Patent Information
- Application Number
- JP2025502436
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-12-22
- Filing Date
- 2024-10-09
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-10-09
AI Technical Summary
Sodium-ion layered metal oxide cathode materials experience severe structural degradation and capacity attenuation during charge-discharge cycles due to high voltage charging, leading to large volume deformation, electrolyte decomposition, and co-intercalation of solvent molecules.
A sodium-ion layered metal oxide material with a specific chemical formula Na x Ni a Mn b Ti (0.5-b) M (0.5-a) O (2-y) F y is developed, where F doping and controlled doping of elements like Zn, Mg, Sn, Sb, and Cu improve material stability by altering bond energies and suppressing lattice distortion, and a precise calcination process ensures uniform distribution and reduces impurity phases.
The material exhibits improved structural stability, higher discharge ratio capacity, and enhanced cycle performance, with a 10-15% increase in capacity retention after 100 cycles.
Smart Images

Figure 0007949152000001 
Figure 0007949152000002 
Figure 0007949152000003
Abstract
Description
[Technical Field]
[0001] The present invention belongs to the technical field of sodium-ion batteries, and more particularly to sodium-ion layered metal oxide materials, methods for producing the same, positive electrode materials, and sodium-ion batteries. [Background technology]
[0002] The commercialization of electrochemical power sources, particularly lithium-ion batteries (LIBs), has ushered in a new era for portable electronic products and electric vehicles, bringing great convenience to daily life. However, concerns about the depletion of lithium resources and the increasing price fluctuations of lithium, nickel, and cobalt raw materials have led to intensive research into sodium-ion batteries (NIBs), which are becoming a strong competitor in the field of energy storage, such as national power grids and household energy storage. The cathode is an indispensable part of NIBs and directly determines all of their important performance characteristics, such as cost, safety, energy density, power density, and cycle life. In addition, ideal cathode materials are relatively environmentally friendly and easy to mass-produce, transport, and store.
[0003] Cost is a major factor driving competition between sodium-ion batteries and lithium-ion batteries. Manganese has advantages such as being environmentally friendly, low-cost, and having a high annual production volume. Manganese-rich layered sodium ion transition metal oxide material (Mn-based Na x TMO2 contains many elements with electrochemical redox activity, such as Mn, Fe, Cu, Ni, Co, Cr, Ir, Ru, and O, and its chemical composition can be flexibly designed. Furthermore, it has a high specific capacity and excellent safety performance, making it a strong competitor to commercially available sodium-ion battery cathode materials.
[0004] Currently, sodium ion layered transition metal oxide cathode materials have the general formula Na x It is TMO2, Na +Different structures are formed as the content changes, the common structures have O3, P3, O'3 and P2 phases, the transition metal sites in the layered oxide are occupied by various metal ions (such as Li, Na, Mg, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Sn, Ir, Ru, etc.), and there are large differences in the extranuclear electron arrangement, oxidation state, and TM-O bond energy of these metal ions, Na + Different structures of layered oxide positive electrode materials are formed as the content changes. O3-type high-nickel materials have high specific capacity, but when charged to a high voltage, they not only cause multi-phase transition leading to large volume deformation, but also further accelerate the decomposition of the electrolyte, induce co-intercalation of solvent molecules, and ultimately cause severe structural degradation and capacity attenuation of the electrode material during the charge-discharge process. SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION
[0005] In view of the problems existing in the background art, the present invention aims to provide a sodium-ion layered metal oxide material, its preparation method, a positive electrode material and a sodium-ion battery, so as to solve the problems of severe structural degradation and capacity attenuation of the positive electrode material during the charge-discharge process. MEANS FOR SOLVING THE PROBLEMS
[0006] In a first aspect, the present invention provides a sodium-ion layered metal oxide material having the chemical formula shown in Formula I, Na x Ni a Mn b Ti (0.5-b) M (0.5-a) O (2-y) F y Formula I, Here, 0.9≦x≦1.0, 0.3≦a<0.5, 0.3≦b≦0.4, 0.1≦1-a-b≦0.35, 0≦y<0.1, and M includes at least one of Zn, Mg, Sn, Sb, Y and Cu.
[0007] In the examples of the present invention, the M element is Sodium ion layered metal oxideIt contributes to improving the stability of the material, F - The radius is O 2- Similar to radius, substituting O with F is feasible, and by controlling the amount of F doping, by doping with F Sodium ion layered metal oxide material This can avoid having too many impurities inside, and the strong electronegativity of F can change the bond energy of the oxygen element in the lattice, thereby Na + Improve the diffusion rate of Mn 3+ This suppresses lattice distortion caused by the Jahn-Teller effect of active ions, thereby improving structural stability. Preferably, the sodium ion layered metal oxide material is an O3-type manganese-based layered oxide material.
[0008] In a second embodiment, the present invention provides a method for producing the sodium ion layered metal oxide material described above, wherein the production method is A) A step in which Na source, Ni source, Mn source, Ti source, M source, and F source are mixed with a solvent according to the stoichiometric ratio in formula I, and then rough polishing is performed to obtain a first slurry, B) The step of polishing the first slurry to obtain a second slurry, C) The step of spray-drying the second slurry to obtain the first powder, D) A step of obtaining a second powder by calcining the aforementioned powder in the following process, In an oxygen-containing atmosphere, 3 ℃ / min A heating rate of ~5°C / min from room temperature to 110°C ℃ Heat up to ~130℃, 2 time Keep warm for 4 hours, then for another 5 ℃ / min 440 with a heating rate of ~8℃ / min ℃ Heat up to ~460℃, 1 time Keep warm for 3 hours, then for another 5 ℃ / min 850 with a heating rate of ~8℃ / min ℃ Heat up to ~950℃, 10 time The step involves keeping it warm for up to 20 hours, E) The second powder is pulverized and sieved to remove iron, thereby obtaining a sodium ion layered metal oxide material having the chemical formula of formula I, Nax Ni a Mn b Ti (0.5-b) M (0.5-a) O (2-y) F y Equation I, Here, 0.9≦x≦1.0, 0.3≦a<0.5, 0.3≦b≦0.4, 0.1≦1-ab≦0.35, 0≦y<0.1, and M includes at least one of Zn, Mg, Sn, Sb, Y, and Cu.
[0009] In embodiments of the present invention, by raising the temperature using a specific process to calcine the second powder, the occurrence of side reactions is reduced, the formation of impurity phases is reduced, and moreover, Sodium ion layered metal oxide material inside M To make the distribution more uniform, Sodium ion layered metal oxide This can improve material uniformity and product stability, and further enhance electrochemical performance.
