Steel plate conveying equipment and method for manufacturing annealed steel plates

Brush rolls with radially protruding metal wires and a polishing member are used to address the issue of deposit growth on conveying rolls, ensuring high-quality annealed steel production by reducing adhesion and facilitating easy deposit removal.

JP7948155B2Active Publication Date: 2026-11-11JFE STEEL CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023214761
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-20
Publication Date
2026-11-11
Estimated Expiration
2043-12-20

AI Technical Summary

Technical Problem

Existing technologies are insufficient in suppressing the rapid growth of deposits on conveying rolls in continuous annealing facilities due to the oxidation of elements like Si and Mn, leading to press marks and indentation defects on steel sheets.

Method used

The use of brush rolls with radially protruding metal wires for conveying rolls, combined with a polishing member, to reduce adhesion and facilitate easy removal of deposits, along with a recovery device to collect detached material.

Benefits of technology

The solution effectively reduces the adhesive force of deposits on conveying rolls, preventing their growth and subsequent indentation defects on steel sheets, thereby enhancing the quality of annealed steel production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948155000003
    Figure 0007948155000003
  • Figure 0007948155000004
    Figure 0007948155000004
  • Figure 0007948155000005
    Figure 0007948155000005
Patent Text Reader

Abstract

To provide steel sheet transport equipment capable of inhibiting growth of an attached matter attached to a transport roll.SOLUTION: Steel sheet transport equipment transports a steel sheet in continuous annealing equipment. The steel sheet transport equipment includes: a transport roll that transports a steel sheet; and a polishing member that polishes the transport roll. The transport roll is a brush roll including a plurality of metallic wires projecting from a peripheral surface in a radial direction.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a steel sheet conveying apparatus for conveying a steel sheet in continuous annealing equipment and a method for manufacturing an annealed steel sheet.

Background Art

[0002] In recent years, demand for high-tensile steel sheets has increased, and the production ratio of high-tensile steel sheets is rising. It has been shown that high-tensile steel sheets can potentially be manufactured to have properties advantageous for strength and workability by adding elements such as Si and Mn. On the other hand, when manufacturing high-tensile steel sheets in a continuous annealing process, a treatment for cooling the heated steel sheet is required from the viewpoint of increasing strength. Furthermore, from the viewpoint of press formability, a tempering treatment that reheats the cooled steel sheet becomes necessary.

[0003] The steel sheet is, for example, preheated to about 150°C in a preheating zone, heated to about 800°C in an oxidation-reduction zone, rapidly cooled to 500°C in a rapid cooling zone, and then subjected to a tempering treatment through such an annealing process. At that time, for steel sheets containing easily oxidizable elements such as Si and Mn, additive elements such as Si and Mn concentrate on the steel sheet surface in the reduction zone, and oxides of these elements are generated. The roll deposits formed by these oxides adhering to the conveying rolls cause press marks (surface defects) on the steel sheet.

[0004] As a technique for preventing press marks on steel sheets caused by roll deposits, Patent Document 1 discloses a method of preventing press marks by using an abrasion-resistant coating that causes roll deposit substances to fall off as abrasion proceeds. Patent Document 2 discloses a method of detecting deposits with an image processing device and removing the deposits on the roll surface with a contact member.

Prior Art Documents

Patent Documents

[0005]

Patent Document 1

Patent Document 2

Summary of the Invention

[0006] Although the technologies disclosed in Patent Documents 1 and 2 can remove deposits from the rolls, they are insufficient to suppress the rapid growth of deposits on the conveying rolls of steel sheets containing easily oxidizable elements such as Mn and Si in a high-temperature environment in a continuous annealing facility. The present invention has been made in view of these problems of the prior art, and its purpose is to provide a steel sheet conveying facility that can suppress the growth of deposits adhering to the conveying rolls, and a method for manufacturing annealed steel sheets by conveying steel sheets with the conveying facility and manufacturing annealed steel sheets in a continuous annealing facility. [Means for solving the problem]

