Method for producing cellulose fiber-containing resin pellets and method for producing molded articles

By melt-kneading cellulose fiber-containing resin sheets in a screw-type kneader with controlled ratios and rates, the method addresses productivity and resistance issues in fiber-reinforced plastic molded products, achieving high-quality cellulose fiber-containing resin pellets and molded articles with enhanced bending and impact resistance.

JP7948065B2Active Publication Date: 2026-11-11OJI HLDG CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023071767
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2026-11-11
Estimated Expiration
2043-04-25

Smart Images

  • Figure 0007948065000003
    Figure 0007948065000003
  • Figure 0007948065000001
    Figure 0007948065000001
  • Figure 0007948065000002
    Figure 0007948065000002
Patent Text Reader

Abstract

To provide a method for producing a cellulose fiber-containing resin pellet that is more excellent in productivity which can obtain a molded body excellent in rigidity to bending and impact resistance from the pellet; and a method for producing a molded body obtained by molding the pellet.SOLUTION: There is provided a method for producing a cellulose fiber-containing resin pellet which melts and kneads a cellulose fiber-containing resin sheet by a screw type kneader, wherein a ratio (cross-sectional area of cellulose fiber-containing resin sheet / loading port area of screw type kneader) of the cross-sectional area of the cellulose fiber-containing resin sheet to the loading port area of the screw type kneader is 0.065 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for producing cellulose fiber-containing resin pellets and a method for producing a molded article using the pellets. [Background technology]

[0002] Fiber-reinforced plastic molded products, formed from nonwoven fabrics containing reinforcing fibers such as carbon fibers and glass fibers (also known as sheets for fiber-reinforced plastic molded products), are already used in various fields, including sports and leisure goods, aircraft materials, and electronic equipment components. While thermosetting resins and thermoplastic resins are used as the matrix resin in fiber-reinforced plastic molded products, the development of fiber-reinforced plastic molded products using thermoplastic resins has been progressing in recent years.

[0003] Reinforcing fibers include carbon fibers, glass fibers, and aramid fibers. These reinforcing fibers increase the strength of fiber-reinforced plastic molded products. When disposing of such molded products, they are typically landfilled or incinerated. However, molded products using the aforementioned reinforcing fibers have low biodegradability after landfilling, and incineration places a heavy burden on incinerators and other equipment.

[0004] For this reason, in recent years, the use of pulp fibers as reinforcing fibers has been proposed (for example, Patent Documents 1 to 3). In Patent Documents 1 and 2, a slurry containing pulp fibers and thermoplastic resin is made into paper, and a molded intermediate product is obtained by heating and pressurizing the resulting product. In Patent Document 3, it is proposed to form pellets from a slurry containing pulp fibers and thermoplastic resin, and then manufacture a molded product by injection molding these pellets. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 6-322699 [Patent Document 2] Japanese Patent Application Publication No. 6-346399 [Patent Document 3] Japanese Patent Application Publication No. 6-345944 [Overview of the project] [Problems that the invention aims to solve]

[0006] The present invention aims to provide a method for producing cellulose fiber-containing resin pellets that is more productive, and a method for producing molded articles with excellent rigidity against bending and impact resistance from the pellets, as well as a method for producing molded articles obtained by molding the pellets. [Means for solving the problem]

[0007] The present inventors have found that, in a method for producing cellulose fiber-containing resin pellets, which includes a step of melt-kneading a cellulose fiber-containing resin sheet in a screw-type kneader to produce cellulose fiber-containing resin pellets, by setting the ratio of the cross-sectional area of ​​the cellulose fiber-containing sheet to the input port area of ​​the screw-type kneader to a specific value or less, the productivity is excellent, and a molded article with excellent rigidity against bending and impact resistance can be obtained from the resulting cellulose fiber-containing resin pellets, thus completing the present invention. The present invention relates to the following: <1> ~ <14> Regarding. <1> A method for producing cellulose fiber-containing resin pellets by melt-kneading a cellulose fiber-containing resin sheet in a screw-type kneader, wherein the ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the input area of ​​the screw-type kneader (cross-sectional area of ​​the cellulose fiber-containing resin sheet / input area of ​​the screw-type kneader) is 0.065 or less. <2> Cross-sectional area (cm²) of cellulose fiber-containing resin sheet relative to screw diameter (mm) of screw-type kneader 2 ) ratio (cross-sectional area (cm²) of cellulose fiber-containing resin sheet 2) / screw diameter (mm)) is 0.100 or less, the method for producing cellulose fiber-containing resin pellets according to <1>. <3> The method for producing cellulose fiber-containing resin pellets according to <1> or <2>, wherein the ratio of the discharge rate (kg / h) to the peripheral speed (m / min) of the screw of the screw-type kneader (discharge rate / peripheral speed) is 0.50 or more. <4> The method for producing cellulose fiber-containing resin pellets according to any one of <1> to <3>, wherein the content of cellulose fibers in the cellulose fiber-containing resin pellets is 10 mass% or more and 90 mass% or less. <5> The method for producing cellulose fiber-containing resin pellets according to any one of <1> to <4>, wherein the cellulose fiber-containing resin sheet is produced by a production method comprising the following step 1 and step 2. Step 1: A fiber aggregate production step of producing a fiber aggregate containing cellulose fibers and resin A by dry papermaking Step 2: A cellulose fiber-containing resin sheet production step of compressing the fiber aggregate to produce a cellulose fiber-containing resin sheet <6> The method for producing cellulose fiber-containing resin pellets according to <5>, wherein the resin A comprises resin fibers. <7> The method for producing cellulose fiber-containing resin pellets according to any one of <1> to <6>, wherein T / Y is 0.5 or more and 1.5 or less, where T is the tensile strength in the first direction of the cellulose fiber-containing resin sheet, and Y is the tensile strength in the second direction orthogonal to the first direction. <8> The method for producing cellulose fiber-containing resin pellets according to any one of <1> to <7>, wherein the bulk specific gravity of the cellulose fiber-containing resin sheet is 0.10 g / mL or more and 0.60 g / mL or less. <9> A method for producing a molded article, comprising the step of producing cellulose fiber-containing resin pellets by the method according to any one of <1> to <8>, and the step of molding the cellulose fiber-containing resin pellets. <10> The method for producing a molded article according to <9>, wherein the molding step is a step of injection-molding the cellulose fiber-containing resin pellets. <11> The density of the resulting molded body is 0.8 g / cm³ 3 More than 1.5g / cm 3 The following is: <9> or <10> A method for manufacturing a molded article as described above. <12> The thickness of the resulting molded body is 2 mm or more. <9> ~ <11> A method for manufacturing a molded article as described in any one of the following. <13> The resulting molded article has a flexural modulus of 1.5 GPa or higher, as measured in accordance with JIS K 7171:2016. <9> ~ <12> A method for manufacturing a molded article as described in any one of the following. <14> The resulting molded article, measured in accordance with JIS K 7111-1:2012, has a Charpy impact strength of 2.0 kJ / m². 2 That's all. <9> ~ <13> A method for manufacturing a molded article as described in any one of the following. [Effects of the Invention]

[0008] The present invention provides a method for producing cellulose fiber-containing resin pellets that is more productive, the method for producing cellulose fiber-containing resin pellets that yield a molded article with excellent rigidity against bending and impact resistance from the pellets, and the method for producing a molded article obtained by molding the pellets. [Brief explanation of the drawing]

[0009] [Figure 1] Figure 1 shows the web forming apparatus used in the example. [Modes for carrying out the invention]

[0010] [Method for manufacturing cellulose fiber-containing resin pellets] The method for producing cellulose fiber-containing resin pellets (hereinafter also simply referred to as "pellets") according to this embodiment is a method for producing cellulose fiber-containing resin pellets by melt-kneading a cellulose fiber-containing resin sheet (hereinafter also simply referred to as "sheet") in a screw-type kneader, wherein the ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the input port area of ​​the screw-type kneader (cross-sectional area of ​​the cellulose fiber-containing resin sheet / input port area of ​​the screw-type kneader) is 0.065 or less. The manufacturing method of the present invention offers superior productivity compared to conventional methods. Furthermore, the molded articles obtained from these pellets exhibit excellent rigidity against bending and impact resistance.

[0011] The detailed mechanism by which the above effects are achieved can be partially understood as follows. In the melt-mixing process, when cellulose fibers and resin components are supplied and melt-mixed, the cellulose fibers are hydrophilic while the resin components are generally hydrophobic. This leads to aggregation of the cellulose fibers, resulting in poor dispersion of the cellulose fibers within the resin components. Furthermore, the need to apply high shear force can cause cellulose fiber breakage or the formation of fine fibers. Molded articles obtained from pellets produced in this manner are considered to have poor bending rigidity and impact resistance. The present inventors have been investigating the above problems, and as described in PCT / JP2022 / 040342, a fiber aggregate containing cellulose fibers such as pulp fibers and a resin component (resin A) is manufactured in advance by dry papermaking, and this is compressed into a sheet. The fiber aggregate sheet is then melt-kneaded to produce pellets, and these pellets are then molded to produce a molded body. In the example in PCT / JP2022 / 040342, when supplying the material to the melt-kneader, it is cut to a size that can be supplied to the melt-kneader. However, it has been found that when supplying cut raw materials, productivity is low because the raw materials are bulky and it is difficult for them to be fed into the screw inside the melt-kneader. The inventors hypothesized that by supplying sheet-like raw materials directly to a melting and mixing machine, the productivity of pellets would be greatly improved because, once the sheets become embedded in the screw of the melting and mixing machine, they would be continuously supplied. After diligent research, they discovered that by setting the ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the input area of ​​the screw-type mixing machine to 0.065 or less, it is possible for the sheets to become embedded in the screw and for continuous supply to the screw-type mixing machine to be possible. Furthermore, as described above, molded articles produced using pellets obtained by continuously supplying sheet-like raw materials exhibited excellent rigidity against bending and impact resistance, similar to pellets obtained by supplying cut raw materials. Moreover, it was found that supplying sheet-like raw materials resulted in even greater rigidity against bending and impact resistance compared to supplying cut raw materials. This is thought to be because the smoother supply to the kneader reduced the residence time inside the kneader, decreasing the time the cellulose fibers were exposed to heat, thus suppressing the cutting and thermal degradation of the cellulose fibers. Furthermore, the mechanism by which the effects of the present invention are obtained is not limited to those described above. The present invention will be described in further detail below.

