AI Technical Summary
Thick heat-shrinkable polyester films used for packaging become waste after use, and reducing their thickness to minimize waste leads to decreased firmness and potential wrinkling due to poor air release when rolled, while biaxial stretching methods are complex and costly.
A heat-shrinkable polyester film with specific properties, including a hot water heat shrinkage rate, surface roughness, and air release time, achieved through uniaxial stretching and lamination with fine particles, maintaining transparency and printability while preventing wrinkles when rolled.
The film maintains transparency and printability, prevents wrinkling when wound into a roll, and achieves the desired shrinkage rates while being cost-effective and simpler to produce compared to biaxial stretching methods.
Abstract
Description
Heat-shrinkable polyester film
[0001] The present invention relates to a heat-shrinkable polyester film, and more particularly to a heat-shrinkable polyester film that is transparent, has few wrinkles when rolled, and is suitable for processing such as printing, a heat-shrinkable label, and a packaging material.
[0002] In recent years, polyester heat-shrinkable films, which offer high heat resistance, ease of incineration, and excellent solvent resistance, have been widely used as shrink labels for applications such as label packaging, cap seals, and stacked packaging, which combine the protection of glass or plastic bottles with product labeling. Their usage has been increasing with the increase in PET (polyethylene terephthalate) bottle containers. Until now, thick heat-shrinkable films have been used for PET bottle labels. However, heat-shrinkable films used for packaging simply become waste after the contents have been used. Therefore, in response to growing environmental awareness to reduce waste as much as possible, film manufacturers have also attempted to reduce the thickness of heat-shrinkable polyester films in order to reduce the thickness of labels. However, the inventors have discovered that reducing the film thickness reduces the film's stiffness and makes it easier for air to enter when rolled up, resulting in wrinkles when the film is rolled up if the air does not escape easily.
[0003] Japanese Patent No. 5240387 Japanese Patent Application Laid-Open No. 2020-117700
[0004] Typical heat-shrinkable films are uniaxially stretched, resulting in high tensile break strength in the main shrinkage direction (stretching direction) and low tensile break strength in the non-shrinkage direction (direction perpendicular to the main shrinkage direction). In contrast, Patent Document 1 (Patent Document 1) describes a heat-shrinkable polyester film with high strength produced by biaxially stretching the film to increase its tensile break strength in both the longitudinal and transverse directions. However, compared to typical heat-shrinkable film production methods, this method has issues such as a very complicated film production process, the need for large-scale equipment, and high initial investment costs. Patent Document 2 (Patent Document 2) also specifies the surface roughness and inorganic particle content of biaxially stretched polyester films. Patent Document 2 relates to crystalline biaxially stretched polyester films. Heat-shrinkable polyester films made from amorphous raw materials and only uniaxially stretched differ from biaxially stretched polyester films in terms of surface roughness due to surface protrusions and air escape when rolled. Therefore, the present invention aims to provide a heat-shrinkable polyester film that has good air release, good winding quality, is less likely to cause wrinkles, and has good printability, even when the film has a thickness of 15 μm to 50 μm.
[0005] The present invention, which has solved the above-mentioned problems, comprises the following: 1. A heat-shrinkable polyester film characterized by satisfying the following requirements (1) to (5): (1) When the film is immersed in 90°C hot water for 10 seconds, the hot water heat shrinkage is 40% or more and 80% or less in the film width direction; (2) When the film is immersed in 90°C hot water for 10 seconds, the hot water heat shrinkage is -5% or more and 10% or less in the film longitudinal direction; (3) The maximum protrusion height Sp of at least one film surface is 0.8 μm or more and 3.0 μm or less; (4) The arithmetic mean height Sa of at least one film surface is 0.03 μm or more and 0.2 μm or less; and (5) The air escape time between the front and back surfaces of the film is 14 seconds or less. 2. The heat-shrinkable polyester film according to 1., characterized in that the film thickness is 15 μm or more and 50 μm or less. 3. 1. or 2., characterized in that the haze at a film thickness of 30 μm is 2% or more and 11% or less. 4. The heat-shrinkable polyester film according to any one of 1. to 3., which is a laminated heat-shrinkable polyester film having at least two or more layers laminated together. 5. A heat-shrinkable label using the heat-shrinkable polyester film according to any one of 1. to 4.. 6. A package formed by covering at least a portion of the outer periphery of an object to be packaged with the heat-shrinkable label according to 5. and heat-shrinking it.
[0006] The heat-shrinkable polyester film of the present invention maintains transparency and printability by controlling the surface roughness and air release within a certain range, and even if the film thickness is thin, wrinkles and printability can be maintained well when wound into a roll.
[0007] FIG. 1 is a diagram showing a method for measuring the air release time of the present invention.
[0008] The heat-shrinkable polyester film of the present invention will be described in detail below. The method for producing the heat-shrinkable polyester film will be described in detail later. The heat-shrinkable film is usually obtained by conveying and stretching the film using rolls or the like. The conveying direction of the film (film-forming direction) is referred to as the longitudinal direction, and the direction perpendicular to the longitudinal direction is referred to as the width direction of the film.
[0009] The heat-shrinkable polyester film of the present invention is a heat-shrinkable polyester film characterized by satisfying the following requirements (1) to (5): (1) When the film is immersed in hot water at 90°C for 10 seconds, the hot water heat shrinkage is 40% to 80% in the width direction of the film; (2) When the film is immersed in hot water at 90°C for 10 seconds, the hot water heat shrinkage is -5% to 10% in the length direction of the film; (3) The maximum protrusion height Sp of at least one film surface is 0.8 μm to 3 μm; (4) The arithmetic mean height Sa of at least one film surface is 0.03 μm to 0.2 μm; and (5) The air escape time between the front and back surfaces of the film is 14 seconds or less.
[0010] The polyester used in the heat-shrinkable polyester film of the present invention is one having ethylene terephthalate units as its main constituent component. The ethylene terephthalate units preferably account for 50 mol% or more, more preferably 60 mol% or more, and even more preferably 70 mol% or more of the 100 mol% of the constituent units of the polyester. Other dicarboxylic acid components constituting the polyester of the present invention include aromatic dicarboxylic acids such as isophthalic acid, orthophthalic acid, and 2,6-naphthalenedicarboxylic acid; aliphatic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, and decanedicarboxylic acid; and alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid. It is also preferable that the polyester does not contain trivalent or higher polycarboxylic acids (e.g., trimellitic acid, pyromellitic acid, and anhydrides thereof). Heat-shrinkable polyester films obtained using polyesters containing these polycarboxylic acids are less likely to achieve the required high shrinkage.
