Laminate

A laminate with a composite base layer, adhesive resin, and ethylene vinyl alcohol copolymer layer addresses the issues of gas barrier and secondary processability in paper-based laminates, providing effective packaging solutions.

JP7947739B2Active Publication Date: 2026-11-11TOSOH CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022053568
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-03-29
Publication Date
2026-11-11
Estimated Expiration
2042-03-29

AI Technical Summary

Technical Problem

Existing laminates using paper-based materials for food and beverage packaging suffer from poor gas barrier properties and lack secondary processability, as oxygen can pass through sealed portions and they cannot be formed without generating a sealed portion.

Method used

A laminate structure comprising a base layer of a composite material with cellulose-based materials and thermoplastic resins, an adhesive resin layer, and an ethylene vinyl alcohol copolymer layer, optimized for gas barrier properties and secondary processability, is produced through co-extrusion lamination.

Benefits of technology

The laminate achieves excellent gas barrier properties and adhesiveness, allowing for secondary processing without heat sealing, suitable for packaging materials and containers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007947739000001
    Figure 0007947739000001
Patent Text Reader

Abstract

To provide a laminate which is excellent in gas barrier property, adhesion, and secondary workability.SOLUTION: A laminate includes at least a base material layer, and a layer (C), a layer (B) and a layer (A) that are adjacent to each other from the base material layer side, wherein the base material layer is composed of a composite base material (S) satisfying (i) to (ii), the layer (A) is composed of polyolefin (a), the layer (B) is composed of an adhesive resin (b), and the layer (C) is composed of an ethylene-vinyl alcohol copolymer (c) satisfying (iii). (i) The composite base material contains a cellulose-based material and a thermoplastic resin, (ii) the percentage content of the cellulose-based material is 25 wt.% or more and 75 wt.% or less, and (iii) the ethylene content C2 is 50 mol% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a laminate. BACKGROUND ART

[0002] As packaging materials made of thermoplastic resins for food, beverages, pharmaceuticals and the like, ethylene-vinyl alcohol copolymers (hereinafter sometimes abbreviated as EVOH), which are excellent in gas barrier properties, aroma retention properties, solvent resistance and the like for the purpose of preventing deterioration of contents, are used in various applications, and laminates obtained by co-extruding a polyethylene-based resin, an acid-modified polyolefin, and EVOH onto a paper base material such as paperboard (for example, see Patent Document 1) and the like are being produced.

[0003] However, when a laminate using such a paper base material is formed into a box by heat sealing, oxygen and the like pass through the sealed portion, so that the gas barrier property as a container is poor. On the other hand, even if vacuum forming, draw forming or the like that does not generate a sealed portion is performed, the laminate using the paper base material cannot be formed because it does not have secondary processability.

[0004] Against this background, a laminate excellent in gas barrier properties, adhesiveness, and secondary processability has been conventionally desired. PRIOR ART DOCUMENTS PATENT DOCUMENTS

[0005] PATENT DOCUMENT 1 Japanese Unexamined Patent Publication No. 1992-234645 SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a laminate exhibiting excellent gas barrier properties, adhesiveness, and secondary processability. MEANS FOR SOLVING THE PROBLEMS

[0007] As a result of diligent research to solve the aforementioned problems, the inventors of the present invention discovered that a specific laminate exhibits excellent gas barrier properties, adhesive properties, and secondary processability, and thus completed the present invention.

[0008] Each aspect of the present invention is shown below [1] to

[12] . [1] A laminate comprising at least a base layer and adjacent (C) layer / (B) layer / (A) layer from the base layer side, wherein the base layer is composed of a composite base material (S) satisfying (i) to (ii), the (A) layer is composed of a polyolefin (a), the (B) layer is composed of an adhesive resin (b), and the (C) layer is composed of an ethylene vinyl alcohol copolymer (c) satisfying (iii).

[0009] (i) Includes cellulose-based materials and thermoplastic resins (ii) Cellulose content of 25% by weight or more and 75% by weight or less (iii) Ethylene content C2 is 50 mol% or less [2] The laminate according to [1] above, wherein the content of cellulose-based material in the composite substrate (S) is 35% by weight or more and 65% by weight or less. [3] The laminate according to any one of the above [1] to [2], wherein the cellulose-based material contained in the composite substrate (S) is pulverized pulp fibers and / or paper. [4] The laminate according to [3] above, wherein the composite substrate (S) is a sheet made of a melt-kneaded product of crushed paper and a thermoplastic resin containing polyolefin and / or polyester. [5] The laminate according to [3] above, wherein the composite substrate (S) is a mixed paper made of pulp fibers and polyolefin fibers and / or polyester fibers. [6] The laminate according to any one of the above [1] to [5], wherein the polyolefin (a) satisfies (iv) to (vi).

[0010] (iv) Melt mass flow rate (MFR) measured according to JIS K6922-1 (1997) PO ) 1.0g / 10 mins or more, 10.0g / 10 mins or less (v) Melt tension (MS) measured at a temperature of 190°C and a take-up speed of 10 m / min PO ) is 3 mN or more and 50 mN or less (vi) MFR PO (g / 10 min) and MS PO (mN) product MFR PO ×MS PO is 70 or more and 250 or less [7] The laminate according to any one of the above [1] to [6], wherein the polyolefin (a) comprises an ethylene·α-olefin copolymer and / or a high-pressure low-density polyethylene. [8] The laminate according to any one of the above [1] to [7], wherein the adhesive resin (b) comprises maleic anhydride-modified polyolefin. [9] C2 (mol%) of the ethylene·vinyl alcohol copolymer (c) and the density D at 20°C measured according to ISO 1183-3 EVOH (kg / m 3 ) satisfies the following formula (1), the laminate according to any one of the above [1] to [8].

[0011] D EVOH <-4.265×C2+1325 (1)

[10] The laminate according to any one of the above [1] to [9], further comprising an (E) layer / (D) layer between the base material layer and the (C) layer, wherein the (E) layer is adjacent to the base material layer, the (D) layer is adjacent to the (C) layer, the (E) layer is composed of polyethylene (e), and the (D) layer is composed of an adhesive resin (d).

