Power storage device, and method for manufacturing power storage device
Patent Information
- Application Number
- JP2023575306
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Priority Date
- 2023-01-20
- Filing Date
- 2023-01-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Current power storage devices, such as capacitors and all-solid-state batteries, have limitations in achieving high capacity density due to insufficient interface area between electrodes and solid electrolyte layers.
The introduction of a composite layer containing a carbon material and a second solid electrolyte at specific boundaries between electrodes and solid electrolyte layers, along with a manufacturing method involving a laminate forming step and firing process to create a solid electrolyte layer and composite layer, increases the interface area and enhances lithium ion conductivity.
This configuration significantly increases the capacity density of the electricity storage device by expanding the interface area between electrodes and solid electrolyte layers, leading to improved power storage capabilities.
Abstract
Description
Electricity storage device and method for manufacturing the same
[0001] The present disclosure relates to an electricity storage device and a method for manufacturing an electricity storage device.
[0002] Capacitors and all-solid-state batteries using solid electrolytes have been disclosed. Patent Document 1 (JP 2008-130844 A) discloses "an all-solid-state electric double layer capacitor comprising a solid electrolyte and a current collector, wherein the solid electrolyte is an inorganic solid electrolyte."
[0003] Patent Document 2 (JP 2017-147397 A) discloses "a capacitor including a substrate having a solid electrolyte layer containing a solid electrolyte having lithium ion conductivity, and a first electrode and a second electrode arranged to face each other via the solid electrolyte layer, wherein the first electrode is a first metal layer arranged on one main surface in the thickness direction of the solid electrolyte layer so as to be in contact with the one main surface, and the second electrode is made of a composite material containing the solid electrolyte and a metal including nickel, and has a composite layer arranged on the other main surface in the thickness direction of the solid electrolyte layer so as to be in contact with the other main surface, and a second metal layer arranged to cover the composite layer."
[0004] Patent Document 3 (JP 2019-087346 A) discloses "an all-solid-state battery comprising: a solid electrolyte layer made of an oxide-based solid electrolyte; a first electrode layer formed on one surface of the solid electrolyte layer and containing ceramic particles; and a second electrode layer formed on the other surface of the solid electrolyte layer and containing ceramic particles, wherein at least one of the first electrode layer and the second electrode layer contains particulate carbon and plate-like carbon."
[0005] JP 2008-130844 A JP 2017-147397 A JP 2019-087346 A
[0006] Currently, there is a demand for further improvement in the capacity density of power storage devices. One of the objects of the present disclosure is to provide a power storage device with high capacity density.
[0007] One aspect of the present disclosure relates to an electric storage device including at least one layered first electrode, at least one layered second electrode, and at least one solid electrolyte layer disposed between the first electrode and the second electrode and including a first solid electrolyte, and further including a composite layer including a carbon material and a second solid electrolyte at at least one boundary selected from the group consisting of a first boundary between the first electrode and the solid electrolyte layer and a second boundary between the second electrode and the solid electrolyte layer.
[0008] One aspect of the present disclosure relates to a method for manufacturing an electricity storage device including a solid electrolyte layer and a composite layer adjacent to the solid electrolyte layer, the method including: a stack-forming step of forming a first stack including a first mixture layer and a second mixture layer stacked on the first mixture layer; and a firing step of firing the first stack to form a second stack including the solid electrolyte layer and the composite layer, wherein the solid electrolyte layer includes the first solid electrolyte, the composite layer includes a carbon material and a second solid electrolyte, the first mixture layer includes a material that will become the solid electrolyte layer by the firing step, and the second mixture layer includes a material that will become the composite layer by the firing step.
[0009] According to the present disclosure, an electricity storage device with high capacity density can be obtained. The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.
[0010] It is a cross-sectional view showing the structure of the electricity storage device of Embodiment 1. It is a cross-sectional view showing the structure of the laminate produced in the example.
[0011] Below, embodiments of the electricity storage device according to the present disclosure will be described using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values and materials may be exemplified, but other numerical values and materials may be applied as long as the effects of the present disclosure are obtained. In this specification, the expression "numerical value A to numerical value B" includes numerical value A and numerical value B and can be read as "numerical value A or more and numerical value B or less." In the following description, when lower and upper limits of numerical values related to specific physical properties or conditions are exemplified, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit. In the following description, the expression "including A" can include "a form substantially consisting of A" and "a form consisting of A."
