Manufacturing method for polyurethane foam sheet and manufacturing method for synthetic leather

JPWO2024122084A5Active Publication Date: 2024-11-28DIC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024555172
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-08
Filing Date
2023-06-08
Publication Date
2024-11-28
Estimated Expiration
2043-06-08

AI Technical Summary

Technical Problem

There is a need for a method to produce polyurethane foam sheets that utilize biomass raw materials, achieving high biomass content, excellent foam retention, and good texture, while also being environmentally friendly and suitable for use as an adhesive layer in synthetic leather production.

Method used

A moisture-curable polyurethane hot melt resin composition is used, comprising a urethane prepolymer derived from specific biomass-derived polyols and polyisocyanates, applied as a sheet and foamed with water vapor, incorporating a polyol composition with an amine catalyst having a foaming constant of 10 or more to enhance foam retention and texture.

Benefits of technology

The method produces polyurethane foam sheets with excellent foam retention and texture, high biomass content, and superior adhesive properties, making them suitable for use in synthetic leather as an adhesive layer, while being environmentally friendly.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a moisture-curable polyurethane hot-melt resin composition including a urethane prepolymer (i) that has an isocyanate group and is a reaction product of a polyol (A) and a polyisocyanate (B), said moisture-curable polyurethane hot-melt resin composition characterized in that the polyol (A) includes polytetramethylene glycol or a polycarbonate polyol (a1) that is derived from biomass, a polyol (a2) that has an aromatic ring, and a polyester polyol (a3) that is different from (a2) and is solid at room temperature. Additionally, the present invention provides a manufacturing method for a synthetic leather that has at least a substrate, an adhesive layer, and a surface skin layer, said manufacturing method for a synthetic leather characterized in that the adhesive layer is obtained through said manufacturing method for a polyurethane foam sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing polyurethane foam sheet and method for manufacturing synthetic leather

[0001] The present invention provides a method for producing a polyurethane foam sheet and a method for producing synthetic leather.

[0002] As restrictions on the use of dimethylformamide (DMF) become more widespread in Europe, there is a strong demand for solvent-free, energy-saving, and environmentally friendly resins. Solvent-free moisture-curable hot-melt urethane compositions have attracted attention and are widely used in the manufacture of building materials, automotive interior materials, and electrical and electronic devices such as refrigerators, smartphones, personal computers, and car navigation systems. In particular, in recent years, there has been an increasing trend to foam moisture-curable polyurethane hot-melt compositions to produce foamed and cured products for the purposes of improving impact resistance and texture through their cushioning effect, reducing the amount of moisture-curable hot-melt urethane composition used, and so on.

[0003] As a method for foaming and curing the moisture-curable hot-melt urethane composition, a water foaming method using water or steam has been widely studied (see, for example, Patent Documents 1 and 2). However, there is a demand for foamed sheets with better texture.

[0004] On the other hand, as the issue of marine plastics has recently been attracting attention, interest in bio-based resins that aim to move away from petroleum resources is increasing day by day, and moisture-curing polyurethane resin compositions are no exception. However, it has been pointed out that increasing the biomass content can lead to a decrease in texture, etc., and achieving both of these properties has been a major challenge.

[0005] Japanese Patent Application Laid-Open No. 2004-115705 Japanese Patent Application Laid-Open No. 2003-306526

[0006] An object of the present invention is to provide a method for producing a polyurethane foam sheet that has an increased biomass content using a biomass raw material, excellent foam retention properties, and a good texture.

[0007] The present invention provides a method for producing a polyurethane foam sheet, comprising: mixing a moisture-curable polyurethane hot-melt resin composition (X) containing a urethane prepolymer (i), which is a reaction product of a polyol (A) and a polyisocyanate (B), with a polyol composition (Y); applying the mixture to a substrate in the form of a sheet; and bringing the sheet-like mixture into contact with water vapor to water-foam the mixture. The method is characterized in that the polyol (A) contains a biomass-derived polytetramethylene glycol or polycarbonate polyol (a1), a polyol (a2) having an aromatic ring, and a polyester polyol (a3) ​​other than (a2) that is solid at room temperature; and the polyol composition (Y) contains an amine catalyst (y1) having a foaming constant (Kw) of 10 or more.

[0008] The present invention also provides a method for producing synthetic leather having at least a substrate, an adhesive layer, and a surface layer, wherein the adhesive layer is obtained by the method for producing a polyurethane foam sheet.

[0009] According to the method for producing a polyurethane foam sheet of the present invention, a polyurethane foam sheet having excellent foam retention and a good texture can be obtained. The polyurethane foam sheet of the present invention has a high biomass content using biomass raw materials and is an environmentally friendly sheet. Furthermore, the polyurethane foam sheet also has excellent adhesive properties, making it particularly suitable for use as an adhesive layer for synthetic leather.

[0010] The method for producing a polyurethane foam sheet of the present invention includes mixing a moisture-curable polyurethane hot-melt resin composition (X) containing a urethane prepolymer (i) that is a reaction product of a polyol (A) and a polyisocyanate (B) with a polyol composition (Y), applying the mixture obtained by mixing the mixture in the form of a sheet on a substrate, and bringing the mixture into contact with water vapor to water-foam the mixture, and the method for producing a polyurethane foam sheet includes using specific polyols (A) and polyol composition (Y).

