Adhesive composition, production method therefor, adhesive, patch, wearable device, and wearable device kit
Patent Information
- Application Number
- JP2025512505
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Priority Date
- 2023-10-03
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-10
AI Technical Summary
Current adhesives for skin patches and wearable devices lack a balance between adhesion to the skin and the device, often causing skin irritation, toxicity, and inadequate antibacterial properties.
A pressure-sensitive adhesive composition comprising a hydroxyl-terminated urethane prepolymer and a polyisocyanate compound, formed using a tin-free catalyst, which provides a balanced adhesion to the skin and devices while being gentle and non-toxic, with improved antibacterial properties.
The adhesive composition achieves a good balance between skin adhesion and device adhesion, is gentle on the skin, has low toxicity, and passes antibacterial tests, making it suitable for long-term use on the skin without causing irritation or residue.
Abstract
Description
Adhesive composition and method for producing the same, as well as adhesive, patch, wearable device, and wearable device kit
[0001] The present invention relates to an adhesive composition for obtaining an adhesive that can be applied to the skin, a method for producing the same, an adhesive, an adhesive patch, a wearable device, and a wearable device kit.
[0002] These adhesives are used in adhesive skin patches such as bandages, surgical tapes, poultices, and plasters, as well as in adhesives used to attach patch-type wearable devices to the skin for continuously acquiring biological information such as body temperature and brain waves.
[0003] As an example of a pressure-sensitive adhesive, Patent Document 1 describes an acrylic pressure-sensitive adhesive that is not intended for use on the skin, but that contains an organic iodine-based living radical polymerization initiator and has improved antibacterial properties due to the inclusion of iodine.
[0004] Furthermore, Patent Document 2 describes a non-sensitizing pressure-sensitive adhesive that is useful in medical applications and other uses that come into contact with the skin, and is an acrylic adhesive selected so that the cured adhesive passes an in vitro cytotoxicity test in accordance with ISO 10993-5:2009.
[0005] Japanese Patent Application Laid-Open No. 2022-98300 Special Publication No. 2022-541292
[0006] However, an adhesive that has a good balance of adhesive strength to the skin and adhesive strength to the device, is gentle on the skin (allows the adherend to be attached and detached gently to the skin, and is low toxic), and has improved antibacterial properties has not yet been obtained, and there has been a strong desire to develop such an adhesive.
[0007] The present invention has been made in view of the above circumstances, and aims to provide an adhesive composition and a method for producing the same, which provide an adhesive that has a good balance of adhesive strength to the skin and adhesive strength to a device, is gentle on the skin (allows the adherend to be fixed and detached gently to the skin, and is low toxic), and has improved antibacterial properties, as well as an adhesive, a patch, a wearable device, and a wearable device kit obtained using the adhesive composition.
[0008] The present invention is based on the discovery of a polyurethane-based adhesive that has a good balance of adhesive strength to the skin and adhesive strength to devices, without using a tin-based catalyst, the use of which is being restricted due to its impact on health, etc.
[0009] The present invention provides the following means: [1] A pressure-sensitive adhesive composition comprising a hydroxyl-terminated urethane prepolymer and a polyisocyanate compound, wherein the hydroxyl-terminated urethane prepolymer is a reaction product of an oxyalkylene polymer and a diisocyanate compound in the presence of a tin-free catalyst, the oxyalkylene polymer comprising an oxyalkylene polymer A having two or more hydroxyl groups per molecule and an oxyalkylene polymer B having one hydroxyl group per molecule, and the hydroxyl-terminated urethane prepolymer has an average content of ethylene oxide-based structural units of 8 to 50 mass%. [2] The pressure-sensitive adhesive composition according to [1] above, wherein the content of the tin-free catalyst is more than 0.001 part by mass and less than 0.050 part by mass per 100 parts by mass of the oxyalkylene polymer. [3] The pressure-sensitive adhesive composition according to [1] or [2] above, wherein the tin-free catalyst is an organometallic catalyst. [4] The pressure-sensitive adhesive composition according to any one of [1] to [3] above, wherein the tin-free catalyst contains one or more metals selected from zinc and bismuth. [5] The pressure-sensitive adhesive composition according to any one of [1] to [4] above, wherein the oxyalkylene polymer has an average content of structural units derived from ethylene oxide of 8 to 50% by mass. [6] The pressure-sensitive adhesive composition according to any one of [1] to [5] above, wherein the oxyalkylene polymer has an average number of hydroxyl groups per molecule of 1.5 to 3.0. [7] The pressure-sensitive adhesive composition according to any one of [1] to [6] above, wherein the oxyalkylene polymer A comprises an oxyalkylene polymer A1 having 3 hydroxyl groups per molecule and an oxyalkylene polymer A2 having 2 hydroxyl groups per molecule. [8] The pressure-sensitive adhesive composition according to any one of [1] to [7] above, wherein the oxyalkylene polymer A has an average content of structural units derived from ethylene oxide of 0 to 80% by mass. [9] The pressure-sensitive adhesive composition according to any one of the above-mentioned [1] to [8], wherein the oxyalkylene polymer B has a number average molecular weight of 4000 to 30000.
[10] The pressure-sensitive adhesive composition according to any one of the above-mentioned [1] to [9], which is used to form a pressure-sensitive adhesive to be in contact with skin.
[11] A pressure-sensitive adhesive composition comprising a hydroxyl-terminated urethane prepolymer, a polyisocyanate compound, and a tin-free catalyst, wherein the hydroxyl-terminated urethane prepolymer has an average content of ethylene oxide-based structural units of 8 to 50% by mass.
[12] A method for producing a pressure-sensitive adhesive composition by reacting an oxyalkylene polymer and a diisocyanate compound in the presence of a tin-free catalyst to obtain a hydroxyl-terminated urethane prepolymer, and then mixing the hydroxyl-terminated urethane prepolymer with a polyisocyanate compound, wherein the oxyalkylene polymer comprises oxyalkylene polymer A having two or more hydroxyl groups per molecule and oxyalkylene polymer B having one hydroxyl group per molecule, and the hydroxyl-terminated urethane prepolymer has an average content of ethylene oxide-based structural units of 8 to 50% by mass.
[13] A pressure-sensitive adhesive composition comprising a cured product of the pressure-sensitive adhesive composition according to any one of [1] to
[11] above.
[14] The adhesive according to
[13] above, which passes the antibacterial test standards described in ISO 22196:2011 or JIS Z2801:2010.
[15] A patch having a substrate and an adhesive layer provided on at least a portion of the surface of the substrate, the adhesive layer comprising the adhesive according to
[13] or
[14] above.
[16] The patch according to
[15] above, which is an adhesive tape.
[17] A wearable device having a wearable device main body and an adhesive layer, the adhesive layer being provided on at least a portion of the surface of the wearable device facing the skin and comprising the adhesive according to
[13] or
[14] above.
[18] A wearable device kit comprising a wearable device main body and at least one of the adhesive according to
[13] or
[14] above and the patch according to
[15] or
[16] above.
[0010] The present invention provides an adhesive composition and a method for producing the same, which provide an adhesive that has a good balance of adhesive strength to the skin and adhesive strength to a device, is gentle on the skin (allows adherends to be attached and detached gently to the skin, and is low toxic), and has improved antibacterial properties.The present invention also provides an adhesive, a patch using the same, a wearable device, and a wearable device kit.
[0011] The definitions and meanings of terms and notations used in this specification are as follows. Skin refers to human skin. The number average molecular weight (Mn) and weight average molecular weight (Mw) are polystyrene-equivalent molecular weights determined by gel permeation chromatography (GPC) based on a calibration curve prepared using a standard polystyrene sample. The hydroxyl value is determined by measurement in accordance with JIS K 1557-1:2007. The degree of unsaturation is determined by measurement in accordance with JIS K 1557-3:2007. The colony formation rate is determined by a cytotoxicity test using a colony formation method using an extraction method in accordance with ISO 10993-5:2009 "Biological evaluation of medical devices - Part 5: In vitro cytotoxicity testing." Specifically, it can be determined by the method described in the Examples. The isocyanate index is the equivalent ratio ([isocyanate group] / [active hydrogen-containing group]) of the isocyanate group to be reacted to an active hydrogen-containing group (e.g., a hydroxyl group), expressed as a percentage.
