Laminates and rolls

The laminate with a fluorine-containing polymer and woven fabric addresses the issue of unstable unwinding by enhancing adhesion, ensuring stable unwinding and preventing blocking in laminates with a releaseable substrate.

JP7948319B2Active Publication Date: 2026-11-11AGC INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024535043
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-07-20
Filing Date
2023-07-12
Publication Date
2026-11-11
Estimated Expiration
2043-07-12

AI Technical Summary

Technical Problem

Existing laminates containing a releaseable substrate and a solid polymer electrolyte membrane face issues with unstable unwinding from rolls due to poor adhesion between the release layer and the solid polymer electrolyte membrane.

Method used

A laminate configuration comprising a solid polymer electrolyte membrane with a fluorine-containing polymer having ion exchange groups and a woven fabric, where the woven fabric creates a minute uneven structure on the surface, enhancing adhesion and allowing stable unwinding by preventing blocking.

Benefits of technology

The laminate exhibits excellent adhesion between the release layer and the solid polymer electrolyte membrane, ensuring stable unwinding from a roll, thereby improving handling and reducing the risk of blocking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948319000014
    Figure 0007948319000014
  • Figure 0007948319000015
    Figure 0007948319000015
  • Figure 0007948319000016
    Figure 0007948319000016
Patent Text Reader

Abstract

Provided is a laminate which has excellent adhesion between a release layer and a solid polymer electrolyte membrane, and has excellent properties of being unwound from a roll body obtained through winding. The laminate comprises: a peelable substrate including a support and a release layer; and a solid polymer electrolyte membrane disposed on the release layer of the peelable substrate, wherein the solid polymer electrolyte membrane includes a fluorine-containing polymer having an ion exchange group, and a woven fabric.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to laminates and rolls. [Background technology]

[0002] Solid polymer electrolyte membranes can be applied to a variety of uses, and various studies are being conducted on them. For example, solid polymer electrolyte membranes are applied to membrane electrode assemblies. Depending on the application, various films can be laminated onto the surface of a solid polymer electrolyte membrane. For example, when a solid polymer electrolyte membrane is used in a membrane electrode assembly, an electrode film (catalyst layer or electrode-catalyst layer) is laminated onto the surface of the solid polymer electrolyte membrane, and such electrode films may be formed by casting or coating methods. For example, Patent Document 1 (paragraph 0051) discloses a technique for applying a catalyst to the surface of an electrolyte sheet in a sheet in which an electrolyte sheet is attached to a polyethylene terephthalate backsheet via a release layer. [Prior art documents] [Patent Documents]

[0003] [Patent Document 1] Japanese Patent Publication No. 2020-107430 [Overview of the project] [Problems that the invention aims to solve]

[0004] When using a releaseable substrate including a support such as polyethylene terephthalate and a release layer, as described in Patent Document 1, good adhesion between the release layer and the solid polymer electrolyte membrane is required so that the solid polymer electrolyte membrane placed on the release layer does not peel off during handling. Furthermore, laminates containing a releaseable substrate and a solid polymer electrolyte membrane are often wound up and transported as rolls, and the laminates are unwound from the rolls for use. The present inventors have found that when unwinding a laminate containing a releaseable substrate and a solid polymer electrolyte membrane, as described in Patent Document 1, from a roll, it is not possible to stably unwind the laminate from the roll. Hereinafter, the ability to stably unwind the film from the roll will also be referred to as "excellent unwinding properties."

[0005] The present invention has been made in view of the above circumstances, and aims to provide a laminate that exhibits excellent adhesion between the release layer and the solid polymer electrolyte membrane, and excellent unwinding from a roll obtained by winding. Furthermore, the present invention also aims to provide a roll body. [Means for solving the problem]

[0006] As a result of diligent research into the above problems, the inventors have found that the above problems can be solved by the following configuration. (1) A releaseable substrate including a support and a release layer, It includes a solid polymer electrolyte membrane disposed on a release layer in a releaseable substrate, A laminate comprising a solid polymer electrolyte membrane, a fluorine-containing polymer having ion exchange groups, and a woven fabric. (2) The laminate according to (1), wherein the ion exchange capacity of the fluorine-containing polymer is 0.90 to 2.00 milliequivalents / gram dry resin. (3) The woven fabric is composed of yarn A extending in one direction and yarn B extending in a direction substantially perpendicular to yarn A, The laminate according to (1) or (2), wherein the opening ratio of the woven fabric is 50% or more. (4) The laminate according to (3), wherein the denier count of yarn A and the denier count of yarn B are independently 15 to 50. (5) The laminate according to (3) or (4), wherein yarn A and yarn B are each independently composed of at least one material selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, polyether ether ketone, and polyphenylene sulfide. (6) The laminate according to any one of (3) to (5), wherein the density of yarn A and yarn B is independently 70 to 150 threads / inch. (7) A laminate according to any one of (1) to (6), wherein the ion exchange group is a sulfonic acid type functional group. (8) A laminate according to any one of (1) to (7), wherein the fluorine-containing polymer comprises units based on a fluorine-containing olefin and units having a sulfonic acid-type functional group and a fluorine atom. (9) The laminate according to (8), wherein the fluorine-containing olefin is a fluoroolefin having 2 to 3 carbon atoms and having one or more fluorine atoms in the molecule. (10) The laminate according to (8) or (9), wherein the unit having a sulfonic acid type functional group and a fluorine atom is a unit represented by formula (1) described later. (11) The laminate according to any one of (1) to (10), wherein the elastic modulus of the support at 160°C is greater than the elastic modulus of the release layer at 160°C. (12) A laminate according to any one of (1) to (11), wherein the elastic modulus of the release layer at 160°C is 1 MPa or less. (13) The woven fabric is composed of yarn A extending in one direction and yarn B extending in a direction substantially perpendicular to yarn A, The maximum film thickness TA and minimum film thickness TB of the solid polymer electrolyte membrane are measured for each of 10 different cross-sections obtained by cutting the solid polymer electrolyte membrane at midpoints between the threads A, in a direction parallel to the direction in which the threads A extend within the solid polymer electrolyte membrane. Furthermore, the maximum film thickness TA and minimum film thickness TB of the solid polymer electrolyte membrane were measured for each of 10 different cross-sections obtained by cutting the solid polymer electrolyte membrane at midpoints between threads B, in a direction parallel to the direction in which the threads B extend within the solid polymer electrolyte membrane. The average minimum film thickness TB obtained by arithmetic mean of the 20 TBs obtained AVE Then, the average maximum film thickness TA obtained by arithmetic mean TA of the 20 TAs obtained AVE In this case, the average maximum film thickness TA AVE and average minimum film thickness TB AVE A laminate described in any of (1) to (12) that satisfies the relationship of equation (X) described later. (14) A roll body formed by winding a laminate described in any of (1) to (13). [Effects of the Invention]

[0007] According to the present invention, it is possible to provide a laminate that exhibits excellent adhesion between the release layer and the solid polymer electrolyte membrane, and excellent unwinding properties from the roll obtained by winding. Furthermore, according to the present invention, a roll body can be provided. [Brief explanation of the drawing]

[0008] [Figure 1] This is a cross-sectional view showing an example of the laminate of the present invention. [Figure 2] A cross-sectional view showing another example of the laminate of the present invention. [Figure 3] This is a cross-sectional view showing an example of a solid polymer electrolyte membrane cut in a direction parallel to the direction in which thread A extends. [Figure 4] This is a cross-sectional view showing an example of a solid polymer electrolyte membrane cut in a direction parallel to the direction in which thread B extends. [Figure 5] This is a schematic plan view showing an example of a woven fabric contained in a solid polymer electrolyte membrane, viewed in the direction of the membrane's film thickness. [Modes for carrying out the invention]

[0009] The following definitions of terms apply throughout this specification and the claims unless otherwise specified. An "ion exchange group" is a group that can exchange at least some of the ions it contains with other ions. Examples include the sulfonic acid type functional group and the carboxylic acid type functional group described below. A "sulfonic acid type functional group" refers to a sulfonic acid group (-SO3H) or a sulfonic acid base (-SO3M). 2 However, M 2 It means an alkali metal or quaternary ammonium cation. A "carboxylic acid-type functional group" refers to a carboxylic acid group (-COOH) or a carboxylic acid base (-COOH). 1 However, M 1 It means an alkali metal or quaternary ammonium cation. A "precursor membrane" is a membrane containing a polymer that has groups that can be converted into ion exchange groups. "Groups that can be converted into ion exchange groups" refers to groups that can be converted into ion exchange groups through treatments such as hydrolysis or acidification. "A group that can be converted to a sulfonic acid type functional group" refers to a group that can be converted to a sulfonic acid type functional group through treatments such as hydrolysis or acidification.

