Piezoelectric element, piezoelectric actuator, droplet dispensing head, droplet dispensing device, and ferroelectric memory

By aligning the crystal planes of the Si substrate or Pt electrode with the PZT film and using a dielectric film, the piezoelectric element achieves a higher electromechanical coupling coefficient, improving the performance of piezoelectric actuators and ferroelectric memories.

JP7948194B2Active Publication Date: 2026-11-11KONICA MINOLTA INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023548416
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-09-16
Filing Date
2022-09-06
Publication Date
2026-11-11
Estimated Expiration
2042-09-06

AI Technical Summary

Technical Problem

Existing piezoelectric elements, particularly those using PZT films grown epitaxially, suffer from insufficient electromechanical coupling coefficients, necessitating the development of a piezoelectric element with higher piezoelectric characteristics.

Method used

The alignment of the (110) plane of the Si substrate or Pt electrode with the (100) plane of the PZT film, along with specific crystal orientations and the use of a dielectric film with a lower dielectric constant, allows for a piezoelectric element with a high electromechanical coupling coefficient by ensuring the PZT film is epitaxial rather than oriented.

Benefits of technology

This configuration results in a piezoelectric element with a higher electromechanical coupling coefficient, enhancing the performance of piezoelectric actuators, droplet ejection heads, and ferroelectric memories by improving piezoelectric constants and reducing dielectric constants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948194000009
    Figure 0007948194000009
  • Figure 0007948194000010
    Figure 0007948194000010
  • Figure 0007948194000011
    Figure 0007948194000011
Patent Text Reader

Abstract

The problem addressed by the present invention is to provide a piezoelectric element having a high electromechanical coupling coefficient, a piezoelectric actuator comprising the piezoelectric element, a liquid droplet discharging head, a liquid droplet discharging device, and a ferroelectric memory. The piezoelectric element of the present invention comprises a first electrode, a second electrode, and a lead zirconate titanate film positioned between the first electrode and the second electrode, and is characterized in that: the piezoelectric element is manufactured on a Si substrate, with a principal face of the Si substrate being a (001) face; the Si substrate has aligned crystal orientations in the in-plane direction and the out-of-plane direction; the (110) plane of the Si substrate and the (100) plane of the lead zirconate titanate film are parallel; and in an X-ray diffraction rocking curve measurement, the plane of symmetry reflection peak of the lead zirconate titanate film acquired by X rays input from the [100] direction of the Si substrate can be fitted with three component peaks.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a piezoelectric element, a piezoelectric actuator, a droplet discharge head, a droplet discharge apparatus, and a ferroelectric memory. More specifically, the present invention relates to a piezoelectric element and the like having a high electromechanical coupling coefficient.

BACKGROUND ART

[0002] Piezoelectric elements using PZT (lead zirconate titanate: Pb(Zr,Ti)O3) as a piezoelectric body are widely used. Further, in order to obtain a piezoelectric element with higher piezoelectric characteristics, development of a technique for epitaxially growing PZT to obtain a single-crystal PZT film has been carried out.

[0003] For example, Patent Document 1 discloses a ferroelectric thin film element formed by epitaxially growing PZT on a silicon substrate, a (TiAl)N thin film, and a SrRuO3 thin film. Further, Patent Document 2 discloses a film structure formed by epitaxially growing PZT on a silicon substrate, a ZrO2 film, a Pt film, and a SrRuO3 film.

[0004] However, even in piezoelectric elements formed by epitaxially growing PZT using the above-described techniques, the electromechanical coupling coefficient, which is an indicator of piezoelectric characteristics, is not sufficient, and a piezoelectric element with a higher electromechanical coupling coefficient has been demanded.

PRIOR ART DOCUMENTS

PATENT DOCUMENTS

[0005]

PATENT DOCUMENT 1

PATENT DOCUMENT 2

SUMMARY OF THE INVENTION

PROBLEMS TO BE SOLVED BY THE INVENTION

[0006] The present invention has been made in view of the above-mentioned problems and circumstances, and its objective is to provide a piezoelectric element with a high electromechanical coupling coefficient, as well as a piezoelectric actuator, a droplet ejection head, a droplet ejection device, and a ferroelectric memory equipped with the piezoelectric element. [Means for solving the problem]

[0007] In order to solve the above problems, the inventors investigated the causes of the above problems and found that, in a piezoelectric element comprising a first electrode, a second electrode, and a lead zirconate titanate film (hereinafter also referred to as "PZT film") located between the first and second electrodes, by aligning the (110) plane of the Si substrate or Pt electrode with the (100) plane of the PZT film, and forming the PZT film such that, in X-ray diffraction rocking curve measurement, the peak of the symmetry plane reflection of the PZT film obtained with X-rays incident from the

[0100] direction of the Si substrate or Pt electrode fits with three component peaks, it is possible to provide a piezoelectric element with a high electromechanical coupling coefficient, and thus arrived at the present invention. In other words, the above-mentioned problems according to the present invention are solved by the following means.

[0008] 1. A piezoelectric element comprising a first electrode, a second electrode, and a lead zirconate titanate film positioned between the first electrode and the second electrode, The piezoelectric element is fabricated on a Si substrate whose main surface is the (001) plane. The Si substrate has crystal orientations aligned in both the in-plane and out-of-plane directions. The (110) plane of the Si substrate and the (100) plane of the lead zirconate titanate film are parallel. In the rocking curve measurement using X-ray diffraction, the peak of the plane of symmetry reflection of the lead zirconate titanate film obtained with X-rays incident from the

[0100] direction of the Si substrate can be fitted with three component peaks. The angle of the interfacial angle formed by the (001) plane of the Si substrate and the (001) plane of the lead zirconate titanate film is within the range of 0.34 to 0.35°. A piezoelectric element characterized by the following features.

[0009] 2. A piezoelectric element comprising a first electrode, a second electrode, and a lead zirconate titanate film located between the first electrode and the second electrode, At least one of the first electrode or the second electrode includes a Pt electrode whose main surface is the (001) surface, The Pt electrode has crystal orientations aligned in both the in-plane and out-of-plane directions. The (110) plane of the Pt electrode and the (100) plane of the lead zirconate titanate film are parallel. In X-ray diffraction rocking curve measurement, the peak of the plane of symmetry reflection of the lead zirconate titanate film obtained with X-rays incident from the

[0100] direction of the Pt electrode can be fitted with three component peaks. A piezoelectric element characterized by the following features.

[0011] 4. The angle of the interfacial angle formed by the (001) plane of the Pt electrode and the (001) plane of the lead zirconate titanate film is within the range of 0.34 to 0.35°. The piezoelectric element according to paragraph 2, characterized in that it is a piezoelectric element.

[0012] 4. The angle of the interfacial angle formed by the (100) plane of the Si substrate and the (100) plane of the lead zirconate titanate film is within the range of 40 to 50°. Characterized by Section 1 The piezoelectric element described above.

[0013] 5. The angle of the interfacial angle formed by the (100) plane of the Pt electrode and the (100) plane of the lead zirconate titanate film is within the range of 40 to 50°. Characterized by Section 3 The piezoelectric element described above.

[0014] 6. The diffraction peak of the (004) plane of the lead zirconate titanate film, obtained by an out-of-plane 2θ-ω scan using X-ray diffraction, can be fitted with three component peaks. The first paragraph characterized by or paragraph 2 The piezoelectric element described above.

[0015] 7. The composition of the lead zirconate titanate constituting the lead zirconate titanate film is Pb X (Zr Y , Ti 1-Y )O3[1.0≦X≦1.2, 0.4≦Y≦0.6] The first paragraph characterized by or paragraph 2 The piezoelectric element described above.