[0012] <Pellet Manufacturing Process> The method for producing cellulose fiber-containing resin pellets according to this embodiment includes the step of melting and kneading a cellulose fiber-containing resin sheet in a screw-type kneader to produce pellets.

[0013] (Cross-sectional area of ​​cellulose fiber resin-containing sheet / Inlet area of ​​screw-type kneader) In this embodiment, the ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the input port area of ​​the screw-type kneader (cross-sectional area of ​​the cellulose fiber-containing resin sheet (cm²) 2 ) / Inlet area of ​​screw-type kneader (cm²) 2) is 0.065 or less. By setting the above ratio to 0.065 or less, the cellulose fiber-containing resin sheet easily bites into the screw of the kneader, and the cellulose fiber-containing resin sheet can be continuously supplied to the kneader. The above ratio is preferably 0.063 or less, more preferably 0.061 or less, still more preferably 0.060 or less, and the lower limit is not particularly limited, but from the viewpoint of productivity, it is preferably 0.010 or more, more preferably 0.020 or more, still more preferably 0.030 or more. The cross-sectional area of the cellulose fiber-containing resin sheet is calculated from the width and thickness of the sheet. The width and thickness of the sheet are measured by the methods described in the Examples. In addition, the inlet area of the screw-type kneader may be measured with a caliper or the like.

[0014] The cross-sectional area (cm of the cellulose fiber-containing resin sheet described above 2 ) and the inlet area (cm of the screw-type kneader 2 ) can vary greatly depending on the scale of the kneader used. For example, the cross-sectional area (cm of the cellulose fiber-containing resin sheet 2 ) is preferably 0.5 cm 2 or more, more preferably 1.0 cm 2 or more, and preferably 100 cm 2 or less, more preferably 50 cm 2 or less. In addition, the inlet area (cm of the screw-type kneader 2 ) is, for example, preferably 5 cm 2 or more, more preferably 10 cm 2 or more, and preferably 30000 cm 2 or less, more preferably 10000 cm 2 or less, still more preferably 5000 cm 2 or less.

[0015] In the present embodiment, the cross-sectional area (cm of the cellulose fiber-containing resin sheet relative to the screw diameter (mm) of the screw-type kneader 2The ratio (cellulose fiber-containing resin sheet / screw diameter) is preferably 0.100 or less. A ratio of 0.100 or less is preferable because it makes it easier for the cellulose fiber-containing resin sheet to bite into the screw of the kneader, allowing for a continuous supply of the cellulose fiber-containing resin sheet to the kneader. The above ratio is more preferably 0.090 or less, even more preferably 0.085 or less, and even more preferably 0.085 or less, and the lower limit is not particularly limited, but from the viewpoint of productivity, it is preferably 0.010 or more, more preferably 0.020 or more, and even more preferably 0.030 or more.

[0016] The screw diameter (mm) of the screw-type kneader described above can vary greatly depending on the scale of the kneader used, but for example, it is preferably 10 mm or more, more preferably 20 mm or more, even more preferably 30 mm or more, and preferably 500 mm or less, more preferably 300 mm or less, and even more preferably 150 mm or less. The screw diameter (mm) is often disclosed by the manufacturer of the mixing machine, and the manufacturer's value may be used. Alternatively, it may be measured using calipers or similar tools.

[0017] In this embodiment, the ratio of the discharge speed (kg / h) to the peripheral speed (m / min) of the screw of the screw-type kneader (discharge speed / peripheral speed) is preferably 0.50 or higher. A discharge speed of 0.50 or higher to peripheral speed is preferable because it increases productivity and suppresses excessive shearing that cuts and refines cellulose fibers. The ratio of the discharge speed to the peripheral speed is more preferably 0.60 or higher, even more preferably 0.70 or higher, even more preferably 0.80 or higher, and particularly preferably 0.90 or higher. There is no particular upper limit, but from the viewpoint of ease of manufacture, it is preferably 3.00 or lower, more preferably 2.50 or lower, and even more preferably 2.00 or lower.

[0018] The peripheral speed (m / min) of the screw of a screw-type kneader is preferably 0.3 m / min or more, more preferably 1.0 m / min or more, and even more preferably 3 m / min or more, from the viewpoint of productivity, and preferably 500 m / min or less, more preferably 300 m / min or less, and even more preferably 100 m / min or less, from the viewpoint of suppressing shear heat. The peripheral speed of the screw (m / min) should be set appropriately during the operation of the mixer. Furthermore, the discharge speed (kg / h) can vary greatly depending on the scale of the kneader used, but from the viewpoint of productivity, it is preferably 1 kg / h or more, more preferably 3 kg / h or more, and even more preferably 5 kg / h or more. There is no particular upper limit, but from the viewpoint of ease of manufacturing, it is preferably 1000 kg / h or less.

[0019] <Cellulose fiber-containing resin sheet> The pellet manufacturing method of this embodiment includes a step of producing pellets by melting and kneading a cellulose fiber-containing resin sheet in a screw-type kneader. In this embodiment, the cellulose fiber-containing resin sheet is supplied in sheet form from the raw material inlet of the screw-type kneader. The cellulose fiber-containing resin sheet contains a resin component (resin A) in addition to cellulose fibers. Resin A is preferably a thermoplastic resin and preferably contains fibrous resin (resin fibers). The cellulose fiber-containing resin sheet may be obtained by any method, but it is preferable that it be manufactured by steps 1 and 2 described below. Step 1: A fiber aggregate manufacturing process in which a fiber aggregate containing cellulose fibers and resin A is produced by dry papermaking. Step 2: Cellulose fiber-containing resin sheet manufacturing process, which involves compressing the fiber aggregate to produce a cellulose fiber-containing resin sheet. The following describes in detail a method for producing a cellulose fiber-containing resin sheet, which is preferred in this embodiment and includes steps 1 and 2 described above.

[0020] (Process 1) Step 1 is a fiber aggregate manufacturing process in which a fiber aggregate containing cellulose fibers and resin A is produced by dry papermaking.

[0021] [Cellulose fiber] There are no particular limitations on the manufacturing method or type of cellulose fiber. The cellulose fiber is preferably pulp fiber, and may include, for example, chemical pulp such as kraft pulp from hardwoods and / or softwoods, mechanical pulp such as SGP, RGP, BCTMP, and CTMP, recycled paper pulp such as deinked pulp, and non-wood pulp such as kenaf, jute, bagasse, bamboo, straw, and hemp. Chlorine-free pulp such as ECF pulp and TCF pulp can also be used. While pulp fibers are preferred as the cellulose fibers, the material is not limited to them, and other materials such as paper powder or wood powder may also be used.

[0022] Among the pulp fibers mentioned above, kraft pulp fibers, particularly long-fiber coniferous kraft pulp fibers (NBKP), are preferable as cellulose fibers because they exhibit superior flexural modulus and impact resistance in the resulting molded articles.

[0023] The average fiber length of the cellulose fibers is preferably 0.1 mm or more, more preferably 0.5 mm or more, even more preferably 1 mm or more, and preferably 50 mm or less, more preferably 10 mm or less, even more preferably 5 mm or less, and even more preferably 2.5 mm or less, from the viewpoint of improving the flexural modulus and impact resistance of the resulting molded article and from the viewpoint of ease of manufacturing the fiber aggregate. The average fiber length of cellulose fibers is measured by the method described in the examples.

[0024] The average fiber width of the cellulose fibers is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, even more preferably 15 μm or more, and preferably 150 μm or less, more preferably 100 μm or less, even more preferably 80 μm or less, and even more preferably 50 μm or less, from the viewpoint of improving the rigidity and impact resistance of the resulting molded article against bending and from the viewpoint of ease of manufacturing the fiber aggregate. The average fiber width of cellulose fibers is measured by the method described in the examples.

[0025] In this embodiment, when forming a fiber aggregate by the airlaid method, the cellulose fibers can be in the form of, for example, defibrated dry pulp.

[0026] From the viewpoint of improving the impact resistance of the resulting molded article, it is preferable that the cellulose fibers be unbeaten cellulose fibers. In a molded article, impact resistance requires that cellulose fibers be properly extracted from the resin when an impact is applied. For this reason, it is preferable to use unbeaten cellulose fibers with a low ratio of fine fibers, and more preferably unbeaten pulp fibers. Furthermore, from the above viewpoint, the ratio of fine fibers in the cellulose fibers is preferably 50% or less, more preferably 30% or less, and even more preferably 20% or less, with no particular lower limit. The fine fiber ratio of cellulose fibers is measured by the method described in the examples.

