Non-aqueous electrolyte secondary battery

JPWO2023162933A5Pending Publication Date: 2024-11-05
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024503140
Authority / Receiving Office
JP · JP
Patent Type
Applications
Filing Date
2024-08-20
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Nonaqueous electrolyte secondary batteries face issues with electrode deformation due to negative electrode expansion, leading to internal short circuits and reduced performance, particularly in lithium-ion and lithium metal secondary batteries using Si-based materials.

Method used

Incorporating a reverse running portion on the negative electrode that winds in the opposite direction at the start of the electrode group, which suppresses elongation and deformation, thereby alleviating stress and preventing internal short circuits.

Benefits of technology

This configuration enhances cycle characteristics and maintains high capacity by preventing electrode deformation, even with high expansion rates, effectively addressing the challenges of electrode expansion in lithium-ion and lithium metal secondary batteries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This non-aqueous electrolyte secondary battery comprises a non-aqueous electrolyte and a winding electrode group 10 in which a positive electrode 11 and a negative electrode 12 with a separator 13 placed therebetween are wound in a winding direction. The negative electrode 12 has a reverse portion 12A at the end of the electrode 12 from where winding of the winding electrode group 10 starts, the reverse portion 12A not opposing the positive electrode 11 and being wound in the opposite direction to said winding direction.
Need to check novelty before this filing date? Find Prior Art

Description

Non-aqueous electrolyte secondary battery

[0001] The present invention relates to a non-aqueous electrolyte secondary battery.

[0002] Non-aqueous electrolyte secondary batteries have high voltage and high energy density, and are therefore expected to be used in small consumer applications, power storage devices, and electric vehicles. Lithium-ion secondary batteries and lithium secondary batteries (lithium metal secondary batteries) use Si-based materials, including silicon (which alloys with lithium), as the negative electrode active material, due to their high theoretical capacity density and the ease of achieving high battery energy density. In lithium secondary batteries, lithium metal precipitates on the negative electrode during charging, and dissolves in the non-aqueous electrolyte during discharging.

[0003] On the other hand, lithium-ion secondary batteries or lithium secondary batteries using the above-mentioned Si-based materials as the negative electrode active material have a large expansion of the negative electrode during charging. As a result, the expanded negative electrode presses on the positive electrode, causing local distortion or deformation of the electrode plate around the pressed area, which can cause an internal short circuit or a decrease in battery performance.

[0004] The nonaqueous electrolyte secondary battery described in Patent Document 1 includes a wound electrode body in which a positive electrode and a negative electrode having a negative electrode composite layer formed on a negative electrode core are spirally wound with a separator interposed therebetween. The negative electrode includes a non-facing portion wound from the inner end of the wound electrode body in the winding direction through the separator, not facing the positive electrode, for 1.25 or more turns. The non-facing portion has a negative electrode composite layer forming portion on at least one surface, in which a negative electrode composite layer is formed, extending continuously from the outer end in the winding direction to the inner side in the winding direction, and the negative electrode composite layer forming portion is wound for 0.75 or more turns. This ensures that even in the event of a fire in the secondary battery, an exhaust path is secured by the negative electrode composite layer forming portion, allowing for efficient exhaust of high-temperature and high-pressure gas generated inside the battery upon fire.

[0005] The secondary battery described in Patent Document 2 includes a wound body formed by stacking and winding a positive electrode having a positive electrode active material layer provided on a positive electrode current collector having a pair of opposing surfaces, and a negative electrode having a negative electrode active material layer provided on a negative electrode current collector having a pair of opposing surfaces. The negative electrode has a double-sided opposing region where the negative electrode active material layer and the positive electrode active material layer face each other on both the outer peripheral surface side and the inner peripheral surface side, and an outer peripheral opposing region where the negative electrode active material layer and the positive electrode active material layer face each other only on the outer peripheral surface side, the outer peripheral opposing region being in a range of 2 to 3.25 turns toward the winding center. This appropriately reduces the energy density toward the winding center, relieves stress associated with occlusion of electrode reactants, relieves local distortion, and improves cycle characteristics.

[0006] Re-listed Patent Publication No. 2018-116876 JP 2006-24464 A

[0007] The present invention provides a non-aqueous electrolyte secondary battery that suppresses electrode deformation due to expansion of the negative electrode and has high cycle characteristics.

[0008] One aspect of the present invention relates to a non-aqueous electrolyte secondary battery including a wound electrode group in which a positive electrode and a negative electrode are wound in a winding direction with a separator interposed between them, and a non-aqueous electrolyte, wherein the negative electrode has a reverse running part at an end of the wound electrode group on the winding start side that does not face the positive electrode and is wound in a direction opposite to the winding direction.

[0009] According to the nonaqueous electrolyte secondary battery according to the present disclosure, deformation of the electrode due to expansion of the negative electrode is suppressed, and high cycle characteristics can be achieved.

[0010] The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.

[0011] 1 is a schematic cross-sectional view of a wound electrode group used in a nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure, taken along a plane perpendicular to the winding axis, illustrating the state at the start of winding of the wound electrode group.

[0012] Hereinafter, embodiments of the present disclosure will be described using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values, materials, etc. may be exemplified. However, other numerical values, materials, etc. may be applied as long as the effects of the present disclosure are obtained. Note that components other than those characteristic of the present disclosure may be those of known secondary batteries. In this specification, when a "range from numerical value A to numerical value B" is used, the range includes numerical value A and numerical value B, and can be interpreted as "greater than or equal to numerical value A and less than or equal to numerical value B." In the following description, when lower and upper limits for specific physical properties or conditions are exemplified, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not greater than the upper limit. When multiple materials are exemplified, one material may be selected from the materials and used alone, or two or more materials may be used in combination.

[0013] The present disclosure also encompasses combinations of two or more features arbitrarily selected from the appended claims, i.e., two or more features arbitrarily selected from the appended claims can be combined unless a technical contradiction arises.

