Steel plate, resistance spot welding method, resistance spot welded member, and method for manufacturing steel plate
Patent Information
- Application Number
- JP2024522713
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-18
- Filing Date
- 2023-12-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-12-18
AI Technical Summary
Current steel sheets with high tensile strength (1450 MPa or more) face challenges in achieving both excellent formability (hole spreadability) and weldability, particularly due to the narrow appropriate current range and reduced cross tensile strength resulting from the addition of alloying elements.
The steel sheet composition is optimized with a mass percentage range of specific elements, including C, Si, Mn, P, S, Al, N, Nb, Ti, B, and Sb, along with controlled microstructure and precipitate distribution, to achieve the desired strength, formability, and weldability.
This approach results in a steel sheet with a tensile strength of 1450 MPa or more, combined with improved hole spreadability and resistance spot weldability, characterized by a wide appropriate current range and enhanced cross tensile strength.
Description
[Technical field]
[0001] The present invention relates to a steel sheet, and in particular to a steel sheet that can be suitably used as a material for structural parts of automobiles, etc. The present invention also relates to a resistance spot welding method using the steel sheet, a resistance spot welded component, and a method for manufacturing the steel sheet. [Background technology]
[0002] In recent years, CO2 emission regulations have become stricter due to growing environmental concerns, and in the automotive industry, reducing the weight of car bodies to improve fuel efficiency has become an issue. As a result, the use of high-strength steel sheets to reduce the thickness of automotive parts has been promoted, and in particular, the use of steel sheets with a tensile strength (TS) of 1450 MPa or more has been promoted.
[0003] On the other hand, high-strength steel sheets used for structural and reinforcing components of automobiles are required to have not only strength but also excellent formability. In particular, to be used as materials for parts with complex shapes, the steel sheets are required to have excellent hole expansion properties.
[0004] However, in order to secure a tensile strength of 1450 MPa or more, it is necessary to add a large amount of alloying elements to the steel sheet, but the addition of alloying elements reduces the hole expandability, making it difficult to achieve both high strength and excellent hole expandability.
[0005] Furthermore, in the manufacture of automobiles, resistance spot welding is widely used from the viewpoints of cost and production efficiency. However, the addition of alloying elements reduces the resistance spot weldability (hereinafter simply referred to as "weldability") of steel sheets. Specifically, when a large amount of alloying elements is added, the appropriate current range for obtaining the required nugget diameter by resistance spot welding becomes extremely narrow. In addition, the cross tensile strength (CTS) of the joint after resistance spot welding is significantly reduced. Therefore, it has been difficult to achieve both high strength and excellent weldability.
[0006] Therefore, various methods have been considered to solve the above problems.
[0007] For example, Patent Document 1 proposes a method for improving the weldability of high-strength steel plates by adjusting the welding conditions.
[0008] Moreover, Patent Document 2 proposes a method for improving the formability and weldability of a high-strength steel plate by controlling the microstructure. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2011-005544 A [Patent Document 2] JP 2008-231541 A Summary of the Invention [Problem to be solved by the invention]
[0010] According to the method proposed in the above Patent Document 1, the occurrence of shrinkage defects and cracks in the weld metal part can be suppressed. However, the above method does not improve the appropriate current range and cross tensile strength. In addition, the above method requires pressure and current application under specific conditions after welding current application, which increases the time required for welding and reduces productivity. In addition, the method proposed in Patent Document 1 adjusts the welding conditions and does not contribute to improving the formability of the steel sheet.
[0011] In addition, according to the method proposed in Patent Document 2, a certain degree of improvement in formability and weldability is observed. However, the tensile strength of the steel plate obtained by the method in Patent Document 2 is less than 1000 MPa, and a tensile strength of 1450 MPa or more cannot be achieved. Furthermore, as mentioned above, excellent hole expandability is required for manufacturing components having complex shapes. However, in Patent Document 2, elongation (El) is used as an index of the formability of the steel plate, and hole expandability is not taken into consideration.
[0012] Thus, the reality is that a steel plate that combines a tensile strength of 1450 MPa or more with high levels of formability (hole expandability) and weldability (wide range of appropriate current, cross tensile strength) has yet to be realized.
[0013] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a steel sheet that combines a tensile strength of 1450 MPa or more with high levels of formability (hole expandability) and weldability (wide range of appropriate current, cross tensile strength). [Means for solving the problem]
[0014] As a result of studies conducted to solve the above problems, the inventors discovered that a steel sheet that satisfies the above requirements can be obtained by controlling the volume fraction of martensite in the surface layer of the steel sheet and the number density of fine Ti precipitates and Nb precipitates present in the steel, in addition to the component composition of the steel sheet.
[0015] The present invention has been completed based on the above findings, and the gist of the present invention is as follows.
[0016] 1. The composition, in mass%, is C: 0.18-0.38%, Si: 0.2-1.8%, Mn: 2.4-3.5%, P: 0.03% or less, S: 0.003% or less, Al: 0.01 to 0.50%, N: 0.008% or less, Nb: 0.005 to 0.08% and / or Ti: 0.005 to 0.08%, and Contains one or both of B: 0.0002 to 0.0050% and Sb: 0.001 to 0.012%, The balance consists of Fe and unavoidable impurities, and The A value defined by the following formula (1) is 0.9 to 6.0, The microstructure at the 1 / 4 position of the plate thickness satisfies the following conditions: Martensite volume fraction: 93% or more, Volume fraction of ferrite: 0-5%, Volume fraction of retained austenite: 0-7%, Average grain size of martensite: 7 μm or less, Average grain size of ferrite: 3μm or less Average grain size of retained austenite: 3μm or less, The microstructure from the surface to a depth of 7 μm satisfies the following conditions: Martensite volume fraction: 0-20%, The number density of Ti precipitates with a grain size of 0.005 μm or more and less than 0.10 μm and Nb precipitates with a grain size of 0.005 μm or more and less than 0.10 μm in the range of 50 to 100 μm deep from the surface is 20 / 100 μm 2 That's it, steel plate. A=([C]+[Si] / 8+[Mn] / 20) / (2×([Ti]+[Nb])+85×([B]+[Sb] / 20) ) …(1) However, the parentheses in the above formula (1) represent the content (mass%) of the element in the parentheses, and if the element is not contained, the value is set to 0.
[0017] 2. The composition further comprises, in mass%, V: 0.05% or less, Cu: 0.50% or less, Ni: 0.50% or less, Mo: 0.50% or less Cr: 0.50% or less, Sn: 0.30% or less, Ca: 0.0050% or less, and REM: 0.0050% or less The steel sheet according to claim 1, further comprising at least one selected from the group consisting of:
[0018] 3. The steel sheet according to 1 or 2 above, further comprising a zinc-based plating layer on at least one surface.
[0019] 4. A resistance spot welding method in which a sheet assembly including at least one steel plate according to any one of 1 to 3 above is clamped between a pair of welding electrodes and joined by passing an electric current through the sheet assembly while applying pressure.
[0020] 5. A resistance spot welded component comprising at least one steel plate according to any one of 1 to 3 above in a plate assembly.
[0021] 6. Continuously cast the molten steel having the composition described in 1 or 2 above into a steel slab; The steel slab is cooled at an average cooling rate of 100°C / h or more in a temperature range up to 600°C, The cooled steel slab is reheated by heating it to a heating temperature of 1250 to 1450 ° C. and holding it at the heating temperature for 60 minutes or more; The reheated steel slab is hot-rolled under a finish rolling temperature of 850 to 950°C to obtain a hot-rolled steel sheet. The hot-rolled steel sheet is cooled at an average cooling rate of 80°C / s or more to a cooling stop temperature of 480°C or less, The cooled hot-rolled steel sheet is coiled at a coiling temperature of 480°C or less. The hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. The cold-rolled steel sheet is annealed in an atmosphere having a dew point of more than -20°C. In the annealing, the cold-rolled steel sheet is Heat to an annealing temperature of 780 to 980°C at an average heating rate of 3 to 30°C / s. The annealing temperature is maintained for a holding time of 15 to 360 seconds, Cooling from the annealing temperature to room temperature at an average cooling rate of 3°C / s or more; Manufacturing method of steel plate.
[0022] 7. The method for producing a steel sheet according to claim 6, further comprising electroplating the annealed steel sheet to form a zinc-based plating layer on at least one surface of the steel sheet.
[0023] 8. Continuously cast the molten steel having the composition described in 1 or 2 above into a steel slab; The steel slab is cooled at an average cooling rate of 100°C / h or more in a temperature range up to 600°C, The cooled steel slab is reheated by heating it to a heating temperature of 1250 to 1450 ° C. and holding it at the heating temperature for 60 minutes or more; The reheated steel slab is hot-rolled under a finish rolling temperature of 850 to 950°C to obtain a hot-rolled steel sheet. The hot-rolled steel sheet is cooled at an average cooling rate of 80°C / s or more to a cooling stop temperature of 480°C or less, The cooled hot-rolled steel sheet is coiled at a coiling temperature of 480°C or less, The hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. The cold-rolled steel sheet is annealed in an atmosphere having a dew point of more than -20°C, The annealed steel sheet is subjected to hot-dip galvanization by immersing the steel sheet in a hot-dip galvanizing bath to form a zinc-based plating layer on at least one surface of the steel sheet; The method for producing a steel sheet, comprising cooling the hot-dip galvanized steel sheet to room temperature at an average cooling rate of 3° C. / s or more; In the annealing, the cold-rolled steel sheet is Heat to an annealing temperature of 780 to 980°C at an average heating rate of 3 to 30°C / s. The annealing temperature is maintained for a holding time of 15 to 360 seconds, Cooling from the annealing temperature to the immersion in the hot-dip galvanizing bath at an average cooling rate of 3° C. / s or more; Manufacturing method of steel plate.