[11] The method for producing a laminate according to any one of the above [1] to

[10] , wherein the (C) layer / (B) layer / (A) layer or the (E) layer / (D) layer / (C) layer / (B) layer / (A) layer are simultaneously formed by coextrusion lamination molding.

[12] A method for producing a container, comprising molding the laminate according to any one of the above [1] to

[10] by secondary processing. [Effects of the Invention]

[0012] According to the present invention, a laminate excellent in gas barrier properties, adhesiveness, and secondary processability can be provided. [Modes for Carrying Out the Invention]

[0013] A laminate according to one aspect of the present invention will be described in detail below.

[0014] The present invention relates to a laminate comprising at least a base layer and adjacent (C) layer / (B) layer / (A) layer from the base layer side, wherein the base layer is composed of a composite base material (S) satisfying (i) to (ii), the (A) layer is composed of a polyolefin (a), the (B) layer is composed of an adhesive resin (b), and the (C) layer is composed of an ethylene vinyl alcohol copolymer (c) satisfying (iii).

[0015] (i) Includes cellulose-based materials and thermoplastic resins (ii) Cellulose content of 25% by weight or more and 75% by weight or less (iii) Ethylene content C2 is 50 mol% or less Layer (A) is composed of polyolefin (a).

[0016] Polyolefin (a) is not particularly limited and includes homopolymers or copolymers thereof of α-olefins having 2 to 12 carbon atoms, such as ethylene, propylene, and 1-butene, as well as copolymers of ethylene with vinyl esters and / or acrylic acid esters. More specifically, examples include ethylene homopolymers such as high-pressure low-density polyethylene and high-density polyethylene, ethylene-α-olefin copolymers such as ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-octene copolymer, and ethylene-4-methyl-1-pentene copolymer, ethylene-based polymers such as ethylene-vinyl acetate copolymer, ethylene-acrylic acid ester copolymer, and ethylene-methacrylic acid ester copolymer, propylene homopolymer, propylene-ethylene copolymer, propylene-1-butene copolymer, poly-1-butene, poly-1-hexene, and poly-4-methyl-1-pentene. Polyolefin (a) may be used alone or in compositions of two or more types. Among these, ethylene homopolymers, ethylene-α-olefin copolymers, and ethylene-based copolymers are preferred due to their excellent ease of opening, and high-pressure low-density polyethylene and ethylene-α-olefin copolymers are even more preferred. Furthermore, from the viewpoint of moldability, it is preferable that the ethylene-α-olefin copolymer contains high-pressure low-density polyethylene.

[0017] A high-pressure method for producing low-density polyethylene can be exemplified by high-pressure radical polymerization. Such resins can be conveniently selected from commercially available products, for example, one sold by Tosoh Corporation under the trade name Petrocene.

[0018] Ethylene-α-olefin copolymers can be obtained by copolymerizing ethylene and α-olefins using high, medium, or low-pressure ionic polymerization methods employing Ziegler-Natta catalysts, Philips catalysts, or metallocene catalysts.

[0019] Examples of α-olefins constituting the ethylene-α-olefin copolymer include propylene, 1-butene, 4-methyl-1-pentene, 3-methyl-1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, and 1-dodecene, and one or more of these can be used. Among these α-olefins, α-olefins with 5 or fewer carbon atoms are preferred due to their excellent ease of opening.

[0020] Such ethylene-α-olefin copolymers can be conveniently selected from commercially available products. For example, they are commercially available from Tosoh Corporation under the product names Nipolon-L, Nipolon-Z, and Lumitac.

[0021] Melt mass flow rate (hereinafter referred to as "MFR") measured according to JIS K6922-1 (1997) for polyolefin (a) PO Since it exhibits excellent co-extrusion lamination (migration) properties with adhesive resins and ethylene-vinyl alcohol copolymers, a range of 1.0 g / 10 min to 10.0 g / 10 min is preferred, more preferably 1.0 g / 10 min to 6.0 g / 10 min, and most preferably 3.0 g / 10 min to 5.0 g / 10 min.

[0022] Furthermore, the melt tension (hereinafter referred to as "MS") of polyolefin (a) was measured at a temperature of 190°C and a take-up speed of 10 m / min. PO The (abbreviated as ") is preferable in the range of 3mN to 50mN, more preferably 10mN to 45mN, and most preferably 15mN to 40mN, as it offers excellent productivity.

[0023] MS in the present invention PO The values ​​were measured under the following conditions: a capillary viscometer with a barrel diameter of 9.55 mm, a die with a length of 8 mm, a diameter of 2.095 mm, and an inlet angle of 90°, and a heat-insulating chamber, with an extrusion speed of 10 m / min, a take-up speed of 10 m / min, and a set temperature of 190°C.

[0024] Polyolefin (a) MFR PO (g / 10 min) and MS PO (mN) product MFR PO ×MS PO Because of its excellent productivity, the range is preferably 70 to 250, more preferably 70 to 200, and most preferably 90 to 160. PO ×MS PO A value below 70 is undesirable due to poor lamination properties, and a value above 250 is undesirable due to poor stretchability. Such MFR PO ×MS PO This value correlates with the ratio of the melt elasticity to the melt viscosity of polyethylene, i.e., with the nonlinearity of polyethylene during melt deformation.

[0025] The density of polyolefin (a), as measured according to JIS K6922-1 (1997) (hereinafter simply referred to as density), is not particularly limited, but is 910-930 kg / m³ due to its excellent moldability. 3 A range of 914 to 925 kg / m² is preferred, and more preferably 914 to 925 kg / m². 3 It is within the range.

[0026] Other thermoplastic resins may be added to polyolefin (a) insofar as the objective is achieved.

[0027] When mixing polyolefin (a) with thermoplastic resin, a pellet mixture may be obtained by mixing polyolefin pellets and thermoplastic resin pellets in a solid state. However, a mixture obtained by melt-kneading using a single-screw extruder, twin-screw extruder, kneader, Banbury, etc., is preferable because it yields a product with more stable quality. When using a melt-kneading apparatus, the melting temperature is preferably around the melting point of the polyolefin to 300°C.

