Frame-mounted membrane electrode structure and method for manufacturing the same

The framed membrane electrode structure for fuel cells improves production efficiency by integrating a single adhesive application with joint and protective portions, addressing the inefficiencies of multiple adhesive points and enhancing durability.

JP7949091B2Active Publication Date: 2026-11-11HONDA MOTOR CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2025051076
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-03-26
Publication Date
2026-11-11
Estimated Expiration
2045-03-26

AI Technical Summary

Technical Problem

The production efficiency of framed membrane electrode structures for fuel cells is low due to the multiple application points of adhesive, which complicates the manufacturing process.

Method used

A framed membrane electrode structure with a resin frame and adhesive configuration that includes a joining portion and protective portion, allowing for a single application of adhesive to bond and protect the laminate and electrodes, using a method that involves coating and pressing steps to form joint and protective portions.

Benefits of technology

This approach reduces the number of adhesive applications, improves production efficiency, and minimizes material costs while effectively preventing foreign matter ingress, thus enhancing the durability and performance of the fuel cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007949091000001
    Figure 0007949091000001
  • Figure 0007949091000002
    Figure 0007949091000002
  • Figure 0007949091000003
    Figure 0007949091000003
Patent Text Reader

Abstract

The present invention provides a framed membrane electrode structure and a method for manufacturing a framed membrane electrode structure with improved production efficiency. [Solution] The adhesive 80 in the framed MEA10 has a joint portion 82 and a protective portion 84. The joint portion 82 joins the resin frame 60 and the MEA22. The protective portion 84 has a first protective portion 85a and a second protective portion 85b. The first protective portion 85a is integrally connected to the first joint portion 83a, which is part of the joint portion 82, and covers at least a part of the outer surface 71 of the laminate 29 and a part of the first end face 61a. The second protective portion 85b is integrally connected to the second joint portion 83b, which is another part of the joint portion 82, and covers at least a part of the outer surface 74 of the second electrode 30 and a part of the second end face 61b.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present disclosure relates to a framed membrane electrode assembly for a fuel cell and a method for manufacturing the same. BACKGROUND ART

[0002] A framed membrane electrode assembly used in a fuel cell includes a membrane electrode assembly and a resin frame that supports the membrane electrode assembly. As described in International Publication No. 2024 / 202862, the membrane electrode assembly and the resin frame are bonded via an adhesive.

[0003] As shown in Figure 4 of International Publication No. 2024 / 202862, the resin frame has a first end surface that is one surface in the thickness direction, and a second end surface that is the back surface of the first end surface. Of the membrane electrode assembly, the cathode electrode and the anode electrode each have a first gas diffusion layer and a second gas diffusion layer. In this configuration, the adhesive is applied to a first location, a second location, and a third location. The first location is the first end surface. The second location is around the outer side surface of the first gas diffusion layer. The third location is around the outer side surface of the second gas diffusion layer.

[0004] The adhesive applied to the first location is interposed between the electrolyte membrane and the first end surface, and bonds the electrolyte membrane and the first end surface. The adhesive applied to the second location covers a part of the first end surface and the side surface of the first gas diffusion layer. The adhesive applied to the third location covers a part of the second end surface and the side surface of the second gas diffusion layer. The adhesive applied to the second location and the third location respectively prevents foreign matter from entering from the side surface of the first gas diffusion layer and the side surface of the second gas diffusion layer. PRIOR ART DOCUMENTS PATENT DOCUMENTS

[0005] PATENT DOCUMENT 1 International Publication No. 2024 / 202862 SUMMARY OF INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION

[0006] There is a need to improve the production efficiency of framed membrane electrode structures.

[0007] This disclosure aims to solve the problems described above. [Means for solving the problem]

[0008] A first aspect of the present disclosure is a framed membrane electrode structure for a fuel cell, comprising a membrane electrode structure, a resin frame surrounding the outer periphery of the membrane electrode structure, and an adhesive for joining the membrane electrode structure and the resin frame, wherein the membrane electrode structure has a laminate of a first electrode and an electrolyte membrane, and a second electrode; the resin frame has a first end face which is one side in the thickness direction, a second end face which is the back surface of the first end face, and a through-hole that extends from the first end face to the second end face and in which the membrane electrode structure is arranged; the adhesive has a joining portion and a protective portion, the joining portion interposed between the laminate and the first end face and joining the laminate and the resin frame The framed film electrode structure has a bonding portion, a second bonding portion interposed between the second end face and the second electrode to bond the resin frame and the second electrode, and a third bonding portion integrally connected to the first bonding portion and the second bonding portion, and interposed between the laminate and the second electrode within the through-hole to bond the laminate and the second electrode, and the protective portion has a first protective portion integrally connected to the first bonding portion and covering at least a part of the outer surface of the laminate and a part of the first end face, and a second protective portion integrally connected to the second bonding portion and covering at least a part of the outer surface of the second electrode and a part of the second end face.