[0027] From the viewpoint of obtaining a molded article with excellent flexural modulus and impact resistance, as well as from the viewpoint of productivity and ease of manufacturing of the cellulose fiber-containing resin sheet, the cellulose fiber content in the cellulose fiber-containing resin sheet is preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more, even more preferably 25% by mass or more, even more preferably 85% by mass or less, even more preferably 80% by mass or less, and even more preferably 75% by mass or less.

[0028] [Resin A] Examples of components of resin A include polyolefins, polyvinyl chloride, polystyrene, ABS (acrylonitrile-butadiene-styrene), acrylonitrile-styrene, polyester, acrylic resin, polyamide, polyacetal, polycarbonate, polybutylene succinate, and polylactic acid. In addition, resins or elastomers exemplified in the lubricants, plasticizers, nucleating agents, flame retardants, antistatic agents, fillers, and papermaking chemicals described later in the [Other Components] section may be used. In other words, resin A refers to the resin components contained in the molded article. Furthermore, as described in the method for manufacturing the molded article later, the molded article of this embodiment is preferably manufactured by a process in which a cellulose fiber aggregate containing cellulose fibers and resin A is produced by dry papermaking, and then compressed to produce a cellulose fiber-containing resin sheet. That is, it is preferable that at least resin A is blended into the cellulose fiber aggregate. In addition, further resins or elastomers may be added during the manufacturing of the molded article.

[0029] In the present invention, the resin A contained in the fiber aggregate can be any of fibers, powder, granules, or pellets. Among these, from the viewpoint of ease of papermaking in step 1 described later, the resin A contained in the fiber aggregate is preferably fibers or powder, and more preferably fibers. That is, the resin A contained in the fiber aggregate preferably contains resin fibers or resin powder, more preferably resin fibers, and even more preferably resin fibers. Preferred examples of resin A fibers to be included in the fiber aggregate include polyolefin fibers, polyvinyl chloride fibers, polyester fibers, acrylic fibers, polyamide fibers, polycarbonate fibers, and polylactic acid fibers. Preferred components of the resin A powder, granules, and pellets to be contained in the fiber aggregate include polyolefins, polyvinyl chloride, polyester, acrylic, polyamide, polycarbonate, polylactic acid, polystyrene, ABS, acrylonitrile styrene, polyacetal, and polybutylene succinate. In particular, preferred examples of resin A powder include polyolefin powder, polystyrene powder, ABS powder, acrylonitrile styrene powder, polyacetal powder, and polybutylene succinate powder. The polyolefins mentioned above are the same as the specific examples of polyolefins shown in the polyolefin fibers below. Among these, polyolefin fibers are preferred as resin A to be contained in the fiber aggregate. Furthermore, the resin A contained in the fiber aggregate can be one type or a combination of two or more types. For example, resin A may be a combination of two types: polylactic acid fiber and polybutylene succinate powder.

[0030] -Polyolefin fiber- In this embodiment, when polyolefin fibers are used as resin A to be contained in the fiber aggregate, the polyolefin constituting the polyolefin fibers is not particularly limited, and examples include polyolefin (unmodified polyolefin) and modified polyolefin. The melting point of the polyolefin constituting the polyolefin fiber is preferably 200°C or lower, more preferably 195°C or lower, even more preferably 180°C or lower, and preferably 80°C or higher, more preferably 90°C or higher, and even more preferably 100°C or higher, from the viewpoint of ease of molding and suppression of degradation of cellulose fibers.

[0031] Examples of polyolefins include polyethylene, polypropylene, and ethylene-propylene copolymer (also called propylene-ethylene copolymer), with polyethylene and polypropylene being preferred. Furthermore, in modified polyolefins, examples of methods for modifying polyolefins include acid modification and chlorination, and among these, acid modification is preferred from the viewpoint of improving affinity with cellulose fibers. The acid-modifying component used for acid-modified polyolefins is preferably an unsaturated carboxylic acid component. The unsaturated carboxylic acid component is a component derived from an unsaturated carboxylic acid and its acid anhydride. Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, maleic acid, maleic anhydride, itaconic acid, fumaric acid, and crotonic acid. Among these, the unsaturated carboxylic acid component is preferably at least one selected from acrylic acid, methacrylic acid, maleic acid, and maleic anhydride, and particularly preferably at least one selected from maleic acid and maleic anhydride. Polyolefins modified with at least one of maleic acid and maleic anhydride are also called maleic acid-modified polyolefins. The acid-modified polyolefin is preferably a maleic acid-modified polyolefin, and more preferably a maleic acid-modified polyethylene or a maleic acid-modified polypropylene. It is sufficient that at least a portion of the acid-modified polyolefin is acid-modified.

[0032] The polyolefin is preferably at least one selected from the group consisting of polyethylene, polypropylene, polyethylene and polypropylene that are at least partly modified with maleic acid, and ethylene-propylene copolymers. From the viewpoint of improving the flexural modulus of the resulting molded article, it is preferable that the polyolefin contains an acid-modified polyolefin, more preferably that the polyolefin contains at least one of polyethylene that is at least partly maleic acid-modified and polypropylene that is at least partly maleic acid-modified, and even more preferably that it contains at least partly maleic acid-modified polyethylene. Furthermore, from the viewpoint of improving the impact resistance of the resulting molded article, it is preferable that it does not contain acid-modified polyolefins, and it is more preferable that the polyolefin contains only polyethylene, polypropylene, and ethylene-propylene copolymers. Polyolefin fibers may be used individually or in combination of two or more types.

[0033] Polyolefin fibers may be composite fibers composed of two or more polyolefins, and examples include split fibers, sea-island fibers, core-sheath fibers, and bonded fibers. Among these, core-sheath fibers are preferred from the viewpoint of obtaining a molded article with excellent rigidity against bending and impact resistance. In the case of core-sheath fibers, fibers with a concentric cross-sectional structure or an eccentric cross-sectional structure are used, but fibers with a concentric cross-sectional structure are preferred. Using fibers with a concentric cross-sectional structure is preferable because it allows for a more uniform fiber aggregate.

[0034] From the viewpoint of obtaining a uniform fiber aggregate and ease of manufacturing the fiber aggregate, the fiber length of the polyolefin fiber is preferably 0.1 mm or more, more preferably 1.0 mm or more, even more preferably 2.0 mm or more, even more preferably 3.0 mm or more, and preferably 50 mm or less, more preferably 20 mm or less, and even more preferably 10 mm or less. The fiber length of the polyolefin fiber is measured by the method described in the examples.

[0035] From the viewpoint of obtaining a uniform fiber aggregate and ease of manufacturing the fiber aggregate, the fiber diameter of the polyolefin fiber is preferably 0.1 μm or more, more preferably 1 μm or more, even more preferably 10 μm or more, and preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 50 μm or less. The fiber diameter of the polyolefin fiber is measured by the method described in the examples.

[0036] From the viewpoint of obtaining a uniform fiber aggregate and ease of manufacturing the fiber aggregate, the fineness of the polyolefin fiber is preferably 0.01 dtex or more, more preferably 0.1 dtex or more, even more preferably 1 dtex or more, and preferably 100 dtex or less, more preferably 50 dtex or less, and even more preferably 10 dtex or less.

[0037] When the resin A contained in the fiber aggregate is polyolefin fiber, the polyolefin fiber content in the fiber aggregate is preferably 90% by mass or less from the viewpoint of obtaining a molded article with excellent rigidity against bending and impact resistance, more preferably 80% by mass or less, even more preferably 65% ​​by mass or less from the viewpoint of productivity and ease of manufacturing, and even more preferably 50% by mass or less, particularly preferably 45% by mass or less from the viewpoint of biomassification degree and productivity. Also, from a similar viewpoint, it is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and even more preferably 25% by mass or more. When using two or more types of polyolefin fibers, the above content refers to the total content of polyolefin fibers.

[0038] If resin A is a fiber other than polyolefin fiber, the preferred fiber length, fiber diameter, fineness, and content of the said fiber are the same as those of the preferred fiber length, fiber diameter, fineness, and content of polyolefin fiber, respectively. Furthermore, if resin A is in the form of powder, granules, or pellets, the preferred content of such powder, granules, or pellets is the same as the preferred content of the polyolefin fibers. Also, if resin A is in the form of powder, granules, or pellets, the particle size of such powder, granules, or pellets is not particularly limited.

[0039] [Other ingredients] In this embodiment, if resin A in the fiber aggregate is polyolefin fiber, the fiber aggregate may contain other components in addition to the cellulose fiber and polyolefin fiber described above. Other components include elastomers and binder components, which will be described later. When a binder component is included, the binder component content is preferably 0.1% to 40% by mass, more preferably 0.3% to 30% by mass, even more preferably 0.4% to 20% by mass, and even more preferably 0.5% to 10% by mass, based on the total mass of the fiber aggregate. By setting the binder component content within the above range, handling properties and other factors during the manufacturing of the molded article can be improved. Suitable binder components include various starches, casein, sodium alginate, hydroxyethylcellulose, carboxymethylcellulose, acrylic resin, styrene-(meth)acrylic acid ester copolymer resin, urethane resin, polyvinyl alcohol (PVA) resin, various starches, cellulose derivatives, sodium polyacrylate, polyacrylamide, polyvinylpyrrolidone, acrylamide-acrylic acid ester-methacrylic acid ester copolymer, styrene-maleic anhydride copolymer alkali salt, isobutylene-maleic anhydride copolymer alkali salt, polyvinyl acetate resin, vinyl chloride-vinyl acetate copolymer, ethylene-vinyl acetate copolymer, and the like.