[0028] Furthermore, polyolefin (a) may be supplemented with additives commonly used in polyolefin resins, such as antioxidants, light stabilizers, antistatic agents, lubricants, and antiblocking agents, as needed, to the extent that it does not impair the objectives of the present invention.

[0029] In the laminate of the present invention, layer (B) is composed of an adhesive resin (b).

[0030] The adhesive resin (b) is not particularly limited as long as the objective is achieved, and known adhesive resins used in molding applications can be cited as examples. Examples of such adhesive resins include unsaturated carboxylic acids such as maleic acid and maleic anhydride, or acid-modified polyolefins modified with their anhydrides or boronic acid, polyamide-grafted polyolefins, homopolymers of 2-12 carbon atoms such as ethylene, propylene, and 1-butene, or modified copolymers thereof, copolymers of ethylene with vinyl esters and / or unsaturated carboxylic acid esters such as acrylic acid esters, methacrylic acid esters, and glycidyl methacrylate, saponified ethylene-vinyl ester copolymers, copolymers of ethylene with unsaturated carboxylic acids such as acrylic acid and methacrylic acid and their ionomers. Among these, from the viewpoint of adhesion and cost, it is preferable to include at least maleic anhydride-modified polyolefin, and more preferably maleic anhydride-modified polyethylene (hereinafter abbreviated as MAH-PE).

[0031] Such maleic anhydride-modified polyolefins are not particularly limited; they may be copolymers of an olefin component and maleic anhydride, or polyolefins graft-modified with maleic anhydride. Furthermore, there are no particular limitations on the method for producing such resins.

[0032] The olefin components constituting maleic anhydride-modified polyolefins are not particularly limited, and examples include vinyl esters such as ethylene, propylene, 1-butene, 1-hexene, 1-octene, vinyl acetate, and vinyl benzoate; acrylic acid esters such as acrylic acid, methacrylic acid, methyl acrylate, and ethyl acrylate; methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, and glycidyl methacrylate; and unsaturated carboxylic acids such as acrylic acid and methacrylic acid. These may be used individually or in combination of two or more types.

[0033] The maleic anhydride content of such maleic anhydride-modified polyolefins is preferably 0.10 to 1.2% by weight, more preferably 0.40 to 1.0% by weight, and most preferably 0.40 to 0.80% by weight, as this provides excellent adhesion and film appearance.

[0034] Such resins can be conveniently selected from commercially available products. For example, copolymers of olefin components and maleic anhydride are commercially available from Dow Chemical Japan Ltd. under the trade name Amplify, and from SK Geo Centric Japan Co., Ltd. under the trade names Rotader, Bondine, and OREVAC T. In addition, polyolefins graft-modified with maleic anhydride are commercially available from Mitsui Chemicals, Inc. under the trade name Admer, from Mitsubishi Chemical Corporation under the trade name Modic, from Dow Chemical Japan Ltd. under the trade name Fusabond, from SK Geo Centric Japan Co., Ltd. under the trade name OREVAC G, and from Addivant Japan LLC under the trade name Polybond.

[0035] As for the adhesive resin (b), from the viewpoint of adhesion and film appearance, it is preferable that it be a polyolefin composition containing at least a polyolefin and a maleic anhydride-modified polyolefin.

[0036] From the viewpoint of adhesion and film appearance, the polyolefin composition contains 50 to 90 parts by weight of polyolefin and 10 to 50 parts by weight of maleic anhydride-modified polyolefin (total of polyolefin and maleic anhydride-modified polyolefin is 100 parts by weight), and more preferably contains 65 to 85 parts by weight of polyolefin and 15 to 35 parts by weight of maleic anhydride-modified polyolefin (total of polyolefin and maleic anhydride-modified polyolefin is 100 parts by weight).

[0037] There are no particular limitations on the polyolefins, and examples include homopolymers or copolymers thereof of α-olefins having 2 to 12 carbon atoms, such as ethylene, propylene, and 1-butene, as well as copolymers of ethylene with vinyl esters and / or acrylic acid esters.

[0038] Examples include ethylene homopolymers such as high-pressure low-density polyethylene and high-density polyethylene, ethylene-1-butene copolymers, ethylene-1-hexene copolymers, ethylene-1-octene copolymers, ethylene-4-methyl-1-pentene copolymers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid ester copolymers, ethylene-methacrylic acid ester copolymers, and other ethylene-based polymers, as well as propylene homopolymers, propylene-ethylene copolymers, propylene-1-butene copolymers, poly-1-butene, poly-1-hexene, and poly-4-methyl-1-pentene. Polyolefins may be used individually or in compositions of two or more types. Among these, at least one from the group consisting of high-pressure low-density polyethylene, ethylene-vinyl acetate copolymer, high-density polyethylene, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, and polypropylene is preferred from the viewpoint of moldability, and these compositions are most preferred because they also have excellent moldability.

[0039] A high-pressure method for producing low-density polyethylene can be exemplified by high-pressure radical polymerization. Such resins can be conveniently selected from commercially available products, for example, one sold by Tosoh Corporation under the trade name Petrocene. The methods for producing high-density polyethylene, ethylene-1-butene copolymer, and ethylene-1-hexene copolymer are not particularly limited, but examples include high, medium, and low-pressure ionic polymerization using Ziegler-Natta catalysts, Philips catalysts, and metallocene catalysts. Such resins can be conveniently selected from commercially available products. For example, these are commercially available from Tosoh Corporation under the trade names Nipolon Hard, Nipolon-L, Nipolon-Z, and Lumitac, respectively.

[0040] The method for producing ethylene-vinyl acetate copolymer is not particularly limited, but known methods include high-pressure radical polymerization, solution polymerization, and latex polymerization. Such resins can be conveniently selected from commercially available products, and ethylene-vinyl acetate copolymer is commercially available from Tosoh Corporation under the trade name UltraCen.

[0041] The method of mixing such polyolefin compositions is not particularly limited; a pellet mixture may be obtained by mixing polyolefin pellets and maleic anhydride-modified polyolefin pellets in a solid state, but a melt-kneaded mixture is preferred from the viewpoint of quality stability.