[0016] 8. The thickness of the lead zirconate titanate film is within the range of 0.1 to 5.0 μm. The first paragraph characterized by or paragraph 2 The piezoelectric element described above.

[0017] 9. At the interface between the second electrode and the lead zirconate titanate film, there is a dielectric film composed of a dielectric with a lower dielectric constant than the lead zirconate titanate constituting the lead zirconate titanate film. The dielectric film and the lead zirconate titanate film are in an epitaxial relationship such that the (100) plane of the dielectric film and the (100) plane of the lead zirconate titanate film are parallel. The first paragraph characterized by or paragraph 2 The piezoelectric element described above.

[0018] 10. The dielectric is lead lanthanum titanate. Characterized by Section 9 The piezoelectric element described above.

[0019] 11. The total thickness of the lead zirconate titanate film and the dielectric film is within the range of 0.1 to 5.0 μm. Characterized by Section 9 The piezoelectric element described above.

[0020] 13. The RMS value of the surface roughness on the second electrode side of the dielectric film is 5.0 nm or less. Characterized by Section 9 The piezoelectric element described above.

[0021] 14. When the first electrode is grounded and a voltage of 30V is applied to the second electrode, the piezoelectric constant measured is A, and when a voltage of 10V is applied to the second electrode, the piezoelectric constant measured is B, then B is 95% or more of A. The first paragraph characterized by or paragraph 2 The piezoelectric element described above.

[0022] 15. A piezoelectric actuator equipped with a piezoelectric element, The piezoelectric element is, , paragraph 2, paragraph 4, or paragraph 5 The piezoelectric element described above. A piezoelectric actuator characterized by the following features.

[0023] 16. A droplet dispensing head equipped with a piezoelectric actuator, The piezoelectric actuator, Section 15 The piezoelectric actuator described above. A droplet dispensing head characterized by the following features.

[0024] 17. A droplet dispensing device equipped with a droplet dispensing head, The aforementioned droplet dispensing head Section 16 This is a droplet dispensing head as described above. A droplet dispensing device characterized by the following features.

[0025] 18. A ferroelectric memory equipped with a piezoelectric element, The piezoelectric element is, or paragraph 2 The piezoelectric element described above. A ferroelectric memory characterized by the following features. [Effects of the Invention]

[0026] The above means of the present invention make it possible to provide a piezoelectric element with a high electromechanical coupling coefficient, as well as a piezoelectric actuator, a droplet ejection head, a droplet ejection device, and a ferroelectric memory equipped with the piezoelectric element.

[0027] The mechanism by which the effects of this invention manifest or the mechanism of action are speculated to be as follows.

[0028] The fact that the (110) plane of the Si substrate or Pt electrode is parallel to the (100) plane of the PZT film, and that the peak of the plane of symmetry reflection of the PZT film obtained with X-rays incident from the

[0100] direction of the Si substrate or Pt electrode in X-ray diffraction rocking curve measurement can be fitted with three component peaks, indicates that the crystalline phase of the PZT film is a mixed crystal of monoclinic and rhombus phases, and that the PZT film is an epitaxial film rather than an oriented film.

[0029] Here, an "oriented film" refers to a film whose crystal orientation is aligned in the out-of-plane direction but random in the in-plane direction, and is also called a "uniaxially oriented film." An "epitaxial film" refers to a film whose crystal orientation is aligned both in the out-of-plane and in-plane directions. Epitaxial films are formed when crystals grow aligned in a specific direction based on the regularity of the atomic arrangement of the crystals in the underlying layer. This type of growth is called "epitaxial growth." The relationship between an epitaxially grown film and the films that make up the layer on which that epitaxial growth originated is called an "epitaxial relationship."

[0030] In oriented films, the in-plane polarization is randomly oriented, so when an electric field is applied, the polarization rotates, and the dielectric constant increases. In contrast, epitaxial films are single-domain, so when an electric field is applied, the polarization rotates less easily, and the dielectric constant decreases. On the other hand, the remanent polarization is high, so despite the low dielectric constant, they can have a high piezoelectric constant.

[0031] The electromechanical coupling coefficient, which serves as an indicator of piezoelectric properties, is a value that can be obtained by the following equation (1).

[0032]

number

[0033] k 31,f 2 : Electromechanical coupling coefficient [%] d 31,f Piezoelectric constant [m / V] ε: Dielectric constant [F / m] s: Elastic compliance [m 2 / N]

[0034] As can be seen from this equation, a higher piezoelectric constant and a lower dielectric constant result in a higher electromechanical coupling coefficient. Therefore, the electromechanical coupling coefficient is higher in piezoelectric elements where the PZT film is an epitaxial film than in piezoelectric elements where the PZT film is an oriented film.

[0035] Furthermore, in the piezoelectric elements described in Patent Documents 1 and 2, although the PZT film is an epitaxial film, the (001) plane of the Si substrate and the (001) plane of the PZT film are parallel. In contrast, as can be seen from the fact that the peak of the symmetry plane reflection of the piezoelectric element of the present invention can be fitted with three component peaks, the (001) plane of the PZT film is not parallel to the (001) plane of the Si substrate, etc. Due to this difference, the piezoelectric element of the present invention has a different crystalline phase of the PZT film from conventional piezoelectric elements, and a high electromechanical coupling coefficient can be obtained.

[0036] These mechanisms of expression or action make it possible to provide piezoelectric elements and the like with high electromechanical coupling coefficients. [Brief explanation of the drawing]

[0037] [Figure 1] schematic cross-sectional view of a piezoelectric element [Figure 2] Schematic diagram of a sample used for measuring piezoelectric constants. [Figure 3] Schematic diagram of a piezoelectric constant measuring device [Figure 4] Results of out-of-plane XRD measurement of piezoelectric element No. 1 [Figure 5] Out-of-plane XRD measurement results of piezoelectric element No. 1 (enlarged) [Figure 6] Fitting curve when fitting a single component peak to the peak originating from the (004) plane of the PZT film of piezoelectric element No. 1. [Figure 7]Fitting curve when fitting the peak originating from the (004) plane of the PZT film of piezoelectric element No. 1 with three component peaks. [Figure 8] Results of in-plane XRD measurement of piezoelectric element No. 1 [Figure 9] Fitting curve when fitting a single component peak to the peak of symmetry plane reflection in RC measurement of piezoelectric element No. 1. [Figure 10] Fitting curve when fitting the peak of symmetry plane reflection from RC measurement of piezoelectric element No. 1 with two component peaks. [Figure 11] Fitting curve when fitting the peak of symmetry plane reflection from RC measurement of piezoelectric element No. 1 with three component peaks. [Figure 12] Results of out-of-plane XRD measurement of piezoelectric element No. 2 [Figure 13] Out-of-plane XRD measurement results of piezoelectric element No. 2 (enlarged) [Figure 14] Fitting curve when fitting a single component peak to the peak originating from the (004) plane of the PZT film of piezoelectric element No. 2. [Figure 15] Results of in-plane XRD measurement of piezoelectric element No. 2 [Figure 16] Fitting curve when fitting a single component peak to the peak of symmetry plane reflection in RC measurement of piezoelectric element No. 2. [Figure 17] Atomic force microscope image of the PLT film of piezoelectric element No. 1 [Figure 18] Atomic force microscope image of the PLT film of piezoelectric element No. 2. [Modes for carrying out the invention]

[0038] In one embodiment, the piezoelectric element of the present invention comprises a first electrode, a second electrode, and a lead zirconate titanate film located between the first electrode and the second electrode, wherein the piezoelectric element is fabricated on a Si substrate whose main surface is the (001) plane, the Si substrate has aligned crystal orientations in the in-plane and out-of-plane directions, the (110) plane of the Si substrate and the (100) plane of the lead zirconate titanate film are parallel, and in X-ray diffraction rocking curve measurement, the peak of the plane of symmetry reflection of the lead zirconate titanate film obtained with X-rays incident from the

[0100] direction of the Si substrate can be fitted with three component peaks.

