Laminates, packaging materials, packaging bodies and packaging articles
A laminate with a polypropylene substrate, anchor coat, vapor-deposited, and overcoat layers with specific axial stiffness ratios and thicknesses addresses the issue of maintaining oxygen barrier properties after bending and retort processing, enhancing durability and barrier performance.
Patent Information
- Application Number
- JP2022154798
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-09-28
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-09-28
AI Technical Summary
Conventional gas barrier films using polypropylene as a base material face challenges in maintaining high oxygen barrier properties after repeated bending and retort processing, leading to damage of the gas barrier layer.
A laminate structure comprising a polypropylene substrate, an anchor coat layer, a vapor-deposited layer of inorganic compounds, and an overcoat layer, with specific axial stiffness ratios and layer thicknesses, enhances the laminate's durability and barrier properties.
The laminate maintains high oxygen barrier properties even after repeated bending and retort treatment, ensuring the integrity of the packaging material.
Smart Images

Figure 0007947863000002 
Figure 0007947863000003 
Figure 0007947863000001
Abstract
Description
[Technical Field]
[0001] The present invention relates to laminates, packaging materials, packaging bodies, and packaging articles. [Background technology]
[0002] Many gas barrier films are widely used as packaging materials for food, medical products, and pharmaceuticals. In research and development related to these gas barrier films, minimizing oxygen permeability has been a particularly important consideration.
[0003] Packaging materials, such as food and pharmaceuticals, that are wrapped in gas barrier film are often subjected to retort processing. In barrier films used for packaging materials subjected to retort processing, highly heat-resistant polyethylene terephthalate film is generally used as the base material. However, in recent years, awareness of environmental issues has increased. Consequently, there is growing interest in so-called monomaterial packaging materials, which use a single material to ensure recyclability.
[0004] Conventional gas barrier films generally use polyethylene terephthalate film as the base material. In recent years, however, base materials made of polypropylene, an olefin component, have come into use as gas barrier films for monomaterial packaging. [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] International Publication No. 2021 / 220977 [Overview of the project] [Problems that the invention aims to solve]
[0006] The present invention aims to provide a laminate that maintains high oxygen barrier properties even after repeated bending and retort processing. [Means for solving the problem]
[0007] According to one aspect of the present invention, the present invention comprises a polypropylene substrate, an anchor coat layer, a vapor-deposited layer made of an inorganic compound, and a resin-containing overcoat layer in this order, wherein one side of the vapor-deposited layer is in contact with the anchor coat layer and the other side is in contact with the overcoat layer, and the axial rigidity S of the overcoat layer O and the axial stiffness S of the anchor coat layer A The ratio S O / S A A laminate is provided in which the range is between 2 and 13.
[0008] According to another aspect of the present invention, a laminate relating to the above aspect is provided in which the anchor coat layer has a thickness of 0.1 μm or more and 1 μm or less.
[0009] According to yet another aspect of the present invention, a laminate according to any of the above aspects is provided, in which the anchor coat layer is made of a urethane-based adhesive.
[0010] According to yet another aspect of the present invention, the anchor coat layer is provided as a laminate relating to any of the above aspects, comprising a reaction product of an acrylic polyol with tolylene diisocyanate and hexamethylene diisocyanate.
[0011] According to yet another aspect of the present invention, a laminate is provided in which the overcoat layer has a thickness of 0.1 μm or more and 1 μm or less, according to any of the above aspects.
[0012] According to yet another aspect of the present invention, a laminate according to any of the above aspects is provided, wherein the overcoat layer further comprises a reaction product of at least one of an alkoxide and a silane coupling agent, and the resin contained in the overcoat layer is a water-soluble polymer having hydroxyl groups.
[0013] According to still another aspect of the present invention, there is provided the laminate according to any one of the above aspects, wherein the reaction product is a silicon-containing oxide, and in the overcoat layer, the proportion of the amount of silicon in the total amount of silicon and the water-soluble polymer is in the range of 9 to 90 mass%.
[0014] According to still another aspect of the present invention, there is provided the laminate according to any one of the above aspects, wherein the vapor deposition layer contains at least one of aluminum oxide and silicon oxide.
[0015] According to still another aspect of the present invention, there is provided a packaging material comprising the laminate according to any one of the above aspects and a sealant layer.
[0016] According to still another aspect of the present invention, there is provided a package including the packaging material according to the above aspect.
[0017] According to still another aspect of the present invention, there is provided a packaged article comprising the package according to the above aspect and an article accommodated in the package. [Effects of the Invention]
[0018] According to the present invention, there is provided a laminate that maintains high oxygen barrier properties even after repeated bending or retort treatment. [Brief Description of the Drawings]
[0019] [Figure 1] Figure 1 is a cross-sectional view of a laminate according to an embodiment of the present invention. [Figure 2] Figure 2 is a cross-sectional view showing an example of a packaging material including the laminate of Figure 1. [Mode for Carrying Out the Invention]
[0020] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments described below are more specific implementations of any of the above aspects. The matters described below may be incorporated into each of the above aspects alone or in combination of a plurality thereof.
[0021] Furthermore, the embodiments shown below illustrate configurations for realizing the technical concept of the present invention, and the technical concept of the present invention is not limited by the material, shape, and structure of the components described below. Various modifications can be made to the technical concept of the present invention within the technical scope defined by the claims described in the claims.
[0022] Elements with similar or identical functions are given the same reference numerals in the drawings referenced below, and redundant explanations are omitted. Furthermore, the drawings are schematic, and the relationships between dimensions in one direction and those in another, and the relationships between the dimensions of one component and those of other components, may differ from reality.
