Method for improving the air stability of sulfide solid electrolytes

By forming a mercaptan coating on sulfide solid electrolytes through simultaneous spraying and drying, the method addresses air stability issues, enhancing protection against moisture and oxygen, thus facilitating commercialization.

JP7948557B2Active Publication Date: 2026-11-11SHENZHEN GUYAN NEW MATERIAL TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2025546184
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2025-04-16
Filing Date
2025-05-16
Publication Date
2026-11-11
Estimated Expiration
2045-05-16

AI Technical Summary

Technical Problem

The poor air stability of sulfide solid electrolytes prevents their commercialization due to high chemical activity leading to reactions with moisture and oxygen, producing toxic hydrogen sulfide gas and increasing manufacturing costs, and existing coating methods are complex and costly.

Method used

A method involving mixing sulfide solid electrolytes with mercaptan and solvent to form slurries, followed by simultaneous spraying and drying in an air drying device to form a protective mercaptan coating on the electrolyte surface, enhancing air stability through chemical and physical barriers.

Benefits of technology

The method forms a stable mercaptan coating that physically isolates the electrolyte from air, reducing hydrolysis and redox reactions, improving air stability and reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948557000004
    Figure 0007948557000004
  • Figure 0007948557000005
    Figure 0007948557000005
  • Figure 0007948557000006
    Figure 0007948557000006
Patent Text Reader

Abstract

The present invention belongs to the art of batteries, and more particularly to a method for improving the air stability of a sulfide solid electrolyte. The method includes the steps of forming slurry 1 by mixing a sulfide solid electrolyte with a solvent, forming slurry 2 by mixing a mercaptan with a solvent, and improving the air stability of the sulfide solid electrolyte by simultaneously spraying slurry 1 and slurry 2 into the center of a raw material mixing apparatus equipped with an air drying device, and drying them in the air drying device. The present invention simultaneously sprays a sulfide solid electrolyte and a mercaptan so that they collide with each other in a predetermined airflow. This allows for the formation of a mercaptan or complex with good stability by coordinating thiol groups in the mercaptan with metal cations or exposed sulfur voids on the surface of the sulfide solid electrolyte, and enables particle coating or partial coating of the sulfide solid electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention belongs to the field of battery technology, and more particularly to a method for improving the air stability of sulfide solid electrolytes. [Background technology]

[0002] Solid-state batteries are a key development direction for next-generation high-energy-density, high-safety energy storage devices, capable of replacing conventional liquid lithium-ion batteries. The core advantage of solid-state batteries is that, by using a solid electrolyte instead of a liquid electrolyte, the risks of flammability and leakage associated with liquid electrolytes are completely eliminated. Furthermore, because solid-state batteries can simultaneously utilize either a lithium metal negative electrode or a high-voltage positive electrode, their theoretical energy density can reach over 500 Wh / kg. In other words, the energy density of solid-state batteries is significantly higher than that of conventional liquid batteries (approximately 300 Wh / kg). Furthermore, solid-state batteries have advantages such as high mechanical stability, a cycle life of over 45,000 cycles, and fast charging and discharging (it takes about 15 minutes to fully charge), making them suitable for a wide range of applications in fields such as electric vehicles and energy storage systems.

[0003] In the field of solid-state battery technology, sulfide solid electrolytes have attracted the attention of researchers due to their extremely high ionic conductivity and excellent interface contact. Furthermore, by synthesizing sulfide solid electrolytes using either a solid-state method or a liquid-phase method, direct contact between the sulfide system and lithium metal can be achieved, significantly reducing interface impedance. However, the poor air stability of sulfide solid electrolytes has prevented their commercialization.

[0004] Therefore, it is necessary to improve and modify conventional technologies. [Overview of the project] [Problems that the invention aims to solve]

[0005] To overcome the shortcomings of conventional technologies, the object of the present invention is to provide a method for improving the air stability of sulfide solid electrolytes, thereby solving the drawback of poor air stability of conventional sulfide solid electrolytes. [Means for solving the problem]

[0006] The technical aspects of this invention are as follows: The present invention provides a method for improving the air stability of a sulfide solid electrolyte. Step S1 involves mixing a sulfide solid electrolyte and a solvent to form a slurry 1, Step S2 involves mixing mercaptan and a solvent to form slurry 2, The method includes step S3, which improves the air stability of the sulfide solid electrolyte by simultaneously spraying slurry 1 and slurry 2 into one location of a raw material mixing device equipped with an air drying device, and drying them with the air drying device.