[0011] The urethane prepolymer (i) may be a reaction product of a specific polyol (A) and a polyisocyanate (B).

[0012] The polyol (A) contains, as essential components, biomass-derived polytetramethylene glycol or polycarbonate polyol (a1), a polyol (a2) having an aromatic ring, and a polyester polyol (a3) ​​other than (a2) that is solid at room temperature, in order to increase the biomass content of the resin and obtain excellent foam retention, texture, and adhesiveness.

[0013] The biomass-derived polytetramethylene glycol or polycarbonate polyol (a1) is an essential component for increasing the biomass content of the resin and for imparting basic physical properties such as excellent mechanical strength to the adhesive film.

[0014] The biomass-derived polytetramethylene glycol is commercially available as, for example, "Bio PTMG" manufactured by Mitsubishi Chemical Corporation.

[0015] The biomass-derived polycarbonate polyol may be a polycarbonate polyol made from a biomass-derived glycol having 1 to 10 carbon atoms, more preferably 3 to 10, as a raw material, and is commercially available, for example, as "Benebiol NL-2010DB" manufactured by Mitsubishi Chemical Corporation, "Benebiol NL-3010DB" manufactured by Mitsubishi Chemical Corporation, "Benebiol NL-2000D" manufactured by Mitsubishi Chemical Corporation, or "PCDX222" manufactured by Asahi Kasei Corporation. These polycarbonate polyols may be used alone or in combination of two or more.

[0016] The number average molecular weight of the biomass-derived polytetramethylene glycol or polycarbonate polyol (a1) is preferably 500 to 100,000, and more preferably 700 to 50,000. The number average molecular weight of the biomass-derived polytetramethylene glycol or polycarbonate polyol (a1) is a value measured by gel permeation chromatography (GPC).

[0017] The amount of the biomass-derived polytetramethylene glycol or polycarbonate polyol (a1) used is preferably 50 to 90 mass %, more preferably 60 to 80 mass %, of the polyol (A).

[0018] The polyol (a2) having an aromatic ring provides the coating with excellent flexibility, texture, and adhesiveness, and examples of the polyol that can be used include polyether polyols having an aromatic ring and polyester polyols having an aromatic ring.

[0019] Examples of the polyether polyol having an aromatic ring include bisphenol A, bisphenol F, and their alkylene oxide adducts. These polyols may be used alone or in combination of two or more. Among these, polyether polyols that are alkylene oxide adducts of bisphenol A are preferred. The alkylene oxide is preferably an alkylene oxide having 2 to 8 carbon atoms, and the number of moles of the alkylene oxide added is preferably 2 to 10 moles, more preferably 4 to 8 moles.

[0020] As the polyester polyol having an aromatic ring, for example, a reaction product of a compound having a hydroxyl group and a polybasic acid shown below can be used.

[0021] Examples of the compound having a hydroxyl group that can be used include ethylene glycol, propylene glycol, 1,4-butanediol, pentanediol, 2,4-diethyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, hexanediol, neopentyl glycol, hexamethylene glycol, glycerin, trimethylolpropane, bisphenol A, bisphenol F, and alkylene oxide adducts thereof. Among these, it is preferable to use an alkylene oxide adduct of bisphenol A. Furthermore, the alkylene oxide is preferably an alkylene oxide having 2 to 8 carbon atoms, and the number of moles of the alkylene oxide added is preferably 2 to 10 moles, and more preferably 4 to 8 moles.

[0022] Examples of the polybasic acid that can be used include adipic acid, glutaric acid, pimelic acid, suberic acid, dimer acid, sebacic acid, undecanedicarboxylic acid, hexahydroterephthalic acid, phthalic acid, phthalic anhydride, isophthalic acid, and terephthalic acid.

[0023] The number average molecular weight of the polyol (a2) having an aromatic ring is preferably 500 to 10,000, and more preferably 500 to 5,000. The number average molecular weight of the polyol (a2) having an aromatic ring is a value measured by gel permeation chromatography (GPC).

[0024] The amount of the polyol (a2) having an aromatic ring used is preferably from 10 to 40% by mass, more preferably from 20 to 30% by mass, in the polyol (A).

[0025] The polyester polyol (a3) ​​other than (a2) that is solid at room temperature is an essential component for fixing bubbles, suppressing penetration of the adhesive into the fabric, and achieving excellent texture. The term "solid at room temperature" means that the polyester polyol does not exhibit flowability at 25°C.

[0026] The polyester polyol (a3) ​​is preferably at least one selected from the group consisting of polyester polyols (a3-1) made from diethylene glycol and sebacic acid, polyester polyols (a3-2) made from 1,3-propanediol and sebacic acid, polyester polyols (a3-3) made from diethylene glycol, neopentyl glycol, and phthalic acid, and polyester polyols (a3-4) made from diethylene glycol and phthalic acid.

[0027] Furthermore, as the polyester polyol (a3), polyester polyol (a3-1) made from diethylene glycol and sebacic acid and / or polyester polyol (a3-2) made from 1,3-propanediol and sebacic acid are preferred, in terms of increasing the biomass content of the resin. Note that examples of commercially available biomass raw materials for the polyester polyols include biomass-derived sebacic acid ("Bio Seb" manufactured by Toyokuni Oil Mills), biomass-derived 1,3-propanediol ("SUSTERRA Propanediol" manufactured by DuPont), and biomass-derived diethylene glycol ("Bio DEG" manufactured by India Glycols).