[0023] <1> Laminate Figure 1 is a cross-sectional view of a laminate according to one embodiment of the present invention. The laminate 10 shown in Figure 1 is a gas barrier film. The laminate 10 includes a substrate 11, an anchor coat layer 12, a vapor deposition layer 13, and an overcoat layer 14 in that order. The term "film" used herein does not include the concept of thickness.
[0024] <1.1> Base material The substrate 11 is a film (base film) that serves as a support in the laminate 10. The substrate 11 contains polypropylene. Preferably, the substrate 11 is a polypropylene film. The polypropylene film may be a stretched film or an unstretched film, but preferably a stretched polyolefin film. An example of a stretched polyolefin film is a biaxially oriented polyolefin film. Alternatively, a film derived from recycled resin, such as polypropylene recycled from industrial waste, may be used. The substrate 11 may further contain additives such as heat stabilizers, antioxidants, crystal nucleating agents, lubricants, antistatic agents, viscosity modifiers, ultraviolet absorbers, plasticizers, and light stabilizers. The surface of the substrate 11 may be subjected to modification treatments such as corona treatment, flame treatment, plasma treatment, or easy-adhesion treatment.
[0025] In the example shown in Figure 1, the substrate 11 includes a core layer 11A, a skin layer 11B1, and a skin layer 11B2.
[0026] The core layer 11A is made of, for example, polypropylene, or polypropylene and one or more other components in smaller amounts. For example, the core layer 11A is made of 99 to 75% by mass of crystalline polypropylene resin and 1 to 25% by mass of petroleum resin. Examples of the petroleum resin include resins obtained by polymerizing or copolymerizing cyclopentene fractions and / or cyclohexene fractions and then hydrogenating them; resins obtained by hydrogenating alicyclic polymers obtained by polymerizing or copolymerizing cyclic olefins such as cyclopentene derivatives and cyclohexene derivatives; and cyclopentadiene-based hydrogenated petroleum resins. The petroleum resin is preferably a cyclopentadiene-based hydrogenated petroleum resin. The core layer 11A may contain only one type of petroleum resin, or it may contain two or more types.
[0027] Skin layer 11B1 is provided on one side of core layer 11A. Skin layer 11B2 is provided on the other side of core layer 11A. Skin layers 11B1 and 11B2 are layers mainly composed of polypropylene copolymer. Skin layers 11B1 and 11B2 can improve the adhesion between the substrate 11 and other adjacent layers.
[0028] The polypropylene copolymers constituting the skin layers 11B1 and 11B2 are preferably those with relatively low stereoregularity, such as random copolymers of ethylene and propylene and ethylene-propylene-butylene copolymers. The skin layers 11B1 and 11B2 may also be composed of a mixture of polypropylene and polybutylene. Preferably, the skin layers 11B1 and 11B2 consist of random copolymers of ethylene and propylene.
[0029] The core layer 11A, skin layers 11B1 and 11B2 may further contain additives such as thermal stabilizers, antioxidants, nucleating agents, lubricants, antistatic agents, viscosity modifiers, ultraviolet absorbers, plasticizers, and light stabilizers.
[0030] The thickness of the substrate 11 is preferably in the range of 10 to 100 μm, and more preferably in the range of 10 to 20 μm. If the substrate 11 includes skin layers 11B1 and 11B2, the thickness of each of them is preferably 0.2 μm or more. The thickness of each of the skin layers 11B1 and 11B2 is, for example, 2.0 μm or less.
[0031] <1.2> Anchor Coat Layer The anchor coat layer 12 is provided on one side of the substrate 11. The anchor coat layer 12 is made of, for example, a urethane-based adhesive. The anchor coat layer 12 can be formed by, for example, preparing a composite solution by mixing a polyol and an isocyanate compound at any concentration, coating this onto the substrate 11, and drying and curing the coating film.
[0032] The polyol used here is a polymer having two or more hydroxyl groups at its terminus, which will be reacted with the isocyanate group of the isocyanate compound added later. Preferably, this polyol is an acrylic polyol, such as a polyol obtained by polymerizing an acrylic acid derivative monomer or a polyol obtained by copolymerizing an acrylic acid derivative monomer with other monomers.
[0033] Isocyanate compounds are added to enhance adhesion to the substrate 11 and the vapor-deposited layer 13 through urethane bonds formed by reaction with polyols such as acrylic polyols, and primarily act as crosslinking agents or curing agents. Specific examples of isocyanate compounds exhibiting such functions include aromatic compounds such as tolylene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI), aliphatic compounds such as xylylene diisocyanate (XDI) and hexamethylene diisocyanate (HMDI), monomers such as isophorone diisocyanate (IPDI), polymers thereof, and derivatives thereof, one or more of which can be selected.
[0034] The mixing ratio of polyol to isocyanate compound is not particularly limited. However, if the isocyanate compound is too little, curing failure may occur, and if the isocyanate compound is too much, blocking may occur, causing processing problems. Therefore, it is preferable to mix the polyol and isocyanate compound such that the NCO groups derived from the isocyanate compound are 50 times or less the OH groups derived from the polyol, and it is particularly preferable that the NCO groups and OH groups are approximately equivalent in weight. The mixing method can be any well-known method and is not particularly limited.
[0035] The elastic modulus of the anchor coat layer 12 can be adjusted by appropriately selecting the material of the anchor coat layer 12. For example, the elastic modulus of the anchor coat layer 12 can be made different depending on whether an aromatic compound or an aliphatic material is used as the isocyanate compound. Therefore, for example, by appropriately selecting the type of compound used as the isocyanate compound, or, if two or more compounds are used as the isocyanate compound, the mixing ratio thereof, an anchor coat layer 12 having a desired elastic modulus can be formed. For example, if the anchor coat layer 12 contains reaction products of acrylic polyol, tolylene diisocyanate, and hexamethylene diisocyanate, the elastic modulus of the anchor coat layer 12 can be changed depending on the mixing ratio of tolylene diisocyanate and hexamethylene diisocyanate.