[0007] The means to solve the above problems are as follows: [1] Steel plate conveying equipment for conveying steel plates in a continuous annealing apparatus, comprising a conveying roll for conveying the steel plates and a polishing member for polishing the conveying roll, wherein the conveying roll is a brush roll having a plurality of metal wires protruding radially from its circumferential surface. [2] The steel plate conveying equipment according to [1], wherein the diameter of the wire is 20 μm or more and 500 μm or less. [3] The steel plate conveying equipment according to [1] or [2], wherein the length of the wire is 1 mm or more and 30 mm or less. [4] The steel plate conveying equipment according to any one of [1] to [3], wherein the wire is made of tungsten, molybdenum, cobalt, nickel-chromium alloy or stainless steel. [5] The steel plate conveying equipment according to any one of [1] to [4], wherein the abrasive member is a flat plate, a grinding wheel, or a grinding roll. [6] A steel plate conveying apparatus according to any one of [1] to [5], comprising a recovery device for collecting material that has fallen off the conveying roll. [7] A method for manufacturing annealed steel sheets, comprising transporting steel sheets using steel sheet transport equipment described in any of [1] to [3], and annealing the steel sheets using the continuous annealing equipment to produce annealed steel sheets. [Effects of the Invention]

[0008] In the steel plate conveying equipment according to the present invention, by using brush rolls for the conveying rolls that transport the steel plates, the contact area between the adhering material and the conveying rolls is reduced, thereby reducing the adhesive force. Therefore, by using brush rolls for the conveying rolls, oxides that adhere to the material can be easily removed, and the growth of adhering material on the conveying rolls can be suppressed. [Brief explanation of the drawing]

[0009] [Figure 1] Figure 1 is a schematic diagram showing an example of the configuration of a continuous annealing facility. [Figure 2] Figure 2 is a schematic side view showing an example of the configuration of a steel plate conveying equipment according to this embodiment. [Figure 3] Figure 3 is a schematic side view showing another configuration example of the steel plate conveying equipment according to this embodiment. [Figure 4] Figure 4 is a schematic side view showing another configuration example of the steel plate conveying equipment according to this embodiment. [Modes for carrying out the invention]

[0010] The present invention will be described below through embodiments of the present invention. However, the following embodiments are merely preferred examples of the present invention, and the present invention is not limited in any way by these embodiments.

[0011] The steel plate conveying equipment according to this embodiment is suitably used for conveying steel plates 10 in a continuous annealing equipment 100. First, the continuous annealing equipment 100 will be described. Figure 1 is a schematic diagram showing an example of the configuration of the continuous annealing equipment 100. The continuous annealing equipment 100 includes a heating zone 12, a soaking zone 14, a cooling zone 16, and an over-aging zone 18. The continuous annealing equipment 100 may also be equipped with equipment for surface treatment such as zinc plating, as needed.

[0012] The heating zone 12 is equipped with a device for raising the temperature of the steel plate 10. In the heating zone 12, a direct flame or radiant combustion burner is used. In the heating zone 12, the steel plate 10 is heated to a preset temperature of approximately 600 to 900°C, depending on its composition.

[0013] The uniform temperature zone 14 is equipped with a device for maintaining the steel plate 10 at a predetermined temperature. The device for maintaining the steel plate 10 at a predetermined temperature has a heating capacity sufficient to compensate for the heat dissipated from the furnace body, etc.

[0014] The cooling zone 16 is equipped with facilities for cooling the steel plate 10 to a predetermined temperature. Cooling methods used in the cooling zone 16 include liquid cooling, gas jet cooling, roll cooling, and mist cooling (gas-liquid mixed cooling). Liquid cooling is often performed by water cooling (water quenching). Water cooling is a cooling method in which the steel plate 10 is immersed in a water tank installed downstream of the uniform zone 14. Gas jet cooling is a cooling method in which gas is blown onto the surface of the steel plate 10 from a nozzle. Roll cooling is a cooling method in which the steel plate 10 is cooled by contacting it with a water-cooled roll. Mist cooling is a cooling method in which water is sprayed in a fine mist form, and the steel plate 10 is cooled by the absorption of heat of vaporization. In mist cooling, the size of the sprayed water droplets is often about 0.1 to 1 mm.

