Film deposition method and film deposition apparatus
The method enhances the density and uniformity of self-assembled monolayers on substrates with different materials by alternating gas supplies, addressing film formation challenges and improving blocking performance and reducing surface roughness.
Patent Information
- Application Number
- JP2022153617
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-09-27
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-09-27
AI Technical Summary
Existing film forming methods using Self-Assembled Monolayers (SAMs) face challenges in achieving high density and uniformity, particularly when forming films on substrates with different materials, leading to issues with film formation and blocking performance.
A method involving the selective formation of a self-assembled monolayer on specific substrate surfaces by alternating supplies of organic compound and oxygen-containing gases, followed by controlled film deposition and etching to enhance density and uniformity.
Improves the density and uniformity of the self-assembled monolayer, allowing precise film formation and reduced surface roughness, thereby enhancing the blocking performance and reducing wiring resistance.
Smart Images

Figure 0007948716000006 
Figure 0007948716000007 
Figure 0007948716000008
Abstract
Description
Technical Field
[0001] The present disclosure relates to a film forming method and a film forming apparatus.
Background Art
[0002] Patent Document 1 describes a film forming method that uses a Self-Assembled Monolayer (SAM) to inhibit the formation of a target film on a part of the substrate surface while forming the target film on another part of the substrate surface. The film forming method described in Patent Document 1 includes reducing a natural oxide film formed on the surface of a first material layer before forming the SAM on the surface of the first material layer, and oxidizing the surface of the first material layer.
Prior Art Documents
Patent Documents
[0003]
Patent Document 1
Summary of the Invention
Problem to be Solved by the Invention
[0004] One aspect of the present disclosure provides a technique for improving the density of a self-assembled monolayer.
Means for Solving the Problem
[0005] A film forming method according to one aspect of the present invention is The method includes: preparing a substrate having a first film and a second film formed of a different material from the first film in different regions of its surface; selectively forming a self-assembled monolayer on the surface of the second film relative to the surface of the first film by supplying an organic compound gas and an oxygen-containing gas that does not contain OH groups into a processing container containing the substrate; and forming the target film on the surface of the first film while inhibiting the formation of the target film on the surface of the second film using the self-assembled monolayer. Before forming the target film, the self-assembled monolayer is formed by repeatedly supplying the organic compound gas and the oxygen-containing gas that does not contain OH groups alternately multiple times into the processing container.
Effects of the Invention
[0006] According to one aspect of the present disclosure, the density of the self-assembled monolayer is improved.
Brief Description of the Drawings
[0007] [Figure 1] Figure 1 is a flowchart showing a film forming method according to an embodiment. [Figure 2] Figure 2(A) shows step S1 according to one embodiment, Figure 2(B) shows step S2 according to one embodiment, Figure 2(C) shows step S3 according to one embodiment, Figure 2(D) shows step S4 according to one embodiment, Figure 2(E) shows step S5 according to one embodiment, and Figure 2(F) shows step S6 according to one embodiment. [Figure 3] Figure 3 is a flowchart showing an example of the subroutine in step S4. [Figure 4] Figure 4 is a flowchart showing an example of the subroutine in step S5. [Figure 5] Figure 5 is a flowchart showing an example of the subroutine in step S6. [Figure 6] Figure 6(A) shows step S1 of the first modified example, Figure 6(B) shows step S2 of the first modified example, Figure 6(C) shows step S3 of the first modified example, Figure 6(D) shows step S4 of the first modified example, Figure 6(E) shows step S5 of the first modified example, and Figure 6(F) shows step S6 of the first modified example. [Figure 7] Figure 7(A) shows step S1 of the second modified example, Figure 7(B) shows step S2 of the second modified example, Figure 7(C) shows step S3 of the second modified example, Figure 7(D) shows step S4 of the second modified example, Figure 7(E) shows step S5 of the second modified example, and Figure 7(F) shows step S6 of the second modified example. [Figure 8] Figure 8 is a plan view showing a film deposition apparatus according to one embodiment. [Figure 9] Figure 9 is a cross-sectional view showing an example of the first processing unit shown in Figure 8. [Figure 10] Figure 10 shows the XPS spectra of the substrate surface obtained in Examples 2-1 to 2-3. [Modes for carrying out the invention]
[0008] Embodiments of this disclosure will be described below with reference to the drawings. In each drawing, the same or corresponding components are denoted by the same reference numerals, and their descriptions may be omitted.
[0009] A film deposition method according to one embodiment will be described with reference to Figures 1 and 2. The film deposition method includes, for example, steps S1 to S7 shown in Figure 1. However, the film deposition method only needs to include steps S1 and S4, and does not need to include, for example, steps S2 to S3 and S5 to S7. Furthermore, the film deposition method may include steps other than steps S1 to S7 shown in Figure 1.
[0010] Step S1 in Figure 1 includes preparing the substrate 1 as shown in Figure 2(A). The substrate 1 has a base substrate 10. The base substrate 10 is, for example, a silicon wafer, a compound semiconductor wafer, or a glass substrate. The substrate 1 has an insulating film 11 and a conductive film 12 in different regions of the substrate surface 1a. The substrate surface 1a is, for example, the top surface of the substrate 1. The insulating film 11 and the conductive film 12 are formed on the base substrate 10. Another functional film may be formed between the base substrate 10 and the insulating film 11, or between the base substrate 10 and the conductive film 12. The insulating film 11 is an example of a first film, and the conductive film 12 is an example of a second film. The materials of the first film and the second film are not particularly limited.
[0011] The insulating film 11 is, for example, an interlayer insulating film. The interlayer insulating film is preferably a low-dielectric constant (Low-k) film. The insulating film 11 is not particularly limited, but is, for example, an SiO film, a SiN film, a SiOC film, a SiON film, or a SiCN film. Here, an SiO film means a film containing silicon (Si) and oxygen (O). The atomic ratio of Si to O in an SiO film is usually 1:2, but the atomic ratio of Si to O in the SiO film in this application is not limited to 1:2. The same applies to SiN films, SiOC films, SiON films, and SiCN films. The insulating film 11 has recesses on the substrate surface 1a. The recesses are trenches, contact holes, or via holes.
