Biaxially oriented laminated polypropylene film and release film

The biaxially oriented laminated polypropylene film addresses release and winding issues by controlling peel force and surface texture, ensuring stable film rolling and effective adhesion, using a branched polypropylene surface layer for optimal performance.

JP7947939B2Active Publication Date: 2026-11-11TORAY INDUSTRIES INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022188886
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-22
Filing Date
2022-11-28
Publication Date
2026-11-11
Estimated Expiration
2042-11-28

AI Technical Summary

Technical Problem

Existing biaxially oriented laminated polypropylene films suffer from insufficient release properties and winding issues due to inadequate surface roughness, leading to excessive adhesion, wrinkling, and misalignment during film rolling.

Method used

A biaxially oriented laminated polypropylene film with controlled peel force, minimum autocorrelation length (Sal), and surface texture parameters, including a surface layer containing 10-30% branched polypropylene, to achieve optimal release and winding properties.

Benefits of technology

The film exhibits excellent release properties and winding characteristics, preventing damage to adherends and stabilizing film behavior during rolling, with improved slipperiness and reduced wrinkling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007947939000001
    Figure 0007947939000001
Patent Text Reader

Abstract

To provide a biaxially-oriented laminated polypropylene film with excellent releasability and windability.SOLUTION: A biaxially-oriented laminated polypropylene film has at least one face with a peeling force of 1.0 N or more and 2.2 N or less; at least one face with a minimum self-correlation length (Sal) of 41 μm or more and 100 μm or less; and a Sal difference between both faces of 5 μm or more and 40 μm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a biaxially oriented laminated polypropylene film excellent in releasability and winding property, and a release film using the same. BACKGROUND ART

[0002] Polypropylene films such as biaxially oriented laminated polypropylene films are excellent in various properties such as transparency, mechanical properties and electrical properties, and thus are used in various applications including packaging applications, release applications, tape applications, and electrical applications including cable wrapping and capacitors. In particular, due to their excellent surface peeling properties and mechanical properties, they are suitably used as release films and process films for various members such as plastic products, building materials and optical members.

[0003] In recent years, polypropylene films are sometimes used as cover films for adhesive resin layers such as photosensitive resin layers. When a polypropylene film is used as such a cover film, if the releasability is poor, the polypropylene film cannot be peeled off cleanly from the adherend, which may cause the shape of the resin layer of the adherend to change or leave peeling marks on the resin layer of the adherend. To solve such problems, a method is used to improve the releasability by roughening the film surface to reduce the contact area with the resin layer. On the other hand, increasing the roughness of the cover film surface tends to form coarse protrusions, and the surface irregularities of the cover film caused by the coarse protrusions may be transferred to the resin layer of the adherend, affecting the visibility and the like of the product.

[0004] In view of the above, in fields such as optical members that have high required properties for releasability and surface uniformity, in order to use a polypropylene film as a release film, it is required to have a uniformly and finely roughened surface with few coarse protrusions. As a means for obtaining such a polypropylene film having a dense rough surface, for example, the following methods are known.

[0005] Patent Document 1 describes an example in which low-melting-point polypropylene is added to the surface of a polypropylene film and stretched at a temperature above its melting point, causing partial melting and roughening of the surface, thereby improving release properties and quality. Patent Documents 2 to 5 describe an example in which a dense, rough surface is created by using a high-melting-point polypropylene resin in the main layer of a polypropylene film, thereby improving surface smoothness and release properties. Furthermore, Patent Document 6 describes an example in which a β-crystal nucleating agent is added to the surface layer to roughen the film surface even more than in the examples of Patent Documents 2 to 5, thereby improving release properties. Patent Documents 1 to 6 all describe an example in which the size of craters on the film surface is controlled by adjusting the degree of formation of β-crystal spherulites, one of the crystalline forms of polypropylene, during stretching, thereby improving release properties, quality, and process transportability. [Prior art documents] [Patent Documents]

[0006] [Patent Document 1] International Publication No. 2020 / 071291 [Patent Document 2] International Publication No. 2018 / 147334 [Patent Document 3] International Publication No. 2017 / 169952 [Patent Document 4] Japanese Patent Publication No. 2020-132877 [Patent Document 5] Japanese Patent Publication No. 2021-20472 [Patent Document 6] International Publication No. 2016 / 006578 [Overview of the Initiative] [Problems that the invention aims to solve]

[0007] However, the methods described in Patent Documents 1 to 5 mentioned above had insufficient surface roughness of the polypropylene film, resulting in problems with release properties, transportability, and winding properties. More specifically, in the method described in Patent Document 1, when used as a release film, the smooth surface adhered excessively strongly to the adherend, resulting in insufficient release properties. In addition, the flexible surface formed by low-melting-point polypropylene resin, etc., caused wrinkles to form when the laminated films were wound into a roll because they did not slide against each other. In the methods described in Patent Documents 2 to 6, the surface, which has densely arranged sharp protrusions formed by highly stereoregular polypropylene resin, etc., came into contact with the adherend. As the protrusions dug into the adherend, the polypropylene film and adherend adhered strongly, resulting in insufficient release properties.

[0008] Therefore, the object of the present invention is to solve the above-mentioned problems. In other words, the object of the present invention is to provide a biaxially oriented laminated polypropylene film with excellent release properties and winding properties. [Means for solving the problem]

[0009] To solve the above-mentioned problems, the biaxially oriented laminated polypropylene film of the present invention has the following configuration. Specifically, the biaxially oriented laminated polypropylene film of the present invention is characterized in that the peel force of at least one surface is 1.0 N or more and 2.2 N or less, the minimum autocorrelation length (Sal) of at least one surface is 41 μm or more and 100 μm or less, and the difference in Sal between both surfaces is 5 μm or more and 40 μm or less.

[0010] Furthermore, the biaxially oriented laminated polypropylene film of the present invention can also be in the following forms and can be suitably used as a release film. (1) A biaxially oriented laminated polypropylene film characterized in that the peel force of at least one surface is 1.0 N or more and 2.2 N or less, the minimum autocorrelation length (Sal) of at least one surface is 41 μm or more and 100 μm or less, and the difference in Sal between both surfaces is 5 μm or more and 40 μm or less. (2) The biaxially oriented laminated polypropylene film according to (1), wherein the arithmetic mean height (Sa) of at least one surface is 80 nm or more and 700 nm or less, and the difference in Sa between the two surfaces is 50 nm or more and 400 nm or less. (3) The biaxially oriented laminated polypropylene film according to (1) or (2), wherein the aspect ratio (Str) of the surface properties of at least one of the faces is 0.40 or more and 0.90 or less. (4) A biaxially oriented laminated polypropylene film according to any one of (1) to (3), having a surface layer (layer A) and a base layer (layer B), wherein layer A, layer B, and layer A are located in this order, and layer A contains 10% by mass or more and 30% by mass or less of branched polypropylene. (5) A biaxially oriented laminated polypropylene film according to any of (1) to (4), wherein the static friction coefficient (μs) and the kinetic friction coefficient (μd), measured by bringing one surface into contact with the opposite surface, are both 0.40 or more and 0.55 or less. (6) A release film made using a biaxially oriented laminated polypropylene film as described in any of (1) to (5). [Effects of the Invention]

[0011] The present invention provides a biaxially oriented laminated polypropylene film that has excellent release properties and winding properties, and can be suitably used as a release film. [Modes for carrying out the invention]

[0012] The biaxially oriented laminated polypropylene film of the present invention is characterized in that the peel strength of at least one side is 1.0 N or more and 2.2 N or less, the minimum autocorrelation length (Sal) of at least one side is 41 μm or more and 100 μm or less, and the difference in Sal between both sides is 5 μm or more and 40 μm or less. The biaxially oriented laminated polypropylene film of the present invention will be described in detail below.