[0014] A non-aqueous electrolyte secondary battery according to an embodiment of the present disclosure includes a wound electrode group in which a positive electrode and a negative electrode are wound in a winding direction with a separator interposed therebetween, and a non-aqueous electrolyte. The negative electrode has a reverse running portion at an end of the wound electrode group on the winding start side that does not face the positive electrode and is wound in the opposite direction to the winding direction.

[0015] A wound electrode assembly is typically constructed by stacking a positive electrode and a negative electrode with a separator interposed therebetween, and then winding the positive electrode and the negative electrode with the separator interposed around a predetermined winding core. The positive electrode, the negative electrode, and the separator may each be, for example, in the form of a long sheet. The winding core is typically removed from the center of the electrode assembly.

[0016] In contrast, in the nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure, the wound electrode group is formed by first winding the negative electrode around a winding core by a predetermined length in a direction opposite to the winding direction, and then stacking the positive electrode and negative electrode with a separator interposed therebetween, and winding them in the winding direction.

[0017] In this case, when the wound electrode group is viewed from above (perpendicular to the winding axis), the negative electrode is folded back at the winding start side (inner periphery side) of the wound electrode group. Two negative electrode portions extend in the winding direction, starting from the folding position X. Of the two negative electrode portions, one extending in the winding direction from the folding position X toward the inner periphery is the reverse running portion, while the other extends in the winding direction all the way to the winding end side (outer periphery side) of the wound electrode group (see FIG. 2 ). When viewed from the winding start position O of the winding as the starting point, the reverse running portion runs in the opposite direction to the winding direction.

[0018] When the negative electrode expands due to charging, stress is applied to the inner peripheral end of the negative electrode, which is located at the beginning of the winding, causing it to stretch in the circumferential direction. This stretching of the inner peripheral end may pierce the positive electrode, which is located further outward, resulting in an internal short circuit. Furthermore, the stretching of the inner peripheral end may promote buckling deformation of the wound electrode assembly.

[0019] However, because the negative electrode is folded back at the winding start end of the negative electrode by the reverse running portion, elongation of the winding start end is suppressed. As a result, internal short circuits due to end elongation are suppressed. Furthermore, deformation of the wound electrode assembly, such as buckling deformation, is suppressed. Furthermore, the strength of the wound electrode assembly at the inner periphery is increased by the folded portion, which also contributes to suppressing deformation of the wound electrode assembly. Therefore, deformation of the electrode due to expansion of the negative electrode is suppressed, thereby achieving high cycle characteristics.

[0020] The reverse-running portion may be wound in the opposite direction to the winding direction for at least 0.5 turns to suppress elongation at the winding start end of the negative electrode. On the other hand, the reverse-running portion is a portion that does not face the positive electrode and does not contribute to capacity. To maintain high capacity, the reverse-running portion may be wound in the opposite direction to the winding direction for at most 1.25 turns.

[0021] The length of the reverse-running portion, or the number of turns of the winding that the length of the reverse-running portion corresponds to, may be evaluated as follows.

[0022] The length of the reverse-running portion is determined by X-raying a cross section perpendicular to the winding axis of a wound electrode group removed from a discharged battery and performing image analysis on the cross-sectional photograph. In the cross-sectional image, the area of ​​the region S inside the wound electrode group that is not occupied by the negative electrode, positive electrode, or separator is determined, and the diameter of a circle having an area equal to this area is defined as the inner diameter r of the wound electrode group. However, on the inner peripheral surface of the wound electrode group, a connection portion with the winding core may remain protruding toward the central axis of the wound electrode group. When calculating the inner diameter r, the area occupied by such a protruding portion is not included in the area occupied by the wound electrode group, but is added to the region S.

[0023] The fold position X of the negative electrode is identified by image analysis, the length l of the reverse-running portion (excluding the protruding portion) is determined, and n = l / πr is derived. In this case, the reverse-running portion has a length equivalent to n turns of the winding and is wound in the opposite direction to the winding direction. n is 0.5 to 1.25.

[0024] The present invention is not limited to the configuration of the positive electrode, negative electrode, and non-aqueous electrolyte, and is effective for non-aqueous electrolyte secondary batteries in which the negative electrode repeatedly expands and contracts with charge and discharge and which use a wound electrode group. The non-aqueous electrolyte secondary battery may be, for example, a lithium ion battery using an active material in the negative electrode that absorbs lithium ions during charge and releases lithium ions during discharge, or a lithium secondary battery (also called a lithium metal secondary battery) in which lithium metal is deposited on the negative electrode during charge and dissolves in the non-aqueous electrolyte during discharge. In lithium secondary batteries, the negative electrode has at least a negative electrode current collector, and lithium metal is deposited directly or indirectly on the negative electrode current collector.

[0025] Here, the expansion coefficient of the negative electrode is defined as the ratio T1 / T0 of the thickness of the negative electrode T1 at an SOC (State of Charge) of 100% to the thickness T0 of the negative electrode at an SOC of 0%. The thickness of the negative electrode is determined by taking out the battery in a discharged state and a charged state and averaging the thicknesses of the negative electrode at any 10 or more different points.

[0026] A state of 100% SOC is a state in which the battery is charged at a predetermined current value (e.g., 0.1 It) up to a predetermined charge end voltage corresponding to the rated capacity C. A state of 0% SOC is a state in which the battery is discharged from a state of 100% SOC to a predetermined discharge end voltage at a predetermined current value (e.g., 0.1 It), and is a state in which an amount of electricity equivalent to the rated capacity C is discharged from a state of 100% SOC. Here, It represents the time rate. When an amount of electricity equivalent to the rated capacity C (mAh) flows for t hours (h), the current value I (mA) of the t-hour rate is expressed as C / t.

[0027] The expansion rate of the negative electrode may be 108% or more (T1 / T0≧1.08). In the nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure, even when the negative electrode has such an expansion rate, the provision of the reverse running portion suppresses deformation of the electrode due to expansion of the negative electrode, thereby achieving high cycle characteristics.