[0024] 9. The method for producing a steel sheet according to the above item 8, further comprising the step of: after the hot-dip plating, performing an alloying treatment prior to the cooling to room temperature. Effect of the Invention
[0025] According to the present invention, it is possible to provide a steel sheet that combines a tensile strength of 1450 MPa or more with high levels of formability (hole expandability) and weldability (wide range of appropriate current, cross tensile strength). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, an embodiment of the present invention will be described. Note that the following description shows a preferred embodiment of the present invention, and the present invention is not limited by the following description. In addition, the unit of content, "%", represents "mass %" unless otherwise specified.
[0027] [Component composition] The steel sheet of the present invention has the above-mentioned composition. The reasons for limiting the composition will be explained below.
[0028] C: 0.18-0.38% C is an element that contributes to the formation of martensite, which is a hard phase, and the addition of C is essential to obtain a desired tensile strength. In addition, C reacts with Ti and Nb to form precipitates. Therefore, the addition of C is important to obtain a desired number density of precipitates. If the C content is less than 0.18%, the required volume fraction of martensite cannot be ensured. Therefore, the C content is set to 0.18% or more, preferably 0.19% or more. On the other hand, if the C content exceeds 0.38%, the toughness of the nugget after spot welding decreases, and as a result, the cross tensile strength decreases. Therefore, the C content is set to 0.38% or less, preferably 0.34% or less.
[0029] Silicon: 0.2 to 1.8% Si is an element that has the effect of improving weldability. This is because the addition of Si alleviates Mn segregation, and as a result, the variation in hardness in the plate thickness direction is reduced. In order to obtain the above effect, the Si content is set to 0.2% or more, preferably 0.3% or more. On the other hand, if the Si content exceeds 1.8%, liquid metal embrittlement occurs during resistance spot welding. Therefore, the Si content is set to 1.8% or less, preferably 1.6% or less.
[0030] Mn: 2.4-3.5% Mn is an element that contributes to improving the strength of steel sheets through solid solution strengthening and the formation of hard phases. In addition, Mn is an element that stabilizes austenite and is an element necessary for controlling the fraction of hard phases. In order to obtain the above effect, the Mn content is set to 2.4% or more. On the other hand, if the Mn content is higher than 3.5%, the toughness of the nugget after spot welding decreases, and the cross tensile strength decreases. In addition, when hydrogen penetrates into the steel sheet, the slip constraint of the grain boundaries increases, making it easier for cracks to progress at the crystal grain boundaries. As a result, the delayed fracture resistance after resistance welding decreases. Therefore, the Mn content is set to 3.5% or less, preferably 3.2% or less.
[0031] P:0.03% or less If the P content is higher than 0.03%, segregation of P to grain boundaries becomes significant. As a result, the grain boundaries become embrittled and resistance weldability decreases. Therefore, the P content is set to 0.03% or less, preferably 0.02% or less. On the other hand, the lower limit of the P content is not particularly limited and may be 0%. However, since excessive reduction of the P content increases the steelmaking cost, the P content is preferably set to 0.005% or more.
[0032] S: 0.003% or less If the S content is higher than 0.003%, the resistance weldability is reduced. This is because a large amount of sulfides such as MnS is generated, and cracks are generated starting from the sulfides when hydrogen penetrates. Therefore, the S content is set to 0.003% or less, preferably 0.002% or less. On the other hand, the lower limit of the S content is not particularly limited and may be 0%. However, since excessive reduction in the S content increases the steelmaking cost, it is preferable that the S content is 0.0002% or more.
[0033] Al: 0.01 to 0.50% Al is an element necessary for deoxidation. If the Al content is less than 0.01%, the deoxidation effect is insufficient. Therefore, the Al content is set to 0.01% or more, preferably 0.02%. On the other hand, if the Al content is more than 0.50%, the ferrite phase is excessively generated during annealing, making it difficult to ensure strength. Therefore, the Al content is set to 0.50% or less, preferably 0.45% or less.
[0034] N: 0.008% or less N is an element that deteriorates hole expandability by forming coarse nitrides. If the N content is higher than 0.008%, the deterioration of hole expandability becomes significant. Therefore, the N content is set to 0.008% or less, preferably 0.007% or less. On the other hand, the lower limit of the N content is not particularly limited and may be 0%. However, since excessive reduction of the N content increases the steelmaking cost, the N content is preferably set to 0.001% or more.
[0035] The chemical composition of the steel plate of the present invention contains one or both of Nb and Ti in the following amounts. Nb and Ti are elements that have a common function of improving resistance weldability by forming fine carbonitrides.
[0036] Nb: 0.005 to 0.08% Nb is an element that has the effect of improving resistance weldability by forming fine carbonitrides. When Nb is added to obtain the above effect, the Nb content is set to 0.005% or more, preferably 0.01% or more. On the other hand, if a large amount of Nb is added, not only does the elongation decrease significantly, but also slab cracks occur after continuous casting. Therefore, the Nb content is set to 0.08% or less, preferably 0.07% or less, more preferably 0.05% or less.
[0037] Ti: 0.005~0.08% Ti, like Ti, is an element that has the effect of improving resistance weldability by forming fine carbonitrides. When Ti is added to obtain the above effect, the Ti content is set to 0.005% or more, preferably 0.008% or more. On the other hand, if a large amount of Ti is added, the elongation significantly decreases. Therefore, the Ti content is set to 0.08% or less, preferably 0.07% or less. Ti also has the effect of preventing B from reacting with N. In addition, the fine carbonitrides of Ti become hydrogen trapping sites and increase the hydrogen overvoltage, thereby improving the delayed fracture resistance after resistance welding. From the viewpoint of obtaining these effects, it is preferable to add Ti at the above content.
[0038] The chemical composition of the steel sheet of the present invention contains one or both of B and Sb in the amounts shown below. Both B and Sb are elements having a common function of improving cross tensile strength by strengthening grain boundaries.
[0039] B: 0.0002% to 0.0050% B is an element that has the effect of strengthening grain boundaries by segregating at the grain boundaries, and adding B can improve the cross tensile strength. When B is added to obtain the above effect, the B content is set to 0.0002% or more, preferably 0.0004% or more. On the other hand, when the B content exceeds 0.0050%, the effect is saturated, and the amount of B segregated at the grain boundaries increases, resulting in a decrease in hole expandability. Therefore, the B content is set to 0.0050% or less, preferably 0.0040% or less. B improves hardenability and contributes to further improving the strength of the steel sheet by generating a hard phase. In addition, B is an element that can improve hardenability without lowering the martensitic transformation starting point. From the viewpoint of obtaining these effects, it is preferable to add B at the above content.
[0040] Sb: 0.001 to 0.012% Like B, Sb is an element that has the effect of strengthening grain boundaries by segregating there, and adding Sb can improve cross tensile strength. When Sb is added to obtain the above effect, the Sb content is set to 0.001% or more, preferably 0.002% or more. On the other hand, since Sb has the effect of preventing decarburization of the steel sheet surface, if the Sb content exceeds 0.012%, the specified steel sheet structure of the surface layer cannot be obtained, and as a result, the resistance weldability is reduced. Therefore, the Sb content is set to 0.012% or less, preferably 0.010% or less.
[0041] A steel sheet according to one embodiment of the present invention has a composition containing the above-mentioned components with the balance being Fe and unavoidable impurities.
[0042] When Co is contained as the unavoidable impurities, the Co content is preferably 0.10% or less.When Zn is contained as the unavoidable impurities, the Zn content is preferably 0.10% or less.
[0043] In addition, the composition of the steel sheet according to another embodiment of the present invention may further contain at least one of the following elements in addition to the above-mentioned elements. Note that all of the following elements can be added as desired, and therefore their inclusion is not essential. Therefore, the lower limit of the content may be 0%.
[0044] V:0.05% or less V is an element that has the effect of further improving strength by forming fine carbonitrides. However, when the V content exceeds 0.05%, the effect of the addition is saturated, and it is not possible to obtain an effect commensurate with the increase in alloy cost. Therefore, when V is added, the V content is set to 0.05% or less, preferably 0.04% or less. On the other hand, from the viewpoint of increasing the effect of adding V, it is preferable that the V content is set to 0.005% or more.
[0045] Cr:0.50% or less Cr is an element that has the effect of further improving strength by generating a hard phase. However, if the Cr content exceeds 0.50%, surface defects are likely to occur. Therefore, when Cr is added, the Cr content is set to 0.50% or less, preferably 0.45% or less. On the other hand, from the viewpoint of enhancing the effect of adding Cr, the Cr content is preferably set to 0.02% or more, more preferably 0.05% or more.
[0046] Sn: 0.30% or less Sn is an element that increases the hydrogen overvoltage of the steel sheet, thereby further improving the delayed fracture resistance. However, if the Sn content exceeds 0.30%, the effect saturates and the ductility decreases. Therefore, when Sn is added, the Sn content is set to 0.30% or less, preferably 0.25% or less. On the other hand, from the viewpoint of increasing the effect of adding Sn, the Sn content is preferably set to 0.005% or more, and more preferably 0.01% or more.