[0028] In addition, as the polyester polyol (a3), polyester polyol (a3-3) made from diethylene glycol, neopentyl glycol, and phthalic acid and / or polyester polyol (a3-4) made from diethylene glycol and phthalic acid are preferred, with polyester polyol (a3-3) made from diethylene glycol, neopentyl glycol, and phthalic acid being particularly preferred, in terms of obtaining even better texture. Note that the diethylene glycol may be derived from petroleum or biomass, but it is preferable to use biomass-derived diethylene glycol in order to increase the biomass content.

[0029] The number average molecular weight of the polyester polyol (a3) ​​is preferably 500 to 10,000, and more preferably 800 to 5,000. The number average molecular weight of the polyester polyol (a3) ​​is a value measured by gel permeation chromatography (GPC).

[0030] The amount of the polyester polyol (a3) ​​used is preferably from 10 to 30% by mass, more preferably from 10 to 20% by mass, in the polyol (A).

[0031] The polyol (A) essentially contains the components (a1) to (a3) ​​described above, but may contain other polyols as necessary. The total content of the components (a1) to (a3) ​​in the polyol (A) is preferably 20% by mass or more, and more preferably 50% by mass or more.

[0032] Examples of the other polyols that can be used include polyester polyols other than (a2) and (a3), polycarbonate polyols other than (a1), polyether polyols other than (a1), polybutadiene polyols, and polyacrylic polyols. These polyols may be used alone or in combination of two or more. These polyols may be used alone or in combination of two or more.

[0033] The number average molecular weight of the other polyols is, for example, 500 to 100,000. The number average molecular weight of the other polyols is a value measured by gel permeation chromatography (GPC).

[0034] Examples of the polyisocyanate (B) that can be used include aromatic polyisocyanates such as polymethylene polyphenyl polyisocyanate, diphenylmethane diisocyanate, polymeric diphenylmethane diisocyanate, carbodiimide-modified diphenylmethane diisocyanate, xylylene diisocyanate, phenylene diisocyanate, tolylene diisocyanate, and naphthalene diisocyanate; and aliphatic or alicyclic polyisocyanates such as hexamethylene diisocyanate, lysine diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and tetramethylxylylene diisocyanate. These polyisocyanates may be used alone or in combination of two or more. Among these, aromatic polyisocyanates are preferred, and diphenylmethane diisocyanate is more preferred, because they provide good adhesion, reactivity, and mechanical properties.

[0035] The urethane prepolymer (i) can be produced, for example, by adding the polyol (A) dropwise to a reaction vessel containing the polyisocyanate (B), followed by heating, and reacting under conditions in which the isocyanate groups of the polyisocyanate (B) are in excess relative to the hydroxyl groups of the polyol (A).

[0036] When producing the urethane prepolymer (i), the equivalent ratio ([NCO / OH]) of the isocyanate groups in the polyisocyanate (B) to the hydroxyl groups in the polyol (A) is preferably 1.1 to 5.0, more preferably 1.5 to 3.5, from the viewpoints of adhesiveness, texture, and mechanical strength.

[0037] The isocyanate group content (hereinafter abbreviated as "NCO %") of the urethane prepolymer (i) is preferably 1.1 to 5.0 mass %, more preferably 1.5 to 3.5 mass %, from the viewpoints of adhesiveness, texture, and mechanical strength. The isocyanate group content of the urethane prepolymer (i) is a value measured by potentiometric titration in accordance with JIS K1603-1:2007.

[0038] The moisture-curable polyurethane hot-melt composition (X) used in the present invention contains the urethane prepolymer (i) as an essential component, but may also contain other additives as necessary.

[0039] The other additives that can be used include, other than the polyol composition (Y) described below, for example, a silane coupling agent, a thixotropy-imparting agent, an antioxidant, a plasticizer, a filler, a dye, a pigment, a wax, etc. These additives may be used alone or in combination of two or more.

[0040] By mixing the polyol composition (Y) with the moisture-curable polyurethane hot-melt composition, the isocyanate groups of the urethane prepolymer (i) react with the polyol in the polyol composition (Y), thereby appropriately increasing the viscosity and fixing bubbles in the polyurethane foam sheet when foamed with water. This also contributes to the flexibility, mechanical strength, and durability of the resulting polyurethane foam sheet.

[0041] Examples of the polyol that can be used include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butanediol, 1,4-butanediol, 2,2-dimethyl-1,3-propanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,8-octanediol, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, etc. These compounds may be used alone or in combination of two or more.

[0042] The content of the polyol in the polyol composition (Y) is preferably 0.1 to 10.0% by mass, more preferably 0.5 to 5.0% by mass.

[0043] In the present invention, in order to obtain an excellent texture, it is essential that the polyol composition (Y) contains an amine catalyst (y1) having a foaming constant (Kw) of at least 10. The use of the specific amine catalyst (y1) can accelerate the reaction between the isocyanate groups of the urethane prepolymer (i) and water during water foaming, allowing the formation of large cells and enabling the temperature and humidity during water foaming to be set under milder conditions than before, thereby obtaining an excellent texture.

[0044] In the present invention, the foaming constant (Kw) of the amine catalyst (y1) is the catalytic activity constant (L 2 / (wq.mol hr)), and specifically, JP-A-2019-85513, JP-A-2009-14981, etc. can be referenced.

