Thermoplastic elastomer composition containing magnetic powder
The thermoplastic elastomer composition with specific thermal and viscosity properties and high magnetic powder content addresses the fluidity and durability issues of conventional resin compositions, enabling low-pressure molding and reducing material damage from thermal expansion.
Patent Information
- Application Number
- JP2023525769
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-02
- Filing Date
- 2022-05-26
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-05-26
AI Technical Summary
Conventional resin compositions containing magnetic powder have low fluidity, requiring high-pressure injection molding, which can damage parts and result in poor dimensional accuracy and low productivity, while molded compositions with high magnetic powder content become hard and prone to thermal expansion damage.
A thermoplastic elastomer composition with a glass transition temperature below 0°C, melt viscosity of 1 to 5000 dPa·s, and containing 70% by mass or more of magnetic powder, preferably rare earth magnetic powder, exhibits excellent fluidity and low elasticity, allowing for low-pressure injection molding and improved thermal cycle durability.
The composition achieves high filling performance in injection molding, enables complex shape formation, and suppresses damage to contacting materials due to thermal expansion, with low elasticity and improved thermal cycle durability.
Smart Images

Figure 0007948179000001
Abstract
Description
[Technical Field]
[0001] This invention relates to a thermoplastic elastomer composition containing magnetic powder. [Background technology]
[0002] Because resin compositions containing magnetic powder are easier to mold than sintered magnets, they are used as magnetic components in various fields, such as electric vehicles, home appliances like PCs and vacuum cleaners, medical equipment like MRI machines, and power generators like wind turbines. As an example of a resin composition containing magnetic powder, Patent Document 1 discloses a bonded magnet having rare earth-based magnetic powder, a polyamide-based thermoplastic elastomer, and a polyamide-based thermoplastic resin. Patent Document 2 also discloses a bonded magnet containing a binder resin which is a polyimide that can be molded at 400°C or below, and magnetic powder. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2004-186214 [Patent Document 2] Japanese Patent Publication No. 2005-093835 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] In recent years, with the miniaturization and increased precision of equipment, higher moldability is required for resin compositions containing magnetic powder. Conventional resin compositions have low fluidity, requiring high-pressure injection molding. However, injecting resin compositions at high pressure can cause damage to parts containing the resin composition. While parts can be molded by encapsulation molding such as compression molding even with poor fluidity of the resin composition, dimensional accuracy is poor and productivity is low. Furthermore, molded resin compositions containing a large amount of magnetic powder become hard, and thermal expansion can compress and damage materials such as parts in contact with the molded body.
[0005] The present invention has been made in view of the above circumstances, and its objective is to provide a thermoplastic elastomer composition containing magnetic powder that has excellent fluidity during molding and low elasticity after molding. [Means for solving the problem]
[0006] The present invention, which solves the above problems, has the following configuration. [1] A thermoplastic elastomer composition comprising a thermoplastic elastomer having a glass transition temperature of less than 0°C and a melt viscosity of 1 to 5000 dPa·s at 250°C, and a magnetic powder.
[0007] [2] The thermoplastic elastomer composition according to [1], wherein the melting point of the thermoplastic elastomer is 30 to 195°C.
[0008] [3] The thermoplastic elastomer composition according to [1] or [2], comprising 70% by mass or more of the magnetic powder.
[0009] [4] The magnetic powder is a rare earth magnetic powder. The thermoplastic elastomer composition according to any one of [1] to [3].
[0010] [5] The thermoplastic elastomer composition according to any one of [1] to [4], wherein the thermoplastic elastomer is a polyester elastomer or a polyamide elastomer.
[0011] [6] The thermoplastic elastomer composition according to [5], wherein the polyester elastomer is a copolymerized polyester elastomer having 10% by mass or more of at least one selected from the group consisting of polyether polyols, polycarboxylic acids having one or more aliphatic hydrocarbon groups having 8 to 50 carbon atoms, and polyols having one or more aliphatic hydrocarbon groups having 8 to 50 carbon atoms as copolymerization units.
[0012] [7] The thermoplastic elastomer composition according to [5], wherein the polyamide elastomer is a copolymerized polyamide elastomer, and has, as a copolymerization unit, a polycarboxylic acid having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms.
[0013] [8] A molded article formed by molding the thermoplastic elastomer composition according to any one of [1] to [7].
Effects of the Invention
[0014] The thermoplastic elastomer composition containing the magnetic powder of the present invention has high fluidity. Therefore, the thermoplastic elastomer composition of the present invention has excellent filling performance in injection molding, and can be molded into various shapes. In addition, since the molded article of the thermoplastic elastomer composition of the present invention has low elasticity, damage to materials such as components in contact with the molded article can be suppressed even when thermal expansion occurs.
Modes for Carrying Out the Invention
[0015] The thermoplastic elastomer composition of the present invention is characterized by comprising a thermoplastic elastomer having a glass transition temperature of less than 0°C and a melt viscosity at 250°C of 1 to 5000 dPa·s, and magnetic powder. The thermoplastic elastomer composition of the present invention has good fluidity during molding due to the predetermined thermoplastic elastomer described above, and a molded article obtained by molding the composition has low elasticity.