[0007] In the exemplary embodiment of the present invention, the raw material mixing apparatus includes a reactor, two atomizers and an air drying apparatus. The two atomizers are respectively mounted on both sides of the upper portion of the reactor and are in communication with the reactor. The air drying apparatus is mounted on the upper portion of the reactor so as to feed air into the lower portion. The direction in which the atomizer sprays air is inclined relative to the vertical center line of the reactor.

[0008] In the exemplary embodiment of the present invention, the temperature of the reactor is 100 to 200°C.

[0009] In the exemplary embodiment of the present invention, a material collection container is attached to the bottom of the reactor, so that the material that has undergone a complete reaction can be easily collected.

[0010] In the exemplary embodiment of the present invention, the solvent is an aromatic hydrocarbon solvent or an ester solvent. A preferred solvent is xylene.

[0011] In the exemplary embodiment of the present invention, the solid content of Slurry 1 is 10 to 40%.

[0012] In the exemplary embodiment of the present invention, the solid content of Slurry 2 is 10 to 40%.

[0013] In the exemplary embodiment of the present invention, the particle diameter of the sulfide solid electrolyte is 400 nm to 10 μm.

[0014] In the exemplary embodiment of the present invention, the mercaptan is any one of hexanethiol, octanethiol, sec-butyl mercaptan, cyclohexyl mercaptan, n-octadecanethiol, and ethyl mercaptan.

[0015] In the exemplary embodiment of the present invention, the flow rate for spraying the Slurry 1 and the Slurry 2 is 1 to 5 m 3 / h.

[0016] In the exemplary embodiment of the present invention, the air flow rate of the air drying apparatus is 100 to 300 m 3 / h. Effects of the Invention

[0017] This invention involves simultaneously spraying a sulfide solid electrolyte and a mercaptan into a single raw material mixing device, causing the sulfide solid electrolyte and the mercaptan to collide with each other due to a predetermined airflow. This allows the thiol groups (-SH) in the mercaptan to interact with the metal cations (Li) on the surface of the sulfide solid electrolyte. + P5 + By coordinating (etc.) or exposed sulfur voids, a stable mercaptan or complex can be formed, and particle coating or partial coating of the sulfide solid electrolyte can be achieved. Furthermore, because the mercaptan molecule is hydrophobic, self-fusion of the mercaptan and the sulfide solid electrolyte can form a monolayer or nanoscale protective film on the surface of the sulfide solid electrolyte, thereby achieving the effect of physically isolating active molecules from the air.

[0018] Optimization of chemical compatibility The hydrophobic nature of mercaptans (for example, ethyl mercaptan has a solubility of only 1.5 g / 100 mL in water) reduces hydrolysis reactions caused by contact between electrolytes and water molecules. Furthermore, the good flexibility of the molecular chain improves the interface contact stability between sulfide solid electrolytes and electrode materials (e.g., lithium metal). The acidity of mercaptans (pKa ≈ 10) -10 The chemical adsorption strength of the coating layer can be enhanced by the fusion of the acid (mol / L, this acidity is stronger than that of alcoholic chemicals) with the alkaline portion of the sulfide solid electrolyte surface.

[0019] Reducible protective framework The thiol groups (-SH) in mercaptans have strong reducing properties, which allows them to react with oxidizing substances in the air (such as oxygen and water vapor) to form stable disulfides (SS fusions). For example, mercaptans react with oxygen to form peroxides or disulfides. This consumes free radicals of reactive oxygen species that cause decomposition of sulfide solid electrolytes in the air, thus reducing the PS4 in the sulfide solid electrolyte. 3- This invention can prevent redox reactions in the tetrahedral structure (e.g., the formation of Li2S and Li3P) and thus prevent the breakdown of the electrolyte structure. The mercaptan of this invention possesses reducing protective properties for sulfide solid electrolytes.