[0042] Such a melt-mixing method is not particularly limited as long as the melt-mixing apparatus can uniformly disperse each component, and can be manufactured using commonly used resin mixing equipment. Examples of melt-mixing apparatuses include single-screw extruders, multi-screw extruders, Banbury mixers, pressure kneaders, rotary rolls, and Laboplast mills. The melting temperature is preferably around the melting point of polyolefin, or about 260°C.

[0043] The melt mass flow rate (hereinafter referred to as "MFR") of adhesive resin (b) measured according to JIS K6922-1 (1997). ADD Since it exhibits excellent co-extrusion lamination (migration) properties with polyolefins and ethylene-vinyl alcohol copolymers, a range of 1.0 g / 10 min to 10.0 g / 10 min is preferred, more preferably 1.0 g / 10 min to 6.0 g / 10 min, and most preferably 3.0 g / 10 min to 5.0 g / 10 min.

[0044] Other thermoplastic resins may be blended with the adhesive resin (b) as long as the objective is achieved. When mixing a thermoplastic resin with the adhesive resin (b), a pellet mixture may be obtained by mixing pellets of ethylene-vinyl ester copolymer saponified material and pellets of thermoplastic resin in a solid state. However, a mixture obtained by melt-kneading using a single-screw extruder, twin-screw extruder, kneader, Banbury, etc., is preferred because it yields a product with more stable quality. When using a melt-kneading apparatus, the melting temperature is preferably around the melting point of the adhesive resin to 300°C.

[0045] Furthermore, the adhesive resin (b) may, if necessary, contain additives commonly used in polyolefin resins, such as antioxidants, light stabilizers, antistatic agents, lubricants, and antiblocking agents, to the extent that they do not impair the objectives of the present invention.

[0046] The ethylene content (hereinafter sometimes abbreviated as C2) of the ethylene-vinyl alcohol copolymer (c) is 50 mol% or less, preferably 20-35 mol%, in order to obtain excellent gas barrier properties. This further improves the gas barrier properties. Here, C2 (mol%) refers to the content of the ethylene component in the monomer units contained in the ethylene-vinyl alcohol copolymer (c).

[0047] There are no particular limitations on the method for producing the ethylene-vinyl alcohol copolymer (c). For example, EVOH can be produced by producing a copolymer of ethylene and a fatty acid vinyl ester according to a known method, and then hydrolyzing (saponifying) it.

[0048] The degree of saponification of such ethylene-vinyl alcohol copolymer (c) is preferably in the range of 80% by weight or more, as this provides excellent gas barrier properties.

[0049] Furthermore, in addition to ethylene units and vinyl alcohol units, EVOH may also contain other constituent units in small amounts.

[0050] Such resins can be conveniently selected from commercially available products; for example, they are sold under the product names EVAL by Kuraray Co., Ltd., and Soanol and G-Soanol by Mitsubishi Chemical Corporation.

[0051] The melt mass flow rate (MFR) of such ethylene-vinyl alcohol copolymer (c) at 190°C, measured in accordance with ISO 1133 (temperature 190°C, load 2.16 kg, hereafter referred to as "MFR") was measured. EVOH From the viewpoint of moldability and film appearance, the melt mass flow rate (abbreviated as ") is preferably in the range of 1.0 g / 10 min to 8.0 g / 10 min, more preferably in the range of 1.0 g / 10 min to 6.0 g / 10 min, and most preferably in the range of 1.0 g / 10 min to 3.0 g / 10 min. Furthermore, from the viewpoint of moldability and film appearance, the melt mass flow rate at 210°C (temperature 210°C, load 2.16 kg) of ethylene-vinyl alcohol copolymer (c), measured in accordance with ISO 1133, is preferably in the range of 2.5 to 20.0 g / 10 min, more preferably in the range of 2.5 to 15.0 g / 10 min, and most preferably in the range of 2.5 to 7.5 g / 10 min.

[0052] Density of ethylene vinyl alcohol copolymer (c) at 20°C measured in accordance with ISO 1183-3 (hereinafter referred to as "D EVOH (abbreviated as ")" is 1190 kg / m² from the viewpoint of film appearance and adhesion. 3 Preferably less than 1100-1180 kg / m³ 3 It is more preferable that the weight be 1140-1180 kg / m 3 It is most preferable that this be the case.

[0053] Furthermore, due to its excellent film appearance and adhesion, the C2 (mol%) and D of the ethylene-vinyl alcohol copolymer (c) are used. EVOH (kg / m 3 It is preferable that ) satisfies equation (1) below, and more preferably that it satisfies equation (2) below.

[0054] D EVOH <-4.265 × C2 + 1325 (1) DEVOH <-4.265 × C2 + 1315 (2) Note that the slopes in equations (1) and (2) are based on C2 and D of the standard and semi-standard grades of ethylene-vinyl alcohol copolymer manufactured by Kuraray. EVOH The calculation was performed using the following method. Specifically, C2 was 27 mol%, D EVOH 1210 kg / m 3 It is an ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name EVAL L171B), C2 is 32 mol%, D EVOH 1190 kg / m 3 This is an ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name EVAL F171B), with C2 at 35 mol%, D EVOH 1180 kg / m 3 This is an ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name EVAL C109B), with C2 at 38 mol%, D EVOH 1170 kg / m 3 It is an ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name EVAL H171B), C2 is 44 mol%, D EVOH 1140 kg / m 3 Ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name EVAL E105B), C2 is 48 mol%, D EVOH 1120 kg / m 3 C2 and D of ethylene vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name EVAL G156B) EVOH It was calculated from the correlation. In the laminate of the present invention, the base material layer is composed of a composite base material (S) containing a cellulose-based material and a thermoplastic resin.

[0055] The cellulose-based material constituting the composite substrate (S) is not particularly limited, and examples include mechanical pulp fibers, chemical pulp fibers, microfibrillated cellulose, nanocellulose materials such as cellulose nanofibers and cellulose nanocrystals, crushed paper products, films made of modified cellulose such as cellophane, and crushed products thereof. Examples of such paper products include kraft paper, fine paper, stretched paper, glassine paper, and cardboard such as cup paper and photographic paper. One or more of these cellulose-based materials can be used to constitute the composite substrate (S) of the present invention.