[0013] A polypropylene film refers to a sheet-like molded article whose main component is polypropylene resin. The main component refers to the component that is present in an amount greater than 50% by mass and less than or equal to 100% by mass when the total constituent components of the object (in this case, the film) are set to 100% by mass, and the same interpretation can be applied to the main component hereafter. If multiple components that correspond to polypropylene resin are present, the product is considered to have polypropylene resin as its main component if their total amount is greater than 50% by mass. A polypropylene resin refers to a resin whose main constituent unit is the propylene unit, and the main constituent unit refers to the constituent unit that is present in an amount greater than 50 mol% and less than or equal to 100 mol% when the total constituent units are set to 100 mol% (this definition can be applied to other olefin resins as well, except that the propylene unit is replaced by other olefin units). Biaxial orientation refers to having molecular orientation in two orthogonal directions, and can be achieved by stretching an unstretched sheet in two orthogonal directions (usually the longitudinal and width directions). Lamination refers to the stacking of two or more layers with different compositions in the thickness direction.

[0014] From the viewpoint of release properties, the biaxially oriented laminated polypropylene film of the present invention is important in that the peel force of at least one side is 1.0 N or more and 2.2 N or less, the minimum autocorrelation length (Sal) of at least one side is 41 μm or more and 100 μm or less, and the difference in Sal between both sides is 5 μm or more and 40 μm or less. Note that the "peel force of 1.0 N or more and 2.2 N or less" and the "minimum autocorrelation length (Sal) of 41 μm or more and 100 μm or less" only need to be satisfied on at least one side, and it is not necessarily required that both sides be satisfied simultaneously. However, from the viewpoint of release properties, it is preferable that both sides be satisfied simultaneously on the same side, and more preferable that both sides be satisfied simultaneously.

[0015] Peel force refers to the force (N) measured when peeling a polyester adhesive tape under the conditions of a peeling speed of 300 mm / min and a peeling angle of 180°, after one surface of a biaxially oriented laminated polypropylene film is laminated with a polyester adhesive tape having a tape width of 19 mm. Here, as the polyester adhesive tape, Polyester Adhesive Tape No.31B manufactured by Nitto Denko Corporation, or a polyester adhesive tape having an adhesive strength equivalent thereto shall be used.

[0016] The minimum autocorrelation length (Sal) is one of the three-dimensional parameters of surface texture, and is a parameter that serves as an indicator of the in-plane period of the surface texture. More specifically, the autocorrelation length (Sal) is the horizontal distance in the direction in which the autocorrelation function specified in ISO 25178-2 (2012) attenuates the fastest to a specific value s (s=0.2 in the present invention). A small value of the minimum autocorrelation length (Sal) indicates that the surface has finer (shorter-period) irregular shapes in the in-plane direction, while a large value of the minimum autocorrelation length (Sal) indicates that the surface has coarser (longer-period) irregular shapes in the in-plane direction. Hereinafter, "minimum autocorrelation length Sal" and "difference in Sal between both surfaces" may be simply referred to as "Sal" and "Sal difference", respectively. By adopting an embodiment in which the Sal of at least one surface is 41 μm or more and 100 μm or less, excellent releasability and winding property can be achieved when the corresponding surface of the biaxially oriented laminated polypropylene film is bonded so as to be in contact with an adherend.

[0017] Sal, the arithmetic mean height Sa described later, and the surface texture aspect ratio Str can be measured using a known layer cross-sectional shape measuring apparatus. As the measuring apparatus, for example, a non-contact surface / layer cross-sectional shape measuring system "VertScan" (registered trademark) 2.0 manufactured by Ryoka Systems Inc. can be used. A specific method for measuring these parameters using the same apparatus will be described later.

[0018] The biaxially oriented laminated polypropylene film of the present invention has a peel force of at least one surface of 1.0 N or more and 2.2 N or less, preferably 1.2 N or more and 2.0 N or less, from the viewpoints of releasability and winding property. Similarly, Sal is 41 μm or more and 100 μm or less, preferably 43 μm or more and 90 μm or less, more preferably 45 μm or more and 85 μm or less on at least one surface. It is preferable that the peel force and Sal simultaneously fall within the above ranges on one surface. The Sal difference is 5 μm or more and 40 μm or less, preferably 6 μm or more and 35 μm or less.

[0019] When a biaxially oriented laminated polypropylene film that does not have a surface with each of the above parameters falling within the above ranges is used as a release film, various problems in terms of releasability occur as described below. If the peel force of the surface to be laminated to an adherend (hereinafter sometimes referred to as the X-surface; an embodiment in which both surfaces are X-surfaces is also possible) is less than 1.0 N, the adhesion force is insufficient when laminating the adherend and the biaxially oriented laminated polypropylene film, which may cause peeling during the conveyance process. On the other hand, if the peel force of the X-surface exceeds 2.2 N, the adherend and the biaxially oriented laminated polypropylene film adhere excessively strongly. If the adhesion between the two becomes excessively strong, when the biaxially oriented laminated polypropylene film is peeled from the adherend, the biaxially oriented laminated polypropylene film may pull and peel off part of the surface of the adherend, or break the adherend.

[0020] Furthermore, if the Salt of both the X-surface and the opposite surface is less than 41 μm, problems arise due to the excessively small size of the protrusions on the surface of the biaxially oriented laminated polypropylene film. Specifically, if the Salt of the X-surface is less than 41 μm, the protrusions tend to dig into the adherend, causing the X-surface and adherend to adherend to be excessively tight. When peeling the biaxially oriented laminated polypropylene film from the adherend, this can result in partial peeling of the adherend, indentations from the protrusions remaining on the adherend surface, or even fracture of the adherend. Also, if the Salt of the opposite surface is less than 41 μm, the protrusions on the surfaces that come into contact when the biaxially oriented laminated polypropylene film is wound into a roll do not interfere with each other. This causes the biaxially oriented laminated polypropylene film to slip excessively during the winding process, leading to misalignment of the film roll.

[0021] On the other hand, if the Sal (salt) of both the X-surface and the opposite surface exceeds 100 μm, problems arise due to the excessively large size of the protrusions on the surface of the biaxially oriented laminated polypropylene film. Specifically, if the Sal (salt) of the X-surface exceeds 100 μm, the protrusion size becomes excessively large and the surface becomes smoother, which can cause the X-surface to adhere strongly to the adherend, resulting in poor release properties. Furthermore, if the Sal (salt) of the opposite surface exceeds 100 μm, the protrusions on the surfaces that come into contact when the biaxially oriented laminated polypropylene film is wound into a roll interfere excessively with each other, reducing the slipperiness of the film during lamination and causing wrinkles in the film roll.