[0045] Examples of the specific amine catalyst (y1) include N,N,N',N''-pentamethyldiethylenetriamine (PMDETA, Kw=159), N,N,N',N'',N''-pentamethylethylenepropylenetriamine (PMEPTA, Kw=21.5), N,N,N',N'',N'',N''-pentamethylethylenepropylenetriamine (PMEPTA, Kw=21.5), Examples of catalysts that can be used include N,N,N'-pentamethyldipropylenetetraamine (PMDPTA, Kw=11.6), 1,1,4,7,10,10-hexamethyltriethylenetetramine (HMTETA, Kw=84.8), bis(2-dimethylaminoethyl)ether (DMAEE, Kw=25.5), N,N,N'-trimethylaminoethylethanolamine (TMAEEA, Kw=43.4), bis(2-dimethylaminoethyl)ether (BDMEE, Kw=117), and 1,4-diazabicyclo[2.2.2]octane=triethylenediamine (TEDA, Kw=14.5). These catalysts may be used alone or in combination of two or more.

[0046] As the amine catalyst (y1), it is preferable to use 1,4-diazabicyclo[2.2.2]octane=triethylenediamine in combination with another amine catalyst, in order to obtain a more excellent texture. In this case, the mass ratio is preferably 1 / 1 to 1 / 10, and more preferably 1 / 1 to 1 / 5, in order to obtain a more excellent texture.

[0047] The amount of the amine catalyst (y1) used is preferably from 1.0 to 20% by mass, more preferably from 1.0 to 10% by mass, in the polyol composition (Y).

[0048] The polyol composition (Y) may contain other additives in addition to the amine catalyst (y1). Examples of the other additives include catalysts other than (y1), foam stabilizers, flame retardants, antistatic agents, fillers, conductive agents, moisture absorbents, inert gases, silane coupling agents, thixotropic agents, tackifiers, waxes, plasticizers, heat stabilizers, light stabilizers, pigments, and hydrolysis inhibitors, which may be used alone or in combination. These additives may be used alone or in combination of two or more.

[0049] The amount of the polyol composition (Y) used is preferably 1.0 to 50 parts by mass, more preferably 1.0 to 35 parts by mass, per 100 parts by mass of the moisture-curable polyurethane hot-melt resin composition (X).

[0050] Next, the method for producing the polyurethane foam sheet of the present invention will be described.

[0051] The method for producing a polyurethane foam sheet of the present invention includes the steps of: mixing the moisture-curable polyurethane hot-melt resin composition (X) heated and melted at, for example, 70 to 150°C with the polyol composition (Y); applying the mixture obtained by mixing the moisture-curable polyurethane hot-melt resin composition (X) and the polyol composition (Y) in a sheet form onto a substrate; and bringing the sheet-like mixture into contact with water vapor to water-foam the mixture.

[0052] Examples of a method for mixing the moisture-curable polyurethane hot-melt resin composition (X) and the polyol composition (Y) include a method using a high-speed mixing head or a disper.

[0053] Examples of a method for applying the mixture in the form of a sheet onto a substrate such as release paper include methods using a roll coater, a spray coater, a T-die coater, a knife coater, etc. The thickness of the mixture applied in the form of a sheet is, for example, 50 to 500 μm.

[0054] The sheet-like mixture thus obtained is brought into contact with water vapor to cause water foaming. The technical term "water foaming" as used in the present invention means that the water contained in the water vapor is used as a foaming agent, and foaming occurs as a result of the reaction between the isocyanate groups in the urethane prepolymer (i) used in the present invention and the water, generating carbon dioxide gas.

[0055] The conditions for contacting with water vapor include, for example, setting the ambient temperature on the surface of the sheet-like mixture to, for example, 20 to 120°C, preferably less than 80°C, and more preferably 20 to 35°C, setting the ambient humidity on the surface of the sheet-like mixture to, for example, 50% or more, preferably 60% or more but less than 95%, and more preferably 60 to 85%, and setting the humidification time to 0.5 seconds to 10 minutes.

[0056] The method of contacting the mixture with water vapor includes using a humidifying chamber, a water vapor spraying device, or the like, which can maintain constant atmospheric temperature, atmospheric humidity, and humidifying time conditions on the surface of the mixture. The use of a device that generates saturated water vapor is more preferable, since the water vapor is less likely to cool and turn into water droplets during circulation in the production line. Furthermore, in order to further improve the thickness accuracy of the polyurethane foam sheet, it is preferable to use a pressure belt press, nip roll, flat press, or the like in combination after the humidifying treatment.

[0057] After contact with water vapor, the film may be aged for 0.5 to 3 days at a temperature of 20 to 80° C. and a relative humidity of 50 to 90%, for example.

[0058] As described above, the method for producing a polyurethane foam sheet of the present invention can provide a polyurethane foam sheet having a good texture. Furthermore, the polyurethane foam sheet has excellent adhesive properties, making it particularly suitable for use as an adhesive layer for synthetic leather.

[0059] Next, the method for producing the synthetic leather of the present invention will be described.

[0060] The synthetic leather has at least a substrate, an adhesive layer, and a surface layer, and the adhesive layer may be obtained by the method for producing a polyurethane foam sheet.

