Method for manufacturing a negative electrode for a non-aqueous secondary battery, a negative electrode for a non-aqueous secondary battery, and a non-aqueous secondary battery
A manufacturing method for non-aqueous secondary battery negative electrodes with an undercoat layer and oriented particulate carbon material addresses adhesiveness and rate characteristic issues, resulting in improved impact resistance and charge carrier movement.
Patent Information
- Application Number
- JP2022057628
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-30
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-03-30
AI Technical Summary
The use of resin binders in negative electrodes for non-aqueous secondary batteries improves rate characteristics but reduces adhesiveness and impact resistance, leading to potential bonding issues with separators.
A method involving a primary sheet molding, laminate formation, slicing, firing, and attachment process is used to create a negative electrode with an undercoat layer on a current collector, utilizing particulate carbon material oriented perpendicular to the surface, with minimal resin content and a binder in the undercoat layer, to enhance impact resistance and rate characteristics.
The method produces a negative electrode with improved impact resistance and rate characteristics, ensuring strong bonding and efficient charge carrier movement, thereby enhancing the performance of non-aqueous secondary batteries.
Smart Images

Figure 0007947740000001
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method for manufacturing a negative electrode for a non-aqueous secondary battery, a negative electrode for a non-aqueous secondary battery, and a non-aqueous secondary battery. [Background technology]
[0002] Non-aqueous secondary batteries, such as lithium-ion batteries (hereinafter sometimes simply referred to as "secondary batteries"), are small, lightweight, have high energy density, and can be repeatedly charged and discharged, making them suitable for a wide range of applications. Therefore, in recent years, improvements to battery components such as electrodes (positive and negative electrodes) have been considered in order to further enhance the performance of secondary batteries.
[0003] In this context, the negative electrode used in secondary batteries such as lithium-ion batteries typically comprises a current collector and an electrode composite layer (negative electrode composite layer) formed on the current collector. This negative electrode composite layer (sometimes referred to as the "negative electrode active material layer") contains, for example, a negative electrode active material and a resin component such as a binder, which may be used as needed.
[0004] Therefore, in recent years, attempts have been made to further improve the performance of secondary batteries by improving this negative electrode composite layer. For example, in Patent Document 1, in order to improve the input / output characteristics (rate characteristics) of a secondary battery, at least 50 percent of the total amount of negative electrode active material in the negative electrode active material layer is oriented such that the direction in which the charge carrier is absorbed and released is 45° to 90° with respect to the surface of the current collector. [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] International Publication No. 2013 / 088540 [Overview of the Initiative] [Problems that the invention aims to solve]
[0006] However, when a negative electrode is fabricated using a resin binder, as described in Patent Document 1, it is expected that the binder component will inhibit the charge carrier intercalation / release reaction of the negative electrode active material, thereby degrading the battery characteristics, such as the rate characteristics of the secondary battery. Therefore, it is expected that battery characteristics can be improved by minimizing the amount of binder component in the negative electrode. On the other hand, a binder is necessary to properly form the negative electrode composite layer.
[0007] Therefore, the inventors considered removing the binder component by firing the negative electrode, which was made using a binder, at a high temperature, in the hope of obtaining a secondary battery with good rate characteristics. However, it was found that although removing the binder component by high-temperature firing can improve the rate characteristics of the secondary battery, the absence of the binder component, which acted as an adhesive, reduces the adhesiveness, which in turn reduces the strength (impact resistance) of the negative electrode, and the negative electrode may not withstand the bonding process with the separator.
[0008] Therefore, the present invention aims to provide a negative electrode and a method for manufacturing the same that have excellent impact resistance and can exhibit excellent rate characteristics in non-aqueous secondary batteries. Furthermore, the present invention aims to provide a non-aqueous secondary battery with excellent rate characteristics. [Means for solving the problem]
[0009] The inventors of the present invention have diligently conducted research with the aim of solving the above problems. The inventors have found that when manufacturing a negative electrode using a negative electrode material sheet for non-aqueous secondary batteries (hereinafter also simply referred to as "negative electrode material sheet") which is made by firing a predetermined sheet containing resin and particulate carbon material, if a predetermined undercoat layer is provided on the current collector and the negative electrode material sheet is bonded to the undercoat layer before the coating film of the undercoat layer dries (i.e., while it is still wet), a negative electrode can be obtained that has excellent impact resistance and can exhibit excellent rate characteristics in non-aqueous secondary batteries.
[0010] In other words, the present invention aims to advantageously solve the above problems, and the present invention provides a method for manufacturing a negative electrode for a non-aqueous secondary battery, comprising: a primary sheet molding step of pressurizing a composition containing a resin and particulate carbon material to form a sheet to obtain a primary sheet; a laminate formation step of stacking a plurality of primary sheets in the thickness direction, or folding or winding the primary sheets to obtain a laminate; a slicing step of slicing the laminate at an angle of 45° or less with respect to the stacking direction to obtain a secondary sheet; a firing step of firing the secondary sheet to obtain a negative electrode material sheet for a non-aqueous secondary battery; a coating film forming step of applying an undercoat layer forming slurry composition containing a carbon material and a binder onto a current collector to form a coating film; and an attachment step of attaching the negative electrode material sheet for a non-aqueous secondary battery to the coating film before the coating film dries. In this way, by providing an undercoat layer on the current collector and attaching a predetermined negative electrode material sheet to the coating film before the undercoat layer dries, it is possible to manufacture a negative electrode that has excellent impact resistance and can exhibit excellent rate characteristics in non-aqueous secondary batteries. In this invention, "the coating film dries" means that 70% or more of the solvent components contained in the coating film, which is made of the undercoat layer forming slurry composition, are removed by volume.
[0011] In the present invention, the method for manufacturing a negative electrode for a non-aqueous secondary battery preferably involves firing the secondary sheet at a temperature of 300°C to 2000°C. By firing the secondary sheet within this predetermined temperature range, it is possible to ensure sufficiently high strength in the manufactured negative electrode material sheet while further improving the rate characteristics of the non-aqueous secondary battery.
[0012] In the present invention, the method for manufacturing a negative electrode for a non-aqueous secondary battery preferably involves the particulate carbon material containing flake graphite. Thus, by including flake graphite in the particulate carbon material, the non-aqueous secondary battery can exhibit even better rate characteristics.
[0013] Furthermore, this invention aims to advantageously solve the above problems, and the negative electrode for a non-aqueous secondary battery of the present invention comprises a current collector, an undercoat layer formed on the current collector, and a negative electrode composite layer formed on the undercoat layer and adhered to the undercoat layer, wherein the undercoat layer contains a carbon material and a binder, the negative electrode composite layer contains a particulate carbon material, the particulate carbon material is oriented perpendicular to the surface of the negative electrode composite layer, the resin content in the negative electrode composite layer is 8% by mass or less, and the negative electrode composite layer exists as a self-supporting film. In this way, if a negative electrode composite layer having predetermined properties is adhered to a predetermined undercoat layer on the current collector, it can exhibit excellent impact resistance and excellent rate characteristics in a non-aqueous secondary battery. In this invention, the orientation of the particulate carbon material, the resin content in the negative electrode composite layer, and the self-supporting film properties of the negative electrode composite layer can be measured by the method described in the examples.
[0014] In the negative electrode for a non-aqueous secondary battery of the present invention, the thickness of the undercoat layer is preferably 1 μm or more and 15 μm or less. When the thickness of the undercoat layer is within the above predetermined range, it exhibits excellent impact resistance and can provide even better rate characteristics for the non-aqueous secondary battery. In this invention, the thickness of the undercoat layer can be measured by the method described in the examples.
[0015] In the negative electrode for a non-aqueous secondary battery of the present invention, it is preferable that the ratio I(110) / I(004) of the diffraction intensity of the (110) plane to the diffraction intensity of the (004) plane in the X-ray diffraction of the surface of the negative electrode composite layer is 1.1 or higher. Thus, if the ratio I(110) / I(004) of the diffraction intensity of the (110) plane to the diffraction intensity of the (004) plane in the X-ray diffraction of the surface of the negative electrode composite layer is 1.1 or higher, the non-aqueous secondary battery can exhibit even better rate characteristics. In this invention, the ratio I(110) / I(004) of the diffraction intensity of the (110) plane to the diffraction intensity of the (004) plane in the X-ray diffraction of the surface of the negative electrode composite layer can be measured by the method described in the examples.
[0016] In the negative electrode for non-aqueous secondary batteries of the present invention, the density of the negative electrode mixture layer is preferably 1.3 g / cm 3 or less. As described above, when the density of the negative electrode mixture layer is not more than the above upper limit value, the non-aqueous secondary battery can exhibit further excellent rate characteristics. Incidentally, in the present invention, the density of the negative electrode mixture layer can be measured by the method described in the Examples.
