Steel parts
By controlling the number density and morphology of carbonitrides in the nitrogen diffusion layer, the steel components achieve improved surface fatigue properties, addressing the inadequacies of existing soft nitriding steels in sliding contact applications.
Patent Information
- Application Number
- JP2024006948
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-01-19
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-01-19
AI Technical Summary
Existing soft nitriding steels exhibit inadequate surface fatigue strength, particularly in components experiencing sliding contact, and existing technologies do not adequately address the properties of the inner regions beyond the surface layer.
Control the number density and morphology of carbonitrides within the nitrogen diffusion layer, ensuring a longitudinal length of 3 nm to 20 nm and specific number densities at varying depths from the surface to enhance surface fatigue properties.
The controlled microstructure in the nitrogen diffusion layer significantly improves surface fatigue characteristics, providing enhanced resistance to dislocation movement and stress, making the steel suitable for machine structural components.
Smart Images

Figure 0007948223000005 
Figure 0007948223000006 
Figure 0007948223000007
Abstract
Description
[Technical Field]
[0001] The present invention relates to steel parts, and more particularly to steel parts that have a diffusion layer containing a large number of fine carbonitrides due to soft nitriding treatment, and that have excellent surface fatigue properties, making them suitable for use in parts for automobiles, construction machinery, and the like. [Background technology]
[0002] Automotive gears and other mechanical structural components require excellent fatigue properties, such as surface fatigue characteristics and bending fatigue characteristics, and therefore surface hardening treatments are commonly performed. Well-known surface hardening treatments include carburizing, high-frequency induction hardening, and nitriding.
[0003] Of these methods, carburizing is effective in improving fatigue properties because it allows carbon to penetrate and diffuse in the high-temperature austenite region, resulting in a deep hardened layer. However, since carburizing causes heat treatment distortion, it has been difficult to apply to parts that require strict dimensional accuracy from the standpoint of quietness and other factors.
[0004] Furthermore, since high-frequency induction hardening is a process that hardens the surface layer using high-frequency induction heating, heat treatment distortion still occurs, and there were problems in terms of dimensional accuracy, similar to carburizing.
[0005] On the other hand, nitriding is a process that increases surface hardness by infiltrating and diffusing nitrogen in a relatively low temperature range below the Ac1 transformation point, so the heat treatment distortion described above is small. However, it has the problem of requiring a long processing time of 50 to 100 hours, and the need to remove the brittle compound layer on the surface after processing.
[0006] For this reason, a so-called soft nitriding process has been developed that shortens the processing time at a similar processing temperature to nitriding, and in recent years it has become widely used for mechanical structural parts and the like. This soft nitriding process involves simultaneously introducing N and C at a temperature range of 500-600°C, forming a nitride compound layer with solid-solution C on the outermost surface, and further diffusing N into the base metal to form a nitrogen diffusion layer and harden the surface. This process makes it possible to reduce the processing time to less than half compared to conventional nitriding.
[0007] However, while the aforementioned carburizing treatment can increase core hardness through quenching, the soft nitriding treatment is performed at a temperature below the transformation point of steel, so core hardness does not increase, and soft nitrided materials have the problem of having inferior fatigue properties compared to carburized materials.
[0008] Therefore, in order to improve the fatigue properties of soft-nitrided materials, quenching and tempering treatments are usually performed before soft-nitriding to increase the core hardness. However, the resulting fatigue properties are not always satisfactory, and the manufacturing costs increase, as well as a decrease in machinability, is unavoidable.
[0009] To solve these problems, Patent Document 1 proposes a steel for soft nitriding that allows for high bending fatigue properties after soft nitriding treatment by incorporating elements such as Ni, Cu, Al, Cr, and Ti into the steel. Specifically, in this steel, the core is age-hardened with Ni-Al, Ni-Ti intermetallic compounds or Cu compounds through soft nitriding treatment, while the surface layer is precipitation-hardened with nitrides and carbides such as Cr, Al, and Ti within the nitrided layer, thereby improving the bending fatigue properties.