[0028] For example, in a lithium-ion secondary battery that uses a Si-based material as a negative electrode active material that occludes lithium ions, the expansion rate of the negative electrode can be as high as 120% or more (T1 / T0≧1.2). However, in a nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure, even when the negative electrode has such a high expansion rate, the provision of a reverse running portion suppresses electrode deformation due to the expansion of the negative electrode, thereby achieving high cycle characteristics.

[0029] Furthermore, for example, in a lithium secondary battery (lithium metal secondary battery) in which lithium metal precipitates on the negative electrode during charging and dissolves in the non-aqueous electrolyte during discharge, the expansion rate of the negative electrode may be extremely high, at 140% or more (T1 / T0≧1.4). However, in a non-aqueous electrolyte secondary battery according to an embodiment of the present disclosure, by providing a reverse running portion, even when the negative electrode has such an extremely high expansion rate, deformation of the electrode due to expansion of the negative electrode is suppressed, and high cycle characteristics can be achieved.

[0030] The inner diameter r of the wound electrode assembly may be 5 mm or less. The inner diameter r is calculated by the method described above through image analysis of a cross-sectional photograph of the wound electrode assembly. If the inner diameter r is 5 mm or less, the curvature of the negative electrode is large on the inner circumferential side of the wound electrode assembly, and expansion of the negative electrode is likely to cause an internal short circuit due to elongation of the end portion on the winding start side or deformation of the wound electrode assembly. However, in a nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure, by providing a reverse running portion, deformation of the electrode due to expansion of the negative electrode is suppressed, and high cycle characteristics can be achieved, even when the wound electrode assembly has a small inner diameter r of 5 mm or less.

[0031] The inner diameter r of the wound electrode assembly may be 2.5 mm or less. If the inner diameter r is 2.5 mm or less, the curvature of the negative electrode is particularly large on the inner circumferential side of the wound electrode assembly, and internal short circuits or deformation of the wound electrode assembly due to elongation of the end portion at the winding start side becomes significant. However, in a nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure, by providing a reverse running portion, even when the wound electrode assembly has such an extremely small inner diameter r, deformation of the electrode due to expansion of the negative electrode is suppressed, and high cycle characteristics can be achieved.

[0032] The nonaqueous electrolyte battery may have an outer diameter R of 3 mm or more and 6.5 mm or less, and a height H of 15 mm or more and 65 mm or less. The outer diameter R may be 3 mm to 5.5 mm. The height H may be 15 to 45 mm. The outer diameter R of the lithium secondary battery is the maximum outer diameter of the battery case of the battery (the assembled battery). The height H of the battery is the height of the assembled battery, and is the distance from the bottom surface of the battery (the outer bottom surface of the battery case) to the top surface of the battery (the top surface of the sealing member).

[0033] When the outer diameter R is small, the inner diameter r of the wound electrode group also becomes small according to the outer diameter R. When the outer diameter R is 3 mm to 6.5 mm, in order to obtain a high capacity, the inner diameter r is 5 mm or less, and it is also possible that the inner diameter r may be 2.5 mm or less. Note that a nonaqueous electrolyte secondary battery having a small outer diameter R as described above is also called a "pin-type battery." The nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure is particularly effective as a pin-type battery.

[0034] The components of a non-aqueous electrolyte secondary battery will be specifically described below using a lithium secondary battery (lithium metal secondary battery) as an example.

[0035] (Negative electrode) The negative electrode has at least a negative electrode current collector. Lithium metal is deposited on the surface of the negative electrode upon charging. More specifically, lithium ions contained in the non-aqueous electrolyte receive electrons on the negative electrode upon charging, becoming lithium metal, which is then deposited on the surface of the negative electrode. The lithium metal deposited on the surface of the negative electrode dissolves as lithium ions in the non-aqueous electrolyte upon discharging. The lithium ions contained in the non-aqueous electrolyte may be derived from a lithium salt added to the non-aqueous electrolyte, may be supplied from the positive electrode active material upon charging, or may be both.

[0036] The negative electrode may include a negative electrode current collector and a sheet of lithium metal or lithium alloy in close contact with the surface of the negative electrode current collector. That is, a base layer containing lithium metal may be provided on the negative electrode current collector in advance. The lithium alloy may contain elements such as aluminum, magnesium, indium, and zinc in addition to lithium. By providing a base layer containing lithium metal and depositing lithium metal on the base layer during charging, dendritic deposition can be suppressed. The thickness of the base layer containing lithium metal is not particularly limited, but may be, for example, in the range of 5 μm to 25 μm.

[0037] The negative electrode may include a lithium ion occlusion layer (a layer that exhibits capacity by occlusion and release of lithium ions by a negative electrode active material (such as graphite)) supported on a negative electrode current collector. In this case, too, the open circuit potential of the negative electrode when fully charged may be 70 mV or less relative to lithium metal (lithium dissolution and deposition potential). When the open circuit potential of the negative electrode when fully charged is 70 mV or less relative to lithium metal, lithium metal is present on the surface of the lithium ion occlusion layer when fully charged.

[0038] The lithium ion occlusion layer is a layer of a negative electrode mixture containing a negative electrode active material. The negative electrode mixture may contain a binder, a thickener, a conductive material, etc. in addition to the negative electrode active material.

[0039] Examples of the negative electrode active material include a carbonaceous material, a Si-containing material, and a Sn-containing material. The negative electrode may contain one or more negative electrode active materials. Examples of the carbonaceous material include graphite, easily graphitizable carbon (soft carbon), and hardly graphitizable carbon (hard carbon).

[0040] The conductive material is, for example, a carbon material, such as carbon black, acetylene black, ketjen black, carbon nanotubes, and graphite.

[0041] Examples of the binder include fluororesin, polyacrylonitrile, polyimide resin, acrylic resin, polyolefin resin, rubber polymer, etc. Examples of the fluororesin include polytetrafluoroethylene, polyvinylidene fluoride, etc.

[0042] The negative electrode current collector may be a conductive sheet, such as a foil or film.

