Double-glazed glass panels

A double-glazed glass panel design with a zeolite-based getter material and inorganic binder, along with a metallic getter opposite the suction hole, addresses gas adsorption and thermal insulation issues, ensuring stable performance and appearance.

JP7948765B2Active Publication Date: 2026-11-11NIPPON SHEET GLASS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022022228
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-02-16
Publication Date
2026-11-11
Estimated Expiration
2042-02-16

AI Technical Summary

Technical Problem

The gas adsorption performance of getter materials in double-glazed glass panels is compromised due to packaging materials and reduced contact area with gases, leading to decreased thermal insulation performance.

Method used

A configuration featuring a zeolite-based nonmetallic getter material with an inorganic binder, positioned apart from the glass plates, and a metallic getter material opposite a suction hole, ensuring stable gas adsorption and thermal insulation without packaging, while maintaining holding strength and appearance.

Benefits of technology

Stable gas adsorption performance and thermal insulation are maintained with a simple configuration, minimizing visual impact and preserving the integrity of the glass panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948765000001
    Figure 0007948765000001
  • Figure 0007948765000002
    Figure 0007948765000002
  • Figure 0007948765000003
    Figure 0007948765000003
Patent Text Reader

Abstract

To provide a multilayer glass panel capable of stably securing a gas absorption performance of a gas adsorbent with a simple configuration.SOLUTION: A multilayer glass panel includes: a pair of glass panes 1A, 1B facing each other; a circumference encapsulation material 5 disposed on an entire outer edge of the pair of glass panes 1A, 1B and forming a void part V sealed between the pair of glass panes 1A, 1B; a plurality of interval holding members 2 arranged at the void part V; and a gas adsorbent 6 provided on one surface 13 of a pair of plate surfaces 12, 13 facing each other at a side of the void part V of the pair of glass panes 1A, 1B and alienated from the other surface 12 of the pair of plate surfaces 12, 13. The gas adsorbent 6 includes: a zeolite-based nonmetal getter material having a multicellular structure; and an inorganic binder material having a nonmetal getter material.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a double-glazed glass panel. [Background technology]

[0002] Patent Document 1 discloses a method for manufacturing a double-glazed glass panel in which a reduced-pressure space is formed between a pair of glass plates. The double-glazed glass panel has a gas adsorbent material placed in the reduced-pressure space to adsorb gases released from the frame and the like. The double-glazed glass panel can improve its thermal insulation performance because the gas adsorbent material adsorbs gases remaining in the reduced-pressure space, further reducing the thermal transmittance (U-value) of the reduced-pressure space.

[0003] In the double-glazed glass panel described in Patent Document 1, the gas adsorbent is composed of a getter material (zeolite). The getter material is heated and activated during the manufacturing of the double-glazed glass panel, thereby adsorbing gases released from the frame, etc. However, the getter material cannot be used if it cannot be heated to a temperature above its activation temperature. Therefore, in the method for manufacturing a double-glazed glass panel described in Patent Document 1, the getter material is covered with a package material containing powder, the getter material wrapped in the package material is heated and activated in the activation step, and then the getter material is sealed in the sealing step with the package material in which the powder has melted. By heating in the sealing step at a temperature higher than the heating temperature in the activation step, the getter material is sealed in an activated state, and the activated state of the getter material is maintained. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] International Publication No. 2019 / 003997 [Overview of the project] [Problems that the invention aims to solve]

[0005] However, in the double-layered glass panel described in Patent Document 1, the getter material, which is a gas adsorbent, is covered by the packaging material, so the gas adsorption performance of the getter material may decrease due to the influence of the packaging material. Furthermore, if the gas adsorbent is in contact with both of the pair of glass plates, the gas adsorbent's contact with the gas is hindered at the part of the gas adsorbent that is in contact with the glass plate, reducing the contact area with the gas, which also reduces the gas adsorption performance of the gas adsorbent.

[0006] Therefore, there is a need for a double-glazed glass panel that can stably ensure the gas adsorption performance of a gas adsorbent material with a simple configuration. [Means for solving the problem]

[0007] The characteristic configuration of the multilayer glass panel according to the present invention comprises a pair of opposing glass plates, a peripheral sealing material provided over the entire outer edge of the pair of glass plates and forming a sealed gap between the pair of glass plates, a plurality of spacing members disposed in the gap, a gas adsorbent disposed on one side of the pair of opposing plate surfaces of the pair of glass plates on the side of the gap and spaced apart from the other side of the pair of plate surfaces, and a suction hole sealing material that seals the suction hole when the gap is depressurized through a suction hole that penetrates from front to back in either of the glass plates, wherein the gas adsorbent includes a zeolite-based nonmetallic getter material having a porous structure, an inorganic binder material connecting the nonmetallic getter materials, and a metallic getter material, and the metallic getter material is disposed at a position opposite to the suction hole. In a view perpendicular to the plate surface, the suction hole sealing material has a portion that overlaps with the metal getter material. It's at a single point.

[0008] Gas adsorbents are typically composed of a zeolite-based nonmetallic getter material in powder form. In this configuration, the gas adsorbent includes a zeolite-based nonmetallic getter material having a porous structure and an inorganic binder material that connects the nonmetallic getter materials. As a result, the powdered nonmetallic getter material is stably held by the inorganic binder material. This eliminates the need to cover the nonmetallic getter material with a packaging material, as in the multi-layer glass panel described in Patent Document 1, and allows the multi-layer glass panel to stably ensure the gas adsorption performance of the gas adsorbent with a simple configuration.

[0009] Here, if the binder material contained in the gas adsorbent is made of organic material, gas will be generated from the organic material when the gas adsorbent is heated to its activation temperature. As a result, gas may remain in the gaps of the double-glazed panel, potentially reducing its thermal insulation performance. On the other hand, in this configuration, the gas adsorbent contains an inorganic binder material, so even if the gas adsorbent is heated to its activation temperature, no gas will be generated from the inorganic binder material. This makes it possible to maintain the thermal insulation performance of double-glazed glass panels.

[0010] Furthermore, in this configuration, the gas adsorbent is placed on one side of the pair of glass plates facing each other on the gap side, and is spaced apart from the other side. As a result, the gas adsorbent can secure a large contact area with the gas without the other side of the glass plate reducing its contact area with the gas. Consequently, the double-glazed glass panel can stably ensure the gas adsorption performance of the gas adsorbent with a simple configuration.

[0011] Another characteristic feature is that the gas adsorbent and the spacing member are positioned at different locations when viewed perpendicular to the plate surface.

[0012] According to this configuration, the double-glazed glass panel is a reduced-pressure double-glazed glass panel in which the gap is depressurized, and the gas adsorbent is positioned differently from the spacing member when viewed perpendicular to the surface of the glass plate. As a result, the gas adsorbent is positioned in a suitable location different from the spacing member in the depressurized gap, and its surface area is ensured. Consequently, even in a reduced-pressure double-glazed glass panel, the gas adsorption performance of the gas adsorbent can be stably ensured with a simple configuration.

[0013] Another characteristic feature is that the gas adsorbent is positioned between the peripheral sealing material and the spacing member.

[0014] As in this configuration, when the gas adsorbent is placed between the peripheral sealant and the spacing member, the gas adsorbent can be positioned near the periphery of the double-glazed glass panel. This suppresses the visual impact of the gas adsorbent on the double-glazed glass panel. Furthermore, if the gas adsorbent were placed between multiple adjacent spacing members, the spacing between the adjacent spacing members would need to be increased to accommodate the dimensions of the gas adsorbent, which could reduce the holding strength of the pair of glass plates in the double-glazed glass panel. On the other hand, as in this configuration, when the gas adsorbent is placed between the peripheral sealant and the spacing member, the spacing between multiple adjacent spacing members can be set to a constant pitch, making it easier to maintain the holding strength of the pair of glass plates between the multiple spacing members in the double-glazed glass panel. This suppresses a decrease in the holding strength of the pair of glass plates in the double-glazed glass panel.

[0015] Another characteristic feature is that the gas adsorbent is positioned between a plurality of adjacent spacing members.