[0047] Mo: 0.50% or less Mo, like Cr, is an element that has the effect of further improving strength by generating a hard phase. Mo also contributes to further increasing strength by generating carbides. However, when the Mo content exceeds 0.50%, the addition effect is saturated, and it is not possible to obtain an effect commensurate with the increase in alloy cost. Therefore, when Mo is added, the Mo content is set to 0.50% or less, preferably 0.45% or less. On the other hand, from the viewpoint of increasing the effect of adding Mo, the Mo content is preferably set to 0.02% or more, and more preferably 0.05% or more.
[0048] Cu: 0.50% or less Cu is an element that has the effect of increasing hydrogen overvoltage and, as a result, improving delayed fracture resistance after resistance welding. However, if the Cu content exceeds 0.50%, the additive effect is saturated and surface defects are likely to occur. Therefore, the Cu content is set to 0.50% or less. On the other hand, from the viewpoint of increasing the additive effect of Cu, the Cu content is preferably set to 0.005% or more.
[0049] Ni: 0.50% or less Ni, like Cu, is an element that has the effect of increasing hydrogen overvoltage and improving delayed fracture resistance. In addition, when Ni is added together with Cu, it has the effect of suppressing surface defects caused by Cu. However, when the Ni content exceeds 0.50%, the effect of addition is saturated. Therefore, when Ni is added, the Ni content is set to 0.50% or less. On the other hand, from the viewpoint of increasing the effect of adding Ni, it is preferable that the Ni content is set to 0.005% or more.
[0050] Ca: 0.0050% or less Ca is an element that has the effect of further improving hole expandability by making the shape of sulfides spherical. Ca also contributes to improving delayed fracture resistance after resistance welding. However, when the Ca content exceeds 0.0050%, the effect is saturated, so when Ca is added, the Ca content is set to 0.0050% or less. On the other hand, from the viewpoint of enhancing the effect of adding Ca, the Ca content is preferably set to 0.0005% or more.
[0051] REM: 0.0050% or less Like Ca, REM (rare earth metal) is an element that has the effect of further improving hole expandability by making the shape of sulfides spherical. REM also contributes to improving delayed fracture resistance after resistance welding. However, when the REM content exceeds 0.0050%, the effect is saturated, so when REM is added, the REM content is set to 0.0050% or less. On the other hand, from the viewpoint of increasing the effect of adding REM, the REM content is preferably set to 0.0005% or more.
[0052] A value: 0.9~6.0 The composition of the steel sheet of the present invention further has an A value defined by the following formula (1) of 0.9 to 6.0. A=([C]+[Si] / 8+[Mn] / 20) / (2×([Ti]+[Nb])+85×([B]+[Sb] / 20) ) …(1) However, the parentheses in the above formula (1) represent the content (mass%) of the element in the parentheses, and if the element is not contained, the value is set to 0.
[0053] If the A value is less than 0.9, the desired hole expandability cannot be obtained. This is because the amount of Ti, Nb, B, and Sb added is excessive relative to the carbon equivalent. If the amount of Ti and Nb added is too much, Ti precipitates and Nb precipitates become excessive, and the hole expandability decreases. If the amount of B and Sb added is too much, B and Sb will segregate excessively at the grain boundaries, and the hole expandability will decrease. Therefore, the A value is set to 0.9 or more, preferably 1.0 or more. On the other hand, if the A value is greater than 6.0, the weldability, especially the cross tensile strength, will decrease. This is because the amount of Ti, Nb, B, and Sb added is insufficient relative to the carbon equivalent. Therefore, the A value is set to 6.0 or less, preferably 5.8 or less, and more preferably 5.0 or less.
[0054] [Microstructure] In the steel sheet of the present invention, the microstructure at the 1 / 4 position of the sheet thickness and the microstructure at a depth of 7 μm from the surface of the steel sheet must each satisfy specific conditions. The reasons for this will be explained below.
[0055] (Microstructure at 1 / 4 thickness position) M:93% or more If the volume fraction of martensite (M) is less than 93%, the desired tensile strength and hole expandability cannot be obtained. In addition, if the total volume fraction is less than 93%, the delayed fracture resistance also deteriorates. Therefore, the volume fraction of martensite (M) at the 1 / 4 position of the plate thickness is set to 93% or more, preferably 95% or more. The upper limit of the volume fraction is not particularly limited, but may be 100%.
[0056] In the present invention, tempered martensite is also defined as being included in "martensite". This is because it is difficult to distinguish between martensite and tempered martensite in the microstructure of the steel sheet of the present invention. In addition, the "tempered martensite" includes martensite generated by self-tempering during cooling in annealing from cooling below the martensitic transformation start point (Ms point) to room temperature, as well as martensite generated by further tempering thereafter.
[0057] Average grain size of M: 7μm or less If the average grain size of martensite is larger than 7 μm, voids generated at the interface between martensite and ferrite are easily connected, and the hole expandability is deteriorated. In addition, the grains after resistance welding become coarse, and the cross tensile strength is reduced. Therefore, the average grain size of martensite at the 1 / 4 position of the plate thickness is set to 7 μm or less, preferably 6 μm or less. On the other hand, the lower limit of the average grain size of martensite is not particularly limited, but may be, for example, 2 μm or more.
[0058] F: 0~5% If the volume fraction of ferrite (F) exceeds 5%, the amount of voids generated during punching increases, resulting in a decrease in hole expandability. Also, if the ferrite fraction is high, the hardness of martensite must be increased in order to ensure the desired strength. Therefore, the volume fraction of ferrite at the 1 / 4 position of the plate thickness is set to 5% or less, preferably 3% or less, and more preferably 1% or less. On the other hand, from the above viewpoint, the lower the volume fraction of ferrite, the better, so the lower limit is set to 0%.
[0059] Average grain size of F: 3μm or less If the average grain size of ferrite is larger than 3 μm, the voids generated on the punched end surface during hole expansion tend to connect during hole expansion, making it impossible to obtain the desired hole expandability. Therefore, the average grain size of ferrite at the 1 / 4 position of the plate thickness is set to 3 μm or less, preferably 2.5 μm or less. On the other hand, the lower limit of the average grain size of ferrite is not particularly limited, but may be, for example, 1 μm or more, or 2 μm or more.
[0060] RA: 0-7% If the volume fraction of retained austenite (RA) exceeds 7%, the amount of voids generated increases due to the formation of martensite during punching, and the hole expandability decreases. Therefore, the volume fraction of retained austenite at the 1 / 4 position of the plate thickness is set to 7% or less, preferably 5% or less. On the other hand, from the above viewpoint, the lower the volume fraction of retained austenite, the better, so the lower limit is set to 0%.
[0061] Average crystal grain size of RA: 3μm or less If the average grain size of the retained austenite exceeds 3 μm, the hole expandability decreases. This is because the amount of voids generated increases as a result of martensite generation during punching due to the influence of the C distribution in the retained austenite. Therefore, the average grain size of the retained austenite is set to 3 μm or less, preferably 2.5 μm or less. On the other hand, although there is no particular lower limit, if the average grain size is 0.3 μm or more, the elongation is further improved. Therefore, the average grain size of the retained austenite is preferably set to 0.3 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more.
[0062] The microstructure at the 1 / 4 position of the sheet thickness may contain other structures in addition to the structures described above. However, the volume fraction of the other structures is set to 7% or less. The other structures may be, for example, at least one structure selected from the group consisting of bainite, cementite, and pearlite.
[0063] (Microstructure from the surface to a depth of 7 μm) In the present invention, it is important to control the microstructure in the range from the surface of the steel sheet to a depth of 7 μm, the reason for which will be explained below.
[0064] As an index of the hole expandability of a steel sheet, the hole expansion ratio measured by a hole expansion test is generally used. In this hole expansion test, when a steel sheet is punched with a punch, the movement of the punch is stopped at the moment when a crack penetrates the thickness direction of the test piece, and the diameter of the hole is measured. The crack advances by gradually connecting voids generated in the center of the sheet thickness, and finally penetrates to the surface layer of the steel sheet. The inventors have found that by reducing the hard phase (martensite) in the steel sheet surface layer, it is possible to suppress the crack from finally progressing to the surface layer. In addition, it has been found that the surface layer structure with the reduced hard phase has the effect of suppressing spatter (dust) generated at high current density because it is preferentially deformed when pressed by an electrode during spot welding. Furthermore, by providing a surface layer structure with a reduced hard phase, the strength of the corona bond part after spot welding is also improved.
[0065] M: 0~20% As described above, in order to improve formability and weldability, it is important to reduce the hard phase in the surface layer of the steel sheet. Specifically, if the volume fraction of martensite in the range from the surface to a depth of 7 μm is higher than 20%, the hole expandability decreases, the appropriate current range during welding becomes narrow, and the cross tensile strength decreases. Therefore, the volume fraction is set to 20% or less, preferably 15% or less. On the other hand, the lower limit of the volume fraction is set to 0%.
[0066] The microstructure in the range from the surface to a depth of 7 μm may be such that the volume fraction of martensite satisfies the above condition, and other structures are not particularly limited. However, when the above steel plate is manufactured by the manufacturing process described below, the microstructure in the range from the surface to a depth of 7 μm typically becomes a structure mainly composed of ferrite as a result of decarburization during the annealing process. Therefore, the microstructure in the range from the surface to a depth of 7 μm may be a structure mainly composed of ferrite. More specifically, the volume fraction of ferrite is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more.
[0067] The microstructure in the range from the surface to a depth of 7 μm may further contain 0 to 15% by volume of retained austenite. The microstructure may also contain other structures besides martensite, ferrite, and retained austenite. However, the volume fraction of the other structures is preferably 7% or less. The other structures may be, for example, at least one selected from the group consisting of bainite, cementite, and pearlite.