[0011] Examples of diol components constituting the polyester include, in addition to ethylene glycol, aliphatic diols such as 1,3-propanediol, 2,2-diethyl-1,3-propanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2-isopropyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, 1,4-butanediol, hexanediol, neopentyl glycol, and hexanediol; alicyclic diols such as 1,4-cyclohexanedimethanol; and aromatic diols such as bisphenol A. Among these, it is preferable to use cyclic diols such as 1,4-cyclohexanedimethanol, and diols having 3 to 6 carbon atoms (e.g., 1,3-propanediol, 1,4-butanediol, neopentyl glycol, and hexanediol). In particular, the use of 1,4-butanediol or neopentyl glycol makes it easier to obtain a polyester that satisfies the essential requirements of the present invention.
[0012] Furthermore, the polyester has a total amorphous content of 17 mol% or more, preferably 18 mol% or more, more preferably 19 mol% or more, and particularly preferably 20 mol% or more, based on 100 mol% of the polyhydric alcohol component and 100 mol% of the polycarboxylic acid component in the entire polyester resin (i.e., a total of 200 mol%). Among the aforementioned monomer components, examples of monomers that can become amorphous components include neopentyl glycol, 1,4-cyclohexanedimethanol, isophthalic acid, 1,4-cyclohexanedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,2-diethyl-1,3-propanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2-isopropyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, and hexanediol. The upper limit of the total amorphous content is not particularly limited, but it is preferably 30 mol% or less. By adjusting the amount of amorphous components to the above range, a polyester having a glass transition point (Tg) adjusted to 60 to 80°C can be obtained.
[0013] It is preferable that the polyester does not contain diols having 8 or more carbon atoms (e.g., octanediol, etc.) or polyhydric alcohols having a valence of 3 or more (e.g., trimethylolpropane, trimethylolethane, glycerin, diglycerin, etc.). Heat-shrinkable polyester films obtained using polyesters containing these diols or polyhydric alcohols are unlikely to achieve the required high shrinkage ratio. It is also preferable that the polyester does not contain diethylene glycol, triethylene glycol, or polyethylene glycol as much as possible.
[0014] Various additives, such as waxes, antioxidants, antistatic agents, crystal nucleating agents, viscosity reducers, heat stabilizers, coloring pigments, color inhibitors, and ultraviolet absorbers, may be added to the resin forming the heat-shrinkable polyester film of the present invention, as needed.
[0015] It is preferable to add fine particles to the resin forming the heat-shrinkable polyester film of the present invention to achieve a predetermined range for the maximum protrusion height (Sp), arithmetic mean height (Sa), and air escape time between the front and back surfaces of the film. Any fine particles can be selected, but examples include inorganic fine particles such as silica, alumina, titanium dioxide, calcium carbonate, kaolin, and barium sulfate, and organic fine particles such as acrylic resin particles, melamine resin particles, silicone resin particles, and cross-linked polystyrene particles. The average particle size of the fine particles is within the range of 1.0 to 5.0 μm (as measured with a Coulter counter), preferably within the range of 2.0 to 5.0 μm, and can be selected as needed. Regarding particle shape, either spherical or amorphous is acceptable, but spherical particles tend to produce more protrusions on the film surface than amorphous particles. However, spherical particles are generally more expensive than amorphous particles, so it is desirable to select them according to the purpose. The amount of fine particles added to the front and back layers of the heat-shrinkable polyester film is preferably 350 ppm to 20,000 ppm. If the amount of fine particles added is less than 350 ppm, the maximum protrusion height Sp and arithmetic mean height Sa on the film surface will be low, making it impossible to keep the air venting time within the specified range, which is undesirable. Furthermore, if the amount of fine particles added is more than 20,000 ppm, the air venting time will be shortened, which is preferable, but the maximum protrusion height Sp and arithmetic mean height Sa will be increased, which is undesirable as it will deteriorate transparency and printability. A concentration of 450 ppm or more and 19,000 ppm or less is more preferable, and a concentration of 550 ppm or more and 18,000 ppm or less is particularly preferable. By using the above-mentioned preferred fine particles in combination with the preferred manufacturing method described below, protrusions suitable for the present invention can be formed on the film surface, and the maximum protrusion height Sp, arithmetic mean height Sa, and air venting time can be controlled within the specified ranges.
[0016] The method of incorporating the particles into the resin that forms the heat-shrinkable polyester film can be, for example, adding them at any stage in the production of the polyester resin, but it is preferable to add them as a slurry dispersed in ethylene glycol or the like at the stage of esterification or after the completion of the transesterification reaction and before the start of the polycondensation reaction, and then proceed with the polycondensation reaction. Also preferred is a method of blending a slurry of particles dispersed in ethylene glycol or water or the like with a polyester resin raw material using a vented kneading extruder, or a method of blending dried particles with a polyester resin raw material using a kneading extruder.