[0016] In a double-glazed glass panel having multiple spacing members, if the distance between the peripheral sealant and the spacing member adjacent to the peripheral sealant is smaller than the width of the gas adsorbent, the gas adsorbent cannot be placed between them. In such cases, as in this configuration, the gas adsorbent can be reliably placed in the double-glazed glass panel by placing it between multiple adjacent spacing members. The gas adsorbent can be placed, for example, between the spacing member adjacent to the peripheral sealant and the spacing member adjacent to that spacing member, thereby being positioned near the periphery of the pair of glass plates. This makes it possible to suppress the visual impact of the gas adsorbent on the double-glazed glass panel.

[0017] Other characteristic features include the fact that the distance between the gas adsorbent and the peripheral sealing material and the spacing member is 40 mm or less, and the distance between the gas adsorbent and the peripheral sealing material, and the distance between the gas adsorbent and the spacing member are both 1 mm or more.

[0018] In a double-glazed glass panel, if the distance between the peripheral sealant and the spacing member becomes too large, the holding strength of the pair of glass plates decreases. Therefore, in this configuration, the distance between the peripheral sealant where the gas adsorbent is placed and the spacing member is kept to 40 mm or less. This suppresses the decrease in the holding strength of the pair of glass plates in a double-glazed glass panel. Furthermore, in this configuration, the distance between the gas adsorbent and the peripheral sealant, and the distance between the gas adsorbent and the spacing member are both 1 mm or more, so the gas adsorbent can be placed at a distance from the peripheral sealant and the spacing member. This allows the gas adsorbent to secure a large contact area with the gas on its surface. As a result, the gas adsorption performance of the gas adsorbent can be stably ensured in a double-glazed glass panel.

[0019] Other characteristic features include the fact that the gas adsorbent material has a distance of 40 mm or less between adjacent spacing members, and the distance between the gas adsorbent material and adjacent spacing members is 1 mm or more in all cases.

[0020] In a multi-layer glass panel, if the distance between a plurality of adjacent spacing members becomes excessively large, the holding strength of the pair of glass plates in the multi-layer glass panel decreases. Therefore, in this configuration, the distance between the plurality of adjacent spacing members is set to 40 mm or less. This makes it possible to suppress a decrease in the holding strength of the pair of glass plates in the multi-layer glass panel. Further, in this configuration, since the distance between the gas adsorbent and each of the plurality of adjacent spacing members is 1 mm or more, the gas adsorbent can be arranged in a state separated from the plurality of adjacent spacing members. As a result, the gas adsorbent can secure a large contact area with gas on its surface. As a result, the gas adsorption performance of the gas adsorbent in the multi-layer glass panel can be stably secured.

[0021] Another characteristic configuration is that the gas adsorbent is arranged in a linear shape along the plate surface of the one surface, has a width of 1 mm or more and 15 mm or less, a length of 1 mm or more and 2000 mm or less, and a height relative to the plate surface of 10 μm or more and 190 μm or less.

[0022] According to this configuration, the gas adsorbent is arranged in a linear shape along the plate surface on one side of a glass plate, and the width and length of the gas adsorbent are within predetermined ranges. In the multi-layer glass panel, this allows the gas adsorbent to sufficiently exhibit gas adsorption performance and suppress adverse effects on the external appearance. If the width of the gas adsorbent is less than 1 mm, the gas adsorption performance cannot be sufficiently exhibited, and if the width exceeds 15 mm, the gas adsorbent becomes too conspicuous and impairs the external appearance of the multi-layer glass panel. Further, if the length of the gas adsorbent is less than 1 mm, the gas adsorbent cannot sufficiently exhibit its gas adsorption performance, and if the length exceeds 2000 mm, the gas adsorbent becomes too conspicuous and impairs the external appearance of the multi-layer glass panel. Furthermore, in this configuration, the gas adsorbent has a height of 10 μm or more and 190 μm or less relative to the plate surface. Thereby, in the multi-layer glass panel, the gas adsorbent can sufficiently exhibit gas adsorption performance and is less likely to come into contact with the other side of the glass plate, so that it is possible to avoid a situation in which the glass plate comes into contact with the high-hardness gas adsorbent and is damaged. On the other hand, if the height of the gas adsorbent is less than 10 μm, the gas adsorption performance cannot be sufficiently exhibited, and if the height exceeds 190 μm, the gas adsorbent easily comes into contact with the other side of the glass plate when an impact or the like acts on the glass plate. When the gas adsorbent comes into contact with the other side of the glass plate, the glass plate may be damaged by the high-hardness gas adsorbent. In addition, when the height of the gas adsorbent exceeds 190 μm and the gas adsorbent comes into contact with both surfaces of the pair of glass plates, heat transfer occurs between the pair of glass plates due to the gas adsorbent, so that the heat insulation performance of the multi-layer glass panel is also reduced.

[0023] Another characteristic configuration resides in that the inorganic binder material is composed of a material having gas adsorption performance.

[0024] As in this configuration, the inorganic binder material contained in the gas adsorbent is composed of a material having gas adsorption performance, so that in the multi-layer glass panel, gas adsorption by the gas adsorbent in the gap portion is further promoted by the inorganic binder material. As a result, the heat transmission coefficient (U value) of the gap portion of the multi-layer glass panel is reduced, so that the heat insulation property can be further improved.

[0025] Another characteristic feature is that the gas adsorbent is arranged in a continuous single region on the one surface.

[0026] If the gas adsorbent is placed in multiple regions on one side of the glass plate, the appearance of the double-glazed glass panel may be significantly affected by the presence of gas adsorbents in multiple regions. Furthermore, if the distance between the peripheral sealant and the spacing member, or the distance between multiple adjacent spacing members, is increased to accommodate the gas adsorbent, the holding strength of the pair of glass plates will decrease in that area. Therefore, in this configuration, the gas adsorbent is placed in a single, continuous region on one side of the glass plate. This suppresses the appearance impact of the gas adsorbent on the double-glazed glass panel and also suppresses the decrease in the holding strength of the pair of glass plates.

[0027] Other characteristic features include the fact that the pair of glass plates are formed in a rectangular shape with a long side and a short side, and the gas adsorbent is positioned within the gap on the side of the short side.

[0028] When a pair of glass plates are formed in a rectangular shape with a long side and a short side, the gas adsorbent can be placed on either the long side or the short side to minimize its impact on the appearance of the double-glazed panel. In this configuration, since the gas adsorbent is placed on the short side, the length of the gas adsorbent placed on the pair of glass plates can be shortened. As a result, the impact of the gas adsorbent on the appearance of the double-glazed panel can be further suppressed.

[0029] Another characteristic feature is that the inorganic binder material contains a dispersant.

[0030] In gas adsorbents, the inclusion of an inorganic binder ensures that the powdered nonmetallic getter material is stably held by the inorganic binder. Such gas adsorbents are typically applied to the surface of a glass plate, for example, by mixing them with water. In this case, the gas adsorbent needs to be dispersed in water, but the nonmetallic getter material that constitutes the gas adsorbent is not easily mixed with water. Therefore, the gas adsorbent applied to the surface of a glass plate often lacks sufficient gas adsorption performance. To address this, the inorganic binder material in the gas adsorbent contains a dispersant. This makes it easier for the nonmetallic getter material to be mixed with water by the dispersant, thus facilitating sufficient gas adsorption performance in the gas adsorbent applied to the surface of a glass plate.

[0031] Another characteristic feature is that, when viewed perpendicular to the plate surface, the metal getter material and the non-metal getter material are positioned at different locations.

[0032] In this configuration, the gas adsorbent further includes a metal getter material in addition to the non-metallic getter material, and by positioning the metal getter material at a different location from the non-metallic getter material, the gas adsorbent can also adsorb gas using the metal getter material. Specifically, the non-metallic getter material adsorbs gas in the short term by physical adsorption, while the metal getter material adsorbs gas in the long term by chemical adsorption; thus, the two materials work differently. In this way, the gas adsorption performance of the gas adsorbent can be further improved by having a non-metallic getter material and a metal getter material that exhibit different gas adsorption performance for different periods. Note that the metal getter material and the non-metallic getter material may be placed on one side, or the non-metallic getter material may be placed on one side and the metal getter material on the other side, as long as they are in different positions when viewed perpendicular to the plate surface.