[0039] Furthermore, in one embodiment, the piezoelectric element of the present invention is a piezoelectric element comprising a first electrode, a second electrode, and a lead zirconate titanate film located between the first electrode and the second electrode, wherein at least one of the first electrode or the second electrode includes a Pt electrode whose main surface is the (001) plane, the crystal orientation of the Pt electrode is aligned in the in-plane and out-of-plane directions, the (110) plane of the Pt electrode and the (100) plane of the lead zirconate titanate film are parallel, and in rocking curve measurement by X-ray diffraction, the peak of the plane of symmetry reflection of the lead zirconate titanate film obtained with X-rays incident from the

[0100] direction of the Pt electrode can be fitted with three component peaks.

[0040] These features are technical features common to or corresponding to the embodiments described below.

[0041] In embodiments of the piezoelectric element of the present invention, from the viewpoint of crystal structure, it is preferable that the angle formed between the (001) plane of the Si substrate or the Pt electrode and the (001) plane of the lead zirconate titanate film is within the range of 0.34 to 0.35°.

[0042] In embodiments of the piezoelectric element of the present invention, from the viewpoint of crystal structure, it is preferable that the angle formed between the (100) plane of the Si substrate or the Pt electrode and the (100) plane of the lead zirconate titanate film is within the range of 40 to 50°.

[0043] As an embodiment of the piezoelectric element of the present invention, from the viewpoint of crystal structure, it is preferable that the diffraction peak of the (004) plane of the lead zirconate titanate film obtained by out-of-plane 2θ-ω scanning of the X-ray diffraction method can be fitted with three component peaks.

[0044] As an embodiment of the piezoelectric element of the present invention, from the viewpoint of the piezoelectric constant, the composition of lead zirconate titanate constituting the lead zirconate titanate film is Pb X (Zr Y ,Ti 1-Y )O₃ [1.0≦X≦1.2, 0.4≦Y≦0.6] is preferable.

[0045] As an embodiment of the piezoelectric element of the present invention, the thickness of the lead zirconate titanate film is preferably in the range of 0.1 to 5.0 μm. Thereby, the displacement generating force required for the piezoelectric element can be obtained.

[0046] As an embodiment of the piezoelectric element of the present invention, at the interface between the second electrode and the lead zirconate titanate film, there exists a dielectric film composed of a dielectric material having a lower dielectric constant than lead zirconate titanate constituting the lead zirconate titanate film, and it is preferable that the dielectric film and the lead zirconate titanate film have an epitaxial relationship such that the (100) plane of the dielectric film and the (100) plane of the lead zirconate titanate film are parallel to each other. Thereby, the dielectric constant can be lowered, and the electromechanical coupling coefficient can be further improved.

[0047] As an embodiment of the piezoelectric element of the present invention, from the viewpoint of dielectric constant, it is preferable that the dielectric is lead lanthanum titanate.

[0048] As an embodiment of the piezoelectric element of the present invention, the total thickness of the lead zirconate titanate film and the dielectric film is preferably in the range of 0.1 to 5.0 μm. Thereby, the displacement generating force required for the piezoelectric element can be obtained.

[0049] In an embodiment of the piezoelectric element of the present invention, it is preferable that the RMS value of the surface roughness on the second electrode side of the dielectric film is 5.0 nm or less. This improves reliability during long-term operation and film adhesion.

[0050] In an embodiment of the piezoelectric element of the present invention, from the viewpoint of the linearity of the piezoelectric constant, when the first electrode is grounded and a voltage of 30V is applied to the second electrode, the piezoelectric constant measured is A, and when a voltage of 10V is applied to the second electrode, the piezoelectric constant measured is B, and it is preferable that B is 95% or more of A.

[0051] The piezoelectric actuator of the present invention is a piezoelectric actuator equipped with a piezoelectric element, characterized in that the piezoelectric element is the piezoelectric element of the present invention.

[0052] The droplet dispensing head of the present invention is a droplet dispensing head equipped with a piezoelectric actuator, wherein the piezoelectric actuator is the piezoelectric actuator of the present invention.

[0053] The droplet dispensing device of the present invention is a droplet dispensing device equipped with a droplet dispensing head, characterized in that the droplet dispensing head is the droplet dispensing head of the present invention.

[0054] The ferroelectric memory of the present invention is a ferroelectric memory equipped with a piezoelectric element, characterized in that the piezoelectric element is the piezoelectric element of the present invention.

[0055] The present invention, its components, and embodiments and models for carrying out the present invention will be described in detail below. In this application, "~" is used to mean that the numerical values ​​before and after it are included as the lower limit and upper limit.

[0056] <1. Overview of the piezoelectric element of the present invention> In one embodiment, the piezoelectric element of the present invention comprises a first electrode, a second electrode, and a PZT film located between the first and second electrodes, and is fabricated on a Si substrate whose main surface is the (001) plane, wherein the Si substrate has aligned crystal orientations in the in-plane and out-of-plane directions, the (110) plane of the Si substrate and the (100) plane of the PZT film are parallel, and the peak obtained by rocking curve measurement can be fitted with three component peaks to the symmetry plane reflection peak of the lead zirconate titanate film obtained by X-ray diffraction using X-rays incident from the

[0100] direction of the Si substrate.

[0057] Furthermore, in one embodiment, the piezoelectric element of the present invention is a piezoelectric element comprising a first electrode, a second electrode, and a PZT film located between the first electrode and the second electrode, wherein at least one of the first electrode or the second electrode includes a Pt electrode whose main surface is the (001) plane, the crystal orientation of the Pt electrode is aligned in the in-plane and out-of-plane directions, the (110) plane of the Pt electrode and the (100) plane of the PZT film are parallel, and the peak obtained by rocking curve measurement can be fitted with three component peaks in the symmetry plane reflection peak of the lead zirconate titanate film obtained by X-ray diffraction using X-rays incident from the

[0100] direction of the Pt electrode.

[0058] The PZT film and other materials used in piezoelectric elements are composed of crystals. In this invention, the "crystal planes" and "crystal orientations" of these crystals are expressed using Miller indices. A crystal is a collection of unit cells, and a unit cell is made up of a collection of planes made up of atoms. These planes made up of atoms are called "crystal planes." Furthermore, crystals are composed of crystal planes arranged parallel to each other at equal intervals, and the direction of this arrangement of crystal planes (perpendicular to the crystal planes) is called the "crystal orientation." Crystal planes are expressed using the plane index of the Miller indices, such as (100) plane, (110) plane, etc. Crystal orientations are expressed using the direction index (orientation index) of the Miller indices, such as the

[0100] direction.

[0059] In this invention, as the basis for Miller indices, the out-of-plane direction, which is the normal direction to the main surface of the Si substrate, is defined as the

[0001] direction, and the in-plane direction, which is parallel to the main surface of the Si substrate, and which is perpendicular to the (100) plane or the (010) plane, is defined as the

[0100] direction or the

[0010] direction, respectively. The

[0100] direction and the

[0010] direction are not distinguished because Si is a cubic phase and has rotational symmetry. Similarly, when defining the relationship with a Pt electrode instead of a Si substrate, the out-of-plane direction, which is the normal direction to the main surface of the Pt electrode, is defined as the

[0001] direction, and the in-plane direction, which is parallel to the main surface of the Pt electrode, and which is perpendicular to the (100) plane or the (010) plane, is defined as the

[0100] direction or the

[0010] direction, respectively. Pt also has rotational symmetry in the in-plane direction, so the

[0100] direction and the

[0010] direction are not distinguished.