[0061] Examples of the substrate include fiber substrates such as nonwoven fabrics, woven fabrics, and knitted fabrics made from polyester fibers, polyethylene fibers, nylon fibers, acrylic fibers, polyurethane fibers, acetate fibers, rayon fibers, polylactic acid fibers, cotton, hemp, silk, wool, glass fibers, carbon fibers, and blends thereof; nonwoven fabrics impregnated with resins such as polyurethane resins; nonwoven fabrics further provided with a porous layer; resin substrates such as thermoplastic urethane (TPU), as well as genuine leather and split leather.

[0062] Examples of materials that can be used to form the surface layer include aqueous urethane resins, solvent-based urethane resins, solventless urethane resins, aqueous acrylic resins, solvent-based acrylic resins, solventless acrylic resins, solvent-based silicone resins, aqueous silicone resins, solventless silicone resins, vinyl chloride resins, thermoplastic polyurethane resins, thermoplastic polyester resins, thermoplastic amide resins, and thermoplastic polyolefin resins. These materials may be used alone or in combination of two or more.

[0063] Examples of methods for producing the synthetic leather include a method in which a mixture obtained by mixing the moisture-curable polyurethane hot-melt resin composition (X) and the polyol composition (Y) is applied in the form of a sheet onto a surface layer formed on release paper, water vapor is brought into contact with the sheet-like mixture to water-foam the mixture as described above, and the resulting foamed sheet is bonded to an adhesive layer and the substrate.

[0064] If necessary, a surface treatment layer (top coat layer) may be provided on the skin layer.

[0065] The present invention will be described in more detail below using examples.

[0066] Synthesis Example 1 A four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux condenser was charged with 70 parts by mass of biomass-derived polytetramethylene glycol ("Bio PTMG" manufactured by Mitsubishi Chemical Corporation, number average molecular weight: 2,000), 20 parts by mass of a polyether polyol having an aromatic ring (a polyether polyol which is an adduct of 6 moles of propylene oxide with bisphenol A, number average molecular weight: 508), and 10 parts by mass of a biomass-derived polyester polyol (a reaction product of biomass-derived sebacic acid ("Bio Seb" manufactured by Toyokuni Oil Mills, number average molecular weight: 2,000) and biomass-derived diethylene glycol ("Bio DEG" manufactured by India Glycols), number average molecular weight: 2,000), and the mixture was dried under reduced pressure at 110°C to dehydrate it until the water content was 0.05% by mass or less. Next, after cooling to 60°C, 33 parts by mass of diphenylmethane diisocyanate was added, the temperature was raised to 110°C, and the mixture was allowed to react for 2 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer (i-1) having an NCO% of 3.32% by mass and a biomass content of 60.2% by mass, which was designated as a moisture-curable polyurethane hot-melt resin composition (X1).

[0067] Synthesis Example 2 Into a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux condenser, 70 parts by mass of biomass-derived polytetramethylene glycol ("Bio PTMG" manufactured by Mitsubishi Chemical Corporation, number average molecular weight: 2,000), 20 parts by mass of a polyester polyol having an aromatic ring (a reaction product of a propylene oxide 6-mol adduct of bisphenol A, isophthalic acid, and biomass-derived sebacic acid ("Bio Seb" manufactured by Toyokuni Oil Mills, number average molecular weight: 2,000), and 10 parts by mass of a biomass-derived polyester polyol (a reaction product of biomass-derived sebacic acid ("Bio Seb" manufactured by Toyokuni Oil Mills, number average molecular weight: 2,000) and biomass-derived diethylene glycol ("Bio Seb" manufactured by India Glycols, number average molecular weight: 2,000). DEG "), number average molecular weight; 2,000) 10 parts by mass of the reaction product was charged, dried under reduced pressure at 110 ° C., and dehydrated until the water content was 0.05% by mass or less. Next, after cooling to 60 ° C., 23.5 parts by mass of diphenylmethane diisocyanate was added, the temperature was raised to 110 ° C., and the isocyanate group content was reacted for 2 hours until a constant NCO%; 3.33% by mass, biomass degree; 65.4% by mass urethane prepolymer (i-2) was obtained, and it was designated as a moisture-curable polyurethane hot melt resin composition (X2).

[0068] Synthesis Example 3 A four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux condenser was charged with 70 parts by mass of biomass-derived polytetramethylene glycol ("Bio PTMG" manufactured by Mitsubishi Chemical Corporation), 20 parts by mass of a polyester polyol having an aromatic ring (a reaction product of a propylene oxide 6-mol adduct of bisphenol A, isophthalic acid, and biomass-derived sebacic acid ("Bio Seb" manufactured by Toyokuni Oil Mills), number average molecular weight: 2,000), and 10 parts by mass of a biomass-derived polyester polyol (a reaction product of biomass-derived 1,3-propanediol ("SUSTERRA Propanediol" manufactured by DuPont) and biomass-derived sebacic acid ("Bio Seb" manufactured by Toyokuni Oil Mills), number average molecular weight: 2,000), and the mixture was dried under reduced pressure at 110°C to dehydrate it until the water content was 0.05% by mass or less. Next, after cooling to 60°C, 23.5 parts by mass of diphenylmethane diisocyanate was added, the temperature was raised to 110°C, and the reaction was carried out for 2 hours until the isocyanate group content became constant. This gave a urethane prepolymer (i-3) with an NCO% of 3.33% by mass and a biomass content of 65.4% by mass, which was designated as a moisture-curable polyurethane hot-melt resin composition (X3).

