Laminate and method for manufacturing circuit board
Patent Information
- Application Number
- JP2025512454
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-05
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2044-03-07
AI Technical Summary
Existing laminate technologies face issues with acid resistance and interlayer adhesion, leading to poor reliability of circuit boards due to erosion of metal plating layers and stress-induced delamination during manufacturing processes.
A laminate comprising a film with a thermoplastic polyimide resin layer, a palladium-based catalyst layer, and an electroless plating layer containing nickel and copper, along with an optional electrolytic plating layer, is developed to enhance acid resistance and interlayer adhesion, utilizing specific composition and processing conditions to form a robust circuit board structure.
The proposed laminate structure significantly improves acid resistance and interlayer adhesion, thereby increasing the reliability of circuit boards by preventing erosion and delamination, ensuring durable and reliable circuit performance.
Abstract
Description
Laminate and method for manufacturing circuit board
[0001] The present invention relates to a laminate and a method for manufacturing a circuit board.
[0002] 2. Description of the Related Art Circuit boards on which integrated circuits (ICs) can be mounted have fine wiring formed thereon.
[0003] Patent Document 1 discloses a laminate as a component constituting a circuit board, which includes a substrate, a plating layer laminated on the substrate, and a metal plating layer laminated on the plating layer. The plating layer is composed of a thermoplastic resin and a plating catalyst.
[0004] Patent Document 2 discloses a laminate including a substrate made of glass cloth and resin, a copper layer formed on the substrate, a first insulating material layer formed on the copper layer, and a seed layer formed on the first insulating material layer. The first insulating material layer is made of a thermosetting resin and has a catalyst adsorbed on its surface. The seed layer is made of electroless plating containing nickel and copper.
[0005] International Publication No. WO 2020 / 050338 International Publication No. WO 2020 / 130101
[0006] The laminate disclosed in Patent Document 1 has the following problem when forming fine wiring on the laminate: A resist pattern made of resin is formed on a metal plating layer, and wiring is formed by electrolytic plating. The resist pattern is then removed, and the metal plating layer exposed after removal and the plating formation layer underneath are removed with an acidic chemical solution. During this process, the metal plating layer underneath the wiring is easily eroded by the chemical solution. Therefore, the laminate disclosed in Patent Document 1 may have poor acid resistance. As a result, the reliability of the circuit on a circuit board using this laminate may be poor.
[0007] Furthermore, the laminate disclosed in Patent Document 2 has the following problem during its manufacturing process: The seed layer is formed on the first insulating material layer by electroless plating. During this process, stress is generated within the seed layer. The laminate cannot relieve this stress, and peeling is likely to occur between the first insulating material layer and the seed layer. Therefore, the laminate disclosed in Patent Document 2 may have poor interlayer adhesion between the first insulating material layer and the seed layer. As a result, the reliability of the circuit on a circuit board using this laminate may be poor.
[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a laminate having excellent acid resistance and interlayer adhesion, and a method for producing a circuit board using the laminate.
[0009] The present invention is as follows: [1] A laminate according to the present invention comprises a film, a resin layer containing a thermoplastic polyimide resin and formed on at least one surface of the film, a catalyst layer containing palladium and a dispersant covering the palladium and formed on the resin layer, and an electroless plated layer containing nickel and copper and formed on the catalyst layer, wherein the nickel content is 8.0 mass % or more and 13.0 mass % or less relative to the total mass of the electroless plated layer.
[0010] [2] The amount of palladium contained in the catalyst layer is 1 dm 2 The amount may be 0.05 mg or more and 0.18 mg or less per unit area.
[0011] [3] The laminate may further include an electrolytically plated layer containing copper and formed on the electrolessly plated layer.
[0012] [4] A method for manufacturing a circuit board according to the present invention includes: a resist layer forming step of forming a resist layer on the electroless plated layer that constitutes the laminate described in [1] above; an exposure step of exposing the resist layer; a resist pattern forming step of developing the resist layer exposed in the exposure step to form a resist pattern corresponding to the wiring to be formed; a wiring layer forming step of forming a conductive wiring layer on the electroless plated layer exposed after the resist pattern forming step; a resist pattern removing step of removing the resist pattern; a flash etching step of removing the electroless plated layer exposed after the resist pattern removing step; and a catalyst layer removing step of removing the catalyst layer exposed after the flash etching step.
[0013] [5] A method for manufacturing a circuit board according to the present invention includes an electrolytic plating layer forming step of forming an electrolytic plating layer on the electroless plating layer constituting the laminate described in [1] above; a resist layer forming step of forming a resist layer on the electrolytic plating layer; an exposure step of exposing the resist layer to light; a resist pattern forming step of developing the resist layer exposed in the exposure step to form a resist pattern corresponding to the wiring to be formed; a wiring layer forming step of forming a conductive wiring layer on the electrolytic plating layer exposed after the resist pattern forming step; a resist pattern removing step of removing the resist pattern; a flash etching step of removing the electrolytic plating layer exposed after the resist pattern removing step and the electroless plating layer formed below the electrolytic plating layer; and a catalyst layer removing step of removing the catalyst layer exposed after the flash etching step.
[0014] [6] A method for manufacturing a circuit board according to the present invention includes: a resist layer forming step of forming a resist layer on the electrolytic plated layer that constitutes the laminate described in [3] above; an exposure step of exposing the resist layer; a resist pattern forming step of developing the resist layer exposed in the exposure step to form a resist pattern corresponding to the wiring to be formed; a wiring layer forming step of forming a conductive wiring layer on the electrolytic plated layer exposed after the resist pattern forming step; a resist pattern removing step of removing the resist pattern; a flash etching step of removing the electrolytic plated layer exposed after the resist pattern removing step and the electroless plated layer formed below the electrolytic plated layer; and a catalyst layer removing step of removing the catalyst layer exposed after the flash etching step.
[0015] According to the present invention, it is possible to provide a laminate having excellent acid resistance and interlayer adhesion, and a method for producing a circuit board using the laminate.
[0016] 1 is a schematic cross-sectional view of a laminate according to an embodiment of the present invention;
[0017] Hereinafter, a laminate and a method for manufacturing a circuit board, which are modes for carrying out the present invention (hereinafter referred to as embodiments), will be described in detail. The following embodiments are examples for explaining the present invention, and are not intended to limit the present invention to the following content. The present invention can be carried out with appropriate modifications within the scope of its gist.
[0018] [Laminate 10] As shown in FIG. 1 , laminate 10 of the embodiment includes film 11, resin layer 13 containing a thermoplastic polyimide resin and formed on at least one surface of film 11, catalyst layer 15 containing palladium and a dispersant that covers the palladium and formed on resin layer 13, and electroless plating layer 17 containing nickel and copper and formed on catalyst layer 15.
[0019] The laminate 10 has the above-described structure, which provides excellent acid resistance and interlayer adhesion. Furthermore, the reliability of the circuit of a circuit board using such a laminate 10 is improved. The film 11, resin layer 13, catalyst layer 15, and electroless plating layer 17 that constitute the laminate 10 will be described below.
[0020] (Film 11) The film 11 is preferably a film having dimensional stability, heat resistance, dielectric properties, etc. Examples of resins constituting a film having these properties include thermosetting polyimide, polyamideimide, liquid crystal polymer, polyphenylene sulfide, syndiotactic polystyrene, polyethylene terephthalate, polyethylene naphthalate, polycarbonate, polybutylene terephthalate, polyether ether ketone, polyether sulfone, polyphenylene ether, and fluorine-based resins.