[0020] Physical barrier effect Mercaptan molecules undergo physical adsorption or chemical fusion (for example, Li on the surface of a sulfide solid electrolyte). + A dense protective layer can be formed on the surface of the electrolyte by (or by coordinating with a PS bond). The protective layer effectively blocks the penetration of moisture and oxygen, and can suppress side reactions at the interface (e.g., release of hydrogen sulfide (H2S) or growth of dendrite lithium) by the sulfide solid electrolyte absorbing moisture or undergoing oxidation. [Brief explanation of the drawing]

[0021] [Figure 1] This flowchart illustrates a method for improving the air stability of a sulfide solid electrolyte according to an embodiment of the present invention. [Figure 2] This figure shows the structure of a raw material mixing apparatus according to an embodiment of the present invention. [Figure 3] This figure shows the relationship between the specific capacity and voltage during charging and discharging of battery 1 (before processing). [Figure 4] This figure shows the relationship between the specific capacity and voltage during charging and discharging of battery 2 (after processing). [Modes for carrying out the invention]

[0022] This invention provides a method for improving the air stability of sulfide solid electrolytes. To explain the object, technical aspects, and effects of the invention in more detail and clarity, the aspects of the invention will be described in more detail below with reference to the following examples. It should be noted that the following specific examples are illustrative of the invention and do not limit it.

[0023] The poor air stability of conventional sulfide solid electrolytes is primarily due to the following two points:

[0024] The first reason is their high chemical activity. Sulfides readily react with moisture and oxygen in the air to produce toxic hydrogen sulfide (H2S) gas. This hydrogen sulfide gas not only harms human health but can also damage electrolyte structures and reduce ionic conductivity.

[0025] The second issue is that production and coating cannot be easily facilitated. Because the synthesis, processing, and assembly of the sulfides must be carried out under strict protection with an inert gas (such as argon), manufacturing costs increase significantly. For example, in one company, strictly sealing an entire production line with an output of around 100 tons with an inert gas can result in production costs per batch reaching 10,000 to 40,000 yuan / kg.

[0026] In the current industry, coating methods are frequently used to improve stability. In particular, wet coating methods are more commonly used. However, wet coating methods have drawbacks, such as being complex and costly, and making it difficult to easily manufacture large products, as molding cannot be achieved without performing multiple steps.

[0027] Therefore, in the embodiments of the present invention, a method for improving the stability of sulfide solid electrolyte air is provided. As shown in Figure 1, the method is Step S1 of forming slurry 1 by mixing a sulfide solid electrolyte and a solvent, Step S2 of forming slurry 2 by mixing mercaptan and a solvent, Step S3 of improving the air stability of the sulfide solid electrolyte by simultaneously spraying slurry 1 and slurry 2 to one location of a raw material mixing device in which an air drying device 3 is installed, and drying them with the air drying device.

[0028] Since the thiol group (-SH) in mercaptan has strong nucleophilicity, it forms a stable mercaptan or complex by coordinating with metal cations (Li + , P5 + etc.) on the surface of the sulfide solid electrolyte or exposed sulfur vacancies. The present invention can achieve the predetermined effects by appropriately designing the process flow and apparatus. Specifically, first, slurry 1 is formed by mixing a sulfide solid electrolyte and a solvent, and slurry 2 is formed by mixing mercaptan and a solvent. Next, slurry 1 and slurry 2 containing the sulfide solid electrolyte and mercaptan are respectively sprayed so that slurry 1 and slurry 2 collide with each other, and they are dried at a predetermined temperature and with an air flow. Thereby, the thiol group (-SH) in mercaptan coordinates with the metal cations (Li + , P5 + etc.) on the surface of the sulfide solid electrolyte or the exposed sulfur vacancies, so that a stable mercaptan or complex is formed, and particle coating or partial coating can be performed on the sulfide solid electrolyte.

[0029] Simultaneously, because mercaptan molecules are hydrophobic, when mercaptans come into contact with sulfide solid electrolytes, they can form a monolayer or nano-level protective film on the surface of the sulfide solid electrolyte through self-fusion. This allows for the physical isolation of active molecules from the air.