[0012] The conductive film 12 is filled into, for example, the recess of the insulating film 11. The conductive film 12 is, for example, a metal film. The metal film is, for example, a Cu film, a Co film, a Ru film, or a W film. Note that the conductive film 12 may be a cap film. That is, as shown in FIG. 7(A), the second conductive film 15 may be embedded in the recess of the insulating film 11, and the conductive film 12 may cover the second conductive film 15. The second conductive film 15 is formed of a metal different from that of the conductive film 12.
[0013] The substrate 1 may further have a third film on the substrate surface 1a. The third film is, for example, a barrier film 13. The barrier film 13 is formed between the insulating film 11 and the conductive film 12, and suppresses metal diffusion from the conductive film 12 to the insulating film 11. The barrier film 13 is not particularly limited, and is, for example, a TaN film or a TiN film. Here, the TaN film means a film containing tantalum (Ta) and nitrogen (N). The atomic ratio of Ta to N in the TaN film is not limited to 1:1. The same applies to the TiN film.
[0014] Table 1 collectively shows specific examples of the insulating film 11, the conductive film 12, and the barrier film 13.
[0015]
Table 1
[0016] Note that the combination of the insulating film 11, the conductive film 12, and the barrier film 13 is not particularly limited.
[0017] As shown in FIG. 2(A), contaminants 22 may be present on the surface of the conductive film 12. The contaminants 22 include, for example, at least one of a metal oxide and an organic substance. The metal oxide is an oxide formed by the reaction between the conductive film 12 and the atmosphere, and is a so-called natural oxide film. The organic substance adheres during the processing of the substrate 1. Although not shown, contaminants such as organic substances may also be present on the surface of the insulating film 11 and the surface of the barrier film 13.
[0018] Step S2 in Figure 1 includes removing contaminants 22, as shown in Figure 2(B). This exposes the surface of the conductive film 12. For example, step S2 includes supplying a cleaning gas to the substrate surface 1a. The cleaning gas may be plasma-generated to improve the efficiency of removing contaminants 22. The cleaning gas includes a reducing gas, such as H2 gas. The reducing gas removes oxides such as native oxide films. In addition to the reducing gas, the cleaning gas may also include N2 gas to remove organic matter.
[0019] An example of the processing conditions for step S2 is shown below. H2 gas flow rate: 50 sccm to 5000 sccm N2 gas flow rate: 50 sccm to 10000 sccm Ar gas flow rate: 20 sccm to 10000 sccm Percentage of H2 gas in the cleaning gas: 10% to 60% by volume Percentage of N2 gas in the cleaning gas: 10% to 80% by volume Power supply frequency for plasma generation: 10MHz~40MHz Power for plasma generation: 100W~400W Processing time: 5 sec to 120 sec Processing temperature (substrate temperature): 80℃~350℃ Processing pressure: 50 Pa to 2000 Pa.
[0020] Step S3 in Figure 1 includes forming an oxide film 32 by oxidizing the surface of the conductive film 12, as shown in Figure 2(C). For example, step S3 includes forming the oxide film 32 by supplying an oxygen-containing gas to the substrate surface 1a. The oxygen-containing gas includes at least one gas that does not contain OH groups, such as O2 gas, O3 gas, NO gas, NO2 gas, and N2O gas. Note that the surface oxidation of the conductive film 12 may be a wet process rather than a dry process.
[0021] Since the contaminants 22 are removed before step S3, step S3 yields an oxide film 32 having the desired film thickness and film quality. Film quality includes the surface state of the film. Unlike native oxide films, the film thickness and film quality of the oxide film 32 can be controlled by the source gas and deposition conditions. By forming an oxide film 32 having the desired film thickness and film quality, a dense self-assembled monolayer (SAM) can be formed on the surface of the conductive film 12 in step S4 described later.
[0022] An example of the processing conditions for step S3 is shown below. O2 gas flow rate: 50 sccm to 4000 sccm Processing time: 1 sec to 300 sec Processing temperature: 80℃~350℃ Processing pressure: 50 Pa to 2000 Pa.
[0023] Step S4 in Figure 1 involves supplying an organic compound gas and an oxygen-containing gas into a processing vessel containing the substrate 1 (for example, the processing vessel 210 in Figure 9) to selectively form SAM 17 on the surface of the conductive film 12 relative to the surface of the insulating film 11, as shown in Figure 2(D). The organic compound gas is the raw material for SAM 17. The organic compound gas is not particularly limited, but for example, it is a thiol compound.
[0024] Thiol compounds have a hydrogenated sulfur group as their head group and are represented by the general formula "R-SH". R is, for example, a hydrocarbon group, or a hydrocarbon group in which at least some of the hydrogen atoms are replaced with fluorine. Specific examples of thiol compounds include CF3(CF2)5CH2CH2SH (1H,1H,2H,2H-perfluorooctanethiol: PFOT) and CF3(CF2)7CH2CH2SH (1H,1H,2H,2H-perfluorodecanethiol: PFDT).
[0025] Thiol compounds are more readily chemiadsorbed onto the surface of the conductive film 12 than onto the surface of the insulating film 11. Therefore, SAM 17 is selectively formed on the surface of the conductive film 12 compared to the surface of the insulating film 11. If the oxide film 32 is formed before the formation of SAM 17, the density of SAM 17 can be improved compared to when the oxide film 32 is not formed, and the blocking performance of SAM 17 can be improved in step S5 described later. Since the thiol compounds are chemiadsorbed while reducing the oxide film 32, the oxide film 32 does not need to remain after step S4 (see Figures 2(D), 6(D), and 7(D)).