[0016] Thermoplastic Elastomer Glass transition temperature: less than 0°C The thermoplastic elastomer of the present invention has a glass transition temperature of less than 0°C. By setting the glass transition temperature to less than 0°C, the molded article of the thermoplastic elastomer composition has low elasticity. It also contributes to improving thermal cycle durability. The thermal cycle durability means that when a component including a molded article of a thermoplastic elastomer composition is exposed to a thermal history of repeating high and low temperatures to cause thermal expansion and thermal contraction of the molded article, even if the material of the component (in particular, the component in contact with the molded article) (hereinafter referred to as a member) and the molded article have different expansion coefficients, damage such as cracking or peeling of the molded article does not occur at the contact interface portion between the molded article and the member, and no damage occurs on the member side in contact with the molded article. If the elastic modulus of the molded article is too high, cracking and peeling tend to occur during cooling. When the glass transition temperature of the thermoplastic elastomer is lower than 0°C, the elastic modulus can be kept low, and the thermal cycle durability can be improved. In addition, when the glass transition temperature is lower than 0°C, even if the molded article of the thermoplastic elastomer composition thermally expands, it has low elasticity, so the compressive stress on the contact member is relaxed, and damage to the member can also be prevented. The glass transition temperature of the thermoplastic elastomer is lower than 0°C, more preferably -10°C or lower, and even more preferably -30°C or lower. The lower limit is preferably -100°C or higher in consideration of blocking resistance. In the present invention, low elasticity means that the tensile elastic modulus at normal temperature based on JIS K6251:2017 is preferably less than 100 MPa, more preferably 80 MPa or less. The molded article of the thermoplastic elastomer composition and the member may be in a contact state or a non-contact state at normal temperature. Even if the molded article of the thermoplastic elastomer composition and the member are arranged so as not to be in contact with each other at normal temperature, the molded article of the thermoplastic elastomer composition may be exposed to a high temperature, thermally expand, and come into contact with the material.
[0017] Melt viscosity: 1 to 5000 dPa·s The thermoplastic elastomer of the present invention has a melt viscosity of 1 to 5000 dPa·s at 250°C. When the melt viscosity is within this range, the fluidity is excellent, so several hundred N / cm 2High filling rates can be achieved even with low injection pressure (hereinafter referred to as low injection pressure), and complex shapes can be molded. If the melt viscosity of the thermoplastic elastomer is too low, adhesion and cohesive force cannot be obtained. On the other hand, if the melt viscosity of the thermoplastic elastomer is too high, high-pressure injection molding is required to mold complex shapes, which can damage the mold or parts being enclosed. The melt viscosity of the thermoplastic elastomer is 1 dPa·s or more, preferably 5 dPa·s or more, more preferably 10 dPa·s or more, even more preferably 50 dPa·s or more, and even more preferably 100 dPa·s or more, and 5000 dPa·s or less, preferably 4000 dPa·s or less, more preferably 3000 dPa·s or less, and even more preferably 2000 dPa·s or less (i.e., 1 to 5000 dPa·s, preferably 5 to 4000 dPa·s, more preferably 10 to 3000 dPa·s, even more preferably 50 to 2000 dPa·s, and even more preferably 100 to 2000 dPa·s).
[0018] The method for measuring melt viscosity is as follows: The melt viscosity of thermoplastic elastomers is measured using a flow tester (Shimadzu CFT-500C). Specifically, the sample is dried to a moisture content of 0.1% or less, then heated to 250°C to stabilize it, and then passed through a die with a pore size of 1.0 mm and a thickness of 10 mm to measure 98 N / cm². 2 This is the viscosity when passed through under a certain pressure.
[0019] Melting point: 30℃~195℃ The melting point of the thermoplastic elastomer of the present invention is preferably 30°C to 195°C. If the melting point of the thermoplastic elastomer is too low, it will be liquid at room temperature, causing stickiness and burrs. If the thermoplastic elastomer composition is solid at the temperature of use, for example, room temperature, injection molding is possible and good handling is obtained. On the other hand, if the melting point of the thermoplastic elastomer is too high, the compatibility between the hard segments and soft segments will decrease, forming a non-uniform structural structure, which may reduce the mechanical properties of the molded article of the thermoplastic elastomer composition. The melting point of the thermoplastic elastomer is preferably 30°C or higher, more preferably 50°C or higher, even more preferably 70°C or higher, even more preferably 90°C or higher, and most preferably 110°C or higher, and preferably 195°C or lower, more preferably 180°C or lower, and even more preferably 170°C or lower (i.e., preferably 30-195°C, more preferably 50-180°C, even more preferably 70-170°C, even more preferably 90-170°C, and most preferably 110-170°C). Furthermore, any two or all of the above glass transition temperature, melt viscosity, and melting point of the thermoplastic elastomer can be combined, and any preferred configurations can be combined as desired.
[0020] Thermoplastic elastomer The thermoplastic elastomer of the present invention is preferably a thermoplastic elastic body having a polymer constituting a hard segment and a polymer constituting a soft segment. The thermoplastic elastomer of the present invention only needs to satisfy at least the above glass transition temperature and melt viscosity, and preferably have a melting point within a predetermined range. Examples include polyester elastomers, polyamide elastomers, polyolefin elastomers, and polyurethane elastomers. One type of thermoplastic elastomer may be used alone, or two or more types may be used in combination as appropriate. From the viewpoint of dispersibility of magnetic powder, preferred thermoplastic elastomers are polyester elastomers and polyamide elastomers. When using two or more types in combination, the following examples can be arbitrarily combined.
[0021] The composition and composition ratio of the thermoplastic elastomer of the present invention are determined by dissolving the sample in a solvent such as deuterated chloroform. 1 H-NMR and 13 It is calculated from the integrated value obtained by 13C-NMR.
[0022] The following describes the preferred polyester elastomers and polyamide elastomers used as thermoplastic elastomers in the present invention.
[0023] Polyester elastomer The polyester elastomer is preferably a copolymerized polyester elastomer. The copolymerized polyester elastomer is composed of a hard segment and a soft segment, and the hard segment is preferably polyester, and the soft segment is preferably at least one selected from the group consisting of polyether polyols, polycarboxylic acids having one or more aliphatic hydrocarbon groups having 8 to 50 carbon atoms, and polyols having one or more aliphatic hydrocarbon groups having 8 to 50 carbon atoms. A polyester elastomer that satisfies the above glass transition temperature and melt viscosity, and preferably the melting point, has high fluidity. Furthermore, a molded article of a composition containing the polyester elastomer and magnetic powder has low elasticity and contributes to the effect of improving thermal cycle durability.