[0033] Another characteristic feature is that the metal getter material is an evaporation-type metal getter material.

[0034] As in this configuration, if the metal getter material is an evaporative metal getter material, heating and activating the metal getter material causes a portion of the metal getter material to evaporate, releasing the adsorbed molecules, which then disperse into the gaps. As a result, the gas adsorbent can effectively adsorb the gas in the gaps using these adsorbed molecules. Consequently, the gas adsorption performance of the gas adsorbent material in a double-glazed glass panel can be further improved.

[0035] Other characteristic features include the fact that the evaporative metal getter material is composed of an alloy containing barium and aluminum, and the peripheral sealant is glass frit.

[0036] As shown in this configuration, the evaporative metal getter material constituting the gas adsorbent is composed of an alloy containing barium and aluminum. When the evaporative metal getter material is heated and activated, the barium sublimes. As a result, the adsorbent molecules dispersed in the gaps due to the sublimation of barium adsorb the gas, thus reliably improving the gas adsorption performance of the gas adsorbent in a double-glazed glass panel.

[0037] In this configuration, activating the alloy containing barium and aluminum, which are evaporation-type metal getter materials, requires heating to a high temperature of 800°C or higher. In double-glazed panels, it is preferable to place the gas adsorbent (evaporation-type metal getter material) close to the periphery sealant to minimize its impact on appearance. However, if the periphery sealant has a low melting point, heating the alloy containing barium and aluminum as the evaporation-type metal getter material may cause the periphery sealant to melt, making it impossible to place the gas adsorbent (evaporation-type metal getter material) close to the periphery sealant. Therefore, in this configuration, the periphery sealant is glass frit. Glass frit is a glassy inorganic material with a softening point ranging from 300°C to 950°C, and its composition can be selected according to the application. For this reason, even when heated to activate the alloy containing barium and aluminum as the evaporation-type metal getter material, the periphery sealant is less likely to melt. Therefore, with this configuration, an alloy containing barium and aluminum as a gas adsorbent (evaporative metal getter material) can be placed near the peripheral sealant, which has little impact on the appearance of the double-glazed panel. [Brief explanation of the drawing]

[0038] [Figure 1] This is a partially cutaway perspective view of a double-glazed glass panel in the first embodiment. [Figure 2] This is a longitudinal cross-sectional view of the area around the suction hole of the double-glazed glass panel in the first embodiment. [Figure 3] This is a plan view of the double-glazed glass panel in the first embodiment. [Figure 4] This is a flowchart showing a method for manufacturing a double-glazed glass panel. [Figure 5] This is a longitudinal cross-sectional view of the area around the suction hole in a modified example of the first embodiment. [Figure 6] This is a longitudinal cross-sectional view of the area around the suction hole of the double-glazed glass panel in the second embodiment. [Figure 7] This is a longitudinal cross-sectional view of the area around the suction port in a modified example of the second embodiment. [Figure 8] This is an explanatory diagram of the glass panel in the test model. [Figure 9] This is a graph showing the results of Test 1 (U-value evaluation). [Figure 10] This is a graph showing the results of Test 2 (U-value evaluation). [Modes for carrying out the invention]

[0039] Embodiments of the multi-layer glass panel according to the present invention will be described below with reference to the drawings. In this embodiment, a vacuum multi-layer glass panel will be described as an example of a multi-layer glass panel. However, the invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the invention.

[0040] [First Embodiment] As shown in Figures 1 and 2, the double-layered glass panel (hereinafter referred to as "glass panel") P comprises a pair of opposing glass plates 1A and 1B, a peripheral sealant 5, a suction hole sealant 15, a plurality of spacers 2 (an example of spacing members), and a gas adsorbent 6. The peripheral sealant 5 is provided over the entire outer edge 3 of the pair of glass plates 1A and 1B, forming a sealed gap V between the pair of glass plates 1A and 1B. The plurality of spacers 2 are arranged in the gap V. The pair of glass plates 1A and 1B are composed of a first glass plate 1A and a second glass plate 1B.

[0041] Here, of the two surfaces of the first glass plate 1A, the side not facing the second glass plate 1B is defined as the first surface 11, the side facing the second glass plate 1B is defined as the second surface 12, and of the two surfaces of the second glass plate 1B, the side facing the second surface 12 is defined as the third surface 13, and the side not facing the second surface 12 is defined as the fourth surface 14.

[0042] The first glass plate 1A has a suction hole 4 that penetrates through both sides. The suction hole 4 is sealed with a suction hole sealing material 15 that covers the suction hole 4 and its periphery. The suction hole sealing material 15 seals the suction hole 4 in one of the pair of glass plates 1A, 1B when the gap V between them is depressurized through the suction hole 4.

[0043] In a glass panel P, for example, a pair of glass plates 1A and 1B are transparent float glass. However, the pair of glass plates 1A and 1B are not limited to this. Depending on the application as described above, various types of glass can be appropriately selected and used for the pair of glass plates 1A and 1B, such as patterned glass, frosted glass with light diffusion function due to surface treatment, wired glass, reinforced glass plate, tempered glass, double-tempered glass, low-reflection glass, high-transmittance glass plate, ceramic glass plate, special glass with heat ray and ultraviolet absorbing function, or combinations thereof. Furthermore, the composition of the pair of glass plates 1A and 1B can also be soda silicate glass, soda lime glass, borosilicate glass, aluminosilicate glass, various crystallized glasses, etc.

[0044] The gap V formed between the pair of glass plates 1A and 1B is, for example, 1.33 Pa (1.0 × 10⁻⁶). -2 The pressure is reduced to below Torr. The gap V is depressurized by the discharge of air inside it to the outside through the suction hole 4, and is sealed by the peripheral sealant 5 and the suction hole sealant 15 to maintain the above-mentioned depressurized state. The glass panel P may be configured to reduce the pressure in the gap V until it is almost a vacuum, or it may be configured not to reduce the pressure in the gap V.

[0045] Spacer 2 is cylindrical, with a diameter of 0.3 mm to 1.0 mm and a height of 30 μm to 1.0 mm. Spacer 2 is made of a material that does not buckle even when subjected to compressive stress caused by atmospheric pressure acting on glass plates 1A and 1B, for example, a compressive strength of 4.9 × 10⁸ Pa (5 × 10³ kgf / cm²). 2 It is made of a material of the above quality, preferably stainless steel (SUS304) or the like.

[0046] However, the spacer 2 is not limited to stainless steel, but may be made of metals such as Inconel, iron, aluminum, tungsten, nickel, chromium, and titanium; alloys such as carbon steel, chromium steel, nickel steel, nickel-chromium steel, manganese steel, chromium-manganese steel, chromium-molybdenum steel, silicon steel, brass, solder, and duralumin; or ceramics and glass, or other materials with high rigidity. Furthermore, the spacer 2 is not limited to a cylindrical shape, but may also be in various shapes such as angular or spherical.

[0047] The second glass plate 1B has a Low-E film 17 formed on its third surface 13. The Low-E film 17 is composed of a low-emission layer, for example, one mainly composed of silver.

[0048] As the peripheral sealant 5 and the suction hole sealant 15, glass frit or solder with a melting temperature of 250°C or less, for example, solder having a composition of 91.2Sn-8.8Zn (eutectic point temperature: 198°C), can be used. The peripheral sealant 5 is not limited to this, and the outer edges of the pair of glass plates 1A and 1B may be sealed using a sealing material made of a metallic material containing at least one material selected from the group consisting of Sn, Cu, In, Bi, Zn, Pb, Sb, Ga, and Ag, with a melting temperature of 250°C or less, or a sealing material made of a resin that solidifies at room temperature.

[0049] Furthermore, the above-mentioned metallic material may include at least one material selected from the group consisting of Ti, Al, and Cr. This improves the adhesion between the peripheral sealant 5 and the glass components of the pair of glass plates 1A and 1B.

[0050] The gas adsorbent 6 is placed on the third surface 13 of the second glass plate 1B. The gas adsorbent 6 is composed of a first gas adsorbent 61 containing a nonmetallic getter material and a second gas adsorbent 62 containing a metallic getter material 63. The first gas adsorbent 61 further contains an inorganic binder material in addition to the nonmetallic getter material.