[0026] Thiol compounds are more readily chemisorbed onto the barrier film 13 than onto the insulating film 11. Therefore, SAM 17 is selectively formed on the surface of the barrier film 13. Furthermore, thiol compounds are more readily chemisorbed onto the surface of the conductive film 12 than onto the surface of the barrier film 13, and SAM 17 is more likely to form on the surface of the conductive film 12 than on the surface of the barrier film 13.
[0027] Furthermore, the raw materials for SAM17 are not limited to thiol compounds. For example, the raw materials for SAM17 may also be phosphonic acid compounds. Phosphonic acid compounds are represented by the general formula "RP(=O)(OH)2". R is, for example, a hydrocarbon group, or a hydrocarbon group in which at least some of the hydrogen atoms are replaced with fluorine.
[0028] Step S4 in Figure 1 includes, for example, steps S41 to S43 shown in Figure 3. Step S41 includes supplying an oxygen-containing gas that does not contain OH groups into the processing container that houses the substrate 1. Step S42 includes supplying an organic compound gas into the processing container. Note that the order of steps S41 and S42 may be reversed.
[0029] By performing steps S41 and S42 alternately, while oxygen-containing gas is supplied to the processing container in step S41, organic compound gas can be stored in an external tank, and then supplied from the external tank to the processing container in step S42. This is effective when the vapor pressure of the organic compound is low and it takes time to secure a sufficient amount of organic compound gas.
[0030] Step S43 includes checking whether steps S41 to S42 have been performed the set number of times. If the number of executions has not reached the set number (step S43, NO), the density of SAM17 is insufficient, so steps S41 to S42 are performed again. On the other hand, if the number of executions has reached the set number (step S43, YES), the density of SAM17 is sufficient, so the current process is terminated.
[0031] In this embodiment, as shown in Figure 3, the supply of oxygen-containing gas and the supply of organic compound gas are carried out sequentially, not simultaneously, but may be carried out simultaneously. In any case, the conductive film 12 can be oxidized by supplying oxygen-containing gas. The oxidation of the conductive film 12 can be carried out dispersedly in steps S3 and S4.
[0032] According to this embodiment, the oxidation of the conductive film 12 can be carried out in a dispersed manner in steps S3 and S4. Dispersive oxidation of the conductive film 12 can also be carried out by repeatedly performing steps S41 and S42 multiple times. Compared to the case in which an oxide film 32 of sufficient thickness to form a dense SAM 17 is formed all at once in step S3, surface roughness of the conductive film 12 due to oxidation can be suppressed. Therefore, it is possible to achieve both suppression of surface roughness on the substrate surface and improvement of the density of the SAM 17.
[0033] The oxygen-containing gas used in step S4, like the oxygen-containing gas used in step S3, includes at least one gas that does not contain OH groups, such as O2 gas, O3 gas, NO gas, NO2 gas, and N2O gas. When using a gas containing OH groups, such as H2O, as the oxygen-containing gas, it is difficult to form a uniform oxide film on the surface of the conductive film 12 with good controllability. The oxide film may be too thin or uneven. Furthermore, H2O tends to remain on the inner wall surface of the processing container or the substrate surface 1a, and depending on the type of SAM 17, it may inhibit the adsorption of SAM 17 to the conductive film 12.
[0034] The number of times step S43 is set may be once, but it is preferable to set it multiple times. By repeatedly supplying oxygen-containing gas and organic compound gas in sequence, the oxidation of the conductive film 12 can be gradually advanced, and surface roughening of the conductive film 12 due to oxidation can be further suppressed. The number of times step S43 is set is, for example, 2 to 15.
[0035] An example of the processing conditions for step S4 is shown below. Step S41 O2 gas flow rate: 100 sccm to 4000 sccm Processing time: 3 sec to 120 sec Step S42 PFOT gas flow rate: 50 sccm~200 sccm Processing time: 3 sec to 120 sec • Common processing conditions for steps S41 to S42 Processing temperature: 80℃~250℃ Processing pressure: 50 Pa to 4000 Pa.
[0036] Step S5 in Figure 1 includes forming the target film 18 on the surface of the insulating film 11 while inhibiting the formation of the target film 18 on the surface of the conductive film 12 using the SAM 17, as shown in Figure 2(E). The target film 18 is, for example, an insulating film and is formed on the insulating film 11. According to this embodiment, the SAM 17 has a high density, so the blocking performance of the SAM 17 is good.
[0037] As described above, SAM17 is formed not only on the surface of the conductive film 12 but also on the surface of the barrier film 13. In this case, step S5 may also include forming the target film 18 on the surface of the insulating film 11 while using SAM17 to inhibit the formation of the target film 18 on the surface of the conductive film 12 and the surface of the barrier film 13. Note that the blocking performance of SAM17 is not perfect, and the target film 18 may extend laterally from the surface of the insulating film 11 and cover the surface of the barrier film 13.
[0038] The target film 18 is not particularly limited, but examples include AlO films, SiO films, SiN films, ZrO films, or HfO films. Here, an AlO film means a film containing aluminum (Al) and oxygen (O). The atomic ratio of Al to O in an AlO film is usually 2:3, but the atomic ratio of Al to O in the AlO film in this application is not limited to 2:3. The same applies to SiO films, SiN films, ZrO films, and HfO films. The target film 18 is formed by the CVD (Chemical Vapor Deposition) method or the ALD (Atomic Layer Deposition) method.
[0039] When forming an AlO film by the ALD method, an Al-containing gas such as TMA (trimethylaluminum) gas and an oxidizing gas such as water vapor (H2O gas) are alternately supplied to the substrate surface 1a. The AlO film deposition method includes, for example, steps S51 to S55 shown in Figure 4.