[0056] Furthermore, such cellulose may be modified. Examples of such modified cellulose include ester cellulose such as cellulose acetate, ether cellulose such as methyl cellulose, carboxyalkyl cellulose such as carboxymethyl cellulose, viscose, and rayon.

[0057] The thermoplastic resin constituting the composite substrate (S) is not particularly limited, and examples include polyolefins, polyvinyl alcohol, polyesters, polyamides, polyacetals such as polyoxymethylene, liquid crystal polymers such as polycondensates of ethylene terephthalate and parahydroxybenzoic acid, fluorine-based resins such as polyvinylidene fluoride, crystalline thermoplastic resins such as polylactic acid and polyglycolic acid, cycloolefin polymers made from cyclic olefins such as norbornene, ethylene cycloolefin copolymers which are copolymers of ethylene and cyclic olefins such as norbornene, polycarbonates, polyarylates which are copolymers of bisphenol A and terephthalic acid, polyphenylene ethers, modified polyphenylene ethers which are polymer alloys of polyphenylene ether and polystyrene (including high-impact polystyrene), amorphous thermoplastic resins such as polyvinyl chloride, polyphenylene sulfide, polyethersulfone, polyamide-imide, polyetherimide, and polyester carbonate, and one or more of these can be used. Among these, the thermoplastic resin is preferably a polyolefin and / or polyester because of its excellent secondary processability.

[0058] Examples of such polyolefins include homopolymers or copolymers thereof of α-olefins having 2 to 12 carbon atoms, such as ethylene, propylene, and 1-butene, as well as copolymers of ethylene with vinyl esters and / or acrylic acid esters.

[0059] Examples include ethylene homopolymers such as high-pressure low-density polyethylene and high-density polyethylene, ethylene-1-butene copolymers, ethylene-1-hexene copolymers, ethylene-1-octene copolymers, ethylene-4-methyl-1-pentene copolymers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid ester copolymers, ethylene-methacrylic acid ester copolymers, and other ethylene-based polymers, as well as propylene homopolymers, propylene-ethylene copolymers, propylene-1-butene copolymers, poly-1-butene, poly-1-hexene, and poly-4-methyl-1-pentene. Polyolefins may be used individually or in compositions of two or more types.

[0060] Examples of such polyesters include polycondensates of aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and 2,6-naphthalenedicarboxylic acid with aliphatic diols such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, and cyclohexanedimethanol, or aromatic diols such as bisphenol A. Examples include polyethylene terephthalate, a polycondensate of terephthalic acid and ethylene glycol; polybutylene terephthalate, a polycondensate of terephthalic acid and 1,4-butanediol; and polyethylene naphthalate, a polycondensate of 2,6-naphthalenedicarboxylic acid and ethylene glycol. These aromatic dicarboxylic acids, aliphatic diols, and aromatic diols may be used individually or in combination of two or more.

[0061] There are no particular limitations on the method of compounding the cellulose-based material and the thermoplastic resin in the composite substrate (S). Examples include dry blending of the cellulose-based material and thermoplastic resin pellets, melt kneading of the cellulose-based material and the thermoplastic resin, and blending of fibers made from cellulose-based material and fibers made from thermoplastic resin.

[0062] Among such composite substrates (S), a sheet made from a melt-kneaded product of a cellulose-based material and polyolefin and / or polyester, or a mixed paper made from pulp fibers and polyolefin fibers and / or polyester fibers is preferred due to its excellent secondary processability.

[0063] Such cellulose-based materials are commercially available as melt-blended products of polyolefins and / or polyesters, including a melt-blended product of pulp fibers and polypropylene from Daicel Mirise Co., Ltd. under the trade name Cellblen, a melt-blended product of crushed paper and polyolefin from Environmental Management Research Institute Co., Ltd. under the trade name MAPKA, a melt-blended product of cellulose nanofiber and polyolefin from Daio Paper Corporation under the trade name Cellulose Composite Resin Pellet, and from Seikoh PMC Co., Ltd. under the trade name STARCEL. In addition, a sheet made from a melt-blended product of crushed paper and polyolefin is commercially available from Environmental Management Research Institute Co., Ltd. under the trade name MAPKA Sheet.

[0064] Furthermore, as a blended paper made from cellulose-based materials and thermoplastic resin fibers, blended paper made from pulp fibers and polyester fibers is commercially available from Tomoegawa Paper Co., Ltd. under the product name Conversion Sheet, from Hirose Paper Co., Ltd. under the product name HOS-PF, and from Kinsei Paper Co., Ltd. under the product name Airlaid; blended paper made from pulp fibers and polyolefin fibers is commercially available from Kinsei Paper Co., Ltd. under the product name Airlaid; blended paper made from pulp fibers, polyolefin fibers, and polyester fibers is commercially available from Daio Paper Corporation under the product name Chemical Fiber Blended Paper, and from Kinsei Paper Co., Ltd. under the product name Airlaid; and blended paper made from rayon fibers and thermoplastic resin fibers is commercially available from Kinsei Paper Co., Ltd. under the product name Chemical Bond.

[0065] The content of cellulose-based material in the composite substrate (S) is in the range of 25% by weight or more and 75% by weight or less, more preferably in the range of 35% by weight or more and 65% by weight or less, and most preferably in the range of 45% by weight or more and 55% by weight or less, in order to obtain excellent secondary processability and laminate appearance. A cellulose-based material content of less than 25% by weight is undesirable because it results in poor laminate appearance, and a content exceeding 75% by weight is undesirable because it results in poor secondary processability.

[0066] Basis weight (g / m²) of composite substrate (S) 2 There are no particular limitations on the thickness (mm) and it can be selected as appropriate depending on the application.

[0067] One embodiment of the present invention is characterized by comprising at least a base layer and (C) layer / (B) layer / (A) layer from the base layer side, and may consist not only of these four components but also of other components, such as (D) layer, (E) layer, and (F) layer. Specifically, examples include base layer / (C) layer / (B) layer / (A) layer, (D) layer / base layer / (C) layer / (B) layer / (A) layer, base layer / (D) layer / (C) layer / (B) layer / (A) layer, (E) layer / base layer / (D) layer / (C) layer / (B) layer / (A) layer, base layer / (E) layer / (D) layer / (C) layer / (B) layer / (A) layer, and (F) layer / base layer / (E) layer / (D) layer / (C) layer / (B) layer / (A) layer. The symbol / between layers indicates adjacent layers.