[0012] [Adhesive Composition] An adhesive composition according to an embodiment of the present invention (hereinafter referred to as the present embodiment) comprises a hydroxyl-terminated urethane prepolymer and a polyisocyanate compound, the hydroxyl-terminated urethane prepolymer being a reaction product of an oxyalkylene polymer and a diisocyanate compound in the presence of a tin-free catalyst, the oxyalkylene polymer comprising an oxyalkylene polymer A having two or more hydroxyl groups per molecule and an oxyalkylene polymer B having one hydroxyl group per molecule, the hydroxyl-terminated urethane prepolymer having an average content of ethylene oxide-based structural units of 8 to 50 mass%. An adhesive composition using a hydroxyl-terminated urethane prepolymer having an average content of ethylene oxide-based structural units within a predetermined range, which is produced by reacting a specific oxyalkylene polymer with a diisocyanate compound in the presence of a tin-free catalyst, provides an adhesive having a good balance of adhesion to skin and adhesion to devices, and is gentle on the skin (enabling adherends to be attached and detached gently to the skin, and having low toxicity). The adhesive composition of this embodiment can be used to form an adhesive that comes into contact with the skin.
[0013] The average content of ethylene oxide-based structural units (hereinafter abbreviated as "EO units") in the pressure-sensitive adhesive composition is not particularly limited, but from the viewpoint of obtaining a pressure-sensitive adhesive that has a good balance between adhesive strength to the skin and adhesive strength to a device, is gentle on the skin (allows the adherend to be fixed and detached gently to the skin, and is low toxic), and has improved antibacterial properties, it is preferably 8 to 50 mass%, more preferably 8 to 30 mass% or less, even more preferably 8 to 20 mass%, even more preferably 8 to 13 mass%, and particularly preferably 8 to 11 mass%. The average content of EO units in the pressure-sensitive adhesive composition is derived from EO units that constitute the oxyalkylene chain of the oxyalkylene polymer in the hydroxyl-terminated urethane prepolymer, and is 13 It can be determined by analyzing the monomer composition of the oxyalkylene chain in the pressure-sensitive adhesive composition by C-NMR (nuclear magnetic resonance) measurement.
[0014] (Hydroxyl Group-Terminated Urethane Prepolymer) The hydroxyl group-terminated urethane prepolymer of this embodiment is a reaction product of an oxyalkylene polymer and a diisocyanate compound in the presence of a tin-free catalyst.
[0015] The average content of EO units in the hydroxyl-terminated urethane prepolymer is not particularly limited as long as it is 8 to 50% by mass, but is preferably 8 to 30% by mass, more preferably 8 to 20% by mass, even more preferably 8 to 13% by mass, and particularly preferably 8 to 11% by mass. The lower the average content of EO units in the hydroxyl-terminated urethane prepolymer, the lower the toxicity to the skin. By keeping the average content of EO units in the hydroxyl-terminated urethane prepolymer within the above range, it is possible to fix and detach an adherend gently to the skin, and a pressure-sensitive adhesive having a good balance of adhesion to the skin and adhesion to a device and improved antibacterial properties can be easily obtained.
[0016] The EO units in the hydroxyl group-terminated urethane prepolymer are derived from the EO units constituting the oxyalkylene chain of the oxyalkylene polymer, 13 The average content can be determined by analyzing the monomer composition of the oxyalkylene chain in the hydroxyl-terminated urethane prepolymer by C-NMR (nuclear magnetic resonance) measurement.
[0017] <Oxyalkylene Polymer> The oxyalkylene polymer includes an oxyalkylene polymer A (hereinafter also simply referred to as "polymer A") having two or more hydroxyl groups per molecule, and an oxyalkylene polymer B (hereinafter also simply referred to as "polymer B") having one hydroxyl group per molecule. It is preferred that the hydroxyl groups of polymer A and polymer B react with the isocyanate group of the diisocyanate compound to form a urethane bond, and that the unreacted hydroxyl groups are terminal hydroxyl groups of the molecular chain of the hydroxyl-terminated urethane prepolymer.
[0018] The average content of EO units in the oxyalkylene polymer is not particularly limited, but is preferably 8 to 50% by mass, more preferably 8 to 30% by mass, even more preferably 8 to 20% by mass, even more preferably 8 to 13% by mass, and particularly preferably 8 to 11% by mass. The average content of EO units in the oxyalkylene polymer refers to a weighted average value of the contents of EO units in each oxyalkylene polymer based on the blend amounts of multiple oxyalkylene polymers used in the synthesis of the hydroxyl group-terminated urethane prepolymer. The content of EO units in each oxyalkylene polymer is a value calculated based on the blend amount of EO in the raw materials used in the synthesis of the oxyalkylene polymer. Note that the content of EO units in the oxyalkylene polymer, like the content of EO units in the hydroxyl group-terminated urethane prepolymer, 13 The smaller the average content of EO units in the oxyalkylene polymer, the lower the toxicity to the skin, and by keeping the average content within the above range, it is possible to easily obtain a pressure-sensitive adhesive that can gently fix and detach an adherend to the skin, has a good balance of adhesive strength to the skin and adhesive strength to a device, and has improved antibacterial properties.
[0019] From the viewpoint of obtaining a pressure-sensitive adhesive that is gentle on the skin (allows for gentle fixation and detachment of an adherend to the skin and is low in toxicity) and has a good balance of adhesive strength to the skin and adhesive strength to a device, the oxyalkylene polymer preferably has an average number of hydroxyl groups per molecule of 1.5 to 3.0, more preferably 1.7 to 2.8, and even more preferably 1.9 to 2.6. The average number of hydroxyl groups per molecule of the oxyalkylene polymer refers to a weighted average value based on the blend amounts of multiple oxyalkylene polymers used in the synthesis of the hydroxyl-terminated urethane prepolymer. The oxyalkylene polymer may be one type of oxyalkylene polymer, or two or more types of oxyalkylene polymers.
[0020] The total content of polymer A and polymer B in the oxyalkylene polymer is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and still more preferably 100% by mass. From the viewpoint of obtaining a pressure-sensitive adhesive having a good balance between adhesive strength to skin and adhesive strength to a device, the content ratio of polymer A to polymer B in the oxyalkylene polymer is preferably 10 / 90 to 95 / 5, more preferably 30 / 70 to 90 / 10, even more preferably 50 / 50 to 90 / 10, and still more preferably 60 / 40 to 90 / 10, in terms of a mass ratio (polymer A / polymer B).
[0021] <<Oxyalkylene Polymer A>> Polymer A has two or more hydroxyl groups per molecule, preferably two to six. Polymer A may be one type of oxyalkylene polymer, or two or more types of oxyalkylene polymers. When polymer A is composed of two or more types of oxyalkylene polymers, it is easy to adjust the adhesive strength of the adhesive. When polymer A is composed of two or more types of oxyalkylene polymers, the average number of hydroxyl groups per molecule of polymer A is preferably 2.1 to 3.0, more preferably 2.2 to 2.9, and even more preferably 2.3 to 2.8. When the average number of hydroxyl groups of polymer A is within the above range, it is easy to obtain an adhesive that reduces the load on the skin to which the device is fixed and is less likely to leave adhesive residue on the skin. The average number of hydroxyl groups per molecule of polymer A can be calculated from the measured hydroxyl value and Mn of polymer A using the formula: hydroxyl value × Mn / 56100.
[0022] When polymer A is composed of two or more types of oxyalkylene polymers, examples of polymer A include an oxyalkylene polymer A1 (hereinafter simply referred to as "polymer A1") having three hydroxyl groups per molecule, and an oxyalkylene polymer A2 (hereinafter simply referred to as "polymer A2") having two hydroxyl groups per molecule. Polymer A1 may be a single type or two or more types. Similarly, polymer A2 may be a single type or two or more types. Polymer A may contain an oxyalkylene polymer having four or more hydroxyl groups per molecule. When polymer A is composed of polymer A1 and polymer A2, the weighted average value based on the composition ratio (blending amount) of polymer A1 and polymer A2, where polymer A1 has three hydroxyl groups per molecule and polymer A2 has two hydroxyl groups per molecule, can be considered to be the average number of hydroxyl groups of polymer A. For example, the average number of hydroxyl groups per molecule of Polymer A in Example 1 (Synthesis Example 1) described later can be calculated by the following formula (1): (3×0.36 / 8470+2×0.48 / 9510) / (0.36 / 8470+0.48 / 9510)=2.5...formula (1).
[0023] From the viewpoint of ease of adjustment, such as the ability to adjust the adhesive strength of the PSA by adjusting the ratio of polymer A1 and polymer A2, the total amount of polymer A1 and polymer A2 in 100 parts by mass of polymer A is preferably 85 parts by mass or more, more preferably 90 parts by mass or more, and even more preferably 95 parts by mass or more. It is particularly preferable that the total amount of polymer A1 and polymer A2 in 100 parts by mass of polymer A is 100 parts by mass, i.e., polymer A consists of polymer A1 and polymer A2.
