Silicon particles, composite active material for secondary batteries, secondary battery, method for producing silicon particles, and method for producing composite active material for secondary batteries

JPWO2024101262A5Inactive Publication Date: 2024-10-09
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024515880
Authority / Receiving Office
JP · JP
Patent Type
Applications
Filing Date
2024-03-12
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Silicon-based active materials for lithium-ion batteries suffer from poor charge/discharge performance due to the formation of a solid electrolyte interface layer, leading to decreased capacity retention and initial Coulombic efficiency, caused by the vigorous electrochemical reaction between silicon particles and the electrolyte during repeated charging and discharging.

Method used

The application of a film-like or particulate silicon nitride or silicon carbide phase, catalyzed by a transition metal element such as Mn, Fe, or Ni, on the surface of silicon particles to enhance chemical durability and reduce the formation of the solid electrolyte interface layer, thereby maintaining high charge/discharge performance.

Benefits of technology

The silicon particles with a silicon nitride or silicon carbide phase and transition metal elements exhibit improved chemical durability and retention of high charge/discharge performance, including capacity retention rate and initial Coulombic efficiency, by suppressing the formation of the solid electrolyte interface layer.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The purpose of the present invention is to provide: silicon particles which are suppressed in disintegration and enables a secondary battery, if used therein, to maintain high charge and discharge performance including capacity retention rate and initial coulombic efficiency; a composite active material for secondary batteries; and a secondary battery which comprises this composite active material for secondary batteries. Silicon particles according to the present invention each have a silicon nitride phase and / or a silicon carbide phase in the surface, while containing a transition metal element. It is preferable that the transition metal element is at least one element that is selected from the group consisting of Fe, Mn, Ni, Cr, Cu, Nb, Mo, Ru, Rh, Pd and La.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon particles, composite active material for secondary battery, secondary battery, method for manufacturing silicon particles, and method for manufacturing composite active material for secondary battery

[0001] The present invention relates to silicon particles, a composite active material for secondary batteries containing the silicon particles, and a secondary battery containing the composite active material for secondary batteries. The present invention also relates to methods for producing the silicon particles and the composite active material for secondary batteries.

[0002] In response to environmental concerns about energy demand, the deployment of electric vehicles (EVs) is rapidly progressing, expanding the scope of use of lithium-ion batteries (LIBs). Graphite, the mainstream LIB anode material, has a low theoretical capacity density (372 mAh / g). To improve battery capacity, active materials using silicon, tin, and oxides have been actively developed. However, these materials undergo large volume expansion and contraction upon absorption and desorption of lithium ions, resulting in the active material becoming pulverized with repeated charge / discharge cycles, which leads to poor charge / discharge characteristics.

[0003] Patent Document 1 describes a negative electrode material for a lithium ion secondary battery that includes a carbon material and flaky silicon particles, in which at least a portion of the surface of the flaky silicon particles is coated with an oxide film or a thin graphite film, and the flaky silicon particles are dispersed in the carbon material to form a particle shape as a whole.

[0004] Patent Document 2 describes that composite particles in a negative electrode material for a lithium secondary battery are formed by coating the surfaces of silicon particles with a carbide layer, and voids are formed inside the carbide layer.

[0005] In Patent Document 3, a composite negative electrode active material includes a coating layer disposed on a silicon material core, and the coating layer contains a water-soluble polymer and F - , P.O. 4 3- , P.F. 6- , B.O. 3 3- and BF 4- It is disclosed that the composition comprises a water-insoluble polymer complex to which one or more anionic components selected from the group consisting of the following are chemically bonded, and that the lifespan characteristics are improved.

[0006] Japanese Patent Publication No. 2018-113187 Japanese Patent Publication No. 2017-69165 Japanese Patent Publication No. 2017-63026

[0007] However, in the case of the active materials containing silicon particles described in Patent Documents 1 to 3, repeated charge and discharge cycles cause the electrochemical reaction between the silicon particles and the electrolyte to proceed vigorously, resulting in the continued formation of a solid electrolyte interface (SEI) layer on the surface of the silicon particles, which causes a problem of a decrease in both the initial coulombic efficiency and the charge and discharge capacity due to the large amount of lithium ion consumption. As a result, the capacity retention rate of the active material may gradually decrease, and further improvements are required in terms of the battery's cycle characteristics and initial coulombic efficiency.

[0008] An object of the present invention is to provide silicon particles and a composite active material for a secondary battery that can suppress the formation of an SEI layer on the silicon particles and maintain high charge-discharge performance, such as capacity retention and initial coulombic efficiency, when used in a secondary battery, as well as a secondary battery containing the composite active material for a secondary battery.An object of the present invention is also to provide methods for producing the silicon particles and the composite active material for a secondary battery.

[0009] The present inventors believed that the silicon particles described in the above Patent Documents 1 to 3 lacked sufficient chemical durability on the silicon particle surface, resulting in insufficient charge / discharge performance when used in secondary batteries, and therefore investigated methods for improving the chemical durability of the silicon particle surface. As a result, the present inventors found that by supporting a transition metal element on silicon particles, it is possible to impart a film-like or particulate silicon nitride phase or silicon carbide phase to the silicon particle surface through the catalytic action of the element, thereby improving chemical durability.

[0010] The present invention has the following aspects. [1] Silicon particles having a silicon nitride phase and / or silicon carbide phase on the surface and containing a transition metal element. [2] Silicon particles according to [1], wherein the transition metal element is at least one selected from the group consisting of Fe, Mn, Ni, Cr, Cu, Nb, Mo, Ru, Rh, Pd, and La. [3] Silicon particles according to [1] or [2], wherein the transition metal element is Mn. [4] Silicon particles according to any one of [1] to [3], wherein the content of the transition metal element is 0.01 atm % to 5 atm % relative to the total amount of silicon present in the silicon particles. [5] Solid 29

[0023] The silicon particles according to any one of [1] to [4], wherein a Si-NMR spectrum detects a peak A in the chemical shift range of 0 ppm to -20 ppm, which is attributable to a silicon carbide phase, a peak B in the chemical shift range of -30 ppm to -60 ppm, which is attributable to a silicon nitride phase, and a peak C in the chemical shift range of -70 ppm to -100 ppm, which is attributable to silicon, and the area ratio R of the peaks calculated by the following formula (1) is in the range of 0.1 to 1.0: R = (A + B) / C (1) [6] The silicon particles according to any one of [1] to [5], wherein a peak is detected near 2θ = 28.4° in XRD measurement. [7] The silicon particles according to any one of [1] to [6], further comprising an amorphous oxide film present on the surface, the thickness of which is 8 nm or less. [8] A method for producing silicon particles, comprising at least the steps of wet-pulverizing raw silicon under conditions in which a dispersant is added, supporting a transition metal element-containing compound on the surface of the pulverized raw silicon, and performing high-temperature treatment in a non-oxidizing atmosphere at a temperature range of 900°C to 1300°C. [9] A method for producing a composite active material for secondary batteries, comprising the method for producing silicon particles according to [8].