[0010] Furthermore, Patent Document 2 proposes a steel for soft nitriding in which excellent bending fatigue properties are obtained after soft nitriding treatment by hot forging a steel containing 0.5 to 2% Cu, air cooling to obtain a ferrite-dominant structure with dissolved Cu, precipitation hardening of Cu during soft nitriding treatment at 580°C for 120 minutes, and further precipitation hardening of Ti, V and Nb carbonitrides.
[0011] Further, Patent Document 3 proposes a soft nitriding steel in which Ti-Mo carbides, or carbides further containing one or more of Nb, V and W dispersed therein.
[0012] Patent Document 4 proposes a soft nitriding steel in which dislocation structures are formed at high density in the soft nitriding steel to promote nitride formation during soft nitriding treatment.
[0013] Patent Document 5 proposes a steel part having excellent surface fatigue properties by appropriately controlling the morphology of the compound layer and the hardness of the diffusion layer. [Prior Art Documents] [Patent Documents]
[0014] [Patent Document 1] Japanese Unexamined Patent Publication No. H5-59488 [Patent Document 2] Japanese Unexamined Patent Publication No. 2002-69572 [Patent Document 3] Japanese Unexamined Patent Publication No. 2010-163671 [Patent Document 4] Japanese Patent No. 6323554 [Patent Document 5] International Publication No. 2021 / 230384 [Disclosure of the Invention] [Problems to be Solved by the Invention]
[0015] However, although the soft nitriding steels described in Patent Documents 1 to 3 are excellent in bending fatigue strength, no consideration is given to surface fatigue strength. When contact accompanied by sliding occurs in a part, if the surface fatigue strength is insufficient, cracking will originate from the contact portion. The technique described in Patent Document 4 takes into account the hardness at 50 μm from the surface layer and carbonitrides, but does not consider the properties of the inner region beyond that. Furthermore, although the technique described in Patent Document 5 evaluates surface fatigue strength at 2600 MPa, in view of application to members requiring higher surface fatigue strength, a steel material exhibiting even more excellent surface fatigue strength is desirable.
[0016] The present invention significantly solves the above-mentioned problems, and in particular aims to provide steel parts with excellent surface fatigue characteristics. [Means for solving the problem]
[0017] To solve the above problems, the inventors diligently investigated the optimal microstructure in the nitrogen diffusion layer. As a result, they found that controlling the number density and morphology of carbonitrides with a longitudinal length of 3 nm to 20 nm in the nitrogen diffusion layer is effective in improving surface fatigue properties.
[0018] Furthermore, when steel components are subjected to resistance involving sliding, shear stress is applied due to the normal force. This stress is greatest at a depth of approximately 400 μm from the surface layer, so controlling the internal structure as well as the surface layer is important to achieve excellent surface fatigue characteristics.
[0019] This invention was completed after further consideration based on the above findings, and the gist of the present invention is as follows.
[0020] 1. From the surface inward, it has a nitride compound layer and a nitrogen diffusion layer, The nitrogen diffusion layer has carbonitrides that match the matrix ferrite, and the number density of carbonitrides with a longitudinal length of 3 nm to 20 nm is 1.0 × 10⁻¹⁴ at a position 50 μm inward from the surface. 23 / m 3 In summary, at a distance of 200 μm from the surface inward, the measurement is 0.3 × 10⁻⁶. 23 / m 3 In summary, at a distance of 400 μm from the surface inward, the measurement is 0.1 × 10⁻⁶. 23 / m 3 The steel parts are as described above.
