Composite semipermeable membrane and separation membrane element comprising a composite semipermeable membrane
The composite semipermeable membrane with a substrate and porous layer of controlled roughness and mass, combined with a cross-linked polyamide functional layer, addresses the issue of reduced efficiency at high pressures, ensuring effective solute removal and water production.
Patent Information
- Application Number
- JP2025555780
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-09-27
- Filing Date
- 2025-09-16
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-09-16
AI Technical Summary
Existing composite semipermeable membranes experience a decrease in water permeability and solute removal efficiency when operated at high pressures, leading to reduced water production rates and solute removal performance.
A composite semipermeable membrane design with a substrate having specific surface roughness characteristics, including a porous layer with controlled mass and thickness, and a separation functional layer composed of cross-linked polyamide, enhances solute removal efficiency and maintains water production even under high-pressure conditions.
The membrane achieves high solute removal performance and maintains water production capacity under high-pressure operation, improving overall water treatment efficiency.
Smart Images

Figure 0007948455000005 
Figure 0007948455000006 
Figure 0007948455000001
Abstract
Description
Technical Field
[0001] The present invention relates to a composite semipermeable membrane and a separation membrane element provided with the composite semipermeable membrane.
Background Art
[0002] A composite semipermeable membrane generally obtained by coating a porous layer with a separation functional layer composed of a polyamide obtained by a polycondensation reaction between a polyfunctional amine and a polyfunctional acid halide has high water permeability and high solute removal properties, and is used in reverse osmosis treatment for removing solutes from raw water, such as seawater desalination.
[0003] In reverse osmosis treatment, a pressure equal to or higher than the difference between the osmotic pressure on the feed water side and the osmotic pressure on the permeate side is applied to the feed water side of the composite semipermeable membrane. In recent years, reverse osmosis treatment has been sometimes used for ZLD (Zero Liquid Discharge) that eliminates wastewater or for concentration in valuable material recovery processes, and depending on the solute concentration, cases of operation at higher pressures than before are also increasing.
[0004] In such high-pressure operation of reverse osmosis treatment, the water permeability of the composite semipermeable membrane may decrease, that is, the water production rate may decrease. When there is no pressure history, the water permeability of the porous layer is about 100 times or more the water permeability of the separation functional layer, so the water permeability of the composite semipermeable membrane is dominated by the separation functional layer. However, it is pointed out in Patent Documents 1 and 2 that the consolidation of the porous layer caused by high-pressure operation reduces the water production rate of the composite semipermeable membrane.
[0005] Patent Documents 1 and 2 disclose a method that suppresses a decrease in the water production rate of the composite semipermeable membrane and improves the water treatment efficiency of brine at a brackish water concentration by thinning the substrate and the porous layer constituting the composite semipermeable membrane to reduce the permeation resistance of the composite of the substrate and the porous layer. Furthermore, in the methods described in Patent Documents 1 and 2, more composite semipermeable membranes can be incorporated into the separation membrane element to increase the effective membrane area per unit volume of the separation membrane element, so that the water treatment efficiency can be improved without changing the size of the spiral-type separation membrane element.
Prior Art Documents
[0006] [Patent Document 1] Japanese Patent Publication No. 2015-089532 [Patent Document 2] Japanese Patent Publication No. 2016-068019 [Overview of the project] [Problems that the invention aims to solve]
[0007] On the other hand, the configurations in Patent Documents 1 and 2 had the problem that solute removal efficiency decreased significantly when the operating pressure was increased to treat saltwater with seawater concentration. The present invention aims to provide a composite semipermeable membrane that has high solute removal efficiency and can maintain the amount of water produced even after high-pressure operation. [Means for solving the problem]
[0008] To solve the above problems, the present invention includes the following configurations [1] to
[10] . [1] A composite semipermeable membrane comprising a substrate, a porous layer provided on one surface of the substrate, and a separation functional layer provided on the porous layer, wherein the mass of the porous layer is 3 g / m 2 More than 13g / m 2 A composite semipermeable membrane, wherein the root mean square height Rq of the surface of the substrate on the side where the porous layer is provided is 1.0 μm or more and 6.0 μm or less. [2] The surface of the substrate on the side where the porous layer is provided has an uneven shape, and the number of recesses with a depth of 20 μm or more is equal to the number of recesses with a depth of 20 μm or more and an area of 500 μm 2 The composite semipermeable membrane described in [1] above, wherein the proportion of the above-mentioned recesses is 15% or less. [3] The surface of the substrate on the side where the porous layer is provided has an uneven shape, with an average area of 500 μm². 2 More than 2000μm 2 The composite semipermeable membrane described in [1] or [2] above, which is as follows: [4] The surface of the base material on the side where the porous layer is provided has an uneven shape, and relative to the number of recesses with a depth of 10 μm or more, the number of recesses with a depth of 10 μm or more and an area of 500 μm 2 or more is 20% or less, the composite semipermeable membrane according to any one of the above [1] to [3]. [5] The composite semipermeable membrane according to any one of the above [1] to [4], wherein the root mean square height Rq of the surface of the base material on the side where the porous layer is provided is 2.0 μm or more and 5.0 μm or less. [6] The mass of the porous layer is 3 g / m 2 or more and 10 g / m 2 or less, the composite semipermeable membrane according to any one of the above [1] to [5]. [7] The composite semipermeable membrane according to any one of the above [1] to [6], wherein the root mean square height Rq of the surface of the base material on the side where the porous layer is provided is 2.0 μm or more and 4.5 μm or less. [8] The root mean square height Rq of the surface of the porous layer on the side where the separation functional layer is provided after supplying an aqueous solution with a NaCl concentration of 3.5 mass% and a pH of 6.5 for 2 hours under the conditions of 5.5 MPa and 25°C is 1.0 μm or more and 2.5 μm or less, the composite semipermeable membrane according to any one of the above [1] to [7]. [9] The polymer impregnation amount of the base material is 0.5 g / m 2 or more and 2.5 g / m 2 or less, the composite semipermeable membrane according to any one of the above [1] to [8].
[10] A separation membrane element comprising the composite semipermeable membrane according to any one of the above [1] to [9]. [Effects of the Invention]
[0009] According to the present invention, it is possible to obtain a composite semipermeable membrane that has high solute removal performance and can maintain water production even after high-pressure operation, and to improve water treatment efficiency. [Brief Description of the Drawings]
[0010] [Figure 1] Figure 1 is a cross-sectional view of a composite semipermeable membrane according to an embodiment of the present invention. [Figure 2]Figure 2 is an exploded view of a separation membrane element according to one embodiment of the present invention. [Modes for carrying out the invention]
[0011] Embodiments of the present invention will be described in detail below, but the present invention is not limited thereto. In this specification, "mass" is synonymous with "weight."
[0012] 1.Composite semipermeable membrane As an embodiment of the present invention, a composite semipermeable membrane 1 having a substrate 2, a porous layer 3 provided on the substrate 2, and a separation functional layer 4 provided on the porous layer 3 will be described below, as shown in Figure 1. The composite in which the porous layer 3 is provided on the substrate 2 will also be referred to as a porous support.
[0013] 1.1 Base material The substrate provides physical strength to the composite semipermeable membrane. Examples of substrates include fabrics composed of polymers such as polyester, polyamide, polyolefin, or mixtures thereof or copolymers thereof.
[0014] As the fabric used as the base material, it is preferable to use a nonwoven fabric from the viewpoint of strength, ability to form irregularities, and fluid permeability. As the nonwoven fabric, both long-fiber nonwoven fabrics and short-fiber nonwoven fabrics can be preferably used.
[0015] The fibers constituting the substrate in the composite semipermeable membrane according to this embodiment may be single-component fibers, composite fibers composed of multiple components, or so-called blended fibers made by mixing multiple types of fibers. Among these, composite fibers in which a low-melting-point polymer having a melting point lower than that of the high-melting-point polymer is arranged around a high-melting-point polymer are preferably used. By using composite fibers, the fibers in the nonwoven fabric adhere firmly to each other by heat-compression bonding. Therefore, when a nonwoven fabric is used as the substrate, it is possible to suppress non-uniformity during casting of the polymer solution for forming the porous layer (hereinafter also simply referred to as "polymer solution") due to fluffing, and to suppress film defects. Furthermore, when using the above-mentioned composite fibers, the number of adhesion points is increased compared to blended fibers made by mixing fibers made only of high-melting-point polymers and fibers made only of low-melting-point polymers, so the number of recessed areas in the substrate is reduced, and a composite semipermeable membrane that can withstand high-pressure operation can be produced even when the strength of the porous layer is low.
[0016] 1.1.1 Basis weight of the base material The basis weight of the substrate in the composite semipermeable film according to this embodiment is 30 g / m². 2 More than 100g / m 2 The following is preferable: 60 g / m 2 More than 80g / m 2 The following is more preferable: Base material weight of 30 g / m² 2 With the above conditions, excessive permeation during polymer solution casting is minimized, resulting in good film formation, high film peel strength and mechanical strength, and a highly durable separation film. On the other hand, if the basis weight of the substrate is 100 g / m² 2 The following conditions allow for a reduction in the thickness of the composite semipermeable membrane and an increase in the membrane area per composite semipermeable membrane element.
[0017] 1.1.2 Density of the substrate The density of the substrate in the composite semipermeable film according to this embodiment is 0.70 g / cm³. 3 More than 1.05g / cm 3 The following is preferable: The density of the base material is 0.70 g / cm³. 3As a result, excessive permeability during polymer solution casting is minimized, allowing for good film formation and the creation of a composite semipermeable film with high mechanical strength and excellent durability. On the other hand, if the density of the substrate is 1.05 g / cm³ 3 As described below, the polymer solution penetrates rapidly into the nonwoven fabric during porous layer formation, resulting in strong adhesion between the substrate and the porous layer, and a semipermeable film with excellent peel strength can be obtained.