[0060] <2. Configuration of the piezoelectric element> The piezoelectric element of the present invention comprises a first electrode, a second electrode, and a PZT film located between the first electrode and the second electrode.

[0061] Furthermore, it is preferable that the piezoelectric element of the present invention is fabricated on a Si substrate whose main surface is the (001) plane. However, since the Si substrate can be removed and used after the PZT film or the like is fabricated, the piezoelectric element of the present invention is not limited to being fabricated on a Si substrate.

[0062] Here, the term "main surface" in this invention refers to the surface with the largest surface area.

[0063] The materials for the first and second electrodes are not particularly limited, and Cr, Ni, Cu, Pt, Ir, Ti, Ir-Ti alloy, LaNiO3, SRO (SrRuO3), STO (SrTiO3), etc., can be used. The first electrode may consist of two or more electrodes. Similarly, the second electrode may also consist of two or more electrodes.

[0064] Preferably, at least one of the first or second electrode includes a Pt electrode, and the Pt electrode preferably has a (001) plane as its main surface and its crystal orientation is aligned in both the in-plane and out-of-plane directions. If one of the first or second electrode includes a Pt electrode, the other is preferably a Cu electrode.

[0065] Furthermore, the first or second electrode, which includes the Pt electrode, is preferably a two-layer structure that further includes an electrode made of another material. Examples of electrodes made of other materials include SRO electrodes and STO electrodes, with SRO electrodes being more preferable. The electrodes made of other materials are also preferably aligned in the in-plane and out-of-plane directions, similar to the Pt electrode.

[0066] The PZT film according to the present invention has a PZT composition in which Pb X (Zr Y , Ti 1-Y It is preferable in terms of the piezoelectric constant that O3[1.0≦X≦1.2, 0.4≦Y≦0.6].

[0067] In the piezoelectric element of the present invention, it is preferable that a dielectric film composed of a dielectric with a lower dielectric constant than the PZT constituting the PZT film exists at the interface between the second electrode and the PZT film. This allows for a reduction in dielectric constant and further improvement of the electromechanical coupling coefficient. The crystalline structure of the dielectric constituting the dielectric film is preferably a perovskite type structure. Examples of dielectrics with a perovskite type crystalline structure include lead titanate (PbTiO3), lead lanthanum titanate (PLT:(Pb,La)TiO3), and barium titanate (BaTiO3). Among these, those containing lead are preferred, and PLT is particularly preferred in terms of dielectric constant.

[0068] The piezoelectric element of the present invention may have other layers, for example, a ZrO2 layer or an HfO2 layer between the Si substrate and the first electrode.

[0069] The following are preferred configuration examples of the piezoelectric element of the present invention. However, the configuration of the piezoelectric element of the present invention is not limited to these. (1)Second electrode / dielectric film (PLT film) / PZT film / first electrode (SRO electrode + Pt electrode) / ZrO2 layer / Si substrate (2) Second electrode / dielectric film (PLT film) / PZT film / first electrode (SRO electrode + Pt electrode) / HfO2 layer / Si substrate (3) Second electrode / dielectric film (PLT film) / PZT film / first electrode (STO electrode + Pt electrode) / ZrO2 layer / Si substrate (4) Second electrode / dielectric film (PLT film) / PZT film / first electrode (STO electrode + Pt electrode) / HfO2 layer / Si substrate (5) 2nd electrode / dielectric film (PLT film) / PZT film / 1st electrode (SRO electrode + Pt electrode) / ZrO2 layer (6)Second electrode / PZT film / Second electrode (SRO electrode + Pt electrode) / ZrO2 layer / Si substrate (7)Second electrode / dielectric film (PLT film) / PZT film / first electrode (Pt electrode) / ZrO2 layer / Si substrate (8) 2nd electrode / dielectric film (PLT film) / PZT film / 1st electrode (SRO electrode + Pt electrode) / Si substrate

[0070] Among the above configuration examples, configuration (1) is particularly preferred. A schematic cross-sectional view of a piezoelectric element with configuration (1) is shown in Figure 1. The piezoelectric element 10 shown in Figure 1 is constructed by stacking a ZrO2 layer 12, a first electrode 13 (Pt electrode 14, SRO electrode 15), a PZT film 16, a dielectric film 17, and a second electrode 18 on a Si substrate 11.

[0071] In the piezoelectric element of the present invention, the thickness of the PZT film is preferably in the range of 0.1 to 5.0 μm. Furthermore, if a dielectric film is present, the total thickness of the PZT film and the dielectric film is preferably in the range of 0.1 to 5.0 μm. This ensures that the displacement generating force required for the piezoelectric element is obtained.

[0072] <3. Crystal structure> The piezoelectric element of the present invention is characterized in that the (110) plane of the Si substrate or Pt electrode and the (100) plane of the PZT film are parallel. When the PZT film is epitaxially grown in a relationship where the (110) plane of the Si substrate or Pt electrode and the (100) plane of the PZT film are parallel, the epitaxial strain received from the layer below the PZT film (e.g., the SRO layer) changes from compressive strain to tensile strain, stabilizing the mixed crystal state of the monoclinic phase and the rombohedral phase, and resulting in a high piezoelectric constant. Furthermore, because the PZT film is an epitaxial film, the dielectric constant is lower compared to an oriented film, and the electromechanical coupling coefficient can be increased.

[0073] In this invention, "the (110) plane of the Si substrate and the (100) plane of the PZT film are parallel" means that in in-plane X-ray diffraction (XRD) measurements, when X-rays are incident on the Si substrate from the

[0110] direction, a diffraction peak is obtained on the (H00) plane of the PZT film. Similarly, "the (110) plane of the Pt electrode and the (100) plane of the PZT film are parallel" means that in in-plane X-ray diffraction measurements, when X-rays are incident on the Pt electrode from the

[0110] direction, a diffraction peak is obtained on the (H00) plane of the PZT film.

[0074] From the viewpoint of crystal structure, the piezoelectric element of the present invention preferably has an interfacial angle formed by the (100) plane of the Si substrate or Pt electrode and the (100) plane of the PZT film in the range of 40 to 50°.

[0075] The angle of the interplanar angle formed by the (100) plane of the Si substrate or Pt electrode and the (100) plane of the PZT film can be confirmed in in-plane measurement by X-ray diffraction, from the diffraction peak of the (H00) plane of the PZT film when X-rays are incident from the

[0110] direction of the Si substrate or Pt electrode.

[0076] Furthermore, in piezoelectric elements having a dielectric film, it is preferable that the (100) plane of the dielectric film and the (100) plane of the PZT film are in an epitaxial relationship such that they are parallel.

[0077] The epitaxial relationship between the (100) plane of the dielectric film and the (100) plane of the PZT film, where they are parallel, can be confirmed by in-plane X-ray diffraction measurements, where diffraction peaks are obtained for both the (H00) plane of the PZT film and the (H00) plane of the dielectric film when X-rays are incident from the

[0110] direction of the Si substrate or Pt electrode.

[0078] The piezoelectric element of the present invention is characterized in that, in rocking curve measurement by X-ray diffraction, the peak of the symmetry plane reflection of the PZT film obtained with X-rays incident from the

[0100] direction of the Si substrate or Pt electrode can be fitted with three component peaks. A PZT film satisfying this condition has a monoclinic phase and a rombohedral phase, thus obtaining a high piezoelectric constant. Furthermore, since the PZT film is an epitaxial film, the dielectric constant is lower compared to an oriented film, and the electromechanical coupling coefficient can be increased.