[0010] Preferably, the sodium ion layered metal oxide material is Na 0.95 Ni 0.45 Mn 0.3 Cu 0.05 Ti 0.2 O 1.95 F 0.05 NaNi 0.48 Mn 0.4 Y 0.02 Ti 0.1 O 1.999 F 0.001 and Na 0.9 Ni 0.48 Mn 0.39 Cu 0.02 Mg 0.01 Ti 0.1 It is one or more types of O2.
[0011] Preferably, the firing process is as follows: In an oxygen-containing atmosphere, 4 ℃ / min A heating rate of ~5°C / min from room temperature to 120°C ℃ Heat up to ~125℃, 2 time Keep warm for 3 hours, then for another 5 ℃ / min 450 with a heating rate of ~7℃ / min ℃The temperature is raised to ~455°C, 1 time held for ~2 hours, and further at a heating rate of 5 ℃ / min ~8°C / min to 850 ℃ ~950°C, 13 time held for ~20 hours.
[0012] Preferably, the solvent used for rough grinding in the aforementioned step A) is water and / or alcohol, and the solid content of the first slurry is 10 % ~40%, which ensures the production yield and avoids clogging of the rough grinder, sand mill and connecting pipelines; the particle size of the first slurry is D100<10μm, 1 which prevents the particles in the slurry from clogging the filter screen of the sand mill.
[0013] Preferably, the particle size of the second slurry is D50<3μm and D100<8μm, which ensures that the particle size distribution of the first powder obtained after spray drying is more concentrated, avoids the formation of large particles, 2nd the slurry is uniform, and in addition, the second slurry has a small particle size, so that the insoluble particulate matter is in sufficient contact with each other, Sodium ion layered metal oxide material which is advantageous for ensuring the uniformity of the cation distribution in the system.
[0014] In the embodiments of the present invention, grinding after rough grinding can ensure that each insoluble particle in the slurry is sufficiently ground, ensure the uniformity of the slurry, and improve the grinding efficiency, Preferably, the particle size of the first powder is 2μm<D50<15μm, D100<40μm, the moisture content is less than 1.5%, and BET>15m 2 / g.
[0015] In the embodiments of the present invention, the first powder satisfying the above indexes ensures that less water vapor is generated during the firing process, which can avoid the precipitation of sodium; the small particle size and large BET of the first powder ensure that the contact between particles is more sufficient during the firing process, which facilitates ion exchange and migration, thereby firing This ensures that the resulting material has higher crystallinity, a more uniform cation distribution, and fewer impurities.
[0016] Preferably, the oxygen content in the firing process is 20 % The composition is approximately 35%, with a water content of less than 3% and a carbon dioxide concentration of less than 1%.
[0017] In embodiments of the present invention, firing The process involves detecting the moisture, oxygen, and carbon dioxide content in the high-temperature furnace online, and adjusting the gas flow rate, exhaust rate, and the ratio of oxygen and nitrogen gases in the flowing gas in a timely manner. By controlling the moisture, oxygen, and carbon dioxide content in the high-temperature furnace within the control range, if the oxygen content is too high, firing This prevents the formation of too many impurity phases during the process.
[0018] Preferably, rapid cooling is performed after firing to obtain a second powder, and this rapid cooling is a quenching treatment.
[0019] In the embodiments of the present invention, accelerating the cooling rate during the cooling process after firing allows for more Mn 3+ It contributes to the formation of a metastable phase containing and having a high content of interlayer sodium, thereby Sodium ion layered metal oxide To improve the reversible capacity of the material.
[0020] In a third embodiment, the present invention provides a positive electrode sheet comprising the sodium ion layered metal oxide material described above or a sodium ion layered metal oxide material manufactured by the manufacturing method described above.
[0021] In the embodiments of the present invention, the positive electrode sheet contains the above-mentioned sodium ion layered metal oxide material, and therefore has good structural stability, high discharge ratio capacity, and high capacity retention rate.
[0022] In a fourth embodiment, the present invention provides a sodium-ion battery including the positive electrode sheet described above. [Effects of the Invention]
[0023] In the embodiment of the present invention, the sodium-ion battery includes the above-mentioned positive electrode sheet and therefore has a high discharge ratio capacity and high cycle performance. [Brief explanation of the drawing]
[0024] To more clearly illustrate embodiments of the present invention or technical solutions in the prior art, the following briefly introduces the drawings necessary for use in describing the embodiments or the prior art. Clearly, the drawings in the following description are simply embodiments of the present invention, and those skilled in the art can obtain other drawings based on the provided drawings without any creative effort. [Figure 1] This is a SEM diagram of the sodium ion layered metal oxide material in Example 1 of the present invention. [Figure 2] This is an XRD diagram of the sodium ion layered metal oxide material in Example 1 of the present invention. [Figure 3] This is the charge / discharge curve of the button battery in Example 1 of the present invention. [Figure 4] This is the charge / discharge curve of the button battery in Example 2 of the present invention. [Figure 5] This is a SEM diagram of the sodium ion layered metal oxide material in Example 2 of the present invention. [Figure 6] This is the charge / discharge curve of the button battery in Example 3 of the present invention. [Figure 7] This is a SEM diagram of the sodium ion layered metal oxide material in Example 3 of the present invention. [Modes for carrying out the invention]
[0025] The following examples of embodiments of the technical solution of the present application will be described in detail with reference to the drawings. The following embodiments are provided solely to illustrate the technical solution of the present application more clearly and are therefore not intended to limit the scope of protection of the present application, but are merely examples.
[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as that generally understood by those skilled in the art of the present application. The terms used herein are for the sole purpose of describing specific embodiments and are not intended to limit the present application. The terms “including” and “having,” and any variations thereof, in the description of the present specification, claims, and drawings are intended to cover exclusive inclusion.
[0027] In the description of the embodiments of this application, technical terms such as "first," "second," etc., are used solely to distinguish between different subjects and cannot be understood as indicating or suggesting relative importance, or implying the number, specific order, or primary relationship of the indicated technical features. In the description of the embodiments of this application, the meaning of "plural" is two or more unless a particularly specific limitation is clearly stated.
[0028] In this specification, the term "Examples" means that the specific features, structures, or properties described in conjunction with the Examples are included in at least one Example of the Application. The appearance of the term at each location in the description does not necessarily refer to the same Example, nor does it imply an independent or alternative Example that excludes other Examples. Those skilled in the art will understand, both clearly and implicitly, that the Examples described herein can be combined with other Examples.