[0021] Among the above-mentioned resins, thermosetting polyimides, which have excellent heat resistance and dimensional stability, and liquid crystal polymers and fluorine-based resins, which have excellent dielectric properties, are preferred. These resins are also preferred from the viewpoint of excellent processability. The resin constituting the film 11 may be composed of one type of resin or two or more types of resins.
[0022] The thickness of the film 11 is preferably, for example, 5 μm or more and 100 μm or less, more preferably 7.5 μm or more and 100 μm or less, and even more preferably 10 μm or more and 50 μm or less, from the viewpoint of alleviating stress that occurs when the electroless plating layer 17 is formed in the laminate 10 and from the viewpoint of improving processability.
[0023] From the viewpoint of alleviating stress generated when electroless plated layer 17 is formed and improving processability, the tensile modulus of film 11 is preferably, for example, 2 GPa or more and 10 GPa or less, and more preferably 3 GPa or more and 8 GPa or less. This alleviates stress generated when electroless plated layer 17 is formed, and prevents peeling between catalyst layer 15 and electroless plated layer 17. In other words, a laminate 10 having excellent interlayer adhesion can be obtained. The tensile modulus of film 11 can be measured by a measurement method in accordance with JIS K7161.
[0024] (Resin Layer 13) The resin constituting the resin layer 13 includes a thermoplastic polyimide resin. By including the thermoplastic polyimide resin in the resin layer 13, the interlayer adhesion between the resin layer 13 and the film 11 is improved. Furthermore, since the thermoplastic polyimide resin has a high affinity with the dispersant contained in the catalyst layer 15, the interlayer adhesion between the resin layer 13 and the catalyst layer 15 is improved. The amount of the thermoplastic polyimide resin contained in the resin layer 13 is, for example, 1% by mass or more and 100% by mass or less, preferably 20% by mass or more and 100% by mass or less, and more preferably 40% by mass or more and 100% by mass or less, relative to the total mass of the resin layer 13. The amount of the thermoplastic polyimide resin contained in the resin layer 13 represents the amount of the thermoplastic polyimide resin only, excluding volatile components such as organic solvents.
[0025] The thermoplastic polyimide resin contained in the resin layer 13 is made of, for example, a condensation polyimide, which is obtained by copolymerizing an acid dianhydride and a diamine.
[0026] The acid dianhydride may be any acid dianhydride that undergoes a condensation reaction with a diamine. Examples of the acid dianhydride include 3,4,3',4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,3,2',3'-biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, and 3,4,9,10-perylenetetracarboxylic dianhydride. Examples of the dianhydride include bis(3,4-dicarboxyphenyl)propane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)ethane dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, p-phenylene bis(trimellitic acid monoester acid anhydride), ethylene bis(trimellitic acid monoester acid anhydride), and bisphenol A bis(trimellitic acid monoester acid anhydride).
[0027] The diamine may be any diamine that undergoes a condensation reaction with an acid dianhydride, such as p-phenylenediamine, m-phenylenediamine, 2,4-diaminotoluene, 4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy) )phenyl]sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)benzidine, 2,2-bis(4-aminophenoxyphenyl)isopropane, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, and the like.
[0028] Furthermore, from the viewpoint of improving the adhesion between the resin layer 13 and the catalyst layer 15, the thermoplastic polyimide resin contained in the resin layer 13 preferably has a storage modulus at 300° C. that is less than 20% of the storage modulus at 30° C. The storage modulus can be measured by a dynamic viscoelasticity measurement method.
[0029] The tensile modulus of resin layer 13 is preferably, for example, 5 GPa or less. When the tensile modulus of resin layer 13 is 5 GPa or less, stress generated when electroless plated layer 17 is formed on catalyst layer 15 (described later) is alleviated by resin layer 13, thereby suppressing delamination between catalyst layer 15 and electroless plated layer 17. The tensile modulus of resin layer 13 can be measured in accordance with JIS K7161.
[0030] The resin layer 13 is formed on at least one surface of the film 11. The thickness of the resin layer 13 may be any thickness that can improve the adhesive strength between the resin layer 13 and the catalyst layer 15, and is, for example, from 0.01 μm to 10.0 μm, and preferably from 0.02 μm to 1.0 μm.
[0031] (Catalyst layer 15) The catalyst layer 15 is laminated on the resin layer 13. The catalyst layer 15 contains palladium that bonds with the copper contained in the electroless plating layer 17 and a dispersant that covers the palladium. The electroless plating layer 17 is formed using this palladium as a scaffold. This improves the adhesion between the electroless plating layer 17 and the catalyst layer 15. The amount of palladium contained in the catalyst layer 15 is, for example, 1 dm 2 per unit area of the surface of the resin layer 13. 2 The amount is 0.05 mg or more and 0.18 mg or less, preferably 0.08 mg or more and 0.18 mg or less, and more preferably 0.10 mg or more and 0.16 mg or less.
[0032] The dispersant that coats the palladium is composed of a compound that can bond with palladium, such as a nitrogen-containing compound containing nitrogen in its terminal functional group and / or a compound having an unsaturated bond. The bond between palladium and this compound is, for example, a coordinate bond, an ionic bond, or a covalent bond. Examples of the nitrogen-containing compound include a polymer having an ammonium group in its terminal functional group. Examples of the compound having an unsaturated bond include polyethylene glycol alkyl ether acrylate. From the viewpoint of improving the interlayer adhesion between the catalyst layer 15 and the resin layer 13, a nitrogen-containing compound is preferred, and more specifically, a polymer having an ammonium group in its terminal functional group is preferred.
[0033] (Electroless Plated Layer 17) The electroless plated layer 17 contains nickel and copper and is laminated on the catalytic layer 15. The nickel content is 8.0 mass% or more and 13.0 mass% or less, based on the total mass of the electroless plated layer 17. The electroless plated layer 17 containing nickel in the above amount has a high nickel content at the interface of the electroless plated layer 17 in contact with the catalytic layer 15. In other words, because there is little copper at the interface of the electroless plated layer 17 in contact with the catalytic layer 15, the electroless plated layer 17 is less likely to be corroded even if an acidic chemical solution penetrates the interface between the catalytic layer 15 and the electroless plated layer 17. Therefore, the acid resistance of the laminate 10 composed of the electroless plated layer 17 containing nickel in the above amount is improved. Furthermore, the above nickel content ensures that the electroless plated layer 17, which should be removed in the flash etching process described below, can be reliably removed. The nickel content can be determined by inductively coupled plasma (ICP) atomic emission spectroscopy.
[0034] The thickness of the electroless plated layer 17 may be any thickness as long as it allows a uniform electroless plated layer 17 to be formed on the catalyst layer 15, and is preferably, for example, 0.05 μm or more and 2.0 μm or less, and more preferably 0.10 μm or more and 2.0 μm or less.
[0035] The laminate 10, which is composed of the film 11, resin layer 13, catalyst layer 15, and electroless plated layer 17, has excellent acid resistance and interlayer adhesion, thereby improving the reliability of the circuit of a circuit board using the laminate 10.
[0036] In addition, with respect to the above-described film 11, a gas barrier layer that suppresses oxygen permeation may be formed on at least one surface of the film 11 in order to reduce oxygen penetration into the laminate 10. Forming a gas barrier layer on the film 11 can suppress oxygen penetration into the laminate 10. A laminate 10 composed of such a film 11 suppresses oxidation of the electroless plated layer 17, even when exposed to a high-temperature atmosphere of, for example, 150°C for 400 hours or more. This improves interlayer adhesion between the catalyst layer 15 and the electroless plated layer 17. Furthermore, because oxygen permeation through such a film 11 is low, deterioration of the resin layer due to oxygen is suppressed, and interlayer adhesion between the film 11 and the resin layer 13 is improved.