[0040] The fiber aggregate may further contain fillers and papermaking chemicals. Examples of fillers include mineral pigments such as kaolin, calcined kaolin, calcium carbonate, calcium sulfate, barium sulfate, titanium dioxide, talc, zinc oxide, alumina, magnesium carbonate, magnesium oxide, silica, white carbon, bentonite, zeolite, sericite, and smectite, as well as organic pigments such as polystyrene resins, urea resins, melamine resins, acrylic resins, and vinylidene chloride resins. Examples of papermaking chemicals include paper strength enhancers, yield enhancers, water drainage enhancers, dyes, fluorescent whitening agents, pH adjusters, defoamers, pitch control agents, and slime control agents. Examples of paper strength enhancers include polyacrylamide. Furthermore, wet paper strength enhancers can also be used in combination, such as polyamide resins, melamine-formaldehyde resins, urea-formaldehyde resins, polyamide-polyamine-epichlorohydrin resins, and polyethyleneimine resins.

[0041] The fiber aggregate may further contain a fatty acid metal salt. The fatty acid metal salt is preferably a metal salt of an aliphatic carboxylic acid, and the aliphatic carboxylic acid is preferably a saturated aliphatic carboxylic acid or an unsaturated aliphatic carboxylic acid having 12 to 24 carbon atoms. Specifically, examples include lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, arachidic acid, henicosyl acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, myristoleic acid, palmitoleic acid, sapienic acid, oleic acid, and elaidic acid. Examples of metal elements that form metal salts include Group 1 elements (alkali metals) such as sodium and potassium; Group 2 elements (alkaline earth metals) such as calcium, magnesium, and barium; and Group 3 elements such as zinc and aluminum, with calcium, magnesium, zinc, and aluminum being preferred. Examples of fatty acid metal salts include magnesium stearate, calcium stearate, zinc stearate, barium stearate, aluminum stearate, lithium stearate, zinc laurate, and barium laurate. Among these, calcium stearate, magnesium stearate, zinc stearate, aluminum stearate, calcium oleate, magnesium oleate, zinc oleate, aluminum oleate, zinc laurate, or calcium laurate are preferred from the viewpoint of excellent rigidity against bending and impact resistance, with calcium stearate being more preferred. The fatty acid metal salt content in the molded article is 0.1% by mass or more and 10% by mass or less, preferably 0.3% by mass or more, more preferably 0.5% by mass or more, even more preferably 0.8% by mass or more, and preferably 9% by mass or less, more preferably 8% by mass or less, even more preferably 7% by mass or less, and even more preferably 6% by mass or less, from the viewpoint of rigidity against bending and impact resistance.

[0042] If other components are present, the content of the other components, excluding cellulose fibers and polyolefin fibers, is preferably 0.1% to 40% by mass, more preferably 0.3% to 30% by mass, even more preferably 0.4% to 20% by mass, and even more preferably 0.5% to 10% by mass, based on the total mass of the fiber aggregate.

[0043] [Fiber assembly manufacturing process] Next, we will describe the manufacturing process of the fiber aggregate. In the following description of the manufacturing process for the fiber aggregate, the explanation assumes that a preferred polyolefin fiber is used as resin A. If a resin other than polyolefin fiber is used as resin A, the resin used should be read as such, and the rest of the explanation remains the same. As described later, resin A can be used as one type or a combination of two or more types.

[0044] In the fiber aggregate manufacturing process of Step 1 of this embodiment, cellulose fibers and resin A are manufactured by dry papermaking. The manufacturing process for the fiber aggregate preferably includes a step of mixing cellulose fibers and polyolefin fibers in air and depositing them. In other words, the fiber aggregate of this embodiment is preferably a dry nonwoven fabric.

[0045] When manufacturing fiber aggregates using the dry papermaking method, it is preferable to employ the airlaid method. The airlaid method is a method of forming an airlaid web by discharging an airflow containing raw fibers, such as polyolefin fibers and cellulose fibers uniformly mixed in an airflow, onto a mesh-like endless belt equipped with a suction box on the lower side. In other words, the airlaid method is a method that includes the step of mixing cellulose fibers and polyolefin fibers in air and depositing them. In the airlaid method, the above operation may be repeated multiple times as needed.

[0046] The web formed by the above method is then formed into a sheet by a fiber bonding process as described below. The fiber bonding process includes methods such as the needle punch method, where needles are passed perpendicular to the web surface to entangle polyolefin fibers or cellulose fibers and form a sheet. Such bonding processes are preferably used in combination with the carding method for web formation. Furthermore, the fiber bonding process can employ methods such as the thermal bonding method (where a heat-fusible adhesive blended into the dry web is heated to bond the raw fibers), the chemical bonding method (where an adhesive is applied to the resulting dry web to bond the raw fibers), or a combination of the thermal bonding and chemical bonding methods (multi-bonding method).

[0047] In the thermal bonding method, it is preferable to heat the heat-fusible adhesive at a temperature at least 20°C higher than its melting point. Heat treatments include hot air treatment and low-pressure hot pressure treatment after hot air treatment.

[0048] When thermal bonding or multi-bonding methods are employed, it is preferable to use a particulate or fibrous heat-fusible adhesive. The heat-fusible adhesive may be the polyolefin fibers or binder components mentioned above. As particulate heat-sealable adhesives, heat-sealable resin particles such as polyethylene, polypropylene, polyester low-melting-point polyethylene terephthalate, low-melting-point polyamide, low-melting-point polylactic acid, and polybutylene succinate are used. Fibrous heat-sealable adhesives include polyesters such as low-melting-point polyethylene terephthalate, low-melting-point polylactic acid, polybutylene succinate (PBS), and polyethylene terephthalate (PET), as well as resins such as low-melting-point polyamides, acrylic resins, and vinyl acetate (PVAc). Furthermore, as a heat-fusible synthetic fiber, a heat-fusible composite synthetic fiber with a core-sheath structure, obtained by compounding two types of resins with different melting points, in which only the surface of the fiber melts, can also be preferably used. A heat-fusible composite synthetic fiber with a core-sheath structure has a structure in which a sheath made of a resin with a lower melting point is formed on the outer circumference of a core made of a resin with a higher melting point. Specifically, examples include forms that combine two types of resins with different melting points (PET / PET composite fiber, PE / PET composite fiber, MAPE / PP composite fiber, PP / PET composite fiber, PE / PP composite fiber, PVAc / PET composite resin).

[0049] Furthermore, when a chemical bonding method is used to bond fibers, it is preferable to add a binder component to fix the fibers together. The binder component can be appropriately selected as needed, and for example, solution-type binders such as starch, casein, sodium alginate, hydroxyethylcellulose, sodium carboxymethylcellulose salt, polyvinyl alcohol (PVA), and sodium polyacrylate can be used, as well as emulsion-type binders such as polyacrylic acid esters, acrylic styrene copolymers, polyvinyl acetate, ethylene vinyl acetate copolymers, acrylonitrile butadiene copolymers, methyl methacrylate butadiene copolymers, urea-melamine resins, and styrene-butadiene copolymer resins can be used. It is also preferable to use the binder components mentioned above. The binder can be used in various forms, such as fibers, powders, granules, solutions, or emulsions, and two or more types can be used in combination.

[0050] In the fiber aggregate produced by the dry papermaking method described above, each fiber constituting the fiber aggregate is randomly oriented in three dimensions in the longitudinal, width, and thickness directions. Therefore, in this embodiment, the tensile strength in the first direction and the tensile strength in the second direction of the fiber aggregate are approximately the same. In other words, in this embodiment, a fiber aggregate with excellent isotropy in the planar direction is obtained.

[0051] Furthermore, in the manufacturing process of the fiber aggregate, a laminated sheet may be produced by laminating any sheet that does not hinder moldability onto the fiber aggregate. For example, any sheet can be laminated onto the surface of the fiber aggregate or between sheets when laminating the fiber aggregate. As the sheet to be laminated, sheets such as tissue or nonwoven fabric can be used. These sheets are laminated for the purpose of improving the surface properties of the fiber aggregate or cellulose fiber-containing resin sheet in the manufacturing process, improving productivity, or imparting other functions.

[0052] (Process 2) Step 2 is a process for manufacturing a cellulose fiber-containing resin sheet by compressing the fiber aggregate obtained in Step 1. By compressing the fiber aggregate obtained in Step 1, a sheet-like cellulose fiber-containing resin sheet is obtained. The above compression may be performed simultaneously with or after the heat treatment.

[0053] Compression of a fiber aggregate can be achieved by pressurizing the fiber aggregate using a roll press. Alternatively, heating may be applied simultaneously during the roll press process, resulting in a heated-pressure treatment. Roll press processing allows for arbitrary control of the density of the resulting cellulose fiber-containing resin sheet by applying pressure with metal or resin rolls. Specifically, by setting the number of rolls, temperature, and clearance for the roll press process, and then heating and pressurizing the sheet, a cellulose fiber-containing resin sheet of any desired density can be obtained. The sheet may also be compressed to the desired density by passing it through multiple rolls.