[0009] A second aspect of the present disclosure relates to a method for manufacturing a framed membrane electrode structure for a fuel cell, comprising a membrane electrode structure and a resin frame surrounding the outer periphery of the membrane electrode structure, comprising: a coating step of applying an adhesive to the electrolyte membrane in a laminate in which an electrolyte membrane is bonded to a first electrode; and a pressing step of sandwiching the resin frame between the laminate and the second electrode, and pressing the laminate, the resin frame and the second electrode between a first pressing die and a second pressing die, with the resin frame protruding from the outer surface of the laminate and the outer surface of the second electrode, wherein the resin frame has a first end surface which is one side in the thickness direction and a second end surface which is the back surface of the first end surface The present invention relates to a method for manufacturing a framed film electrode structure, wherein in the pressing step, the adhesive is flowed between the laminate and the first end face of the resin frame toward the outer circumference of the resin frame, causing the adhesive to reach the outer surface of the laminate and the portion of the first end face of the resin frame located outside the laminate to form a first protective portion, and the adhesive is flowed between the second electrode and the second end face of the resin frame toward the outer circumference of the resin frame, causing the adhesive to reach the outer surface of the second electrode and the portion of the second end face of the resin frame located outside the second electrode to form a second protective portion. [Effects of the Invention]

[0010] According to this disclosure, the number of times adhesive is applied to obtain a framed film electrode structure can be reduced. Therefore, the production efficiency of the framed film electrode structure can be improved. [Brief explanation of the drawing]

[0011] [Figure 1] Figure 1 is an exploded perspective view of a unit cell that makes up a fuel cell stack. [Figure 2] Figure 2 is a partially abbreviated longitudinal cross-sectional view along the line II-II in Figure 1. [Figure 3] Figure 3 is an exploded cross-sectional view of the main part of the pressing device. [Figure 4] Figure 4 is a schematic flow chart of a method for manufacturing a framed membrane electrode structure according to the present disclosure. [Figure 5]Figure 5 is a cross-sectional view of the main part showing the state in which the adhesive is flowing. [Figure 6] Figure 6 is a cross-sectional view of the main part showing the state after the adhesive has finished flowing. [Modes for carrying out the invention]

[0012] Hereafter, membrane electrode structures may be referred to as "MEA".

[0013] Figure 1 is an exploded perspective view of a unit cell 12 that constitutes a fuel cell stack. The unit cell 12 comprises a framed MEA 10 and a first separator 16 and a second separator 18 disposed on both sides of the framed MEA 10. The first separator 16 in the unit cell 12 and the second separator 18 in another unit cell 12 adjacent to the unit cell 12 are joined to each other to form a joining separator 20.

[0014] One end edge of the unit cell 12 in the direction of its long side (the end edge in the direction of arrow B1) is provided with an oxidizer gas supply port 42a, a cooling medium supply port 44a, and a fuel gas discharge port 46b. The oxidizer gas supply port 42a, the cooling medium supply port 44a, and the fuel gas discharge port 46b are arranged in the direction of the short side of the unit cell 12 (in the direction of arrow C).

[0015] The other edge of the longer side of the unit cell 12 (the edge in the direction of arrow B2) is provided with a fuel gas supply port 46a, a cooling medium discharge port 44b, and an oxidizer gas discharge port 42b. The fuel gas supply port 46a, the cooling medium discharge port 44b, and the oxidizer gas discharge port 42b are arranged in the direction of arrow C.

[0016] An oxidant gas (e.g., an oxygen-containing gas) flows through the oxidant gas supply port 42a in the direction of arrow A2. A cooling medium (e.g., pure water, ethylene glycol, oil, etc.) flows through the cooling medium supply port 44a in the direction of arrow A2. A fuel gas (e.g., a hydrogen-containing gas) flows through the fuel gas discharge port 46b in the direction of arrow A1.

[0017] Fuel gas flows through the fuel gas supply communication hole 46a in the direction of arrow A2. A cooling medium flows through the cooling medium discharge communication hole 44b in the direction of arrow A1. Oxidant gas flows through the oxidant gas discharge communication hole 42b in the direction of arrow A1.

[0018] In the first separator 16, an oxidant gas flow channel 50 extending in the long side direction (arrow B direction) of the unit cell 12 is provided on the surface 48a facing the framed MEA 10. The oxidant gas flow channel 50 communicates with the oxidant gas supply communication hole 42a and the oxidant gas discharge communication hole 42b. The oxidant gas flow channel 50 supplies oxidant gas to the first electrode 28.

[0019] In the second separator 18, a fuel gas flow channel 54 extending in the long side direction (arrow B direction) of the unit cell 12 is provided on the surface 52a facing the framed MEA 10. The fuel gas flow channel 54 communicates with the fuel gas supply communication hole 46a and the fuel gas discharge communication hole 46b. The fuel gas flow channel 54 supplies fuel gas to the second electrode 30.

[0020] As shown in Figure 1, in the joined separator 20, a cooling medium flow channel 56 is formed between the back surface 48b of the first separator 16 and the back surface 52b of the second separator 18. The cooling medium flow channel 56 communicates with the cooling medium supply communication hole 44a and the cooling medium discharge communication hole 44b.

[0021] The framed MEA 10 will be described. The framed MEA 10 includes an MEA (membrane-electrode assembly) 22 and a resin frame 60. The resin frame 60 is provided on the outer peripheral portion of the MEA 22 so as to protrude outward from the outer peripheral portion of the MEA 22 (the outer peripheral portion 70 of the laminate 29 and the outer peripheral portion 73 of the second electrode 30). That is, the resin frame 60 surrounds the outer periphery of the MEA 22.