[0037] Furthermore, the electroless plated layer 17, which has been prevented from being oxidized, has corrosion resistance against acidic chemicals. As a result, even if an acidic chemical penetrates the interface between the catalyst layer 15 and the electroless plated layer 17, the electroless plated layer 17 is less likely to be corroded. The acid resistance of the laminate 10 formed from such a film 11 is improved.
[0038] The gas barrier layer is made of, for example, silicon dioxide, zinc oxide, etc. The thickness of the gas barrier layer is preferably, for example, 10 nm or more and 100 nm or less.
[0039] 2 , an electrolytic plated layer 19 may be further formed on the electroless plated layer 17 of the laminate 10. That is, as shown in FIG. 2 , the laminate 20 of the embodiment includes a film 11, a resin layer 13 formed on at least one surface of the film 11, a catalyst layer 15 formed on the resin layer 13, an electroless plated layer 17 formed on the catalyst layer 15, and an electrolytic plated layer 19 formed on the electroless plated layer 17.
[0040] The laminate 20 includes an electrolytic plating layer 19 on its surface, which has superior conductivity to the electroless plating layer 17, thereby reducing the surface resistivity to, for example, 0.1 Ω / □. Furthermore, when manufacturing a circuit board, a conductive wiring layer can be formed on the electrolytic plating layer 19 in a short period of time. From the viewpoint of interlayer adhesion with the electroless plating layer 17, the electrolytic plating layer 19 preferably contains copper. From the viewpoint of facilitating the formation of a wiring layer, the thickness of the electrolytic plating layer 19 is preferably, for example, 0.1 μm or more and 35.0 μm or less, and more preferably 0.2 μm or more and 18.0 μm or less. The film, resin layer, catalyst layer, and electroless plating layer constituting the laminate 20 are the same as the film and each layer constituting the laminate 10, and therefore are denoted by the same reference numerals as those used for the laminate 10.
[0041] (Manufacturing method for laminate 10 having resin layer 13, catalyst layer 15, and electroless plating layer 17 formed in this order on one side of film 11) Laminate 10 having resin layer 13, catalyst layer 15, and electroless plating layer 17 formed in this order on one side of film 11 can be produced, for example, by the following manufacturing method.
[0042] First, a resin composition containing polyamic acid, which is a precursor of thermoplastic polyimide resin, is applied to one side of film 11, and the mixture is heated at 60°C to 120°C for 1 minute to 30 minutes to form resin layer 13. A catalyst solution containing palladium and a dispersant is applied to resin layer 13, and the mixture is heated at 80°C to 150°C for 1 minute to 60 minutes to form catalyst layer 15. Thereafter, laminate 10, in which resin layer 13 and catalyst layer 15 are formed in this order on one side of film 11, is heated at 200°C to 300°C for 1 minute to 30 minutes to imidize the polyamic acid contained in the resin composition to obtain a thermoplastic polyimide resin.
[0043] Next, laminate 10 is immersed for 30 seconds to 30 minutes in a plating solution containing nickel and copper and maintained at a pH of 7 to 10, to form electroless plated layer 17 on catalyst layer 15. Thereafter, laminate 10 is subjected to a heat treatment (annealing treatment) at 120°C to 350°C in a nitrogen atmosphere for 1 minute to 60 minutes, to obtain laminate 10 having resin layer 13, catalyst layer 15, and electroless plated layer 17 formed in this order on one side of film 11.
[0044] Any plating solution that can form the electroless plated layer 17 can be used, and examples thereof include electroless nickel plating solutions. One example is OPC Allo Copper solution manufactured by Okuno Chemical Industries, Ltd. The concentration of nickel contained in the plating solution is, for example, 0.10 g / L or more and 0.40 g / L or less, and the concentration of copper is, for example, 2.0 g / L or more and 4.0 g / L or less.
[0045] The laminate 10 obtained above is immersed in an electrolytic plating solution containing copper, and a current of, for example, 0.05 A / dm 2 10.0A / dm or more 2 Subsequently, electrolytic plating may be performed for 1 minute to 60 minutes to obtain a laminate 20 in which an electrolytic plated layer 19 is further formed on the electroless plated layer 17. Usable electrolytic plating solutions include, for example, an electrolytic plating solution containing copper sulfate, an electrolytic copper plating solution containing copper pyrophosphate, and an electrolytic copper plating solution containing copper cyanide. One example is Top Lucina SF solution manufactured by Okuno Chemical Industries, Ltd. The concentration of copper sulfate pentahydrate contained in this solution is, for example, 60 g / L to 110 g / L.
[0046] (Method for Manufacturing a Laminate Having Resin Layer 13, Catalyst Layer 15, and Electroless Plated Layer 17 Formed in That Order on Both Sides of Film 11) A laminate having resin layer 13, catalyst layer 15, and electroless plated layer 17 formed in that order on both sides of film 11 can be manufactured, for example, by the following manufacturing method. First, a resin composition containing polyamic acid, a precursor of thermoplastic polyimide resin, is applied to both sides of the film, and heated at 60°C to 250°C for 1 minute to 30 minutes to form resin layers 13 on both sides of film 11. A catalyst solution containing palladium and a dispersant is applied to these resin layers 13, and heated at 80°C to 150°C for 1 minute to 60 minutes to form catalyst layers 15 on both sides of film 11. Then, to imidize the polyamic acid contained in the resin composition to obtain a thermoplastic polyimide resin, the laminate having resin layer 13 and catalyst layer 15 formed in that order on both sides of film 11 is heated at 200°C to 300°C for 1 minute to 30 minutes.
[0047] Next, this laminate is immersed for 30 seconds to 30 minutes in a plating solution containing nickel and copper and maintained at a pH of 7 to 10, to form electroless plated layer 17 on catalyst layer 15. Thereafter, this laminate is heat-treated in a nitrogen atmosphere at 120°C to 350°C for 1 minute to 60 minutes, to obtain a laminate having resin layer 13, catalyst layer 15, and electroless plated layer 17 formed in this order on both sides of film 11.
[0048] The plating solution that can be used in this manufacturing method includes the same plating solution as that used in the manufacturing method of laminate 10 in which resin layer 13, catalyst layer 15, and electroless plated layer 17 are formed in this order on one side of film 11.
[0049] The laminate obtained above is immersed in an electrolytic plating solution containing copper, and a current of, for example, 0.05 A / dm 2 10.0A / dm or more 2 Subsequently, electrolytic plating may be performed for 1 minute to 60 minutes to obtain a laminate in which an electrolytic plated layer 19 is further formed on the electroless plated layer 17. Usable electrolytic plating solutions include, for example, an electrolytic plating solution containing copper sulfate, an electrolytic copper plating solution containing copper pyrophosphate, and an electrolytic copper plating solution containing copper cyanide. One example is Top Lucina SF solution manufactured by Okuno Chemical Industries, Ltd. The concentration of copper sulfate pentahydrate contained in this solution is, for example, 60 g / L to 110 g / L.
[0050] In addition, examples of catalyst solutions that can be used in the step of forming the catalyst layer 15 in the two laminate manufacturing methods described above include catalyst solutions containing a dispersant, palladium covered by the dispersant, and a solvent. The dispersant is composed of a compound that can bond with palladium, such as a nitrogen-containing compound containing nitrogen in its terminal functional group and / or a compound having an unsaturated bond. The bond between palladium and the compound can be, for example, a coordinate bond, an ionic bond, or a covalent bond, with coordinate bonds being preferred from the perspective of dispersibility. Examples of nitrogen-containing compounds include polymers having ammonium groups in their terminal functional groups. Examples of compounds having unsaturated bonds include polyethylene glycol alkyl ether acrylate. The content of the dispersant contained in the catalyst solution is 0.1% by mass or more and 90% by mass or less, preferably 0.2% by mass or more and 50% by mass or less, and more preferably 0.3% by mass or more and 30% by mass or less, relative to the total mass of the catalyst solution. Using such a catalyst solution allows palladium to be uniformly deposited on the surface of the resin layer.