[0017] The heat-shrinkable polyester film of the present invention can also be subjected to corona treatment, coating treatment, flame treatment, etc. to improve the adhesion of the film surface. The heat-shrinkable polyester film of the present invention also includes a laminated polyester film having at least one polyester resin layer. When two or more polyester resin layers are laminated, the polyester resin layers may be polyesters of the same composition or different compositions. Furthermore, the other layers that can be laminated are not particularly limited as long as they are thermoplastic resin layers, but polystyrene resin layers are preferred in terms of cost and heat shrinkage properties. In a laminate of two or more polyester resin layers, a polyester resin layer containing fine particles must be on the front and back surfaces. This is because, in a film roll, the front and back layers overlap, and by setting the maximum protrusion height Sp and arithmetic mean height Sa on the film surface within a specified range, wrinkling of the film roll can be suppressed. The layer structure can be one type of two-layer, two types of three-layer, three types of three-layer, or three types of five-layer, but a two-type, three-layer structure is suitable for preventing equipment size increase and controlling the protrusions and transparency of the film surface. In a two-kind three-layer structure, a polyester resin layer containing fine particles / a polyester resin layer not containing fine particles / a polyester resin layer containing fine particles is preferred. Using the same polyester resin layer containing fine particles has the advantage of being able to control the protrusions on the front and back of the film to be the same. Furthermore, using a layer not containing fine particles as the intermediate layer can improve transparency. In a two-kind three-layer structure, the polyester resin layers containing fine particles on the front and back preferably account for 4% to 70% of the total thickness. If the thickness is less than 4%, the thickness of one side of the polyester resin layer will be less than 2%, and if the thickness accuracy of the polyester resin layer containing fine particles during film production deteriorates, the thickness of the polyester resin layer containing fine particles will become thin, making it impossible to obtain the desired surface protrusions, which is undesirable. A thickness greater than 70% is acceptable, but a thick polyester resin layer not containing fine particles will deteriorate transparency, which is undesirable. In a two-kind three-layer structure, the thickness ratio of the polyester resin layer containing fine particles among the two types constituting the polyester resin layer containing fine particles / a polyester resin layer not containing fine particles / a polyester resin layer containing fine particles is more preferably 8% to 60%, and particularly preferably 10% to 50%.
[0018] It is preferable to add a thermoplastic resin and / or a rubber component to the polystyrene resin. Examples of the thermoplastic resin include styrene resins such as polystyrene having an atactic structure, AS resin, and ABS resin, polyester resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate, polyamide resins such as nylon 6, nylon 66, nylon 12, nylon 4, and polyhexamethylene adipamide, and polyolefin resins such as polyethylene, polypropylene, and polybutene.
[0019] On the other hand, the rubber component is preferably a rubbery copolymer containing a styrene-based compound as its constituent, and examples thereof include random, block, or graft copolymers obtained by copolymerizing one or more types of styrene and one or more rubber components. Examples of such rubbery copolymers include styrene-butadiene copolymer rubber, styrene-isoprene block copolymers, rubbers in which the butadiene moiety thereof has been partially or completely hydrogenated, methyl acrylate-butadiene-styrene copolymer rubber, acrylonitrile-butadiene-styrene copolymer rubber, acrylonitrile-alkyl acrylate-butadiene-styrene copolymer rubber, and methyl methacrylate-alkyl acrylate-butadiene-styrene copolymer rubber. Rubbery copolymers containing the above-mentioned styrene-based compounds as their constituents have styrene units, which allows for good dispersibility in polystyrene-based resins having a syndiotactic structure and a significant effect of improving the plasticity of polystyrene-based resins. Furthermore, rubbery copolymers containing the above-mentioned styrene-based compounds as their constituents can be suitably used as compatibility modifiers.
[0020] On the other hand, other rubber components that can be used include natural rubber, polybutadiene, polyisoprene, polyisobutylene, neoprene, ethylene-propylene copolymer rubber, urethane rubber, silicone rubber, acrylic rubber, polyether-ester rubber, polyester-ester rubber, and the like.
[0021] Furthermore, the weight-average molecular weight of the polystyrene-based resin is preferably 10,000 or more, and more preferably 50,000 or more. A weight-average molecular weight of less than 10,000 is undesirable because the film's strength and elongation properties and heat resistance tend to decrease. While there is no particular upper limit for the weight-average molecular weight, a weight-average molecular weight exceeding 1,500,000 is undesirable because it can cause breakage due to increased stretching tension. Various grades of polystyrene-based resins are commercially available from various manufacturers, and commercially available resins may be used. The other layers may be one layer or two or more layers. In multilayer films with polystyrene, it is recommended to use a polyester layer / polystyrene layer / polyester layer structure from the film surface, with the polyester layer, which has excellent gloss and printability, as the outermost layer. However, polyester and polystyrene are incompatible resins, which can lead to the problem of relative peeling. Therefore, a three-type, five-layer structure is preferred, with the adhesive layer sandwiched between the film surface: polyester layer / adhesive layer / polystyrene layer / adhesive layer / polyester layer. It is also possible to use a 3-type 7-layer structure or a 3-type 9-layer structure, but the equipment will be larger than that for a 3-type 5-layer structure.
[0022] In a three-kind, five-layer film, the polyester layer preferably accounts for 20% to 80% of the total thickness. If it is less than 20%, the thickness of one side of the polyester layer will be less than 10%, which is undesirable as it will result in a film with insufficient printability and gloss. If it is more than 80%, the polystyrene layer will become thin and the effect of suppressing the shrinkage rate in the longitudinal direction will be reduced, which is undesirable. In a three-kind, five-layer film, the polyester layer more preferably accounts for 25% to 75% of the total thickness, and particularly preferably 30% to 70%.
[0023] In a three-kind, five-layer film, the adhesive layer preferably accounts for 1% to 14% of the total thickness. A thickness of less than 1% is undesirable because adhesiveness decreases. A thickness of more than 14% is undesirable because the thicknesses of the polyester and polystyrene layers become thin and thermal shrinkage properties decrease. In a three-kind, five-layer film, the adhesive layer more preferably accounts for 2% to 12% of the total thickness, and particularly preferably 3% to 10%. In a three-kind, five-layer film, the polystyrene layer preferably accounts for 20% to 80% of the total thickness. A thickness of less than 20% is undesirable because the effect of suppressing longitudinal shrinkage is reduced. A thickness of 80% or more is undesirable because the thickness of one side of the polyester layer becomes less than 10%, resulting in insufficient printability and gloss of the film. In a three-kind, five-layer film, the polystyrene layer more preferably accounts for 25% to 75% of the total thickness, and particularly preferably 30% to 70%.