[10] A composite active material for secondary batteries, comprising silicon particles according to any one of [1] to [7].

[11] The composite active material for secondary batteries according to

[10] , wherein the silicon particles have an average particle size in the range of 10 nm to 300 nm.

[12] A secondary battery, comprising in its negative electrode the composite active material for secondary batteries according to

[10] or

[11] .

[0011] The silicon particles of the present invention have improved chemical durability on the particle surface, and can maintain high charge-discharge performance such as capacity retention rate and initial coulombic efficiency in secondary batteries.

[0012] The present invention will be described below, but the present invention is not limited by the examples in the following description. In this specification, the term "to" indicating a numerical range includes the upper and lower limits. In this specification, "A and / or B" means either A or B, or both. Furthermore, in this specification, a ratio (percentage, etc.) based on mass is the same as a ratio (percentage, etc.) based on weight.

[0013] [Silicon Particles] The silicon particles of the present invention have a silicon nitride phase and / or a silicon carbide phase on their surfaces and contain a transition metal element (hereinafter referred to as "silicon particles of the first embodiment"). The silicon particles of the first embodiment are not simply composed of elemental Si, but have a structure comprising silicon particles and a silicon nitride phase and / or a silicon carbide phase formed on their surfaces. The silicon nitride phase and / or the silicon carbide phase may be present continuously or intermittently on the surfaces of the silicon particles. That is, the silicon particles of the first embodiment have a portion or all of their surfaces covered with the silicon nitride phase and / or the silicon carbide phase. By making the silicon particles have a silicon nitride phase and / or a silicon carbide phase on their surfaces, chemical durability can be improved, and charge / discharge performance such as capacity retention and initial coulombic efficiency can be improved when applied to secondary batteries.

[0014] The silicon particles of the first embodiment support a transition metal element. The transition metal element may be present in a silicon nitride phase or silicon carbide phase on the surface of the silicon particle, or may be present in the interior of the silicon particle.

[0015] The transition metal element in the silicon particles of the first embodiment is preferably at least one element selected from the group consisting of Fe, Mn, Ni, Cr, Cu, Nb, Mo, Ru, Rh, Pd, and La, and particularly preferably Mn, because it is likely to have a catalytic action and effectively form a silicon nitride phase or a silicon carbide phase on the surface of the silicon particles. The transition metal element is considered to exist in the state of metal ions. In other words, when the transition metal element is Mn, Mn 2+It is thought to exist as

[0016] The content of the transition metal element is preferably 0.01 atm% to 5 atm%, more preferably 0.05 atm% to 4 atm%, and even more preferably 0.1 atm% to 3 atm%, relative to the total amount of silicon (Si element) present in the silicon particles of the present invention. When the content of the transition metal element is within the above range, catalytic action is likely to occur, and silicon nitride phases and silicon carbide phases are likely to be effectively formed on the surfaces of the silicon particles. The content of the transition metal element can be measured by various quantitative element content analyses of the silicon particles, such as ICP mass (inductively coupled plasma mass) analysis, energy dispersive X-ray fluorescence (EDX) analysis, X-ray fluorescence (XRF) analysis, and EPMA (electron probe microanalyzer) analysis.

[0017] The silicon nitride phase on the surface of the silicon particles of the first embodiment is an inorganic compound represented by the chemical formula SiNx (0.1≦x≦1.33), and has electrochemical reactivity with lithium ions, as well as excellent fracture toughness, high-temperature properties, and thermal shock resistance. 3 N 4 The crystalline body may be either an α-phase or a β-phase, as an example of the silicon nitride phase (x=1.33).

[0018] Silicon nitride phases are structures formed by solid-state reactions at high temperatures (e.g., 1200°C or higher), but they can also be easily formed at lower temperatures due to the catalytic effect of transition metal ions. The composition and crystalline state of the silicon nitride phase can be appropriately controlled by changing the type and amount of transition metal ions added and the solid-state reaction conditions. Furthermore, a native oxide film is typically present on silicon particles. During high-temperature firing, transition metal ions can diffuse through this native oxide film, causing a catalytic effect that significantly accelerates the nitridation reaction of silicon. As a result, silicon nitride crystals can form between the surface oxide film and the silicon crystals at the center of the particles, blocking contact between the silicon crystals and oxygen from outside the silicon or from the surrounding area, thereby suppressing oxidation reactions on the silicon particle surface.

[0019] Silicon carbide in the silicon carbide phase is represented by the chemical formula SiC, and is a compound of carbon and silicon in a 1:1 ratio. It has properties intermediate between those of diamond and silicon, and has excellent hardness, heat resistance, and chemical stability.

[0020] In the silicon particles of the first embodiment, the shape of the silicon nitride phase and / or silicon carbide phase is not particularly limited, and examples thereof include needle-like, particulate, film-like, etc. From the viewpoint of suppressing oxidation reaction on the silicon particle surface, it is preferable that the silicon nitride phase and / or silicon carbide phase be in the form of a film or particulate on the silicon particle surface.

[0021] The silicon particles of the present invention are solid 29 In the Si-NMR spectrum, a peak A in the chemical shift range of 0 ppm to -20 ppm, which is attributable to the silicon carbide phase, a peak B in the chemical shift range of -30 ppm to -60 ppm, which is attributable to the silicon nitride phase, and a peak C in the chemical shift range of -70 ppm to -100 ppm, which is attributable to silicon, are detected, and the area ratio R of the above peaks calculated by the following formula (1) is in the range of 0.1 to 1.0 (hereinafter referred to as "silicon particles of the second embodiment"). R=(A+B) / C (1)

[0022] In the silicon particles of the second embodiment, there is no particular limitation on the structure of the silicon nitride phase or silicon carbide phase, and both crystalline and amorphous structures are applicable. The silicon nitride phase or silicon carbide phase can be in a solid state regardless of whether it is in a crystalline state or an amorphous state. 29This can be confirmed by Si-NMR spectroscopy. Peaks A and B are Si-C and Si-N, respectively, composed of non-zero valent Si elements, and peak C is zero valent Si. The area ratio R of each peak calculated by formula (1) being within the above range means that the proportion of Si (zero valent) is higher than Si (non-zero valent), which indicates that oxidation has not progressed in the silicon particles of the second embodiment (they are in a low oxidation state). The low oxygen state of the silicon particles can effectively improve the initial Coulomb efficiency when used as a negative electrode active material. Furthermore, the presence of a silicon nitride phase or silicon carbide phase on the surface of the silicon particles increases the chemical stability of the silicon particles and improves their cycle characteristics during charge and discharge. The area ratio R of each peak calculated by formula (1) is more preferably within the range of 0.1 to 1.0, even more preferably within the range of 0.2 to 0.9, even more preferably within the range of 0.25 to 0.8, and particularly preferably within the range of 0.3 to 0.7.