[0054] Compression of fiber aggregates can also be achieved by pressurization treatment using a hot press. By pressurizing fiber aggregates cut to an appropriate size, or cellulose fiber-containing resin sheets that have undergone the above-mentioned roll press treatment, using an autoclave method or a die press method, the density of the resulting cellulose fiber-containing resin sheet can be arbitrarily controlled. By heating to a temperature of 100°C or higher and pressurizing to 2 MPa or higher, a cellulose fiber-containing resin sheet with a higher density than that obtained by pressurization treatment using a roll press can be obtained. Furthermore, a preliminary pressing step may be performed before obtaining the above heating and pressing conditions. It is also preferable to perform a preliminary pressing at a lower pressure under the desired heating conditions, and then increase the pressure for hot pressing.

[0055] The pressurizing process using hot pressing may be replaced with a stamping molding method. The stamping molding method involves preheating the fiber aggregate to melt and soften the polyolefin, placing it inside a mold, then closing the mold to clamp it, and finally pressurizing and cooling it. For heating, heating devices such as far-infrared heaters, heating plates, high-temperature ovens, and dielectric heating devices can be used.

[0056] The pressurization process using hot pressing may be performed by vacuum forming. Vacuum forming improves moldability by creating a vacuum between the fiber assembly and the mold, thereby increasing the adhesion between the fiber assembly and the mold. Vacuum forming is preferably performed in the mold clamping step of the stamping molding method described above. Specifically, vacuum forming is performed in the step of heating the fiber assembly to melt and soften the polyolefin, placing it inside the mold, and then closing the mold to clamp it. In vacuum forming, vacuum suction is performed from the mold side. The molding pressure in vacuum forming is usually 1.0 kg / cm². 2 The following procedure is followed, and the molding process is performed for approximately 0.1 seconds to 60 seconds.

[0057] The pressurization process using hot pressing may be replaced with a pressure forming method. The pressure forming method involves blowing compressed air onto the fiber assembly to ensure close contact with the mold, thereby improving the adhesion between the fiber assembly and the mold. Pressure forming is preferably performed during the mold clamping step of the stamping molding method described above. Specifically, the fiber assembly is heated to melt and soften the polyolefin, then placed in the mold, and finally molded by blowing compressed air from the fiber assembly side. The pressure used for pressure forming is 3 kg / cm². 2 More than 8kg / cm 2 The process is often carried out using the following compressed air pressures, and it is preferable to perform the molding for 0.1 seconds to 60 seconds or more.

[0058] Compression of fiber aggregates can also be achieved by supercalendering. In the supercalendering process described above, the fiber aggregate is formed by passing it between heated rollers while applying nip pressure. The heating temperature of the rollers used is preferably 10°C or more, more preferably 20°C or more, and even more preferably 30°C or more, above the melting point of the polyolefin fiber, and preferably 100°C or less, more preferably 90°C or less, and even more preferably 80°C or less, above the melting point of the polyolefin fiber. Furthermore, the nip pressure is preferably 100 kg / cm or more, more preferably 150 kg / cm or more, even more preferably 200 kg / cm or more, and preferably 450 kg / cm or less, more preferably 400 kg / cm or less, and even more preferably 350 kg / cm or less. Furthermore, the number of nip stages is preferably 1 or more, more preferably 3 or more, even more preferably 5 or more, and preferably 20 or less, more preferably 18 or less, and even more preferably 16 or less. Furthermore, when compressing a fiber aggregate to produce a cellulose fiber-containing resin sheet, multiple cellulose fiber-containing resin sheets may be laminated and compressed as appropriate, depending on the desired thickness of the cellulose fiber-containing resin sheet.

[0059] In this embodiment, the cellulose fiber-containing resin sheet preferably has a tensile strength ratio of 0.5 to 1.5, where T is the tensile strength in a first direction and Y is the tensile strength in a second direction perpendicular to the first direction. This ratio is preferable because the fibers constituting the cellulose fiber-containing resin sheet are mixed very uniformly, resulting in a molded article that is excellent not only in bending rigidity and strength but also in impact resistance. T / Y is preferably 0.60 or higher, more preferably 0.70 or higher, even more preferably 0.80 or higher, and even more preferably 0.85 or higher, and preferably 1.40 or lower, more preferably 1.30 or lower, even more preferably 1.20 or lower, and even more preferably 1.15 or lower. The first direction of a cellulose fiber-containing resin sheet is any one direction in the planar direction of the cellulose fiber-containing resin sheet. However, if the fibers contained in the cellulose fiber-containing resin sheet are oriented in any direction in the planar direction, that orientation direction shall be considered the first direction. Furthermore, if the flow direction in the dry papermaking process of the fiber aggregate is known, that flow direction shall be considered the first direction. When the flow direction in the manufacturing process of the fiber aggregate is known, the flow direction in the manufacturing process is sometimes called the first direction (MD direction), and the flow direction in the obtained fiber aggregate and cellulose fiber-containing resin sheet may be called the T direction. The second direction of the fiber aggregate is one direction in the planar direction of the fiber aggregate and is perpendicular to the first direction. If the flow direction in the manufacturing process of the fiber aggregate is known, the direction perpendicular to the flow direction in the manufacturing process is called the second direction (CD direction), and the second direction in the obtained fiber aggregate and cellulose fiber-containing resin sheet is sometimes called the Y direction. The tensile strength of the cellulose fiber-containing resin sheet in the first and second directions is measured in accordance with JIS P 8113:2006. The tensile strength in each direction was measured using a Tensilon tensile testing machine manufactured by A&D Co., Ltd., with a 15±0.1 mm × 180±1 mm strip at a speed of 20±5 mm / min.

[0060] In this embodiment, the cellulose fiber-containing resin sheet is obtained by dry-processing a mixture of at least cellulose fibers and resin A (preferably polyolefin fibers), and is in sheet form. The sheet is obtained by press-processing a cotton-like fiber aggregate (hereinafter also referred to as a cotton-like fiber aggregate) after dry-processing, and may have various bulk densities. The bulk density of the cellulose fiber-containing resin sheet to be fed into the screw-type kneader is preferably 0.10 g / mL or more, more preferably 0.15 g / mL or more, and preferably 0.60 g / mL or less, more preferably 0.50 g / mL or less, and even more preferably 0.40 g / mL or less, from the viewpoint of ease of compression in step 2, ease of subsequent melt kneading, and ease of cutting when cutting for supply to the melt kneader. The bulk density of the cellulose fiber-containing resin sheet is measured by the method described in the examples.

[0061] (The process of manufacturing pellets) The method for producing cellulose fiber-containing resin pellets according to this embodiment includes the step of melting and kneading a cellulose fiber-containing resin sheet in a screw-type kneader to produce pellets. Here, the cellulose fiber-containing resin sheet is supplied to the melting kneader in sheet form. At this time, from the viewpoint of ensuring that the ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the area of ​​the screw-type kneader's inlet is within a desired range, the cellulose fiber-containing sheet may be cut to a desired width if necessary. Also, if the kneader has multiple inlets, the cellulose fiber-containing sheet may be supplied from multiple inlets.

[0062] The method for producing the pellets is not particularly limited; it can be done by supplying a cellulose fiber-containing resin sheet and melt-mixing it in a screw-type kneader. Examples of screw-type kneaders include single-screw kneaders and twin-screw kneaders, and from the viewpoint of kneading efficiency, twin-screw kneaders are preferred. After supplying the cellulose fiber-containing resin sheet to a screw-type kneader and melt-mixing it, (1) A method for obtaining cellulose-containing resin pellets by extruding in strand form and cooling and solidifying, (2) A method of obtaining cellulose fiber-containing resin pellets by cooling and solidifying the molten mixture either as is or after stretching it into a sheet, and then crushing it with a crusher. (3) A method for obtaining cellulose fiber-containing resin pellets by extruding them into a rod or cylindrical shape and cooling them, (4) A method of obtaining cellulose fiber-containing resin in the form of a sheet or film by extruding it from a T-die, and then cutting or crushing it to obtain cellulose fiber-containing resin pellets, (5) A method for obtaining cellulose fiber-containing resin pellets by cutting the molten mixture immediately after extrusion with a rotating blade in air or water. Examples include the following. The size of the resulting pellets is not particularly limited, but it is preferably 1 to 10 mm in size from the viewpoint of ease of loading into the injection molding machine.

[0063] The melting and mixing temperature (barrel setting temperature) is not particularly limited, but it is preferable to adjust the barrel setting temperature so that the temperature of the molten mixture (the temperature of the mixture actually obtained, the resin temperature) is 5°C or more higher than the melting point of the polyolefin, more preferably 10°C or more higher, even more preferably 15°C or more higher, and from the viewpoint of degradation of cellulose fibers, it is preferable that the temperature is 100°C or more higher than the melting point of the polyolefin, more preferably 90°C or less higher, and even more preferably 80°C or less higher. The temperature of the molten mixture becomes higher than the molten mixture temperature (barrel setting temperature) due to shear adiabatic adiabatic effects during molten mixture mixing. In other words, it varies depending on various conditions during molten mixture mixing, such as the molten mixture temperature (barrel setting temperature), discharge speed, rotation speed, and screw design of the molten mixture mixer. In the method described in the examples, the temperature of the molten mixture becomes about 20 to 40°C higher than the molten mixture temperature (barrel setting temperature), so the molten mixture temperature (barrel setting temperature) becomes about 20 to 40°C lower than the preferred temperature of the molten mixture.