[0021] 2. The steel part is a toothed part, and the steel part according to claim 1 has the nitride compound layer and the nitrogen diffusion layer at least in the tooth portion. [Brief explanation of the drawing]
[0022] [Figure 1] This is a diagram showing the HAADF-STEM image of carbonitrides present in steel. [Figure 2] This is a diagram showing a typical manufacturing method for soft-nitrided components. [Figure 3] This is a diagram showing a roller pitting test specimen. SUMMARY OF THE INVENTION EFFECTS OF THE INVENTION
[0023] According to the present invention, it is possible to provide a steel component having improved surface fatigue properties by controlling the microstructure in the diffusion layer through soft nitriding treatment. Therefore, the steel of the present invention is extremely useful as a material for machine structural components such as automobiles. MODE FOR CARRYING OUT THE INVENTION
[0024] Hereinafter, the present invention will be specifically described. As described above, in order for a steel component to exhibit excellent surface fatigue properties, it is important to control not only the surface layer of the steel component but also the internal microstructure. In order to improve the surface fatigue properties of steel, it is important to precipitate fine carbonitrides at a high density and even into the interior. The presence of a large amount of carbonitrides in the surface layer inhibits dislocation movement under surface pressure load, making it possible to exhibit excellent surface fatigue properties.
[0025] That is, in a steel component having a nitride compound layer and a nitrogen diffusion layer in order from the surface inward, the nitrogen diffusion layer containing carbonitrides that are coherent with the parent phase ferrite, the number density of carbonitrides having a longitudinal length of 3 nm or more and 20 nm or less among the carbonitrides is 1.0×10 at a position 50 μm inward from the surface 23 / m 3 or more, 0.3×10 at a position 200 μm inward from the surface 23 / m 3 or more, and 0.1×10 at a position 400 μm inward from the surface 23 / m 3 or more, is critical.
[0026] [Carbonitrides in the nitrogen diffusion layer] First, let's explain the carbonitride in the nitrogen diffusion layer. In this invention, the carbonitride needs to be matched with the matrix ferrite. When the carbonitride is matched with the matrix ferrite, it generates matched strain, which increases resistance to dislocations and improves fatigue properties.
[0027] Here, "matching with the matrix ferrite" means that the matrix ferrite and the carbonitride have a crystal orientation relationship known as the Baker-nutting relationship. In this case, the (001) of the ferrite and the (011) of the NaCl-type carbonitride are matched, and the misfit (ε) between the two is important in order to generate sufficient matched strain. This misfit (ε) is calculated according to the following equation (1). In the present invention, a carbonitride that matches with the matrix ferrite is a carbonitride in which the above ε is 10% or less. Carbonitrides with ε exceeding 10% have a smaller inhibitory effect on dislocation motion. ε = |a0 - ap| / ap × 100 (%) …(1) Here, a0 represents the interplanar spacing of the ferrite, and ap represents the interplanar spacing of the carbonitride.
[0028] The method for measuring the interplanar spacing described above is not particularly limited, but it can be confirmed by direct observation of the interface region using high-resolution electron microscopy. For example, Figure 1 shows carbonitrides <001> The image obtained using HAADF-STEM (High Angle Annular Dark-Field Scanning Transmission Electron Microscopy) is shown. As shown in Figure 1, it is possible to directly measure the interplanar spacing ap of the carbonitrides from this image.
[0029] The carbonitride material described above preferably has a hardness of 1000 HV or higher in order to have sufficient shear strength. Carbonitride material precipitated by soft nitriding treatment can satisfy this hardness requirement.
[0030] To improve the surface fatigue properties of steel parts, the number density of carbonitrides that match the matrix ferrite and have a longitudinal length of 3 nm to 20 nm (hereinafter also called compatible diameter carbonitrides) should be 1.0 × 10⁻¹⁶ at a position 50 μm inward from the surface. 23 / m 3 In summary, at a distance of 200 μm from the surface inward, the measurement is 0.3 × 10⁻⁶. 23 / m 3 In summary, at a distance of 400 μm from the surface inward, the measurement is 0.1 × 10⁻⁶. 23 / m 3 It is important that these conditions are met. If these conditions are not met, dislocation movement cannot be sufficiently inhibited, and therefore excellent surface fatigue characteristics cannot be obtained.
