Piezoelectric thin film device and method for manufacturing the same

The piezoelectric thin-film device with a recess and impurity layer addresses warping issues by allowing individual adjustment of formation conditions, enhancing yield and performance by reducing stress differences and achieving a flat film shape.

JP7948423B2Active Publication Date: 2026-11-11DENSO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2025512410
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-04-03
Filing Date
2023-12-28
Publication Date
2026-11-11
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

Piezoelectric thin film devices often suffer from warping due to stress differences in their multilayer film structures, leading to reduced yield and productivity, particularly in devices like piezoelectric MEMS microphones, where warping can cause pressure escape and narrow the detection bandwidth.

Method used

A piezoelectric thin-film device design that includes a substrate with a recess forming a thin film portion and an impurity layer containing a second element different from the first element, allowing for individual adjustment of formation conditions to correct warpage, reducing stress differences and improving yield.

Benefits of technology

The formation of an impurity layer in the piezoelectric film reduces stress differences, enabling precise correction of warpage across multiple devices, enhancing yield and ensuring a flat film shape, thus improving the performance and reliability of piezoelectric devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948423000001
    Figure 0007948423000001
  • Figure 0007948423000002
    Figure 0007948423000002
  • Figure 0007948423000003
    Figure 0007948423000003
Patent Text Reader

Abstract

The present invention is provided with a substrate (10), a lower electrode (13) laminated on the substrate, a piezoelectric film (14) that is formed from a piezoelectric body and is laminated on the lower electrode, and an upper electrode (15) laminated on the piezoelectric film, wherein: with a recess (16) formed on a surface of the substrate opposite to the lower electrode, a thin film part (17) composed of the lower electrode, the piezoelectric film, and the upper electrode is formed; and when the element forming the piezoelectric body is regarded as a first element, an impurity layer (14a) containing a second element different from the first element is formed on the surface layer part of the piezoelectric film.
Need to check novelty before this filing date? Find Prior Art

Description

Cross-Reference to Related Applications

[0001] This application is based on Japanese Patent Application No. 2023-060324 filed on April 3, 2023, the entire content of which is incorporated herein by reference. TECHNICAL FIELD

[0002] The present disclosure relates to a piezoelectric thin film device and a method for manufacturing the same. BACKGROUND ART

[0003] Some piezoelectric thin film devices have a multilayer film structure in shapes such as a cantilever beam, a doubly supported beam, and a diaphragm. Examples include piezoelectric MEMS (Micro Electro Mechanical Systems) mirrors, BAW (Bulk Acoustic Wave) devices, and piezoelectric MEMS microphones. A piezoelectric MEMS microphone is composed of a piezoelectric element having a laminated structure of electrodes and a piezoelectric film (see, for example, Patent Document 1). In the manufacturing process of the piezoelectric element, a lower electrode, a piezoelectric film, and an upper electrode are laminated on the upper surface of a wafer-shaped substrate. A recess is formed on the lower surface of the substrate, and slits are formed in the laminated structure of the electrodes and the piezoelectric film, whereby the laminated structure is cantilever-supported at the opening end of the substrate to serve as a vibration region. PRIOR ART DOCUMENTS PATENT DOCUMENTS

[0004] PATENT DOCUMENT 1 Japanese Unexamined Patent Application Publication No. 2022-7879 SUMMARY OF THE INVENTION

[0005] In such devices, it is ideal for the multilayer film to be formed in a flat shape. However, in reality, warping can occur due to stress differences in the films that make up the multilayer film, potentially causing the device to fail to meet specifications. For example, in the microphone described above, the vibration region vibrates when pressure such as sound pressure is applied, and the charge generated in the piezoelectric film is output as a detection signal. However, if warping occurs in the vibration region, the slit may widen, causing pressure to escape and potentially narrowing the detection bandwidth.

[0006] To reduce warpage and suppress yield and productivity declines, one approach is to control film stress through deposition conditions. However, the deposition conditions required for flat multilayer films differ from region to region on the wafer surface. Therefore, if deposition conditions are set to flatten the multilayer film of a MEMS device formed in a portion of the wafer, warpage will increase in other regions. Consequently, it is difficult to reduce warpage across the entire wafer and improve yield using deposition conditions alone. This disclosure aims to provide piezoelectric thin-film devices and methods for manufacturing the same that can improve yield.

[0007] One aspect of this disclosure is a piezoelectric thin-film device comprising a substrate, a lower electrode laminated on the substrate, a piezoelectric film laminated on the lower electrode and composed of a piezoelectric material, and an upper electrode laminated on the piezoelectric film, wherein a recess formed on the side of the substrate opposite to the lower electrode forms a thin film portion comprising the lower electrode, the piezoelectric film, and the upper electrode, and the elements constituting the piezoelectric material are designated as a first element, and an impurity layer is formed in the piezoelectric film containing a second element different from the first element in addition to the first element. The substrate is composed of a first substrate (11) and a second substrate (12) laminated on the upper surface of the first substrate. The recess penetrates the first substrate, and a recess (20) is formed on the outside of the thin film portion, penetrating the piezoelectric film and the upper electrode to expose the upper surface of the lower electrode. The region of the second substrate and the lower electrode located below the exposed recess is called the outer region (21). The outer region has higher strength than the thin film portion, and the second element contained in the impurity layer is also distributed in the outer region. Yes, they are.

[0008] According to this method, the formation of an impurity layer reduces the stress difference between the films constituting the thin film, thereby correcting the warpage of the thin film. The formation conditions for the impurity layer are easier to set individually for multiple piezoelectric thin film devices on a substrate compared to the formation conditions for multilayer films. By appropriately setting the formation conditions for the impurity layer, the amount of correction for the warpage of the thin film can be made to correspond to the amount of warpage. Therefore, the warpage of multiple piezoelectric thin film devices formed on a substrate can be corrected individually to reduce variations in the amount of warpage and improve yield.

[0009] Another aspect of this disclosure is a method for manufacturing a piezoelectric thin film device, comprising: forming a lower electrode on the upper surface of a substrate; forming a piezoelectric film composed of a piezoelectric material on the upper surface of the lower electrode; forming an upper electrode on the upper surface of the piezoelectric film; forming a recess on the surface of the substrate opposite to the lower electrode, thereby forming a thin film portion comprising the lower electrode, the piezoelectric film, and the upper electrode; and forming an impurity layer in the piezoelectric film, in addition to the first element, which is a second element different from the first element, with the elements constituting the piezoelectric material being the first element. Furthermore, when forming an impurity layer, the second element is selected according to the magnitude of warping that occurs in the thin film portion. .

[0010] According to this method, the formation of an impurity layer reduces the stress difference between the films constituting the thin film, thereby correcting the warpage of the thin film. The formation conditions for the impurity layer are easier to set individually for multiple piezoelectric thin film devices on a substrate compared to the formation conditions for multilayer films. By appropriately setting the formation conditions for the impurity layer, the amount of correction for the warpage of the thin film can be made to correspond to the amount of warpage. Therefore, the warpage of multiple piezoelectric thin film devices formed on a substrate can be corrected individually to reduce variations in the amount of warpage and improve yield.

[0011] The reference numerals in parentheses attached to each component indicate an example of the correspondence between that component and the specific components described in the embodiments described later. [Brief explanation of the drawing]