[0068] [Precipitate] The inventors have found that by dispersing fine Ti- or Nb-based precipitates in the steel sheet structure, the grain size at the nugget edge is refined even after spot welding, improving toughness. Therefore, it has been found that the cross tensile strength can be improved extremely effectively by combining the above-mentioned control of the microstructure of the steel sheet surface layer with the control of the number density of fine precipitates. Specifically, the number density of precipitates is controlled as follows.
[0069] Precipitate density: 20 / 100μm 2 End The number density of Ti precipitates having a grain size of 0.005 μm or more and less than 0.10 μm and Nb precipitates having a grain size of 0.005 μm or more and less than 0.10 μm in a range of 50 to 100 μm deep from the surface of the steel plate is 20 / 100 μm. 2If the number density is less than 20 grains / 100 μm, the grain size at the nugget edge is not sufficiently refined, and the cross tensile strength is reduced. In addition, the function as a hydrogen trap site after resistance spot welding is also insufficient, and the delayed fracture resistance is reduced. 2 On the other hand, the upper limit of the number density is not particularly limited, but in order to ensure moldability, it is set to 250 pieces / 100 μm 2 It is preferable to have less than 100 pieces / 100 μm 2 More preferably, it should be 40 pieces / 100 μm or less. 2 More preferably, the number is 30 / 100 μm or less. 2 It is most preferred that:
[0070] [Zinc-based plating layer] The steel sheet of the present invention may be a cold-rolled steel sheet having no plating layer on its surface, but it is preferable that the steel sheet has a zinc-based plating layer on at least one surface.
[0071] As the zinc-based plating layer, either a zinc plating layer or a zinc alloy plating layer can be used. In other words, the steel sheet of the present invention may be a zinc-plated steel sheet or a zinc alloy-plated steel sheet. The zinc alloy plating layer is not particularly limited, and a plating layer made of any zinc alloy can be used. As the zinc alloy plating layer, it is preferable to use a zinc alloy plating layer having any composition selected from the group consisting of Zn-Al, Zn-Al-Mg, Zn-Al-Si, Zn-Al-Mg-Si, and Zn-Al-Mg-Ni.
[0072] The zinc-based plating layer can be formed by any method. For example, the zinc-based plating layer may be any of a hot-dip zinc-based plating layer, a galvannealed hot-dip zinc-based plating layer, and an electrolytic zinc-based plating layer. In other words, the steel sheet of the present invention may be any of a hot-dip zinc-based plated steel sheet, a galvannealed hot-dip zinc-based plating steel sheet, and an electrolytic zinc-based plating steel sheet.
[0073] The coating weight of the zinc-based coating layer is not particularly limited, but from the viewpoints of corrosion resistance and ease of coating weight control, it is preferably 25 g / m per one side of the steel sheet. 2 On the other hand, from the viewpoint of adhesion of the coating layer, it is preferable that the thickness is 80 g / m2 or more per one side of the steel sheet. 2 It is preferable that:
[0074] [Pre-plated layer] When the steel sheet has a zinc-based plating layer, a pre-plating layer may be further provided between the steel sheet (base steel sheet) and the zinc-based plating layer.
[0075] The pre-plating layer is not particularly limited and may be a plating layer of any composition, but is preferably an Fe-based plating layer, and more preferably an Fe-based electroplating layer.
[0076] The Fe-based plating layer may be, for example, an Fe plating layer or an Fe alloy plating layer. Here, the Fe plating layer is a plating layer made of Fe and unavoidable impurities, and is also called a "normal Fe plating layer". On the other hand, the Fe alloy plating layer is not particularly limited and any plating layer made of an Fe alloy may be used. The Fe alloy plating layer may be, for example, a plating layer made of at least one alloy selected from the group consisting of an Fe-B alloy, an Fe-C alloy, an Fe-P alloy, an Fe-N alloy, an Fe-O alloy, an Fe-Ni alloy, an Fe-Mn alloy, an Fe-Mo alloy, and an Fe-W alloy.
[0077] In one embodiment of the present invention, the Fe-based electroplating layer preferably has a composition containing at least one selected from the group consisting of B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co in a total amount of 10% or less, with the balance being Fe and unavoidable impurities. By keeping the total amount of elements other than Fe to 10% or less, it is possible to prevent a decrease in electrolysis efficiency and form the Fe-based electroplating layer at low cost.
[0078] Since the Fe-based plating layer functions as a soft layer, the application of the Fe-based plating layer can alleviate the stress applied to the steel sheet surface during welding. Furthermore, the presence of the Fe-based plating layer not only reduces the residual stress in the resistance weld, but also improves delayed fracture resistance by allowing diffusible hydrogen to escape efficiently from the steel sheet surface.
[0079] The amount of the Fe-based coating layer is not particularly limited, but from the viewpoint of enhancing the above-mentioned effect, it is preferable to use a coating weight of 0.5 g / m2 per one side of the steel sheet. 2 It is preferable that the content is 1.0 g / m or more. 2 On the other hand, from the viewpoint of cost, the coating weight of the Fe-based plating layer is preferably 60 g / m per side. 2 It is preferable that the thickness is less than 50 g / m 2 More preferably, it is 40 g / m or less. 2 More preferably, it is 30 g / m or less. 2 It is most preferred that:
[0080] The adhesion weight of the Fe-based plating layer is measured as follows. A sample of 10×15 mm size is taken from the steel sheet after the formation of the zinc-based plating layer and embedded in resin to obtain a cross-section embedded sample. Three arbitrary points on the cross section are observed using a scanning electron microscope (SEM) to determine the thickness of the Fe-based plating layer. The acceleration voltage for the SEM observation may be 15 kV. The magnification for the SEM observation is 2000 to 10000 times depending on the thickness of the Fe-based plating layer. The average thickness measured at the three points is multiplied by the specific gravity of iron to convert it into the adhesion weight per side of the Fe-based plating layer.
[0081] [Spot welding method] In a spot welding method according to an embodiment of the present invention, a plate assembly including at least one of the above-described steel plates is clamped between a pair of welding electrodes and joined by passing current through the electrodes while applying pressure. The conditions for spot welding are not particularly limited, and general welding conditions can be adopted.
[0082] For example, two steel sheets are overlapped to form a sheet assembly. Next, the sheet assembly is sandwiched between a pair of welding electrodes from above and below, and current is passed through the sheet assembly while applying pressure and controlling it to achieve predetermined welding conditions. In this way, the steel sheets constituting the sheet assembly are joined to form a resistance spot welded member. When a cold-rolled steel sheet and a zinc-based plated steel sheet are overlapped to form a sheet assembly, the multiple steel sheets may be overlapped so that the surface of the zinc-based plated steel sheet having the zinc-based plating layer faces the cold-rolled steel sheet.
[0083] A resistance spot welding method in one embodiment of the present invention can include a main current application step of clamping the sheet assembly with the pair of welding electrodes and applying current while applying pressure to form a nugget.
[0084] The energization conditions and pressure conditions for forming the nugget in the main energization step are not particularly limited. From the viewpoint of application to structural parts of automobiles and the like, it is preferable to adjust the energization conditions and pressure conditions to the following ranges.
[0085] For example, the current value in the main current application process can be preferably 3.0 to 15.0 kA in order to obtain a stable nugget diameter. The nugget diameter adopted in the spot welded part of the steel sheet for automobiles is generally 3.0√t to 6.0√t (t is the thinnest sheet thickness in the sheet combination), and if the current value is too small, the target nugget diameter cannot be obtained stably. On the other hand, if the current value in the main current application process is larger than the above range, the nugget diameter may become too large, or the melting degree of the steel sheet may increase, and the melted weld may go out of the gap between the sheets as splashes, resulting in a small nugget diameter.
[0086] The current application time of the main current application step is preferably 0.18 to 1.0 s. This is the time required to obtain a target nugget diameter, similar to the current value of the main current application step. If the current application time of the main current application step is less than 0.18 s, it becomes difficult to form a nugget. On the other hand, if the current application time of the main current application step exceeds 1.0 s, the nugget diameter may become large, and there is a concern that the workability may decrease. However, as long as the required nugget diameter is obtained, the current application time tW of the main current application step may be shorter or longer than the above-mentioned preferred range.
[0087] The pressure conditions for the main current application process are preferably a pressure of 2.0 kN to 7.0 kN. If the pressure F in the main current application process is too large, the current diameter will increase, making it difficult to ensure the nugget diameter. On the other hand, if the pressure F in the main current application process is too small, the current diameter will become small and splashing will be more likely to occur. Therefore, it is preferable that the pressure F in the main current application process is within the above-mentioned preferred range. Note that the pressure may be limited by the capacity of the device. However, as long as the pressure is such that the required nugget diameter can be obtained, the pressure F in the main current application process may be lower or higher than the above-mentioned preferred range.
[0088] In the resistance spot welding method according to one embodiment of the present invention, a post-current may be applied after the main current step. The post-current may be applied under any conditions without particular limitations, but the current value in the post-current is preferably higher than the current value in the main current step. Specifically, the current value is preferably 1.1 times or more the current value in the main current step. The welding time in the post-current is preferably 1.0 second or less. The post-current may be applied in multiple stages, in which case the total current application time in the post-current is preferably 1.0 second or less.
[0089] In addition, after the main current application process, a tempering process may be performed to temper the periphery of the nugget. The conditions of the tempering process are not particularly limited, but the current value in the tempering process is preferably lower than the current value in the main current application process, specifically, it is preferably 0.9 times or less the current value in the main current application process. In addition, the current application time in the tempering process is preferably 2.0 seconds or less.