[0024] From the viewpoint of good adhesive strength of the PSA and suppression of adhesive residue, the amount of polymer A1 is preferably 20 parts by mass or more, more preferably 25 to 95 parts by mass, and even more preferably 30 to 90 parts by mass, per 100 parts by mass of the total of polymer A1 and polymer A2. From the same viewpoint, the amount of polymer A2 is preferably 80 parts by mass or less, more preferably 5 to 75 parts by mass, and even more preferably 10 to 70 parts by mass, per 100 parts by mass of the total of polymer A1 and polymer A2. When polymer A consists of polymer A1 and polymer A2, from the viewpoint of good adhesive strength of the PSA and suppression of adhesive residue, the amount of polymer A2 is preferably 10 parts by mass or more, more preferably 10 to 300 parts by mass, and even more preferably 50 to 200 parts by mass, per 100 parts by mass of polymer A1.
[0025] For example, when polymer A consists of polymer A1 and polymer A2, the content of polymer A1 is preferably 10 to 45 parts by mass, more preferably 15 to 40 parts by mass, and even more preferably 30 to 40 parts by mass, per 100 parts by mass of polymer A1, polymer A2, and polymer B in the oxyalkylene polymer, from the viewpoint of obtaining a pressure-sensitive adhesive having a good balance between adhesive strength to skin and adhesive strength to a device. From the same viewpoint, the content of polymer A2 is preferably 15 to 50 parts by mass, more preferably 30 to 50 parts by mass, and even more preferably 40 to 50 parts by mass, per 100 parts by mass of polymer A1, polymer A2, and polymer B in the oxyalkylene polymer. From the same viewpoint, the content of polymer B is preferably 5 to 40 parts by mass, more preferably 10 to 35 parts by mass, and even more preferably 10 to 20 parts by mass, per 100 parts by mass of polymer A1, polymer A2, and polymer B in the oxyalkylene polymer. The content ratios of polymer A1, polymer A2 and polymer B are preferably polymer A2, polymer A1 and polymer B in descending order.
[0026] The average content of EO units in polymer A is preferably 0 to 80% by mass, more preferably 0 to 70% by mass, even more preferably 0 to 60% by mass, and still more preferably 0 to 50% by mass. 13The monomer composition of the oxyalkylene chain in polymer A can be analyzed and determined by C-NMR measurement. For example, when the oxyalkylene chain in polymer A is composed of EO units and PO units, the content of EO units can be calculated based on the area of the peak representing the methylene group of the EO unit and the area of the peak representing the methyl group of the PO unit. When polymer A is composed of, for example, polymer A1 and polymer A2, the content of EO units for each of polymer A1 and polymer A2 is also calculated similarly. The average content of EO units in polymer A can be considered to be a value calculated from the amount of EO in the raw materials used to synthesize polymer A. When polymer A is composed of, for example, polymer A1 and polymer A2, the weighted average of the content of EO units in polymer A1 and the content of EO units in polymer A2 based on the compositional proportions (amounts) of polymer A1 and polymer A2 can be considered to be the average content of EO units in polymer A.
[0027] From the viewpoints of achieving good adhesive strength of the PSA, suppressing adhesive residue, and forming a PSA layer with good flexibility, the Mn of polymer A is preferably 1,000 to 50,000, more preferably 5,000 to 30,000, and even more preferably 8,000 to 25,000. The Mw / Mn (molecular weight distribution) of polymer A is close to 1. The narrower the molecular weight distribution, the less likely the hydroxyl-terminated urethane prepolymer to become highly viscous, and the more efficient the synthesis. Therefore, the Mw / Mn is preferably 1.25 or less, more preferably 1.22 or less, and even more preferably 1.20 or less. Furthermore, from the viewpoints of achieving good curing of the hydroxyl-terminated urethane prepolymer and suppressing adhesive residue of the PSA, the closer the unsaturation level of polymer A is to 0 meq / g, the more preferable it is, and the more preferable it is 0.020 meq / g or less, more preferably 0.018 meq / g or less, and even more preferably 0.015 meq / g or less. When polymer A is composed of two or more kinds of oxyalkylene polymers, it is preferable that each of the oxyalkylene polymers has Mn, Mw / Mn and degree of unsaturation within the above ranges.
[0028] The synthesis method of polymer A is not particularly limited, but can be obtained, for example, by ring-opening addition polymerization of a compound having a cyclic ether structure, preferably an alkylene oxide, with an initiator having two or more active hydrogens in the presence of a catalyst. When polymer A consists of polymer A1 and polymer A2, a method can also be used in which an initiator having three active hydrogens and an initiator having two active hydrogens are used in combination to perform ring-opening addition polymerization of a compound having a cyclic ether structure, thereby simultaneously producing polymer A1 and polymer A2. From the viewpoint of more accurately adjusting the blending amounts of polymer A1 and polymer A2, a method in which polymer A1 obtained by ring-opening addition polymerization of a compound having a cyclic ether structure with an initiator having three active hydrogens and polymer A2 obtained by ring-opening addition polymerization of a compound having a cyclic ether structure with an initiator having two active hydrogens are separately synthesized and then mixed is preferred.
[0029] The compound having a cyclic ether structure is preferably linear or branched and has 2 to 14 carbon atoms, more preferably 2 to 10 carbon atoms, and even more preferably 2 to 4 carbon atoms. The compound having a cyclic ether structure may be one type alone or two or more types. Examples of compounds having a cyclic ether structure include ethylene oxide (EO), propylene oxide (PO), 1,2-butylene oxide, 2,3-butylene oxide, methyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, lauryl glycidyl ether, hexyl glycidyl ether, and tetrahydrofuran. Of these, EO and PO are preferred.
[0030] When two or more compounds having a cyclic ether structure are used in combination, the arrangement of the oxyalkylene groups derived from each compound in the polymer A may be random or block.
[0031] Examples of groups having active hydrogen in the initiator include a hydroxyl group, a carboxyl group, and an amino group having a hydrogen atom bonded to a nitrogen atom. Of these, a hydroxyl group is preferred, and an alcoholic hydroxyl group is more preferred. Examples of initiators having three hydroxyl groups include glycerin, trimethylolethane, trimethylolpropane, and 1,2,6-hexanetriol. Of these, one type may be used alone, or two or more types may be used in combination. Examples of initiators having two hydroxyl groups include ethylene glycol, diethylene glycol, propylene glycol, and dipropylene glycol. Of these, one type may be used alone, or two or more types may be used in combination.
[0032] The number of active hydrogens in the initiator usually corresponds to the number of hydroxyl groups per molecule of the oxyalkylene polymer. Polymer A1 can be synthesized, for example, using glycerin as an initiator. Polymer A2 can be synthesized, for example, using propylene glycol as an initiator. The initiators used as raw materials for synthesizing the oxyalkylene polymer are: 13 When polymer A is composed of polymer A1 and polymer A2, the type and amount of polymer A can be identified by C-NMR measurement. 13 The ratio of polymer A1 to polymer A2 is determined by determining the content of oxyalkylene groups such as EO units and PO units bound to each initiator from information on the type and amount of the initiator obtained by C-NMR measurement.
[0033] Ring-opening addition polymerization can be carried out using known catalysts, such as alkali catalysts such as potassium hydroxide, transition metal compound-porphyrin complex catalysts such as complexes obtained by reacting an organoaluminum compound with porphyrin, composite metal cyanide complex catalysts, and catalysts made of phosphazene compounds. Among these catalysts, composite metal cyanide complex (DMC) catalysts are preferred because they tend to produce oxyalkylene polymers with narrow molecular weight distributions and relatively low viscosity. Known compounds can be used as composite metal cyanide complexes, such as zinc hexacyanocobaltate complexes with tert-butanol as a ligand. Synthesis of oxyalkylene polymers by ring-opening addition polymerization using a DMC catalyst can be carried out by known methods, for example, production methods described in WO 2003 / 062301, WO 2004 / 067633, JP 2004-269776 A, JP 2005-15786 A, WO 2013 / 065802, JP 2015-10162 A, etc. can be applied.
[0034] As the polymer A, commercially available products can also be used. Commercially available products of polymer A include, for example, "Preminol (registered trademark; hereinafter, abbreviated) S 4013F," "Preminol S 4318F," "Preminol S 3011," "Preminol 5001F," "Preminol 7001K," "Preminol 7012," "Preminol S 4011," "Preminol S 4015," "Preminol S 3025," and "Preminol S 6420" (all manufactured by AGC Inc.); "ACCLAIM (registered trademark; hereinafter, abbreviated) 4200," "ACCLAIM 8200," "ACCLAIM 2220N," "ACCLAIM 3300N," "ACCLAIM 4220N," "ACCLAIM 6300," "Acclaim 2200," and "ACCLAIM 6320N" (both manufactured by Covestro).
[0035] <<Oxyalkylene Polymer B>> The oxyalkylene polymer B has one hydroxyl group per molecule. The polymer B may be one type of oxyalkylene polymer, or two or more types of oxyalkylene polymers. The number of hydroxyl groups of the polymer B is, like the polymer A, 13 This can be confirmed by identifying the type and amount of the initiator used in the synthesis by C-NMR measurement.