[0022] Furthermore, if the difference in Sal on both sides of a biaxially oriented laminated polypropylene film is less than 5 μm, the lack of a difference in protrusion size between the front and back sides can result in poor slipperiness, which may make it more prone to wrinkling when rolled up. On the other hand, if the difference in Sal on both sides of a biaxially oriented laminated polypropylene film exceeds 40 μm, the difference in protrusion size between the front and back sides is maximized, resulting in high slipperiness, which may cause the films to slip against each other when rolled up, potentially leading to misalignment in the width direction.

[0023] In other words, the biaxially oriented laminated polypropylene film of the present invention has a peel force of 1.0 N to 2.2 N on at least one side, a Sal content of 41 μm to 100 μm on at least one side, and a Sal content difference of 5 μm to 40 μm on both sides, thereby reducing damage to the adherend and stabilizing the film's behavior during roll winding. As a result, it exhibits excellent release properties and winding characteristics, making it suitable for use as a release film.

[0024] To ensure that the peel force and Sal on at least one side, and the difference in Sal between both sides, are within the above range, it is effective to set the raw material composition and film-forming conditions of the biaxially oriented laminated polypropylene film within the range described below. More specifically, by using a resin composition containing a preferred amount of branched-chain polypropylene resin (described below) to form the surface layer, or both the surface layer and the base layer (the film itself in the case of a single-layer film), and setting the surface temperature of the casting drum within the preferred range described below, and setting the film temperature (preheating temperature) when stretching in the longitudinal direction within the range described below, the peel force, Sal, and Sal difference can be controlled to a preferred range. Here, the longitudinal direction refers to the direction in which the film travels during the film manufacturing process, and when it becomes a film roll, it refers to its winding direction. The direction perpendicular to the longitudinal direction within the film surface is called the width direction.

[0025] The biaxially oriented laminated polypropylene film of the present invention has no particular limitations as long as the peel force of at least one side is 1.0 N or more and 2.2 N or less, the Sal of at least one side is 41 μm or more and 100 μm or less, and the difference in Sal between both sides is 5 μm or more and 40 μm or less. However, from the viewpoint of release properties and winding properties, it is more preferable that there is a side in which both the peel force and Sal are within the above ranges. Furthermore, considering the suppression of dent transfer on the back side and the improvement of the transportability and winding properties of the biaxially oriented laminated polypropylene film itself, it is even more preferable that both sides have peel force and Sal within the above ranges.

[0026] The biaxially oriented laminated polypropylene film of the present invention preferably has an arithmetic mean height (Sa) of 80 nm to 700 nm on at least one surface, more preferably 150 nm to 650 nm, and even more preferably 250 nm to 600 nm, from the viewpoint of reducing damage to the adherend and improving the transportability and winding properties of the film. Also, from the same viewpoint, the difference in Sa between both surfaces is preferably 50 nm to 400 nm, and more preferably 55 nm to 350 nm. Hereinafter, "arithmetic mean height Sa" and "difference in Sa between both surfaces" may simply be referred to as "Sa" and "Sa difference".

[0027] The arithmetic mean height (Sa) is one of the three-dimensional parameters of surface texture as defined in ISO 25178-2 (2012). It represents the average of the absolute differences in heights at each point relative to the average height of the surface.

[0028] By having Sa of 80 nm or more on at least one, preferably both, of the X-plane and the opposite plane, the adhesion force between the adherend and the biaxially oriented laminated polypropylene film is not excessively large, thereby improving release properties. This prevents the biaxially oriented laminated polypropylene film from pulling and peeling off a portion of the adherend surface, and also suppresses dents on the adherend surface. Furthermore, the roughened surface that comes into contact when the film is wound into a roll allows for moderate slippage, and the stiffness of the film naturally alleviates wrinkles that occur during the conveying process and between the roll layers, improving winding performance.

[0029] On the other hand, if the Sa of at least one, preferably both, of the X-surface and the opposite surface is 700 nm or less, it is possible to prevent insufficient adhesion when bonding the adherend and the biaxially oriented laminated polypropylene film, which would otherwise peel off during the transport process. Furthermore, the contact surface when wound into a roll does not become excessively rough, the film is appropriately fixed as it is being laminated into a roll, and winding misalignment can be suppressed.

[0030] Furthermore, an Sa difference of 50 nm or more allows the films to slide appropriately against each other when wound into a roll, suppressing the occurrence of wrinkles. On the other hand, an Sa difference of 400 nm or less suppresses excessive sliding between the films when wound into a roll, preventing misalignment in the width direction.

[0031] To ensure that the Sa of at least one side is in the range of 80 nm to 700 nm, it is effective to set the raw material composition of the film within the range described later, and to set the film-forming conditions within the range described later. More specifically, a method similar to the method for controlling the peel force, Sal, and Sal difference within a preferred range can be used. Furthermore, from the viewpoint of suppressing dent transfer on the back surface and the transportability and winding properties of the film, it is preferable that the Sa of both sides of the biaxially oriented laminated polypropylene film be 80 nm to 700 nm, more preferably 150 nm to 650 nm, and even more preferably 250 nm to 600 nm. Also, from a similar viewpoint, it is preferable that the Sa difference be 55 nm to 350 nm, and more preferably 60 nm to 300 nm.

[0032] The biaxially oriented laminated polypropylene film of the present invention preferably has a surface aspect ratio Str of 0.40 or more and 0.90 or less on at least one surface, and more preferably 0.45 or more and 0.85 or less, from the viewpoint of improving release properties, transportability, and winding properties. Hereinafter, "surface aspect ratio Str" may be simply referred to as "Str".

[0033] Str is one of the three-dimensional parameters of surface properties and is used as an indicator of the isotropy of the surface properties. More specifically, Str is the value obtained by dividing the horizontal distance in the direction in which the autocorrelation function defined in ISO 25178-2 (2012) decays fastest to a specific value s (s=0.2 in this invention) (corresponding to the aforementioned Sal) by the horizontal distance in the direction in which it decays slowest to the value s. In other words, theoretically, the Str of a biaxially oriented laminated polypropylene film will be a value between 0 and 1. A Str close to 0 means that the biaxially oriented laminated polypropylene film has a highly anisotropic, regular pattern of surface properties, while a Str close to 1 means that the biaxially oriented laminated polypropylene film has a highly isotropic, random pattern of surface properties.