[0023] Furthermore, if the silicon nitride phase or silicon carbide phase is in a crystalline state, it can be confirmed by XRD (X-ray diffraction, CuKα light source) measurement. 3 N 4 (PDF#41-0360), β-Si 3 N 4 When X-ray diffraction peaks consistent with those of silicon nitride (PDF#33-1160), α-SiC (PDF#49-1430), and β-SiC (PDF#29-1129) are detected within the 2θ range of 10° to 80°, it is determined that the various crystalline structures of silicon nitride and silicon carbide are present.

[0024] The silicon particles of the present invention preferably exhibit a peak detected at around 2θ=28.4° in XRD (X-ray diffraction) measurement. Detection of this peak indicates the presence of Si crystalline bodies having a major crystal face (111). The Si crystalline bodies have the property of being able to exhibit high charge / discharge performance, particularly in secondary batteries, such as charge / discharge capacity and initial coulombic efficiency.

[0025] The total thickness of the silicon nitride phase and silicon carbide phase present on the surface of the silicon particles is preferably 0.1 nm to 10 nm, more preferably 0.3 nm to 8 nm, and particularly preferably 0.5 nm to 6 nm. This thickness range can impart excellent fracture toughness, high-temperature properties, thermal shock resistance, and chemical stability to the silicon particle surface, and can suppress the collapse of the silicon particles due to charging and discharging. This thickness can be measured by cutting the sample with a focused ion beam (FIB) and observing the cross section with an FE-SEM, or by slicing the sample and observing the cross section of the silicon particles with a TEM.

[0026] The average particle size of the silicon particles of the present invention is preferably in the range of 10 nm to 300 nm, more preferably 30 nm to 250 nm, and even more preferably 50 nm to 200 nm. When the average particle size of the silicon particles is in this range, collapse of the silicon particles can be suppressed, and high charge / discharge performance such as capacity retention rate and initial coulombic efficiency in the secondary battery can be maintained. In this specification, the "average particle size" refers to the D50 value, which can be measured using a laser diffraction particle size analyzer or the like. In other words, when a volume cumulative distribution curve is drawn from the small diameter side in the particle size distribution, the particle size at which the cumulative 50% is reached is the average particle size.

[0027] The specific surface area of ​​the silicon particles of the present invention is 50 m from the viewpoint of charge / discharge capacity, initial coulomb efficiency, and cycle characteristics. 2 / g~400m 2 / g is preferred, and 100m 2 / g to 300m 2 / g is more preferred, and 150m 2 / g~230m 2 / g is more preferable. In this specification, the "specific surface area" is a value determined by the BET method, and can be determined by nitrogen gas adsorption measurement, for example, using a specific surface area measuring device. In addition, in order to remove organic deposits on the silicon particles, it is preferable to perform a heat treatment at 500°C for 2 hours in a nitrogen atmosphere before measuring the specific surface area.

[0028] The silicon particles may be granular, needle-like, or flake-like in shape, or may be crystalline, but are preferably crystalline. When the silicon particles are crystalline, a crystallite diameter obtained from the diffraction peak attributed to Si (111) in X-ray diffraction is preferably in the range of 5 nm to 14 nm from the viewpoint of initial Coulomb efficiency and cycle characteristics. The crystallite diameter is preferably 12 nm or less, and more preferably 10 nm or less.

[0029] From the viewpoint of charge / discharge performance when used as a composite active material for a secondary battery, the silicon particles of the present invention preferably have a length in the major axis direction of 30 nm to 300 nm and a thickness of 1 nm to 60 nm. From the viewpoint of charge / discharge performance when used as a negative electrode active material, a needle-like or flake-like shape with an aspect ratio (length-to-thickness ratio) of 0.5 or less is preferred. The morphology of silicon particles can be measured by dynamic light scattering to measure the average particle size, but the aspect ratio of a sample can be more easily and precisely identified by using analytical tools such as a transmission electron microscope (TEM) or a field emission scanning electron microscope (FE-SEM). In the case of silicon particles of the present invention, a sample can be cut with a focused ion beam (FIB) and the cross section can be observed with an FE-SEM, or the sample can be sliced ​​and the state can be identified by TEM observation. The aspect ratio of the silicon particles is a calculation result based on the major portion of 50 particles of the sample within the field of view of the TEM image.

[0030] The silicon particles of the present invention preferably further have an amorphous oxide film on at least a portion of the outer surface. The amorphous oxide film is an oxide film in an amorphous state, preferably an oxide film of silicon (Si), particularly preferably SiO 2 When such an amorphous oxide film is present on at least a portion of the outer surface of silicon particles having a silicon nitride phase and / or a silicon carbide phase on the surface, the silicon particle surface can be endowed with superior fracture toughness, high-temperature characteristics, thermal shock resistance, and chemical stability without significantly adversely affecting charge / discharge performance (capacity, initial coulombic efficiency), and collapse of the silicon particles due to charge / discharge can be suppressed. The amorphous oxide film can be formed on the surface of the silicon particles by an oxidation reaction during high-temperature firing.

[0031] The thickness of the amorphous oxide film is preferably 8 nm or less, more preferably 1 nm to 7 nm, and particularly preferably 2 nm to 6 nm, from the viewpoint of achieving a good balance between the effects (positive and negative) resulting from the amorphous oxide film. When the thickness is within this range, the extent of deterioration in the charge / discharge performance of the silicon particles (capacity and initial coulombic efficiency) can be minimized, and cycle characteristics can be improved by suppressing silicon particle collapse during charge / discharge. The formation and thickness of the amorphous oxide film can be confirmed by TEM observation. The thickness of the amorphous oxide film is the average value measured at three locations.

[0032] [Composite active material for secondary batteries] The composite active material for secondary batteries of the present invention is not particularly limited as long as it contains the silicon particles, but in addition to the silicon particles, it may also contain, for example, carbon or a silicon-based material. Among these, it is preferable that the composite active material for secondary batteries of the present invention contains a silicon-based material. The silicon particles alone serve as an active material for secondary batteries and act as lithium storage sites that repeatedly insert and extract lithium ions and the like during charge and discharge. However, by including a silicon-based material, it is possible to suppress the expansion of the silicon particles, maintain the electrode structure, and improve stability.

[0033] A silicon-based material contains silicon, carbon, and oxygen elements and has a three-dimensional network structure of a silicon-oxygen-carbon skeleton. Preferably, the silicon-based material further contains carbon (carbonaceous phase). The three-dimensional network structure of a silicon-oxygen-carbon skeleton has relatively high chemical stability, and by forming a composite structure with carbon (carbonaceous phase), it is possible to reduce the volume change due to the absorption and desorption of lithium. Note that the silicon-based material may contain nitrogen element in addition to silicon, carbon, and oxygen elements.

[0034] The average particle size of the silicon particles in the composite active material for a secondary battery of the present invention is preferably in the range of 10 nm to 300 nm, more preferably 30 nm to 250 nm, and even more preferably 50 nm to 200 nm. When the average particle size of the silicon particles is in this range, collapse of the Si particles tends to be suppressed, and charge / discharge performance such as cycle characteristics and initial coulombic efficiency in the secondary battery tends to be maintained at a high level.