[0030] Chemical compatibility optimization The hydrophobic nature of mercaptans (for example, ethyl mercaptan has a solubility of only 1.5 g / 100 mL in water) reduces hydrolysis reactions caused by contact between electrolytes and water molecules. Furthermore, the good flexibility of the molecular chain ensures stable interface contact between the sulfide solid electrolyte and the electrode material (e.g., lithium metal). The acidity of mercaptans (pKa ≈ 10) -10 The fusion of the acid (mol / L, this acidity is stronger than that of alcoholic chemicals) with the alkaline portion of the sulfide solid electrolyte surface can enhance the chemical adsorption strength of the coating layer.

[0031] Reducibility protection framework The thiol groups (-SH) in mercaptans have strong reducing properties, which allows them to react with oxidizing substances in the air (such as oxygen and water vapor) to form stable disulfides (SS fusions). For example, mercaptans react with oxygen to form peroxides or disulfides. This consumes free radicals of active oxygen that cause decomposition of sulfide solid electrolytes in the air, thus reducing the PS4 in the sulfide solid electrolyte. 3-The mercaptan of this invention can prevent redox reactions (e.g., the formation of Li2S and Li3P) in the tetrahedral structure, thereby preventing the breakdown of the electrolyte structure. The mercaptan of this invention possesses reducing protective properties against sulfide solid electrolytes.

[0032] Physical barrier effect Mercaptan molecules undergo physical adsorption or chemical fusion (for example, Li on the surface of a sulfide solid electrolyte). + Alternatively, a dense protective layer can be formed on the surface of the electrolyte by coordinating with a PS bond. This protective layer effectively blocks the penetration of moisture and oxygen, and can suppress side reactions at the interface (e.g., release of hydrogen sulfide (H2S) or growth of lithium dendrites) by preventing the sulfide solid electrolyte from absorbing moisture or undergoing oxidation.

[0033] In an embodiment of the present invention, as shown in Figure 2, the raw material mixing apparatus includes a reactor 1 and a sprayer 2 that is attached to the top of the reactor 1 and is in communication with the reactor 1. The air drying apparatus 3 is attached to the top of the reactor 1 to supply air downwards. The sprayer 2 is attached to spray air in an inclined direction.

[0034] In the embodiments of the present invention, the raw materials can be rapidly dried by a sprayer causing a high-speed collision reaction between the sulfide solid electrolyte and the mercaptan in the reactor 1. Furthermore, when the mercaptan and the sulfide solid electrolyte come into contact, a monolayer or nanoscale protective film can be formed on the surface of the sulfide solid electrolyte by self-fusion. This makes it possible to achieve the effect of physically isolating active molecules from the air.

[0035] In embodiments of the present invention, the temperature of the reactor 1 can be 100 to 200°C. For example, it can be 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, or other temperatures.

[0036] Because the overall volume of the reactor is large, temperature control zones of a predetermined length (for example, an upper temperature control zone and a lower temperature control zone) can be installed vertically in the reactor to equalize the temperature inside the reactor. This makes it possible to make the temperature of the upper temperature control zone and the lower temperature control zone the same.

[0037] In the embodiment of the present invention, a substance collection container 4 is attached to the bottom of the reactor 1, allowing for easy collection of the substance after a complete reaction.

[0038] In the embodiments of the present invention, the solvent is an aromatic hydrocarbon solvent or an ester solvent. Preferred aromatic hydrocarbon solvents are toluene, ethylbenzene, or naphtha solvent. Preferred ester solvents are ethyl acetate, butyl acetate, or isoamyl acetate.

[0039] In the embodiments of the present invention, the solid content of slurry 1 can be 10 to 40%. For example, the solid content of slurry 1 can be 10%, 20%, 30%, 40%, or any of these ranges.

[0040] In embodiments of the present invention, the solid content of slurry 2 can be 10-40%. For example, the solid content of slurry 2 can be 10%, 20%, 30%, 40%, or any of these ranges. If the solid content is too low, a large amount of solvent will need to be used, which may lead to contamination problems and increased costs. If the solid content is too high, the raw material outlet of the sprayer may easily become clogged, which may affect subsequent processes.

[0041] In embodiments of the present invention, the sulfide solid electrolyte is Li7P2S8X, where X is Cl, Br, I and / or F, or Li3PS4, or Li 10 It can be GeP2S12. Li is preferred. 5.5 PS 4.5 Cl 1.5 (The name of this chemical is lithium phosphorus sulfur chloride, and its abbreviation is LPSC.)