[0090] [Resistance spot welding components] A resistance spot welded component according to an embodiment of the present invention is a resistance spot welded component including at least one of the above-mentioned steel plates in a plate set. The resistance spot welded component can be manufactured by a general resistance spot welding method as described above.
[0091] [Steel plate manufacturing method] Next, a method for manufacturing the steel sheet of the present invention will be described. As described above, the steel sheet of the present invention may be a cold-rolled steel sheet having no plating layer on its surface, or a zinc-based plated steel sheet having a zinc-based plating layer on its surface. The zinc-based plated steel sheet may be any of an electroplated steel sheet, a hot-dip plated steel sheet, and an alloyed hot-dip plated steel sheet. Therefore, a suitable manufacturing method will be described below for each case.
[0092] First embodiment In the first embodiment of the present invention, a steel sheet satisfying the above-mentioned conditions can be manufactured by using molten steel having the above-mentioned composition as a starting material and sequentially carrying out the following steps. Note that if no plating is performed after annealing, a steel sheet (cold-rolled steel sheet) without a plating layer on the surface can be obtained. (1) Continuous casting (2) Cooling (3) Reheating (4) Hot rolling (5) Cooling (6) Winding (7) Cold rolling (8) Annealing
[0093] (1) Continuous casting First, molten steel having the above-mentioned composition is continuously cast into a steel slab. The continuous casting method has higher production efficiency than the mold casting method. The continuous casting can be performed using any continuous casting machine, but it is preferable to use a vertical bending type continuous casting machine. The vertical bending type continuous casting machine has an excellent balance between equipment cost and the surface quality of the resulting steel slab. In addition, the vertical bending type continuous casting machine is also excellent in the effect of suppressing surface cracks.
[0094] (2) Cooling Next, the steel slab obtained by the continuous casting is cooled. In the cooling, if the average cooling rate in the temperature range up to 600°C is less than 100°C / h, the weldability is reduced. This is because Mn segregation is promoted and coarse Ti-based precipitates and Nb-based precipitates remain even after final annealing. Therefore, the steel slab is cooled under the condition that the average cooling rate in the temperature range up to 600°C is 100°C / h or more. On the other hand, the upper limit of the average cooling rate is not particularly limited, but it is preferably 150°C / h or less, and more preferably 130°C / h or less.
[0095] In the present invention, as described above, it is sufficient to control the average cooling rate in the temperature range up to 600° C., and the cooling stop temperature is not particularly limited. In other words, it can be cooled to any temperature below 600° C. For example, it may be cooled to room temperature, reheated and hot rolled, or it may be cooled to a temperature higher than room temperature to form a hot slab, which is then reheated and hot rolled.
[0096] (3) Reheating Next, the cooled steel slab is reheated, which allows the Ti-based precipitates, Nb-based precipitates, and other precipitates contained in the steel to be redissolved.
[0097] ·Heating temperature: 1250~1450℃ If the heating temperature in the reheating is less than 1250°C, the precipitates cannot be sufficiently redissolved, and the coarse precipitates remain even after the final annealing. As a result, the number density of fine Ti precipitates and Nb precipitates cannot be set within the desired range, and the weldability is reduced. Therefore, the heating temperature is set to 1250°C or higher, preferably 1270°C or higher. On the other hand, if the heating temperature is higher than 1450°C, the crystal grains become coarse. As a result, the desired crystal grain size cannot be obtained after the final annealing, and the hole expandability and resistance weldability are reduced. Therefore, the heating temperature is set to 1450°C or lower, preferably 1410°C or lower.
[0098] ·Holding time: 60 minutes or more If the holding time in the reheating is less than 60 minutes, the precipitates cannot be sufficiently redissolved, and coarse precipitates remain even after the final annealing. As a result, the number density of fine Ti precipitates and Nb precipitates cannot be set within the desired range, and weldability is reduced. Therefore, the holding time is set to 60 minutes or more. On the other hand, the upper limit of the holding time is not particularly limited, but from the viewpoint of productivity, it is preferably set to 180 minutes or less, and more preferably set to 150 minutes or less.
[0099] (4) Hot rolling Next, the reheated steel slab is hot-rolled to obtain a hot-rolled steel sheet. In the hot rolling, the structure in the steel sheet is made uniform and the anisotropy of the material is reduced, thereby improving the elongation and hole expandability after annealing.
[0100] Finish rolling temperature: 850~950℃ In order to obtain the above effect, it is necessary to finish hot rolling in the austenite single phase region. Therefore, the finish rolling end temperature is set to 850°C or higher. On the other hand, if the finish rolling end temperature is higher than 950°C, the structure of the hot rolled steel sheet becomes coarse and the properties after annealing deteriorate. Therefore, the finish rolling end temperature is set to 950°C or lower.
[0101] (5) Cooling Next, the hot-rolled steel sheet is cooled. The steel sheet structure of the hot-rolled steel sheet is controlled by quenching to a temperature range where bainite transformation occurs without causing ferrite transformation. This homogenized hot-rolled structure control has the effect of refining the final steel sheet structure, mainly ferrite and martensite.
[0102] ·Average cooling rate: 80℃ / s or more In order to obtain the above-mentioned effect, the average cooling rate is set to 80°C / s or more. If the average cooling rate is less than 80°C / s, ferrite transformation will start, so that the steel sheet structure of the hot-rolled steel sheet will become inhomogeneous, and the hole expandability and resistance weldability after annealing will decrease. On the other hand, the upper limit of the average cooling rate is not particularly limited, but is preferably set to 200°C / s or less, more preferably set to 150°C / s or less, and even more preferably set to 120°C / s or less.
[0103] ·Cooling stop temperature: 480℃ or less Similarly, in order to obtain the above effect, the cooling stop temperature is set to 480°C or less, preferably 450°C or less. If the cooling stop temperature is higher than 480°C, pearlite is generated excessively, the steel sheet structure of the hot-rolled steel sheet becomes inhomogeneous, and the hole expandability and resistance weldability after annealing are reduced. On the other hand, the lower limit of the cooling stop temperature is not particularly limited, but it is preferably set to 250°C or more.
[0104] (6) Winding · Winding temperature: 480℃ or less Next, the cooled hot-rolled steel sheet is coiled at a coiling temperature of 480°C or less. If the coiling temperature is higher than 480°C, Ti-based precipitates and Nb-based precipitates become coarse, and resistance weldability is reduced. Therefore, the coiling temperature is set to 480°C or less, preferably 450°C or less. Although there is no particular limit to the lower limit of the coiling temperature, if the coiling temperature is too low, hard martensite is excessively generated, and the cold rolling load increases. Therefore, the coiling temperature is preferably set to 250°C or more, more preferably 300°C or more, and even more preferably 350°C or more.
[0105] (7) Cold rolling After the coiling, the hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. The cold-rolling conditions are not particularly limited, and the cold-rolling can be performed according to a conventional method.
[0106] In addition, it is preferable to carry out pickling prior to the cold rolling. By carrying out pickling, scale on the surface layer of the hot-rolled sheet can be removed. The conditions for the pickling are not particularly limited, and the pickling can be carried out according to a conventional method.
[0107] (8) Annealing Next, the cold-rolled steel sheet is annealed, which promotes recrystallization and forms a structure (martensite) required to obtain a desired hardness.
[0108] ·Dew point: over -20℃ In the annealing, the C concentration in the steel sheet surface layer decreases as a result of the reaction of C with moisture in the atmosphere. This allows the volume fraction of martensite in the steel sheet surface to be reduced. However, if the dew point is less than -20°C, the microstructure of the steel sheet surface layer will not be as desired, resulting in reduced resistance weldability. Therefore, the dew point of the annealing atmosphere is set to be greater than -20°C, preferably -15°C or higher, and more preferably -10°C or higher. There is no particular upper limit to the dew point of the annealing atmosphere, but from the viewpoint of improving adhesion when a zinc-based plating layer is provided on the steel sheet surface, it is preferably set to 30°C or lower, more preferably 10°C or lower, and even more preferably 5°C or lower.
[0109] In the annealing, first, the cold-rolled steel sheet is heated to an annealing temperature of 780 to 980° C. at an average heating rate of 3 to 30° C. / s, and then held (soaked) at the annealing temperature for a holding time of 15 to 360 seconds.
[0110] ·Average heating rate: 3~30℃ / s The annealing can refine the crystal grains. However, if the material is heated too quickly, recrystallization does not proceed sufficiently, and the desired crystal grain size cannot be obtained. Therefore, the average heating rate in the heating is set to 30°C / s or less. On the other hand, if the heating rate is too slow, the Ti-based precipitates and Nb-based precipitates become coarse, and the resistance weldability is reduced. Therefore, the average heating rate is set to 3°C / s or more, and preferably 5°C / s or more.
[0111] Annealing temperature: 760~980℃ The annealing must be performed in the two-phase region of ferrite and austenite or in the austenite single-phase region. If the annealing temperature is less than 760°C, the ferrite fraction increases, making it impossible to achieve strength, hole expandability, and resistance weldability at the same time. Therefore, the annealing temperature is set to 760°C or higher, preferably 820°C or higher, and more preferably 850°C or higher. On the other hand, if the annealing temperature is too high, the growth of austenite crystal grains becomes significant, and the crystal grains become coarse, resulting in a decrease in resistance weldability. Therefore, the annealing temperature is set to 980°C or lower, and preferably 950°C or lower.