[0035] The composite active material for secondary batteries preferably has a carbon coating on at least a portion of its surface. From the viewpoint of process feasibility, a carbon coating made of low-crystalline carbon is preferred. Unlike graphitic carbon materials, low-crystalline carbon refers to an amorphous carbon material in which a lattice period-ordered structure is rarely observed or only a trace amount of short-period structure is present. From the viewpoint of improving chemical stability and thermal stability, the amount of the carbon coating is preferably 0.1% by mass to 30% by mass, more preferably 1% by mass to 25% by mass, and even more preferably 5% by mass to 20% by mass, based on 100% by mass of the composite active material for secondary batteries. Furthermore, from the viewpoint of improving chemical stability and thermal stability, the average thickness of the carbon coating is preferably 10 nm to 300 nm. The amount of the carbon layer (carbon coating) can be measured by thermal analysis.

[0036] The composite active material for secondary batteries preferably has a carbon coating on at least a portion of its surface, more preferably on 1% or more, and even more preferably on 10% or more of the surface of the composite active material from the viewpoint of improving chemical stability and thermal stability. The composite active material for secondary batteries may have the carbon coating on its surface continuously or intermittently. The carbon coating is preferably formed on the surface of the composite active material by chemical vapor deposition.

[0037] The true density of the composite active material for secondary batteries is 1.6 g / cm 3 2.0g / cm or more 3 When the true density is within the above range, the energy density of the resulting secondary battery can be improved. 3 More preferably, 1.80 g / cm 3 The above is more preferable. The true density is a value measured using a true density measuring device.

[0038] The average particle size of the composite active material for secondary batteries is preferably 2 μm or more and 15 μm or less. If the average particle size of the composite active material for secondary batteries is 2 μm or more, a significant increase in the specific surface area can be suppressed, and when used as a secondary battery, the generation of SEI during charge and discharge can be suppressed, and a decrease in the reversible charge and discharge capacity per unit volume can be suppressed. Furthermore, if the average particle size is 15 μm or less, peeling from the current collector during electrode film production can be suppressed. The average particle size of the composite active material for secondary batteries is more preferably 2.5 μm or more, and even more preferably 3.0 μm or more. Furthermore, the average particle size of the composite active material for secondary batteries is more preferably 12 μm or less, and even more preferably 10 μm or less.

[0039] The specific surface area of ​​the composite active material for secondary batteries is 0.3 m 2 / g or more 10m 2 / g or less. The specific surface area is preferably 0.5 m 2 / g or more is more preferable, and 1.0m 2 When the specific surface area is in the above range, the amount of solvent absorbed during electrode production can be kept appropriate, and the amount of binder used to maintain binding properties can also be kept appropriate.

[0040] [Method for producing silicon particles] The method for producing silicon particles of the present invention includes at least a step of wet-pulverizing raw silicon under conditions in which a dispersant is added (wet-pulverization step), a step of supporting a transition metal element-containing compound on the surface of the pulverized raw silicon (transition metal element supporting step), and a step of performing high-temperature treatment in a non-oxidizing atmosphere at a temperature range of 900° C. to 1300° C. (high-temperature treatment step). Note that the above-mentioned silicon particles of the present invention are not limited to those obtained by the method for producing silicon particles of the present invention.

[0041] <Wet-milling step> In the wet-milling step, raw silicon is dispersed in a solvent such as an organic solvent to obtain a silicon slurry, which is a silicon dispersion liquid. The silicon slurry is obtained by adjusting the raw silicon while pulverizing it in a wet-milling device. In the present invention, a dispersant is added to the organic solvent to promote the pulverization of the raw silicon. Examples of wet-milling devices include a roller mill, a high-speed rotary mill, a container-driven mill, and a bead mill. The preferred average particle size of the pulverized raw silicon in the obtained silicon slurry is the same as the average particle size of the silicon particles described above in [Composite active material for secondary batteries].

[0042] Examples of the organic solvent include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and diisobutyl ketone; alcohols such as ethanol, methanol, normal propyl alcohol, and isopropyl alcohol; and aromatics such as benzene, toluene, and xylene.

[0043] The type of the dispersant can be aqueous or non-aqueous dispersant, and non-aqueous dispersant is preferred.The type of non-aqueous dispersant can be exemplified by polymer type such as polyether type, alcohol type, polyalkylene polyamine type, polycarboxylic acid partial alkyl ester type, low molecular type such as polyhydric alcohol ester type, alkyl polyamine type, and inorganic type such as polyphosphate type.The concentration of the solid content of raw material silicon in silicon slurry is not particularly limited, but is preferably in the range of 5 mass% to 40 mass%, more preferably 10 mass% to 30 mass%, with the total amount of organic solvent, dispersant and raw material silicon being 100 mass%.

[0044] <Transition Metal Element Supporting Step> In the transition metal element supporting step, a transition metal element-containing compound is added to the silicon slurry obtained in the wet grinding step, followed by stirring, and the solvent is removed and then drying. This allows the transition metal element to be supported on the pulverized raw silicon. The transition metal element-containing compound is preferably a salt of at least one transition metal element selected from the group consisting of Fe, Mn, Ni, Cr, Cu, Nb, Mo, Ru, Rh, Pd, and La. Examples of salts include inorganic salt compounds such as sulfates, hydrochlorides, acetates, and carbonates, as well as organic salt compounds such as acetate anhydrides and acetylacetonate ligand compounds. That is, for example, when the transition metal element is manganese (Mn), examples of the transition metal element-containing compound include manganese(II) chloride, manganese(II) acetate anhydride, manganese(II) sulfate, manganese(II) acetate, and manganese(II, III) acetylacetonate. The metal element-containing compound may be added by dispersing it in an organic solvent (polar or nonpolar).

[0045] The stirring can be carried out using a stirrer equipped with stirring blades, and the stirring time is, for example, 5 minutes to 2 hours, preferably 10 minutes to 1 hour. The stirring can be carried out at room temperature, or while heating to about 30 to 50°C. The solvent can be removed by a conventional method such as filtration. The drying can be carried out using, for example, a dryer, a reduced pressure dryer, or a spray dryer. The drying temperature is preferably 80°C or higher and 120°C or lower. Drying can also be carried out under reduced pressure.

[0046] <High-Temperature Treatment Step> In the high-temperature treatment step, the pulverized raw silicon supporting the transition metal element obtained in the transition metal element supporting step is fired in a non-oxidizing atmosphere. The equipment used for the high-temperature treatment can be selected appropriately depending on the purpose, such as a fluidized bed reactor, a rotary furnace, a vertical moving bed reactor, a tunnel furnace, a batch furnace, or a rotary kiln. The high-temperature treatment is carried out according to a firing program defined by the temperature rise rate, the holding time at a constant temperature, and the like. The firing temperature preferably has a maximum temperature in the range of 900 to 1300°C, for example. This allows the silicon particles of the present invention to be obtained.

[0047] The non-oxidizing atmosphere during the high-temperature firing refers to an atmosphere having an oxygen concentration of 100 ppm or less. There are no particular limitations on the type of gas used as the non-oxidizing atmosphere, and examples include nitrogen, argon, hydrogen, and a nitrogen-hydrogen mixed gas. Among these, nitrogen gas is preferred from the viewpoint of promoting silicon nitride formation.