[0012] [Figure 1]FIG. 1 is a cross-sectional view of the piezoelectric thin film device according to the first embodiment. [Figure 2] FIG. 2 is an enlarged view of part II in FIG. 1. [Figure 3A] FIGS. 3A to 3C are cross-sectional views showing the manufacturing process of the piezoelectric thin film device. [Figure 3B] FIG. 3B is a cross-sectional view showing the manufacturing process of the piezoelectric thin film device subsequent to FIG. 3A. [Figure 3C] FIG. 3C is a cross-sectional view showing the manufacturing process of the piezoelectric thin film device subsequent to FIG. 3B. [Figure 4] FIG. 4 is a diagram showing an example of the amount of warpage in each region of the wafer. [Figure 5A] FIG. 5A is a cross-sectional view showing the manufacturing process of the piezoelectric thin film device subsequent to FIG. 3B. [Figure 5B] FIG. 5B is a cross-sectional view showing the manufacturing process of the piezoelectric thin film device subsequent to FIG. 5A. [Figure 5C] FIG. 5C is a cross-sectional view showing the manufacturing process of the piezoelectric thin film device subsequent to FIG. 5B. [Figure 5D] FIG. 5D is a cross-sectional view showing the manufacturing process of the piezoelectric thin film device subsequent to FIG. 5C. [Figure 6] FIG. 6 is a diagram showing a state of scanning with an ion beam. [Figure 7A] FIG. 7A is a diagram showing the resist thickness and ion implantation depth in a region with a small amount of warpage. [Figure 7B] FIG. 7B is a diagram showing the resist thickness and ion implantation depth in a region with a moderate amount of warpage. [Figure 7C] FIG. 7C is a diagram showing the resist thickness and ion implantation depth in a region with a large amount of warpage. [Figure 8A] FIG. 8A is a diagram showing the distribution of the second element when the acceleration voltage is 20 keV. [Figure 8B] FIG. 8B is a diagram showing the distribution of the second element when the acceleration voltage is 60 keV. [Figure 8C] FIG. 8C is a diagram showing the distribution of the second element when the acceleration voltage is 100 keV. [Figure 9] FIG. 9 is a diagram showing the relationship between acceleration voltage and displacement amount. [Figure 10] FIG. 10 is a cross-sectional view of the piezoelectric thin film device according to the second embodiment. [Figure 11] This is an enlarged view of part XI in Figure 10. [Figure 12A] This is a cross-sectional view showing the subsequent manufacturing process of the piezoelectric thin film device following Figure 5A. [Figure 12B] This is a cross-sectional view showing the subsequent manufacturing process of the piezoelectric thin film device following Figure 12A. [Figure 12C] This is a cross-sectional view showing the subsequent manufacturing process of the piezoelectric thin film device following Figure 12B. [Figure 12D] This is a cross-sectional view showing the subsequent manufacturing process of the piezoelectric thin film device following Figure 12C. [Figure 13A] This is a top view of the piezoelectric thin film device according to the third embodiment. [Figure 13B] This is a cross-sectional view taken along line XIIIB-XIIIB in Figure 13A. [Figure 14] This is a perspective view of the piezoelectric thin film device drawn with the section taken along line XIV-XIV in Figure 13. [Figure 15] This is a cross-sectional view showing a state where warpage occurs in the thin film portion during the manufacturing process. [Figure 16] This is a perspective view depicting a state where warpage occurs in the thin film portion during the manufacturing process, with the section taken at the position corresponding to line XIV-XIV in Figure 13. [Figure 17] This is a cross-sectional view of the piezoelectric thin film device according to the fourth embodiment. [Figure 18] This is a perspective view of the piezoelectric thin film device shown in Figure 17. [Figure 19] This is a cross-sectional view showing a state where warpage occurs in the thin film portion during the manufacturing process. [Figure 20] This is a cross-sectional view of a piezoelectric thin film device according to another embodiment. [Description of Embodiments]

[0013] Hereinafter, embodiments of the present disclosure will be described based on the drawings. Note that in the following respective embodiments, parts that are identical or equivalent to each other will be described with the same reference numerals assigned thereto.

[0014] (First Embodiment) A first embodiment will be described. The piezoelectric thin-film device of this embodiment shown in Figure 1 comprises a semiconductor substrate 10. The semiconductor substrate 10 is configured such that a second substrate 12 is laminated on the upper surface of a first substrate 11. The first substrate 11 and the second substrate 12 are made of, for example, silicon (Si). The first substrate 11 and the second substrate 12 may be directly joined, or they may be joined via an embedded oxide film or the like. For example, when the first substrate 11 and the second substrate 12 are constructed using an SOI (Silicon on Insulator) substrate, the first substrate 11 and the second substrate 12 are joined via an embedded oxide film.

[0015] The piezoelectric thin-film device also includes a lower electrode 13 laminated on the upper surface of the second substrate 12, a piezoelectric film 14 laminated on the upper surface of the lower electrode 13, and an upper electrode 15 laminated on the upper surface of the piezoelectric film 14. The lower electrode 13 and the upper electrode 15 are made of a conductive metal such as molybdenum (Mo). The piezoelectric film 14 is made of a piezoelectric material. For example, the piezoelectric film 14 is made using lead-free piezoelectric ceramics such as barium titanate (BaTiO3), scandium aluminum nitride (ScAlN), aluminum nitride (AlN), or lead zirconate titanate (PZT). The elements constituting the piezoelectric material of the piezoelectric film 14 are referred to as the first elements. For example, if the piezoelectric film 14 is made of AlN, the first elements are aluminum (Al) and nitrogen (N).

[0016] A recess 16 is formed on the semiconductor substrate 10 on the side opposite to the lower electrode 13. The recess 16 is formed by removing a portion of the first substrate 11 to expose the lower surface of the second substrate 12 on the side of the first substrate 11, and opens, for example, in a rectangular shape on the lower surface of the semiconductor substrate 10. By removing the first substrate 11 with the recess 16, a portion of the piezoelectric thin film device is thinned. This thinned portion is referred to as the thin film portion 17. The thin film portion 17 only needs to include at least the lower electrode 13, the piezoelectric film 14, and the upper electrode 15, and in this example, it also includes the second substrate 12, but it may also be configured with other films, such as a protective film formed on the surface.

[0017] The laminate comprising the second substrate 12 including the thin film portion 17, the lower electrode 13, the piezoelectric film 14, and the upper electrode 15 is cantilevered to the first substrate 11 at the open end of the recess 16, and the thin film portion 17 is exposed with its side surface 18 separated from the other parts.

[0018] An impurity layer 14a is formed on the surface layer of the piezoelectric film 14, near the upper electrode 15. The surface layer of the piezoelectric film 14 referred to here is not a separate part of the piezoelectric film 14, but rather the upper side of the piezoelectric film 14, i.e., the part on the upper electrode 15 side, or the lower side of the piezoelectric film 14, i.e., the part on the lower electrode 13 side. In this embodiment, the impurity layer 14a is formed on the upper side of the piezoelectric film 14 as the surface layer of the piezoelectric film 14. Here, the impurity layer 14a is formed on the surface layer of the piezoelectric film 14, but the impurity layer 14a may be formed at any depth of the piezoelectric film 14 as long as it is contained within the piezoelectric film 14. However, since forming it at a deep position may degrade the piezoelectric function of the piezoelectric film 14, it is preferable that it be formed at a position shallower than half the thickness of the piezoelectric film 14 from the surface of the piezoelectric film 14. Furthermore, it is preferable that the impurity layer 14a is formed at a shallow position in contact with the surface of the piezoelectric film 14 so as to minimize degradation of the piezoelectric function, but it may also be formed at a position away from the surface of the piezoelectric film 14. The impurity layer 14a is composed of a first element, which is a constituent element of the piezoelectric film 14, as well as a second element different from the first element. The second element is an element that has little effect on the piezoelectric properties of the piezoelectric film 14, and is, for example, phosphorus (P), a group 15 element, boron (B), a group 13 element, magnesium (Mg), a group 2 element, and other elements of the same group are also included. The impurity layer 14a contains more vacancies or amorphous layers than the parts of the piezoelectric film 14 that do not contain the impurity layer 14a.

[0019] On the outer side of the thin film portion 17, a recess 20 is formed that penetrates the piezoelectric film 14 and the upper electrode 15, exposing the upper surface of the lower electrode 13. The region of the second substrate 12 and the lower electrode 13 located below the recess 20 is defined as the outer region 21. The second element contained in the impurity layer 14a is also distributed in the outer region 21.

[0020] Of the surfaces of the thin film portion 17, the side on the same side as the upper electrode 15 relative to the piezoelectric film 14 is designated as one surface 22, and the side on the same side as the lower electrode 13 relative to the piezoelectric film 14 is designated as the other surface 23. In this embodiment, the upper surface of the upper electrode 15 opposite to the piezoelectric film 14 is one surface 22, and the lower surface of the second substrate 12 opposite to the lower electrode 13 is the other surface 23. If a protective film or the like is formed on the upper surface of the upper electrode 15, the upper surface of this protective film or the like becomes one surface 22.

[0021] Of the two surfaces, one surface 22 and the other 23, the surface closer to the impurity layer 14a has a rougher surface than the other surface. In this embodiment, the impurity layer 14a is formed on the surface of the piezoelectric film 14, close to the upper electrode 15. As shown in Figure 2, the other surface 23 is flat, while the one surface 22 has irregularities. That is, the one surface 22 has a rougher surface than the other surface 23.