[0036] From the viewpoints of forming a pressure-sensitive adhesive layer with good flexibility, achieving good adhesive strength of the pressure-sensitive adhesive, and suppressing adhesive residue, the Mn of polymer B is preferably 4,000 to 30,000, more preferably 4,500 to 25,000, and even more preferably 5,000 to 20,000. The Mw / Mn of polymer B is preferably less than 1.20, more preferably less than 1.13, and even more preferably less than 1.10, because the closer to 1 and the narrower the molecular weight distribution, the less likely the hydroxyl-terminated urethane prepolymer will become highly viscous and the more efficient the synthesis. Furthermore, from the viewpoints of achieving good curing of the hydroxyl-terminated urethane prepolymer and suppressing adhesive residue in the pressure-sensitive adhesive layer, the degree of unsaturation of polymer B is preferably 0.015 meq / g or less, more preferably 0.013 meq / g or less, and even more preferably 0.010 meq / g or less, with the degree of unsaturation being closer to 0 meq / g being preferable. When polymer B is composed of two or more kinds of oxyalkylene polymers, it is preferable that each of the oxyalkylene polymers has Mn, Mw / Mn and degree of unsaturation within the above ranges.
[0037] The synthesis method of polymer B is not particularly limited, but it can be obtained, for example, by ring-opening addition polymerization of a compound having a cyclic ether structure, preferably an alkylene oxide, to an initiator having one active hydrogen in the presence of a catalyst. The compound having a cyclic ether structure is the same as that described for polymer A. Preferably, PO is used alone, or EO and PO are used in combination.
[0038] From the viewpoint of obtaining a pressure-sensitive adhesive having a good balance between adhesive strength to skin and adhesive strength to a device and having suppressed crystallinity, the average content of EO units in Polymer B is preferably 0 to 80 mass%, more preferably 0 to 60 mass%, and even more preferably 0 to 50 mass%. The average content of EO units in Polymer B is determined in the same manner as in the case of Polymer A.
[0039] Examples of the group having an active hydrogen in the initiator include the same as those in the case of polymer A, with a hydroxyl group being preferred and an alcoholic hydroxyl group being more preferred. As the initiator having one hydroxyl group, from the viewpoint of availability and the like, a monohydric alcohol having 2 to 4 carbon atoms is preferred, for example, n-propanol, isopropanol, n-butanol, sec-butanol, isobutanol, and tert-butanol are mentioned, and among these, n-butanol, sec-butanol, isobutanol, and tert-butanol are preferred. The initiator may be used alone or in combination of two or more types. The ring-opening addition polymerization can be carried out by a known method, as in the case of polymer A.
[0040] Commercially available products can also be used as the polymer B. Examples of commercially available products of the polymer B include "Preminol S 1011" and "Preminol S 1004F" (manufactured by AGC Inc.).
[0041] <Diisocyanate Compound> The diisocyanate compound used in the synthesis of the hydroxyl group-terminated urethane prepolymer is an organic compound having two isocyanate groups per molecule. The diisocyanate compound may be any of an aliphatic diisocyanate compound, an alicyclic diisocyanate compound, an aromatic diisocyanate compound, and an araliphatic diisocyanate compound. The diisocyanate compound may be used alone or in combination of two or more types.
[0042] The aliphatic diisocyanate compound may be either linear or branched, and examples thereof include tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2-methylpentane-1,5-diisocyanate, and 3-methylpentane-1,5-diisocyanate. Examples of alicyclic diisocyanate compounds include isophorone diisocyanate (IPDI), hydrogenated xylylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate (HMDI), 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, and 1,3-bis(isocyanatomethyl)cyclohexane. Examples of aromatic diisocyanate compounds include tolylene diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, dialkyldiphenylmethane diisocyanate, and tetraalkyldiphenylmethane diisocyanate. Examples of aromatic aliphatic diisocyanate compounds include xylylene diisocyanate and tetramethylxylylene diisocyanate (TMXDI). Of these, HDI, IPDI, HMDI, and TMXDI are preferred, with HDI being more preferred, from the viewpoints of obtaining a pressure-sensitive adhesive layer with good curing properties of the hydroxyl group-terminated urethane prepolymer and good flexibility.
[0043] Furthermore, as the diisocyanate compound, a bifunctional isocyanate-terminated urethane prepolymer obtained by previously reacting the above-mentioned diisocyanate compound with a diol (for example, ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, etc.) can also be used.
[0044] <Tin-free catalyst> The tin-free catalyst is a urethane-forming catalyst that does not contain tin. In this embodiment, a tin-containing catalyst is not used as the urethane-forming catalyst. The pressure-sensitive adhesive of this embodiment does not contain tin or tin compounds, from the viewpoint of obtaining a pressure-sensitive adhesive that is low-toxic and can fix and detach an adherend gently to the skin.
[0045] Examples of tin-free catalysts include tertiary amine catalysts and catalysts containing metals other than tin. The catalysts may be used alone or in combination of two or more. From the viewpoint of better reaction promotion, the tin-free catalyst is preferably a catalyst containing a metal other than tin. Examples of metals contained in organometallic catalysts containing metals other than tin include zinc, bismuth, titanium, lead, iron, cobalt, and zirconium. Among these, from the viewpoints of low toxicity to the skin, ease of handling, etc., zinc and bismuth are preferred, and zinc is more preferred. From the viewpoint of better reaction promotion, the catalyst containing a metal other than tin is preferably an organometallic catalyst containing a metal other than tin. The metals contained in organometallic catalysts are the same as the metals contained in the catalysts containing metals other than tin, and the preferred metals are also the same.
[0046] Examples of tertiary amine catalysts include triethylamine, triethylenediamine, 1,8-diazabicyclo[5.4.0]-7-undecene (DBU), etc. Examples of organometallic catalysts containing metals other than tin include zinc compounds such as zinc carboxylates (e.g., zinc naphthenate, zinc 2-ethylhexanoate), and zinc acetylacetonate; bismuth compounds (e.g., bismuth 2-ethylhexanoate, bismuth neodecanoate); titanium compounds (e.g., dibutyltitanium dichloride, tetrabutyltitanium, butoxytitanium trichloride); lead compounds (e.g., lead oleate, lead 2-ethylhexanoate, lead benzoate, lead naphthenate); iron compounds (e.g., iron 2-ethylhexanoate, iron acetylacetonate); cobalt compounds (e.g., cobalt benzoate, cobalt 2-ethylhexanoate); and zirconium compounds (e.g., zirconium naphthenate).
[0047] The amount of the tin-free catalyst used in the reaction between the oxyalkylene polymer and the diisocyanate compound is preferably more than 0.001 part by mass and less than 0.050 part by mass, more preferably 0.005 to 0.045 parts by mass, and particularly preferably 0.010 to 0.040 parts by mass, per 100 parts by mass of the oxyalkylene polymer, from the viewpoints of providing a good reaction-accelerating effect and reducing the amount of residual metal components.
[0048] (Polyisocyanate Compound) The polyisocyanate compound is a curing agent for the hydroxyl-terminated urethane prepolymer. The polyisocyanate compound is a compound having two or more isocyanate groups per molecule, and may be used alone or in combination of two or more. As the polyisocyanate compound, a diisocyanate compound is preferred from the viewpoints of availability and reactivity. Furthermore, from the viewpoints of good adhesive strength of the pressure-sensitive adhesive and suppression of adhesive residue, a polyisocyanate compound having three or more isocyanate groups per molecule is preferred. The amount of the polyisocyanate compound to be added is not particularly limited, but is preferably 1 to 40 parts by mass, more preferably 2 to 30 parts by mass, and particularly preferably 5 to 20 parts by mass per 100 parts by mass of the hydroxyl-terminated urethane prepolymer.
[0049] Specific examples of the diisocyanate compound include the same as the specific examples of the diisocyanate compound constituting the hydroxyl group-terminated urethane prepolymer described above. Examples of the polyisocyanate compound having three or more isocyanate groups per molecule include isocyanurate-modified compounds, biuret-modified compounds, and allophanate-modified compounds, which are derivatives of the diisocyanate compounds described above, and trifunctional or higher isocyanate group-terminated urethane prepolymers (adducts), which are reaction products of diisocyanate compounds with polyols having three or more hydroxyl groups per molecule (e.g., trimethylolpropane).