[0024] The heat-shrinkable polyester film of the present invention preferably has a heat shrinkage rate in the width direction, which is the main shrinkage direction of the film, of 40% or more and 80% or less when treated in hot water at 90°C under no load for 10 seconds, calculated from the lengths before and after shrinkage using the following formula 1 (i.e., hot water heat shrinkage rate at 90°C): Heat shrinkage rate = {(length before shrinkage - length after shrinkage) / length before shrinkage} x 100 (%) Formula 1
[0025] If the hot water heat shrinkage rate in the main shrinkage direction at 90°C is less than 40%, when used as a film for beverage labels or lunch box packaging, the small shrinkage amount will result in label wrinkles and sagging after heat shrinkage, which is undesirable. A hot water shrinkage rate of 43% or more at 90°C is more preferable, 46% or more is particularly preferable, and 50% or more is most preferable. There is no problem even if the hot water heat shrinkage rate in the main shrinkage direction at 90°C is higher than 80%, but since it was not possible to obtain a film with a hot water heat shrinkage rate at 90°C higher than 80% in the present invention, the upper limit was set to 80%.
[0026] The heat-shrinkable polyester film of the present invention preferably has a hot water shrinkage rate at 90°C in the longitudinal direction perpendicular to the main shrinkage direction of the film from -5% to 10%. If the hot water shrinkage rate at 90°C in the longitudinal direction is less than -5%, when used as a beverage label, the label will stretch, undesirably increasing the height of the label on the PET bottle. A hot water shrinkage rate at 90°C in the longitudinal direction is more preferably -4% or more, and particularly preferably -3% or more. If the hot water shrinkage rate at 90°C in the longitudinal direction is greater than 10%, when used as a beverage label, the label will shrink, undesirably decreasing the height of the label on the PET bottle. This may also cause distortion of the label after shrinkage. A hot water shrinkage rate at 90°C in the longitudinal direction is more preferably 9% or less, even more preferably 8% or less, particularly preferably 7% or less, and most preferably 6% or less.
[0027] The maximum protrusion height Sp on at least one surface of the heat-shrinkable polyester film of the present invention is preferably 3.0 μm or less, more preferably 2.5 μm or less, and even more preferably 2.0 μm or less. If the maximum protrusion height Sp is higher than 3.0 μm, the formation of coarse protrusions can result in print defects, poor print appearance, poor design, and other impairments to film quality, which is undesirable. The maximum protrusion height Sp on at least one surface of the heat-shrinkable polyester film of the present invention is preferably 0.8 μm or more, more preferably 1.2 μm or more, and even more preferably 1.6 μm or more. If the maximum protrusion height Sp is less than 0.8 μm, the air entrained during winding onto a roll cannot be uniformly released, which can easily cause poor appearance such as wrinkles and pimples on the air bubbles, and can easily deteriorate winding properties.
[0028] The arithmetic mean height Sa of at least one surface of the heat-shrinkable polyester film of the present invention is preferably 0.2 μm or less, more preferably 0.18 μm or less, and even more preferably 0.16 μm or less. If the arithmetic mean height Sa is higher than 0.2 μm, the film surface may become rough, which may impair transparency or deteriorate printability. The arithmetic mean height Sa of at least one surface of the heat-shrinkable polyester film of the present invention is preferably 0.03 μm or more, more preferably 0.035 μm or more, and even more preferably 0.04 μm or more. If the arithmetic mean height Sa is less than 0.03 μm, the air entrained during winding onto a roll may not be uniformly released, which may result in poor appearance such as wrinkles and pimples on air bubbles, and the winding property may be easily deteriorated.
[0029] The air escape time between the front and back surfaces of the heat-shrinkable polyester film of the present invention is preferably 14 seconds or less, more preferably 13 seconds or less, even more preferably 12 seconds or less, and particularly preferably 10 seconds or less. If the air escape time exceeds 14 seconds, the air wound into the roll will not be uniformly released during the production process and when the film is wound into a roll by rewinding, slitting, etc., which is likely to cause poor appearance such as wrinkles and air bubbles.
[0030] The heat-shrinkable polyester film of the present invention has a haze of 11% or less at a film thickness of 30 μm, more preferably 9% or less, even more preferably 7% or less, and particularly preferably 5% or less. If the haze at a film thickness of 30 μm exceeds 11%, the print appearance deteriorates and it becomes difficult to detect foreign matter during high-speed processing, making it difficult to obtain sufficient quality.
[0031] The thickness of the heat-shrinkable polyester film of the present invention is preferably 15 μm or more and 50 μm or less. If the film thickness is less than 15 μm, the stiffness of the film will be significantly reduced, making the roll prone to wrinkles, which is undesirable. On the other hand, even if the film thickness is thick, there will be no problem as a film roll, but from the viewpoint of cost and environment, it is preferable to make the film thinner. The film thickness is more preferably 17 μm or more and 45 μm, and particularly preferably 20 μm or more and 40 μm.
[0032] The heat-shrinkable polyester film of the present invention can be obtained by melt-extruding the above-mentioned polyester raw material using an extruder to form an unstretched film, and then uniaxially stretching the unstretched film in the transverse direction and heat-treating it using the predetermined method described below. For lamination, multiple extruders, feed blocks, or multi-manifolds can be used. The polyester can be obtained by polycondensing the above-mentioned suitable dicarboxylic acid component and diol component using a known method. Typically, two or more types of chip-like polyester are mixed and used as the raw material for the film. For lamination, multiple extruders can be used.
[0033] When melt-extruding the raw resin, it is preferable to dry the polyester raw material using a dryer such as a hopper dryer or paddle dryer, or a vacuum dryer. After drying the polyester raw material in this manner, it is melted and extruded into a film using an extruder at a temperature of 200 to 300°C. Any existing method, such as a T-die method or a tubular method, can be used for extrusion. An unstretched film can be obtained by quenching the extruded sheet-like molten resin. A suitable method for quenching the molten resin is to cast the molten resin from a die onto a rotating drum and rapidly cool and solidify it to obtain a substantially unoriented resin sheet.
[0034] Furthermore, the obtained unstretched film can be stretched in the width direction under predetermined conditions as described below to obtain the heat-shrinkable polyester film of the present invention. Preferred stretching methods for obtaining the heat-shrinkable polyester film of the present invention are described below. By adopting the preferred stretching method and conditions described below, it is possible to form a film surface state suitable for the present invention.
[0035] Ordinary heat-shrinkable polyester films are produced by stretching an unstretched film in the direction in which shrinkage is desired. Alternatively, there is a biaxial stretching method in which longitudinal stretching is followed by transverse stretching, but biaxial stretching requires large-scale equipment. In the present invention, uniaxial stretching is performed in the width direction, which is the main shrinkage direction. Note that the production method using uniaxial stretching in the width (transverse) direction has the advantage that it can be produced with simple equipment because it does not require longitudinal stretching equipment.