[0042] In embodiments of the present invention, the particle diameter of the sulfide solid electrolyte can be 400 nm to 10 μm. Preferred particle diameters can be 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, or any particle diameter within the above range. The method of the present invention can be used for sulfide solid electrolytes having various particle diameters. That is, by treating a sulfide solid electrolyte having a particle diameter of 400 nm or a sulfide solid electrolyte having a particle diameter of 10 μm with the method of the present invention, the air stability of the sulfide solid electrolyte can be improved. Since sulfide solid electrolytes with smaller particle diameters absorb water more easily, improving the air stability of sulfide solid electrolytes with smaller particle diameters can broaden the value and prospects of applications for sulfide solid electrolytes and gain greater significance.

[0043] In the examples of the present invention, mercaptan refers to a non-aromatic compound containing a thiol functional group (-SH). The mercaptan in these examples can be any one of the following: hexanethiol, octanethiol, sec-butyl mercaptan, cyclohexyl mercaptan, n-octadecanethiol, or ethyl mercaptan.

[0044] In the embodiments of the present invention, the flow velocity for spraying slurry 1 and slurry 2 is 1 to 5 m / s. 3 The preferred flow velocity is 1 m / h. 3 / h, 1.5m 3 / h, 2m 3 / h, 2.5m 3 / h, 3m 3 / h, 3.5m 3 / h, 4m 3 / h, 5m 3 The flow rate is / h. If the spray velocity is too low, the raw materials are sprayed too slowly, causing the slurry to settle before it is sprayed. This can result in an uneven distribution of solids in the spray, potentially reducing the effectiveness of the coating. If the spray velocity is too high, the raw materials are sprayed too quickly, preventing the two raw materials from making complete contact. Unless the temperature is properly adjusted, the raw materials may not dry completely.

[0045] In the embodiment of the present invention, the airflow rate of the air drying apparatus is 100 to 300 m³. 3 The preferred airflow rate is 100 m / h. 3 / h, 150m 3 / h, 200m 3 / h, 250m 3 / h, 300m 3The wind speed is / h. If the wind speed is too low, the raw materials cannot come into even contact with each other, and the reaction cannot proceed sufficiently. If the wind speed is too high, the raw materials will be blown away before they can react, so they cannot react sufficiently.

[0046] The aspects of the present invention will be described in more detail below with reference to specific examples.

[0047] Example 1 The method for improving the air stability of the sulfide solid electrolyte in this embodiment is: A step of forming a slurry 1 by mixing a sulfide solid electrolyte (LPSC) and a solvent (xylene), wherein the solid content of the slurry 1 is 20%. A step of forming slurry 2 by mixing mercaptan (hexanethiol) and solvent (xylene), wherein the solid content of slurry 2 is 20%. The method includes the step of simultaneously spraying slurry 1 and slurry 2 into the center of a raw material mixing device equipped with an air drying device 3, and drying them in the air drying device 3 to improve the air stability of the sulfide solid electrolyte.

[0048] As shown in Figure 2, the raw material mixing apparatus includes a reactor 1, two sprayers 2, and an air drying device 3. The two sprayers 2 are mounted on both sides of the top of the reactor 1 and are in communication with the reactor 1. The air drying device 3 is mounted on the top of the reactor 1 to supply air downwards. The direction in which the sprayers 2 spray air is inclined relative to the vertical centerline of the reactor 1.

[0049] The temperature of reactor 1 is 120°C.

[0050] A substance collection container 4 for collecting substances is attached to the bottom of the reactor 1.

[0051] The particle diameter of the sulfide solid electrolyte is 500 nm.

[0052] The flow velocity for spraying slurry 1 and slurry 2 is 2.5 m / s. 3 It is / h.

[0053] The airflow rate of the air drying device 3 is 200 m³. 3 It is / h.

[0054] Example 2 The difference between Example 2 and Example 1 is that the temperature of reactor 1 is 100°C.

[0055] Example 3 The difference between Example 3 and Example 1 is that the temperature of reactor 1 is 140°C.

[0056] Example 4 The difference between Example 4 and Example 1 is that the temperature of reactor 1 is 160°C.

[0057] Performance measurement 1. Before processing, measure the charging capacity, discharge capacity, and ICE (Initial Coulombic Efficiency) of Example 1.