[0051] [Method for Manufacturing Circuit Board] A method for manufacturing a circuit board using laminate 10 will be described using as an example laminate 10 in which resin layer 13, catalyst layer 15, and electroless plating layer 17 are formed in this order on one side of film 11. The method for manufacturing a circuit board includes a resist layer forming step, an exposure step, a resist pattern forming step, a wiring layer forming step, a resist pattern removing step, a flash etching step, and a catalyst layer removing step.
[0052] (Resist Layer Forming Process) A resist layer for forming a resist pattern is formed on the electroless plating layer. The resist material constituting the resist layer may be any material that can be developed after exposure to form a resist pattern, and examples thereof include positive resist materials and negative resist materials. Positive resist materials dissolve in a developer when exposed to light, but do not dissolve in the developer when not exposed to light. Examples of positive resist materials include positive resist liquids and positive dry films. Negative resist materials do not dissolve in a developer when exposed to light, but dissolve in the developer when not exposed to light. Examples of negative resist materials include negative resist liquids and negative dry films.
[0053] In the resist layer forming step, the resist layer may be formed using a positive resist material or a negative resist material.
[0054] The resist layer formation process of this embodiment will be described using a resist layer formation process using a negative dry film as an example. A negative dry film is laminated on the electroless plating layer, and then heated and pressurized. The heating and pressurizing conditions are sufficient to ensure close contact between the electroless plating layer and the negative dry film. For example, when using a vacuum laminator, the heating and pressurizing conditions are 30°C to 100°C, 0.1 MPa to 1.0 MPa, and 5 seconds to 60 seconds. This results in a resist layer being formed on the electroless plating layer. The heating and pressurizing may be performed in a reduced pressure atmosphere. When using a negative resist liquid, the negative resist liquid may be applied to the electroless plating layer and then heated. This results in a resist layer composed of the negative resist liquid being formed on the electroless plating layer.
[0055] (Exposure process) To form a resist pattern, the resist layer is exposed to light through a photomask. The photomask used in this process is a photomask corresponding to the wiring to be formed, and has, for example, a light-shielding area that blocks light and is formed in the shape of a desired circuit, and an opening area that transmits light. The wavelength of the light used in the exposure may be any wavelength that can form a fine pattern, for example, 200 nm or more and 500 nm or less. The exposure conditions may be any wavelength that can form a fine pattern, and may be, for example, a high-pressure mercury lamp with an integrated light dose of 50 mJ / cm. 2 More than 1500mJ / cm 2 The following conditions are included:
[0056] (Resist Pattern Formation Process) The exposed resist layer is developed. When the resist layer is exposed through this photomask and developed, only the portions of the resist layer that were not exposed to light are dissolved in the developer, exposing the electroless plating layer directly below the dissolved resist layer. This exposure and development process forms a resist pattern in the resist layer. In the next process, the wiring layer formation process, a conductive wiring layer is formed on the laminate on which this resist pattern has been formed, for example by electroplating.
[0057] The developer used in the development may be any solution capable of developing the exposed resist layer, and examples thereof include an alkaline aqueous solution such as an aqueous sodium carbonate solution. The resist pattern of this embodiment refers to a resist layer formed by exposure and development into a shape corresponding to the outline of the opening region of the photomask.
[0058] (Wiring Layer Formation Process) A conductive wiring layer is formed on the exposed electroless plated layer 17. This wiring layer can be formed by, for example, electrolytic plating. The electrolytic plating method may be any method that can form a wiring layer on the electroless plated layer. For example, an apparatus that can pass electricity through an electrolytic plating solution containing copper and the laminate 10 and plate the laminate 10 is prepared. Next, the laminate 10 is immersed in the electrolytic plating solution and plated at 0.05 A / dm 2 10.0A / dm or more 2Examples of electrolytic plating methods include those for 1 minute to 60 minutes. Examples of copper-containing electrolytic plating solutions include copper sulfate plating solutions, copper pyrophosphate plating solutions, and copper cyanide plating solutions. One example is Top Lucina SF solution manufactured by Okuno Chemical Industries, Ltd. The concentration of copper sulfate pentahydrate contained in this solution is 60 g / L to 110 g / L.
[0059] (Resist Pattern Removal Process) After the wiring layer is formed in the wiring layer formation process, the resist pattern is removed. The solvent used to remove the resist pattern may be any solvent that can remove the resist material that constitutes the resist pattern, and examples thereof include organic amine solvents, ketone solvents, and alkaline solvents.
[0060] (Flash Etching Process) The electroless plating layer 17 exposed by removing the resist pattern is removed. The etching solution used to remove the exposed electroless plating layer 17 may be any etching solution that can remove electroless plating layer 17 containing nickel and copper, and examples thereof include a sulfuric acid / peroxide-based etching solution, a sodium persulfate-based etching solution, a ferric chloride-based etching solution, and a cupric chloride-based etching solution. Note that, because the wiring layer is thicker than the electroless plating layer 17, the flash etching process has little effect on the wiring layer.
[0061] (Catalyst Layer Removal Process) The exposed catalyst layer 15 is removed by removing the electroless plating layer 17. The chemical solution used to remove the exposed catalyst layer 15 may be any chemical solution that can remove the palladium-containing catalyst layer 15, and examples thereof include hydrochloric acid-based chemical solutions, nitric acid-based chemical solutions, and permanganate-based chemical solutions. A circuit board can be obtained through the above processes.
[0062] [Method for manufacturing a circuit board including an electrolytic plating layer forming step] Next, a method for manufacturing a circuit board including an electrolytic plating layer forming step will be described using as an example the laminate 10 used in the above-described method for manufacturing a circuit board, i.e., the laminate 10 having the resin layer 13, the catalyst layer 15, and the electroless plating layer 17 formed in this order on one side of the film 11.
[0063] This circuit board manufacturing method includes an electrolytic plating layer forming step, a resist layer forming step, an exposure step, a resist pattern forming step, a wiring layer forming step, a resist pattern removing step, a flash etching step, and a catalyst layer removing step. Hereinafter, the circuit board manufacturing method including the electrolytic plating layer forming step differs from the circuit board manufacturing method described above in that it includes an electrolytic plating layer forming step before the resist layer forming step. Below, this electrolytic plating layer forming step will be described in detail, and the other steps will be briefly described.
[0064] (Electrolytic Plated Layer Forming Step) An electrolytic plated layer 19 is formed on the electroless plated layer 17 of the laminate 10, which is formed on one side of the film 11 in this order: the resin layer 13, the catalyst layer 15, and the electroless plated layer 17. The electrolytic plating method may be any method that can form the electrolytic plated layer 19 on the electroless plated layer 17 of the laminate 10. For example, an apparatus is prepared that can pass electricity through an electrolytic plating solution containing copper and the laminate 10, and can plate on the electroless plated layer 17 of the laminate 10. Next, the laminate 10 is immersed in the electrolytic plating solution, and a current of 0.05 A / dm 2 10.0A / dm or more 2 The conditions for electrolytic plating treatment for 1 minute or more and 60 minutes or less are as follows.
