starting material for the composite oxide, and the same procedure as in Example 1 was followed, except that the molar ratio of Li:Mn:Mg:Ce:F was weighed out to be 1.25:0.45:0.025:0.025:0.5. 1.25 Mn 0.45 Mg 0.025 Ce 0.025 O 1.5 F 0.5 A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.

[0067] And Li 1.25 Mn 0.45 Mg 0.025 Ce 0.025 O 1.5 F 0.5 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0068] <Comparative Example 3> Li was prepared using lithium fluoride (LiF), lithium manganese oxide (LiMnO2), manganese(III) oxide (Mn2O3), and lithium peroxide (Li2O2) as the starting materials for the composite oxide, and weighed out so that the molar ratio of Li:Mn:F was 1.667:0.333:1.333. The procedure was the same as in Example 1, except that Li 1.667 Mn 0.333 O 0.667 F 1.333 A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to Fm-3m.

[0069] And Li 1.667 Mn 0.333 O 0.667 F 1.333 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0070] <Comparative Example 4> LiF was used as the starting material for the composite oxide, and the same procedure as in Example 1 was followed, except that the molar ratio of Li:Mn:Ti:F was weighed out to be 1.2:0.6:0.2:0.2. 1.2 Mn 0.6 Ti 0.2 O 1.8 F 0.2 A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to Fm-3m.

[0071] And Li 1.2 Mn 0.6 Ti 0.2 O 1.8 F 0.2 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0072] <Comparative Example 5> A composite oxide represented by LiMnO2 was obtained by performing the same procedure as in Example 1, except that LiMnO2 was used as the composite oxide. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to Fm-3m.

[0073] Then, using a composite oxide represented by LiMnO2, a test cell was prepared in the same manner as in Example 1.

[0074] <Comparative Example 6> Li was prepared using lithium fluoride (LiF), lithium manganese oxide (LiMnO2), manganese(III) oxide (Mn2O3), and lithium peroxide (Li2O2) as the starting materials for the composite oxide, and weighed out so that the molar ratio of Li:Mn:F was 1.1:0.6:0.7. The procedure was the same as in Example 1. 1.1 Mn 0.6 O 1.3 F 0.7 A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to Fm-3m.

[0075] And Li 1.1 Mn 0.6 O 1.3 F 0.7 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0076] <Comparative Example 7> Li was prepared using lithium fluoride (LiF), lithium manganese oxide (LiMnO2), manganese(III) oxide (Mn2O3), and lithium peroxide (Li2O2) as the starting materials for the composite oxide, and weighed out so that the molar ratio of Li:Mn:F was 1.14:0.86:0.7. The procedure was the same as in Example 1. 1.14 Mn 0.86 O 1.3 F 0.7 A composite oxide represented by [formula] was obtained. Powder X-ray diffraction measurements were performed on the obtained composite oxide, and the crystal structure was analyzed. It was confirmed that the crystal structure of the composite oxide belongs to Fm-3m.

[0077] And Li 1.14 Mn 0.86 O 1.3 F 0.7 Using the composite oxide represented by [formula], a test cell was prepared in the same manner as in Example 1.

[0078] [Charge / Discharge Test] Each example and comparative example test cell was charged with a constant current of 0.1C at a temperature of 25°C until the battery voltage reached 4.95V, and then charged with a constant voltage until the current value reached 0.05C at 4.95V. Subsequently, a constant current discharge was performed with a constant current of 0.1C until the battery voltage reached 2.5V. The discharge voltage was then calculated by dividing the total energy during discharge by the total current. The discharge capacity (mAh / g) during the above constant current discharge was also determined.

[0079] Table 1 shows the composition of the composite oxide for each example and each comparative example, and the composition (Li x TM tm M y O 2-f F f (TM is a transition metal, M is a non-transition metal) The values ​​of x+tm+y, the value of f, and 2×tm×{1-(1-f / 2) 5 The values ​​of Q, as well as the discharge capacity and discharge voltage, were summarized.

[0080] [Table 1]

[0081] Each of Examples 1 to 11 exhibited a higher discharge voltage and provided a higher discharge capacity as compared with Comparative Examples 1 to 7. From these results, it has a crystal structure belonging to the space group Fm-3m, and is represented by the general formula: Li x TM tm M y O 2-f F f The composite oxide represented by, wherein in the general formula, TM is a transition metal, M is a non-transition metal, x, tm, y, and f satisfy 1.75≦x+tm+y≦2 and 0<f≦0.7, and Q=2×tm×{1-(1-f / 2) 5}, it can be said that a high discharge voltage can be obtained by using the composite oxide that satisfies 0.8≦Q≦1.5.

[0082] FIGS. 5 and 6 show charge-discharge curves of Example 1 and Example 11, respectively. From these figures, it is confirmed that the examples according to the present invention exhibit a high discharge voltage and provide a high discharge capacity. Also for the other Examples 2 to 10, since similar charge-discharge curves were obtained, favorable results as shown in Table 1 were obtained. On the other hand, FIG. 7 shows a charge-discharge curve of Comparative Example 1. From this figure, Comparative Example 1 has a low discharge voltage, and only a low discharge capacity is obtained. Also for the other Comparative Examples 2 to 7, similar charge-discharge curves were obtained, and results inferior to the examples as shown in Table 1 were obtained. [Description of Symbols]

[0083] 10 Non-aqueous electrolyte secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode assembly, 15 Battery case, 16 Case main body, 17 Sealing body, 18,19 Insulating plate, 20 Positive electrode lead, 21 Negative electrode lead, 22 Overhanging portion, 23 Filter, 24 Lower valve body, 25 Insulating member, 26 Upper valve body, 27 Cap, 28 Gasket.

Claims

1. It has a crystal structure belonging to the space group Fm-3m, and its general formula is Li x TM tm M y O 2-f F f The composite oxide is represented by the following general formula, where TM is a transition metal, M is a non-transition metal, and x, tm, y, and f satisfy 1.75 ≤ x + tm + y ≤ 2, 1.0 < x ≤ 1.4, 0.4 ≤ tm < 1.0, 0 ≤ y ≤ 0.2, and 0.2 ≤ f ≤ 0.6, and Q = 2 × tm × {1 - (1 - f / 2)} 5 When}, the condition 0.8 ≤ Q ≤ 1.5 is satisfied, The composite oxide contains Mn as the transition metal (TM), and in the general formula, the molar ratio of Mn in tm, tm_Mn, is 0.6 < tm_Mn < 0.

8. The composite oxide further comprises at least three elements from among the five elements Gd, Ce, and Nb, which are transition metals (TM), and Mg and Ga, which are non-transition metals (M), as a positive electrode active material for a non-aqueous electrolyte secondary battery.

2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein in the composite oxide, the molar ratio B of Mg, Gd, Ce, Nb, and Ga is 0 < B ≤ 0.025 for each of them.

Citation Information

Patent Citations

  • Cation-disordered rock-salt lithium metal oxides and oxyfluorides and methods for their preparation

    JP2020534234A

  • JP202954A

  • Positive electrode active material and battery

    WO2018163519A1