[0043] The material of the negative electrode current collector (conductive sheet) may be any conductive material other than lithium metal and lithium alloys. The conductive material may be a metallic material such as a metal or alloy. The conductive material is preferably a material that does not react with lithium. More specifically, a material that does not form an alloy or an intermetallic compound with lithium is preferred. Examples of such conductive materials include copper (Cu), nickel (Ni), iron (Fe), and alloys containing these metal elements, as well as graphite with a preferentially exposed basal plane. Examples of alloys include copper alloys and stainless steel (SUS). Among these, copper and / or copper alloys with high conductivity are preferred.

[0044] The thickness of the negative electrode current collector is not particularly limited and is, for example, 5 μm or more and 300 μm or less.

[0045] (Positive Electrode) The positive electrode includes, for example, a positive electrode current collector and a positive electrode composite layer supported on the positive electrode current collector. The positive electrode composite layer includes, for example, a positive electrode active material, a conductive material, and a binder. The positive electrode composite layer may be formed on only one side of the positive electrode current collector, or may be formed on both sides. The positive electrode is obtained, for example, by applying a positive electrode composite slurry including the positive electrode active material, the conductive material, and the binder to both sides of the positive electrode current collector, drying the coating, and then rolling.

[0046] The positive electrode active material is a material that absorbs and releases lithium ions. Examples of the positive electrode active material include lithium-containing transition metal oxides, transition metal fluorides, polyanions, fluorinated polyanions, and transition metal sulfides. Among these, lithium-containing transition metal oxides are preferred because of their low production cost and high average discharge voltage.

[0047] The lithium contained in the lithium-containing transition metal oxide is released from the positive electrode as lithium ions during charging and precipitates as lithium metal on the negative electrode or negative electrode current collector. During discharging, the lithium metal dissolves from the negative electrode, releasing lithium ions, which are then absorbed into the composite oxide of the positive electrode. In other words, the lithium ions involved in charging and discharging are generally derived from the solute in the nonaqueous electrolyte and the positive electrode active material.

[0048] Examples of transition metal elements contained in the lithium-containing transition metal oxide include Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, and W. The lithium-containing transition metal oxide may contain one or more transition metal elements. The transition metal element may be Co, Ni, and / or Mn. The lithium-containing transition metal oxide may contain one or more typical elements as needed. Examples of typical elements include Mg, Al, Ca, Zn, Ga, Ge, Sn, Sb, Pb, and Bi. The typical element may be Al, etc.

[0049] Among lithium-containing transition metal oxides, composite oxides containing Ni as a transition metal element, Co and / or Mn, and optionally Al, and having a layered rock-salt crystal structure are preferred in terms of achieving high capacity. In lithium secondary batteries, the molar ratio mLi / mM of the total amount of lithium in the positive and negative electrodes mLi to the amount mM of metals other than lithium M in the positive electrode may be set to, for example, 1.1 or less. In the case of pin-type batteries, mLi / mM may be set to 2.0 or less.

[0050] As the binder, conductive agent, etc., for example, those exemplified for the negative electrode can be used. The shape and thickness of the positive electrode current collector can be selected from the shape and range of the positive electrode current collector.

[0051] Examples of the material of the positive electrode current collector (conductive sheet) include metal materials containing Al, Ti, Fe, etc. The metal material may be Al, an Al alloy, Ti, a Ti alloy, an Fe alloy, etc. The Fe alloy may be stainless steel (SUS).

[0052] The thickness of the positive electrode current collector is not particularly limited and is, for example, 5 μm or more and 300 μm or less.

[0053] (Separator) The separator may be any separator used in lithium secondary batteries or lithium ion secondary batteries without any particular limitations. Such a separator is a porous sheet having ion permeability and insulating properties. Examples of porous sheets include porous membranes, woven fabrics, nonwoven fabrics, etc. The porous membrane may be a uniaxially or biaxially stretched sheet, etc. The material of the porous sheet is not particularly limited, but may be a polymeric material. Examples of polymeric materials include polyolefin resins, polyamide resins, polyimide resins, cellulose, etc. Examples of polyolefin resins include polyethylene, polypropylene, and copolymers of ethylene and propylene, etc. The porous sheet may contain one material or two or more materials. The porous sheet may contain additives as needed. Examples of additives include inorganic fillers, etc.

[0054] The thickness of the separator is not particularly limited and can be appropriately selected from the range of, for example, 5 μm to 300 μm. The thickness of the porous membrane is, for example, 5 μm to 50 μm.

[0055] The separator may have a heat-resistant layer on at least one surface. That is, the separator may include a substrate and a heat-resistant layer. The heat-resistant layer is formed on at least one of the two main surfaces of the substrate. The heat-resistant layer has insulating properties.

[0056] The heat-resistant layer can suppress the shrinkage of the substrate when the temperature of the electrode assembly rises excessively. If the substrate shrinks, the positive electrode and the negative electrode are likely to short-circuit, which further increases the temperature of the electrode assembly. By including the heat-resistant layer in the separator, the shrinkage of the substrate can be suppressed, thereby suppressing a further increase in the temperature of the electrode assembly.

[0057] The substrate may be the porous sheet described above, i.e., a separator used in lithium secondary batteries or lithium ion secondary batteries. The substrate may be, for example, a porous film containing a polyolefin resin. Polyolefin resins are desirable because they have excellent durability and a function of closing pores when the temperature rises to a certain level (i.e., a shutdown function). The substrate may have a single-layer structure, a two-layer structure, or a three- or more-layer structure.

[0058] The heat-resistant layer may contain inorganic particles (or inorganic fillers) and a polymer (or polymer or resin). The polymer binds the inorganic particles to the substrate. It is desirable to use a heat-resistant resin as the polymer, which has higher heat resistance than the main component of the substrate. The heat-resistant layer may contain inorganic particles as the main component (e.g., 80% by mass or more), or may contain a heat-resistant resin as the main component (e.g., 40% by mass or more). The heat-resistant layer may not contain inorganic particles, but may contain a heat-resistant resin.