[0058] A sample of sulfide solid electrolyte (LPSC) whose performance is not improved by the method according to the embodiment of the present invention will be referred to as the LPSC before treatment.

[0059] A compressed sheet is manufactured from powder. By compressing the sulfide solid electrolyte before treatment and the sulfide solid electrolyte treated by the method of Example 1, a compressed sheet before LPSC treatment and the compressed sheet of Example 1 are manufactured. When manufacturing the compressed sheet, the raw material is compressed at a pressure of 400 MPa to produce a compressed sheet with a thickness of approximately 0.5 mm and a diameter of 10 mm. By ensuring the tightness of the compressed sheet (porosity ≤ 5%) and applying force evenly to the compressed sheet, it is possible to avoid the compressed sheet tearing or the formation of indentation defects, and to avoid affecting the measurement results. Next, the 811 cathode material (the 811 cathode material refers to a high nickel ternary material in which the chemical composition ratio of the cathode material in a nickel-cobalt-manganese ternary lithium-ion battery is nickel (Ni):cobalt (Co):manganese (Mn) = 8:1:1. Its chemical formula is LiNi 0.8 Co 0.1 Mn 0.1 Compressed sheets of 811 cathode material and graphite anode material are manufactured by compressing O2 (which is O2) and graphite anode material at a pressure of 300 MPa.

[0060] Battery 1 (before processing) and Battery 2 (after processing) are manufactured by compressing two sets of batteries at a pressure of 4 MPa: one set consisting of a compressed sheet of 811 positive electrode material, a compressed sheet before LPSC processing, and a compressed sheet of graphite negative electrode material, and another set consisting of a compressed sheet of 811 positive electrode material, a compressed sheet from Example 1, and a compressed sheet of graphite negative electrode material. Next, the batteries are sent into a battery cabinet for measurement. In both cases, a constant current charging and discharging method at 0.1C is used as the measurement program. Figure 3 shows the relationship between the specific capacity and voltage during charging and discharging of Battery 1 (before processing), Figure 4 shows the relationship between the specific capacity and voltage during charging and discharging of Battery 2 (after processing), and Table 1 shows the measurement results of the charging capacity, discharging capacity, and ICE of Battery 1 (before processing) and Battery 2 (after processing). As shown in Figures 3, 4 and Table 1, the method according to the embodiment of the present invention does not have a significant effect on the charging and discharging of the sulfide solid electrolyte and the ICE. The measurement results for the charge capacity, discharge capacity, and ICE of batteries manufactured in other embodiments are similar to those of Embodiment 1. This means that the method according to the embodiments of the present invention does not have a significant effect on the charge / discharge and ICE of the sulfide solid electrolyte.

[0061] Table 1. Measurement results of charge capacity, discharge capacity, and ICE for Battery 1 (before treatment) and Battery 2 (after treatment). [Table 1]

[0062] 2. Air Stability Measurement Multiple powder materials before LPSC treatment (comparison set) and multiple powder materials after LPSC treatment according to Examples 1-4 were placed in an experiment box with a humidity of 5%, and the ionic conductivity of the specified powder materials was measured at various time points (1h, 2h, 3h, 4h, 8h, 18h, 24h).

[0063] The specific measurement methods include sample preparation, electrochemical impedance measurement, and geometric parameter measurement. Sample manufacturing Compressed sheets are manufactured by compressing the powder materials of the comparison sets at various time points, and the powder materials that have undergone LPSC treatment according to Examples 1 to 4, at a pressure of 400 MPa. The thickness of the compressed sheet is approximately 0.5 mm, and the diameter is 10 mm. Next, the thickness of the compressed sheet of sulfide solid electrolyte is measured using a micrometer.

[0064] Electrochemical impedance survey (EIS) The sample is held between blocking electrodes (e.g., stainless steel, sputtering metal film), and an AC voltage (with an amplitude of 10 mV and a frequency range of 1 MHz to 0.1 Hz) is applied.

[0065] By fitting a semicircular intercept in the high-frequency region using EIS, the body phase resistance (R) is increased. bulk It acquires body phase resistance, and in the low-frequency region, it exhibits interface resistance and the electrical double layer effect.