[0029] In the description of the embodiments of this application, the terms "and / or" do not merely describe a related relationship, but indicate that three types of relationships may exist. For example, A and / or B can refer to three cases: when A exists alone, when A and B exist simultaneously, and when B exists alone. In this specification, the letter " / " generally indicates that the preceding and succeeding related objects are in an "or" relationship.
[0030] In the description of the embodiments of this application, the term "multiple" means two or more (including two), similarly, "multiple sets" means two or more sets (including two sets), and "multiple sheets" means two or more sheets (including two sheets).
[0031] In the description of the embodiments of this application, the directions or positional relationships indicated by technical terms such as "center," "vertical direction," "horizontal direction," "length," "width," "thickness," "top," "bottom," "front," "back," "left," "right," "vertical," "horizontal," "top," "bottom," "inside," "outside," "clockwise," "counterclockwise," "axial direction," "radial direction," and "circumferential direction" are based on the directions or positional relationships shown in the drawings. They are merely used to describe the embodiments of this application and simplify the explanation, and do not indicate or imply that the referred device or element has a specific direction or must be configured and operated in a specific direction. Therefore, they cannot be understood as limiting the embodiments of this application.
[0032] In the description of the embodiments of this application, unless otherwise specifically defined and limited, technical terms such as "attachment," "connection," "bonding," and "fixing" should be understood in a broad sense. For example, these may be fixed connections, removable connections, integral connections, mechanical connections, electrical connections, direct connections, indirect connections via an intermediate medium, internal communication between two elements, or interaction relationships between two elements. Those skilled in the art will be able to understand the specific meaning of these terms in the embodiments of this application depending on the specific circumstances.
[0033] Currently, in the structure of sodium ion layered transition metal oxide cathode materials, O3-type high-nickel materials have high specific capacity, but when charged to high voltages, they not only undergo multiphase transitions and large volume deformations, but also promote the decomposition of the electrolyte and induce co-doping of solvent molecules, ultimately causing serious structural degradation and capacity decay during the charge-discharge process of the electrode material.
[0034] To solve the above problems, the present invention provides a sodium ion layered metal oxide material, a method for producing the same, a positive electrode sheet, and a sodium ion battery, wherein by doping with element F and element M, Sodium ion layered metal oxide It contributes to improving the stability of the material, and the strong electronegativity of F can change the bond energy of the oxygen element in the lattice, thereby Na + Improve the diffusion rate of Mn3+ This invention suppresses lattice distortion caused by the Jahn-Teller effect of active ions, thereby improving structural stability. Furthermore, by employing a specific process to raise the temperature and calcine the second powder, the present invention reduces the occurrence of side reactions and the formation of impurity phases, and moreover, Sodium ion layered metal oxide material inside M To make the distribution more uniform, Sodium ion layered metal oxide This improves material uniformity and product stability, and further enhances electrochemical performance. As a result, positive electrode sheets and sodium-ion batteries using this sodium-ion layered metal oxide material have high discharge ratio capacity and high cycle performance.
[0035] In a first embodiment, the present invention provides a sodium ion layered metal oxide material, the sodium ion layered metal oxide material being an O3-type manganese-based layered oxide material having the chemical formula shown in formula I. Na x Ni a Mn b Ti (0.5-b) M (0.5-a) O (2-y) F y Equation I, Here, 0.9≦x≦1.0, 0.3≦a<0.5, 0.3≦b≦0.4, 0.1≦1-ab≦0.35, 0≦y<0.1, and M contains at least one of Zn, Mg, Sn, Sb, Y, and Cu.
[0036] In one embodiment of the present invention, 0.9 ≤ x ≤ 1.0, preferably 0.92 ≤ x ≤ 0.98, where x is, for example, 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, or 1.0, and preferably a range value with any of the above values as the upper or lower limit.
[0037] In one embodiment of the present invention, 0.3 ≤ a < 0.5, preferably 0.35 ≤ a ≤ 0.45, where a is, for example, 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, and preferably a range value with any of the above values as the upper or lower limit.
[0038] In one embodiment of the present invention, 0 < (0.5-a) ≤ 0.2, preferably 0.01 ≤ (0.5-a) ≤ 0.05, and element M has poor compatibility with oxides of elements such as Ni, Mn, and Ti during the calcination process. Within that range, the proportion of element M is too high. complete Sodium ion layered metal oxide material The amount of impurity phase inside increases, and further Sodium ion layered metal oxide The energy density of the material is too low. This can be avoided. .
[0039] In one embodiment of the present invention, 0.3 ≤ b ≤ 0.4, preferably 0.32 ≤ b ≤ 0.38, where b is, for example, 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, or 0.4, and preferably a range value with any of the above values as the upper or lower limit.
[0040] In one embodiment of the present invention, 0.1 ≤ 1 - ab ≤ 0.35, and preferably 0.2 ≤ 1 - ab ≤ 0.3.
[0041] In one embodiment of the present invention, 0 ≤ y < 0.1, preferably 0.01 ≤ y ≤ 0.08, where y is, for example, 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, preferably a range value with any of the above values as the upper or lower limit. If the y value is within the above range, the proportion of element F is too high, Sodium ion layered metal oxide material This is due to an increase in the amount of impurity phase (e.g., nickel oxide) inside. Sodium ion layered metal oxide This helps to avoid the problem of the material's energy density being too low, which would result in poor structural stability.
[0042] Specifically, in the embodiment of the present invention, the sodium ion layered metal oxide material is Na 0.95 Ni 0.45 Mn 0.3 Cu 0.05 Ti 0.2 O 1.95 F 0.05 NaNi 0.48 Mn 0.4 Y 0.02 Ti 0.1 O 1.999 F 0.001 and Na 0.9 Ni 0.48 Mn 0.39 Cu 0.02 Mg 0.01 Ti 0.1 It is one or more types of O2.
[0043] This invention involves doping with elements F and M, Sodium ion layered metal oxide The capacity retention rate of the material after 100 cycles of 1C improves by 10% to 15%.