[0022] Such a piezoelectric thin-film device can be used, for example, as a microphone. That is, when pressure such as sound pressure is applied to the thin-film portion 17, the thin-film portion 17 vibrates, and a voltage is generated between the lower electrode 13 and the upper electrode 15 due to the deformation of the piezoelectric film 14. By measuring this voltage, pressure such as sound pressure can be detected. Although not shown in the figures, the portion of the lower electrode 13 that is exposed in the outer region 21 and the upper electrode 15 can be electrically connected to the outside via bonding wires or the like. The upper electrode 15 may also be extended from the end face of the piezoelectric film 14 to the surface of the second substrate 12 at a different position from where the lower electrode 13 is extended, so that the portion on the surface of the second substrate 12 is electrically connected to the outside. Even in that case, it is sufficient that the upper electrode 15 is electrically isolated from the lower electrode 13. With these configurations, when a voltage is generated between the lower electrode 13 and the upper electrode 15, it is transmitted to an external measuring device, and pressure such as sound pressure can be detected.

[0023] The method for manufacturing the piezoelectric thin film device of this embodiment will now be described. In this embodiment, first, a piezoelectric thin film device for measuring the amount of warpage, which will be described later, is manufactured. Then, the piezoelectric thin film device that will become the product is manufactured using the measurement results of the amount of warpage. The piezoelectric thin film device for measuring the amount of warpage is manufactured by performing the steps shown in Figures 3A to 3C using a semiconductor manufacturing apparatus.

[0024] In the process shown in Figure 3A, a wafer-shaped semiconductor substrate 10 is prepared, consisting of a first substrate 11 and a second substrate 12 bonded together. Alternatively, the second substrate 12 may be formed by laminating it onto the surface of the first substrate 11 after it has been prepared. Multiple piezoelectric thin-film devices are formed on the semiconductor substrate 10, and Figures 3A to 3C illustrate regions corresponding to one of these piezoelectric thin-film devices.

[0025] In the process shown in Figure 3B, the lower electrode 13, piezoelectric film 14, and upper electrode 15 are sequentially laminated on the upper surface of the second substrate 12. Specifically, the lower electrode 13 is formed on the upper surface of the second substrate 12, the piezoelectric film 14 is formed on the upper surface of the lower electrode 13, and the upper electrode 15 is formed on the upper surface of the piezoelectric film 14. The lower electrode 13, piezoelectric film 14, and upper electrode 15 are deposited by general sputtering or CVD (Chemical Vapor Deposition) methods.

[0026] In the process shown in Figure 3C, a thin film portion 17 is formed. Specifically, the second substrate 12, lower electrode 13, piezoelectric film 14, and a portion of the upper electrode 15 are removed by etching using a mask (not shown) to form a side surface 18. In addition, outside the region that will become the thin film portion 17, the piezoelectric film 14 and upper electrode 15 are removed to form a recess 20. Subsequently, a resist (not shown) is formed on the upper surface of the lower electrode 13 exposed from the recess 20, the upper surface of the upper electrode 15, and the portion of the lower surface of the first substrate 11 where the recess 16 is not to be formed. Then, using this resist as a protective film, a portion of the first substrate 11 is removed by etching to form the recess 16. This forms a thin film portion 17 that is cantilevered to the first substrate 11. After the thin film portion 17 is formed, the resist (not shown) is peeled off.

[0027] When the recess 16 is formed, warping occurs in the thin film portion 17 due to the stress difference in the film constituting the thin film portion 17. Of the surfaces of the thin film portion 17, the surface that is convex toward the outside is defined as the convex surface 24, and the concave surface on the opposite side of the convex surface 24 is defined as the concave surface 25. In this embodiment, we will describe the case where the other surface 23, which is the lower surface of the thin film portion 17, is the convex surface 24, and the upper surface 22 is the concave surface 25, that is, the case in which the free end side of the thin film portion 17 is displaced upward due to the deformation of the thin film portion 17.

[0028] In the process shown in Figure 3C, multiple thin film portions 17 are formed on the wafer-shaped semiconductor substrate 10 so that multiple piezoelectric thin film devices are formed on it.

[0029] After the process shown in Figure 3C, the amount of warpage of the thin film portion 17 is measured. The amount of warpage of the thin film portion 17 is measured, for example, by measuring the height of the leading edge of the other surface 23 from the top surface of the first substrate 11, as shown in Figure 3C. The measurement results are as shown in Figure 4, for example. Figure 4 shows the results of measuring the amount of warpage for one thin film portion 17 selected from each of the multiple rectangular regions of the semiconductor substrate 10, with the unit of warpage being μm. Figure 4 shows the measurement results of the amount of warpage in an experiment conducted by the inventors, and regions without numerical values ​​are regions where the amount of warpage was not measured during the experiment.

[0030] After measuring the amount of warpage in this manner, the piezoelectric thin-film device that will become the final product is manufactured. The piezoelectric thin-film device that will become the final product is manufactured by following the steps shown in Figures 3A and 3B, similar to the piezoelectric thin-film device used for measuring the amount of warpage, followed by the steps shown in Figures 5A to 5D. In the manufacturing of the piezoelectric thin-film device that will become the final product, the film deposition conditions in the step shown in Figure 3B are set in the same way as when manufacturing the piezoelectric thin-film device used for measuring the amount of warpage.

[0031] In the process shown in Figure 5A, the side surface 18 and recess 20 are formed. Specifically, the side surface 18 is formed by etching using a mask (not shown) to remove part of the second substrate 12, lower electrode 13, piezoelectric film 14, and upper electrode 15. In addition, the recess 20 is formed by removing the piezoelectric film 14 and upper electrode 15 outside the area that will become the thin film portion 17.

[0032] Because the film deposition conditions in the process shown in Figure 3B are set as described above, a stress difference similar to that of a piezoelectric thin-film device for measuring warpage occurs in the region from the second substrate 12 to the upper electrode 15 that will become the thin-film portion 17. That is, if the recess 16 is formed immediately after the process shown in Figure 5A, the thin-film portion 17 deforms so that one surface 22 becomes a concave surface 25 and the other surface 23 becomes a convex surface 24. In this case, the amount of warpage of the thin-film portion 17 in each piezoelectric thin-film device on the semiconductor substrate 10 follows the same trend as the distribution shown in Figure 4.

[0033] In the process shown in Figure 5B, a silicon oxide film is formed on the upper surface of the lower electrode 13 exposed from the recess 20 and on the upper surface of the upper electrode 15. This silicon oxide film serves as the through-film 26 for ion implantation, which is performed in the process shown in Figure 5C. A resist 27 is then applied on top of the through-film 26. Alternatively, the resist 27 may be applied to the upper surfaces of the lower electrode 13 and the upper electrode 15 without forming the through-film 26.

[0034] In the process shown in Figure 5C, a second element different from the first element is added to the surface layer of the piezoelectric film 14 near the concave surface 22, which was created in the process shown in Figure 3C, to form an impurity layer 14a. Specifically, the ionized second element is accelerated by voltage in a vacuum and injected into the piezoelectric film 14 from the surface 22 side. The injection of the second element is performed by scanning the ion beam emitted from the ion implanter 100 in the X and Y directions as indicated by arrow A1, as shown in Figure 6, and irradiating each piezoelectric thin film device on the semiconductor substrate 10. The X direction is parallel to the upper surface of the semiconductor substrate 10, and the Y direction is parallel to the upper surface of the semiconductor substrate 10 and perpendicular to the X direction.

[0035] In the process shown in Figure 5D, a portion of the first substrate 11 is removed by etching using the resist 27 as a protective film to form a recess 16. At this time, the resist 27 is formed not only in the portion formed in the process shown in Figure 5B, but also in the portion of the lower surface of the first substrate 11 where the recess 16 is not to be formed. The thickness of the portion of the resist 27 formed on the lower surface of the first substrate 11 can be set independently of the process shown in Figure 5C, as long as it is thick enough to withstand etching of the recess 16. As a result, during etching, the first substrate 11 is removed in the portion where the resist 27 opens, forming the recess 16. This forms a thin film portion 17 that is cantilevered to the first substrate 11. After forming the thin film portion 17, the through-film 26 and the resist 27 are peeled off, and the wafer-shaped semiconductor substrate 10 is divided into chip units to form the piezoelectric thin film device shown in Figure 1. The width of each chip is, for example, several millimeters to several tens of millimeters.

[0036] When ion implantation is performed in this manner, the bonds within the crystal lattice of the piezoelectric film 14 are broken, and compressive stress is applied to the portion of the thin film 17 on the side of surface 22. As a result, the stress difference in the film constituting the thin film 17 is reduced, and the thin film 17 approaches an ideal shape, i.e., a flat shape, as shown in Figure 1. Because the polycrystalline structure of the piezoelectric film 14 is destroyed by ion implantation, vacancies and amorphous layers are formed, so the impurity layer 14a has more vacancies and / or amorphous layers than other parts of the piezoelectric film 14. In addition, because the concave surface 25 is damaged by ion implantation and irregularities are formed, the surface roughness of surface 22 is greater than that of surface 23.