[0034] In a biaxially oriented laminated polypropylene film, having an Str value of 0.40 or higher on the X-side results in a surface texture that exhibits a moderately anisotropic random pattern. Therefore, when the adherend and the biaxially oriented laminated polypropylene film are bonded together on this surface, unevenness in adhesion is suppressed, improving release properties. This prevents the biaxially oriented laminated polypropylene film from pulling and peeling off parts of the adherend surface, and also suppresses dents on the adherend surface. Furthermore, by setting the Str value to 0.40 or higher on at least one side of the biaxially oriented laminated polypropylene film, trapped air can be moderately removed when the film is wound into a roll. This naturally reduces wrinkles generated during the transport process and wrinkles between roll layers due to the film's own stiffness, improving winding performance. On the other hand, if the Str value is 0.90 or less on at least one surface of the biaxially oriented laminated polypropylene film, a moderate degree of uneven adhesion remains when the adherend and the biaxially oriented laminated polypropylene film are bonded to the adherend, thereby reducing delamination of the two during the transport process and improving release properties. From the above viewpoint, it is preferable that the Str value is 0.40 or more and 0.90 or less or within the above preferred range on the X-surface, and more preferable that it is 0.40 or more and 0.90 or less or within the above preferred range on both sides.

[0035] To set the Str of at least one face to a value within the above range, it is effective to set the raw material composition and film-forming conditions of the biaxially oriented laminated polypropylene film to the range described later. More specifically, a method similar to the method for controlling the peel force, Sal, and Sal difference to a preferred range can be used.

[0036] The biaxially oriented laminated polypropylene film of the present invention has a surface layer (layer A) and a base layer (layer B) from the viewpoint of achieving both heat resistance and release properties, wherein layer A, layer B, and layer A are arranged in this order, and it is preferable that layer A contains 10% to 30% by mass of branched polypropylene. "Layer A contains 10% to 30% by mass of branched polypropylene" means that when the total components constituting layer A are taken as 100% by mass, the content of branched polypropylene in layer A is 10% to 30% by mass. From the above viewpoint, the amount of branched polypropylene in layer A is more preferably 13% to 27% by mass, and even more preferably 16% to 24% by mass. "Layer A contains 10% to 30% by mass of branched polypropylene" means that at least one of the layers A contains 10% to 30% by mass of branched polypropylene, but it is more preferable that both layers A contain 10% to 30% by mass of branched polypropylene.

[0037] Furthermore, in the biaxially oriented laminated polypropylene film of the present invention, from the viewpoint of controllability of surface roughness, branched-chain polypropylene may also be included in layer B, within a range lower than the branched-chain polypropylene content (mass%) in layer A. When layer B contains branched-chain polypropylene, it is preferably 15% by mass or less, more preferably 10% by mass or less, even more preferably 5.0% by mass or less, and particularly preferably 2.5% by mass or less, when the total components constituting layer B are taken as 100% by mass.

[0038] The branched-chain polypropylene referred to here is a polypropylene resin that has five or fewer internally trisubstituted propylene atoms per 10,000 carbon atoms in its molecular chain, and the presence of these internally trisubstituted propylene atoms is significant.1 This can be confirmed by the proton ratio in the 1H-NMR spectrum.

[0039] By adopting this configuration, it is possible to provide a layer (layer B) that plays a role in ensuring the thermal dimensional stability of the biaxially oriented laminated polypropylene film, and a layer (layer A) that plays a role in achieving excellent release properties when bonded to an adherend. This makes it easy to produce a biaxially oriented laminated polypropylene film that combines heat resistance and release properties.

[0040] Furthermore, by including 10% by mass or more of branched polypropylene in layer A, the size of the spherulites generated during the cooling process of the melt-extruded polypropylene resin can be increased, resulting in a biaxially oriented laminated polypropylene film with excellent release properties. On the other hand, by including 30% by mass or less of branched polypropylene in layer A, the size of the spherulites generated during the cooling process of the melt-extruded polypropylene resin does not become excessively large. As a result, the height of the protrusions does not become excessively high, and the adherend can be peeled off the surface of layer A (corresponding to the X surface mentioned above) without damaging the adherend.

[0041] Furthermore, by including branched polypropylene in layer B, more protrusions can be formed from within. This allows the surface of the biaxially oriented laminated polypropylene film to be moderately dense and rough, enabling broader control over surface roughness. On the other hand, if there is an excess of branched polypropylene in layer B, excessive protrusion formation occurs, causing the surface of the biaxially oriented laminated polypropylene film to become smoother, beyond a moderately dense and rough surface, and worsening its release properties. By limiting the branched polypropylene content in layer B to 15% by mass or less, the smoothing due to the above mechanism is suppressed, making it easier to produce a biaxially oriented laminated polypropylene film with excellent release properties, and also reducing winding misalignment due to poor slipperiness.

[0042] Furthermore, in order to reduce problems such as meandering and wrinkling during film transport, winding, and unwinding, the biaxially oriented laminated polypropylene film of the present invention preferably has a static friction coefficient (μs) and a dynamic friction coefficient (μd) of 0.40 or more and 0.55 or less, measured by bringing one surface into contact with the opposite surface, and more preferably both are 0.42 or more and 0.53 or less. The static friction coefficient and dynamic friction coefficient referred to here are values ​​calculated using the following formula from the maximum resistance value at the moment the upper film starts to slide and the resistance value during the sliding, when films are stacked so that different surfaces are in contact with each other in an environment with a temperature of 23±3℃ and a humidity of 65±5%, a load of 200g is applied from above, and the upper film is slid. Hereinafter, "static friction coefficient (μs)" and "dynamic friction coefficient (μd)" may be collectively referred to as friction coefficients, and both can be calculated using the following formula. Coefficient of friction = resistance (g) / load (g) Equation (1).

[0043] A friction coefficient of 0.40 or higher for biaxially oriented laminated polypropylene film ensures a certain degree of slipperiness, which reduces problems such as wrinkles forming in the film during transport and winding, thus leading to a more stable winding. On the other hand, a friction coefficient of 0.55 or lower prevents excessive slipperiness, reducing meandering and winding misalignment that can occur when winding biaxially oriented laminated polypropylene film as a roll.

[0044] The coefficient of friction can be adjusted, for example, by adjusting Sa, and more specifically, by lowering Sa, the coefficient of friction can be increased. The method for adjusting Sa is as described above.

[0045] Next, the layer structure and raw materials of the biaxially oriented laminated polypropylene film of the present invention will be described, but the layer structure and raw materials of the biaxially oriented laminated polypropylene film of the present invention are not necessarily limited to those described herein.

[0046] The biaxially oriented laminated polypropylene film of the present invention preferably has a polypropylene resin content of 95% by mass or more and 100% by mass or less, more preferably 96% by mass or more and 100% by mass or less, even more preferably 97% by mass or more and 100% by mass or less, and particularly preferably 98% by mass or more and 100% by mass or less, when the total components constituting the film are taken as 100% by mass.

[0047] The film thickness of the biaxially oriented laminated polypropylene film of the present invention is not particularly limited, but from the viewpoint of handling, it is preferably 1 μm to 100 μm, more preferably 5 μm to 50 μm, and even more preferably 10 μm to 30 μm. The film thickness can be measured with a known electronic micrometer (details will be described later) and can be adjusted by the screw rotation speed of the extruder, the width of the unstretched sheet, the film formation speed, the stretching ratio, etc.