[0051] The nonmetallic getter material of the first gas adsorbent 61 is a nonmetallic getter material having a porous structure capable of adsorbing gas molecules, and examples include zeolite-based, activated carbon, and magnesium oxide getter materials. Zeolite-based getter materials contain ion-exchanged zeolite. Ion-exchange substances include, for example, K, NH4, Ba, Sr, Na, Ca, Fe, Al, Mg, Li, H, and Cu. Because the first gas adsorbent 61 contains a nonmetallic getter material, it can effectively adsorb gas molecules of hydrocarbon gases (CH4, C2H6, etc.) and ammonia gas (NH3), which are difficult to adsorb with metal getter materials 63.

[0052] The first gas adsorbent 61 is positioned, for example, by being applied to the third surface 13 of the second glass plate 1B. Specifically, the first gas adsorbent 61 is positioned by adding an inorganic binder material and water to a powdered nonmetallic getter material, mixing the nonmetallic getter material into the water to form a paste, and then applying this paste to the plate surface (third surface 13) of the second glass plate 1B. Because the first gas adsorbent 61 contains an inorganic binder material, the first gas adsorbent 61 is stably held by the inorganic binder material into which the powdered nonmetallic getter material is mixed. Examples of inorganic binder materials include alkali silicates (sodium silicate, potassium silicate, etc.), phosphates (sodium phosphate, aluminum phosphate, magnesium phosphate, etc.), and clay minerals (kaolin, smectite, talc, etc.).

[0053] The inorganic binder material contained in the first gas adsorbent 61 is preferably composed of a material having gas adsorption properties. Furthermore, it is even more preferable that the inorganic binder material contains a dispersant. Examples of dispersants include thickeners such as smectite, bentonite, and fumed silica. In the sample, the mixing ratio of zeolite as a nonmetallic getter material, kaolin as an inorganic binder material, and water is appropriately adjusted, with a guideline of zeolite 10: kaolin 1: water 16-18.

[0054] When the first gas adsorbent 61 is made into a paste (or liquid), the nonmetallic getter material contained in the first gas adsorbent 61 needs to be dispersed in water. However, since the powdered nonmetallic getter material in the first gas adsorbent 61 is not easily mixed with water, the first gas adsorbent 61 applied to the surface (third surface 13) of the second glass plate 1B does not easily have sufficient gas adsorption performance. On the other hand, the inorganic binder material contained in the first gas adsorbent 61 contains a dispersant, which makes it easier for the nonmetallic getter material to be mixed with water by the dispersant. As a result, the paste-like first gas adsorbent 61 applied to the surface (third surface 13) of the second glass plate 1B has the nonmetallic getter material appropriately dispersed, making it easier to ensure sufficient gas adsorption performance. If the first gas adsorbent 61 contains, for example, zeolite (non-metallic getter material), kaolin (inorganic binder material), and smectite (dispersant), the mixing ratio of these with water can be set to zeolite 10: kaolin 1: smectite 1: water 16-18, making it suitable for application to the surface of the glass panel P.

[0055] The second gas adsorbent 62 is composed of an annular container 64 having a groove that encloses a metal getter material 63. As shown in Figures 2 and 3, a housing hole 18 for housing the second gas adsorbent 62 is formed in an annular shape on the third surface 13 of the second glass plate 1B, and the second gas adsorbent 62 is placed at the bottom surface of the housing hole 18. The housing hole 18 is formed in the second glass plate 1B at a position opposite to the suction hole 4. The metal getter material 63 housed in the housing hole 18 is enclosed in, for example, an annular container 64 made of stainless steel.

[0056] The metal getter material 63 of the second gas adsorbent 62 is a metallic getter material having a metallic surface capable of chemically adsorbing gas molecules. As the metal getter material 63, a non-evaporative zirconium-based (Zr-Al, Zr-V-Fe, etc.) getter material, or an evaporative metal such as Ti, Ba, Mg, or alloys such as BaAl, MgAl is used. Because the second gas adsorbent 62 contains the metal getter material 63, it can effectively adsorb gas molecules such as H2O, N2, O2, H2, and CO2.

[0057] For the metal getter material 63, an evaporative metal getter material 63 is preferred, and for example, an alloy containing barium and aluminum can be used. When a predetermined amount of heat is applied to the evaporative metal getter material 63, it evaporates and adheres to the second surface 12 of the first glass plate 1A. The metal getter material 63 adhering to the second surface 12 adsorbs various gas molecules scattered in the gap V. Since the adsorption capacity of the metal getter material 63 adhering to the second surface 12 is proportional to the area over which the metal getter material 63 adheres to the second surface 12, it is preferable for the evaporated metal getter material 63 to adhere over a wide area of ​​the second surface 12 in the glass panel P.

[0058] Thus, the gas adsorbent 6 is arranged such that the first gas adsorbent 61 and the second gas adsorbent 62 are spaced apart on the third surface 13 (an example of one surface) of the pair of plate surfaces 12 and 13 of the pair of glass plates 1A and 1B that face each other on the side of the gap V, and are spaced apart from the third surface 13 (an example of the other surface) of the pair of plate surfaces 12 and 13.

[0059] The first gas adsorbent 61 is arranged in a continuous single region on the third surface 13 of the second glass plate 1B. If the first gas adsorbent 61 were arranged in multiple regions on the third surface 13 of the second glass plate 1B, the appearance of the glass panel P would be greatly affected by the presence of the first gas adsorbent 61 in multiple regions. Furthermore, if the distance D1 between the peripheral sealing material 5 and the spacer 2 were increased in order to arrange the first gas adsorbent 61, the holding strength of the pair of glass plates 1A and 1B would decrease in that area. As in this embodiment, by arranging the first gas adsorbent 61 in a continuous single region on the third surface 13 of the second glass plate 1B, the appearance effect of the first gas adsorbent 61 on the glass panel P can be suppressed, and the decrease in the holding strength of the pair of glass plates 1A and 1B can also be suppressed.

[0060] The second gas adsorbent 62 is composed of an evaporative metal getter material 63 (for example, an alloy containing barium and aluminum). When the evaporative metal getter material 63 is heated and activated, the barium sublimes. As a result, the adsorbent molecules dispersed in the gap V by the sublimation of barium adsorb the gas, thereby reliably improving the gas adsorption performance of the gas adsorbent 6 in the glass panel P. Here, to activate the evaporative metal getter material 63, which is an alloy containing barium and aluminum, it is necessary to heat it to a high temperature of 800°C or higher. The second gas adsorbent 62 (evaporative metal getter material 63) is preferably placed close to the peripheral sealant 5 in order to minimize its impact on the appearance of the glass panel P. However, if the melting point of the peripheral sealant 5 is low, there is a possibility that the peripheral sealant 5 will melt when the alloy containing barium and aluminum, which is the evaporative metal getter material 63, is heated, so the second gas adsorbent 62 (evaporative metal getter material 63) cannot be placed close to the peripheral sealant 5.

[0061] Therefore, glass frit, which has a higher melting point than solder, is preferred as the peripheral sealant 5. Glass frit is a glassy inorganic material, and its softening point can be set in the range of 300°C to 950°C, allowing for the selection of its composition according to the application. For this reason, even when heated to activate the alloy containing barium and aluminum, which is the evaporation-type metal getter material 63, the glass frit, which is the peripheral sealant 5, is not easily melted. Thus, by using glass frit as the peripheral sealant 5, the alloy containing barium and aluminum, which is the second gas adsorbent 62 (evaporation-type metal getter material 63), can be placed near the peripheral sealant 5 in the glass panel P, where it has less impact on the appearance.

[0062] The first gas adsorbent 61 is typically composed of a zeolite-based nonmetallic getter material in powder form. According to this embodiment, the first gas adsorbent 61 is composed of a zeolite-based nonmetallic getter material having a porous structure and an inorganic binder material that connects the nonmetallic getter material. As a result, the powdered nonmetallic getter material is stably held by the inorganic binder material in the first gas adsorbent 61. This eliminates the need to cover the nonmetallic getter material with a packaging material, and the glass panel P can stably ensure the gas adsorption performance of the gas adsorbent 6 with a simple configuration. However, if the binder material contained in the first gas adsorbent 61 is composed of an organic material, gas will be generated from the organic material when the first gas adsorbent 61 is heated to its activation temperature. Therefore, gas may remain in the gaps V in the glass panel P, potentially reducing its thermal insulation performance. On the other hand, in this embodiment, since the first gas adsorbent 61 includes an inorganic binder material, no gas is generated from the inorganic binder material even when the first gas adsorbent 61 is heated to its activation temperature. As a result, the heat insulation performance of the glass panel P can be maintained.