[0024] As the acid component of the polyester constituting the hard segment, dicarboxylic acids such as aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and aliphatic dicarboxylic acids are preferred. Examples of aromatic dicarboxylic acids include terephthalic acid, 2,6-naphthalenedicarboxylic acid, diphenyldicarboxylic acid, isophthalic acid, orthophthalic acid, and 5-sodium sulfisoisophthalic acid. Examples of alicyclic dicarboxylic acids include cyclohexanedicarboxylic acid and tetrahydrophthalic anhydride. Examples of aliphatic dicarboxylic acids include oxalic acid, malonic acid, ethyl malonic acid, diethyl malonic acid, succinic acid, methyl succinic acid, 2,2-dimethyl succinic acid, 2,3-dimethyl succinic acid, tetramethyl succinic acid, glutaric acid, adipic acid, pimelic acid, and suberic acid. Among these, preferred are aromatic dicarboxylic acids such as terephthalic acid, 2,6-naphthalenedicarboxylic acid, and diphenyldicarboxylic acid, and more preferably terephthalic acid and 2,6-naphthalenedicarboxylic acid. The acidic components of the polyester that make up the hard segment may be used alone or in combination of two or more types.
[0025] The diol component of the polyester constituting the hard segment is not particularly limited, but aliphatic diols or alicyclic diols are preferably used. Examples of aliphatic diols include ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, 2-methyl-1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,2-butanediol, 1,5-heptanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,8-octanediol, 2-methyloctanediol, 1,9-nonanediol, 1,10-decanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 2,2,4-trimethyl-1,3-pentanediol, neopentyl hydroxypivalate, and 2-butyl-2-ethyl-1,3-propanediol. Examples of alicyclic diols include 1,4-cyclohexanedimethanol, ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, ethylene oxide adducts, propylene oxide adducts of hydrogenated bisphenol A, and tricyclodecanedimethyl. Among these, aliphatic diols are preferred, and ethylene glycol and 1,4-butanediol are more preferred. The polyester diol components that make up the hard segment may be used individually or in combination of two or more types.
[0026] The components constituting the soft segment are preferably at least one selected from the group consisting of polyether polyols, polycarboxylic acids having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms, and polyols having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms. These may be used individually or in combination of two or more.
[0027] A polyol having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms is preferably a dimer ol. The dimer ol is preferably a reduction reaction product derived from, for example, a dimer acid. The number of carbon atoms in the dimer ol is preferably 22 or more, more preferably 24 or more, preferably 44 or less, more preferably 40 or less, and most preferably 36 or less (i.e., preferably 22 to 44, more preferably 24 to 40, and most preferably 24 to 36). Examples of dimer ols include dimer dilinoleyl alcohol and dimer oleyl alcohol.
[0028] A polyether polyol can be any polyol having at least two ether bonds within its molecule. Furthermore, the repeating units in the main skeleton of the polyether polyol may be either saturated hydrocarbons or unsaturated hydrocarbons. Examples of polyether polyols include polyether polyols having an alicyclic structure or aliphatic polyether polyols, with aliphatic polyether polyols being preferred. Furthermore, the number of carbon atoms in the repeating units of the aliphatic polyether polyol is not particularly limited, but the number of carbon atoms in the repeating units is preferably 2 or more, more preferably 3 or more, even more preferably 4 or more, preferably 20 or less, more preferably 15 or less, and even more preferably 12 or less (i.e., preferably 2 to 20, more preferably 3 to 15, and even more preferably 4 to 12).
[0029] Examples of polyether polyols having an alicyclic structure include alkylene oxide diols of hydrogenated bisphenol A, alkylene oxide diols of hydrogenated bisphenol F, and alkylene oxide diols of 1,4-cyclohexanediol. Aliphatic polyether polyols include, for example, polyethylene glycol, polypropylene glycol, poly-1,2-propylene glycol, poly-2-methyl-1,3-propylene glycol, polytetramethylene glycol (PTMG), poly(tetramethylene glycol-neopentyl glycol) copolymers, block or random copolymers of ethylene oxide and propylene oxide, random copolymers of tetrahydrofuran and 3-methyltetrahydrofuran, and the like. Among these, polytetramethylene glycol (PTMG) is preferred, as it contributes to improving the fluidity of the polyester elastomer, imparts low elasticity to the molded article of the composition, and contributes to improving the durability of the thermal cycle. The components that make up the soft segment may be used individually or in combination of two or more types.
[0030] The number-average molecular weight of the polyether polyol constituting the soft segment is not particularly limited, but increasing the number-average molecular weight can improve thermal cycling durability and hydrolysis resistance. On the other hand, if the number-average molecular weight of the polyether polyol becomes too high, its compatibility with the hard segment may decrease. The number-average molecular weight of the polyether polyol is preferably 400 or more, more preferably 500 or more, even more preferably 600 or more, and particularly preferably 700 or more, and preferably 10,000 or less, more preferably 6,000 or less, even more preferably 4,000 or less, and particularly preferably 3,000 or less (i.e., preferably 400 to 10,000, more preferably 500 to 6,000, even more preferably 600 to 4,000, and particularly preferably 700 to 3,000).