[0015] The overaging zone 18 is equipment that reheats the steel plate 10 to a temperature of approximately 300-400°C and holds it at that temperature for a predetermined time to perform overaging treatment. In such continuous annealing equipment 100, the steel plate 10 is heated and reduced in the heating zone 12 and the homogenizing zone 14 in a reducing atmosphere consisting of a mixed gas of hydrogen, nitrogen, etc., cooled in the cooling zone 16, and tempered in the overaging zone 18.

[0016] When the content of Si or Mn in the steel sheet 10 processed by the continuous annealing facility 100 is 0.3 mass% or more, Si and Mn in the steel sheet 10 are oxidized and tend to concentrate in the surface layer. Si and Mn are elements effective for improving the mechanical properties of the steel sheet 10, and Si is more easily oxidized than Mn among the two. For this reason, in Si-added steel, Si oxide is generated in the surface layer of the steel sheet 10, while the generation of Mn oxide tends to be suppressed. However, in a steel sheet with a low Si content, Mn is most likely to concentrate in the surface layer, so Mn oxide of the steel sheet 10 is generated and concentrates in the surface layer.

[0017] The concentration of oxides in the surface layer of the steel sheet 10 and the adhesion of such oxides to the conveying rolls are highly correlated with the temperature of the steel sheet 10. As the temperature of the steel sheet 10 increases, the concentration of Si and Mn oxides in the surface layer of the steel sheet 10 is promoted. The Si and Mn oxides concentrated in the surface layer of the steel sheet 10 adhere to the surface of the conveying rolls. When the Si and Mn oxides adhering to the surface of the conveying roll are heated, a sintered body of the oxides is formed and fixed to the surface of the conveying roll. Since the temperature at which the sintered body is formed is about half the melting point of the oxides, this phenomenon becomes prominent when the surface temperature of the conveying roll reaches 700°C or higher.

[0018] In a vertical continuous annealing facility, the steel sheet 10 is conveyed while being wound around the conveying rolls, so strain corresponding to the roll curvature of the conveying rolls is introduced. In order to reduce the introduction of strain during conveyance, conveying rolls with a larger diameter are used in the vertical continuous annealing facility compared with horizontal continuous annealing facilities. Conveying rolls with a diameter of 400 mm or more are suitably used in vertical continuous annealing facilities.

[0019] On the other hand, when the diameter of the conveying roll increases, the diameter of the axially central portion of the conveying roll becomes larger than the diameter of both end portions due to thermal expansion, and the difference in roll peripheral length between the central portion and both end portions increases. As a result, a speed difference occurs between the steel sheet 10 and the conveying roll depending on the axial position of the conveying roll, and the steel sheet 10 rubs against the surface of the conveying roll, making the oxides concentrated in the surface layer of the steel sheet 10 more likely to adhere to the conveying roll.

[0020] The conveying rolls of the continuous annealing equipment 100 are coated with cermet or ceramics to reduce reactivity and adhesion with adhering materials. However, even with such rolls, if the oxide concentrated on the surface of the steel plate 10 adheres firmly to the conveying roll, it does not easily fall off the roll surface, and the adhering material grows from that point, causing indentation defects in the conveyed steel plate 10.

[0021] To suppress the occurrence of such indentation defects, the steel plate conveying equipment according to this embodiment uses a brush roll on the conveying roll, which has a plurality of metal wires protruding radially from the circumferential surface of the roll. By using a brush roll, even if oxides concentrated on the surface of the steel plate 10 adhere to the surface of the conveying roll, the starting point of adhesion becomes the tip of the wire rather than the surface, reducing the contact area and thus reducing the adhesion force. As a result, the adhered material on the brush roll easily falls off, and can be removed by, for example, a slight difference in speed or impact when the steel plate passes through, thereby suppressing the growth of the adhered material. In this way, by using a brush roll on the conveying roll, the growth of adhered material on the surface of the conveying roll can be suppressed, thereby suppressing the occurrence of indentation defects on the steel plate 10.