[0022] As shown in Figure 2, the MEA22 has a first electrode 28, an electrolyte membrane 26, and a second electrode 30. The electrolyte membrane 26 is laminated on the first electrode 28 to form a laminate 29. Hereinafter, an example will be described in which the first electrode 28 is the cathode and the second electrode 30 is the anode, but the first electrode 28 may be the anode and the second electrode 30 may be the cathode.

[0023] The first electrode 28 has a first gas diffusion layer 34 and a first electrode catalyst layer 32. The second electrode 30 has a second gas diffusion layer 38 and a second electrode catalyst layer 36. Since the first gas diffusion layer 34, the first electrode catalyst layer 32, the second gas diffusion layer 38, and the first electrode catalyst layer 32 in the fuel cell stack are well known, a detailed description of each layer will be omitted.

[0024] The material of the electrolyte membrane 26 is, for example, a solid polymer electrolyte membrane (cation exchange membrane). The solid polymer electrolyte membrane is, for example, a thin film of perfluorosulfonic acid containing water. The electrolyte membrane 26 may also be an HC (hydrocarbon)-based electrolyte.

[0025] In the power generation region EF of MEA22, the laminate 29 and the second electrode 30 are joined to each other. Specifically, one surface of the electrolyte membrane 26 in the thickness direction, the first surface 26a, is joined to the first electrode catalyst layer 32. The other surface of the electrolyte membrane 26 in the thickness direction, the second surface 26b, is joined to the second electrode catalyst layer 36.

[0026] In the illustrated example, the resin frame 60 is a single plate. However, the resin frame 60 may be constructed by joining two plate materials together.

[0027] An illustrated example will be described. The resin frame 60, which is a single plate, has a first end face 61a and a second end face 61b. The first end face 61a is one side in the thickness direction. The second end face 61b is the back surface of the first end face 61a. The resin frame 60 further has a through opening 62. The through opening 62 extends along the thickness direction of the resin frame 60 and penetrates from the first end face 61a to the second end face 61b. Therefore, in the illustrated example, the resin frame 60 has a rectangular shape. The resin frame 60 has an inner circumference 64 which is around the through opening 62 and an outer circumference 66.

[0028] The MEA22 is positioned in the through-hole 62. As shown in Figure 2, in the resin frame 60, the inner circumference 64 surrounding the through-hole 62 is sandwiched between the outer circumference 70 of the laminate 29 and the outer circumference 73 of the second electrode 30. In this state, the framed MEA10 includes an adhesive 80 that joins the resin frame 60 and the MEA22. The adhesive 80 also serves to protect the electrolyte membrane 26. This point will be explained.

[0029] The adhesive 80 has a bonding portion 82 and a protective portion 84. The bonding portion 82 has a first bonding portion 83a, a second bonding portion 83b, and a third bonding portion 83c. The first bonding portion 83a is interposed around the entire circumference between the outer periphery 70 of the laminate 29 (the outer periphery of the electrolyte membrane 26) and the first end face 61a of the inner periphery 64 of the resin frame 60. For this reason, the first bonding portion 83a has an annular shape. The first bonding portion 83a hardens at this location, thereby bonding the laminate 29 and the resin frame 60.

[0030] The second bonding portion 83b is interposed around the entire circumference between the outer periphery 73 of the second electrode 30 (the outer periphery of the second electrode catalyst layer 36) and the second end face 61b on the inner periphery 64 of the resin frame 60. For this reason, the second bonding portion 83b has an annular shape. The second bonding portion 83b hardens at this location, thereby bonding the resin frame 60 and the second electrode 30.

[0031] The third bonding portion 83c is located within the through-hole 62, integrally connected to the first bonding portion 83a and the second bonding portion 83b. Therefore, the third bonding portion 83c is located further inward on the resin frame 60 compared to the first bonding portion 83a and the second bonding portion 83b. The third bonding portion 83c fills the space 75 between the laminate 29 and the second electrode 30 in the through-hole 62. In other words, the third bonding portion 83c hardens while being interposed around the entire circumference between the laminate 29 and the second electrode 30. Based on this, the third bonding portion 83c bonds the laminate 29 and the second electrode 30. In this case, the second surface 26b of the electrolyte membrane 26 in the laminate 29 and the second electrode catalyst layer 36 are bonded via the third bonding portion 83c.

[0032] The protective portion 84 of the adhesive 80 is the part that protects the electrolyte membrane 26. The protective portion 84 has a first protective portion 85a and a second protective portion 85b. The first protective portion 85a is integrally connected to the first bonding portion 83a and is exposed from the outer peripheral portion 70 of the laminate 29. The first protective portion 85a covers at least a part of the outer surface 71 of the laminate 29 and a part of the first end face 61a of the resin frame 60. As a result, the first protective portion 85a shields at least a part of the outer surface 71 of the laminate 29. The outer surface 71 of the laminate 29 refers to the surface extending along the thickness direction (first height direction) on the outer peripheral portion 70 of the laminate 29.

[0033] The direction perpendicular to the first end face 61a and away from the first end face 61a is defined as the first height direction. The first height direction is indicated by arrow X1. Although not mandatory, it is preferable that the dimension H1 along the first height direction (hereinafter referred to as "first height") in the first protective portion 85a is less than or equal to the thickness T1 of the laminate 29.

[0034] The second protective portion 85b is integrally connected to the second bonding portion 83b and is exposed from the outer periphery 73 of the second electrode 30. The second protective portion 85b covers at least a part of the outer surface 74 of the second electrode 30 and a part of the second end face 61b of the resin frame 60. As a result, the second protective portion 85b shields at least a part of the outer surface 74 of the second electrode 30. The outer surface 74 of the second electrode 30 refers to the surface extending along the thickness direction (second height direction) on the outer periphery 73 of the second electrode 30.