[0044] In a second embodiment, the present invention further provides a method for producing a sodium ion layered metal oxide material, wherein the production method is A) A step in which Na source, Ni source, Mn source, Ti source, M source, and F source are mixed with a solvent according to the stoichiometric ratio in formula I, and then rough polishing is performed to obtain a first slurry, B) The step of polishing the first slurry to obtain a second slurry, C) The step of spray-drying the second slurry to obtain the first powder, D) A step of obtaining a second powder by calcining the aforementioned powder in the following process, In an oxygen-containing atmosphere, 3 ℃ / min A heating rate of ~5°C / min from room temperature to 110°C ℃ Heat up to ~130℃, 2 time Keep warm for 4 hours, then for another 5 ℃ / min 440 with a heating rate of ~8℃ / min ℃ Heat up to ~460℃, 1 time Keep warm for 3 hours, then for another 5 ℃ / min 850 with a heating rate of ~8℃ / min ℃Heat up to ~950℃, 10 time The step involves keeping it warm for up to 20 hours, E) The step of grinding the second powder, sieving it to remove iron, and obtaining a sodium ion layered metal oxide material having the chemical formula of formula I. Na x Ni a Mn b Ti (0.5-b) M (0.5-a) O (2-y) F y Equation I
[0045] In one embodiment of the present invention, the Na source is preferably one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, sodium acetate, sodium oxalate, and sodium citrate; the Ni source is preferably one or more of nickel monoxide (NiO), nickel oxide (Ni2O3), nickel hydroxide "Ni(OH)2", high nickel hydroxide "Ni(OH)3", nickel carbonate, and nickel oxalate; and the Mn source is preferably trimethylamine tetroxide. The Ti source is one or more of manganese, manganese dioxide, dimanganese trioxide, manganese monoxide, manganese carbonate, and manganese oxalate, the Ti source is preferably titanium dioxide and / or metatitanium (H2TiO3), the M source is preferably at least one of oxides of M, hydroxides of M, carbonates of M, oxalates of M, and citrates of M, if element M is yttrium (Y), the M source is preferably an oxide of Y, and the F source is preferably sodium fluoride. In the present invention, the Na source, Ni source, Mn source, Ti source, M source, and F source are all weighed and mixed according to the number of moles of the metal element in the chemical formula shown in formula I, and since this is a common technical means in the art, the present invention will not be described here.
[0046] In one embodiment of the present invention, the solvent used for rough polishing is preferably water and / or alcohol, more preferably deionized water and / or alcohol, and the time for the rough polishing is preferably 1 time ~3 hours, more preferably 1 timeis about 2 hours. The operating frequency of the coarse grinding is preferably 10 Hz to 50 Hz, more preferably 20 to 40 Hz.
[0047] In one embodiment of the present invention, the solid content of the first slurry obtained after coarse grinding is preferably 10 % to 40%, more preferably 20 % to 30%, for example 10%, 15%, 20%, 25%, 30%, 35%, 40%, preferably a range value with any of the above numerical values as the upper limit or lower limit. The particle size of the first slurry is preferably D100<10 μm, more preferably D100<5 μm. After obtaining the first slurry, the present invention transfers and circulates the first slurry in a sand mill in a circulation manner between tank A and tank B for circulating grinding, to obtain a second slurry.
[0048] In one embodiment of the present invention, the grinding time is preferably 2 time to 5 hours, more preferably 3 time to 4 hours. The rotation speed of the sand mill is preferably 200 r / min to 1500 r / min, more preferably 500 r / min to 1000 r / min. The particle size of the second slurry is D50<3 μm and D100<8 μm, preferably D50<2 μm and D100<5 μm. After obtaining the second slurry, the present invention subjects the second slurry to spray drying to obtain a first powder.
[0049] In one embodiment of the present invention, the particle size of the first powder obtained by spray drying is preferably 2 μm<D50<15 μm, D100<40 μm, with a moisture content of less than 1.5%, and BET>15 m 2 / g, more preferably 5 μm<D50<12 μm, D100<30 μm, with a moisture content of less than 1.0%, and BET>15 m 2 / g.
[0050] After obtaining the first powder, the present invention calcines it, and the calcination is preferably carried out by the following process. In an oxygen-containing atmosphere, 3 ℃ / min A heating rate of ~5°C / min from room temperature to 110°C ℃ Heat up to ~130℃, 2 time Keep warm for 4 hours, then for another 5 ℃ / min 440 with a heating rate of ~8℃ / min ℃ Heat up to ~460℃, 1 time Keep warm for 3 hours, then for another 5 ℃ / min At a heating rate of ~8°C / min 850℃ ~ 950 Heat up to ℃, 10 time Keep warm for up to 20 hours.
[0051] In one embodiment of the present invention, the oxygen-containing atmosphere is preferably a dry oxygen gas or dry air, or a mixed gas of dry oxygen gas and nitrogen gas, thereby, Sodium ion layered metal oxide During the cooling process of the material Sodium ion layered metal oxide To avoid deterioration of the material due to contact with water and carbon dioxide. Preferably, the oxygen-containing atmosphere is a mixture of dry oxygen gas and nitrogen gas, and the volume fraction of oxygen gas is preferably 25%. % The oxygen content is approximately 35%, more preferably 30%, and controls the oxygen gas content in the high-temperature furnace, as well as the water and carbon dioxide in the gas that flows through it. Sodium ion layered metal oxide material To avoid adverse effects on the free sodium content in the sodium ion layered metal oxide material and Sodium ion layered metal oxide material It contributes to reducing the pH, Sodium ion layered metal oxide The high free sodium content and pH of the materials prevent the slurry from gelling during the battery manufacturing process.
[0052] In one embodiment of the present invention, the first step is to first 3 ℃ / min A heating rate of ~5°C / min from room temperature to 110°C ℃ Heat up to ~130℃, 2 time The temperature is maintained for approximately 4 hours. The purpose of this step is primarily to reduce the moisture content of the first powder, so that in the subsequent rapid heating process, the moisture content in the high-temperature furnace atmosphere is excessive and side reactions occur. Sodium ion layered metal oxide materialThe goal is to avoid having too high an impurity phase.
[0053] At this stage, the heating rate is preferably 3 ℃ / min ~5℃ / min, far, 3 ℃ / min The temperature is ~4°C / min, and the firing temperature is preferably 110°C. ℃ ~130℃, more preferably 115 ℃ The temperature is ~125°C, for example, 110°C, 115°C, 120°C, 125°C, 130°C, preferably within a range of any of the above values as the upper or lower limit, and the time of the heat retention is preferably 2 time ~4 hours, more preferably 2 time It takes approximately 3 hours.
[0054] After the first stage of firing is complete, 5 ℃ / min 440 with a heating rate of ~8℃ / min ℃ Heat up to ~460℃, 1 time The mixture is kept warm for approximately 3 hours, and then the second stage of firing is performed. This stage primarily promotes the decomposition and melting of the M element compound, improving the compatibility of the M element with other elements. Sodium ion layered metal oxide material To make the distribution of element M more uniform, Sodium ion layered metal oxide This is to improve the uniformity of materials and ensure product stability. Otherwise, Sodium ion layered metal oxide material The distribution of element M inside is non-uniform, Sodium ion layered metal oxide material The electrical performance of the sampling tests at different points does not match, leading to low product stability, or poor compatibility between element M and other elements. Sodium ion layered metal oxide material A high level of impurities in the oxide of element M within the material leads to poor electrical performance.