[0037] The thickness of the resist 27 is adjusted according to the amount of warpage of the thin film portion 17 measured after the process shown in Figure 3C. Specifically, the thickness of the resist 27 on the entire wafer is adjusted such that the less the warpage of the thin film portion 17, the thicker the resist 27 becomes, and the greater the warpage, the thinner the resist 27 becomes. As a result, the amount of ions injected into the thin film portion 17 increases in areas with greater warpage, and the amount of warpage correction increases. The thickness of the resist 27 is controlled by the exposure amount of the exposure apparatus. For example, a stepper is used as the exposure apparatus.

[0038] For example, in the region R1 with a small amount of warpage in Figure 4, the resist 27 is exposed to less light and remains thick, as shown in Figure 7A. As a result, as indicated by the white arrows, the implanted ions are absorbed by the resist 27 and have difficulty reaching the through-film 26 and the thin film portion 17.

[0039] Furthermore, in region R2, where the amount of warpage is greater than in region R1 in Figure 4, the resist 27 is exposed to a larger amount of light and is thinner than the resist 27 in region R1, as shown in Figure 7B. The dashed line in Figure 7B indicates the thickness of the resist 27 in region R1. As a result, as indicated by the white arrows, the implanted ions pass through the resist 27 and the through-film 26 and reach the thin film portion 17.

[0040] Furthermore, in region R3, where the amount of warping is greater than in region R2 in Figure 4, the exposure of the resist 27 is further increased, and as shown in Figure 7C, the resist 27 is removed and the upper surface of the through-film 26 is exposed. The dashed line in Figure 7C shows the thickness of the resist 27 in region R2. As a result, as indicated by the white arrows, the implanted ions can reach the thin film portion 17 more easily. Also, the implanted ions can reach deeper parts of the thin film portion 17.

[0041] In this way, by making the resist 27 sufficiently thick in areas with small warpage, ion implantation into the thin film portion 17 is suppressed, and ion implantation can be performed only in areas where correction of anticipated warpage is necessary. Alternatively, warpage correction by ion implantation may be performed only in areas where the amount of warpage exceeds a standard value. Furthermore, the thickness of the resist 27 may be adjusted using a pattern such as a gray tone mask. For example, when exposing the resist 27 with an exposure apparatus, the exposure amount can be adjusted for each shot to correspond to the desired thickness of the resist 27. Specifically, in shots where correction is necessary, the resist 27 is made thinner and the exposure amount is increased so that ions reach the thin film portion 17, while in shots where correction is not necessary, the resist 27 is made thicker and the exposure amount is decreased so that ion implantation does not reach the thin film portion 17. When using a pattern such as a gray tone mask, a gray tone mask corresponding to the desired thickness of the resist 27 can be selected to create a gradient in the exposure amount.

[0042] The amount of warpage correction varies depending not only on the thickness of the resist 27, but also on the ion implantation acceleration voltage and the type of second element.

[0043] Specifically, the greater the accelerating voltage, the greater the correction amount for warping. Figures 8A to 8C show the relationship between the depth from one surface 22 and the concentration of the second element when phosphorus is used as the second element. Figures 8A to 8C are graphs for accelerating voltages of 20 keV, 60 keV, and 100 keV, respectively. The dose of phosphorus is 1 × 10⁻⁶ 13 / cm 2 It is said that...

[0044] Figures 8A to 8C show that the greater the accelerating voltage, the deeper the second element is injected. Specifically, when the accelerating voltage is 20 keV, the phosphorus concentration in the piezoelectric film 14 is almost 0, as shown in Figure 8A. However, when the accelerating voltage is 60 keV, phosphorus is diffused into the surface layer of the piezoelectric film 14, as shown in Figure 8B. Furthermore, when the accelerating voltage is 100 keV, phosphorus is diffused to an even deeper location, specifically to a depth of 200 nm from the surface of the upper electrode 15, as shown in Figure 8C.

[0045] Note that in all of Figures 8A to 8C, a drop in concentration is observed in the surface layer of the upper electrode 15, but this data is considered to be noise. In other words, the positions of the concentration peaks in Figures 8A to 8C are thought to be as shown by the dashed lines L1, L2, and L3, respectively. Specifically, when the acceleration voltage is 20 keV, the concentration peak is located in the middle layer of the upper electrode 15. When the acceleration voltage is 60 keV, the concentration peak is located deeper than the middle layer of the upper electrode 15. When the acceleration voltage is 100 keV, the concentration peak is located near the interface between the upper electrode 15 and the piezoelectric film 14.

[0046] Figure 9 is a graph showing the relationship between the accelerating voltage and the displacement of the thin film portion 17 due to ion implantation, i.e., the warpage correction amount. Figure 9 shows the measurement results of the displacement when phosphorus is selected as the second element and when boron is selected. In Figure 9, the dose amounts for both phosphorus and boron are 1 × 10⁻⁶. 13 / cm 2 It is said that...

[0047] When phosphorus is used, as shown in Figures 8A to 8C and Figure 9, the higher the accelerating voltage, the deeper the concentration peak position of the second element becomes, and the larger the correction amount for warping. Figures 8A to 8C correspond to plots P1 to P3 in Figure 9. In plot P4, where the accelerating voltage is 260 keV, the concentration peak position is even deeper than in the distribution in Figure 8C, and the concentration peak position is in the deeper part of the piezoelectric film 14.

[0048] Similarly, when using boron, the higher the acceleration voltage, the deeper the concentration peak position of the second element becomes, and the greater the amount of warping correction. When using boron, the concentration peak reaches the piezoelectric film 14 at an acceleration voltage of 60 keV, and the concentration peak reaches the deeper part of the piezoelectric film 14 at an acceleration voltage of 140 keV.

[0049] Therefore, in areas with significant warping, increasing the acceleration voltage increases the amount of warping correction, causing the thin film portion 17 to approach a flatter shape.

[0050] As shown in Figure 9, when the acceleration voltage becomes sufficiently large, the correction amount changes proportionally to the acceleration voltage, making it easier to control the correction amount. Furthermore, as the acceleration voltage increases even further, the change in the correction amount in response to the change in acceleration voltage becomes smaller. According to the inventors' studies, at the acceleration voltage where the concentration peak reaches the piezoelectric film 14, the change in the correction amount becomes small. In this region where the change in the correction amount is small, controlling the correction amount becomes even easier.

[0051] Furthermore, as shown in Figure 9, when phosphorus is used, the correction amount is larger when the acceleration voltage is 100 keV or higher compared to when boron is used. Therefore, when the warpage of the thin film portion 17 is large, using an element that produces a large correction amount, such as phosphorus, as the second element makes it easier to bring the thin film portion 17 closer to a flat shape. On the other hand, when the warpage of the thin film portion 17 is small, there is no need to increase the correction amount, so it is desirable to use an element that produces a small change in the correction amount in response to changes in acceleration voltage, such as boron, as the second element to improve the controllability of warpage correction. As shown in Figure 9, when boron is used as the second element, the change in the correction amount becomes small above 60 keV, when the concentration peak reaches the piezoelectric film 14, and the controllability of warpage correction is improved, so it is desirable to set the acceleration voltage within this range.

[0052] Furthermore, according to the inventors' studies, by setting the ion implantation conditions as follows, it is possible to efficiently correct the warpage of the thin film portion 17 while suppressing damage to the concave surface 25. That is, the dose amount is 1 × 10⁻⁶. 15 / cm2 The following conditions apply, with the acceleration voltage being between 20 keV and 200 keV. Furthermore, the second element should have minimal influence on the piezoelectric properties of the piezoelectric film 14 and should have a large atomic weight. For example, phosphorus, boron, magnesium, etc., should be used as the second element. Additionally, the ion beam spot diameter should be larger than the element dimensions of the piezoelectric thin-film device to ensure uniform ion beam irradiation across the entire element.

[0053] Furthermore, by making the spot diameter of the ion beam larger than the width of the thin film portion 17, ions are also implanted in the outer region 21. However, since the second substrate 12 and the lower electrode 13 on the first substrate 11 have higher intensity than the thin film portion 17, the thin film portion 17 is compensated to be more favorably treated than the outer region 21 by appropriately setting the ion implantation conditions.