[0050] (Other Components) The pressure-sensitive adhesive composition may contain other components in addition to the hydroxyl-terminated urethane prepolymer and the polyisocyanate compound. Examples of other components include various additives such as plasticizers, antioxidants, antistatic agents, fillers, UV absorbers, light stabilizers, conductivity-imparting agents, and leveling agents. A solvent may also be contained. The other components may be used alone or in combination of two or more, and may be blended in a content range that does not impair the effects of the present invention. In the pressure-sensitive adhesive composition (excluding the solvent), the total content of the hydroxyl-terminated urethane prepolymer and the polyisocyanate compound is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and even preferably 100% by mass, from the viewpoint of fully exhibiting the effects of the present invention.
[0051] The plasticizer can be selected from the viewpoints of compatibility with other components and wettability of the pressure-sensitive adhesive layer to the adherend, and examples thereof include fatty acid esters having 8 to 30 carbon atoms and phosphate esters. The antioxidant contributes to suppressing thermal degradation of the pressure-sensitive adhesive layer and includes, for example, phenolic, amine, sulfur, and phosphorus antioxidants. Of these, phenolic antioxidants are preferred due to their low toxicity to the skin. The antistatic agent contributes to suppressing damage to the circuit pattern due to electrostatic discharge and includes, for example, inorganic salts; ionic liquids containing imidazolium ions, pyridinium ions, ammonium ions, and the like; and surfactants. Examples of fillers include talc, calcium carbonate, and titanium oxide. Examples of UV absorbers include benzophenone-based, benzotriazole-based, salicylic acid-based, oxalic acid anilide-based, cyanoacrylate-based, and triazine-based UV absorbers. Examples of light stabilizers include hindered amine-based light stabilizers and UV stabilizers. Examples of conductivity-imparting agents include metal fine particles such as silver nanoparticles. Examples of the leveling agent include polymer leveling agents such as acrylic, vinyl, silicone, and fluorine-based leveling agents.
[0052] An adhesive composition according to one embodiment of the present invention comprises a hydroxyl-terminated urethane prepolymer, a polyisocyanate compound, and a tin-free catalyst, wherein the hydroxyl-terminated urethane prepolymer has an average content of ethylene oxide-based structural units of 8 to 50 mass%. The hydroxyl-terminated urethane prepolymer, polyisocyanate compound, and tin-free catalyst in the adhesive composition are preferably the same as the hydroxyl-terminated urethane prepolymer, polyisocyanate compound, and tin-free catalyst described above, respectively. Components other than the hydroxyl-terminated urethane prepolymer, polyisocyanate compound, and tin-free catalyst are also the same as the other components described above.
[0053] [Method for producing pressure-sensitive adhesive composition] The method for producing a pressure-sensitive adhesive composition of this embodiment is a method for producing a pressure-sensitive adhesive composition by reacting an oxyalkylene polymer and a diisocyanate compound in the presence of a tin-free catalyst to obtain a hydroxyl-terminated urethane prepolymer, and mixing the hydroxyl-terminated urethane prepolymer with a polyisocyanate compound, wherein the oxyalkylene polymer comprises an oxyalkylene polymer A having two or more hydroxyl groups per molecule and an oxyalkylene polymer B having one hydroxyl group per molecule, and the hydroxyl-terminated urethane prepolymer has an average content of ethylene oxide-based structural units of 8 to 50 mass%. Note that when mixing the hydroxyl-terminated urethane prepolymer with the polyisocyanate compound, other components that can be contained in the pressure-sensitive adhesive composition described above may also be mixed.
[0054] The hydroxyl-terminated urethane prepolymer is obtained by reacting an oxyalkylene polymer and a diisocyanate compound in the presence of a tin-free catalyst. The oxyalkylene polymer, diisocyanate compound, and tin-free catalyst are the same as those described above. The hydroxyl-terminated urethane prepolymer can be produced, for example, by a method in which the oxyalkylene polymer, diisocyanate compound, catalyst, and solvent are all charged into a reaction vessel at once, or by a method in which the diisocyanate compound is added dropwise or later to a reaction vessel containing the oxyalkylene polymer, catalyst, and solvent. From the viewpoint of ease of control of the molecular weight distribution of the hydroxyl-terminated urethane prepolymer due to preferential reaction of low-molecular-weight components in the synthetic raw materials, the method of adding the diisocyanate compound later is preferred.
[0055] Examples of the solvent include ketones such as acetone and methyl ethyl ketone; esters such as ethyl acetate; and aromatic hydrocarbons such as toluene and xylene. The solvent may be used alone or in combination of two or more. When a solvent is used, the amount used is preferably 50 to 500 parts by mass, more preferably 70 to 400 parts by mass, and even more preferably 80 to 300 parts by mass per 100 parts by mass of the oxyalkylene polymer in terms of the uniformity of the reaction system and synthesis efficiency.
[0056] Furthermore, from the viewpoint of efficiently obtaining a hydroxyl group-terminated urethane prepolymer having an appropriate molecular chain length, it is preferable to react the oxyalkylene polymer with the diisocyanate compound at an isocyanate index of less than 100, preferably 30 to 95, and more preferably 50 to 95.
[0057] From the viewpoint of promoting the urethanization reaction and suppressing side reactions, the reaction temperature is preferably less than 100° C., more preferably 70 to 95° C., and even more preferably 75 to 90° C. After completion of the reaction, a reaction terminator such as acetylacetone may be added to deactivate the catalyst.
[0058] The average number of hydroxyl groups per molecule of the hydroxyl-terminated urethane prepolymer is preferably less than 3.0, more preferably 1.7 to 2.9, and even more preferably 1.8 to 2.5, from the viewpoint of obtaining a pressure-sensitive adhesive having a good balance between adhesive strength to skin and adhesive strength to a device.
[0059] The isocyanate index of the polyisocyanate compound to be reacted with the hydroxyl group-terminated urethane prepolymer is preferably greater than 100, more preferably from 101 to 1,500, and even more preferably from 105 to 1,000.
[0060] [Adhesive] The adhesive of this embodiment is a cured product of the adhesive composition of this embodiment described above. The adhesive is obtained as a reaction product between a hydroxyl group-terminated urethane prepolymer in the adhesive composition and a polyisocyanate compound. As described below, for example, the adhesive composition can be applied to a substrate and cured to form an adhesive layer.
[0061] In the reaction between the hydroxyl-terminated urethane prepolymer and the polyisocyanate compound, a catalyst and a solvent may be used as necessary. When a catalyst is used, the urethane-forming catalyst, which is a non-tin-containing catalyst as described above, can be used. The catalyst may be the same as or different from the catalyst used in the synthesis of the hydroxyl-terminated urethane prepolymer. If the catalyst used in the synthesis of the hydroxyl-terminated urethane prepolymer remains, the remaining catalyst may also exert a catalytic effect in the reaction between the hydroxyl-terminated urethane prepolymer and the polyisocyanate compound. When a catalyst is added during the reaction between the hydroxyl-terminated urethane prepolymer and the polyisocyanate compound, the amount added is preferably more than 0.001 part by mass and less than 0.050 parts by mass, preferably 0.005 to 0.045 parts by mass, more preferably 0.010 to 0.040 parts by mass, per 100 parts by mass of the hydroxyl-terminated urethane prepolymer and the polyisocyanate compound combined. When a catalyst is added, it is preferable to add a reaction terminator to deactivate the catalyst after completion of the reaction.
[0062] The solvent used in the reaction between the hydroxyl-terminated urethane prepolymer and the polyisocyanate compound may be the same as that used in the synthesis of the hydroxyl-terminated urethane prepolymer described above. The solvent may be the same as or different from that used in the synthesis of the hydroxyl-terminated urethane prepolymer. If any solvent remains from the synthesis of the hydroxyl-terminated urethane prepolymer, it may be used as is. When a solvent is used, the amount used is preferably 50 to 500 parts by mass, more preferably 70 to 400 parts by mass, and even more preferably 80 to 300 parts by mass per 100 parts by mass of the total of the hydroxyl-terminated urethane prepolymer and the polyisocyanate compound.
[0063] The reaction temperature between the hydroxyl group-terminated urethane prepolymer and the polyisocyanate compound is preferably less than 120°C, more preferably 40 to 110°C, and even more preferably 50 to 100°C, from the viewpoint of promoting the urethane reaction and suppressing side reactions.
[0064] The pressure-sensitive adhesive of the present embodiment is preferably low in toxicity when applied to the skin, and the colony formation rate in a cytotoxicity test using the colony formation method specified in ISO 10993-5:2009 is preferably 50% or more, more preferably 70% or more.
[0065] When applied to the skin, the pressure-sensitive adhesive of the present embodiment preferably passes the antibacterial test standards described in ISO22196:2011 or JIS Z2801:2010.
[0066] [Patch] The patch of the present embodiment has a substrate and a pressure-sensitive adhesive layer provided on at least a part of the surface of the substrate, and the pressure-sensitive adhesive layer contains the pressure-sensitive adhesive of the present embodiment described above. A patch having a pressure-sensitive adhesive layer formed using the pressure-sensitive adhesive composition of the present embodiment has good adhesive strength to the skin of the pressure-sensitive adhesive layer, is less likely to leave adhesive residue, and can be suitably applied to the skin.