[0031] Here, the carbonitrides are defined as having a longitudinal length of 3 nm or more and 20 nm or less because, firstly, carbonitrides with a longitudinal length of less than 3 nm have difficulty exhibiting a sufficient inhibitory effect on dislocation motion even if they are well-matched with the matrix ferrite. Secondly, if the carbonitride is longer than 20 nm, the matching with the matrix ferrite becomes poor, resulting in reduced resistance to dislocation motion.
[0032] Furthermore, the number density of the suitable diameter carbonitrides described above is defined at positions 50 μm, 200 μm, and 400 μm from the surface, as explained above for the 400 μm position. On the other hand, compressive stress becomes a problem at the 50 μm and 200 μm positions. That is, compressive stress is maximum at the surface and gradually decreases, but in order to create a structure that can withstand this compressive stress, microstructure control is required at depths of 50 and 200 μm from the surface in stages. By defining the number density of suitable diameter carbonitrides at these two depth positions, it is possible to withstand gradually changing compressive stress. The reason for limiting the number density of suitable diameter carbonitrides at each position is as follows.
[0033] [1.0 × 10 at a position 50 μm from the surface inward] 23 / m 3 [End] The number density of suitable diameter carbonitrides at a position of 50 μm is 1.0 × 10⁻⁶ 23 / m 3 The reason for setting it above is to ensure sufficient resistance to the dislocation motion described above. While there is no particular need to limit the upper limit, from the perspective of alloy cost, 4.0 × 10 23 / m 3 The following is preferable.
[0034] [0.3 × 10 at a position 200 μm from the surface inward] 23 / m 3 [End] The number density of suitable diameter carbonitrides at a position of 200 μm is 0.3 × 10⁻⁶. 23 / m 3 The reason for setting it above is to ensure sufficient resistance to dislocation motion. While there is no particular upper limit, from the perspective of alloy cost, 2.5 × 10 23 / m 3 The following is preferable.
[0035] [0.1 × 10 at a position 400 μm from the surface inward] 23 / m 3 [End] The number density of suitable diameter carbonitrides at a position of 400 μm is 0.1 × 10⁻⁶. 23 / m 3 The reason for setting it above is to ensure sufficient resistance to dislocation motion. While there is no particular upper limit, from the perspective of alloy cost, 0.6 × 10 23 / m 3 The following is preferable.
[0036] Carbonitrides that match the above-mentioned ferrite matrix precipitate on the {001} plane of the ferrite matrix, satisfying the Baker-Nutting relationship. Therefore, the number density of carbonitrides is calculated as follows. First, the {001} plane of the matrix ferrite was observed using a transmission electron microscope (TEM), and the number of carbonitrides in the field of view was measured. Next, the relative film thickness of the sample in each observation field was measured using electron energy loss spectroscopy (EELS), and the volume of the observation field was calculated. Then, the number density was calculated by dividing the number of carbonitrides by the volume. Here, carbonitrides precipitate on the (001), (010), and (100) planes, but for example, when observed with (001) incidence, carbonitrides on the (001) plane cannot be observed, so only two planes can be observed with TEM observation. For this reason, the number of carbonitrides was taken by multiplying the number of carbonitrides observed by TEM by 1.5. The film thickness was measured by multiplying the relative film thickness measured by EELS by the mean free path λ calculated from the formula by Iakoubovskii et al. JPEG0007948223000001.jpg14170 Here, E0: Acceleration voltage, α: angle of convergence, β: angle of entry, ρ: sample density, F = (1 + E0 / 1022) / (1 + E0 / 511) 2 , θ E = 5.5ρ 0.3 / FE0, θ c =20mrad That's what I decided.