[0031] The aliphatic hydrocarbon groups contained in the polycarboxylic acid having one or more aliphatic hydrocarbon groups having 8 to 50 carbon atoms may be either linear or branched, and the aliphatic hydrocarbon groups may be either aliphatic saturated hydrocarbon groups or aliphatic unsaturated hydrocarbon groups. The number of carbon atoms in the aliphatic hydrocarbon groups is 8 or more, preferably 10 or more, more preferably 15 or more, and 50 or less, preferably 45 or less, more preferably 40 or less (i.e., 8 to 50, preferably 10 to 45, more preferably 15 to 40). Furthermore, the polycarboxylic acid may also be a polymer of an unsaturated monocarboxylic acid or a polymer of an unsaturated dicarboxylic acid. Therefore, polycarboxylic acids having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms include, for example, polycarboxylic acids having one or more aliphatic unsaturated hydrocarbon groups with 8 to 50 carbon atoms, and polycarboxylic acids having one or more aliphatic saturated hydrocarbon groups with 8 to 50 carbon atoms. Examples of aliphatic unsaturated monocarboxylic acids include angelic acid, tigric acid, 4-pentenoic acid, 2-ethyl-2-butenoic acid, 2,4-hexadienoic acid, 10-undecenoic acid, oleic acid, 9-octadecenoic acid, 9-octadecinic acid, 9,12-octadecadienoic acid (linoleic acid), octadecatrienoic acid (linolenic acid), 5,8,11,14-eicosatetraenoic acid, 13-docosenoic acid, 11-octadecen-9-icic acid, and 21-triaconthenic acid. Examples of aliphatic unsaturated dicarboxylic acids include citraconic acid, mesaconic acid, 2-pentenioic acid, methylene succinic acid, allylmalonic acid, 2,4-hexadienioic acid, isopropylidene succinic acid, and dimer acids having an unsaturated group. Examples of aliphatic saturated dicarboxylic acids include azelaic acid, sebacic acid, dodecanediic acid, tridecanediic acid, and dimer acids that do not have an unsaturated group. Preferably, it is an aliphatic saturated carboxylic acid, more preferably a dicarboxylic acid having one or more aliphatic saturated hydrocarbon groups, and even more preferably a dimer acid without unsaturated groups. When it does not contain unsaturated bonds, it not only has excellent weather resistance and heat resistance, but can also contribute to improved fluidity and reduced elasticity. Examples of dimer acids that do not have unsaturated groups include plant fatty acids, preferably aliphatic unsaturated monocarboxylic acids with about 11 to 22 carbon atoms, more preferably aliphatic unsaturated monocarboxylic acids with about 18 carbon atoms such as oleic acid, linoleic acid, and linolenic acid, which are dimerized and then hydrogenated to saturate the unsaturated bonds. Dimer acids that do not have unsaturated groups may contain residual unsaturated bonds in their molecules.
[0032] Increasing the content of at least one of the following elements that constitute the soft segment of the polyester elastomer: polyether polyols, polycarboxylic acids having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms, and polyols having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms, results in good fluidity, elasticity, and thermal cycle durability. The content of at least one substance selected from the group consisting of polyether polyols, polycarboxylic acids having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms, and polyols having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms, which constitute the soft segments contained in the polyester elastomer, is preferably 10% by mass or more, more preferably 40% by mass or more, and even more preferably 60% by mass or more. There is no particular upper limit, but considering heat resistance and blocking resistance, the content of polyols and / or polycarboxylic acids having one or more hydrocarbon groups with 8 to 50 carbon atoms is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less. Note that the content is the total amount when two or more substances are used in combination (i.e., preferably 10 to 80% by mass, more preferably 40 to 75% by mass, and even more preferably 60 to 70% by mass). Furthermore, any two or all of the following can be combined: the content, the number-average molecular weight, and the ester group concentration. In addition, any combination of preferred configurations can be used.
[0033] number average molecular weight The number average molecular weight of the polyester elastomer of the present invention is not particularly limited, but increasing the number average molecular weight can improve the mechanical strength. On the other hand, if the number average molecular weight of the polyester elastomer is too large, the melt viscosity at 200°C may become excessively high. The number average molecular weight of the polyester elastomer is preferably 3000 or more, more preferably 5000 or more, still more preferably 7000 or more, and preferably 50000 or less, more preferably 40000 or less, still more preferably 30000 or less (that is, preferably 3000 to 50000, more preferably 5000 to 40000, still more preferably 7000 to 30000). The number average molecular weight can be measured in a chloroform solvent using gel permeation chromatography (GPC), with a polystyrene solution as the standard substance and the sample for the GPC calibration curve.
[0034] Ester group concentration The ester group concentration of the polyester elastomer is not particularly limited, but increasing the ester group concentration can improve the chemical resistance to gasoline, engine oil, alcohol, general-purpose solvents and the like. On the other hand, if the ester group concentration is too high, the hydrolysis resistance to withstand high-temperature steam may decrease, resulting in poor long-term durability. The ester group concentration of the polyester elastomer is preferably 1500 equivalents / 10 6 g or more, more preferably 2000 equivalents / 10 6 g or more, and preferably 8000 equivalents / 10 6 g or less, more preferably 7500 equivalents / 10 6 g or less, still more preferably 7000 equivalents / 10 6 g or less (that is, preferably 1500 to 8000 equivalents / 10 6 g, more preferably 2000 to 7500 equivalents / 10 6 g, still more preferably 2000 to 7000 equivalents / 10 6 g). The unit of the ester group concentration is expressed as the number of equivalents per 1 ton of resin, and is a value calculated from the composition of the polyester resin and its copolymerization ratio.
[0035] The hard segment components and soft segment components of the polyester elastomer may be copolymerized or mixed together. The polyester elastomer of the present invention can be produced by known methods. For example, a method in which a dicarboxylic acid component and a diol component, which are hard segment components, and a soft segment component are subjected to a transesterification or esterification reaction in the presence of a catalyst, and the resulting reaction product is polycondensed; a method in which a hard segment polyester is prepared in advance, and a soft segment component is added to it and randomized by a transesterification reaction; and a method in which the hard segment and soft segment are linked together with a chain linker.
[0036] Polyamide elastomer The polyamide elastomer is preferably a copolymerized polyamide elastomer. The copolymerized polyamide elastomer is preferably composed of a hard segment and a soft segment, where the hard segment is preferably a polyamide and the soft segment is preferably a polycarboxylic acid having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms. A polyamide elastomer that satisfies the above glass transition temperature and melt viscosity, and preferably the melting point, has high fluidity. Furthermore, a molded article of a composition containing the polyamide elastomer and magnetic powder has low elasticity and contributes to the improvement of thermal cycle durability.