[0012] (Electricity Storage Device) The electricity storage device according to this embodiment may be referred to as "electricity storage device (D)" below. The electricity storage device (D) includes at least one layered first electrode, at least one layered second electrode, and at least one solid electrolyte layer disposed between the first electrode and the second electrode and including a first solid electrolyte. The electricity storage device (D) further includes a composite layer including a carbon material and a second solid electrolyte at at least one boundary selected from the group consisting of a first boundary between the first electrode and the solid electrolyte layer and a second boundary between the second electrode and the solid electrolyte layer.
[0013] In the electricity storage device (D), during charging, lithium ions (Li + ) migrate, forming an electric double layer between the negative electrode and the solid electrolyte layer. That is, it is thought that lithium ions gather near the interface of the solid electrolyte layer facing the negative electrode, and electrons gather near the interface of the negative electrode facing the solid electrolyte. On the other hand, during charging, it is thought that an electric double layer is formed at the interface between the positive electrode and the solid electrolyte of the electricity storage device (D) by vacancies (negatively charged) from which lithium ions have been removed and vacancies (positive holes) in the positive electrode. As a result, power is stored in the electricity storage device (D). From one perspective, the electricity storage device (D) is a capacitor.
[0014] The all-solid-state battery described in Patent Document 3 is a battery including a positive electrode active material and a negative electrode active material. In contrast, the electricity storage device (D) is not a battery including a positive electrode active material and a negative electrode active material.
[0015] In order to increase the capacity density of an electricity storage device, it is important to increase the area of the interface between the electrode and the solid electrolyte layer. In the electricity storage device (D), a composite layer is disposed on at least a part of the interface between the electrode and the solid electrolyte layer. This increases the area of the interface between the electrode and the solid electrolyte layer, thereby increasing the capacity density (e.g., volumetric capacity density).
[0016] Either the first electrode or the second electrode can be used as a positive electrode, and the other can be used as a negative electrode. That is, the electricity storage device (D) can be used as an electricity storage device including a positive electrode and a negative electrode. The composite layer is disposed at at least one boundary selected from the group consisting of the boundary between the positive electrode and the solid electrolyte and the boundary between the negative electrode and the solid electrolyte. The composite layer may be disposed only at the boundary between the positive electrode and the solid electrolyte layer, or only at the boundary between the negative electrode and the solid electrolyte layer, or may be disposed at both of these two boundaries.
[0017] The electricity storage device (D) may satisfy the following conditions (1) and / or (2). By satisfying both conditions (1) and (2), it is possible to particularly increase the capacity density. (1) The first electrode is a positive electrode, and the composite layer is disposed only at the first boundary. (2) The first solid electrolyte is a lithium ion conductor, and the first solid electrolyte has a NASICON-type crystal structure and contains Li, Al, Ti, P, and O.
[0018] A solid electrolyte (lithium ion conductor) having a NASICON-type crystal structure and containing Li, Al, Ti, P, and O can be, for example, a solid electrolyte represented by the formula Li 1+X Al X Ti 2-X (P.O. 4 ) 3 (wherein X is, for example, in the range of 0.3 to 0.4), and Li 1.3 Al 0.3 Ti 1.7 (P.O. 4 )3 The solid electrolyte (compound) represented by these formulas may be referred to as "LATP" below.
[0019] The specific surface area of the carbon material is 30m 2 / g or more. 2 By using a carbon material with a specific surface area of 10 m / g or more, the contact area between the electrode and the solid electrolyte layer can be increased, resulting in an increased capacity density. 2 Although there is no particular upper limit to the specific surface area of the carbon material, the specific surface area may be 2000 m 2 / g or less (for example, 1500m 2 / g or less). Carbon materials having a variety of specific surface areas are commercially available, so a commercially available carbon material that satisfies the above conditions may be used, or a carbon material may be produced according to a known method. The specific surface area can be measured by the BET method.