[0035] The direction perpendicular to the second end face 61b and away from the second end face 61b is defined as the second height direction. The second height direction is indicated by arrow X2. Although not mandatory, it is preferable that the dimension H2 along the second height direction (hereinafter referred to as "second height") in the second protective portion 85b is less than or equal to the thickness T2 of the second electrode 30.

[0036] As can be understood from the above, in the adhesive 80, the joint portion 82 and the protective portion 84 are integrally connected to each other. That is, the first joint portion 83a, the second joint portion 83b, the third joint portion 83c, the first protective portion 85a, and the second protective portion 85b are all parts of the same adhesive 80.

[0037] A fuel cell stack is formed by stacking unit cells 12 configured as described above in the direction of arrow A. A fuel cell stack is installed, for example, as an on-board fuel cell stack in a fuel cell electric vehicle (not shown).

[0038] The unit cell 12 configured in this way operates as follows:

[0039] As shown in Figure 1, the oxidizer gas is supplied to the oxidizer gas supply port 42a. The fuel gas is supplied to the fuel gas supply port 46a. The cooling medium is supplied to the cooling medium supply port 44a.

[0040] The oxidizing gas is introduced into the oxidizing gas flow path 50 of the first separator 16 through the oxidizing gas supply communication hole 42a. Furthermore, the oxidizing gas moves along the oxidizing gas flow path 50 in the direction of arrow B and is supplied to the first electrode 28 of the MEA 22.

[0041] On the other hand, as shown in Figure 1, fuel gas is introduced into the fuel gas passage 54 of the second separator 18 from the fuel gas supply communication hole 46a. The fuel gas moves along the fuel gas passage 54 in the direction of arrow B and is supplied to the second electrode 30 of the MEA 22.

[0042] In MEA22, the oxidizer gas supplied to the first electrode 28 and the fuel gas supplied to the second electrode 30 are consumed by electrochemical reactions within the first electrode catalyst layer 32 and the second electrode catalyst layer 36. This generates electricity.

[0043] As shown in Figure 1, excess oxidizer gas moves from the oxidizer gas flow path 50 to the oxidizer gas discharge port 42b and is discharged along the oxidizer gas discharge port 42b in the direction of arrow A1. Similarly, excess fuel gas moves from the fuel gas flow path 54 to the fuel gas discharge port 46b and is discharged along the fuel gas discharge port 46b in the direction of arrow A1.

[0044] Furthermore, the cooling medium supplied to the cooling medium supply communication hole 44a is introduced into the cooling medium flow path 56 inside the joining separator 20 (between the first separator 16 and the second separator 18) and flows in the direction of arrow B. After cooling the MEA 22, the cooling medium is discharged from the cooling medium discharge communication hole 44b.

[0045] The oxidizing gas and fuel gas contain moisture. In addition, moisture is generated in MEA22 as a result of the electrochemical reaction described above. Therefore, the environment around MEA22 becomes humid. The main materials of the first separator 16 and the second separator 18 are Fe-containing metals such as stainless steel. In this case, it is expected that Fe ions will leach from the first separator 16 and the second separator 18 in a humid environment. That is, Fe-containing water containing Fe ions may be generated around MEA22. If Fe-containing water reaches the electrolyte membrane 26, the electrolyte membrane 26 will be more susceptible to deterioration.

[0046] However, in this embodiment, the first protective portion 85a covers at least a portion of the outer surface 71 of the laminate 29. Therefore, the penetration of Fe-containing water into the interior of the laminate 29 from the outer surface 71 of the first gas diffusion layer 34, the first electrode catalyst layer 32, or the electrolyte membrane 26 is suppressed. Similarly, since the second protective portion 85b covers at least a portion of the outer surface 74 of the second electrode 30, the penetration of Fe-containing water into the interior from the outer surface 74 of the second gas diffusion layer 38 or the second electrode catalyst layer 36 is suppressed. Thus, the user of the fuel cell stack can obtain a predetermined amount of power from the fuel cell stack over a long period of time.

[0047] The framed MEA10 described above can be manufactured, for example, using the pressing device 100 shown in Figure 3. This pressing device 100 will be briefly described below.

[0048] The pressing device 100 comprises a first pressing type 102 and a second pressing type 106. In this pressing device 100, the first pressing type 102 and the second pressing type 106 are arranged along the vertical direction. The first pressing type 102 is positioned and fixed on a support base (not shown). The second pressing type 106 is displaced vertically above the first pressing type 102 by a displacement mechanism (such as a hydraulic cylinder, not shown). Specifically, the second pressing type 106 moves closer to or further away from the first pressing type 102.

[0049] In this case, the first pressing die 102 has a first inclined portion 104 on the first pressing surface 103 facing the second pressing die 106. The second pressing die 106 has a second inclined portion 108 on the second pressing surface 107 facing the first pressing die 102. The first inclined portion 104 and the second inclined portion 108 face each other. The inclination direction of the first inclined portion 104 and the second inclined portion 108 is such that they move further apart from each other as they approach the outer circumference 66 of the resin frame 60.

[0050] A heating element 110 is provided inside each of the first pressing type 102 and the second pressing type 106. The heating element 110 is controlled by a control device (not shown).