[0037] Examples of polyamides that constitute the hard segment include (1) condensed polymers of lactams, (2) polycondensates of ω-aminocarboxylic acids, and (3) copolymers of diamines and dicarboxylic acids. Examples of (1) lactams include aliphatic lactams such as lauryl lactam, ε-caprolactam, udecan lactam, ω-enanthractam, and 2-pyrrolidone. Examples of (2) ω-aminocarboxylic acids include aliphatic ω-aminocarboxylic acids such as 6-aminocaproic acid, 7-aminoheptanoic acid, 8-aminooctanoic acid, 10-aminocapric acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid. (3) Examples of diamines include aliphatic diamines such as ethylenediamine, trimethylenediamine, tetramethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 3-methylpentamethylenediamine, and metaxylenediamine. Examples of dicarboxylic acids include aliphatic dicarboxylic acids, alicyclic dicarboxylic acids, and aromatic dicarboxylic acids. Specifically, aliphatic dicarboxylic acids such as oxalic acid, malonic acid, ethyl malonic acid, diethyl malonic acid, succinic acid, methyl succinic acid, 2,2-dimethyl succinic acid, 2,3-dimethyl succinic acid, tetramethyl succinic acid, glutaric acid, adipic acid, pimelic acid, and suberic acid; and aromatic dicarboxylic acids such as terephthalic acid, 2,6-naphthalenedicarboxylic acid, diphenyldicarboxylic acid, isophthalic acid, orthophthalic acid, and 5-sodium sulfisoisophthalic acid. These may be used individually or in combination of two or more types.
[0038] Specific examples of polyamides include polybutyroamide (nylon 4), polycaproamide (nylon 6), polyhexamethylene adipamide (nylon 66), polytetramethylene adipamide (nylon 46), polytetramethylene sevacamide (nylon 410), polypentamethylene adipamide (nylon 56), polypentamethylene sevacamide (nylon 510), polyhexamethylene sevacamide (nylon 610), polyhexamethylene dodecamide (nylon 612), polydecamethylene adipamide (nylon 106), polydecamethylene sevacamide (nylon 1010), polydecamethylene dodecamide (nylon 1012), polyundecaneamide (nylon 11), and polydodecaneamide (nylon 12). Mixtures and copolymers of these materials are also examples. Among these, nylon 6 is preferred. Compositions containing nylon 6 and magnetic powder exhibit excellent fluidity and contribute to reducing the elasticity and improving the thermal cycle durability of molded polyamide elastomer compositions.
[0039] The polycarboxylic acid having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms that constitute the soft segment is the same as the polycarboxylic acid having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms that constitute the soft segment of the polyester elastomer described above, so no further explanation is provided. The soft segment of the polyamide elastomer is also preferably the dimer acid described above.
[0040] Increasing the content of polycarboxylic acids having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms in the polyamide elastomer results in good fluidity, elasticity, and thermal cycle durability. The polyamide elastomer contains polycarboxylic acids having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms, preferably 10% by mass or more, more preferably 40% by mass or more, and even more preferably 60% by mass or more. There is no particular upper limit, but considering heat resistance and blocking resistance, the content of polycarboxylic acids having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less (i.e., preferably 10 to 80% by mass, more preferably 40 to 75% by mass, and even more preferably 60 to 70% by mass). Furthermore, the content and the number-average molecular weight described below can be arbitrarily combined to create any preferred configuration.
[0041] number average molecular weight The number-average molecular weight of the polyamide elastomer of the present invention is not particularly limited, but increasing the number-average molecular weight can improve mechanical strength. On the other hand, if the number-average molecular weight of the polyamide elastomer is too high, the melt viscosity at 200°C may become too high. The number-average molecular weight of the polyamide elastomer is preferably 3000 or more, more preferably 5000 or more, even more preferably 7000 or more, preferably 50000 or less, more preferably 40000 or less, and even more preferably 30000 or less (i.e., preferably 3000 to 50000, more preferably 5000 to 40000, and even more preferably 7000 to 30000).
[0042] The hard segment components and soft segment components of the polyamide elastomer may be copolymerized or may be a mixture. The polyamide elastomer of the present invention can be produced by known methods. Examples include single-step polymerization, double-step polymerization, and prepolymerization methods.
[0043] magnetic powder The magnetic powder used in this invention can be any magnetic powder, and may be either soft magnetic powder or hard magnetic powder; various known magnetic powders can be used. Examples of magnetic powders include ferrite magnetic powder, alnico (Al-Ni-Co-Fe) magnetic powder, and rare earth magnetic powder. Among these, rare earth magnetic powder is preferred due to its excellent magnetic properties. Magnetic powder may be used individually or in combination of two or more types. When using two or more types in combination, the following examples can be arbitrarily combined.
[0044] Examples of ferrite magnetic powders include spinel-type ferrite magnetic powder and magnetoplanbite-type ferrite magnetic powder, with magnetoplanbite-type ferrite magnetic powder being preferred as it possesses magnetism even without an external magnetic field. Magnetoplumbite-type ferrite magnetic powders are magnetic powders represented by the chemical formula MO·6Fe2O3 (where M is an alkaline earth metal), and examples include barium ferrite magnetic powder, strontium ferrite magnetic powder, and barium-strontium ferrite magnetic powder.
[0045] Rare earth magnetic powder is an intermetallic compound containing a rare earth element and a transition metal, and may further contain boron (B). Examples of rare earth elements include La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Lu, and Y, and these may be used individually or in combination of two or more. Examples of transition metals include Fe, Co, and Ni, and these may be used individually or in combination of two or more. Rare earth magnetic powders include neodymium magnetic powders such as Nd-Fe-B, Nd-Fe-Co-B, (Nd,Pr)-Fe-B, (Nd,Pr)-Fe-Co-B, etc.; samarium cobalt magnetic powders such as Sm-Co, Sm-Co-Fe, Sm-Co-Mn; and Sm2-Fe. 17 -N3, Sm-Fe9-N 1.5 Examples include samarium iron nitrogen magnetic powders, and one or more of these may be used.