[0079] In this invention, "fitting is possible with three component peaks" means that when fitting is performed while increasing the number of component peaks under the following fitting conditions, the coefficient of determination R 2 This means that the number of component peaks that do not exceed a certain value is three.

[0080] (Fitting conditions) We adopt the Symmetric Pseudo Voigt probability density distribution function, which is a mixture of the Lorentz function and the Gaussian function, as the fitting function. The function f is given by equation (2) below.

[0081]

number

[0082] In equation (2), I: peak intensity, η: ratio of Lorentz function to Gaussian function, h l h g: represents the full width at half maximum, and x0 represents the peak position. The combination of multiple peaks is given by the sum of their respective distribution functions. In this invention, each of the peaks that forms the basis of the combination is called a "component peak".

[0083] Also, the coefficient of determination R 2 It is defined by the following equation (3).

[0084]

number

[0085] In equation (3), yi = {y1, ... y N}: Observation point, y bar: Average of observation points, fi = {f1,···f N}: Represents an estimated value.

[0086] Furthermore, it is preferable that the piezoelectric element of the present invention has an interfacial angle formed by the (001) plane of the Si substrate or Pt electrode and the (001) plane of the PZT film within the range of 0.34 to 0.35°. This angle can be determined from the split width of each component peak when the peak of the symmetry plane reflection of the PZT film, acquired with X-rays incident from the

[0100] direction of the Si substrate or Pt electrode, is fitted with three component peaks in a rocking curve measurement by X-ray diffraction. Specifically, when the angles (3 in total) that maximize the peak intensity at each component peak are denoted as ω1, ω2, and ω3, respectively, the difference between ω1 and ω2, and the difference between ω2 and ω3 are calculated. The average value of these two differences (in other words, the value obtained by (ω3-ω1) / 2) becomes the interfacial angle formed by the (001) plane of the Si substrate or Pt electrode and the (001) plane of the PZT film.

[0087] <4. Piezoelectric constant> The piezoelectric element of the present invention, from the viewpoint of the linearity of the piezoelectric constant, has a piezoelectric constant d measured by grounding the first electrode and applying a voltage of 30V to the second electrode. 31,f Let A be the piezoelectric constant d measured by applying a voltage of 10V to the second electrode. 31,fWhen B is denoted as such, it is preferable that B is 95% or more of A. Also, from the viewpoint of polarization retention characteristics, the piezoelectric constant d measured by applying a voltage of -20V to the second electrode is also considered. 31,f When C is denoted as such, it is preferable that C is within the range of 40-50% of A. When C is within the range of 40-50% of A, it suggests that a ferroelectric material is imprinted, which relaxes the decrementing field and improves the polarization retention characteristics.

[0088] In the present invention, the piezoelectric constant d of the piezoelectric element 31,f This involves preparing a sample for measurement and performing measurements using that sample. Note that the piezoelectric constant d in this invention is... 31,f This refers to the piezoelectric constant obtained by the inverse piezoelectric effect.

[0089] The measurement sample is prepared using a piezoelectric element without a second electrode, fabricated on a Si substrate. The piezoelectric element without a second electrode is cut into strips measuring 2 mm x 15 mm. Next, approximately 3 mm of one end in the longitudinal direction is masked, and a second electrode of Cu, Al, Ag, etc., is deposited by sputtering or vacuum deposition. The thickness of the second electrode should be in the range of 0.05 to 0.2 μm. Next, the mask is removed, and a portion of the material other than the first electrode (approximately 2 mm at the end) in the area where the second electrode is not formed is removed by etching. After etching, Ag paste is applied to the exposed first electrode to serve as the first electrode contact for measurement. By performing the above operations, a sample for measuring the piezoelectric constant is prepared.

[0090] Figure 2 is a schematic diagram of a piezoelectric constant measurement sample viewed from above (the side of the second measurement electrode). The measurement sample 20 shown in Figure 2 consists of an exposed first electrode 13, a first electrode contact 22 coated on the first electrode 13, an exposed interelectrode layer 21, and a second electrode 18. Although not shown, a Si substrate is located below the first electrode. Here, "interelectrode layer 21" refers to the layer between the first electrode 12 and the second electrode 18, which includes a PZT film, a dielectric film, etc.

[0091] The sample to be measured is sandwiched between the lower and upper supports, and one end is restrained and fixed in a cantilever-like manner. The restraint point is at the same position as either the upper or lower support, and the distance from the upper restraint point to the other end of the sample to be measured is measured to determine the sample length l [m]. A lead wire is connected and drawn out from the first electrode contact, and on the second electrode side, a thin wire-like object that does not interfere with vibration is attached to the end of which the second electrode contact is formed, and a sine wave generated by a waveform generator is applied between the first electrode and the second electrode to be measured. The measurement frequency is 500 Hz, and the applied voltage is in the range of -30 V to +30 V. A laser is shone on the end of the sample to be measured, which vibrates due to the applied waveform, using a Doppler displacement meter to obtain a signal. The displacement δ [m] is calculated by performing a Fourier transform on this signal.

[0092] Figure 3 is a schematic diagram of the measuring device viewed from the side. One side of the measurement sample 20 is fixed by a lower support 31 and an upper support 32. The second electrode contact 23 is in contact with the second electrode 18 of the measurement sample. The measuring device 30 also includes a waveform generator 33 and a Doppler displacement meter 34.

[0093] The piezoelectric constant d is calculated using the calculated displacement and the following equation (4). 31,f It is possible to find this.

[0094]

number

[0095] δ: Displacement [m] d 31,f Piezoelectric constant [m / V] l: Length of the sample for measurement [m] V: Applied voltage [V] s1: Elastic compliance of PZT film [m 2 / N] s2: Elastic compliance of Si substrate [m 2 / N] t1: Distance between electrodes [m] t2: Si substrate thickness [m]

[0096] The elastic compliance s1 of the PZT film and the elastic compliance s2 of the Si substrate can be based on literature values.

[0097] <5. Surface roughness of the dielectric film> As described above, in the piezoelectric element of the present invention, it is preferable that a dielectric film is present at the interface between the second electrode and the PZT film. Furthermore, it is preferable that the RMS (root mean square) value of the surface roughness on the second electrode side of the dielectric film is 5.0 nm or less. More preferably, it is 2.0 nm or less, and even more preferably 1.6 nm or less. This improves reliability during long-term operation and film adhesion.

[0098] The RMS value of surface roughness can be measured, for example, using an atomic force microscope (Dimension Icon, manufactured by Bruker).

[0099] <6. Applications of Piezoelectric Elements> The piezoelectric actuator, droplet ejection head, droplet ejection device, and ferroelectric memory of the present invention are characterized by comprising the piezoelectric element of the present invention. The piezoelectric actuator, etc., is not particularly limited in its other configurations as long as it comprises the piezoelectric element of the present invention, and can be constructed using commonly used components.

[0100] In addition to the above, the piezoelectric element of the present invention can be used in applications such as piezoelectric microphones, vibration sensors, displacement sensors, ultrasonic detectors, oscillation circuits, resonators, ceramic filters, piezoelectric transformers, piezoelectric buzzers, ultrasonic motors, and the like. [Examples]

[0101] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, the units "parts" or "%" are used, and unless otherwise specified, they represent "parts by mass" or "mass%".

[0102] Piezoelectric elements No. 1 (the present invention) and No. 2 (a comparative example) were fabricated, and XRD, surface roughness of the PLT film, and electrical properties were measured using these piezoelectric elements. These measurements were performed under conditions of 23°C.