[0059] The heat-resistant resin may be a polyamide resin, a polyimide resin, a polyamideimide resin, or the like. Among these, it is preferable to use at least one selected from the group consisting of aromatic polyamides, aromatic polyimides, and aromatic polyamideimides. These are known as polymers with particularly high heat resistance. From the viewpoint of heat resistance, aramids, i.e., meta-aramids (meta-wholly aromatic polyamides) and para-aramids (para-wholly aromatic polyamides), are preferred.

[0060] The inorganic particles are particles made of insulating inorganic compounds. Examples of materials for the inorganic particles include oxides, oxide hydrates, hydroxides, nitrides, carbides, sulfides, etc., which may contain metal elements.

[0061] Specific examples include aluminum oxide, boehmite, magnesium oxide, titanium oxide, zirconium oxide, silicon oxide, yttrium oxide, zinc oxide, silicon nitride, aluminum nitride, boron nitride, titanium nitride, silicon carbide, boron carbide, barium sulfate, aluminum hydroxide, etc. Among these, at least one selected from the group consisting of aluminum oxide, boehmite, talc, titanium oxide, and magnesium oxide is preferred in terms of insulation properties, heat resistance, etc.

[0062] The inorganic particles may include a lithium-containing phosphate. The lithium-containing phosphate may be lithium phosphate (Li 3 P.O. 4 ), dilithium hydrogen phosphate (Li 2 HPO 4 ) and lithium dihydrogen phosphate (LiH 2 P.O. 4 Among these, lithium phosphate is preferred because it is highly effective in suppressing heat generation in the battery during abnormal conditions.

[0063] The average particle size of the inorganic particles is not particularly limited, but may be, for example, 0.2 μm to 2 μm. The average particle size of the lithium-containing phosphate may be 0.1 μm to 1.0 μm, or 0.1 μm to 0.5 μm. By setting the average particle size to 0.1 μm or more, sufficient pores necessary for the non-aqueous electrolyte to penetrate can be secured. By setting the average particle size to 1.0 μm or less, a heat-resistant layer in which the lithium-containing phosphate is densely packed can be formed.

[0064] (Non-aqueous electrolyte) The non-aqueous electrolyte may be any non-aqueous electrolyte having lithium ion conductivity, and includes a solvent and an electrolyte salt dissolved in the solvent. The solvent includes an ether compound as a main component. The electrolyte salt includes at least a lithium salt. The lithium salt dissolves in the solvent to generate lithium ions and anions. The non-aqueous electrolyte may be liquid, or the liquid non-aqueous electrolyte may be gelled by a polymer that absorbs the solvent.

[0065] In addition to ether compounds, examples of the solvent include ester compounds, nitrile compounds, amide compounds, and halogen-substituted compounds thereof. The nonaqueous electrolyte may contain one or more of these nonaqueous solvents. Examples of halogen-substituted compounds include fluorides.

[0066] Examples of ester compounds include carbonate esters and carboxylic acid esters. Examples of cyclic carbonate esters include ethylene carbonate, propylene carbonate, and fluoroethylene carbonate (FEC). Examples of chain carbonate esters include dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC). Examples of cyclic carboxylic acid esters include γ-butyrolactone and γ-valerolactone. Examples of chain carboxylic acid esters include ethyl acetate, methyl propionate, and methyl fluoropropionate.

[0067] Examples of the ether compound include cyclic ethers and chain ethers, and particularly, compounds represented by the general formula (1): R1-(OCH 2 CH 2 ) n It is desirable to use a first ether compound (non-fluorinated ether) represented by —OR2 (in formula (1), R1 and R2 each independently represent an alkyl group having 1 to 5 carbon atoms, and n is 1 to 3).

[0068] The lowest unoccupied molecular orbital (LUMO) of a non-fluorinated ether exists at a high energy level. Therefore, the non-fluorinated ether is not easily reductively decomposed even when it comes into contact with lithium metal, which has a strong reducing power. Furthermore, oxygen in the non-fluorinated ether skeleton strongly interacts with lithium ions, so that the lithium salt contained as an electrolyte salt in the non-aqueous electrolyte can be easily dissolved.

[0069] Non-fluorinated ethers are suitable as solvents for non-aqueous electrolytes in lithium secondary batteries, because they suppress side reactions between lithium metal and non-aqueous electrolytes and increase the solubility of lithium salts in the solvent.

[0070] Specific examples of the first ether compound (non-fluorinated ether) include 1,2-dimethoxyethane, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol dibutyl ether, triethylene glycol dimethyl ether, etc. One type of first ether compound may be used alone, or two or more types may be used in combination.

[0071] The ether compound may contain a fluorinated ether. The interaction of the oxygen in the ether skeleton of a fluorinated ether with lithium ions is weaker than that of a non-fluorinated ether. This is thought to be because the strong electronegativity of the fluorine atom attracts electrons from the entire molecule toward the inner core, lowering the orbital level of the lone electron pair of oxygen in the ether skeleton that would interact with lithium ions.

[0072] Among the fluorinated ethers, those represented by the general formula (2): C a1 H b1 F c1 O d1 (CF 2 OCH 2 ) C a2 H b2 F c2 O d2 (in formula (2), a1≧1, a2≧0, b1≦2a1, b2≦2a2, c1=(2a1+1)−b1, c2=(2a2+1)−b2, d1≧0, and d2≧0) is preferably used.

[0073] The ether compound may be a combination of a fluorinated ether and a non-fluorinated ether. For example, when the second ether compound is used together with the first ether compound, the charge / discharge reaction in the lithium secondary battery proceeds more uniformly. This is thought to be due to a better balance of the solvation energies between the ether compound and lithium ions.

[0074] The fluorination rate of the second ether compound may be 60% or more. The fluorination rate of the second ether compound is the ratio of the number of fluorine atoms to the total number of fluorine atoms and hydrogen atoms contained in the second ether compound, expressed as a percentage (%).