[0036] The anchor coat layer 12 may further contain reaction products of the silane coupling agent. Silane coupling agents include compounds containing an isocyanate group, such as γ-isocyanatetopropyltriethoxysilane and γ-isocyanatetopropyltrimethoxysilane; compounds containing a mercapto group, such as γ-mercaptopropyltriethoxysilane; and compounds containing an amino group, such as γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltriethoxysilane, and γ-phenylaminopropyltrimethoxysilane. The silane coupling agent may also be a compound containing an epoxy group, such as γ-glycidooxypropyltrimethoxysilane or β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. The material of the anchor coat layer 12 may further contain silane coupling agents such as vinyltrimethoxysilane and vinyltris(β-methoxyethoxy)silane to which alcohols or the like have been added to add hydroxyl groups or the like. The material of the anchor coat layer 12 may contain one or more of these.
[0037] Silane coupling agents have an organic functional group at one end that interacts with the polyol and isocyanate compound in the complex. When a silane coupling agent containing a functional group that reacts with the hydroxyl group of the polyol or the isocyanate group of the isocyanate compound is used, a covalent bond can also be formed.
[0038] The elastic modulus of the anchor coat layer 12 can also be adjusted by controlling the silane coupling agent content.
[0039] Alternatively, alkoxysilanes or their hydrolysates can be used in place of or in conjunction with silane coupling agents. Examples of alkoxysilanes include tetramethoxysilane and tetraethoxysilane.
[0040] Known methods can be used to form the anchor coat layer 12. Specifically, wet deposition methods using coaters such as gravure coaters, dip coaters, reverse coaters, wire bar coaters, and die coaters can be used. The thickness of the anchor coat layer 12 is preferably 0.08 μm or more and 1 μm or less, and more preferably 0.1 μm or more and 0.8 μm or less.
[0041] <1.3> Vapor deposited layer The vapor-deposited layer 13 is provided on the anchor coat layer 12. One side of the vapor-deposited layer 13 is in contact with the anchor coat layer 12, and the other side is in contact with the overcoat layer 14. The vapor-deposited layer 13 is made of an inorganic compound. The vapor-deposited layer 13 may have a single-layer structure or a multilayer structure.
[0042] Examples of inorganic compounds included in the vapor-deposited layer 13 include silicon oxide, aluminum oxide, magnesium oxide, and metal oxides such as tin oxide. From the viewpoint of barrier properties, the inorganic compound preferably contains at least one of silicon oxide and aluminum oxide, and preferably consists of at least one of silicon oxide and aluminum oxide. The vapor-deposited layer 13 may also contain nitrogen or aluminum atoms. By using an inorganic compound, high barrier properties can be obtained with an extremely thin layer that does not affect the recyclability of the laminate 10.
[0043] The thickness of the vapor-deposited layer 13 is preferably 3 nm to 100 nm, and more preferably 5 nm to 50 nm. To obtain high gas barrier properties, it is preferable to form the vapor-deposited layer 13 to be sufficiently thick. However, increasing the thickness of the vapor-deposited layer 13 makes it easier for cracks to occur due to increased curing shrinkage. In addition, increasing the thickness of the vapor-deposited layer 13 tends to increase costs due to increased material usage and longer film formation times.
[0044] The deposited layer 13 can be formed, for example, by resistance heating vacuum deposition, electron beam heating vacuum deposition, or induction heating vacuum deposition.
[0045] <1.4> Overcoat layer The overcoat layer 14 is provided on the vapor-deposited layer 13. The overcoat layer 14 contains resin. The overcoat layer 14 is formed by a process of forming a resin-containing coating film on the vapor-deposited layer 13.
[0046] The coating agent used to form the coating film preferably contains the following components: (A) Alkoxide or hydrolysate thereof (hereinafter sometimes referred to as component A) (B) Water-soluble polymer (hereinafter sometimes referred to as component B) If component A contains an alkoxide, it undergoes hydrolysis, followed by dehydration condensation of the alkoxide hydrolysates (e.g., sol-gel method). In addition, the alkoxide hydrolysates and water-soluble polymers form organic-inorganic complexes through hydrogen bonding and dehydration condensation. For example, alkoxysilanes form Si-O bonds through hydrolysis and polycondensation reactions, and the silanol groups produced by hydrolysis form hydrogen bonds with the hydroxyl groups of water-soluble polymers. These reactions are presumed to result in excellent resistance to hot water and tension in the overcoat layer 14.
[0047] The alkoxide is preferably an alkoxysilane. The alkoxysilane has the general formula Si(OR) n The compound may be represented by (where R is an alkyl group such as CH3 and C2H5), for example, tetramethoxysilane [Si(OCH3)4] and tetraethoxysilane [Si(OC2H5)4]. Furthermore, the hydrolysis products of alkoxysilanes are obtained by hydrolysis of the above alkoxysilanes and have a silanol group. Among the above alkoxysilanes, tetraethoxysilane is preferred because it is relatively stable in aqueous solvents after hydrolysis.