[0017] In the negative electrode for non-aqueous secondary batteries of the present invention, the thickness of the negative electrode mixture layer is preferably 80 μm or more. As described above, when the thickness of the negative electrode mixture layer is not less than the above lower limit value, the non-aqueous secondary battery can have increased capacity. Incidentally, in the present invention, the thickness of the negative electrode mixture layer can be measured by the method described in the Examples.
[0018] In the negative electrode for non-aqueous secondary batteries of the present invention, the particulate carbon material preferably includes flaky graphite. As described above, when the particulate carbon material includes flaky graphite, the non-aqueous secondary battery can exhibit further excellent rate characteristics.
[0019] Moreover, the present invention aims to advantageously solve the above-mentioned problems, and the non-aqueous secondary battery of the present invention is characterized by including any one of the negative electrodes for non-aqueous secondary batteries described above. As described above, since the non-aqueous secondary battery of the present invention is provided with the above-described negative electrode for non-aqueous secondary batteries, it can exhibit excellent rate characteristics.
Effects of the Invention
[0020] According to the present invention, it is possible to provide a negative electrode that is excellent in impact resistance and can cause a non-aqueous secondary battery to exhibit excellent rate characteristics, and a method for producing the same. Further, according to the present invention, a non-aqueous secondary battery excellent in rate characteristics can be provided.
Mode for Carrying Out the Invention
[0021] Hereinafter, embodiments of the present invention will be described in detail. The method for manufacturing the negative electrode for a non-aqueous secondary battery of the present invention (hereinafter also simply referred to as "negative electrode") can be used, for example, in the manufacture of the negative electrode of the present invention. The non-aqueous secondary battery of the present invention (hereinafter also simply referred to as "secondary battery") is equipped with the negative electrode of the present invention.
[0022] (Method for manufacturing a negative electrode for non-aqueous secondary batteries) The present invention provides a method for manufacturing a negative electrode for a non-aqueous secondary battery, comprising: (A) a primary sheet molding step of pressurizing a composition containing a resin and particulate carbon material to form a sheet to obtain a primary sheet; (B) a laminate formation step of stacking multiple primary sheets in the thickness direction, or folding or winding the primary sheets to obtain a laminate; (C) a slicing step of slicing the laminate at an angle of 45° or less with respect to the stacking direction to obtain a secondary sheet; (D) a firing step of firing the secondary sheet to obtain a negative electrode material sheet for a non-aqueous secondary battery; (E) a coating film forming step of applying a slurry composition for forming an undercoat layer containing a binder and carbon material onto a current collector to form a coating film; and (F) an attachment step of attaching a negative electrode material sheet for a non-aqueous secondary battery to the coating film before the coating film dries. The present invention also provides a method for manufacturing a negative electrode for a non-aqueous secondary battery, which may optionally include other steps other than those described in (A) to (F) above.
[0023] The method for manufacturing a negative electrode for a non-aqueous secondary battery of the present invention makes it possible to manufacture a negative electrode for a secondary battery that has excellent shock resistance and can exhibit excellent performance in a secondary battery. Furthermore, the method for manufacturing a negative electrode for a non-aqueous secondary battery of the present invention makes it possible to efficiently manufacture the negative electrode for a secondary battery of the present invention.
[0024] <(A) Primary sheet forming process> In the primary sheet molding process, a composition containing resin and particulate carbon material is compressed and molded into a sheet to obtain a primary sheet.
[0025] <<Composition>> The above composition comprises a resin and particulate carbon material. The above composition may further contain fibrous carbon material. Furthermore, the above composition may further contain components other than the resin, particulate carbon material, and fibrous carbon material (other components).
[0026] [resin] The resin is not particularly limited, and any resin can be used. For example, both liquid resins and solid resins can be used. One type of resin may be used alone, or two or more types may be used in combination. For example, both liquid resins and solid resins can be used. When using both liquid resins and solid resins, the mass ratio of the liquid resin to the solid resin can be adjusted within a range that yields the desired effects of the present invention. The higher the proportion of liquid resin in the total resin, the easier it is to increase the packing density of particulate carbon material in the primary sheet. On the other hand, the higher the proportion of solid resin in the total resin, the higher the strength of the primary sheet can be increased.
[0027] -Liquid resin- Furthermore, as for the liquid resin, there are no particular limitations as long as it is liquid at room temperature and atmospheric pressure; for example, a thermoplastic resin that is liquid at room temperature and atmospheric pressure can be used. In this invention, "room temperature" refers to 23°C, and "atmospheric pressure" refers to 1 atm (absolute pressure).
[0028] Examples of liquid resins include fluororesins, silicone resins, acrylic resins, epoxy resins, acrylonitrile-butadiene copolymers (nitrile rubber), and polybutene. These may be used individually or in combination of two or more.
[0029] -Solid resin- As for the solid resin, there are no particular limitations as long as it is not liquid at room temperature and pressure. For example, thermoplastic resins that are solid at room temperature and pressure, thermosetting resins that are solid at room temperature and pressure, etc., can be used.
[0030] Examples of thermoplastic resins that are solid at room temperature and pressure include acrylic resins such as poly(2-ethylhexyl acrylate), copolymers of acrylic acid and 2-ethylhexyl acrylate, polymethacrylic acid or its esters, polyacrylic acid or its esters; silicone resins; fluororesins; polyethylene; polypropylene; ethylene-propylene copolymers; polymethylpentene; polyvinyl chloride; polyvinylidene chloride; polyvinyl acetate; ethylene-vinyl acetate copolymers; polyvinyl alcohol; polyacetal; polyethylene terephthalate; polybutylene terephthalate; polyethylene naphthalate; polystyrene; polyacrylonitrile; styrene-A Examples include crironitrile copolymers; acrylonitrile-butadiene copolymers (nitrile rubber); acrylonitrile-butadiene-styrene copolymers (ABS resin); styrene-butadiene block copolymers or their hydrogenated versions; styrene-isoprene block copolymers or their hydrogenated versions; butyl rubber, butadiene rubber, polyphenylene ether; modified polyphenylene ether; aliphatic polyamides; aromatic polyamides; polyamide-imides; polycarbonates; polyphenylene sulfide; polysulfone; polyethersulfone; polyethernitrile; polyether ketone; polyketone; polyurethane; liquid crystal polymers; ionomers; and others. These may be used individually or in combination of two or more. In this invention, rubber is included in the term "resin".
[0031] Examples of thermosetting resins that are solid at room temperature and pressure include natural rubber, butadiene rubber, isoprene rubber, nitrile rubber, hydrogenated nitrile rubber, chloroprene rubber, ethylene propylene rubber, chlorinated polyethylene, chlorosulfonated polyethylene, butyl rubber, halogenated butyl rubber, polyisobutylene rubber, epoxy resin, polyimide resin, bismaleimide resin, benzocyclobutene resin, phenolic resin, unsaturated polyester, diallyl phthalate resin, polyimide silicone resin, polyurethane, thermosetting polyphenylene ether, thermosetting modified polyphenylene ether, and the like. These may be used individually or in combination of two or more.
[0032] [Particulate carbon material] Particulate carbon materials are particulate materials formed from carbon-carbon-containing substances that can intercept and release charge carriers such as lithium, and are used as negative electrode active materials in non-aqueous secondary batteries. Particulate carbon materials are not particularly limited and include, for example, graphite and carbon black. Graphite can be categorized into natural graphite and artificial graphite depending on its origin. Furthermore, graphite can be categorized into flaky graphite, massive graphite (scaly graphite), earthy graphite, flaked graphite, and spheroidal graphite (elliptical graphite) depending on its morphological characteristics. Graphite may or may not be treated. Treated graphite can be, for example, acid-treated graphite (e.g., expandable graphite, expanded graphite). Carbon black is an aggregate of graphite-like carbon microcrystals forming a chaotic layered structure, and specific examples include acetylene black, Ketjen black, furnace black, channel black, and thermal lamp black. Furthermore, carbon black may contain heteroatoms other than the main component, carbon (e.g., silicon, nitrogen, boron, etc.). These particulate carbon materials may be used individually or in combination of two or more types. The particulate carbon material preferably contains flake graphite, and more preferably consists of flake graphite. This is because using flake graphite allows for excellent vertical orientation in the resulting negative electrode material sheet, thereby further improving the rate characteristics of the secondary battery. Furthermore, using flake graphite improves packing and adhesion, resulting in improved bonding strength between negative electrode active materials and thus further improving the strength of the resulting negative electrode material sheet. Examples of flake graphite include "UP20α" manufactured by Nippon Graphite Industries Co., Ltd.