[0051] Next, the manufacturing method of the framed MEA10 according to this embodiment will be described with reference to Figures 3 to 6. As shown in Figure 4, this manufacturing method includes a coating step S1 and a pressing step S2.

[0052] First, as shown in Figure 3, the laminate 29, in which the first surface 26a of the electrolyte membrane 26 is bonded to the first electrode catalyst layer 32, is placed on the first pressing surface 103 of the first pressing mold 102 with the second surface 26b of the electrolyte membrane 26 facing upwards. In this state, the coating process S1 is performed. Specifically, the worker uses a coating device such as a dispenser to apply the uncured adhesive 80 to a predetermined area on the second surface 26b of the electrolyte membrane 26. The predetermined area is the area where the inner circumference 64 of the resin frame 60 is placed. The coating trajectory of the adhesive 80 is annular (for example, rectangular) corresponding to the inner circumference 64 of the resin frame 60. That is, the adhesive 80 is applied so as to adhere to the entire circumference of the inner circumference 64.

[0053] Next, the resin frame 60 is placed on the upper surface of the laminate 29 (the second surface 26b of the electrolyte membrane 26). In this placement, the edge of the through-hole 62 on the first end face 61a of the resin frame 60 is aligned with the application position of the adhesive 80. A portion of the adhesive 80 is interposed between the electrolyte membrane 26 and the first end face 61a of the resin frame 60. Another portion of the adhesive 80 may be located at the through-hole 62. As a result, the first end face 61a on the inner circumference 64 of the resin frame 60 is placed on the outer circumference 70 of the laminate 29.

[0054] Furthermore, the second electrode 30 is placed on the second end face 61b of the inner circumference 64 of the resin frame 60 and on the upper surface of the laminate 29 (the second surface 26b of the electrolyte membrane 26). As a result, the outer circumference 73 of the second electrode 30 is placed on the second end face 61b of the inner circumference 64 of the resin frame 60. Consequently, the resin frame 60 is sandwiched between the laminate 29 and the second electrode 30, and the resin frame 60 protrudes from the outer surface 71 of the laminate 29 and the outer surface 74 of the second electrode 30.

[0055] Next, as shown in Figure 5, the second pressing die 106 approaches the first pressing die 102. As a result, the adhesive 80 is pressed and spread by the first pressing surface 103 and the second pressing surface 107. The adhesive 80 interposed between the electrolyte membrane 26 and the first end surface 61a of the resin frame 60 mainly flows between the electrolyte membrane 26 and the first end surface 61a of the resin frame 60 toward the outer periphery 66 of the resin frame 60. As shown in Figure 6, a portion of the adhesive 80 leaks out from the outer surface 71 of the laminate 29 and reaches the outer surface 71 of the laminate 29 and the portion of the first end surface 61a of the resin frame 60 that is located outside the laminate 29. In other words, the adhesive 80 that leaked out from the outer surface 71 of the laminate 29 covers at least a portion of the outer surface 71 of the laminate 29 and a portion of the first end surface 61a of the resin frame 60. Thus, the first joint portion 83a and the first protective portion 85a are formed.

[0056] On the other hand, as shown in Figure 5, the adhesive 80 interposed between the second end face 61b of the resin frame 60 and the second electrode 30 mainly flows between the second end face 61b of the resin frame 60 and the second electrode 30 toward the outer periphery 66 of the resin frame 60. As shown in Figure 6, a portion of the adhesive 80 leaks out from the outer surface 74 of the second electrode 30 and reaches the outer surface 74 of the second electrode 30 and the portion of the second end face 61b of the resin frame 60 that is located outside the second electrode 30. In other words, the adhesive 80 that leaked out from the outer surface 74 of the second electrode 30 covers at least a portion of the outer surface 74 of the second electrode 30 and a portion of the second end face 61b of the resin frame 60. As a result, the second joint portion 83b and the second protective portion 85b are formed.

[0057] The adhesive 80 located at the through-hole 62 deforms to fill the space 75 surrounded by the inner circumferential surface of the through-hole 62, the other surface of the electrolyte membrane 26, and the second electrode catalyst layer 36. This forms the third joint portion 83c. Alternatively, the adhesive 80 interposed between the laminate 29 and the first end face 61a of the resin frame 60, and the adhesive 80 interposed between the second end face 61b of the resin frame 60 and the second electrode 30 may be allowed to flow into the through-hole 62, and the third joint portion 83c may be formed with this adhesive 80.

[0058] In this embodiment, the first pressing die 102 has a first inclined portion 104, and the second pressing die 106 has a second inclined portion 108. In the space sandwiched between the first inclined portion 104 and the second inclined portion 108, the flow resistance of the adhesive 80 is smaller than in other parts. Therefore, the adhesive 80 flows easily toward the outer periphery 66 of the resin frame 60. That is, the adhesive 80 preferentially flows toward the outer surface 71 of the laminate 29 and the outer surface 74 of the second electrode 30. This prevents the adhesive 80 from flowing into the power generation region EF of the MEA 22.

[0059] In addition, it is preferable that the amount of adhesive 80 applied in the coating process S1 is such that the first height H1 of the first protective portion 85a is less than or equal to the thickness T1 of the laminate 29, and the second height H2 of the second protective portion 85b is less than or equal to the thickness T2 of the second electrode 30.