[0048] Examples of water-soluble polymers include polyvinyl alcohol or its modified form, polyvinylpyrrolidone, starch, methylcellulose, carboxymethylcellulose, and sodium alginate. Preferably, the water-soluble polymer is a water-soluble polymer having hydroxyl groups. Among these, polyvinyl alcohol (hereinafter sometimes abbreviated as PVA) or its modified form is preferred because it can provide excellent gas barrier properties for the overcoat layer 14. Here, PVA is generally obtained by saponifying polyvinyl acetate. As PVA, for example, so-called partially saponified PVA, in which several tens of percent of acetate groups remain, and completely saponified PVA, in which only a few percent of acetate groups remain, can be used. Furthermore, as a modified form of PVA, it is also acceptable to use PVA into which an amount of ethylene groups has been introduced to maintain water solubility.
[0049] The overcoat layer 14 can be formed from a coating agent containing components A and B as described above. The coating agent may further contain a solvent. Examples of solvents include water, alcohol, and a mixed solvent of water and alcohol.
[0050] The overcoat layer 14 can be formed by coating the vapor-deposited layer 3 with a solution of component A and component B, or a solution of component B mixed with component A that has been pre-treated by hydrolysis, and then heating and drying the coating film. At this time, the elastic modulus of the overcoat layer 14 can be adjusted by adjusting the ratio of the silicon atom content in component A to the content of component B.
[0051] The overcoat layer 14 further contains, in addition to the water-soluble polymer described above, a reaction product of at least one of an alkoxide and a silane coupling agent. This reaction product is preferably a silicon-containing oxide. In this case, the proportion of silicon to the total amount of silicon and water-soluble polymer in the overcoat layer 14 is preferably in the range of 9 to 90% by mass, and more preferably in the range of 40 to 80% by mass.
[0052] The coating agent for forming the overcoat layer 14 may contain a silane coupling agent in place of or in addition to component A. Furthermore, the coating agent may contain, as necessary, other components to improve gas barrier properties, in addition to components A and B described above. Water-based materials are preferred as the other components. Examples of other components include aqueous dispersions of polyacrylic acid, polyurethane, acrylic resin, and polyester resin, and metal oxide precursors produced by the sol-gel method.
[0053] The coating agent may optionally contain one or more other components, such as leveling agents, defoaming agents, UV absorbers, antioxidants, and metal chelating agents.
[0054] As a method for forming the overcoat layer 14, a known method can be used. Specifically, a wet film formation method using a coater such as a gravure coater, a dip coater, a reverse coater, a wire bar coater, and a die coater can be used.
[0055] The thickness of the overcoat layer 14 is preferably 0.1 μm or more and 1 μm or less, and more preferably 0.2 μm or more and 0.8 μm or less.
[0056] <1.5>Axial stiffness In the laminate 10 described above, the axial stiffness S of the overcoat layer 14 O and the axial stiffness S of the anchor coat layer 12 A the ratio S O / S A is in the range of 2 to 13. The ratio S O / S A is preferably in the range of 2.5 to 12.0.
[0057] The axial stiffness S O and S A are determined by preparing a sample and performing force curve measurement according to the following method.
[0058] <1.5.1>Sample preparation A sample with the cross section of the laminate 10 exposed is prepared by the following method. First, corona treatment is performed as a surface treatment on both surfaces of the laminate 10. This prevents the film piece of the laminate 10 and the embedding resin described later from peeling off from each other.
[0059] Next, using a razor, a strip-shaped or wedge-shaped film piece is cut out from the laminate 10, and this is embedded with an embedding resin. As the embedding resin, a photocurable resin D-800 manufactured by Toagosei Co., Ltd. is used. The resin in which the film piece is embedded is cured by light irradiation.
[0060] The composite, consisting of the film piece of the laminate 10 and the cured embedding resin, is fixed using an insert for an atomic force microscope (AFM) sample holder. Next, trimming and cutting are performed on this composite at room temperature (25°C) using a glass knife. This cutting is performed so that the cross-section of the film piece is exposed. Subsequently, cutting is further performed on this composite at a low temperature (-120°C) using a diamond knife. This cutting is performed with a cutting speed of 1.0 mm / s and a cutting film thickness of 100 nm, until the previously cut surface becomes mirror-like. Leica's ultramicrotome EM UC7 and cryosystem EM FC7 are used as cross-sectional cutting equipment. The cutting direction is parallel to the interface of the layer containing the film piece of the laminate 10.
[0061] As described above, a sample for force curve measurement is obtained. This sample is then fixed in an AFM sample holder insert and used for the following force curve measurement.
[0062] <1.5.1> Force Curve Measurement Method For force curve measurement, an MFP-3D-SA atomic force microscope (AFM) manufactured by Oxford Instruments is used. AC mode (tapping mode) is used for shape measurement, and Contact mode is used for force curve measurement. After shape measurement, the force curve is acquired by specifying the measurement location, and the modulus of elasticity is calculated by analyzing the force curve. Igor Pro 3.8801 is used as the analysis software. For the calculation of the modulus of elasticity, the bottom 10% to top 90% of the indentation depth data during indentation is used from the force curve data, and the Hertz model analysis method is employed.
[0063] For this force curve measurement, a B20-NCH (manufactured by nanotools) cantilever with a radius of curvature of 20 nm and a spring constant of 40 N / m is used. The radius of curvature is the value provided by nanotools, the cantilever manufacturer. The spring constant is the value calculated using the thermal method.
[0064] When measuring force curves using Oxford Instruments' AFM and Igor Pro6.38801, it is desirable to set the measurement conditions as follows. Imaging Mode Off Mode Force Distance 0.1μm Scan Rate 0.25Hz Velocity 50nm / s Sample Rate 8kHz (8.333kHz) Low-pass filter 4kHz (4.167kHz) Trigger Channel Force 200nN.