[0067] The patch may be in the form of a sheet of a desired size depending on the mode of use, or may be cut to a desired size for use. From the viewpoint of convenience, the patch is preferably an adhesive tape.
[0068] The pressure-sensitive adhesive composition used to form the pressure-sensitive adhesive layer may be a one-component type in which a hydroxyl-terminated urethane prepolymer and a polyisocyanate compound as a curing agent are pre-mixed, depending on the mode of use of the patch, or may be a two-component type consisting of a first part containing a hydroxyl-terminated urethane prepolymer and a second part containing a polyisocyanate compound as a curing agent.
[0069] The thickness of the adhesive layer is preferably 5 to 100 μm, more preferably 10 to 80 μm, and even more preferably 20 to 50 μm, from the viewpoint of ensuring good adhesive strength to the skin.
[0070] The substrate is preferably made of a material that has good conformability to the shape of the skin or device of the patch and is not easily broken during use of the patch, and examples thereof include resin films, cloths, paper, etc. The substrate may be made of one type alone or two or more types in combination, or may be a composite material formed by lamination or the like. Examples of materials for the resin film include polyurethane; polyamide; acrylic resin; polyolefins such as polyethylene, polypropylene, and ethylene-vinyl acetate copolymer; polyester, etc. Of these, polyurethane and polyamide are preferred, and thermoplastic polyurethane is more preferred, from the viewpoint of good moisture permeability when applied to the skin. Examples of cloth include woven fabrics, nonwoven fabrics, knitted fabrics, nets, etc., and examples of materials include the resins used for the resin films described above, as well as natural fibers such as cotton, silk, and wool.
[0071] The thickness of the substrate is not particularly limited as long as it can ensure conformability to the shape of the skin and the device and is not easily broken when the patch is used, and is, for example, 10 to 500 μm.
[0072] The surface of the adhesive layer of the patch is preferably covered with a release liner to protect the surface of the adhesive layer before use. The release liner is appropriately peeled off from the surface of the adhesive layer when the patch is used. Release liners used in known adhesive tapes for skin can be applied. Examples of release liners include high-quality paper, glassine paper, and parchment paper coated with a release agent such as silicone resin or fluororesin, as well as resin anchor coated or polyethylene-laminated high-quality paper coated with a release agent such as silicone resin or fluororesin. Transparent resin films can also be used as release liners, such as polyester films. The thickness of the release liner is not particularly limited as long as it can protect the adhesive layer and is easy to peel off during use, and is, for example, 15 to 200 μm.
[0073] The pressure-sensitive adhesive layer may be provided, for example, in one or more locations on a portion of the surface of the resin film substrate, on only a portion of one side, or on the entire surface of one side, or on both sides of the surface of the substrate.
[0074] The adhesive strength of the adhesive layer to the skin is preferably 1.0 to 5.0 N / 15 mm, more preferably 1.0 N / 15 mm or more but less than 3.0 N / 15 mm, which can be said to have adequate adhesive strength to the skin. Furthermore, when the adhesive layer is adhered to a device sealant, for example, it is preferable that the adhesive strength to phenolic resin, a common sealant material, is greater than the adhesive strength to the skin. From the viewpoint of adequately fixing the device, the adhesive strength to phenolic resin is preferably 2.5 N / 15 mm or more, more preferably 3.0 N / 15 mm or more. The difference between the adhesive strength to phenolic resin and the adhesive strength to the skin is preferably 1.8 N / 15 mm or more, more preferably 2.5 N / 15 mm or more. Such a difference indicates a good balance between the adhesive strength to the skin and the adhesive strength to the device, and can be said to impose a low load on the skin to which the device is fixed. The adhesive strength referred to here is a value measured according to a method in accordance with JIS Z 0237:2009, specifically, measured by the method described in the Examples.
[0075] The adhesive patch can be produced using known methods, such as a method of applying a pressure-sensitive adhesive composition to a release liner, curing the composition to form a pressure-sensitive adhesive layer, and laminating a substrate. Another example is a method of applying a pressure-sensitive adhesive composition to a substrate, curing the composition to form a pressure-sensitive adhesive layer, and laminating a release liner. The method for applying the pressure-sensitive adhesive composition is not particularly limited, and known methods such as bar coating, knife coating, roll coating, blade coating, die coating, microgravure coating, comma coating, slot die coating, lip coating, and cast coating can be used. After application, the pressure-sensitive adhesive composition is preferably cured by, for example, hot air drying at 40 to 80°C to sufficiently volatilize the solvent contained in the pressure-sensitive adhesive composition, thereby forming a pressure-sensitive adhesive layer.
[0076] [Wearable Device] The wearable device of the present embodiment is a wearable device having a wearable device main body and an adhesive layer, the adhesive layer being provided on at least a portion of the surface of the wearable device facing the skin, and containing the adhesive of the present embodiment. By using the adhesive composition of the present embodiment described above, an adhesive layer is formed that has a good balance of adhesive strength to the skin and adhesive strength to the device, and is gentle on the skin (allowing the adherend to be gently fixed and detached from the skin, and is low-toxicity). For this reason, the adhesive of the present embodiment is suitable for application to wearable devices that are attached to the skin.
[0077] The adhesive layer can be formed in the form of the adhesive patch described above, for example. Alternatively, the adhesive layer can be formed in a form sandwiched between release liners on both sides, and the wearable device body can be adhered to the skin via the adhesive layer alone, without using a substrate.
[0078] Examples of wearable devices that are attached to the skin include biosensors and environmental sensors, which can detect, for example, cardiac potential, pulse wave, body temperature, acceleration, heart rate, pulse rate, respiratory rate, electrocardiogram, electromyogram, activity level, blood pressure, and electroencephalogram.
[0079] [Wearable Device Kit] The wearable device kit of this embodiment includes a wearable device main body and at least one of the adhesive of this embodiment and the patch of this embodiment. In this way, the wearable device main body does not have to have an adhesive layer in advance, but may include the adhesive or the patch as a separate component so that the adhesive layer can be formed during use. The adhesive and the patch may be used alone or in combination.
[0080] The present invention will be specifically described below based on examples, but the present invention is not limited to the following examples, and various modifications are possible within the scope of the gist of the present invention.
[0081] [Measurement Methods] The methods for measuring various physical properties in the following Synthesis Examples and Production Examples are as follows.
[0082] (Number average molecular weight (Mn) and weight average molecular weight (Mw)) Mn and Mw were measured by gel permeation chromatography (GPC) under the following measurement conditions (polystyrene equivalent), and the molecular weight distribution (Mw / Mn) was calculated from these values. [Measurement conditions] - Instrument used: "HLC-8320GPC", manufactured by Tosoh Corporation - Column used: "TSKgel (registered trademark) SuperMultiporeHZ-M", manufactured by Tosoh Corporation - Detector: Refractive index (RI) detector - Detection temperature: 40°C - Eluent: Tetrahydrofuran - Flow rate: 0.350 mL / min - Sample concentration: 0.5% by mass - Sample injection amount: 10 μL - Standard sample: Polystyrene
[0083] (Ethylene oxide (EO) unit content) The EO unit content of each oxyalkylene polymer was determined based on the amounts of propylene oxide (PO) and EO used in the synthesis, and the amount of EO charged was considered to be the EO unit content in the oxyalkylene polymer. The average EO unit content of the hydroxyl group-terminated urethane prepolymer was taken as the weighted average of the EO unit contents in each of the raw material components.
[0084] (Hydroxyl Value) The hydroxyl value was determined in accordance with Method B (automatic potentiometric titration) of JIS K 1557-1:2007.
[0085] (Degree of unsaturation) The degree of unsaturation was measured in accordance with JIS K 1557-3:2007.
[0086] (Average Number of Hydroxyl Groups per Molecule of Oxyalkylene Polymer A) The number of hydroxyl groups per molecule of each of the oxyalkylene polymers A1-1 to A2-2 used as the oxyalkylene polymer A (the number of hydroxyl groups per molecule of the initiator used in the synthesis) was weighted based on the blending amount of each of the oxyalkylene polymers A1-1 to A2-2, and the weighted average was used as the average number of hydroxyl groups per molecule.
[0087] (Average number of hydroxyl groups per molecule of oxyalkylene polymer) The number of hydroxyl groups per molecule of each oxyalkylene polymer (oxyalkylene polymers A1-1 to A2-2 and B1) used in the synthesis of the hydroxyl-terminated urethane prepolymer was weighted and averaged based on the blending amount of each oxyalkylene polymer, and this value was regarded as the average number of hydroxyl groups per molecule.