[0075] Specific examples of the second ether compound (fluorinated ether) include 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether, etc. One type of second ether compound may be used alone, or two or more types may be used in combination.

[0076] The total amount of the first ether compound and the second ether compound may be 80% by volume or more of the total amount of the solvent, and when the total amount is 80% by volume or more, the effect of improving the cycle characteristics of the lithium secondary battery becomes more pronounced.

[0077] The volume ratio V1 / V2 of the volume V1 of the first ether compound to the volume V2 of the second ether compound is preferably 1 / 0.5 to 1 / 4, and more preferably 1 / 0.5 to 1 / 2.

[0078] As the anion of the lithium salt, a known anion used in the non-aqueous electrolyte of a lithium secondary battery can be used. Specifically, BF 4 - , ClO 4 - , P.F. 6 - , C.F. 3 SO 3 - , C.F. 3 CO 2 - , imide anion, oxalate complex anion, etc.

[0079] In order to prevent lithium metal from being deposited in a dendrite form, the electrolyte salt contains imide anions, PF 6 -and oxalate complex anions. Among these, the oxalate complex anions tend to precipitate lithium metal uniformly in the form of fine particles through their interaction with lithium.

[0080] The imide anion is N(SO 2 F) 2 - , N(SO 2 CF 3 ) 2 - , N(C m F 2m+1 SO 2 ) x (C n F 2n+1 SO 2 ) y - (wherein m and n are each independently an integer of 0 or 1 or more, and x and y are each independently 0, 1, or 2, and x + y = 2 is satisfied.) Among these, bis(fluorosulfonyl)imide anion (N(SO 2 F) 2 - Therefore, it is preferable that the lithium salt contains lithium bis(fluorosulfonyl)imide (hereinafter also referred to as "LiFSI").

[0081] Examples of the oxalate complex anion include bisoxalate borate anion and difluorooxalate borate anion (BF 2 (C 2 O 4 ) - ), P.F. 4 (C 2 O 4 ) - , P.F. 2 (C 2 O 4 ) 2 - Among them, difluorooxalate borate anion (BF 2 (C 2 O 4 ) -Therefore, it is preferable that the lithium salt contains lithium difluorooxalatoborate (hereinafter also referred to as "LiFOB").

[0082] As described above, the electrolyte salt is LiPF 6 It is desirable that the non-aqueous electrolyte contains at least one selected from the group consisting of lithium salts, imide salts, and oxalate complex salts. The concentration of the lithium salt in the non-aqueous electrolyte is, for example, 0.5 mol / L or more and 3.5 mol / L or less. The concentration of the oxalate complex salt in the non-aqueous electrolyte may be 0.05 mol / L or more and 1 mol / L or less.

[0083] An example of a nonaqueous electrolyte secondary battery according to the present embodiment will be specifically described below with reference to the drawings. The components described above can be applied to the components of the example nonaqueous electrolyte secondary battery described below. The components of the example described below can be modified based on the above description. The matters described below may also be applied to the above embodiment. In the nonaqueous electrolyte secondary battery described below, components that are not essential for the nonaqueous electrolyte secondary battery according to the present disclosure may be omitted. Note that the scale of the components has been changed in the following drawings to facilitate understanding.

[0084] Fig. 1 is a schematic longitudinal sectional view of a pin-shaped nonaqueous electrolyte secondary battery (lithium secondary battery) according to an embodiment of the present disclosure. Fig. 2 is a schematic sectional view showing an example of a wound electrode group used in the nonaqueous electrolyte secondary battery (lithium secondary battery) shown in Fig. 1, particularly showing a cut-out view of the start of winding.

[0085] The nonaqueous electrolyte secondary battery 100 includes a cylindrical battery case 20 with an opening and a bottom, a wound electrode group 10 and a nonaqueous electrolyte (not shown) housed in the battery case 20, and a sealing member 40 that seals the opening of the battery case 20. The electrode group 10 is composed of a positive electrode 11, a negative electrode 12, and a separator 13 interposed between them.

[0086] The closing member 40 is hat-shaped and has a ring-shaped collar (brim 40a) and cylindrical terminals 40b and 40c that protrude in the thickness direction from the inner periphery of the brim 40a. A ring-shaped insulating gasket 30 is disposed around the periphery of the closing member 40 so as to cover the brim 40a. The open end of the battery case 20 is bent inward via the gasket 30 and crimped to the periphery of the closing member 40, thereby insulating the battery case 20 from the closing member 40 and sealing the battery case 20.

[0087] A space is formed between the upper end surface (top surface) of the electrode group 10 and the bottom surface of the sealing member 40. A first insulating ring 50A is disposed in this space to regulate contact between the electrode group 10 and the sealing member 40.

[0088] A doughnut-shaped second insulating ring 50B made of an electrically insulating material is disposed so as to cover the outer surface of the bent open end of the battery case 20 and the surface of the gasket 30 around it.

[0089] One end of the positive electrode current collecting lead 60 is connected to the positive electrode 11 by welding or the like, and the other end is connected to the bottom surface of the sealing member 40 by welding or the like through a hole formed in the center of the first insulating ring 50A. In other words, the positive electrode 11 and the sealing member 40 are electrically connected via the positive electrode current collecting lead 60, and the sealing member 40 functions as an external positive electrode terminal.

[0090] One end of a negative electrode current collector lead 70 is connected by welding or the like to the negative electrode 12 on the outermost side of the electrode group 10. The other end of the negative electrode current collector lead 70 is connected to the inner wall of the battery case 20 at a welding point 70a. In other words, the negative electrode 12 and the battery case 20 are electrically connected via the negative electrode current collector lead 70, and the battery case 20 functions as an external negative electrode terminal. The welding point 70a is formed, for example, on the inner wall closer to the opening of the battery case 20 than the upper end surface of the electrode group 10.