[0048] Furthermore, the fired product obtained in the high-temperature treatment step is pulverized and, if necessary, classified to obtain silicon particles of the desired particle size. The pulverization may be carried out in one step until the desired particle size is reached, or may be carried out in several steps. If the silicon particles after firing are lumps or agglomerates with a particle size of 10 mm or more, they may be coarsely pulverized using a jaw crusher, roll crusher, or the like, then pulverized using a glow mill, ball mill, or the like, and further pulverized using a bead mill, jet mill, or the like. The particle size is the average particle size, and is the D50 value.

[0049] Furthermore, if the silicon particles produced by pulverization contain coarse particles, it is preferable to remove them and fine powder to adjust the particle size distribution by performing classification. The classifier used may be an air classifier, a wet classifier, or the like, depending on the purpose, but when removing coarse particles, a classification method using a sieve is preferable because it can reliably achieve the purpose.

[0050] [Method of Manufacturing a Composite Active Material for Secondary Batteries] The method of manufacturing a composite active material for secondary batteries of the present invention is not particularly limited as long as it includes the method of manufacturing silicon particles described above, but may include a homogenization step before the high-temperature treatment step and after the wet-pulverization step, and before or after the transition metal element supporting step. This homogenization step is a step when the composite active material for secondary batteries contains a silicon-based material having a matrix structure containing carbon element as a main component. In this case, in the method of manufacturing a composite active material for secondary batteries of the present invention, an active material precursor containing a pulverized carbon-based material and raw material silicon is subjected to the high-temperature treatment step.

[0051] In the homogenization step, the carbon source resin and the silicon slurry obtained in the wet pulverization step are mixed uniformly, and then the solvent is removed and the mixture is dried.

[0052] The carbon source resin can be carbonized by high-temperature calcination in a non-oxidizing atmosphere and used as the carbon material in the method for producing a composite active material for a secondary battery of the present invention. The carbon source resin or the resin contained in the carbon source resin composition is not particularly limited, as long as it contains a molecular structure having a benzene ring or an aromatic functional group. Examples include thermosetting resins; thermoplastic resins; petroleum-based or coal-based tar or pitch, such as petroleum tar or pitch produced as a by-product during ethylene production, coal tar produced during coal carbonization, heavy components or pitch obtained by distilling off low-boiling components of coal tar, and tar or pitch obtained by coal liquefaction; and crosslinked versions of the above tar or pitch. These resins can be used alone or in combination.

[0053] The thermosetting resin is not particularly limited, and examples thereof include phenolic resins such as novolac phenolic resins and resol phenolic resins; epoxy resins such as bisphenol epoxy resins and novolac epoxy resins; melamine resins; urea resins; aniline resins; cyanate resins; furan resins; ketone resins; unsaturated polyester resins; and urethane resins. Modified versions of these resins with various components can also be used. When a thermosetting resin is used, a curing agent for the resin can be used in combination.

[0054] The thermoplastic resin is not particularly limited, and examples thereof include polyethylene, polystyrene, polyacrylonitrile, acrylonitrile-styrene (AS) resin, acrylonitrile-butadiene-styrene (ABS) resin, polypropylene, vinyl chloride, methacrylic resin, polyethylene terephthalate, polyamide, polycarbonate, polyacetal, polyphenylene ether, polybutylene terephthalate, polyphenylene sulfide, polysulfone, polyethersulfone, polyetheretherketone, polyetherimide, polyamideimide, polyimide, and polyphthalamide.

[0055] In the method for producing a composite active material for a secondary battery according to the present invention, the resin or resin composition used as the raw material for the carbon material preferably contains a nitrogen-containing resin as the main component resin in order to promote silicon nitride formation. Carbonizing such a resin enhances the catalytic activity of the transition metal ions in the formation of nitrogen compounds, and also allows the production of a nitrogen-containing carbon material. When nitrogen is contained in the carbon, the electronegativity of nitrogen can impart favorable electrical properties to the carbon (carbon material for a lithium-ion secondary battery). This promotes the absorption and release of lithium ions, resulting in excellent charge / discharge characteristics.

[0056] Examples of the nitrogen-containing resins include the following: Thermosetting resins include melamine resins, urea resins, aniline resins, cyanate resins, and urethane resins, as well as phenolic resins and epoxy resins modified with a nitrogen-containing component such as an amine.

[0057] Furthermore, when a nitrogen-containing compound is used as a component other than the main component resin, the type of compound is not particularly limited. For example, hexamethylenetetramine, which is a curing agent for novolac phenolic resin, aliphatic polyamines, aromatic polyamines, dicyandiamide, and the like, which are curing agents for epoxy resins, as well as nitrogen-containing compounds such as amine compounds, ammonium salts, nitrates, and nitro compounds, which do not function as curing agents, can be used in addition to the curing agent component.

[0058] The nitrogen-containing compound may be used alone or in combination of two or more types, whether or not the main component resin contains nitrogen-containing resins.

[0059] The method for preparing the resin composition used as the raw material for the carbon material in the method for producing a composite active material for a secondary battery of the present invention is not particularly limited. Examples of the preparation method include blending the above-mentioned main component resin and other components in a predetermined ratio, dissolving these components in a solvent, and mixing them, or mixing these components with the above-mentioned silicon slurry to prepare a precursor for the composite active material for a secondary battery of the present invention.

[0060] A transition metal element-containing compound is added to the silicon slurry obtained in the wet grinding step, followed by stirring, and the solvent is removed and then the mixture is dried to carry out a transition metal element supporting step. After that, a carbon source resin is added and the mixture is stirred. This produces an active material precursor containing the carbon source resin and the ground raw material silicon supported with the transition metal element.

[0061] The stirring can be carried out using a stirrer equipped with stirring blades, and the stirring time is, for example, 5 minutes to 2 hours, preferably 10 minutes to 1 hour. The stirring can be carried out at room temperature, or while heating to about 30 to 50°C. The solvent can be removed by a conventional method such as filtration. The drying can be carried out using, for example, a dryer, a reduced pressure dryer, or a spray dryer. The drying temperature is preferably 80°C or higher and 120°C or lower. Drying can also be carried out under reduced pressure.

[0062] Then, in the high-temperature treatment step, the active material precursor obtained above is calcined in a non-oxidizing atmosphere. The apparatus used for the high-temperature treatment can be appropriately selected depending on the purpose, such as a fluidized bed reactor, a rotary furnace, a vertical moving bed reactor, a tunnel furnace, a batch furnace, or a rotary kiln. The high-temperature treatment is carried out according to a calcination program defined by the temperature rise rate, the holding time at a constant temperature, and the like. The calcination temperature is preferably, for example, such that the maximum temperature reaches a range of 900°C to 1300°C. This allows the composite active material for a secondary battery of the present invention to be obtained.

[0063] The non-oxidizing atmosphere during the high-temperature firing is not particularly limited to the type of gas used, and examples include nitrogen, argon, hydrogen, a nitrogen-hydrogen mixed gas, etc. From the viewpoint of promoting the formation of silicon nitride, the use of nitrogen gas is preferred.