[0046] The average particle size of the magnetic powder is not particularly limited, but considering handling, miscibility with the resin, and the fluidity of the resin composition, the average particle size of the magnetic powder is preferably 1.0 μm or more, more preferably 2.0 μm or more, preferably 200 μm or less, and more preferably 100 μm or less. It is also preferable to mix magnetic powders with different particle sizes; for example, magnetic powders with particle sizes of 1 to 50 μm and magnetic powders with particle sizes of 50 to 100 μm may be mixed and used. When using multiple types of magnetic powder, they may be adjusted in advance to achieve the desired size, for example, by grinding them using a grinding device such as a jet mill, atomizer, ball mill, or bead mill. The magnetic powder may also be classified using a sieve or similar device as needed.
[0047] Thermoplastic elastomer composition The amount of magnetic powder contained in the thermoplastic elastomer composition can be adjusted as appropriate depending on the application, but if the amount of magnetic powder is too low, a sufficient magnetic flux density may not be obtained. On the other hand, if the amount of magnetic powder is too high, the fluidity and shape retention of the thermoplastic elastomer composition may decrease. The magnetic powder content is preferably 70% by mass or more, 80% by mass or more, 85% by mass or more, 90% by mass or more, and 95% by mass or more, in that order, with the upper limit preferably being less than 100% by mass, more preferably 99% by mass or less, and even more preferably 98% by mass or less (i.e., preferably 70 to less than 100% by mass, preferably 80 to less than 100% by mass, more preferably 85 to 99% by mass, more preferably 90 to 99% by mass, and even more preferably 95 to 98% by mass).
[0048] The thermoplastic elastomer composition may contain, as necessary, known additives in addition to the thermoplastic elastomer and magnetic powder. Furthermore, it may contain other thermoplastic elastomers not mentioned above.
[0049] In the thermoplastic elastomer composition, the amount of the thermoplastic elastomer in the remaining portion after removing the magnetic powder (hereinafter referred to as the non-magnetic powder portion) is preferably 30% by mass or more, 40% by mass or more, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, and 90% by mass or more, in that order, with higher amounts being preferable, and it may also be 100% by mass. If the content of the thermoplastic elastomer of the present invention is too low, sufficient fluidity may not be obtained, or the elasticity may not be sufficiently reduced, making it difficult to obtain the desired effects.
[0050] The thermoplastic elastomer composition may contain resins other than the thermoplastic elastomer of the present invention, preferably thermoplastic elastomers with a different composition from the thermoplastic elastomer of the present invention (hereinafter referred to as "other thermoplastic elastomers"), for the purpose of improving desired properties such as adhesion, flexibility, and durability. Examples of other thermoplastic elastomers include polyester elastomers, polyamide elastomers, polyolefin elastomers, epoxy elastomers, polycarbonate elastomers, acrylic elastomers, ethylene vinyl acetate elastomers, and phenol elastomers. One or more types of other thermoplastic elastomers may be included, but the content of other thermoplastic elastomers should not hinder the effects of the present invention, such as fluidity and elasticity.
[0051] The thermoplastic elastomer composition may contain various known additives as needed. Examples of additives include flame retardants, weathering agents, lightfastness agents, colorants, stress relievers, mold release agents, curing accelerators, antistatic agents, lubricants, slip agents, tackifiers, sealant improvers, antifogging agents, fragrances, and the like. In 100% by mass of the thermoplastic elastomer composition, the total content of various additives is preferably 5% by mass or less, more preferably 2% by mass or less, even more preferably 1% by mass or less, preferably 0.01% by mass or more, more preferably 0.1% by mass or more (i.e., preferably 5 to 0.01% by mass, more preferably 2 to 0.1% by mass, and even more preferably 1 to 0.1% by mass).
[0052] Examples of typical additives from the above list are provided below. Examples of flame retardants include halogen-based, phosphorus-based, nitrogen-based, and complex organic flame retardants; and inorganic flame retardants such as metal hydroxides, antimony-based, red phosphorus-based, silicone-based, and borate-based flame retardants. These may be used individually or in combination of two or more types. Examples of weather-resistant agents include antioxidants such as phenol and ultraviolet absorbers such as benzophenone compounds. Examples of light-resistant agents include benzophenone compounds, salicylate compounds, benzotriazole compounds, and hindered amine compounds. Examples of colorants include pigments such as kaolin, synthetic iron oxide red, cadmium yellow, nickel titanium yellow, strontium yellow, hydrated chromium oxide, chromium oxide, cobalt aluminate, and synthetic ultramarine blue; and dyes such as isoindolinone, isoindoline, quinophthalone, xanthene, diketopyrrolopyrrole, perylene, perinone, anthraquinone, indigoid, oxazine, quinacridone, benzimimidazolone, violancelon, phthalocyanine, and azomethine. These may be used individually or in combination of two or more. Examples of stress-relaxing agents include silicone oil, silicone rubber, acrylic rubber, urethane rubber, acrylonitrile-butadiene rubber, and thermoplastic elastomers. Examples of release agents include waxes such as fatty acid-based, fatty acid metal salt-based, and mineral-based waxes. Examples of curing accelerators include modified imidazole-based curing accelerators, modified aliphatic polyamine-based accelerators, and modified polyamine-based accelerators.
[0053] The thermoplastic elastomer composition of the present invention is obtained by mixing the above-mentioned predetermined thermoplastic elastomer with magnetic powder. In this case, after mixing each component in a predetermined proportion using a mixer, blender, etc., the thermoplastic elastomer composition may be granulated into any shape such as granules or pellets by adjusting it using a heat-pressure kneader, extruder, etc.