[0088] [Materials Used] Details of the materials used in the following synthesis examples are shown below. TBA-DMC catalyst: zinc hexacyanocobaltate complex with tert-butanol as a ligand Adsorbent: synthetic magnesium silicate, "Kyoward (registered trademark) 600S", manufactured by Kyowa Chemical Industry Co., Ltd. 50M-HDI: hexamethylene diisocyanate (HDI), "Duranate (registered trademark) 50M-HDI", manufactured by Asahi Kasei Corporation XK627: "K-KAT XK627", manufactured by KING INDUSTRIES; zinc carboxylate: zinc (Zn)-containing urethanization catalyst Dibutyltin dilaurate, manufactured by Tokyo Chemical Industry Co., Ltd.; tin (Sn)-containing urethanization catalyst Dioctyltin dilaurate, "Neostan (registered trademark) U-810", manufactured by Nitto Kasei Kogyo Co., Ltd.; Sn-containing urethanization catalyst Curing agent (polyisocyanate compound): HDI-based polyisocyanate; "Duranate (registered trademark) E402-80B", manufactured by Asahi Kasei Corporation; solid content: approximately 80% by mass
[0089] [Synthesis of Oxyalkylene Polymer] (Synthesis Example 1-1) 1000 g of glycerin as an initiator and a TBA-DMC catalyst (metal concentration 46 ppm by mass) were placed in a pressure vessel, and the vessel was purged with nitrogen. The reaction solution was heated to 135°C while stirring, and 120 g of propylene oxide (PO) was added and reacted. After the temperature rise of the reaction solution stopped, it was cooled to 135°C, and while stirring the reaction solution, 3782.4 g of PO and 945.6 g of ethylene oxide (EO) were added to the vessel. After confirming that the internal pressure had not changed, an adsorbent was added, and neutralization and catalyst removal were performed to obtain an oxyalkylene polymer A1-1.
[0090] Synthesis Example 1-2 Oxyalkylene polymer A1-2 was synthesized in the same manner as in Synthesis Example 1-1, except that EO was not added and the amount of EO added was replaced with the amount of PO added.
[0091] Synthesis Example 1-3 An oxyalkylene polymer A2-1 was synthesized in the same manner as in Synthesis Example 1-1, except that the initiator in Synthesis Example 1-1 was changed from glycerin to propylene glycol.
[0092] Synthesis Example 1-4 An oxyalkylene polymer A2-2 was synthesized in the same manner as in Synthesis Example 1-2, except that in Synthesis Example 1-2, the initiator was changed from glycerin to propylene glycol, EO was not added, and the amount of EO added was replaced with the amount of PO added.
[0093] Synthesis Example 1-5 Oxyalkylene polymer B1 was synthesized in the same manner as in Synthesis Example 1-1, except that the initiator in Synthesis Example 1-1 was changed from glycerin to n-butanol, and after cooling the reaction solution, 2364 g of PO was added instead of EO.
[0094] Table 1 below shows various physical properties of the oxyalkylene polymers A1-1 to A2-2 and B1 produced in the above Synthesis Examples 1-1 to 1-5.
[0095]
[0096] [Synthesis of Hydroxyl-Terminated Urethane Prepolymer] (Synthesis Example 2-1) A reaction vessel equipped with a thermometer, a stirrer, and a cooling tube was charged with oxyalkylene polymer A1-1 (36 parts by mass), oxyalkylene polymer A2-1 (48 parts by mass), oxyalkylene polymer B1 (16 parts by mass), toluene 50.6 parts by mass, and ethyl acetate 50.6 parts by mass, and zinc (Zn)-containing urethanization catalyst K-KAT XK627 (0.038 parts) was added, and after mixing at 40 ° C., 1.7 parts by mass of HDI (isocyanate index 85) was added and reacted at 80 ° C. The average number of hydroxyl groups per molecule of the blended oxyalkylene polymer A (oxyalkylene polymers A1-1 and A2-1) was 2.5, and the average number of hydroxyl groups per molecule of the oxyalkylene polymer (oxyalkylene polymers A1-1, A2-1, and B1) was 2.1. The mixture was kept at 80° C. while being appropriately diluted with ethyl acetate, and reacted for 7 hours to obtain a transparent solution of hydroxyl-terminated urethane prepolymer U1 having a concentration of 50% by mass.
[0097] Synthesis Examples 2-2 to 2-11 Using the formulations shown in Table 2, hydroxyl group-terminated urethane prepolymers U2 to U11 were produced in the same manner as in Synthesis Example 1-1.
[0098]
[0099] [Production of adhesive patches] (Example 1) A liquid (adhesive composition) obtained by mixing 100 parts by mass of a 50% by mass solution of hydroxyl-terminated urethane prepolymer U1 and 5 parts by mass of curing agent (E402-80B) was degassed, and then coated on a polyester film (thickness 38 μm) serving as a release liner using a knife coater and dried for 2 minutes at 100° C. to form an adhesive layer with a thickness of 25 μm. A polyester film (thickness 75 μm) serving as a substrate was laminated on top of this adhesive layer, and the layer was cured in a hot air dryer at 40° C. for 3 days to produce an adhesive patch.
[0100] Examples 2 to 11 Patches were prepared in the same manner as in Example 1, except that the hydroxyl group-terminated urethane prepolymer U1 in Example 1 was changed to U2 to U11, respectively.
[0101] (Examples 12 to 14) Patches were prepared in the same manner as in Example 1, except that the adhesive composition obtained by mixing the hydroxyl-terminated urethane prepolymer U1 and the curing agent in Example 1 was changed to the following commercially available products. Example 12: Commercially available acrylic adhesive (1525L: manufactured by 3M) Example 13: Commercially available silicone adhesive (Micropore S2552: manufactured by 3M) Example 14: Commercially available silicone adhesive (2476P: manufactured by 3M)
[0102] [Evaluation of Patches] The following various evaluations were carried out on the patches prepared in Examples 1 to 14. The evaluation results are shown in Tables 3 and 4. Examples 1 to 4 are working examples, and Examples 5 to 14 are comparative examples.
[0103] <Adhesive Strength> (against Phenol Resin) The adhesive layer side of a patch (100 mm long, 15 mm wide) from which the release liner had been peeled off was placed on a phenolic resin plate ("SUMILITE (registered trademark) PL-1102", manufactured by Sumitomo Bakelite Co., Ltd.; 125 mm long, 30 mm wide, 2 mm thick), and a rubber roller was rolled back and forth from the substrate side of the patch at a load of 2 kg and a speed of 300 mm / min, thereby pressing the adhesive layer onto the phenolic resin plate. After leaving to stand for 20 minutes, the patch was peeled off at a peel angle of 90° and a speed of 300 mm / min, to measure the adhesive strength when the adherend was a phenolic resin (against phenolic resin) using a method in accordance with JIS Z 0237:2009. Table 3 shows the average of three measured values. The measured adhesive strength was also evaluated according to the following evaluation criteria (phenolic resin). A: 3.0 (N / 15mm) or more B: 2.5 (N / 15mm) or more but less than 3.0 (N / 15mm) C: 2.0 (N / 15mm) or more but less than 2.5 (N / 15mm) D: Less than 2.0 (N / 15mm) In the cases of ratings A and B, it can be said that the adhesive strength to phenolic resin, which is a typical material for sealing the circuit patterns of wearable devices, is sufficient. On the other hand, in the cases of ratings C and D, the adhesive strength to phenolic resin was insufficient.
[0104] (Against Skin) When the adherend was the skin of the forearm of a human (three subjects), the adhesive strength was measured in the same manner as when the adherend was a phenolic resin.
[0105] Table 3 shows the average values of the measured values. The measured adhesive strength was evaluated according to the following evaluation criteria (against skin). A+: 1.0 N / 15 mm or more and less than 2.7 N / 15 mm A: 2.7 N / 15 mm or more and less than 3.0 N / 15 mm B: Less than 1.0 N / 15 mm C: 3.0 N / 15 mm or more In the case of evaluation A, the adhesive strength to the skin is moderate and it can be said to be gentle on the skin. In the case of evaluation A+, it is said that there is little pain to the skin and the adhesive strength to the skin is more moderate. On the other hand, in the case of evaluation B, the adhesive strength to the skin is too small and it is easy to peel off. In addition, in the case of evaluation C, the adhesive strength is too large and it is difficult to peel off from the skin and it may be painful to peel off.
[0106] (Difference) The difference in adhesive strength between the phenolic resin and the skin was calculated by subtracting the adhesive strength to the skin from the adhesive strength to the phenolic resin measured above. The difference in adhesive strength between the phenolic resin and the skin was evaluated according to the following criteria: A: 2.5 N / 15 mm or more B: 1.8 N / 15 mm or more and less than 2.5 N / 15 mm C: 1.5 N / 15 mm or more and less than 1.8 N / 15 mm D: Less than 1.5 N / 15 mm
[0107] In the cases of ratings A and B, it can be said that the wearable device can be gently fixed to and detached from the skin. On the other hand, in the cases of ratings C and D, it is difficult to stably fix the wearable device to the skin.