[0064] Various conditions during melting and mixing, such as discharge speed and rotation speed, can be adjusted according to known methods. It is preferable to adjust the discharge speed (discharge rate) as appropriate so that it falls within the desired range relative to the peripheral speed of the screw. If the equipment used for melt-mixing is a twin-screw extruder, it is desirable to design the screw to minimize the mixing force. In this invention, the cellulose fibers and resin A are uniformly dispersed in the fiber aggregate sheet beforehand, and even if melt-mixing is performed without applying high shear force, the dispersion state of the cellulose fibers in the fiber aggregate sheet is maintained, resulting in pellets with excellent cellulose fiber dispersibility. Therefore, by minimizing the mixing force, it is possible to avoid cutting the cellulose fibers. Specifically, the kneading parts primarily consist of R-type kneading parts, and the number of L-type and N-type kneading parts is preferably the same as or less than the number of R-type kneading parts, and more preferably less than the number of R-type kneading parts. When melt-kneading is performed using only the cut chips of the fiber aggregate sheet, the kneading parts may consist only of R-type kneading parts without using L-type or N-type kneading parts. The kneading parts are preferably 5 or fewer out of 10 parts of the entire screw, and more preferably 3 or fewer. When melt kneading is performed using only the cut tips of the fiber aggregate sheet, the kneading parts may consist of only 1 part.

[0065] Furthermore, during melt kneading, additional resin components may be added along with the cellulose fiber-containing resin sheet during melt kneading. Examples of resin components include the resin components listed in Resin A above, and elastomers described later, with polyolefin resins and elastomers described later being preferred. During melt kneading, it is preferable to add at least one selected from Resin A and elastomers, as this yields a molded article with superior impact resistance. In other words, the obtained cellulose fiber-containing resin pellets may contain components added during the melt-kneading process, in addition to components derived from the cellulose fiber-containing resin sheet. In melt mixing, elastomers refer to polymer compounds that exhibit elastic deformation, soften and become fluid when heated, and return to a rubbery state when cooled. Specifically, elastomers have a structure consisting of two polymer segments: a hard segment and a soft segment. The hard segment acts as a crosslinking point, and the soft segment exhibits rubber elasticity, resulting in elasticity. Therefore, at room temperature, the hard segment aggregates to form a pseudo-crosslinked state and exhibits rubber-like properties, but at high temperatures, it melts and loses its function as a crosslinking point, allowing for plastic deformation. Polylastic elastomers are classified into categories such as polystyrene-based, olefin / alkene-based, polyester-based, polyvinyl chloride-based, polyurethane-based, polyamide-based, polyacrylic-based, silicone-based, and polyimide-based, depending on the combination of hard-segment polymers and soft-segment polymers. Furthermore, even within the same system, the properties differ depending on the ratio of hard-segment to soft-segment polymers and their molecular weights. For example, in the case of polystyrene-based elastomers, there are those that use styrene for the hard segment and butadiene for the soft segment. In this case, a higher styrene content results in high hardness and improved compatibility with polystyrene and polyphenylene ether, while a lower styrene content results in low hardness, high flexibility, and improved compatibility with polyolefins. Furthermore, a higher molecular weight improves temperature characteristics and mechanical properties, while a lower molecular weight improves processability and transparency. An example of a polystyrene-based elastomer is the ToughTec series manufactured by Asahi Kasei Corporation. For example, there are olefin / alkene compounds that combine ethylene, propylene, and 1-butene. The density, modulus of elasticity, and melting point can be altered depending on the combination and ratio. Furthermore, the structure when mixed with resins differs, sometimes resulting in island-like dispersion and other times in a miscible state. An example of an olefin / alkene elastomer is the Tuffmer series manufactured by Mitsui Chemicals, Inc. Among these, polystyrene-based elastomers and olefin / alkene-based elastomers are preferred from the viewpoint of impact resistance and other factors. Examples of elastomers include the various elastomers described in paragraphs 0043 to 0065 of the revised edition of the Japanese Patent Publication No. 2020 / 080328. The method of adding the elastomer is not particularly limited, but it is preferable to supply it together with the cellulose fiber-containing resin sheet during the melt-kneading process of the cellulose fiber-containing resin sheet and then melt-knead it.

[0066] When the cellulose fiber-containing resin pellets contain the elastomer, the elastomer content is preferably 55% by mass or less, more preferably 50% by mass or less, even more preferably 45% by mass or less, even more preferably 40% by mass or less, and particularly preferably 35% by mass or less, relative to the total mass of resin A and elastomer, from the viewpoint of improving the flexural modulus. Furthermore, when the elastomer is included, the elastomer content is preferably 5% by mass or more, more preferably 8% by mass or more, even more preferably 10% by mass or more, even more preferably 12% by mass or more, and particularly preferably 15% by mass or more, relative to the total mass of resin A and elastomer, from the viewpoint of improving impact resistance.

[0067] In this embodiment, the cellulose fiber content in the cellulose fiber-containing resin pellets is preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more, even more preferably 25% by mass or more, even more preferably 80% by mass or less, even more preferably 70% by mass or less, and even more preferably 60% by mass or less, from the viewpoint of obtaining a molded article with excellent flexural modulus and impact resistance.

[0068] <Application> The cellulose fiber-containing resin pellets of this embodiment are suitably used as resin pellets for various molding applications.

[0069] [Method for manufacturing molded products] The method for manufacturing the molded article of this embodiment comprises the steps of manufacturing the cellulose fiber-containing resin pellets described above, and molding the cellulose fiber-containing resin pellets. Various molding methods can be employed in the molding process, including, for example, injection molding (e.g., injection compression molding (press injection, hot flow stamping molding, gas injection compression molding), gas injection molding, and ultra-high-speed injection molding), various extrusion molding methods (cold runner or hot runner method), compression (press) molding, insert molding, in-mold coating molding, heat-insulating mold molding, rapid heating and cooling mold molding, and various shape extrusion molding methods (e.g., two-color molding and sandwich molding). For example, various extrusion molding methods are suitable for molding sheets, films, fibers, etc. For molding sheets or films, inflation molding, calendering, casting, etc., can also be used. Furthermore, specific stretching operations may be applied. It is also possible to produce hollow molded products by rotational molding or blow molding, etc. Furthermore, multiple molding processes may be combined, or multiple processes may be carried out simultaneously as a single process. For example, a molded body may be obtained by forming cellulose fiber-containing resin pellets into a sheet and then hot-press molding, or by forming cellulose fiber-containing resin pellets into a sheet and then supercalendering. Alternatively, after forming into a sheet, the molded body may be formed by vacuum forming, pressure forming, or the like. Among these, injection molding is a preferred example.

[0070] If the molding process is an injection molding process, the injection molding process involves, for example, using a known injection molding machine to melt and knead the cellulose fiber-containing resin pellets described above, and then injecting the molten mixture into a mold to form the product. When melting and kneading, any known kneader may be used, such as a single-screw kneader or a twin-screw kneader. Examples of known injection molding machines include screw-type injection molding machines, screw-pre-plasticized injection molding machines, plunger-pre-plasticized injection molding machines, and plunger-type injection molding machines. Examples of drive systems include hydraulic, electric, and hydraulic-electric hybrid systems.

[0071] The injection molding temperature conditions are determined appropriately according to the type of resin contained in the pellets, and it is preferable to set the cylinder temperature of the injection molding machine to a temperature 0 to 100°C higher than the flow start temperature of the resin used. The mold temperature can be appropriately selected from the standpoint of the cooling rate of the resin used and productivity. For example, in the case of polyolefins, it is preferable to set the temperature in the range of room temperature (e.g., 23°C) to 120°C. Other injection conditions, such as screw rotation speed, back pressure, injection speed, holding pressure, and holding pressure time, can be adjusted as appropriate.

[0072] The cellulose fiber-containing resin pellets of this embodiment may also contain other resins, such as elastomers, by adding and melt-kneading other resins, such as elastomers, during the molding process. Furthermore, in the manufacturing process of the molded product, other resins, various additives, masterbatches containing various additives, etc., may be added in addition to the cellulose fiber-containing resin pellets during injection molding. Examples of additives include those typically used in resin compositions. Such additives include stabilizers, UV absorbers, plasticizers, flame retardants, flame retardant enhancers, antistatic agents, surfactants, colorants, lubricants, and mold release agents. Examples of stabilizers include hindered phenols, hydroquinones, phosphites, and their substituted derivatives. Examples of UV absorbers include resorcinol, salicylate, benzotriazole, and benzophenone. Examples of colorants include dyes such as nitrosine, and materials containing pigments such as cadmium sulfide, phthalocyanine, and carbon black. Examples of lubricants include fatty acids such as stearic acid and montanic acid, their amides, their esters, their half-esters with polyhydric alcohols, stearyl alcohol, stearamide, polyethylene wax, and paraffin wax.