[0065] When calculating the modulus of elasticity from the force curve in the Hertz model, the following items need to be set in Igor Pro 6.38801:
[0066] Tip Radius (curvature radius) Value provided by nanotools Geometry Sphere Sample Poisson ratio: 0.33 Tip Properties Diamond Synthetic Segment EXT (force curve when pressed).
[0067] Axial stiffness S of the overcoat layer 14 O To obtain this, first, the force curve described above is acquired on the overcoat layer 14 of the sample, changing the measurement location about 20 times. Next, the elastic modulus is calculated for each measurement location, and these are arithmetic mean. to Thickness of overcoat layer 14 Multiply by As a result, the axial stiffness S of the overcoat layer 14 O To obtain.
[0068] Axial stiffness S of anchor coat layer 12 ATo obtain this, first, the force curve described above is acquired on the anchor coat layer 12 of the sample, changing the measurement location about 20 times. Next, the elastic modulus is calculated for each measurement location, and these are arithmetic mean. to Thickness of anchor coat layer 12 Multiply by As a result, the axial stiffness S of the anchor coat layer 12 A To obtain.
[0069] The thickness of the overcoat layer 14 and the anchor coat layer 12 are determined from the shape image obtained in the shape measurement described above.
[0070] <1.6> Effect Generally, barrier films using polypropylene as the base material exhibit superior flexibility compared to barrier films using polyethylene terephthalate as the base material. However, barrier films using polypropylene as the base material are generally prone to damage to the gas barrier layer due to physical impacts after repeated bending or retort processing. Therefore, conventional barrier films using polypropylene as the base material have the problem of not being able to maintain low oxygen barrier properties after Gelboflex testing or retort processing testing.
[0071] As a result of diligent research, the inventors have determined that the axial stiffness S of the overcoat layer 14 is O and the axial stiffness S of the anchor coat layer 12 A The ratio S O / S A We found that laminates 10 within the above range maintain high oxygen barrier properties even after repeated bending and retort treatment. In other words, the above laminates 10 can keep their oxygen barrier properties low even after gel flex tests and retort treatment tests.
[0072] <2> packaging material The above laminate 10 can be used in packaging materials.
[0073] Figure 2 is a cross-sectional view showing an example of a packaging material including the laminate shown in Figure 1. The packaging material 1 shown in Figure 2 includes the laminate 10, a base layer 20, a sealant layer 30, and adhesive layers 40A and 40B.
[0074] <2.1> Base material layer The base layer 20 faces the base material 11 of the laminate 10. The base layer 20 may also face the overcoat layer 14 of the laminate 10. If the overcoat layer 14 of the laminate 10 faces the sealant layer 30, the base layer 20 may be omitted.
[0075] The base layer 20 is a polymer film. When the packaging material 1 is a monomaterial packaging material, the base layer 20 is preferably a polypropylene film. As the polypropylene film, for example, those exemplified for the base material 11 can be used.
[0076] <2.2>Sealant layer The sealant layer 30 faces the base layer 20 with the laminate 10 in between. When the packaging material 1 is a monomaterial packaging material, the sealant layer 30 preferably contains a polypropylene film, and more preferably is made of polypropylene. The sealant layer 30 is preferably an unstretched film.
[0077] <2.3>Adhesive layer Adhesive layer 40A is interposed between the laminate 10 and the base material layer 20, bonding them together. Adhesive layer 40B is interposed between the laminate 10 and the sealant layer 30, bonding them together. At least one of adhesive layers 40A and 40B may be omitted.
[0078] For example, a general-purpose dry laminating adhesive can be used as the adhesive for forming the adhesive layers 40A and 40B.
[0079] The adhesive layers 40A and 40B consist of at least one type of adhesive. The adhesive may be a one-component curing adhesive, a two-component curing adhesive, or a non-curing adhesive. Furthermore, the adhesive may be a solvent-free adhesive or a solvent-based adhesive.
[0080] Examples of adhesives include polyether-based adhesives, polyester-based adhesives, silicone-based adhesives, epoxy-based adhesives such as polyamine-based adhesives, urethane-based adhesives, rubber-based adhesives, vinyl-based adhesives, silicone-based adhesives, epoxy-based adhesives, phenol-based adhesives, and olefin-based adhesives. Adhesives containing biomass components can also be preferably used. Preferably, the adhesive is a polyamine-based adhesive or a urethane-based adhesive that has gas barrier properties.
[0081] The adhesive layers 40A and 40B may be cured products of a resin composition containing a polyester polyol, an isocyanate compound, and a phosphate-modified compound. Such adhesive layers 40A and 40B can further improve the oxygen barrier and water vapor barrier properties of the laminate 10A1.
[0082] The thickness of the adhesive layers 40A and 40B is preferably in the range of 0.1 μm to 20 μm, more preferably in the range of 0.5 μm to 10 μm, and even more preferably in the range of 1 to 5 μm.
[0083] The adhesive layers 40A and 40B can be formed by applying them onto the substrate layer 20 and the sealant layer 30 using conventionally known methods such as the direct gravure roll coating method, gravure roll coating method, kiss coating method, reverse roll coating method, fontein method, and transfer roll coating method, and then drying the coating film.
[0084] <2.4> Other layers Packaging material 1 may further include one or more other layers. For example, the packaging material 1 may further include one or more printed layers. The printed layers can be provided, for example, between the layers of the laminate 10 and the base material layer 20. The printed layers may also be provided between the layers of the laminate 10 and the sealant layer 30, or on the back surface of the base material layer 20 facing the sealant layer 30.