[0103] <Fabrication of Piezoelectric Element No. 1> An 8-inch substrate (manufactured by KRYSTAL) was used, consisting of layers in the order of SRO / Pt / ZrO2 / Si. In this substrate, the Si layer corresponds to the Si substrate in the present invention. In this substrate, the Pt layer and the SRO layer correspond to the first electrode, which consists of two layers: a Pt electrode and an SRO electrode. Each layer of this substrate has a crystal orientation aligned in both the in-plane and out-of-plane directions, and the main plane is the (001) plane.

[0104] A PZT film was formed on the SRO layer of the substrate by RF magnetron sputtering. The PZT ceramic target had an excess lead composition (Pb) with 25% more Pb than the stoichiometric composition. 1.25 (Zr 0.52 , Ti 0.48 We used the O3 product.

[0105] The thickness of the PZT film and the sputtering conditions are as follows: Thickness: 3.38 μm RF power supply...3.0kW Gas flow rate: Ar:O2 = 39.5:0.5 sccm Sputtering pressure: 0.2 Pa Circuit board setting temperature: 550℃

[0106] In the PZT film formation process described above, the PZT film was formed in two stages, with cleaning performed between the first and second stages.

[0107] Next, a dielectric film (PLT film) was formed on the PZT film by RF magnetron sputtering. The PLT ceramic target had an excess lead composition with 25% more Pb than the stoichiometric composition of Pb:La = 0.9:0.1 ((Pb 1.125 ,La 0.1We used TiO3.

[0108] The thickness of the dielectric film (PLT film) and the sputtering conditions are as follows: Thickness: 0.12 μm RF power supply...2.0kW Gas flow rate: Ar:O2 = 39.5:0.5 sccm Sputtering pressure: 0.2 Pa Circuit board setting temperature: 560℃

[0109] Piezoelectric element No. 1, without the second electrode formed, was fabricated using the procedure described above.

[0110] <Fabrication of Piezoelectric Element No. 2> A first electrode was formed on an 8-inch bare-Si wafer (Si substrate) with the (001) plane as its main surface using RF magnetron sputtering with an Ir-Ti alloy target.

[0111] The thickness of the first electrode and the sputtering conditions are as follows: Thickness: 0.12 μm RF power supply...0.75kW Gas flow rate: Ar:O2 = 38:2 sccm Sputtering pressure: 0.2 Pa Circuit board setting temperature: 350℃

[0112] Next, a dielectric film (PLT film) on the first electrode side was formed on the first electrode using the RF magnetron sputtering method. The PLT ceramic target had an excess lead composition with 25% more Pb than the stoichiometric composition of Pb:La = 0.9:0.1 ((Pb 1.125 ,La 0.1 We used TiO3.

[0113] The thickness of the dielectric film (PLT film) on the first electrode side and the sputtering conditions are as follows. Thickness: 0.12 μm RF power supply...2.0kW Gas flow rate: Ar:O2 = 39.5:0.5 sccm Sputtering pressure: 0.2 Pa Circuit board setting temperature: 560℃

[0114] Next, a PZT film was formed on the dielectric film on the first electrode side by RF magnetron sputtering. The PZT ceramic target had an excess lead composition (Pb) with 25% more Pb than the stoichiometric composition. 1.25 (Zr 0.52 , Ti 0.48 We used the O3 product.

[0115] The thickness of the PZT film and the sputtering conditions are as follows: Thickness: 3.26 μm RF power supply...3.0kW Gas flow rate: Ar:O2 = 39.5:0.5 sccm Sputtering pressure: 0.2 Pa Circuit board setting temperature: 550℃

[0116] Next, a dielectric film (PLT film) was formed on the PZT film by RF magnetron sputtering. The PLT ceramic target had an excess lead composition with 25% more Pb than the stoichiometric composition of Pb:La = 0.9:0.1 ((Pb 1.125 ,La 0.1 We used TiO3.

[0117] The thickness of the dielectric film (PLT film) and the sputtering conditions are as follows: Thickness: 0.12 μm RF power supply...2.0kW Gas flow rate: Ar:O2 = 39.5:0.5 sccm Sputtering pressure: 0.2 Pa Circuit board setting temperature: 560℃

[0118] Piezoelectric element No. 2, without the second electrode formed, was fabricated using the procedure described above.

[0119] <XRD measurement of piezoelectric element No. 1> Out-of-plane XRD measurements (out-of-plane 2θ-ω scan) were performed on piezoelectric element No. 1, which lacked a second electrode, under the following conditions. The out-of-plane measurements were performed in the range of 2θ = 10 to 110°. The X-rays were incident from the

[0100] direction on the Si substrate.

[0120] (Out-of-plane XRD measurement conditions) Measurement device: Rigaku SmartLab X-ray generation unit: Cathode Cu Output: 45kV 200mA Detection unit: Semiconductor detector Incident optical system: Ge(220) channel-cut monochromator Solar slit: Incident side - : Light receiving side 5.0° Slit: Incident side IS = 1 (mm) Length limit: 10 (mm) : Light receiving side RS1=1 RS2=1.1(mm) Scanning conditions: Scanning axis 2θ / ω Scanning mode: Continuous scanning Scanning range: 10-110° Step width 0.024° Scanning speed: 2° / min

[0121] Figure 4 shows the results of out-of-plane XRD measurement of piezoelectric element No. 1. From Figure 4, the 00L preferred orientation of the PZT and PLT films was confirmed. Focusing on the diffraction peak of the (004) plane observed at 2θ = 90 to 110°, the range of the horizontal axis is expanded to 2θ = 90 to 110°, resulting in Figure 5 below.

[0122] Figure 5 confirms that the diffraction peak of the (004) plane of the PZT film near 2θ=98° is not a single peak, but rather a peak formed by the superposition of multiple peaks.

[0123] The peak originating from the (004) plane of the PZT film near 2θ = 98° was fitted under the conditions described above.

[0124] When fitting is performed using one component peak, the graph is as shown in Figure 6, and the coefficient of determination is R 2 = 0.997724. On the other hand, when fitting was performed with three component peaks, the graph shown in Figure 7 was obtained, and the coefficient of determination was R 2 The result was 0.999931. Furthermore, even when fitting was performed with four or more component peaks, the peaks were either split into the same peak or no increase in the coefficient of determination was observed. From the above, it was confirmed that the diffraction peak of the (004) plane of the PZT film can be fitted with three component peaks at 2θ = 97.28°, 97.94°, and 98.47°.

[0125] Next, in-plane XRD measurements were performed on piezoelectric element No. 1, which lacked a second electrode, under the following conditions. Here, X-rays were incident from the

[0110] direction on the Si substrate. Measurements were taken in the range of 2θ = 10 to 110°.

[0126] (In-plane XRD measurement conditions) Measurement device: Rigaku SmartLab X-ray generation unit: Cathode Cu Output: 45kV 200mA Detection unit: Semiconductor detector Solar slit: Incident side vertical divergence angle 0.5° : Receiver side vertical divergence angle 0.5° Slit: Incident side IS = 0.1 (mm) Length limit: 10 (mm) : Receiver side RS1=20 RS2=20.1(mm) Scanning conditions: Scanning axis 2θχ / φ :Incidence angle ω 0.60° Scanning mode: Continuous scanning Scanning range: 10-110° Step width 0.024° Scanning speed: 2° / min

[0127] Figure 8 shows the results of in-plane XRD measurement of piezoelectric element No. 1. By incidenting X-rays parallel to the (110) plane of the Si substrate, the diffraction peak of the (H00) plane of the PZT film was obtained as shown in Figure 8, confirming that the (110) plane of the Si substrate and the (100) plane of the PZT film are parallel. Furthermore, since the (110) plane of the Si substrate and the (110) plane of the Pt electrode are parallel, it can be seen that the (110) plane of the Pt electrode and the (100) plane of the PZT film are parallel.