[0055] In one embodiment of the present invention, the second step firing The heating rate is preferably 5 ℃ / min ~8°C / min, more preferably 6 ℃ / min The temperature is ~7°C / min, and the firing temperature is preferably 440°C. ℃ ~460℃, more preferably 445 ℃The temperature is ~455°C, for example, 440°C, 445°C, 450°C, 455°C, 460°C, preferably within a range of any of the above values as the upper or lower limit, and the time of the heat retention is preferably 1 time ~3 hours, more preferably 1 time It takes approximately 2 hours.
[0056] After the second stage of firing is completed, the present invention proceeds to 5 ℃ / min At a heating rate of ~8°C / min 850℃ ~ 950 Heat up to ℃, 10 time Keep warm for approximately 20 hours, then perform the third stage of firing. Firing at this temperature and time is necessary because the temperature may be too high or too low. firing This is advantageous in avoiding the formation of too many impurity phases during the process. Sodium ion layered metal oxide material This contributes to improving the crystallinity and purity of the material, thereby improving the charge-discharge ratio capacity.
[0057] In one embodiment of the present invention, the heating rate is preferably 5 ℃ / min ~8°C / min, more preferably 6 ℃ / min The temperature is ~7°C / min, and the firing temperature is preferably 850°C. ℃ ~950°C, more preferably 860°C ℃ The temperature is ~940°C, for example, 850°C, 860°C, 870°C, 880°C, 890°C, 900°C, 910°C, 920°C, 930°C, 940°C, 950°C, preferably within a range where any of the above values are the upper or lower limit, and the time for keeping the temperature warm is preferably 10 time ~20 hours, more preferably 15 time It takes approximately 16 hours.
[0058] In the entire firing process described above, the water content in the high-temperature furnace is controlled to be less than 3%, the carbon dioxide concentration to be less than 1%, and the oxygen content to be between 20% and 50%. If the oxygen content is too high, firing This process avoids the formation of too many impurity phases. firingDuring the process, the contents of moisture, oxygen and carbon dioxide in the high-temperature furnace are detected online, the gas flow rate, discharge amount, and the proportions of oxygen gas and nitrogen gas in the flowing gas are timely adjusted, so that the contents of moisture, oxygen and carbon dioxide in the high-temperature furnace are controlled within the control range.
[0059] After the calcination is completed, the product is cooled to room temperature to obtain a second powder. Natural cooling is allowed, and the present invention preferably rapidly cools the calcined product to room temperature, for example, a quenching treatment may be mentioned, which accelerates the cooling rate and contributes to retaining more Mn 3+ and forming a metastable phase with high interlayer sodium content, thereby improving the reversible capacity of the material. Sodium ion layered metal oxide In the present invention, the quenching treatment preferably adopts cooling with chilled water or cooling with liquid nitrogen.
[0060] After obtaining the second powder, the present invention pulverizes and sieves it to remove iron, so as to obtain a sodium ion layered metal oxide material. The environmental humidity during pulverization and sieving is controlled to be less than 15%. The obtained sodium ion layered metal oxide material has a particle size range of 0.5μm<D50<12μm and D100<40μm, a magnetic foreign matter content of less than 150ppm, and manganese elution amount of less than 0.5ppm, free sodium of less than 100ppm, and moisture of less than 1000ppm.
[0061] In one embodiment of the present invention, the pulverization method is preferably a jet mill or a mechanical mill. During sieving, the material passes through at least two stages of sieves, and the mesh number of the first-stage sieve is preferably 80 mesh to 100 mesh, and the mesh number of the second-stage sieve is 120 mesh to 320 mesh.
[0062] Pulverization and sieving can improve the uniformity Sodium ion layered metal oxide material of Sodium ion layered metal oxide materialTo avoid large particles in the sample negatively affecting electrical performance, the humidity of the environment during grinding and sieving is controlled to be less than 15%, and the absorption of water from the sample is controlled. Sodium ion layered metal oxide To avoid material degradation, impurity generation, and deterioration of electrical performance.
[0063] In one embodiment of the present invention, the processes of grinding, sieving, and iron removal of the second powder are continuous operations, connected via piping in between, and transported using negative pressure. Sodium ion layered metal oxide material After degassing, the material enters the crushing equipment, and dry nitrogen gas is flowed through both the sieving and iron removal processes for protection. Sodium ion layered metal oxide This prevents the material from coming into contact with water and carbon dioxide, which can lead to the generation of impurities.
[0064] In a third embodiment, the present invention provides a positive electrode sheet comprising the sodium ion layered metal oxide material described above, and the present invention does not particularly limit other materials used in the positive electrode sheet, such as current collectors, conductive agents, adhesives, etc., and general manufacturing raw materials for positive electrode sheets commonly used in the art may be used.
[0065] The 4 In one embodiment, the present invention provides a sodium-ion battery including the positive electrode sheet described above. The present invention does not particularly limit other materials used in sodium-ion batteries, such as negative electrodes and separators, and may employ general manufacturing raw materials for sodium-ion batteries commonly used in the art.
[0066] The following are some specific examples, but these examples are illustrative and used only to illustrate the present application, and should not be understood as limiting the present application. Examples that do not specify specific techniques or conditions are carried out in accordance with techniques or conditions described in the literature in the art or in accordance with the product instructions. Reagents or instruments used whose manufacturers are not specified are all common products available from the market.