[0033] The volume-average particle diameter of the particulate carbon material is preferably 3 μm or more, more preferably 5 μm or more, even more preferably 8 μm or more, even more preferably 12 μm or more, even more preferably 16 μm or more, preferably 200 μm or less, more preferably 150 μm or less, even more preferably 100 μm or less, and even more preferably 50 μm or less. If the volume-average particle diameter of the particulate carbon material is above the lower limit above, the density of the negative electrode material sheet decreases appropriately, which facilitates the movement of charge carriers such as lithium, and thus further improves the rate characteristics of the resulting secondary battery. On the other hand, if the volume-average particle diameter of the particulate carbon material is below the upper limit above, the density of the negative electrode material sheet increases appropriately, which allows for a higher capacity secondary battery. In this invention, "volume-average particle diameter" can be measured in accordance with JIS Z8825 and represents the particle diameter at which the cumulative volume calculated from the smallest diameter side accounts for 50% of the particle size distribution (volume-based) measured by laser diffraction.
[0034] Furthermore, the particulate carbon material preferably has an aspect ratio (major axis / minor axis) greater than 1.2, more preferably greater than 1.5, preferably 3 or less, and more preferably 2.1 or less. If the aspect ratio of the particulate carbon material is within the above predetermined range, the orientation angle of the particulate carbon material with respect to the surface of the negative electrode material sheet can easily fall within the desired range, which facilitates the movement of charge carriers such as lithium, and thus further improves the rate characteristics of the resulting secondary battery. In this invention, the aspect ratio of particulate carbon material refers to the ratio of the major axis length to the minor axis length in the plane where the cross-sectional area of the particle is maximized (i.e., maximum major axis length / maximum minor axis length). From the viewpoint of ease of measurement and reduction of measurement error, it is preferable to determine the aspect ratio of particulate carbon material using the maximum major axis length and maximum minor axis length of flake graphite. The apparatus for measuring the particle dimensions is not particularly limited, and can be suitably measured using, for example, a scanning electron microscope (SEM).
[0035] Furthermore, the content of particulate carbon material in the composition is preferably 50 parts by mass or more, more preferably 80 parts by mass or more, even more preferably 120 parts by mass or more, even more preferably 180 parts by mass or more, even more preferably 250 parts by mass or more, preferably 500 parts by mass or less, more preferably 450 parts by mass or less, and even more preferably 400 parts by mass or less, based on 100 parts by mass of resin. If the content of particulate carbon material in the composition is above the lower limit above, the density of the manufactured negative electrode material sheet can be moderately increased to improve the strength of the negative electrode material sheet, and the secondary battery manufactured using the negative electrode equipped with the negative electrode material sheet can be made to have a higher capacity. On the other hand, if the content of particulate carbon material in the composition is below the upper limit above, the density of the manufactured negative electrode material sheet can be moderately decreased to further improve the rate characteristics of the secondary battery manufactured using the negative electrode equipped with the negative electrode material sheet, and the electrolyte injection properties of the secondary battery can be improved.
[0036] Furthermore, the volume of particulate carbon material in the composition is preferably 25% by volume or more, preferably 37% by volume or more, more preferably 45% by volume or more, even more preferably 53% by volume or more, preferably 75% by volume or less, more preferably 70% by volume or less, and even more preferably 65% by volume or less, relative to the total volume of resin and particulate carbon material. If the ratio of the volume of particulate carbon material to the total volume of resin and particulate carbon material in the composition is above the lower limit above, the density of the manufactured negative electrode material sheet can be moderately increased to improve the strength of the negative electrode material sheet, and the secondary battery manufactured using the negative electrode equipped with the negative electrode material sheet can be made to have a higher capacity. On the other hand, if the ratio of the volume of particulate carbon material to the total volume of resin and particulate carbon material in the composition is below the upper limit above, the density of the manufactured negative electrode material sheet can be moderately decreased to further improve the rate characteristics of the secondary battery manufactured using the negative electrode equipped with the negative electrode material sheet, and the electrolyte pourability of the secondary battery can be improved.
[0037] [Fibrous carbon materials] The fibrous carbon material that the composition may optionally contain is a material that can improve the strength of the resulting negative electrode material sheet. The fibrous carbon material is not particularly limited, and examples include carbon nanotubes, vapor-grown carbon fibers, carbon fibers obtained by carbonizing organic fibers, and cut pieces thereof. These may be used individually or in combination of two or more.
[0038] Among the above, it is preferable to use fibrous carbon nanostructures such as carbon nanotubes as the fibrous carbon material, and it is even more preferable to use fibrous carbon nanostructures containing carbon nanotubes. By using fibrous carbon nanostructures such as carbon nanotubes, the strength of the resulting anode material sheet can be further improved.
[0039] The content of fibrous carbon material in the composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 2 parts by mass or less, per 100 parts by mass of resin. If the content of fibrous carbon material in the composition is above the lower limit, the strength of the manufactured negative electrode material sheet can be increased. On the other hand, if the content of fibrous carbon material in the composition is below the upper limit, a sufficiently high content of particulate carbon material can be secured in the manufactured negative electrode material sheet, so that the secondary battery manufactured using the negative electrode equipped with the negative electrode material sheet can be made to have a sufficiently high capacity.
[0040] Furthermore, the content of fibrous carbon material in the composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, even more preferably 0.4 parts by mass or more, preferably 5 parts by mass or less, more preferably 2 parts by mass or less, and even more preferably 1 part by mass or less, per 100 parts by mass of particulate carbon material. If the content of fibrous carbon material in the composition is above the lower limit, the strength of the manufactured anode material sheet can be increased. On the other hand, if the content of fibrous carbon material in the composition is below the upper limit, a sufficiently high content of particulate carbon material can be secured in the manufactured anode material sheet, so that the secondary battery manufactured using the anode equipped with the anode material sheet can be made to have a sufficiently high capacity.
[0041] [Other ingredients] Other components that the composition may optionally contain include, for example, silicon active materials and dispersants. The silicon active materials and dispersants are not particularly limited, and known ones can be used. The content of silicon active materials and dispersants in the composition can be adjusted within a range that yields the desired effects of the present invention.
[0042] Furthermore, in the composition that forms the primary sheet, the ratio of the volume of particulate carbon material to the total volume of solid components (i.e., the total volume of resin, particulate carbon material, and optionally added fibrous carbon material and other components) is preferably 25% by volume or more, more preferably 37% by volume or more, even more preferably 45% by volume or more, even more preferably 53% by volume or more, preferably 75% by volume or less, more preferably 70% by volume or less, and even more preferably 65% by volume or less. If the ratio of the volume of particulate carbon material to the total volume of solid components of resin and particulate carbon material in the composition is above the above lower limit, the density of the manufactured negative electrode material sheet can be appropriately increased, improving the strength of the negative electrode material sheet, and the capacity of the secondary battery manufactured using the negative electrode equipped with the negative electrode material sheet can be increased. On the other hand, if the ratio of the volume of particulate carbon material to the total volume of the resin and particulate carbon material components in the composition is less than or equal to the above upper limit, the density of the manufactured negative electrode material sheet can be appropriately reduced, further improving the rate characteristics of a secondary battery manufactured using a negative electrode equipped with the negative electrode material sheet, and also improving the electrolyte injection properties of the secondary battery.
[0043] [Preparation of composition] The composition is not particularly limited and can be prepared by mixing the above-mentioned components. The mixing of the above-mentioned components can be carried out using known mixing equipment such as a kneader, mixer (e.g., Henschel mixer, Hobart mixer, high-speed mixer), twin-shaft kneader, or rolls, without any particular limitations. The mixing may also be carried out in the presence of a solvent such as ethyl acetate. The resin may be dissolved or dispersed in the solvent beforehand to form a resin solution, which can then be mixed with the particulate carbon material, and optionally added fibrous carbon material and other components. When using fibrous carbon nanostructures containing CNTs as the fibrous carbon material, a dispersion may be prepared by dispersing the fibrous carbon nanostructures containing CNTs and a dispersant in a solvent such as methyl ethyl ketone. A small amount of resin may then be added to the dispersion, and the solvent may be removed by distillation to obtain a masterbatch, which can then be mixed with the resin and particulate carbon material. The mixing time can be, for example, 5 minutes to 60 minutes. The mixing temperature can be, for example, 5°C to 150°C.
[0044] <<Formation of the composition>> The composition prepared as described above can be optionally degassed and crushed, and then pressed to form a sheet. This pressed-formed sheet can be used as the primary sheet. If a solvent is used during mixing, it is preferable to remove the solvent before forming the sheet. For example, if degassing is performed using vacuum degassing, the solvent can be removed simultaneously with the degassing.
[0045] Here, the composition can be formed into a sheet using known molding methods such as press molding, rolling molding, or extrusion molding, as long as the molding method involves applying pressure. In particular, it is preferable to form the composition into a sheet by rolling molding (primary pressure), and more preferably by passing it between rolls while sandwiched between protective films. The protective film is not particularly limited, and can be a sandblasted polyethylene terephthalate (PET) film or the like. The roll temperature can be 5°C to 150°C, the roll gap can be 50 μm to 2500 μm, the roll linear pressure can be 1 kg / cm to 3000 kg / cm, and the roll speed can be 0.1 m / min to 20 m / min.