[0010] In polymers, a "unit" refers to an atomic group derived from one monomer molecule, formed by the polymerization of monomers. A unit may be an atomic group directly formed by a polymerization reaction, or it may be an atomic group in which a portion of the atomic group is converted to a different structure by processing the polymer obtained by the polymerization reaction.

[0011] A numerical range represented using "~" means a range that includes the numbers written before and after "~" as the lower and upper limits, respectively.

[0012] [Laminated structure] The laminate of the present invention comprises a releaseable substrate including a support and a release layer, and a solid polymer electrolyte membrane disposed on the release layer in the releaseable substrate, wherein the solid polymer electrolyte membrane comprises a fluorine-containing polymer having ion exchange groups and a woven fabric. The laminate of the present invention exhibits excellent adhesion between the release layer and the solid polymer electrolyte membrane, as well as excellent unwinding properties when unwinding the laminate from a roll obtained by winding the laminate. The detailed reasons for this are not yet clear, but it is presumed to be due to the following reasons. The solid polymer electrolyte membrane in the laminate of the present invention includes a woven fabric. Due to the presence of this woven fabric, a minute uneven structure is formed on the surface of the solid polymer electrolyte membrane. It is presumed that because the surface on the release layer side of the solid polymer electrolyte membrane has such an uneven structure, the material of the release layer enters into the depressions of the uneven structure on the surface on the release layer side of the solid polymer electrolyte membrane, creating an anchoring effect, and as a result, the adhesion between the two is improved. Furthermore, because the solid polymer electrolyte membrane has an uneven surface on the side opposite to the release layer, when the laminate is wound into a roll, this uneven structure comes into contact with the surface of the support side of the releaseable substrate. It is presumed that this uneven structure suppresses so-called blocking, allowing the laminate to be unwound stably. Furthermore, it is presumed that even if the surface of the support in the release substrate opposite to the release layer side is treated with a textured finish, the laminate can still be unwound stably. Furthermore, if a laminate is formed by laminating a fluorine-based film or polyethylene film with excellent release properties to the surface of the support in the release substrate that is opposite to the release layer side, it is presumed that the blocking described above will be suppressed, and the laminate can be unwound more stably. Moreover, even if the surface of the laminated fluorine-based film or polyethylene film opposite to the release substrate side is textured, it is presumed that the laminate can be unwound stably in the same way as described above.

[0013] Figure 1 is a cross-sectional view showing an example of a laminate of the present invention. The laminate 10 includes a releaseable substrate 12 and a solid polymer electrolyte membrane 14, the releaseable substrate 12 including a support 16 and a release layer 18. In the releaseable substrate 12, the release layer 18 is located on the solid polymer electrolyte membrane 14 side, and the solid polymer electrolyte membrane 14 is located in contact with the release layer 18. The following provides a detailed description of each component within the laminate.

[0014] [Releasable substrate] The peelable substrate is a substrate that supports a solid polymer electrolyte membrane and is peeled off. The releaseable substrate includes a support and a release layer. The following provides a detailed description of each component included in the releaseable substrate.

[0015] (Support) The support is a component that supports the release layer. Specific examples of support materials include resin plates, glass plates, and metal plates. When the support is a resin plate, examples of materials included in the support include resins such as polyester, polyolefin, polyamide, polyimide, polycarbonate, polyphenylene ether, polyphenylene sulfide, and cellulose derivatives. Among these, polyester or polyimide is preferred from the viewpoint of heat resistance and flexibility, and polyester is more preferred. Examples of polyesters include polyethylene terephthalate and polyethylene naphthalate.

[0016] When the support is a resin plate, the resin content in the support is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, based on the total mass of the support. The upper limit is 100% by mass.

[0017] The thickness of the support is preferably 5 to 188 μm, and more preferably 25 to 100 μm. When the thickness of the support is within the above range, it offers an excellent balance between handling and thinning, and can be suitably applied to roll-to-roll methods involving heat treatment. The thickness of the support mentioned above is the average thickness, obtained by measuring the thickness at five or more arbitrary points on the support and taking the arithmetic mean of those measurements.

[0018] The elastic modulus of the support at 160°C is preferably 5 to 100 MPa, and more preferably 20 to 60 MPa. When the thickness of the support is within the above range, it offers an excellent balance between dimensional stability and thinning, and is suitable for use in roll-to-roll methods involving heat treatment. One method for measuring the elastic modulus of a support is the method based on JIS K7161.

[0019] (Release layer) The release layer is a layer that is placed in contact with the solid polymer electrolyte membrane, which will be described later. Examples of materials included in the release layer include resins such as polyolefins. Polyethylene and polypropylene are particularly preferred because they offer an excellent balance between adhesion to the solid polymer electrolyte membrane and release properties.

[0020] The weight-average molecular weight of polyethylene is preferably 20,000 to 7,000,000, and more preferably 20,000 to 300,000. The weight-average molecular weight of polypropylene is preferably 40,000 to 300,000, and more preferably 40,000 to 200,000.

[0021] If the release layer contains resin, the resin content in the release layer is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, based on the total mass of the release layer. The upper limit is 100% by mass.

[0022] The thickness of the release layer is preferably 5 to 200 μm, and more preferably 25 to 100 μm. When the thickness of the release layer is within the above range, an excellent balance is achieved between adhesion to the solid polymer electrolyte membrane and thinning. The thickness of the release layer mentioned above is the average thickness, obtained by measuring the thickness at five or more arbitrary points on the release layer and taking the arithmetic mean of those measurements.

[0023] The modulus of elasticity of the release layer at 160°C is preferably 1 MPa or less, and more preferably 0.5 MPa or less. There is no particular lower limit to the modulus of elasticity, however, in this specification, if the test specimen melts and falls off when gripped by the grips of a tensile testing machine in an environment of 160°C, making measurement impossible, the modulus of elasticity shall be stated as 0 MPa. The elastic modulus of the support at 160°C is preferably greater than that of the release layer at 160°C. For example, it is more preferable that the elastic modulus of the support at 160°C is 1 to 80 MPa greater than that of the release layer at 160°C, and even more preferable that it is 5 to 50 MPa greater. When the elastic modulus of the support at 160°C is greater than that of the release layer at 160°C, the dimensional stability of the laminate is excellent when the laminate is applied to a roll-to-roll method involving heat treatment. The method for measuring the elastic modulus of the release layer is the same as the method for measuring the elastic modulus of the support.

[0024] (Other layers) The release substrate may include layers other than the support and release layer. For example, the release substrate may include an adhesion layer between the support and the release layer to improve their adhesion. Examples of adhesive layers include adhesive layers using adhesives and adhesive layers using tacks.

[0025] (Method for manufacturing a releaseable substrate) Methods for manufacturing a releaseable substrate include, for example, applying a release layer-forming composition containing a resin and solvent capable of forming a release layer onto a support, and then performing drying and curing treatments as necessary to form a release layer. Another method involves coating the support with a molten resin to form a release layer. Yet another method involves applying an adhesive solution to the support, drying it, and then bonding a release layer to it using a dry lamination method.

[0026] [Solid polymer electrolyte membrane] The solid polymer electrolyte membrane includes a fluorine-containing polymer having ion exchange groups (hereinafter also referred to as "fluorine-containing polymer (I)") and a woven fabric. Below, we will first describe in detail the materials contained in the polymer electrolyte membrane, and then describe in detail the properties of the solid polymer electrolyte membrane.

[0027] (Fluorine polymer (I)) The ion exchange capacity of the fluorine-containing polymer (I) is preferably 0.90 milliequivalents / gram dry resin or higher, more preferably greater than 1.10 milliequivalents / gram dry resin, even more preferably 1.15 milliequivalents / gram dry resin or higher, particularly preferably 1.20 milliequivalents / gram dry resin or higher, and most preferably 1.25 milliequivalents / gram dry resin or higher, as this allows for a greater reduction in the electrolytic voltage when the solid polymer electrolyte membrane is applied to a membrane electrode assembly. The upper limit of the ion exchange capacity of the fluorine-containing polymer (I) is preferably 2.00 milliequivalents / gram dry resin or less, more preferably 1.50 milliequivalents / gram dry resin or less, and even more preferably 1.43 milliequivalents / gram dry resin or less, from the viewpoint of superior properties of the solid polymer electrolyte membrane.