[0037] Next, the microstructure of the compound layer and diffusion layer of the steel of the present invention will be described. The compound layer and diffusion layer are formed during the soft nitriding treatment, and are formed by the diffusion of nitrogen and carbon in the soft nitriding treatment atmosphere into the steel. That is, a compound layer is formed on the outermost surface of the steel, with iron nitride (Fe3N or Fe4N), which is formed when Fe, the main component of the steel subjected to the soft nitriding treatment, combines with N, as the matrix phase, and other constituent components precipitated as carbonitrides by combining with nitrogen and carbon. It is preferable that the compound layer be formed over a thickness of 3 to 40 μm.
[0038] Furthermore, the diffusion layer is a layer in which nitrogen diffuses into the steel, resulting in a higher nitrogen concentration than before the soft nitriding treatment. It is formed adjacent to the inside of the compound layer. The unhardened portion is the area where nitrogen diffusion does not occur, and therefore has the component composition of the unhardened portion as described above. In contrast, the compound layer and the diffusion layer have a component composition with a higher nitrogen content compared to the component composition of the unhardened portion. The structure of the diffusion layer and the unhardened portion inside it forms a matrix of ferrite or bainite. It is preferable to form the diffusion layer inside the compound layer with a thickness of 400 to 1000 μm.
[0039] The steel parts according to the present invention have been described above. The steel parts according to the present invention are in the shape of various parts, preferably machine structural parts, and more preferably toothed parts such as gears.
[0040] Furthermore, even for steel parts that are not toothed, if there are areas where contact involving sliding occurs, the surface fatigue characteristics of these areas are important for ensuring the durability of the part. Therefore, by forming the aforementioned diffusion layer on such areas, the effect of improving surface fatigue characteristics can be obtained. Thus, the steel parts of the present invention are not limited to toothed parts.
[0041] Next, the manufacturing method for the steel parts of the present invention will be described.
[0042] Figure 2 shows a typical manufacturing process for producing steel parts using steel bars for soft nitriding. Here, S1 is the manufacturing process for the steel bars (steel for soft nitriding) that serve as the raw material, S2 is the transport process, and S3 is the manufacturing process for the parts (soft nitrided parts).
[0043] First, in the steel bar manufacturing process (S1), the steel ingot is hot-rolled and / or hot-forged to form steel bars, which are then shipped after quality inspection. After transportation (S2), in the soft nitriding parts finishing process (S3), the steel bars are cut to predetermined dimensions, hot-forged or cold-forged, and then, if necessary, cut to the desired shape (e.g., gear shape or shaft shape) by drilling, turning, etc. Finally, they undergo soft nitriding treatment to become products (steel parts).
[0044] In addition, hot-rolled material may be shaped into the desired form by machining processes such as turning or drilling, and then subjected to soft nitriding to produce the final product (steel part). In the case of hot forging, cold straightening may be performed after hot forging. Furthermore, the final product may be coated with paint, plating, or other finishes.
[0045] Here, it is desirable to perform soft nitriding at 520-550°C for more than 2 hours, and then continue the soft nitriding process while increasing the temperature by 20-30°C / h until it reaches 560-590°C, after which it is desirable to perform soft nitriding for another hour or more. By performing soft nitriding in this gradient manner, N and C can be diffused to deeper regions, and carbonitrides can be formed in deeper regions.
[0046] In soft nitriding, N and C are simultaneously introduced into the steel to form a nitride compound layer in which C is dissolved, and then N is diffused into the base metal to form a nitrogen diffusion layer. Therefore, soft nitriding should be performed in a mixed atmosphere of nitrogenous gases such as NH3 and N2 and carburizing gases such as CO2 and CO, for example, an atmosphere of NH3:N2:CO2 = 50:45:5.
[0047] By performing the above soft nitriding treatment, a compound layer formed of Fe3N, Fe4N, or both is created on the surface with a thickness of 3 to 40 μm, and a nitrogen diffusion layer with numerous carbonitrides precipitated is created inside the compound layer with a thickness of 400 μm or more from the surface of the nitrided compound layer. The nitrogen diffusion layer and the structure inside it form a matrix of ferrite, pearlite, or bainite. It is preferable that the nitrogen diffusion layer be formed inside the nitrided compound layer with a thickness of 400 to 1000 μm.