[0036] For width direction stretching, the unstretched film is introduced into a tenter device capable of heating by holding both ends of the film with clips, and the film is heated to a predetermined temperature with hot air. After that, the film is stretched by increasing the distance between the clips while being transported in the longitudinal direction. The preheating temperature of the unstretched film is preferably Tg+10°C or more and +80°C or less. More preferably, it is Tg+20°C or more and +60°C or less. A temperature lower than Tg+10°C is undesirable because the preheating temperature is insufficient, resulting in high stretching force and prone to breakage. Furthermore, heating at a temperature higher than Tg+80°C is undesirable because the stretching force in the width direction of the unstretched sheet is reduced, resulting in poor thickness accuracy (thickness deviation) in the width direction. A more preferable temperature is Tg+30°C or more and +50°C or less.
[0037] The film temperature during width direction stretching is preferably Tg°C or higher and Tg+30°C or lower. If the film temperature is lower than Tg, the stretching force becomes too high, making the film more susceptible to breakage, which is undesirable. If the film temperature exceeds Tg+30°C, the stretching force is too low, resulting in a low width direction heat shrinkage measured at 90°C as described above, which is undesirable. The temperature is more preferably Tg+3°C or higher and +25°C or lower, and even more preferably Tg+5°C or higher and +20°C or lower.
[0038] The stretching ratio in the width direction is preferably 3.5 times or more and 6 times or less. If the stretching ratio is less than 3.5 times, the stretching force will be insufficient, resulting in poor thickness accuracy in the width direction of the film (so-called thickness deviation). Furthermore, if the stretching ratio exceeds 6 times, the risk of breakage during film production will increase and the equipment will become long, which is undesirable. A more preferable range is 3.7 times or more and 5.5 times or less. Furthermore, although not particularly limited, heat treatment may be performed after width direction stretching to adjust the shrinkage rate. The film temperature during heat setting is preferably equal to or higher than the width direction film stretching temperature and equal to or lower than the width direction film stretching temperature + 30°C. If the film heat setting temperature is lower than the width direction film stretching temperature, molecular relaxation in the width direction will be insufficient, resulting in no heat setting effect, which is undesirable. If the film heat setting temperature exceeds the width direction film stretching temperature + 30°C, the film will crystallize, resulting in a low shrinkage rate, which is undesirable. More preferably, it is the film stretching temperature in the width direction +1°C or more and the film stretching temperature in the width direction +25°C or less, and even more preferably, it is the film stretching temperature in the width direction +2°C or more and the film stretching temperature in the width direction +20°C or less.
[0039] The heat-shrinkable polyester film of the present invention can be made into labels by conventionally known methods. For example, a tube film is produced by cutting a heat-shrinkable polyester film to a desired width, applying an appropriate print, and then overlapping and bonding the left and right ends of the film together using solvent bonding or the like. This tube film is then cut to an appropriate length to form a tubular label. Preferred organic solvents for adhesive use are cyclic ethers such as 1,3-dioxolane or tetrahydrofuran. Other examples include aromatic hydrocarbons such as benzene, toluene, xylene, and trimethylbenzene; halogenated hydrocarbons such as methylene chloride and chloroform; phenols such as phenol; and mixtures thereof.
[0040] After perforations are formed in the label by a known method, it is placed on a PET bottle, and the PET bottle is placed on a belt conveyor or the like and passed through a shrink tunnel that blows steam (steam tunnel) or a shrink tunnel that blows hot air (hot air tunnel). The label shrinks thermally as it passes through these tunnels, and the label is attached to the bottle container, such as a PET bottle.
[0041] The packaging of the present invention is formed by covering at least a portion of the outer periphery of an object to be packaged with a label having perforations or notches obtained from the heat-shrinkable polyester film of the present invention and then heat-shrinking the label. Examples of packaging objects include PET beverage bottles, various bottles, cans, plastic containers for confectionery and lunch boxes, and paper boxes. Typically, when covering such packaging objects with a label obtained from the heat-shrinkable polyester film by heat-shrinking, the label is heat-shrunk by approximately 5 to 70% to be tightly attached to the packaging object. The label to be covered on the object to be packaged may or may not be printed.
[0042] Next, the present invention will be specifically explained using examples and comparative examples, but the present invention is not limited to the embodiments of these examples and can be appropriately modified within the scope of the present invention. The film evaluation methods are shown below.
[0043] [Heat shrinkage (hot water heat shrinkage)] The film was cut into a 10 cm x 10 cm square and immersed in 90°C ± 0.5°C hot water for 10 seconds without load to allow it to heat shrink, then immersed in 25°C ± 0.5°C water for 10 seconds, and after removing it from the water, the dimensions of the film in the length (vertical) and width (horizontal) directions were measured, and the heat shrinkage ratio was calculated according to the following formula (1). The direction with the larger heat shrinkage ratio was defined as the main shrinkage direction. Heat shrinkage ratio = {(length before shrinkage - length after shrinkage) / length before shrinkage} × 100 (%) Formula (1)
[0044] [Arithmetic mean height Sa, maximum height Sp] In accordance with ISO 25178, an area of 10 cm in the longitudinal direction x 10 cm in the width direction was cut out from the obtained film, and scanned using a white laser interferometer (NEW VIEW 8300) manufactured by Zygo under the following observation conditions to measure the arithmetic mean height Sa (μm) and the maximum projection height Sp (μm). The measurement was performed on the surface excluding foreign matter such as unmelted material and dust. Measurements were performed at 10 arbitrary points on a 10 cm x 10 cm sample, and the average values were taken as the arithmetic mean height Sa and the maximum projection height Sp, respectively. (Observation conditions) ・Objective lens: 10x ・Zoom lens: 1x ・Field of view: 0.82 x 0.82 mm ・Sampling interval: 0.803 μm ・Estimated measurement time: 4 seconds ・Type: Surface ・Mode: CSI ・Z resolution: High ・Scan length: 20 μm ・Camera mode: 1024 x 1024 @ 100 Hz ・Shutter speed: 100% ・Light intensity: 1.3% ・Options: SureScan Off SmartPsi Averages 4 Noise reduction ・Signal processing options: Fringe order analysis Advanced Fringe removal ON
[0045] [Air Release Time] As shown in Figure 1, film 4 is placed on base plate 1. Next, film holder 2 is placed on top of film 4 and secured in place, applying tension to film 4. Next, film 5 is placed on film holder 2, with the side opposite to the top surface of film 4 placed on base plate 1 facing downward. Next, film holder 8 is placed on top of film 5, and film holders 8, 2, and base plate 1 are secured using screws 3. Next, cavity 2a in film holder 2 is connected to vacuum pump 6 via small holes 2c in film holder 2 and pipe 7. When vacuum pump 6 is driven, film 5 is sucked into cavity 2a, applying tension to film 5. At the same time, the pressure at the overlapping surfaces of film 4 and film 5 is reduced through small holes 2d circumferentially provided in film holder 2, and film 4 and film 5 begin to adhere to each other from the outer periphery of the overlapping surfaces. The adhesion process can be easily observed by observing interference fringes from above the overlapping surfaces. The time (seconds) from when interference fringes appear on the periphery of the overlapping surfaces of films 4 and 5 until the fringes spread to the front of the overlapping surfaces and stop moving is measured, and this time (seconds) is taken as the air release time. The measurement is repeated five times by replacing the two films, and the average value is used.