[0054] Molded body Various molded articles of any shape can be manufactured using the thermoplastic elastomer composition of the present invention. The thermoplastic elastomer composition can be molded using various known methods for thermoplastic elastomer compositions, such as injection molding, extrusion molding, compression molding, casting molding, and transfer molding. In particular, because the thermoplastic elastomer composition of the present invention has excellent fluidity, various molded articles of different shapes can be manufactured by injection molding. For example, in injection molding, a thermoplastic elastomer composition obtained by mixing magnetic powder, thermoplastic elastomer, and various additives in a mixer can be pelletized to facilitate injection molding. This pelletized composition is then filled into an injection molding machine, heated and melted, and injected into a mold to obtain a molded body. The molded body may be magnetized by applying an external magnetic field as needed. For example, in compression molding, a thermoplastic elastomer composition obtained by mixing magnetic powder, thermoplastic elastomer, and various additives in a mixer is filled into a compression molding machine, heated to the melting temperature, press-molded, and then cooled and solidified to obtain a molded body. The molded body may be magnetized by applying an external magnetic field as needed.
[0055] In particular, the thermoplastic elastomer composition of the present invention has excellent fluidity, making it suitable for injection molding and ideal for molding small, precise magnetic components.
[0056] Molded articles obtained by molding the thermoplastic elastomer composition of the present invention are suitable as magnetic components, such as rubber magnets for sensors and magnets for motor units. Examples of magnets for motor units include magnetic components for spindle motors for CDs, DVDs, and HDDs, vibration motors for mobile phones, actuators for digital cameras, and motors for automotive electrical components. Other examples of magnetic components include core magnets such as motor cores, stator cores, and rotor cores, and magnets for motor stators.
[0057] Because the thermoplastic elastomer composition of the present invention has excellent fluidity, magnetic resin solids with complex surface shapes, magnetic resin solids with thin-walled sections, and the like can be easily manufactured by molding them in the following process.
[0058] The thermoplastic elastomer composition of the present invention is heated to a temperature above the melting point of the thermoplastic elastomer, then the heated thermoplastic elastomer composition is poured into a mold, and subsequently cooled and solidified to complete the process.
[0059] The thermoplastic elastomer composition of the present invention is introduced into a mold and molded into a desired shape. The term "mold" refers to the inside of a mold having a certain shape, and examples include the inside of a container for molding, the inside of a mold, gaps in electronic components, and the inside of recesses on the surface of electronic components. The material of the mold is not particularly limited, but examples include metal and resin, and heat-resistant materials are preferred.
[0060] The method for introducing the thermoplastic elastomer composition of the present invention into a mold is not particularly limited and includes methods such as injecting the thermoplastic elastomer composition into the mold, dropping it into the mold, or pressing it into the mold. Specifically, methods such as injection molding, transfer molding, insert molding, compression molding, and hot melt molding can be used. The pressure when introducing the thermoplastic elastomer composition into the mold can be appropriately adjusted, for example, within a range of 0.1 MPa or more and 10 MPa or less.
[0061] A magnetic resin solid (molded product) is a thermoplastic elastomer composition that has been introduced into a mold and given a specific shape. The magnetic resin solid is not limited to having a specific shape when released from the mold, but may also have a specific shape within the mold. Furthermore, the magnetic resin solid can be used for purposes such as bonding, fixing, and sealing. For example, the magnetic resin solid may be bonded to the mold, or to a component other than the mold (hereinafter sometimes referred to as "other components"). The magnetic resin solid may also be bonded, fused, etc., to the mold and other components to bond or fix them together. The magnetic resin solid may also seal the mold, seal other components, or seal the mold and other components. Examples of other components include electronic components, resin plates, metal plates, resin rods, and metal rods. The shape of the magnetic resin solid is not particularly limited, but examples include sheet-like, polygonal prism-like, cylindrical, rectangular parallelepiped, rectangular prism-like, conical, pyramidal, and spherical shapes.
[0062] This application claims the benefit of priority based on Japanese Patent Application No. 2021-093228, filed on June 2, 2021. The entire specification of Japanese Patent Application No. 2021-093228, filed on June 2, 2021, is incorporated herein by reference. [Examples]
[0063] The present invention will be described in more detail below with reference to examples, but the present invention is not limited by the following examples, and it is certainly possible to implement it with appropriate modifications within the scope that is consistent with the spirit of the preceding and following descriptions, and all such modifications are included within the technical scope of the present invention. In the following, unless otherwise specified, "parts" means "parts by mass" and "%" means "percent mass".
[0064] Melting point, glass transition temperature Using a differential scanning calorimetry analyzer (Seiko Electronics Industries, Ltd., DSC220 model), 5 mg of the sample was placed in an aluminum pan, sealed by pressing down on the lid, and held at 255°C for 5 minutes to completely melt the sample. After rapid cooling with liquid nitrogen, measurements were taken from -150°C to 260°C at a heating rate of 20°C / min. The inflection point of the obtained curve was defined as the glass transition temperature, and the endothermic peak as the melting point. Melting points within the range of 30 to 195°C were rated as good (○), and those outside this range were rated as poor (×). A glass transition temperature of 0°C or less was evaluated as good (○), and outside this range was evaluated as poor (×).
[0065] melt viscosity Using a flow tester (Shimadzu Corporation CFT-500C model), a resin sample dried to a moisture content of 0.1% or less was filled into a cylinder in the center of a heating element set to 250°C. After 1 minute, a load (98N) was applied to the sample via a plunger, and the molten sample was extruded from a die (pore diameter: 1.0 mm, thickness: 10 mm) at the bottom of the cylinder. The descent distance and descent time of the plunger were recorded, and the melt viscosity was calculated. A melt viscosity within the range of 1 to 5000 dPa·s was evaluated as good (〇), and outside this range as poor (×).