[0073] <Characteristics of the molded product> In this embodiment, the density of the resulting molded article is preferably 0.5 g / cm³. 3 More preferably 0.8 g / cm³ 3 More preferably 0.95 g / cm³ 3 More preferably, 1.0 g / cm³ 3 That concludes the explanation. Furthermore, the density of the molded body is preferably 2.0 g / cm³. 3 More preferably, 1.5 g / cm³ 3 More preferably, 1.2 g / cm³ 3 The following applies:

[0074] The thickness of the molded body is not particularly limited, but is 0.5 mm or more, more preferably 1 mm or more, even more preferably 2 mm or more, and preferably 200 mm or less, more preferably 100 mm or less, even more preferably 50 mm or less, even more preferably 20 mm or less, and especially preferably 10 mm or less. Furthermore, since the molded body can be suitably used in applications requiring impact resistance by having a thickness of 2 mm or more, a thickness of 2 mm or more is particularly preferable.

[0075] The molded article of this embodiment preferably has a high flexural modulus, which is preferable because a high flexural modulus results in a molded article with excellent rigidity against bending. The flexural modulus of the molded article is preferably 1.5 GPa or higher, more preferably 2.0 GPa or higher, even more preferably 2.5 GPa or higher, even more preferably 3.0 GPa or higher, and still more preferably 3.0 GPa or higher. There is no particular upper limit, but from the viewpoint of ease of manufacture, it is preferably 10 GPa or lower. The flexural modulus of the molded article is measured in accordance with JIS K 7171:2016.

[0076] The molded article of this embodiment preferably has high bending strength, which is preferable because it results in a molded article with excellent rigidity. The bending strength of the molded article is preferably 20 MPa or more, more preferably 30 MPa or more, and even more preferably 35 MPa or more. There is no particular upper limit, but from the viewpoint of ease of manufacturing, it is preferably 100 MPa or less. The bending strength of the molded product is measured in accordance with JIS K 7171:2016.

[0077] The molded article of this embodiment preferably has a high Charpy impact strength, and the Charpy impact strength of a molded article with a thickness of 4 mm is preferably 1.5 kJ / m 2 More preferably 2.0 kJ / m 2 More preferably, 3.0 kJ / m 2 More preferably, 4.0 kJ / m 2 That concludes the explanation. There is no particular upper limit, but from the viewpoint of ease of manufacture, it is preferably 100 kJ / m³. 2 The following applies: Furthermore, a higher Charpy impact strength value indicates superior impact resistance. The Charpy impact strength was measured in accordance with JIS K 7111-1:2012, and in detail, by the method described in the examples.

[0078] (Application) The molded articles obtained by the manufacturing method of this embodiment are preferably used in electrical and electronic equipment, office automation equipment, home appliances, civil engineering and construction equipment, automobiles, aircraft parts, structural parts and housings, containers (for example, food containers, pharmaceutical packaging containers, cosmetic packaging containers, medical device packaging containers), furniture, daily necessities, medical devices, and the like. Among these, it is particularly suitable for applications requiring impact resistance, such as civil engineering and construction, automobile or aircraft parts, structural components, and enclosures. [Examples]

[0079] The features of the present invention will be further described below with reference to examples and comparative examples. The materials, amounts used, proportions, processing content, and processing procedures shown in the following examples can be modified as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the following specific examples.

[0080] (Example 1) <Preparation of fiber aggregates> NBKP was treated with a swirling-flow jet defibration apparatus to obtain defibrated dry pulp. The processing air velocity in the defibration apparatus was 45 m / min, and turbulence was created by baffles installed in the apparatus. The average fiber length of the obtained defibrated dry pulp was 2.38 mm, the average fiber width was 34.3 μm, and the fine fiber ratio was 11.4%. Next, the obtained defibrated dry pulp, polypropylene fibers (melting point 160°C, fineness 6.6 dtex, fiber length 5 mm, fiber diameter 30 μm, also called "PP fibers"), and polyethylene / polypropylene composite core-sheath fibers (core melting point 160°C, sheath melting point 110°C, fineness 1.7 dtex, fiber length 5 mm, fiber diameter 15 μm, core diameter 10.6 μm, core mass / sheath mass = 1 / 1, also called "PE / PP composite fibers") were uniformly mixed by airflow in a ratio of 30 / 55 / 15 (mass ratio) to obtain a fiber mixture.

[0081] Next, an airlaid web was formed from the fiber mixture using the web forming apparatus 1 shown in Figure 1. Specifically, the first carrier sheet 41 was fed onto a permeable endless belt 20 mounted on a conveyor 10 by the first carrier sheet supply means 40. In Example 1, tissue paper (basis weight 14 g / m²) was used as the first carrier sheet 41. 2 ) was used. At this time, the width was 1200 mm. The basis weight was measured according to "Paper and cardboard - Method for measuring basis weight" as described in JIS P8124:2011.

[0082] While the permeable endless belt 20 is sucked by the suction box 60, the fiber mixture is dropped and deposited onto the first carrier sheet 41 from the fiber mixture supply means 30 along with the airflow, thereby obtaining a cotton-like fiber aggregate. At this time, the set basis weight of the airlaid web portion was 400 g / m². 2 The fiber mixture was supplied in such a manner. Next, the second carrier sheet supply means 50 laminated the second carrier sheet 51 onto the cotton-like fiber aggregate on the first carrier sheet 41 to obtain a fiber aggregate containing an airlaid web. In Example 1, tissue paper (basis weight 14 g / m²) was used as the second carrier sheet 51. 2 ) was used. In other words, in Example 1, the same sheet was used for the first carrier sheet 41 and the second carrier sheet 51.

[0083] <Preparation of cellulose fiber-containing resin sheets> The resulting fiber aggregate containing the airlaid web was passed through a box-type dryer with a hot air circulation conveyor oven system and treated with hot air at a temperature of 140°C. Subsequently, the density was adjusted by roll pressing to a bulk density of 0.3 g / mL, and the basis weight was 416 g / m² without separating the first and second carrier sheets. 2 A cellulose fiber-containing resin sheet was obtained. The T / Y ratio of the cellulose fiber-containing resin sheet was 0.88, the bulk density was 0.32 g / mL, and the thickness was 1.3 mm. The aforementioned cellulose fiber-containing resin sheet was slit using a slitter machine to obtain sheets with a width of 150 mm.

[0084] <Preparation of cellulose fiber-containing resin pellets> The aforementioned cellulose fiber-containing resin sheet is placed at the base of a twin-screw compounding extruder (Shibaura Machinery Co., Ltd., TEM-37SX, screw diameter 37 mm) with a cross-sectional area of ​​57 cm². 2The material was introduced into the opening. The mixture was melted, kneaded, and dispersed at a mixing temperature of 165°C and a rotation speed of 70 rpm (peripheral speed 8.1 m / min). The screw used for mixing consisted of an R-type kneading part and a feed screw for all other components, resulting in a weak kneading configuration. After cooling the strand extruded from the 4 mmφ die by air cooling, it was cut with a pelletizer to obtain cellulose fiber-containing resin pellets with a length of 3 mm. The extrusion rate of the kneaded material, as measured by the method described later, was 9.7 kg / h.

[0085] (Example 2) Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 1, except that the rotation speed was changed to 300 rpm (peripheral speed 34.9 m / min). The discharge rate of the kneaded material was 47.3 kg / h.

[0086] (Example 3) Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 1, except that the rotation speed was changed to 500 rpm (peripheral speed 58.1 m / min). The discharge rate of the kneaded material was 78.6 kg / h.

[0087] (Example 4) Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 1, except that the width was set to 200 mm. The discharge rate of the kneaded material was 11.7 kg / h.

[0088] (Example 5) In Example 1, in the <Preparation of Cellulose Fiber-Containing Resin Sheet>, the width was set to 100 mm, and in the <Preparation of Cellulose Fiber-Containing Resin Pellets>, the sheet input section was located in the middle of the extruder with a cross-sectional area of ​​22 cm². 2 Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 1, except that a vent port was used. The discharge rate of the kneaded material was 7.5 kg / h.

[0089] (Example 6) Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 4, except that the fiber mixture was changed to a ratio of 50 / 35 / 15 (mass ratio) in the <Preparation of Fiber Aggregates> of Example 1. The basis weight of the cellulose fiber-containing resin sheet was 411 g / m². 2 The T / Y ratio was 0.88, the bulk density was 0.29 g / mL, and the thickness was 1.44 mm. The dispensing rate of the kneaded material was 13.8 kg / h.

[0090] (Comparative Example 1) In Example 1, <Preparation of Cellulose Fiber-Containing Resin Sheet>, the cellulose fiber-containing resin sheet was shredded using a shredder (AFS100M, manufactured by Iris Ohyama Co., Ltd.) to obtain press-shredded chips of approximately 4 mm x 13 mm, and cellulose fiber-containing resin pellets were obtained in the same manner as in Example 1, except that the press-shredded chips were fed into a twin-screw extruder. The discharge rate of the kneaded material was 3.8 kg / h.

[0091] (Comparative Example 2) Cellulose fiber-containing resin pellets were obtained in the same manner as in Comparative Example 1, except that the rotation speed was changed to 300 rpm (peripheral speed 34.9 m / min). The discharge rate of the kneaded material was 12.5 kg / h.

[0092] (Comparative Example 3) Cellulose fiber-containing resin pellets were obtained in the same manner as in Comparative Example 1, except that the rotation speed was changed to 500 rpm (peripheral speed 58.1 m / min). The discharge rate of the kneaded material was 24.8 kg / h.