[0040] Step S51 includes supplying an Al-containing gas to the substrate surface 1a. Step S52 includes supplying an inert gas such as Ar gas to the substrate surface 1a and purging any excess Al-containing gas that was not adsorbed on the substrate surface 1a. Step S53 includes supplying an oxidizing gas to the substrate surface 1a. Step S54 includes supplying an inert gas such as Ar gas to the substrate surface 1a and purging any excess oxidizing gas that was not adsorbed on the substrate surface 1a. Note that the order of steps S51 and S53 may be reversed.
[0041] Step S55 includes checking whether steps S51 to S54 have been performed the set number of times. If the number of executions has not reached the set number (step S55, NO), steps S51 to S54 are performed again. On the other hand, if the number of executions has reached the set number (step S55, YES), the AlO film thickness has reached the target thickness, and the process is terminated. The set number of executions in step S55 is set according to the target thickness of the AlO film, for example, between 10 and 100 times.
[0042] An example of the processing conditions for step S5 is shown below. Step S51 TMA gas flow rate: 10 sccm~100 sccm Processing time: 0.05 sec to 10 sec Step S52 Ar gas flow rate: 1000 sccm to 8000 sccm Processing time: 0.5 sec to 10 sec Step S53 H2O gas flow rate: 50 sccm to 500 sccm Processing time: 0.1 sec to 10 sec Step S54 Ar gas flow rate: 1000 sccm to 8000 sccm Processing time: 0.5 sec to 10 sec • Common processing conditions for steps S51 to S54 Processing temperature: 100℃~350℃ Processing pressure: 133 Pa to 1200 Pa.
[0043] Incidentally, as shown in Figure 2(E), SAM17 inhibits the formation of the target film 18, but the blocking performance of SAM17 is not perfect, and the target film 18 protrudes laterally from the surface of the insulating film 11. The width W of this protruding portion, that is, the unwanted portion, is, for example, about 2 nm to 10 nm.
[0044] Step S6 in Figure 1 includes etching away unwanted portions of the target film 18, as shown in Figure 2(F). This enlarges the openings in the target film 18 and reduces the wiring resistance of the substrate 1.
[0045] If the organic compound used as a raw material for SAM17 contains fluorine, step S6 includes supplying an H2O-containing gas to the substrate surface 1a. Hydrofluoric acid is produced by the reaction between the H2O-containing gas and SAM17. The produced hydrofluoric acid can etch unwanted parts of the target film 18, as shown in Figure 2(F). The products produced by etching are volatile, vaporize, and are exhausted. The target film 18 is, as described above, for example, an AlO film, an SiO film, a SiN film, a ZrO film, or an HfO film. All of these films can be etched with hydrofluoric acid.
[0046] As described above, hydrofluoric acid is produced by the reaction of a gas containing H2O with SAM17. Therefore, hydrofluoric acid is produced only in the vicinity of SAM17. Consequently, unwanted parts of the target film 18 are etched, while necessary parts of the target film 18 (parts deposited on the surface of the insulating film 11) are not etched. Unwanted parts of the target film 18 can be selectively removed. According to this embodiment, the density of SAM17 can be increased by supplying oxygen-containing gas and organic compound gas in step S4, making it easier to produce hydrofluoric acid.
[0047] Step S6 in Figure 1 includes, for example, steps S61 to S63 shown in Figure 5. Step S61 includes supplying an H2O-containing gas to the substrate surface 1a. The H2O-containing gas may consist of H2O gas alone, or it may consist of H2O gas and a carrier gas.
[0048] Step S62 involves supplying a plasma-forming gas to the substrate surface 1a. The plasma-forming gas is obtained by plasma-forming at least one gas selected from, for example, H2 gas, Ar gas, N2 gas, and NH3 gas. The supply of the plasma-forming gas can decompose the SAM 17 and promote the generation of hydrofluoric acid. It is preferable that the plasma-forming gas is a reducing gas or an inert gas plasma-forming gas so that the conductive film 12 or barrier film 13 exposed after the decomposition of the SAM 17 is not oxidized. Note that the order of steps S61 and S62 may be reversed.
[0049] Step S63 includes checking whether steps S61 to S62 have been performed the set number of times. If the number of executions has not reached the set number (step S63, NO), steps S61 to S62 are performed again. On the other hand, if the number of executions has reached the set number (step S63, YES), the current process is terminated.
[0050] In Figure 5, the H2O-containing gas and the plasma-forming gas are supplied sequentially, not simultaneously, although they may be supplied simultaneously. In any case, the supply of the plasma-forming gas can decompose SAM17 and promote the generation of hydrofluoric acid. However, by supplying the H2O-containing gas and the plasma-forming gas sequentially, the plasma formation of the H2O-containing gas can be prevented, the generation of oxygen plasma can be prevented, and oxidation of the substrate surface 1a can be prevented.
[0051] The number of times step S63 is set may be once, but it is preferable to set it multiple times. By dividing the supply of plasma gas into multiple sets, the decomposition of SAM17 can be gradually advanced, hydrofluoric acid can be generated over a long period of time, and the width W of the unnecessary parts can be narrowed. As a result, the wiring resistance of the substrate 1 can be reduced. The number of times step S63 is set may be, for example, 1 to 50.
[0052] An example of the processing conditions for step S6 is shown below. Step S61 H2O gas flow rate: 10 sccm to 500 sccm Processing time: 0.1 sec to 120 sec Step S62 H2 gas flow rate: 200 sccm~3000 sccm Ar gas flow rate: 100 sccm to 6000 sccm Percentage of H2 gas in a mixed gas of H2 and Ar gas: 20% to 90% by volume Power supply frequency for plasma generation: 10MHz~60MHz Power for plasma generation: 50W~600W Processing time: 2 sec to 120 sec • Processing conditions common to steps S61-S62 Processing temperature: 100℃~350℃ Processing pressure: 50 Pa to 1200 Pa.
[0053] Step S6 may include disassembling and removing the SAM17, as shown in Figure 2(F). After step S6, the SAM17 does not need to remain on the substrate surface 1a.