[0112] ·Holding time: 15~360 seconds By holding at the annealing temperature, recrystallization is promoted and part or all of the structure is transformed into austenite. If the holding time is less than 15 seconds, the desired microstructure cannot be obtained. Therefore, the holding time is set to 15 seconds or more. On the other hand, if the holding time is longer than 360 seconds, Ti-based precipitates or Nb-based precipitates become coarse, which reduces resistance weldability. Therefore, the holding time is set to 360 seconds or less, preferably 300 seconds or less.
[0113] After holding at the annealing temperature, the material is cooled to room temperature at an average cooling rate of 3° C. / s or more.
[0114] ·Average cooling rate: 3℃ / s or more If the average cooling rate in the cooling is less than 3°C / s, the desired martensite volume fraction cannot be obtained, and the strength and hole expandability are reduced. Therefore, the average cooling rate is set to 3°C / s or more. On the other hand, the upper limit of the average cooling rate is not particularly limited, but it is preferably less than 100°C / s, more preferably 50°C / s or less, and even more preferably 20°C / s or less.
[0115] After the annealing, temper rolling may be further performed. The temper rolling may be performed under any conditions, but it is preferable that the elongation rate is 0.05% to 2.0%.
[0116] Second embodiment In a second embodiment of the present invention, the annealed steel sheet may be electroplated to form a zinc-based plating layer on at least one surface of the steel sheet. By this method, an electrolytic zinc-based plated steel sheet can be obtained.
[0117] (Electroplating) The electroplating can be carried out under any conditions without any particular limitation. That is, in the present invention, the desired characteristics are achieved by controlling the microstructure and precipitates of the base steel sheet, so that the plating treatment conditions are not limited and the plating can be carried out according to a conventional method.
[0118] Third embodiment In the third embodiment of the present invention, a steel sheet satisfying the above-mentioned conditions can be manufactured by using molten steel having the above-mentioned composition as a starting material and sequentially carrying out the following steps. According to this method, a hot-dip galvanized steel sheet having a hot-dip galvanized layer on the surface can be obtained. (1) Continuous casting (2) Cooling (3) Reheating (4) Hot rolling (5) Cooling (6) Winding (7) Cold rolling (8) Annealing (9) Hot-dip plating (10) Cooling
[0119] In this embodiment, the above steps (1) to (7) can be carried out under the same conditions as in the first embodiment, so steps (8) to (10) will be described below.
[0120] (8) Annealing In this embodiment, the cold-rolled steel sheet obtained in the cold rolling process is annealed prior to hot-dip plating.
[0121] ·Dew point: over -20℃ In the annealing, the C concentration in the steel sheet surface layer decreases as a result of the reaction of C with moisture in the atmosphere. This allows the volume fraction of martensite in the steel sheet surface to be reduced. However, if the dew point is less than -20°C, the microstructure of the steel sheet surface layer will not be as desired, resulting in reduced resistance weldability. Therefore, the dew point of the annealing atmosphere is set to be greater than -20°C, preferably -15°C or higher, and more preferably -10°C or higher. There is no particular upper limit to the dew point of the annealing atmosphere, but from the viewpoint of improving adhesion when a zinc-based plating layer is provided on the steel sheet surface, it is preferably set to 30°C or lower, more preferably 10°C or lower, and even more preferably 5°C or lower.
[0122] In the annealing, first, the cold-rolled steel sheet is heated to an annealing temperature of 780 to 980° C. at an average heating rate of 3 to 30° C. / s, and then held (soaked) at the annealing temperature for a holding time of 15 to 360 seconds.
[0123] ·Average heating rate: 3~30℃ / s The annealing can refine the crystal grains. However, if the material is heated too quickly, recrystallization does not proceed sufficiently, and the desired crystal grain size cannot be obtained. Therefore, the average heating rate in the heating is set to 30°C / s or less. On the other hand, if the heating rate is too slow, the Ti-based precipitates and Nb-based precipitates become coarse, and the resistance weldability is reduced. Therefore, the average heating rate is set to 3°C / s or more, and preferably 5°C / s or more.
[0124] Annealing temperature: 760~980℃ The annealing must be performed in the two-phase region of ferrite and austenite or in the austenite single-phase region. If the annealing temperature is less than 760°C, the ferrite fraction increases, making it impossible to achieve strength, hole expandability, and resistance weldability at the same time. Therefore, the annealing temperature is set to 760°C or higher, preferably 820°C or higher, and more preferably 850°C or higher. On the other hand, if the annealing temperature is too high, the growth of austenite crystal grains becomes significant, and the crystal grains become coarse, resulting in a decrease in resistance weldability. Therefore, the annealing temperature is set to 980°C or lower, and preferably 950°C or lower.
[0125] ·Holding time: 15~360 seconds By holding at the annealing temperature, recrystallization is promoted and part or all of the structure is transformed into austenite. If the holding time is less than 15 seconds, the desired microstructure cannot be obtained. Therefore, the holding time is set to 15 seconds or more. On the other hand, if the holding time is longer than 360 seconds, Ti-based precipitates or Nb-based precipitates become coarse, which reduces resistance weldability. Therefore, the holding time is set to 360 seconds or less, preferably 300 seconds or less.
[0126] ·Average cooling rate: 3℃ / s or more After the above-mentioned holding, the steel sheet is cooled from the annealing temperature to the immersion in the hot-dip galvanizing bath at an average cooling rate of 3°C / s or more. If the average cooling rate in the above-mentioned cooling is less than 3°C / s, the desired martensite volume fraction cannot be obtained, and the strength and hole expandability are reduced. Therefore, the average cooling rate is set to 3°C / s or more. On the other hand, the upper limit of the average cooling rate is not particularly limited, but it is preferably less than 100°C / s, more preferably 50°C / s or less, and even more preferably 20°C / s or less.
[0127] (9) Hot-dip plating In the present embodiment, the annealed steel sheet is subjected to hot-dip galvanization to form a hot-dip galvanized layer on at least one surface of the steel sheet. By this method, a hot-dip galvanized steel sheet can be obtained.
[0128] The hot-dip galvanizing can be carried out by any method. That is, in the present invention, the desired characteristics are achieved by controlling the microstructure and precipitates of the base steel sheet, so that the plating treatment conditions are not particularly limited and the hot-dip galvanizing can be carried out according to a conventional method.
[0129] In the hot-dip plating, any hot-dip plating bath can be used without any particular limitation, but it is preferable to use a hot-dip plating bath having a composition consisting of Al, Zn, and unavoidable impurities. The Al concentration in the plating bath is not particularly limited, but may be, for example, 0.05% to 0.25%. If the Al concentration is 0.05% or more, the generation of bottom dross is suppressed, and the dross can be prevented from adhering to the steel sheet and causing defects. On the other hand, if the Al concentration is 0.25% or less, the increase in top dross is suppressed, and the dross can be prevented from adhering to the steel sheet and causing defects. In addition, by lowering the Al concentration, the material cost can be reduced.
[0130] Other conditions for the hot-dip galvanizing are not particularly limited. For example, the temperature of the hot-dip galvanizing bath is preferably 440 to 500°C, which is the bath temperature in general hot-dip galvanizing. In addition, the temperature of the steel sheet when entering the hot-dip galvanizing bath (entry sheet temperature) is preferably 440 to 550°C.
[0131] In addition, after the hot-dip galvanizing process, the coating weight may be adjusted. The method for adjusting the coating weight is not particularly limited, but typically, the coating weight is adjusted by gas wiping. The coating weight is adjusted by adjusting the gas wiping conditions, such as the gas pressure and the distance between the wiping nozzle and the steel sheet.
[0132] (10) Cooling Next, the steel sheet after the hot dip plating is cooled to room temperature at an average cooling rate of 3°C / s or more. If the average cooling rate in the cooling is less than 3°C / s, the desired martensite volume fraction cannot be obtained, and the strength and hole expandability are reduced. Therefore, the average cooling rate is set to 3°C / s or more. On the other hand, the upper limit of the average cooling rate is not particularly limited, but it is preferably less than 100°C / s, more preferably 50°C / s or less, and even more preferably 20°C / s or less.
[0133] Thus, in this embodiment, in order to obtain a desired microstructure, it is important to set the average cooling rate in both the annealing process and the cooling after hot-dip plating to 3° C. / s or more.
[0134] Fourth embodiment In a fourth embodiment of the present invention, after the hot-dip plating, an alloying treatment is performed prior to the cooling to room temperature. The hot-dip galvanized layer is alloyed by the alloying treatment, and a galvannealed steel sheet can be obtained.
[0135] (Alloying treatment) The alloying treatment can be carried out under any conditions without any particular limitation. That is, in the present invention, the desired properties are achieved by controlling the microstructure and precipitates of the base steel sheet, so that the alloying treatment conditions are not limited and can be carried out according to a conventional method.
[0136] The alloying treatment is preferably carried out at a temperature of 450°C or higher and 600°C or lower. By carrying out the alloying treatment at 450°C or higher, it is possible to provide a steel sheet with excellent press formability without leaving η phase in the plating layer. Furthermore, by carrying out the alloying treatment at 600°C or lower, good plating adhesion can be obtained. The alloying time is preferably 5 to 60 seconds.
[0137] (Pre-plating) Furthermore, in another embodiment of the present invention, prior to plating to form a zinc-based plating layer, pre-plating can be optionally further performed to form a pre-plated layer on the steel sheet surface.