[0028] The fluorine-containing polymer (I) used in the solid polymer electrolyte membrane may be a single type, or two or more types may be used in a laminated or mixed configuration. The solid polymer electrolyte membrane may contain polymers other than fluorine-containing polymer (I) (hereinafter also referred to as "other polymers"), but it is preferable that the polymers in the solid polymer electrolyte membrane consist substantially of fluorine-containing polymer (I). "Consistently consisting of fluorine-containing polymer (I)" means that the content of fluorine-containing polymer (I) is 95% by mass or more of the total mass of polymers in the solid polymer electrolyte membrane. An upper limit for the content of fluorine-containing polymer (I) is 100% by mass of the total mass of polymers in the solid polymer electrolyte membrane. Other specific examples of polymers include one or more polyazole compounds selected from the group consisting of polymers of heterocyclic compounds containing one or more nitrogen atoms in the ring, and polymers of heterocyclic compounds containing one or more nitrogen atoms and oxygen and / or sulfur atoms in the ring. Specific examples of polyazole compounds include polyimidazole compounds, polybenzimidazole compounds, polybenzobisimidazole compounds, polybenzoxazole compounds, polyoxazole compounds, polythiazole compounds, and polybenzothiazole compounds. Further, from the viewpoint of oxidation resistance of the solid polymer electrolyte membrane, examples of other polymers also include polyphenylene sulfide resins and polyphenylene ether resins.

[0029] The fluoropolymer (I) has ion exchange groups. Specific examples of the ion exchange groups include sulfonic acid-type functional groups and carboxylic acid-type functional groups, and sulfonic acid-type functional groups are preferred from the viewpoint that the electrolysis voltage can be further reduced when the solid polymer electrolyte membrane is applied to a membrane-electrode assembly. Hereinafter, embodiments of the fluoropolymer having a sulfonic acid-type functional group (hereinafter also referred to as "fluoropolymer (S)") will be mainly described in detail.

[0030] The fluoropolymer (S) preferably comprises units based on a fluoroolefin, as well as units having a sulfonic acid-type functional group and a fluorine atom. Examples of the fluoroolefin include fluoroolefins having 2 to 3 carbon atoms and one or more fluorine atoms in the molecule. Specific examples of the fluoroolefin include tetrafluoroethylene (hereinafter also referred to as "TFE"), chlorotrifluoroethylene, vinylidene fluoride, vinyl fluoride, and hexafluoropropylene. Among these, TFE is preferred from the viewpoints of excellent monomer production cost, reactivity with other monomers, and properties of the resulting fluoropolymer (S). The fluoroolefins may be used alone, or two or more thereof may be used in combination.

[0031] As the unit having a sulfonic acid-type functional group and a fluorine atom, a unit represented by formula (1) is preferred. Formula (1) -[CF2-CF(-L-(SO3M) n )]-

[0032] L is an n+1 valent perfluorohydrocarbon group which may contain an etheric oxygen atom. The etheric oxygen atom may be located at a terminal of the perfluorohydrocarbon group, or may be located between carbon atoms. The number of carbon atoms in the n+1 valent perfluorohydrocarbon group is preferably 1 or more, more preferably 2 or more, preferably 20 or less, and more preferably 10 or less.

[0033] As L, an n+1 valent perfluoroaliphatic hydrocarbon group which may contain an etheric oxygen atom is preferred, and more preferably, a divalent perfluoroalkylene group which may contain an etheric oxygen atom in the n=1 embodiment, or a trivalent perfluoroaliphatic hydrocarbon group which may contain an etheric oxygen atom in the n=2 embodiment. The above-mentioned divalent perfluoroalkylene group may be in either a linear or branched chain configuration.

[0034] M is a hydrogen atom, an alkali metal, or a quaternary ammonium cation. n is either 1 or 2. If n is 2, the multiple Ms may be the same or different.

[0035] The units represented by formula (1) are preferably those represented by formula (1-1), formula (1-2), formula (1-3), or formula (1-4). Equation (1-1) -[CF2-CF(-OR f1 -SO3M)]- Equation (1-2) -[CF2-CF(-R f1 -SO3M)]-

[0036] [ka]

[0037] [ka]

[0038] R f1This is a perfluoroalkylene group which may contain an oxygen atom between carbon atoms. The number of carbon atoms in the above perfluoroalkylene group is preferably 1 or more, more preferably 2 or more, preferably 20 or less, and more preferably 10 or less.

[0039] R f2 This is a perfluoroalkylene group which may contain a single bond or an oxygen atom between carbon atoms. The number of carbon atoms in the above perfluoroalkylene group is preferably 1 or more, more preferably 2 or more, preferably 20 or less, and more preferably 10 or less.

[0040] R f3 This is a perfluoroalkylene group which may contain a single bond or an oxygen atom between carbon atoms. The number of carbon atoms in the above perfluoroalkylene group is preferably 1 or more, more preferably 2 or more, preferably 20 or less, and more preferably 10 or less.

[0041] r is either 0 or 1. m is either 0 or 1. M is a hydrogen atom, an alkali metal, or a quaternary ammonium cation.

[0042] The units represented by formula (1-1) and formula (1-2) are preferably the units represented by formula (1-5). Equation (1-5) -[CF2-CF(-(CF2) x -(OCF2CFY) y -O-(CF2) z -SO3M)]- x is 0 or 1, y is an integer between 0 and 2, z is an integer between 1 and 4, and Y is either F or CF3. M is as described above.

[0043] The following are specific examples of units represented by equation (1-1). In the equation, w is an integer from 1 to 8, and x is an integer from 1 to 5. The definition of M in the equation is as described above. -[CF2-CF(-O-(CF2) w -SO3M)]- -[CF2-CF(-O-CF2CF(CF3)-O-(CF2) w -SO3M)]- -[CF2-CF(-(O-CF2CF(CF3)) x -SO3M)]-

[0044] The following are specific examples of units represented by equation (1-2). In the equation, w is an integer from 1 to 8. The definition of M in the equation is as described above. -[CF2-CF(-(CF2) w -SO3M)]- -[CF2-CF(-CF2-O-(CF2) w -SO3M)]-

[0045] The unit represented by formula (1-3-1) is preferred over the unit represented by formula (1-3-3). The definition of M in the formula is as described above.

[0046] [ka]

[0047] R f4 R is a linear perfluoroalkylene group having 1 to 6 carbon atoms, f5 is a linear perfluoroalkylene group having 1 to 6 carbon atoms, which may contain single bonds or oxygen atoms between carbon atoms. The definitions of r and M are as described above.

[0048] The following are specific examples of units represented by equation (1-3-1):

[0049] [ka]

[0050] The unit represented by formula (1-4) is preferably the unit represented by formula (1-4-1). f1 , R f2 The definition of M is as described above.

[0051] [ka]

[0052] The following are specific examples of units represented by equation (1-4-1):

[0053] [ka]

[0054] The units having a sulfonic acid-type functional group and a fluorine atom may be used individually or in combination of two or more types.

[0055] The fluorine-containing polymer (S) may include units based on fluorine-containing olefins, as well as units based on monomers other than those having sulfonic acid-type functional groups and fluorine atoms (hereinafter also referred to as "other monomers"). Other specific examples of monomers include CF2 = CFR f6 (However, R f6 CF2=CF-OR f7 (However, R f7 ) is a perfluoroalkyl group having 1 to 10 carbon atoms. ), CF2 = CFO(CF2) v One example is CF = CF² (where v is an integer between 1 and 3). The content of units based on other monomers is preferably 30% by mass or less relative to the total units in the fluorine-containing polymer (S), in order to maintain ion exchange performance.

[0056] (woven fabric) The opening ratio of the woven fabric is preferably 50.0% or more, more preferably 55.0% or more, even more preferably 60.0% or more, and particularly preferably 70.0% or more, as this allows for a further reduction in the electrolysis voltage when the solid polymer electrolyte membrane is applied to the membrane electrode assembly. The upper limit of the opening ratio of the woven fabric is preferably 90.0% or less, and more preferably 80.0% or less, in that it provides superior strength to the solid polymer electrolyte membrane. The opening ratio of a woven fabric is calculated using the following formula (ε), based on the average diameter R1 of the yarn and the average spacing P1 between adjacent yarns (hereinafter also referred to as "pitch P1"). Here, the average thread diameter R1 refers to the arithmetic mean of the diameters of 10 different threads arbitrarily selected based on a magnified image (e.g., 100x) of the woven fabric surface obtained using a microscope. The pitch P1 refers to the arithmetic mean of the intervals between 10 different points arbitrarily selected based on a magnified image (e.g., 100x) of the woven fabric surface obtained using a microscope. Opening ratio of woven fabric (%) = [P1 / (P1+R1)] 2 ×100 (ε)

[0057] The denier counts of yarn A and yarn B constituting the woven fabric are preferably 2.0 or higher, more preferably 10.0 or higher, and even more preferably 15.0 or higher, independently of each other, in terms of providing superior strength and dimensional stability of the solid polymer electrolyte membrane. The upper limits for the denier count of yarn A and yarn B constituting the woven fabric are, independently, preferably 60.0 or less, more preferably 50.0 or less, and even more preferably 20.0 or less, in terms of being able to further reduce the electrolysis voltage when the solid polymer electrolyte membrane is applied to the membrane electrode assembly. The denier count is the mass of 9000 meters of yarn expressed in grams (g / 9000m).