[0068] Layers (D), (E), and (F) can be layers formed from synthetic polymers, woven fabrics, nonwoven fabrics, metal foils, papers, cellophane, etc. Examples include polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyamide resins such as nylon 6 and nylon 66, polyethylene resins such as high-density polyethylene, low-density polyethylene, linear low-density polyethylene, ethylene-ethyl acrylate copolymer, ethylene-methacrylic acid copolymer, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ionomer, polypropylene resin, polybutene, acrylic resin, polyvinyl alcohol, polymethylpentene, polyvinyl chloride, polyvinylidene chloride, polystyrene, polycarbonate, polyurethane, cellulose resin, etc. Furthermore, these polymer films and sheets may be further treated with aluminum vapor deposition, alumina vapor deposition, silicon dioxide vapor deposition, or acrylic treatment. In addition, these polymer films and sheets may be further printed using urethane-based inks, etc. Examples of metal foils include aluminum foil and copper foil, while examples of paper include kraft paper, fine paper, stretchable paper, glassine paper, and cardboard such as cup paper and photographic paper.

[0069] Among these laminates, a laminate comprising at least adjacent base layer / (E) layer / (D) layer / (C) layer / (B) layer / (A) layer is preferred because it offers superior productivity and gas barrier properties, characterized in that layer (E) is polyethylene (e) and layer (D) is acid-modified polypropylene (d). Here, the polyethylene (a) constituting layer (A) and the polyethylene (e) constituting layer (E) may be independently identical or different, but from the viewpoint of productivity, it is more preferable that they be of the same component. Similarly, the acid-modified polypropylene (b) constituting layer (B) and the acid-modified polypropylene (e) constituting layer (D) may be independently identical or different, but from the viewpoint of productivity, it is more preferable that they be of the same component. There are no particular limitations on the extrusion lamination method used to obtain the laminate, and various extrusion lamination methods can be exemplified, such as tandem lamination, in which each layer is laminated sequentially, and co-extrusion lamination, in which several layers are laminated simultaneously. Among these, from a cost perspective, it is preferable that layers (C) / (B) / (A) or (E) / (D) / (C) / (B) / (A) are formed simultaneously by co-extrusion lamination. Furthermore, the most preferable method is a 3-type 5-layer extrusion lamination method in which layers (A) and (E) have the same component, and layers (B) and (D) have the same component. In such an extrusion lamination method, the resin temperature is preferably in the range of 180 to 280°C, and the surface temperature of the cooling roll is preferably in the range of 10 to 50°C.

[0070] Furthermore, in extrusion lamination, it is preferable to use a method in which, immediately after extruding the thermoplastic resin constituting the substrate layer and the adjacent layer in a molten state to form the substrate layer, the substrate bonding surface of the said layer is exposed to oxygen-containing gas or ozone-containing gas and then bonded to the substrate, as this results in excellent adhesion to the substrate layer. When improving the adhesion between the thermoplastic resin and the substrate with ozone-containing gas, the amount of ozone gas to be treated is 1 m of film made of thermoplastic resin extruded from the die. 2 It is preferable to blow 0.5 mg or more of ozone per unit.

[0071] In the extrusion lamination method for obtaining laminates, heat treatment can be performed for 10 hours or more at a temperature such that the resin in each layer does not foam, for example, 30°C to 60°C, in order to further improve the adhesion between the thermoplastic resin layer and the substrate layer. Furthermore, known surface treatments such as corona treatment, flame treatment, or plasma treatment may be applied to the bonding surface of the substrate layer as needed. Additionally, an anchor coating agent may be applied to the substrate layer if necessary.

[0072] Laminates can be molded into containers without heat sealing by performing secondary processing. Therefore, they have superior gas barrier properties compared to containers made by heat sealing. There are no particular limitations on such secondary processing, and examples include vacuum forming, pressure forming, vacuum pressure forming, deep drawing, and press forming.

[0073] The laminate exhibits high film appearance, adhesion, and gas barrier properties against oxygen, etc., and also has excellent secondary processability. Therefore, it can be suitably used in packaging materials and containers made from thermoplastic resins for foods, beverages, pharmaceuticals, and other products where these properties are required. [Examples]

[0074] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited thereto. (1) Meltmass flow rate (MFR) MFR was measured in accordance with either JIS K6922-1 (1997) or ISO 1133. (2) Density Density was measured in accordance with either JIS K6922-1 (1997) or ISO 1183-3. (3) Melt tension (MS) In a constant temperature room set to 23°C, the temperature was set to 190°C. A capillary viscometer (Toyo Seiki Seisakusho, product name: Capillograph) with a barrel diameter of 9.55 mm, equipped with a die with a length of 8 mm, a diameter of 2.095 mm, and an inlet angle of 90°, and a heat-insulating chamber, was filled with 18 g of polyolefin. The piston descent speed was set to 10 mm / min and the take-up speed to 10 m / min. The load required for take-up (mN) was measured as the melt tension (MS). (4) Migration Migration was measured by visually inspecting the molten film extruded from the T-die, with the rotation speed of each extruder set to achieve the thicknesses described in the examples (10 / 5 / 5 / 5 / 10 μm) at a processing speed of 50 m / min. The molten film directly below the die was observed, and the width of the EVOH layer that did not wrap around to both ends of the molten film was measured. The sum of these widths at both ends of the molten film was defined as migration (mm). Smaller migration indicates better productivity. (5) Maximum processing speed / productivity The maximum processing speed was determined by increasing the rotational speed and processing speed of each extruder in conjunction with each other so that the thickness of the laminate was the thickness described in the example (10 / 5 / 5 / 5 / 10 μm), and the processing speed at which film breakage occurred was defined as the maximum processing speed (m / min). A higher maximum processing speed indicates better productivity. A maximum processing speed of less than 20 was marked with ×, 20 to less than 50 was marked with △, and 75 or higher was marked with ○, with productivity being considered good for a rating between △ and ○. (6) Appearance of the laminate The appearance of the laminate was evaluated by visually observing the substrate side of the laminate obtained in the example. Significant irregularities on the substrate were marked with ×, slight irregularities with △, and no irregularities with ○. An appearance was considered good if judged between △ and ○. (7) Vacuum forming / secondary workability A compact vacuum forming machine 450DT (manufactured by Formech) equipped with a mold (made of chemical wood, concave, with multiple degassing holes (1 mmφ)) with a bottom inner diameter of 58.0 mm, a drawing depth of 5.8 mm, and a drawing angle of 10° was used to place the laminate obtained in the example (heating surface: (A) layer surface of the laminate, suction surface: composite substrate (S) surface of the laminate). The heater output was set to a heater surface temperature of 500°C (heater 1 84%, heater 2 84%, heater 3 94%, heater 4 86%), and vacuum forming was performed with a heating time of 30 seconds and a forming time of 20 seconds. The laminate after vacuum forming was observed and its secondary processability was evaluated. If the laminate fractured or could not be formed, it was marked with ×; if it was formed but the mold contact surface was not sharp, it was marked with △; if the mold contact surface was somewhat sharp, it was marked with ○; and if the mold contact surface was sharp, it was marked with ◎. A rating from △ to ◎ indicated good secondary processability.