[0020] The first solid electrolyte and the second solid electrolyte may have different crystal structures. Alternatively, the first solid electrolyte and the second solid electrolyte may have the same crystal structure. For example, when the first solid electrolyte has a NASICON-type crystal structure (e.g., in the case of the above condition (2)), the second solid electrolyte may also have a NASICON-type crystal structure. For example, the second solid electrolyte may be a lithium ion conductor and have a NASICON-type crystal structure. In that case, the second solid electrolyte may contain Li, Al, Ti, P, and O.
[0021] The first solid electrolyte and the second solid electrolyte may be solid electrolytes made of the same raw material. By using the first and second solid electrolytes as solid electrolytes made of the same material (e.g., the same solid electrolyte), it becomes easier to form the electrolyte of the solid electrolyte layer and the solid electrolyte of the composite layer as an integrated unit. As a result, lithium ion conductivity between the solid electrolyte layer and the composite layer can be improved. The first solid electrolyte and the second solid electrolyte may be different solid electrolytes or the same solid electrolyte.
[0022] The electricity storage device (D) may include a plurality of first electrodes, a plurality of second electrodes, or a plurality of solid electrolyte layers. For example, the electricity storage device (D) may include a plurality of first electrodes, a plurality of second electrodes, and a plurality of solid electrolyte layers. When the electricity storage device (D) includes a plurality of first electrodes and a plurality of second electrodes, the first electrodes and the second electrodes are usually arranged alternately. The solid electrolyte layer is then arranged between the first electrodes and the second electrodes.
[0023] The number of first electrodes and the number of second electrodes are not particularly limited and may be in the range of 1 to 1000 (for example, in the range of 2 to 100). The number of solid electrolyte layers disposed between the first electrodes and the second electrodes varies depending on the number of first and second electrodes and the structure of the electricity storage device (D).
[0024] The first electrode and the second electrode may be disposed only on the outside of the stack including the solid electrolyte layer and the composite layer, or the first electrode and the second electrode may be internal electrodes disposed inside the stack including the solid electrolyte layer and the composite layer.
[0025] The thickness of the solid electrolyte layer between the first electrode and the second electrode is not particularly limited and may be in the range of 1 to 30 μm (e.g., 1 to 10 μm). The thickness of the composite layer is not particularly limited and may be in the range of 1 to 30 μm (e.g., 1 to 10 μm). When the first electrode and the second electrode are internal electrodes embedded in the solid electrolyte layer, the thickness of one internal electrode may be in the range of 1 to 10 μm (e.g., 1 to 5 μm).
[0026] Examples of the configuration and components of the electricity storage device (D) are described below. The configuration and components of the electricity storage device (D) are not limited to the following examples.
[0027] The electricity storage device (D) includes a first electrode, a second electrode, a solid electrolyte layer, and a composite layer. If necessary, the electricity storage device (D) may include other components, such as a current collector and an exterior body. Typically, the first electrode, the second electrode, the solid electrolyte layer, and the composite layer are each layered. They are stacked to form a laminate.
[0028] (Electrodes) The first and second electrodes are each electrically conductive. The first and second electrodes can be made of a material containing a metal. Examples of metals include Pd, Pt, Ag, Cu, Ni, Au, and other metals, and may also be alloys.
[0029] The electrodes may be formed by vapor deposition or the like. Alternatively, the electrodes may be formed by applying a paste containing metal particles and then heating (e.g., baking) the paste. The paste containing metal particles may be a commercially available metal paste (e.g., silver paste).
[0030] The first electrode and the second electrode may be formed of the same material, or the first electrode and the second electrode may be formed of different materials.
[0031] (Solid Electrolyte) Examples of the solid electrolyte (first and second solid electrolytes) include solid electrolytes having lithium ion conductivity. The solid electrolyte is an inorganic solid electrolyte. The solid electrolyte may have a NASICON-type crystal structure and contain Li, Al, Ti, P, and O. Examples of such solid electrolytes include the above-mentioned LATP.
[0032] (Composite Layer) The composite layer includes a solid electrolyte and a carbon material. The solid electrolyte may be any of the above-described solid electrolytes. The carbon material may be a conductive carbon material. Examples of the carbon material include graphite (natural graphite, artificial graphite, etc.), carbon black (acetylene black, ketjen black, etc.), carbon fiber, carbon nanotube, graphene, etc.