[0046] <(B) Laminate formation process> In the laminate formation process, multiple primary sheets obtained in the primary sheet molding process are stacked in the thickness direction, or the primary sheets are folded or wound to obtain a laminate in which multiple primary sheets containing resin and particulate carbon material are formed in the thickness direction. Here, the formation of a laminate by folding primary sheets is not particularly limited and can be done by folding the primary sheets to a certain width using a folding machine. The formation of a laminate by winding primary sheets is not particularly limited and can be done by winding the primary sheets around an axis parallel to the short or long direction of the primary sheets. Furthermore, the formation of a laminate by stacking primary sheets is not particularly limited and can be done using a stacking device. For example, by using a sheet stacking device (manufactured by Nikkiso Co., Ltd., product name "High Stacker"), it is possible to suppress the intrusion of air between layers, thereby efficiently obtaining a good laminate.
[0047] Furthermore, in the lamination process, it is preferable to heat the resulting laminate while applying pressure in the lamination direction (secondary pressurization). By performing secondary pressurization, which involves heating the laminate while applying pressure in the lamination direction, the fusion between the laminated primary sheets can be promoted.
[0048] Here, the pressure applied to the laminate in the stacking direction can be between 0.05 MPa and 0.50 MPa. Furthermore, the heating temperature of the laminate is not particularly limited, but it is preferably between 50°C and 170°C. Furthermore, the heating time for the laminate can be, for example, between 10 seconds and 30 minutes.
[0049] Furthermore, in laminates obtained by stacking, folding, or winding primary sheets, it is presumed that the particulate carbon material is oriented in a direction approximately perpendicular to the stacking direction. For example, if the particulate carbon material is in the form of flakes, it is presumed that the direction of the major axis of the main surface of the flakes is approximately perpendicular to the stacking direction.
[0050] <(C) Slicing process> In the slicing process, the laminate is sliced at an angle of 45° or less with respect to the lamination direction to obtain a secondary sheet consisting of sliced pieces of the laminate. The method for slicing the laminate is not particularly limited, and examples include the multi-blade method, laser processing method, water jet method, and knife processing method. Among these, the knife processing method is preferred because it makes it easier to ensure uniform thickness of the secondary sheet. Furthermore, the cutting tool used for slicing the laminate is not particularly limited, and a slicing member having a smooth surface with slits and a blade protruding from these slits (for example, a plane or slicer with a sharp blade) can be used.
[0051] The slicing angle of the laminate is preferably 30° or less with respect to the lamination direction, more preferably 15° or less with respect to the lamination direction, and preferably approximately 0° with respect to the lamination direction (i.e., in the direction along the lamination direction). In the secondary sheet obtained in this way, the particulate carbon material is well oriented in the thickness direction. For example, if the particulate carbon material is in the shape of flakes, the direction of the major axis of the main surface of the flake shape is approximately the same as the thickness direction of the secondary sheet.
[0052] <(D) Firing process> In the firing process, the secondary sheet is fired to burn and remove the resin contained in the secondary sheet, thereby obtaining the negative electrode material sheet.
[0053] The heating temperature when firing the secondary sheet is preferably 300°C or higher, more preferably 500°C or higher, even more preferably 700°C or higher, preferably 2000°C or lower, more preferably 1500°C or lower, and even more preferably 1200°C or lower. If the heating temperature when firing the secondary sheet is above the lower limit, the resin content in the manufactured negative electrode material sheet can be reduced, further improving the rate characteristics of the secondary battery manufactured using the negative electrode equipped with the negative electrode material sheet. On the other hand, if the heating temperature when firing the secondary sheet is below the upper limit, damage to the structure of the manufactured negative electrode material sheet due to excessive heating can be suppressed, and the strength of the negative electrode material sheet can be ensured to be sufficiently high.
[0054] The heating time for firing the secondary sheet can be adjusted according to the heating temperature, but for example, it can be between 30 minutes and 72 hours.
[0055] <<Negative electrode material sheet>> The negative electrode material sheet obtained as described above contains particulate carbon material and may optionally further contain resin, fibrous carbon material, and / or other components. Other components include the silicon active material described in the section <(A) Primary Sheet Molding Process> above.
[0056] [Particulate carbon material] The particulate carbon material is oriented perpendicular to the surface of the negative electrode material sheet. Here, "perpendicular orientation" means that the long axis of the particulate carbon material is oriented at an angle greater than or equal to a predetermined value relative to the surface of the negative electrode material sheet. If the particulate carbon material is oriented perpendicular to the surface of the negative electrode material sheet, the movement of charge carriers such as lithium is facilitated, and the rate characteristics of the resulting secondary battery can be further improved. The orientation of such particulate carbon material can be evaluated, for example, using the measured orientation angle of the particulate carbon material as an indicator. The orientation of the particulate carbon material can be adjusted by, for example, the manufacturing process of the negative electrode material sheet described above, the properties of the particulate carbon material used (e.g., aspect ratio), molding conditions including the film thickness of the primary sheet described later, the cutting angle of the laminate, and firing conditions (e.g., temperature and time).
[0057] When using the orientation angle of particulate carbon material as an indicator, the orientation of the particulate carbon material perpendicular to the surface of the negative electrode material sheet is preferably 60° or more, more preferably 65° or more, even more preferably 70° or more, and preferably 90° or less with respect to the surface of the negative electrode material sheet. If the orientation angle of the particulate carbon material is within the above predetermined range with respect to the surface of the negative electrode material sheet, the movement of charge carriers such as lithium becomes easier, and the rate characteristics of the resulting secondary battery can be further improved. In this invention, the orientation angle of the particulate carbon material with respect to the surface of the negative electrode material sheet can be measured by the method described in the examples of this specification.
[0058] The content of particulate carbon material in the negative electrode material sheet is preferably 92% by mass or more, more preferably 95% by mass or more, even more preferably 97% by mass or more, and can be 100% by mass or less. If the content of particulate carbon material in the negative electrode material sheet is above the lower limit mentioned above, the rate characteristics of the resulting secondary battery can be further improved, and the capacity of the secondary battery can be increased.
[0059] [resin] The resin optionally included in the negative electrode material sheet is, for example, a portion of the aforementioned resin used to mold the primary and secondary sheets, which are precursors to the negative electrode material sheet, that remained unburned during the firing process.
[0060] The resin content of the negative electrode material sheet is usually 8% by mass or less, preferably 3% by mass or less, and more preferably 1% by mass or less. If the resin content in the negative electrode material sheet is below the above predetermined value, there will be less resin that can hinder the movement of charge carriers such as lithium, thus facilitating the movement of charge carriers, and thus enabling the resulting secondary battery to exhibit excellent rate characteristics. Furthermore, the resin content in the negative electrode material sheet is not particularly limited and can be 0% by mass or more. However, from the viewpoint of further improving the rate characteristics of the resulting secondary battery, it is particularly preferable that the resin content in the negative electrode material sheet be 0% by mass. The resin content in the negative electrode material sheet can be adjusted, for example, by the manufacturing process of the negative electrode material sheet described above, the type and amount of resin used, and the firing conditions (e.g., temperature and time).
[0061] [Fibrous carbon materials] When the negative electrode material sheet contains fibrous carbon material, the content of fibrous carbon material in the negative electrode material sheet is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, even more preferably 0.4% by mass or more, preferably 5% by mass or less, more preferably 2.5% by mass or less, and even more preferably 1% by mass or less. If the content of fibrous carbon material in the negative electrode material sheet is above the lower limit, the strength of the negative electrode material sheet can be further increased. On the other hand, if the content of fibrous carbon material in the negative electrode material sheet is below the upper limit, a sufficiently high content of particulate carbon material in the negative electrode material sheet can be secured, and the resulting secondary battery can be made to have a sufficiently high capacity.
[0062] [Ratio of diffraction intensities on the surface of the negative electrode material sheet: I(110) / I(004)] The ratio I(110) / I(004) of the diffraction intensity of the (110) plane to the diffraction intensity of the (004) plane in the X-ray diffraction of the surface of the negative electrode material sheet is preferably 1.1 or more, more preferably 3 or more, even more preferably 5 or more, even more preferably 10 or more, and particularly preferably 20 or more. In this case, the particulate carbon material used as the negative electrode active material shows peaks attributable to the (004) plane and peaks attributable to the (110) plane in its X-ray diffraction pattern. Since the (110) plane in the crystal structure of the particulate carbon material is a plane perpendicular to the plane consisting of six-membered carbon rings (i.e., a plane equivalent to the (004) plane), the ratio of the peak intensity of the (110) plane to the peak intensity of the (004) plane in X-ray diffraction indicates the crystal orientation of the particulate carbon material. A high I(110) / I(004) value in the X-ray diffraction of the surface of the negative electrode material sheet indicates a high orientation of the (004) plane in the direction perpendicular to the surface of the negative electrode material sheet (typically coinciding with the direction perpendicular to the surface of the negative electrode current collector). Therefore, if the diffraction intensity ratio I(110) / I(004) is greater than or equal to the predetermined value, the orientation of the (004) plane in the direction perpendicular to the surface of the negative electrode material sheet increases, which facilitates the movement of charge carriers such as lithium, and thus the resulting secondary battery can exhibit excellent rate characteristics. Furthermore, the diffraction intensity ratio I(110) / I(004) is not particularly limited, but is preferably 90 or less. The diffraction intensity I(110) / I(004) can be adjusted by, for example, the manufacturing process of the negative electrode material sheet described above, the properties of the particulate carbon material used (e.g., aspect ratio), the molding conditions including the film thickness of the primary sheet described later, and the firing conditions (e.g., temperature and time).