[0060] In the pressing step S2, the heating element 110 generates heat. As a result, the second electrode catalyst layer 36 is bonded to the second surface 26b of the electrolyte membrane 26. This results in the framed MEA 10.

[0061] The adhesive 80 is, for example, a UV-curing adhesive. In this case, after the mold is opened, the adhesive 80 is cured by irradiating it with ultraviolet light.

[0062] As can be understood from the above, in this embodiment, the adhesive 80 is applied only once. Moreover, the application area of ​​the adhesive 80 is small. Therefore, the time required to perform the application process S1 is short. As a result, the production efficiency of the framed MEA 10 can be improved. Furthermore, since the amount of adhesive 80 applied is small, material costs can be reduced.

[0063] The framed MEA 10 is sandwiched between the first separator 16 and the second separator 18 shown in Figure 1. As a result, the unit cell 12 shown in Figure 1 is obtained. When the first height H1 of the first protective portion 85a is less than or equal to the thickness T1 of the laminate 29, and the second height H2 of the second protective portion 85b is less than or equal to the thickness T2 of the second electrode 30, the first protective portion 85a and the second protective portion 85b are prevented from blocking the flow path (fuel gas flow path 54, etc.) in the bonding separator 20.

[0064] This embodiment provides the following effects.

[0065] As shown in Figure 2, the framed MEA 10 is equipped with an adhesive 80. The adhesive 80 has a joint portion 82 and a protective portion 84. The resin frame 60 and the MEA 22 are joined by the first joint portion 83a and the second joint portion 83b of the joint portion 82. The laminate 29 and the second electrode 30 are joined by the third joint portion 83c of the joint portion 82.

[0066] On the other hand, the protective portion 84 has a first protective portion 85a and a second protective portion 85b. The first protective portion 85a is integrally connected to the first bonding portion 83a and covers at least a part of the outer surface 71 of the laminate 29 and a part of the first end face 61a. The second protective portion 85b is integrally connected to the second bonding portion 83b and covers at least a part of the outer surface 74 of the second electrode 30 and a part of the second end face 61b. The first protective portion 85a prevents foreign matter such as Fe-containing water from entering from the outer surface 71 of the laminate 29, and the second protective portion 85b prevents foreign matter from entering from the outer surface 74 of the second electrode 30. Therefore, for example, the mixing of Fe-containing water into the electrolyte membrane 26 is avoided. This makes it possible to suppress the deterioration of the electrolyte membrane 26.

[0067] In a preferred embodiment, the first height H1 of the first protective portion 85a is less than or equal to the thickness T1 of the laminate 29, and the second height H2 of the second protective portion 85b is less than or equal to the thickness T2 of the second electrode 30. This prevents the first protective portion 85a and the second protective portion 85b from blocking the flow paths of the first separator 16 and the second separator 18.

[0068] In a preferred embodiment, the resin frame 60 is a single plate and has no adhesive other than the adhesive 80. Therefore, the amount of adhesive 80 applied can be reduced.

[0069] As shown in Figure 5, in the pressing step S2 of the manufacturing method for the framed MEA 10, the adhesive 80 is allowed to flow between the laminate 29 and the first end face 61a of the resin frame 60 toward the outer periphery 66 of the resin frame 60, so that the adhesive 80 reaches the outer surface 71 of the laminate 29 and the first end face 61a of the resin frame 60. Similarly, the adhesive 80 is allowed to flow between the second electrode 30 and the second end face 61b of the resin frame 60 toward the outer periphery 66 of the resin frame 60, so that the adhesive 80 reaches the outer surface 74 of the second electrode 30 and the second end face 61b of the resin frame 60.

[0070] As a result, the first bonding portion 83a, the first protective portion 85a, the second bonding portion 83b, and the second protective portion 85b shown in Figures 2 and 6 are formed. Thus, according to the above manufacturing method, a bonding portion 82 that joins the resin frame 60 and the MEA 22, and a protective portion 84 that protects the outer surface 71 of the laminate 29 and the outer surface 74 of the second electrode 30 can be formed by the simple operation of pressing and stretching the adhesive 80 applied to the electrolyte membrane 26.

[0071] Therefore, it is possible to apply the adhesive 80 only once. This improves the production efficiency of the framed MEA 10. In addition, since the amount of adhesive 80 applied is small, material costs can be reduced.

[0072] As shown in Figures 3, 5, and 6, when manufacturing the framed MEA 10, it is preferable to use a first pressing die 102 having a first inclined portion 104 and a second pressing die 106 having a second inclined portion 108. The first inclined portion 104 and the second inclined portion 108 are inclined to move apart from each other as they approach the outer circumference 66 of the resin frame 60.

[0073] In the space between the first inclined portion 104 and the second inclined portion 108, the flow resistance of the adhesive 80 is smaller compared to other parts. Therefore, the adhesive 80 can easily flow toward the outer circumference 66 of the resin frame 60, while it is difficult for the adhesive 80 to flow toward the power generation region EF of the MEA 22. Consequently, the flow of the adhesive 80 into the power generation region EF of the MEA 22 is avoided.

[0074] The following additional information is disclosed regarding the above embodiments.