[0065] Examples of copper-containing electroplating solutions used in this process include copper sulfate plating solutions, copper pyrophosphate plating solutions, and copper cyanide plating solutions. The copper concentration in the electroplating solution is, for example, 10 g / L or more and 110 g / L or less. One example is Top Lucina SF solution manufactured by Okuno Chemical Industries, Ltd. The concentration of copper sulfate pentahydrate in this solution is, for example, 60 g / L or more and 110 g / L or less. In this process, an electroplated layer 19 is further laminated on the electroless plated layer 17, thereby providing the surface of the laminate with an electroplated layer 19 having superior conductivity to the electroless plated layer 17. This allows the surface resistivity of the laminate surface to be reduced to, for example, 0.1 Ω / □. Furthermore, reducing the surface resistivity to 0.1 Ω / □ facilitates the formation of a dense conductive wiring layer on the electroplated layer 19. The surface resistivity can be measured in accordance with JIS K7194.
[0066] (Resist Layer Formation Process) A resist layer is formed on the electroplated layer 19 to form a resist pattern corresponding to the wiring to be formed. In the resist layer formation process, the resist layer may be formed using a positive resist material or a negative resist material. In the resist layer formation process of this embodiment, a resist layer formation process using a dry film-type negative resist material will be described as an example. A dry film is laminated on the electroplated layer 19, and heat and pressure are applied. The heating and pressure conditions are sufficient to ensure close contact between the electroplated layer 19 and the dry film. For example, when using a vacuum laminator, the heating and pressure are 30°C to 100°C, 0.1 MPa to 1.0 MPa, and 5 seconds to 60 seconds. This forms a resist layer on the electroplated layer 19. The heating and pressure may be performed in a reduced pressure atmosphere. When a resist liquid is used as the resist material, the resist liquid may be applied to the electroplated layer 19 and heated. This forms a resist layer composed of the resist liquid on the electroplated layer 19.
[0067] (Exposure Step) To form a resist pattern, the resist layer is exposed to light through a photomask.
[0068] (Resist Pattern Formation Process) The exposed resist layer is developed, thereby forming a resist pattern on the electroplated layer 19 that corresponds to the wiring to be formed.
[0069] (Wiring Layer Forming Process) By electrolytic plating the laminate 10 on which the resist pattern has been formed, a conductive wiring layer is formed on the exposed electrolytic plating layer 19 .
[0070] (Resist Pattern Removal Process) The resist pattern is removed.
[0071] (Flash Etching Step) The electrolytic plating layer 19 exposed by removing the resist pattern is removed, as well as the electroless plating layer 17 formed below the electrolytic plating layer 19. The etching solution used to remove these layers may be any etching solution that can remove the copper-containing electrolytic plating layer 19 and the nickel- and copper-containing electroless plating layer 17, and examples thereof include a sulfuric acid / peroxide-based etching solution, a sodium persulfate-based etching solution, a ferric chloride-based etching solution, and a cupric chloride-based etching solution.
[0072] (Catalyst Layer Removal Step) The catalyst layer 15 exposed by removing the electroless plated layer 17 is removed. As described above, a circuit board can be obtained by the method for manufacturing a circuit board including the electrolytic plated layer formation step.
[0073] [Method for Manufacturing a Circuit Board Using Laminate 20 Having Electrolytic Plated Layer 19 Formed on Electroless Plated Layer 17] A method for manufacturing a circuit board using laminate 20 will be described using, as an example, laminate 20 having electrolytic plated layer 19 formed on electroless plated layer 17, i.e., laminate 20 having resin layer 13, catalyst layer 15, electroless plated layer 17, and electrolytic plated layer 19 formed in this order on one side of film 11. This circuit board manufacturing method includes a resist layer forming step, an exposure step, a resist pattern forming step, a wiring layer forming step, a resist pattern removing step, a flash etching step, and a catalyst layer removing step. Hereinafter, the method for manufacturing a circuit board using laminate 20 having electrolytic plated layer 19 further formed on electroless plated layer 17 will only be briefly described, as it includes substantially the same steps as the circuit board manufacturing method described above.
[0074] (Resist Layer Forming Step) A resist layer for forming a resist pattern is formed on the electrolytic plating layer 19 .
[0075] (Exposure Step) To form a resist pattern, the resist layer is exposed to light through a photomask.
[0076] (Resist Pattern Formation Process) The exposed resist layer is developed, thereby forming a resist pattern on the electroplated layer 19 that corresponds to the wiring to be formed.
[0077] (Wiring Layer Forming Process) Electrolytic plating is performed on the laminate 20 on which the resist pattern has been formed, to form a conductive wiring layer on the exposed electrolytic plating layer 19 .
[0078] (Resist Pattern Removal Process) The resist pattern is removed.
[0079] (Flash Etching Step) The electrolytic plated layer 19 exposed by removing the resist pattern and the electroless plated layer 17 formed below the electrolytic plated layer 19 are removed.
[0080] (Catalyst Layer Removal Step) The catalyst layer 15 exposed by removing the electroless plating layer 17 is removed.
[0081] As described above, a circuit board can be obtained by the method for manufacturing a circuit board using laminate 20 in which electrolytic plated layer 19 is further formed on electroless plated layer 17 .
[0082] The method for manufacturing a circuit board according to this embodiment has been described above using laminate 10 in which resin layer 13, catalyst layer 15, and electroless plated layer 17 are formed in this order on one side of film 11, and laminate 20 in which electrolytic plated layer 19 is further formed on electroless plated layer 17 as an example.
[0083] It should be noted that the present invention is not limited to these laminates, and it is also possible to use, for example, a laminate in which resin layer 13, catalyst layer 15, and electroless plated layer 17 are formed in this order on both sides of film 11, or a laminate in which resin layer 13, catalyst layer 15, electroless plated layer 17, and electrolytic plated layer 19 are formed in this order on both sides of a film. Furthermore, in the method for manufacturing a circuit board of this embodiment, various photoetching steps can be selected as appropriate.
[0084] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0085] Example 1 (Preparation of Laminate) (1) Preparation of Resin Layer 13 (1-1) Preparation of Polyamic Acid Solution Into a reaction vessel, 85 g of N,N-dimethylacetamide (manufactured by Mitsubishi Gas Chemical Company, Inc., DMAc), 1.034 g (0.003 mol) of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (manufactured by Wakayama Seika Kogyo Co., Ltd., BAPP), and 6.628 g (0.023 mol) of 1,3-bis(4-aminophenoxy)benzene (manufactured by Wakayama Seika Kogyo Co., Ltd., TPE-R) were added and stirred at room temperature to dissolve the BAPP and TPE-R in the DMAc. To the resulting solution, 7.338 g (0.025 mol) of 3,4,3',4'-biphenyltetracarboxylic dianhydride (manufactured by Ube Industries, Ltd., BPDA) was gradually added, and the mixture was stirred at room temperature for 3 hours to obtain a resin composition containing polyamic acid. The resulting resin composition was diluted with DMAc to a solids concentration of 2% by mass to obtain a polyamic acid solution. (1-2) Formation of Resin Layer 13: The polyamic acid solution prepared above was applied to one side of a 25 μm thick polyimide film (Kapton (registered trademark) 100EN-C, manufactured by DuPont-Toray Co., Ltd.) using a bar coater so that the thickness after heating would be 100 nm. After application, the film was heated at 120°C for 5 minutes to obtain a laminate in which a resin layer 13 was formed on one side of the polyimide film.
[0086] (2) Preparation of catalyst layer 15 A catalyst solution containing 0.45% by mass of palladium (CP-018, manufactured by Nissan Chemical Industries, Ltd.) was applied onto the resin layer 13 of the laminate obtained in (1-2) using a bar coater. After application, the laminate was heated at 120°C for 10 minutes to obtain a laminate in which the catalyst layer 15 was formed on the resin layer 13. The laminate was further heated at 240°C for 15 minutes. The surface of the resin layer 13 of the obtained laminate had a surface area of 1 dm 2 It was confirmed that 0.15 mg of palladium was attached per 1000g sample. The amount of palladium attached was measured by ICP emission spectroscopy. The device used for the measurement was an ICPE-9800 series manufactured by Shimadzu Corporation.