[0054] As described above, in this embodiment, an impurity layer 14a is formed on the surface layer of the piezoelectric film 14, containing a second element different from the first element in addition to the first element that constitutes the piezoelectric film 14. This reduces the stress difference of the films constituting the thin film portion 17 and corrects the warpage of the thin film portion 17. Furthermore, by appropriately setting conditions such as the thickness of the resist 27, the acceleration voltage, and the type of the second element when forming the impurity layer 14a, the amount of correction for the warpage of the thin film portion 17 can be made to correspond to the amount of warpage. Moreover, these conditions can be easily set individually for multiple piezoelectric thin film devices formed on a wafer-shaped semiconductor substrate 10. For example, the thickness of the resist 27 on each piezoelectric thin film device can be adjusted by the exposure amount, and the acceleration voltage can be changed during ion beam scanning. Therefore, the warpage of multiple piezoelectric thin film devices can be individually corrected to reduce variations in the amount of warpage and improve yield.

[0055] Furthermore, according to the above embodiment, the following effects can be obtained.

[0056] (1) The impurity layer 14a contains more vacancies or amorphous layers than the parts of the piezoelectric film 14 that do not contain the impurity layer 14a. By destroying part of the crystal structure of the piezoelectric film 14 through ion implantation and forming vacancies and amorphous layers, the bonds within the crystal lattice of the piezoelectric film 14 are broken, and compressive stress is applied to the part of the thin film portion 17 that is on one side 22. This makes it possible to correct the warpage of the thin film portion 17.

[0057] (2) Of the two surfaces, one surface 22 and the other 23, the surface closer to the impurity layer 14a has a rougher surface than the other surface. By performing ion implantation from the side of surface 22, the impurity layer 14a is formed on the surface of the piezoelectric film 14 that is closer to surface 22, and the warping of the thin film portion 17 is corrected. At this time, surface 22 is damaged, so surface 22 has a rougher surface than the other surface 23.

[0058] (3) An impurity layer 14a is formed on the surface layer of the piezoelectric film 14 that is close to the concave surface 22 when warping occurs in the thin film portion 17. This applies compressive stress to the portion of the thin film portion 17 that is on the side of the surface 22, and the stress difference of the film constituting the thin film portion 17 is reduced, so that the thin film portion 17 approaches a flat shape.

[0059] (4) The second element is selected according to the degree of warping of the thin film portion 17. By appropriately selecting the second element, it is possible to increase the amount of correction and improve the controllability of the correction.

[0060] (5) The ionized second element is accelerated by voltage and implanted into the piezoelectric film 14. This ion implantation can correct the warping of the thin film portion 17.

[0061] (6) The thickness of the resist 27 is varied in different locations according to the degree of warping of the thin film portion 17, and the second element is introduced into the piezoelectric film 14 using the resist 27. This allows the correction amount to be adjusted according to the amount of warping of each thin film portion 17.

[0062] (7) The thickness of the resist 27 is controlled by the exposure apparatus. This allows the thickness of the resist 27 to be varied depending on the location, and the amount of correction can be adjusted according to the amount of warping of each thin film portion 17.

[0063] (Second Embodiment) A second embodiment will now be described. This embodiment is the same as the first embodiment except that the position of the impurity layer 14a has been changed. Therefore, only the parts that differ from the first embodiment will be described.

[0064] As shown in Figure 10, in this embodiment, an impurity layer 14a is formed on the other surface 23 of the piezoelectric film 14, in other words, on the surface layer close to the lower electrode 13. Furthermore, as shown in Figure 11, while one surface 22 is flat, the other surface 23 has irregularities. That is, the other surface 23 has a greater surface roughness than the one surface 22.

[0065] In this embodiment, a piezoelectric thin-film device is manufactured by performing the steps shown in Figures 3A, 3B, and 5A, followed by the steps shown in Figures 12A to 12D. In the step shown in Figure 3B, the film deposition conditions for the lower electrode 13, the piezoelectric film 14, and the upper electrode 15 are set so that the thin film portion 17 becomes convex upward due to the formation of recesses 16, etc.

[0066] In the process shown in Figure 12A, resist 27 is applied to the upper surface of the lower electrode 13 exposed from the recess 20, the upper surface of the upper electrode 15, and the portion of the lower surface of the first substrate 11 where the recess 16 is not to be formed. In the process shown in Figure 12B, a portion of the first substrate 11 is removed by etching using the resist 27 as a protective film to form the recess 16.

[0067] In the process shown in Figure 12C, the resist 27 is peeled off. Because the film formation conditions in the process shown in Figure 3B are set as described above, the peeling off of the resist 27 causes the thin film portion 17 to deform so that it becomes convex upwards. That is, the free end of the thin film portion 17 is displaced downwards, so that one surface 22, which is the upper surface of the thin film portion 17, becomes a convex surface 24, and the other surface 23, which is the lower surface, becomes a concave surface 25.

[0068] In the process shown in Figure 12D, ion implantation is performed from the lower side of the semiconductor substrate 10. As a result, as shown in Figure 10, an impurity layer 14a is formed on the surface of the piezoelectric film 14 that is close to the other surface 23, and the warpage of the thin film portion 17 is corrected. In this embodiment, the amount of warpage is measured after the process shown in Figure 12C, and the correction amount is adjusted according to the acceleration voltage and the type of second element based on the measurement result.

[0069] To reduce the surface roughness of the upper electrode 15, the deposition conditions can be adjusted so that the free end of the thin film portion 17 is displaced downward, and the warpage can be corrected by performing ion implantation from the lower side, thereby suppressing the increase in surface roughness of the upper electrode 15.

[0070] This embodiment, with the same configuration and operation as the first embodiment, can obtain the same effects as the first embodiment.

[0071] (Third embodiment) A third embodiment will now be described. This embodiment applies the present disclosure to a piezoelectric MEMS mirror having a double-supported beam structure as a piezoelectric thin-film device. The basic structure of the piezoelectric thin-film device of this embodiment is the same as that of the piezoelectric thin-film device described in the first embodiment, so the differences from the first embodiment will be mainly described. The piezoelectric thin-film device of this embodiment will be described below with reference to Figures 13A, 13B, and 14 to 16. To make the figures easier to see, hatching is shown on the lower electrode 13, the piezoelectric film 14, and the upper electrode 15 in Figures 13A, 14, and 16.

[0072] The piezoelectric thin-film devices shown in Figures 13A, 13B, and 14 constitute a piezoelectric MEMS mirror. This piezoelectric thin-film device has a structure in which the outer edge of the thin-film portion 17 is supported by a first substrate 11 which has a rectangular frame shape with a recess 16. The thin-film portion 17 has a mirror portion 200, a peripheral portion 201 arranged around the mirror portion 200, and a support portion 202 connecting the mirror portion 200 and the peripheral portion 201. The mirror portion 200 is supported by the peripheral portion 201 in a double-supported manner by the support portion 202. The peripheral portion 201 refers to the portion of the second substrate 12, lower electrode 13, piezoelectric film 14, and upper electrode 15 that is located outside the mirror portion 200 and the support portion 202, and also includes the portion located outside the thin-film portion 17.

[0073] Specifically, as shown in Figure 13B, a thin-film second substrate 12 is laminated on a first substrate 11, and a recess 16 is formed in the inner portion of the first substrate 11 excluding the outer edge, with a mirror portion 200 provided, for example, at the center of the portion where the recess 16 is formed. A peripheral portion 201 is formed to surround the mirror portion 200, and in a part of the peripheral portion 201, a lower electrode 13, a piezoelectric film 14, and an upper electrode 15 are sequentially laminated on the surface of the second substrate 12. An impurity layer 14a containing a second element in addition to the first element is formed in the surface layer on the upper electrode 15 side of the piezoelectric film 14. Then, as shown in Figure 13A, a slit 203 is formed in the portion where the recess 16 is formed by patterning the second substrate 12. This slit 203 separates the mirror portion 200 from the peripheral portion 201 and also forms a support portion 202 that connects the mirror portion 200 and the peripheral portion 201.

[0074] More specifically, the slit 203 has two parallel sections 203a and 203b extending in the left-right direction of the paper in Figure 13A, and two parallel sections 203c and 203d extending in the right-up direction of the paper, perpendicular to the slit 203a and 203b. Sections 203c and 203d are divided at an intermediate position, and this divided section constitutes the support section 202. Sections 203a and 203b also extend beyond the mirror section 200. The mirror section 200 is formed by the rectangular section enclosed by sections 203a to 203d, and the mirror section 200 is supported by the support sections 202 in the peripheral section 201, which is located on the left and right sides of the paper, flanking the mirror section 200. In other words, the mirror section 200 is in a floating state due to the formation of the slit 203 and recess 16, and is supported by the peripheral section 201 as a double-support beam with the support sections 202 on both sides. Although not shown in the diagram, a thin metal film, such as an aluminum film, is formed on the surface of the mirror portion 200, creating a mirror surface.