[0018] 1.1.3 Thickness of the base material In the composite semipermeable membrane according to this embodiment, the thickness of the substrate is preferably 50 μm to 120 μm, more preferably 50 μm to 110 μm, and even more preferably 60 μm to 100 μm. When the thickness of the substrate is within the above range, sufficient strength for pressure resistance can be maintained, and the effective membrane area when used as a separation membrane element can be increased.
[0019] 1.1.4 Pure water permeability coefficient of the substrate The pure water permeability coefficient of the substrate in the composite semipermeable membrane according to this embodiment at 25°C is 50 × 10 -9 m 3 / (m 2 ·s·Pa) or more 1500×10 -9 m 3 / (m 2 Preferably less than 100 × 10 -9 m 3 / (m 2 ·s·Pa) or more 1000×10 -9 m 3 / (m 2 A value of less than or equal to (s·Pa) is more preferable. When the pure water permeability coefficient is within the above range, it does not affect the permeability resistance which would lead to a decrease in the amount of water produced by the composite semipermeable membrane. Furthermore, because the polymer solution penetrates quickly into the nonwoven fabric when the porous layer is formed, the substrate and the porous layer adhere strongly, and a semipermeable membrane with excellent membrane peel strength can be obtained.
[0020] The pure water permeability coefficient of the substrate can be determined by the following method. Cut out a circle of the substrate with a diameter of 4.3 cm, and set the cut-out sample in a stirring-type ultra-holder (UHP-43K, manufactured by Advantec Toyo Co., Ltd.). Next, fill the cell with pure water at 25°C, attach the cap, and then increase the pressure to a constant level using nitrogen or compressed air. Finally, measure the amount of pure water permeate over a certain period of time and calculate the pure water permeability coefficient from the following formula (1). Pure water permeability coefficient [m 3 / (m 2 (·s·Pa) = Pure water permeability / (Effective filtration area of substrate × Water collection time × Supply pressure) ... Equation (1)
[0021] 1.1.5 Root mean square height Rq of the substrate The composite semipermeable membrane of the present invention has a root mean square height Rq (hereinafter also simply referred to as "substrate Rq") of the surface of the substrate on the side where the porous layer is provided, which is 1.0 μm or more and 6.0 μm or less. A substrate Rq of 2.0 μm or more and 5.5 μm or less is more preferable, 2.0 μm or more and 5.0 μm or less is even more preferable, and 2.0 μm or more and 4.5 μm or less is particularly preferable. When the substrate Rq is 6.0 μm or less, deformation of the porous layer and the separation functional layer due to irregularities in the substrate when the composite semipermeable membrane is operated under high pressure can be prevented, and a composite semipermeable membrane with high solute removal performance can be obtained regardless of the strength of the porous layer. Furthermore, when the substrate Rq is 1.0 μm or more, the adhesive strength between the substrate and the porous layer is increased, and a decrease in the performance of the separation membrane element due to delamination occurring near the interface between the substrate and the porous layer is less likely to occur.
[0022] The Rq of the substrate can be calculated by observing the surface of the substrate on the side where the porous layer is provided using a laser microscope. Specifically, it is calculated using the method described in "Root Mean Square Height Rq of Substrate" in the examples described later. If the substrate already has a porous layer, it can be observed by immersing it in a suitable solvent that can dissolve the porous layer, leaving only the substrate. The Rq of the substrate can be controlled, for example, by the number of times, temperature, and linear pressure of the thermocompression bonding using a flat roll as described in "2.1 Substrate Formation Process" below.
[0023] 1.1.6 Average area of recesses in the substrate In this embodiment, the surface of the substrate on the side where the porous layer is provided in the composite semipermeable membrane has an uneven shape, with an average area of 500 μm². 2 More than 2000μm 2 Preferably, the following, 500 μm 2 More than 1500μm 2 The following is more preferable: The average area of the recesses is 2000 μm². 2 The following conditions prevent deformation of the porous layer and separation function layer caused by irregularities in the substrate when the composite semipermeable membrane is operated under high pressure. Furthermore, the average area of the recesses is 500 μm². 2 As a result, the adhesive strength between the substrate and the porous layer is increased, and the performance degradation of the separation membrane element due to delamination occurring near the interface between the substrate and the porous layer is less likely to occur.
[0024] The number of recesses on the surface of the substrate is preferably 100 to 600 per 1224 μm square, more preferably 200 to 600, and even more preferably 200 to 550. When the number of recesses on the surface of the substrate is 100 or more, the adhesive strength between the substrate and the porous layer is increased, and the performance degradation of the separation membrane element due to delamination occurring near the interface between the substrate and the porous layer is less likely to occur. Furthermore, when the number of recesses on the surface of the substrate is 600 or less, deformation of the porous layer and the separation functional layer due to the unevenness of the substrate can be prevented when the composite semipermeable membrane is operated under high pressure, and a composite semipermeable membrane with high solute removal performance can be obtained regardless of the strength of the porous layer.
[0025] The average area of the recesses in the substrate can be calculated by observing the surface of the substrate on the side where the porous layer is provided using a laser microscope. Specifically, it is calculated using the method described in "Average Area of Recesses in the Substrate" in the examples described later. If the substrate already has a porous layer, it can be observed by immersing it in a good solvent that can dissolve the porous layer, leaving only the substrate. The average area of the recesses in the substrate can be controlled, for example, by using a composite fiber in which a low-melting-point polymer having a lower melting point than the high-melting-point polymer is arranged around the high-melting-point polymer, or by the number of times, temperature, and linear pressure of the heat-compression bonding with a flat roll as described in "2.1 Substrate Formation Process" below.
[0026] 1.1.7 Percentage of recesses in the substrate In the composite semipermeable membrane according to this embodiment, the surface of the substrate on the side where the porous layer is provided has an uneven shape, and the number of recesses with a depth of 10 μm or more is equal to the area of recesses with a depth of 10 μm or more and an area of 500 μm. 2 The proportion of the number of recesses (hereinafter also referred to as the "proportion of 10 μm recesses") is preferably 20% or less, more preferably 15% or less, and even more preferably 10% or less. Depth 10 μm or more and area 500 μm 2 If more than 20% of the substrate has the above-mentioned recesses, deformation of the porous layer and separation functional layer due to the recesses in the substrate will occur when the composite semipermeable membrane is operated at high pressure, and the solute removal performance is likely to decrease. When the proportion of 10 μm recesses is within the above range, high solute removal performance can be obtained even when the composite semipermeable membrane is operated at high pressure. From the viewpoint of minimizing deformation of the porous layer and separation functional layer due to the recesses in the substrate, it is most desirable that there are no recesses with a depth of 10 μm or more, and the lower limit of the proportion of 10 μm recesses is 0%.
[0027] Furthermore, the surface of the substrate on the side where the porous layer is provided in the composite semipermeable membrane according to this embodiment has a depth of 20 μm or more and an area of 500 μm, relative to the number of recesses with a depth of 20 μm or more. 2 The proportion of the above-mentioned recesses (hereinafter also referred to as the "proportion of 20 μm recesses") is preferably 15% or less, more preferably 10% or less, and even more preferably 5% or less. When the proportion of 20 μm recesses is within the above range, deformation of the porous layer and separation functional layer caused by recesses in the substrate can be suppressed when the composite semipermeable membrane is operated under high pressure, and a decrease in solute removal performance can be prevented. From the viewpoint of minimizing deformation of the porous layer and separation functional layer caused by recesses in the substrate, it is most desirable that there are no recesses with a depth of 20 μm or more, and the lower limit of the proportion of 20 μm recesses is 0%.
[0028] The ratio of recesses in the substrate can be calculated by observing the surface of the substrate on the side where the porous layer is provided using a laser microscope. Specifically, it is calculated using the method described in "Ratio of Recesses in Substrate" in the examples described later. If the substrate already has a porous layer, it can be observed by immersing it in a suitable solvent that can dissolve the porous layer, leaving only the substrate. The ratio of recesses in the substrate can be controlled, for example, by using a composite fiber in which a low-melting-point polymer having a lower melting point than the high-melting-point polymer is arranged around the high-melting-point polymer, or by the number of times, temperature, and linear pressure of the heat-compression bonding with a flat roll as described in "2.1 Substrate Formation Process" below.
[0029] 1.1.8 Polymer impregnation amount of the substrate The amount of polymer impregnation in the substrate of the composite semipermeable film according to this embodiment is 0.5 g / m². 2 More than 2.5g / m 2 The following is preferable: 1.0 g / m 2 More than 2.3g / m 2 The following is more preferable: 1.2 g / m 2 More than 2.1g / m 2 The following is even more preferable: The polymer impregnation amount of the substrate is 2.5 g / m². 2 The following conditions allow for suppression of the penetration of the sealing material by the polymer impregnated in the substrate when impregnating the sealing portion of the separation membrane element with the sealing material, thereby obtaining a separation membrane element that is sufficiently impregnated with the sealing material. Furthermore, the polymer impregnation amount of the substrate is 0.5 g / m². 2 As a result, the adhesive strength between the substrate and the porous layer is increased, and performance degradation of the composite semipermeable membrane and separation membrane element due to delamination occurring near the interface between the substrate and the porous layer is less likely to occur. Polymer impregnation amount refers to the amount of polymer that forms the porous layer contained in the substrate after the porous layer has been peeled off, and is measured by the method described in "Polymer Impregnation Amount of Substrate" in the examples described later.