[0046] [Film Thickness] Measured using a dial gauge in accordance with JIS K7130-1999 Method A.
[0047] [Film Haze] According to JIS K7361-1, the film was cut into a square shape with each side being 10 cm, and the haze was measured using a haze meter NDH2000 manufactured by Nippon Denshoku Co., Ltd. Measurements were performed at three locations, and the average value was taken as the actual haze measurement value, and the haze converted into 30 μm was calculated using the following formula (2): Haze = Actual haze measurement value × 30 / Film thickness (% / 30 μm) Formula (2)
[0048] [Tg (glass transition point)] Tg was determined according to JIS-K7121-1987 using a differential scanning calorimeter (model: DSC220) manufactured by Seiko Instruments Inc. Specifically, 10 mg of unstretched film was heated from -40°C to 120°C at a heating rate of 10°C / min, and an endothermic curve was measured. Tangent lines were drawn before and after the inflection point of the obtained endothermic curve, and the intersection point was defined as the glass transition point (Tg; °C).
[0049] [Intrinsic viscosity (IV)] 0.2 g of polyester was dissolved in 50 ml of a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (60 / 40 (weight ratio)), and the intrinsic viscosity was measured using an Ostwald viscometer at 30° C. The unit is dl / g.
[0050] [Composition Analysis] Each sample was dissolved in a solvent prepared by mixing chloroform D (manufactured by Eurisop) and trifluoroacetic acid D1 (manufactured by Eurisop) in a 10:1 (volume ratio) mixture to prepare a sample solution. NMR of the protons in the sample solution was measured using an NMR "GEMINI-200" (manufactured by Varian) at a temperature of 23°C and an accumulation number of 64. In the NMR measurement, the peak intensity of a predetermined proton was calculated, and the amount of the component in 100 mol% of the diacid component and the amount of the component in 100 mol% of the polyhydric alcohol component were measured.
[0051] [Shrinkage Finish] The edges of the heat-shrinkable film were welded using an impulse sealer (manufactured by Fuji Impulse Co., Ltd.) to obtain a cylindrical label with the width direction as the circumferential direction. 0.5 mm holes were also made in the longitudinal direction of the film at 3 mm intervals. Similarly, 0.5 mm holes were made in the longitudinal direction of the film at 10 mm intervals (so-called perforations for easy label peeling) at 3 mm intervals (so-called perforations for easy label peeling). The diameter of the label in the shrinkage direction was 68 mm. This label was placed on a commercially available 500 ml PET bottle (filled; body diameter 62 mm, minimum neck diameter 25 mm) and heat-shrunk by passing it through steam using a Fuji Astec Inc. steam tunnel (model: SH-1500-L) adjusted to 90°C (tunnel passage time: 5 seconds). The shrinkage finish of the label was visually evaluated according to the following criteria. A 5-point scale was used for visual evaluation according to the following criteria. The defects described below include jumping up, wrinkles, insufficient shrinkage, folded label edges, whitening due to shrinkage, etc. A rating of 3 or higher was considered acceptable. 5: Best finish (no defects) 4: Good finish (one defect) 3: Two defects 2: 3 to 5 defects 1: Many defects (6 or more)
[0052] [Evaluation of Wrinkles in Film Rolls] The produced heat-shrinkable polyester film was wound up to a width of 500 mm and a roll length of 1000 m, and the wrinkles on the surface of the roll were visually evaluated according to the following criteria. Evaluations of ○ and △ were judged to be pass. ○: No wrinkles △: Weak wrinkles were present, but the wrinkles disappeared when a tension of about 20 N / m was applied to the drawn-out film ×: Strong wrinkles were present, and the wrinkles did not disappear even when a tension of about 20 N / m was applied to the drawn-out film
[0053] [Evaluation of Printability] A film roll having a width of 500 mm and a roll length of 1000 m was printed (one-color printing) using grass green ink manufactured by Toyo Ink Mfg. Co., Ltd. The ink thickness after printing was 1 μm. The area of the film after printing was 900 mm per measurement. 2The print was inspected for missing dots using a magnifying glass at a magnification of 5x (30 mm in the longitudinal direction and 30 mm in the width direction). Measurements were taken at three arbitrary points in the width direction of the roll after printing. In addition, measurements were taken at three points in the width direction (total of six points) at a position 50 m away in the longitudinal direction from the position where the measurement was taken in the width direction, and an area of 900 mm was measured. 2 The sample was measured (30 mm in the longitudinal direction and 30 mm in the width direction) using a magnifying glass at a magnification of 5 times, and judged as ◯ or △ to be acceptable. ◯: Missing dots less than 1% △: Missing dots 1% to less than 3% ×: Missing dots 3% or more
[0054] [Preparation of polyester raw material] A stainless steel autoclave equipped with a stirrer, thermometer, and partial reflux condenser was charged with 100 mol% dimethyl terephthalate (DMT) as a dibasic acid component and 100 mol% ethylene glycol (EG) as a glycol component, with the glycol being 2.2 times the methyl ester in molar ratio. Using 0.05 mol% (relative to the acid component) of zinc acetate as a transesterification catalyst, a transesterification reaction was carried out while distilling off the resulting methanol. Subsequently, 0.025 mol% (relative to the acid component) of antimony trioxide was added as a polycondensation catalyst, and a polycondensation reaction was carried out at 280°C under reduced pressure of 26.6 Pa (0.2 Torr), yielding a polyester (A) with an intrinsic viscosity of 0.75 dl / g. This polyester was polyethylene terephthalate.