[0054] Although not shown in the diagram, step S6 may include forming and replenishing SAM17 on the surface of the conductive film 12 midway through the process. By replenishing SAM17, hydrofluoric acid can be generated over a long period of time, the width W of the unnecessary parts can be narrowed, and the wiring resistance of the substrate 1 can be reduced. In that case, supplying O2 gas or the like before SAM17 formation will allow for the formation of more SAM17.
[0055] Step S7 in Figure 1 includes checking whether steps S3 to S6 have been performed the set number of times. If the number of executions has not reached the set number (step S7, NO), steps S3 to S6 are performed again. On the other hand, if the number of executions has reached the set number (step S7, YES), the AlO film thickness has reached the final target thickness, and the process is terminated. The set number of executions in step S7 is determined according to the final target thickness of the AlO film.
[0056] The number of times step S7 is set may be once, but it is preferable to set it multiple times. If the AlO film is formed in multiple steps, the width W of the unnecessary portion of the target film 18 can be narrowed in each step S5 compared to when it is performed in one step. The narrower the width W, the easier it is to remove the unnecessary portion. Therefore, if the AlO film is formed in multiple steps, the width W of the unnecessary portion of the final target film 18 can be narrowed compared to when it is performed in one step, and the wiring resistance of the substrate 1 can be reduced.
[0057] As shown in Figure 1, step S3 may be performed after the nth (where n is a natural number greater than or equal to 1)th step S6 and before the (n+1)th step S4. Repeating step S3 is effective when plasma-treated H2 gas is supplied to the substrate surface 1a in step S6. In this case, the surface of the conductive film 12 is reduced in step S6, similar to step S2. Performing step S3 after step S6 allows the surface of the conductive film 12 to be oxidized appropriately. As a result, a dense SAM 17 can be formed on the surface of the conductive film 12 in the subsequent step S4.
[0058] Next, with reference to Figure 6, the processing of the substrate 1 according to the first modified example will be described. As shown in Figure 6(A), the substrate 1 of this modified example has a liner film 14 on its surface 1a in addition to an insulating film 11, a conductive film 12, and a barrier film 13. The liner film 14 is formed between the conductive film 12 and the barrier film 13. The liner film 14 is formed on top of the barrier film 13 and assists in the formation of the conductive film 12. The conductive film 12 is formed on top of the liner film 14. The liner film 14 is not particularly limited, but for example, it may be a Co film or a Ru film.
[0059] Table 2 shows specific examples of the insulating film 11, conductive film 12, barrier film 13, and liner film 14.
[0060] [Table 2]
[0061] The combination of the insulating film 11, the conductive film 12, the barrier film 13, and the liner film 14 is not particularly limited.
[0062] As shown in Figure 6(A), contaminants 22 may be present on the surface of the liner film 14, similar to the surface of the conductive film 12. The contaminants 22 include, for example, at least one of a metal oxide and an organic substance. The metal oxide is an oxide formed by the reaction of the conductive film 12 with the atmosphere, and is a so-called native oxide film.
[0063] Step S2 of this modified example includes removing the contaminants 22, as shown in Figure 6(B). This exposes the surface of the conductive film 12 and the surface of the liner film 14.
[0064] Step S3 of this modified example includes forming an oxide film 32 by oxidizing the surface of the conductive film 12 and the surface of the liner film 14, as shown in Figure 6(C). This allows for the formation of a dense SAM 17 on the surface of the conductive film 12 and the surface of the liner film 14 in step S4, which will be described later.
[0065] Step S4 of this modified example includes selectively forming SAM17 on the surface of the conductive film 12, the barrier film 13, and the liner film 14 on the surface of the insulating film 11, as shown in Figure 6(D). SAM17 does not need to be formed on the insulating film 11.
[0066] Step S5 of this modified example includes forming the target film 18 on the surface of the insulating film 11 while inhibiting the formation of the target film 18 on the surface of the conductive film 12, the barrier film 13, and the liner film 14 using the SAM 17, as shown in Figure 6(E). Although the SAM 17 inhibits the formation of the target film 18, the blocking performance of the SAM 17 is not perfect, and the target film 18 protrudes laterally from the surface of the insulating film 11.
[0067] Step S6 of this modified example includes etching the portion of the target film 18 that extends laterally from the surface of the insulating film 11 by supplying a gas containing H2O to the substrate surface 1a, as shown in Figure 6(F). By etching the unnecessary portion of the target film 18, the wiring resistance of the substrate 1 can be reduced.
[0068] Next, with reference to Figure 7, the processing of the substrate 1 according to the second modified example will be described. In this modified example, as shown in Figure 7(A), the conductive film 12 is a cap film. Specific examples of the conductive film (cap film) 12, barrier film 13, liner film 14, and second conductive film 15 are summarized in Table 3.
[0069] [Table 3]
[0070] The combination of the insulating film 11, the conductive film 12, the barrier film 13, the liner film 14, and the second conductive film 15 is not particularly limited.
[0071] Steps S2 to S6 of this modified example (see Figures 7(B) to 7(F)) are carried out in the same manner as steps S2 to S6 of the first modified example (see Figures 6(B) to 6(F)).
[0072] In the above embodiments, the first modified example, and the second modified example, the insulating film 11 corresponds to the first film and the conductive film 12 corresponds to the second film, but the combination of the first and second films is not particularly limited. Table 4 shows candidate combinations of the first film, the second film, and the target film 18 when the raw material for SAM17 is a thiol-based compound.
[0073] [Table 4]
[0074] The candidates listed in Table 4 can be used in any combination. Preferably, the first film is an insulating film, the second film is a conductive film, and the target film 18 formed on the surface of the first film is an insulating film.