[0075] Example 1 The polyethylene constituting layers (A) and (E) has an MFR of 3.7 g / 10 min and a density of 923 kg / m³. 3 30 parts by weight of high-pressure low-density polyethylene (Tosoh Corporation, product name Petrocene 225), with an MFR of 4.0 g / 10 min and a density of 922 kg / m³. 3A low-density polyethylene composition (MFR) is prepared by blending 70 parts by weight of high-pressure low-density polyethylene (Tosoh Corporation, product name Petrocene 190) and melt-kneading it at a resin temperature of 160°C using a single-screw extruder (Placo Corporation, 40mm diameter). PO 3.9g / 10min, density 922kg / m 3 MS PO 33mN)(A1) is used as the adhesive resin for layers (B) and (D), with 80 parts by weight of polyethylene (A1), an MFR of 7.0g / 10min, and a density of 930kg / m³. 3 A polyolefin resin composition (MFR) is prepared by blending 20 parts by weight of maleic anhydride-modified polyethylene (manufactured by SK Geo Centric Japan Co., Ltd., product name OREVAC G OE850, M1) with an MAH content of 0.60% by weight, and melt-kneading it at a resin temperature of 160°C using a single-screw extruder (manufactured by Placo Co., Ltd., 40 mm bore). ADD 4.4g / 10min, density 926kg / m 3 (B1) contains 0.12% by weight of MAH, and MFR is used as the ethylene vinyl alcohol copolymer constituting the (C) layer. EVOH The ethylene content is 2.0 g / 10 min, the saponification level is 32 mol%, the degree of saponification is 100% by weight, and the density is 1160 kg / m³. 3 , an ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name EVAL SP482B) (C1) with an MFR of 4.1 g / 10 min at 210°C, and a composite base material (S) of a cellulose-based material and thermoplastic resin which is the base layer, made of pulp fibers, polyolefin fibers and polyester fibers, which is a blended paper (manufactured by Daio Paper Corporation, product name Synthetic Fiber Blended Paper, basis weight 25 g / m²) 2 Cellulose-based material content of 55% by weight (S1) was used.

[0076] First, (A1) was supplied to a single-screw extruder (manufactured by Sumitomo Heavy Industries Modern Co., Ltd.) with a 40 mm diameter screw set to 260°C, (B1) was supplied to a single-screw extruder (manufactured by Sumitomo Heavy Industries Modern Co., Ltd.) with a 40 mm diameter screw set to 260°C, and (C1) was supplied to a single-screw extruder (manufactured by Sumitomo Heavy Industries Modern Co., Ltd.) with a 40 mm diameter screw set to 260°C. The extruded materials were then extruded from the T-die at a temperature of 260°C, and the extrusion rotation speed was set to the speed required to produce the extruded laminate film shown below. Migration was then evaluated from the molten film. Next, on a PET film with a thickness of 25 μm (manufactured by Toyobo Co., Ltd., product name Toyobo Polyester Film E5100), extrusion lamination was started with a processing speed of 20 m / min and an air gap length of 110 mm, so that the thicknesses of (A1), (B1), (C1), (B1), and (A1) were 10 μm, 5 μm, 5 μm, 5 μm, and 10 μm, respectively. The maximum processing speed was evaluated by increasing the extrusion rotation speed and processing speed in conjunction. Then, immediately before the extrusion lamination of the three types of five layers, 31 W·min / m was applied to the bonding surface with layer (E). 2 On a composite substrate (S1) that has been corona-treated with the specified treatment strength, a 3-type 5-layer extrusion lamination is performed at a processing speed of 50 m / min and an air gap length of 110 mm, so that (A1), (B1), (C1), (B1), and (A1) have thicknesses of 10 μm, 5 μm, 5 μm, 5 μm, and 10 μm respectively. Furthermore, 78 mg / m² is applied to the surface of the (E) layer, which adheres to the composite substrate (S1) of the 3-type 5-layer film in its molten state immediately after being extruded from the T-die. 2 By applying ozone treatment at a specified treatment strength, a laminate was obtained consisting of layers in the following order: composite substrate (S1), polyethylene (A1) ((E) layer), adhesive resin (B1) ((D) layer), ethylene-vinyl alcohol copolymer (C1) ((C) layer), adhesive resin (B1) ((B) layer), and polyethylene (A1) ((A) layer). The appearance and secondary processability of the obtained laminate were evaluated. The results are shown in Table 1.

[0077] Example 2 Except for using a sheet (S2) made of a melt-kneaded mixture of paper powder (a pulverized product of paper) and polyolefin as the composite substrate (S) of a cellulose-based material and thermoplastic resin, which serves as the base layer, the migration and maximum processing speed were evaluated using the same method as in Example 1, and then a laminate was obtained. The appearance and secondary processing properties of the obtained laminate were evaluated. The results are shown in Table 1.