[0048] The main component of the base layer (layer B) of the biaxially oriented laminated polypropylene film of the present invention is preferably a polypropylene resin. Hereinafter, the polypropylene resin that is the main component of the base layer (layer B) of the biaxially oriented laminated polypropylene film may be referred to as polypropylene resin I. The polypropylene resin I of the base layer (layer B) is more preferably 90% by mass or more and 100% by mass or less, even more preferably 95% by mass or more and 100% by mass or less, even more preferably 96% by mass or more and 100% by mass or less, particularly preferably 97% by mass or more and 100% by mass or less, and most preferably 98% by mass or more and 100% by mass or less.

[0049] In the biaxially oriented laminated polypropylene film of the present invention, homopolypropylene is preferred for the polypropylene resin I from the viewpoint of strength and heat resistance. Homopolypropylene refers to a polypropylene resin in which, when the total constituent units of the resin are set to 100 mol%, 99 mol% to 100 mol% are propylene units.

[0050] The polypropylene resin I preferably has a melting point of 155°C or higher, and more preferably 160°C or higher. A melting point of 155°C or higher improves the heat resistance of the biaxially oriented laminated polypropylene film. Therefore, when the biaxially oriented laminated polypropylene film is used, for example, as a release film, softening of the biaxially oriented laminated polypropylene film and elongation in the tensile direction due to softening during the heat-applied process after bonding with the adherend are suppressed, and deformation of the adherend is reduced. Furthermore, the melting point is preferably 200°C or lower, more preferably 190°C or lower, and even more preferably 180°C or lower. A melting point of 200°C or lower for the polypropylene resin I makes it less likely for equipment constraints to occur during melt extrusion.

[0051] The mesopentad fraction of polypropylene resin I is preferably 0.90 or higher, more preferably 0.93 or higher, and even more preferably 0.94 or higher. The mesopentad fraction is an index indicating the stereoregularity of the crystalline phase of polypropylene, as measured by nuclear magnetic resonance (NMR) spectroscopy. Generally, the higher the value, the higher the degree of crystallinity and melting point. Therefore, by using polypropylene with a high mesopentad fraction as polypropylene resin I, the dimensional stability at high temperatures is improved when it is made into a film. There is no particular upper limit specified for the mesopentad fraction, but from the viewpoint of use in film manufacturing, it is set at 0.99.

[0052] To obtain polypropylene with a high mesopentade fraction, methods such as washing the obtained resin powder with a solvent such as n-heptane, or appropriately selecting a catalyst and / or co-catalyst and selecting its composition are preferably employed. Typically, polymerization catalysts containing metallocene compounds having a cyclopentadienyl skeleton in their molecule are preferably used as catalysts.

[0053] Furthermore, from the viewpoint of film-forming properties and strength when formed into a film, the melt flow rate (MFR) of polypropylene resin I is preferably 1 g / 10 min to 10 g / 10 min, more preferably 1 g / 10 min to 8 g / 10 min, and even more preferably 2 g / 10 min to 5 g / 10 min. Here, MFR refers to the MFR measured under conditions of a temperature of 230°C and a load of 21.18 N, and the same applies to MFR hereafter. In order to achieve the above values ​​for the melt flow rate (MFR) of the polypropylene resin, methods such as controlling the average molecular weight and molecular weight distribution are employed. More specifically, the MFR can be increased by reducing the number average or weight average molecular weight and molecular weight distribution.

[0054] Polypropylene resin I may contain copolymer components made of unsaturated hydrocarbons other than the main constituent units, to the extent that it does not impair the objectives of the present invention. Examples of monomers constituting such copolymer components include ethylene, 1-butene, 1-pentene, 3-methylpentene-1, 3-methylbutene-1, 1-hexene, 4-methylpentene-1, 5-ethylhexene-1, 1-octene, 1-decene, 1-dodecene, vinylcyclohexene, styrene, allylbenzene, cyclopentene, norbornene, and 5-methyl-2-norbornene. The copolymerization amount is preferably less than 1 mol% from the viewpoint of dimensional stability when it is made into a film.

[0055] Furthermore, the base layer (layer B) may contain polyolefin resins other than the main component, polypropylene resin I. Here, polyolefin resins other than polypropylene resin I refer to polyolefin resins whose main constituent units differ from those of polypropylene resin I. Examples of the main constituent units of polyolefin resins other than polypropylene resin I include constituent units derived from ethylene, 1-butene, 1-pentene, 3-methylpentene-1, 3-methylbutene-1, 1-hexene, 4-methylpentene-1, 5-ethylhexene-1, 1-octene, 1-decene, 1-dodecene, vinylcyclohexene, styrene, allylbenzene, cyclopentene, norbornene, 5-methyl-2-norbornene, etc. The content of polyolefin resins other than polypropylene resin I is preferably 15% by mass or less, and more preferably 10% by mass or less, when the total components constituting the base layer (layer B) are considered as 100% by mass. Furthermore, the base layer (layer B) may also contain branched polypropylene resin as a polyolefin resin other than polypropylene resin I, from the viewpoint of controlling surface roughness, and the preferred content is as described above.

[0056] When polypropylene resin I is a polypropylene resin and polyethylene is included as a polyolefin resin other than polypropylene resin I, the polyethylene resin contained in the base layer (layer B) is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less. The higher the polyethylene resin content, the lower the crystallinity when it is made into a film, making it easier to improve transparency. On the other hand, by limiting the polyethylene resin content to 10% by mass or less, the decrease in strength and heat resistance when it is made into a film can be reduced, as can the degradation of the resin during the extrusion process and the occurrence of fish eyes when it is made into a film.

[0057] Next, the polypropylene resin used in the surface layer (layer A) of the biaxially oriented laminated polypropylene film of the present invention will be described. From the viewpoint of achieving both heat resistance and release properties, it is preferable to use a resin composition containing branched polypropylene resin in polypropylene resin I for the surface layer (layer A) of the present invention. The branched polypropylene resin in the surface layer (layer A) is preferably 10% to 30% by mass, more preferably 13% to 27% by mass, and even more preferably 16% to 24% by mass of the total components constituting the layer.

[0058] As the branched-chain polypropylene resin, it is preferable to use a polypropylene resin having a branched structure in its molecular chain. A "polypropylene resin having a branched structure in its molecular chain" is defined as a polypropylene resin having five or fewer internally trisubstituted propylene atoms per 10,000 carbon atoms in the molecular chain, and the presence of these internally trisubstituted propylene atoms is important. 1 This can be confirmed by the proton ratio of the 1H-NMR spectrum. Furthermore, the MFR of the branched polypropylene resin is preferably 1.0 g / 10 min to 10.0 g / 10 min from the viewpoint of film formation stability. The same branched polypropylene resin is also preferred for the B layer.

[0059] Examples of branched polypropylene resins that can be suitably used in the surface layer (layer A) or base layer (layer B) of the biaxially oriented laminated polypropylene film of the present invention include "Profax" (registered trademark) (PF-814, etc.) from Lyondell Basell, "Daploy" (trademark) (WB130HMS, WB135HMS, etc.) from Borealis, and "WAYMAX" (registered trademark) (MFX3, MFX6, MFX8, EX6000, EX8000, etc.) from Nippon Polypropylene Co., Ltd.