[0091] The negative electrode 12 of the wound electrode group 10 has a reverse running portion 12A. As shown in FIG. 2 , the negative electrode 12 is folded back at a folding position X shown in FIG. 2 . The portion of the negative electrode located outer than the folding position X is wound clockwise, and at least its outer surface faces the positive electrode 11 with the separator 13 interposed between them. On the other hand, the portion of the negative electrode located inner than the folding position X is the reverse running portion 12A. The reverse running portion 12A is the portion of the negative electrode from the winding start position O to the folding position X, and when the winding start position O is taken as the starting point, it is wound in the opposite direction (counterclockwise) to the winding direction of the positive electrode 11 (i.e., reverse running).

[0092] The reverse-running portion 12A does not face the positive electrode 11 but faces the negative electrode 12. Therefore, when using a negative electrode in which a negative electrode mixture layer (e.g., a lithium ion occlusion layer) containing a negative electrode active material is formed on a negative electrode current collector, the negative electrode mixture layer may not be formed in the reverse-running portion 12A, and the negative electrode current collector may be exposed.

[0093] EXAMPLES The present invention will be specifically described below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0094] In the following Examples and Comparative Examples, cylindrical lithium secondary batteries were fabricated as shown in Fig. 1. The cylindrical lithium secondary batteries had an outer diameter R of 4 mm and a height H of 25 mm.

[0095] (Example 1) (1) Preparation of Positive Electrode 11 A positive electrode slurry was prepared by mixing 100 parts by mass of a lithium-containing transition metal oxide (NCA: positive electrode active material) having a layered rock salt crystal structure, containing Li, Ni, Co, and Al (the molar ratio of Li to the total of Ni, Co, and Al was 1.0), 4 parts by mass of acetylene black as a conductive agent, and 4 parts by mass of polyvinylidene fluoride (PVdF) as a binder, with N-methyl-2-pyrrolidone (NMP) as a dispersion medium. The positive electrode slurry was applied to both sides of aluminum foil (thickness 15 μm) as a positive electrode current collector, dried, and then compressed in the thickness direction to prepare a positive electrode 11 (thickness 80 μm) having a positive electrode composite layer on the surface of the positive electrode current collector. During production, the positive electrode 11 was provided with an exposed portion of the positive electrode current collector in the width direction of the positive electrode (the direction parallel to the winding axis of the electrode group), and one end of a ribbon-shaped aluminum positive electrode current collector lead 60 (width 1.0 mm, thickness 0.05 mm) was connected to the exposed portion.

[0096] (2) Preparation of Negative Electrode 12 A 20 μm thick lithium metal foil was attached to both sides of a copper foil (thickness: 10 μm) serving as a negative electrode current collector to prepare a negative electrode 12 (thickness: 50 μm). An exposed portion of the negative electrode current collector was provided in a portion corresponding to the outermost periphery of the negative electrode 12 in the electrode group 10, and one end of a ribbon-shaped nickel negative electrode current collector lead 70 (width: 1.5 mm, thickness: 0.05 mm) was connected to the exposed portion.

[0097] (3) Preparation of Electrode Assembly 10 The electrode assembly 10 was formed by winding the positive electrode 11 and the negative electrode 12 with the separator 13 interposed therebetween. A reverse run portion 12A where no lithium metal foil was attached was provided at the end of the negative electrode 12 at the start of winding, and the positive electrode 11 and the negative electrode 12 were overlapped with the separator 13 interposed therebetween so that the reverse run portion 12A did not overlap with the positive electrode 11. The reverse run portion 12A was wound in a direction facing the positive electrode 11, and then the positive electrode 11 and the portion of the negative electrode 12 other than the reverse run portion were wound in the opposite direction with the separator 13 interposed therebetween, to obtain an electrode assembly 10 whose initial winding state is shown in FIG. 2 .

[0098] The length of the reverse-running portion 12A was set to a length equivalent to 0.75 turns of the winding. An insulating tape was attached to the end of the winding to fix the electrode group 10. A porous polyethylene film having a thickness of 16 μm was used as the separator.

[0099] (4) Preparation of non-aqueous electrolyte: Dimethoxyethane (DME) and 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether (H(CF 2 ) 2 CH 2 O (CF 2 ) 2 A non-aqueous electrolyte was prepared by dissolving LiFSI and LiFOB in a mixed solvent containing HCl (H) and HCl (H) in a mass ratio of 25:75. The LiFSI concentration in the non-aqueous electrolyte was 1.0 mol / L, and the LiFOB concentration was 0.05 mol / L.

[0100] (5) Fabrication of Cylindrical Lithium Secondary Battery 100 The electrode group 10 obtained in (3) above was inserted into a cylindrical battery case 20 made of nickel-plated iron plate with an opening and a bottom, and the other end of the negative electrode current collector lead 70 was welded to the inner wall of the battery case 20 at a welding point 70a. A first insulating ring 50A was placed on top of the electrode group 10, and the other end of the positive electrode current collector lead 60, which had been pulled out from the electrode group 10, was connected to the bottom surface of a nickel-plated iron sealing member 40 through a hole in the first insulating ring 50A at the welding point 70a. A ring-shaped insulating gasket 30 was attached to the periphery of the sealing member 40. The nonaqueous electrolyte prepared in (4) above was injected into the battery case 20 at 2.5 μL per 1 mAh of discharge capacity. The sealing member 40 was placed in the opening of the battery case 20, and the opening edge of the battery case 20 was crimped to the peripheral edge of the sealing member 40 via the gasket 30 to seal the opening. A butyl rubber-based insulating paint was applied in a doughnut shape to cover the outer surface of the opening edge of the bent battery case 20 and the surface of the gasket 30, forming a second insulating ring 50B. In this way, a cylindrical lithium secondary battery 100 (battery A1) with a rated capacity of 45 mAh was obtained.

[0101] Comparative Example 1 In the production of the electrode group 10, the reverse running portion 12A was not provided on the negative electrode 12, and the positive electrode 11 and the negative electrode 12 were wound with the separator 13 interposed therebetween to form the electrode group 10. A cylindrical lithium secondary battery (battery B1) was produced in the same manner as in Example 1 except for this.