[0033] From one perspective, the carbon material of the composite layer can be considered to function as a part of the electrode, and the solid electrolyte of the composite layer can be considered to function as a part of the solid electrolyte layer, and therefore, it can be considered that the use of the composite layer can increase the area of the interface between the electrode and the solid electrolyte layer.
[0034] The composite layer may or may not contain components other than the solid electrolyte and the carbon material. The carbon material may have a larger specific surface area than the metal fine particles. Therefore, a preferred example of the composite layer does not contain metal fine particles such as nickel.
[0035] In the composite layer, the solid electrolyte content Rs may be in the range of 50 to 98 mass %, and the carbon material content Rc may be in the range of 2 to 50 mass %, 80 to 98 mass % (e.g., 90 to 95 mass %), and the carbon material content Rc may be in the range of 2 to 20 mass % (e.g., 5 to 10 mass %).
[0036] When the electricity storage device (D) includes an exterior body, the exterior body is not limited, and the same exterior body as that used in electrolytic capacitors or batteries may be used. When the electricity storage device (D) includes a current collector, the current collector is not limited, and the same current collector as that used in electrolytic capacitors or batteries may be used.
[0037] (Method for manufacturing an electricity storage device) A manufacturing method according to this embodiment will be described below. This manufacturing method will be referred to as "manufacturing method (M)" below. The manufacturing method (M) is a method for manufacturing an electricity storage device. According to the manufacturing method (M), an electricity storage device (D) can be manufactured. Since the matters described for the electricity storage device (D) can be applied to the manufacturing method (M), duplicated explanations may be omitted. Furthermore, the matters described for the manufacturing method (M) may also be applied to the electricity storage device (D). The electricity storage device (D) may also be manufactured by a method other than the manufacturing method (M).
[0038] The manufacturing method (M) is a method for manufacturing an electricity storage device including a solid electrolyte layer and a composite layer adjacent to the solid electrolyte layer. The manufacturing method (M) includes a laminate formation step and a firing step, in this order. These steps are described below.
[0039] (Laminate Forming Step) The laminate forming step is a step of forming a first laminate including a first mixture layer and a second mixture layer laminated on the first mixture layer. The solid electrolyte layer is the solid electrolyte layer described in the electricity storage device (D) and includes a first solid electrolyte. The composite layer is the composite layer described in the electricity storage device (D) and includes a carbon material and a second solid electrolyte. The first mixture layer includes a material that will become a solid electrolyte layer by a firing step. The second mixture layer includes a material that will become a composite layer by a firing step.
[0040] The material for the solid electrolyte layer is a material that becomes a solid electrolyte by firing and contains elements that constitute the solid electrolyte. For example, when forming a solid electrolyte having a NASICON-type crystal structure and containing Li, Al, Ti, P, and O, the material may be, for example, a lithium compound (Li 2 CO 3 etc.), phosphorus compounds (AlPO 4 and H 3 P.O. 4 etc.), aluminum compounds (AlPO 4 , Al 2 O 3 etc.), Ti compounds (TiO 2 A mixture of a carbon material and a material that becomes a solid electrolyte when fired can be used. The material that becomes a solid electrolyte when fired can be used as a powder of the solid electrolyte. A commercially available powder can be used as the powder of the solid electrolyte.
[0041] The method for forming the first mixture layer and the second mixture layer is not particularly limited, and they may be formed by a known method, for example, a method similar to that used in the manufacture of multilayer ceramic capacitors (MLCCs).
[0042] The first layer may be formed by the following procedure. First, solid electrolyte material (e.g., powder) and a liquid medium are mixed. The solid electrolyte material is mixed in a predetermined ratio so that the desired solid electrolyte is formed when fired. Mixing (e.g., pulverization and mixing) can be performed by a known method such as a ball mill. A liquid medium and additives are added to the mixed powder obtained in this manner and kneaded to obtain a slurry. Examples of additives include binders and plasticizers. These liquid mediums and additives can be the same as those used in manufacturing electrolytic capacitors and batteries. Examples of liquid mediums include butyl acetate, etc. Examples of binders include butyral resin, etc.