[0128] Furthermore, in Figure 8, the diffraction peak of the (H00) plane of the PZT film can be seen, confirming that the interfacial angle formed by the (100) plane of the Si substrate and the (100) plane of the PZT film is 45°. Additionally, since the (100) plane of the Si substrate and the (100) plane of the Pt electrode are parallel, it can be seen that the interfacial angle formed by the (100) plane of the Pt electrode and the (100) plane of the PZT film is 45°.

[0129] Furthermore, in Figure 8, the diffraction peaks of the (H00) plane of the PZT film and the (H00) plane of the PLT film can be observed, confirming that the (100) plane of the PLT film and the (100) plane of the PZT film are in an epitaxial relationship, being parallel to each other.

[0130] Rocking curve (RC) measurements were performed on the 002 lattice point reflection (2θ=44.3°) of the PZT film under the following conditions.

[0131] (Rocking curve measurement conditions) Measurement device: Rigaku SmartLab X-ray generation unit: Cathode Cu Output: 45kV 200mA Detection unit: Semiconductor detector Incident optical system: Ge(220) channel-cut monochromator Solar slit: Incident side - : Light receiving side 5.0° Slit: Incident side IS = 1 (mm) Length limit: 10 (mm) : Light receiving side RS1=1 RS2=1.1(mm) Scanning conditions: Evaluation diffraction plane PZT(002) :scan axis ω Scanning mode: Continuous scanning Scanning range: 10-30° Step width 0.024° Scanning speed: 2° / min

[0132] The peaks obtained from the rocking curve measurement were fitted under the conditions described above.

[0133] When fitting is performed using one component peak, the graph is as shown in Figure 9, and the coefficient of determination is R 2 = 0.992506. When fitting was performed with two component peaks, the graph was as shown in Figure 10, and the coefficient of determination was R 2 = 0.997887. When fitting was performed with three component peaks, the graph was as shown in Figure 11, and the coefficient of determination was R 2 The result was 0.999929. Even when fitting with four or more component peaks, the peaks were either split into the same peaks as when fitting with three component peaks, or no increase in the coefficient of determination was observed.

[0134] From these results, it was confirmed that, in X-ray diffraction rocking curve measurement, the symmetry plane reflection peaks of the PZT film obtained with X-rays incident from the

[0100] direction on the Si substrate and Pt electrode can be fitted with three component peaks.

[0135] Furthermore, from the split width of each component peak when fitting was performed using the three component peaks, it was confirmed that the interfacial angle formed by the (001) plane of the Si substrate and the (001) plane of the lead zirconate titanate film is 0.35°.

[0136] From the XRD measurement results above, it was confirmed that the crystal structure of the PZT film of piezoelectric element No. 1 is a mixed crystal of monoclinic and rhombus phases.

[0137] <XRD measurement of piezoelectric element No. 2> Out-of-plane XRD measurements (out-of-plane 2θ-ω scan) were performed on piezoelectric element No. 2, which lacked a second electrode, under the same conditions as described above. The out-of-plane measurements were performed in the range of 2θ = 10 to 110°. The X-rays were incident from the

[0100] direction on the Si substrate.

[0138] Figure 12 shows the results of out-of-plane XRD measurement of piezoelectric element No. 2. From Figure 12, the 00L preferred orientation of the PZT film was confirmed. Focusing on the diffraction peak of the (004) plane observed at 2θ = 90 to 110°, expanding the range of the horizontal axis to 2θ = 90 to 110° results in Figure 13 below.

[0139] Furthermore, the peak originating from the (004) plane of the PZT film near 2θ = 98° was fitted under the same conditions as described above.

[0140] When fitting is performed on one component peak, the graph shown in Figure 14 is obtained, and the coefficient of determination is R 2 The result was 0.99559. Furthermore, increasing the number of component peaks beyond that did not increase the coefficient of determination. From the above, it was confirmed that the diffraction peak of the (004) plane is a single peak.

[0141] Next, in-plane XRD measurements were performed on piezoelectric element No. 2, which lacked a second electrode, under the same conditions as above.

[0142] Figure 15 shows the results of in-plane XRD measurement of piezoelectric element No. 2. From the results shown in Figure 15, peaks originating from polycrystalline material were obtained, confirming that the crystals are random in the in-plane direction. Therefore, it was confirmed that the PZT film of piezoelectric element No. 2 is aligned in the out-of-plane direction, but randomly oriented in the in-plane direction.

[0143] Rocking curve measurements were performed on the PZT film at the 001 lattice point reflection (2θ = 21.74°) under the same conditions as above. Incidence was from the

[0100] direction of the Si substrate.

[0144] The peak obtained by rocking curve measurement was fitted under the same conditions as described above. As a result, the coefficient of determination was the largest when fitting was performed with one component peak, and R 2 =0.92402 was obtained. A graph when fitting is performed with one component peak is shown in Figure 16.

[0145] From the results of the above XRD measurement, it was confirmed that the crystal structure of the PZT film of piezoelectric element No. 2 was a tetragonal phase.

[0146] <Measurement of Surface Roughness of PLT Film> Using an atomic force microscope (Dimension Icon manufactured by Bruker), the surface roughness of the PLT film of each piezoelectric element on which the second electrode was not formed was measured.

[0147] An atomic force microscope image of the PLT film of piezoelectric element No. 1 is shown in Figure 17. The RMS value of the surface roughness of the PLT film was 1.49 nm. Further, an atomic force microscope image of the PLT film of piezoelectric element No. 2 is shown in Figure 18. The RMS value of the surface roughness of the PLT film was 4.97 nm.

[0148] <Measurement of Dielectric Constant ε and Relative Dielectric Constant ε r > The second electrode was formed on each piezoelectric element on which the second electrode was not formed, by an RF magnetron sputtering method using a Cu target.

[0149] The thickness of the second electrode and the sputtering conditions are as follows. Thickness ······· 0.1 μm RF power supply ····· 1 kW Gas flow rate ····· Ar = 50 sccm Sputtering pressure ····· 0.15 Pa Substrate set temperature ··· Room temperature

[0150] The second electrode (Cu electrode) formed as described above was patterned using a metal mask to have an area of 0.0314 mm 2The element was patterned in a circular shape. The capacitance of this piezoelectric element was measured using an LCR meter (HIOKI IM3523) under the following conditions. Excitation voltage: 1V Excitation frequency: 1kHz Circuit model: Parallel capacitance model Measurement item: Cp-D

[0151] From the measured capacitance and other values, the dielectric constant ε and relative permittivity ε are calculated using the following formula (5). r The following was determined. The measurement results are shown in Table I.

[0152]

number

[0153] ε: Dielectric constant [F / m] ε0: Permittivity of vacuum [F / m] (8.85 × 10⁻⁶) -12 F / m) ε r : relative permittivity C: Electrical capacitance [F] d: Distance between electrodes [m] S: Electrode area [m 2 ]

[0154] <Piezoelectric constant d> 31,f Measurement > Each piezoelectric element without a second electrode was cut into a 2mm x 15mm strip. Next, approximately 3mm of one end in the longitudinal direction was masked, and the electrode was formed using RF magnetron sputtering with a Cu target.

[0155] The thickness of the second electrode and the sputtering conditions are as follows: Thickness: 0.1m RF power supply...1kW Gas flow rate: Ar = 50 sccm Sputtering pressure: 0.15 Pa Circuit board set temperature...room temperature

[0156] The mask was removed, and a portion of the material other than the first electrode (approximately 2 mm at the edges) in the area where the second measuring electrode was not formed was removed by etching. Then, Ag paste was applied to the first electrode exposed after etching to serve as the first electrode contact for measurement. The sample for measurement was prepared using the above procedure.