[0087] (3) Preparation of Electroless Plated Layer 17 OPC Allo Copper (manufactured by Okuno Chemical Industries, Ltd.) (initial copper concentration: 3.16 g / L, nickel concentration: 0.14 g / L, sodium hypophosphite concentration: 24 g / L) was prepared as the electroless plating solution used to deposit the electroless plated layer 17 on the catalyst layer 15. Sodium hydroxide was added to the plating solution to prepare an electroless plating solution with a pH of 9.0. This electroless plating solution was placed in a plating bath, and the solution temperature was adjusted to 50°C. The laminate obtained in (2) was immersed in this plating bath for 10 minutes. The laminate was then removed, washed with water, dried, and subjected to a heat treatment at 300°C for 5 minutes in a nitrogen atmosphere. After cooling, a laminate 10 was obtained in which the electroless plated layer 17 was formed on the catalyst layer 15. The resulting laminate 10 was used to evaluate adhesion.
[0088] The thickness of the electroless plated layer 17 of the obtained laminate 10 was 0.15 μm. The thickness of the electroless plated layer 17 was measured by ICP atomic emission spectroscopy. The device used for the measurement was an ICPE-9800 series manufactured by Shimadzu Corporation.
[0089] The nickel content of this electroless plated layer 17 was 8.0% by mass. The nickel content was determined as follows. First, a laminate 10 with an electroless plated layer 17 formed thereon was prepared, cut into a 50 mm x 50 mm square. Next, 15 mL of an aqueous solution containing 60% by mass of nitric acid aqueous solution, 35% by mass of hydrochloric acid, and pure water in a 1:1:1 ratio was added to a beaker. The beaker was heated, and when the aqueous solution boiled, the cut laminate 10 was added and stirred for 3 minutes while maintaining the boiling state. After that, the beaker was cooled to room temperature, and the liquid in the beaker was transferred to a 100 mL measuring flask. The remaining liquid adhering to the beaker was washed three times with small amounts of pure water, and this liquid was also transferred to the measuring flask. Pure water was then added to the measuring flask to bring the volume to 100 mL. The copper, nickel, and phosphorus contained in the resulting aqueous solution were quantitatively analyzed using an ICP atomic emission spectrometer. The weight of copper (X) was 3.084 mg, the weight of nickel (Y) was 0.271 mg, and the weight of phosphorus (Z) was 0.024 mg. The weights obtained were substituted into (Y × 100) / (X + Y + Z) to calculate the weight of nickel relative to the weight of electroless plated layer 17.
[0090] (4) Preparation of Electroplated Layer 19 A plating bath was filled with an electroplating solution (Top Lucina SF manufactured by Okuno Chemical Industries Co., Ltd.), and the solution temperature was set to 25° C. The laminate 10 obtained in (3) was immersed in this plating bath, and a current of 1 A / dm 2 for 3 minutes, then 2 A / dm 2 This resulted in a laminate 20 having an electrolytic plating layer 19 with a thickness of 12 μm formed thereon. The acid resistance and peel strength of this resulting laminate 20 were evaluated.
[0091] In addition, in the evaluation of the insulation resistance value, the laminate 10 obtained in (3) was immersed in the plating bath described above, and 2 The laminate 20 was used after electrolytic plating treatment at 1000 kJ / min for 10 minutes, and an electrolytic plating layer 19 having a thickness of 2 μm was formed.
[0092] The thickness of the electrolytic plating layer 19 of the resulting laminate 20 was measured using a micrometer.
[0093] (Acid Resistance) To evaluate acid resistance, a sample was prepared using a laminate 20 having an electroplated layer 19 with a thickness of 12 μm. First, a laminate 20 cut into a 100 mm × 100 mm square was prepared. Next, a photosensitive dry film was laminated onto the electroplated layer 19 of the laminate 20 and bonded using a vacuum laminator. The conditions were 50°C, 0.5 MPa, 10 seconds, and a vacuum level of 3 hPa or less. The photosensitive dry film was a negative dry film, and Sunfort AQ-2075 manufactured by Asahi Kasei Corporation was used.
[0094] Next, the surface of the dry film is irradiated with 80 mJ / cm 2 through a photomask having rectangular openings with a width of 3 mm and a length of 20 mm. 2The dry film was exposed to light with a sodium carbonate solution. The unexposed portions of the dry film were then removed using an aqueous sodium carbonate solution (development). The electrolytic plating layer 19 exposed by development, the electroless plating layer 17 formed thereunder, and the catalyst layer 15 formed thereunder were removed. After this removal, the exposed dry film was removed using an aqueous sodium hydroxide solution. It was confirmed that the electrolytic plating layer 19 exposed after removing the dry film and the electroless plating layer 17 formed thereunder had been etched into a predetermined rectangular shape when viewed perpendicular to the main plane of the laminate 20. This was used as a sample. The etching solution used for etching was a ferric chloride solution manufactured by Toagosei Co., Ltd.
[0095] Next, the obtained sample was heated at 160°C for 1 hour. After heating, the sample was immersed in a 10% hydrochloric acid solution at 23°C for 30 minutes, rinsed with water, and dried. The rectangular electroplated layer 19 and electroless plated layer 17 were then observed using an optical microscope (Keyence VHX-8000). During observation, the sample was positioned so that the polyimide film surface was facing the lens of the optical microscope. The degree of corrosion was confirmed using software installed in the VHX-8000. Evaluation was based on the following criteria: Good: The depth of corrosion of the rectangular electroplated layer 19 and electroless plated layer 17 was less than 5 μm; Poor: The depth of corrosion of the rectangular electroplated layer 19 and electroless plated layer 17 was 5 μm or greater.
[0096] (Interlayer Adhesion) The interlayer adhesion of the laminate was evaluated by (i) evaluating adhesion and (ii) evaluating peel strength, which will be described later. (i) Evaluation of Adhesion The adhesion between the resin layer 13 and the catalyst layer 15, and the adhesion between the catalyst layer 15 and the electroless plated layer 17 in the laminate 10 obtained in (3) were visually observed. Specifically, the laminates on which the electroless plated layer 17 was formed, cut into 100 mm x 100 mm squares, i.e., the laminates 10 obtained in (3) producing the electroless plated layer 17, were visually observed for the presence or absence of peeling between the layers. In addition, five laminates were checked for evaluation and evaluated according to the following criteria: Good: The number of laminates on which peeling occurred was less than two; Poor: The number of laminates on which peeling occurred was two or more.
[0097] (ii) Evaluation of Peel Strength The peel strength of the electrolytic plated layer 19 before and after heat treatment was measured for the laminate 20 obtained in (4), specifically, the laminate 20 having an electrolytic plated layer 19 with a thickness of 12 μm, in accordance with JIS C6471.
[0098] First, a laminate 20 cut into a 100 mm x 100 mm square was prepared. Next, a photosensitive dry film was laminated onto the electrolytic plating layer 19 of the laminate 20 and bonded using a vacuum laminator. The conditions were 50°C, 0.5 MPa, 10 seconds, and a vacuum level of 3 hPa or less. The photosensitive dry film was a negative dry film, and Sunfort AQ-2075 manufactured by Asahi Kasei Corporation was used.