[0022] Furthermore, as described above, when the surface temperature of the conveying rolls exceeds 700°C, oxides tend to adhere to the conveying rolls and become fixed. Therefore, the steel plate conveying equipment according to this embodiment is preferably used for conveying steel plates 10 in the heating zone 12 or homogenization zone 14 of the continuous annealing equipment 100 where the steel plates 10 are heated to 700°C or higher. However, since deposits can adhere to the conveying rolls even at temperatures below 700°C, the steel plate conveying equipment according to this embodiment may also be applied to steel plates 10 conveyed at temperatures below 700°C.

[0023] Figure 2 is a schematic side view showing an example of the configuration of the steel plate conveying equipment 20 according to this embodiment. The steel plate conveying equipment 20 according to this embodiment includes a conveying roll 22, a polishing roll 24, and a recovery container 26. The conveying roll 22 is a brush roll having a plurality of metal wires protruding radially from the circumferential surface of the roll. Note that a conventional drive device for rotating a non-brush roll can be used to rotate the conveying roll 22.

[0024] The diameter of the multiple metal wires protruding radially from the roll surface is preferably between 20 μm and 500 μm. This allows for improved adhesion removal while suppressing increases in manufacturing costs and shortening of the brush roll's lifespan. On the other hand, if the wire diameter is less than 20 μm, mass production of the brush roll becomes difficult, increasing the manufacturing cost, which is undesirable. Furthermore, if the wire diameter is less than 20 μm, the wire wears faster, shortening the brush roll's lifespan, which is also undesirable. In addition, if the wire diameter is larger than 500 μm, the contact area between the adhesion and the wire increases, reducing the adhesion removal efficiency, which is also undesirable.

[0025] The length from the tip of each of the multiple metal wires protruding radially from the roll surface is preferably between 1 mm and 30 mm. This helps to prevent the brush roll from becoming too short and allows for stable transport of the steel plate 10. On the other hand, if the wire length is less than 1 mm, the brush roll will be shortened due to wire wear, which is undesirable. Also, if the wire length is longer than 30 mm, the wire will deform due to a decrease in density at the tip, making the transport of the steel plate 10 unstable, which is also undesirable.

[0026] The wire is preferably made of tungsten, molybdenum, cobalt, nickel-chromium alloy, or stainless steel, which have heat resistance and wear resistance. This allows the conveyor rolls to be polished and deposits removed even in high-temperature environments of 700°C or higher.

[0027] It is preferable to use a heat-resistant metal such as heat-resistant cast steel, chromium alloy, or nickel alloy for the roll portion of the brush roll. Furthermore, it is preferable that the wire density in the brush roll be 3 / 5 or more of the roll surface area in which the wires are embedded. By using a high-density brush roll with a high wire density, wire damage due to wear is reduced, and the durability of the brush roll is improved.

[0028] The polishing roll 24 is, for example, a roll made of heat-resistant cast steel with a cermet or ceramic coating applied to its circumferential surface. The polishing roll 24 is positioned in contact with the circumferential surface of the conveying roll 22 to remove any deposits adhering to it. Preferably, the polishing roll 24 rotates in a direction opposite to the rotation direction of the conveying roll 22 at the contact point with the conveying roll 22. This promotes the removal of deposits from the conveying roll 22. The polishing roll 24 is an example of a polishing member used to polish the conveying roll 22. Instead of the polishing roll 24, a steel or ceramic flat plate or grinding wheel with the same width as the conveying roll 22 may be used as the polishing member. When a flat plate is used as the polishing member, it is preferable that the mounting angle of the flat plate is an acute angle less than 90° with respect to the roll surface of the conveying roll 22. This suppresses increases and fluctuations in the torque load of the conveying roll without hindering the rotation of the conveying roll 22.

[0029] Furthermore, if there is a difference in peripheral speed between the polishing roll 24 and the conveying roll 22, it is not necessary to rotate the polishing roll 24 in the opposite direction to the conveying roll 22 at the contact point. In other words, if there is a difference in peripheral speed between the polishing roll 24 and the conveying roll 22, the polishing roll 24 may be rotated in the same direction as the conveying roll 22 at the contact point with the conveying roll 22. The difference in peripheral speed between the polishing roll 24 and the conveying roll 22 should be between 1 m / min and 1000 m / min. This allows the polishing roll 24 to remove any deposits adhering to the surface of the conveying roll 22.