[0060] Although branched polypropylene resin itself has the effect of nucleating α-crystals or β-crystals, other nucleating agents such as α-crystal nucleating agents (e.g., dibenzylidene sorbitols, sodium benzoate, etc.) and β-crystal nucleating agents (e.g., potassium 1,2-hydroxystearate, magnesium benzoate, amide compounds such as N,N'-dicyclohexyl-2,6-naphthalenedicarboxamide, quinacridone compounds, etc.) may be added to the extent that it does not contradict the purpose of the present invention. These nucleating agents may be added to either the base layer (layer B), the surface layer (layer A), or both.

[0061] However, excessive addition of the above-mentioned other types of nucleating agents may cause a decrease in the stretchability of the film and a decrease in transparency and strength due to void formation, etc. Therefore, the amount added is usually 0.5% by mass or less, preferably 0.1% by mass or less, and more preferably 0.05% by mass or less, when the total components constituting the film are considered to be 100% by mass.

[0062] The biaxially oriented laminated polypropylene film of the present invention may contain various additives, such as antioxidants, heat stabilizers, lubricants, antistatic agents, antiblocking agents, fillers, viscosity modifiers, and color inhibitors, as long as they do not impair the objectives of the present invention. Among these, the selection of the type and amount of antioxidant is important from the viewpoint of antioxidant bleed-out. As such antioxidants, sterically hindered phenolic types are preferred, and when multiple types of antioxidants are used in combination, at least one type with a molecular weight of 500 or more is preferred. Various specific examples can be given, but it is preferable to use 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene (e.g., BASF's "Irganox"® 1330: molecular weight 775.2) or tetrakis[methylene-3(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane (e.g., BASF's "Irganox"® 1010: molecular weight 1177.7) in combination with 2,6-di-t-butyl-p-cresol (BHT: molecular weight 220.4).

[0063] The total content of these antioxidants is preferably in the range of 0.03% to 1.0% by mass, when the total raw materials for obtaining a biaxially oriented laminated polypropylene film are considered as 100% by mass, from the viewpoint of reducing discoloration due to polymer degradation and a decrease in transparency due to antioxidant bleed-out. A antioxidant content of 0.03% by mass or more can reduce film discoloration caused by polymer degradation during the extrusion process and a decrease in long-term heat resistance. On the other hand, a antioxidant content of 1.0% by mass or less suppresses a decrease in transparency due to antioxidant bleed-out. From the above viewpoint, a more preferable antioxidant content is 0.05% to 0.9% by mass, and even more preferably 0.1% to 0.8% by mass. These antioxidants may be added to either the base layer (layer B), the surface layer (layer A), or both.

[0064] Furthermore, it is preferable that the biaxially oriented laminated polypropylene film of the present invention does not contain organic or inorganic particles. For example, the polypropylene resin that can be suitably used in the biaxially oriented laminated polypropylene film of the present invention has low affinity for organic and inorganic particles. As a result, these particles may fall off during the manufacturing process, contaminating the production line or the product, or coarse protrusions formed by hard particles may be transferred as unevenness to the resin layer of the adherend. Therefore, when used as a protective film for optical components or a manufacturing base film for products requiring high quality, such as display components, it is preferable that the biaxially oriented laminated polypropylene film does not contain lubricants such as organic or inorganic particles.

[0065] As a method for biaxial stretching to obtain the biaxially oriented laminated polypropylene film of the present invention, any of the following methods may be employed: simultaneous inflation biaxial stretching, simultaneous stentor biaxial stretching, or sequential stentor biaxial stretching. Among these, sequential stentor biaxial stretching is preferred in terms of controlling film formation stability, thickness uniformity, high rigidity, and dimensional stability of the film. Here, sequential stentor biaxial stretching refers to a method in which stretching in the longitudinal direction and the width direction are performed in separate processes, and at least the stretching in the width direction is performed by a stentor.

[0066] Next, one embodiment of the method for manufacturing the biaxially oriented laminated polypropylene film of the present invention will be described, but is not necessarily limited thereto. First, polypropylene resin I or a mixture of polypropylene resin I and branched polypropylene resin is supplied to a single-screw extruder for the base layer (layer B), and the mixture of polypropylene resin I and branched polypropylene resin is supplied to a single-screw extruder for the surface layer (layer A). Then, melt extrusion is performed at 200°C to 280°C, more preferably 220°C to 280°C, and even more preferably 240°C to 270°C. After removing foreign matter and modified polymers using a filter installed in the middle of the polymer tube, the layers are laminated in an A / B / A layer configuration using a multi-manifold type composite T-die, and the material is discharged onto a casting drum and cooled and solidified to obtain an unstretched sheet.

[0067] In this process, casting is performed in two stages, and the surface temperature of both casting drums is preferably 40°C to 100°C, more preferably 50°C to 100°C, and even more preferably 60°C to 100°C. By keeping the surface temperatures of the two casting drums within the above range, it is possible to create spherulites of an appropriate size, resulting in a biaxially oriented laminated polypropylene film with excellent release properties. Furthermore, it is preferable that the temperatures of the two casting drums are different. In this case, the difference in surface temperature between the two casting drums (surface temperature of the first casting drum - surface temperature of the second casting drum) is preferably 5°C to 60°C, more preferably 10°C to 50°C, and even more preferably 15°C to 40°C. By using two casting drums with a temperature difference, it is possible to create a difference in the size of the spherulites on both sides of the film, improving winding performance.

[0068] Any of the following methods can be used to adhere the film to the casting drum: electrostatic application, adhesion using the surface tension of water, air knife method, press roll method, or underwater casting method. However, the air knife method is preferred from the viewpoint of improving the flatness of the film and facilitating control of surface roughness. The air temperature of the air knife is preferably 40°C to 80°C, and the blown air speed is preferably 130 m / s to 150 m / s. In addition, it is preferable to appropriately adjust the position of the air knife so that the air flows to the downstream side of the film formation in order to prevent vibration of the sheet.

[0069] Next, the obtained unstretched sheet is biaxially stretched and biaxially oriented. The specific stretching and preheating conditions are as follows. The preheating method can be one or a combination of methods such as using a temperature-controlled rotary roll or using a hot air oven. The preheating temperature for both sides of the unstretched film is preferably 130°C to 160°C, more preferably 135°C to 160°C, and even more preferably 140°C to 154°C, considering the viewpoint of controlling the protrusions on the film surface to a desirable range by high-temperature stretching. At this time, it is preferable that the preheating temperatures for both sides of the unstretched film are different, and the difference in preheating temperature between the two sides of the unstretched film is preferably 5°C to 30°C, more preferably 5°C to 20°C, and even more preferably 5°C to 13°C, within the above preferred range. By creating a difference in preheating temperature for both sides of the unstretched film, it is possible to create a difference in the height of the protrusions on both sides, which improves winding performance.