[0085] The printed layer is composed of an ink made by adding various pigments, extenders, plasticizers, drying agents, and stabilizers to a conventional ink binder resin such as urethane, acrylic, nitrocellulose, rubber, and vinyl chloride. It is preferable to use a biomass-derived ink as the printing ink. Biomass inks containing biomass-derived materials are also preferably used. Light-shielding inks are also preferably used. Examples of light-shielding inks include white ink, black ink, silver ink, and sepia ink.
[0086] As for the printing method, well-known printing methods such as offset printing, gravure printing, flexographic printing, and screen printing, as well as well-known coating methods such as roll coating, knife-edge coating, and gravure coating, can be used.
[0087] <3> packaging The above-mentioned packaging material 1 can be used in packaging. For example, the packaging is a bag such as a flat pouch, a standing pouch, or a gusseted pouch. The bag can be manufactured by overlapping the edges of one or more film pieces cut from the packaging material 1 so that the sealant layers 30 come into contact with each other and then heat-sealing them. In other examples, the packaging includes a container body having an opening and a lid that closes this opening. A film piece cut from packaging material 1 can be used as the lid.
[0088] <4> packaging goods The packaged article includes the packaging body described above and the article contained therein. The contents may be liquid, solid, or a mixture thereof. The contents may be, for example, food or medicine. [Examples]
[0089] The tests conducted in connection with the present invention are described below.
[0090] (1) Manufacturing of laminates (1.1) Example 1 The laminate 10 shown in Figure 1 was manufactured by the following method. First, a biaxially oriented polypropylene film (OPP film) with a thickness of 20 μm was prepared as the base material 11.
[0091] An isocyanate compound was added to an acrylic polyol in an equal amount to the OH groups of the acrylic polyol, and the mixture was diluted with ethyl acetate to a total of 2% by mass. Tolylene diisocyanate (TDI) and hexamethylene diisocyanate (HMDI) were used as the isocyanate compound in a 50:50 mass ratio. The anchor coat layer solution prepared in this way was applied to the substrate 11 by gravure coating to form an anchor coat layer 12 with a thickness of 120 nm (dry film thickness).
[0092] Next, silicon oxide was deposited on the anchor coat layer 12 using an electron beam vacuum deposition method to form a 30 nm thick deposition layer 13 made of silicon oxide.
[0093] A solution containing hydrolyzed tetraethoxysilane was prepared by mixing tetraethoxysilane, methanol, and 0.1N hydrochloric acid in a mass ratio of 45:15:40. This solution was mixed with a 5% aqueous solution of polyvinyl alcohol (PVA) so that the ratio of silicon atom content (a parts by mass) to PVA content (b parts by mass) was 50 / 50 by mass to obtain an overcoat coating solution. This overcoat coating solution was applied onto the vapor-deposited layer 13 by gravure coating to form an overcoat layer 14 with a thickness of 350 nm (dry film thickness). In this way, the laminate 10 shown in Figure 1 was obtained.
[0094] (1.2) Example 2 The laminate 10 shown in Figure 1 was manufactured by the following method. First, a biaxially oriented polypropylene film (OPP film) with a thickness of 20 μm was prepared as the base material 11.
[0095] An isocyanate compound was added to an acrylic polyol in an equal amount to the OH groups of the acrylic polyol, and the mixture was diluted with ethyl acetate to a total of 2% by mass. Tolylene diisocyanate (TDI) and hexamethylene diisocyanate (HMDI) were used as the isocyanate compound in a mass ratio of 70:30. The anchor coat layer solution prepared in this way was applied to the substrate 11 by gravure coating to form an anchor coat layer 12 with a thickness of 120 nm (dry film thickness).
[0096] Next, silicon oxide was deposited on the anchor coat layer 12 using an electron beam vacuum deposition method to form a 30 nm thick deposition layer 13 made of silicon oxide.
[0097] A solution containing hydrolyzed tetraethoxysilane was prepared by mixing tetraethoxysilane, methanol, and 0.1N hydrochloric acid in a mass ratio of 45:15:40. This solution was mixed with a 5% aqueous solution of polyvinyl alcohol (PVA) so that the ratio of silicon atom content (a parts by mass) to PVA content (b parts by mass) was 10 / 90 by mass ratio to obtain an overcoat coating solution. This overcoat coating solution was applied onto the vapor-deposited layer 13 by gravure coating to form an overcoat layer 14 with a thickness of 280 nm (dry film thickness). In this way, the laminate 10 shown in Figure 1 was obtained.
[0098] (1.3) Comparative Example 1 A laminate containing a substrate, an anchor coat layer, a vapor-deposited layer, and an overcoat layer in that order was manufactured by the following method.
[0099] First, a biaxially oriented polypropylene film (OPP film) with a thickness of 20 μm was prepared as the base material.
[0100] An ethylene-vinyl alcohol copolymer (EVOH) adhesive was prepared as the anchor coating agent. This adhesive was applied to the substrate by gravure coating to form an anchor coating layer with a thickness of 1 μm (dry film thickness).
[0101] Next, silicon oxide was deposited onto the anchor coat layer using an electron beam vacuum deposition method to form a 25 nm thick deposition layer made of silicon oxide.
[0102] A solution containing hydrolyzed tetraethoxysilane was prepared by mixing tetraethoxysilane, methanol, and 0.1N hydrochloric acid in a mass ratio of 45:15:40. This solution was mixed with a 5% aqueous solution of polyvinyl alcohol (PVA) so that the ratio of silicon atom content (a parts by mass) to PVA content (b parts by mass) was 75 / 25 by mass to obtain an overcoat coating solution. This overcoat coating solution was applied onto the vapor-deposited layer by gravure coating to form an overcoat layer with a thickness of 300 nm (dry film thickness). In this way, a laminate was obtained.