[0069] Synthesis Example 4 A four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux condenser was charged with 70 parts by mass of biomass-derived polytetramethylene glycol ("Bio PTMG" manufactured by Mitsubishi Chemical Corporation, number average molecular weight: 2,000), 20 parts by mass of a polyester polyol having an aromatic ring (a reaction product of a propylene oxide 6-mol adduct of bisphenol A, isophthalic acid, and biomass-derived sebacic acid ("Bio Seb" manufactured by Toyokuni Oil Mills, number average molecular weight: 2,000), and 10 parts by mass of a biomass-derived polyester polyol (a reaction product of biomass-derived diethylene glycol ("Bio DEG" manufactured by India Glycols), neopentyl glycol, and orthophthalic acid, number average molecular weight: 1,000), and the mixture was dried under reduced pressure at 110°C to dehydrate it until the water content was 0.05% by mass or less. Next, after cooling to 60°C, 26.5 parts by mass of diphenylmethane diisocyanate was added, the temperature was raised to 110°C, and the reaction was carried out for 2 hours until the isocyanate group content became constant. This gave a urethane prepolymer (i-4) with an NCO% of 3.39% by mass and a biomass content of 63.9% by mass, which was designated as a moisture-curable polyurethane hot-melt resin composition (X4).

[0070] [Comparative Synthesis Example 1] A four-necked flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux condenser was charged with 100 parts by weight of biomass-derived polytetramethylene glycol (Mitsubishi Chemical Corporation "Bio PTMG", number average molecular weight: 2,000), and dried under reduced pressure at 110 ° C., and dehydrated until the water content was 0.05% by weight or less. Then, after cooling to 60 ° C., 25.0 parts by weight of diphenylmethane diisocyanate was added, the temperature was raised to 110 ° C., and the isocyanate group content was reacted for 2 hours until a constant NCO%; 3.36% by weight, biomass degree; 80% by weight urethane prepolymer (iR-1) was obtained, and a moisture-curable polyurethane hot melt resin composition (XR1) was obtained.

[0071] Comparative Synthesis Example 2 A four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux condenser was charged with 70 parts by mass of biomass-derived polytetramethylene glycol ("Bio PTMG" manufactured by Mitsubishi Chemical Corporation, number average molecular weight: 2,000) and 30 parts by mass of biomass-derived polyester polyol (a reaction product of biomass-derived sebacic acid ("Bio Seb" manufactured by Toyokuni Oil Mills) and biomass-derived diethylene glycol ("Bio DEG" manufactured by India Glycols), number average molecular weight: 2,000), and the mixture was dried under reduced pressure at 110°C to dehydrate it until the water content was 0.05% by mass or less. Next, after cooling to 60°C, 25.0 parts by mass of diphenylmethane diisocyanate was added, the temperature was raised to 110°C, and the mixture was allowed to react for 2 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer (iR-2) with an NCO % of 3.36% by mass and a biomass content of 80% by mass, which was designated as a moisture-curable polyurethane hot-melt resin composition (XR2).

[0072] [Comparative Synthesis Example 3] thermometer, stirrer, a four-necked flask equipped with an inert gas inlet and a reflux condenser, biomass-derived polytetramethylene glycol (manufactured by Mitsubishi Chemical Corporation "Bio PTMG", number average molecular weight; 2,000) 70 parts by mass, polyether polyol having an aromatic ring (polyether polyol which is a propylene oxide 6 mole adduct of bisphenol A, number average molecular weight; 508) 30 parts by mass was charged, dried under reduced pressure at 110 ° C., and dehydrated until the water content was 0.05% by mass or less. Next, after cooling to 60 ° C., 25.0 parts by mass of diphenylmethane diisocyanate was added, the temperature was raised to 110 ° C., and the isocyanate group content was reacted for 2 hours until a constant, NCO%; 3.36% by mass, biomass degree; 56% by mass of urethane prepolymer (iR-3) was obtained, and a moisture-curable polyurethane hot melt resin composition (XR3) was obtained.

[0073] [Method for Measuring Number Average Molecular Weight] The number average molecular weight of the polyols used in the synthesis examples and the like is a value measured by gel permeation chromatography (GPC) under the following conditions.

[0074] Measurement apparatus: High-speed GPC apparatus ("HLC-8220GPC" manufactured by Tosoh Corporation) Column: The following columns manufactured by Tosoh Corporation were used, connected in series: "TSKgel G5000" (7.8 mm I.D. x 30 cm) x 1, "TSKgel G4000" (7.8 mm I.D. x 30 cm) x 1, "TSKgel G3000" (7.8 mm I.D. x 30 cm) x 1, "TSKgel G2000" (7.8 mm I.D. x 30 cm) x 1 Detector: RI (differential refractometer) Column temperature: 40°C Eluent: Tetrahydrofuran (THF) Flow rate: 1.0 mL / min Injection volume: 100 μL (tetrahydrofuran solution with a sample concentration of 0.4% by mass) Standard sample: A calibration curve was prepared using the following standard polystyrene.