[0030] The amount of polymer impregnation into the substrate can be controlled, for example, by conditions such as the coating thickness of the polymer solution on the substrate and the polymer solution temperature in "2.2 Porous Layer Formation Process" described later, or by the number of times, temperature, and linear pressure of the heat-compression bonding with a flat roll as described in "2.1 Substrate Formation Process" described later.
[0031] 1.2 Porous layer In the composite semipermeable membrane according to this embodiment, the material of the porous layer is preferably a thermoplastic polymer. Here, "thermoplastic polymer" means a polymer made of chain-like polymers that exhibits the property of deforming or flowing when heated by an external force.
[0032] Examples of thermoplastic polymers include homopolymers of polysulfone, polyethersulfone, polyamide, polyester, cellulose polymers, vinyl polymers, polyphenylene sulfide, polyphenylene sulfide sulfone, polyphenylene sulfone, and polyphenylene oxide, as well as copolymers thereof. One type may be used alone, or two or more types may be used in combination.
[0033] Examples of cellulosic polymers include cellulose acetate and cellulose nitrate, while examples of vinyl polymers include polyethylene, polypropylene, polyvinyl chloride, chlorinated vinyl chloride, and polyacrylonitrile. Among these, polysulfone (hereinafter referred to as "Psf"), polyacrylonitrile, polyamide, polyester, polyvinyl alcohol, polyphenylene sulfide sulfone, polyphenylene sulfone, polyphenylene sulfide, polyethersulfone, polyvinylidene fluoride, cellulose acetate, polyvinyl chloride, or chlorinated vinyl chloride are preferred. Among these, Psf is more preferred because it has high chemical, mechanical, and thermal stability and is easy to mold. The porous layer preferably contains these listed compounds as its main components.
[0034] The mass-average molecular weight (hereinafter referred to as "Mw") of Psf, measured by gel permeation chromatography (GPC) with N-methylpyrrolidone as the solvent and polystyrene as the standard substance, is preferably between 10,000 and 200,000, and more preferably between 15,000 and 100,000. When the Mw of Psf is 10,000 or higher, desirable mechanical strength and heat resistance can be obtained as a porous layer. Furthermore, when the Mw is 200,000 or lower, the viscosity of the solution is within an appropriate range, and good moldability can be achieved.
[0035] 1.2.1 Mass of the porous layer The mass of the porous layer in the composite semipermeable membrane of the present invention is 3 g / m². 2 More than 13g / m 2 The following applies: 3g / m 2 More than 10g / m 2 The following is preferable: 4 g / m 2 More than 8g / m 2 The following is more preferable: The mass of the porous layer is 3 g / m 2 The above conditions provide the necessary strength and surface morphology for a porous layer. On the other hand, the higher the mass of the porous layer, the less it is affected by deformation due to the shape of the substrate, and solute removal performance is maintained, but water production capacity tends to decrease. 2 The following conditions result in a composite semipermeable membrane with high water production capacity retention. Furthermore, the effective membrane area of the separation membrane element can also be increased. The mass of the porous layer can be controlled by, for example, the polymer concentration in the polymer solution, the thickness of the polymer solution applied to the substrate, and the temperature of the coagulation solution. Note that the mass of the porous layer (g / m 2 ) more specifically refers to the mass of the porous layer per unit area, and is calculated by the method described in the "Mass of the Porous Layer" section of the examples described later.
[0036] In addition to water production capacity retention, high solute removal performance is also crucial for the performance of composite semipermeable membranes. The inventors found that when the mass of the porous layer in a composite semipermeable membrane is controlled within the above range, the porous layer and separation functional layer deform, leading to a decrease in solute removal performance. Through diligent research to address this issue, they discovered that the surface roughness of the substrate, represented by Rq, is important among the indicators of substrate smoothness. Conventionally, indicators of surface smoothness of substrates forming porous layers have focused on macroscopic areas, such as Beck smoothness, core level difference (Sk), and 75-degree specular gloss. However, controlling these indicators has not been able to suppress deformation of the porous layer and separation functional layer by the substrate. In other words, the present invention has found that by setting the Rq of the substrate forming the porous layer to 1.0 μm or more and 6.0 μm or less, deformation of the porous layer and the separation functional layer due to the substrate is suppressed even when the mass of the porous layer is within the above range, thereby achieving both water production volume retention and high solute removal performance.
[0037] 1.2.2 Thickness of the porous layer In the composite semipermeable membrane according to this embodiment, the thickness of the porous layer is preferably 4 μm to 25 μm, more preferably 4 μm to 18 μm, and even more preferably 4 μm to 12 μm. When the thickness of the porous layer is 4 μm or more, the polymer solution for forming the porous layer can be applied without causing surface defects, and it can function as a scaffold for interfacial polycondensation to form a separation functional layer. Furthermore, when the thickness of the porous layer is 25 μm or less, a composite semipermeable membrane with high water production capacity can be obtained.
[0038] Furthermore, the thickness of the porous layer after supplying the composite semipermeable membrane according to this embodiment with an aqueous solution of 3.5% by mass and pH 6.5 under conditions of 7.0 MPa and 45°C for 24 hours (hereinafter also simply referred to as "thickness of the porous layer after pressurization") is preferably 3 μm to 12 μm, and more preferably 3 μm to 7 μm. When the thickness of the porous layer after pressurization is within the above range, sufficient strength for pressure resistance can be maintained, and the effective membrane area of the separation membrane element can be increased. The thickness of the porous layer can be controlled, for example, by the thickness of the polymer solution applied to the substrate, the temperature of the coagulation solution, etc.
[0039] 1.2.3 Root mean square height Rq of porous layer The root mean square height Rq of the porous layer on the side with the separation functional layer (hereinafter also simply referred to as "Rq of the porous layer after pressurization") after supplying an aqueous solution with a NaCl concentration of 3.5% by mass and a pH of 6.5 to the composite semipermeable membrane according to this embodiment for 2 hours under conditions of 5.5 MPa and 25°C is preferably 1.0 μm or more and 2.5 μm or less, and more preferably 1.0 μm or more and 2.0 μm or less. Having the above range for the Rq of the porous layer after pressurization means that the deformation of the porous layer is small during high-pressure operation, and a composite semipermeable membrane with high solute removal capacity and water production capacity retention can be obtained even during high-pressure operation.
[0040] The Rq of the porous layer after pressurization can be calculated by observing the surface of the porous layer on the side where the separation functional layer is provided using a laser microscope after pressurization. Specifically, it is calculated using the method described in "Root Mean Square Height Rq of Porous Layer" in the examples described later. If a separation functional layer is already provided in the porous layer, the measurement may be taken with the separation functional layer formed, or the measurement may be taken after decomposing and removing the separation functional layer with sodium hypochlorite.
[0041] The mass of the porous layer is 3 g / m 2 More than 13g / m 2The following applies, and the Rq of the porous layer after pressurization can be controlled within the above range by, for example, the number of times, temperature, and linear pressure of thermocompression bonding with a flat roll as described in "2.1 Formation Process of Substrate" below. Another method is to improve the strength of the porous layer by using a high-strength thermoplastic polymer.
[0042] 1.3 Separation functional layer The separation functional layer of the composite semipermeable membrane according to this embodiment preferably contains polyamide, and more preferably contains polyamide as the main component. "Main component" means a component that accounts for 50% by mass or more of the components of the separation functional layer. Furthermore, the polyamide contained in the separation functional layer is preferably a crosslinked polyamide, and more preferably a crosslinked aromatic polyamide.
[0043] "Polyamide" refers to a polycondensate formed by polycondensing a polyfunctional amine and a polyfunctional acid halide.
[0044] "Cross-linked polyamide" refers to a polyamide having a cross-linked structure. Examples include a form in which a cross-linked structure is formed via a cross-linking agent, and a form in which at least one of a polyfunctional amine and a polyfunctional acid halide is trifunctional or more, and the polyamide forms a network-like cross-linked structure. Examples of cross-linked polyamides include cross-linked aromatic polyamides and cross-linked aliphatic polyamides.
[0045] "Cross-linked aromatic polyamide" refers to a cross-linked polyamide composed of polyfunctional aromatic amines and polyfunctional aromatic acid halides.
[0046] "Cross-linked aliphatic polyamide" refers to a cross-linked polyamide composed of a polyfunctional aliphatic amine and a polyfunctional aromatic acid halide.
[0047] The presence of polyamide in the separation functional layer can be confirmed, for example, by ATR-FTIR (total internal reflection-Fourier transform infrared spectroscopy).
[0048] In particular, the separation functional layer preferably contains 50% by mass or more of cross-linked polyamide, more preferably 80% by mass or more, and even more preferably 90% by mass or more, from the viewpoint of exhibiting high solute removal performance.
[0049] From the viewpoint of obtaining rigid molecular chains and forming a pore structure suitable for the removal of fine solutes such as hydrated ions and boron, it is preferable that the crosslinked polyamide contains at least one of a polyfunctional amine and a polyfunctional acid halide that is trifunctional or greater. In particular, the separation functional layer preferably contains a crosslinked aromatic polyamide obtained by polycondensation of a polyfunctional aromatic amine and a polyfunctional aromatic acid halide.