[0103] (1.4) Comparative Example 2 A laminate containing a substrate, an anchor coat layer, a vapor-deposited layer, and an overcoat layer in that order was manufactured by the following method.
[0104] First, a biaxially oriented polypropylene film (OPP film) with a thickness of 20 μm was prepared as the base material.
[0105] An isocyanate compound was added to an acrylic polyol in an equal amount to the OH groups of the acrylic polyol, and the mixture was diluted with ethyl acetate to a total of 2% by mass. Tolylene diisocyanate (TDI) and hexamethylene diisocyanate (HMDI) were used as the isocyanate compound in a mass ratio of 70:30. The anchor coat layer solution prepared in this way was applied to the substrate by gravure coating to form an anchor coat layer with a thickness of 120 nm (dry film thickness).
[0106] Next, silicon oxide was deposited onto the anchor coat layer using an electron beam vacuum deposition method to form a 30 nm thick deposition layer made of silicon oxide.
[0107] A solution containing hydrolyzed tetraethoxysilane was prepared by mixing tetraethoxysilane, methanol, and 0.1N hydrochloric acid in a mass ratio of 45:15:40. This solution was mixed with a 5% aqueous solution of polyvinyl alcohol (PVA) so that the ratio of silicon atom content (a parts by mass) to PVA content (b parts by mass) was 70 / 30 by mass to obtain an overcoat coating solution. This overcoat coating solution was applied onto the vapor-deposited layer by gravure coating to form an overcoat layer with a thickness of 750 nm (dry film thickness). In this way, a laminate was obtained.
[0108] (1.5) Reference example A laminate containing a substrate, an anchor coat layer, a vapor-deposited layer, and an overcoat layer in that order was manufactured by the following method.
[0109] First, a biaxially oriented polyethylene terephthalate film (PET film) with a thickness of 20 μm was prepared as the base material.
[0110] An isocyanate compound was added to an acrylic polyol in an equal amount to the OH groups of the acrylic polyol, and the mixture was diluted with ethyl acetate to a total of 2% by mass. Tolylene diisocyanate (TDI) was used as the isocyanate compound. The anchor coat layer solution prepared in this way was applied to a substrate by gravure coating to form an anchor coat layer with a thickness of 50 nm (dry film thickness).
[0111] Next, aluminum oxide was deposited onto the anchor coat layer using an electron beam vacuum deposition method to form a 50 nm thick deposition layer made of aluminum oxide.
[0112] A solution containing hydrolyzed tetraethoxysilane was prepared by mixing tetraethoxysilane, methanol, and 0.1N hydrochloric acid in a mass ratio of 45:15:40. This solution was mixed with a 5% aqueous solution of polyvinyl alcohol (PVA) so that the ratio of silicon atom content (a parts by mass) to PVA content (b parts by mass) was 70 / 30 by mass to obtain an overcoat coating solution. This overcoat coating solution was applied onto the vapor-deposited layer by gravure coating to form an overcoat layer with a thickness of 320 nm (dry film thickness). In this way, a laminate was obtained.
[0113] (2) Measurement and evaluation (2.1) Measurement of elastic modulus For each of the above laminates, the elastic modulus of the anchor coat layer and the overcoat layer was measured by the following method.
[0114] First, corona treatment was performed on both sides of the laminate at 0.20kW. A corona treatment machine CT-0212 manufactured by Kasuga Electric Co., Ltd. was used for the corona treatment.
[0115] Next, a razor was used to cut out strip-shaped film pieces from the laminate, each with a base length of 1.00 mm and a height of 5.0 mm. These film pieces were embedded in embedding resin. Toagosei's D-800 photocurable resin was used as the embedding resin. The resin in which the film pieces were embedded was cured by light irradiation using a halogen lamp KTX-100R.
[0116] The composite, consisting of a film piece and a cured embedding resin, was fixed using an insert for an atomic force microscope (AFM) sample holder. Next, trimming and cutting were performed on this composite at room temperature (25°C) using a glass knife. This cutting was carried out to expose the cross-section of the film piece. Subsequently, further cutting was performed on this composite at a low temperature (-120°C) using a diamond knife. This cutting was carried out at a cutting speed of 1.0 mm / s and a cutting thickness of 100 nm until the previously cut surface became mirror-like. Leica's ultramicrotome EM UC7 and cryosystem EM FC7 were used as cross-sectional cutting equipment. The cutting direction was parallel to the interface of the layer contained in the film piece.
[0117] As described above, samples for force curve measurement were obtained. Two force curve measurement samples were prepared for each laminate. Each of these samples was fixed in an AFM sample holder insert and used for the following force curve measurements.
[0118] For force curve measurements, we used an MFP-3D-SA atomic force microscope (AFM) manufactured by Oxford Instruments. For the cantilever, we used a nanotools B20-NCH, which is specifically designed for force curve measurements.
[0119] To measure the modulus of elasticity, shape measurements were first performed using these methods. Next, force curves were acquired by specifying the measurement points, and the modulus of elasticity was calculated by analyzing the force curves. Igor Pro 3.8801 was used as the analysis software. For the calculation of the modulus of elasticity, the bottom 10% to top 90% of the indentation depth data during indentation from the force curve data was used, and the Hertz model analysis method was employed.
[0120] Here, the radius of curvature was calculated using the value provided by nanotools, a cantilever manufacturer. The spring constant was calculated using the thermal method. As a result, the spring constant was 42.95 N / m.
[0121] Shape measurements were performed using an AFM and Igor Pro 6.38801 from Oxford Instruments, with the following measurement conditions. Imaging Mode AC mode(tapping mode) Scan Points 256 Scan Lines 256 Scan Rate 1.0Hz Scan size 5.0μm~0.5μm.