[0063] Furthermore, in this embodiment, the gas adsorbent 6 is positioned on the third surface 13 (an example of one surface) of a pair of opposing plate surfaces 12 and 13 of the pair of glass plates 1A and 1B on the side of the gap V, and is spaced apart from the second surface 12 (an example of the other surface). As a result, the gas adsorbent 6 can secure a large contact area with the gas without the contact area with the gas being reduced by the second surface 12 (the other surface) of the glass plate 1A. Consequently, the glass panel P can stably ensure the gas adsorption performance of the gas adsorbent 6 with a simple configuration.

[0064] As shown in Figure 3, in the glass panel P, the pair of glass plates 1A and 1B (only the second glass plate 1B is shown in Figure 3) are formed in a rectangular shape. The pair of glass plates 1A and 1B have left and right long sides 3a and 3b extending in the vertical direction and upper and lower short sides 3c and 3d extending in the left and right direction. In this embodiment, the first gas adsorbent 61 is placed on the lower short side 3d of the glass panel P and is arranged linearly along the third surface 13 of the second glass plate 1B (see Figure 2). Although not shown, the first gas adsorbent 61 may also be placed on the upper short side 3c of the glass panel P.

[0065] When a pair of glass plates 1A and 1B are formed in a rectangular shape and have long sides 3a and 3b and short sides 3c and 3d, the first gas adsorbent 61 can be placed on the long sides 3a and 3b or the short sides 3c and 3d to suppress its impact on the appearance of the glass panel P. In this embodiment, since the first gas adsorbent 61 is placed on the short side 3d (or 3c), the length of the first gas adsorbent 61 placed on the pair of glass plates 1A and 1B can be shortened. As a result, the impact of the first gas adsorbent 61 on the appearance of the glass panel P can be further suppressed.

[0066] Furthermore, in the glass panel P, the first gas adsorbent 61, the second gas adsorbent 62, and the spacer 2 are positioned at different locations when viewed perpendicular to the surface of the pair of glass plates 1A and 1B. Therefore, the gas adsorbent 6 is positioned at a different location from the spacer 2 in the depressurized gap V, and its surface area is ensured. As a result, in the glass panel P, which is a depressurized double-layered glass panel, the gas adsorption performance of the gas adsorbent 6 can be stably ensured with a simple configuration.

[0067] Furthermore, as in this embodiment, by arranging the first gas adsorbent 61 between the peripheral sealing material 5 and the spacer 2, the first gas adsorbent 61 can be positioned close to the outer edge 3 of the glass panel P. This makes it possible to suppress the visual impact of the gas adsorbent 6 on the glass panel P.

[0068] If the first gas adsorbent 61 is placed between a plurality of adjacent spacers 2,2, it would be necessary to increase the spacing between the adjacent spacers 2,2 to match the dimensions of the first gas adsorbent 61, which could reduce the holding strength of the pair of glass plates 1A,1B in the glass panel P. On the other hand, as in this embodiment, if the first gas adsorbent 61 is placed between the peripheral sealing material 5 and the spacers 2, the spacing between the plurality of adjacent spacers 2,2 can be set to a constant value by a predetermined pitch Pd, making it easier for the glass panel P to maintain the holding strength of the pair of glass plates 1A,1B between the plurality of spacers 2,2. This makes it possible to suppress a decrease in the holding strength of the pair of glass plates 1A,1B in the glass panel P.

[0069] Preferably, the first gas adsorbent 61 has a distance D1 between the peripheral sealant 5 and the spacer 2 of 40 mm or less, and the distance D2 between the first gas adsorbent 61 and the peripheral sealant 5, and the distance D3 between the first gas adsorbent 61 and the spacer 2 are both 1 mm or more.

[0070] In the glass panel P, if the distance D1 between the peripheral sealant 5 and the spacer 2 becomes too large, the holding strength of the pair of glass plates 1A and 1B decreases. By keeping the distance D1 between the peripheral sealant 5 and the spacer 2 where the first gas adsorbent 61 is placed at 40 mm or less, the decrease in the holding strength of the pair of glass plates 1A and 1B in the glass panel P can be suppressed. Furthermore, by keeping the distance D2 between the first gas adsorbent 61 and the peripheral sealant 5, and the distance D3 between the first gas adsorbent 61 and the spacer 2 at 1 mm or more, the first gas adsorbent 61 can be placed at a distance from the peripheral sealant 5 and the spacer 2. This allows the first gas adsorbent 61 to secure a large contact area with the gas on its surface. As a result, the gas adsorption performance of the first gas adsorbent 61 can be stably ensured in the glass panel P.

[0071] Preferably, the first gas adsorbent 61 is arranged linearly along the surface of the third surface 13, has a width W (see Figure 2) of 1 mm or more and 15 mm or less, a length L (see Figure 3) of 1 mm or more and 2000 mm or less, and a height H (see Figure 2) relative to the surface (third surface 13) of 10 μm or more and 190 μm or less.

[0072] In this way, the first gas adsorbent 61 is arranged linearly along the surface of the third surface 13 of the second glass plate 1B, and the width W and length L of the first gas adsorbent 61 are within a predetermined range, so that the first gas adsorbent 61 can fully exhibit its gas adsorption performance in the glass panel P and the impact on appearance can be suppressed. If the width of the first gas adsorbent 61 is less than 1 mm, it will not be able to fully exhibit its gas adsorption performance, and if the width exceeds 15 mm, the first gas adsorbent 61 will be too conspicuous and will spoil the appearance of the glass panel P. Also, if the length L of the first gas adsorbent 61 is less than 1 mm, it will not be able to fully exhibit its gas adsorption performance, and if the length exceeds 2000 mm, the first gas adsorbent 61 will be too conspicuous and will spoil the appearance of the glass panel P. Furthermore, if the height H of the first gas adsorbent 61 relative to the plate surface (third surface 13) is 10 μm or more and 190 μm or less, the first gas adsorbent 61 can fully exhibit its gas adsorption performance in the glass panel P, and it becomes less likely to come into contact with the second surface 12 of the first glass plate 1A, thus avoiding the first glass plate 1A being damaged by contact with the high-hardness first gas adsorbent 61. On the other hand, if the height H of the first gas adsorbent 61 is less than 10 μm, it cannot fully exhibit its gas adsorption performance, and if the height H exceeds 190 μm, the first gas adsorbent 61 is more likely to come into contact with the second surface 12 of the first glass plate 1A when an impact or the like acts on the first glass plate 1A, and if the first gas adsorbent 61 comes into contact with the second surface 12 of the first glass plate 1A, there is a risk that the first glass plate 1A will be damaged by the high-hardness first gas adsorbent 61. Furthermore, if the height of the first gas adsorbent 61 exceeds 190 μm, and the first gas adsorbent 61 is in contact with both sides (second surface 12 and third surface 13) of the pair of glass plates 1A and 1B, heat transfer will occur between the pair of glass plates 1A and 1B due to the first gas adsorbent 61, which will reduce the thermal insulation performance of the glass panel P.

[0073] Furthermore, in this embodiment, since the inorganic binder material contained in the first gas adsorbent 61 is made of a material having gas adsorption properties, gas adsorption by the first gas adsorbent 61 in the gap V of the glass panel P is further promoted by the inorganic binder material. As a result, the thermal transmittance (U value) of the gap V of the glass panel P is reduced, and thus the thermal insulation performance can be further improved.