[0058] The densities of threads A and B are preferably 50 threads / inch (19.7 threads / cm) or more, more preferably 70 threads / inch (27.6 threads / cm) or more, and even more preferably 90 threads / inch (35.4 threads / cm) or more, respectively, in terms of excellent strength and dimensional stability of the solid polymer electrolyte membrane. In terms of further reducing the electrolytic voltage when the solid polymer electrolyte membrane is applied to a membrane electrode assembly, the densities are preferably 200 threads / inch (78.7 threads / cm) or less, more preferably 150 threads / inch (59.1 threads / cm) or less, and even more preferably 100 threads / inch (39.4 threads / cm) or less.

[0059] Threads A and B may consist of either a monofilament made of one filament or a multifilament made of two or more filaments, with monofilaments being preferred.

[0060] Yarn A and yarn B are preferably each independently composed of at least one material selected from the group consisting of polytetrafluoroethylene (hereinafter also referred to as "PTFE"), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (hereinafter also referred to as "PFA"), polyether ether ketone (hereinafter also referred to as "PEEK"), and polyphenylene sulfide (hereinafter also referred to as "PPS"), in order to have superior yarn durability. Threads A and B are preferably composed of slit yarns because they offer superior durability and strength.

[0061] In the woven fabric, it is preferable that yarn A and yarn B are approximately perpendicular. Approximately perpendicular means that the angle between yarn A and yarn B is 90 ± 10 degrees. Thread A may be either a warp thread or a weft thread in a woven fabric, but if thread A is a weft thread, then thread B is a warp thread, and if thread A is a warp thread, then thread B is a weft thread.

[0062] When the material constituting the woven fabric is PTFE, the basis weight of the fabric should be 20.0 to 40.0 g / m², as this provides an excellent balance between the strength and handling properties of the solid polymer electrolyte membrane. 2 Preferably, 30.0-40.0 g / m 2 This is preferable. When the material constituting the woven fabric is PFA, the basis weight of the woven fabric should be between 10.0 and 30.0 g / m², as this provides an excellent balance between the strength and handling properties of the solid polymer electrolyte membrane. 2 Preferably, 10.0 to 20.0 g / m 2 This is preferable. When the material constituting the woven fabric is PEEK, the basis weight of the woven fabric should be between 5.0 and 40.0 g / m², as this provides an excellent balance between the strength and handling properties of the solid polymer electrolyte membrane.2 Preferably, 5.0 to 30.0 g / m² 2 This is preferable. When the material constituting the woven fabric is PPS, the basis weight of the woven fabric should be between 5.0 and 40.0 g / m², as this provides an excellent balance between the strength and handling properties of the solid polymer electrolyte membrane. 2 Preferably, 5.0 to 30.0 g / m² 2 This is preferable.

[0063] (Properties of solid polymer electrolyte membranes) The solid polymer electrolyte membrane may have a single-layer structure or a multi-layer structure, but a single-layer structure is preferred. In the case of a multilayer structure, for example, one embodiment involves stacking multiple layers containing a fluorine-containing polymer (I) with different ion exchange capacities.

[0064] The surface of the solid polymer electrolyte membrane on the release layer side preferably has an uneven structure. Having an uneven surface on the release layer side of the solid polymer electrolyte membrane allows the release layer material to penetrate into the recesses of the uneven structure, resulting in improved adhesion between the solid polymer electrolyte membrane and the release layer. The above-mentioned uneven structure is formed by including a woven fabric within the solid polymer electrolyte membrane. For example, the height of the protrusions in the uneven structure can be adjusted by adjusting the film thickness of the solid polymer electrolyte membrane.

[0065] It is preferable that the surface of the solid polymer electrolyte membrane opposite to the release layer side has an uneven surface. When the laminate is wound into a roll, the surface of the solid polymer electrolyte membrane opposite to the release layer side and the surface of the release substrate opposite to the release layer side slide easily, and as a result, the laminate can be unwound stably from the roll. The above-mentioned uneven structure is formed by including a woven fabric within the solid polymer electrolyte membrane. For example, the height of the protrusions in the uneven structure can be adjusted by adjusting the film thickness of the solid polymer electrolyte membrane. Furthermore, when manufacturing solid polymer electrolyte membranes, flat plate presses and hot roll presses are mentioned as methods for laminating woven fabric onto the precursor membrane of the solid polymer electrolyte membrane. When continuously laminating with a hot roll press, back tension is sometimes applied to the unwinding of the woven fabric and precursor membrane to stabilize their transport. When back tension is applied to the woven fabric, the back tension acts on the threads extending in the MD (Machine Direction), causing the threads extending in the MD to become taut. At the same time, the threads extending in the TD (Traverse Direction) become more three-dimensionally deformed compared to when no back tension is applied. When the woven fabric is laminated onto the precursor membrane in this state, the shape of the threads extending in the TD, which have become more three-dimensionally deformed, is maintained. In other words, the height of the convex parts of the uneven structure can also be adjusted by adjusting the back tension during hot roll pressing.

[0066] When the woven fabric contained in a solid polymer electrolyte membrane is composed of thread A extending in one direction and thread B extending in a direction substantially perpendicular to thread A, the maximum thickness TA and minimum thickness TB of the solid polymer electrolyte membrane are measured for each of 10 different cross-sections obtained by cutting the solid polymer electrolyte membrane at a midpoint between threads A, in a direction parallel to the direction in which thread A extends. Furthermore, the maximum thickness TA and minimum thickness TB of the solid polymer electrolyte membrane are measured for each of 10 different cross-sections obtained by cutting the solid polymer electrolyte membrane at a midpoint between threads B, in a direction parallel to the direction in which thread B extends. The average minimum thickness TB is calculated by arithmetic mean of the 20 obtained TBs. AVE The average maximum film thickness TA obtained by arithmetic meaning the 20 TAs obtained. AVE In this case, the average maximum film thickness TA AVE and average minimum film thickness TB AVE It is preferable that the following relationship (X) is satisfied. Formula (X) 0.5μm≦(TA AVE -TB AVE ) / 2 In other words, the average maximum film thickness TA AVE and average minimum film thickness TB AVE The difference (TA)AVE -TB AVE Half the value of ((TA AVE -TB AVE ) / 2) is preferably 0.5 μm or larger. The above (TA) AVE -TB AVE When the ) / 2 is 0.5 μm or greater, the adhesion between the release layer and the solid polymer electrolyte membrane is improved, or the unwinding from the roll obtained by winding the laminate is improved. In particular, the above (TA) AVE -TB AVE The value of (TA) / 2 is more preferably 1.0 μm or more, even more preferably 2.0 μm or more, even more preferably 3.0 μm or more, particularly preferably 5.0 μm or more, and most preferably 10.0 μm or more. AVE -TB AVE There is no particular upper limit to the value of ) / 2, but it is often 30.0 μm or less, and more often 20.0 μm or less. The above (TA) AVE -TB AVE The method for calculating ) / 2 will be explained using a diagram.

[0067] Figure 3 is a cross-sectional view showing an example of a solid polymer electrolyte membrane included in the laminate of the present invention when cut in a direction parallel to the direction in which yarn A extends. Specifically, it is the cross-section exposed when the solid polymer electrolyte membrane is cut along the line A-A' in Figure 5, which will be described later. In the cross-section of the solid polymer electrolyte membrane 14 in Figure 3, the electrolyte 20 containing a fluorine-containing polymer (I) and the yarns 22a, 22b, and 22c arranged in the electrolyte 20 are exposed. Yarns 22a, 22b, and 22c correspond to yarn B that constitutes the woven fabric 22. Figure 4 is a cross-sectional view showing an example of a solid polymer electrolyte membrane included in the laminate of the present invention being cut in a direction parallel to the direction in which yarn B extends. Specifically, it is the cross-section exposed when the solid polymer electrolyte membrane is cut along the line B-B' in Figure 5, which will be described later. In the cross-section of the solid polymer electrolyte membrane 14 in Figure 4, the electrolyte 20 containing a fluorine-containing polymer (I) and the yarns 22A, 22B, and 22C arranged in the electrolyte 20 are exposed. Yarns 22A, 22B, and 22C correspond to yarn A that constitutes the woven fabric 22. Figure 5 is a schematic plan view of the woven fabric 22 in the solid polymer electrolyte membrane 14 as seen in the direction of film thickness. As shown in Figure 5, the woven fabric 22 includes yarns A, namely yarns 22A, 22B, and 22C, and yarns B, namely yarns 22a, 22b, and 22c, which are substantially perpendicular to yarn A.