[0138] The timing of the pre-plating is not particularly limited, and may be any timing before plating for forming a zinc-based plating layer. Typically, when a zinc-based plating layer is formed by electroplating, it is preferable to perform pre-plating after the annealing and before the electroplating. That is, annealing, pre-plating, and electrogalvanizing may be sequentially performed on the cold-rolled steel sheet. On the other hand, when a zinc-based plating layer is formed by hot-dip plating, it is preferable to perform pre-plating after the cold rolling and before the annealing. That is, the treatments may be performed in the order of cold rolling, pre-plating, annealing, and hot-dip zinc-based plating. In addition, when an alloying treatment is performed, it may be performed after the hot-dip zinc plating as usual.
[0139] In the pre-plating, any pre-plating layer can be formed, but it is preferable to form an Fe-based plating layer. The Fe-based plating layer is preferably formed by electroplating. Hereinafter, a case where an Fe-based plating layer is formed as a pre-plating layer by performing an Fe-based electroplating process will be described.
[0140] The Fe-based electroplating method is not particularly limited. For example, any bath such as a sulfuric acid bath, a hydrochloric acid bath, or a sulfuric acid + hydrochloric acid bath can be used as the Fe-based electroplating bath.
[0141] The Fe ion content in the Fe-based electroplating bath before the start of current application is 2+ The Fe ion content in the Fe-based electroplating bath is preferably 1.0 mol / L or more. 2+ If the concentration of the iron in the bath is 1.0 mol / L or more, a sufficient amount of iron can be deposited. The iron-based electroplating bath may contain Fe ions, as well as alloying elements such as B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co, and may also contain conductivity aids such as sodium sulfate and potassium sulfate as additives or impurities. Metal elements may be contained as metal ions, and nonmetal elements may be contained as parts of boric acid, phosphoric acid, nitric acid, organic acids, etc. The iron sulfate plating solution may also contain conductivity aids such as sodium sulfate and potassium sulfate, chelating agents, and pH buffers.
[0142] It is also possible to subject the cold-rolled steel sheet to Fe-based electroplating treatment without carrying out oxidation treatment in a preheating furnace or the like.
[0143] Other conditions for the Fe-based electroplating bath are not particularly limited. The bath temperature is preferably 30°C or higher in consideration of the ability to maintain a constant temperature. The pH of the Fe-based electroplating bath is not particularly specified, but is preferably 3.0 or less in consideration of the electrical conductivity of the Fe-based electroplating bath. The current density is not particularly limited, but is usually 10 to 150 A / dm 2 The sheet passing speed may be 5 mpm or more and 150 mpm or less. If the sheet passing speed is less than 5 mpm, the productivity is poor, while if the sheet passing speed is 150 mpm or more, it is difficult to stably control the coating weight.
[0144] In addition, as a treatment before the Fe-based electroplating treatment, a degreasing treatment and water washing for cleaning the surface of the cold-rolled steel sheet, and further, a pickling treatment and water washing for activating the surface can be performed. It is preferable to perform the Fe-based electroplating treatment following these pretreatments. The method of the degreasing treatment and water washing is not particularly limited, and a normal method can be used. In the pickling treatment, various acids such as sulfuric acid, hydrochloric acid, nitric acid, and mixtures thereof can be used. Among them, sulfuric acid, hydrochloric acid, or mixtures thereof are preferable. The concentration of the acid is not particularly specified, but considering the ability to remove the oxide film and the prevention of roughness (surface defects) due to excessive pickling, it is preferable to have a concentration of about 1 to 20 mass%. In addition, the pickling treatment solution may contain an antifoaming agent, a pickling promoter, a pickling inhibitor, etc. EXAMPLES
[0145] In order to confirm the effects of the present invention, steel sheets were produced by the following procedure, and their properties were evaluated. Four types of steel sheets were produced: cold-rolled steel sheet (CR), electrogalvanized steel sheet (EG), hot-dip galvanized steel sheet (GI), and galvannealed steel sheet (GA).
[0146] First, molten steel having the composition shown in Table 1 was continuously cast into a steel slab, which was then cooled at the average cooling rate shown in Table 2.
[0147] The cooled steel slab was reheated under the conditions shown in Table 2, and then hot rolled under the conditions shown in Table 2 to obtain a hot-rolled steel sheet. The hot-rolled steel sheet was cooled to a coiling temperature (CT) under the conditions shown in Table 2, and wound into a coil. Thereafter, the hot-rolled steel sheet was pickled and cold-rolled at a reduction ratio of 50% to obtain a cold-rolled steel sheet having a thickness of 1.4 mm.
[0148] In producing the cold-rolled steel sheets (CR), the cold-rolled steel sheets were annealed under the conditions shown in Table 2, and then cooled to room temperature at the average cooling rate shown in Table 2.
[0149] In the production of the electrogalvanized steel sheet (EG), the cold-rolled steel sheet was first annealed under the conditions shown in Table 2 and cooled to room temperature at the average cooling rate shown in Table 2. Then, electroplating was performed to form an electrogalvanized layer on the surface of the steel sheet. 2+ The plating was carried out using a sulfuric acid bath containing 1.5 mol / L of ...
[0150] In the production of hot-dip galvanized steel sheet (GI), the cold-rolled steel sheet was first annealed under the conditions shown in Table 2, and then cooled to the point of entering the hot-dip galvanizing bath at the average cooling rate shown in Table 2. The steel sheet was then immersed in the hot-dip galvanizing bath to form a hot-dip galvanized layer on the surface of the steel sheet. The hot-dip galvanizing bath used was a plating bath consisting of Al, Zn, and unavoidable impurities, with an Al concentration of 0.14% in the bath. The temperature of the hot-dip galvanizing bath was 460°C.
[0151] In the production of the alloyed hot-dip galvanized steel sheet (GA), the cold-rolled steel sheet was first annealed under the conditions shown in Table 2, and then cooled to the point of immersion in the hot-dip galvanizing bath at the average cooling rate shown in Table 2. Thereafter, the hot-dip galvanized layer was alloyed by an alloying treatment. The hot-dip galvanizing bath had the same composition as the galvanizing bath used in the production of the hot-dip galvanized steel sheet (GI), and the temperature of the galvanizing bath was also the same. The alloying treatment was carried out at a temperature of 550°C.
[0152] Next, the microstructure and precipitate density of the obtained steel sheet were measured by the following procedure. The obtained results are shown in Table 3.
[0153] (Microstructure at 1 / 4 thickness position) Ferrite, martensite The volume fractions of ferrite and martensite in the steel sheet were measured by the following procedure. First, a cross section of the steel sheet parallel to the rolling direction was polished and etched with 3% nital to reveal the structure. The cross section was then observed at a magnification of 3000 times using a SEM (scanning electron microscope), and an SEM image of the microstructure at the 1 / 4 position of the sheet thickness was obtained. The area fractions of ferrite and martensite in the SEM image were calculated by the point count method (in accordance with ASTM E562-83 (1988)), and these area fractions were taken as volume fractions.
[0154] The average grain size of ferrite and martensite was determined by image analysis of the SEM image obtained by the above SEM observation. Specifically, the area of each grain of ferrite and martensite in the SEM image was first determined by image analysis. Next, the circle equivalent diameter of the grain was calculated from the area, and the average value was taken as the average grain size. Image-Pro by Media Cybernetics was used for the image analysis.
[0155] ·Residual austenite The volume fraction of the retained austenite was determined by X-ray diffraction. Specifically, the steel sheet was first polished to 1 / 4 of the sheet thickness direction, and the diffracted X-ray intensity at the 1 / 4 sheet thickness direction was measured by X-ray diffraction. The measurement was performed using an X-ray diffractometer RINT2200 manufactured by Rigaku Corporation, with Mo Kα radiation as the radiation source and an acceleration voltage of 50 keV. The integrated intensities of X-ray diffraction lines of the {200}, {211}, and {220} planes of ferrite and the {200}, {220}, and {311} planes of austenite were measured, and the volume fraction of the retained austenite was calculated from the obtained integrated intensities. For the calculation, a calculation formula described on pages 26, 62-64 of "X-ray Diffraction Handbook" (2000, Rigaku Denki Co., Ltd.) was used.
[0156] The average grain size of the retained austenite grains was determined by polishing the cross section up to 1 / 4 of the plate thickness, corroding it with 3% nital, and analyzing the TEM image obtained by TEM observation. Specifically, first, a TEM was used to observe at a magnification of 15,000 times to obtain a TEM image of the microstructure at the 1 / 4 plate thickness position. The obtained TEM image was analyzed to determine the area of each retained austenite grain. Next, the circle equivalent diameter of each grain was calculated from the area, and the average value was taken as the average grain size of the retained austenite. Media Cybernetics' Image-Pro was used for the image analysis.
[0157] (Microstructure from the surface of the steel plate to a depth of 7 μm) The microstructure of the steel sheet in the range from the surface to a depth of 7 μm was observed by SEM, and the volume fraction of martensite was calculated. When the measurement target was a steel sheet having a plating layer (EG, GI, and GA), the intensity profile was measured from the surface of the steel sheet by glow discharge optical emission spectrometry, and the point where the intensity profile of Fe exceeded the intensity profile of Zn was defined as the steel sheet surface. The martensite volume fraction was calculated from the SEM image in the same manner as the calculation of the martensite volume fraction at the 1 / 4 position of the sheet thickness.