[0070] From the viewpoint of controlling the protrusions on the film surface to a desirable range by high-temperature stretching after preheating under the above conditions, the stretching temperature when stretching in the longitudinal direction is preferably 140°C to 160°C, more preferably 144°C to 158°C, and even more preferably 148°C to 155°C. Also, from the same viewpoint, it is preferable that the stretching temperature in the longitudinal direction be higher than or equal to the preheating temperature of the side with a relatively higher preheating temperature.

[0071] The stretching ratio is preferably 3.0 to 6.0 times, more preferably 4.0 to 5.7 times, and even more preferably 4.5 to 5.5 times, in order to control the mechanical and thermal properties within a desirable range. When the stretching ratio is 3.0 times or higher, more uniform stretching is possible and thickness variations are suppressed. On the other hand, when the stretching ratio is 6.0 times or lower, film breakage in the longitudinal stretching process and the subsequent transverse stretching process is reduced.

[0072] Next, the longitudinally uniaxially oriented film obtained by stretching in the longitudinal direction is cooled to a temperature of 10°C to 70°C. If the cooling temperature is 10°C or higher, curling of the film can be suppressed. On the other hand, if the cooling temperature is 70°C or lower, the promotion of thermal crystallization can be suppressed. After that, it is guided to a tenter, and after preheating by gripping both ends in the width direction with clips, it is transversely stretched to a width of 7.0 to 13 times. Considering the viewpoint of controlling the protrusions on the film surface to a desirable range by high-temperature stretching, the preheating and stretching temperatures are 156°C to 166°C, more preferably 159°C to 165°C, and even more preferably 160°C to 164°C.

[0073] Furthermore, heat treatment may be performed directly within the tenter. In this case, to control the thermal shrinkage rate in the width direction, the heat treatment temperature is preferably 110°C or higher and less than 170°C, and more preferably 150°C or higher and 165°C or lower. In addition, the heat treatment may be performed while relaxing the film in the width direction. In particular, by setting the relaxation rate in the width direction to 2.0% or higher and 20.0% or lower, more preferably 7.0% or higher and 15.0% or lower, the thermal shrinkage rate in the width direction can be set to an appropriate range, and the balance of dimensional stability can be appropriately adjusted.

[0074] The biaxially oriented laminated polypropylene film obtained as described above can be used in a variety of applications, including packaging films, surface protection films, process films, sanitary products, agricultural products, construction products, and medical products. However, due to its excellent surface smoothness, it is particularly suitable for use as a surface protection film, process film, and release film. [Examples]

[0075] The biaxially oriented laminated polypropylene film of the present invention will be described in more detail below with reference to examples, but the biaxially oriented laminated polypropylene film of the present invention is not limited to these embodiments. The properties were measured and evaluated by the following methods.

[0076] [Evaluation methods for each characteristic] (1) Film thickness Five biaxially oriented laminated polypropylene films were stacked to form a measurement sample, and the thickness of the sample was measured using an electronic micrometer (TESA TT80). Next, the obtained value was divided by 5 to calculate the thickness of each biaxially oriented laminated polypropylene film. Furthermore, the same measurement was performed at a position shifted by 50 mm in the width direction, and the same measurement was repeated a total of five times. From the obtained measurement results, the maximum, minimum, and average values ​​of the thickness of each biaxially oriented laminated polypropylene film were determined, and the average value was taken as the film thickness (μm).

[0077] (2) Minimum autocorrelation length (Sal), arithmetic mean height (Sa), surface texture aspect ratio (Str) Measurements were taken using the "VertScan" (registered trademark) 2.0 (model: R3300GL-Lite-AC) non-contact surface and layer cross-sectional shape measurement system manufactured by Ryoka Systems Co., Ltd., under the following procedure and conditions. First, a biaxially oriented laminated polypropylene film was unwound from a film roll, and 10 measurement samples were taken at randomly determined points on a straight line passing through the center in the width direction and parallel to the longitudinal direction. Sal, Sa, and Str were measured at these 10 points. The average value of each obtained measurement was calculated and designated as the Sal and Sa of the biaxially oriented laminated polypropylene film. Note that one measurement was performed using one field of view (field of view area: 939 μm vertical × 1,252 μm horizontal = 1,175,628 μm). 2 Measurements were taken of the following:

[0078] A. Measurement conditions CCD camera: SONY HR-57 1 / 2 Objective lens: 10X Lens tube: 0.5X BODY Wavelength filter: 530 white Measurement mode: Wave Field of view size: 640 x 480 Scan range: (Start) 5μm, (Stop) -5μm.

[0079] B. Method for fixing the measurement sample A dedicated sample holder was used to secure the measurement samples. The sample holder consisted of two detachable metal plates with a circular hole in the center. The measurement sample was placed between the plates, ensuring there were no wrinkles, and measurements were taken on the sample located within the circular hole.

[0080] C. Analysis method The data obtained from the above measurements was analyzed using the image analysis software VS-Viewer of "VertScan" (registered trademark) 2.0. First, noise was removed using a median filter (5x5), and then undulation components were removed using a Gaussian filter with a cutoff value of 250 μm. Next, Sal, Sa, and Str, as defined in ISO25178 (2012), were measured using the "ISOPara" function. In the "ISOPara" function, the S-Filter was set to 6.0 μm.

[0081] (3) Evaluation of release force and mold release properties A sample was prepared by applying Nitto Denko Corporation's polyester adhesive tape No. 31B to a biaxially oriented laminated polypropylene film using a roller, and then cutting it into 19mm wide strips. These samples were then peeled using a Kyowa Interface Science Co., Ltd. tensile testing machine (model: VPA-2) at a peeling speed of 300mm / min and a peeling angle of 180°. The value output by the tensile testing machine was defined as the peeling force (N). Release properties were evaluated according to the following criteria (○ and △ indicate that the film can be used without problems as a release film, and these were considered acceptable). The peeling force was evaluated on both sides. After evaluating the release properties on both sides, the side with the better evaluation when applied to the following three criteria was adopted. ○: No delamination occurred between the surface and base layers, and delamination was possible at a constant rate. △: No delamination occurred between the surface and base layers, but the delamination resistance was somewhat high, resulting in unstable delamination. ×: It failed to meet any of the requirements marked with ○ or △, and the delamination behavior was accompanied by defects exceeding those marked with △.

[0082] (4) Coefficient of friction Test specimens (measurement standard length: width 75 mm x length 100 mm), which had been temperature and humidity controlled under specified conditions (temperature: 23±3℃, humidity: 65±5%), were stacked so that different sides were in contact with each other and set in a measuring instrument (slip tester). A load of 200 g was placed on the two stacked test specimens, and the resistance value was measured by sliding the upper test specimen using the measuring instrument. The coefficient of friction was calculated using the following formula (1). Note that both the static friction coefficient (μs) and the kinetic friction coefficient (μd) were calculated using the following formula (1), but for the resistance value (g), the maximum resistance value at the moment the sliding began was used for the former calculation, and the resistance value during the sliding was used for the latter calculation. Coefficient of friction = resistance (g) / load (g). Equation (1).