[0030] Preferably, the polishing roll 24 has a control configuration (not shown) that can control the pressing force against the conveyor roll 22 based on its rotational load. Having such a control configuration avoids excessive wear of the wire due to contact with the conveyor roll 22 and allows the appropriate external force to be applied to the conveyor roll 22 for removing deposits. Alternatively, the polishing roll 24 may be brought into contact with the conveyor roll 22 when deposit removal is necessary, and the pressing force of the polishing roll 24 may be set to 0, i.e., the polishing roll 24 may not be brought into contact with the conveyor roll 22, when deposit removal is not necessary. This further reduces wire wear on the brush roll and extends the life of the brush roll.

[0031] It is preferable to use a polishing roll 24 with a diameter smaller than that of the conveying roll 20 and with a roll diameter of 100 mm or more. This suppresses a decrease in the roll life of the first polishing roll 32 and deformation due to bending. It is also preferable to use a polishing roll 24 that has a shorter axial length than the conveying roll 22. By moving the polishing roll 24, which has a shorter axial length than the conveying roll 22, in the axial direction of the conveying roll 22 to polish the conveying roll 22, the conveying roll 22 can be polished uniformly in the width direction along the crown shape of the conveying roll 22 that has been deformed by thermal crowning. Furthermore, it is even more preferable that the polishing roll 24 is a barrel-shaped roll (crown roll) in which the diameter of the central part in the axial direction is larger than the diameters of the ends, and the central part and the ends are smoothly connected by a tapered or R shape. By using a barrel-shaped roll, uneven contact with the conveying roll 22 is suppressed, and the conveying roll 22 can be polished uniformly in the width direction.

[0032] The recovery container 26 is a steel box for recovering material (hereinafter referred to as "removed material") that falls off the conveyor roll 22. By providing the recovery container 26, the removed material from the conveyor roll 22 can be recovered, and it is possible to prevent the removed material from reattaching to the steel plate 10 or to the continuous annealing equipment 100. Note that the recovery container 36 is an example of a recovery device for recovering material removed from the conveyor roll 22.

[0033] Figure 3 is a schematic side view showing another configuration example of the steel plate conveying equipment according to this embodiment. In the steel plate conveying equipment 30 shown in Figure 3, the same reference numerals are used for components that are the same as those in the steel plate conveying equipment 20 shown in Figure 2, and their descriptions are omitted. The steel plate conveying equipment 30 shown in Figure 3 differs from the steel plate conveying equipment 20 shown in Figure 2 in that it has brush rolls as polishing rolls 32 and a steel flat plate 34 for polishing the brush rolls.

[0034] As shown in Figure 3, a brush roll having multiple metal wires on its surface may be used as the polishing roll 32 for polishing the conveying roll 22. This reduces the adhesion between the polishing roll and the adhering material, even if it adheres to the polishing roll 32, allowing the material to be easily removed from the polishing roll 32. Furthermore, by providing a flat plate 34 for polishing the polishing roll 32, the material can be easily removed from the polishing roll 32.

[0035] Figure 4 is a schematic side view showing another configuration example of the steel plate conveying equipment according to this embodiment. In the steel plate conveying equipment 40 shown in Figure 4, the same reference numerals are used for components that are the same as those in the steel plate conveying equipment 20 shown in Figure 2, and their descriptions are omitted. The steel plate conveying equipment 40 shown in Figure 4 differs from the steel plate conveying equipment 20 shown in Figure 2 in that the conveying rolls 22 are located on the hearth side and that it has a dust collection device 42 but does not have a recovery container 26.