[0066] Geometrical parameter measurement Thickness (L): Measure the thickness of the compressed sheet directly using a micrometer. Area (A): The effective contact area is calculated based on the diameter of the electrode.

number

[0067] Table 2 shows the results of calculating the ionic conductivity of a given material using formula (1). As shown in Table 2, when a comparison set (before LPSC treatment) that was not treated in Examples 1-4 of the present invention is left for 18 hours, the raw materials are almost completely insulated. Compared with the comparison set (before LPSC treatment), the initial ionic conductivity of the raw materials treated in Examples 1-4 of the present invention decreases. The shorter the time of exposure to air, the more significantly the ionic conductivity of the LPSCs in Examples 1-4 of the present invention exceeds that of conventional technologies. Even after leaving the raw material of Example 1 of the present invention for 24 hours, it can still maintain an ionic conductivity of 1.885 mS / cm. This means that the air stability of sulfide solid electrolytes can be improved by the method according to the examples of the present invention.

[0068] Table 2 Conductivity when the air stability of each example and comparison set differs [Table 2]

[0069] As described above, the method for improving the air stability of sulfide solid electrolytes according to the embodiments of the present invention can improve the air stability of sulfide solid electrolytes, and therefore can play a role in commercializing the product.

[0070] Although the aspects of the present invention have been described in detail above with reference to preferred embodiments, these preferred embodiments are merely illustrative examples of the present invention, and therefore the present invention is not limited to these embodiments. Persons skilled in the art can make design changes, improvements, etc., within the scope that does not depart from the technical aspects and the gist of the invention, and such design changes, improvements, etc., will naturally still be included within the scope of the claims of the present invention.

Claims

1. The process involves forming a slurry 1 by mixing a sulfide solid electrolyte with a solvent, The process involves a step of forming slurry 2 by mixing mercaptan and a solvent, The method includes the step of simultaneously spraying slurry 1 and slurry 2 into one location of a raw material mixing apparatus equipped with an air drying device (3) so that the sulfide solid electrolyte and mercaptan collide with each other, and drying them in the air drying device (3) to improve the air stability of the sulfide solid electrolyte, The raw material mixing apparatus includes a reactor (1), two sprayers (2), and an air drying device (3), wherein the two sprayers (2) are mounted on both sides of the top of the reactor (1) and are in communication with the reactor (1), the air drying device (3) is mounted on the top of the reactor (1) to supply air downwards, and the direction in which the sprayers (2) spray air is inclined relative to the vertical centerline of the reactor (1). The flow rate for spraying slurry 1 and slurry 2 is 1 to 5 m³ / h. The airflow rate of the aforementioned air drying apparatus is 100 to 300 m³ / h. A method for improving the air stability of a sulfide solid electrolyte, characterized by the features described above.

2. The method for improving the air stability of a sulfide solid electrolyte according to claim 1, characterized in that the temperature of the reactor (1) is 100 to 200°C.

3. The method for improving the air stability of a sulfide solid electrolyte according to claim 1, characterized in that a substance collection container (4) for collecting substances is attached to the bottom of the reactor (1).

4. The method for improving the air stability of a sulfide solid electrolyte according to claim 1, characterized in that the solvent is an aromatic hydrocarbon solvent or an ester solvent.

5. The method for improving the air stability of a sulfide solid electrolyte according to claim 1, characterized in that the solid content of the slurry 1 is 10 to 40%, and the mercaptan content of the slurry 2 is 10 to 40%.

6. The method for improving the air stability of a sulfide solid electrolyte according to claim 1, characterized in that the particle diameter of the sulfide solid electrolyte is 400 nm to 10 μm.

7. The method for improving the air stability of a sulfide solid electrolyte according to claim 1, characterized in that the mercaptan is one of hexanethiol, octanthiol, sebutyl mercaptan, cyclohexyl mercaptan, n-octadecanethiol, and ethyl mercaptan.

Citation Information

Patent Citations

  • Method for processing active materials used in secondary electrochemical cells

    JP2010503606A

  • Manufacturing method for solid electrolyte sheet

    JP2011054327A

  • Organic coating for sulfide-containing solid electrolyte material, solid electrolyte and solid state battery containing the same

    US20240405259A1

  • Solid electrolyte producing method

    WO2021230189A1

  • Method for producing sulfide solid electrolyte

    WO2024158030A1