[0075] The lower electrode 13, the piezoelectric film 14, and the upper electrode 15 are formed in the peripheral portion 201 so as to fit onto the second substrate 12 within the recess 16, and are arranged so that the lower electrode 13 and the upper electrode 15 face each other with the piezoelectric film 14 in between. More specifically, the lower electrode 13, the piezoelectric film 14, and the upper electrode 15 are formed in the peripheral portion 201 located between portions 203a and 203b of the slit 203. The lower electrode 13 is extended onto the surface of the second substrate 12 in the outer region 21 so as to be exposed from the piezoelectric film 14, and is electrically connectable to the outside via bonding wires or the like. The portion of the upper electrode 15 exposed on the piezoelectric film 14 is also electrically connectable to the outside via bonding wires or the like. These lower electrode 13 and upper electrode 15 are electrically connected to the outside separately on each side of the mirror portion 200, and voltage can be applied independently. Of course, the upper electrode 15 may also be extended from the end face of the piezoelectric film 14 to the surface of the second substrate 12 at a different position from the lower electrode 13, so that an electrical connection to the outside is made at the portion on the surface of the second substrate 12.

[0076] The piezoelectric thin-film device of this embodiment is constructed in this manner. This piezoelectric thin-film device is driven, for example, by electrically connecting the lower electrode 13 and the upper electrode 15 to a control circuit (not shown). When a voltage is applied that generates a periodically changing potential difference between the lower electrode 13 and the upper electrode 15 on each side of the mirror portion 200, the piezoelectric film 14 is displaced by the piezoelectric effect. As a result, the mirror portion 200 is oscillated around the support portion 202, so when laser light is shone toward the mirror portion 200, the optical path of the reflected light changes. Based on this, laser scanning can be performed.

[0077] The piezoelectric thin-film device described above, although different in that it has a double-supported beam structure, can generally be manufactured by following the same process as shown in Figures 3A, 3B, and 5A to 5D described in the first embodiment.

[0078] Furthermore, even in piezoelectric thin-film devices like the one in this embodiment, if ion implantation of the second element is not performed, warping will occur in the thin-film portion 17. In other words, warping occurs in the peripheral portion 201 due to the stress difference in the multilayer film in which the lower electrode 13, the piezoelectric film 14, and the upper electrode 15 are stacked. For this reason, similar to the first embodiment, a piezoelectric thin-film device for measuring the amount of warping is manufactured for the piezoelectric thin-film device of this embodiment by performing the same process as in Figures 3A to 3C, and the amount of warping is measured. Based on the measurement results, the manufacturing process for the piezoelectric thin-film device that will become the final product is then carried out.

[0079] For example, suppose that when a piezoelectric thin-film device for measuring warpage is formed using the same process as in Figures 3A to 3C, warpage as shown in Figures 15 and 16 occurs. Specifically, suppose that each of the multilayer films located on both sides of the mirror portion 200 warps such that the upper electrode 15 side becomes concave, with the inner position being more recessed than the outer position, and the lower electrode 13 side becomes convex, with the inner position protruding more than the outer position. In this case, one surface 22 on the upper electrode 15 side becomes a concave surface 25, and the other surface 23 on the lower electrode 13 side becomes a convex surface 24.

[0080] Therefore, as shown in the process in Figure 3C, the amount of warpage is measured by measuring the height of the tip of the other surface 23 from the top surface of the first substrate 11, or by measuring the height of one side of the mirror portion 200 on the other surface 23 side from the top surface of the first substrate 11. When manufacturing the piezoelectric thin film device to be produced, the film deposition conditions for forming the multilayer film are the same as those for manufacturing the piezoelectric thin film device used for measuring the amount of warpage, and the thickness of the resist 27 formed on the upper electrode 15, etc., is adjusted in accordance with the measurement result of the amount of warpage. As a result, the amount of ion implantation of the impurity layer 14a can be adjusted based on the thickness of the resist 27, so that the correction amount increases in areas with a large amount of warpage by increasing the amount of ion implantation in areas with a large amount of warpage.

[0081] This allows for individual correction of the warpage of multiple piezoelectric thin-film devices according to the amount of warpage, making it possible to bring the thin-film portion 17 closer to a flat surface, as shown in Figures 13B and 14. Therefore, even for piezoelectric thin-film devices having double-supported beams as in this embodiment, it is possible to reduce variations in the amount of warpage and improve yield, thus achieving the same effects as in the first embodiment.

[0082] Furthermore, when forming a metal thin film that constitutes a mirror surface on the surface of the mirror portion 200 as in this embodiment, for example, the metal thin film can be applied while covering areas other than the application area with a resist, and then the metal thin film on the resist can be removed together with the resist by lift-off. Also, when forming a mirror surface with a metal thin film, ion implantation of the second element from one side 22 can be performed before the formation of the metal thin film, or ion implantation can be performed while the metal thin film is covered and protected with a resist. In this way, it is possible to prevent damage to the metal thin film and ensure a mirror surface.

[0083] (Fourth Embodiment) A fourth embodiment will now be described. This embodiment applies the present disclosure to an FBAR (Film Bulk Acoustic Resonator), which has a structure that supports the thin film portion 17 all around as a piezoelectric thin film device. The basic structure of the piezoelectric thin film device of this embodiment is the same as that of the piezoelectric thin film device described in the first embodiment, so the differences from the first embodiment will be mainly described. The piezoelectric thin film device of this embodiment will be described below with reference to Figures 17 to 19. To make the figures easier to see, in Figures 18 and 19, hatching is shown even in parts that are not cross-sections of the lower electrode 13 and the upper electrode 15.

[0084] The piezoelectric thin-film device shown in Figures 17 and 18 constitutes an FBAR. This piezoelectric thin-film device has a structure in which the outer edge of the thin-film portion 17 is supported by a first substrate 11 which has a rectangular frame shape with a recess 16. As shown in Figure 17, a second substrate 12 which has been thinned is laminated on the first substrate 11, and a lower electrode 13, a piezoelectric film 14, and an upper electrode 15 are laminated in order on the surface of the second substrate 12. The lower electrode 13 and the upper electrode 15 are facing each other within the recess 16 with the piezoelectric film 14 in between. In addition, an impurity layer 14a containing a second element in addition to the first element is formed on the surface layer on the lower electrode 13 side within the piezoelectric film 14.

[0085] The upper electrode 15 has a strip-like shape when viewed from above, and is drawn out from the surface of the piezoelectric film 14 to its end face and then to the surface of the second substrate 12, and is electrically connectable to the outside via bonding wires or the like on the surface of the second substrate 12. Furthermore, the lower electrode 13 also has a strip-like shape when viewed from above, and is drawn out to the surface of the second substrate 12 so as to be exposed from the piezoelectric film 14 on the opposite side of the upper electrode 15, and is electrically connectable to the outside via bonding wires or the like.

[0086] Piezoelectric thin-film devices with this structure are used as filters when connected to electrical circuits. For example, the piezoelectric action of the piezoelectric film 14 between the lower electrode 13 and the upper electrode 15 causes the thin-film portion 17 to resonate, allowing it to extract only signals in the frequency band near the resonant frequency from signals of various frequencies flowing through the electrical circuit.

[0087] The piezoelectric thin-film device of this embodiment described above can also be manufactured by following generally the same processes as those described in Figures 3A, 3B, and 5A to 5D in the first embodiment. However, even in the piezoelectric thin-film device of this embodiment, if ion implantation of the second element is not performed, warping will occur in the thin-film portion 17. Therefore, similar to the first embodiment, a piezoelectric thin-film device for measuring the amount of warping is manufactured for the piezoelectric thin-film device of this embodiment by following the same processes as in Figures 3A to 3C, and the amount of warping is measured. Based on the measurement results, the manufacturing process for the final piezoelectric thin-film device is then carried out.

[0088] For example, suppose that when a piezoelectric thin-film device for measuring warpage is deposited using the same process as in Figures 3A to 3C, warpage as shown in Figure 19 occurs. Specifically, suppose that the thin film portion 17 protrudes on the side opposite to the first substrate 11, and warpage occurs such that the thin film portion 17 is concave when viewed from the concave portion 16 side. In this case, one surface 22 on the upper electrode 15 side becomes a convex surface 24, and the other surface 23 on the lower electrode 13 side becomes a concave surface 25. If such warpage occurs, ion implantation of the second element will be performed on the concave side of the piezoelectric film 14, so as shown in Figure 19, the second element will be ion-implanted from below the plane of the paper through the concave portion 16 to the other surface 23 of the thin film portion 17.