[0074] Furthermore, in this embodiment, the gas adsorbent 6 further includes a metal getter material 63 (second gas adsorbent 62) in addition to the non-metallic getter material (first gas adsorbent 61), and the metal getter material 63 (second gas adsorbent 62) is positioned differently from the non-metallic getter material (first gas adsorbent 61). As a result, the gas adsorbent 6 can also adsorb gas by the metal getter material 63 (second gas adsorbent 62). Specifically, the non-metallic getter material adsorbs gas in the short term by physical adsorption, while the metal getter material 63 adsorbs gas in the long term by chemical adsorption, thus the two materials have different effects. In this way, the gas adsorption performance of the gas adsorbent 6 can be further improved by having a non-metallic getter material (first gas adsorbent 61) and a metal getter material 63 (second gas adsorbent 62) that exhibit different gas adsorption performance for different periods.

[0075] Furthermore, the metal getter material (second gas adsorbent 62) and the non-metal getter material (first gas adsorbent 61) may be placed on the same surface (second surface 12 or third surface 13) of the pair of glass plates 1A and 1B, as long as they are in different positions when viewed perpendicular to the surface (e.g., first surface 11). Alternatively, the non-metal getter material may be placed on one surface of the second surface 12 and third surface 13, and the metal getter material 63 may be placed on the other surface of the second surface 12 and third surface 13. As described above, since the second gas adsorbent 62 is composed of an evaporative metal getter material 63, it will sublimate when the evaporative metal getter material 63 is heated and activated. If this metal getter material 63 adheres to the first gas adsorbent 61, the gas adsorption performance may decrease. However, by placing the first gas adsorbent 61 and the second gas adsorbent 62 in different positions, the gas adsorption performance of the first gas adsorbent 61 can be maintained.

[0076] Furthermore, in this embodiment, since the metal getter material 63 constituting the second gas adsorbent 62 is an evaporative metal getter material, heating and activating the metal getter material 63 causes a portion of the metal getter material 63 to evaporate, releasing the adsorbed molecules, which then disperse into the gap V. As a result, the second gas adsorbent 62 can effectively adsorb the gas in the gap V using these adsorbed molecules. Consequently, the gas adsorption performance of the gas adsorbent 6 in the glass panel P can be further improved.

[0077] The glass panel P is manufactured based on the flowchart shown in Figure 4. First, two glass sheets (not shown) of a predetermined thickness made of float glass are cut to predetermined dimensions, for example, 1200 mm x 900 mm, to prepare glass plates 1A and 1B of the same shape and size (step S31). Next, a suction hole 4 is drilled into the first glass plate 1A near one of its four corners (step S32), and a groove-shaped housing hole 18 is drilled into the second glass plate 1B at a position opposite the suction hole 4 (step S33) (drilling step).

[0078] Next, in a space where the air contamination level can be controlled chemically or physically, such as a cleanroom or chemical cleanroom, the pair of glass plates 1A and 1B are cleaned using a liquid cleaning method (step S34) (cleaning step). The cleaning solution used in this liquid cleaning method contains, for example, an alkaline detergent or ozonated water. The cleaning solution also contains an abrasive. As the abrasive, for example, fine particles mainly composed of cerium oxide are used.

[0079] Next, the second glass plate 1B is supported almost horizontally, spacers 2 are arranged at a constant pitch Pd, and the evaporative metal getter material 63 is placed in the receiving hole 18, while the first gas adsorbent 61 is applied to a predetermined location on the second glass plate 1B (step S35) (getter material placement step). After that, the first glass plate 1A is placed on the second glass plate 1B from above to pair the pair of glass plates 1A and 1B (step S36). The first gas adsorbent 61 is made by powdering a zeolite-based non-metallic getter material, and then adding kaolin, smectite, and water to make a paste.

[0080] Furthermore, the paired glass plates 1A and 1B are kept nearly horizontal, and the outer edges of the paired glass plates 1A and 1B are sealed using glass frit with a softening point of 400°C to 500°C as the peripheral sealant 5 (step S37) (sealing step). Solder with a melting point of 250°C or less may be used as the peripheral sealant 5. For example, solder having a composition of, for example, 91.2Sn-8.8Zn (eutectic point temperature: 198°C) may be used as the peripheral sealant 5.

[0081] If the peripheral sealant 5 is glass frit, the pair of glass plates 1A and 1B and the peripheral sealant 5 are heated to approximately 400°C to weld them together. This seals the outer edges of the pair of glass plates 1A and 1B with the peripheral sealant 5 (glass frit).

[0082] If the peripheral sealant 5 is solder, in step S37, the moving mechanism (not shown) is moved at a constant speed along the peripheral edge V1 of the gap V between the pair of glass plates 1A and 1B on a rail member (not shown), and an introduction plate (not shown) is inserted into the gap V from the groove portion 19 of the pair of glass plates 1A and 1B (see Figure 1). As a result, the peripheral sealant 5 penetrates through the introduction plate over the entire peripheral edge V1 of the pair of glass plates 1A and 1B, and the peripheral edge V1 of the pair of glass plates 1A and 1B is airtightly sealed by the peripheral sealant 5. Here, the groove portion 19 is provided at the corner of the glass panel P, and the corner on the gap V side of the pair of glass plates 1A and 1B is chamfered to facilitate insertion of the introduction plate into the gap V. Here, the pair of glass plates 1A and 1B and the peripheral sealant 5 are heated to approximately 200°C to weld them together. As a result, the outer edges of the pair of glass plates 1A and 1B are sealed by the peripheral sealant 5 (solder).

[0083] In the next step S38, a vacuum is evacuated to expel the gas from the gap V to the outside in order to reduce the pressure in the gap V to 1.33 Pa or less. Specifically, an exhaust cup is attached to the main surface of the first glass plate 1A on the atmospheric side so as to cover the suction hole 4 near the suction hole 4, and the gas from the gap V is sucked out by a rotary pump or turbomolecular pump (not shown) connected to this exhaust cup.

[0084] However, the pump used in step S38 is not limited to the rotary pump or turbomolecular pump mentioned above; any pump that can be connected to an exhaust cup and is capable of suction is acceptable.

[0085] The activation of the first gas adsorbent 61 is performed before, during, or in parallel with the depressurization process. For example, if the peripheral sealant 5 is glass frit, the nonmetallic getter material of the first gas adsorbent 61 is heated to approximately 400°C to activate it after sealing with the peripheral sealant 5. If the peripheral sealant 5 is solder, the nonmetallic getter material of the first gas adsorbent 61 is heated to approximately 200°C to activate it after sealing with the peripheral sealant 5. Alternatively, the nonmetallic getter material of the first gas adsorbent 61 may be activated while the gap V is being depressurized at a high temperature, or the nonmetallic getter material of the first gas adsorbent 61 may be activated separately by local heating.

[0086] Next, a suction hole sealing material 15 is dropped to cover the suction hole 4, causing the glass surface near the suction hole 4 to adhere to the suction hole sealing material 15 and seal the suction hole 4 (step S39). If the suction hole sealing material 15 is glass frit, the suction hole sealing material 15 is heated to approximately 300°C to seal the suction hole 4. If the suction hole sealing material 15 is solder, the suction hole sealing material 15 is heated to approximately 200°C to seal the suction hole 4. This seals the gap V formed between the pair of glass plates 1A and 1B.

[0087] Furthermore, of the steps described above, from cleaning the main surfaces of the pair of glass plates 1A and 1B (step S34) to bonding the glass surface near the suction hole 4 with the suction hole sealing material 15 and sealing it (step S39), all are carried out in an atmospheric environment.

[0088] Next, the evaporative metal getter material 63 contained in the containment hole 18 is locally heated using a high-frequency device (not shown) (step S40). Specifically, the evaporative metal getter material 63 is activated (flashed) by maintaining it at 800°C to 1200°C for about 15 seconds, causing the metal getter material 63 to be deposited onto the inner main surface (second surface 12) of the glass plate 1A. The metal getter material 63 attached to the second surface 12 of the glass plate 1A comes into contact with various gas molecules scattered in the gap V, adsorbs and removes gases such as water, CO, CO2, N2, H2, and O2 consisting of those gas molecules, and the process is completed.