[0099] Next, the surface of the dry film is irradiated with 80 mJ / cm 2 through a photomask having rectangular openings with a width of 3 mm and a length of 20 mm. 2The dry film was exposed to light with a sodium carbonate solution. The unexposed portions of the dry film were then removed using an aqueous sodium carbonate solution (development). The electrolytic plating layer 19 exposed by development, the electroless plating layer 17 formed thereunder, and the catalyst layer 15 formed thereunder were removed. After this removal, the exposed dry film was removed using an aqueous sodium hydroxide solution. It was confirmed that the electrolytic plating layer 19 exposed after removing the dry film and the electroless plating layer 17 formed thereunder had been etched into a predetermined rectangular shape when viewed perpendicular to the main plane of the laminate 20. This was used as a sample. The etching solution used for etching was a ferric chloride solution manufactured by Toagosei Co., Ltd.
[0100] (ii-1) Peel strength before heat treatment The film constituting the obtained sample and a stainless steel reinforcing plate were attached with double-sided tape to obtain a measurement sample. (ii-2) Peel strength after heat treatment The obtained sample was stored in an atmosphere of 150°C for 240 hours. After that, after storing it at 25°C and 50% RH for 24 hours, the film constituting the obtained sample and a stainless steel reinforcing plate were attached with double-sided tape to obtain a measurement sample. (ii-3) Measurement Using an Autograph AGS-500 manufactured by Shimadzu Corporation, the peel strength in the 90° direction (the direction perpendicular to the surface of the measurement sample) was measured under the following measurement conditions. The measurement conditions were copper plating and a test speed of 50 mm / min. The evaluation criteria were as follows. Excellent: peel strength is 5 N / cm or more; Good: peel strength is less than 5 N / cm and 3 N / cm or more; Poor: peel strength is less than 3 N / cm.
[0101] The results of evaluating the acid resistance and interlayer adhesion of the laminate of Example 1 are shown in Table 1. The laminate of Example 1 exhibited excellent acid resistance, and also showed good results in adhesion and peel strength. This indicates that the laminate of Example 1 has excellent acid resistance and interlayer adhesion. Furthermore, the reliability of the circuit of a circuit board using such a laminate is improved.
[0102] Example 2 A laminate was produced in the same manner as in Example 1, except that an electroless plating solution containing 0.2 g / L of nickel (Ni) was used.
[0103] Example 3 A laminate was produced in the same manner as in Example 1, except that an electroless plating solution containing 0.34 g / L of nickel (Ni) was used.
[0104] (Example 4) A laminate was produced in the same manner as in Example 1, except that a catalyst solution in which the amount of palladium was changed to 0.3 mass % and an electroless plating solution in which the nickel (Ni) concentration was changed to 0.34 g / L were used. Note that the surface of the resin layer 13 of the laminate obtained in the process of producing the laminate of Example 4 had a surface area of 1 dm 2 It was confirmed that 0.08 mg of palladium was attached per unit area.
[0105] (Example 5) A laminate was produced in the same manner as in Example 1, except that a catalyst solution in which the amount of palladium was changed to 0.57 mass % and an electroless plating solution in which the nickel (Ni) concentration was changed to 0.34 g / L were used. Note that the surface of the resin layer 13 of the laminate obtained in the process of producing the laminate of Example 5 had a thickness of 1 dm2. 2 It was confirmed that 0.2 mg of palladium was attached per unit area.
[0106] (Example 6) A laminate was produced in the same manner as in Example 1, except that a catalyst solution in which the amount of palladium was changed to 0.15 mass % and an electroless plating solution in which the nickel (Ni) concentration was changed to 0.34 g / L were used. Note that the surface of the resin layer 13 of the laminate obtained in the process of producing the laminate of Example 6 had a thickness of 1 dm2. 2 It was confirmed that 0.05 mg of palladium was attached per unit area.
[0107] Comparative Example 1 A laminate was produced in the same manner as in Example 1, except that an electroless plating solution containing 0.1 g / L of nickel (Ni) was used.
[0108] Comparative Example 2 A laminate was produced in the same manner as in Example 1, except that an electroless plating solution containing 0.44 g / L of nickel (Ni) was used.
[0109] The measurement and evaluation methods for the prepared samples of Examples 2 to 6 and Comparative Examples 1 and 2 were the same as those for Example 1.
[0110] The evaluation results of these Examples and Comparative Examples are shown in Tables 1 and 2. It can be seen from Table 1 that the laminates of Examples 2 to 6 also have excellent acid resistance and interlayer adhesion. Furthermore, the reliability of the circuit of a circuit board using such a laminate is improved.
[0111] The laminates of Examples 1 to 6 are believed to have excellent interlayer adhesion because they include a film that relieves stress generated during the formation of the electroless plated layer 17, a resin layer 13 containing a thermoplastic polyimide resin, and a catalyst layer 15 containing palladium, which serves as a scaffold for the formation of the electroless plated layer 17. Furthermore, the electroless plated layer 17, which contains a predetermined amount of nickel, has a large amount of nickel present, particularly at the interface of the electroless plated layer 17 in contact with the catalyst layer 15. Therefore, even if an acidic chemical solution penetrates the interface between the catalyst layer 15 and the electroless plated layer 17, the electroless plated layer 17 is not easily corroded. In other words, the laminates have excellent acid resistance. Furthermore, the reliability of the circuit of a circuit board using such a laminate is enhanced.
[0112]
[0113]
[0114] The laminates of Examples 1 to 6 were further evaluated for surface resistivity, insulation resistance, and solder heat resistance.
[0115] (Surface Resistivity) The surface resistivity was measured for laminate 10 on which electroless plated layer 17 was formed before electrolytic plated layer 19 was laminated, which was obtained during the process of producing the laminate in Example 1, i.e., laminate 10 obtained by (3) producing electroless plated layer 17. If this surface resistivity is low, when the electrolytic plated layer is formed on the electroless plated layer, sparks caused by unexpected large currents flowing in the electroless plated layer and burning caused by current concentrating in areas where current easily flows are less likely to occur.
[0116] (Measurement of surface resistivity) Surface resistivity was measured in accordance with JIS K7194. The surface of the laminate cut into a square shape of 80 mm x 50 mm was measured at five points with a four-point probe using a Loresta-GP MCP-T610 manufactured by Mitsubishi Chemical Corporation. If the surface resistivity is 2.3 Ω / □ or less, sparks and burns are unlikely to occur, and this is considered good. The surface resistivity of Example 1 was 0.8 Ω / □, which was found to be good.
[0117] For the laminates of Examples 2 to 6, laminates 10 were prepared on which electroless plated layer 17 was formed before electrolytic plated layer 19 was laminated. The surface resistivity of the laminates of each Example was measured using the same method as that used to measure the surface resistivity of the laminate of Example 1. The surface resistivity of Example 2 was 1.2 Ω / □. The surface resistivity of Example 3 was 2.0 Ω / □. The surface resistivity of Example 4 was 2.0 Ω / □. The surface resistivity of Example 5 was 2.0 Ω / □. The surface resistivity of Example 6 was 2.0 Ω / □. All Examples were found to have good surface resistivities of 2.3 Ω / □ or less.
[0118] (Insulation Resistance Value) The insulation resistance value of the laminate 20 obtained in (4) Preparation of Electroplated Layer 19 in Example 1, specifically, the laminate 20 on which a 2 μm-thick electroplated layer was formed, was measured. If the insulation resistance value between the wirings formed in the laminate is high, it means that there is little conductive material, such as copper, remaining between the wirings during the wiring formation process, and the conductive material has been reliably removed. Furthermore, circuit boards constructed from such laminates are less likely to short-circuit.