[0089] Then, as shown in Figure 3C, the amount of warpage is measured by measuring the height from the top surface of the first substrate 11 to the center of the other surface 23, that is, the depth of the recess in the other surface 23. Furthermore, when manufacturing the piezoelectric thin film device to be produced, the film deposition conditions for forming the multilayer film are the same as the film deposition conditions for the multilayer film used to manufacture the piezoelectric thin film device for measuring the amount of warpage. In addition, the thickness of the resist 27 formed on the surface of the second substrate 12 on the other surface 23 side is adjusted in accordance with the measurement result of the amount of warpage. This allows the amount of ion implantation of the impurity layer 14a to be adjusted based on the thickness of the resist 27, so that the correction amount increases in areas with a large amount of warpage by increasing the amount of ion implantation in those areas.

[0090] This allows for individual correction of the warpage of multiple piezoelectric thin-film devices according to the amount of warpage, making it possible to bring the thin-film portion 17 closer to a flat surface, as shown in Figures 17 and 18. Therefore, the piezoelectric thin-film devices constituting the FBAR in this embodiment can also achieve the same effects as in the first embodiment, such as reducing variations in the amount of warpage and improving yield.

[0091] In Figure 19, an example is given where the thin film portion 17 protrudes on the side opposite to the first substrate 11, and warping occurs such that the thin film portion 17 is concave when viewed from the side of the recess 16, that is, one side 22 becomes a convex surface 24 and the other side 23 becomes a concave surface 25. Since the ion implantation of the second element is performed on the side where the piezoelectric film 14 is concave, in Figure 19, as in the second embodiment, the second element is ion-implanted from below the plane of the paper through the recess 16 to the other side 23 of the thin film portion 17. Conversely, if warping occurs on the opposite side of Figure 19, that is, when the thin film portion 17 is concave toward the first substrate 11 and enters the recess 16, then, as in the first embodiment, the second element can be ion-implanted from above the plane of the paper in Figure 19 to the one side 22 of the thin film portion 17.

[0092] (Other embodiments) This disclosure is not limited to the embodiments described above, and may be modified as appropriate within the scope of the claims. Furthermore, it goes without saying that the elements constituting the embodiments are not necessarily essential unless explicitly stated to be particularly essential or considered fundamentally essential. Also, when numerical values ​​such as the number, numerical values, quantities, or ranges of the components of an embodiment are mentioned, the embodiments are not limited to those specific numbers unless explicitly stated to be particularly essential or considered fundamentally limited to those specific numbers. Furthermore, when the shapes, positional relationships, etc., of components are mentioned in the embodiments, the embodiments are not limited to those shapes, positional relationships, etc., unless explicitly stated or considered fundamentally limited to those specific shapes, positional relationships, etc.

[0093] As shown in Figure 13, the present disclosure may also be applied to a piezoelectric thin-film device equipped with an intermediate electrode 28. In this piezoelectric thin-film device, the intermediate electrode 28 is positioned between the lower electrode 13 and the upper electrode 15, and a piezoelectric film 29, which is the first piezoelectric film, and a piezoelectric film 14, which is the second piezoelectric film, are formed between the lower electrode 13 and the intermediate electrode 28, and between the intermediate electrode 28 and the upper electrode 15, respectively. The piezoelectric film 14 and the piezoelectric film 29 are composed of a piezoelectric material. Taking the elements constituting this piezoelectric material as the first element, an impurity layer 14a is formed in the surface layer of the piezoelectric film 14 near the upper electrode 15, containing a second element different from the first element in addition to the first element that constitutes the piezoelectric film 14. The thin-film portion 17 is composed of a second substrate 12, a lower electrode 13, a piezoelectric film 29, an intermediate electrode 28, a piezoelectric film 14, and an upper electrode 15. Such a piezoelectric thin-film device can be used, for example, as a microphone. In other words, when pressure such as sound pressure is applied to the thin film portion 17 and the thin film portion 17 vibrates, for example, if the free end side of the thin film portion 17 is displaced upward, tensile stress is generated in the piezoelectric film 29 and compressive stress is generated in the piezoelectric film 14. At this time, the pressure such as sound pressure can be detected by measuring the voltage generated between the lower electrode 13 and the upper electrode 15. In such a piezoelectric thin film device, the warping of the thin film portion 17 can be corrected by forming an impurity layer 14a. Furthermore, the amount of correction can be easily adjusted according to the amount of warping.

[0094] The present disclosure may also be applied to piezoelectric thin-film devices other than microphones. Furthermore, the present disclosure may be applied to piezoelectric thin-film devices in which the thin-film portion 17 is supported on both sides by the first substrate 11, or to piezoelectric thin-film devices in which no side surface 18 is formed and the entire upper part of the recess 16 is covered by the thin-film portion 17.

[0095] In the first embodiment, a case was described in which ions accelerated by voltage in a vacuum are implanted into the piezoelectric film 14, but ion implantation may be performed by other methods. For example, ions may be implanted by applying a bias voltage to the thin film portion 17 in a vacuum.

[0096] In the first embodiment, a method for controlling the amount of warpage correction was described by combining the thickness of the resist 27, the acceleration voltage, the type of the second element, etc., but the amount of correction may be controlled by only some of these. Also, in the first embodiment, a method for setting conditions such as the acceleration voltage according to the amount of warpage of each piezoelectric thin film device and performing ion implantation individually was described, but when controlling the amount of correction by the thickness of the resist 27, ion implantation may be performed on multiple piezoelectric thin film devices at once. That is, the spot diameter of the ion beam may be made larger than the width of one piezoelectric thin film device so that the ion beam is irradiated on multiple piezoelectric thin film devices simultaneously.

[0097] In the first embodiment, a piezoelectric thin-film device for measuring warpage was manufactured before the piezoelectric thin-film device that would become the final product. However, the piezoelectric thin-film device that will become the final product may also be used for measuring warpage. For example, consider a case where piezoelectric thin-film devices are formed on multiple wafer-shaped semiconductor substrates 10. In this case, the process shown in Figures 3A to 3C is performed on the first semiconductor substrate 10 to measure the warpage, and then ion implantation is performed to correct the warpage. The piezoelectric thin-film device formed on this semiconductor substrate 10 may then be used as the final product. In this ion implantation, the correction amount can be adjusted by the dose, acceleration voltage, or type of second element. For the second and subsequent semiconductor substrates 10, the ion implantation conditions are set based on the measurement results of the warpage on the first semiconductor substrate 10, and piezoelectric thin-film devices can be formed by performing the process shown in Figures 3A, 3B, and 5A to 5D, similar to the first embodiment. In addition, the warpage of the second and subsequent semiconductor substrates 10 may also be measured periodically, and manufacturing may be carried out while updating the measurement results and ion implantation conditions. Furthermore, the semiconductor substrates 10 from the second onward, for which warpage measurements have been taken, may also be subjected to ion implantation after the process shown in Figures 3A to 3C, similar to the first semiconductor substrate 10, and then used for manufacturing piezoelectric thin-film devices. The measurement of warpage and updating of ion implantation conditions for the second and subsequent semiconductor substrates 10 may be performed every few substrates, or it may be performed for all semiconductor substrates 10.

[0098] In the third embodiment, for a piezoelectric thin-film device having a double-supported beam, warpage is corrected by ion implantation on one surface 22 of the thin-film portion 17 on the upper electrode 15 side. This is merely one example, and warpage can also be corrected by ion implantation on the other surface 23 of the thin-film portion 17 on the lower electrode 13 side, as in the second embodiment. That is, in the third embodiment, an example is given where the multilayer films located on both sides of the mirror portion 200 have one surface 22 side as a concave surface 25 and the other surface 23 side as a convex surface 24. Since the ion implantation of the second element is performed on the concave side of the piezoelectric film 14, in the third embodiment, as in the first embodiment, the second element is ion-implanted from the top of the paper in Figures 15 and 16 onto the one surface 22 of the thin-film portion 17. Conversely, if the direction of warping of the multilayer film is reversed, with one surface 22 becoming a convex surface 24 and the other surface 23 becoming a concave surface 25, the warping can be corrected by performing ion implantation on the other surface 23, as in the second embodiment.