[0064] The fired product obtained in the high-temperature treatment step is then pulverized and, if necessary, classified to obtain a composite active material of the desired particle size. The pulverization may be performed in one step until the desired particle size is reached, or in several separate steps. If the fired composite active material is in the form of lumps or agglomerates with a particle size of 10 mm or more, the particles may be coarsely pulverized using a jaw crusher, roll crusher, or the like, then pulverized using a glow mill, ball mill, or the like, and further pulverized using a bead mill, jet mill, or the like. The particle size is the average particle size, or the D50 value.

[0065] Furthermore, when the active material for a secondary battery produced by pulverization contains coarse particles, it is preferable to carry out classification to remove the coarse particles and to adjust the particle size distribution by removing fine powders. The classifier to be used may be an air classifier, a wet classifier, or the like, depending on the purpose, but when removing coarse particles, a classification method using a sieve is preferable because it can reliably achieve the purpose.

[0066] When the composite active material for a secondary battery further has a carbon coating on its surface, the obtained active material is coated with the carbon coating in a chemical vapor deposition apparatus in a flow of a pyrolytic carbon source gas and a carrier inert gas at a temperature ranging from 700°C to 1000°C. Examples of the pyrolytic carbon source gas include acetylene, ethylene, acetone, alcohol, propane, methane, and ethane. Examples of the inert gas include nitrogen, helium, and argon, with nitrogen being commonly used.

[0067] [Secondary Battery] The secondary battery of the present invention is not particularly limited as long as it contains the composite active material for secondary batteries described above, but may also contain other components such as an organic binder and a conductive additive. The secondary battery of the present invention can be produced by applying a thin film of a slurry containing an organic binder and, if necessary, other components such as a conductive additive onto a copper foil current collector. A negative electrode can also be produced by adding a carbon material such as graphite to the slurry. Examples of carbon materials include natural graphite, artificial graphite, and amorphous carbon such as hard carbon or soft carbon.

[0068] For example, the negative electrode material can be obtained by kneading a composite active material for a secondary battery and a binder, which is an organic binding material, together with a solvent using a dispersing device such as a stirrer, a ball mill, a super sand mill, or a pressure kneader to prepare a negative electrode material slurry, which is then applied to a current collector to form a negative electrode layer. Alternatively, the negative electrode material can be obtained by forming the paste-like negative electrode material slurry into a shape such as a sheet or pellet, and integrating this with a current collector.

[0069] Examples of the organic binder include styrene-butadiene rubber copolymers (hereinafter also referred to as "SBR"); unsaturated carboxylic acid copolymers such as ethylenically unsaturated carboxylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, (meth)acrylonitrile, and hydroxyethyl (meth)acrylate, and (meth)acrylic copolymers composed of ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, fumaric acid, and maleic acid; and polymer compounds such as polyvinylidene fluoride, polyethylene oxide, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polyimide, polyamideimide, and carboxymethyl cellulose (hereinafter also referred to as "CMC").

[0070] Depending on their physical properties, these organic binders may be dispersed or dissolved in water, or dissolved in an organic solvent such as N-methyl-2-pyrrolidone (NMP). The content of the organic binder in the negative electrode layer of the lithium ion secondary battery negative electrode is preferably 1% by mass to 30% by mass, more preferably 2% by mass to 20% by mass, and even more preferably 3% by mass to 15% by mass.

[0071] When the content of the organic binder is 1% by mass or more, adhesion is improved and destruction of the negative electrode structure due to expansion and contraction during charge and discharge is further suppressed, while when the content of the organic binder is 30% by mass or less, an increase in electrode resistance is further suppressed.

[0072] The negative electrode material slurry may contain a conductive additive, if necessary. Examples of the conductive additive include carbon black, graphite, acetylene black, and conductive oxides and nitrides. The amount of the conductive additive used is preferably 1 to 15% by mass relative to the composite active material of the present invention.

[0073] The current collector may be made of copper, nickel, titanium, stainless steel, or the like in the form of a foil, perforated foil, mesh, or other strip. Porous materials such as porous metal (foamed metal) and carbon paper may also be used.

[0074] Examples of methods for applying the negative electrode material slurry to the current collector include metal mask printing, electrostatic coating, dip coating, spray coating, roll coating, doctor blade coating, gravure coating, screen printing, etc. After application, it is preferable to perform a rolling treatment using a flat plate press, a calender roll, or the like, as necessary.

[0075] The negative electrode material slurry can be formed into a sheet or pellet form, and the sheet or pellet can be integrated with the current collector by, for example, rolling, pressing, or a combination thereof.

[0076] The negative electrode layer formed on the current collector or the negative electrode layer integrated with the current collector is preferably heat-treated depending on the organic binder used. The heat treatment temperature is not particularly limited, but for example, when an aqueous styrene-butadiene rubber copolymer (SBR) or the like is used, the heat treatment may be performed at 100 to 130°C, and when an organic binder having a polyimide or polyamideimide main skeleton is used, the heat treatment is preferably performed at 150 to 450°C.

[0077] This heat treatment removes the solvent and hardens the binder, increasing strength and improving adhesion between particles and between the particles and the current collector. These heat treatments are preferably carried out in an inert atmosphere such as helium, argon, or nitrogen, or in a vacuum atmosphere, to prevent oxidation of the current collector during treatment.

[0078] After the heat treatment, the negative electrode is preferably subjected to pressure treatment. 3 to 1.8 g / cm 3 and preferably 1.1 g / cm 3 to 1.7 g / cm 3 More preferably, it is 1.2 g / cm 3 to 1.6 g / cm 3It is more preferable that the electrode density is higher. The higher the electrode density, the better the adhesion and the volumetric capacity density of the electrode tend to be. On the other hand, if the electrode density is too high, the voids in the electrode are reduced, which weakens the effect of suppressing the volume expansion of silicon and the like, and the capacity retention rate may decrease. Therefore, an optimal range of electrode density is selected.

[0079] The secondary battery of the present invention includes the composite active material for secondary batteries of the present invention. As secondary batteries containing the composite active material for secondary batteries, non-aqueous electrolyte secondary batteries and solid electrolyte secondary batteries are preferred, and the composite active material for secondary batteries exhibits excellent performance particularly when used as a negative electrode of a non-aqueous electrolyte secondary battery.

[0080] When the secondary battery of the present invention is used as, for example, a wet electrolyte secondary battery, it can be constructed by disposing a positive electrode and a negative electrode containing the composite active material for a secondary battery of the present invention opposite each other with a separator interposed therebetween and injecting an electrolytic solution.

[0081] The positive electrode can be obtained by forming a positive electrode layer on the surface of a current collector in the same manner as the negative electrode. In this case, the current collector can be a strip-shaped current collector made of a metal or alloy such as aluminum, titanium, or stainless steel, in the form of a foil, perforated foil, mesh, or the like.