[0075] Next, with reference to Figure 8, a film deposition apparatus 100 for carrying out the above film deposition method will be described. As shown in Figure 8, the film deposition apparatus 100 has a first processing unit 200A, a second processing unit 200B, a third processing unit 200C, a transport unit 400, and a control unit 500. The first processing unit 200A carries out steps S2 to S3 in Figure 1. The second processing unit 200B carries out step S4 in Figure 1. The third processing unit 200C carries out steps S5 to S6 in Figure 1. The first processing unit 200A, the second processing unit 200B, and the third processing unit 200C may have the same structure or may have different structures. It is also possible for the first processing unit 200A alone to carry out all of steps S2 to S6 in Figure 1. The transport unit 400 transports the substrate 1 to the first processing unit 200A, the second processing unit 200B, and the third processing unit 200C. The control unit 500 controls the first processing unit 200A, the second processing unit 200B, the third processing unit 200C, and the transport unit 400.
[0076] The transport unit 400 includes a first transport chamber 401 and a first transport mechanism 402. The internal atmosphere of the first transport chamber 401 is an atmospheric atmosphere. The first transport mechanism 402 is provided inside the first transport chamber 401. The first transport mechanism 402 includes an arm 403 for holding the substrate 1 and travels along a rail 404. The rail 404 extends in the direction of the arrangement of the carriers C.
[0077] Furthermore, the transport unit 400 includes a second transport chamber 411 and a second transport mechanism 412. The internal atmosphere of the second transport chamber 411 is a vacuum atmosphere. The second transport mechanism 412 is provided inside the second transport chamber 411. The second transport mechanism 412 includes an arm 413 for holding the substrate 1, and the arm 413 is arranged to be movable in the vertical and horizontal directions and rotatable around a vertical axis. The first processing unit 200A, the second processing unit 200B, and the third processing unit 200C are connected to the second transport chamber 411 via different gate valves G.
[0078] Furthermore, the conveying section 400 has a load lock chamber 421 between the first conveying chamber 401 and the second conveying chamber 411. The internal atmosphere of the load lock chamber 421 is switched between a vacuum atmosphere and an atmospheric atmosphere by a pressure regulating mechanism (not shown). This allows the inside of the second conveying chamber 411 to always be maintained in a vacuum atmosphere. It also prevents gas from flowing from the first conveying chamber 401 into the second conveying chamber 411. Gate valves G are provided between the first conveying chamber 401 and the load lock chamber 421, and between the second conveying chamber 411 and the load lock chamber 421.
[0079] The control unit 500 is, for example, a computer and includes a CPU (Central Processing Unit) 501 and a storage medium 502 such as memory. The storage medium 502 stores programs that control various processes performed in the film deposition apparatus 100. The control unit 500 controls the operation of the film deposition apparatus 100 by causing the CPU 501 to execute the programs stored in the storage medium 502. The control unit 500 controls the first processing unit 200A, the second processing unit 200B, the third processing unit 200C, and the transport unit 400 to carry out the above-described film deposition method.
[0080] Next, the operation of the film deposition apparatus 100 will be described. First, the first transport mechanism 402 removes the substrate 1 from the carrier C, transports the removed substrate 1 to the load lock chamber 421, and exits the load lock chamber 421. Next, the internal atmosphere of the load lock chamber 421 is switched from an atmospheric atmosphere to a vacuum atmosphere. After that, the second transport mechanism 412 removes the substrate 1 from the load lock chamber 421 and transports the removed substrate 1 to the first processing unit 200A.
[0081] Next, the first processing unit 200A performs steps S2 to S3. After that, the second transport mechanism 412 removes the substrate 1 from the first processing unit 200A and transports the removed substrate 1 to the second processing unit 200B. During this time, the surrounding atmosphere of the substrate 1 can be maintained in a vacuum atmosphere, and unintended oxidation of the substrate 1 can be suppressed.
[0082] Next, the second processing unit 200B performs step S4. After that, the second transport mechanism 412 removes the substrate 1 from the second processing unit 200B and transports the removed substrate 1 to the third processing unit 200C. During this time, the surrounding atmosphere of the substrate 1 can be maintained in a vacuum atmosphere, and the deterioration of the blocking performance of the SAM 17 can be suppressed.
[0083] Next, the third processing unit 200C performs steps S5 to S6. Subsequently, the control unit 500 checks whether steps S3 to S6 have been performed the set number of times. If the number of times has not reached the set number, the second transport mechanism 412 removes the substrate 1 from the third processing unit 200C and transports the removed substrate 1 to the first processing unit 200A. After that, the control unit 500 controls the first processing unit 200A, the second processing unit 200B, the third processing unit 200C, and the transport unit 400 to perform steps S3 to S6.
[0084] On the other hand, if the number of executions reaches the set number, the second transport mechanism 412 removes the substrate 1 from the third processing unit 200C, transports the removed substrate 1 to the load lock chamber 421, and exits the load lock chamber 421. Subsequently, the internal atmosphere of the load lock chamber 421 is switched from a vacuum atmosphere to an atmospheric atmosphere. After that, the first transport mechanism 402 removes the substrate 1 from the load lock chamber 421 and places the removed substrate 1 into the carrier C. Then, the processing of the substrate 1 is completed.
[0085] Next, the first processing unit 200A will be described with reference to Figure 9. Note that the second processing unit 200B and the third processing unit 200C are configured similarly to the first processing unit 200A, and therefore their illustrations and descriptions are omitted.
[0086] The first processing unit 200A includes a substantially cylindrical, airtight processing container 210. An exhaust chamber 211 is provided in the center of the bottom wall of the processing container 210. The exhaust chamber 211 has a shape that protrudes downward, for example, a substantially cylindrical shape. An exhaust pipe 212 is connected to the exhaust chamber 211, for example, on the side of the exhaust chamber 211.
[0087] An exhaust source 272 is connected to the exhaust piping 212 via a pressure controller 271. The pressure controller 271 includes a pressure regulating valve, such as a butterfly valve. The exhaust piping 212 is configured to reduce the pressure inside the processing container 210 by the exhaust source 272. The pressure controller 271 and the exhaust source 272 constitute a gas discharge mechanism 270 that discharges gas from inside the processing container 210.