[0043] Next, the obtained slurry is used to form a first mixture layer. Specifically, the first mixture layer can be formed by applying the slurry in a layer form, and then drying and / or rolling it as necessary. The second mixture layer can also be formed in the same manner as the first mixture layer. The first mixture layer and the second mixture layer are laminated to obtain a first laminate.
[0044] The first laminate may be a laminate obtained by dividing the laminate formed by the above procedure.
[0045] (Firing step) The firing step is a step of forming a second laminate including a solid electrolyte layer and a composite layer by firing the first laminate, and the second laminate (fired body) in which the solid electrolyte layer and the composite layer are stacked is obtained by the firing step.
[0046] The firing conditions for the firing step are not particularly limited, as long as they allow the second laminate (fired body) to be obtained. The firing conditions may be selected according to the type of solid electrolyte. An example of the firing step is performed by heating at a temperature in the range of 500 to 1000°C for 2 to 10 hours. The firing step is preferably performed in an inert atmosphere (e.g., a nitrogen atmosphere). A step of volatilizing the binder may be performed before the firing step. For example, the first laminate may be heated in the air at a high temperature (e.g., about 400°C) for about 2 to 5 hours.
[0047] In this manner, a second laminate is obtained. Thereafter, electrodes and / or current collectors are formed as necessary to obtain an energy storage element. The obtained energy storage element is housed in an exterior body as necessary. In this manner, an energy storage device is obtained.
[0048] The first laminate may include a plurality of first mixture layers, a plurality of second mixture layers, a plurality of layered first electrode material layers, and a plurality of layered second electrode material layers. That is, the laminate formation step may be a step of forming such a first laminate. In this case, the second mixture layer is disposed at at least one boundary selected from the group consisting of the boundary between the first mixture layer and the first electrode material layer and the boundary between the first mixture layer and the second electrode material layer. The first electrode material layer and the second electrode material layer are respectively formed into a first internal electrode (first electrode) and a second internal electrode (second electrode) by a firing step. According to this configuration, a second laminate including a plurality of first electrodes and a plurality of second electrodes is obtained. In this case, the manufacturing method (M) may further include a step of forming a first current collector connected to the first internal electrode and a second current collector connected to the second internal electrode.
[0049] The process for forming the current collectors (first and second current collectors) is not particularly limited, and any known method may be used. For example, the current collectors may be formed using a metal paste, or may be formed by a method such as vapor deposition. A plating layer may be formed on the formed current collectors.
[0050] The electrode material layers (first electrode material layer and second electrode material layer) may be formed of a material that becomes an electrode upon firing. Examples of such a material include the above-mentioned paste containing metal particles.
[0051] Below, examples of the electricity storage device (D) will be specifically described with reference to the drawings. The components described above can be applied to the components of the electricity storage device in the example described below. Furthermore, the electricity storage device in the example described below can be modified based on the above description. Furthermore, the matters described below may be applied to the above embodiment. Furthermore, in the embodiment described below, components that are not essential for the electricity storage device (D) may be omitted.
[0052] (Embodiment 1) A cross-sectional view of an electricity storage device 100 of Embodiment 1 is shown schematically in Figure 1. The electricity storage device 100 includes a laminate (second laminate) 110. The laminate 110 includes a plurality of first electrodes (first internal electrodes) 111, a plurality of second electrodes (second internal electrodes) 112, a composite layer 113, and a solid electrolyte layer 115. The electricity storage device 100 further includes a first current collector 121 and a second current collector 122. In the electricity storage device 100, the first electrode 111 is a positive electrode, and the second electrode 112 is a negative electrode.
[0053] The first electrodes 111 and the second electrodes 112 are arranged alternately. A solid electrolyte layer 115 is arranged between the first electrodes 111 and the second electrodes 112. One ends of the plurality of first electrodes 111 are connected to a first current collector (positive electrode current collector) 121. One ends of the plurality of second electrodes 112 are connected to a second current collector (negative electrode current collector) 122.
[0054] The composite layer 113 is disposed at the boundary between the first electrode 111 (positive electrode) and the solid electrolyte layer 115. The composite layer 113 is formed on the main surface of the first electrode 111 that faces the solid electrolyte layer 115. In the example shown in FIG. 1 , the composite layer 113 is formed on both surfaces of the first electrode 111.