[0082] The positive electrode material used for the positive electrode layer is not particularly limited. When a lithium ion secondary battery is produced among non-aqueous electrolyte secondary batteries, for example, a metal compound, metal oxide, metal sulfide, or conductive polymer material capable of doping or intercalating lithium ions may be used. For example, lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMnO 2 ), and their composite oxides (LiCoxNiyMnzO 2 , x + y + z = 1), lithium manganese spinel (LiMn 2 O 4 ), lithium vanadium compounds, V 2 O 5 , V 6 O 13 , V.O. 2 , MnO 2 , TiO2 , MoV 2 O 8 , TiS 2 , V 2 S 5 , V.S. 2 , MoS 2 , MoS 3 , Cr 3 O 8 , Cr 2 O 5 , olivine-type LiMPO 4 (wherein M is Co, Ni, Mn or Fe), conductive polymers such as polyacetylene, polyaniline, polypyrrole, polythiophene and polyacene, porous carbon, etc. can be used alone or in combination.

[0083] The separator may be, for example, a nonwoven fabric, cloth, or microporous film primarily composed of a polyolefin such as polyethylene or polypropylene, or a combination thereof. Note that if the nonaqueous electrolyte secondary battery to be fabricated has a structure in which the positive electrode and the negative electrode are not in direct contact with each other, it is not necessary to use a separator.

[0084] The electrolyte may be, for example, LiClO 4 , LiPF 6 , LiAsF 6 , LiBF 4 , LiSO 3 CF 3 A so-called organic electrolyte solution can be used in which a lithium salt such as ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, fluoroethylene carbonate, cyclopentanone, sulfolane, 3-methylsulfolane, 2,4-dimethylsulfolane, 3-methyl-1,3-oxazolidin-2-one, γ-butyrolactone, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, butyl methyl carbonate, ethyl propyl carbonate, butyl ethyl carbonate, dipropyl carbonate, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, methyl acetate, ethyl acetate, or the like is dissolved in a non-aqueous solvent of a single component or a mixture of two or more components.

[0085] The structure of the secondary battery of the present invention is not particularly limited, but typically, a positive electrode, a negative electrode, and an optional separator are wound into a flat spiral to form a wound electrode assembly, or these are stacked as flat plates to form a stacked electrode assembly, and these electrode assembly are sealed in an outer casing. Note that the half cells used in the examples described below are configured so that the negative electrode mainly comprises the present negative electrode active material, and a simple evaluation is performed using metallic lithium as the counter electrode, in order to more clearly compare the cycle characteristics of the active material itself.

[0086] The secondary battery of the present invention is not particularly limited, and can be used as a paper battery, a button battery, a coin battery, a laminated battery, a cylindrical battery, a prismatic battery, etc. The above-mentioned negative electrode active material of the present invention can also be applied to general electrochemical devices that use the insertion and desorption of lithium ions as a charge / discharge mechanism, such as hybrid capacitors and solid-state lithium secondary batteries.

[0087] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In these examples, [%] represents "% by mass" unless otherwise specified.

[0088] "Synthesis Example: Preparation of Silicon Slurry (Si1-Si6)" Zirconia beads (particle size range: 0.1 mm to 0.2 mm) and 100 ml of methyl ethyl ketone solvent (MEK) were placed in a container (150 ml) of a small bead mill device at a filling rate of 60%, and then raw silicon (commercially available product, average particle size 5 μm) and a cationic dispersant liquid (BYK Japan Co., Ltd., BYK145) were added as shown in the table below, and wet milling was carried out under the conditions shown in Table 1 below to obtain a dark brown liquid silicon slurry (solid concentration 20% by mass; Si1-6). The average particle size (D50) of the pulverized raw silicon was measured using a laser diffraction particle size distribution analyzer (Malvern Panalytical, Mastersizer 3000), and the D50 of the pulverized raw silicon was confirmed by TEM observation.

[0089]

[0090] Example 1: To 100 g of silicon slurry (Si1 prepared in the above synthesis example, average particle size D50 = 57 nm, Si content = 16.7 mass%), manganese (III) acetylacetonate solution (concentration 5 mass%; solvent ethanol) was added to adjust the Mn / Si (molar ratio) to 1.5 / 100, followed by stirring at room temperature for 1 hour and drying under reduced pressure at 110 ° C. The resulting dried product was fired at a high temperature in a nitrogen atmosphere at 1000 ° C. for 2 hours to obtain silicon particles. After crushing, the mixture was classified using a 20 μm sieve.

[0091] The XRD pattern of the silicon particles shows strong peaks (28.4°, 47.4°, 55.9°) attributed to Si(111) and weak peaks attributed to the silicon nitride crystal structure (α-Si 3 N 4 The XRD device used was an Ultima IV manufactured by Rigaku Corporation, and measurements were performed under the conditions of Cu / Kα radiation, 40 kV / 40 mA, a scan speed of 2 degrees / minute, and a scan range of 10 degrees or more and 70 degrees or less.

[0092] solid 29 The Si-NMR (JNM-ECA600, manufactured by JEOL RESONANCE) measurement results showed that peak A (chemical shift range: 0 ppm to -20 ppm) attributed to the silicon carbide phase, peak B (chemical shift range: -30 ppm to -60 ppm) attributed to the silicon nitride phase, and peak C (chemical shift range: -70 ppm to -100 ppm) attributed to zero-valent silicon were detected, and the peak area ratio R was 0.82 (Equation (1): R = (A + B) / C). 4 The peak at around −110 ppm attributed to was not detected.

[0093] According to the results of EDS elemental analysis, it was confirmed that the Mn / Si molar ratio of the silicon particles was 1.48 / 100, which was close to the amount of the charged amount. 2 The amorphous oxide film was found to have a thickness of 4 nm (average value of three locations). Quantitative elemental analysis using energy dispersive X-ray spectroscopy revealed that the measured Mn / Si molar ratio was as shown in Table 2 below.

[0094] Furthermore, 80 parts by mass of the silicon particles obtained above were mixed with 10 parts by mass of acetylene black as a conductive additive and 10 parts by mass of a mixture of CMC and SBR as a binder to prepare a slurry. The resulting slurry was formed into a film on copper foil. After drying under reduced pressure at 110°C, a coin-type lithium-ion battery was fabricated as a half cell using Li metal foil as the counter electrode. The charge / discharge characteristics of the fabricated half cell were evaluated at 25°C using a secondary battery charge / discharge tester (manufactured by Hokuto Denko Corporation). The cutoff voltage range was 0.005 to 1.5 V. The charge / discharge measurement results showed an initial discharge capacity of 1520 mAh / g, an initial coulombic efficiency of 75.1%, and a capacity retention rate of 62% after 10 charge / discharge cycles (Table 2).