[0119] (Measurement of insulation resistance value) The insulation resistance value was measured in accordance with JIS C6471. Specifically, a laminate cut into a 100 mm x 100 mm square was prepared. Next, a photosensitive dry film was laminated on the electroplated layer of the laminate and bonded using a vacuum laminator. The conditions were 50°C, 0.5 MPa, 10 seconds, and a vacuum level of 3 hPa or less. The photosensitive dry film was a negative dry film, and Sunfort AQ-2075 manufactured by Asahi Kasei Corporation was used.
[0120] Next, the surface of the dry film was irradiated with 80 mJ / cm 2 through a photomask on which a pattern corresponding to the shape of the electrodes for measuring the insulation resistance value in accordance with JIS C6471 was formed. 2 The laminate was exposed to light with a sodium carbonate solution. The unexposed dry film was then removed using an aqueous sodium carbonate solution (development). The resulting laminate was immersed in an aqueous flash etching solution for 60 seconds to remove the electrolytic plating layer 19 exposed by development and the electroless plating layer 17 formed thereunder. The exposed dry film was then removed using an aqueous sodium hydroxide solution. Next, the laminate was immersed in remover solution 1 (MEC Corporation, MEC Remover EM-1924) for 10 seconds, and then further immersed in remover solution 2 (MEC Corporation, MEC Remover CH-1925) for 40 seconds to remove the catalyst layer 15. A measurement sample was obtained through the above procedure.
[0121] The insulation resistance between the measurement electrodes formed on this measurement sample was measured using a Digital Ultra High Resistance 5451 manufactured by ADC Corporation after applying a DC voltage of 500 V for 1 minute. When the insulation resistance value was 1.0 × 10 12 If the insulation resistance is 1.0×10 Ω or more, there is little conductive material such as copper remaining between the wirings, and this is considered to be good. 12 It was over Ω, which was good.
[0122] The photomask used was prepared in accordance with JIS C 6471. The flash etching solution used was an aqueous solution prepared by diluting Mitsubishi Gas Chemical Company's CPE-800D five times.
[0123] The insulation resistance of the laminates of Examples 2 to 6 was measured in the same manner as that of the laminate of Example 1. The insulation resistance of Examples 2 to 4 was 1.0×10 12 The insulation resistance value of Example 5 was 1.0×10 8 The insulation resistance value of Example 6 was 1.0×10 12 It was above Ω.
[0124] As described above, the laminates of Examples 2 to 4 and Example 6 maintained high insulation resistance values, which was favorable. Circuit boards made from these laminates are less likely to short-circuit.
[0125] (Soldering Heat Resistance) The soldering heat resistance was evaluated for the laminate 20 in Example 1 (4) on which the electrolytic plating layer 19 was formed, specifically, the laminate 20 on which the electrolytic plating layer 19 having a thickness of 12 μm was formed.
[0126] (Measurement of soldering heat resistance) A laminate cut into a 30 mm x 30 mm square was prepared. The laminate was floated in a solder bath at 340°C for 60 seconds so that the electrolytic plating layer was in contact with the solder. The laminate was then removed from the solder bath and visually inspected for blistering or peeling. A laminate without blistering or peeling has excellent soldering heat resistance. No blistering or peeling was observed in the laminate of Example 1, and it was found to have excellent soldering heat resistance.
[0127] The laminates of Examples 2 to 6 were also evaluated for solder heat resistance using the same method as in Example 1. No swelling or peeling was observed in any of the laminates of Examples 2 to 6, and it was found that they had excellent solder heat resistance.
[0128] As described above, it was found that the laminates of Examples 1 to 6 have excellent acid resistance and interlayer adhesion, as well as low surface resistivity and excellent solder heat resistance. Furthermore, it was found that the laminates of Examples 1 to 4 and 6 have high insulation resistance values. It was also found that the use of such laminates can provide circuit boards that are less susceptible to short circuits. Furthermore, the reliability of the circuitry of a circuit board using such laminates is improved.
[0129] The present invention allows various embodiments and modifications without departing from the broad spirit and scope of the present invention. Furthermore, the above-described embodiments are intended to explain the present invention and do not limit the scope of the present invention. That is, the scope of the present invention is defined by the claims, not the embodiments. Various modifications made within the scope of the claims and within the scope of the meaning of the invention equivalent thereto are considered to be within the scope of the present invention.
[0130] This application is based on Japanese Patent Application No. 2023-061292, filed on April 5, 2023. The specification and claims of Japanese Patent Application No. 2023-061292 are incorporated herein by reference.
[0131] 10, 20 Laminate, 11 Film, 13 Resin layer, 15 Catalyst layer, 17 Electroless plated layer, 19 Electrolytic plated layer.
Claims
1. A laminate comprising: a film; a resin layer containing a thermoplastic polyimide resin and formed on at least one surface of the film; a catalyst layer containing palladium and a dispersant covering the palladium and formed on the resin layer; and an electroless plating layer containing nickel and copper and formed on the catalyst layer, wherein the nickel content is 8.0 mass% or more and 13.0 mass% or less relative to the total mass of the electroless plating layer.
2. The amount of palladium contained in the catalyst layer is 1 dm 2 The laminate according to claim 1, wherein the average particle diameter is 0.05 mg or more and 0.18 mg or less per unit area.
3. The laminate according to claim 1 or 2, further comprising an electrolytically plated layer containing copper and formed on the electrolessly plated layer.
4. A method for manufacturing a circuit board comprising: a resist layer formation step of forming a resist layer on the electroless plating layer that constitutes the laminate described in claim 1; an exposure step of exposing the resist layer; a resist pattern formation step of developing the resist layer exposed in the exposure step to form a resist pattern corresponding to the wiring to be formed; a wiring layer formation step of forming a conductive wiring layer on the electroless plating layer exposed after the resist pattern formation step; a resist pattern removal step of removing the resist pattern; a flash etching step of removing the electroless plating layer exposed after the resist pattern removal step; and a catalyst layer removal step of removing the catalyst layer exposed after the flash etching step.
5. A method for manufacturing a circuit board comprising: an electrolytic plating layer formation step of forming an electrolytic plating layer on the electroless plating layer that constitutes the laminate described in claim 1; a resist layer formation step of forming a resist layer on the electrolytic plating layer; an exposure step of exposing the resist layer; a resist pattern formation step of developing the resist layer exposed in the exposure step to form a resist pattern corresponding to the wiring to be formed; a wiring layer formation step of forming a conductive wiring layer on the electrolytic plating layer exposed after the resist pattern formation step; a resist pattern removal step of removing the resist pattern; a flash etching step of removing the electrolytic plating layer exposed after the resist pattern removal step and the electroless plating layer formed below the electrolytic plating layer; and a catalyst layer removal step of removing the catalyst layer exposed after the flash etching step.
6. A method for manufacturing a circuit board comprising: a resist layer formation step of forming a resist layer on the electrolytic plating layer constituting the laminate described in claim 3; an exposure step of exposing the resist layer; a resist pattern formation step of developing the resist layer exposed in the exposure step to form a resist pattern corresponding to the wiring to be formed; a wiring layer formation step of forming a conductive wiring layer on the electrolytic plating layer exposed after the resist pattern formation step; a resist pattern removal step of removing the resist pattern; a flash etching step of removing the electrolytic plating layer exposed after the resist pattern removal step and the electroless plating layer formed below the electrolytic plating layer; and a catalyst layer removal step of removing the catalyst layer exposed after the flash etching step.
Citation Information
Patent Citations
Method of manufacturing circuit base for electronic part
JP2004152852A
Conductor coating polyimide film and manufacturing method thereof
JP2005116745A
Method of manufacturing laminated body and method of manufacturing circuit wiring board
JP2010157537A
Flexible circuit board and method for manufacturing same
WO2010137549A1
Laminate and method of manufacturing same
WO2019171990A1