[0068] First, the maximum film thickness TA and minimum film thickness TB of the solid polymer electrolyte membrane are measured for each of 10 different cross-sections obtained by cutting the solid polymer electrolyte membrane at midpoints between threads A, in a direction parallel to the direction in which threads A extend within the membrane. Specifically, in the example shown in Figure 5, the solid polymer electrolyte membrane 14 is cut along the A-A' line, which is located midway between thread A (thread 22A) and thread 22B. This exposes the cross-section of the solid polymer electrolyte membrane 14 as shown in Figure 3. Similarly, the solid polymer electrolyte membrane 14 is cut at a location other than the midpoint between threads 22A and 22B (for example, midway between threads 22B and 22C) to expose the cross-section of the solid polymer electrolyte membrane 14. After obtaining 10 different cross-sections in this manner, the maximum film thickness TA and minimum film thickness TB are measured for each cross-section. Furthermore, the maximum film thickness TA and minimum film thickness TB of the solid polymer electrolyte membrane are measured for each of 10 different cross-sections obtained by cutting the solid polymer electrolyte membrane at midpoints between threads B, in a direction parallel to the direction in which the threads B extend within the solid polymer electrolyte membrane. Specifically, in the example shown in Figure 5, the solid polymer electrolyte membrane 14 is cut along the B-B' line, which is located midway between threads 22a and 22b (which are thread B). This exposes the cross-section of the solid polymer electrolyte membrane 14 as shown in Figure 4. Similarly, the solid polymer electrolyte membrane 14 is cut at a location other than the midpoint between threads 22a and 22b (for example, midway between threads 22b and 22c) to expose the cross-section of the solid polymer electrolyte membrane 14. After obtaining 10 different cross-sections in this manner, the maximum film thickness TA and minimum film thickness TB are measured for each cross-section. Next, the average maximum film thickness TA was obtained by arithmetic mean TA of the 20 TAs obtained. AVE Then, the arithmetic mean of the 20 obtained TBs is calculated to find the average minimum film thickness TB. AVE To find the average maximum film thickness TA, AVE and average minimum film thickness TB AVE Find the difference between and then divide that value by 2 to get (TA AVE -TB AVE Let's assume ) / 2.

[0069] The above (TA) AVE -TB AVE While not limited to this method, one way to adjust the size of ) / 2 is to sandwich the precursor film of the solid polymer electrolyte film between low-melting-point films (described later) and heat-press it during the manufacturing of the solid polymer electrolyte film. As a result, the low-melting-point film deforms to conform to the surface shape of the precursor film, and a solid polymer electrolyte film is obtained having an uneven surface structure in which the parts where threads A and B constituting the woven fabric are present are convex, and the parts where threads A and B are absent are concave. Furthermore, as mentioned above, by adjusting the back tension during hot roll pressing, the height of the protrusions in the uneven structure can be adjusted, and together with (TA AVE -TB AVE You can also adjust the size of ) / 2.

[0070] In this case, for measuring the film thickness of the solid polymer electrolyte membrane, the solid polymer electrolyte membrane is peeled from the laminate and dried at 90°C for 2 hours to obtain a sample. Furthermore, the maximum film thickness TA and minimum film thickness TB are measured using magnified images (e.g., 100x magnification) of the cross-section of the solid polymer electrolyte membrane taken with an optical microscope (product name "BX-51", manufactured by Olympus Corporation).

[0071] Average maximum film thickness TA of solid polymer electrolyte membranes AVE When a solid polymer electrolyte membrane is applied to a membrane electrode assembly, the electrolytic voltage can be further reduced, so a thickness of 60 to 250 μm is preferred, 60 to 200 μm is more preferred, 60 to 140 μm is even more preferred, 60 to 120 μm is particularly preferred, and 60 to 100 μm is most preferred. Average minimum film thickness of solid polymer electrolyte membranes TB AVE The thickness of the membrane electrode assembly containing the solid polymer electrolyte membrane is preferably 30 to 220 μm, more preferably 30 to 200 μm, even more preferably 30 to 130 μm, particularly preferably 30 to 100 μm, particularly preferably 30 to 80 μm, and particularly preferably 30 to 70 μm, as this can further improve the strength of the membrane electrode assembly containing the solid polymer electrolyte membrane.

[0072] (Method for manufacturing solid polymer electrolyte membranes) One method for producing a solid polymer electrolyte membrane involves producing a precursor membrane containing a polymer of a fluorine-containing monomer (hereinafter also referred to as "fluorine-containing monomer (I')") having a group that can be converted into an ion exchange group (hereinafter also referred to as "fluorine-containing polymer (I')") and a membrane containing a woven fabric (hereinafter also referred to as "precursor membrane (I')"), and then producing the membrane by converting the groups in the precursor membrane (I') that can be converted into ion exchange groups into ion exchange groups.

[0073] In this context, a preferred embodiment of the method for producing the precursor film (I') is a method in which a laminate in which a fluorine-containing polymer (I') is arranged on both sides of a woven fabric is sandwiched between transfer substrates such as a low-melting-point film with a melting point of 70 to 180°C, and then heated and pressed. Specific examples of low-melting-point films include polyethylene film, polypropylene film, and polystyrene film.

[0074] The form of the woven fabric is as described above. As the fluorine-containing polymer (I'), a polymer of a fluorine-containing monomer having a group that can be converted to a sulfonic acid-type functional group (hereinafter also referred to as "fluorine-containing polymer (S')") is preferred, and a fluorine-containing polymer (S') obtained by copolymerizing a fluorine-containing olefin with a monomer having a group that can be converted to a sulfonic acid-type functional group and a fluorine atom is particularly preferred. The following provides a detailed explanation of fluorine-containing polymers (S').

[0075] Methods for copolymerizing fluorine-containing polymers (S') can include known methods such as solution polymerization, suspension polymerization, and emulsion polymerization.

[0076] Examples of fluorine-containing olefins include those exemplified above, and TFE is preferred due to its superior monomer production cost, reactivity with other monomers, and the characteristics of the resulting fluorine-containing polymer (S). Fluorine-containing olefins may be used individually or in combination of two or more types.

[0077] Examples of fluorine-containing monomers (S') include compounds that have one or more fluorine atoms in the molecule, have an ethylenically active double bond, and have a group that can be converted to a sulfonic acid-type functional group. As the fluorine-containing monomer (S'), the compound represented by formula (2) is preferred due to its superior manufacturing cost, reactivity with other monomers, and the characteristics of the resulting fluorine-containing polymer (S). Equation (2) CF2 = CF - L - (A) n The definitions of L and n in equation (2) are as described above. A is a group that can be converted to a sulfonic acid type functional group. Preferably, the group can be converted to a sulfonic acid type functional group by hydrolysis. Specific examples of groups that can be converted to a sulfonic acid type functional group include -SO2F, -SO2Cl, and -SO2Br.

[0078] The compounds represented by formula (2) are preferably those represented by formula (2-1), formula (2-2), formula (2-3), or formula (2-4). Equation (2-1) CF2 = CF - OR f1 -A Equation (2-2) CF2 = CF - R f1 -A

[0079] [ka]

[0080] R in the formula f1 , R f2 The definitions of r and A are as described above.

[0081] [ka]

[0082] R in the formula f1 , R f2 , R f3 The definitions of r, m, and A are as described above.

[0083] The compound represented by formula (2-1) and, more preferably, the compound represented by formula (2-5). Equation (2-5) CF2 = CF - (CF2) x -(OCF2CFY) y -O-(CF2) z -SO2F The definitions of x, y, z, and Y in the equation are as described above.

[0084] Specific examples of compounds represented by formula (2-1) include the following compounds. In the formula, w is an integer from 1 to 8, and x is an integer from 1 to 5. CF2 = CF - O - (CF2) w -SO2F CF2 = CF - O - CF2CF(CF3) - O - (CF2) w -SO2F CF2=CF-[O-CF2CF(CF3)] x -SO2F

[0085] Specific examples of the compound represented by formula (2-2) include the following compounds. w in the formula is an integer of 1 to 8. CF2=CF-(CF2) w -SO2F CF2=CF-CF2-O-(CF2) w -SO2F

[0086] As the compound represented by formula (2-3), the compound represented by formula (2-3-1) is preferred.

[0087] [Chemical Formula]

[0088] R in the formula f4 , R f5 , r and A are as defined above.

[0089] Specific examples of the compound represented by formula (2-3-1) include the following.

[0090] [Chemical Formula]

[0091] As the compound represented by formula (2-4), the compound represented by formula (2-4-1) is preferred.

[0092] [Chemical Formula]

[0093] R in the formula f1 , R f2 and A are as defined above.

[0094] Specific examples of compounds represented by formula (2-4-1) include the following:

[0095] [ka]

[0096] Fluorine-containing monomers (S') may be used individually or in combination of two or more. In addition to fluorine-containing olefins and fluorine-containing monomers (S'), other monomers may also be used in the production of fluorine-containing polymers (S'). Examples of other monomers include those exemplified above.

[0097] The ion exchange capacity of the fluorine-containing polymer (I') can be adjusted by changing the content of groups that can be converted into ion exchange groups in the fluorine-containing polymer (I').