[0095] Examples 2 to 7 100 g of silicon slurry (Synthesis Example Si2: average particle size D50 = 100 nm, Si content = 16.7 mass%) was adjusted to a Mn / Si (molar ratio) of 0.03 / 100 (Example 2); 0.1 / 100 (Example 3); 0.5 / 100 (Example 4); 1.5 / 100 (Example 5); 2.5 / 100 (Example 6); 4.7 / 100 (Example 7) and an appropriate amount of manganese (III) acetylacetonate solution (concentration 5 mass%, solvent ethanol) was added, followed by stirring at room temperature for 1 hour and drying under reduced pressure at 110 ° C. Other operations were carried out under the same conditions as in Example 1. Table 2 shows the obtained analysis results and the charge / discharge evaluation results of the half cell.

[0096] Examples 8 to 11 100 g of silicon slurry (Synthesis Example Si2: average particle size D50 = 100 nm, Si content = 16.7 mass%) was added with various metal ions (Mn 2+ , Fe 3+ , Ni + , Cu 2+ , La 3+After adding a solution of Mn / Si, the mixture was stirred at room temperature for 1 hour and dried under reduced pressure at 110°C. Example 8: Mn / Si (molar ratio) = 0.5 / 100 (manganese(III) acetylacetonate solution used); Fe / Si (molar ratio) = 0.3 / 100 (iron(II) acetate anhydride solution used, solvent: ethanol) Example 9: Mn / Si (molar ratio) = 0.5 / 100 (manganese(III) acetylacetonate solution used); Ni / Si (molar ratio) = 0.1 / 100 (nickel acetate anhydride solution used, solvent: methanol) Example 10: Cu / Si (molar ratio) = 1.0 / 100 (copper(II) acetate anhydride solution used, solvent: ethanol) Example 11: La / Si (molar ratio) = 1.0 / 100 (lanthanum(III) acetate anhydride solution used, solvent: ethanol) Other operations were performed under the same conditions as in Example 1. Table 2 shows the analytical results and the results of charge / discharge evaluation of the half cells.

[0097] Examples 12 to 14: 100 g of silicon slurry (Synthesis Example Si2: average particle size D50 = 100 nm, Si content = 16.7 wt%) was adjusted to a Mn / Si (molar ratio) of 1.5 / 100, and an appropriate amount of manganese (III) acetylacetonate solution (5 wt%, solvent: ethanol) was added, followed by stirring at room temperature for 1 hour and drying under reduced pressure at 110 ° C. Then, the samples were fired at 700 ° C. (Example 12), 900 ° C. (Example 13), and 1250 ° C. (Example 14), respectively, and various evaluations were performed. The relevant results are shown in Table 2.

[0098] Examples 15 to 20: To 100 g of silicon slurry (Example 15: Synthesis Example Si6 / average particle size D50 = 15 nm; Example 16: Synthesis Example Si1 / average particle size D50 = 57 nm; Example 17: Synthesis Example Si2 / average particle size D50 = 100 nm; Example 18: Synthesis Example Si3 / average particle size D50 = 150 nm; Example 19: Synthesis Example Si4 / average particle size D50 = 250 nm; Example 20: Synthesis Example Si5 / average particle size D50 = 400 nm; Si content = 16.7 mass%), an appropriate amount of manganese (III) acetylacetonate solution (concentration 5 mass%; solvent ethanol) was added so that the Mn / Si (molar ratio) was 1.5 / 100, and the mixture was stirred at room temperature for 1 hour. After high-temperature baking, a phenolic resin (average molecular weight 3000) was added to the product so that the silicon particle content was 50 mass%, and the mixture was thoroughly mixed in a stirrer, followed by drying at 110 ° C. under reduced pressure. The dried material was then sintered at a high temperature of 1100°C for 2 hours in a nitrogen atmosphere to obtain a sintered Si / C composite active material. Other operations were carried out under the same conditions as in Example 1. The analytical results and the charge / discharge evaluation results of the half-cell are shown in Table 2.

[0099] Comparative Example 1 100 g of silicon slurry (Synthesis Example Si2: average particle size D50 = 100 nm, Si content = 16.7 mass%) was dried under reduced pressure at 110°C. The sample was fired in a nitrogen atmosphere at 1000°C, and various evaluations were performed. The related results are shown in Table 2.

[0100] Comparative Example 2: Commercially available silicon nanoparticles (average particle size 100 nm) were thoroughly mixed with phenolic resin (average molecular weight 3000) to adjust the silicon particle content in the product after high-temperature sintering to 50% by mass, and then dried under reduced pressure at 110°C. The resulting dried product was sintered at 1100°C for 2 hours in a nitrogen atmosphere to obtain a sintered Si / C composite active material. The results of various evaluations are shown in Table 2.

[0101]

[0102] From Table 2 above, it can be seen that the silicon particles of the present invention containing transition metal elements (Examples 1 to 20) have higher capacity retention rates and initial coulombic efficiencies when used in secondary batteries than the silicon particles not containing transition metal elements (Comparative Examples 1 and 2). This demonstrates that the silicon particles of the present invention can improve the chemical durability of the particle surface and maintain high charge / discharge performance, such as capacity retention rate and initial coulombic efficiencies, in secondary batteries.

[0103] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2022-178740) filed on November 8, 2022, the contents of which are incorporated herein by reference.

Claims

1. Silicon particles having a silicon nitride phase on the surface and containing a transition metal element.

2. A silicon particle as described in claim 1, further comprising a silicon carbide phase on the surface of the silicon particle.

3. The silicon particles according to claim 1, wherein the transition metal element is at least one selected from the group consisting of Fe, Mn, Ni, Cr, Cu, Nb, Mo, Ru, Rh, Pd, and La.

4. The silicon particles according to claim 1 , wherein the transition metal element is Mn.

5. 4. The silicon particles according to claim 1, wherein the content of the transition metal element is 0.01 atm % to 5 atm % based on the total amount of silicon present in the silicon particles.

6. solid 29 In the Si-NMR spectrum, peak A in the chemical shift range of 0 ppm to -20 ppm, which is assigned to a silicon carbide phase, peak B in the chemical shift range of -30 ppm to -60 ppm, which is assigned to a silicon nitride phase, and peak C in the chemical shift range of -70 ppm to -100 ppm, which is assigned to silicon, are detected; The silicon particles according to any one of claims 1 to 3, wherein the area ratio R of each of the peaks calculated by the following formula (1) is in the range of 0.1 to 1.

0. R=(A+B) / C ‥(1)

7. The silicon particles according to any one of claims 1 to 3, in which a peak is detected at about 2θ = 28.4° in XRD measurement.

8. 4. The silicon particles according to claim 1, further comprising an amorphous oxide film present on the surface thereof, the thickness of which is 8 nm or less.

9. A method for producing silicon particles comprising at least the steps of wet-pulverizing raw material silicon under conditions where a dispersant is added, supporting a transition metal element-containing compound on the surface of the pulverized raw material silicon, and performing high-temperature treatment in a non-oxidizing atmosphere at a temperature range of 900°C to 1300°C.

10. A method for producing a composite active material for a secondary battery, comprising the method for producing silicon particles according to claim 9.

11. A composite active material for a secondary battery comprising the silicon particles according to any one of claims 1 to 3.

12. 12. The composite active material for a secondary battery according to claim 11, wherein the silicon particles have an average particle size in the range of 10 nm to 300 nm.