[0067] (Example 1) The chemical formula for a sodium ion layered metal oxide material is Na 0.95 Ni 0.45 Mn 0.3 Cu 0.05 Ti 0.2 O 1.95 F 0.05 And, Sodium ion layered metal oxide Based on the molar ratio of the metal elements in the chemical formula of the materials, sodium carbonate, nickel oxide, trimanganese tetroxide, titanium oxide, copper oxide, sodium fluoride, and deionized water were uniformly mixed in a coarse grinder for 2 hours at an operating frequency of 30 Hz to obtain a first slurry (solid content of 25%, particle size D100 < 8.5 μm). The first slurry was polished and mixed in a sand mill using an A / B tank circulation system, switching between tanks for a polishing time of 3 hours, with a sand mill rotation speed of 1000 r / min, to obtain the second slurry (particle size D50 < 3 μm, D100 < 8 μm). The second slurry was spray-dried to obtain the first powder (particle size D50 < 10 μm, D100 < 35 μm, moisture content 0.5%, BET 30 m 2 ( / g) is obtained The first powder is placed in a high-temperature furnace and fired, with the firing temperature curve rising from room temperature at a rate of 5°C / min to 120°C, held for 2 hours, rising further at a rate of 5°C / min to 450°C, held for 2 hours, rising further at a rate of 5°C / min to 900°C, held for 13 hours, the atmosphere in the high-temperature furnace is a mixture of dry oxygen gas and nitrogen gas (of which oxygen gas accounts for 25%), and the fired powder is then rapidly cooled to room temperature with chilled water to obtain the second powder. Book firing During the process, maintaining the temperature at 120°C for 2 hours primarily reduces the moisture content of the first powder, and in the subsequent rapid heating process, the moisture content in the high-temperature furnace atmosphere becomes too high, causing side reactions. Sodium ion layered metal oxide material This is to avoid having too high an impurity phase, and the 2-hour incubation at 450°C mainly promotes the decomposition and melting of copper oxide, improving the compatibility of copper with other elements. Sodium ion layered metal oxide material To make the distribution of copper inside more uniform, Sodium ion layered metal oxideThis is to improve the uniformity of the materials and ensure the stability of the product. Otherwise, Sodium ion layered metal oxide material The uneven distribution of copper elements within it means that Sodium ion layered metal oxide material The electrical performance of the sampling tests at different points does not match, leading to low product stability, or poor compatibility between copper and other elements. Sodium ion layered metal oxide material A high level of copper oxide impurities inside causes poor electrical performance.
[0068] Book firing During the process, the water content in the high-temperature furnace was controlled to be less than 3%, the carbon dioxide concentration to be less than 1%, and the oxygen content to be between 20% and 35%.
[0069] The second powder is ground, sieved, and iron is removed to obtain a sodium ion layered metal oxide material. The humidity of the environment during grinding and sieving is controlled to be less than 15%, and the obtained sodium ion layered metal oxide material is granular. diameter and Furthermore, D50 was 8.5 μm, D100 was 36 μm, the magnetic foreign matter content was less than 150 ppm, and manganese elution occurred. amount The concentration is less than 0.5 ppm, free sodium is less than 100 ppm, and water is less than 1000 ppm. The SEM image of the sodium ion layered metal oxide material is shown in Figure 1. The sodium ion layered metal oxide exhibits a typical layered structure, with small particles aggregating to form larger particles, and the primary particle size is 0.7 μm The size was approximately 7 μm.
[0070] The XRD of the sodium ion layered metal oxide material is as shown in Figure 2. A button battery is manufactured using a sodium ion layered metal oxide material as the positive electrode. V The charge-discharge curve within the ~4.0V range is shown in Figure 3, and the discharge ratio capacity at 0.1C is 138mAh / g, until Cu and F are doped. Sodium ion layered metal oxide The capacity retention rate of the material at 1C after 100 cycles was approximately 80%. After doping with F and Cu elements, the discharge ratio capacity at 0.1C remained almost unchanged compared to the undoped state. Sodium ion layered metal oxideThe 100-cycle capacity retention rate of the material at 1C is 91.2%, which is an improvement of about 11% After doping with F and Cu elements. , compared with the case where only the Cu element is doped Sodium ion layered metal oxide the 100-cycle capacity retention rate of the material at 1C Approximately is improved by 5% (The capacity retention rate of a sodium ion layered metal oxide material doped only with Cu is 85.3% after 100 cycles at 1C.) . The introduction of the M element is also beneficial for improving the environmental stability of the layered metal oxide, and compared with the material not doped with the M element Sodium ion layered metal oxide , after being left to stand for the same time in the same air atmosphere and doped with the M element Sodium ion layered metal oxide the discharge specific capacity of the material is improved by 5% to 10%.
[0071] (Comparative Example 1) A sodium-ion layered metal oxide material was produced and a button cell was assembled by the method in Example 1, with the difference that the chemical formula of the sodium-ion layered metal oxide material is Na 0.95 Ni 0.5 Mn 0.3 Ti 0.2 O2 A button cell was produced by the method in Example 1 and subjected to an electrochemical performance test, and the results showed that the discharge specific capacity at 0.1C was 135.5 mAh / g, Sodium ion layered metal oxide and the 100-cycle capacity retention rate of the material at 1C was about 80%.
[0072] (Comparative Example 2) A sodium-ion layered metal oxide material was produced and a button cell was assembled by the method in Example 1, with the difference that the chemical formula of the sodium-ion layered metal oxide material is Na 0.95 Ni 0.45 Mn 0.3 Cu 0.05 Ti 0.2 O2 A button cell was produced by the method in Example 1 and subjected to an electrochemical performance test, and the results showed that the discharge specific capacity at 0.1C was 137 mAh / g, Sodium ion layered metal oxide and the 100-cycle capacity retention rate of the material at 1C was about 85.3%.
[0073] (Comparative Example 3) A sodium ion layered metal oxide material was manufactured using the method in Example 1, and a button battery was assembled. However, the chemical formula of the sodium ion layered metal oxide material is Na 0.95 Ni 0.5 Mn 0.3 Ti 0.2 O 1.95 F 0.05 There was a difference in that. A button cell was manufactured using the method described in Example 1, and electrochemical performance tests were conducted. The discharge ratio capacity at 0.1C was 136 mAh / g. Sodium ion layered metal oxide The results showed that the capacity retention rate of the 1C material after 100 cycles was approximately 82.4%.
[0074] (Comparative Example 4) In Example 1, a sodium ion layered metal oxide material was manufactured and a button battery was assembled using the method described in Example 1. However, there was a difference in that the first heating step was omitted, and the temperature was directly raised to 450°C at 5°C / min, maintained for 3 hours, and then further raised to 900°C at 5°C / min, maintained for 13 hours. When a button battery was manufactured using the method in Example 1 and subjected to electrochemical performance testing, 2 V The results showed that the discharge ratio capacity within the ~4.0V charge / discharge range was 125mAh / g.
[0075] (Comparative Example 5) In Example 1, a sodium ion layered metal oxide material was manufactured and a button battery was assembled, but the first heating step was omitted. Instead, the temperature was directly raised to 900°C at 5°C / min, and then maintained at 13 hours. V One difference was that the discharge ratio capacity within the ~4.0V charge / discharge range was 121mAh / g.