[0122] Force curve measurements were performed using an Oxford Instruments AFM and Igor Pro6.38801, with the following measurement conditions. Imaging Mode Off Mode Force Distance 0.1μm Scan Rate 0.25Hz Velocity 50nm / s Sample Rate 8kHz (8.333kHz) Low-pass filter 4kHz (4.167kHz) Trigger Channel Force200nN The temperature at the sample placement site during measurement was 28°C.
[0123] When calculating the modulus of elasticity from the force curve in the Hertz model, the following settings were made in Igor Pro 6.38801.
[0124] Tip Radius (curvature radius) 21nm Geometry Sphere Sample Poisson ratio: 0.33 Tip Properties Diamond Synthetic Segment EXT (force curve when pressed).
[0125] Axial stiffness S of the overcoat layer O To obtain this, first, the force curve described above was obtained at 20 locations on the overcoat layer of each sample. Next, the elastic modulus was calculated for each measurement location for each sample, and these were arithmetic mean. to Thickness of the overcoat layer Multiply by This allowed us to obtain the axial stiffness of the overcoat layer. The thickness of the overcoat layer was determined from the shape image obtained in the shape measurement described above. For each laminate, the arithmetic mean of the axial stiffness obtained for two samples was calculated. This arithmetic mean was given as the axial stiffness S of the overcoat layer. O It was obtained as such.
[0126] Furthermore, the axial stiffness S of the anchor coat layer A To obtain this, first, the force curve described above was acquired at 20 locations on the anchor coat layer of each sample. Next, the elastic modulus was calculated for each measurement location for each sample, and these were arithmetic mean. to Thickness of the anchor coat layer Multiply by This allowed us to obtain the axial stiffness of the anchor coat layer. The thickness of the anchor coat layer was determined from the shape image obtained in the shape measurement described above. For each laminate, the arithmetic mean of the axial stiffness obtained for two samples was calculated. This arithmetic mean was used to determine the axial stiffness S of the anchor coat layer.A It was obtained as such.
[0127] (2.2) Evaluation (2.2.1) Oxygen barrier properties after retort processing test Three-side-seal bags were made from each of the above laminates, each bag was filled with water, and then the opening was heat-sealed to obtain packaged articles. Each packaged article was subjected to retort processing, and then film pieces were cut from them. The oxygen transmission rate (OTR) of each film piece was then measured at 30°C and 70% relative humidity. An oxygen permeability analyzer (OXTRAN-2 / 20, manufactured by MOCON) was used for this measurement.
[0128] (2.2.2) Oxygen barrier properties after the Gelboflex test Film pieces were cut from the laminate described above, and each of these film pieces was bent 10 times using a gel flex tester. Then, the oxygen transmission rate (OTR) of each film piece was measured at 30°C and 70% relative humidity. An oxygen permeability analyzer (MOCON OXTRAN-2 / 20) was used for this measurement.
[0129] (3) Results The results of the above measurements, along with the composition of each laminate, are summarized in Table 1 below. In Table 1, "AC layer" represents the anchor coat layer, and "OC layer" represents the overcoat layer.
[0130] [Table 1]
[0131] As shown in Table 1, the axial stiffness S of the overcoat layer O and the axial stiffness S of the anchor coat layer A The ratio S O / S ALaminates with a value within the range of 2 to 13 exhibited excellent oxygen barrier properties after both the retort treatment test and the Gelboflex test. In contrast, the laminates according to the comparative example exhibited poor oxygen barrier properties after either the retort treatment test or the Gelboflex test. [Explanation of symbols]
[0132] 1...Packaging material, 10...Laminate, 11...Base material, 11A...Core layer, 11B1...Skin layer, 11B2...Skin layer, 12...Anchor coat layer, 13...Vaporized layer, 14...Overcoat layer, 20...Base material layer, 30...Sealant layer, 40A...Adhesive layer, 40B...Adhesive layer.
Claims
1. The material comprises a polypropylene substrate, an anchor coat layer, a vapor-deposited layer made of an inorganic compound, and a resin-containing overcoat layer in this order, wherein one side of the vapor-deposited layer is in contact with the anchor coat layer and the other side is in contact with the overcoat layer, and the axial rigidity S of the overcoat layer O and the axial stiffness S of the anchor coat layer A The ratio S O / S A The range is between 2 and 13. The anchor coat layer contains the reaction product of acrylic polyol, tolylene diisocyanate, and hexamethylene diisocyanate. The overcoat layer has a thickness of 0.1 μm or more and 350 nm or less, and further contains a reaction product of at least one of an alkoxide and a silane coupling agent, and the resin contained in the overcoat layer is a water-soluble polymer having hydroxyl groups.
2. The laminate according to claim 1, wherein the anchor coat layer has a thickness of 0.1 μm or more and 1 μm or less.
3. The laminate according to claim 1, wherein the reaction product is a silicon-containing oxide, and in the overcoat layer, the ratio of the amount of silicon to the total amount of silicon and the water-soluble polymer is in the range of 9 to 90% by mass.
4. The laminate according to claim 1, wherein the vapor-deposited layer comprises at least one of aluminum oxide and silicon oxide.
5. A packaging material comprising a laminate according to any one of claims 1 to 4 and a sealant layer.
6. A package containing the packaging material described in claim 5.
7. A packaged article comprising a packaging body according to claim 6 and an article contained in the packaging body.
Citation Information
Patent Citations
Gas barrier film and method for producing the same
JP2021138057A
Barrier laminate, heat-sealable laminate assembled with barrier laminate, and packaging container assembled with heat-sealable laminate
JP2021151791A
Gas barrier laminate and packaging bag
WO2021220977A1