[0075] (Standard polystyrene) "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation

[0076] Preparation Example 1 <Method of Producing a Surface Film> A pigment (DILAC BLACK HS6001 (DIC Corporation)) and 0.3 parts by mass of an antifoaming agent (TEGO Foamex 800 manufactured by EVONIK Corporation) were mixed with Hydran WLS 230 (DIC Corporation), a water-based urethane resin for the surface layer of synthetic leather. The mixture was applied to a release paper (EV 130TPD manufactured by Lintec Corporation) in an amount of 100 g / m using a comma coater. 2 After uniformly applying the coating to a wet state, the coating was dried at 70°C for 2 minutes and then at 120°C for 2 minutes to prepare a skin film having a thickness of 30 µm.

[0077] Example 1 Manufacturing Method of Polyurethane Foam Sheet The moisture-curable polyurethane hot-melt resin composition (X1) obtained in Synthesis Example 1 was heated to 120°C and melted. 100 parts by mass of the urethane prepolymer (i-1) was mixed with 2.0 parts by mass of 1,4-butanediol (hereinafter abbreviated as "14BG"), 0.15 parts by mass of PMDETA, 0.15 parts by mass of TEDA, and 1.0 part by mass of a silicone foam stabilizer ("SF-2962" manufactured by Dow Corning Corporation, hereinafter abbreviated as "SF2962") to prepare a polyurethane foam sheet. 3.3 parts by mass of the polyol composition was mixed by stirring using a Homodisper at 6,000 rpm for 20 seconds, and then immediately applied to a release paper ("DK-100" manufactured by Lintec Corporation) using an applicator to a thickness of 200 μm. A polyethylene film having a thickness of 50 μm was then laminated thereon. The mixture was then humidified with water vapor for 1 minute in an atmosphere of 30°C and 80% humidity, and left to stand for 1 day in an environment of 23°C and 65% humidity to obtain a polyurethane foam sheet.

[0078] <Preparation of Synthetic Leather> The moisture-curable polyurethane hot-melt resin composition (X1) obtained in Synthesis Example 1 was heated to 120°C to melt, and a mixture of 2.0 parts by mass of 1,4-butanediol (hereinafter abbreviated as "14BG"), 0.15 parts by mass of PMDETA, 0.15 parts by mass of TEDA, and a silicone foam stabilizer ("SF-2962" manufactured by Dow Corning Corporation, hereinafter abbreviated as "SF2962") was added to 100 parts by mass of the urethane prepolymer (i-1). 3.3 parts by mass of a polyol composition prepared by mixing 1.0 part by mass of ethanol and 1.0 part by mass of ethanol was mixed with a homodisper at 6,000 rpm for 20 seconds, and immediately applied to the surface film in a thickness of 200 μm using an applicator. A rayon napped fabric was attached to the surface film, and the resulting mixture was then humidified with water vapor for 1 minute in an atmosphere of 30° C. and 80% humidity, and left to stand for 1 day in an environment of 23° C. and 65% humidity to obtain a synthetic leather.

[0079] [Example 2] A polyurethane foam sheet and synthetic leather were obtained in the same manner as in Example 1, except that the type of moisture-curable polyurethane hot-melt resin composition (X1) was changed to the moisture-curable polyurethane hot-melt resin composition (X2).

[0080] [Example 3] A polyurethane foam sheet and synthetic leather were obtained in the same manner as in Example 1, except that the type of moisture-curable polyurethane hot-melt resin composition (X1) was changed to the moisture-curable polyurethane hot-melt resin composition (X3).

[0081] Example 4 A polyurethane foam sheet and synthetic leather were obtained in the same manner as in Example 1, except that the type of moisture-curable polyurethane hot-melt resin composition (X1) was changed to the moisture-curable polyurethane hot-melt resin composition (X4).

[0082] Example 5 A polyurethane foam sheet and synthetic leather were obtained in the same manner as in Example 2, except that HMTETA was used instead of PMDETA.

[0083] Example 6 A polyurethane foam sheet and synthetic leather were obtained in the same manner as in Example 2, except that PMDPTA was used instead of PMDETA.

[0084] Comparative Example 1 <Method for producing polyurethane foam sheet> The moisture-curable polyurethane hot-melt resin composition (XR1) obtained in Comparative Synthesis Example 1 was heated and melted to 120°C, and 100 parts by mass of the urethane prepolymer (iR-1) was mixed with 0.5 parts by mass of 14BG, 0.10 parts by mass of N,N-dimethylcyclohexylamine (Kw = 8.3, hereinafter abbreviated as "DMCHA"), and 0.1 parts by mass of SF-2962 to produce a polyol composition. The mixture was stirred and mixed in a homodisper at 6,000 rpm for 20 seconds, and then immediately applied to a release paper ("DK-100" manufactured by Lintec Corporation) using an applicator to a thickness of 200 μm. A 50 μm-thick polyethylene film was then laminated thereon. The mixture was then humidified with water vapor for 1 minute in an atmosphere of 30°C and 80% humidity, and left to stand for 1 day in an environment of 23°C and 65% humidity to obtain a polyurethane foam sheet.

[0085] <Preparation of Synthetic Leather> The moisture-curable polyurethane hot melt resin composition (XR1) obtained in Comparative Synthesis Example 1 was heated to 120°C and melted. 100 parts by mass of the urethane prepolymer (iR-1) was mixed with 0.5 parts by mass of 14BG, 0.10 parts by mass of N,N-dimethylcyclohexylamine (Kw = 8.3, hereinafter abbreviated as "DMCHA"), and 0.1 parts by mass of SF-2962 to prepare a polyol composition. The mixture was stirred and mixed in a homodisper at 6,000 rpm for 20 seconds, and then immediately applied to a thickness of 200 μm on the surface of the skin film using an applicator. A rayon napped fabric was then attached, and the mixture was moistened with water vapor for 1 minute in an atmosphere of 30°C and 80% humidity. The mixture was then left to stand for 1 day in an environment of 23°C and 65% humidity to obtain a synthetic leather.