[0048] By using the above method, it is possible to produce a structure having the high-density carbonitride morphology described above. Note that the soft nitriding treatment is not limited to the method described above; any method capable of forming the diffusion layer structure defined in this invention is acceptable. [Examples]
[0049] The following describes specific embodiments of the present invention. Steel (steel grades A to K) with the compositions shown in Table 1 were cast into slabs with a cross-section of 300 mm x 400 mm using a continuous casting machine. After soaking at 1250°C for 30 minutes, these slabs were hot-rolled into rectangular steel billets with sides of 140 mm. These steel billets were further hot-rolled to obtain 80 mmφ steel bars (as-hot-rolled material). These steel bars were held at 1200°C for 1 hour and then hot-forged to obtain smaller diameter steel bars of 35 mmφ.
[0050] [Table 1]
[0051] Furthermore, roller pitting test specimens, as shown in Figure 3, were taken from the hot-forged material (steel bar) described above, parallel to the longitudinal direction (axial direction), and these specimens were subjected to soft nitriding treatment. The soft nitriding temperature and soft nitriding time were adjusted as shown in Table 2 to obtain the desired diffusion layer structure.
[0052] [Table 2]
[0053] For the obtained soft-nitrided material, the number density of carbonitrides was measured at 50 μm, 200 μm, and 400 μm from the surface, and the surface fatigue characteristics were evaluated.
[0054] Specifically, the number density of carbonitrides was measured using a TEM to capture three fields of view at a magnification of 640,000x, and calculated according to the method described above. Furthermore, consistency was determined by using HAADF-STEM images obtained with {001} plane incidence on the matrix ferrite of the soft-nitrided material described above. If ε was 10% or less, it was judged as consistent (○). If ε was greater than 10%, it was judged as inconsistent (×).
[0055] For surface fatigue characteristics evaluation, fatigue life was measured using a Nikko Create RPT-402 on roller pitting test specimens that had undergone soft nitriding treatment. The fatigue life was 1.0 × 10⁻⁶. 6Fatigue life is good (〇) if it occurs more than once, 1.0 × 10 6 Rollers with fewer than 100 cycles were classified as having poor fatigue life (×). The roller pitting test conditions were a maximum contact stress of 3000 MPa and a slip ratio of 40%, using gear oil (BESCO transaxle) as the lubricant at an oil temperature of 80°C. The rotational speed during the test was 2000 rpm. Hardened and tempered SUJ2 rollers with a crowning radius of 150 mm were used for the large rollers that came into contact with the transfer surface. The evaluation results are shown in Table 3.
[0056] [Table 3]
Claims
1. From the surface inward, it has a nitride compound layer and a nitrogen diffusion layer, The nitrogen diffusion layer has carbonitrides that match the matrix ferrite, and the number density of carbonitrides with a longitudinal length of 3 nm to 20 nm is 1.0 × 10⁻¹⁴ at a position 50 μm inward from the surface. 23 / m 3 In summary, at a position 200 μm from the surface inward, the measurement is 0.3 × 10⁻⁶. 23 / m 3 In summary, at a distance of 400 μm from the surface inward, the measurement is 0.1 × 10⁻⁶. 23 / m 3 The steel parts are as described above.
2. The steel component according to claim 1, wherein the steel component is a toothed component and has the nitride compound layer and the nitrogen diffusion layer at least in the toothed portion.
Citation Information
Patent Citations
Electromagnetic reciprocating machine
JP1988023554A
Precipitation hardening type high strength steel for soft-nitriding excellent in machinability
JP1993059488A
Gear on which soft nitriding treatment is applied and manufacture thereof
JP1999072159A
Soft-nitriding steel having excellent bending fatigue strength
JP2002069572A
Soft nitriding treated steel superior in wear resistance
JP2005264318A