[0050] A "polyfunctional amine" refers to an amine having at least two primary and / or secondary amino groups in one molecule. Examples of polyfunctional amines include polyfunctional aromatic amines in which two amino groups are bonded to the aromatic ring in an ortho, meta, or para position, such as o-phenylenediamine, m-phenylenediamine (hereinafter referred to as "m-PDA"), p-phenylenediamine, o-xylylenediamine, m-xylylenediamine, p-xylylenediamine, o-diaminopyridine, m-diaminopyridine, and p-diaminopyridine; and polyfunctional aromatic amines such as 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 3,5-diaminobenzoic acid, 3-aminobenzylamine, and 4-aminobenzylamine. Furthermore, examples of polyfunctional amines include aliphatic amines such as ethylenediamine and propylenediamine, and alicyclic polyfunctional amines such as 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, piperazine, 2,5-dimethylpiperazine, 2-methylpiperazine, 2,6-dimethylpiperazine, 2,3,5-trimethylpiperazine, 2,5-diethylpiperazine, 2,3,5-triethylpiperazine, 2-n-propylpiperazine, 2,5-di-n-butylpiperazine, 1,3-bispiperidylpropane, and 4-aminomethylpiperazine. These polyfunctional amines may be used individually or in combination of two or more.
[0051] In particular, from the viewpoint of solute removal, water permeability, and heat resistance of the composite semipermeable membrane, it is preferable to use m-PDA, p-phenylenediamine, and 1,3,5-triaminobenzene as the polyfunctional amine. Among these, it is more preferable to use m-PDA due to its availability and ease of handling. These polyfunctional aromatic amines may be used individually or in combination of two or more.
[0052] "Polyfunctional acid halides" refer to acid halides or polyfunctional acid anhydride halides having at least two halogenated carbonyl groups in one molecule, and are not particularly limited as long as they form a separation functional layer of polyamide through polycondensation with the above-mentioned polyfunctional amines. For example, trifunctional acid halides include trimesic acid chloride (hereinafter referred to as "TMC"), 1,3,5-cyclohexanetricarboxylic acid trichloride, and 1,2,4-cyclobutanetricarboxylic acid trichloride. Examples of difunctional acid halides include aromatic difunctional acid halides such as biphenyldicarboxylic acid dichloride, biphenylenecarboxylic acid dichloride, azobenzenedicarboxylic acid dichloride, terephthalic acid chloride, isophthalic acid chloride, and naphthalenedicarboxylic acid chloride; aliphatic difunctional acid halides such as adipoyl chloride and sebacoyl chloride; and alicyclic difunctional acid halides such as cyclopentanedicarboxylic acid dichloride, cyclohexanedicarboxylic acid dichloride, and tetrahydrofrancicarboxylic acid dichloride. These polyfunctional acid halides may be used individually or in combination of two or more.
[0053] From the viewpoint of solute removal and heat resistance of the composite semipermeable membrane, the polyfunctional acid halide is more preferably a polyfunctional aromatic acid chloride having 2 to 4 carbonyl chloride groups in one molecule.
[0054] 1.4 Separation membrane element An example of the configuration of a separation membrane element equipped with a composite semipermeable membrane according to this embodiment will be described with reference to Figure 2.
[0055] As shown in Figure 2, the separation membrane element 5 comprises a composite semipermeable membrane 1, a supply-side channel material 8, a permeable-side channel material 9, a water collection pipe 10, and end plates 6 and 7. The supply-side channel material 8 is positioned opposite the supply side of the composite semipermeable membrane 1 and is wrapped around the water collection pipe 10 together with the composite semipermeable membrane 1. A net is preferred as the supply-side channel material 8. By using a supply-side channel material 8 with a thickness of 0.3 mm to 1.0 mm, the water treatment efficiency of the separation membrane element using the composite semipermeable membrane of the present invention can be further improved. The permeable channel material 9 is positioned opposite the permeable side of the composite semipermeable membrane 1 and is spirally wound around the water collection pipe 10 together with the composite semipermeable membrane 1. When using the composite semipermeable membrane according to this embodiment, it can withstand the winding pressure, thereby suppressing deformation of the porous layer and the separation functional layer, and improving the initial processing efficiency of the separation membrane element. For example, tricot or a protrusion-adhering sheet can be used as the permeable channel material 9. By using a permeable channel material 9 with a thickness of 0.1 mm to 0.5 mm, the processing efficiency of the separation membrane element using the composite semipermeable membrane according to this embodiment can be further improved. The water collection pipe 10 is a hollow cylindrical member having multiple holes on its side. The end plates 6 and 7 are disc-shaped members equipped with multiple supply ports (or discharge ports).
[0056] The separation of fluids by the separation membrane element 5 will now be explained. The supply water 11 is supplied to the separation membrane element 5 from multiple supply ports on the end plate 6. The supply water 11 moves within the supply-side channel formed by the supply-side channel material 8 on the supply side of the composite semipermeable membrane 1. The fluid that permeates through the composite semipermeable membrane 1 (shown as permeate water 12 in the figure) moves within the permeate-side channel formed by the permeate-side channel material 9. The permeate water 12 that reaches the collection pipe 10 enters the inside of the collection pipe 10 through the holes in the collection pipe 10. The permeate water 12 that has flowed inside the collection pipe 10 is discharged to the outside from the end plate 7. On the other hand, the fluid that did not permeate through the composite semipermeable membrane 1 (shown as concentrated water 13 in the figure) moves within the supply-side channel and is discharged to the outside from the end plate 7. In this way, the supply water 11 is separated into permeate water 12 and concentrated water 13.
[0057] 2.1 Substrate Formation Process In the composite semipermeable film according to this embodiment, the substrate is preferably a laminate of multiple nonwoven fabrics or the like, formed by applying heat and pressure to obtain sufficient strength and smoothness, and it is more preferable to apply heat and pressure multiple times. If the number of laminates is two or more, the texture is improved compared to a single layer, and sufficient uniformity can be obtained. Furthermore, if the number of laminates is five or less, it is possible to suppress wrinkle formation during lamination and to suppress delamination between layers.
[0058] The base material is obtained by heat-pressing, for example, using two or more sets of flat rolls, either continuously or discontinuously, in a 2-roll x 2 set system, a 2-roll x 3 set system, or a 3-roll system such as elastic / metal / elastic, elastic / metal / metal, or metal / elastic / metal, using metal / metal / elastic flat rolls during the manufacturing process.
[0059] A "flat roll" refers to a roll with no irregularities on its surface. For example, by using a combination of a metal roll and an elastic roll, it is possible to suppress the fusion of fibers on the surface of a nonwoven fabric and maintain its shape.
[0060] Examples of elastic rolls include so-called paper rolls such as paper, cotton, and aramid paper, and resin rolls such as urethane resin, epoxy resin, silicone resin, polyester resin, and hard rubber.
[0061] The surface temperature of the metal roll is preferably 20 to 90°C lower than the melting point of the polymer constituting at least the surface of the fibers constituting the base material, and more preferably 30 to 70°C lower. If the surface temperature of the metal roll is 20°C or more lower than the melting point of the polymer constituting at least the surface of the fibers constituting the base material, excessive fusion of the surface fibers of the base material can be suppressed, the polymer solution for forming the porous layer can penetrate more easily, and a porous support with excellent adhesive strength can be obtained. On the other hand, if the difference between the surface temperature of the metal roll and the melting point of the polymer constituting at least the surface of the fibers constituting the nonwoven fabric is 90°C or less, the fibers constituting the base material can be firmly bonded to each other, and the unevenness and recess area of the base material can be controlled.
[0062] Furthermore, it is also preferable to create a temperature difference between the metal roll and the elastic roll, so that the surface temperature of the elastic roll is 10 to 120°C lower than the surface temperature of the metal roll.
[0063] Furthermore, the linear pressure of the flat roll is preferably 196 N / cm or more and 4900 N / cm or less, more preferably 490 N / cm or more and 4900 N / cm or less, and even more preferably 980 N / cm or more and 4900 N / cm or less. When the linear pressure of the flat roll is 196 N / cm or more, the fibers constituting the substrate are firmly bonded to each other, and the unevenness and recess area of the substrate can be controlled. Also, when the linear pressure of the flat roll is 4900 N / cm or less, excessive fusion of the substrate surface fibers can be suppressed, and the penetration of the polymer solution for forming the porous layer into the substrate is not hindered, resulting in a porous support with excellent film adhesion strength.
[0064] 2.2 Process for forming a porous layer The process for forming the porous layer in the composite semipermeable membrane according to this embodiment is as follows: Step (a) A step of forming a flat film from a polymer solution for forming a porous layer, which is obtained by dissolving a thermoplastic polymer in a good solvent. The process includes step (b) a step of obtaining a porous layer by solidifying the thermoplastic polymer in a solidification solution containing a non-solvent and a good solvent for the thermoplastic polymer.
[0065] The process for forming a porous layer may further include a step of preparing a polymer solution by dissolving a thermoplastic polymer, which is a component of forming the porous layer, in a good solvent for the thermoplastic polymer.
[0066] The preferred material for the thermoplastic polymer that forms the main component of the porous layer is as described above. The following conditions are particularly preferred when the thermoplastic polymer is Psf.
[0067] A "good solvent" is one that dissolves thermoplastic polymers. By selecting a good solvent, the rate at which the good solvent flows out of the polymer solution in step (b) above can be adjusted. As a result, the surface properties of the porous layer, the density layer thickness, and the surface roughness can be controlled. As a good solvent, at least one solvent selected from the group consisting of amides such as N-methylpyrrolidone, tetrahydrofuran, dimethyl sulfoxide, tetramethylurea, N,N-dimethylacetamide, N,N-dimethylformamide (hereinafter referred to as "DMF"), N,N-dimethylisobutylamide, N,N-diisopropylisobutylamide, and N,N-bis(2-ethylhexyl)isobutylamide, lower alkyl ketones such as acetone and methyl ethyl ketone, esters such as trimethyl phosphate, and lactones such as γ-butyrolactone is preferably used. Among these, dimethyl sulfoxide and DMF are preferably used as good solvents.
[0068] Step (a) can be carried out by coating a polymer solution onto a substrate or by immersing the substrate in a polymer solution.