[0075] (Note 1) The framed membrane electrode structure (10) of the present disclosure comprises a membrane electrode structure (22), a resin frame (60) surrounding the outer circumference of the membrane electrode structure, and an adhesive (80) for joining the membrane electrode structure and the resin frame, wherein the membrane electrode structure has a laminate (29) of a first electrode (28) and an electrolyte membrane (26), and a second electrode (30), the resin frame has a first end face (61a) which is one side surface in the thickness direction, a second end face (61b) which is the back surface of the first end face, and a through-hole (62) through which the membrane electrode structure is positioned from the first end face to the second end face, the adhesive has a joining portion (82) and a protective portion (84), the joining portion is interposed between the laminate and the first end face The protective portion includes a first joining portion (83a) that joins the laminate and the resin frame, a second joining portion (83b) that is interposed between the second end face and the second electrode to join the resin frame and the second electrode, and a third joining portion (83c) that is integrally connected to the first joining portion and the second joining portion and is interposed between the laminate and the second electrode within the through-hole to join the laminate and the second electrode, and the protective portion includes a first protective portion (85a) that is integrally connected to the first joining portion and covers at least a part of the outer surface (71) of the laminate and a part of the first end face, and a second protective portion (85b) that is integrally connected to the second joining portion and covers at least a part of the outer surface (74) of the second electrode and a part of the second end face.

[0076] The first protective portion covering the outer surface of the laminate and the second protective portion covering the outer surface of the second electrode prevent foreign matter (e.g., Fe-containing water) from penetrating the first and second electrodes. Therefore, contamination of the electrolyte membrane by foreign matter is prevented. This suppresses the degradation of the electrolyte membrane.

[0077] (Note 2) In the framed film electrode structure described in Appendix 1, when the direction perpendicular to the first end face and away from the first end face is defined as the first height direction, the dimension (H1) in the first protective portion along the first height direction is less than or equal to the thickness (T1) of the laminate, and when the direction perpendicular to the second end face and away from the second end face is defined as the second height direction, the dimension (H2) in the second protective portion along the second height direction may be less than or equal to the thickness (T2) of the second electrode.

[0078] The first and second protective portions are prevented from blocking the flow path of the reaction gas in the pair of separators that sandwich the framed membrane electrode structure.

[0079] (Note 3) In the framed membrane electrode structure described in Appendix 1 or 2, the resin frame is a single plate and does not need to have any adhesive other than the adhesive described above.

[0080] This allows for a reduction in the amount of adhesive applied.

[0081] (Note 4) A method for manufacturing a framed membrane electrode structure (10) of the present disclosure comprises a membrane electrode structure (22) and a resin frame (60) surrounding the outer circumference of the membrane electrode structure, and comprises a coating step (S1) of applying an adhesive (80) to the electrolyte membrane in a laminate (29) in which an electrolyte membrane (26) is bonded to a first electrode (28), and a pressing step (S2) of sandwiching the resin frame between the laminate and the second electrode (30), and pressing the laminate, the resin frame and the second electrode between a first pressing die (102) and a second pressing die (106) with the resin frame protruding from the outer surface (71) of the laminate and the outer surface (74) of the second electrode, wherein the resin frame is in the thickness direction The resin frame has a first end face (61a) which is one side surface and a second end face (61b) which is the back surface of the first end face. In the pressing step, the adhesive is flowed between the laminate and the first end face of the resin frame toward the outer circumference of the resin frame, so that the adhesive reaches the outer surface of the laminate and the portion of the first end face of the resin frame that is located outside the laminate, thereby forming a first protective portion (85a). The adhesive is also flowed between the second electrode and the second end face of the resin frame toward the outer circumference of the resin frame, so that the adhesive reaches the outer surface of the second electrode and the portion of the second end face of the resin frame that is located outside the second electrode, thereby forming a second protective portion (85b).

[0082] As described above, by the simple operation of pressing and stretching the adhesive applied to the electrolyte membrane, a joint portion that joins the resin frame and the MEA, and a protective portion that protects the outer surface of the laminate and the outer surface of the second electrode can be formed.

[0083] (Note 5) In the method for manufacturing a framed film electrode structure as described in Appendix 4, when the direction perpendicular to the first end face and away from the first end face is defined as the first height direction, and the direction perpendicular to the second end face and away from the second end face is defined as the second height direction, in the coating step, the adhesive may be applied in an amount such that the dimension (H1) along the first height direction in the first protective portion is less than or equal to the thickness (T1) of the laminate, and the dimension (H2) along the second height direction in the second protective portion is less than or equal to the thickness (T2) of the second electrode.

[0084] The first and second protective portions are prevented from blocking the flow path of the reaction gas in the pair of separators that sandwich the framed membrane electrode structure.

[0085] (Note 6) In the method for manufacturing a framed film electrode structure as described in Appendix 4 or 5, the first pressing surface (103) of the first pressing mold facing the second pressing mold and the second pressing surface (107) of the second pressing mold facing the first pressing mold may each have a first inclined portion (104) and a second inclined portion (108) that are inclined to move apart from each other as they move toward the outer circumference (66) of the resin frame.

[0086] By using these first and second pressing types, the adhesive is prevented from flowing toward the power generation region of the membrane electrode structure.