[0076] (Example 2) The chemical formula for sodium ion layered metal oxide material is NaNi 0.48 Mn 0.4 Y 0.02 Ti 0.1 O 1.999 F 0.001 And, Sodium ion layered metal oxideBased on the metering ratio of the number of moles of metal elements in the chemical formula of the material, sodium bicarbonate, nickel oxide, trimanganese tetroxide, titanium oxide, sodium fluoride, yttrium oxide and a certain amount of deionized water are put into a coarse grinder and mixed uniformly, the material mixing time is 2 h, the operating frequency is 30 Hz, to obtain a first slurry (with a solid content of 30% and a particle size of D100 < 7 μm), The first slurry is ground and mixed in a sand mill by switching tanks in an A / B tank circulation mode, the grinding time is 3 h, the rotation speed of the sand mill is 1000 r / min, to obtain a second slurry (with a particle size of D50 < 2 μm and D100 < 7 μm), The second slurry is spray-dried to obtain a first powder (with a particle size of 3 μm < D50 < 10 μm, D100 < 30 μm, a moisture content of less than 1%, and a BET of 30 m 2 / g), The first powder is placed in a high-temperature furnace for calcination, and the calcination temperature curve is: rising from room temperature to 120°C at 4°C / min, holding for 2 h, further rising to 455°C at 6°C / min, holding for 2 h, further rising to 850°C at 7°C / min, and holding for 20 h, then the calcined material is rapidly cooled, and the rapid cooling method may be cooling with liquid nitrogen or cooling with chilled water, This firing In the process, holding at 120°C for 2 h mainly reduces the water content of the first powder, and avoids that in the subsequent rapid temperature rise process, the water content in the high-temperature furnace atmosphere is too high, side reactions occur, Sodium ion layered metal oxide material the impurity phase is too high, and when the maximum firing temperature is 850°C, the compatibility between Y and other elements can be improved, Sodium ion layered metal oxide material making the distribution of Y element in it more uniform, Sodium ion layered metal oxide improving the uniformity of the material and ensuring the stability of the product. Otherwise, Sodium ion layered metal oxide material the non-uniform distribution of Y element in it will lead to Sodium ion layered metal oxide material inconsistent electrical performance of sampling tests at different points in the process, ultimately resulting in poor product consistency, in addition, firing when the temperature is 850°C, Sodium ion layered metal oxide materialprimary particles are too large, and the degradation of electrical performance can be avoided.
[0077] The present firing process was controlled such that the water content in the high-temperature furnace was less than 2%, the carbon dioxide concentration was less than 1%, and the oxygen content was 20% to 50%.
[0078] The second powder was pulverized, sieved, and iron-removed to obtain a sodium-ion layered metal oxide material, the environmental humidity for pulverization and sieving was controlled to be less than 10%, and the resulting sodium-ion layered metal oxide material had a particle size range of 2 μm < D50 < 10 μm, 25 μm < D100 < 35 μm, a magnetic foreign matter content of less than 150 ppm, and manganese elution amount of less than 0.5 ppm, free sodium of less than 100 ppm, and water content of less than 1000 ppm.
[0079] The SEM of the sodium-ion layered metal oxide material is as shown in Figure 5. The sodium-ion layered metal oxide exhibits a typical layered structure, small particles agglomerate to form large particles, and the primary particle size is 0.2 μm ~4.5 μm.
[0080] A button cell was fabricated using the sodium-ion layered metal oxide material as the positive electrode, and 2 V The charge-discharge curve in the ~4.0 V interval is as shown in Figure 4, the 0.1C discharge specific capacity is 135 mAh / g, and the 1C 100-cycle capacity retention rate is about 85.2%. Before doping Y and F, (NaNi 0.5 Mn 0.4 Ti 0.1 O2) Sodium ion layered metal oxide The 1C 100-cycle capacity retention rate of the material is about 80%, and the 0.1C discharge specific capacity is 135.5 mAh / g. After doping with Y and F elements, the 0.1C discharge specific capacity is slightly reduced compared with the case without doping, but Sodium ion layered metal oxide the 1C 100-cycle capacity retention rate of the material is improved by about 5%. After doping with Y, the layered metal oxide material has strong Y-O bonds, forms a stable structure, Sodium ion layered metal oxide The material was surrounded by a Y2O3 protective layer. The expanded Na layer further caused sodium ions to intercalate not only on the surface but also into the bulk. Therefore, after Y was doped Sodium ion layered metal oxide the recycling performance of the material was improved. In addition, yttrium oxide does not decompose or melt at 850°C, which corresponds to the introduction of a small amount of impurity phase. However, in this product, the added amount of yttrium oxide is small, and no adverse effect on the electrical performance was caused.
[0081] (Example 3) The chemical formula of the sodium-ion layered metal oxide material is Na 0.9 Ni 0.48 Mn 0.39 Cu 0.02 Mg 0.01 Ti 0.1 O2, Sodium ion layered metal oxide Based on the stoichiometric ratio of the number of moles of metal elements in the chemical formula of the material, sodium carbonate, nickel hydroxide, manganese dioxide, titanium oxide and alcohol are put into a rough grinder and mixed uniformly, the material mixing time is 2 h, the operating frequency is 30 Hz, to obtain a first slurry (with a solid content of 20% and a particle size of D100<10 μm), The first slurry is ground and mixed in a sand mill by switching tanks in an A / B tank circulation mode, the grinding time is 3 h, the rotation speed of the sand mill is 1000 r / min, to obtain a second slurry (with a particle size of D50<3 μm and D100<10 μm), The second slurry is spray-dried to obtain a first powder (with a particle size of 3 μm<D50<8 μm, D100<35 μm, a moisture content of less than 1%, and a BET of 30 m 2 / g), The first powder is placed in a high-temperature furnace for calcination. The calcination temperature curve is: rising from room temperature at 4°C / min to 120°C, holding for 3 h, further rising at 7°C / min to 450°C, holding for 1 h, further rising at 8°C / min to 950°C, and holding for 15 h. The atmosphere in the high-temperature furnace is dry oxygen gas, followed by rapid cooling to room temperature to obtain a second powder. The rapid cooling method may be cooling with liquid nitrogen or cooling with chilled water, This firing In the process, maintaining the temperature at 120°C for 3 h mainly reduces the water content of the first powder, so as to avoid excessive water content in the high-temperature furnace atmosphere during the subsequent rapid temperature rise process, which would cause side reactions, Sodium ion layered metal oxide material and excessively high impurity phases. Maintaining the temperature at 450°C for 3 h mainly promotes the decomposition and melting of copper oxide, improves the compatibility between copper and other elements, Sodium ion layered metal oxide material makes the distribution of copper in the material more uniform, Sodium ion layered metal oxide improves the uniformity of the material, and ensures the stability of the product. Otherwise, Sodium ion layered metal oxide material the non-uniform distribution of copper element in the material will lead to Sodium ion layered metal oxide material inconsistent electrical performance of sampling tests at different points on the product, resulting in low product stability, or poor compatibility between copper element and other elements, Sodium ion layered metal oxide material and high copper oxide impurities in the material will lead to poor electrical performance.