[0098] A specific example of a method for manufacturing a precursor film is the extrusion method. More specifically, a film (I') made of a fluorine-containing polymer (I') is formed, and then the film (I'), woven fabric, and film (I') are arranged in that order and stacked using a lamination roll or a vacuum lamination apparatus.

[0099] Specific examples of methods for converting groups in a precursor membrane that can be converted into ion exchange groups include methods of subjecting the precursor membrane to hydrolysis treatment or acidification treatment. Among these methods, the method of contacting the precursor film with an alkaline aqueous solution is preferred.

[0100] Specific examples of methods for bringing a precursor film into contact with an alkaline aqueous solution include immersing the precursor film in an alkaline aqueous solution and spraying the alkaline aqueous solution onto the surface of the precursor film. The temperature of the alkaline aqueous solution is preferably 30 to 100°C, and more preferably 40 to 100°C. The contact time between the precursor film and the alkaline aqueous solution is preferably 3 to 150 minutes, and more preferably 5 to 50 minutes.

[0101] The alkaline aqueous solution preferably contains an alkali metal hydroxide, a water-soluble organic solvent, and water. Examples of alkali metal hydroxides include sodium hydroxide and potassium hydroxide. In this specification, a water-soluble organic solvent is an organic solvent that dissolves readily in water. Specifically, an organic solvent with a solubility of 0.1 g or more in 1000 ml of water (20°C) is preferred, and an organic solvent with a solubility of 0.5 g or more is more preferred. The water-soluble organic solvent preferably contains at least one selected from the group consisting of aprotic organic solvents, alcohols, and amino alcohols, and more preferably contains an aprotic organic solvent. Water-soluble organic solvents may be used individually or in combination of two or more types.

[0102] Specific examples of aprotic organic solvents include dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, and N-ethyl-2-pyrrolidone, with dimethyl sulfoxide being preferred. Specific examples of alcohols include methanol, ethanol, isopropanol, butanol, methoxyethoxyethanol, butoxyethanol, butylcarbitol, hexyloxyethanol, octanol, 1-methoxy-2-propanol, and ethylene glycol. Specific examples of amino alcohols include ethanolamine, N-methylethanolamine, N-ethylethanolamine, 1-amino-2-propanol, 1-amino-3-propanol, 2-aminoethoxyethanol, 2-aminothioethoxyethanol, and 2-amino-2-methyl-1-propanol.

[0103] The concentration of alkali metal hydroxide in the alkaline aqueous solution is preferably 1 to 60% by mass, and more preferably 3 to 55% by mass. The content of the water-soluble organic solvent is preferably 1 to 60% by mass, and more preferably 3 to 55% by mass, in the alkaline aqueous solution. The water concentration is preferably 39-80% by mass in the alkaline aqueous solution.

[0104] After contact between the precursor film and the alkaline aqueous solution, a treatment to remove the alkaline aqueous solution may be performed. One method for removing the alkaline aqueous solution is to wash the precursor film that has been in contact with the alkaline aqueous solution with water.

[0105] After contacting the precursor film with an alkaline aqueous solution, the resulting film may be brought into contact with an acidic aqueous solution to convert the ion exchange groups to the acidic form. Specific examples of methods for bringing a precursor film into contact with an acidic aqueous solution include immersing the precursor film in an acidic aqueous solution and spraying the acidic aqueous solution onto the surface of the precursor film. An acidic aqueous solution preferably contains an acidic component and water. Specific examples of acidic components include hydrochloric acid and sulfuric acid.

[0106] [Method for manufacturing laminates] One method for manufacturing the laminate is to heat-press the release substrate and the solid polymer electrolyte membrane so that the solid polymer electrolyte membrane faces the release layer side of the release substrate. When heat-pressing, a roll-to-roll method using a hot roll press may be used. When using a hot roll press for heat sealing, the roll temperature is preferably 60 to 200°C, and more preferably 90 to 170°C.

[0107] [Rolled form] A roll body is obtained by winding the laminate of the present invention. The roll body form facilitates handling, such as transportation. When winding the laminate, the laminate may be wound around a winding core if necessary.

[0108] [Application] The laminate of the present invention can be used for various applications. For example, it can be used to form a membrane electrode assembly. More specifically, a catalyst layer can be formed on a solid polymer electrolyte membrane in the laminate, a peelable substrate can be peeled off, and a further catalyst layer can be formed on the surface of the exposed solid polymer electrolyte membrane to form a membrane electrode assembly. The method for manufacturing the catalyst layer involves applying a catalyst layer forming coating solution to a predetermined location and drying it as necessary. The catalyst layer forming coating solution is a liquid in which a polymer having ion exchange groups and a catalyst are dispersed in a dispersion medium.

[0109] The resulting membrane electrode assembly can be used in a water electrolysis apparatus (specifically, a solid polymer water electrolysis apparatus). Furthermore, the membrane electrode assembly can be used as a diaphragm in an electrolytic hydrogenation apparatus for aromatic compounds (e.g., toluene). [Examples]

[0110] The present invention will be described in detail below with reference to examples. Examples 1 to 10 are examples, and Example 11 is a comparative example. However, the present invention is not limited to these examples. [film thickness] Average maximum film thickness TA of solid polymer electrolyte membranes AVE , average minimum film thickness TB AVE , and, (TA AVE -TB AVE ) / 2 was calculated according to the method described in the section on the solid polymer electrolyte membrane above.

[0111] [Ion exchange capacity of fluorine-containing polymers] A fluorine-containing polymer was placed in a glove box circulating dry nitrogen for 24 hours, and its dry mass was measured. Subsequently, the fluorine-containing polymer was immersed in a 2 mol / L sodium chloride aqueous solution at 60°C for 1 hour. After washing the fluorine-containing polymer with ultrapure water, it was removed, and the ion exchange capacity (milliequivalents / gram dry resin) of the fluorine-containing polymer was determined by titrating the immersion solution with a 0.1 mol / L sodium hydroxide aqueous solution.

[0112] [Fabric weight] The used original woven fabric was cut into a size of 20×20 cm, and the mass was measured. The above measurement was performed 5 times, and based on the average value, the basis weight of the woven fabric (g / m 2 ) was determined.

[0113] [Density of Warp and Weft Constituting Woven Fabric] The density of the warp and weft constituting the woven fabric was calculated according to the following method. For each of the warp and weft, from the observation image of an optical microscope, the average value of 5 measurements of the length formed by 10 yarns was converted and calculated as the density (yarns / inch).

[0114] [Open Area Ratio of Woven Fabric] Using a sample obtained by cutting the used original woven fabric into a size of 20×20 cm, the calculation was performed according to the method described in the section explaining the woven fabric above.

[0115] [Denier Number of Warp and Denier Number of Weft Constituting Woven Fabric] The denier number of the warp and the denier number of the weft constituting the woven fabric were calculated according to the following method. Five opening regions were randomly selected, the opening ratio was calculated from the observation image of an optical microscope, and the average value was taken as the open area ratio.

[0116] [Adhesion Evaluation] The peel force between the peelable substrate and the solid polymer electrolyte membrane was measured in accordance with JIS Z0237 using a Tensilon universal material testing machine RTF-2430 (manufactured by A&D Co., Ltd.) under the conditions of a peel angle of 180 degrees, a peel speed of 300 mm / min, a test piece width of 25 mm, and a test piece length of 50 mm, in an environment at a temperature of 23°C and a relative humidity of 50%. The measured peel force was evaluated according to the following criteria. "○": Peel force of 0.1 to 3 N / 25 mm "△": Peel force exceeding 3 N / 25 mm "×": Peel force less than 0.1 N / 25 mm Note that the peel force is preferably 0.1 N / 25 mm or more from the viewpoint that peeling of the solid polymer electrolyte membrane from the peelable substrate is less likely to occur. Furthermore, if the peeling force is too strong, there is a higher risk of localized rupture of the solid polymer electrolyte membrane during separation of the peelable substrate and the solid polymer electrolyte membrane; therefore, a peeling force of 3N / 25mm or less is preferable.