[0087] While this disclosure has been described in detail, it is not limited to the individual embodiments described above. These embodiments can be added, replaced, modified, partially deleted, etc., in any way that does not depart from the gist of this disclosure or from the intent of this disclosure derived from the claims and their equivalents. These embodiments can also be implemented in combination. For example, the order of operations and processes in the embodiments described above are given as examples only and are not limited thereto. The same applies when numerical values ​​or mathematical formulas are used in the description of the embodiments described above. [Explanation of symbols]

[0088] 10…Framed membrane electrode structure 12…Unit cell 22...Membrane electrode structure 26...Electrolyte membrane 28...First electrode 29...Laminate 30...Second electrode 60...Resin frame 61a...First end surface 61b...Second end surface 62... Through-hole 80... Adhesive 82…Joint part 83a…First joint part 83b...Second joint part 83c...Third joint part 84...Protection part 85a...First protection part 85b...Second protective part 100...Pressing device 102...First pressing type 104...First inclined section 106...Second pressing type 108...Second inclined section

Claims

1. A framed membrane electrode structure for a fuel cell, comprising a membrane electrode structure, a resin frame surrounding the outer periphery of the membrane electrode structure, and an adhesive for joining the membrane electrode structure and the resin frame, The aforementioned membrane electrode structure comprises a laminate of a first electrode and an electrolyte membrane, and a second electrode. The resin frame has a first end face which is one side in the thickness direction, a second end face which is the back surface of the first end face, and a through-hole which extends from the first end face to the second end face and in which the film electrode structure is arranged. The resin frame further has an inner circumference which is the area around the through-hole, and the film electrode structure sandwiches the inner circumference between the outer circumference of the laminate and the outer circumference of the second electrode. The adhesive has a joint portion and a protective portion. The joint portion includes a first joint portion interposed between the laminate and the first end face to join the laminate and the resin frame, a second joint portion interposed between the second end face and the second electrode to join the resin frame and the second electrode, and a third joint portion integrally connected to the first joint portion and the second joint portion, and interposed between the laminate and the second electrode within the through-hole to join the laminate and the second electrode. The protective portion comprises a first protective portion integrally connected to the first bonding portion and covering at least a part of the outer surface and a part of the first end face of the laminate, and a second protective portion integrally connected to the second bonding portion and covering at least a part of the outer surface and a part of the second end face of the second electrode, wherein the film electrode structure has a frame.

2. In the framed film electrode structure according to claim 1, when the direction perpendicular to the first end face and away from the first end face is defined as the first height direction, the dimension of the first protective portion along the first height direction is less than or equal to the thickness of the laminate. A framed film electrode structure in which, when the direction perpendicular to the second end face and away from the second end face is defined as the second height direction, the dimension of the second protective portion along the second height direction is less than or equal to the thickness of the second electrode.

3. A framed membrane electrode structure according to claim 1 or 2, wherein the resin frame is a single plate and does not have any adhesives other than the adhesive.

4. A method for manufacturing a framed membrane electrode structure for a fuel cell, comprising a membrane electrode structure and a resin frame surrounding the outer periphery of the membrane electrode structure, The resin frame has a first end face which is one side in the thickness direction, a second end face which is the back surface of the first end face, a through-hole which extends from the first end face to the second end face and in which the film electrode structure is arranged, and an inner circumferential portion which is the periphery of the through-hole. A coating step of applying an adhesive to the electrolyte membrane in a laminate in which an electrolyte membrane is bonded to a first electrode, The process includes a pressing step in which the inner circumference of the resin frame is sandwiched between the outer circumference of the laminate and the outer circumference of the second electrode, and the laminate, the resin frame, and the second electrode are sandwiched and pressed between a first pressing die and a second pressing die, with the resin frame protruding from the outer surface of the laminate and the outer surface of the second electrode. In the pressing step, the adhesive is flowed between the laminate and the first end face of the resin frame toward the outer circumference of the resin frame, so that the adhesive reaches the outer surface of the laminate and the portion of the first end face of the resin frame that is located outside the laminate, thereby forming a first protective portion, and the adhesive is flowed between the second electrode and the second end face of the resin frame toward the outer circumference of the resin frame, so that the adhesive reaches the outer surface of the second electrode and the portion of the second end face of the resin frame that is located outside the second electrode, thereby forming a second protective portion. Furthermore, a method for manufacturing a framed film electrode structure, wherein the adhesive is used to form a joint portion having: a first joint portion interposed between the laminate and the first end face to join the laminate and the resin frame; a second joint portion interposed between the second end face and the second electrode to join the resin frame and the second electrode; and a third joint portion integrally connected to the first joint portion and the second joint portion, and interposed between the laminate and the second electrode within the through-hole to join the laminate and the second electrode.

5. A method for manufacturing a framed film electrode structure according to claim 4, wherein the direction perpendicular to the first end face and away from the first end face is defined as the first height direction, and the direction perpendicular to the second end face and away from the second end face is defined as the second height direction, and in the coating step, the adhesive is applied in an amount such that the dimension of the first protective portion along the first height direction is less than or equal to the thickness of the laminate, and the dimension of the second protective portion along the second height direction is less than or equal to the thickness of the second electrode.

6. A method for manufacturing a framed membrane electrode structure according to claim 4 or 5, wherein the first pressing surface of the first pressing mold facing the second pressing mold and the second pressing surface of the second pressing mold facing the first pressing mold each have a first inclined portion and a second inclined portion that are inclined to move apart from each other as they move toward the outer circumference of the resin frame.

Citation Information

Patent Citations

  • MEA with resin frame and manufacturing method thereof

    JP2022151538A

  • Membrane electrode structure for fuel cell and method for manufacturing membrane electrode structure for fuel cell

    WO2024202862A1