[0063] [Density of the negative electrode material sheet] The density of the negative electrode material sheet is 1.3 g / cm³. 3 Preferably, it is 1.26 g / cm³. 3 It is more preferable that the following is the case: 1.23 g / cm³ 3It is more preferable that it is not more than the above value. When the density of the negative electrode material sheet is not more than the predetermined value described above, the voids in the negative electrode material sheet increase, which facilitates the movement of charge carriers such as lithium, so that the obtained secondary battery can exhibit excellent rate characteristics. Furthermore, when the density of the negative electrode material sheet is not more than the predetermined value described above, the voids in the negative electrode material sheet increase, so that the electrolyte injectability of the obtained secondary battery can be enhanced. In addition, the density of the negative electrode material sheet is not particularly limited, but is preferably 0.7 g / cm 3 or more, more preferably 0.85 g / cm 3 or more, and still more preferably 1.05 g / cm 3 or more. When the density of the negative electrode material sheet is at least the above lower limit, the strength of the negative electrode material sheet can be sufficiently ensured to be high. In addition, when the density of the negative electrode material sheet is at least the above lower limit, the capacity of the obtained secondary battery can be increased. The density of the negative electrode material sheet can be adjusted by, for example, the above-described production process of the negative electrode material sheet, the type, properties and amount ratio of the resin and particulate carbon material to be used, the firing conditions (e.g., temperature and time), and the like.
[0064] [Thickness of Negative Electrode Material Sheet] The thickness of the negative electrode material sheet is preferably 80 μm or more, more preferably 90 μm or more, still more preferably 100 μm or more, and is preferably 500 μm or less, more preferably 300 μm or less, still more preferably 200 μm or less. When the thickness of the negative electrode material sheet is at least the above lower limit, the capacity of the obtained secondary battery can be increased. On the other hand, when the thickness of the negative electrode material sheet is not more than the above upper limit, the obtained secondary battery can be made thinner.
[0065] [Basis Weight of Negative Electrode Material Sheet] The basis weight of the negative electrode material sheet is preferably 7.5 g / cm 2 or more, more preferably 9 g / cm 2 or more, still more preferably 11 g / cm 2 or more, and 12 g / cm2 It is even more preferable that the above conditions are met. If the basis weight of the negative electrode material sheet is equal to or greater than the above predetermined value, the resulting secondary battery can be made to have a higher capacity. Furthermore, the basis weight of the negative electrode material sheet is not particularly limited, but is 30 g / cm². 2 Preferably, it is 15 g / cm³ 2 The following is more preferable: If the basis weight of the negative electrode material sheet is less than or equal to the above predetermined value, the movement of charge carriers such as lithium becomes easier, and a sufficiently high rate characteristic of the resulting secondary battery can be ensured. In this invention, the basis weight of the negative electrode material sheet can be measured by the method described in the examples of this specification.
[0066] <(E) Paint film formation process> In the coating film formation process, a slurry composition for forming the undercoat layer (hereinafter also simply referred to as "slurry composition") is applied to the current collector to form a coating film consisting of the slurry composition. The slurry composition is not particularly limited and can be applied using known methods. Among these, it is preferable to apply the slurry composition by the bar coating method. The amount of slurry composition applied can be appropriately adjusted according to the desired thickness of the undercoat layer (thickness after drying).
[0067] <<Slurry Composition>> The above slurry composition can be prepared by mixing carbon material and binder, and optionally other components (other components) in a solvent. These components can be mixed using known mixing equipment such as a kneader; a mixer such as a Henschel mixer, Hobart mixer, or high-speed mixer; a twin-shaft kneader; or rolls.
[0068] [binder] As the binder, the resins listed in the section "(A) Primary Sheet Molding Process" above can be used. In particular, styrene-butadiene rubber (SBR) is preferred as the binder.
[0069] [Carbon materials] The carbon material is not particularly limited, but examples include particulate carbon material and fibrous carbon material. In particular, it is preferable to use at least one of particulate carbon material and fibrous carbon material, and it is more preferable to use particulate carbon material.
[0070] - Particulate carbon materials - The particulate carbon material is not particularly limited, but can be any of the spheroidal graphite (elliptical graphite) such as flake graphite, lump graphite (scaly graphite), earthy graphite, or flaked graphite, as listed in section (A) Primary Sheet Forming Process, or those obtained by acid treatment (expandable graphite, expanded graphite). These can be used individually or in combination of two or more. In particular, from the viewpoint of further improving the impact resistance of the resulting negative electrode and further improving the rate characteristics of the resulting secondary battery, it is preferable to use expanded graphite as the particulate carbon material. Furthermore, from the viewpoint of further improving the impact resistance of the resulting negative electrode and the rate characteristics of the resulting secondary battery, the volume average particle diameter of the particulate carbon material is preferably 1 μm or more, more preferably 2 μm or more, more preferably 20 μm or less, and more preferably 10 μm or less.
[0071] -Fibrous carbon materials- While there are no particular limitations on the fibrous carbon material, fibrous carbon nanostructures such as carbon nanotubes, as listed in section (A) Primary Sheet Forming Process, can be used. In particular, it is preferable to use fibrous carbon nanostructures containing carbon nanotubes, and more preferable to use carbon nanotubes.
[0072] [Other ingredients] Other components include thickeners to improve the coating properties of the slurry composition, and dispersants to effectively disperse optionally included fibrous carbon nanostructures and other materials. The thickening agent is not particularly limited and includes cellulosic polymers such as carboxymethylcellulose, methylcellulose, and hydroxypropylcellulose, as well as ammonium salts thereof. These thickening agents can be used individually or in combination of two or more. Among these, carboxymethylcellulose is preferred. Furthermore, the dispersant is not particularly limited, and known dispersants can be used.
[0073] [solvent] The solvent that can be used in the slurry composition is not particularly limited, and either water or an organic solvent can be used. Examples of organic solvents include acetonitrile, N-methyl-2-pyrrolidone, tetrahydrofuran, acetone, acetylpyridine, cyclopentanone, dimethylformamide, dimethyl sulfoxide, methylformamide, methyl ethyl ketone, furfural, ethylenediamine, dimethylbenzene (xylene), methylbenzene (toluene), cyclopentyl methyl ether, and isopropyl alcohol. Among these, water is preferred. Furthermore, these solvents can be used individually or as a mixture of two or more in any desired ratio.
[0074] [Solid content concentration] The solid content concentration of the slurry composition is not particularly limited, but from the viewpoint of improving the coating properties of the slurry composition, it is preferably 35% by mass or more and 58% by mass or less.
[0075] <(F) Pasting Process> In the application process, the negative electrode material sheet obtained through steps (A) to (D) above is applied to the coating film formed in step (E) above before it dries. In other words, in the application process, the negative electrode material sheet is applied to the wet undercoat layer. If the negative electrode material sheet is applied after the coating film has dried, adhesion between the negative electrode material sheet and the undercoat layer cannot be established, and the impact resistance of the resulting negative electrode will deteriorate. When attaching the negative electrode material sheet, the reduction rate of the solvent component contained in the coating film is preferably 65% by volume or less, more preferably 30% by volume or less, and particularly preferably 0% by volume, i.e., no reduction in the solvent component. The smaller the reduction rate of the solvent component, the higher the adhesion (bonding) between the negative electrode material sheet and the undercoat layer. The application of the negative electrode material sheet is not particularly limited, and can be done, for example, by placing the negative electrode material sheet on the coating before it dries (i.e., the coating while it is still wet) and pressing it against the coating.
[0076] <Other processes> Other steps include a drying step in which the laminated electrode (negative electrode), which is obtained through step (F) above and consists of a current collector, an undercoat layer, and a negative electrode material sheet, is further dried. The temperature for drying the laminate can be, for example, 10°C to 100°C, and the drying time can be, for example, 1 minute to 24 hours. Drying may also be carried out while the laminated electrode is pressurized.