[0055] A description will be given of an example of a manufacturing method (M) for manufacturing the electricity storage device 100. In the following, an example will be described in which LATP is used as the solid electrolyte, but other solid electrolytes may also be used.
[0056] (1) Formation of the First Mixture Layer First, predetermined amounts of raw materials are weighed and mixed. For example, when the lithium ion conductor to be prepared is LATP, Li 2 CO 3 Li compounds such as AlPO 4 and H 3 P.O. 4 P compounds such as AlPO 4 , Al 2 O 3 An Al compound such as TiO or the like is prepared. Then, predetermined amounts of these raw materials are weighed and wet-mixed using a ball mill to obtain a mixture.
[0057] Next, the resulting mixture is dehydrated and dried, and the dried powder is heat-treated to obtain a calcined powder of LATP. Next, the resulting calcined powder is placed in a grinder (e.g., a ball mill) together with a liquid medium such as an organic solvent and wet-ground. The resulting powder is dried to obtain a pulverized powder of LATP. As mentioned above, commercially available solid electrolyte powders may also be used.
[0058] Next, an organic binder such as butyral resin, a liquid medium mainly consisting of butyl acetate, and a plasticizer are added to the obtained powder and mixed and dispersed in a wet process to obtain a slurry. The obtained slurry is applied to a film (e.g., a PET film) by a doctor blade method and formed into a layer to obtain an LATP green sheet (first green sheet). The first green sheet corresponds to the first mixture layer.
[0059] (2) Formation of Electrode Layer and Composite Layer A paste that will become the composite layer is printed in a predetermined pattern on the LATP green sheet by screen printing. The paste contains the pulverized LATP powder and a powder of a carbon material. In this way, a second mixture layer that will become the composite layer is formed. Next, an electrode paste that will become the first electrode 111 is printed on the second mixture layer to form a first electrode material layer. Furthermore, a second mixture layer is again formed on the first electrode material layer. In this way, a second green sheet is obtained in which the second mixture layer / first electrode material layer / second mixture layer is stacked on a portion of the first mixture layer.
[0060] Furthermore, a second electrode material layer is formed on the LATP green sheet by screen printing an electrode paste that will become the second electrode 112. In this way, a third green sheet is obtained in which the second electrode material layer is formed on a portion of the first mixture layer.
[0061] (3) Formation of Laminate Next, the first to third green sheets are stacked to form a laminate (first laminate). When forming the laminate 110 (second laminate) shown in FIG. 1, the first laminate is formed by stacking the second green sheet, the third green sheet, the second green sheet, the third green sheet, the second green sheet, and the first green sheet in this order. Next, the obtained first laminate is cut to a desired size to obtain a plurality of unfired elements (first laminate).
[0062] (4) Firing Step Next, the resulting unfired element is heated in air at 400°C for 2 to 5 hours to remove the organic binder. Thereafter, the unfired element is fired under predetermined firing conditions in a nitrogen atmosphere. In this way, a second laminate (energy storage element) is obtained.
[0063] (5) Current Collector Formation Step Next, a metal paste that will become the external electrodes is applied to both end surfaces of the second laminate and fired under predetermined conditions in a nitrogen atmosphere to form current collectors (external electrodes). The metal paste contains a powder of a metal such as Ag, Cu, Ni, Pt, Pd, an Ag-Pd alloy, or an Ag-Pt alloy. If necessary, a plating layer may be formed on the current collector. For example, a Ni layer (underlayer) and a Sn layer (surface layer) may be plated.
[0064] The electricity storage device 100 can be manufactured in the above manner. The electricity storage device (D) may also be manufactured by other methods. For example, the first laminate may be formed by sequentially stacking material layers. Alternatively, the electricity storage device (D) may be manufactured by the method described in the examples.
[0065] The electricity storage device according to the present disclosure will be described in more detail with reference to Examples. In these Examples, a plurality of electricity storage devices were fabricated and evaluated by the following method.
[0066] (Device A1) Device A1 (electricity storage device) was fabricated by the following method. The solid electrolyte material was LATP powder manufactured by Toshima Manufacturing Co., Ltd. Li was added to the LATP powder as a sintering aid. 2 CO 3The powder was added at 15 mol % and then an organic binder was added and mixed to obtain a first mixed powder.