[0069] The application of polymer solutions to substrates can be carried out by various coating methods. Among these, pre-metering coating methods such as die coating, slide coating, and curtain coating, which allow for the application of precise amounts of solution, are preferred. Furthermore, in the formation of porous layers, the slit die method for applying polymer solutions is even more preferably used.
[0070] The polymer concentration (i.e., solid content concentration) in the polymer solution is preferably 15% by mass or more and 30% by mass or less, more preferably 16% by mass or more and 25% by mass or less, and even more preferably 17% by mass or more and 20% by mass or less.
[0071] If the polymer concentration is 15% by mass or higher, the mass of the porous layer is 3 g / m 2 More than 13g / m 2 Sufficient porous layer strength can be obtained even under the following conditions. Furthermore, when the polymer concentration is 30% by mass or less, the viscosity of the polymer solution falls within an appropriate range, allowing for the application of a precise amount of solution using various coating methods.
[0072] The temperature of the polymer solution when applied to the substrate is preferably between 10°C and 60°C. When the polymer solution temperature is within this range, the polymer does not precipitate, and the polymer solution is sufficiently impregnated into the spaces between the fibers of the substrate before solidifying. As a result, a porous support can be obtained in which the porous layer is firmly bonded to the substrate by impregnation. The preferred temperature range of the polymer solution can be appropriately adjusted depending on the viscosity of the polymer solution used.
[0073] Furthermore, the thermoplastic polymer contained in the polymer solution can be selected as appropriate, taking into consideration various properties such as the strength characteristics, permeability characteristics, and surface characteristics of the porous layer to be manufactured. For example, by pouring a polymer solution onto a substrate to a certain thickness and then wet-solidifying it in a solidification bath, a porous layer can be obtained in which most of the surface has fine pores with a diameter of several 1 to 30 nm.
[0074] The solvent contained in the polymer solution may be the same solvent as the polymer solution or a different solvent, as long as it is a good solvent for thermoplastic polymers. It can be adjusted as appropriate, taking into account the strength characteristics of the porous layer to be manufactured and the impregnation of the polymer solution into the substrate.
[0075] As described above, applying a polymer solution to a substrate causes the polymer solution to impregnate the substrate. To control the impregnation of the polymer solution into the substrate, methods include controlling the time between applying the polymer solution to the substrate and immersing it in a solidification solution (solidification bath), or adjusting the viscosity by controlling the temperature or concentration of the polymer solution. It is also possible to combine these methods.
[0076] In step (b), a polymer solution placed on a substrate is immersed in a coagulation solution having a polymer solubility lower than that of a good solvent in the polymer solution, thereby solidifying the polymer and forming a three-dimensional network structure.
[0077] Furthermore, by including a non-solvent such as water and a good solvent in the coagulation solution, it becomes possible to form a dense layer on the film surface through non-solvent-induced phase separation.
[0078] Examples of non-solvents include aliphatic hydrocarbons such as water, hexane, pentane, benzene, toluene, methanol, ethanol, trichloroethylene, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butylene glycol, pentanediol, hexanediol, and low molecular weight polyethylene glycol, as well as aromatic hydrocarbons, aliphatic alcohols, or mixtures thereof. These may be used individually or in combination of two or more.
[0079] The temperature of the coagulation solution is preferably between 5°C and 50°C, and more preferably between 5°C and 30°C. When the temperature of the coagulation solution is 50°C or lower, the vibration of the coagulation bath surface due to thermal motion does not become excessive, and the surface smoothness of the porous layer is improved. Furthermore, when the temperature of the coagulation solution is 5°C or higher, a sufficient coagulation rate is obtained, and film formation is good. In addition, when the temperature of the coagulation solution is within the above range, a porous layer with a surface pore size of 3 nm to 10 nm is easily obtained.
[0080] Next, it is preferable to wash the porous support with hot water to remove any remaining film-forming solvent. The temperature of the hot water at this time is preferably 50°C to 100°C, and more preferably 60°C to 95°C. If the temperature of the hot water is 100°C or lower, the degree of shrinkage of the porous support can be kept to a minimum. Also, if the temperature of the hot water is 50°C or higher, a high cleaning effect can be obtained.
[0081] 2.3 Process for forming the separation functional layer The separation functional layer can be obtained, for example, by forming a polyamide by polycondensation of a polyfunctional amine and a polyfunctional acid halide, as described above. Interfacial polymerization is the most preferred method of polycondensation from the viewpoint of productivity and performance. That is, the separation functional layer is preferably formed by performing interfacial polycondensation on the surface of the porous layer using an aqueous solution containing a polyfunctional amine and an organic solvent containing a polyfunctional acid halide. This process forms the polyamide. The following describes a specific process for forming a crosslinked aromatic polyamide using a polyfunctional aromatic amine as the polyfunctional amine and a polyfunctional aromatic acid chloride as the polyfunctional acid halide, but the present invention is not limited thereto.
[0082] Interfacial polymerization includes the following steps (c) and (d). Step (c) A step of bringing an aqueous solution containing a polyfunctional aromatic amine into contact with a porous layer. Step (d) is a step in which, after step (c), a solution containing a polyfunctional aromatic acid chloride is brought into contact with the porous layer.
[0083] In step (c), the concentration of the polyfunctional aromatic amine in the aqueous solution of the polyfunctional aromatic amine is preferably 0.1% by mass or more and 20% by mass or less, and preferably 0.5% by mass or more and 15% by mass or less. When the concentration of the polyfunctional aromatic amine is within the above range, sufficient solute removal performance and water permeability can be obtained.
[0084] It is preferable to apply the polyfunctional aromatic amine aqueous solution uniformly and continuously to the porous layer. Specifically, examples include coating the porous layer with the polyfunctional aromatic amine aqueous solution or immersing the porous layer in the polyfunctional aromatic amine aqueous solution. The contact time between the porous layer and the polyfunctional aromatic amine aqueous solution is preferably 1 second to 10 minutes, and more preferably 10 seconds to 3 minutes.
[0085] After contacting the porous layer with the polyfunctional aromatic amine aqueous solution, it is preferable to remove any remaining liquid droplets from the surface of the porous support. Removing the liquid can suppress the occurrence of defects in the separation functional layer. Methods for removing the liquid include, for example, holding the porous support vertically after contact with the polyfunctional aromatic amine aqueous solution to allow excess solution to flow naturally, or forcibly removing the liquid by blowing a stream of air such as nitrogen from an air nozzle. After removing the liquid, the film surface can also be dried to remove some of the water from the aqueous solution.
[0086] In step (d), the concentration of polyfunctional aromatic acid chloride in the solution is preferably 0.01% by mass or more and 10% by mass or less, and more preferably 0.02% by mass or more and 2.0% by mass or less. A sufficient reaction rate can be obtained when the concentration of polyfunctional aromatic acid chloride in the solution is 0.01% by mass or more. Furthermore, the occurrence of side reactions can be suppressed when the concentration of polyfunctional aromatic acid chloride in the solution is 10% by mass or less.
[0087] The solvent used in the solution for dissolving the polyfunctional aromatic acid chloride is preferably an organic solvent that is immiscible with water, dissolves the polyfunctional aromatic acid chloride without destroying the porous support, and is inert to the polyfunctional aromatic amine and the polyfunctional aromatic acid chloride. Preferred examples of organic solvents include hydrocarbon compounds such as n-nonane, n-decane, n-undecane, n-dodecane, isooctane, isodecane, and isododecane, or mixtures thereof.
[0088] The method for contacting a porous layer containing a polyfunctional aromatic acid chloride solution with an aqueous polyfunctional aromatic amine solution can be carried out in the same manner as the method for coating the porous layer with the aqueous polyfunctional aromatic amine solution.
[0089] After the reaction, the organic solvent is removed from the film surface. Methods for removing the organic solvent include, for example, vertically gripping the porous support and allowing excess organic solvent to drain naturally; drying the organic solvent by blowing air with a fan; or removing excess organic solvent with a water-air mixture.
[0090] 3. Methods of using composite semipermeable membranes As described above, the composite semipermeable membrane according to this embodiment is suitably used as a spiral-type separation membrane element. Furthermore, these elements can be connected in series or parallel and housed in a pressure vessel to form a separation membrane module.
[0091] Furthermore, the above-mentioned composite semipermeable membranes, separation membrane elements, and separation membrane modules can be combined with pumps that supply water to them, and devices that pre-treat the supply water to constitute a fluid separation system. By using this separation system, for example, gas separation or separation of supply water into permeate water such as drinking water and concentrated water that did not permeate the membrane can be performed to obtain water suitable for the purpose.
[0092] Examples of feedwater treated by the composite semipermeable membrane according to this embodiment include liquid mixtures containing 500 mg / L to 100 g / L of TDS (Total Dissolved Solids), such as seawater, brine, and wastewater. Generally, TDS is expressed as "mass / volume" or "mass ratio". According to the definition, it can be calculated from the mass of the residue after evaporating a solution filtered through a 0.45 micron filter at a temperature of 39.5 to 40.5°C, but a simpler method is to convert it from the practical salinity (S).
[0093] A higher operating pressure when permeating feedwater through the composite semipermeable membrane improves the solute removal rate. However, considering the increased energy required for operation and the durability of the composite semipermeable membrane, the operating pressure when permeating feedwater through the composite semipermeable membrane is preferably between 0.5 MPa and 12 MPa. As the feedwater temperature increases, the solute removal rate decreases, and as it decreases, the amount of water produced decreases. Therefore, the feedwater temperature is preferably between 5°C and 55°C.