[0078] Example 3 (A) and (E) layers are composed of polyethylene, and MFR PO The amount is 3.7g / 10min, and the density is 923kg / m³. 3 MS PO Except for using high-pressure low-density polyethylene (Tosoh Corporation, product name Petrocene 225) (A2) with a pressure of 105 mN, migration and maximum processing speed were evaluated using the same method as in Example 1, and then a laminate was obtained. The appearance and secondary processing properties of the obtained laminate were evaluated. The results are shown in Table 1.

[0079] Example 4 (A) and (E) layers are composed of polyethylene, and MFR PO Its density is 919 kg / m³, with a g / m³ of 13 g / m³. 3 MS PO Except for using high-pressure low-density polyethylene (Tosoh Corporation, product name Petrocene 212) (A3) with a pressure of 13 mN, migration and maximum processing speed were evaluated using the same method as in Example 1, and then a laminate was obtained. The appearance and secondary processing properties of the obtained laminate were evaluated. The results are shown in Table 1.

[0080] Comparative Example 1 Instead of the composite substrate (S) consisting of a cellulose-based material and a thermoplastic resin, which forms the base layer, kraft paper (manufactured by Chuetsu Package Co., Ltd., unbleached kraft paper, basis weight 50g / m²) is used. 2Except for using a cellulose-based material with a content of 100% by weight (S5), migration and maximum processing speed were evaluated using the same method as in Example 1, and then a laminate was obtained. The appearance and secondary processability of the obtained laminate were evaluated. The results are shown in Table 1. Due to fracture of the laminate during vacuum forming, the secondary processability was poor.

[0081] Comparative Example 2 Instead of the composite substrate (S) consisting of a cellulose-based material and a thermoplastic resin, which forms the base layer, cardboard (manufactured by Nippon Paper Industries Co., Ltd., uncoated cup paper, basis weight 300g / m²) is used. 2 Except for using a cellulose-based material with a content of 100% by weight (S6), migration and maximum processing speed were evaluated using the same method as in Example 1, and then a laminate was obtained. The appearance and secondary processability of the obtained laminate were evaluated. The results are shown in Table 1. The laminate was unable to form during vacuum forming, resulting in poor secondary processability.

[0082] [Table 1] [Industrial applicability]

[0083] The laminate of the present invention can be used in laminates where adhesion, gas barrier properties, and secondary processing properties are required, and is particularly suitable for use in laminates used in packaging materials for food, beverages, pharmaceuticals, and the like.

Claims

1. A laminate comprising at least a base layer and adjacent (C) layer / (B) layer / (A) layer from the base layer side, wherein the base layer is composed of a composite base material (S) satisfying (i) to (ii), the (A) layer is a polyolefin (a), the (B) layer is an adhesive resin (b), and the (C) layer is composed of an ethylene vinyl alcohol copolymer (c) satisfying (iii), wherein the C of the ethylene vinyl alcohol copolymer (c) 2 (mol%) and density D at 20°C as measured by ISO 1183-3 EVOH (kg / m 3 A laminate for secondary molding, wherein the following equation (1) is satisfied. (i) containing cellulose-based materials and thermoplastic resins (ii) Cellulose-based material content is 25% by weight or more and 75% by weight or less (iii) Ethylene content C2 is 50 mol% or less D EVOH <-4.265×C 2 +1325 (1)

2. The laminate for secondary molding according to claim 1, wherein the content of cellulose-based material contained in the composite substrate (S) is 35% by weight or more and 65% by weight or less.

3. A laminate for secondary molding according to any one of claims 1 to 2, wherein the cellulose-based material contained in the composite substrate (S) is pulverized pulp fibers and / or paper products.

4. The laminate for secondary molding according to claim 3, wherein the composite base material (S) is a sheet made of a melt-kneaded product of crushed paper and a thermoplastic resin containing polyolefin and / or polyester.

5. The laminate for secondary molding according to claim 3, wherein the composite substrate (S) is a mixture of fibers made of a cellulose-based material and fibers made of a thermoplastic resin.

6. The laminate for secondary molding according to claim 3, wherein the composite base material (S) is a mixed paper made of pulp fibers and polyolefin fibers and / or polyester fibers.

7. A laminate for secondary molding according to any one of claims 1 to 6, wherein polyolefin (a) satisfies (iv) to (vi). (iv) Melt mass flow rate (MFR) measured according to JIS K6922-1 (1997) PO ) 1.0g / 10 min or more, 10.0g / 10 min or less (v) Melt tension (MS) measured at a temperature of 190°C and a take-up speed of 10 m / min PO ) 3 mN or more and 50 mN or less (vi) MFR PO (g / 10 min) and MS PO (mN), the product MFR PO ×MS PO is 70 or more and 250 or less

8. A laminate for secondary molding according to any one of claims 1 to 7, wherein polyolefin (a) comprises an ethylene-α-olefin copolymer and / or high-pressure low-density polyethylene.

9. The laminate for secondary molding according to any one of claims 1 to 8, wherein the adhesive resin (b) comprises a maleic anhydride-modified polyolefin.

10. Between the base layer and layer (C), there are further layers (E) and (D), with layer (E) adjacent to the base layer and layer (D) adjacent to layer (C), and layer (E) being polyethylene (e) and layer (D) being adhesive resin A laminate for secondary molding according to any one of claims 1 to 9, comprising fat (d).

11. A method for manufacturing a laminate for secondary molding according to any one of claims 1 to 10, wherein the (C) layer / (B) layer / (A) layer, or the (E) layer / (D) layer / (C) layer / (B) layer / (A) layer are simultaneously formed by co-extrusion lamination.

12. A method for manufacturing a container, comprising forming a laminate for secondary molding according to any one of claims 1 to 10 by secondary processing.

Citation Information

Patent Citations

  • Paperboard container and manufacture thereof

    JP1992234645A

  • Multi-layered plastic molded article and manufacture thereof

    JP1993147170A

  • Coextruded multilayer protective film with at least one ethylene-vinyl alcohol-copolymer (evoh) film layer, method of making and use thereof

    JP2008545558A

  • Multi-layer laminated film

    JP2019171680A

  • Molded body and manufacturing method for molded body

    WO2017094851A1