[0067] The carbonaceous powder contained in the composite layer was Ketjenblack EC600JD (manufactured by Lion Specialty Chemicals Co., Ltd.). This carbonaceous powder was added to the first mixed powder to obtain a second mixed powder. The ratio of the carbonaceous material to the total of the LATP powder and the carbonaceous material was 5% by mass.
[0068] The first mixed powder and the second mixed powder were sequentially filled into a cylindrical mold having an inner diameter of 13 mm. 2 The mixture was press-molded at a pressure of 1000 kJ / cm 2 to obtain a disk-shaped pellet (first laminate). The obtained pellet was heated at 400°C in air to volatilize the organic binder. The pellet was then fired at 800°C in a nitrogen atmosphere to obtain a sintered body (second laminate). The firing transformed the first mixed powder into a solid electrolyte layer, and the second mixed powder into a composite layer. The pellets were prepared so that the thicknesses of the solid electrolyte layer and the composite layer after firing would be as shown in Table 1.
[0069] In this way, a second laminate 110a was obtained as shown in Fig. 2. The laminate 110a in Fig. 2 includes a solid electrolyte layer 115 and a composite layer 113 laminated on the solid electrolyte layer 115.
[0070] Next, as shown in FIG. 2, a first electrode 111 and a second electrode 112 made of gold were formed on both sides of the obtained laminate 110a by sputtering. The electrodes were circular (diameter 8.5 mm). In this manner, an electricity storage device (Device A1) was obtained. The first electrode 111 was used as a positive electrode, and the second electrode 112 was used as a negative electrode.
[0071] (Device A2) Device A2 was fabricated under the same conditions and by the same method as for fabricating device A1, except that the composite layer was disposed only on the second electrode 112 side (negative electrode side).
[0072] (Device A3) Device A3 was fabricated under the same conditions and by the same method as for fabricating device A1, except that composite layers were disposed on both sides of solid electrolyte layer 115.
[0073] (Device A4) Device A4 was fabricated under the same conditions and by the same method as for fabricating device A1, except that composite layers were disposed on both sides of solid electrolyte layer 115 and the thickness of the composite layers was changed.
[0074] (Device C1) Device C1 was fabricated under the same conditions and by the same method as for fabricating device A1, except that the composite layer was not formed.
[0075] (Evaluation of Electricity Storage Device) The volumetric capacity density of the above electricity storage device was evaluated by the following method. First, the fabricated electricity storage device was charged at a constant voltage of 0.5 V for 5 minutes. Thereafter, the electricity storage device was discharged at a current value of 10 μA, and the discharge capacity C (F) at that time was measured. The discharge capacity C was calculated using the following formula: C = t·I / ΔV t: discharge time (sec) I: discharge current (A) ΔV: discharge start voltage (V) - discharge end voltage (V)
[0076] The measured discharge capacity was divided by the volume of the storage element to obtain the volumetric capacity density (mF / cm 3 ) was calculated. Table 1 shows some of the manufacturing conditions and evaluation results of the electricity storage devices. In Device A3, the thickness of the composite layer on the positive electrode side and the thickness of the composite layer on the negative electrode side were each 0.185 mm. In Device A4, the thickness of the composite layer on the positive electrode side and the thickness of the composite layer on the negative electrode side were each 0.278 mm.
[0077]
[0078] As shown in Table 1, devices A1 to A4, which had a composite layer formed thereon, had significantly higher volumetric capacitance densities than comparative device C1.