[0036] Since the weight of the steel plate 10 does not act on the conveying roll 22 on the hearth side, the surface pressure from the steel plate 10 is reduced. As a result, the growth of deposits adhering to the conveying roll 22 is less than in the configuration shown in Figure 2. However, even in the configuration shown in Figure 4, deposits adhere to the conveying roll and grow from these deposits. Therefore, by using the steel plate conveying equipment 40 according to this embodiment, the deposits adhering to the roll surface can be easily removed, and as a result, the growth of deposits on the surface of the conveying roll 22 can be suppressed.

[0037] In the configuration shown in Figure 4, unlike the configuration shown in Figure 2, there is no space to collect the fallen material due to gravity, so it is preferable to provide a dust collection device 42 instead of a collection container 26. By providing a dust collection device 42 in this way, it is possible to suppress the reattachment of material that has fallen from the conveyor roll 22 to the steel plate 10 or the conveyor roll 22. Note that the dust collection device 42 is another example of a collection device for collecting material that has fallen from the conveyor roll 22.

[0038] As described above, by using the steel plate conveying equipment according to this embodiment, any deposits adhering to the surface of the conveying rolls can be easily removed, thereby suppressing the growth of deposits on the surface of the conveying rolls 22. Furthermore, by suppressing the growth of deposits on the conveying rolls 22 in this way, the occurrence of indentation defects in the steel plate 10 caused by such deposits can also be suppressed. In other words, by conveying the steel plate 10 using the steel plate conveying equipment according to this embodiment in the continuous annealing equipment 100, it becomes possible to manufacture annealed steel plates with suppressed indentation defects.

[0039] In this embodiment, the steel plate conveying equipment 20, 30, and 40 have been described in an example where they have a recovery device, but the embodiment is not limited to this. To solve the problem of easily removing deposits adhering to the conveying roll 22 and suppressing the growth of such deposits, the steel plate conveying equipment 20, 30, and 40 do not necessarily have a recovery device. However, as described above, having a recovery device suppresses the re-adhesion of deposits detached from the conveying roll and the first polishing roll to the steel plate 10 and the conveying roll 22, so it is preferable that the steel plate conveying equipment 20, 30, and 40 have a recovery device. [Examples]

[0040] [Example 1] Next, we will describe Example 1, in which we continuously annealed 2000 tons or more of steel sheets containing 0.3 mass% or more of Si or Mn in the continuous annealing equipment 100 shown in Figure 1, and then confirmed the number of deposits of 100 μm or more attached to the conveyor rolls. In Example 1, the thickness of the steel sheets continuously annealed was in the range of 0.6 to 1.8 mm, and the width was in the range of 800 to 1500 mm. The continuous annealing conditions were as follows.

[0041] Ambient temperature: 700℃ or higher Atmospheric gas: 5% hydrogen by volume, 95% nitrogen by volume Dew point: -35℃

[0042] After continuous annealing, the conveyor roll installed on the furnace top side of the lower stage of the soaking zone, where the steel plate temperature is highest within the continuous annealing equipment 100, was removed, and the number of deposits attached to the conveyor roll was checked.

[0043] In this invention example, a brush roll was used as the conveyor roll. The brush roll had a diameter of 800 mm, the wire material was a Ni-Cr alloy, the wire diameter was 10 μm, the length to the wire tip was 15 mm, and the wire density was 3 / 5, which is the ratio of the wire embedding area to the roll surface area. When a polishing member was used to polish the conveyor roll, a polishing roll was used, which was a heat-resistant cast steel roll with cermet sprayed onto its circumferential surface. By bringing the polishing roll into contact with the brush roll at a predetermined peripheral speed difference, the deposits adhering to the brush roll were removed. The pressing force of the polishing roll against the brush roll was adjusted to 0.02 kgf / mm. The removed deposits (detached material) were collected in a collection container. After continuous annealing, the brush roll was removed, and the number of deposits larger than 100 μm was checked on the brush roll surface using a laser microscope.