[0157] Using the prepared sample for measurement, the displacement δ was calculated using the measurement method described above, and furthermore, the piezoelectric constant d at each applied voltage (-20V, 10V, 20V, 30V) was calculated using the following equation (4). 31,f The following was determined. The sample length l for measurement was set to 19.5 mm. The elastic compliance s1 of the PZT film and the elastic compliance s2 of the Si substrate were taken from the values ​​described in the reference (I. Kanno et al., Piezoelectric properties of c-axis oriented Pb(Zr,Ti)O3thin films, APL 70, 1378 (1997)). The calculation results are shown in Table I.

[0158]

number

[0159] δ: Displacement [m] d 31,f Piezoelectric constant [m / V] l: Length of the sample for measurement [m] V: Applied voltage [V] s1: Elastic compliance of PZT film [m 2 / N] s2: Elastic compliance of Si substrate [m 2 / N] t1: Distance between electrodes [m] t2: Si substrate thickness [m]

[0160] < Electromechanical coupling coefficient k 31,f 2 Calculation > The dielectric constant ε and piezoelectric constant d when 30V is applied, as measured above. 31,f Therefore, using the following equation (1), the electromechanical coupling coefficient k31,f 2 The calculation was performed. The results are shown in Table I.

[0161]

number

[0162] k 31,f 2 : Electromechanical coupling coefficient [%] d 31,f Piezoelectric constant [m / V] ε: Dielectric constant [F / m] s: Elastic compliance [m 2 / N]

[0163] [Table 1]

[0164] The evaluation results shown in Table I confirm that the piezoelectric element of the present invention has a higher electromechanical coupling coefficient compared to the comparative example. This is because the dielectric constant is significantly lower than that of the comparative example, and the piezoelectric constant is maintained despite the low dielectric constant. [Industrial applicability]

[0165] The present invention can be used in piezoelectric elements with a high electromechanical coupling coefficient, as well as in piezoelectric actuators, droplet ejection heads, droplet ejection devices, and ferroelectric memories equipped with such piezoelectric elements. [Explanation of symbols]

[0166] 10 Piezoelectric element 11 Si substrate 12 ZrO2 layer 13 1st electrode 14 Pt electrode 15 SRO electrode 16 PZT membrane 17 Dielectric film 18 2nd electrode 20 Samples for measurement 21 Interelectrode layer 22 1st electrode contact 23 2nd electrode contact 30 Measuring device 31 Lower support 32 Upper support 33 Waveform generator 34. Doppler displacement sensor

Claims

1. A piezoelectric element comprising a first electrode, a second electrode, and a lead zirconate titanate film positioned between the first electrode and the second electrode, The piezoelectric element is fabricated on a Si substrate whose main surface is the (001) plane. The Si substrate has crystal orientations aligned in both the in-plane and out-of-plane directions. The (110) plane of the Si substrate and the (100) plane of the lead zirconate titanate film are parallel. In the rocking curve measurement using X-ray diffraction, the peak of the plane of symmetry reflection of the lead zirconate titanate film obtained with X-rays incident from the [100] direction on the Si substrate can be fitted with three component peaks. The angle of the interfacial angle formed by the (001) plane of the Si substrate and the (001) plane of the lead zirconate titanate film is within the range of 0.34 to 0.35°. A piezoelectric element characterized by the following features.

2. A piezoelectric element comprising a first electrode, a second electrode, and a lead zirconate titanate film positioned between the first electrode and the second electrode, At least one of the first electrode or the second electrode includes a Pt electrode whose main surface is the (001) surface, The Pt electrode has crystal orientations aligned in both the in-plane and out-of-plane directions. The (110) plane of the Pt electrode and the (100) plane of the lead zirconate titanate film are parallel. In X-ray diffraction rocking curve measurement, the peak of the plane of symmetry reflection of the lead zirconate titanate film obtained with X-rays incident from the [100] direction of the Pt electrode can be fitted with three component peaks. A piezoelectric element characterized by the following features.

3. The angle of the interfacial angle formed by the (001) surface of the Pt electrode and the (001) surface of the lead zirconate titanate film is within the range of 0.34 to 0.35°. The piezoelectric element according to feature 2.

4. The angle of the interfacial angle formed by the (100) plane of the Si substrate and the (100) plane of the lead zirconate titanate film is within the range of 40 to 50°. The piezoelectric element according to feature 1.

5. The angle of the interfacial angle formed by the (100) plane of the Pt electrode and the (100) plane of the lead zirconate titanate film is within the range of 40 to 50°. The piezoelectric element according to feature 3.

6. The diffraction peak of the (004) plane of the lead zirconate titanate film, obtained by an out-of-plane 2θ-ω scan using X-ray diffraction, can be fitted with three component peaks. The piezoelectric element according to feature 1 or 2.

7. The composition of lead zirconate titanate constituting the aforementioned lead zirconate titanate film is Pb X (Zr Y , Ti 1-Y ) O 3 [1.0 ≤ X ≤ 1.2, 0.4 ≤ Y ≤ 0.6] The piezoelectric element according to feature 1 or 2.

8. The thickness of the lead zirconate titanate film is in the range of 0.1 to 5.0 μm. The piezoelectric element according to feature 1 or 2.

9. At the interface between the second electrode and the lead zirconate titanate film, there is a dielectric film composed of a dielectric with a lower dielectric constant than the lead zirconate titanate that constitutes the lead zirconate titanate film. The dielectric film and the lead zirconate titanate film are in an epitaxial relationship such that the (100) plane of the dielectric film and the (100) plane of the lead zirconate titanate film are parallel. The piezoelectric element according to feature 1 or 2.

10. The dielectric is lead lanthanum titanate. The piezoelectric element according to feature 9.

11. The total thickness of the lead zirconate titanate film and the dielectric film is within the range of 0.1 to 5.0 μm. The piezoelectric element according to feature 9.

12. The total thickness of the lead zirconate titanate film and the dielectric film is within the range of 0.1 to 5.0 μm. The piezoelectric element according to feature 10.

13. The RMS value of the surface roughness on the second electrode side of the dielectric film is 5.0 nm or less. The piezoelectric element according to feature 9.

14. When the first electrode is grounded and a voltage of 30V is applied to the second electrode, the piezoelectric constant measured is A, and when a voltage of 10V is applied to the second electrode, the piezoelectric constant measured is B. Then B is 95% or more of A. The piezoelectric element according to feature 1 or 2.

15. A piezoelectric actuator equipped with a piezoelectric element, The piezoelectric element is the piezoelectric element described in any one of claims 1, 2, 4, or 5. A piezoelectric actuator characterized by the following features.

16. A droplet dispensing head equipped with a piezoelectric actuator, The piezoelectric actuator is the piezoelectric actuator described in claim 15. A droplet dispensing head characterized by the following features.

17. A droplet dispensing device equipped with a droplet dispensing head, The droplet dispensing head is the droplet dispensing head described in claim 16. A droplet dispensing device characterized by the following features.

18. A ferroelectric memory equipped with a piezoelectric element, The piezoelectric element is the piezoelectric element described in claim 1 or 2. A ferroelectric memory characterized by the following features.

Citation Information

Patent Citations

  • Ferroelectric thin-film element and manufacture thereof

    JP2000091533A

  • plt / pzt ferroelectric structure

    JP2008522426A

  • Electro-mechanical conversion element, method of manufacturing electro-mechanical conversion element, droplet discharge head, and droplet discharge device

    JP2015225957A

  • Film structure, actuator, motor, and method of manufacturing film structure

    JP2017112306A

  • Film structure body and method for manufacturing the same

    JP2019016793A