[0083] (5) Product rolled up After winding the product rolls, wrinkles and misalignment were visually inspected and evaluated according to the following criteria. A result of ○ or △ was considered acceptable. ○: No wrinkles or misalignment occurred in the product roll. △: Wrinkles and misalignment occurred in the product rolls, but these were minor and did not cause any actual damage during processing. ×: Wrinkles and misalignment occurred in the product rolls, resulting in an excessive level of damage to the processing.

[0084] [Raw materials] The following raw materials were used to manufacture the biaxially oriented laminated polypropylene films of the Examples and Comparative Examples. Note that the antioxidants listed below were already mixed into polypropylene resin I and branched-chain polypropylene resin, so no fine adjustments were made to their content in the Examples and Comparative Examples. Furthermore, the amount of antioxidant contained in each resin is trace (less than 1.0% by mass in total), and considering the volatile content when the film is formed, the amount of antioxidant will be even less. Therefore, the manufacturing methods and Table 1 of the Examples and Comparative Examples described below will not include this information.

[0085] (1) Resin Polypropylene resin I (homopolypropylene resin): Manufactured by Prime Polymer Co., Ltd., this is a highly stereoregular homopolypropylene resin with an MFR of 2.9 g / 10 min, a melting point of 164 °C, and a mesopentade fraction of 0.94. Branched-chain polypropylene resin: "WAYMAX" (registered trademark) (MFX3) manufactured by Nippon Polypropylene Co., Ltd., with an MFR of 9.0 g / 10 min. Polymethylpentene (PMP) resin: Mitsui Chemicals, Inc. "TPX" (registered trademark) MX004.

[0086] (2) Antioxidants Antioxidant 1: BASF Japan's "Irganox" (registered trademark) 1010. Antioxidant 2: 2,6-di-t-butyl-p-cresol (BHT) manufactured by ADEKA.

[0087] (Example 1) As raw material for the base layer (layer B), a mixture of 98 parts by mass of polypropylene resin I and 2 parts by mass of branched-chain polypropylene resin was supplied to a single-screw extruder, and as raw material for the surface layer (layer A), a mixture of 80 parts by mass of polypropylene resin I and 20 parts by mass of branched-chain polypropylene resin was supplied to another single-screw extruder, and both were melt-extruded at 260°C. Next, after removing foreign matter with a 20 μm cut sintered filter, each raw material was laminated in a feed-block type composite T-die so that the thickness ratio of layer A / layer B / layer A was 1 / 8 / 1, formed into a sheet, and extruded. This was then brought into contact with a casting drum using an air knife, cooled and solidified to obtain an unstretched sheet. At this time, two types of casting drums were used. First, the side that would become the inner surface when ultimately made into a film roll was brought into contact with a casting drum whose surface temperature was adjusted to 90°C, and then the side that would become the outer surface when ultimately made into a film roll was brought into contact with a casting drum whose surface temperature was set to 60°C. Furthermore, on the first casting drum, compressed air at a temperature of 65°C was blown onto the non-drum contact surface at an air velocity of 140 m / s to cool the sheet. Note that an air knife was not used on the second casting drum. Next, the inner surface of the unstretched sheet was preheated to 142°C and the outer surface to 151°C using a conveyor roll. Then, the unstretched sheet was stretched 5.0 times in the longitudinal direction between rolls at a temperature of 155°C with a difference in peripheral speed, and cooled on a roll at 40°C to obtain a uniaxially oriented film. Next, the uniaxially oriented film was introduced into a tenter-type stretcher with both ends in the width direction gripped with clips, preheated at 162°C for 3 seconds, stretched 8.8 times at 162°C, and heat treated at 163°C while allowing 10.5% relaxation in the width direction. After a cooling process at 135°C, the film was guided to the outside of a tenter-type stretcher, the clips at the widthwise ends were released, and the widthwise ends (the parts that the clips had been holding) were cut off with a slitter. The film was then wound up with a winding machine to obtain a biaxially oriented laminated polypropylene film with a thickness of 15 μm. The physical properties and evaluation results of the obtained biaxially oriented laminated polypropylene film are shown in Table 1. Note that the winding inner surface refers to the surface located on the core side of the film roll when the film is wound into a roll, and the winding outer surface refers to the surface opposite the winding inner surface.

[0088] (Examples 2-7, Comparative Examples 1-7) In Example 1, a biaxially oriented laminated polypropylene film with the thickness shown in Table 1 was obtained using the same method as in Example 1, except that the film composition and film formation conditions were as shown in Table 1. The physical properties and evaluation results of the obtained biaxially oriented laminated polypropylene film are shown in Table 1. The film thickness was adjusted by the screw rotation speed of the extruder, the width of the unstretched sheet, the film formation speed, the stretching ratio, etc.

[0089] [Table 1]

[0090] In the table, antioxidants are present in extremely small amounts relative to the resin in the film composition and therefore are not considered in the composition calculations. [Industrial applicability]

[0091] As described above, the biaxially oriented laminated polypropylene film of the present invention has excellent release properties and winding properties, making it suitable for use as a release film or process film, and is particularly suitable as a release film for cover films of adhesive resin layers. Furthermore, since the biaxially oriented laminated polypropylene film of the present invention also has excellent surface smoothness, it can be suitably used as a release film or process film in applications where surface smoothness of the product is required. In addition, the biaxially oriented laminated polypropylene film of the present invention, possessing the above characteristics, can be used in a variety of applications such as packaging films, process films, sanitary products, agricultural products, construction products, and medical products.

Claims

1. A biaxially oriented laminated polypropylene film characterized in that the peel force of at least one surface is 1.0 N or more and 2.2 N or less, the minimum autocorrelation length (Sal) of at least one surface is 41 μm or more and 100 μm or less, the difference in Sal between the two surfaces is 5 μm or more and 40 μm or less, and it has a surface layer (layer A) and a base layer (layer B), the layers A, B, and A are arranged in this order, and the layer A contains 10% by mass or more and 30% by mass or less of branched polypropylene.

2. The biaxially oriented laminated polypropylene film according to claim 1, wherein the arithmetic mean height (Sa) of at least one surface is 80 nm or more and 700 nm or less, and the difference in Sa between the two surfaces is 50 nm or more and 400 nm or less.

3. The biaxially oriented laminated polypropylene film according to claim 1 or 2, wherein the aspect ratio (Str) of the surface properties of at least one of the faces is 0.40 or more and 0.90 or less.

4. The biaxially oriented laminated polypropylene film according to claim 1 or 2, wherein the static friction coefficient (μs) and the kinetic friction coefficient (μd), measured by bringing one surface into contact with the opposite surface, are both 0.40 or more and 0.55 or less.

5. A release film made using the biaxially oriented laminated polypropylene film described in claim 1 or 2.

Citation Information

Patent Citations

  • Polypropylene film for mold release

    JP2007126644A

  • Polyolefin film for surface protection

    JP2009143074A

  • Release sheet and resin article

    JP2019218658A

  • Biaxially oriented polypropylene film, metal film laminated film, and film capacitor

    JP2020132877A

  • Polyolefin film, and release film

    JP2020203486A