[0088] A transport port 215 is provided on the side of the processing container 210. The transport port 215 is opened and closed by a gate valve G. The substrate 1 is loaded and unloaded between the processing container 210 and the second transport chamber 411 (see Figure 8) through the transport port 215.
[0089] A stage 220, which is a holding part for holding the substrate 1, is provided inside the processing container 210. The stage 220 holds the substrate 1 horizontally with the substrate surface 1a facing upwards. The stage 220 is formed in a substantially circular shape in plan view and is supported by a support member 221. A substantially circular recess 222 is formed on the surface of the stage 220 for placing a substrate 1, for example, with a diameter of 300 mm. The recess 222 has an inner diameter slightly larger than the diameter of the substrate 1. The depth of the recess 222 is set to be approximately the same as the thickness of the substrate 1, for example. The stage 220 is formed of a ceramic material such as aluminum nitride (AlN). Alternatively, the stage 220 may be formed of a metallic material such as nickel (Ni). Instead of the recess 222, a guide ring for guiding the substrate 1 may be provided on the peripheral edge of the surface of the stage 220.
[0090] A lower electrode 223, for example, grounded, is embedded in the stage 220. A heating mechanism 224 is embedded below the lower electrode 223. The heating mechanism 224 is powered by a power supply unit (not shown) based on a control signal from the control unit 500 (see Figure 8), and heats the substrate 1 placed on the stage 220 to a set temperature. If the entire stage 220 is made of metal, the entire stage 220 functions as the lower electrode, so the lower electrode 223 does not need to be embedded in the stage 220. The stage 220 is provided with a plurality of (e.g., three) lifting pins 231 for holding and raising / lowering the substrate 1 placed on the stage 220. The material of the lifting pins 231 may be, for example, ceramics such as alumina (Al2O3) or quartz. The lower ends of the lifting pins 231 are attached to a support plate 232. The support plate 232 is connected via a lifting shaft 233 to a lifting mechanism 234 located outside the processing container 210.
[0091] The lifting mechanism 234 is installed, for example, at the bottom of the exhaust chamber 211. The bellows 235 is provided between the opening 219 for the lifting shaft 233 formed on the lower surface of the exhaust chamber 211 and the lifting mechanism 234. The shape of the support plate 232 may be such that it can move up and down without interfering with the support member 221 of the stage 220. The lifting pin 231 is configured to move up and down between the upper surface of the stage 220 and the lower surface of the stage 220 by the lifting mechanism 234.
[0092] A gas supply unit 240 is provided on the top wall 217 of the processing container 210 via an insulating member 218. The gas supply unit 240 forms the upper electrode and faces the lower electrode 223. A high-frequency power supply 252 is connected to the gas supply unit 240 via a matching unit 251. By supplying high-frequency power of 450 kHz to 100 MHz from the high-frequency power supply 252 to the upper electrode (gas supply unit 240), a high-frequency electric field is generated between the upper electrode (gas supply unit 240) and the lower electrode 223, and a capacitively coupled plasma is generated. The plasma generation unit 250 that generates the plasma includes a matching unit 251 and a high-frequency power supply 252. Note that the plasma generation unit 250 is not limited to generating capacitively coupled plasma, but may generate other plasmas such as inductively coupled plasma. Note that in steps that do not generate plasma (for example, steps S4 and S5), it is not necessary for the gas supply unit 240 to form the upper electrode, and the lower electrode 223 is also unnecessary.
[0093] The gas supply unit 240 includes a hollow gas supply chamber 241. On the lower surface of the gas supply chamber 241, numerous holes 242 are evenly arranged, for example, to distribute and supply the processing gas into the processing container 210. Above the gas supply chamber 241 in the gas supply unit 240, for example, a heating mechanism 243 is embedded. The heating mechanism 243 is heated to a set temperature by being powered from a power supply unit (not shown) based on a control signal from the control unit 500.
[0094] A gas supply mechanism 260 is connected to the gas supply room 241 via a gas supply passage 261. The gas supply mechanism 260 supplies the gas used in at least one of steps S2 to S6 in Figure 1 to the gas supply room 241 via the gas supply passage 261. Although not shown, the gas supply mechanism 260 includes individual piping for each type of gas, an on / off valve installed in the middle of the individual piping, and a flow controller installed in the middle of the individual piping. When the on / off valve opens the individual piping, gas is supplied from the supply source to the gas supply passage 261. The amount of gas supplied is controlled by the flow controller. On the other hand, when the on / off valve closes the individual piping, the supply of gas from the supply source to the gas supply passage 261 is stopped.
[0095] [Examples] Next, we will describe the examples. Example 1-1 below is an example, and Example 1-2 is a comparative example. Examples 2-1 to 2-3 are for reference only.
[0096] <Example 1-1> In Example 1-1, the substrate 1 shown in Figure 2(A) was prepared. The base substrate 10 was a silicon wafer, the insulating film 11 was a SiOC film, the conductive film 12 was a Cu film, and the barrier film 13 was a TaN film. On the surface of the SiOC film, the trench width was 20 nm and the trench pitch was 40 nm.
[0097] In Example 1-1, steps S1 to S7 shown in Figure 1 were performed. In step S2, a plasma-generated cleaning gas was supplied to the substrate surface 1a. The cleaning gas contained H2 gas, N2 gas, and Ar gas. In step S3, O2 gas was supplied to the substrate surface 1a as an oxygen-containing gas.
[0098] In step S4, SAM17 was formed by performing steps S41 to S43 as shown in Figure 3. O2 gas was used as the oxygen-containing gas, and PFOT gas was used as the organic compound gas. The number of times set for step S43, that is, the number of repetitions of steps S41 to S42, was 5.