[0093] (Comparative Example 4) In Example 1, the preparation of a cellulose fiber-containing resin sheet was carried out in the same manner as in Example 1, except that the width was set to 300 mm. However, the cellulose fiber-containing resin sheet was not properly engaged with the screw of the kneader, and cellulose fiber-containing resin pellets could not be obtained.

[0094] [Measurement and Evaluation Methods] (Method for measuring fiber length and fiber diameter of polyolefin fibers) Twenty randomly selected polyolefin fibers were observed under an optical microscope, and their fiber length and diameter were measured.

[0095] (Method for measuring the average fiber length, average fiber diameter, and fine fiber ratio of pulp fibers (cellulose fibers)) In accordance with ISO 16065-2, the average fiber length and average fiber diameter of pulp fibers were measured using a fiber image analysis device (Valmet FS5, manufactured by Valmet Co., Ltd.). The proportion of fine fibers 0.1 mm or less in the measured length-weighted average fiber length distribution was defined as the fine fiber ratio.

[0096] (Method for measuring the melting point of polyolefin fibers) If a catalog value is available for the melting point of the polyolefin fiber, that value may be used. In this example, the catalog value was used. If a catalog value is not available, it can be measured using the following method. A 5 mg sample of polyolefin fiber is cut out, and its melting point is measured using a differential scanning calorimeter (DSC). The melting point is measured using a PerkinElmer Diamond DSC under a nitrogen atmosphere, with the temperature increased from 30°C to 280°C at a rate of 20°C / min.

[0097] (Method for measuring the bulk density of cellulose fiber-containing resin sheets) The bulk density of the cellulose fiber-containing resin sheet was calculated by measuring the thickness and mass of a 50 mm square sheet after conditioned for 24 hours at 23°C and 50% RH. The sheet thickness was measured using a digital thickness gauge (DG-127, manufactured by Ozaki Seisakusho Co., Ltd.).

[0098] (Method for measuring T / Y) In the fiber assembly manufacturing process of the obtained cellulose fiber-containing resin sheet, the flow direction (the direction in which the conveyor 10 travels) was designated as the first direction, and the direction perpendicular to the first direction was designated as the second direction. The tensile strength (in N / m) was measured in accordance with JIS P 8113:2006. The tensile strength in each direction was calculated by dividing this tensile strength by the thickness of the test specimen to obtain the tensile strength (in MPa). A Tensilon tensile testing machine manufactured by A&D Co., Ltd. was used to measure a 15 mm x 180 mm strip at a speed of 20 mm / min.

[0099] (Measurement of the discharge rate of the mixed material) The discharge rate of the compound was determined by measuring the mass of compound discharged from the twin-screw extruder die over a 3-minute period, thereby calculating the discharge rate per hour. The average of two measurements was used as the discharge rate.

[0100] <Rating> Molded bodies were obtained from the resulting cellulose fiber-containing resin pellets using the method described below, and their density, flexural modulus, flexural strength, and impact resistance were measured. The results are shown in Table 2. (Pellet molding) Using the aforementioned pellets, a Type A1 multipurpose test specimen as specified in JIS K 7139:2009 was injection molded under the conditions of a molding temperature of 170°C, a mold temperature of 40°C, and an injection speed of 10 mm / sec to obtain a molded body with a thickness of 4 mm.

[0101] (Method for measuring the density of molded products) The obtained molded product (molded body) was cut into strip-shaped test pieces measuring 80 mm in length and 10 mm in width. The thickness of the strip-shaped test pieces was measured using a constant-pressure thickness gauge (TECLOCK Co., Ltd., model number PG-02J), and the volume of the strip-shaped test pieces was calculated. Furthermore, the density was calculated by measuring the mass of the strip-shaped test pieces.

[0102] (Method for measuring the flexural modulus and flexural strength of molded products) The obtained molded product (molded body) was cut into strip-shaped test pieces measuring 80 mm in length and 10 mm in width, and a three-point bending test was performed in accordance with JIS K 7171:2016. The obtained bending modulus of elasticity and bending strength were evaluated such that higher values ​​indicated superior rigidity and strength against bending, respectively.

[0103] (Method for measuring the impact resistance of molded products) The obtained molded product (molded body) was cut into strip-shaped test pieces measuring 80 mm in length and 10 mm in width, and a notched Charpy impact test (impact direction: edgewise) was performed in accordance with JIS K 7111-1:2012. The obtained Charpy impact strength was evaluated as follows: a higher numerical value indicates better impact resistance and greater resistance to impact.

[0104] [Table 1]

[0105] [Table 2]

[0106] As shown in Table 1, increasing the rotational speed increases the discharge volume. While productivity can be evaluated by the discharge volume at the same rotational speed, it is possible to compare productivity at different rotational speeds by considering the discharge volume per rotational speed (the ratio of discharge speed (kg / h) to the peripheral speed (m / min) of the screw (discharge speed / peripheral speed)). As shown in Examples 1 to 6, the cellulose fiber-containing pellets of the present invention have a large discharge speed / peripheral speed ratio and high productivity. Furthermore, as shown in Table 2, molded articles produced using the cellulose fiber-containing pellets of the present invention exhibited excellent rigidity and strength against bending, as well as impact resistance. [Industrial applicability]

[0107] The method for producing cellulose fiber-containing resin pellets according to this embodiment offers high productivity, and furthermore, molded articles with excellent flexural modulus (rigidity against bending), flexural strength (strength against bending), and impact resistance can be obtained from the pellets. [Explanation of symbols]

[0108] 1 Web forming apparatus 10 Conveyor 20 Breathable endless belt 30 Fiber mixture supply means 40 First carrier sheet supply means 41. First Career Sheet 50 Second carrier sheet supply means 51. Second Career Sheet 60 Suction Box

Claims

1. A method for producing cellulose fiber-containing resin pellets by melt-kneading a cellulose fiber-containing resin sheet in a screw-type kneader, The ratio of the cross-sectional area of ​​the cellulose fiber-containing resin sheet to the inlet area of ​​the screw-type kneader (cross-sectional area of ​​the cellulose fiber-containing resin sheet / inlet area of ​​the screw-type kneader) is 0.065 or less. A method for producing cellulose fiber-containing resin pellets.

2. Cross-sectional area (cm²) of cellulose fiber-containing resin sheet relative to screw diameter (mm) of screw-type kneader 2 ) ratio (cross-sectional area (cm²) of cellulose fiber-containing resin sheet 2 A method for producing cellulose fiber-containing resin pellets according to claim 1, wherein the screw diameter (mm) is 0.100 or less.

3. A method for producing cellulose fiber-containing resin pellets according to claim 1, wherein the ratio of the discharge speed (kg / h) to the peripheral speed (m / min) of the screw of a screw-type kneader (discharge speed / peripheral speed) is 0.50 or more.

4. A method for producing cellulose fiber-containing resin pellets according to claim 1, wherein the cellulose fiber content in the cellulose fiber-containing resin pellets is 10% by mass or more and 90% by mass or less.

5. A method for producing cellulose fiber-containing resin pellets according to claim 1, wherein the cellulose fiber-containing resin sheet is produced by a manufacturing method comprising the following steps 1 and 2. Step 1: A fiber aggregate manufacturing process in which a fiber aggregate containing cellulose fibers and resin A is produced by dry papermaking. Step 2: Cellulose fiber-containing resin sheet manufacturing process, which involves compressing the fiber aggregate to produce a cellulose fiber-containing resin sheet.

6. The method for producing cellulose fiber-containing resin pellets according to claim 5, wherein the resin A contains resin fibers.

7. A method for producing cellulose fiber-containing resin pellets according to claim 1, wherein when the tensile strength of the cellulose fiber-containing resin sheet in a first direction is T, and the tensile strength in a second direction perpendicular to the first direction is Y, T / Y is 0.5 or more and 1.5 or less.

8. A method for producing cellulose fiber-containing resin pellets according to claim 1, wherein the bulk density of the cellulose fiber-containing resin sheet is 0.10 g / mL or more and 0.60 g / mL or less.

9. A step of producing cellulose fiber-containing resin pellets by the method described in any one of claims 1 to 8, and The process includes a step of molding the cellulose fiber-containing resin pellets. A method for manufacturing a molded product.

10. The method for manufacturing a molded article according to claim 9, wherein the molding step is a step of injection molding cellulose fiber-containing resin pellets.

11. The density of the resulting molded body is 0.8 g / cm³. 3 1.5g / cm or more 3 The method for manufacturing a molded article according to claim 9, which is as follows:

12. The method for manufacturing a molded article according to claim 9, wherein the thickness of the resulting molded article is 2 mm or more.

13. The method for manufacturing a molded article according to claim 9, wherein the flexural modulus of the obtained molded article, as measured in accordance with JIS K 7171:2016, is 1.5 GPa or more.

14. The Charpy impact strength of the resulting molded article, measured in accordance with JIS K 7111-1:2012, was 2.0 kJ / m². 2 The method for manufacturing a molded article according to claim 9.

Citation Information

Patent Citations

  • Method of treating waste plastic film or sheet

    JP1987231709A

  • Production of article formed by paper-making process

    JP1994322699A

  • Molding made of biodegradable composite material and its production

    JP1994345944A

  • Production of biodegradable composite paper and sheet

    JP1994346399A

  • Thermoplastic resin composition, process for producing the same, and process for producing molding

    WO2008133214A1