[0055] During the manufacturing process, SiO 2 Polyesters B1 to B8 were prepared by adding 8,000 ppm of SiO to the polyester, and had an intrinsic viscosity of 0.75 dl / g. 2 Polyester B1 had a spherical shape and a weight average particle size of 1 μm, Polyester B2 had an irregular shape and a weight average particle size of 1.5 μm, Polyester B3 had an irregular shape and a weight average particle size of 2 μm, Polyester B4 had an irregular shape and a weight average particle size of 2.5 μm, Polyester B5 had an irregular shape and a weight average particle size of 3 μm, Polyester B6 had an irregular shape and a weight average particle size of 4 μm, Polyester B7 had an irregular shape and a weight average particle size of 5 μm, and Polyester B8 had an irregular shape and a weight average particle size of 6 μm.
[0056] Furthermore, polyesters (C, D, E) shown in Table 1 were synthesized by a method similar to that described above. In the table, NPG stands for neopentyl glycol, CHDM stands for 1,4-cyclohexanedimethanol, and BD stands for 1,4-butanediol. The intrinsic viscosities of polyesters C, D, and E were 0.75 dl / g, 0.75 dl / g, and 1.15 dl / g, respectively. Each polyester was appropriately formed into chips.
[0057] The contents of the raw material chips used in the Examples and Comparative Examples, the resin compositions of the films in the Examples and Comparative Examples, and the layer structures and production conditions are shown in Tables 1 and 2, respectively.
[0058]
[0059]
[0060] Example 1 Using a coextrusion method, the resin for forming the core layer and the resin for forming the skin layer were melt-extruded from separate extruders (first and second extruders), laminated in a die (T-die), and quenched by wrapping around a rotating metal roll cooled to a surface temperature of 30°C. This resulted in a 138 μm thick unstretched film with a two-type, three-layer structure, i.e., a core layer with a skin layer laminated on the outside. For the core layer, the above-mentioned polyester A, polyester C, and polyester E were mixed in a weight ratio of 20:70:10 and fed into the extruder. This mixed resin was melted at 260°C. For the skin layer, the above-mentioned polyester A, polyester B3, polyester C, and polyester E were mixed in a weight ratio of 12:8:70:10 and fed into the extruder. This mixed resin was melted at 260°C. The thickness ratio of skin layer / core layer / skin layer was 1:2:1. The take-up speed of the unstretched film (the rotation speed of the metal roll) was approximately 30 m / min. The Tg of the unstretched film was 69°C. The resulting unstretched film was introduced into a tenter (transverse stretching machine). The temperature in the preheating step was 95°C (Tg + 26°C) and the temperature in the stretching step was 78°C (Tg + 9°C), and the film was stretched 4.6 times. The transversely stretched film was heat-treated under tension at 83°C (stretching temperature + 5°C) for 8 seconds. The film was then cooled, both edges were trimmed and removed, and the film was wound into a roll with a width of 800 mm, continuously producing a 30 μm-thick stretched film over a length of 2000 m. The properties of the resulting film were evaluated using the methods described above. The evaluation results are shown in Table 3. The film exhibited good wrinkle and shrinkage finish in the film roll.
[0061] Example 2 A film having a thickness of 30 μm was prepared in the same manner as in Example 1, except that Polyester B3 was changed to Polyester B4. The evaluation results are shown in Table 3. The air release time was shorter than in Example 1, and the film had good wrinkle and shrinkage finish in the film roll.
[0062] Example 3 A film having a thickness of 30 μm was prepared in the same manner as in Example 1, except that Polyester B3 was changed to Polyester B5. The evaluation results are shown in Table 3. The air release time was shorter than in Example 1, and the film had good wrinkle and shrinkage finish in the film roll.
[0063] Example 4 A film having a thickness of 30 μm was prepared in the same manner as in Example 1, except that Polyester B3 was changed to Polyester B6. The evaluation results are shown in Table 3. The air release time was shorter than in Example 1, and the haze was slightly higher, but the film had good wrinkle and shrinkage finish properties in the film roll.
[0064] Example 5 A film having a thickness of 30 μm was prepared in the same manner as in Example 1, except that Polyester B3 was changed to Polyester B7. The evaluation results are shown in Table 3. The air release time was shorter than in Example 1, and the haze was slightly higher, but the film had good wrinkle and shrinkage finish properties in the film roll.
[0065] Example 6 A film having a thickness of 30 μm was prepared in the same manner as in Example 1, except that the raw material for the core layer in Example 1 was changed to the same raw material as for the skin layer and the layer structure was changed to one type, three layers. The evaluation results are shown in Table 3. The haze was slightly higher, but the film had good wrinkle and shrinkage finish in the film roll.