[0077] (Negative electrode for non-aqueous secondary batteries) The negative electrode for a non-aqueous secondary battery of the present invention is characterized by comprising a current collector, an undercoat layer formed on the current collector, and a negative electrode composite layer formed on and adhered to the undercoat layer. Furthermore, the negative electrode for a non-aqueous secondary battery of the present invention is characterized in that the undercoat layer contains a carbon material and a binder. Moreover, the negative electrode for a non-aqueous secondary battery of the present invention is characterized in that the negative electrode composite layer contains a particulate carbon material, the particulate carbon material is oriented perpendicular to the surface of the negative electrode composite layer, the resin content in the negative electrode composite layer is 8% by mass or less, and the negative electrode composite layer exists as a self-supporting film. The negative electrode for a non-aqueous secondary battery of the present invention has excellent impact resistance and can exhibit excellent rate characteristics in a non-aqueous secondary battery.
[0078] <Negative electrode composite layer> The negative electrode composite layer contains particulate carbon material and may optionally further contain other components such as resin and fibrous carbon material. The negative electrode composite layer can be the negative electrode material sheet described in the section "Method for Manufacturing a Negative Electrode for Non-Aqueous Secondary Batteries" above. The properties and preferred attributes of the negative electrode composite layer, as well as the properties and preferred attributes of each component contained in the negative electrode composite layer, are the same as those of the negative electrode material sheet described above.
[0079] Specifically, the particulate carbon material contained in the negative electrode composite layer is oriented perpendicular to the surface of the negative electrode composite layer. If the particulate carbon material is not oriented perpendicular to the surface of the negative electrode composite layer, the rate characteristics of the resulting secondary battery will deteriorate. Furthermore, the resin content in the negative electrode composite layer is 8% by mass or less. If the resin content in the negative electrode composite layer exceeds 8% by mass, the rate characteristics of the resulting secondary battery will deteriorate. In addition, it is preferable that the particulate carbon material in the negative electrode composite layer contains flake graphite.
[0080] Here, the negative electrode composite layer needs to be adhered to the undercoat layer. Specifically, the negative electrode composite layer needs to be bonded to the current collector via the undercoat layer. If the negative electrode composite layer is not adhered to the undercoat layer, the negative electrode composite layer will not integrate with the current collector, and the impact resistance of the negative electrode cannot be ensured. Adhesion can be achieved, for example, by attaching the negative electrode material sheet before the coating film of the undercoat layer forming slurry composition dries, as described above.
[0081] Furthermore, whether or not the negative electrode composite layer is bonded to the undercoat layer can be confirmed by the method described in the examples.
[0082] Furthermore, the negative electrode composite layer exists as a self-supporting film. By using a negative electrode material sheet as the negative electrode composite layer, the negative electrode composite layer can be made to exist as a self-supporting film in good condition. If the negative electrode composite layer is a self-supporting film, the negative electrode can be manufactured by fabricating and bonding the constituent components of the negative electrode together, thereby improving productivity.
[0083] <Undercoat layer> The undercoat layer comprises a carbon material and a binder, and optionally further comprises components other than the carbon material and binder (other components). The carbon material, binder, and other components can be those described in the section "Method for Manufacturing a Negative Electrode for Non-Aqueous Secondary Batteries" above. The properties and preferred attributes of these components are also the same as those described in the section "Method for Manufacturing a Negative Electrode for Non-Aqueous Secondary Batteries".
[0084] <<Carbon Materials>> The carbon material included in the undercoat layer is not particularly limited, but it preferably includes at least one of particulate carbon material and fibrous carbon material, and more preferably includes particulate carbon material. The carbon material content in the undercoat layer is preferably 90% by mass or more, more preferably 95% by mass or more, preferably 99% by mass or less, and more preferably 98% by mass or less. If the carbon material content in the undercoat layer is within the above range, the rate characteristics of the resulting secondary battery can be further improved.
[0085] <<Binder>> The binder included in the undercoat layer is not particularly limited, but it is preferable that it includes styrene-butadiene rubber (SBR). The binder content in the undercoat layer is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, preferably 0.5% by mass or less, and more preferably 0.4% by mass or less. If the binder content in the undercoat layer is within the above range, the impact resistance of the negative electrode can be improved while further enhancing the rate characteristics of the resulting secondary battery.
[0086] <<Other ingredients>> The proportion of other components in the undercoat layer can be adjusted within a range that does not impair the desired effects of the present invention.
[0087] <<Thickness>> The thickness of the undercoat layer is preferably 1 μm or more, more preferably 2 μm or more, even more preferably 4 μm or more, and preferably 15 μm or less, and more preferably 10 μm or less. If the thickness of the undercoat layer is within the above predetermined range, the impact resistance of the negative electrode can be improved while further improving the rate characteristics of the non-aqueous secondary battery.
[0088] <Current collector> As the current collector, for example, a current collector made of iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc., can be used. Among these, copper foil is particularly preferred as the current collector used for the negative electrode. The above materials may be used individually or in combination of two or more materials in any ratio.
[0089] (Non-aqueous secondary battery) The non-aqueous secondary battery of the present invention is characterized by comprising the negative electrode for the non-aqueous secondary battery of the present invention described above. For example, the non-aqueous secondary battery of the present invention comprises a positive electrode, a negative electrode, an electrolyte, and a separator, and uses the negative electrode for non-aqueous secondary batteries of the present invention as the negative electrode. Since the non-aqueous secondary battery of the present invention uses the negative electrode for non-aqueous secondary batteries of the present invention, it can exhibit excellent rate characteristics. The following description will use the case where the non-aqueous secondary battery is a lithium-ion secondary battery as an example, and will describe the positive electrode, electrolyte, and separator, but the present invention is not limited to these examples.
[0090] <Positive electrode> As the positive electrode, a known positive electrode used for lithium-ion secondary batteries can be used. Specifically, as the positive electrode, for example, a positive electrode formed by creating a positive electrode composite layer on a current collector can be used. Furthermore, the current collector can be made of a metal material such as aluminum. In addition, the positive electrode composite layer can be a layer containing a known positive electrode active material, a conductive material, and a binder.
[0091] <Electrolyte> As the electrolyte, an electrolyte solution in which an electrolyte is dissolved in a solvent can be used. Here, an organic solvent capable of dissolving electrolytes can be used as the solvent. Specifically, as the solvent, an alkyl carbonate solvent such as ethylene carbonate, propylene carbonate, or γ-butyrolactone can be used, to which viscosity-adjusting solvents such as 2,5-dimethyltetrahydrofuran, tetrahydrofuran, diethyl carbonate, ethyl methyl carbonate, dimethyl carbonate, methyl acetate, dimethoxyethane, dioxolane, methyl propionate, or methyl formate can be added. A lithium salt can be used as the electrolyte. For example, the lithium salt described in Japanese Patent Publication No. 2012-204303 can be used. Among these lithium salts, LiPF6, LiClO4, and CF3SO3Li are preferred as electrolytes because they are easily soluble in organic solvents and exhibit a high degree of dissociation.
[0092] <Separator> The separator is not particularly limited and known types can be used; for example, those described in Japanese Patent Application Publication No. 2012-204303 can be used. Among these, a microporous membrane made of polyolefin resin (polyethylene, polypropylene, polybutene, polyvinyl chloride) is preferred because it allows for a thinner overall film thickness of the separator, thereby increasing the ratio of electrode active material in the lithium-ion secondary battery and thus increasing the capacity per unit volume.