[0099] However, in the case of a piezoelectric thin-film device constituting a piezoelectric MEMS mirror, the second substrate 12 is thicker compared to the first embodiment, etc. Therefore, when the second element is ion-implanted from the other side 23, the amount that reaches the piezoelectric film 14 may be small, or it may not reach the film at all and may stop within the second substrate 12. Even in such cases, stress is generated in the second substrate 12, so the warpage correction effect is still achieved. However, in order to reliably implant the second element into the piezoelectric film 14 and to further enhance the warpage correction effect, it is advisable to adjust the film deposition conditions for the multilayer film so that the conditions for ion implantation of the second element are met from the one side 22. Of course, if the thickness of the second substrate 12 is thin and the second element is implanted into the piezoelectric film 14 even when ion implanted from the other side 23, then a sufficient warpage correction effect can be obtained even if ion implantation is performed from the other side 23. Furthermore, even when forming an aluminum thin film or the like that constitutes the mirror surface on the surface of the mirror portion 200, if the second element is ion-implanted from the other side 23, there is no need to worry about damage to the mirror surface, so in that case, ion implantation may be performed after the formation of the aluminum thin film or the like.

[0100] (Features of this disclosure) [First point of view] Piezoelectric thin film device, Circuit board (10) and The lower electrode (13) is laminated on the substrate, A piezoelectric film (14) made of a piezoelectric material is laminated on the lower electrode, The piezoelectric film comprises an upper electrode (15) laminated on the piezoelectric film, A recess (16) formed on the substrate opposite to the lower electrode forms a thin film portion (17) comprising the lower electrode, the piezoelectric film, and the upper electrode. The elements constituting the piezoelectric material are defined as the first element, A piezoelectric thin-film device in which an impurity layer (14a) containing a second element different from the first element is formed within the piezoelectric film. [Second perspective] The piezoelectric thin film device according to the first aspect, wherein the impurity layer is formed on the surface layer on the upper electrode side within the piezoelectric film.

[0101] [Third perspective] The piezoelectric thin film device according to the first aspect, wherein the impurity layer is formed in the surface layer on the lower electrode side within the piezoelectric film. [Fourth perspective] The piezoelectric thin film device according to any one of the first to third aspects, wherein the impurity layer contains more voids or amorphous layers than the portion of the piezoelectric film other than the impurity layer. [Fifth perspective] Of the surfaces of the thin film portion, the side on the same side as the upper electrode relative to the piezoelectric film is designated as one surface (22), and the side on the same side as the lower electrode relative to the piezoelectric film is designated as the other surface (23). A piezoelectric thin film device according to any one of the first to fourth views, wherein of the one surface and the other surface, the surface closer to the impurity layer has a greater surface roughness than the other surface. [Sixth perspective] A method for manufacturing a piezoelectric thin film device, The lower electrode (13) is formed on the upper surface of the substrate (10), A piezoelectric film (14) made of a piezoelectric material is formed on the upper surface of the lower electrode. The upper electrode (15) is formed on the upper surface of the piezoelectric film, By forming a recess (16) on the surface of the substrate opposite to the lower electrode, a thin film portion (17) comprising the lower electrode, the piezoelectric film, and the upper electrode is formed. A method for manufacturing a piezoelectric thin film device, comprising: using the elements constituting the piezoelectric material as the first element, forming an impurity layer (14a) in the piezoelectric film that contains the first element plus a second element different from the first element. [Seventh perspective] Of the surfaces of the thin film portion, the surface that becomes convex outward when warping occurs in the thin film portion is defined as the convex surface (24), and the concave surface on the opposite side of the convex surface is defined as the concave surface (25). The method for manufacturing a piezoelectric thin film device according to a sixth aspect, wherein the impurity layer is formed on the surface layer of the piezoelectric film that is close to the concave surface. [Perspective 8] A method for manufacturing a piezoelectric thin film device according to the sixth or seventh aspect, wherein the second element is selected according to the magnitude of warping that occurs in the thin film portion when forming the impurity layer. [Perspective 9] A method for manufacturing a piezoelectric thin film device according to any one of the sixth to eighth aspects, wherein the formation of the impurity layer involves accelerating the ionized second element with voltage and injecting it into the piezoelectric film. [Perspective 10] By forming the aforementioned impurity layer, A resist (27) is applied to the upper part of the aforementioned substrate. In the event that warping occurs in the thin film portion, the thickness of the resist is varied in different locations according to the magnitude of the warping in each of the thin film portions. A method for manufacturing a piezoelectric thin film device according to any one of the sixth to ninth aspects, wherein the second element is introduced into the piezoelectric film using the resist. [Perspective 11] A method for manufacturing a piezoelectric thin film device according to a tenth aspect, wherein the thickness of the resist is controlled by an exposure apparatus when forming the impurity layer.

Claims

1. Piezoelectric thin film device, The substrate (10) and The lower electrode (13) is laminated on the substrate, A piezoelectric film (14) made of a piezoelectric material is laminated on the lower electrode, The piezoelectric film comprises an upper electrode (15) laminated on the piezoelectric film, A recess (16) formed on the substrate opposite to the lower electrode forms a thin film portion (17) comprising the lower electrode, the piezoelectric film, and the upper electrode. The elements constituting the piezoelectric material are defined as the first element, Within the piezoelectric film, an impurity layer (14a) is formed containing a second element different from the first element in addition to the first element. The substrate is composed of a first substrate (11) and a second substrate (12) laminated on the upper surface of the first substrate. The recess penetrates the first substrate, On the outer side of the thin film portion, a recess (20) is formed that penetrates the piezoelectric film and the upper electrode, exposing the upper surface of the lower electrode. The region of the second substrate and the lower electrode located below the recess to be exposed is defined as the outer region (21). The outer region has higher strength than the thin film portion. The piezoelectric thin film device is such that the second element contained in the impurity layer is also distributed in the outer region.

2. The piezoelectric thin film device according to claim 1, wherein the impurity layer is formed in the surface layer on the upper electrode side within the piezoelectric film.

3. The piezoelectric thin film device according to claim 1, wherein the impurity layer is formed in the surface layer on the lower electrode side within the piezoelectric film.

4. The piezoelectric thin film device according to any one of claims 1 to 3, wherein the impurity layer contains more voids or amorphous layers than the portion of the piezoelectric film other than the impurity layer.

5. Of the surfaces of the thin film portion, the side on the same side as the upper electrode relative to the piezoelectric film is designated as one surface (22), and the side on the same side as the lower electrode relative to the piezoelectric film is designated as the other surface (23). The piezoelectric thin film device according to any one of claims 1 to 3, wherein one of the two surfaces, the one closer to the impurity layer, has a rougher surface than the other surface.

6. A method for manufacturing a piezoelectric thin film device, The lower electrode (13) is formed on the upper surface of the substrate (10), A piezoelectric film (14) made of a piezoelectric material is formed on the upper surface of the lower electrode. The upper electrode (15) is formed on the upper surface of the piezoelectric film, By forming a recess (16) on the surface of the substrate opposite to the lower electrode, a thin film portion (17) comprising the lower electrode, the piezoelectric film, and the upper electrode is formed. The elements constituting the piezoelectric material are designated as the first element, and an impurity layer (14a) containing the first element plus a second element different from the first element is formed within the piezoelectric film. A method for manufacturing a piezoelectric thin film device, wherein the second element is selected according to the magnitude of warping that occurs in the thin film portion when forming the impurity layer.

7. Of the surfaces of the thin film portion, the surface that becomes convex outward when warping occurs in the thin film portion is defined as the convex surface (24), and the concave surface on the opposite side of the convex surface is defined as the concave surface (25). The method for manufacturing a piezoelectric thin film device according to claim 6, wherein the impurity layer is formed in the surface layer of the piezoelectric film that is close to the concave surface.

8. A method for manufacturing a piezoelectric thin film device according to claim 6 or 7, wherein the impurity layer is formed by accelerating the ionized second element with voltage and injecting it into the piezoelectric film.

9. By forming the aforementioned impurity layer, A resist (27) is applied to the upper part of the substrate. In the event that warping occurs in the thin film portion, the thickness of the resist is varied in different locations according to the magnitude of the warping in each of the thin film portions. A method for manufacturing a piezoelectric thin film device according to claim 6 or 7, wherein the second element is introduced into the piezoelectric film using the resist.

10. The method for manufacturing a piezoelectric thin film device according to claim 9, wherein the thickness of the resist is controlled by an exposure apparatus when forming the impurity layer.

Citation Information

Patent Citations

  • Manufacturing method of piezoelectric actuator, piezoelectric actuator, droplet ejection head, image forming device, and micropump

    JP2012253087A

  • Wafer for forming element and production method of the same

    JP2021082734A

  • Piezoelectric element

    JP2022007879A

  • Piezoelectric element and method for manufacturing the same

    JP2022012349A

  • Bulk acoustic wave (BAW) resonator structure having an electrode with a cantilevered portion and a piezoelectric layer with varying amounts of dopant

    US20140125203A1