[0066] Example 7: Using a coextrusion method, the resin for forming the core layer, the resin for forming the skin layer, and the resin for forming the adhesive layer were melt-extruded from separate extruders (first to third extruders), laminated in a die (T-die), and quenched by winding around a rotating metal roll cooled to 30°C using an air knife method to obtain a 138 μm thick unstretched film (polystyrene-based resin laminate sheet) with a three-layer, five-layer structure, i.e., intermediate layers (adhesive layers) laminated on both sides of the core layer, and skin layers laminated on the outer sides of each of the intermediate layers. The method for forming each layer of the unstretched film (processes up to melt extrusion) is as follows. In the following description, the layers are referred to as the first layer, second layer, third layer, fourth layer, and fifth layer from the front to the back of the polystyrene-based mixed resin laminate sheet (i.e., the surface of the fifth layer is the surface that contacts the metal roll). The take-up speed of the unstretched film (rotational speed of the metal roll) was approximately 30 m / min. Formation of the First and Fifth Layers (Skin Layers): Dried polyester A, polyester B4, polyester C, and polyester E were mixed in a ratio of 12:8:70:10 and fed into a first extruder. This mixed resin was melt-extruded at 260°C (so as to be laminated on the outer surface of the intermediate layer, which was laminated on the outer surface of the core layer). To stabilize extrusion from the T-die, a helical-type and parallel-type gear pump was interposed between the extruder and the T-die. Formation of the Second and Fourth Layers (Adhesive Layers): The above-mentioned chips F were pre-dried using a blender, and then the pre-dried chips F were continuously fed into a hopper directly above the second extruder using a constant-rate screw feeder. The fed chips D were then melt-extruded through the T-die of the second extruder (so as to be laminated on the outer surface of the core layer). The temperature of the second extruder was adjusted to 200°C. As with the extrusion using the first extruder, a helical and parallel gear pump was interposed between the extruder and the T-die to stabilize the extrusion from the T-die. Formation of the third layer (core layer): The chips G, H, and I were each pre-dried using a blender, and then charged into the third extruder at a mixing ratio of 43:43:14. The mixed resin was melt-extruded at 200°C.As with the extrusion using the first and second extruders, a helical-type, parallel-type gear pump was interposed between the extruder and the T-die to stabilize extrusion from the T-die. In extruding the resin using each of the extruders, the discharge rates of the first to third extruders in forming the unstretched film were adjusted so that the thicknesses of the first layer, second layer, third layer, fourth layer, and fifth layer were 23 / 3 / 48 / 3 / 23. A 30 μm-thick film was produced from the obtained unstretched film in the same manner as in Example 1, except that the width direction stretching temperature was changed to 82°C. The evaluation results are shown in Table 3. The film exhibited good wrinkle and shrinkage finish in the film roll.
[0067] Example 8 A film having a thickness of 30 μm was prepared in the same manner as in Example 1, except that Polyester C was changed to Polyester D. The Tg of the unstretched film was 69° C. The evaluation results are shown in Table 3. The film had good wrinkle and shrink finish properties in the film roll.
[0068] Example 9: Polyester B3 was changed to Polyester B1, and the raw materials for the skin layer were Polyester A, Polyester B1, Polyester C, and Polyester E in a weight ratio of 4 / 16 / 70 / 10. A 30 μm thick film was prepared in the same manner as in Example 1, except that in the process of stretching the unstretched film in the width direction, the preheating temperature was changed to 100° C., the stretching temperature was changed to 85° C., and the heat treatment temperature was changed to 86° C. The evaluation results are shown in Table 3. The film had good wrinkle and shrinkage finish in the film roll.
[0069] Comparative Example 1 A film having a thickness of 30 μm was prepared in the same manner as in Example 1, except that Polyester B3 was changed to Polyester B1. The evaluation results are shown in Table 3. The air release time was longer than in Example 1, and the film had noticeable wrinkles in the film roll.
[0070] Comparative Example 2 A film having a thickness of 30 μm was prepared in the same manner as in Example 1, except that Polyester B3 was changed to Polyester B2. The evaluation results are shown in Table 3. The air release time was longer than in Example 1, and the film had noticeable wrinkles in the film roll.
[0071] Comparative Example 3 A film having a thickness of 30 μm was prepared in the same manner as in Example 1, except that Polyester B3 was changed to Polyester B8. The evaluation results are shown in Table 3. The air release time was short and wrinkle resistance was good, but the maximum protrusion height Sp of the film surface and the arithmetic mean height of the film surface were high, resulting in missing dots during printing, and the film had poor printability.
[0072] Comparative Example 4 A film having a thickness of 30 μm was prepared in the same manner as in Example 9, except that in the process of stretching an unstretched film in the width direction, the temperature in the preheating step was changed to 95° C., the width direction stretching temperature was changed to 83° C., and the heat treatment temperature was changed to 88° C. The evaluation results are shown in Table 3. The air removal time was longer than in Example 1, and the film had noticeable wrinkles in the film roll.
[0073] Comparative Example 5 A film having a thickness of 30 μm was prepared in the same manner as in Example 1, except that in the process of stretching the unstretched film in the width direction, the preheating and stretching steps were changed to 76°C (Tg + 7°C) and the heat treatment temperature was changed to 88°C. The evaluation results are shown in Table 3. The air release time was longer than in Example 1, and the film had noticeable wrinkles in the film roll. This is thought to be due to the increased stretching stress during film stretching, which made the lubricant more susceptible to crushing.
[0074]
[0075] The heat-shrinkable polyester film of the present invention has a high heat shrinkage rate, is excellent in transparency and printability, and has a short air release time, so that a film roll with a good appearance can be obtained.
[0076] 1. Base 2, 8. Film holder 2a. Slot 3. Screw 4, 5. Film 6. Vacuum pump 7. Pipe X. Film overlap
Claims
1. A heat-shrinkable polyester film characterized by satisfying the following requirements (1) to (6): (1) When the film is immersed in 90°C hot water for 10 seconds, the hot water heat shrinkage rate is 40% or more and 80% or less in the width direction of the film. (2) When the film is immersed in 90°C hot water for 10 seconds, the hot water heat shrinkage rate is -5% or more and 10% or less in the longitudinal direction of the film. (3) The maximum projection height (Sp) of at least one of the film surfaces is 0.8 μm or more and 3.0 μm or less. (4) The arithmetic mean height Sa of at least one of the film surfaces is 0.03 μm or more and 0.2 μm or less. (5) The time required for air to escape between the front and back surfaces of the film is 12 seconds or less. (6) The thickness of the film is 30 μm or more and 50 μm or less.
2. 2. The heat-shrinkable polyester film according to claim 1, wherein the haze at a film thickness of 30 μm is 2% or more and 11% or less.
3. A heat-shrinkable polyester film as described in claim 1 or 2, characterized in that it is a laminated heat-shrinkable polyester film having at least two or more polyester film layers laminated together.
4. A heat-shrinkable label using the heat-shrinkable polyester film according to any one of claims 1 to 3.