[0093] <Manufacturing method for non-aqueous secondary batteries> The non-aqueous secondary battery of the present invention can be produced, for example, by stacking a positive electrode and a negative electrode with a separator interposed therebetween, winding or folding the resulting stack according to the battery shape as necessary, placing the stack in a battery container, injecting an electrolyte into the battery container, and then sealing the battery container. In order to prevent an increase in the internal pressure of the secondary battery, occurrence of overcharge and overdischarge, etc., a fuse, an overcurrent prevention element such as a PTC element, an expanded metal, a lead plate, and the like may be provided as necessary. The shape of the secondary battery may be any of, for example, a coin type, a button type, a sheet type, a cylindrical type, a prismatic type, a flat type, and the like. [Examples]
[0094] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to these Examples. In the following description, "%" and "part" representing amounts are based on mass unless otherwise specified. Various measurements and evaluations in the Examples were performed according to the following methods. <X-ray Diffraction> X-ray diffraction of the surface of the negative electrode material sheet (or the negative electrode mixture layer of the coated electrode) was performed using "X' Pert PRO MPD" manufactured by PANalytical. From the obtained peaks, the peak height (diffraction intensity) at 2Θ=77 degrees corresponding to the (110) plane and the peak height (diffraction intensity) at 2Θ=54.5 degrees corresponding to the (004) plane were used to calculate the value of the ratio I(110) / I(004) of the diffraction intensity of the (110) plane to the diffraction intensity of the (004) plane. <Resin Content Ratio> The following numerical values were calculated from the formulations in each Example and Comparative Example and the comparison of the weights before and after firing. Theoretical residual ratio = (total value of particulate carbon material) ÷ (total value of each formulation) Measured residual ratio = (weight after firing) ÷ (weight before firing) Resin content ratio = 1 - (Theoretical residual ratio) ÷ (Measured residual ratio) <Orientation Angle of Particulate Carbon Material> The orientation angle of particulate carbon material in the negative electrode material sheet (or negative electrode composite layer of the coated electrode) was observed using a scanning electron microscope (SEM, Hitachi High-Technologies "SU-3500") on a cross-section of the negative electrode material sheet cut into a regular octagon, at a magnification that captured the entire sheet from top to bottom. The magnification at this time was 700x. Fifty lines were drawn along the long axis of the particulate carbon material in this cross-section, and the average angle of the long axis relative to the surface of the negative electrode material sheet was calculated. This was performed on eight surfaces, and the value with the largest number of values among the eight surfaces was taken as the orientation angle of particulate carbon material in the negative electrode material sheet (negative electrode composite layer). <Thickness> Using a film thickness gauge (Mitutoyo, product name "Digimatic Indicator ID-C112XBS"), the thickness was measured at five points: approximately the center point and the four corners (squares) of the negative electrode material sheet (or negative electrode composite layer of the coated electrode). The average value (μm) of the measured thicknesses was taken as the thickness of the negative electrode material sheet (negative electrode composite layer). Similarly, the thickness of the undercoat layer (thickness of the dried film) was measured. <density> The mass, area, and thickness of the negative electrode material sheet (or negative electrode composite layer of the coated electrode) were measured, and the density of the negative electrode material sheet (or negative electrode composite layer) was calculated by dividing the mass by the volume (= area × thickness). <Balance of weight> The basis weight of the negative electrode material sheet (or negative electrode composite layer) was calculated by multiplying its density by its thickness. <Presence or absence of adhesion between the negative electrode composite layer and the undercoat layer> When the negative electrodes (layered electrodes) prepared in the examples and comparative examples were tilted 90° from a horizontal position so that the layering direction was parallel to the horizontal direction, if the negative electrode material sheet (or coated electrode) did not detach from the undercoat layer, it was determined that the two were adhered. If the negative electrode material sheet (or coated electrode) detached from the undercoat layer, it was determined that the two were not adhered. <Impact Resistance> Each negative electrode prepared in the examples and comparative examples was punched out using a 13Φ hand punch (manufactured by Nogami Giken). The degree of collapse of the negative electrode upon punching was evaluated based on the following criteria. Note that if the negative electrode composite layer is integrated with the current collector, the negative electrode will not collapse due to the impact of punching; however, if the adhesion is insufficient, the negative electrode will collapse due to the impact of punching. A: No chipping is observed in the negative electrode composite layer after punching. B: Cracks appear in the negative electrode composite layer during punching. C: Two or fewer chips occur in the negative electrode composite layer during punching. D: The negative electrode splits into three or more parts and can no longer maintain its shape. <Self-supporting film> Each negative electrode prepared in the examples and comparative examples was laid on the surface of a 10 cm diameter cylinder with the current collector in close contact with it, thereby peeling the negative electrode material sheet (negative electrode composite layer) from the current collector and the undercoat layer. When only the negative electrode material sheet was peeled off, it was determined that the negative electrode material sheet (negative electrode composite layer) was a self-supporting film, and when the negative electrode material sheet (negative electrode composite layer) was peeled off together with the undercoat layer, it was determined that the negative electrode material sheet (negative electrode composite layer) was not a self-supporting film. While it is possible to determine whether or not detachment has occurred by visual inspection, if visual inspection is difficult, analysis may be performed using a scanning electron microscope (SEM) or similar equipment. <Rate Characteristics> <<Manufacturing of electrode evaluation cells>> A lithium-ion secondary battery half-cell (half-cell) for evaluation was fabricated with the configuration shown below. The half-cell was fabricated by punching out each component to a size of 17 mm in diameter, vacuum drying (120°C for 10 hours), and then drying in a dry box with a dew point of -80°C or lower. [Half-cell configuration] Working electrode: Negative electrode (a negative electrode formed by attaching a negative electrode material sheet to the undercoat layer, or a negative electrode formed by attaching a coated electrode to the undercoat layer) Opposite pole: Li metal Reference pole: Li metal Separator: Glass nonwoven fabric, polyethylene (PE) microporous membrane Electrolyte: 1.0 M LiPF6 solution (solvent is a mixed solvent of ethylene carbonate (EC) / methyl ethyl carbonate (MEC) = 3 / 7 (volume ratio), containing 1 vol% vinylene carbonate (VC) as an additive (solvent ratio)). <<Charge / Discharge Test>> The obtained evaluation half-cells were subjected to charge-discharge tests under the following condition 1. (Charge / discharge test conditions) (Condition 1) Charging conditions: 0.2C, Charging voltage 0.01V-CCCV (0.05C cut) Discharge conditions: 0.2C, cutoff voltage 2.5V-CC Number of cycles: 10 cycles Next, a further charge-discharge test was conducted under the following condition 2. (Condition 2) Test temperature: 25℃ Charging conditions: 0.2C, Charging voltage 0.01V-CCCV (0.05C cut) Discharge conditions: 2.0C, cutoff voltage 2.5V-CC Number of cycles: 10 cycles Test temperature: 25℃ The charge-discharge rate characteristic was calculated as the percentage of the discharge capacity at 2.0C (measured under Condition 2) to the discharge capacity at 0.2C (measured under Condition 1) (= (discharge capacity at 2.0C / discharge capacity at 0.2C) × 100%), and evaluated according to the following criteria. The results are shown in Table 1. A larger value for the charge-discharge rate characteristic indicates lower internal resistance and the ability to perform high-speed charging and discharging (i.e., superior rate characteristics). A: Charge / discharge rate characteristic value is 65% or higher B: Charge / discharge rate characteristic value is between 47.5% and less than 65% C: Charge / discharge rate characteristic value is 30% or more and less than 47.5% D: Charge / discharge rate characteristic value is less than 30%
[0095] (Example 1) <Preparation of composition> 140 parts of liquid nitrile rubber (NBR) (manufactured by Nippon Zeon Co., Ltd., product name "Nipol 1312", decomposition start temperature: 336℃) and 140 parts of solid nitrile rubber (NBR) (manufactured by Nippon Zeon Co., Ltd., product name "Nipol 3350", decomposition start temperature: 375℃) were mixed using a pressurized kneader (manufactured by Nippon Spindle Co., Ltd.) at 150℃ for 20 minutes. Next, the resulting mixture was placed in a crusher (manufactured by Osaka Chemical Co., Ltd., product name "Wonder Crush Mill D3V-10") and crushed for 10 seconds to obtain the composition.
[0096] <Formation of the primary sheet> Next, 50 g of the obtained composition was sandwiched between 50 μm thick PET films (protective films) that had been sandblasted, and rolled (primary pressurized) under the conditions of a roll gap of 1000 μm, a roll temperature of 50°C, a roll linear pressure of 50 kg / cm, and a roll speed of 1 m / min to obtain a primary sheet with a thickness of 0.8 mm.
[0097] <Formation of laminates> Next, the obtained primary sheet was cut to 150 mm in length, 150 mm in width, and 0.8 mm in thickness. 188 sheets were stacked in the thickness direction of the primary sheet, and then pressed (secondary pressurization) in the stacking direction at a temperature of 120°C and a pressure of 0.1 MPa for 3 minutes to obtain a laminate with a height of approximately 150 mm.
[0098] <Formation of the secondary sheet> Subsequently, while pressing the laminated sides of the secondary-pressurized laminate with a pressure of 0.3 MPa, a woodworking slicer (manufactured by Marunaka Iron Works Co., Ltd., product name "Super Finishing Planer Super Mecha S") was used to slice the laminate at a 0-degree angle to the lamination direction (in other words, in the direction normal to the main surface of the laminated primary sheet), thereby obtaining a secondary sheet measuring 150 mm in length, 150 mm in width, and 0.10 mm in thickness.
[0099] <Fabrication of negative electrode material sheets> Subsequently, the obtained secondary sheet was fired at 1000°C for 8 hours under a nitrogen atmosphere to burn off and remove the resin components, thereby obtaining a negative electrode material sheet. For the obtained negative electrode material sheet, the ratio of the diffraction intensity of the (110) plane to the diffraction intensity of the (004) plane (I(110) / I(004)), the orientation angle of the particulate carbon material, thickness, density, and basis weight were measured. The results are shown in Table 1.