[0108] (Skin Observation) In an atmosphere of 23°C and 50% RH, test pieces of the patch (20 mm long, 15 mm wide) were applied to the skin of the forearm of humans (3 subjects). After 1 hour, the test pieces were peeled off the skin, and the condition of the skin was visually observed. The observation results were evaluated according to the following evaluation criteria. A: No change from before application of the test piece. B: Redness was observed on some areas of the skin. C: Residual glue (adhesive residue) was observed on some areas. A rating of A can be said to be gentle on the skin. On the other hand, a rating of B or C is determined to be not gentle on the skin.
[0109] (Cytotoxicity Test) The adhesive layer collected from the adhesive patch was subjected to a cytotoxicity test (cell line: V79 cells, culture medium: MEM10 medium) using a colony formation method by extraction in accordance with ISO 10993-5:2009 "Biological evaluation of medical devices - Part 5: In vitro cytotoxicity tests" to determine the colony formation rate. The test liquid used was an extract obtained by extracting 1 g of the adhesive layer in the culture medium at 37°C for 24 hours.
[0110] The colony formation rate was evaluated according to the following evaluation criteria: A: 70% or more B: 50% or more but less than 70% C: Less than 50%. Grades A and B indicate no or very weak cytotoxicity and can be said to be gentle on the skin. On the other hand, grade C indicates stronger cytotoxicity. Note that "-" in the cytotoxicity test column in Table 3 indicates that the test has not been conducted.
[0111] (Antibacterial Test) The adhesive layer collected from the patch was subjected to an antibacterial test using Staphylococcus aureus and Escherichia coli in accordance with Japanese Industrial Standards JIS Z 2801:2010 (Antibacterial Products - Antibacterial Test Methods and Antibacterial Effect) and ISO22196:2011, Measurement of Antibacterial Activity on Plastics and Other Non-porous Surfaces. 0.4 mL of bacterial solution was dropped onto 50 mm x 50 mm (10 mm thick or less) test pieces (antibacterial processed product and non-processed product) and covered with a 40 mm x 40 mm film. The test pieces were cultured for 24 hours at 35 ± 1 °C and a relative humidity of 90% or more. After standing, the test bacteria on the test piece were washed out and collected, and then 1 cm 2 The number of viable bacteria per 1 cm of the untreated test piece after 24 hours was measured. The antibacterial activity value was calculated using the following formula: R = Ut - At R: antibacterial activity value Ut: 2 At: Average logarithm of viable bacteria count per 1 cm of antibacterial treated test piece after 24 hours 2The antibacterial activity was evaluated according to the following criteria: A: The antibacterial activity values for both Staphylococcus aureus and Escherichia coli were 2.0 or higher B: One of the antibacterial activity values for Staphylococcus aureus and Escherichia coli was 2.0 or higher, and the other was less than 2.0 C: The antibacterial activity values for both Staphylococcus aureus and Escherichia coli were less than 2.0 Evaluation A indicates that there was antibacterial activity. On the other hand, evaluations B and C indicated that there was no antibacterial activity. In Table 3, a "-" in the antibacterial test column indicates that the test had not been conducted.
[0112]
[0113]
[0114] [Evaluation Results] In Table 3, Examples 1 to 4 correspond to Examples of the present invention, and Examples 5 to 11 correspond to Comparative Examples of the present invention. If the adhesive strength (against phenolic resin) is rated A or B, the adhesive strength (against skin) is rated A+ or A, and the adhesive strength difference is rated A or B, low adhesion to the skin and high adhesion to the substrate are both achieved. Furthermore, if the skin observation rating is A, the adhesive can be peeled off without remaining on the skin, and can be said to be a skin-friendly adhesive. If the cytotoxicity rating is A or B, it can be said to be a material that ensures skin damage when applied to the skin and safety during long-term application. If the antibacterial test rating is A, it can be said to be a material that ensures antibacterial properties when applied to the skin and safety for long-term application. The adhesives of Examples 1 to 4 achieve both low adhesion to the skin and high adhesion to the substrate, can be peeled off without remaining on the skin, are skin-friendly, ensures skin damage when applied to the skin and safety during long-term application, and guarantee antibacterial properties when applied to the skin. In contrast, the adhesives of Examples 5 to 7 showed poor results in the antibacterial test and also showed poor adhesive strength. This is thought to be due to the low average content of EO units in the oxyalkylene polymer A used in the synthesis of the hydroxyl-terminated urethane prepolymer. The adhesives of Examples 8 and 9 do not contain oxyalkylene polymer B (monofunctional polyol), and without its use, no adhesive strength is exhibited and they cannot be used as patches. The adhesives of Examples 10 and 11 showed poor cytotoxicity evaluation. This is thought to be due to the use of a tin-based catalyst, which is considered to be highly toxic, in the synthesis of the urethane prepolymer.
[0115] Table 4 shows the results of a comparison of antibacterial tests between commercially available (medical) patches and the patch of the present invention. The commercially available (medical) patches of Examples 12 to 14 did not have antibacterial properties or did not achieve both low adhesion to the skin and high adhesion to the substrate.
Claims
1. A pressure-sensitive adhesive composition comprising a hydroxyl-terminated urethane prepolymer and a polyisocyanate compound, wherein the hydroxyl-terminated urethane prepolymer is a reaction product of an oxyalkylene polymer and a diisocyanate compound in the presence of a tin-free catalyst, the oxyalkylene polymer comprises an oxyalkylene polymer A having two or more hydroxyl groups per molecule, and an oxyalkylene polymer B having one hydroxyl group per molecule, and the hydroxyl-terminated urethane prepolymer has an average content of ethylene oxide-based constituent units of 8 to 50 mass%.
2. The pressure-sensitive adhesive composition according to claim 1, wherein the content of the tin-free catalyst is more than 0.001 parts by mass and less than 0.050 parts by mass per 100 parts by mass of the oxyalkylene polymer.
3. The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the tin-free catalyst is an organometallic catalyst.
4. The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the tin-free catalyst contains one or more metals selected from zinc and bismuth.
5. The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the oxyalkylene polymer has an average content of structural units based on ethylene oxide of 8 to 50 mass %.
6. The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the oxyalkylene polymer has an average number of hydroxyl groups per molecule of 1.5 to 3.
0.
7. The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the oxyalkylene polymer A comprises an oxyalkylene polymer A1 having 3 hydroxyl groups per molecule, and an oxyalkylene polymer A2 having 2 hydroxyl groups per molecule.
8. The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the oxyalkylene polymer A has an average content of structural units based on ethylene oxide of 0 to 80 mass %.
9. The pressure-sensitive adhesive composition according to claim 1 or 2, wherein the oxyalkylene polymer B has a number average molecular weight of 4,000 to 30,000.
10. The adhesive composition according to claim 1 or 2, which is used to form an adhesive for contact with skin.
11. A pressure-sensitive adhesive composition comprising a hydroxyl-terminated urethane prepolymer, a polyisocyanate compound, and a tin-free catalyst, wherein the hydroxyl-terminated urethane prepolymer has an average content of constituent units based on ethylene oxide of 8 to 50 mass%.
12. A method for producing a pressure-sensitive adhesive composition by reacting an oxyalkylene polymer and a diisocyanate compound in the presence of a tin-free catalyst to obtain a hydroxyl-terminated urethane prepolymer, and mixing the hydroxyl-terminated urethane prepolymer with a polyisocyanate compound, wherein the oxyalkylene polymer includes oxyalkylene polymer A having two or more hydroxyl groups per molecule and oxyalkylene polymer B having one hydroxyl group per molecule, and the hydroxyl-terminated urethane prepolymer has an average content of 8 to 50 mass% of constituent units based on ethylene oxide.
13. An adhesive which is a cured product of the adhesive composition according to claim 1.
14. The pressure-sensitive adhesive according to claim 13, which meets the antibacterial test standards set forth in ISO 22196:2011 or JIS Z2801:2010.
15. A patch comprising a substrate and an adhesive layer provided on at least a portion of the surface of the substrate, the adhesive layer comprising the adhesive according to claim 13.
16. The adhesive material according to claim 15, which is an adhesive tape.
17. A wearable device having a wearable device body and an adhesive layer, the adhesive layer being provided on at least a portion of a surface of the wearable device that faces the skin, and comprising the adhesive described in claim 13.
18. A wearable device kit comprising a wearable device body and at least one of the adhesive according to claim 13 and the patch according to claim 15.