[0082] In the present firing process, the water content in the high-temperature furnace is controlled to be less than 2%, and the carbon dioxide concentration is controlled to be less than 1%, firing During the process, the contents of moisture and carbon dioxide in the high-temperature furnace are detected online, the gas flow rate and discharge amount are adjusted in a timely manner, and the contents of moisture and carbon dioxide in the high-temperature furnace are controlled within the control range.
[0083] The second powder is pulverized, sieved and de-ironed to obtain a sodium ion layered metal oxide material. The environmental humidity during pulverization and sieving is controlled to be less than 10%. The obtained sodium ion layered metal oxide material has a particle size range of 3 μm < D50 < 10 μm, 25 μm < D100 < 40 μm, a magnetic foreign matter content of less than 150 ppm, and manganese elution amount of less than 0.5 ppm, free sodium of less than 100 ppm, and moisture of less than 1000 ppm.
[0084] The SEM of the sodium ion layered metal oxide material is as shown in Figure 7. The sodium ion layered metal oxide exhibits a typical layered structure, small particles agglomerate to form large particles, and the primary particle size is 0.5 μmThe size was approximately 5 μm.
[0085] The chemical formula is Na 0.9 Ni 0.48 Mn 0.39 Cu 0.02 Mg 0.01 Ti 0.1 A button battery is manufactured using a sodium ion layered metal oxide material of O2 as the positive electrode. V The charge-discharge curve within the ~4.0V range is shown in Figure 6. The discharge ratio capacity at 0.1C is 129 mAh / g, and the capacity retention rate after 100 cycles at 1C is approximately 92.1%. It takes time to dope with Cu and Mg (i.e., Na 0.9 Ni 0.5 Mn 0.4 Ti 0.1 O2) Sodium ion layered metal oxide The capacity retention rate of the material at 1C after 100 cycles was approximately 80%, and the discharge ratio capacity at 0.1C was 135.5 mAh / g. After doping with Cu and Mg elements, the discharge ratio capacity at 0.1C decreased slightly compared to the undoped material. Sodium ion layered metal oxide The capacity retention rate of the 1C material after 100 cycles improved by approximately 12%. Doping with Mg in addition to doping with Cu is equivalent to substituting trivalent manganese ions with divalent magnesium ions, which can increase the interlayer distance, thereby promoting the diffusion of sodium ions and mitigating lattice strain caused by the desorption process of sodium ions, improving the stability of the layered structure. Furthermore, doping with divalent magnesium ions can mitigate structural deformation or volume changes caused by the charge-discharge cycle process of sodium-ion batteries, suppressing irreversible phase changes. Sodium ion layered metal oxide It has a significant impact on improving the reversible ratio capacity of the material. In addition, Mg has the same Sodium ion layered metal oxide Although the material exhibits non-electrochemical activity and does not intervene in redox reactions, the amount of magnesium oxide added in this product is small and does not adversely affect its electrical performance.
[0086] The above are merely preferred embodiments of the present invention, and it should be noted that those skilled in the art can make several improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for producing a sodium ion layered metal oxide material, The sodium ion layered metal oxide material is a sodium ion layered metal oxide material having the chemical formula shown in formula I, Na x Ni a Mn b Ti (0.5-b) M (0.5-a) O (2-y) F y Formula I, Here, 0.9 ≤ x ≤ 1.0, 0.3 ≤ a < 0.5, 0.3 ≤ b ≤ 0.4, 0.1 ≤ 1 - a - b ≤ 0.35, 0 ≤ y < 0.1, and M includes at least one of Mg, Y, and Cu. The method for producing the sodium ion layered metal oxide material is as follows: A) A step in which Na source, Ni source, Mn source, Ti source, M source, and F source are mixed with a solvent according to the stoichiometric ratio in formula I, and then rough polishing is performed to obtain a first slurry, B) The step of polishing the first slurry to obtain a second slurry, C) The step of spray-drying the second slurry to obtain the first powder, D) A step of obtaining a second powder by calcining the powder in the following process, The process involves heating the temperature from room temperature to 110°C to 130°C in an oxygen-containing atmosphere at a heating rate of 3°C / min to 5°C / min, maintaining the temperature for 2 to 4 hours, then further heating to 440°C to 460°C at a heating rate of 5°C / min to 8°C / min, maintaining the temperature for 1 to 3 hours, and finally heating to 850°C to 950°C at a heating rate of 5°C / min to 8°C / min, maintaining the temperature for 10 to 20 hours. E) The second powder is pulverized and sieved to remove iron, and a sodium ion layered metal oxide material having the chemical formula shown in formula I is obtained, A method for producing a sodium ion layered metal oxide material.
2. The aforementioned sodium ion layered metal oxide material is an O3 type manganese base layered oxide material. A method for producing a sodium ion layered metal oxide material according to feature 1.
3. In step A), the solvent used for rough polishing is water and / or alcohol, the solid content of the first slurry is 10% to 40%, and the particle size of the first slurry is D100 < 10 μm. The manufacturing method according to claim 1, characterized in that it
4. The sodium ion layered metal oxide material is Na 0.95 Ni 0.45 Mn 0.3 Cu 0.05 Ti 0.2 O 1.95 F 0.05 , NaNi 0.48 Mn 0.4 Y 0.02 Ti 0.1 O 1.999 F 0.001, one or more of the foregoing. The manufacturing method according to claim 3, characterized in that it
5. The aforementioned firing process is as follows: The process involves heating the room temperature to 120°C-125°C in an oxygen-containing atmosphere at a rate of 4°C / min-5°C / min, maintaining the temperature for 2-3 hours, then further heating to 450°C-455°C at a rate of 5°C-7°C / min, maintaining the temperature for 1-2 hours, and finally heating to 850°C-950°C at a rate of 5°C-8°C / min, maintaining the temperature for 13-20 hours. The manufacturing method according to feature 4.
6. In the aforementioned firing process, the oxygen content is 20% to 35%, the moisture content is less than 3%, and the carbon dioxide concentration is less than 1%. The manufacturing method according to claim 1, characterized in that it
7. After firing is complete, rapid cooling is performed to obtain the second powder. The aforementioned rapid cooling is a quenching process. The manufacturing method according to claim 1, characterized in that it
Citation Information
Patent Citations
Layered active materials for sodium ion batteries
CN114207878A
Sodium-ion battery positive electrode material and preparation method thereof, positive electrode plate and sodium-ion battery
CN115440975A
Doped nickelate compounds
JP2015536890A
Sodium metal oxide material for secondary batteries and manufacturing method
JP2022504285A