[0100] <Preparation of slurry composition for undercoat layer formation> Expanded graphite with an average particle size of 7 μm (manufactured by Ito Graphite Co., Ltd.: product name "EC-1500") was pulverized to adjust the average particle size to 1.5 μm, and this small-particle graphite powder was mixed with styrene-butadiene rubber (SBR) as a binder and carboxymethylcellulose (CMC) as a thickener, in a mass ratio of 100:0.2:0.2. The resulting mixture was added to water as a solvent and mixed to obtain a slurry composition for forming an undercoat layer, with a solid content concentration of 27%.
[0101] <Fabrication of multilayer electrodes (negative electrodes)> Using a bar coater No. 10 (manufactured by Tester Sangyo Co., Ltd., SA-203, No. 10), the obtained undercoat layer forming slurry composition was applied to the copper foil used as a current collector to obtain a coating film. Then, before the coating film dried completely (solvent reduction rate: 10%), the negative electrode material sheet was placed on the coating film and then lightly pressed with a finger to adhere the negative electrode material sheet to the coating film. The time from application to adhesion with a finger was 3 seconds. The resulting laminate was then vacuum-dried at 60°C for 8 hours to obtain the negative electrode. The dry thickness of the undercoat layer was 4 μm. Various measurements and evaluations were performed using this negative electrode. The results are shown in Table 1.
[0102] (Example 2) The negative electrode was manufactured in the same manner as in Example 1, except that a bar coater No. 22 (manufactured by Tester Industries Co., Ltd., SA-203, No. 22) was used when applying the slurry composition for forming the undercoat layer, and various measurements and evaluations were performed. The results are shown in Table 1.
[0103] (Example 3) The negative electrode was manufactured in the same manner as in Example 1, except that a bar coater No. 6 (manufactured by Tester Industries Co., Ltd., SA-203, No. 6) was used when applying the slurry composition for forming the undercoat layer. Various measurements and evaluations were then performed. The results are shown in Table 1.
[0104] (Example 4) The negative electrode was manufactured in the same manner as in Example 1, except that the amount of flake graphite added was changed from 950 parts to 700 parts (an amount equivalent to 50 parts by volume when the total volume is 100 parts by volume), and various measurements and evaluations were performed. The results are shown in Table 1.
[0105] (Comparative Example 1) The negative electrode was manufactured in the same manner as in Example 1, except that the coating film of the undercoat layer forming slurry composition was vacuum-dried to dryness (solvent reduction rate: 90%) at 60°C for 8 hours before attaching the negative electrode material sheet. Various measurements and evaluations were then performed. The results are shown in Table 1. Although the adhesion between the copper foil, which is the current collector, and the undercoat layer was good, there was no adhesion at all between the negative electrode material sheet and the undercoat layer, resulting in poor impact resistance of the negative electrode. Furthermore, because the negative electrode material sheet did not adhere to the undercoat layer, it was not possible to manufacture a half-cell, and therefore the rate characteristics of the secondary battery could not be measured.
[0106] (Comparative Example 2) The negative electrode was manufactured in the same manner as in Example 1, except that an unfired secondary sheet was used as the negative electrode material sheet instead of the negative electrode material sheet prepared in Example 1. Various measurements and evaluations were then performed. The results are shown in Table 1. Note that because the negative electrode material sheet was not fired and contained a large amount of resin components, the negative electrode did not function as an electrode and showed no battery performance at all.
[0107] (Comparative Example 3) A negative electrode was manufactured in the same manner as in Example 1, except that instead of the negative electrode material sheet prepared in Example 1, a slurry composition for the negative electrode composite layer prepared as described below was applied to the undercoat layer, and the resulting coating film was dried to form a negative electrode composite layer (thickness: 108 μm) on the undercoat layer. Various measurements and evaluations were then performed. The results are shown in Table 1. <Preparation of slurry composition for negative electrode composite layer> The flake-shaped graphite (manufactured by Nippon Graphite Industries Co., Ltd., trade name "UP20α") used as particulate carbon material in Example 1, carboxymethylcellulose (CMC), and styrene-butadiene rubber (SBR) were mixed in a mass ratio of UP20α:CMC:SBR = 97.5:1.0:1.5 to obtain a slurry composition for the negative electrode composite layer. [Table 1]
[0108] Table 1 shows that in Examples 1 to 4, where a negative electrode was manufactured by laminating a negative electrode material sheet, which was made by firing a predetermined secondary sheet before the coating film, consisting of an undercoat layer forming slurry composition, dried, the impact resistance of the negative electrode was excellent, as was the rate characteristics of the non-aqueous secondary battery. [Industrial applicability]
[0109] According to the present invention, it is possible to provide a negative electrode that has excellent shock resistance and can exhibit excellent rate characteristics in non-aqueous secondary batteries, as well as a method for manufacturing the same. Furthermore, according to the present invention, it is possible to provide a non-aqueous secondary battery with excellent rate characteristics.
Claims
1. A primary sheet molding step involves pressurizing a composition containing resin and particulate carbon material to form a sheet and obtain a primary sheet, A laminate formation step is to obtain a laminate by stacking multiple primary sheets in the thickness direction, or by folding or winding the primary sheets, A slicing step in which the laminate is sliced at an angle of 45° or less with respect to the stacking direction to obtain a secondary sheet, A firing step to obtain a negative electrode material sheet for a non-aqueous secondary battery by firing the aforementioned secondary sheet, A coating film forming step involves applying a slurry composition for forming an undercoat layer, which contains carbon material and a binder, onto a current collector to form a coating film, A method for manufacturing a negative electrode for a non-aqueous secondary battery, comprising a bonding step of bonding the negative electrode material sheet for a non-aqueous secondary battery to the coating film before the coating film dries.
2. The method for manufacturing a negative electrode for a non-aqueous secondary battery according to claim 1, wherein the secondary sheet is fired at a temperature of 300°C to 2000°C.
3. A method for producing a negative electrode for a non-aqueous secondary battery according to claim 1 or 2, wherein the particulate carbon material includes flake graphite.
4. The device comprises a current collector, an undercoat layer formed on the current collector, and a negative electrode composite layer formed on the undercoat layer and adhered to the undercoat layer. The undercoat layer comprises a carbon material and a binder. The aforementioned negative electrode composite layer contains particulate carbon material, The particulate carbon material is oriented at an angle of 60° to 90° with respect to the surface of the negative electrode composite layer. The resin content in the negative electrode composite layer is 8% by mass or less. The aforementioned negative electrode composite layer exists as a self-supporting film. The adhesion is determined by the following method: Whether or not the aforementioned negative electrode composite layer is a self-supporting film is determined by the following method, for a negative electrode for a non-aqueous secondary battery. <Presence or absence of adhesion between the negative electrode composite layer and the undercoat layer> When a negative electrode for a non-aqueous secondary battery, which consists of a current collector, an undercoat layer, and a negative electrode composite layer, is tilted 90° from a horizontal position so that the stacking direction is parallel to the horizontal direction, if the negative electrode composite layer does not detach from the undercoat layer, it is determined that the negative electrode composite layer and the undercoat layer are adhered. If the negative electrode composite layer detaches from the undercoat layer, it is determined that the negative electrode composite layer and the undercoat layer are not adhered. <Presence or absence of self-supporting film properties in the negative electrode composite layer> A negative electrode for a non-aqueous secondary battery, consisting of a current collector, an undercoat layer, and a negative electrode composite layer, is laid on the surface of a 10 cm diameter cylinder with the current collector in close contact with it, thereby separating the negative electrode composite layer from the current collector and undercoat layer. If only the negative electrode composite layer is separated, it is determined that the negative electrode composite layer is a self-supporting film. If the negative electrode composite layer is separated together with the undercoat layer, it is determined that the negative electrode composite layer is not a self-supporting film.
5. The negative electrode for a non-aqueous secondary battery according to claim 4, wherein the thickness of the undercoat layer is 1 μm or more and 15 μm or less.
6. The negative electrode for a non-aqueous secondary battery according to claim 4 or 5, wherein the ratio I(110) / I(004) of the diffraction intensity of the (110) plane to the diffraction intensity of the (004) plane in the X-ray diffraction of the surface of the negative electrode composite layer is 1.1 or more.
7. The density of the negative electrode composite layer is 1.3 g / cm³. 3 The negative electrode for a non-aqueous secondary battery according to any one of claims 4 to 6, as follows:
8. The negative electrode for a non-aqueous secondary battery according to any one of claims 4 to 7, wherein the thickness of the negative electrode composite layer is 80 μm or more.
9. The negative electrode for a non-aqueous secondary battery according to any one of claims 4 to 8, wherein the particulate carbon material contains flake graphite.
10. A non-aqueous secondary battery comprising a negative electrode for a non-aqueous secondary battery according to any one of claims 4 to 9.
Citation Information
Patent Citations
Non-aqueous electrolyte secondary battery and method for manufacturing negative electrode for secondary battery
WO2013088540A1
Method for producing composite material sheet and method for producing heat conductive sheet
WO2017081867A1
COIN TYPE LITHIUM SECONDARY BATTERY AND IoT DEVICE
WO2019221141A1