[0089] According to this embodiment, after sealing the outer edges of the pair of glass plates 1A and 1B (step S37) and sealing the suction hole 4 (step S39), the evaporative metal getter material 63 is locally heated (step S40). As a result, the metal getter material 63 adhering to the second surface 12 of glass plate 1A can adsorb gas molecules scattered in the gap V, and the degree of reduced pressure in the gap V can be maintained for a long period of time. Furthermore, even if the pair of glass plates 1A and 1B are not sufficiently cleaned, gas molecules can be adsorbed, and the degree of reduced pressure in the gap V can be maintained for a long period of time. Moreover, since the metal getter material 63 (second gas adsorbent 62) and the non-metallic getter material (first gas adsorbent 61) are in different positions, the first gas adsorbent 61 can effectively adsorb hydrocarbon gases (CH4, C2H6, etc.) and ammonia gas (NH3), which are difficult to adsorb by the metal getter material 63.

[0090] Glass panel P can be used in a variety of applications, such as windows in buildings, automobiles, ships, etc., or doors and walls of various devices such as refrigerators and heating equipment.

[0091] [Modified version of the first embodiment] As shown in Figure 5, in the glass panel P, the first gas adsorbent 61 may be placed on the second surface 12 of the first glass plate 1A. In this case as well, since the first gas adsorbent 61 is applied to the second surface 12, pairing of the pair of glass plates 1A and 1B is easy.

[0092] [Second Embodiment] As shown in Figure 6, in the glass panel P, the first gas adsorbent 61 may be placed between a plurality of adjacent spacers 2, 2 on the third surface 13 of the second glass plate 1B.

[0093] In a glass panel P having multiple spacers 2, if the distance D1 (see Figure 2) between the peripheral sealant 5 and the spacer 2 adjacent to the peripheral sealant 5 is smaller than the width W of the first gas adsorbent 61, the first gas adsorbent 61 cannot be placed between them. In such cases, as in the second embodiment, the first gas adsorbent 61 can be reliably placed on the glass panel P by placing it between multiple adjacent spacers 2. The first gas adsorbent 61 can be placed, for example, between a spacer 2 adjacent to the peripheral sealant 5 and a spacer 2 adjacent to that spacer 2, thereby being placed near the outer edge 3 of the pair of glass plates 1A and 1B. This makes it possible to suppress the visual impact of the first gas adsorbent 61 on the glass panel P.

[0094] Preferably, the first gas adsorbent 61 has a distance D4 (approximately the same as the pitch Pd) between adjacent spacers 2,2 of 40 mm or less, and the distances D5 and D6 between the first gas adsorbent 61 and adjacent spacers 2,2 are both 1 mm or more.

[0095] In the glass panel P, if the distance D4 between adjacent spacers 2,2 becomes too large, the holding strength of the pair of glass plates 1A,1B in the glass panel P decreases. By keeping the distance D4 between adjacent spacers 2,2 at 40mm or less, the decrease in the holding strength of the pair of glass plates 1A,1B in the glass panel P can be suppressed. Furthermore, by keeping the distances D5 and D6 between adjacent spacers 2,2 of the first gas adsorbent 61 at 1mm or more, the first gas adsorbent 61 can be positioned at a distance from the adjacent spacers 2,2. This allows the first gas adsorbent 61 to secure a large contact area with the gas on its surface. As a result, the gas adsorption performance of the first gas adsorbent 61 can be stably ensured in the glass panel P.

[0096] [Modified example of the second embodiment] As shown in Figure 7, in the glass panel P, the first gas adsorbent 61 may be placed on the second surface 12 of the first glass plate 1A. In this case as well, since the first gas adsorbent 61 is applied to the second surface 12, pairing of the pair of glass plates 1A and 1B is easy.

[0097] [Example Test] Figure 8 shows the glass panel P1 used in Test 1 and Test 2. The glass panel P1 consists of a pair of glass plates 1A and 1B, both 300 mm square in shape and made of float glass with a thickness of 3.1 mm. The spacers 2 placed between the pair of glass plates 1A and 1B have a diameter of 0.5 mm and a height of 0.2 mm, and the pitch Pd of the multiple spacers 2 is set to 40 mm. A suction hole 4 is formed in the first glass plate 1A, and a first accommodation hole 21 for accommodating a metal getter material 63 and a second accommodation hole 22 for accommodating a non-metallic getter material are formed on the third surface 13 of the second glass plate 1B. The first accommodation hole 21 is a bottomed cylindrical hole formed in the second glass plate 1B at a position 50 mm above and to the right of the lower left corner C1. The second accommodation hole 22 is a bottomed cylindrical hole formed in the second glass plate 1B at a position 50 mm above and to the left of the lower right corner C2. The first housing hole 21 and the second housing hole 22 both have a diameter of 6 mm and a depth of 1 mm.

[0098] The peripheral sealant 5 that seals the periphery of the glass panel P1 and the suction hole sealant 15 that seals the suction hole 4 are both Sn-Zn alloy "solder" with a melting point of 200°C and a density of 0.0073 (g / mm³). 3 The specific heat is 243,000 (J / g·K). The peripheral sealing temperature, vacuum evacuation temperature, and suction hole sealing temperature are all 200°C or lower.

[0099] [Test 1] In the glass panel of Sample 1, 5 mg of evaporative barium-aluminum (Ba-Al) alloy was contained in the first containment hole 21 as a metallic getter material, and the second containment hole 22 (non-metallic getter material) was not present. The glass panel of Sample 2 included the configuration of the first containment hole 21 of Sample 1, and further contained 1 mg to 20 mg of pelletized zeolite as a non-metallic getter material in the second containment hole 22. The glass panel of Sample 3 included the configuration of the first containment hole 21 of Sample 1, and further contained a getter material in the second containment hole 22 that was made into a paste by mixing zeolite with the inorganic binder material kaolin. When kaolin (inorganic binder material) is mixed with zeolite (non-metallic getter material), the mixing ratio of these with water is set to zeolite 10: kaolin 1: water 16 to 18, which makes it possible to make it into a paste that can be applied to the surface of the glass panel. Therefore, the glass panel of sample 3 contains 0.1 mg to 2 mg of kaolin. Sample 4 includes the configuration of the first containment hole 21 of sample 1, and further contains only kaolin in the second containment hole 22. The glass panel of sample 4 contains 1 mg to 20 mg of kaolin.

[0100] The thermal transmittance (U-value) was measured for each of the samples 1 to 4. The results of Test 1 are shown in Figure 9. In Figure 9, the barium-aluminum (Ba-Al) alloy is abbreviated as "Ba" for samples 1 to 4.

[0101] [Results of Test 1] As shown in Figure 9, the U value for sample 1 is approximately 0.82 (W / m²). 2 K), in sample 2 it was approximately 0.72 (W / m 2 K), in sample 3 it was approximately 0.64 (W / m 2 K), in sample 4 it was approximately 0.78 (W / m 2 The result was K). From the above results, it was demonstrated that the glass panel of sample 3, which contained a gas adsorbent made by mixing an inorganic binder material (kaolin) with a nonmetallic getter material (zeolite), had the lowest U value. From these findings, it can be seen that the gas adsorption performance of the first gas adsorbent 61 is improved by further including an inorganic binder material in addition to the nonmetallic getter material.

[0102] [Exam 2] Sample 5 corresponds to Sample 1, and Sample 6 corresponds to Sample 3. Sample 7 is obtained by adding smectite as a dispersant to the paste-like zeolite and kaolin of Sample 3. For Samples 6 and 7, the total amount of zeolite, kaolin, and smectite added was varied, and the thermal transmittance (U-value) of each was measured. The results of Test 2 are shown in Figure 10. In Figure 10, barium-aluminum (Ba-Al) alloy is abbreviated as "Ba" for Samples 5 to 7.

[0103] When mixing zeolite (non-metallic getter material) with kaolin (inorganic binder material) or smectite (dispersant), the mixture can be made into a paste-like consistency that can be applied to the surface of a glass panel P by using a mixing ratio of zeolite 10:kaolin 1:smectite 1:water 16-18. In sample 6, the total amounts of zeolite and kaolin added were 4 mg and 16 mg, respectively, with a mixing ratio of zeolite 10:kaolin 1. According to this ratio, of the total added amount of 4 mg, zeolite accounts for 3.63 mg (4 mg × 10 / 11) and kaolin for 0.37 mg (4 mg × 1 / 11). Also, of the total added amount of 16 mg, zeolite accounts for 14.54 mg (16 mg × 10 / 11) and kaolin for 1.46 mg (16 mg × 1 / 11).