[0117] [Evaluation of unwinding ability] A cylindrical ABS core (manufactured by Showa Marutsutsu Co., Ltd., outer diameter 88.5 mm, inner diameter 76.5 mm, width 300 mm) was wound with 0.6 m of the laminate obtained in each example, with a width of 280 mm. Then, one end of a biaxially oriented polyester film (manufactured by Teijin DuPont Films Ltd., Merinex®, thickness 0.1 mm, width 280 mm) was connected to the other end of the wound laminate, and then the biaxially oriented polyester film was wound again to obtain a 100 m wound roll. In other words, winding the biaxially oriented polyester film simulated the winding of a laminate with a total length of 100 m. The connection between one end of the laminate and one end of the biaxially oriented polyethylene film was made with heat-resistant polyimide tape (manufactured by 3M Japan Limited, 5412, width 19 mm). The winding tension was based on 30 N / total width. After the obtained rolls were suspended and stored for one month, the biaxially oriented polyester film was unwound from the rolls, and the unwinding performance was evaluated according to the following criteria when unwinding the laminate. "○": The solid polymer electrolyte membrane and the releaseable substrate can be unwound without peeling apart. "×": The solid polymer electrolyte membrane and the release substrate peel off locally, resulting in unstable unwinding. As will be described later, when wrapping the laminate around the ABS core, two types of samples were prepared: one in which the solid polymer electrolyte membrane in the laminate was wrapped outwards so that it was on the outside of the release substrate, and another in which the solid polymer electrolyte membrane in the laminate was wrapped inwards so that it was on the inside of the release substrate. The above evaluation was then performed using both samples.

[0118] [Production of fluorine-containing polymer (S'-1)] CF2=CF2 was copolymerized with monomer (Y) represented by the following formula (Y) to obtain a fluorine-containing polymer (S'-1) (ion exchange capacity: 1.25 milliequivalents / gram dry resin). CF2=CF-O-CF2CF(CF3)-O-CF2CF2-SO2F...(Y)

[0119] [Production of fluorine-containing polymer (S'-2)] CF2=CF2 was copolymerized with the monomer (Y) represented by the above formula (Y) to obtain a fluorine-containing polymer (S'-2) (ion exchange capacity: 1.00 milliequivalent / gram dry resin).

[0120] The ion exchange capacity described in the above section [Production of Fluorine-containing Polymer (S'-1)] represents the ion exchange capacity of the fluorine-containing polymer obtained when fluorine-containing polymer (S'-1) is hydrolyzed according to the procedure described later. Similarly, the ion exchange capacity described in [Production of Fluorine-containing Polymer (S'-2)] represents the ion exchange capacity of the fluorine-containing polymer obtained when fluorine-containing polymer (S'-2) is hydrolyzed by the procedure described later.

[0121] [Manufacturing of film-coated substrate Y1] A film-coated substrate Y1 was obtained by attaching a fluorine-containing polymer (S'-1) to a substrate made of linear low-density polyethylene (LLDPE) film (melting point: 110-120°C, thickness: 0.1 mm) using a melt extrusion method, thereby forming a film α1 (film thickness: 30 μm) made of the fluorine-containing polymer (S'-1) on the substrate.

[0122] [Manufacturing of film-coated substrate Y2] A film-coated substrate Y2 was obtained by attaching a fluorine-containing polymer (S'-1) to a substrate made of biaxially oriented polyester film (Teijin DuPont Films Ltd., Merinex® registered trademark, thickness: 0.1 mm, width: 400 mm) using a melt extrusion method, thereby forming a film α2 (film thickness: 60 μm) made of the fluorine-containing polymer (S'-1) on the substrate.

[0123] [Manufacturing of film-coated substrate Y3] A film-coated substrate Y3 was obtained by attaching a fluorine-containing polymer (S'-2) to a substrate made of biaxially oriented polyester film (manufactured by Teijin DuPont Films Ltd., Merinex® registered trademark, thickness: 0.1 mm, width: 400 mm) using a melt extrusion method, thereby forming a film α3 (film thickness: 60 μm) made of fluorine-containing polymer (S'-2) on the substrate.

[0124] [Manufacturing of film-coated substrate Y4] A film-coated substrate Y4 was obtained by attaching a fluorine-containing polymer (S'-2) to a substrate made of biaxially oriented polyester film (Teijin DuPont Films Ltd., Merinex® registered trademark, thickness: 0.1 mm, width: 400 mm) using a melt extrusion method, thereby forming a film α4 (film thickness: 80 μm) made of fluorine-containing polymer (S'-2) on the substrate.

[0125] [Manufacturing of film-coated substrate Y5] A film-coated substrate Y5 was obtained by attaching a fluorine-containing polymer (S'-2) to a substrate made of biaxially oriented polyester film (Teijin DuPont Films Ltd., Merinex® registered trademark, thickness: 0.1 mm, width: 400 mm) using a melt extrusion method, thereby forming a film α5 (film thickness: 115 μm) made of fluorine-containing polymer (S'-2) on the substrate.

[0126] [Manufacturing of film-coated substrate Y6] A film-coated substrate Y6 was obtained by attaching a fluorine-containing polymer (S'-1) to a substrate made of biaxially oriented polyester film (manufactured by Teijin DuPont Films Ltd., Merinex® registered trademark, thickness: 0.1 mm, width: 400 mm) using a melt extrusion method, thereby forming a film α6 (film thickness: 130 μm) made of fluorine-containing polymer (S'-1) on the substrate.

[0127] [Fabric manufacturing] Fabric A1 was obtained by plain weaving 18.6 denier PFA yarn for both the warp and weft, with a PFA yarn density of 100 threads / inch. The basis weight of fabric A1 was 16.3 g / m². 2The opening ratio of woven fabric A1 was 74.3%. Furthermore, the warp and weft threads were made of slit yarn. Furthermore, threads A and B were composed of monofilaments. Furthermore, woven fabric A2 was manufactured in the same manner as woven fabric A1, except that the types and deniers of the materials constituting the warp and weft threads, as well as the density, basis weight, and opening ratio of the woven fabric were changed to the values ​​listed in Table 1.

[0128] [Manufacturing of releaseable substrate 1] The adhesive was prepared by mixing the main component LX-75A (manufactured by DIC Graphics Co., Ltd.), the hardener KW-75 (manufactured by DIC Graphics Co., Ltd.), and the diluent ethyl acetate in proportions of 60 parts by mass, 10 parts by mass, and 60 parts by mass, respectively. Next, 2 g / m² of solute is added to the support, a biaxially oriented polyester film (manufactured by Teijin DuPont Films Ltd., Merinex® registered trademark, thickness: 50 μm, modulus of elasticity at 160°C: 40 MPa). 2 The above adhesive was applied in such a manner. The solvent of the above adhesive was evaporated in a drying oven to form an adhesive layer. On this adhesive layer, an LDPE film (manufactured by Tamapoly, AJ-1, thickness: 50 μm, modulus of elasticity at 160°C: 0 MPa) was laminated using a dry laminating machine to form a release layer and produce a release substrate 1. At this time, the corona-treated side of the LDPE film was oriented to be bonded to the adhesive layer formed on the support.

[0129] [Manufacturing of releaseable substrate 2] Instead of LDPE film (Tamapoly, AJ-1), LLDPE (low-density polyethylene film (Tamapoly, M-6), thickness: 100 μm, modulus of elasticity at 160°C: 0 MPa) was used to produce release substrate 2, following the same procedure as for the production of release substrate 1.

[0130] [Manufacturing of releaseable substrate 3] A release substrate 3 was manufactured by laminating ETFE (tetrafluoroethylene-ethylene copolymer, single-sided matte film (AGC Corporation, 50HK), thickness: 50 μm, elastic modulus at 160°C: 48 MPa) on the side of the support in the release substrate 2 that does not have a release layer laminated to it, following the same procedure as for manufacturing release substrate 1, with the ETFE and release substrate 2 laminated via an adhesive layer. At this time, the mirrored and corona-treated side of the ETFE film was oriented to be bonded to the adhesive layer formed on the support. [Manufacturing of releaseable substrate 4] A biaxially oriented polyester film (manufactured by Teijin DuPont Films Ltd., Merinex®, thickness: 188 μm, modulus of elasticity at 160°C: 40 MPa) was used as a support, LLDPE (low-density polyethylene film (manufactured by Tamapoly, M-6), thickness: 60 μm, modulus of elasticity at 160°C: 0 MPa) was used as a release layer, and ETFE (tetrafluoroethylene-ethylene copolymer, single-sided frosted film (manufactured by AGC, 30HK), thickness: 30 μm, modulus of elasticity at 160°C: 48 MPa) was used as a release-improving layer on the side of the support that did not have a release layer laminated on it. Following the same procedure as for the manufacture of release substrate 1, each layer was laminated via an adhesive layer, and then the LLDPE side of the release layer was subjected to corona treatment with 42-dyne to manufacture release substrate 4. At this time, the mirror-finish and corona-treated side of the ETFE film was oriented to be bonded to the adhesive layer formed on the support.

[0131] [Example 1] The film-coated substrate Y1, woven fabric A1, and film-coated substrate Y1 were stacked in this order. The film-coated substrate Y1 was positioned so that film α1 on it was in contact with woven fabric A1. Each overlapping component is subjected to a temperature of 160°C and a surface pressure of 30 MPa / m. 2 After heating and pressing the substrates for 10 minutes using a flat plate press, the substrates on both sides were peeled off at a temperature of 50°C to obtain a precursor film.