[0094] The composite semipermeable membrane according to this embodiment allows for appropriate modification of the separation functional layer according to the solute to be removed. For example, by providing a separation functional layer containing crosslinked aromatic polyamide in the composite semipermeable membrane, it can be used as a reverse osmosis membrane for treating seawater or brine. In this case, the water production capacity retention rate of the composite semipermeable membrane, calculated by the method described in the "NaCl high pressure test" of the examples described later, is preferably 90% or higher, more preferably 93% or higher, and even more preferably 95% or higher. Furthermore, the NaCl removal rate of the composite semipermeable membrane, calculated by the method described in the "NaCl removal rate and water production capacity of the composite semipermeable membrane" of the examples described later, is preferably 99.70% or higher, more preferably 99.80% or higher, and even more preferably 99.83% or higher. Moreover, it is preferable that the water production capacity retention rate and the NaCl removal rate simultaneously satisfy the above ranges.
[0095] Furthermore, for example, by providing a separation functional layer containing a cross-linked aliphatic polyamide in the composite semipermeable membrane, it can be used as an NF membrane that separates monovalent and divalent ions. In this case, the water production retention rate of the composite semipermeable membrane, calculated by the method described in the "MgSO4 high pressure test" of the examples described later, is preferably 90% or higher, more preferably 93% or higher, and even more preferably 95% or higher. The MgSO4 removal rate of the composite semipermeable membrane, calculated by the method described in the "Removal rate and water production amount of the composite semipermeable membrane" of the examples described later, is preferably 95.0% or higher, more preferably 96.0% or higher, and even more preferably 97.0% or higher. Moreover, it is preferable that the water production retention rate and the MgSO4 removal rate simultaneously satisfy the above ranges.
[0096] Furthermore, if the pH of the supply water is high, there is a risk of scale formation, such as magnesium, in the case of supply water with high solute concentrations, such as seawater. Also, since there is a concern that filtering high-pH supply water may degrade the membrane, it is preferable that the pH of the supply water be neutral. [Examples]
[0097] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited thereto. Unless otherwise specified, the porous support was obtained by immersing a composite semipermeable membrane in a 2% by mass sodium hypochlorite aqueous solution for 48 hours and removing the separation functional layer. The substrate may be measured before the porous layer is formed, or if a porous layer is already provided on the substrate, the porous support may be immersed in a good solvent (DMF) at 60°C for 24 hours to dissolve the porous layer, replaced with pure water, dried at 120°C for 2 hours, and the substrate from which the porous layer has been removed may be measured.
[0098] <Mass of the porous layer> A porous support was cut into a rectangle measuring 0.11 m × 0.19 m, dried at 120°C for 2 hours, and its mass was measured. Additionally, masking tape (Teraoka Seisakusho P-Cut Tape No. 4140, 100 mm wide) was applied to the porous layer side of the support, and the tape was peeled off twice in the longitudinal (MD) direction to remove the porous layer from the substrate. The mass of the substrate from which the porous layer had been removed was measured, and the mass of the porous layer was calculated using the following formula (2). The same procedure was performed on five different samples, the arithmetic mean of the obtained values was calculated, and the value rounded to the first decimal place was taken as the mass of the porous layer. Mass of porous layer [g / m 2 ] = (mass of porous support - mass of substrate) / (0.11 × 0.19) ... Equation (2)
[0099] <Root mean square height of the base material Rq> The surface of the substrate forming the porous layer was observed using a laser microscope (OLYMPUS OLS4100) with a standard lens at 20x magnification. The lowest concave point was set as the lower height limit, and the highest convex point as the upper height limit, and the surface shape was measured. The observation size of the substrate was 1224 μm square. Next, the data obtained from the measurements was processed using the analysis software (application version: 3.1.1.296) included with the OLYMPUS LEXT OLS5100. Noise was removed by automatic noise reduction and tilt correction was performed. After that, "surface roughness" was selected, and "Rq" was calculated under the analysis conditions shown below. The same operation was performed on five different substrates, and the arithmetic mean of the obtained values was calculated and rounded to the second decimal place to obtain the Rq value for each substrate. [Analysis conditions] Measurement range: Entire area (1224 μm square) Filter type: Gaussian Parameters: Height / Composite Histogram class division method: 200 divisions Load area ratio for V-parameters: p=10%, q=80% Load area ratio for Sxp parameters: p=2.5%, q=50% Correlation threshold: s=0.2 Peak / valley discrimination limit: Szx=5% Smoothing settings: Smoothing is performed as a preprocessing step before calculating shape parameters. Missing Point Interpolation Setting: Calculates roughness parameters by interpolating unmeasured points.
[0100] <Percentage of recesses in the substrate> The data observed using the "root mean square height Rq of the substrate" as described above was processed using the analysis software (application version: 3.1.1.296) included with the OLYMPUS LEXT OLS5100. Automatic noise reduction and tilt correction were performed. The entire corrected image area was selected. Then, "Area / Volume" was selected, and the following analysis conditions were applied: "Depth 10 μm or more and area 500 μm". 2The number of recesses above the specified depth and the number of recesses with a depth of 10 μm or more were calculated. From the obtained data, the percentage of 10 μm recesses in the substrate was calculated using the following formula (3). The same procedure was performed on five different samples, the arithmetic mean of the obtained values was calculated, and the value rounded to the first decimal place was used as the percentage of 10 μm recesses in the substrate. Percentage of 10μm recesses [%] = (depth of 10μm or more and area of 500μm) 2 (Number of recesses above this level / Number of recesses with a depth of 10 μm or more) × 100 ... Equation (3) [Analysis conditions] Measurement range: Entire area (1224 μm square) Threshold 1: -10 μm Measure the lower limit below threshold 1 (100 μm) 2 (Exclude areas below the following size from calculations)
[0101] Also, by selecting "Area / Volume" and using the analysis conditions shown below, "Depth 20 μm or more and area 500 μm" 2 The number of recesses above and below, and the number of recesses with a depth of 20 μm or more were calculated. From the obtained data, the area of 500 μm 2 The number of recesses was calculated, and the percentage of 20 μm recesses in the substrate was calculated using the following formula (4). The same procedure was performed on five different samples, and the arithmetic mean of the obtained values was calculated and rounded to the first decimal place to determine the percentage of 20 μm recesses in the substrate. Percentage of 20μm recesses [%] = (depth 20μm or more and area 500μm) 2 (Number of recesses above this level / Number of recesses with a depth of 20 μm or more) × 100 ... Equation (4) [Analysis conditions] Measurement range: Entire area (1224 μm square) Threshold 1: -20 μm Measure the lower limit below threshold 1 (100 μm) 2 (Exclude areas below the following size from calculations)
[0102] <Average area of recesses in the substrate> The data observed using the "root mean square height Rq of the substrate" as described above was processed using the analysis software (application version: 3.1.1.296) included with the OLYMPUS LEXT OLS5100. Automatic noise reduction and tilt correction were performed. Then, "Area / Volume" was selected, and the "area of the recesses" and "number of recesses" were calculated under the analysis conditions shown below. The average area of the recesses in the substrate was calculated using equation (5) below. The same operation was performed for five different samples, and the arithmetic mean of the obtained values was calculated and rounded to the first decimal place to obtain the average area of the recesses in the substrate. Average area of concave areas [μm²] 2 ] = Total area of recesses / Number of recesses ···Equation (5) [Analysis conditions] Measurement range: Entire area (1224 μm square) Threshold 1: 0 μm Measure the lower limit below threshold 1 (100 μm) 2 (Exclude areas below the following size from calculations)
[0103] <Root mean square height Rq of the porous layer after pressurization> A composite semipermeable membrane was subjected to a 5.5 MPa operation under conditions of 5.5 MPa and 25°C, in which an aqueous solution with a NaCl concentration of 3.5 mass% and a pH of 6.5 was supplied for 2 hours. After the 5.5 MPa operation, the composite semipermeable membrane was immersed in a 2 mass% sodium hypochlorite aqueous solution for 48 hours to remove the separation functional layer and obtain a porous support. The surface of the porous layer of the obtained porous support was observed with a laser microscope (OLYMPUS OLS4100) at 20x magnification with a standard lens. The lowest concave point was set as the lower height limit and the highest convex point as the upper height limit, and the surface shape was measured. Next, the data obtained from the measurement was processed using the analysis software (application version: 3.1.1.296) included with the OLYMPUS LEXT OLS5100 to remove noise and correct the tilt using automatic noise reduction. After that, "surface roughness" was selected, and "Rq" was calculated under the analysis conditions shown below. The same procedure was performed on five different substrates, and the arithmetic mean of the obtained values was calculated and rounded to two decimal places to obtain the Rq value of the porous layer after pressurization. [Analysis conditions] Measurement range: Entire area (1224 μm square) Filter type: Gaussian Parameters: Height / Composite Histogram class division method: 200 divisions Load area ratio for V-parameters: p=10%, q=80% Load area ratio for Sxp parameters: p=2.5%, q=50% Correlation threshold: s=0.2 Peak / valley discrimination limit: Szx=5% Smoothing settings: Smoothing is performed as a preprocessing step before calculating shape parameters. Missing Point Interpolation Setting: Calculates roughness parameters by interpolating unmeasured points.