[0086] Comparative Example 2 A polyurethane foam sheet and synthetic leather were obtained in the same manner as in Comparative Example 1, except that the type of moisture-curable polyurethane hot-melt resin composition (XR1) was changed to moisture-curable polyurethane hot-melt resin composition (XR2).

[0087] Comparative Example 3 <Method for producing polyurethane foam sheet> The moisture-curable polyurethane hot-melt resin composition (XR3) obtained in Comparative Synthesis Example 3 was heated to 120°C and melted. Immediately after that, the composition was applied to a release paper ("DK-100" manufactured by Lintec Corporation) using an applicator to a thickness of 200 μm. A polyethylene film having a thickness of 50 μm was laminated thereon. The composition was then humidified with water vapor for 1 minute in an atmosphere of 30°C and 80% humidity, and left to stand for 1 day in an environment of 23°C and 65% humidity to obtain a polyurethane foam sheet.

[0088] <Preparation of Synthetic Leather> The moisture-curable polyurethane hot-melt resin composition (XR3) obtained in Comparative Synthesis Example 3 was heated to 120°C and melted, and then immediately applied to the surface film to a thickness of 200 µm using an applicator. A rayon napped cloth was then attached, and the resultant was humidified with water vapor for 1 minute in an atmosphere of 30°C and 80% humidity, and then left to stand for 1 day in an environment of 23°C and 65% humidity to obtain synthetic leather.

[0089] [Method for evaluating foam retention] After humidification and curing, each polyurethane foam sheet obtained in Examples and Comparative Examples was left at an ambient temperature of 23°C and a relative humidity of 65% for 30 minutes, and then a 1 kg load was applied to an area of ​​5 cm x 5 cm for 2 hours. After the load was removed, the foam collapse resistance against the stress was visually evaluated as follows: A: The foam retained its foam and no change in appearance. B: The foam was partially collapsed and the appearance changed. C: The foam was entirely collapsed and the appearance changed.

[0090] [Method for evaluating texture] The synthetic leathers obtained in the examples and comparative examples were evaluated based on their flexibility when bent by hand as follows: "1": Very flexible; "2": Slightly hard; "3": Hard.

[0091]

[0092]

[0093] In all of Examples 1 to 6, which are the production methods of the present invention, polyurethane foam sheets having a high biomass content, excellent foam retention properties, and excellent texture were obtained.

[0094] On the other hand, Comparative Examples 1 and 2, which are both embodiments using a polyol (A) and a polyol composition (Y) other than those specified in the present invention, were poor in foam retention and texture.

[0095] Comparative Example 3 was an embodiment in which a polyol (A) other than those specified in the present invention was used and no polyol composition (Y) was used, and the foam retention and feel were significantly poor.

Claims

1. A method for producing a polyurethane foam sheet, comprising: mixing a moisture-curable polyurethane hot-melt resin composition (X) containing a urethane prepolymer (i) which is a reaction product of a polyol (A) and a polyisocyanate (B) with a polyol composition (Y), applying the mixture obtained by mixing the mixture in a sheet form onto a substrate, and contacting the sheet-like mixture with water vapor to water-foam the mixture, The polyol (A) is Biomass-derived polytetramethylene glycol or polycarbonate polyol (a1); A polyol (a2) having an aromatic ring, and (a3) a polyester polyol other than the (a2) that is solid at room temperature; Contains the polyester polyol (a3) ​​is at least one selected from the group consisting of polyester polyols (a3-1) made from diethylene glycol and sebacic acid, polyester polyols (a3-2) made from 1,3-propanediol and sebacic acid, polyester polyols (a3-3) made from diethylene glycol, neopentyl glycol, and phthalic acid, and polyester polyols (a3-4) made from diethylene glycol and phthalic acid; The method for producing a polyurethane foam sheet, wherein the polyol composition (Y) contains an amine catalyst (y1) having a foaming constant (Kw) of 10 or more.

2. 2. The method for producing a polyurethane foam sheet according to claim 1, wherein the amine catalyst (y1) is a combination of 1,4-diazabicyclo[2.2.2]octane=triethylenediamine and another amine catalyst.

3. 2. The method for producing a polyurethane foam sheet according to claim 1, wherein the polycarbonate polyol (a1) is made from a biomass-derived glycol having 1 to 10 carbon atoms.

4. 2. The method for producing a polyurethane foam sheet according to claim 1, wherein the polyol (a2) having an aromatic ring is a polyether polyol which is an alkylene oxide adduct of bisphenol A, or a polyester polyol produced from an alkylene oxide adduct of bisphenol A.

5. 2. The method for producing a polyurethane foam sheet according to claim 1, wherein the temperature during the contact with the water vapor is less than 80° C. and the humidity is less than 95%.

6. 2. A method for producing synthetic leather having at least a substrate, an adhesive layer, and a surface layer, wherein the adhesive layer is obtained by the method for producing a polyurethane foam sheet according to claim 1.