[0079] Device A1, in which a composite layer was formed on the positive electrode side, had a higher volumetric capacity density than Device A2, in which a composite layer was formed on the negative electrode side. The reason for this is currently unclear, but it can be considered as follows. It can be considered that in the energy storage device (D), a first electric double layer is formed at the interface between the positive electrode and the solid electrolyte layer, and a second electric double layer is formed at the interface between the negative electrode and the solid electrolyte layer. Here, the capacity of the first electric double layer is defined as Cp, and the capacity of the second electric double layer is defined as Cn. As described above, during charging, the first electric double layer is formed by the formation of vacancies in the solid electrolyte facing the positive electrode due to the loss of lithium ions. However, in LATP, charge compensation near the electric double layer may occur due to a change in the valence of Ti ions in LATP, potentially reducing the capacity Cp. In other words, when LATP is used as the solid electrolyte, Cp < Cn may be achieved. Therefore, by forming a composite layer on the positive electrode side and increasing Cp, it is possible that the volumetric capacity density could be particularly high. Such an effect may be a phenomenon specific to certain solid electrolyte layers such as LATP, e.g., Li 7 La 3 Zr 2 and Li 3x La 2/3-x TiO 3 This may not occur with solid electrolytes such as
[0080] The present disclosure can be used for an electricity storage device and a method for manufacturing the same. Although the present invention has been described with reference to presently preferred embodiments, such disclosure should not be interpreted as limiting. Various modifications and alterations will undoubtedly become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. Therefore, the appended claims should be construed to cover all modifications and alterations without departing from the true spirit and scope of the present invention.
[0081] 100: Electricity storage device 110, 110a: Laminate (second laminate) 111: First electrode 112: Second electrode 113: Composite layer 115: Solid electrolyte layer
Claims
1. An electricity storage device, at least one layered first electrode; at least one layered second electrode; and at least one solid electrolyte layer disposed between the first electrode and the second electrode and including a first solid electrolyte; the power storage device further comprising a composite layer comprising a carbon material and a second solid electrolyte at at least one boundary selected from the group consisting of a first boundary between the first electrode and the solid electrolyte layer and a second boundary between the second electrode and the solid electrolyte layer.
2. The first electrode is a positive electrode, The power storage device of claim 1 , wherein the composite layer is disposed only at the first boundary.
3. the first solid electrolyte is a lithium ion conductor; The power storage device according to claim 1 , wherein the first solid electrolyte has a NASICON type crystal structure and contains Li, Al, Ti, P, and O.
4. The specific surface area of the carbon material is 30 m 2 The electricity storage device according to claim 1 or 2, wherein the electrical conductivity is 1 / g or more.
5. The electricity storage device according to claim 1 , wherein the first solid electrolyte and the second solid electrolyte have the same crystal structure.
6. The power storage device according to claim 1 , comprising a plurality of the first electrodes and a plurality of the second electrodes.
7. A method for producing an electricity storage device including a solid electrolyte layer and a composite layer adjacent to the solid electrolyte layer, comprising: a laminate formation step of forming a first laminate including a first mixture layer and a second mixture layer laminated on the first mixture layer; a firing step of firing the first laminate to form a second laminate including the solid electrolyte layer and the composite layer; the solid electrolyte layer includes a first solid electrolyte; the composite layer includes a carbon material and a second solid electrolyte; the first mixture layer contains a material that becomes the solid electrolyte layer by the firing step, The method for manufacturing an electricity storage device, wherein the second mixture layer contains a material that will become the composite layer by the firing step.
8. the first laminate includes a plurality of the first mixture layers, a plurality of the second mixture layers, a plurality of layered first electrode material layers, and a plurality of layered second electrode material layers; the second mixture layer is disposed at at least one boundary selected from the group consisting of a boundary between the first mixture layer and the first electrode material layer and a boundary between the first mixture layer and the second electrode material layer; the first electrode material layer and the second electrode material layer become a first internal electrode and a second internal electrode, respectively, through the firing process; The manufacturing method according to claim 7 , further comprising the step of forming a first current collector connected to the first internal electrode and a second current collector connected to the second internal electrode.
9. The first internal electrode is a positive electrode, The method according to claim 8 , wherein the second mixture layer is disposed only at the boundary between the first mixture layer and the first electrode material layer.
10. the first solid electrolyte is a lithium ion conductor; The manufacturing method according to claim 7 or 8, wherein the first solid electrolyte has a NASICON-type crystal structure and contains Li, Al, Ti, P, and O.
11. The specific surface area of the carbon material is 30 m 2 The method according to claim 7 or 8, wherein the molecular weight of the polymer is 1000 or more.
12. The method according to claim 7 or 8, wherein the first solid electrolyte and the second solid electrolyte have the same crystal structure.