[0066] Magnetic properties A 50mm x 10mm x 2mm test piece is placed on a 50mm x 10mm x 2mm steel plate, with a total area of 100mm. 2 The specimens were placed so that they overlapped, and the strength (adhesion strength) when pulled in the planar direction was measured using a load cell to investigate the magnetic properties of the test specimens. ○: Adhesion strength of 0.01 MPa or higher ×: Adhesion strength less than 0.01 MPa (including cases where adhesion does not occur)
[0067] Polyester elastomer (1) (Example 1) Terephthalic acid and 1,4-butanediol were added to a reaction vessel equipped with a stirrer, thermometer, and distillation condenser, and an esterification reaction was carried out at 170-220°C for 2 hours to obtain polybutylene terephthalate. Subsequently, 70 parts by weight of polytetramethylene glycol (PTMG1000, manufactured by Mitsubishi Chemical Corporation) with a number average molecular weight of 1000 was added to 30 parts by mass of the obtained polybutylene terephthalate, and the temperature was raised to 255°C while the pressure in the system was slowly reduced, reaching 665 Pa at 255°C over 60 minutes. A polycondensation reaction was then carried out at 133 Pa or less for 30 minutes to obtain polyester elastomer (1). The melting point of this polyester elastomer (1) was 150°C, the melt viscosity was 500 dPa·s, and the glass transition temperature was -70°C.
[0068] Polyester elastomer (2) (Example 2) Polyester elastomer (2) was synthesized in the same manner as polyester elastomer (1), except that 40 parts by weight of polybutylene terephthalate and 60 parts by weight of PTMG1000 were used. The melting point of polyester elastomer (2) was 160°C, the melt viscosity was 1000 dPa·s, and the glass transition temperature was -50°C.
[0069] Polyamide elastomer (Example 3) PA673 (manufactured by Henkel, melting point 160°C, melt viscosity 50 dPa·s, glass transition temperature -45°C) was used as the organic material (a polyamide elastomer containing dimer acid as a polymerization component).
[0070] Nylon 66 (Comparative Example 2) Gramide T-802 (manufactured by Toyobo Co., Ltd., melting point 220°C, glass transition temperature 50°C) was used as the organic material (nylon 66).
[0071] Polybutylene terephthalate (Comparative Example 3) Juranex 2002 (manufactured by Polyplastics, Inc., melting point 225°C, glass transition temperature 50°C) was used as the organic material (polybutylene terephthalate: PBT).
[0072] Polyester (Comparative Example 4) Byron GM-443 (manufactured by Toyobo Co., Ltd., melting point 140°C, melt viscosity 500 dPa·s, glass transition temperature 15°C) was used as the organic material (polyester).
[0073] Each organic material shown in Table 1 and a filler were mixed in predetermined proportions, and a thermoplastic composition was uniformly prepared in a kneader capable of pressurized heating and cooling. This thermoplastic composition was then fed into an extruder and hot-cut to obtain a granular thermoplastic composition.
[0074] Test specimens were prepared from the obtained granular thermoplastic composition using injection molding. Various physical properties were evaluated on the molded test specimens.
[0075] [Table 1]
[0076] Examples 1 to 3 are examples that satisfy the requirements of the present invention. The thermoplastic elastomer composition obtained by mixing polyester elastomer and magnetic powder exhibited excellent fluidity and good moldability. Furthermore, test specimens with low elasticity were obtained.
[0077] Comparative Example 1 is an example in which silica was used as a filler, and the test specimen did not exhibit magnetic properties. Comparative Examples 2 and 3 had excessively high melt viscosity in their thermoplastic compositions. As a result, the thermoplastic compositions mixed with magnetic powder did not flow during molding, leading to poor moldability. Furthermore, the thermoplastic compositions of Comparative Examples 2 and 3 had high glass transition temperatures, resulting in hard and inflexible test specimens. Comparative Example 4 is an example using a polyester resin with a high glass transition temperature, and the test specimen lacked flexibility.
Claims
1. A thermoplastic elastomer composition comprising a thermoplastic elastomer having a glass transition temperature of less than 0°C and a melt viscosity of 1 to 5000 dPa·s at 250°C, and a magnetic powder, The aforementioned thermoplastic elastomer is Copolymerized polyester elastomer, or A copolymerized polyamide elastomer having a polycarboxylic acid, The copolymerized polyester elastomer is composed of hard segments made of polyester. The copolymerized polyamide elastomer consists of a hard segment composed of polyamide and a soft segment composed of a polycarboxylic acid-derived component having one or more aliphatic hydrocarbon groups with 8 to 50 carbon atoms. The resin component in the thermoplastic elastomer composition consists solely of the copolymerized polyester elastomer or the copolymerized polyamide elastomer. Thermoplastic elastomer composition.
2. The thermoplastic elastomer composition according to claim 1, wherein the melting point of the thermoplastic elastomer is 30 to 195°C.
3. The thermoplastic elastomer composition according to claim 1, comprising 70% by mass or more of the magnetic powder.
4. The thermoplastic elastomer composition according to claim 1, wherein the magnetic powder is a rare earth magnetic powder.
5. The thermoplastic elastomer composition according to claim 1, wherein the copolymerized polyester elastomer contains 10% by mass or more of at least one selected from the group consisting of polyether polyols, polycarboxylic acids having one or more aliphatic hydrocarbon groups having 8 to 50 carbon atoms, and polyols having one or more aliphatic hydrocarbon groups having 8 to 50 carbon atoms, as copolymerization units.
6. The thermoplastic elastomer composition according to claim 5, wherein the polyether polyol is polytetramethylene glycol.
7. The thermoplastic elastomer composition according to claim 1, wherein the polycarboxylic acid is a dimer acid.
8. A molded article obtained by molding a thermoplastic elastomer composition according to any one of claims 1 to 7.
Citation Information
Patent Citations
Bonded magnet, compound therefor bonded magnet, and manufacture thereof
JP2001085209A
Bonding magnet
JP2004186214A
Composition for bonded magnet and the bonded magnet
JP2005072564A
Bond magnet
JP2005093835A
Composite for bonded magnet and its manufacturing method, and rotor magnet and brushless motor using the same