[0104] <Amount of polymer impregnation in the substrate> The mass of the substrate was measured by peeling off the porous layer with tape using the same method as described above for the "mass of the porous layer". The substrate was then immersed in a good solvent (DMF) at 60°C for 24 hours to dissolve the polymer impregnated within it. After removing the substrate from the good solvent and replacing it with pure water, it was dried at 120°C for 2 hours, and the mass of the substrate after immersion in the good solvent was measured. The amount of polymer impregnation in the substrate was calculated using the following formula (6). The same procedure was performed on five different samples, and the arithmetic mean of the obtained values was calculated and rounded to two decimal places to determine the amount of polymer impregnation in the substrate. Polymer impregnation amount of the substrate [g / m 2 ] = (Mass of substrate - Mass of substrate after immersion in good solvent) / (0.11 × 0.19) ... Equation (6)
[0105] <Thickness of the substrate and the porous layer after pressurization> After supplying an aqueous solution with a NaCl concentration of 3.5 mass% and pH 6.5 to the composite semipermeable membrane under conditions of 7.0 MPa and 45°C for 24 hours, the thickness of the composite semipermeable membrane was measured using a dial thickness gauge G-7C (manufactured by Ozaki Mfg. Co., Ltd.). At this time, since the separation functional layer is extremely thin, the thickness of the composite semipermeable membrane was regarded as the sum of the thicknesses of the substrate and the porous layer. Thereafter, the porous layer was peeled off from the substrate with a tape by the method described in the above "Mass of Porous Layer", and the thickness of the obtained substrate was measured with the dial thickness gauge G-7C. The difference between the thickness of the composite semipermeable membrane and the thickness of the substrate was defined as the thickness of the porous layer after pressurization. For each thickness, 20 randomly selected points on the same membrane surface were measured, and the value obtained by rounding the arithmetic mean to the first decimal place was used. In addition, the thickness of the substrate of the composite semipermeable membrane was measured by the same method using the composite semipermeable membrane before operation under the relevant conditions.
[0106] <NaCl removal rate and water production amount of composite semipermeable membrane> Raw water (NaCl concentration 3.2 mass%) adjusted to 25°C and pH 6.5 was supplied to the composite semipermeable membrane at an operating pressure of 5.5 MPa to perform membrane filtration treatment for 2 hours. Thereafter, the electrical conductivities of the feed water and the permeated water were measured with a multi-water quality meter (MM60R) manufactured by Toa DKK Corporation. Next, this conductivity was converted using a previously prepared calibration curve to calculate the NaCl concentration. From the obtained NaCl concentration, the NaCl removal rate, which is the solute removal performance, was determined by the following formula (7). A NaCl removal rate of 99.70% or more is considered good. NaCl removal rate [%] = 100 × {1 - (NaCl concentration in permeated water / NaCl concentration in feed water)} ··· Formula (7) In addition, after performing the above membrane filtration treatment for 2 hours, the amount of membrane permeated water over 30 minutes was measured, and converted to the daily water production amount (cubic meters) per square meter of membrane surface, the water production amount [m 3 / m 2 / day] was calculated.
[0107] <NaCl high pressure test> The composite semipermeable membrane that underwent performance evaluation in the aforementioned "NaCl removal rate and water production amount of composite semipermeable membrane" was supplied with raw water (NaCl concentration 3.2 mass%) adjusted to 45°C and pH 6.5 at an operating pressure of 7.0 MPa, and subjected to membrane filtration treatment for 6 hours. Thereafter, membrane performance evaluation was performed in the same manner as in "NaCl removal rate and water production amount of composite semipermeable membrane", and the water production amount after high-pressure operation was determined. In addition, the quality of the membrane performance was judged as good when the water production retention rate calculated by the following formula (8) was 90% or more. Water production retention rate [%] = Water production amount after high-pressure operation / Water production amount before high-pressure operation × 100 ··· Formula (8)
[0108] <MgSO4 removal rate and water production amount of composite semipermeable membrane> The composite semipermeable membrane was supplied with salt water adjusted to a temperature of 25°C, pH 6.5, and an MgSO4 concentration of 4000 mg / L at an operating pressure of 1.55 MPa, and subjected to membrane filtration treatment for 2 hours. Thereafter, the electrical conductivities of the feed water and permeated water were measured with a multi-water quality meter (MM60R) manufactured by Toa DKK Corporation. Next, using a calibration curve prepared in advance, this electrical conductivity was converted to calculate the MgSO4 concentration. From the obtained MgSO4 concentration, the MgSO4 removal rate, which is the solute removal performance, was determined by the following formula (9). An MgSO4 removal rate of 95.0% or more is considered good. MgSO4 removal rate (%) = 100 × {1 - (MgSO4 concentration in permeated water / MgSO4 concentration in feed water)} ··· Formula (9) In addition, after performing the above membrane filtration treatment for 2 hours, the amount of membrane permeated water for 30 minutes was measured, and converted to the water production amount (cubic meters) per 1 square meter of membrane surface per day, the water production amount [m 3 / m 2 / day] was calculated.
[0109] <MgSO4 high-pressure test> The composite semipermeable membrane, whose performance was evaluated in the "MgSO4 removal rate and water production volume of composite semipermeable membranes" described above, was subjected to membrane filtration treatment for 6 hours by supplying raw water (MgSO4 concentration 4.0 mass%) adjusted to 25°C and pH 6.5 at an operating pressure of 7.0 MPa. Subsequently, the membrane performance was evaluated using the same method as in "MgSO4 removal rate and water production volume of composite semipermeable membranes," and the water production volume after high-pressure operation was determined. Furthermore, the quality of the membrane performance was judged to be good if the water production volume retention rate calculated by the above formula (8) was 90% or higher.
[0110] <Manufacturing of polyester nonwoven fabric> [Reference Example 1] Polyester nonwoven fabric A The core component was a polyethylene terephthalate resin with an intrinsic viscosity (IV value) of 0.65, a melting point of 260°C, and a titanium dioxide content of 0.3% by mass. The sheath component was a copolymerized polyethylene terephthalate resin with an intrinsic viscosity (IV value) of 0.66, an isophthalic acid copolymerization rate of 11 mol%, a melting point of 230°C, and a titanium dioxide content of 0.2% by mass. The core and sheath components were melted in an extruder, weighed to a mass ratio of 80:20, and core-sheath composite fibers were spun. The spun core-sheath composite fibers were cooled and solidified in an atmosphere at room temperature (20°C), passed through a rectangular ejector, the yarn was pulled and stretched, and collected on a moving net to form a nonwoven web. Next, it was temporarily bonded using a pair of upper and lower metal calender rolls, resulting in a basis weight of 36 g / m². 2 A spunbond nonwoven web (a) was obtained. Two of the obtained spunbond nonwoven webs (a) in a temporarily bonded state were stacked on top of each other, and the laminated nonwoven web was passed between the middle and bottom of a set of three flat rolls: the top being a resin elastic roll, the middle a metal roll, and the bottom a resin elastic roll, and heat-pressed. The laminated nonwoven web was then folded back and passed between the top and middle, and heat-pressed again. Subsequently, the back side of the obtained laminated composite nonwoven fabric, which had been in contact with the elastic rolls, was brought into contact with a metal cold roll with a surface temperature of 45°C for 0.6 seconds to produce a polyester nonwoven fabric A with a thickness of 90 μm and Rq = 5.8 μm. At this time, the surface temperatures of the three flat rolls were 140°C for the top, 180°C for the middle, and 140°C for the bottom, and the linear pressure was 1715 N / cm.
[0111] [Reference Example 2] Polyester nonwoven fabric B A polyester nonwoven fabric B with a thickness of 90 μm was manufactured in the same manner as in Reference Example 1, except that the heat-sealing conditions were adjusted so that the Rq of the nonwoven fabric substrate after heat-sealing was 5.6 μm, using the spunbond nonwoven web (a) described in Reference Example 1.
[0112] [Reference Example 3] Polyester nonwoven fabric C A polyester nonwoven fabric C with a thickness of 90 μm was manufactured in the same manner as in Reference Example 1, except that the heat-sealing conditions were adjusted so that the Rq of the nonwoven fabric substrate after heat-sealing was 5.1 μm, using the spunbond nonwoven web (a) described in Reference Example 1.
[0113] [Reference Example 4] Polyester nonwoven fabric D In the spinning, nonwoven web formation, and temporary bonding process described in Reference Example 1, the basis weight is 40 g / m². 2 A spunbond nonwoven web (c) that had been temporarily bonded to the same extent as described in Reference Example 1 was laminated with the spunbond nonwoven web (a) described in Reference Example 1, and a polyester nonwoven fabric D with a thickness of 90 μm was manufactured in the same manner as in Reference Example 1, except that the heat-sealing conditions were adjusted so that the Rq of the nonwoven fabric base material after heat-sealing was 4.2 μm.
[0114] [Reference Example 5] Polyester nonwoven fabric E In the spinning, nonwoven web formation, and temporary bonding process described in Reference Example 1, the basis weight is 50 g / m². 2 A spunbond nonwoven web (d) that had been temporarily bonded to the same extent as described in Reference Example 1 was laminated with the spunbond nonwoven web (a) described in Reference Example 1, and a polyester nonwoven fabric E with a thickness of 90 μm was manufactured in the same manner as in Reference Example 1, except that the heat-sealing conditions were adjusted so that the Rq of the nonwoven fabric base material after heat-sealing was 2.8 μm.
[0115] [Reference Example 6] Polyester nonwoven fabric F A polyester nonwoven fabric F with a thickness of 90 μm was manufactured in the same manner as in Reference Example 1, except that the spunbond nonwoven web (d) described in Reference Example 5 and the spunbond nonwoven web (a) described in Reference Example 1 were laminated together, and the heat-sealing conditions were adjusted so that the Rq of the nonwoven fabric substrate after heat-sealing was 1.0 μm.
[0116] [Reference Example 7] Polyester nonwoven fabric G A polyester nonwoven fabric G with a thickness of 90 μm was manufactured in the same manner as in Reference Example 1, except that the heat-sealing conditions were adjusted so that the Rq of the nonwoven fabric substrate after heat-sealing was 7.2 μm, using the spunbond nonwoven web (a) described in Reference Example 1.