[0158] (Number density of precipitates) The number density of Ti-based precipitates and Nb-based precipitates was determined by TEM-EDS (energy dispersive X-ray analysis). Specifically, first, the L-section of the steel sheet was observed at a magnification of 10,000 times by TEM, and TEM images of 10 locations randomly selected from the range of 5 to 100 μm deep from the surface of the steel sheet were obtained. Next, the Ti-based precipitates and Nb-based precipitates in the TEM images were identified by EDS. The TEM images were analyzed using Image-Pro, and the areas of the individual Ti-based precipitates and Nb-based precipitates were obtained. From the areas, the circle-equivalent diameters of the individual particles were calculated. Then, the number of Ti-based precipitates and Nb-based precipitates with a circle-equivalent diameter of 0.005 μm or more and less than 0.10 μm was counted, and the number density of the precipitates was obtained by dividing the number by the area of the observed range. The number densities of precipitates were calculated in the same manner for the TEM images obtained by observing the above 10 locations, and the average values were taken as the number densities of Ti-based precipitates and Nb-based precipitates.
[0159] Next, the strength, formability, and weldability of the obtained steel sheets were evaluated by the following procedures. The obtained results are shown in Table 3.
[0160] (strength) A JIS No. 5 tensile test piece was taken from the steel plate so that the tensile direction was the direction perpendicular to the rolling direction. A tensile test was then performed using the test piece to measure the tensile strength (TS) of the steel plate. The tensile test was performed in accordance with JIS Z2241 (1998).
[0161] (Moldability) The hole expansion ratio was measured as an index of the formability (hole expandability) of the steel sheet. The measurement was performed in accordance with the Japan Iron and Steel Federation standard (JIS Z2256 (2010)). Specifically, a hole of 10 mmφ was punched with a clearance of 12.5%. Next, the punched test piece was set in a testing machine so that the burr was on the die side, and then formed with a 60° conical punch to measure the hole expansion ratio (λ). If λ (%) is 25% or more, it is considered to have good hole expandability.
[0162] (Weldability) As an index of weldability, the optimum current range in resistance spot welding and cross tensile strength were evaluated.
[0163] - Appropriate current range The appropriate current range was evaluated by the following procedure. First, a test piece of 20 mm x 50 mm was cut out from the steel plate. Next, two of the same test pieces were combined into one plate and resistance spot welded. For the resistance spot welding, a servo motor pressure type single-phase AC (50 Hz) resistance welding machine was used. As the electrode tip, a DR type electrode made of alumina-dispersed copper with a tip curvature radius of R40 mm and tip diameter of 6 mm was used. The welding conditions were a pressure of 4000 N, current flow time of 20 cycles (50 Hz), and hold time of 5 cycles (50 Hz).
[0164] The welding current was increased in 0.1 kA increments from 3.0 kA, and the maximum current value at which no spatter (flash) occurred was recorded. The nugget diameter was measured by observing the cross section of the welded part of the test piece after welding, and the difference between the minimum current at which the nugget diameter was 4.0√t (mm) or more for the plate thickness t (mm) and the maximum current value at which no spatter occurred was determined to be the optimum current range for welding. An optimum current range of 1.2 kA or more was rated "good," and one below 1.2 kA was rated "poor."
[0165] ·Cross tensile strength The cross tensile strength after resistance spot welding was measured based on the cross tensile test method (JIS Z 3137). For the measurement, a 50×150 mm cross tensile test piece cut out from a steel plate was used, and resistance spot welding was performed on a plate set consisting of two of the same type of test pieces. The resistance welding conditions were that resistance spot welding was performed using a servo motor pressure type single-phase AC (50 Hz) resistance welding machine attached to a welding gun, and a tensile test piece having a resistance weld was produced. The pair of electrode tips used were DR type electrodes made of alumina-dispersed copper with a tip curvature radius R40 mm and tip diameter 6 mm. The welding conditions were as follows: pressure: 4000 N, current flow time: 20 cycles (50 Hz), hold time: 5 cycles (50 Hz). The current value was set to a current value at which the nugget diameter was 4.5√t (mm) based on the above-mentioned test in the appropriate current range. If the strength was 5.5 kN or more, the cross tensile strength after resistance spot welding was rated as "good," and if it was less than 5.5 kN, the cross tensile strength after resistance spot welding was rated as "poor."
[0166] As can be seen from the results shown in Table 3, the steel plate satisfying the conditions of the present invention had a tensile strength of 1450 MPa or more, as well as high levels of formability (hole expandability) and weldability (wide range of appropriate current, cross tensile strength).
[0167] [Table 1]
[0168] [Table 2]
[0169] [Table 3]
Claims
1. The composition is, in mass%, C: 0.18-0.38%, Si: 0.2-1.8%, Mn: 2.4 to 3.5%, P: 0.03% or less, S: 0.003% or less, Al: 0.01-0.50%, N: 0.008% or less, Nb: 0.005 to 0.08% and / or Ti: 0.005 to 0.08%, and Contains one or both of B: 0.0002 to 0.0050% and Sb: 0.001 to 0.012%, The balance consists of Fe and unavoidable impurities, and The A value defined by the following formula (1) is 0.9 to 6.0, The microstructure at the 1 / 4 position of the plate thickness satisfies the following conditions: Volume fraction of martensite: 93% or more, Volume fraction of ferrite: 0 to 5%, Volume fraction of retained austenite: 0 to 7%; Average grain size of martensite: 7 μm or less, Average grain size of ferrite: 3 μm or less, Average grain size of retained austenite: 3 μm or less, The microstructure in the range from the surface to a depth of 7 μm satisfies the following conditions: Volume fraction of martensite: 0 to 20%, The number density of Ti precipitates having a grain size of 0.005 μm or more and less than 0.10 μm and Nb precipitates having a grain size of 0.005 μm or more and less than 0.10 μm in the range of a depth from the surface of 50 to 100 μm is 20 / 100 μm. 2 That's it, steel plate. A=([C]+[Si] / 8+[Mn] / 20) / (2×([Ti]+[Nb])+85×([B]+[Sb] / 20)…(1) However, the parentheses in the above formula (1) represent the content (mass %) of the element in the parentheses, and if the element is not contained, the value is set to 0.
2. The composition further comprises, in mass%, V: 0.05% or less, Cu: 0.50% or less, Ni: 0.50% or less, Mo: 0.50% or less, Cr: 0.50% or less, Sn: 0.30% or less, Ca: 0.0050% or less, and REM: 0.0050% or less The steel plate according to claim 1, comprising at least one selected from the group consisting of:
3. The steel sheet according to claim 1 , further comprising a zinc-based plating layer on at least one surface.
4. The steel plate of claim 2, further comprising a zinc-based plating layer on at least one surface.
5. A resistance spot welding method comprising: clamping a plate assembly including at least one steel plate according to any one of claims 1 to 4 between a pair of welding electrodes; and joining the plate assembly by passing current through the plate assembly while applying pressure.
6. A resistance spot welded component comprising at least one steel plate according to any one of claims 1 to 4 in a plate assembly.
7. 3. A steel slab is formed by continuously casting a molten steel having the composition according to claim 1 or 2, The steel slab is cooled at an average cooling rate of 100° C. / h or more in a temperature range up to 600° C., The cooled steel slab is reheated by heating it to a heating temperature of 1250 to 1450°C and holding it at the heating temperature for 60 minutes or more; The reheated steel slab is hot-rolled under a finish rolling temperature of 850 to 950°C to obtain a hot-rolled steel sheet. The hot-rolled steel sheet is cooled at an average cooling rate of 80° C. / s or more to a cooling stop temperature of 480° C. or less, The cooled hot-rolled steel sheet is coiled at a coiling temperature of 480° C. or less, The hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. The cold-rolled steel sheet is annealed in an atmosphere having a dew point of more than −20° C., In the annealing, the cold-rolled steel sheet is Heat to an annealing temperature of 780 to 980°C at an average heating rate of 3 to 30°C / s. Holding at the annealing temperature for a holding time of 15 to 360 seconds; Cooling from the annealing temperature to room temperature at an average cooling rate of 3° C. / s or more; Manufacturing method of steel plate.
8. The method for producing a steel sheet according to claim 7, further comprising electroplating the annealed steel sheet to form a zinc-based plating layer on at least one surface of the steel sheet.
9. The molten steel having the composition according to claim 1 or 2 is continuously cast into a steel slab, The steel slab is cooled at an average cooling rate of 100° C. / h or more in a temperature range up to 600° C., The cooled steel slab is reheated by heating it to a heating temperature of 1250 to 1450°C and holding it at the heating temperature for 60 minutes or more; The reheated steel slab is hot-rolled under a finish rolling temperature of 850 to 950°C to obtain a hot-rolled steel sheet. The hot-rolled steel sheet is cooled at an average cooling rate of 80° C. / s or more to a cooling stop temperature of 480° C. or less, The cooled hot-rolled steel sheet is coiled at a coiling temperature of 480° C. or less, The hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. The cold-rolled steel sheet is annealed in an atmosphere having a dew point of more than −20° C. The annealed steel sheet is subjected to hot-dip galvanization by immersing the steel sheet in a hot-dip galvanizing bath to form a zinc-based plating layer on at least one surface of the steel sheet; The method for producing a steel sheet includes cooling the steel sheet after the hot-dip galvanization to room temperature at an average cooling rate of 3 ° C. / s or more, In the annealing, the cold-rolled steel sheet is Heat to an annealing temperature of 780 to 980°C at an average heating rate of 3 to 30°C / s. Holding at the annealing temperature for a holding time of 15 to 360 seconds; Cooling from the annealing temperature to the immersion in the hot-dip galvanizing bath at an average cooling rate of 3 ° C. / s or more; Manufacturing method of steel plate.
10. The method for producing a steel sheet according to claim 9, further comprising the step of: subjecting the steel sheet to an alloying treatment after the hot-dip galvanizing and before the cooling to room temperature.