[0099] In step S5, an SiO film was formed as the target film 18 by performing steps S51 to S55 as shown in Figure 4. In step S51, a Si-containing gas (specifically tris(tert-pentoxy)silanol: TPSOL((CH3CH2C(CH3)2O)3SiOH) gas) was used instead of an Al-containing gas. In step 53, TMA((CH3)3Al) gas was used instead of an oxidizing gas. The TMA gas in step S53 is a catalyst that promotes the reaction in which TPSOL undergoes dehydration condensation to form an SiO film. The number of times set for step S55, that is, the number of repetitions of steps S51 to S54, was 1. The thickness of the SiO film was 3 nm.
[0100] In step S6, unnecessary parts of the target film 18 were etched by performing steps S61 to S63 as shown in Figure 5. In step S62, plasma-generated H2 gas was used as the plasma gas. The set number of times for step S63, that is, the number of repetitions of steps S61 to S63, was 3.
[0101] The number of times step S7 was set, that is, the number of repetitions of steps S3 to S6, was 4. Subsequently, when the SEM image of the substrate cross-section was observed, it was found that at least a portion of the surface of the Cu film, which is the conductive film 12, was exposed and not covered by the SiO film, which is the target film 18.
[0102] <Example 1-2> In Example 1-2, the substrate was processed under the same conditions as in Example 1-1, except that step S42 (supply of organic compound gas) was repeated five times without performing step S41 (supply of oxygen-containing gas) as shown in Figure 3. Subsequently, when an SEM image of the substrate cross-section was observed, the entire surface of the conductive film 12, which is the Cu film, was found to be covered with the target film 18, which is the SiO film.
[0103] <Examples 2-1 to 2-3> In Examples 2-1 to 2-3, only step S2 (removal of contaminants) was performed on the silicon wafer. Table 5 shows the cleaning gas used in step S2. The cleaning gas was plasma-generated. The silicon wafer was a bare wafer.
[0104] [Table 5]
[0105] The cleaning gases in Examples 2-1 and 2-2 contain N2 gas in addition to H2 gas, whereas the cleaning gas in Example 2-3 does not contain N2 gas in addition to H2 gas.
[0106] Figure 10 shows the XPS (X-ray photoelectron spectroscopy) spectra of the substrate surface obtained in Examples 2-1 to 2-3. As is clear from Figure 10, when the cleaning gas contains N2 gas in addition to H2 gas, the carbon (C) peak is smaller compared to when the cleaning gas contains H2 gas in addition to N2 gas, indicating a higher organic matter removal effect.
[0107] While embodiments of the film deposition method and film deposition apparatus relating to this disclosure have been described above, this disclosure is not limited to the above embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations are possible within the scope of the claims. These, too, naturally fall within the technical scope of this disclosure. [Explanation of symbols]
[0108] 1 circuit board 1a Substrate surface 11. Insulating film (first layer) 12. Conductive film (second film) 22. Contaminants 17 SAM (Self-assembled monolayer)
Claims
1. A substrate is prepared having a first film and a second film formed of a different material from the first film in different regions of its surface. By supplying an organic compound gas and an oxygen-containing gas that does not contain OH groups into a processing container containing the substrate, a self-assembled monolayer is selectively formed on the surface of the second film relative to the surface of the first film. The self-assembled monolayer is used to inhibit the formation of the target film on the surface of the second film while forming the target film on the surface of the first film. Includes, A method for forming a self-assembled monolayer, wherein, before forming the target film, the organic compound gas and the oxygen-containing gas that does not contain OH groups are repeatedly and alternately supplied into the processing container multiple times to form the target film.
2. The film formation method according to claim 1, further comprising forming an oxide film by oxidizing the surface of the second film before forming the self-assembled monolayer.
3. The film formation method according to claim 2, further comprising removing contaminants from the surface of the substrate before forming the oxide film.
4. Removing the contaminants includes supplying a plasma-formed cleaning gas to the surface of the substrate, The film formation method according to claim 3, wherein the cleaning gas comprises hydrogen gas and nitrogen gas.
5. The film formation method according to any one of claims 1 to 4, wherein the first film is an insulating film and the second film is a conductive film.
6. The method for forming a film according to any one of claims 1 to 4, wherein the organic compound gas includes a thiol compound.
7. The oxygen-containing gas that does not contain the aforementioned OH group is O 2 Gas, O 3 Gas, NO gas, NO 2 Gas and N 2 A method for forming a film according to any one of claims 1 to 4, comprising at least one selected from O gases.
8. A film formation method according to any one of claims 1 to 4, comprising etching the portion of the target film that extends laterally from the first film after forming the target film.
9. The aforementioned organic compound gas contains fluorine, Etching the aforementioned portion of the target film is performed on the surface of the substrate. 2 The method for forming a film according to claim 8, comprising supplying an oxygen-containing gas.
10. Etching the aforementioned portion of the target film is performed on the surface of the substrate. 2 The film formation method according to claim 9, comprising supplying an O-containing gas and a plasma-forming gas.
11. The film formation method according to claim 8, comprising repeatedly in this order forming the self-assembled monolayer, forming the target film, and etching the portion of the target film multiple times.
12. Processing container and The processing container includes a holding section for holding the substrate inside, A gas supply mechanism that supplies gas to the inside of the processing container, A gas discharge mechanism for discharging gas from inside the processing container, A transport mechanism for loading and unloading the substrate into and from the processing container, A control unit that controls the gas supply mechanism, the gas discharge mechanism, and the transport mechanism, and carries out the film formation method according to any one of claims 1 to 4, A film deposition apparatus equipped with the following features.
Citation Information
Patent Citations
Inactivation of reaction sites for vapor deposition
JP2013520028A
Film formation method
JP2021052071A
Film formation method
JP2021057563A
Film deposition method and film deposition apparatus
JP2022055462A
Method for cleaning via of interconnect structure of semiconductor device structure
US20170018458A1