[0044] On the other hand, in the comparative example, a conveyor roll was used in which cermet or ceramics was thermally sprayed onto the circumferential surface of a heat-resistant cast steel roll. The diameter of the conveyor roll was 800 mm. Furthermore, when a polishing member was used to polish the conveyor roll, a polishing roll was used in which cermet was thermally sprayed onto the circumferential surface of a heat-resistant cast steel roll. The polishing roll was brought into contact with the conveyor roll with the same pressing force as in the inventive example at a predetermined peripheral speed difference to remove the deposits adhering to the conveyor roll. The removed deposits (detached material) were collected in a collection container. After continuous annealing, the conveyor roll was removed, and the number of deposits larger than 100 μm was checked on the surface of the conveyor roll using a laser microscope. The results of Example 1 are shown in Table 1 below.

[0045] [Table 1]

[0046] In Table 1, a peripheral speed difference of ">160-500" means that the peripheral speed difference fluctuated within the range of 160-500 m / min. This fluctuation in peripheral speed difference is due to fluctuations in the peripheral speed of the conveyor roll caused by fluctuations in the line speed, but on average it was around 300 m / min. As shown in Table 1, in Invention Example 1-5, which uses a brush roll as the conveyor roll, the number of deposits larger than 100 μm adhering to the surface of the conveyor roll after continuous annealing was reduced compared to Comparative Example 1-4, which uses a conventional conveyor roll, regardless of the presence or absence of an abrasive member. Furthermore, by using an abrasive roll as the abrasive member and bringing the abrasive roll into contact with the conveyor roll under conditions where the peripheral speed difference is 1 m / min or more, the number of deposits adhering to the conveyor roll was greatly reduced.

[0047] On the other hand, in Comparative Examples 1-4, which used conventional conveying rolls, even when the polishing roll was brought into contact with the conveying roll at a peripheral speed difference of 160 m / min or more to remove the deposits, the number of deposits was greater than in any of the cases of Invention Examples 1-5. These results confirm that by using the steel plate conveying equipment according to this embodiment, deposits adhering to the surface of the conveying roll can be easily removed, thereby suppressing the growth of deposits on the surface of the conveying roll 22. Furthermore, since the number of deposits adhering to the surface of the conveying roll can be reduced in this way, it is clear that by conveying steel plates with the steel plate conveying equipment according to this embodiment in a continuous annealing facility, it is possible to manufacture high-quality annealed steel plates with fewer indentation defects.

[0048] [Example 2] Next, we will describe Example 2, which confirmed the effect of wire diameter on the brush roll. In Example 2, a small sample of a steel plate with a Si content of 1.6 mass% and a Mn content of 0.3 mass% and a brush roll were slid through a furnace with the furnace temperature controlled to 800°C to check the adhesion of deposits to the brush roll during the transport of the steel plate. The test conditions for Example 2 were as follows.

[0049] Wire material: Ni-Cr alloy Wire length: 12mm Sliding time: 30 hours Sliding speed: 300 mm / min Surface pressure between steel plate and brush roll: 0.001 kg / mm 2 Brush roll wire density: 3 / 5 (ratio of wire embedding area to roll surface area)

[0050] Under the above test conditions, a steel plate was slid against a brush roll for 30 hours. The number of deposits larger than 30 μm attached to the brush roll and the amount of wire wear after sliding were then measured. The number of deposits larger than 30 μm attached to the surface of the brush roll was measured by observing the surface of the brush roll with a laser microscope. The amount of wire wear was determined by measuring the wire length before and after the sliding test, and the difference between these measurements was taken as the amount of wear. The results of Example 2 are shown in Table 2 below.

[0051] [Table 2]

[0052] As shown in Table 2, reducing the diameter of the brush roll wire increased the amount of wire wear. In particular, it was confirmed that the amount of wire wear increased significantly when the wire diameter was less than 20 μm. From these results, it was confirmed that a wire diameter of 20 μm or more is preferable, as this can suppress wire wear.

[0053] On the other hand, as the wire diameter increases, the contact area with the deposits increases, and the adhesion force of the deposits to the brush roll surface increases. In particular, when the wire diameter exceeds 500 μm, the adhesion force of the deposits to the brush roll increases, and the number of deposits larger than 30 μm adhering to the brush roll surface increases significantly. From these results, it was confirmed that the wire diameter of the brush roll is preferably 500 μm or less, as this can suppress the adhesion of deposits.