[0104] In sample 7, the total amounts of zeolite, kaolin, and smectite added were 7 mg and 9 mg, respectively, with a mixing ratio of zeolite 10: kaolin 1: smectite 1. According to this mixing ratio, of the total added amount of 7 mg, zeolite accounted for 5.64 mg (7 mg × 10 / 12), kaolin for 0.58 mg (7 mg × 1 / 12), and smectite for 0.58 mg (7 mg × 1 / 12). Also, of the total added amount of 9 mg, zeolite accounted for 7.50 mg (9 mg × 10 / 12), kaolin for 0.75 mg (9 mg × 1 / 12), and smectite for 0.75 mg (9 mg × 1 / 12). [Results of Test 2] As shown in Figure 10, in Sample 6, when a total of 4 mg of zeolite and kaolin was added, the U-value was approximately 0.82 (W / m at the initial stage (the glass panel of Sample 5) 2 K) decreased significantly to approximately 0.66 (W / m 2 K). For Sample 6, when the total added amount of zeolite and kaolin was increased to 16 mg, the U-value became approximately 0.64 (W / m 2 K), and the decrease in the U-value slowed down. In Sample 7, when a total of 7 mg of zeolite, kaolin, and smectite was added, the U-value decreased from approximately 0.82 at the initial stage (the glass panel of Sample 5) to approximately 0.72 (W / m 2 K). For Sample 7, when the total added amount of zeolite, kaolin, and smectite was increased to 9 mg, the U-value decreased to approximately 0.63 (W / m 2 K). From the above results, it was demonstrated that the U-value is the lowest in the glass panels of Sample 6 containing the gas adsorbent material in which a predetermined amount of the inorganic binder material (kaolin) is mixed into the non-metallic getter material (zeolite), and Sample 7 containing the gas adsorbent material in which a predetermined amount of the inorganic binder material (kaolin) and the dispersant (smectite) are mixed into the non-metallic getter material (zeolite). Although Sample 7 requires a slightly larger coating amount than Sample 6, the dispersant facilitates handling of the first gas adsorbent material 61.

[0105] [Other Embodiments] (1) In the above embodiment, an example is shown in which the first gas adsorbent material 61 is arranged in a linear shape along the plate surface of one surface (the second surface 12 or the third surface 13) of the pair of glass plates 1A, 1B, but the first gas adsorbent material 61 may have a shape other than linear, such as a circular shape or a square shape. Further, in the above embodiment, an example is shown in which the first gas adsorbent material 61 is arranged in a single continuous region on one surface (the second surface 12 or the third surface 13) of the pair of glass plates 1A, 1B, but the first gas adsorbent material 61 may be arranged dispersedly in a plurality of regions on one surface (the second surface 12 or the third surface 13).

[0106] (2) In the above embodiment, an example was shown in which the first gas adsorbent 61 is placed on the short sides 3c and 3d of the rectangular glass panel P, but the first gas adsorbent 61 may also be placed on the long sides 3a and 3b of the rectangular glass panel P.

[0107] (3) In the above embodiment, an example was shown in which an evaporative metal getter material 63 was used as the second gas adsorbent material 62. However, the second gas adsorbent material 62 is not limited to this, and a non-evaporative metal getter material 63 that adsorbs and removes gas molecules when activated by heating may also be used. Furthermore, the second gas adsorbent material 62 may be a combination of a non-evaporative metal getter material and an evaporative metal getter material, and the second gas adsorbent material 62 (metal getter material 63 and receiving holes 18) may be arranged in multiple locations on the glass panel P. Multiple second gas adsorbents 62 may be arranged on one or both of the second surface 12 and the third surface 13 of the pair of glass plates 1A and 1B.

[0108] (4) In the above embodiment, an example was shown in which the Low-E film 17 is formed on the third surface 13 of the second glass plate 1B in the glass panel P, but the Low-E film 17 may also be formed on the second surface 12 of the first glass plate 1A. [Industrial applicability]

[0109] This invention is widely applicable to double-glazed glass panels. [Explanation of symbols]

[0110] 1A: First glass plate 1B: Second glass plate 2: Spacer (spacing member) 3: Outer edge 3a, 3b: Long side 3c, 3d: Short side 4: Suction hole 5: Peripheral sealant 6: Gas adsorbent 11: 1st page 12:Second side 13:Third side 14:Side 4 15: Suction hole sealing material 18: Containment port 61: First gas adsorbent 62: Second gas adsorbent 63: Metal Getter Material 64: Ring-shaped container H: Height of the first gas adsorbent L: Length of the first gas adsorbent P: Glass panel (double-glazed glass panel) V: Gap W: Width of the first gas adsorbent

Claims

1. A pair of opposing glass plates, A peripheral sealant is provided around the entire outer edge of the pair of glass plates, forming a sealed gap between the pair of glass plates. A plurality of spacing-maintaining members are arranged in the gap, A gas adsorbent is placed on one side of the pair of glass plates that face each other on the side of the gap, and is spaced apart from the other side of the pair of glass plates, The device comprises a suction hole sealing material that seals the suction hole in either of the glass plates when the gap is depressurized through the suction hole that penetrates from the front to the back, The gas adsorbent comprises a zeolite-based nonmetallic getter material having a porous structure, an inorganic binder material connecting the nonmetallic getter materials, and a metallic getter material. The metal getter material is positioned opposite the suction hole, In a view perpendicular to the surface of the panel, the suction hole sealing material has a portion that overlaps with the metal getter material in a multilayer glass panel.

2. The double-glazed glass panel according to claim 1, wherein the gas adsorbent and the spacing member are arranged at different positions when viewed perpendicular to the plate surface.

3. The double-layered glass panel according to claim 1 or 2, wherein the gas adsorbent is disposed between the peripheral sealing material and the spacing member.

4. The double-glazed glass panel according to claim 1 or 2, wherein the gas adsorbent is arranged between a plurality of adjacent spacing members.

5. The double-glazed glass panel according to claim 3, wherein the distance between the peripheral sealing material and the spacing member is 40 mm or less, and the distance between the gas adsorbent and the peripheral sealing material, and the distance between the gas adsorbent and the spacing member are both 1 mm or more.

6. The double-glazed glass panel according to claim 4, wherein the gas adsorbent material has a distance of 40 mm or less between adjacent spacing members, and the distance between the gas adsorbent material and adjacent spacing members is 1 mm or more in all cases.

7. The double-glazed glass panel according to any one of claims 1 to 6, wherein the gas adsorbent is arranged linearly along the surface of the plate on one side, has a width of 1 mm or more and 15 mm or less, a length of 1 mm or more and 2000 mm or less, and has a height of 10 μm or more and 190 μm or less relative to the plate surface.

8. The multi-layer glass panel according to any one of claims 1 to 7, wherein the inorganic binder material is a material having gas adsorption properties.

9. The double-glazed glass panel according to any one of claims 1 to 8, wherein the gas adsorbent is arranged in a continuous single region on one of the surfaces.

10. The pair of glass plates are formed in a rectangular shape and have a long side and a short side. The double-glazed glass panel according to any one of claims 1 to 9, wherein the gas adsorbent is disposed within the gap portion on the side of the short side portion.

11. The double-glazed glass panel according to any one of claims 1 to 10, wherein the inorganic binder material contains a dispersant.

12. The double-glazed glass panel according to any one of claims 1 to 11, wherein the metal getter material and the non-metal getter material are arranged in different positions when viewed perpendicular to the surface of the panel.

13. The double-glazed glass panel according to claim 12, wherein the metal getter material is an evaporative metal getter material.

14. The double-glazed glass panel according to claim 13, wherein the evaporation-type metal getter material is composed of an alloy containing barium and aluminum, and the peripheral sealing material is glass frit.

Citation Information

Patent Citations

  • A method for bonding getter material to a surface used in electronic devices.

    JP2007511102A

  • Gas adsorbent, gas adsorbent manufacturing method, and the glass panel unit

    WO2016051788A1

  • Method for manufacturing gas absorption unit, method for manufacturing glass panel unit, and method for manufacturing fitting

    WO2019003997A1

  • Glass panel unit, fitting, and method for activating gas-absorbing body

    WO2019004174A1