[0132] The precursor film was immersed in a solution of dimethyl sulfoxide / potassium hydroxide / water = 30 / 5.5 / 64.5 (mass ratio) at 95°C for 30 minutes to hydrolyze the groups in the precursor film that can be converted to sulfonic acid functional groups, converting them to K-type sulfonic acid functional groups, and then washed with water. Subsequently, the obtained film was immersed in 1M sulfuric acid to convert the terminal groups from K-type to H-type, and then dried to obtain solid polymer electrolyte film 1. Average maximum film thickness TA of solid polymer electrolyte membrane 1 AVE It is 91 μm, and the average minimum film thickness TB AVE It is 60 μm, (TA AVE -TB AVE The diameter of ) / 2 was 15.5 μm.

[0133] Next, using a hot roll press device, the fabricated release substrate 1 and the solid polymer electrolyte membrane 1 were introduced between a metal roll and a rubber roll and bonded together by heat compression to obtain a laminate 1. In this case, the laminate 1 obtained as a transport film was laminated in the order of support, release layer, and solid polymer electrolyte membrane 1. The surface pressure of the rubber roll pressed against the metal roll was 200 N / cm, the temperature of both the metal roll and the rubber roll was 160°C, and the conveying speed was 10 cm / min.

[0134] [Example 2] Laminate 2 was obtained by following the same procedure as in Example 1, except that release substrate 2 was used instead of release substrate 1.

[0135] [Example 3] Laminate 3 was obtained by following the same procedure as in Example 1, except that release substrate 3 was used instead of release substrate 1.

[0136] [Example 4] A laminate 4 was obtained by following the same procedure as in Example 1, except that a release substrate 3 was used instead of release substrate 1, and woven fabric A2 was used instead of woven fabric A1.

[0137] [Example 5] A laminate 5 was obtained by following the same procedure as in Example 1, except that film-coated substrate Y2 was used instead of film-coated substrate Y1, and release substrate 3 was used instead of release substrate 1.

[0138] [Example 6] A laminate 6 was obtained by following the same procedure as in Example 1, except that film-coated substrate Y2 was used instead of film-coated substrate Y1, release substrate 3 was used instead of release substrate 1, and woven fabric A2 was used instead of woven fabric A1.

[0139] [Example 7] A laminate 7 was obtained by following the same procedure as in Example 1, except that film-coated substrate Y3 was used instead of film-coated substrate Y1, and release substrate 3 was used instead of release substrate 1.

[0140] [Example 8] A laminate 8 was obtained by following the same procedure as in Example 1, except that film-coated substrate Y4 was used instead of film-coated substrate Y1, release substrate 3 was used instead of release substrate 1, and woven fabric A2 was used instead of woven fabric A1.

[0141] [Example 9] A laminate 9 was obtained by following the same procedure as in Example 1, except that film-coated substrate Y5 was used instead of film-coated substrate Y1, release substrate 3 was used instead of release substrate 1, and woven fabric A2 was used instead of woven fabric A1. [Example 10] A laminate 10 was obtained by following the same procedure as in Example 1, except that film-coated substrate Y2 was used instead of film-coated substrate Y1, release substrate 4 was used instead of release substrate 1, and the temperature of the metal rolls of the hot roll press was set to 130°C and the temperature of the rubber rolls to 90°C.

[0142] [Example 11] A solid polymer electrolyte membrane 10 was manufactured using a film obtained by peeling the substrate Y6 with a film attached as a precursor membrane. A laminate 10 was obtained by following the same procedure as in Example 1, except that the solid polymer electrolyte membrane 10 was used instead of the solid polymer electrolyte membrane 1, and the peelable substrate 3 was used instead of the peelable substrate 1. The solid polymer electrolyte membrane 10 in the laminate 10 did not contain any woven fabric.

[0143] The "Total Film Thickness (μm)" column in Table 1 represents the total film thickness of the film used in each example. For example, in Example 1, since two film-coated substrates Y1 are used, the total thickness of 60 μm, which is the sum of two 30 μm films, is shown in Table 1. In Table 1, the "Presence / Absence" column under "Woven Fabric" indicates whether the solid polymer electrolyte membrane contains woven fabric. "Presence" means it contains woven fabric, and "Absence" means it does not. In Table 1, the "Type" column in the "Releasable Substrate" column indicates the type of release substrate used in each example, with "1" to "4" representing release substrates 1 to 4, respectively. In Example 11, the evaluation of unwinding performance was "×", so the evaluation of adhesion was not performed, and therefore it is indicated as "-".

[0144] [Table 1]

[0145] As shown in Table 1, the laminate of the present invention was confirmed to exhibit the desired effect.

[0146] Furthermore, the entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2022-115790, filed on July 20, 2022, are incorporated herein by reference as disclosure of the specification of the present invention. [Explanation of Symbols]

[0147] 10 Laminate 12. Peelable substrate 14 Solid polymer electrolyte membrane 16 Support 18 Release layer 19. Layer for improving unwinding performance 20 Electrolytes 22 Woven fabric 22a, 22b, 22c Thread B 22A, 22B, 22C Thread A

Claims

1. A releaseable substrate including a support and a release layer, The release layer in the releaseable substrate contains a solid polymer electrolyte membrane, The solid polymer electrolyte membrane is a laminate comprising a fluorine-containing polymer having ion exchange groups and a woven fabric.

2. The laminate according to claim 1, wherein the ion exchange capacity of the fluorine-containing polymer is 0.90 to 2.00 milliequivalents / gram dry resin.

3. The woven fabric is composed of yarn A extending in one direction and yarn B extending in a direction substantially perpendicular to yarn A. The laminate according to claim 1 or 2, wherein the opening ratio of the woven fabric is 50% or more.

4. The laminate according to claim 3, wherein the denier count of yarn A and the denier count of yarn B are independently 15 to 50.

5. The laminate according to claim 3, wherein each of the yarns A and B is independently composed of at least one material selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, polyether ether ketone, and polyphenylene sulfide.

6. The laminate according to claim 3, wherein the density of yarn A and yarn B is independently 70 to 150 threads / inch.

7. The laminate according to claim 1 or 2, wherein the ion exchange group is a sulfonic acid type functional group.

8. The laminate according to claim 1 or 2, wherein the fluorine-containing polymer comprises units based on fluorine-containing olefins and units having sulfonic acid-type functional groups and fluorine atoms.

9. The laminate according to claim 8, wherein the fluorine-containing olefin is a fluoroolefin having 2 to 3 carbon atoms and having one or more fluorine atoms in the molecule.

10. The laminate according to claim 8, wherein the unit having the sulfonic acid type functional group and the fluorine atom is a unit represented by formula (1). Formula (1) -[CF 2 -CF(-L-(SO 3 M) n )]- L is an n+1 valent perfluorohydrocarbon group which may contain an etheric oxygen atom, M is a hydrogen atom, an alkali metal, or a quaternary ammonium cation, and n is 1 or 2.

11. The laminate according to claim 1 or 2, wherein the elastic modulus of the support at 160°C is greater than the elastic modulus of the release layer at 160°C.

12. The laminate according to claim 1 or 2, wherein the elastic modulus of the release layer at 160°C is 1 MPa or less.

13. The woven fabric is composed of yarn A extending in one direction and yarn B extending in a direction substantially perpendicular to yarn A. The maximum film thickness TA and minimum film thickness TB of the solid polymer electrolyte membrane are measured for each of 10 different cross-sections obtained when the solid polymer electrolyte membrane is cut in a direction parallel to the direction in which the thread A extends within the solid polymer electrolyte membrane, and at the midpoint between the threads A. Furthermore, the maximum film thickness TA and minimum film thickness TB of the solid polymer electrolyte membrane are measured for each of 10 different cross-sections obtained when the solid polymer electrolyte membrane is cut in a direction parallel to the direction in which the thread B extends within the solid polymer electrolyte membrane, and at the midpoint between the threads B. The average minimum film thickness TB obtained by arithmetic mean of the 20 TBs obtained. AVE Then, the average maximum film thickness TA obtained by arithmetic meaning the 20 TAs is AVE In this case, the average maximum film thickness TA AVE and the above average minimum film thickness TB AVE The laminate according to claim 1 or 2, wherein the relationship between and satisfies the following equation (X). Formula (X) 0.5 μm ≤ (TA AVE −TB AVE ) / 2

14. A roll body formed by winding the laminate according to claim 1 or 2.

Citation Information

Patent Citations

  • Composite polymer electrolyte membrane, manufacturing method of the same, and manufacturing method of membrane electrode assembly

    JP2011222499A

  • Composite polymer electrolyte film

    JP2019114504A

  • Device for manufacturing fuel battery cell joined body

    JP2020107430A

  • Method for manufacturing fuel cell

    JP2021152991A

  • Fuel cell electrolyte membrane, method for manufacturing same, membrane electrode-bonded body, and fuel cell

    WO2015059848A1