[0054] [Example 3] Next, we will describe Example 3, in which the meandering behavior of the steel plate was confirmed by changing the length from the roll surface of the brush roll to the wire tip in the radial direction under the same conditions as Example 1. The diameter of the brush roll is 800 mm. The wire material is a high Ni-Cr alloy, the wire diameter is 50 μm, and the length from the roll surface to the wire tip in the radial direction of the roll was changed to 20, 30, and 40 mm. The amount of meandering of the steel plate was confirmed at the steering roll position that controls the meandering of the steel plate on the uniform tropical exit side.

[0055] The results of checking the amount of meandering of the steel plates showed that when the wire length of the brush roll was 20 mm and 30 mm, the average meandering of the steel plates was 32 mm and 35 mm, respectively. However, when the wire length was 40 mm, the average meandering of the steel plates increased to 59 mm, indicating a significant deterioration in the amount of meandering of the steel plates. From these results, it was confirmed that a wire length of 30 mm or less is preferable for the brush roll, as this stabilizes the conveyance of the steel plates and suppresses meandering of the steel plates. [Explanation of symbols]

[0056] 10 steel plate 12 Heating Zone 14. Average Tropical 16 Cooling Zones 18 Overaged zone 20 Steel plate conveying equipment 22 Conveyor Rolls 24 Abrasive Rolls 26 Collection containers 30 Steel plate conveying equipment 32 Abrasive Rolls 34 flat plate 40 Steel plate conveying equipment 42 Dust suction device 100 Continuous Annealing Equipment

Claims

1. A steel plate conveying device for conveying steel plates in a continuous annealing facility, A conveying roll for transporting the steel plate, A polishing member for polishing the aforementioned conveying roll, It has, The conveying roll is a brush roll having multiple metal wires protruding radially from its circumferential surface, and is a steel plate conveying device.

2. The steel plate conveying equipment according to claim 1, wherein the diameter of the wire is 20 μm or more and 500 μm or less.

3. The steel plate conveying equipment according to claim 1 or claim 2, wherein the length of the wire is 1 mm or more and 30 mm or less.

4. The steel plate conveying equipment according to claim 1 or claim 2, wherein the wire is made of tungsten, molybdenum, cobalt, nickel-chromium alloy, or stainless steel.

5. The steel plate conveying equipment according to claim 3, wherein the wire is made of tungsten, molybdenum, cobalt, nickel-chromium alloy, or stainless steel.

6. The steel plate conveying equipment according to claim 1 or claim 2, wherein the abrasive member is a flat plate, a grinding wheel, or a grinding roll.

7. The steel plate conveying equipment according to claim 3, wherein the abrasive member is a flat plate, a grinding wheel, or a grinding roll.

8. The steel plate conveying equipment according to claim 4, wherein the abrasive member is a flat plate, a grinding wheel, or a grinding roll.

9. The steel plate conveying equipment according to claim 1 or claim 2, further comprising a recovery device for recovering material that has fallen off the conveying roll.

10. The steel plate conveying equipment according to claim 3, further comprising a recovery device for recovering material that has fallen off the conveying roll.

11. The steel plate conveying equipment according to claim 4, further comprising a recovery device for recovering material that has fallen off the conveying roll.

12. The steel plate conveying equipment according to claim 5, further comprising a recovery device for recovering material that has fallen off the conveying roll.

13. A method for manufacturing annealed steel sheets, comprising conveying steel sheets using steel sheet conveying equipment according to claim 1 or claim 2, and annealing the steel sheets using the continuous annealing equipment to produce annealed steel sheets.

14. A method for manufacturing annealed steel sheets, comprising conveying steel sheets using the steel sheet conveying equipment described in claim 3, and annealing the steel sheets using the continuous annealing equipment to produce annealed steel sheets.

Citation Information

Patent Citations

  • Preheating furnace

    JP1983180269U

  • The hearth of the deposit removing device

    JP1985097761U

  • Descaling brush device for steel slab

    JP1987034618A

  • Carrying roll for roller hearth type heating furnace

    JP1989201417A

  • Production of polyolefin

    JP1991021606A