[0102] Example 2 In the preparation of the negative electrode, a negative electrode active material was prepared by mixing silicon oxide (SiO) particles and graphite with a mass ratio of 10:90, sodium carboxymethyl cellulose (CMC-Na), styrene butadiene rubber (SBR), and lithium polyacrylate with a mass ratio of 96.5:1:1.5:1, and water was added as a dispersion medium to prepare a negative electrode slurry. The negative electrode slurry was applied to both sides of a copper foil (thickness: 10 μm) serving as a negative electrode current collector, dried, and then compressed in the thickness direction to obtain a negative electrode 12 having a negative electrode composite layer on the surface of the negative electrode current collector. However, the negative electrode slurry was not applied to the region of the negative electrode 12 that would become the reverse-running portion 12A, leaving the negative electrode current collector exposed.

[0103] In preparing the non-aqueous electrolyte, LiPF was dissolved in a mixed solvent containing ethylene carbonate (EC) and diethyl carbonate (DEC) in a mass ratio of 30:70. 6 was dissolved in the solution at a concentration of 1.0 mol / L to obtain a non-aqueous electrolyte. A cylindrical lithium ion secondary battery (battery A2) was fabricated in the same manner as in Example 1 except for this.

[0104] Comparative Example 2 In the production of the electrode group 10, the reverse running portion 12A was not provided on the negative electrode 12, and the positive electrode 11 and the negative electrode 12 were wound with the separator 13 interposed therebetween to form the electrode group 10. A cylindrical lithium-ion secondary battery (battery B2) was produced in the same manner as in Example 2 except for this.

[0105] (Evaluation) For the batteries fabricated in each example, the capacity retention rate (100 cycles) and the expansion rate of the negative electrode were determined according to the following procedure.

[0106] (Capacity Retention Rate) The battery was charged at a constant current of 0.1 It until the closed-circuit voltage reached 4.2 V, and then constant-voltage charged until the current reached 0.05 It at 4.2 V. After a 20-minute break, the battery was discharged at a constant current of 0.1 It until the closed-circuit voltage reached 3.0 V. This cycle was repeated 100 times. The ratio (%) of the discharge capacity at the 100th cycle to the discharge capacity at the first cycle was calculated as the capacity retention rate.

[0107] (Negative Electrode Expansion Rate) Two samples of each battery were prepared. One battery was charged at a constant current of 0.1 It until the closed circuit voltage reached 4.2 V (SOC 100%), and then constant voltage charged at 4.2 V until the current reached 0.05 It. After charging, the battery was disassembled to remove the negative electrode, and the thickness T1 of the negative electrode was measured using the method described above.

[0108] The other battery was discharged at a constant current of 0.1 It until the closed-circuit voltage reached 3.0 V (SOC 0%). After discharging, the battery was disassembled to remove the negative electrode, and the thickness T0 of the negative electrode was determined by the method described above. The negative electrode expansion rate (%) was evaluated as (T1 / T0) × 100.

[0109] Table 1 shows the evaluation results of the capacity retention rate and the negative electrode expansion rate for the examples and comparative examples.

[0110]

[0111] As shown in Table 1, batteries A1 and B1 had a negative electrode expansion rate of 140%, which means that the electrode is susceptible to deformation due to negative electrode expansion, and battery performance is likely to deteriorate due to electrode deformation. However, battery A1 had an improved capacity retention rate compared to battery B1. This is thought to be because the provision of the reverse running section in battery A1 suppressed electrode deformation due to negative electrode expansion, thereby suppressing the deterioration of battery performance due to electrode deformation and allowing the battery to maintain a high capacity retention rate.

[0112] In a comparison of Batteries A2 and B2, which have a negative electrode expansion rate of 120%, Battery A2 also has an improved capacity retention rate compared to Battery B2. This is also thought to be because, as with Battery A1, the provision of the reverse running portion in Battery A2 suppressed electrode deformation due to negative electrode expansion.

[0113] The present disclosure is suitable for cylindrical lithium secondary batteries (particularly pin-type secondary batteries) and can be suitably used as a power source for various portable electronic devices that require a small power source, such as eyeglasses (such as 3D eyeglasses), hearing aids, stylus pens, and wearable devices.

[0114] While the present invention has been described in terms of presently preferred embodiments, such disclosure is not to be interpreted as limiting. Various changes and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. It is therefore intended that the appended claims be interpreted to cover all changes and modifications that do not depart from the true spirit and scope of the invention.

[0115] 10: Wound electrode group 11: Positive electrode 12: Negative electrode 12A: Reverse running portion 13: Separator 20: Battery case 30: Gasket 40: Sealing member 40a: Brim 40b, 40c: Terminal portion 50A: First insulating ring 50B: Second insulating ring 60: Positive electrode current collecting lead 70: Negative electrode current collecting lead 70a: Welding point 100: Cylindrical secondary battery

Claims

1. a wound electrode group in which a positive electrode and a negative electrode are wound in a winding direction with a separator interposed therebetween; A non-aqueous electrolyte secondary battery comprising: the negative electrode has a reverse running portion at an end portion on a winding start side of the wound electrode group, the reverse running portion not facing the positive electrode and wound in a direction opposite to the winding direction.

2. The nonaqueous electrolyte secondary battery according to claim 1 , wherein the reverse running portion is wound in the opposite direction by 0.5 to 1.25 turns.

3. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein an expansion coefficient expressed as a ratio of a thickness of said negative electrode at an SOC of 100% to a thickness of said negative electrode at an SOC of 0% is 108% or more.

4. 4. The nonaqueous electrolyte secondary battery in accordance with claim 3, wherein the expansion rate is 120% or more.

5. 4. The nonaqueous electrolyte secondary battery in accordance with claim 3, wherein the expansion rate is 140% or more.

6. 6. The nonaqueous electrolyte secondary battery according to claim 1, wherein the inner diameter of the wound electrode group is 5 mm or less.

7. 7. The nonaqueous electrolyte secondary battery in accordance with claim 6, wherein the inner diameter is 2.5 mm or less.