[0117] [Reference Example 8] Polyester nonwoven fabric H A polyester nonwoven fabric H with a thickness of 90 μm was manufactured in the same manner as in Reference Example 1, except that the heat-sealing conditions were adjusted so that the Rq of the nonwoven fabric substrate after heat-sealing was 7.5 μm, using the spunbond nonwoven web (b) described in Reference Example 2.
[0118] [Reference Example 9] Polyester Nonwoven Fabric I A polyester nonwoven fabric I with a thickness of 90 μm was manufactured in the same manner as in Reference Example 1, except that the heat-sealing conditions were adjusted so that the Rq of the nonwoven fabric substrate after heat-sealing was 0.1 μm, using the spunbond nonwoven web (d) described in Reference Example 5.
[0119] [Example 1] Using the polyester nonwoven fabric A obtained in Reference Example 1 as the base material, an 18% by mass DMF solution of PSf as a polymer solution was placed on the base material at 25°C, resulting in a porous layer with a mass of 10 g / m². 2 The substrate was coated in such a manner. Subsequently, the substrate coated with the polymer solution was immersed in pure water for 15 seconds to create a porous support with a porous layer formed on the substrate. The porous layer was immersed in pure water and left for 5 minutes, then washed with 90°C hot water for 2 minutes. The washed porous support was immersed in a 3 mass% aqueous solution of m-PDA for 2 minutes. The support was slowly lifted vertically, and excess aqueous solution was removed from the surface of the porous support by blowing nitrogen with an air nozzle. Then, a decane solution containing 0.165 mass% TMC was applied so that the surface of the porous layer was completely wetted, and it was left to stand for 1 minute. Furthermore, the membrane was made vertical to drain and remove excess solution, and washed with pure water to obtain a composite semipermeable membrane having a cross-linked polyamide separation functional layer. Various measurement results are shown in Table 1.
[0120] [Example 2] A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained using the same method as in Example 1, except that polyester nonwoven fabric B obtained in Reference Example 2 was used as the base material. The various measurement results are shown in Table 1.
[0121] [Example 3] The mass of the porous layer is 8 g / m 2 A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 2, except that a polymer solution was applied to achieve the desired result. The various measurement results are shown in Table 1.
[0122] [Example 4] Using the polyester nonwoven fabric C obtained in Reference Example 3 as the base material, the mass of the porous layer is 7 g / m². 2 A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 1, except that a polymer solution was applied to achieve the desired result. The various measurement results are shown in Table 1.
[0123] [Example 5] The mass of the porous layer is 5 g / m 2 A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 1, except that a polymer solution was applied to achieve the desired result. The various measurement results are shown in Table 1.
[0124] [Example 6] A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 5, except that polyester nonwoven fabric C obtained in Reference Example 1 was used as the base material. The various measurement results are shown in Table 2.
[0125] [Example 7] A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 5, except that polyester nonwoven fabric D obtained in Reference Example 4 was used as the base material. The various measurement results are shown in Table 2.
[0126] [Example 8] Using the polyester nonwoven fabric E obtained in Reference Example 5 as the base material, the mass of the porous layer is 3 g / m². 2A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 1, except that the polymer solution was applied so as to achieve this state. The results of various measurements are shown in Table 2.
[0127] [Example 9] A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 8, except that the polyester nonwoven fabric F obtained in Reference Example 6 was used as the substrate. The results of various measurements are shown in Table 2.
[0128] [Example 10] The mass of the porous layer is 13g / m 2 A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 1, except that the polymer solution was applied so as to achieve this state. The results of various measurements are shown in Table 2.
[0129] [Comparative Example 1] The mass of the porous layer is 17g / m 2 A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 1, except that the polymer solution was applied so as to achieve this state. The results of various measurements are shown in Table 3.
[0130] [Comparative Example 2] The mass of the porous layer is 14g / m 2 A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 1, except that the polymer solution was applied so as to achieve this state. The results of various measurements are shown in Table 3.
[0131] [Comparative Example 3] A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Comparative Example 2, except that the polyester nonwoven fabric G obtained in Reference Example 7 was used as the substrate. The results of various measurements are shown in Table 3.
[0132] [Comparative Example 4] A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Comparative Example 2, except that the polyester nonwoven fabric H obtained in Reference Example 8 was used as the substrate. The results of various measurements are shown in Table 3.
[0133] [Comparative Example 5] The mass of the porous layer is 2 g / m 2 A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 8, except that a polymer solution was applied to achieve the desired result. The various measurement results are shown in Table 3.
[0134] [Comparative Example 6] A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 5, except that polyester nonwoven fabric I obtained in Reference Example 9 was used as the base material. The various measurement results are shown in Table 3.
[0135] [Comparative Example 7] A composite semipermeable membrane having a crosslinked polyamide separation functional layer was obtained in the same manner as in Example 5, except that polyester nonwoven fabric H obtained in Reference Example 8 was used as the base material. The various measurement results are shown in Table 3.
[0136] [Example 11] A porous support was prepared in the same manner as in Example 1. The obtained porous support was immersed for 30 seconds in an aqueous solution containing 1.0% by mass of piperazine and 100 ppm of sodium dodecyldiphenyl ether disulfonate. The porous support was then slowly lifted vertically, and nitrogen was blown from an air nozzle to remove excess aqueous solution from the surface of the porous layer. Next, a decane solution containing 0.40% by mass of TMC was applied to the surface of the porous layer until it was completely wet, and it was left to stand for 30 seconds. After that, the film was held vertically, and the excess solution was drained off. The decane solution was then dried by blowing 25°C air using a blower. Finally, a composite semipermeable membrane with a crosslinked aliphatic polyamide separation functional layer was obtained by washing with pure water at 80°C. The results of various measurements are shown in Table 4.
[0137] [Example 12] A composite semipermeable membrane having a crosslinked aliphatic polyamide separation functional layer was obtained in the same manner as in Example 11, except that a porous support was prepared in the same manner as in Example 7. The results of various measurements are shown in Table 4.
[0138] [Comparative Example 8] A composite semipermeable membrane having a crosslinked aliphatic polyamide separation functional layer was obtained in the same manner as in Example 11, except that a porous support was prepared in the same manner as in Comparative Example 7. The various measurement results are shown in Table 4.
[0139] [Table 1]
[0140] [Table 2]
[0141] [Table 3]
[0142] [Table 4]
[0143] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the invention. This application is based on Japanese Patent Application No. 2024-168175, filed on 27 September 2024, the contents of which are incorporated herein by reference. [Industrial applicability]
[0144] The composite semipermeable membrane of the present invention can be used for seawater desalination, brine desalination, drinking water production, industrial ultrapure water production, wastewater treatment, and recovery of valuable materials. [Explanation of Symbols]
[0145] 1 Composite semipermeable membrane 2 Base material 3. Porous layer 4 Separation functional layer 5 Separation membrane element 6 End plate 7 End plate 8 Supply side channel material 9. Through sideflow road materials 10 water collection pipes 11. Water supply 12 Through water 13 Concentrated Water
Claims
1. A composite semipermeable membrane comprising a substrate, a porous layer provided on one surface of the substrate, and a separation functional layer provided on the porous layer, The mass of the porous layer is 3 g / m 2 13g / m or more 2 The following: A composite semipermeable membrane in which the root mean square height Rq of the surface of the substrate on the side where the porous layer is provided is 1.0 μm or more and 6.0 μm or less.
2. The surface of the substrate on the side where the porous layer is provided has an uneven shape, with a depth of 20 μm or more and an area of 500 μm relative to the number of recesses with a depth of 20 μm or more. 2 The composite semipermeable membrane according to claim 1, wherein the proportion of the above-mentioned recesses is 16% or less.
3. The surface of the substrate on the side where the porous layer is provided has an uneven shape, with an average area of 500 μm² for the recesses. 2 2000 μm or more 2 The composite semipermeable membrane according to claim 1 or 2, which is as follows:
4. The surface of the substrate on the side where the porous layer is provided has an uneven shape, and the number of recesses with a depth of 10 μm or more is equal to the area of a recess with a depth of 10 μm or more and an area of 500 μm. 2 The composite semipermeable membrane according to claim 1 or 2, wherein the proportion of the number of recesses is 20% or less.
5. The composite semipermeable membrane according to claim 1 or 2, wherein the root mean square height Rq of the surface of the substrate on the side where the porous layer is provided is 2.0 μm or more and 5.0 μm or less.
6. The mass of the porous layer is 3 g / m 2 10g / m or more 2 The composite semipermeable membrane according to claim 1 or 2, wherein the following applies:
7. The composite semipermeable membrane according to claim 1 or 2, wherein the root mean square height Rq of the surface of the substrate on the side where the porous layer is provided is 2.0 μm or more and 4.5 μm or less.
8. The composite semipermeable membrane according to claim 1 or 2, wherein, after supplying an aqueous solution with a NaCl concentration of 3.5% by mass and a pH of 6.5 for 2 hours under conditions of 5.5 MPa and 25°C, the root mean square height Rq of the surface of the porous layer on the side where the separation functional layer is provided is 1.0 μm or more and 2.5 μm or less.
9. The polymer impregnation amount of the base material is 0.5 g / m 2 or more and 2.5 g / m 2 or less, the composite semipermeable membrane according to claim 1 or 2.
10. A separation membrane element comprising a composite semipermeable membrane according to claim 1 or 2.
Citation Information
Patent Citations
Reverse osmosis composite membrane
JP2001252539A
Composite semipermeable membrane
JP2015089532A
Composite semipermeable membrane and manufacturing method for the same, and spiral type separation membrane
JP2016068019A
Composite semipermeable membrane